An electromagnetic composite field assisted laser cladding device
By using an electromagnetic composite field-assisted laser cladding device, alternating electromagnetic fields are used to refine grains and improve microstructure, solving the microstructural defects of high-hardness alloy coatings, improving the wear resistance and density of the coatings, making it suitable for existing laser equipment, and reducing maintenance costs.
Patent Information
- Application Number
- CN202522390265.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-11
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2035-11-11
AI Technical Summary
Existing laser cladding technology has difficulty completely eliminating structural defects in high-hardness alloy coatings, especially cracks and porosity, which affects coating quality.
An alternating electromagnetic field device combined with a PLC intelligent control system is used to form an electromagnetic composite field that works synergistically on the molten pool to refine grains and improve microstructure uniformity. The coating is effectively improved by using alternating annular alternating electric and magnetic field devices.
It significantly improves the wear resistance of the cladding layer, reduces residual stress, and enhances the density and uniformity of the coating. At the same time, the device has a compact structure, is easy to move and control, is compatible with existing laser equipment, and reduces installation and maintenance costs.
Smart Images

Figure CN224981726U_ABST
Abstract
Description
Technical Field
[0001] This utility model relates to the field of laser cladding technology, and in particular to an electromagnetic composite field assisted laser cladding device. Background Technology
[0002] Laser cladding refers to a process in which selected coating materials are placed on the surface of a substrate using different feeding methods, and then irradiated with a laser to melt the coating material and a thin layer on the substrate surface simultaneously. After rapid solidification, a surface coating with extremely low dilution and metallurgical bonding with the substrate is formed, which significantly improves the wear resistance, corrosion resistance, heat resistance, oxidation resistance and electrical properties of the substrate surface, thereby achieving the purpose of surface modification or repair. It not only meets the requirements for specific surface properties of materials, but also saves a lot of precious elements. Compared with welding, spraying, electroplating and vapor deposition, laser cladding has the characteristics of low dilution, dense structure, good bonding between the coating and the substrate, wide range of applicable materials, and large variation in particle size and content. Therefore, the application prospects of laser cladding technology are very broad. The main characteristics of laser cladding technology are as follows: (1) The laser cladding layer and the substrate are metallurgically bonded, and the bonding strength is not less than 95% of the original substrate material. The strengthening effect is good, the density of the cladding layer is high, and the hardness, wear resistance and corrosion resistance are improved at the same time; (2) The thermal impact on the substrate is small, and the deformation caused is also small. During laser processing, the laser beam has a high energy density and a fast processing speed. It is also a localized process, with little or no impact on areas not irradiated by the laser. Therefore, its heat-affected area is small, the workpiece has little thermal deformation, and the subsequent processing amount is minimal; (3) The range of materials is wide, such as nickel-based, cobalt-based, iron-based alloys, carbide composite materials, etc., which can meet the requirements of different applications and take into account both internal performance and surface characteristics; (4) The cladding layer and its interface structure are dense, with fine grains, no pores, no inclusions, cracks and other defects; (5) It can repair large equipment valuable parts and molds that are locally worn or damaged, reaching or even exceeding the mechanical properties of the base material, extending the service life, with wide application, high flexibility, and adaptability to various complex shapes; (6) It can achieve high-quality and rapid repair of damaged parts, reduce downtime due to failure, and reduce equipment maintenance costs; (7) It has low environmental pollution and no waste liquid or waste gas is discharged; it has a high degree of automation, and the processing system can be designed to be fully computer-controlled; (8) Laser processing is non-contact processing, and there is no direct impact on the workpiece, so there is no mechanical deformation; there is no "tool" wear and no "cutting force" acting on the workpiece during laser processing.
[0003] Laser cladding is a surface modification technology that uses a high-energy laser beam as a heat source to deposit alloy coatings with special properties onto a substrate. It boasts advantages such as low dilution rate, small heat-affected zone, high bonding strength with the substrate, and low environmental pollution, making it widely used for surface repair and strengthening of key components in automotive manufacturing, petrochemicals, and mining machinery. However, laser cladding is a complex metallurgical process involving physics, chemistry, and materials science. Its rapid heating and cooling solidification characteristics often result in defects such as cracks and porosity in the cladding layer. Furthermore, it presents problems such as uneven distribution of internal solute elements and surface irregularities. Cracking, particularly in high-hardness alloy coatings, has become a bottleneck for the application and development of laser cladding technology.
[0004] Previous studies by scholars both domestically and internationally have primarily focused on eliminating or reducing defects in laser cladding coatings through material design and process parameter optimization. However, for high-hardness alloy coatings, modifying existing processes still makes it difficult to completely eliminate microstructural defects. Therefore, it is necessary to consider applying external fields to regulate the solidification structure of the coating, thereby improving its quality. Utility Model Content
[0005] In view of this, the purpose of this utility model is to propose an electromagnetic composite field assisted laser cladding device to solve the problems mentioned in the background art.
