Ceramic bodies and methods for manufacturing them
By using SiC powders with defined particle sizes and ratios, and a controlled impregnation process, the thermal conductivity of ceramic bodies is significantly enhanced, addressing the limitations of conventional methods and improving heat exchanger performance.
Patent Information
- Application Number
- DE102024201215
- Authority / Receiving Office
- DE · DE
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-02-09
- Publication Date
- 2024-10-02
AI Technical Summary
Conventional methods struggle to control the proportion of SiC in ceramic bodies effectively, resulting in insufficient thermal conductivity, which is a critical issue for applications like heat exchangers and other purposes.
A method involving the use of SiC powders with specific average particle sizes (15 to 50 µm and 2 to 8 µm) in a predetermined mass ratio (3:7 to 7:3) for forming and impregnating with metallic Si, followed by firing and impregnation in an inert gas or vacuum at 1400 to 1600°C, to enhance the thermal conductivity of ceramic bodies.
This approach results in a ceramic body with improved thermal conductivity, exceeding 140 W/mK, enhancing heat recovery performance and mechanical strength, particularly in heat exchangers.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
FIELD OF THE INVENTION
[0001] The present invention relates to a ceramic body and a method for producing the same. BACKGROUND OF THE INVENTION
[0002] Recently, there has been a need to improve the fuel efficiency of motor vehicles. In particular A system is expected that contains a coolant, engine oil and an automatic transmission fluid (ATF: Automatic Transmission Fluid) in at an early stage to reduce friction losses and prevent deterioration of fuel efficiency when an engine is cold, such as when the engine is started. Furthermore, a system expected, which heats an exhaust gas purification catalyst to activate the catalyst at an early stage.
[0003] The above system uses a heat exchanger which is provided with a ceramic body (honeycomb structure) with a Honeycomb shape and made of Si-impregnated SiC (Patent Literature 1). The ceramic body is degreased by a ceramic molded body containing silicon carbide (hereinafter referred to as ´´SiC´´) and then impregnating the same with metallic silicon (hereinafter referred to as ´´Si´´). STATE OF THE ART Patent literature
[0004] [Patent Literature 1] Japanese Patent Publication No. 6763699 B SUMMARY OF THE INVENTION Object of the invention
[0005] In recent years, an increase in the thermal conductivity of the ceramic body made of Si-impregnated SiC required to improve the performance of a heat exchanger (e.g. to achieve a heat recovery property improve).
[0006] Since SiC forms the skeleton sections of the ceramic body and has a higher thermal conductivity than Si, assumed that the thermal conductivity of the ceramic body can be increased by increasing a proportion of SiC in the ceramic body can be improved.
[0007] However, a conventional method has problems that it is difficult to control the proportion of SiC in the Ceramic body (skeletal sections) to increase stably, and the thermal conductivity of the ceramic body is not sufficient is improved.
[0008] It should be noted that while the ceramic body used for the heat exchanger is described above as a As described in the example, there is also a need to improve the thermal conductivity of ceramic bodies, which be used for purposes other than heat exchangers.
