THERMOPLASTIC FOAM MADE FROM TWO SPECIAL POLYURETHANE DISPERSIONS
Patent Information
- Application Number
- DE502020009322
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-02-28
- Filing Date
- 2020-02-18
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2040-02-18
AI Technical Summary
Foamed articles, particularly those intended for wound dressings, face challenges with instability, brittleness, and cytotoxicity due to the use of conventional foam stabilizers, which are not skin-compatible and can lead to contamination and aesthetic issues.
A foamed article is produced by mixing two chemically distinct polyurethane dispersions (A and B), with specific compositions and reaction conditions to achieve high stability, tear resistance, and skin compatibility, while minimizing cytotoxic components, and using a manufacturing process that includes isocyanate-functional prepolymers, polyols, and hydrophilizing agents to create a non-cytotoxic and crack-free foam.
The resulting foamed article exhibits high stability, tear resistance, and excellent skin compatibility with minimal toxic components, ensuring improved safety and performance as a wound dressing or hygiene article.
Description
[0001] The invention relates to a foamed article, in particular a hygiene article, a component of a wound dressing, a component of a wearable device or a wound foam, which is available on the basis of two polyurethane dispersions (A) and (B), as well as its manufacturing process, its application and the provision of a kit of parts made from the two polyurethane dispersions (A) and (B).
[0002] Foamed articles are known from the prior art that require various foam stabilizers to produce a stable foam. Most of the foam stabilizers used are unsuitable for bringing the foam into contact with human skin or for producing wound dressings. This is primarily due to the cytotoxic potential of the additives used in the formulations. Such foams are known from patent applications US-2016-0235880-A1 and US-2011-0275728-A1.
[0003] Another common requirement for foamed products is that they should be as free of cracks as possible. This is particularly important if these foamed products are intended for use as wound dressings. Cracks have the disadvantage of not only compromising the overall stability of the foamed product, but also providing entry points for contaminants, usually indicating a certain brittleness of the foam, and generally being visually unacceptable to customers.
[0004] Therefore, one of the objectives of the pending invention was to provide a foamed article or a manufacturing process for such an article which does not exhibit at least one disadvantage of the prior art, at least in part.
[0005] Another objective of the invention was to provide a foamed article that exhibits high stability and high tear resistance while offering high skin compatibility and containing the lowest possible amount of toxic or cytotoxic ingredients.
[0006] Furthermore, the task was to provide a process that enables the production of a foamed article that is as stable, tear-resistant and / or skin-friendly as possible, and in particular non-toxic or non-cytotoxic.
[0007] A first object of the pending invention is a foamed article produced by mixing a first polyurethane dispersion (A) with at least a second polyurethane dispersion (B), optionally with the addition of further additives, foaming and subsequent drying of the mixture, wherein the polyurethane dispersion (A) is obtainable by A) isocyanate-functional prepolymers from A1) organic polyisocyanates, A2) polymeric polyols with number-average molecular weights of 400 to 8000 g / mol, preferably 400 to 6000 g / mol, or more preferably 600 to 3000 g / mol, and OH functionalities of 1.5 to 6, more preferably 1.8 to 3, or more preferably 1.9 to 2.1, and A3) optionally hydroxy-functional compounds with molecular weights of 62 to 399 g / mol, and A4) optionally isocyanate-reactive, anionic or potentially anionic and optionally nonionic hydrophilizing agents, prepared, and B) their free NCO groups then wholly or partially B1) optionally with amino-functional compounds with molecular weights of 32 to 400 g / mol and B2) with amino-functional, anionic or potentially anionic hydrophilizing agents under Chain elongation is implemented and the prepolymers are dispersed in water before, during or after step B).wherein any potentially anionic groups present are converted into the anionic form by partial or complete reaction with a neutralizing agent, and wherein the second polyurethane dispersion (B) is obtainable by reactive reaction of at least the following components: , A. an aliphatic polyisocyanate component with an average isocyanate functionality of ≥ 1.8 and ≤ 2.6, B. a polymeric polyether-polyol component, C. an amino-functional chain extender component with at least 2 isocyanate-reactive amino groups, containing at least one amino-functional compound C1., which has no ionic or ionogenic groups and / or one amino-functional compound C2., which has ionic or ionogenic groups, D. optionally further hydrophilizing components that are different from C2., E. optionally hydroxy-functional compounds with a molecular weight of 62 to 399 mol / g, F. optionally further polymeric polyols that are different from B., G.a compound having exactly one isocyanate-reactive group, or a compound having more than one isocyanate-reactive group, wherein only one of the isocyanate-reactive groups reacts with the isocyanate groups present in the reaction mixture under the chosen reaction conditions, and H. optionally an aliphatic polyisocyanate component with a mean isocyanate functionality of > 2.6 and ≤ 4. wherein components B and F together contain ≤ 30 wt.% of component F, preferably ≤ 20 wt.% of component F, or preferably ≤ 10 wt.% of component F, based on the total mass of components B and F.
