TARGET AND METHOD FOR MAKING A TARGET
Patent Information
- Application Number
- DE502019012045
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-04-12
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2039-04-12
AI Technical Summary
Existing physical vapor deposition processes face challenges in producing highly pure, chemically homogeneous layers with a fine-grained and isotropic microstructure, often resulting in multilayer formation and impurity introduction due to the use of binders and separate targets for titanium diboride and vanadium diboride.
A target composed of a mixture of titanium diboride (TiB2) and vanadium diboride (VB2) with optional carbon, sintered at high temperatures to achieve high density and chemical homogeneity, eliminating the need for binders and maintaining a fine-grained microstructure through hot pressing or spark plasma sintering.
The solution enables the production of highly pure, chemically homogeneous layers with a fine-grained and isotropic microstructure, achieving densities close to theoretical values and maintaining chemical consistency across the target surface, thereby improving the quality of deposited films.
Description
[0001] The present invention relates to a target (a coating source) for physical vapor deposition having the features of the preamble of claim 1 and to a method for producing a target having the features of claim 9.
[0002] In the current state of the art, physical vapor deposition processes are widely used to produce a wide variety of coatings. Due to the broad range of applications of such coatings, it is necessary to be able to deposit a variety of coating materials.
[0003] Various techniques are used in physical vapor deposition, such as evaporation, sputter deposition or arc evaporation (cathodic arc deposition or arc-source evaporation technique).
[0004] A target is suitable for use in a PVD (physical vapor deposition) process for depositing layers onto a designated substrate material. For the purposes of the invention, the term target refers to sputtering targets or arc cathodes.
[0005] Targets are manufactured using different technologies depending on the material. A basic distinction can be made between powder metallurgy and melt metallurgy processes. Powder metallurgy technologies offer many different options, which must be selected according to the composition of the target and the properties of the integrated elements. Examples include pressing, sintering, hot isostatic pressing (HIP), forging, rolling, hot pressing (HP), and spark plasma sintering (SPS), as well as combinations of these.
[0006] Generic targets and methods are described in WO 2008 / 96648 A1, JP 05195199, JP55128560, and WO 2011 / 137472 A1. Further targets and methods are known from EP 0 577 246 A1, US 2013 / 220800 A1, and US 4,430,184 A.
[0007] In particular, JP55128560 describes the production of a sintered body with at least two different diborides, whereby metals such as nickel, iron, and cobalt are necessarily used in the form of bonds as binders and sintering aids to compensate for the disadvantage of low porosity during production at relatively low sintering temperatures. A disadvantage is that these metals impair the purity of the deposited layers when using a sintered body as targets.
[0008] It is also known to produce layers of titanium diboride (TiB 2 ) and vanadium diboride (VB 2 ) by co-sputtering, using separate targets of essentially pure titanium diboride (TiB 2 ) and essentially pure vanadium diboride (VB 2 ). A disadvantage is that in industrial coating processes, the spatial separation of the separate targets with rotating substrates inevitably results in multilayer coatings, rather than a chemically homogeneous coating.
[0009] The object of the invention is to provide a generic target and a generic method for producing a target which has a high density, with which high-purity, chemically homogeneous layers can be produced and which has a fine-grained and isotropic microstructure.
[0010] This object is achieved by a target having the features of claim 1 and a method having the features of claim 9. Advantageous embodiments of the invention are defined in the dependent claims. Protection is also sought for the use of a target according to the invention in a physical vapor deposition (PVD) process for depositing thin films on a substrate.
[0011] The invention does not require the use of binders or sintering aids such as nickel, cobalt or iron as powdered additives because the inventive method for producing a target takes place at relatively high temperatures. However, this inevitably leads to the microstructure becoming considerably coarser at these high temperatures, which in turn would be disadvantageous for use as a target. The invention avoids this coarsening by using a powder consisting of at least two different phases, namely titanium diboride (TiB 2 ), vanadium diboride (VB 2 ), and optionally carbon, preferably graphite (if the carbon is not present in the form of an impurity in one or both of the titanium diboride (TiB 2 ) or vanadium diboride (VB 2 ) phases). This ensures that a fine-grained microstructure is maintained despite the relatively high densification temperature.
