Gas flow path forming element, method for producing the gas flow path forming element and device for forming the gas flow path forming element

The metal lattice structure with annular sections and flat surface portions in the gas flow path-forming element addresses the issues of damage and inefficiency in existing elements, ensuring stable gas diffusion and efficient power generation in fuel batteries.

DE112009001377B4Active Publication Date: 2024-10-10TOYOTA JIDOSHA KK +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
DE112009001377
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2008-10-20
Filing Date
2009-06-16
Publication Date
2024-10-10
Estimated Expiration
2029-06-16

AI Technical Summary

Technical Problem

The existing gas flow path-forming elements in fuel batteries suffer from issues such as the carbon paper sheet being cut or damaged, leading to reduced fuel gas supply, increased pressure loss, and unstable power generation due to the contact sections between the gas flow path-forming element and the carbon paper sheet, as well as inefficient current transmission between the gas flow path-forming element and the separator.

Method used

A gas flow path-forming element with a metal lattice structure is designed, featuring annular sections with flat surface portions that maintain surface contact with both the gas diffusion layer and the separator, preventing damage and ensuring efficient gas diffusion and current transmission, thereby improving power generation efficiency.

Benefits of technology

The solution prevents the gas flow path-forming element from cutting into the gas diffusion layer, maintains a larger usable cross-section, reduces pressure loss, and ensures stable power generation by enhancing electrical contact and reducing electrical resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Gas flow path forming element (321, 322) used in a power-generating cell (12) of a fuel cell battery (11), wherein the power-generating cell (12) has a gas diffusion layer (19, 20) formed in an electrode layer (17, 18) of an electrode structure, and a separator (23, 24) for isolating adjacent power-generating cells (12) from each other, and wherein the gas flow path forming element (321, 322) is arranged between the gas diffusion layer (19, 20) and the separator (23, 24) and has a gas flow path, wherein the power-generating cell (12) is configured to generate power via an electrode reaction generated in the electrode layer (17, 18) by supplying fuel gas or oxidizing gas through the gas flow path to the electrode layer (17, 18). generated, wherein the gas flow path forming element (321, 322) is characterized in that the gas flow path forming element (321,322) consists of a metal lattice structure (25; 325) formed from a thin metal plate (25A; 325A), wherein a plurality of through openings (26; 326) in the metal lattice structure (25; 325) are formed in a lattice-like manner, wherein the gas flow path-forming element (321, 322) has a plurality of annular sections (27; 327) which form the through openings (26; 326), wherein the annular sections (27; 327) each have a flat surface section in a contact section (329) between the annular section (27; 327) and the gas diffusion layer (19, 20), and wherein an upper annular section (R1) of the This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality. ring-shaped section (327) of a pair of inclined plate sections (327a) and a flat plate section (327b),which connects the upper ends of the inclined plate sections (327a), wherein the flat plate section (327b) is formed by a non-bent flat surface section (327f) and a bent flat surface section (329a), and a section of the flat surface section in the contact section (329) between the annular section (327) and the gas diffusion layer (19, 20) corresponds to the bent flat surface section (329a).
Need to check novelty before this filing date? Find Prior Art

Description

FIELD OF TECHNOLOGY

[0001] The present invention relates to a gas flow path forming member disposed between a gas diffusion layer and a separator in a power generating cell of a fuel battery, a method for Manufacturing the gas flow path forming member, a forming device using is used to manufacture the gas flow path forming element, a power generating cell for a fuel battery, which includes the gas flow path forming element, and a method for manufacturing the power generating cell for the fuel battery. TECHNICAL BACKGROUND

[0002] The prior art proposes a polymer electrolyte fuel battery as described in JP 2007-87768 A This type of fuel battery consists of a fuel battery stack formed by stacking power generating cells. Each of the power generating cells has a membrane / electrode arrangement with an electrolyte membrane, an anode electrode layer and a cathode electrode layer. The anode Electrode layer is formed on a first surface of the electrolyte membrane, and the cathode electrode layer is applied to a second surface of the electrolyte membrane. Fuel gas, such as hydrogen gas, and oxidizing gas, such as air, are transferred via a gas flow path forming element (a collector) to the anode electrode layer and to the cathode electrode layer. This causes an electrode reaction in the membrane / electrode assembly, whereby Power is generated. The generated power is transferred to the outside via the collector and a plate-like separator submitted.

[0003] The gas flow path forming element must be able to flow both the fuel gas and the oxidizing gas efficiently to the anode electrode layer and the cathode electrode layer. According to the structure described in JP 2007-87768 A, the gas flow path forming member consists of a metal mesh structure from which a A multitude of small through holes with predetermined shapes are formed in the Metal grid structure is formed. Similarly, by machining a stainless steel plate with a diameter of approximately 0.1 mm into a metal grid structure essentially hexagonal through openings in the manner of a grid in the Metal lattice structure. Ring-shaped sections (strands), each of which forms the hexagonal through-opening are connected to each other in a mutually overlapping state. Thus, the metal grid has a stepped cross-section.

[0004] In the power generating cell, a carbon paper sheet or sheet consisting of conductive fibers is arranged between the surfaces of the individual electrode layers and the gas flow path forming element. The carbon paper sheets diffuse the fuel gas and the oxidizing gas efficiently to the corresponding Electrode layers. If the fuel battery stack is formed by stacking a large number of power-generating cells is constructed, two separators are placed in an upper section and a lower section of each power generating cell are brought closer together to create electrical contact between the carbon paper sheet and the gas flow path forming elements. Fig. 49 shows a conventional Gas flow path forming element 1021, which is bonded between an anode electrode layer 17 Carbon paper sheet 19 and a separator 23. In this state, when the separator 23 is moved downwards pressed, contact portions 1028 of the gas flow path forming member 1021 firmly against the carbon paper sheet 19 pressed and cut into the carbon paper sheet 19, as shown in Fig. 50.

[0005] Thus, the contact portions 1028 can separate a part of the carbon paper sheet 19, whereby the The functionality of the carbon paper sheet 19 as a gas diffusion layer is impaired. Likewise, part of the Gas diffusion layer into the fuel gas flow path in the gas flow path forming element 1021, whereby the usable cross-section of the fuel gas flow path is reduced. This reduces the pressure loss of the fuel gas increased, which reduces the amount of fuel gas supplied and increases the efficiency of power generation Furthermore, separated carbon fibers can be carried along by the fuel gas and stick to the walls of the narrow Gas flow path can get stuck in the gas flow path forming element, thereby blocking the path. The flow of fuel gas is obstructed and the efficiency of power generation is reduced. Likewise, the degree in which the contact sections 1028 cut into the carbon paper sheet 19, from a power generating cells to different from others. This makes the power generation voltage unstable.

[0006] The gas flow path forming member 1021 has contact portions 1030 which are provided at the contact portions 1029 opposite side. Corners of the contact sections 1030 touch the separator 23, whereby the Sepa rator 23 is damaged. In addition, in this case it is difficult to ensure the contact surface required for a Current transmission between the gas flow path forming element 1021 and the separator 23 is necessary. the supply of electric current from the gas flow path forming element 1021 to the separator 23 is obstructed, which reduces the efficiency of power generation.

[0007] In order to solve the problem described above, a metal grid structure forming device is used, such as shown in Fig. 40. As shown in Fig. 40, the metal grid structure forming device comprises a first Shearing tool or a first shearing die 333 with a single shearing edge 333b and a second shearing tool or a second shearing die 334 which is arranged above the first shearing die 333 and has alternately arranged recesses 334b ​​and projections 334a. When using this device, a metal grid structure formed, the recesses 334b ​​and the projections 334a form a single lowering and Lifting cycle of the second shearing die 334 alternately upper semi-annular sections and lower semi-annular In this case, the lower semi-annular sections formed by the projections 334a are deformed downwards, causing the upper semi-annular sections defined by the recesses 334b are formed, sagging diagonally downwards. Each of these lowered sections forms a bent, flat surface portion 1029, as shown in Fig. 51. The bent, flat surface portion 1029 serves as Contact portion 1029 of the gas flow path forming member 1021 and is connected to the gas diffusion layer 1019 in In this way, the problems mentioned above, which are caused by the cutting of the Contact sections 1029 are released. By forming the bent, flat surface section 1029a, however, the thickness T of the gas flow path forming element 1021 decreases. This reduces the usable The cross-section of the gas flow path is reduced and the efficiency of power generation is reduced.

[0008] Furthermore, WO 2007 / 034 617 A1 discloses a separator for a fuel cell for supplying fuel gas and oxidizing gas to corresponding electrode layers of an electrode structure of the fuel cell and for discharging electricity generated by electrode reactions in the electrode layers comprising: a flat, plate-like Separator body formed from an electrically conductive material and containing a mixed flow of fuel gas and oxidizing gas by separating the fuel gas and the oxidizing gas; and a Collector formed from a metal grid having a large number of through holes, each of which has a have a predetermined opening shape, which are formed in a mesh-like, step-like arrangement; which have a Form a gas passage between the separator body and the respective electrode layers to transfer the fuel gas or supplying the oxidizing gas to the electrode layer; and wherein the gases generated by electrode reactions in the Electricity generated by the electrode layers is dissipated.

[0009] US 6 007 933 A discloses a method for promoting fluid operation for a fuel cell assembly, the method comprising: providing a flow field plate of the fuel cell assembly, wherein the Flow field plate has an open-surface flow channel formed in a surface of the plate and extending between inlet and outlet fluid distributors for the fuel cell assembly, wherein the open-area Flow channel is suitable for at least one fluid for a membrane electrode assembly of the fuel cell assembly to supply; arranging an elastic gas diffusion layer between the flow field plate surface and the Membrane electrode assembly, wherein the elastic gas diffusion layer forms a space in the fuel cell assembly dynamically; and retention of the elastic gas diffusion layer against penetration into the open-sided flow channel under a compressive force exerted on the fuel cell assembly, wherein the retention comprises abutting a first side of a support member against the flow field plate surface and abutting a second side of the carrier element against the elastic gas diffusion layer, wherein the carrier element formed with a plurality of openings extending between the first and second sides, whereby the Fluid supply is promoted.

[0010] In addition, DE 24 44859 C2 discloses a method for producing grids for lead-acid batteries by Passing an elongated strip of lead sheet between two rows of converging tools and Cutting devices forming two longitudinally extending cross-linked strip sections by means of Expanded metal forming methoda adjacent to a non-stretched central portion of the strip, wherein successively the cross-linked sections in practically the same plane as the unstretched section of the strip the cross-linked sections are stretched to form cross-linked Mesh openings of predetermined width, and the meshed sections are compressed that the diagonally opposite edges of the nodes connecting adjacent rows of networks connecting, and which protrude from the main planes of the networked sections, are flattened so that the protruding edges are flattened and the nodes are deformed from a rectangular to a polygonal shape, two opposite sides thereof in practically parallel planes to the surfaces of the meshed sections and the nodes to a thickness greater than the thickness of the strip, but substantially less than twice the Thickness of the strip can be reduced. SUMMARY OF THE INVENTION PROBLEM TO BE SOLVED BY THE INVENTION

[0011] Thus, an object of the present invention relates to a gas flow path forming member which can prevent that a contact portion of the gas flow path forming element cuts into a gas diffusion layer, and that thus improving the efficiency of power generation of a fuel battery, a method for producing of the gas flow path forming element, a shaping device used to form the gas flow path forming element, a power generating cell for a fuel battery, which forms the gas flow path forming element, and a method of manufacturing the power generating cell for the fuel battery. MEANS TO SOLVE THE PROBLEMS

[0012] The above problems and the resulting task are solved by the subject matter of the Advantageous developments of the invention are the subject of the subsequent dependent claims.