[0008] Polyurethane dispersions (A) and (B) differ in their composition at least in the selection or quantity of at least one component. Therefore, polyurethane dispersions (A) and (B) are chemically different and distinguishable from one another in at least a portion of their respective polymers.
[0009] Preferably, the components of dispersions (A) and (B), as well as all other components for the formation of the foamed article, are low to non-cytotoxic. Low to non-cytotoxic according to the invention means that the foamed article, and preferably all components of the foamed article, exhibit a viability of ≥ 70%, preferably ≥ 80%, or a classification of 0 to 2 ("no to mild", meaning no to low cytotoxicity) in a cytotoxicity test according to DIN ISO 10993-5:2009-10. Polyurethane dispersion (A)
[0010] In order to achieve anionic hydrophilization in the production of the polyurethane dispersion (A), hydrophilizing agents are preferably used in A4) and / or B2) which have at least one group reactive towards NCO groups, such as amino, hydroxy or thiol groups in the case of A4) and amino groups in the case of B2) and which also have -COO- or -SO 3 - or -PO 3 2-< as anionic or their wholly or partially protonated acid forms as potentially anionic groups.
[0011] Preferred aqueous anionic polyurethane dispersions (A) have a low degree of hydrophilic anionic groups, preferably from 2 to 200 milliequivalents, particularly preferably from less than 10 to 100 milliequivalents per 100 g of solid resin.
[0012] To achieve good sedimentation stability, the number-mean particle size of the polyurethane dispersions (A) is preferably less than 750 nm, particularly preferably less than 500 nm, as determined by laser correlation spectroscopy.
[0013] The ratio of NCO groups of the compounds from component A1) to NCO-reactive groups such as amino, hydroxy or thiol groups of the compounds of components A2) to A4) in the preparation of the NCO-functional prepolymer is 1.05 to 3.5; preferably 1.2 to 3.0 and particularly preferably 1.3 to 2.5.
[0014] The amino-functional compounds in step B) are used in such an amount that the equivalent ratio of isocyanate-reactive amino groups of these compounds to the free isocyanate groups of the prepolymer is 40 to 150%, preferably 50 to 125%, particularly preferably 60 to 100%.
[0015] Suitable polyisocyanates of component A1) are the aromatic, araliphatic, aliphatic or cycloaliphatic polyisocyanates of an NCO functionality of ≥ 2 that are known to the person skilled in the art.
[0016] Examples of such suitable polyisocyanates are 1,4-butylene diisocyanate, 1,6-hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), 2,2,4- and / or 2,4,4-trimethylhexamethylene diisocyanate, the isomeric bis(4,4'-isocyanatocyclohexyl)methanes or mixtures thereof of any isomer content, 1,4-cyclohexylene diisocyanate, 1,4-phenylene diisocyanate, 2,4- and / or 2,6-toluene diisocyanate, 1,5-naphthylene diisocyanate, 2,2'- and / or 2,4'- and / or 4,4'-diphenylmethane diisocyanate, 1,3- and / or 1,4-bis-(2-isocyanato-prop-2-yl)benzene (TMXDI), 1,3-bis-(isocyanatomethyl)benzene (XDI), as well as Alkyl 2,6-diisocyanatohexanoates (lysine diisocyanates) with C1-C8 alkyl groups.
[0017] In addition to the polyisocyanates mentioned above, modified diisocyanates with uretdione, isocyanurate, urethane, allophanate, biuret, iminooxadiazindione and / or oxadiazinetrione structures, as well as non-modified polyisocyanate with more than 2 NCO groups per molecule, such as 4-isocyanatomethyl-1,8-octanediisocyanate (nonane triisocyanate) or triphenylmethane-4,4',4"-triisocyanate, can also be used in proportion.
[0018] Preferably, these are polyisocyanates or polyisocyanate mixtures of the type mentioned above with exclusively aliphatic and / or cycloaliphatic bonded isocyanate groups and a medium NCO functionality of the mixture of 2 to 4, preferably 2 to 2.6 and particularly preferably 2 to 2.4.
[0019] Particularly preferred in A1) are 1,6-hexamethylene diisocyanate, isophorone diisocyanate, the isomeric bis(4,4'-isocyanatocyclohexyl)methanes, and mixtures thereof.