[0012] According to the invention, the sum of the mixture of at least two of the following compounds: titanium diboride (TiB 2 ) and / or vanadium diboride (VB 2 ) and / or the mixed phases ((Ti,V)B 2 ) of titanium diboride (TiB 2 ) and vanadium diboride (VB 2 ) formed during sintering, and the carbon (C) is at least 99.8 mol%. This refers to the metallic purity without considering elements such as oxygen (O), nitrogen (N), or hydrogen (H).
[0013] A powder mixture suitable for the process according to the invention consists of: at least 95 mol% of a mixture of titanium diboride (TiB 2 ) and vanadium diboride (VB 2 ) and optionally 0.01 mol% to 5 mol% carbon (C)
[0014] Due to impurities of titanium diboride (TiB 2 ) and / or vanadium diboride (VB 2 ), borides other than titanium diboride (TiB 2 ) and vanadium diboride (VB 2 ) may be detectable in the targets according to the invention (less than 0.01 mol%).
[0015] In one embodiment of the invention, it is provided that the carbon (C) is in the form of graphite.
[0016] For a mixture of a powder batch for all targets according to the invention discussed below, the following powders were used as examples: TiB 2 with a d50 value for the grain size of 2.4 µm VB 2 with a d50 value for the grain size of 7.0 µm Graphite powder with a grain size of less than 6 µm
[0017] The powders were mixed in a ratio of TiB 2 / VB 2 / C of 74 / 24 / 2 mol% and ground in a grinding unit with grinding balls. The finished ground powder mixture was densified by hot pressing at a pressure of 30 MPa and a temperature of 2000 °C.
[0018] In one embodiment of the invention, it is provided that the titanium diboride (TiB 2 ) and the vanadium diboride (VB 2 ) are distributed homogeneously in the target in such a way that when selecting at least five square or circular different measuring areas each with a size of at least 1 mm 2<, the average chemical composition determined on the surface of the respective measuring area does not deviate by more than 20%, preferably not more than 10%, from an average chemical composition calculated from all selected measuring areas.
[0019] Three such series of measurements for different targets according to the invention are shown in the following table: EDX TiB 2 / VB 2 TiB 2 / VB 2 TiB 2 / VB 2 75 / 25 mol% 87.5 / 12.5 mol% 93.75 / 6.25 mol% measurement Ti at% V at% Ti at% V at% Ti at% V at% 1 76,6 23,4 88,4 11,6 94,1 6,0 2 74,8 25,2 88,9 11,1 94,3 5,7 3 75,6 24,4 88,3 11,7 93,9 6,1 4 76,6 23,4 88,7 11,3 92,9 7,1 5 76,8 23,2 88,9 11,2 94,0 6,0 x 76,1 23,9 88,6 11,4 93,8 6,2
[0020] It is clearly visible that the average chemical composition determined on the surface of the respective measuring area for each of the targets deviates only minimally from the average chemical composition calculated from all selected measuring areas.
[0021] In one embodiment of the invention, it is provided that an isotropic structure without preferred crystallographic grain orientation is recognizable in an X-ray examination of the target, wherein an aspect ratio of grains of the mixture of titanium diboride (TiB 2 ) and / or vanadium diboride (VB 2 ) and / or mixed phases ((Ti,V)B 2 ) of titanium diboride (TiB 2 ) and vanadium diboride (VB 2 ) is less than 1.5, preferably less than 1.2, particularly preferably substantially 1.
[0022] In one embodiment of the invention, it is provided that only titanium diboride (TiB 2 ) and / or vanadium diboride (VB 2 ) and / or mixed phases ((Ti,V)B 2 ) of titanium diboride (TiB 2 ) and vanadium diboride (VB 2 ) are present in the form of X-ray identifiable phases.
[0023] With regard to the method, one embodiment of the invention provides that the hot pressing or spark plasma sintering (SPS) takes place at a pressure of at least 20 MPa, preferably at least 30 MPa.