[0013] According to a first illustrative aspect of the present disclosure, a gas flow path forming Element used in a power-generating cell of a fuel battery. The power generating cell includes a gas diffusion layer formed in an electrode layer of an electrode structure and a separator for isolating adjacent power-generating cells from each other. The gas flow path forming element is arranged between the gas diffusion layer and the separator and has a gas flow path The power generating cell is designed to generate power via an electrode reaction that occurs in the Electrode layer is caused by fuel gas or oxidizing gas flowing through the gas flow path to the electrode layer. The gas flow path forming element consists of a metal mesh structure made of a thin metal plate. A plurality of through openings are arranged in the manner of a grid in the Metal grid structure. The gas flow path forming element has a plurality of annular sections which form the through openings. The ring-shaped sections each have a flat surface portion in a contact portion between the annular portion and the gas diffusion layer.

[0014] In this structure, the flat surface portion in the contact portion between the individual through-openings forming annular portions of the gas flow path forming element and the Gas diffusion layer, for example a sheet of carbon paper. The contact section is thus Surface contact with the gas diffusion layer is maintained. This prevents the contact section from entering the gas diffusion layer, preventing damage to the gas diffusion layer. Fragments of the gas diffusion layer into the gas flow path of the gas flow path forming element. prevents a reduction in the usable cross-section of the gas flow path.

[0015] The said gas flow path forming member preferably has in a contact portion between the Gas flow path forming element and the separator have a flat surface portion.

[0016] In said gas flow path forming member, the through holes and the annular Sections are preferably each formed so that they have a hexagonal cross-section, and each Contact portion is preferably arranged at a portion corresponding to a specific side of the hexagon shape.

[0017] According to a second illustrative aspect of the present disclosure, a method for manufacturing a Gas flow path forming element used in a power generating cell of a fuel battery, The power generating cell has a gas diffusion layer embedded in an electrode layer of a electrode structure, and a separator for mutually isolating adjacent power-generating cells. The gas flow path forming element is arranged between the gas diffusion layer and the separator and has a gas flow path. The power generating cell is designed to generate power through a Electrode reaction is generated, which in the Electrode layer is caused by fuel gas or oxidizing gas flowing through the gas flow path to the The method for manufacturing the gas flow path forming element includes: first step in which a metal lattice structure is formed by forming a plurality of through openings in a thin metal plate in the manner of a grid; and a second step in which, after the first step, a flat surface section in a contact section between the individual through openings of the Ring-shaped sections forming a metal grid structure and the gas diffusion layer.

[0018] In the above-mentioned method for producing a gas flow path forming member, the flat Surface section in the second step is preferably formed by the fact that the surface obtained in the first step Metal grid structure is arranged between a pair of rollers and pressed together to form the contact section to plastically transform.

[0019] In the said method for producing a gas flow path forming member, the formation of the flat surface section in the second step preferably carried out by the contact section in Thickness direction of the metal mesh structure using a fixed die and a movable die in the first step, in which the metal lattice structure is formed, it is plastically deformed.

[0020] According to a third illustrative aspect of the present disclosure, a forming apparatus created, which is used to produce a gas flow path forming element. The forming device includes a fixed cutting die with first recesses and first projections, which alternate with a a predetermined pitch or a predetermined step length, and a movable cutting die with second projections and second recesses which are provided with a predetermined pitch or a predetermined stride length. The second projections engage in the first recesses. The second recesses engage the first projections of the stationary die. The movable die is able to adjust itself in thickness and width direction of the thin metal plate. A plurality of ring-shaped sections, which which define the through openings is formed by forming a plurality of cuts in the thin metal plate in a predetermined pitch and bending and stretching the thin metal plate by engaging the first Recesses and the first projections of the fixed die with the second projections and the second Recesses of the movable die are formed in the thin metal plate. A slanted surface is in a upper surface of each of the first projections of the fixed die. The inclined surface is downwards and inclined downwards in the feed direction of the thin metal plate.

[0021] According to a fourth illustrative aspect of the present disclosure, a forming apparatus created, which is used to produce a gas flow path forming element. The forming device has a fixed cutting die with first recesses and first projections, which alternate with a predetermined pitch, and a movable punching die with second projections and second Recesses arranged at a predetermined pitch. The second projections engage in the first recesses. The second recesses engage with the first projections of the fixed die. The Movable cutting die is capable of moving back and forth in the thickness and width direction of the thin metal plate. A plurality of annular sections defining the through openings are formed by forming a A plurality of cuts in the thin metal plate at a given pitch and bending and stretching of the thin metal plate by engaging the first recesses and the first projections of the fixed Cutting die with the second projections and the second recesses of the movable cutting die in the thin metal plate. An inclined surface is formed in a lower surface of each of the second projections of the movable cutting die. The inclined surface is upwards and opposite to the feed direction of the thin Metal plate tilted upwards.

[0022] In the said forming device, the fixed die or the movable die bends preferably two side portions of each annular portion located on opposite sides of a contact section of the annular section and a gas diffusion layer of the fuel battery, in the direction to the center of the annular section.

[0023] According to a fourth illustrative aspect of the present disclosure, a gas flow path forming An element provided with a gas diffusion layer formed in an electrode layer of an electrode structure, and a gas flow path formed between the gas diffusion layer and a separator to supply fuel gas or oxidizing gas. The gas flow path forming element is designed to have a Electrode reaction caused by Supplying the fuel gas or the oxidizing gas to the electrode layer through the gas flow path in the Electrode layer generates electrical power. The gas flow path forming element is made of a Metal lattice structure formed by forming a plurality of ring-shaped sections in a thin metal plate is constructed like a grid. Each of the ring-shaped sections has a through-opening. A first flat surface portion contacting a surface of the gas diffusion layer is in a first contact portion each of the annular sections. A second flat surface section forming a back side of the separator is formed in a second contact portion of each annular portion. A width of the first flat surface section in the direction of the gas flow path is set to be larger than a width of the second flat surface section in the direction of the gas flow path.

[0024] In this construction, the annular sections forming the through openings are in Gas flow path forming element. The first flat surface portion is formed in the first contact portion, which touches the gas diffusion layer, for example a sheet of carbon paper, by pressing in the outer edge of each annular The first flat surface section is thus provided with a corresponding surface of the Gas diffusion layer is kept in surface contact. This prevents the first contact section from entering the Gas diffusion layer, preventing damage to the gas diffusion layer. that the usable cross-section of the gas flow path is limited by fragments of the gas diffusion layer that are Gas flow path of the gas flow path forming element is reduced.

[0025] The second flat surface portion is formed in the second contact portion contacting the separator by pressing in the outer edge of each annular section. The second flat surface section is thus formed with the Back of the separator is kept in surface contact, preventing damage to the separator and a necessary current transfer surface between the gas flow path forming element and the separator This reduces the electrical resistance caused by power generation, and the efficiency of power generation is improved.

[0026] The width of the first flat surface portion is set to a relatively large value in order to prevent the first flat surface section from cutting into the gas diffusion layer. The width of the second flat surface section is set only so much smaller than the width of the first flat surface section that a Damage to the separator is prevented and that a necessary current transfer surface between the second flat surface section and the separator. This ensures a suitable thickness of the gas flow path forming element and a usable cross section of the gas flow path in the Gas flow path forming element is enabled. If the width of the second flat surface portion of the width of the first flat surface portion, the gas flow path forming element would be excessively pressed together when the first and second flat surface sections are pressed. This would increase the thickness of the gas flow path forming element and the gas flow path can be reduced.

[0027] As stated above, the gas flow path forming member is preferably constructed such that: connecting plate portions which connect the annular portions to each other; a first, semi-annular portion facing the gas diffusion layer is arranged in each annular portion; the first semi-annular portion comprises a pair of first side plate portions connected to the corresponding connecting plate sections, a pair of first inclined plate sections integrally formed with the ends of the first side plate portions, and has a first flat plate portion which is formed integrally with the first inclined plate sections in such a way that it forms the first inclined plate sections together, wherein the first flat plate section has a first contact section, which contacts the gas diffusion layer, wherein the first flat surface portion is formed in the first contact portion a second semi-annular portion facing the separator is formed in each annular portion and the second semi-annular portion is a pair of second inclined plate portions integral with the connecting plate sections, a pair of parallel side plate sections integrally formed with ends the second inclined plate portions are formed, and has a second flat plate portion which is formed integrally with the second side plate sections in such a way that it covers the second side plate sections together, wherein the second flat plate section has a second contact section which contacts the separator, wherein the second flat surface portion is formed in the second contact portion is.

[0028] According to a fifth illustrative aspect of the present disclosure, a method for manufacturing a The method includes: a first step in which, under Using a first shearing die and a second shearing die, alternately the first semi-annular sections, the facing the gas diffusion layer, and the second semi-annular sections facing the separator, at a plurality of locations at one end of the thin metal plate, wherein the first shearing shape is a a plurality of first recesses and a plurality of first projections arranged alternately with a predetermined pitch, and the second shearing shape has second projections and second recesses which are arranged alternately at a plurality of locations with a predetermined pitch, wherein the second projections correspond to the first recesses and the second recesses correspond to the first projections a second step in which the first semi-annular sections and the second semi-annular Section by moving the thin metal plate over a predetermined distance and displacing the first shearing die and the second shearing die perpendicular to a feed direction of the thin metal plate alternately at a plurality of locations of the thin metal plate; a third step in which by forming a plurality of ring-shaped sections, each having a through opening, in the thin metal plate in the manner of a Grid by means of the first semi-annular sections and the corresponding second semi-annular sections, which are in Feed direction of the thin metal plate by alternately repeating a step similar to the first step and a step similar to the second step, are arranged side by side or adjacent to each other, a metal lattice structure is obtained; and a fourth step in which by simultaneously pressing two surfaces the metal grid structure after the third step, a first flat surface section in the first contact section of the first semi-annular portion and a second flat surface portion in the second contact portion of every second semi-annular portion, wherein the width of the first flat surface portion is in the direction of gas flow path is set so that it is smaller than the width of the second flat surface section in Direction of the gas flow path.