[0006] To achieve the above objectives, this utility model provides an electromagnetic composite field-assisted laser cladding device, comprising: an alternating electric field device 1, an alternating magnetic field device 2, a PLC intelligent control system 3, and a work trolley 4.
[0007] The alternating electric field device 1 and the alternating magnetic field device 2 are fixedly installed on the upper part of the work trolley 4;
[0008] The PLC intelligent control system 3 is fixedly installed on one side of the work trolley 4 and is electrically connected to the alternating electric field device 1 and the alternating magnetic field device 2.
[0009] In one embodiment, both the alternating electric field device 1 and the alternating magnetic field device 2 are annular in shape, and they are alternately arranged on the same plane.
[0010] In one embodiment, the alternating electric field device 1 and the alternating magnetic field device 2 are fixed to the surface of the work trolley 4 by welding.
[0011] In one embodiment, the PLC intelligent control system 3 is fixed to the side wall or bracket of the work cart 4 by welding.
[0012] In one embodiment, the PLC intelligent control system 3 includes a power switch 30, an alternating electric field switch 31, an alternating magnetic field switch 32, and an intelligent touch screen 33, with each switch and the touch screen integrated on the same control panel.
[0013] In one embodiment, the smart touch screen 33 is connected to the alternating electric field device 1 and the alternating magnetic field device 2 via internal circuitry to adjust the parameters of the alternating current and magnetic induction intensity.
[0014] In one embodiment, the work trolley 4 is equipped with casters at the bottom for overall movement and positioning of the device.
[0015] As can be seen from the above, the electromagnetic composite field-assisted laser cladding device provided by this utility model forms a precise electromagnetic composite field acting on the molten pool through the alternating arrangement of a ring-shaped alternating electric field and an alternating magnetic field device. This synergistically achieves grain refinement and reduces structural defects, significantly improving the wear resistance of the cladding layer. At the same time, it adopts an integrated work trolley to integrate all functional components, which is compact, easy to move, and can be directly adapted to existing laser cladding equipment. With the independent start-stop control and wide-range parameter adjustment function of the PLC intelligent control system, the operation is intuitive and easy to understand, adaptable to different substrates and cladding requirements. In addition, the dustproof and moisture-proof sturdy structural design ensures stable and reliable operation and low maintenance costs. It comprehensively solves the problems of traditional laser cladding auxiliary devices such as single function, loose structure, and inconvenient control, and has both technological advancement and industrial practicality. Attached Figure Description
[0016] To more clearly illustrate the technical solutions in the embodiments of this utility model or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this utility model. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0017] Figure 1 This is a schematic diagram of an electromagnetic composite field-assisted laser cladding device according to an embodiment of the present invention;
[0018] Figure 2 This is a schematic diagram showing the average Vickers hardness measurement results of the iron-based coating in Comparative Example 1 and Examples 1-4 of this utility model.
[0019] In the diagram, 1-alternating electric field device, 2-alternating magnetic field device, 3-PLC intelligent control system, 4-work trolley, 30-power switch, 31-alternating electric field switch, 32-alternating magnetic field switch, 33-intelligent touch screen. Detailed Implementation
[0020] To make the objectives, technical solutions, and advantages of this utility model clearer, the present utility model will be further described in detail below with reference to specific embodiments and accompanying drawings.
[0021] It should be noted that, unless otherwise defined, the technical or scientific terms used in the embodiments of this utility model should have the ordinary meaning understood by one of ordinary skill in the art to which this utility model pertains. The terms "first," "second," and similar terms used in this utility model do not indicate any order, quantity, or importance, but are merely used to distinguish different components. Terms such as "comprising" or "including" mean that the element or object preceding the word encompasses the elements or objects listed following the word and their equivalents, without excluding other elements or objects. Terms such as "connected" or "linked" are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. Terms such as "upper," "lower," "left," and "right" are only used to indicate relative positional relationships; when the absolute position of the described object changes, the relative positional relationship may also change accordingly.
[0022] In one embodiment, according to Figure 1 An electromagnetic composite field-assisted laser cladding device is described to illustrate this utility model.
[0023] An electromagnetic composite field-assisted laser cladding device includes: an alternating electric field device 1, an alternating magnetic field device 2, a PLC intelligent control system 3, and a work trolley 4.
[0024] Both the alternating electric field device 1 and the alternating magnetic field device 2 are circular in shape. They are arranged alternately along the length of the worktable 4 (electric field-magnetic field-electric field) and are fixed to the upper panel of the worktable 4 by welding to ensure that the central axis of the ring coincides with the processing axis of the laser cladding head, thus ensuring that the composite field accurately covers the molten pool area.