[0024] Example from production using hot pressing: TiB 2 / VB 2 75 / 25 mol% powder mixture manufactured by grinding in a ball mill, hot pressing in a tool with the format of 238 x 353 mm to a plate with the dimensions of 32 x 238 x 353 mm with the following parameters: o 2000 °C o Force of 252 tons, which corresponds to the pressure of 29.5 MPa o Holding time at sintering temperature of 30 minutes
[0025] The achieved density of the plate is 4.54 g / cm 3< and thus approximately 97.8% of the theoretical density for this material of 4.64 g / cm 3< , calculated using the mixing rule for 75 mol% TiB 2 with the theoretical density of 4.5 g / cm 3< and 25 mol% VB 2 with the theoretical density of 5.1 g / cm 3< .
[0026] With regard to the method, one embodiment of the invention provides that the hot pressing or spark plasma sintering (SPS) takes place in a vacuum or in an inert protective gas atmosphere.
[0027] The microstructure of the target made of TiB 2 / VB 2 mixtures described in this disclosure is transferable to other combinations of borides by a person skilled in the art, both with regard to grain size, density, doping, purity and the manufacturing process via hot pressing or SPS, in particular to combinations of the borides TiB 2 , VB 2 , CrB 2 , ZrB 2 , NbB 2 , MoB 2 , MoB, HfB 2 , TaB 2 , WB 2 , W 2 B 5 . The mixtures are systems of at least two borides, e.g. binary systems of two borides or systems of three, four or even more borides simultaneously in a mixture.
[0028] Embodiments of the invention are discussed with reference to the figures. They show: Fig. 1 an SEM (scanning electron microscope) image of a non-inventive target made of pure TiB 2 Fig. 2 an SEM image of another non-inventive target made of pure TiB 2 Fig. 3a,b SEM images of two inventive targets made of TiB 2 / VB 2 Fig. 4 an SEM image of an inventive target made of TiB 2 / VB 2 Fig. 5 an SEM image of an inventive target made of TiB 2 / VB 2 Fig. 6 an SEM image of an inventive target made of TiB 2 / VB 2 Fig. 7a,b an X-ray image (XRD) of an inventive target according to Fig. 3b and an enlarged section of the X-ray image (XRD) Fig. 8a photographic image of the result of a hardness test on a target according to the invention made of TiB 2 / VB 2 75 / 25 mol% Fig. 9a photographic image of the result of a hardness test on a target according to Fig. 4 Fig. 10a photographic image of the result of a hardness test on a target according to Fig. 5
[0029] Fig. 1 and 2 show examples of a microstructure of pure TiB 2 material that was compacted at different temperatures to achieve a correspondingly high density. For ease of comparison, the magnification has been chosen to be identical in both figures. If the temperature is too high, significant grain coarsening occurs.
[0030] Fig. 1 shows pure TiB 2 , hot-pressed at 1650 °C. The microstructure is still relatively fine-grained, with an estimated mean grain size of 2 µm as the d50 value. The density of the material is 4.43 g / cm 3 , which is approximately 98% of the theoretical density of 4.52 g / cm 3 for TiB 2 .
[0031] Fig. 2 shows pure TiB 2 , hot-pressed at 1700 °C. The microstructure is already relatively coarse in places, with individual grains larger than 10 µm. The density of the material is approximately 98.5% of the theoretical density of TiB 2 .
[0032] Fig. 3 to 5show examples of targets according to the invention, in which the molecular ratio of titanium (Ti) to vanadium (V) in the mixture of titanium diboride (TiB 2 ) and / or vanadium diboride (VB 2 ) and / or mixed phases ((Ti,V)B 2 ) of titanium diboride (TiB 2 ) and vanadium diboride (VB 2 ) is in a range of 1:99 to 99:1, preferably in a range of 10:90 to 90:10. The structure of the TiB 2 / VB 2 materials in the Fig. 3 to 5 shows no texturing and an isotropic structure with a grain aspect ratio of essentially 1.
[0033] Fig. 3a shows a detail of a target made of a TiB 2 / VB 2 75 / 25 mol% material, densified via SPS at 1900 °C. The density of the material is 4.19 g / cm 3< and thus approximately 90 % of the theoretical density for this material of 4.64 g / cm 3< , calculated using the mixing rule for 75 mol% TiB 2 with the theoretical density of 4.5 g / cm 3< and 25 mol% VB 2 with the theoretical density of 5.1 g / cm 3< .