[0029] According to a sixth illustrative aspect of the present disclosure, a forming apparatus which is used in a method for manufacturing a gas flow path forming element. The Device includes a first shearing mold, a second shearing mold and a pressing machine which forms the metal grid structure including ring-shaped sections in the thickness direction of a metal grid structure. The metal grid structure is by moving the first shearing die and the second shearing die back and forth in the thickness direction of the thin metal plate and perpendicular to the feed direction of the thin metal plate, which creates an engagement between the first recesses and the second projections and between the first projections and the second recesses, and by bending and stretching the thin metal plate after forming a plurality of cuts in the thin metal plate with a predetermined pitch. The first projections, the first recesses, the second Recesses and the second projections are shaped so that a dimension in which each first semi-annular portion is formed when pressed, and a dimension in which the corresponding second semi-annular section is formed when it is pressed, are different to press the semi-annular sections.

[0030] In the said forming device, each first projection of the first shearing mold and each second Recess of the second shearing die each have a shaping surface for forming a pair of first Side plates forming the first semi-annular portion, a forming surface for forming a pair of first inclined plate sections connected to the first side plates, and a shaping surface to form a first flat plate section which is thus connected to the first oblique plate sections in such a way that it connects the first inclined plate sections. Likewise, each first recess of the first shearing die and each second projection of the second shearing die each have a shaping Surface for forming a pair of second inclined plate sections which define the second semi-annular section, a forming surface for forming a pair of second side plate sections, which the first inclined plate sections are connected, and a shaping surface for forming the second flat plate portion connected to the second side plate portions in such a way that it defines the second Connects side plate sections together.

[0031] According to a seventh illustrative aspect of the present disclosure, a power generating cell for a fuel battery. The cell comprises: an electrode layer, a gas diffusion layer, which is deposited on a surface of the electrode layer, a separator directed to the gas diffusion layer, and a Gas flow path forming Element arranged between the gas diffusion layer and the separator and defining a gas flow path through which fuel gas or oxidizing gas is supplied to the electrode layer. The power-generating cell generates power via an electrode reaction that is induced in the electrode layer. The gas flow path forming Element consists of a metal grid structure formed by a thin metal plate. A large number of annular sections, each having a continuous opening of a predetermined shape, is shown in the The gas flow path forming element is designed in the manner of a grid. A bent flat surface section, which is held in surface contact with a surface of the gas diffusion layer is in each of the annular sections. A non-bent flat surface section is formed between the bent flat surface section and the connecting plate sections, which form the corresponding annular sections The bent flat surface section and the non-bent flat Surface section are in a plurality of successive steps using a device for Formation of a metal lattice structure.

[0032] According to the present disclosure, the bent flat surface portion in which the Gas diffusion layer, for example a carbon paper sheet, touching contact section in the outer edge of each of the annular sections of the gas flow path forming element, which form the through openings, The bent flat surface section is thus provided with a corresponding surface of the Gas diffusion layer is kept in surface contact. This prevents the contact section from entering the gas diffusion layer, thereby preventing damage to the gas diffusion layer. Fragments of the damaged gas diffusion layer into the gas flow path in the gas flow path forming element. Thus prevents the usable cross-section of the gas flow path from being reduced.

[0033] According to the present disclosure, the bent flat surface portions and the non- bent flat surface sections in two metal grid structure machining passes. Thus, compared to a case where a wide bent flat surface section in a single Machining pass in the entire area of ​​each annular section in the width direction of the annular section is formed, the width of the formed bent flat surface portion is reduced and The thickness of the gas flow path forming element is increased accordingly. As a result, the usable The cross-section of the gas flow path is increased and the efficiency of power generation is improved.

[0034] In the power generating cell for a fuel battery according to the present disclosure, each annular section preferably formed in a pentagonal or hexagonal shape.

[0035] According to an eighth illustrative aspect of the present disclosure, a method for producing a power-generating cell for a fuel battery. The process includes a first step, which includes: consecutively processing a plurality of first sections to be processed and a plurality of second sections to be machined in the thin metal plate, which alternate in the feed direction of the thin metal plate are arranged, using a first shearing die and a second shearing die, wherein the first shearing die is a linear first shear edge and the second shear shape has a plurality of recesses and a plurality of projections arranged alternately at a predetermined distance, with second shear edges being arranged in the projections are designed to cooperate with the first shearing edge to form a plurality of incisions in the thin metal plate; and forming the semi-annular portions each corresponding to the bent flat surface section, in the first sections of the thin metal plate to be machined at a stage in each of the first sections to be processed into a shape with respect to the first shearing shape and the second shearing shape middle forming position. The process also includes: a second step in which, after the first step in a stage where each of the first sections to be processed is cut into a shape with respect to the first shearing and the second shearing die was moved to the last position, semi-annular sections, each of which corresponds to the non-bent flat surface portion, are formed in the first sections to be machined; a third Step in which, after the second step, in a stage where each of the second sections to be processed, which is attached to the corresponding first section to be machined in the thin metal plate, from a feed direction of the thin metal plate upper side to the middle in relation to the first shearing form and the second shearing form Forming position was moved by moving the second shearing die perpendicular to the feed direction of the thin Metal plate the semi-circular sections, each having the bent flat surface section, into the second sections to be processed; a fourth step in which, after the third th step in a stage where each of the second sections to be machined is cut into the shape relative to the first shearing and the second shearing form was moved to the last training position, the semi-circular sections, each of which has the non- bent flat portion are formed in the second sections to be machined; and a Step in which by forming the annular sections in the thin metal plate in the manner of a grid by alternately repeating the first and second steps and the third and fourth steps metal lattice structure is formed.

[0036] In the method for manufacturing a power generating cell for a fuel battery according to the In the present disclosure, the second step and the fourth step are preferably carried out multiple times. SHORT DESCRIPTION OF THE DRAWING Fig. 1 is a vertical cross-sectional view of a fuel battery stack containing power-generating cells having a gas flow path forming member according to the present invention; Fig. 2 is an exploded view of a power generating cell; Fig. 3 is a perspective view of a portion of a first gas flow path forming member according to a first embodiment of the present invention with a partial cross-sectional view; Fig. 4 is a cross-sectional view of a processing device for a metal mesh structure; Fig. 5 is a partial perspective view of a fixed cutting die or a fixed punching tool and a movable punching die or a movable punching tool; Fig. 6 is a partial cross-sectional view of the metal mesh structure processing device, where the fixed punching tool and the movable punching tool engage with each other; Fig. 7 is a plan view of a section of the metal grid structure; Fig. 8 is a cross-sectional view taken along line 8-8 of Fig. 7; Fig. 9 is a perspective view of a section of a metal lattice structure before the formation of a flat surface section; Fig. 10 is a schematic diagram of an apparatus for forming a flat surface portion; Fig. 11 is a partial cross-sectional view showing a stage in which a carbon paper sheet, a first gas flow path forming element and a first separator are stacked on top of each other; Fig. 12 is a partial perspective view of a fixed punching tool and a movable Punching tool according to another embodiment; Fig. 13 is a cross-sectional view of a process for forming a flat surface portion in a metal grid structure using the fixed punching tool and the movable punching tool shown in Fig. 12; Fig. 14 is a partial cross-sectional view showing a stage in which a carbon paper sheet, a first gas flow path forming element and a first separator are stacked on top of each other; Fig. 15 is a partial cross-sectional view showing an apparatus for forming a flat surface section according to another embodiment of the invention; Fig. 16 is a cross-sectional view showing a metal lattice structure before the formation of a flat surface section; Fig. 17 is a cross-sectional view showing a metal lattice structure after the formation of a flat surface section; Fig. 18 is a cross-sectional view showing a metal lattice structure before the formation of a flat surface section; Fig. 19 is a cross-sectional view showing the metal grid structure after the formation of the flat surface section; Fig. 20(a) and Fig. 20(b) are partial cross-sectional views each showing a machining device for a Metal grid structure according to another embodiment of the invention; Fig. 21 is a partial cross-sectional view showing a stationary punching tool according to another embodiment of the invention; Fig. 22 is a partial cross-sectional view showing a gas flow path forming member according to a second embodiment of the invention; Fig. 23 is a partial front view showing the gas flow path forming member; Fig. 24 is a partial cross-sectional view of the gas flow path forming element; Fig. 25 is a cross-sectional view of a machining device for a metal mesh structure; Fig. 26 is a partial cross-sectional view showing a first shear shape and a second shear shape; Fig. 27 is a partial cross-sectional view of the machining device for a metal lattice structure, and shows the mode of operation of the device; Fig. 28 is a partial perspective view of a metal lattice structure; Fig. 29 is a partial front view of the metal grid structure; Fig. 30 is a cross-sectional view of the metal grid structure; Fig. 31 is an enlarged partial front view showing an annular section of the metal grid structure; Fig. 32 is a front view of a pressing device; Fig. 33 is an enlarged cross-sectional view of a stacked structure comprising a gas diffusion layer, a first gas flow path forming member and a first separator; Fig. 34 is a partial front view of an annular portion according to another embodiment; Fig. 35 is a partial perspective view of a gas flow path forming member according to a third Embodiment of the invention; Fig. 36 is a front view of a portion of a first gas flow path forming member; Fig. 37 is a cross-sectional view of a portion of the first gas flow path forming member; Fig. 38 is a cross-sectional view of a stack structure containing a gas diffusion layer, the first gas flow path forming element and a first separator; Fig. 39 is a cross-sectional view of a metal grid structure forming device for a metal grid structure; Fig. 40 is a perspective view of a section of a first shearing die and a section of a second shearing shape; Fig. 41(a) and Fig. 41(b) are a side cross-sectional view and a front view of a step in the Manufacturing a gas flow path forming element; Fig. 42(a) and Fig. 42(b) are a side cross-sectional view and a front view of a step in the Manufacturing the gas flow path forming element; Fig. 43(a) and Fig. 43(b) are a side cross-sectional view and a front view of a step in the Manufacturing the gas flow path forming element; Fig. 44(a) and Fig. 44(b) are a side cross-sectional view and a front view of a step in the Manufacturing the gas flow path forming element; Fig. 45(a) and Fig. 45(b) are a side cross-sectional view and a front view of a step in the Manufacturing the gas flow path forming element; Fig. 46(a) and Fig. 46(b) are a side cross-sectional view and a front view of a step in the Manufacturing the gas flow path forming element; Fig. 47(a) and Fig. 47(b) are a side cross-sectional view and a front view of a step in the Manufacturing the gas flow path forming element; Fig. 48(a) and Fig. 48(b) are a side cross-sectional view and a front view of a step in the Manufacturing the gas flow path forming element; Fig. 49 is a cross-sectional view of a stacking stage of a carbon paper sheet, a first Gas flow path forming element and a first separator, which is a conventional power generating form cell; Fig. 50 is a cross-sectional view of the first separator pressed against the carbon paper sheet; and Fig. 51 is a cross-sectional view of a stack structure comprising a gas diffusion layer, a gas flow path forming element and a separator of a conventional power generating cell. BEST MODE FOR CARRYING OUT THE INVENTION (First embodiment)

[0037] An embodiment of a polymer electrolyte fuel battery stack 11 having a first gas flow path forming element according to the present The invention will now be described with reference to Figs. 1 to 21.

