METHOD FOR TREATING USED LITHIUM BATTERIES AND BATTERY PROCESSING PLANT

DE502016016724D1Active Publication Date: 2024-10-02DUESENFELD GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502016016724
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2015-04-28
Filing Date
2016-04-28
Publication Date
2024-10-02
Estimated Expiration
2036-04-28

AI Technical Summary

Technical Problem

Existing methods for processing used lithium batteries often result in contaminated materials due to plastic degradation, high hazard potential, complex structures for partial load operation, and the risk of flammable or explosive gas formation, which complicates safe transportation and recycling.

Method used

A method involving the drying of lithium battery components under vacuum to remove electrolytes, preventing electrochemical reactions and reducing the risk of flammable gas formation, thereby creating a safer and more inert material for transportation and recycling, without the need for additional inactivation materials.

Benefits of technology

The method effectively reduces the hazard potential of lithium battery components, ensuring safe transportation and increasing the purity of materials for subsequent recycling steps by eliminating organic carbonates and preventing the formation of toxic fluorophosphates, thus enhancing the safety and efficiency of the recycling process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a method for treating used lithium batteries according to the preamble of claim 1.

[0002] According to a second aspect, the invention relates to a battery processing plant with the features of claim 6.

[0003] US Patent 2005 / 0241943 A1 discloses a method for reprocessing used batteries in which the batteries are heated before a comminution step, thus destroying the plastic components of the batteries. A disadvantage of this method is that the remaining battery components may be contaminated with plastic degradation products.

[0004] German patent DE 10 2012 024 876 A1 discloses a system for transporting critical electrolyte cells, which are first crushed under inert gas and then dusted with a deactivation powder to prevent spontaneous ignition of the electrochemically active material. A disadvantage of this system is that the resulting material still possesses a comparatively high hazard potential, the dusting powder itself poses an explosion risk, and the formation of a flammable and explosive atmosphere in the transport container cannot be ruled out.

[0005] German patent application DE 10 2011 110 083 A1 discloses a method for recovering active material from a galvanic cell, in which the galvanic cells are first mechanically crushed, then pre-dried, and subsequently screened. Finally, the binder is decomposed in an oven. Such a device is very well suited for the efficient recycling of large quantities of galvanic cells. However, for partial-load operation, this system is comparatively complex in design.

[0006] From WO 2010 / 102377 A1 and US 8 210 456 B2, a method for recycling batteries is known, wherein the batteries are first crushed and then pass through a continuous oven for drying.

[0007] DE 44 24 825 A1 teaches a process of freezing the batteries, then crushing the frozen batteries, and subsequently floating the fragments. Normal pressure conditions should be used for this process.

[0008] Extracting the electrolyte using supercritical CO2 is known from US patent 2003 / 186110 A1. No vacuum is applied for this process.

[0009] US 5 632 863 A describes pyrolysis of the batteries, not drying.

[0010] The invention is based on the objective of reducing disadvantages in the prior art.

[0011] The invention solves the problem by the method specified in claim 1. According to a second aspect, the invention solves the problem by a battery processing plant according to claim 7.

[0012] An advantage of the invention is that drying removes so much electrolyte from the material being ground that an electrochemical reaction is no longer possible or only possible to a negligible extent. Furthermore, no flammable or explosive gas phase forms above the battery fragments, since the organic carbonates of the electrolyte, in particular, have been removed. The ground material is therefore largely inert and can be transported safely, especially when vacuum-packed.

[0013] Another advantage is that no additional material needs to be added to inactivate the shredded material. This reduces the effort required for battery processing, decreases the weight of the inactivated shredded material, and increases purity in subsequent separation and recycling steps. High product purity without the introduction of foreign ions is particularly advantageous in potential subsequent hydrometallurgical processing steps.

[0014] Another advantage is that a transport-safe, pulverized material is obtained. The organic carbonate content is preferably so low that the formation of fluorophosphates in any relevant quantity can be ruled out. Fluorophosphates are often potent neurotoxins, the formation of which must be reliably prevented. Furthermore, the low electrolyte content ensures that no self-reinforcing heat generation can occur due to an electrochemical reaction.