[0009] The present invention has been made to solve the problems as described above. An object of the The present invention is to provide a ceramic body with high thermal conductivity made of Si-impregnated SiC and to provide a method for producing the same. Solution to the task
[0010] As a result of intensive investigations for ceramic bodies made of Si-impregnated SiC, the inventors of present invention that the above objects can be achieved by using a molding material which can combine two types of SiC powders with predetermined average particle sizes D50 in a given ratio, and they have completed the present invention. That is, the present invention is as shown as follows: [1] A method for producing a ceramic body, comprising: a forming step of forming a mold material containing SiC powder having an average Particle size D50 from 15 to 50 µm and SiC powder with an average particle size D50 of 2 to 8 µm in a mass ratio of 3:7 to 7:3 to obtain a shaped body; and a firing and impregnation step of firing the shaped body and impregnating it with metallic Si. [2] A method for producing a ceramic body according to [1], wherein the firing and impregnation step is carried out by Firing of the molded body in contact with the metallic Si. [3] A method for producing a ceramic body according to [2], wherein the firing is carried out in an inert gas atmosphere or in a vacuum at a temperature of 1400 to 1600°C. [4] A method for producing a ceramic body according to any one of claims [1] to [3], wherein ceramic raw materials, contained in the mold material are only the SiC powders. [5] A method for producing a ceramic body according to any one of claims [1] to [4], wherein the shaped body a drying process and / or a degreasing process between the formation step and the firing and impregnation step. [6] A method for producing a ceramic body according to any one of claims [1] to [5], wherein the shaped body has a honeycomb shape, comprising: an outer peripheral wall; and partition walls formed on an inner side of the outer peripheral wall, wherein the partition walls define a plurality of cells, each of which extending from a first end face to a second end face; or a hollow honeycomb shape comprising: a inner peripheral wall; an outer peripheral wall; and partition walls formed between the inner peripheral wall and the outer peripheral wall, wherein the partition walls define a plurality of cells which are each extending from a first end face to a second end face. [7] Ceramic body, comprising: SiC skeleton sections, each containing SiC particles with a particle size of 15 to 50 µm and SiC particles with a particle size of 2 to 8 µm in a volume ratio of 3:7 to 7:3; and Si-impregnated metal sections, each of which is surrounded by at least a part of the SiC skeleton sections are trained. Effects of the invention
[0011] According to the present invention, it is possible to produce a ceramic body with high thermal conductivity made of Si- impregnated SiC, and to provide a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS Fig. 1 is a partially enlarged cross-sectional view of a method for producing a Ceramic body according to an embodiment of the present invention; Fig. 2 is a cross-sectional view of a molded body with a honeycomb shape orthogonal to a direction of extension of cells; and Fig. 3 is a cross-sectional view of a molded body with a hollow honeycomb shape orthogonal to a direction of extension of cells. DETAILED DESCRIPTION OF THE INVENTION
[0012] In the following, embodiments of the present invention will be described with reference to the drawings described in more detail. It is understood that the present invention is not limited to the following embodiments and those who make appropriate changes, improvements and the like to the following Embodiments based on the knowledge of a person skilled in the art, without departing from the spirit of the present invention fall within the scope of the present invention. (1) Method for producing a ceramic body
[0013] A method for producing a ceramic body according to an embodiment of the present invention It includes a forming step and a firing and impregnation step. These steps are described in detail. <formungsschritt>
[0014] The molding step is a step of forming a molding material containing SiC powder having an average Particle size D50 from 15 to 50 µm (hereinafter abbreviated as ´´SiC powder A´´) and SiC powder with a average particle size D50 of 2 to 8 µm (hereinafter abbreviated as ´´SiC powder B´´) in a Mass ratio of 3:7 to 7:3 to obtain a shaped body.
[0015] Here, Fig. 1 shows a partially enlarged cross-sectional view of a prepared under the above conditions As shown in Fig. 1, by using two types of SiC powders A and B with the average particle sizes D50 in the above mass ratio, the SiC powders B with the smaller average Particle size D50 slightly between the SIC powders A with the larger average particle size D50 in the Mold body 10 is filled so that the bulk density of the SiC powders (SiC powders A and B) forming the mold body 10 is increased As a result, the thermal conductivity of the ceramic body, which is obtained by subjecting the mold body 10 the firing and impregnation step. On the other hand, conditions other than the described above does not ensure that the bulk density of the SiC particles forming the molded body is sufficiently increased, so that the thermal conductivity of the ceramic body cannot be sufficiently improved.
[0016] As used herein, the ´´average particle size D50´´ of the SiC powders A and B, which are formation step, a particle size at 50% (D50) of the integrated value in the particle size distribution, which is determined by the laser diffraction / scattering method.
[0017] Although the SiC powders may be of a single type or in combination of two or more types. In particular, two or more types of SiC powders A with an average particle size D50 in the range from 15 to 50 µm can be used.
[0018] Likewise, the SiC powders B may be of a single type or in combination of two or more types. In particular, two or more types of SiC powders B with an average particle size D50 in the range from 2 to 8 µm can be used.
[0019] The average particle size D50 of the SiC powders A is preferably 20 to 45 µm and more preferably 25 to 40 µm from the point of view of stable ensuring the above effects.
[0020] Furthermore, the average particle size D50 of the SiC powder B is preferably 3 to 7 µm and more preferably 4 up to 6 µm from the point of view of stable ensuring the above effects.