[0038] As shown in Fig. 1 and Fig. 2, the fuel battery stack 11 is constructed by stacking a plurality of power generating cells 12. Each of the power generating cells 12 has a first frame 13, a second Frame 14 and an MEA (membrane / electrode assembly) 15, which serves as the electrode structure. The first and second frames 13, 14 are each made of synthetic rubber or synthetic resin and are arranged in a rectangular The first frame 13 and the second frame 14 have a fuel gas passage S1 and a Oxidizing gas passage space S2. The MEA 15 is arranged between the frames 13, 14. Each power generating cell 12 also has a first gas flow path accommodated in the fuel gas passage space S1. forming element 21 and a second gas flow path accommodated in the oxidizing gas passage space S2. forming element 22. The first and second gas flow path forming elements 21, 22 are both made of titanium The power generating cell 12 further comprises a first separator 23 and a second separator 24. The first separator 23 is connected to the upper surface or top side of the first frame 13 and the upper surface or top of the first gas flow path forming member 22. The second separator 24 is connected to the lower Surface or bottom of the second frame 14 and the lower surface or bottom of the gas flow path- forming element 22. The first and second separators 23, 24 are both made of titanium and are bonded to a flat plate. The shapes of the gas flow path-forming elements 21, 22 are shown in simplified form in Fig. 2.

[0039] Gas flow paths 13a, 13b, each formed by an elongated opening, are arranged in a pair opposite edges of the first frame 13. Gas flow paths 14a, 14b, each of which is elongated opening are formed in a pair of opposite edges of the second frame 14 More specifically, the gas flow paths 13a, 13b are formed in the edges of the first frame 13, which are not correspond to the edges of the second frame 14 in which the gas flow paths 14a, 14b are formed.

[0040] The MEA 15 consists of an electrode membrane 16, an anode electrode layer 17, a cathode Electrode layer 18 and carbon paper sheets 19, 20, each serving as a conductive gas diffusion layer. The anode Electrode layer 17 is formed by stacking or placing a predetermined catalyst on top of the Electrode membrane 16 is formed. The cathode electrode layer 18 is formed by applying a predetermined catalyst on the underside of the electrode membrane 16. The carbon paper sheet 19 is glued to the corresponding surface of the Anode electrode layer 17, and the carbon paper sheet 20 is bonded to the corresponding surface of the cathode Electrode layer 18. Gas inlet openings 23a are two edges of the first separator 23, which are perpendicular Gas outlet openings 23b are provided at the two other edges of the first separator 23, which perpendicular to each other. Likewise, gas inlet openings 24a are formed in two edges of the second separator 24, which are perpendicular to each other. Gas outlet openings 24b are formed in the other two edges of the second separator 24, which run perpendicular to each other.

[0041] As shown in Fig. 3, the first and second gas flow path forming elements 21, 22 each consist of a titanium element formed into a lattice structure 25 (hereinafter referred to simply as metal lattice structure) and which has a thickness of about 0.1 mm. Substantially hexagonal through openings 26 are provided on staggered manner in the metal grid structure 25. Ring-shaped sections 27, which form the continuous Openings 26 are connected to each other so that they overlap each other. Each of the annular sections 27 has a first contact portion 28 which contacts the carbon paper sheet 19, 20, and a second contact portion 29, which contacts the inner surface of the first or second separator 23, 24. A first flat surface portion 28a and a second flat surface portion 29a are in the first contact portion 28 and in the second contact portion 29, respectively. The first flat surface portion 28a is brought into surface contact with the carbon paper sheet 19, 20 and the second flat surface portion 29a is held in surface contact with the separator 23, 24.

[0042] The first gas flow path forming element 21 is arranged in such a way in the fuel gas passage space S1 of the first frame 13 is arranged so that it covers the corresponding surface of the carbon paper sheet 19 and the inner surface of the first separator 23. The second gas flow path forming element 22 is thus in the oxidizing gas Passage space S2 of the second frame 14 is arranged so that it covers the corresponding surface of the carbon paper sheet 20 and touches the inner surface of the second separator 24.

[0043] As shown by an arrow G1 in Fig. 2, the first gas flow path forming member 21 supplies fuel gas from the first gas inlet opening 23a of the first separator 23 into the fuel gas passage S1. The fuel gas then flows to the first Gas outlet openings 23b or the gas flow path 14b of the second frame 14 and to the corresponding first Gas outlet opening 24b of the second separator 24.

[0044] As shown by an arrow G2 in Fig. 2, the second gas flow path forming member 22 Oxidizing gas from the second gas inlet opening 23a of the second separator 23 via the gas flow path 13a of the first frame 13 into the oxidizing gas passage space S2. The oxidizing gas then flows over the Gas flow path 13b of the first frame 13 to the second gas outlet opening 23b or to the second gas outlet opening 24b of the second separator 24.

[0045] In order to ensure the tightness of a contact surface between the first frame 13 and the electrode membrane 16 and the second frame 14, the first and second frames 13, 14 are each formed of synthetic resin. Therefore, when the fuel battery stack 11 is constructed by stacking the power generating cells 12, the Load or force generated by clamping the fuel battery stack 11 that the first and second Gas flow path forming elements 21, 22 in a state in which they are separated by the corresponding first and second Separators 23, 24 are pressed against the MEA 15. This ensures an appropriate Contact state between the first flat surface portions 28a of the first contact portion 28 and the Carbon paper sheet 19 and an appropriate contact state between the second flat surface portions 29a of the second contact sections 29 and the first separator 23. Since the second gas flow path forming Element 22 is constructed in the same way as the gas flow path forming element 21, an appropriate Contact state both between the first flat surface portions 28a of the first contact portions 28 and the Carbon paper sheet 20 as well as between the second flat surface portions 29a of the second contact portions 29 and the second separator 24.

[0046] Between each two of the stacked, power-generating cells 12, which are adjacent to each other, are the first gas inlet openings 23a of the first separator 23 via the fuel gas passage space S1 of the first frame 13 and the gas flow path 14a of the second frame 14 with the corresponding first gas inlet openings 24a of the second separator 24. In this way, a fuel gas flow path (a hydrogen gas flow path). The second gas inlet openings 23a of the first separator 23 are above the Gas flow path 13b of the first frame 13 and the oxidizing gas passage space S2 of the second frame 14 with the corresponding first gas inlet openings 24a of the second separator 14. In this way, a Oxidizing gas flow path (an air flow path) is formed.

[0047] The first gas flow path forming member 21 causes the fuel gas in the fuel gas flow path to flow in a uniformly diffused state into the fuel gas passage space S1. The second gas flow path forming Element 22 causes the oxidizing gas in the oxidizing gas passage space S2 to diffuse in a uniform manner. state into the oxidizing gas passage space S2. In other words, the flow of the fuel gas in the fuel gas Passage space S1 flows through the through openings 26 formed in the first gas flow path forming element 21 are formed in a staggered manner, causing turbulence. As a result, the fuel gas in the gas flow Through space S1 is diffused evenly. In this way, the fuel gas is diffused by passing through the carbon paper sheet 19 diffused and evenly delivered to the anode electrode layer 17.

[0048] Likewise, the oxidizing gas in the oxidizing gas passage space S2 flows through the through openings 26, which are formed in the second gas flow path forming element 22 in a staggered manner, whereby turbulence As a result, the oxidizing gas is diffused evenly in the oxidizing gas passage space S2. In this way, the oxidizing gas is diffused by passing through the carbon paper sheet 20 and evenly supplied to the cathode electrode layer 18. This supply of fuel gas and oxidizing gas to the MEA 15 creates a Electrode reaction in the MEA 15, and power is generated. Since a large number of power-generating cells 12 are stacked in the fuel battery stack 11, the desired output power is obtained.

[0049] Now, a method for manufacturing the first and second gas flow path forming members 21, 22 described.

[0050] The first gas flow path forming member 21 is formed using the machining apparatus for a Metal grid structure shown in Fig. 4. The processing device for a metal grid structure has a pair of feed rollers 31 which continuously feed thin titanium plates 25A. The processing device for a Metal grid structure has a forming mechanism 32 to form the metal grid structure 25. The Shaping mechanism 32 forms a plurality of incisions in the thin titanium plate 25A and shapes the thin titanium plate 25A by bending and Stretching plastically. The forming mechanism 32 forms the plurality of hexagonal through openings 26 in the thin titanium plate 25A in the manner of a lattice and brings the thin titanium plate 25A into a stepped shape. The Forming mechanism 32 has a fixed punching tool or a fixed punching die 33, the is fixed immovably in a predetermined position, and a movable punching tool or a movable Cutting die 34, which can move up, down, left and right.

[0051] As shown in Fig. 5, the fixed punching tool 33 has a side wall 33a which is Feed direction of each thin titanium plate 25A is arranged below. A plurality of projections 33b (first projections) and a plurality of recesses 33c (first recesses) are formed in an upper portion of the side wall 33a. The projections 33b and the recesses 33c are alternately formed with a predetermined lateral pitch. A plurality of projections 34a (second projections) which are connected to the corresponding recesses 33c of the fixed punching tool 33, and a plurality of Recesses 34b (second recesses) which correspond to the corresponding projections 33b of the fixed Punching tool 33 are formed in a lower portion of the movable punching tool 34. The projections 34a and the recesses 34b are alternately arranged with a predetermined lateral pitch The stationary punching tool 33 has shearing edges 33d, each of which is arranged at the upper end of the inner surface of the corresponding recess 33c and form a notch in the thin titanium plate 25A. The movable punching tool 34 has shearing edges 34c, each of which is located at the lower end of the associated projection 34a are formed to form a notch in the thin titanium plate 25A.

[0052] As shown in Fig. 4, the feed rollers 31 move a thin titanium plate 25A from the fixed Punching tool 33 via predetermined processing step lengths to the movable punching tool 34. At this stage the shearing edges 33d of the fixed punching tool 33 and the shearing edges 34c of the movable punching tool 34 so that the shearing edges can shear a section of the thin titanium plate 25A to form a A plurality of cuts in the thin titanium plate 25A. The movable punching tool is continuously a lowest position and presses down the thin titanium plate 25, whereby the plate 25A by means of the projections 24a of the movable punching tool 34 is bent and stretched. By such bending and stretching of a Section of the thin titanium plate 25A, the thin titanium plate 25A is formed into a substantially trapezoidal shape, as shown in Fig. 6. After that, the movable punching tool 34 moves upwards from the lowest position and returns to its starting position.

[0053] Then, the feed rollers 31 move the thin titanium plate 25A again over a predetermined step length to the Forming mechanism 32. Synchronously, the movable punching tool 34 moves over a distance which the half of the alignment step of the annular sections 27, to the left or right. The movable Punching tool 34 then lowers again to cut into the previously machined bent-stretched section by offset by half a step, to form incisions in the thin titanium plate 25A, and bends / stretches the thin titanium plate 25A. In this way, by forming the plurality of through holes 26 in the thin Titanium plate 25A and by bending and stretching the thin titanium plate 25A, the metal grid structure 25 is completed.