[0015] In the context of this description, drying is understood to mean, in particular, the removal of at least one solvent from the conducting salt. Specifically, drying is carried out in such a way as to remove dimethyl carbonate and / or ethyl methyl carbonate.

[0016] The term "battery" refers to a lithium battery. A lithium battery is a rechargeable battery in which the electrochemical reaction involves lithium and / or lithium ions and / or a lithium compound.

[0017] A battery processing plant is understood to be a plant for treating used lithium batteries.

[0018] The term "transport container" also includes, in particular, transport packaging. Preferably, the transport packaging is sealed by vacuum welding. Aluminum composite film is especially well-suited as transport packaging.

[0019] It is advantageous if drying takes place after the batteries have been crushed. While it is possible, and represents one embodiment of the invention, to subject the uncrushed batteries to a vacuum so that at least some of the electrolyte evaporates, with the resulting gas either escaping through a safety valve in the battery or the battery being destroyed by the pressure difference between the external environment and the internal pressure, allowing evaporating electrolyte to escape, this process can be time-consuming. This is because the electrolyte is usually located between tightly wound or stacked and compressed layers of electrodes and separator, and within their pores, and is also connected to other battery components.It is therefore often more advantageous, and represents a preferred embodiment of the invention, to mechanically shred the batteries, for example by cutting, shearing, impact, separation and / or crushing. This provides a larger interface for mass transfer into the gas phase.

[0020] Drying can be achieved, for example, by vacuum drying, contact drying, convection drying, and / or radiation drying. It is advantageous if the drying process is carried out while stirring and / or agitating the material being ground.

[0021] Before shredding, the used batteries are preferably disassembled. This means that larger battery systems are broken down into their smaller sub-components, the modules or stacks, or even that the cells containing the electrochemically active material are separated from the control electronics. The control electronics include, for example, semiconductor components and / or sensors and are used to control the charging of the batteries.

[0022] According to the invention, drying is carried out under vacuum. Preferably, the vacuum is chosen to be so high that the vapor pressure of dimethyl carbonate at 80°C, and particularly at 70°C, is undershot. It is advantageous if drying takes place under a pressure of no more than 300 hPa, and particularly no more than 100 hPa. At such low pressures, essential components of most electrolytes, especially dimethyl carbonate and ethyl methyl carbonate, evaporate at temperatures below 80°C. Low temperatures have the advantage of inhibiting the formation of hydrogen fluoride. Hydrogen fluoride poses a potential hazard to the battery processing plant and the environment. It is therefore advantageous to prevent the formation of hydrogen fluoride.

[0023] Preferably, drying takes place at a temperature below the decomposition temperature. The decomposition temperature is understood to be, in particular, the lowest temperature at which, after holding the material being ground at this temperature for one hour, at least 80% by mass of the binder has decomposed into gaseous components. The decomposition temperature can thus be measured by successively increasing the temperature of the material being ground and recording when a loss of mass occurs, particularly due to gas evolution resulting from the decomposition of the binder, and the specified criterion is met. If necessary, the test must be repeated several times with a new sample of the material being ground, each time at an increased temperature.

[0024] It is advantageous if drying takes place under an atmosphere in which the water partial pressure is less than 50 Pa, and especially less than 10 Pa. A low water partial pressure leads to a low reaction rate of lithium compounds to lithium hydroxide and thus to only minimal hydrogen evolution. This prevents the formation of ignitable hydrogen-oxygen mixtures and contributes to plant safety.

[0025] It is also advantageous if the partial pressure of oxygen is no more than 10 millibars, and particularly no more than 5 millibars. This largely suppresses the reaction of oxygen with oxidizable components of the batteries. The low partial pressure of oxygen can be achieved by using low pressure during drying. Alternatively or additionally, drying can be carried out in an inert gas atmosphere.

[0026] A preferred method is one in which the drying of the material to be ground is only stopped when, after drying has ceased, no flammable or explosive gas mixture can form above the packaged material and / or when the material is so dry that a flammable or explosive gas mixture could form in the transport container or during further processing. The feature that drying is stopped when, after drying has ceased, no flammable or explosive gas mixture can form above the packaged material means, in particular, that no ignitable gas mixture forms in a 50-liter transport container, half-filled (based on its volume) with the material to be ground, within one week at 50°C and 1013 hPa. Whether this criterion is met is determined in preliminary tests.If an ignitable gas mixture forms, the drying process must be carried out for a longer time and / or at a lower pressure. The preliminary tests are repeated until a drying time and / or drying pressure is determined at which the characteristic is fulfilled for all three transport containers in a test set of three.