[0021] Furthermore, the mass ratio of the SiC powder A and the SiC powder B is preferably 4:6 to 6:4 from the point of view of stable assurance of the above effects.
[0022] It is preferred that the molding material contains only SiC powders A and B as ceramic raw materials. Each of the SiC powders A and B have high thermal conductivity and a thermal expansion coefficient close to that of metallic Si which is impregnated in a step described later, so that a ceramic body with an improved Resistance to thermal stress can be maintained.
[0023] As used herein, the ceramic raw materials mean the raw materials that form the skeleton sections of the ceramic body after the firing and impregnation step.
[0024] The molding material may optionally contain components known in the art. The known Components include dispersion media, binders, plasticizers and dispersants. The content of these Components are not particularly limited as long as they do not inhibit the effects of the present invention.
[0025] Examples of the dispersion media include water or a mixed solvent of water and a organic solvents such as alcohol and preferably water.
[0026] Examples of the binders include organic binders such as methylcellulose, hydroxypropoxylcellulose, Hydroxyethylcellulose, carboxymethylcellulose and polyvinyl alcohol. In particular, it is preferred to use methylcellulose in Combination with hydroxypropoxylcellulose. The binders can be used alone or in combination of two or be used more.
[0027] Examples of the plasticizers include polyoxyalkylene alkyl ethers, polycarboxylic acid-based polymers and Alkyl phosphate esters.
[0028] The dispersants that can be used here include surfactants such as polyoxyalkylene alkyl ethers, Ethylene glycol, dextrin, fatty acid soaps and polyalcohol. The dispersants can be used alone or in combination with two or more can be used.
[0029] The molding method is not particularly limited, and known methods such as extrusion molding can In extrusion molding, a molded article with a desired shape can be produced by selecting a suitable die and clamping device. For example, if a molded body with a honeycomb shape obtained, a suitable die and clamping device can be selected to determine the shape and density of cells, the number, length and thickness of the partition walls, the shapes and thicknesses of the outer peripheral wall and the inner to control the peripheral wall.
[0030] The shape of the molded article obtained by the molding step includes, but is not particularly limited to, preferably, a honeycomb shape comprising: an outer peripheral wall and partition walls formed on an inner side of the outer peripheral wall and defining a plurality of cells each extending from a first end surface to a second end surface; or a hollow honeycomb shape comprising: an inner peripheral wall, a outer peripheral wall and partition walls arranged between the inner peripheral wall and the outer peripheral wall and which define a plurality of cells each extending from a first end face to a second end face Such a shape, for example when used in a heat exchanger, can increase the performance (e.g. B. heat recovery performance) can be improved.
[0031] Here, Fig. 2 shows a cross-sectional view of the molded body with the honeycomb shape (honeycomb molded body) which is orthogonal to the direction of extension of the cells, and Fig. 3 shows a cross-sectional view of the molded body with the hollow Honeycomb shape (hollow honeycomb body) that is orthogonal to the direction of extension of the cells.
[0032] As shown in Fig. 2, the honeycomb molded body 100 comprises: an outer peripheral wall 110; and partition walls 130, the are arranged on an inner side of the outer peripheral wall 110 and which define a plurality of cells 120 which each extending from a first end face to a second end face. Furthermore, as shown in Fig. 3, the hollow honeycomb molded bodies 200: an inner peripheral wall 140; an outer peripheral wall 110; and partition walls 130, the between the inner peripheral wall 140 and the outer peripheral wall 110 and which have a plurality of Define cells 120, each extending from a first end surface to a second end surface.
[0033] Each of the honeycomb molded body 100 and the hollow honeycomb molded body 200 may have any shape (external shape) including, but not particularly limited to, for example, a cylindrical shape, an elliptical Column shape, a square column shape or another polygonal column shape. That is, any external shape of the Honeycomb molded body 100 and the hollow honeycomb molded body 200 in the cross section orthogonal to the extension direction The cells 120 may be circular, oval, square, or otherwise polygonal. Furthermore, the hollow portion of the hollow Honeycomb molded body 200 has the same or different external shape(s) as or from the hollow honeycomb molded body 200 and can have the various forms as described above.
[0034] The shape of each cell 120 in the cross section orthogonal to the direction of extension of the cells 120 is not limited to the represented shapes and can be a circle, an oval, a polygon such as a triangle or the like.