[0054] By repeating the above-described process, the through openings 26 are formed in the manner of a grid and formed in a staggered manner in the metal grid structure 25, as shown in Fig. 7 to 9. Although the projections 33b and the recesses 33c of the fixed punching tool 33 with the projections 34a and the recesses 34b of the movable punching tool 34, there are non-machined areas in the metal grid structure 25 Sections that are not processed by the lowering movable punching tool 34. The non- machined section, the annular sections 27 are in a mutually overlapping state connected to each other. In this way, the metal grid structure 25 with the stepped cross-section is formed as shown in Fig. 8 and Fig. 9.

[0055] Now, a method for forming the first flat surface portion 28a and the second flat Surface portion 29a in each of the first contact portions 28 and each of the second contact portions 29 described.

[0056] As shown in Fig. 10, a device 40 for forming a flat surface portion comprises a pair Tables 42, 43 which carry the metal grid 25 on top of a support surface 41. A mechanism 44 for Formation of a flat surface section is attached to the support surface 41. The mechanism 44 for Formation of a flat surface section indicates a Column 45, a motor (not shown) mounted on the column 45, and a pair of compression rollers 46, 47, which are rotated by the motor.

[0057] In order to form the flat surface portions 28a, 29a in the first and second contact portions 28, 29 of the To form the metal grid structure 25, the metal grid structure 25 is moved from the table 42 to the position between the Compression rollers 46, 47, which rotate as shown by arrows. The two compression rollers 46, 47 then press the top and bottom of the metal grid structure 25 together and move the metal grid structure 25 to the right as shown in Fig. 10. This operation presses the first and second contact sections 28, 29 of the Metal grid structure 25 from above and below in a predetermined amount. In this way, the first and second contact sections 28, 29 are plastically deformed so that the first flat surface sections 28a in the first contact portions 28 and the second flat surface portions 29a in the second contact section 29 is formed. Thereafter, the metal grid structure 25 is cut to a predetermined size, and the first and second gas flow path forming members 21, 22 are formed.

[0058] As shown in Fig. 11, first gas flow path forming elements 21 are provided in each of the power generating Cells 12 are formed, which are shown in Fig. 1, wherein the first flat surface sections 28a are connected to the top of the carbon paper sheet 19 are kept in surface contact and the second flat surface portions 29a with the underside of the first separator 23 in surface contact.

[0059] The first embodiment has the advantages described below. (1) The first gas flow path forming member 21 provided in the fuel gas passage space S1 of the first frame 13 consists of the metal grid structure 25. The second gas flow path forming element 22, which is accommodated in the oxidizing gas passage space S2 of the second frame 14 also consists of the metal grid structure 25. The first flat surface section 28a is in first contact portion 28 of each of the annular portions 27 touching the carbon paper sheet 19, which form the through openings 26 of the metal grid structure 25. This provides a Surface contact between the first contact sections 28 and the fiber-based Carbon paper sheet 19. This prevents the first contact sections 28 from penetrating the surface of the carbon paper sheet 19. This prevents the carbon paper sheet 19 and the Carbon paper sheet 20 into the fuel gas flow path of the first gas flow path forming member 21 and enter the oxidizing gas flow path of the second gas flow path forming member 22. This results in a reduction of the usable cross sections of the fuel gas passage S1 and the oxidizing gas passage space S2 is prevented. As a result, the supplied Fuel gas and oxidizing gas quantities decrease, and a decrease in the efficiency of the Power generation is avoided.

[0060] Furthermore, in contrast to a case where the first and second contact portions 28, 29 Carbon paper sheets 19, 20 touch linearly, the carbon paper sheets 19, 20 are reliably electrically connected to the corresponding first and second gas flow path forming elements 21, 22. This allows the flow smoothly from the carbon paper sheets 19, 20 to the first and second gas flow path forming elements 11, 22 It also prevents the carbon paper sheets 19, 20 from being transferred by the first and second Contact sections 28, 29 may be damaged. This will prevent clogging of the gas flow paths in the Gas flow path forming elements 21, 22 due to broken or torn carbon fibers is prevented. the power generation capacity is ensured.

[0061] (2) The second flat surface portion 29a is formed in each of the second contact portions 29 of the first and second Gas flow path forming elements 21, 22. This ensures surface contact between the second flat surface sections 29a and the first and second separators 29. Thus, in comparison to a case where the second contact portions 29 linearly contact the first and second separators 23, 24, the first and second gas flow path forming elements 21, 22 are reliably electrically connected to the first and second separators 23, 24. This ensures smooth power transmission from the gas flow path forming Elements 21, 22 to the separators 23, 24 is possible, thereby improving the efficiency of current collection. Likewise, the separators 23, 24 are prevented from being damaged by the second contact sections 29.

[0062] (3) The device 40 for forming the flat surface sections has the two rollers 46, 47, which are arranged in Fig. 10. The use of these rollers 46, 47 facilitates the formation of the flat surface sections 28a, 29a in the first ten and second contact sections 28, 29 of the metal grid structure 25.

[0063] The first embodiment may be modified as follows.

[0064] The structure of the fixed punching tool 33 of the forming mechanism 32 can be changed as shown in Fig. 12 to 24. In this case, inclined surfaces 33e are formed in the tops of the projections 33b of the stationary punching tool 33. The inclined surfaces 33e are in the feed direction of the thin Titanium plate 25A is inclined downwards. Likewise, inclined surfaces 34d are formed in the inner surfaces of the recesses 34b of the movable punching tool 34. Like the inclined surfaces 33e, the inclined surfaces 34d inclined downwards in the feed direction of the thin titanium plate 25A. When the metal grid structure 25 is fixed punching tool 33 and the movable punching tool 34, the inclined surfaces form 33e, 34d bent portions in the first contact portions 28 of the annular portions 27. A surface each of the bent sections forms the first flat surface section 28a. In this case, the first flat surface portions 28a are formed only in the first contact portions 28, which the carbon paper sheet 19 Alternatively, as shown by the double-dotted line in Fig. 13, the thickness of the movable punching tool 34 so that flat sections 34e, each horizontally extending from the corresponding oblique surface 34d, are formed in the movable punching tool 34. This increases the rigidity of the movable punching tool 34 increased.

[0065] The thus prepared first gas flow path forming member 21 is in each of the power generating cells 12 wherein the first flat surface portions 28a of the first contact portions 28 are in contact with the carbon paper sheet 19 of the MEA 15 are kept in surface contact.

[0066] As shown in Fig. 15, inclined surfaces 34f extending in the feed direction of the thin titanium plate 25A inclined upwards, formed in the lower surfaces of the projections 34a of the movable punching tool 34 In this case, the flat surface portions 29a are formed in the second contact portions 29.

[0067] The structure shown in Fig. 12 and the structure shown in Fig. 15 can be used in combination In this case, both the first flat surface sections 28a and the second flat Surface sections 29a at the contact section 28 or at the contact section 29 in the gas flow path forming element 21 trained.

[0068] If using the device 40 shown in Fig. 10 for forming flat Surface sections flat surface sections in the metal grid structure 25 shown in Fig. 16 which are formed by the hexagonal annular sections 27 forming through openings 26 two sides of each hexagonal annular section 27, which are located on opposite sides of the contact section between the annular section 27 and the carbon paper sheet 20, outwards extended, as shown in Fig. 17. This allows the usable cross-section of a gas flow path T, which is carbon paper sheet 20 and the metal grid structure 25. To solve this problem, the sides of each hexagonal annular section 27 so towards the center of the through opening 26 be bent so that, as shown in Fig. 18, essentially L-shaped or curved bent Sections 27a are formed. If the metal grid structure 25 is formed as shown in Fig. 18 and then the Processing by the device 40 to form a flat surface, the surface or Cross section of each through opening 26 is reduced, but the usable cross section of the gas flow path T is enlarged, as shown in Fig. 19. This increases the efficiency of the power generation of the fuel battery improved overall.

[0069] For example, as shown in Fig. 20(a), both sides of each projection 34a and both sides each recess 34b of the movable punching tool 34 is made with inclined surfaces to support the bent sections 27a of the annular sections 27. Alternatively, as shown in Fig. 20(b), both Sides of each projection 33b and both sides of each recess 33c of the fixed punching tool 33 are inclined surfaces can be made.

[0070] The flat surface portions 28a, 29a may be formed in the first and second gas flow path forming Elements 21, 22 by compressing the metal grid structure 25 to a predetermined extent in the thickness direction of the Metal grid structure 25 can be formed using a press machine. The first contact portions 28 and the second contact sections 29 can be formed using a grinding machine or by mechanical processing be trained.

[0071] In addition to stainless steel plates, plates made of conductive metal, for example aluminum nium, copper or titanium as materials for the first and second gas flow path forming elements 21, 22 can be used.

[0072] As shown in Fig. 21, the fixed punching tool 33 may consist of a tool 33h and a lower, movable punching tool 33i, which are separate bodies. In this case, the upper movable punching tool 34 by actuating a lifting mechanism (not shown) or an auxiliary motor M1 up, down, left and right. The stationary punching tool 33 can be made of a die and a lower movable punching tool, which are separate bodies, as in the Structure shown in Fig. 21. (Second embodiment)

[0073] Now, a second embodiment of the present invention will be described with reference to Figs. 22 to 34. a detailed description of components of the second embodiment, the corresponding components of the are similar or identical to the first embodiment, are omitted here.

[0074] As shown in Fig. 23, a semi-annular portion R1 (a first semi-annular portion) which Gas diffusion layer 19, arranged in an upper portion of an annular portion 227. The semi-annular portion R1 consists of a pair of first side plate portions 227a, a pair of first oblique Plate sections 227b and a first flat plate section 227c. The first inclined plate sections 227b are formed integrally with the upper ends of the corresponding side plate portions 227a. The first flat Plate portion 227c is thus integral with the distal ends of the first inclined plate portions designed to connect the distal ends of the first inclined plate sections 227b. semi-annular portion R2 (a second semi-annular portion) contacting the separator 23 is in a lower section of each annular section 227. The semi-annular section R2 consists of a pair of second inclined plate sections 227d, a pair of second side plate sections 227e and a second flat Plate portion 227f. The second side plate portions 227e extend from the distal ends of the corresponding second inclined plate portions 227d downwards. The second flat plate portion 227f is designed such Way integrally formed with the distal ends of the side plate portions 227e, that it the distal ends of the Side plate sections 227e are connected to each other.