[0027] Preferably, the material being ground is dried until the electrolyte content is so low that an electrochemical reaction is impossible. In other words, the electrolyte content is below a threshold value, which is chosen such that the cell voltage drops to at most one-quarter of its normal value when this threshold is undershot. This threshold value is determined, for example, by measuring the cell voltage of a battery as a function of the electrolyte content. Shortly before reaching the threshold value, the cell voltage collapses, meaning it drops by at least 75%. Once the threshold value is undershot, the battery contains so little electrolyte that, to a good approximation, no electrochemical reaction is possible.

[0028] Preferably, the material to be ground is dried for such a long time that a quantity of 50 kg of ground material, compacted in a 50 liter drum, shows no or only such a low heat generation that thermal runaway, i.e. a thermally induced chain reaction, is excluded for at least two months, and that any hydrogen evolution is also so low that no overpressure occurs after two weeks if there is an initial underpressure of 500 hPa.

[0029] It is advantageous if the material to be crushed is dried until the electrolyte content of organic components that are volatile at 80°C is at most 3 wt.%, in particular at most 2 wt.%, and especially preferably at most 1.5 wt.%.

[0030] Preferably, the drying process is carried out for such a long time that the accumulated content of organic carbonates from the electrolyte, which are volatile at 80°C, in the atmosphere above the material being ground is less than 3 vol%.

[0031] In particular, drying is carried out until the content of dimethyl carbonate falls below 4 vol%, in particular 3 vol%, and / or the content of cyclohexylbenzene falls below 1 vol%, in particular 0.5 vol%.

[0032] Preferably, drying takes place immediately after shredding. This means, in particular, that the time between the start of shredding the batteries and the point at which at least part of the resulting shredded material begins to dry is no more than five minutes, and especially no more than one minute. Rapid drying after shredding keeps the mass of material that could potentially react electrochemically to a minimum, and also minimizes the electrochemical reaction time of potential exothermic reactions. This reduces the risk to the equipment and the environment.

[0033] According to the invention, the vacuum is generated by means of a jet pump. Jet pumps are, particularly with a suitable choice of jet medium, largely insensitive to aggressive gases being pumped out. Preferably, the jet medium, which is a liquid, has a pH value of at least 8, particularly at least 9, for example at least 12. In this case, undesirable components of the pumped-out gas can decompose or react to form less harmful substances. For example, dimethyl carbonate and / or ethyl methyl carbonate can be broken down by a saponification reaction. Any hydrogen fluoride contained in the jet medium can be converted to a harmless salt in an acid-base reaction in the alkaline environment.

[0034] According to the invention, the radiation medium contains a fluorine-precipitating substance. For example, the radiation medium can contain sodium carbonate or calcium carbonate. The salts formed during the reaction with a fluorine compound, in particular hydrogen fluoride, are preferably separated, in particular by filtering or sedimentation. In this way, it is at least largely prevented that hydrogen fluoride or other toxic fluorine-containing compounds can be released into the environment.

[0035] Drying is preferably carried out at a temperature of no more than 80°C. In this case, hardly any hydrogen fluoride is produced. This increases the service life of the battery processing plant and reduces the environmental hazard.

[0036] According to a preferred embodiment, the method comprises the steps of condensing components of the electrolyte by cooling and / or pressure increases, resulting in an electrolyte condensate. For example, the condensation is carried out at a point located between the dryer and the vacuum pump with respect to the gas flow. Gases coming from the dryer must therefore first pass through a condenser before they can reach the vacuum pump. This results in at least a predominant portion of the gaseous electrolyte present in the gas generated during drying being deposited in the condenser before the remaining gas reaches the pump. In this way, electrolyte can be recovered. Furthermore, the gas flow through the vacuum pump is reduced, which extends its service life and reduces its energy consumption.