[0020] In A2), polymeric polyols with a number-average molecular weight Mn of 400 to 8000 g / mol, preferably of 400 to 6000 g / mol and particularly preferably of 600 to 3000 g / mol are used. These preferably have an OH functionality of 1.5 to 6, particularly preferably of 1.8 to 3, and most preferably of 1.9 to 2.1.
[0021] Such polymeric polyols are those commonly known in polyurethane coating technology: polyester polyols, polyacrylate polyols, polyurethane polyols, polycarbonate polyols, polyether polyols, polyester polyacrylate polyols, polyurethane polyacrylate polyols, polyurethane polyester polyols, polyurethane polyether polyols, polyurethane polycarbonate polyols, and polyester polycarbonate polyols. These can be used individually or in any mixture with each other in A2).
[0022] Such polyester polyols are the polycondensates of di- and optionally tri- and tetraols and di- and optionally tri- and tetracarboxylic acids or hydroxycarboxylic acids or lactones, which are known per se. Instead of the free polycarboxylic acids, the corresponding polycarboxylic anhydrides or corresponding polycarboxylic acid esters of lower alcohols can also be used to produce the polyesters.
[0023] Examples of suitable diols include ethylene glycol, butylene glycol, diethylene glycol, triethylene glycol, polyalkylene glycols such as polyethylene glycol, as well as 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol and isomers, neopentyl glycol, or hydroxypivalic acid neopentyl glycol esters, with 1,6-hexanediol and isomers, neopentyl glycol, and hydroxypivalic acid neopentyl glycol esters being preferred. In addition, polyols such as trimethylolpropane, glycerol, erythritol, pentaerythritol, trimethylolbenzene, or trishydroxyethyl isocyanurate can also be used.
[0024] Phthalic acid, isophthalic acid, terephthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, cyclohexanedicarboxylic acid, adipic acid, azelaic acid, sebacic acid, glutaric acid, tetrachlorophthalic acid, maleic acid, fumaric acid, itaconic acid, malonic acid, cortic acid, 2-methyl succinic acid, 3,3-diethylglutaric acid, and / or 2,2-dimethyl succinic acid can be used as dicarboxylic acids. The corresponding anhydrides can also be used as the acid source.
[0025] Provided that the average functionality of the polyol to be esterified is greater than 2, monocarboxylic acids such as benzoic acid and hexanecarboxylic acid can also be used.
[0026] Preferred acids are aliphatic or aromatic acids of the type mentioned above. Adipic acid, isophthalic acid, and optionally trimellitic acid are particularly preferred.
[0027] Hydroxycarboxylic acids that can be used as reactants in the production of a polyester polyol with terminal hydroxyl groups include, for example, hydroxycaproic acid, hydroxybutyric acid, hydroxydecanoic acid, hydroxystearic acid, and the like. Suitable lactones are caprolactone, butyrolactone, and their homologs. Caprolactone is preferred.
[0028] Polycarbonates containing hydroxyl groups, preferably polycarbonate diols, with number-average molecular weights Mn of 400 to 8000 g / mol, preferably 600 to 3000 g / mol, can also be used in A2). These are obtainable by reacting carbonic acid derivatives, such as diphenyl carbonate, dimethyl carbonate or phosgene, with polyols, preferably diols.
[0029] Examples of such diols are ethylene glycol, 1,2- and 1,3-propanediol, 1,3- and 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, neopentyl glycol, 1,4-bishydroxymethylcyclohexane, 2-methyl-1,3-propanediol, 2,2,4-trimethylpentanediol-1,3, dipropylene glycol, polypropylene glycols, dibutylene glycol, polybutylene glycols, bisphenol A and lactone-modified diols of the aforementioned type.
[0030] The polycarbonate diol preferably contains 40 to 100 wt% hexanediol, preferably 1,6-hexanediol and / or hexanediol derivatives. Such hexanediol derivatives are based on hexanediol and, in addition to terminal OH groups, have ester or ether groups. Such derivatives are obtainable by reacting hexanediol with excess caprolactone or by etherification of hexanediol with itself to give dihexylene glycol or trihexylene glycol.
[0031] Instead of or in addition to pure polycarbonate diols, polyether-polycarbonate diols can also be used in A2). The polycarbonates containing hydroxyl groups are preferably linear in structure.
[0032] Polyether polyols can also be used in A2). Suitable examples include polytetramethylene glycol polyethers, which are well-known in polyurethane chemistry and can be obtained by polymerizing tetrahydrofuran via cationic ring opening.