[0035] Preferably, each of the honeycomb molded body 100 and the hollow honeycomb molded body 200 has a structure that meets the following characteristics after the firing / impregnation step. It should be noted that each of the honeycomb molded body 100 and the hollow honeycomb molded body 200 after the firing / impregnation step as honeycomb structure.
[0036] A cell density (i.e. the number of cells 120 per unit area) in the cross section of the honeycomb structure orthogonal to the direction of extension of the cells 120 can be selected as required depending on applications or 2 the like and preferably in a range of 4 to 320 cells / cm. In the cross section orthogonal 2 to the extension direction of the cells 120, the cell density of 4 cells / cm or more can increase the strength of the partition walls 130 sufficiently ensure, therefore, the strength of the honeycomb structure itself and effective GSA (geometric surface area). 2 Furthermore, the cell density of 320 cells / cm or less may cause an increase in pressure loss when the fluid flows impede.
[0037] The thickness of the partition walls 130 of the honeycomb structure can be designed as required depending on the purpose but it may preferably be 50 µm to 2 mm and more preferably 60 µm to 600 µm. If the thickness of the Partition walls 130 50 µm or more, the mechanical strength is improved so that any damage that caused by impact or thermal stress can be suppressed. On the other hand, if the thickness of the Partition walls 130 2 mm or less, the ratio of the cell volume to the honeycomb structure increases, which the pressure loss of the fluid is reduced so that a heat exchange rate can be improved.
[0038] The thickness of each of the outer peripheral wall 110 and the inner peripheral wall 140, if any, of the Honeycomb structure can be designed to suit the purpose, but if it is for the Heat exchange application, the thickness is preferably more than 0.3 mm and less than or equal to 10 mm and more preferably 0.5 mm to 5 mm and even more preferably 1 mm to 3 mm. Furthermore, if they are for the Heat storage application is used, the thickness of the outer peripheral wall 110 10 mm or more to ensure the To increase the heat capacity of the outer peripheral wall 110. <Brenn- und Imprägnierschritt>
[0039] The firing and impregnation step is a step of firing the molded body and impregnating it with metallic Si.
[0040] The conditions for the firing and impregnation step are not particularly limited, and this step may according to known methods. Furthermore, in the firing and impregnation step, the firing and Impregnation can be carried out in one step, but firing and impregnation can be carried out in separate In particular, the firing step and the impregnation step can be carried out as separate steps be performed.
[0041] The firing and impregnation step is preferably carried out by firing the shaped body in contact with metallic Si By performing the firing in such a state, the molten metallic Si can be Capillary action in the gaps between the ceramic particles that form the molded body, whereby the molded body impregnated with metallic Si. According to such a process, firing and impregnation can also be carried out in carried out in one step, so that the manufacturing costs can be reduced.
[0042] Although the position in the molded body with which the metallic Si is brought into contact is not particularly limited contacting is preferably carried out while the metallic Si is on the upper surface of the For example, if the honeycomb molded body 100 and the hollow honeycomb molded body 200 are used as molded bodies, the positions with which metallic Si is brought into contact can be any the end surface (first end surface or second end surface), the outer peripheral wall 110 and the inner peripheral wall 140, where present. If the extension direction of the cells 120 is the vertical direction, the metallic Si preferably also placed on the end face (first end faces or second end faces) located above the honeycomb molded body 100 and the hollow honeycomb molded body 200, and brought into contact with them. The Contacting in such a manner leads to slight impregnation with metallic Si due to gravity.
[0043] The firing is preferably carried out in an inert gas atmosphere or in a vacuum at a temperature of 1400 up to 1600°C. Firing under such conditions results in a slight impregnation with metallic Si. It can also suppress insufficient sintering due to oxidation and oxides present in the mold material contained in it.
[0044] Examples of the inert gas atmosphere include a nitrogen gas atmosphere, a noble gas atmosphere such as argon or a mixed gas atmosphere.
[0045] The firing temperature is preferably 1450 to 1550°C from the point of view of ensuring the above stable Effects. It should be noted that the burn time is not particularly limited, but typically ranges from 0.25 to 5 hours.