[0037] According to a preferred embodiment, the method alternatively includes the step of gas purification by adsorption of the volatile organic components onto an activated carbon filter upstream or downstream of the compressor unit.

[0038] Preferably, the method according to the invention alternatively or additionally comprises the step of purifying the gas produced during drying before it reaches the vacuum pump. This can be achieved, for example, by passing the gas through an activated carbon filter and / or a filter containing substances that react with hydrogen fluoride, for example a calcium salt such as calcium carbonate or a potassium salt such as potassium carbonate.

[0039] Preferably, the method according to the invention comprises a drying step at a drying temperature and for a drying duration selected such that the binder, which binds the active material of the lithium battery to a substrate, decomposes at least to a predominant extent. It is advantageous if this drying step, which can also be referred to as high-temperature drying, is carried out spatially separated from a first drying step described above. The latter drying step can also be referred to as low-temperature drying.

[0040] Preferably, the high-temperature drying process, during which the binder decomposes, is carried out in such a way that the resulting decomposition gases do not mix with the gases produced during low-temperature drying. It is possible for the high-temperature and low-temperature drying processes to take place at different pressures. For example, high-temperature drying can be carried out at atmospheric pressure.

[0041] The active material is the substance that reacts electrochemically during battery operation. The carrier for the active material is, in particular, a substrate film onto which the active material is applied in particle form. For example, the substrate film could be made of aluminum or an aluminum alloy. The binder is the substance that bonds the active material to the substrate; for example, the binder contains polyvinylidene fluoride.

[0042] It is advantageous to add liquid nitrogen when shredding the batteries. This cools the batteries, the shredding machine, and the material being shredded, and also displaces oxygen and water vapor from the atmosphere.

[0043] It is advantageous if the comminution takes place at a water vapor partial pressure of no more than 20 Pa and / or an oxygen partial pressure of no more than 40 hPa, in particular no more than 15 hPa.

[0044] According to a preferred embodiment, the method comprises the steps of removing the material to be ground from the transport container, separating any hard parts and / or separating the active material from the carrier, in particular by a second grinding stage and / or air jet sieves, so that an active material fraction and a carrier fraction are produced, and packaging the active material fraction and the carrier fraction separately in their respective transport containers. It is advantageous if these transport containers are airtight. Separating the active material fraction and the carrier fraction generally allows transport without permits. A further advantage is that such separated fractions pose only a low risk.

[0045] The removal of the shredded material from the transport container is preferably carried out under vacuum and / or under protective gas.

[0046] It is possible, but not necessary, to fill the transport container with the material to be ground under vacuum. It is advantageous if the transport container is a vacuum container, especially an evacuated vacuum container, so that a negative pressure or vacuum exists inside the container after sealing. Alternatively, the transport container can be filled with an inert gas.

[0047] In a preferred battery processing plant, the separation unit and the drying device are arranged in a single standard container. This has the advantage that the battery processing plant can be transported particularly easily.

[0048] The drying device is designed to dry the material being ground for a period of time until the electrolyte content is so low that an electrochemical reaction is impossible. If the drying device is operated in batch mode, which is one possible embodiment, the drying process is carried out, for example, for a predetermined period of time. Alternatively or additionally, the concentration of organic substances, such as organic carbonates, in the atmosphere is continuously measured within the drying device, and the drying process is stopped when a predetermined threshold concentration is undershot.

[0049] According to a preferred embodiment, the battery processing plant, in particular the vacuum system, comprises a condenser configured for condensing organic components of the atmosphere in the dryer, especially organic carbonates, for example, dimethyl carbonate, ethyl methyl carbonate, and / or ethylene carbonate. Preferably, the condenser is arranged upstream of a vacuum pump in the material flow direction, by means of which the dryer is evacuated. It is advantageous if the condenser is cooled, preferably to a temperature of no more than 90°C, more preferably no more than 80°C, and more particularly no more than 70°C. To minimize the cooling effort, the condenser, if cooled, is cooled to a temperature of at least -10°C, and more particularly at least 10°C.

[0050] It is advantageous if the drying device has a stirring tool, such as an anchor stirrer or a rod stirrer whose stirring rods can be mounted transversely to a stirring shaft. Alternatively or additionally, the stirring tool can be an external stirring device that moves the dryer as a whole.