[0034] Fig. 3b shows a detail of a target made of a TiB 2 / VB 2 75 / 25 mol% material, densified via SPS at 2000 °C. The density of the material is 4.49 g / cm 3< and thus approximately 97 % of the theoretical density for this material of 4.64 g / cm 3< , calculated using the mixing rule for 75 mol% TiB 2 with the theoretical density of 4.5 g / cm 3< and 25 mol% VB 2 with the theoretical density of 5.1 g / cm 3< .
[0035] Fig. 4 shows a detail of a target made of a TiB 2 / VB 2 87.5 / 12.5 mol% material, densified via SPS at 2000 °C. The density of the material is 4.52 g / cm 3< and thus approximately 99 % of the theoretical density for this material of 4.57 g / cm 3< , calculated using the mixing rule for 87.5 mol% TiB 2 with the theoretical density of 4.5 g / cm 3< and 12.5 mol% VB 2 with the theoretical density of 5.1 g / cm 3< .
[0036] Fig. 5shows a TiB 2 / VB 2 93.75 / 6.25 mol% material densified via SPS at 2000 °C. The density of the material is 4.46 g / cm 3< and thus approximately 98 % of the theoretical density for this material of 4.53 g / cm 3< , calculated using the mixing rule for 93.75 mol% TiB 2 with the theoretical density of 4.5 g / cm 3< and 6.25 mol% VB 2 with the theoretical density of 5.1 g / cm 3< .
[0037] The above-described targets according to the invention were produced by the SPS method, which was carried out in a vacuum.
[0038] Fig. 6For comparison, shows a microstructure that still has a high porosity because it was densified at the lowest acceptable temperature, namely a TiB 2 / VB 2 75 / 25 mol% material densified via SPS at 1750 °C. The density of the material is 4.01 g / cm 3< and thus approximately 86% of the theoretical density for this material of 4.64 g / cm 3< , calculated using the mixing rule for 75 mol% TiB 2 with the theoretical density of 4.5 g / cm 3< and 25 mol% VB 2 with the theoretical density of 5.1 g / cm 3< .
[0039] In the Fig. 7a and 7b is an X-ray spectrum for phase analysis on the target with the composition according to Fig. 3b Of interest are reflections characteristic of the phases TiB 2 , (Ti,V)B 2 , and VB 2 . These three phases, TiB 2 , (Ti,V)B 2 , and VB 2 , are primarily attributable to this spectrum by an expert.
[0040] The Figures 8 to 10Each shows an example of an HV30 hardness indentation measured on the TiB 2 / VB 2 mixed targets. To obtain a representative statement regarding hardness, three HV30 hardness indentations were used.
[0041] Fig. 8 shows one of three HV30 hardness indentations on a TiB 2 / VB 2 75 / 25 mol% target.
[0042] Fig. 9 shows one of three HV30 hardness indentations on a target made of TiB 2 / VB 2 87.5 / 12.5 mol%.
[0043] Fig. 10 shows one of three HV30 hardness indentations on a target made of TiB 2 / VB 2 93.75 / 6.25 mol%.
[0044] The measurement results are summarized in the following table: Impression TiB 2 / VB 2 75 / 25 mol% TiB 2 / VB 2 87.5 / 12.5 mol% TiB 2 / VB 2 93.75 / 6.25 mol% Nr.1 2270 2257 2414 Nr.2 2302 2487 2373 Nr.3 2238 2393 2443 x 2270 HV30 2379 HV30 2410 HV30
Claims
1. Target for physical vapour deposition with the following chemical composition: - at least 95 mol% of a mixture of at least two of the following compounds: titanium diboride (TiB2) and / or vanadium diboride (VB2) and / or mixed phases ((Ti,V)B2) of titanium diboride (TiB2) and vanadium diboride (VB2) - 0.01 mol% to 5 mol% of carbon (C) - less than 0.01 mol% of borides other than titanium diboride (TiB2) and / or vanadium diboride (VB2) and / or mixed phases ((Ti,V)B2) of titanium diboride (TiB2) and vanadium diboride (VB2) wherein, in relation to metallic purity, the sum of the mixture of titanium diboride (TiB2) and / or vanadium diboride (VB2) and / or mixed phases ((Ti,V)B2) of titanium diboride (TiB2) and vanadium diboride (VB2) and the carbon (C) is at least 99.8 mol%, and with the following physical properties: - a density greater than 90%, preferably greater than 95%, of the theoretical density of the chemical composition defined above - a d50 value, as the average grain size, of grains of the mixture of titanium diboride (TiB2) and / or vanadium diboride (VB2) and / or mixed phases ((Ti,V)B2) of titanium diboride (TiB2) and vanadium diboride (VB2), of less than 10 µm, preferably less than 3 µm.