[0046] It should be noted that a kiln used for firing is not particularly limited, but a Electric oven, gas oven and the like can be used. <Anderer Schritt>
[0047] Between the formation step and the firing and impregnation step, the shaped body can be subjected to a drying process and / or a degreasing process. Furthermore, after the firing and impregnation step, a Surface treatment, such as polishing, can be carried out.
[0048] The drying process is not particularly limited, and any known method can be used. For example, the drying process can be carried out using a microwave dryer, a hot air dryer, a dielectric dryer, a negative pressure dryer, a vacuum dryer, a freeze dryer or the like be performed.
[0049] The degreasing process is used to burn and remove components such as binders. Conditions for the degreasing process are not particularly limited as long as the binder and the like can be burned out, and they can be used depending on the type of binder and the like For example, the degreasing process can be adjusted by heating the molded body at 300 to 600 °C for 1 to 10 hours. (2) Ceramic body
[0050] A ceramic body according to an embodiment of the present invention is produced by the above-described Method for producing the ceramic body. The ceramic body comprises SiC skeleton sections and Si- impregnated metal sections.
[0051] The SiC skeleton sections contain SiC particles with a particle size of 15 to 50 µm and SiC particles with a Particle size of 2 to 8 µm in a volume ratio of 3:7 to 7:3. The SiC skeleton sections, which contain two types of SiC Particles with the defined particle sizes in the above volume ratio allow the proportion of SiC particles in the ceramic body, thereby improving the thermal conductivity of the ceramic body.
[0052] Here, the volume ratio of the SiC particles with the particle size of 15 to 50 µm and the SiC particles with the Particle size of 2 to 8 µm in the ceramic body by observing the cross section of the ceramic body under using an SEM. In particular, an SEM image of the cross-section of the ceramic body shows the SiC particles with a particle size of 15 to 50 µm and SiC particles with a particle size of 2 to 8 µm are distinguished. At this time, the particle size of the SiC particles is an equivalent circle diameter. Then, a ratio of the Total area of SiC particles with the particle size of 15 to 50 µm and the total area of SiC particles with the Particle size of 2 to 8 µm in the ceramic body as the volume ratio of SiC particles with the particle size of 15 up to 50 µm and the SiC particles with the particle size of 2 to 8 µm in the ceramic body defined
[0053] The Si-impregnated metal sections are applied to gaps of at least a part of the SiC skeleton sections By forming the Si-impregnated metal sections, the ceramic body can be made tight to To increase thermal conductivity and strength.
[0054] The thermal conductivity of the ceramic body is preferably 140 W / mK or more, and more preferably 150 W / mK or more at 25 °C, although not particularly limited thereto. If the ceramic body in the heat exchanger used, the thermal conductivity of the ceramic body in the above range allows the Heat recovery performance of the heat exchanger is improved. In addition, the value of the thermal conductivity a value measured by the laser flash method (JIS R1611: 1997).
[0055] Other features related to the materials the ceramic body is made of, its shape and the like are the same as those described in the method for producing the ceramic body, and descriptions thereof are omitted here. EXAMPLES
[0056] In the following, the present invention will be described in more detail with reference to examples, but the The present invention is not limited to these examples. (Examples 1 to 4)
[0057] Three types of SiC powders with average particle diameters D50 of 35 µm, 25 µm and 5 µm manufactured.
[0058] Two or three kinds of these SiC powders were then mixed in each mass ratio as shown in Table 1, and 28 parts by mass of water and 7 parts by mass of methylcellulose were further added to 100 parts by mass of the total amount of SiC- Powders were added and mixed to obtain a molding material. The molding material was extruded to form a molded body with a honeycomb structure. The size of each honeycomb body was adjusted to form a Honeycomb structure with the following shape after the firing and impregnation step was: Shape of the honeycomb structure in the cross-section orthogonal to the direction of extension of the cells: circular; Cell shape in the cross section orthogonal to the direction of extension of the cells: quadrangular: length in the Cell extension direction: 100 mm; Outer diameter of the honeycomb structure in the cross-section orthogonal to the direction of extension of the cells: 100 mm; 2 Cell density: 14 cells / cm ; Thickness of the partition: 0.3 mm; and Thickness of the outer peripheral wall: 1.5 mm.