[0051] According to the invention, the battery processing plant has a vacuum system that is connected to the drying device for generating a vacuum in the drying device. It is particularly advantageous if the vacuum system is also arranged in a standard container. The standard container is preferably a container according to ISO standard 668, preferably a 40-foot container or a 20-foot container.

[0052] The vacuum system includes a jet pump, in which a jet medium is used to generate the vacuum.

[0053] Preferably, the battery processing plant comprises a hard metal separator and / or a light fraction separator, a separating device, in particular a classifying device, for separating the active material from the carrier, especially by a second comminution stage and / or air jet sieves, so that an active material fraction and a carrier fraction are produced, and a second filling device for separately filling the active material fraction and the carrier fraction. It is advantageous if this filling device is designed for filling under vacuum and / or inert gas.

[0054] A hard metal separator is understood to be, in particular, a device for separating fragments of peripheral components of the operating system, the battery cell casing, and the electrical contacts. For example, the hard metal separator comprises a magnetic separator and / or a classifier, in particular a cross-flow classifier and / or a zigzag classifier. The separator is understood to be, in particular, a device for separating the separator film.

[0055] The light fraction separation device preferably comprises a zigzag classifier and / or an air separator, with the air being advantageously recirculated. This reduces the environmental exposure to harmful dust.

[0056] Preferably, the second filling device and the separating devices are arranged in a common standard container, for example in the first standard container described above, or in a second standard container. It is advantageous if the container is dustproof.

[0057] Preferably, the battery processing plant includes a sluice gate between the shredding unit and the inactivation device, in particular the drying device. For example, this is a rotary valve. The sluice gate reduces the oxygen input into the inactivation device, especially the drying device.

[0058] The invention will now be explained in more detail with reference to the accompanying drawings. These drawings show Figure 1 shows a flowchart of a method according to the invention, Figure 2 shows a cross-section through a battery processing plant according to the invention, and Figure 3 shows a cross-section through further, optional components of a battery processing plant according to the invention.

[0059] Figure 1Figure 1 shows the flowchart of a method according to the invention. First, batteries 10.1, 10.2, ..., in particular battery systems consisting of several battery modules or battery stacks, which in turn consist of several battery cells, are discharged in a discharge unit 12. This is followed by the disassembly of the batteries 10 at a disassembly station 14, if necessary because the battery systems cannot otherwise be conveyed into the comminution unit for geometric or gravimetric reasons. For this purpose, the battery systems are opened and disassembled to such an extent that the modules / stacks can be removed individually. If necessary, the cells can also be separated from the control electronics. The resulting subunits (modules / stacks) and / or cells 16.1, 16.2, ...are fed to a comminution unit 18, which includes, for example, a rotor shear with one rotor and one with stators or several rotors, or a cutting mill with one rotor and several rotors.

[0060] The shredding unit 18 shreds the batteries 10 under protective gas 20, which is taken, for example, from a protective gas cylinder. Alternatively or additionally, liquid nitrogen can be injected from a liquid nitrogen source 19. The protective gas can be, for example, nitrogen, a noble gas, carbon dioxide, nitrous oxide, or another, preferably non-toxic, gas.

[0061] During the comminution process, comminution material 24 is produced, which is fed to an inactivation device in the form of a drying device 26. A lock 28 is arranged between the comminution unit 18 and the drying device 26, which is gas-tight to such an extent that the pressure device 26 is almost gas-tightly separated from the comminution unit 18.

[0062] The drying device 26 is connected to a vacuum system 29, which includes a vacuum pump 30 and generates a vacuum. The pressure p 26 in the drying device 26 is approximately 100 hPa, preferably 50 hPa. It should be noted that, within the scope of this description, a vacuum pump is understood to be, in particular and more generally, a device that generates a vacuum. It is possible and preferably, but not necessary, for the vacuum pump to simultaneously act as a compressor, so that it discharges gas at a pressure greater than the ambient pressure.