2. Target according to claim 1, wherein the molecular ratio of titanium (Ti) to vanadium (V) in the mixture of titanium diboride (TiB2) and / or vanadium diboride (VB2) and / or mixed phases ((Ti,V)B2) of titanium diboride (TiB2) and vanadium diboride (VB2) lies in a range of from 1:99 to 99:1, preferably in a range of from 10:90 to 90:10.
3. Target according to at least one of the preceding claims, wherein the carbon (C) is present in the form of graphite.
4. Target according to at least one of the preceding claims, wherein only titanium diboride (TiB2) and / or vanadium diboride (VB2) and / or mixed phases ((Ti,V)B2) of titanium diboride (TiB2) and vanadium diboride (VB2) are present in the form of radiographically identifiable phases.
5. Target according to at least one of the preceding claims, wherein the titanium diboride (TiB2) and / or the vanadium diboride (VB2) and / or mixed phases ((Ti,V)B2) of titanium diboride (TiB2) and vanadium diboride (VB2) are present homogeneously distributed in the target such that, if at least five different square or circular measurement areas, with a size of at least 1 mm2 in each case, are selected, the average chemical composition determined on the surface of the respective measurement area does not deviate by more than 20%, preferably not by more than 10%, from an averaged chemical composition calculated from all of the selected measurement areas.
6. Target according to at least one of the preceding claims, wherein an isotropic structure without preferred crystallographic grain orientation is recognizable in a radiographic examination of the target, wherein an aspect ratio of grains of titanium diboride (TiB2) and / or vanadium diboride (VB2) and / or mixed phases ((Ti,V)B2) of titanium diboride (TiB2) and vanadium diboride (VB2) is less than 1.5, preferably less than 1.2, particularly preferably substantially 1.
7. Target according to at least one of the preceding claims, wherein possibly present chemical elements other than titanium (Ti), vanadium (V), boron (B) and carbon (C) are dissolved in the structure of the mixture of titanium diboride (TiB2) and / or vanadium diboride (VB2) and / or mixed phases ((Ti,V)B2) of titanium diboride (TiB2) and vanadium diboride (VB2) and are not radiographically detectable as separate phases.
8. Target according to at least one of the preceding claims, wherein an HV30 Vickers hardness of the target is greater than 1500 HV30, preferably greater than 2000 HV30.
9. Method for producing a target for physical vapour deposition, in particular a target according to at least one of the preceding claims, wherein titanium diboride (TiB2) present in the form of a powder and vanadium diboride (VB2) present in the form of a powder - as well as, where appropriate, pulverulent carbon, unless it is present as an impurity - are mixed and, where appropriate, mechanically ground, and the thus-produced batch of powder is compacted in a shaping die by means of hot pressing or spark plasma sintering (SPS), characterized in that the batch of powder consists of: - at least 95 mol% of a mixture of titanium diboride (TiB2) and vanadium diboride (VB2) - and 0.01 mol% to 5 mol% of carbon (C) wherein, in relation to metallic purity, the sum of the mixture of titanium diboride (TiB2) and vanadium diboride (VB2) and the carbon (C) is at least 99.8 mol%, and in that the hot pressing or spark plasma sintering (SPS) is effected at a temperature of at least 1750°C, preferably at least 1850°C, particularly preferably at least 1950°C.
10. Method according to the preceding claim, wherein the hot pressing or spark plasma sintering (SPS) is effected at a pressure of at least 20 MPa, preferably at least 30 MPa.
11. Method according to at least one of the preceding claims, wherein the hot pressing or spark plasma sintering (SPS) is effected in a vacuum or in an inert protective atmosphere.
12. Use of a target according to at least one of claims 1 to 8 in a physical vapour deposition (PVD) process for depositing thin films on a substrate.