[0075] As shown in Fig. 22, a connecting plate portion 228 corresponds to the second flat plate portion 227f, each forming a semi-annular section R2. The first flat plate section 227c of each semi-annular Section R1 has one end at the connecting plate portion 228 (the second flat plate portion 227f) opposite side. This end is a first contact section 229, which contacts a surface of the gas diffusion layer 19 (or 20). The second flat contact portion 227f (the connecting plate portion 228) of each semi-annular portion R2 has one end on the side opposite the first flat plate portion 227c This end is a second contact portion 230, which contacts the inner surface of the first or second separator 23, 24 as shown in Fig. 24. A first flat surface portion 229a and a second flat Surface portion 230a are formed in the first contact portion 229 and the second contact portion 230, respectively. first and second flat surface portions 229a, 230a are formed by simultaneously pressing together two Surfaces of the metal grid structure 25 in the thickness direction of the metal grid structure 25. The first flat Surface portion 229a and the second flat surface portion 230a are formed parallel to each other.

[0076] The first flat surface portion 229a is in surface contact with the gas diffusion layer 19 (20) The second flat surface portion 230a is held in surface contact with the separator 23 (24). first flat surface portion 229a has a width W1 in the direction of the gas flow path (in the direction indicated by the arrow in Fig. 24). The width W1 is set to 0.2 mm, for example. The second flat Surface portion 230a has a width W2 in the direction of the gas flow path. The width W2 is, for example, set to 0.1 mm. The width W1 is set larger than the width W2.

[0077] Now, a method for manufacturing the first and second gas flow path forming members 221, 222 described.

[0078] A shaping mechanism 232 consists of a first shearing die 233 and a second shearing die 234. The first shearing die 233 is cut in a direction perpendicular to the feed direction of a thin metal plate 225A (in a direction perpendicular towards the surface of Fig. 25) by a displacement mechanism not shown. second shearing die 234 is moved upwards and downwards by a lifting mechanism (not shown) and by the Displacement mechanism moves in a direction perpendicular to the feed direction of the thin metal plate 225A.

[0079] As shown in Fig. 26, the first shearing die 233 has a side wall 233a on which, in the feed direction of the thin Metal plate 225A lower side. Projections 233b, which serve as first projections, and recesses 233c, which serve as first recesses are alternately formed in an upper portion of the side wall 233a. The projections 233b and the recesses 233c are spaced apart by a predetermined horizontal pitch. Projections 234a, which serve as second projections and which engage with the recesses 233c of the first shearing mold 233, and recesses 234b serving as second recesses and which are in contact with the projections 233b of the first shearing die 233 are formed in a lower portion of the second shearing die 234. The projections 234a and the Recesses 234b are alternately formed in the lower portion of the shearing die 234. The projections 234a and the Recesses 234b are spaced apart by a predetermined horizontal pitch. Each of the recesses 233c of the first shearing die 233 has a side surface on the upper side in the feed direction of the thin metal plate 225A side. A shear edge 233d, which forms a notch in the thin metal plate 225A, is located along the upper end the side surface of each recess 233c. A shear edge 234c, which has an inverted trapezoidal shape, is along the lower end and both side ends of each of the projections 234a of the second shearing die 234. The shear edges 234c are located at the positions corresponding to the shear edges 233d. The shear edges 234c cooperate with the shearing edge 233d to form incisions in the thin metal plate 225A.

[0080] As shown in Fig. 26, a pair of forming surfaces 233e, a pair of forming surfaces 233f and a forming surface 233g is formed in each of the projections 233b of the first shearing die 233. The Shaping surfaces 233e form the inner surfaces of the two first side plate sections 227a of each annular portion 227 (the outer surfaces of the second side plate portions 227e). The shaping Surfaces 233f form the inner surfaces of the first two inclined plate sections 227b. The shaping Surface 233g forms the inner surface of the flat plate portion 227c. Likewise, a pair of shaping Surfaces 234d, a pair of shaping surfaces 234e and a shaping surface 234f in each of the Recesses 234b of the second shearing die 234 are formed. The shaping surfaces 234d form the outer Surfaces of the first side plate portions 227a of each annular portion 227 (the inner surfaces of the second inclined plate sections 227e). The shaping surfaces 234e form the outer surfaces of the first inclined plate portions 227b of the annular portion 227 (the inner surfaces of the second inclined Plate sections 227d). The shaping surface 234f forms the outer surface of the flat plate section 227c. A shaping surface 234g, which forms the inner surface of the flat plate portion 227f of the annular portion 227 is formed along the lower end of each projection 234a of the second shearing die 234 trained.

[0081] As shown in Fig. 25, feed rollers 231 move the thin metal plate 225A over a predetermined Step length from the first shearing shape 233 to the second shearing shape 234. In this stage, the shearing edges 233d the first shearing die 233 and the shearing edges 234c of the second shearing die 234, which is lowered, a portion of the thin metal plate 225A. In this way, a plurality of cuts are formed in the thin metal plate 225A. Then the second shearing die 234 is lowered to the lowest position and presses on the thin metal plate 225A, whereby the thin metal plate 225A is bent and stretched by means of the projections 234a of the second shearing die 234. As shown in Fig. 27, the bent-stretched portion of the thin metal plate 225A is formed substantially like a trapezoidal shape. The second shearing mold 234 is then raised from its lowest position and returns to its Return to starting position.

[0082] Then, the feed rollers 231 again move the thin metal plate 225A over a predetermined step length towards the forming mechanism 232. Synchronously, the first shearing die 233 and the second shearing die 234 over a distance corresponding to half the alignment step of the annular sections 227, to the left or to the right. The second shearing die 234 is then lowered again to positions that are half step lengths from previously machined bent-stretched section are offset to the left or to the right, cuts in the thin metal plate 225A, and bends and stretches the thin metal plate 225A. In this way, the annular Sections 227 with the through openings 226 are formed, and a metal grid structure 225 is completed.

[0083] By repeating the above-described process, the plurality of through openings 226 are formed in the manner a grid in the metal grid structure 225, and the annular sections 227 are formed in a staggered manner arranged as shown in Fig. 28 and Fig. 29. At this stage, the projections 233b and the recesses 233c of the first shearing die 233 into the corresponding projections 234a and the corresponding the recesses 233b of the second shearing die 234. In this way, there are non-machined sections that are not processed by the lowered second shearing die 234, in the metal grid structure 225. The non-processed Sections form the connecting plate sections 228 (the second flat plate sections 227f). Connecting plate sections 228 connect the annular sections 227 to each other so that they As a result, the metal grid structure 225 is formed, which has a stepped cross-section, as shown in Fig. 30,

[0084] As shown in Fig. 31, each annular portion 227 is formed in a polygonal shape. annular portion 227 form the first side plate portions 227a and the first inclined plate portions 227b, which are components of the semi-annular section R1, a first forming section F1 which has a plastic deformation of the first flat plate section 227c when the first flat plate section 227c is When external forces act downwards on the flat plate portion 227c, the first Forming-allowing section F1 is formed as shown by the corresponding two-dot / dash lines in Fig. 31 Furthermore, the second side plate sections 227e, which are components of the individual semi-annular Section R2, a second forming section F2, which allows plastic deformation of the second flat plate portion 227f when the second flat plate portion 227f is pressed upwards. If upward external forces act on the second flat plate portion 227f, the second one Forming-allowing section F2 formed as shown by the corresponding two-dot / dash lines in Fig. 31 shown.

[0085] The extent to which the first forming-permitting section F1 is formed is set so that it exceeds the extent to which the second forming-permitting section F2 is formed, if the same external Force on the first deformation-permitting section F1 and the second deformation-permitting section F2 When the downward external force acts on the first flat plate portion 227c of the first deformation permissible section F1, the force is transmitted via the first inclined plate sections 227b to the first side plate sections 227a. As a result, each of the first side plate sections 227a is extended by the proximal End of the first side plate portion 227a is formed to the left or right, and each first inclined plate portion 227b is formed around the connecting portion between the first inclined plate portion 227b and the corresponding first side plate portion 227a is turned downwards. In other words, the first is a forming The permissible section F1 is designed to be easily deformed in response to an external force. If the upward external force on the second flat plate portion 227f of the second forming-permitting section F2, each of the second inclined plate sections 227d is kept in the current state without being moved by the proximal end of the second inclined plate portion 227d. Each of the second Side plate sections 227e are only slightly turned to the left or to the right around the proximal end of the second plate section 227e. That is, the second forming section F2 is designed that the second forming section F2 is less easily formable than the first forming section permitting section F1.

[0086] A method will now be described with which the first and second flat surface portions 229a, 230a in the corresponding first and second contact sections 229, 230 of the metal grid structure 225. Since the Structure of the pressing machine with which the first and second flat surface portions 229a, 230a are formed, the The structure of the press machine 40 according to the second embodiment shown in Fig. 10 is the same, Description of the pressing machine with which the first and second flat surface portions 229a, 230a are formed are omitted here.

[0087] First, the metal grid structure 225 is moved from the table 42 to the position between the compression rollers 46, 47 which rotate as shown by the arrows in Fig. 32. The compression rollers 46, 47 then press the Metal grid structure 225 from above and below and move the metal grid structure 225 to the right, as shown in Fig. 32. In this way, the first and second contact sections 239, 230 of the metal grid structure 225 from above and below to a predetermined extent. By reshaping the first and second Contact sections 229, 230, the first flat surface section 229a is formed in the first contact section 229 and the second flat surface portion 230a is formed in the second contact portion 230. As shown in Fig. 31 As shown, the first deformation-allowing section F1 of each semi-annular section R1 can be more easily compress than the second deformation-permitting section F2 of each semi-annular section R2. As a result, the width W1 of the first flat surface portion 229a of each of the first contact portions 229, as in Fig. 24, in the direction of the gas flow path greater than the width W2 of the second flat surface section 230a of each of the second contact sections 230.

[0088] When the metal grid structure 225 is completed, the metal grid structure 225 is cut to a predetermined size cut so that the first and second gas flow path forming elements 221, 222 are completed. As shown in As shown in Fig. 33, the completed first gas flow path forming element 221 is inserted into each power generating cell 12 recorded, wherein the first flat surface portions 229a are in contact with the top side of the gas diffusion layer 19 in Surface contact and the second flat surface portions 230 with the back of the first Separator 223 are kept in surface contact.

[0089] The second embodiment has the advantages described below. (1) As shown in Fig. 31, the easily formable first forming section F1 in the semi-annular portion R1 of each annular portion 227, and the less easily deformable second forming section F2 is in the semi-annular section R2 of the annular section 227. The first and second flat surface portions 229a, 230 are formed in the corresponding first and second contact sections 229, 230 of the metal grid structure 225. The first and second flat surface sections 229a, 230a are formed by pressing together the two surfaces of the Metal grid structure 225 is formed using the compression rollers 246, 247. The width W1 of each first flat surface portion 229a is set larger than the width W2 of every second flat surface portion 230a. Thus, despite the use of the compression rollers 246, 247, the width W2 of the second flat surface portion 230a regardless of the width W1 of the first flat surface portion 229a is set to a suitable value. As a result, the width W2 of the second flat surface portion 230a is set to a value with which the inner surface of the separator 23 cannot be damaged. Likewise, a suitable current-transmitting surface is required between the outer surface of the separator 23 and every second flat surface portion 230a. Thus As shown in Fig. 24, the thickness T of the gas flow path forming member 221, which is the The effective area of ​​the gas flow path forming element 221 is maintained in a suitable manner. the pressure loss of the gas delivered to the gas flow path is reduced and an appropriate Power generation performance is maintained. If the width W2 of the second flat surface portion 230a of the second contact portion 230 is set to be the same size as the width W1 of the first flat surface portion 229a, the thickness T of the gas flow path forming member 221 reduced and thus the usable cross-section of the gas flow path would be reduced, as corresponding dot / dash lines in Fig. 24.