[0063] In the Figure 1 In the case shown, the vacuum pump is a compressor that draws in and compresses gas 31, which is present in the drying device 26. According to the invention, the vacuum system 29 has a jet pump in which a jet medium in the form of a liquid is passed through a Venturi nozzle at high velocity. The jet medium is alkaline and has a pH value of at least pH 13 and is, for example, a 10% potassium hydroxide solution.

[0064] The vacuum system 29 includes a gas purification device 32, which is arranged between the drying device 26 and the vacuum pump 30 and which, in this case, comprises a condenser 34 and / or an activated carbon filter 36. The condenser is operated at a temperature of -10 °C so that dimethyl carbonate and ethyl methyl carbonate can condense and be discharged into a condensate tank 38. Any water present is also frozen out. A control valve 40 is designed to open when the pressure p 26 becomes too high and to close when the pressure p 26 becomes too low, i.e., when a predetermined threshold value is undershot.

[0065] Preferably, the material to be dried is moved during the drying process. This can be achieved, for example, by stirring with a stirring tool 41, such as an anchor stirrer or a rod stirrer with rods arranged perpendicular to the stirring shaft. Alternatively, it can be achieved by using a moving drying container.

[0066] Drying the comminuted material produces inactivated comminuted material 42, which is fed to a filling device 44. There, the inactivated comminuted material 42 is filled into a transport container 46 under vacuum and / or protective gas. The transport container 46 is preferably gas-tight. It is possible, but not necessary, to fill the transport container 46 with inert gas before transport so that it is at normal pressure. Alternatively, the transport container can be sealed and transported under vacuum. A vacuum-sealed film, for example, an aluminum composite film, can be used as an alternative to the transport container.

[0067] Shielding gas 20 is supplied to the comminution unit 18 by the vacuum pump 30 via a purge line 48. If the vacuum pump 30 also functions as a compressor, as in the present case, which represents a preferred embodiment, the shielding gas can be drawn into a pressurized gas cylinder 50. Alternatively or additionally, the shielding gas 20, optionally after further purification, can be released into the environment.

[0068] Figure 2 Figure 1 schematically shows a cross-section through a battery processing plant 52 according to the invention, which has a standard container 54 in which the shredding unit 18, the drying device 26 and the filling device 44 are arranged. Behind the shredding unit 18, a first gas-tight conveyor 56 is arranged, which comprises, for example, a screw conveyor or a tubular chain conveyor. The first conveyor 56 conveys the shredded material 24 to the drying device 26, which is connected to the Figure 2The drying device 26 is connected to a vacuum generation device that is not visible. A second conveyor 58 is arranged downstream of the drying device 26 in the material flow direction. This conveyor is preferably also gas-tight and may contain a screw conveyor or a tubular chain conveyor. The second conveyor conveys the inactivated comminuted material 42 to the filling device 44.

[0069] Figure 3 Figure 1 shows optional units of the battery processing plant 52 according to the invention, which comprise a pulverizing shredder 60 and a classifier 62. The pulverizing shredder 60 includes a transport container emptying device 64, by means of which inactivated material 42 can be removed from the transport container 46. The pulverizing shredder 60 produces pulverizing material 66, which is fed to the classifier 62. The classifier can, for example, be a zigzag classifier.

[0070] Preferably, the battery processing plant 52 comprises a shredder, which is preferably located in the material flow upstream of the classifying device 74 and contains a high-speed shredding tool, wherein the rotor peripheral speed is greater than 1 m / s, preferably greater than 10 m / s. This shredder comminutes the material to be shredded and mechanically stresses it such that the electrochemically active coating is at least partially detached from the substrate. The presence of such a shredder is a generally preferred feature of a battery processing plant according to the invention.

[0071] The classifier produces a light fraction consisting of separator film and fine coating material, and a heavy fraction consisting of carrier films (aluminum and copper) with a larger, loosely adhering coating. Both fractions are then transferred to separate sieves for further separation into coating and separator film, and coating and metal foil, respectively. The resulting fractions are then processed separately.

[0072] The digestion material 66 is fed to the classifier 62 by means of a third conveyor 68. A fourth conveyor 70 feeds the classified material 72, in particular the material of the light fraction leaving the classifier 62, to a classifying device 74. The classifying device 74 preferably comprises an air jet screen, which simultaneously functions as a separating device for separating the active material from the carrier. The separation produces an active material fraction 76, which is filled into a transport container 78.