[0025] In one embodiment, the control box of the PLC intelligent control system 3 is fixed to the left end of the work trolley 4 by welding. The control box is equipped with a terminal block, which is electrically connected to the alternating electric field device 1 and the alternating magnetic field device 2 through copper core cables, and signal connected through signal lines.
[0026] In one embodiment, the alternating electric field switch 31 and alternating magnetic field switch 32 of the PLC intelligent control system 3 are push-button switches, connected in series with the power supply circuits of the alternating electric field device 1 and the alternating magnetic field device 2, respectively, to achieve independent start-stop control. The intelligent touch screen 33 has a built-in PLC control program, and the alternating current value (0-2000A) and magnetic induction intensity value (0-0.2T) can be set through the touch screen interface, and the operating parameters are displayed in real time.
[0027] In one embodiment, the work trolley 4 is equipped with casters at the bottom for overall movement and positioning of the device.
[0028] The working process of this device is as follows:
[0029] Move the worktable trolley 4 to the processing area of the laser cladding equipment and adjust its position so that the center of the ring device is aligned with the cladding processing path.
[0030] When the power switch 30 is closed, the PLC intelligent control system 3 is powered on, and the intelligent touch screen 33 lights up and enters the operation interface.
[0031] Based on the processing substrate and the thickness of the cladding layer, the alternating current and the magnetic induction intensity are set as fixed parameters on the smart touch screen 33.
[0032] Start the laser cladding equipment. After the molten pool is formed, press the alternating electric field switch 31 and the alternating magnetic field switch 32 respectively. The alternating electric field device 1 and the alternating magnetic field device 2 are activated, forming an electromagnetic composite field that acts on the molten pool.
[0033] During the processing, parameters can be adjusted in real time via the intelligent touch screen 33. After processing is completed, first turn off the alternating electric field switch 31 and the alternating magnetic field switch 32, and then turn off the power switch 30 to complete the operation.
[0034] The technical solutions of this utility model will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of this utility model, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this utility model without creative effort are within the scope of protection of this utility model.
[0035] Comparative Example 1
[0036] The surface of the H13 steel substrate was polished smooth with 400-grit sandpaper, and surface oil was wiped off with acetone solution. The H13 steel substrate was placed in the center of the worktable. Iron-based powder with a particle size of 50-120 μm was used. An iron-based coating was prepared by cladding the powder onto the H13 steel substrate using a laser cladding device at a laser power of 3000 W, a scanning speed of 30 mm / s, and a powder feeding rate of 30 g / min, resulting in a 1.5 mm thick iron-based coating. The iron-based coating was then finished to a smooth surface and placed in a heat treatment furnace, where it was held at 500℃ for 2 hours.
[0037] Example 1
[0038] The surface of the H13 steel substrate was polished smooth with 400-grit sandpaper, and surface oil was wiped off with acetone solution. The H13 steel substrate was placed in the center of the worktable, and the power switch and alternating electric field switch were turned on, setting the alternating current to 1000A. Iron-based powder with a particle size of 50-120μm was used. An iron-based coating was prepared by cladding the powder onto the H13 steel substrate using a laser cladding device at a laser power of 3000W, a scanning speed of 30mm / s, and a powder feeding rate of 30g / min, resulting in a 1.5mm thick iron-based coating. The iron-based coating was then finished to a smooth surface and placed in a heat treatment furnace, where it was held at 500℃ for 2 hours.
[0039] Example 2
[0040] The surface of the H13 steel substrate was polished smooth with 400-grit sandpaper, and surface oil was wiped off with acetone solution. The H13 steel substrate was placed in the center of the worktable, and the power switch and alternating magnetic field switch were turned on, setting the magnetic induction intensity to 0.1T. Iron-based powder with a particle size of 50-120μm was used. An iron-based coating was prepared by cladding the powder onto the H13 steel substrate using a laser cladding device at a laser power of 3000W, a scanning speed of 30mm / s, and a powder feeding rate of 30g / min, resulting in a 1.5mm thick iron-based coating. The iron-based coating was then finished to a smooth surface and placed in a heat treatment furnace, where it was held at 500℃ for 2 hours.
[0041] Example 3
[0042] The surface of the H13 steel substrate was polished smooth with 400-grit sandpaper, and surface oil was wiped off with acetone solution. The H13 steel substrate was placed in the center of the worktable. The power switch, alternating electric field switch, and alternating magnetic field switch were turned on, setting the alternating current to 1000A and the magnetic induction intensity to 0.1T. Iron-based powder with a particle size of 50-120μm was used. An iron-based coating was prepared by cladding the powder onto the H13 steel substrate using a laser cladding device at a laser power of 3000W, a scanning speed of 30mm / s, and a powder feeding rate of 30g / min, resulting in a 1.5mm thick iron-based coating. The iron-based coating was then finished to a smooth surface and placed in a heat treatment furnace, where it was held at 500℃ for 2 hours.