[0090] The second embodiment may be modified into the forms described below.

[0091] As shown in Fig. 34, the first inclined plate portions 227b and the second inclined Plate sections 227d of each annular section 227 are formed into an arc shape. More specifically, the annular Section 227 has a rounded shape overall.

[0092] The first shearing mold 233 shown in Fig. 26 can be divided into a body with the shearing edges 233d and a shearing plate with the projections 233b and the recesses 233c. In this case, the shear plate of the first shearing shape 233 at the position corresponding to the second shearing shape 234. Furthermore, in this case, the body of the second shearing die 233 is fixed at a predetermined position and the shearing plate is shaped so that it can be moved back and forth in a horizontal direction.

[0093] In the second embodiment, the first shearing mold 233 and the second shearing mold 234 are placed in the positions which is moved by a distance corresponding to half the pitch of the projections 234a and the recesses 234b of the second shearing shape 234, is offset to the left or right to form the semi-annular sections R1, R2. However, the degree of this offset can be changed as required. Furthermore, the arrangement of the ring-shaped Section 227 is not limited to the staggered arrangement. (Third embodiment)

[0094] Now, a third embodiment of the present invention will be described with reference to Figs. 35 to 48. detailed description of components of the third embodiment, the components of the first or second Embodiments are similar or identical, is omitted here.

[0095] As shown in Fig. 35 and Fig. 36, the upper semi-annular portion R1 of each annular gen portion 327 of a pair of first inclined plate portions 327a and a first flat plate portion 327b The first two inclined plate sections 327a face each other. The first flat plate section 327b is connected to the inclined plate sections 327a in such a way that it covers the upper ends of the inclined Plate sections 327a interconnected. The lower semi-annular section R2 of each annular section 327 consists of a pair of second inclined plate sections 327c and a second flat plate section 327d. The The two second inclined plate sections 327c face each other. The second flat plate section 327b is connected to the inclined plate sections 327c in such a way that it covers the upper ends of the inclined Plate sections 327c are connected to each other.

[0096] As shown in Fig. 35, a connecting plate portion 328 is connected to the second flat plate portion 327d each annular portion 327 is identical. A first contact portion 329, which is applied to the second flat plate portion 327d of the annular portion 327 is in the first flat plate portion 327b of the annular portion 327. When incorporated into the power generating cell 12, the first contact sections touch 329 a surface of the gas diffusion layer 19. More specifically, a curved flat surface portion 329a in each of the first contact portions 329. As shown in Fig. 37, the flat surface portions 329a held in surface contact with the gas diffusion layer 19 (20). A second contact section 330, which is on the first flat plate portion 327b of each annular portion 327 is directed in the second flat plate portion 327d of the annular portion 327. Accommodated in the power generating cell 12, the second Contact portions 330 linearly contact the inner surface of the first or second separator 23, 24, as shown in Fig. 38.

[0097] A non-bent flat surface portion 327f which is substantially flush with the connecting plate sections 328, is in each flat plate section 327b at a location between the corresponding bent flat surface portion 329a and the connecting plate portion 328 (the lower flat plate portion 327d). The first flat plate portion 327b is formed by the non-bent flat surface portion 327f and the bent flat surface portion 329a. As shown in Fig. 37 shown, the bending angle α of the bent flat surface portion 329a with respect to the Connecting plate portion 328 (the non-bent flat surface portion 327f) in the range of 60° to 70° In the third embodiment, the bending angle α is set to 65°.

[0098] A device for forming a metal lattice structure of the first and second gas flow path forming Elements 321, 322 will now be described.

[0099] As shown in Fig. 40, a forming mechanism 332 comprises a first shearing die 333 and a second Shearing die 334. The first shearing die 333 is fixed to a support table (not shown). A non-shown Lifting mechanism moves the second shearing die 334 up and down. A non-illustrated displacement mechanism moves the second shearing die 334 in the width direction of a thin metal plate 325A back and forth, which is the direction of The rotational axis of each feed roller 331 (a direction perpendicular to the surface of Fig. 39) is a surface 333a the first shearing die 333 serves as a surface that supports the thin metal plate 325A. A linear first shearing edge 333b is formed along one end of the upper side 333a of the first shearing die 333 on a plane extending in the feed direction H of the thin Metal plate 325A lower side. A flat position holding surface 333c is below the first shear edge 333b trained.

[0100] A plurality of projections 334a spaced apart from each other by a predetermined horizontal pitch D are formed in a lower portion of each of the second shearing dies 334. A horizontal forming Surface 334c is formed at the lower end of each of the projections 334a of the second shearing die 334. Slope Shaping surfaces 334d are provided on opposite left and right surfaces of each projection 334a. A horizontal shaping surface 334e is formed between the corresponding inclined shaping Surfaces 334d of each pair of adjacent projections 334a are formed. The inclined shaping Surfaces 334d and the horizontal forming surfaces 334e define a plurality of recesses 334b. The recesses 334b ​​are formed alternately with the projections 334a. A second shear edge 334f, which has a inverted trapezoidal shape, is formed along one end of each shaping surface 334c and along the ends of the associated inclined forming surfaces 334d on an upper in the feed direction of the thin metal plate 325A side. The second shearing edges 334f cooperate with the first shearing edge 333b to form incisions in the thin metal plate 325A.

[0101] Now, a method for forming the gas flow path forming members 321, 322 using the forming device constructed as described above with reference to Figs. 41 to 48 described.

[0102] According to a method of the third embodiment, a plurality of first sections to be machined P1 and a plurality of second sections P2 to be machined, which are alternately arranged along the feed direction H of the thin metal plate 325A are arranged, defined in the thin metal plate 325A. The first to be processed Sections P1 and the second sections P2 to be machined are successively cut into the thin metal plate 325A In a first step, the feed rollers 331 (see Fig. 39 ) move the first Sections P1 of the thin metal plate 235A into a with respect to the first shearing shape 333 and the second shearing shape 334 middle machining position, as shown in Fig. 41(a). In other words, one end of the thin metal plate 325A in the feed direction H by a first feed distance L1 (for example 0.2 mm) from the first shearing edge 333b moved forward. In this state, the second shearing mold 334 is lowered towards the first shearing mold 333, and the first shearing edge 333b and the second shearing edges 334f shear a portion of the first section P1, thereby forming a plurality of cuts in the thin metal plate 325A. Subsequently As shown in Fig. 42(a) and Fig. 42(b), the second shearing die 334 is lowered to a lowest position. the portions of the thin metal plate 325 which contact the projections 334a of the second shearing die 334 are bent and stretched at the bottom. In this way, as shown in Fig. 42(b), the bent and stretched Sections of the thin metal plate 325A are shaped substantially like inverted trapezoids. Since each of the sections between the bent and stretched sections engages in the corresponding recess 334b, the section between the bent and stretched sections essentially shaped like inverted trapezoids.

[0103] In the first step, as shown in Fig. 42(b), the second flat plate portions 327d (the Connecting plate sections 328) which connect the lower semi-annular sections R2 of the annular sections 327 form, pressed downwards and by the horizontal forming surfaces 334c of the projections 334a horizontally The upper semi-annular portions R1 of the annular portions 327, which correspond to the recesses 334b are formed by forming sections with horizontal forming surfaces, such as the projections 334a, are not pressed upwards. Thus, as shown in Fig. 42(a), the first flat Plate sections 327b of the semi-annular sections R1 formed by the recesses 334b, obliquely and hung downwards around the first shearing edge 333b. This way, the bent flat Surface portions 329a are formed in such a way that the bent flat surface portions 329a each have a bending angle α with respect to the horizontal section of the thin metal plate. Each bent flat surface portion 329a serves as the first contact portion 329. Thereafter, the second shearing mold 334 returns, as shown in Fig. 43(a) and Fig. 43(b), from the lowest position to its upper starting position.

[0104] Subsequently, in a second step, as shown in Fig. 43(a), the feed rollers 331 (see Fig. 39 ) the thin metal plate 325A over a predetermined second feed distance L2 (for example 0.1 mm) in Feed direction H. In this way, the first sections P1 of the thin metal plate 325A to be machined are the final processing position with respect to the first shearing die 333 and the second shearing die 334. In At this stage, as shown in Fig. 44(a) and Fig. 44(b), the second shearing die 334 is moved from the position in the first Step again without being displaced in the width direction of the thin metal plate 325A. This will upper semi-annular sections R1 and the lower semi-annular sections R2 of the annular sections 327 in corresponding end of the thin metal plate 325A. At this stage, the first flat Plate portions 327b of the upper semi-annular portions R1 are free, like the first contact portions 329. The second Feed distance L2 is set shorter than the above-mentioned first feed distance L1. Each first flat Plate section 327b is arranged in the vicinity of the shear edge 33b. Thus, the first flat Plate sections 327b in a simple manner along the horizontal shaping surfaces 334e of the recesses 334b of the second shearing die 334. As a result, as shown in Fig. 44(a), the first flat Plate portions 327b, which are arranged behind the bent flat surface portions 329a, in Maintained essentially horizontally without drooping significantly downwards. The first flat plate sections 327b form thus the non-bent flat surface sections 327f. The second step produces the semi-circular Sections R1, R2, which include the non-bent flat surface sections 327f, are completed.

[0105] According to the present invention, the semi-annular sections R1, R2, which are usually in a formed in a single pass, formed in two separate passes, as described above. More precisely, the non-reverse bent flat surface portions 327f are formed after the first pass in which the bent flat surface portions 329a are formed. Thus, the width of each of the bent flat Surface sections 329a in contrast to a conventional method in which the semi-annular sections R1, R2 are formed in a single pass, reduced to an appropriate width.

[0106] Then, in a third step, as shown in Fig. 45(a), after the second shearing mold 334 is inserted into the starting position, the second machining target positions P2, which are connected to the first machining Target positions P1 are adjacent to the middle position with respect to the first shearing shape 333 and the second shearing shape 334 Forming position. In other words, the thin metal plate 325A is again passed over the first Feed path L1 is moved in the feed direction H. Then, as shown in Fig. 45(b), the second shearing die 334 is moved in Width direction of the thin metal plate 325A by half the arrangement pitch D (half a pitch) of the annular sections 327. Then the second shearing mold 334 is lowered and forms the second sections P2 to be processed, as shown in Fig. 46(a) and Fig. 46(b). In this way, the semi-annular sections R1 are formed over the semi-annular sections R2, and the semi-annular Sections R2 are formed under the semi-annular sections R1. As a result, the annular Sections 327 completed.