[0073] A carrier fraction 80 is also produced, which in the present embodiment is fed by a fifth conveyor 82 to a filling unit 84, which fills the carrier fraction 80 into a container 86. The filling unit 84, together with a second filling unit 88, forms part of a second filling device. Reference list

[0074] 10 battery 50 Pressurized gas cylinder 12 discharge unit 52 Battery processing plant 14 Demonstration day station 54 Standard containers 16 cell 56 first supporter 18 Shredding unit 58 second sponsor 19 liquid nitrogen source 60 Digestive shredder 20 Inert gas 62 Sighter 22 Shielding gas cylinder 64 Transport container emptying device 24 material to be shredded 26 Drying device 66 Exploratory material 28 sluice 68 third sponsor 29 vacuum system 70 fourth sponsor 30 vacuum pump 72 material viewed 31 gas 74 Classifying device 32 Gas purification device 76 Active material fraction 34 capacitor 78 Transport container 36 Activated carbon filter 38 Condensate container 80 Supporting faction 82 fifth sponsor 40 Control valve 84 Filling unit 41 Stirring tool 86 container 42 inactive shredded material 88 second filling unit 44 Filling device 46 Transport container p Pressure 48 Flushing line

Claims

1. A method for treating used lithium batteries (10), comprising the steps: (a) comminuting the lithium batteries (10), thereby obtaining comminuted material (24), (b) deactivating the comminuted material (24), thereby obtaining deactivated comminuted material (42), and (c) filling a transport container (46) with the deactivated comminuted material (42), (d) wherein deactivation is achieved by drying the comminuted material (24), and (e) wherein a vacuum is created by means of a jet pump, characterised in that (f) the working medium is circulated and contains a fluorine precipitating substance.

2. The method according to claim 1, characterised in that a working medium of the jet pump has a pH value of at least 8, especially 9.

3. The method according to one of the preceding claims, characterised in that the vacuum is created by drying at a pressure of at most 300 hPa.

4. The method according to one of the preceding claims, characterised in that the comminuted material (24) is dried until an electrolyte content is so low that an electrochemical reaction is impossible.

5. The method according to one of the preceding claims, characterised by the steps: (a) removing the comminuted material (24) from the transport container (46), (b) separating hard parts and / or separating active material from the carrier, in particular by means of air jet sieving or a second comminution stage, thereby obtaining an active material fraction (76) and a carrier fraction (80), and (c) separately packing the active material fraction (76) and the carrier fraction (80) in transport containers (78).

6. A method according to one of the preceding claims, characterised in that the drying of the comminuted material is only terminated if, upon termination of the drying, a flammable or explosive gas mixture can no longer form above the filled comminuted material and / or if the comminuted material is so dry that no flammable or explosive gas mixture can develop in the transport container or during further processing.

7. A battery processing system for treating used lithium batteries with: (a) a comminution unit (18) for comminuting the lithium batteries (10), thereby obtaining comminuted material (24), (b) a deactivation device (26) for deactivating the comminuted material (24), (c) a filling device (44) for filling a transport container (46) with the deactivated comminuted material (24), (d) the deactivation device comprising a drying device (26), (e) a vacuum system that is connected to the drying device (26) for creating a vacuum in the drying device (26) and (f) comprises a jet pump with a working medium, characterised in that (g) the working medium is circulated and contains a fluorine precipitating substance.

8. A battery processing system according to claim 7, characterised in that the drying device (26) is configured to dry the comminuted material (24) until an electrolyte content is so low that an electrochemical reaction is impossible.

9. A battery processing system according to claim 7 or 8, characterised in that that comminution unit and the drying device (26) are arranged in a standard container (54).

10. The battery processing system according to one of the claims 7 to 9, characterised by - a hard metal separation device and / or a light fraction separation device, - a separating device, in particular a classification device (74), for separating active material from the carrier, in particular by means of air jet sieving and / or a second comminution stage, thereby obtaining an active material fraction (76) and a carrier fraction, in particular aluminium and copper foils, and - a second filling device (44) for separately filling the active material fraction (76) and the carrier fraction (80), in particular aluminium and copper foils.