[0043] Example 4
[0044] The surface of the H13 steel substrate was polished smooth with 400-grit sandpaper, and surface oil was wiped off with acetone solution. The H13 steel substrate was placed in the center of the worktable. The power switch, alternating electric field switch, and alternating magnetic field switch were turned on, setting the alternating current to 2000A and the magnetic induction intensity to 0.2T. Iron-based powder with a particle size of 50-120μm was used. An iron-based coating was prepared by cladding the powder onto the H13 steel substrate using a laser cladding device at a laser power of 3000W, a scanning speed of 30mm / s, and a powder feeding rate of 30g / min, resulting in a 1.5mm thick iron-based coating. The iron-based coating was then finished to a smooth surface and placed in a heat treatment furnace, where it was held at 500℃ for 2 hours.
[0045] The Vickers hardness of the laser cladding coatings in Comparative Example 1 and Examples 1-4 was tested using an HV-1000 Vickers hardness tester. The average Vickers hardness of each laser cladding coating was recorded. The test results are shown in […]. Figure 2 ,Depend on Figure 2 It can be seen that the average Vickers hardness of the laser cladding coatings in Comparative Example 1 and Examples 1-4 are 615HV, 743HV, 768HV, 858HV, and 925HV, respectively.
[0046] The electromagnetic composite field-assisted laser cladding device provided by this utility model has the following beneficial effects:
[0047] By using alternating circular alternating electric field devices and alternating magnetic field devices, an electromagnetic composite field is formed that uniformly covers the molten pool. By utilizing the electromigration effect of the electric field and the electromagnetic stirring effect of the magnetic field, the grains of the cladding layer are refined in synergy, the uniformity of the structure is improved, and the residual stress is reduced. Compared with traditional laser cladding layers, the wear resistance is improved.
[0048] Each device is fixed to the work trolley by welding, which is highly integrated, compact, and easy to move. It can be directly used with existing laser cladding equipment without the need for major modifications to the original equipment, resulting in low installation costs.
[0049] The PLC intelligent control system integrates an independent switch and an intelligent touch screen, enabling overall power on / off, independent start / stop of electromagnetic devices, and precise parameter control. The user interface is intuitive and can be quickly mastered without the need for professional technicians, making it suitable for industrial mass production needs.
[0050] The alternating current and magnetic induction intensity parameters have a wide adjustment range, and the electromagnetic parameters can be flexibly adjusted according to different substrates such as carbon steel, alloy steel, and non-ferrous metals, as well as the thickness of the cladding layer, making it suitable for a wide range of applications.
[0051] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the present invention (including the claims) is limited to these examples; within the framework of the present invention, the technical features of the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in the details for the sake of brevity.
[0052] The embodiments of this utility model are intended to cover all such substitutions, modifications, and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this utility model should be included within the protection scope of this utility model.
Claims
1. An electromagnetic complex field assisted laser cladding device, characterized in that, include: Alternating electric field device (1), alternating magnetic field device (2), PLC intelligent control system (3) and work trolley (4); The alternating electric field device (1) and the alternating magnetic field device (2) are fixedly installed on the upper part of the work trolley (4); The PLC intelligent control system (3) is fixedly installed on one side of the work trolley (4) and electrically connected to the alternating electric field device (1) and the alternating magnetic field device (2).
2. The electromagnetic composite field assisted laser cladding device according to claim 1, characterized in that, The alternating electric field device (1) and the alternating magnetic field device (2) are both ring-shaped and are arranged alternately on the same plane.
3. The electromagnetic composite field assisted laser cladding device according to claim 1, characterized in that, The alternating electric field device (1) and the alternating magnetic field device (2) are fixed to the surface of the work trolley (4) by welding.
4. The electromagnetic composite field assisted laser cladding device according to claim 1, characterized in that, The PLC intelligent control system (3) is fixed to the side wall or bracket of the work trolley (4) by welding.
5. The electromagnetic composite field assisted laser cladding device according to claim 1, characterized in that, The PLC intelligent control system (3) includes a power switch (30), an alternating electric field switch (31), an alternating magnetic field switch (32), and an intelligent touch screen (33), with each switch and touch screen integrated on the same control panel.
6. The electromagnetic composite field assisted laser cladding device according to claim 1, characterized in that, The intelligent touch screen (33) is connected to the alternating electric field device (1) and the alternating magnetic field device (2) through an internal circuit, and is used to adjust the parameters of alternating current and magnetic induction intensity.
7. The electromagnetic composite field assisted laser cladding device according to claim 1, characterized in that, The work trolley (4) is equipped with wheels at the bottom for the overall movement and positioning of the device.