[0107] Then, in a fourth step, as shown in Fig. 47(a) and Fig. 47(b), the thin metal plate 325A is offset shear shape 334 is sent along the second feed path L2. The second sections to be machined P2 become the final processing position with respect to the first shearing form 333 and the second shearing form 334 As shown in Fig. 48(a) and Fig. 48(b), the second shearing die 334 is lowered, and the semi-annular Sections R1, R2, which include the non-bent flat surface sections 327f, are completed.

[0108] After that, the first and second steps and the third and fourth steps are repeated alternately. In this way, the sections P1, P2 to be machined are machined alternately, and the pattern shown in Fig. 35 to 37 Metal grid structure 325 is completed. More specifically, the metal grid structure 325 is formed with the plurality of continuous Openings arranged in the manner of a grid, formed in such a way that the annular sections 327 are arranged in a meandering manner.

[0109] In the metal grid structure 325, there are non-machined portions that are not affected by the second shearing die 334 The non-machined sections form the connecting plate sections 328 (the second flat Plate sections 327d) so that the annular sections 327 are in a mutually overlapping state with each other As a result, as shown in Fig. 35 and Fig. 37, the metal grid structure 325 is connected to the stepped cross-section formed.

[0110] The third embodiment has the advantages described below. (1) Conventionally, the semi-annular portions R1, R2 of the annular portions 327 are formed in a single step using the first shearing die 333 having only the first shearing edge 333b, and the second shearing mold 334, which has the projections 334a and the recesses 334b, According to the present invention, the formation of the semi-annular sections R1, R2 in two steps. Thus, compared to the conventional process shown in Fig. 37, Process in which this training is completed in a single step, the width W1 of each bent flat surface portion 329a is reduced, and the thickness T1 of the gas flow path forming element 321 is set to a larger value. This increases the usable cross section of the Gas flow path in the gas flow path forming element 321, whereby a adequate gas supply is enabled. As a result, the efficiency of power generation improved. (2) The conventional device shown in Fig. 39 and Fig. 40 is called metal grid structure This simplifies the design of the forming device and the bent flat surface sections 329a can be easily inserted into the first contact portions 329 of the annular portions 327.

[0111] The third embodiment may be modified in the following forms.

[0112] Shaping surfaces that are applied to the horizontal shaping surfaces 334c of the projections 334a of the second shearing die 334 can be formed in a side surface of the first shearing die 333 on the side in the feed direction H the thin metal plate 325A lower side. In this case, when the second shearing mold 334 is lowered, the forming surfaces of the first shearing die and the horizontal forming surfaces of the second shearing form 334a the thin metal plate 325A. This prevents the second flat plate portions 327d of the annular Sections 327 are bent.

[0113] The second step shown in Fig. 43 and Fig. 44 and the fourth step shown in Fig. 47 and Fig. 48 can each be divided into several separate half-steps.

[0114] In the third embodiment, the second shearing die 334 is formed in the width direction of the thin metal plate 325A by half the pitch D (half a pitch) of the projections 334a and the recesses 334b ​​of the second Shear form 334. However, the offset distance can be changed as required. Furthermore, the annular Sections 327 do not necessarily have to be arranged in a meandering manner.

[0115] The shape of the individual annular sections 327 may, for example, be pentagonal.

Claims

1. A gas flow path forming element (321, 322) used in a power generating cell (12) of a fuel battery (11), wherein the power generating cell (12) comprises a gas diffusion layer (19, 20) arranged in a Electrode layer (17, 18) of an electrode structure, and has a separator (23, 24) for insulating adjacent power generating cells (12) against each other, and wherein the gas flow path forming element (321, 322) is arranged between the gas diffusion layer (19, 20) and the separator (23, 24) and has a gas flow path has, wherein the power generating cell (12) is constructed such that it has an electrode reaction which is in the Electrode layer (17, 18) is produced by supplying fuel gas or oxidizing gas through the gas flow path to electrode layer (17, 18) is supplied, generates power, wherein the gas flow path forming element (321, 322) is characterized in that the gas flow path forming element (321, 322) consists of a metal grid structure (25; 325) which consists of a thin metal plate (25A; 325A) is formed, wherein a plurality of through openings (26; 326) in the metal grid structure (25; 325) in the manner of a grid are formed, wherein the gas flow path forming member (321, 322) has a plurality of annular portions (27; 327), which form the through openings (26; 326), wherein the annular sections (27; 327) each have a flat Surface portion in a contact portion (329) between the annular portion (27; 327) and the gas diffusion layer (19, 20), and wherein an upper annular portion (R1) of the annular portion (327) is formed by a pair of inclined plate portions (327a) and a flat plate portion (327b) which connects upper ends of the inclined plate portions (327a) connecting, wherein the flat plate portion (327b) is formed by a non-bent flat surface portion (327f) and a bent flat surface portion (329a) and a portion of the flat surface portion in the contact portion (329) between the annular portion (327) and the Gas diffusion layer (19, 20) corresponds to the bent flat surface section (329a).

2. Gas flow path forming element (321, 322) according to claim 1, characterized by a flat Surface portion (28a, 29a) in a contact portion (28, 29) between the gas flow path forming member (321, 322) and the separator (23, 24).

3. A gas flow path forming element (321, 322) used in a power generating cell (12) according to claim 1 or 2 is used, characterized in that the through openings (26) of the annular sections (27) each are formed so that they have a hexagonal cross-section, and that each contact section (28, 29) is located at a position corresponding to a specific side of the hexagonal shape.

4. A method for manufacturing a gas flow path forming member (321, 322) used in a power generating Cell (12) of a fuel battery (11), wherein the power generating cell (12) has a gas diffusion layer (19, 20) formed in an electrode layer (17, 18) of an electrode structure, and a separator (23, 24) for isolating adjacent power-generating cells (12) from each other, and wherein the gas flow path forming element (321, 322) is arranged between the gas diffusion layer (19, 20) and the separator (23, 24) and has a gas flow path, wherein the power generating cell (12) is constructed such that it has an electrode reaction which is in the Electrode layer (17, 18) is produced by supplying fuel gas or oxidizing gas through the gas flow path to electrode layer (17, 18) is supplied, generates power, wherein the method for manufacturing the gas flow path forming member (321, 322) is characterized by: a first step in which by forming a plurality of through openings (26; 326) in a thin metal plate (25A; 325A) in the manner of a grid, a metal grid structure (25; 325) is formed; and a second step in which in a contact section (28, 29) between each annular section (27; 327) which through openings (26; 326) of the metal grid structure (25; 325), and the gas diffusion layer (19, 20) according to the first step, a flat surface portion is formed, wherein an upper annular portion (R1) of the annular portion (327) of a pair of inclined plate portions (327a) and a flat plate portion (327b) which connects upper ends of the inclined plate sections (327a) to each other, wherein the flat Plate portion (327b) of a non-bent flat surface portion (327f) and a bent flat surface portion (329a) is formed and a portion of the flat surface portion in the Contact section (329) between the annular section (327) and the gas diffusion layer (19, 20) bent flat surface portion (329a).

5. A method for producing a gas flow path forming member (321, 322) according to claim 4, characterized characterized in that the flat surface portion (28a, 29a) is formed in the second step by metal grid structure (25) obtained in the first step is arranged between a pair of rollers and pressed together to to plastically deform the contact section (28, 29).

6. A method for producing a gas flow path forming member (321, 322) according to claim 4, characterized characterized in that the formation of the flat surface portion (28a, 29a) in the second step is carried out by that the contact section (28, 29) is formed using a fixed punching die (33) and a movable Punching die (34) in the first step of producing the metal grid structure (25) in the thickness direction of the metal grid structure (25) is plastically deformed.

7. A molding device used for the method of manufacturing a gas flow path forming member (321, 322) according to claim 4, wherein the shaping device comprises: a fixed punching die (33) having first recesses (33c) and first projections (33b) which are alternately provided with a are arranged at a specified pitch; and a movable punching die (34) having second projections (34a) and second recesses (34b) which are provided with a predetermined pitch, wherein the second projections (34a) are aligned with the first recesses (33c) the fixed punching die (33) and the second recesses (34b) engage with the first projections of the fixed punching die (33) engage; the forming device being characterized in that: the movable punching die (34) is capable of moving in the thickness direction and in the width direction of the thin metal plate (25A) to move back and forth, by forming a plurality of cuts in the thin metal plate (25A) with predetermined pitches and bending and stretching the thin metal plate (25A) by engaging the first recesses (33c) and the first projections (33b) of the fixed punching die (33) and the second projections (34a) and second recesses (34b) of the movable punching die (34) a plurality of annular (27) sections, which form the through openings (26) are formed in the thin metal plate (25A); and an inclined surface (33e) in an upper surface of each of the first projections (33b) of the fixed die (33), wherein the inclined surface (33e) is directed downwards in the feed direction of the thin metal plate (25A) is inclined.

8. A molding device used for the method of manufacturing a gas flow path forming member (321, 322) according to claim 4, wherein the shaping device comprises: a fixed punching die (33) having first recesses (33c) and first projections (33b) which are alternately provided with a are arranged at a specified pitch; and a movable punching die (34) having second projections (34a) and second recesses (34b) which are provided with a predetermined pitch, wherein the second projections (34a) are aligned with the first recesses (33c) the fixed punching die (33) and the second recesses (34b) with the first projections (33b) engage the fixed punching die (33); the forming device being characterized in that: the movable punching die (34) is capable of moving in the thickness direction and in the width direction of the thin metal plate (25A) to move back and forth, by forming a plurality of cuts in the thin metal plate (25A) with predetermined pitches and bending and stretching the thin metal plate (25A) by engaging the first recesses (33c) and the first projections of the fixed die (33) and the second projections (34a) and second recesses (34b) of the movable punching die (34) a plurality of annular sections (27) which the through openings (26) are formed in the thin metal plate (25A); and an inclined surface (34e) in a lower surface of each of the second projections (34a) of the movable die (34), wherein the inclined surface (34e) is directed against the feed direction of the thin metal plate (25A) is tilted at the top.

9. Shaping device according to claim 7 or 8, characterized in that the fixed punching die (33) or the movable die (34) two side sections of each annular section (27) which are adjacent to each other opposite sides of a contact portion (28, 29) of the annular portion (27) and a gas diffusion layer (19, 20) of the fuel battery (11), towards the centre of the corresponding through opening (26).

Citation Information

Patent Citations

  • Method and apparatus for manufacturing grids for lead-acid batteries

    DE2444859C2

  • Separator for fuel cell

    JP2007087768A

  • Manufacturing method of cell for fuel cell

    JP2008243394A

  • Fuel cell assembly unit for promoting fluid service and electrical conductivity

    US6007933A

  • Separator for fuel cell

    WO2007034617A1