[0059] The honeycomb molded body was then arranged so that the extension direction of the cells was the vertical direction the metallic Si was placed on the upper end surface and then in a vacuum at a temperature of Fired at 1500°C to obtain a honeycomb structure (ceramic body). (Comparison examples 1 and 2)
[0060] A honeycomb structure (ceramic body) was obtained by the same method as that of the above example, with with the exception that SiC powder with an average particle size D50 of 35 µm or SiC powder with a average particle size D50 of 5 µm was used alone.
[0061] The thermal conductivity of each honeycomb structure obtained above was measured at 25°C using the Laser flash method (JIS R1611: 1997). When evaluating thermal conductivity, the honeycomb structure is measured with a thermal conductivity of 150 W / mK or more is represented by a double circle (marked: ⊚), the Honeycomb structure with a thermal conductivity of 140 W / mK or more and less than 150 W / mK is indicated by a circle (good: O) and the honeycomb structure with a thermal conductivity of less than 140 W / mK is shown as x (poor) The results are shown in Table 1. Table 1 SiC powder (D50) thermal conductivity 35 µm 25 µm 5 µm Example: 1 50 0 50 ⊚ Example 2 25 25 50 ⊚ Example 3 70 0 30 ○ See 1 100 0 0 × See 2 0 0 100 ×
[0062] As shown in Table 1, each of the honeycomb structures (ceramic bodies) according to Examples 1 to 4 obtained under Use of SiC powders with an average particle size D50 of 15 to 50 µm and SiC powders with a average particle size D50 of 2 to 8 µm in a mass ratio of 3:7 to 7:3, which have higher Thermal conductivity than any of the honeycomb structures (ceramic bodies) according to Comparative Examples 1 and 2, which were using SiC powder of a single type.
[0063] As can be seen from the above results, according to the present invention, it is possible to obtain a Ceramic body with high thermal conductivity made of Si-impregnated SiC and a method for producing to provide the same. List of reference symbols 10 molded bodies 100 honeycomb moldings 110 outer peripheral wall 120 cells 130 partition wall 140 inner peripheral wall 200 hollow honeycomb molded bodies QUOTES CONTAINED IN THE DESCRIPTION
[0000] This list of documents submitted by the applicant was generated automatically and is intended solely for This list is not part of the German patent or trademark law. Utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature
[0000] JP 6763699 B
[0004] < / formungsschritt>
Claims
1. A method for producing a ceramic body, comprising: a forming step of forming a molding material comprising SiC powder with an average particle size D50 of 15 up to 50 µm and SiC powder with an average particle size D50 of 2 to 8 µm in a mass ratio of 3:7 to 7:3 to obtain a shaped body (10); and a firing and impregnation step of firing the shaped body (10) and impregnating it with metallic Si.
2. A method for producing a ceramic body according to claim 1, wherein the firing and impregnation step is carried out by firing of the shaped body (10) in contact with the metallic Si.
3. A method for producing a ceramic body according to claim 2, wherein the firing is carried out in an inert gas atmosphere or in a vacuum at a temperature of 1400 to 1600°C.
4. A method for producing a ceramic body according to any one of claims 1 to 3, wherein ceramic raw materials which are Mold material contains only the SiC powder.
5. A method for producing a ceramic body according to one of claims 1 to 4, wherein the shaped body (10) is Drying process and / or a degreasing process between the formation step and the firing and impregnation step.
6. A method for producing a ceramic body according to one of claims 1 to 5, wherein the shaped body (10) has a honeycomb shape, comprising: an outer peripheral wall (110); and partition walls (130) arranged on an inner side of the outer peripheral wall (110), wherein the partition walls (130) define a plurality of cells (120) which each extending from a first end face to a second end face; or a hollow honeycomb shape comprising: a inner peripheral wall (140); an outer peripheral wall (110); and partition walls (130) arranged between the inner peripheral wall (140) and the outer peripheral wall (110), wherein the partition walls (130) have a plurality of Define cells (120) each extending from a first end surface to a second end surface.
7. Ceramic body, comprising: SiC skeleton sections, each containing SiC particles with a particle size of 15 to 50 µm and SiC particles with a particle size of 2 to 8 µm in a volume ratio of 3:7 to 7:3; and Si-impregnated metal sections each formed at gaps of at least a part of the SiC skeleton sections are.
Citation Information
Patent Citations
Manufacturing method of honeycomb structure
JP6763699B2