[0033] Also suitable are the addition products of styrene oxide, ethylene oxide, propylene oxide, butylene oxides, and / or epichlorohydrin to di- or polyfunctional starter molecules, which are known per se. Polyether polyols based on the at least partial addition of ethylene oxide to di- or polyfunctional starter molecules can also be used as component A4) (non-ionic hydrophilizing agents).
[0034] Suitable starter molecules include all compounds known in the art, such as water, butyldiglycol, glycerol, diethylene glycol, trimethylpropane, propylene glycol, sorbitol, ethylenediamine, triethanolamine, and 1,4-butanediol. Preferred starter molecules are water, ethylene glycol, propylene glycol, 1,4-butanediol, diethylene glycol, and butyldiglycol.
[0035] Particularly preferred embodiments of the polyurethane dispersions (A) contain as component A2) a mixture of polycarbonate polyols and polytetramethylene glycol polyols, wherein the proportion of polycarbonate polyols in this mixture is 0 to 80 wt.% and the proportion of polytetramethylene glycol polyols is 100 to 20 wt.%. A proportion of 50 to 100 wt.% of polytetramethylene glycol polyols and a proportion of 0 to 50 wt.% of polycarbonate polyols is preferred. Particularly preferred is a proportion of 75 to 100 wt.% of polytetramethylene glycol polyols and a proportion of 0 to 25 wt.% of polycarbonate polyols, in each case with the proviso that the sum of the wt. percent of the polycarbonate and polytetramethylene glycol polyols equals 100% and the proportion of the sum of the polycarbonate and polytetramethylene glycol polyether polyols in component A2) is at least 50 wt.%, preferably 60 wt.% and particularly preferably at least 70 wt.%.
[0036] The compounds of component A3) have molecular weights of 62 to 400 g / mol.
[0037] In A3), polyols of the specified molecular weight range with up to 20 carbon atoms, such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,3-butylene glycol, cyclohexanediol, 1,4-cyclohexanedimethanol, 1,6-hexanediol, neopentyl glycol, hydroquinone dihydroxyethyl ether, bisphenol A (2,2-bis(4-hydroxyphenyl)propane), hydrogenated bisphenol A, (2,2-bis(4-hydroxycyclohexyl)propane), trimethylolpropane, glycerol, pentaerythritol, and any mixtures thereof, can be used.
[0038] Suitable esterdiols include those of the aforementioned molecular weight range, such as α-hydroxybutyl-ε-hydroxycaproic acid esters, ω-hydroxyhexyl-γ-hydroxybutyric acid esters, adipic acid (β-hydroxyethyl) esters or terephthalic acid bis(β-hydroxyethyl) esters.
[0039] Furthermore, monofunctional, isocyanate-reactive, hydroxyl-containing compounds can also be used in A3). Examples of such monofunctional compounds are ethanol, n-butanol, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monomethyl ether, dipropylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monobutyl ether, 2-ethylhexanol, 1-octanol, 1-dodecanol, and 1-hexadecanol.
[0040] Preferred compounds of component A3) are 1,6-hexanediol, 1,4-butanediol, neopentyl glycol, and trimethylolpropane.
[0041] Anionic or potentially anionic hydrophilic compounds of component A4) are understood to be all compounds that possess at least one isocyanate-reactive group, such as a hydroxyl group, and at least one functionality, such as -COO⁻ < M⁺ < , -SO₃⁻ < M⁺ < , -PO(O⁻ < M⁺ < )₂, where M⁺ < is, for example, a metal cation, H⁺ < , NH₄⁺ < , NHR₃⁺ < , where R can be a C1-C12 alkyl group, a C5-C6 cycloalkyl group, and / or a C2-C4 hydroxyalkyl group, which, upon interaction with aqueous media, enters into a pH-dependent dissociation equilibrium and can thus be negatively or neutrally charged. Suitable anionic or potentially anionic hydrophilic compounds are mono- and dihydroxycarboxylic acids, mono- and dihydroxysulfonic acids, and mono- and dihydroxyphosphonic acids and their salts. Examples of such anionic orPotentially anionic hydrophilizing agents are dimethylolpropionic acid, dimethylolbutyric acid, hydroxypivalic acid, malic acid, citric acid, glycolic acid, lactic acid, and the propoxylated adduct of 2-butenediol and NaHSO₃, as described in DE-A 2 446 440, pages 5-9, formulas I-III. Preferred anionic or potentially anionic hydrophilizing agents of component A4) are those of the aforementioned type that possess carboxylate or carboxylic acid groups and / or sulfonate groups.
[0042] Particularly preferred anionic or potentially anionic hydrophilizing agents are those containing carboxylate or carboxylic acid groups as ionic or potentially ionic groups, such as dimethylolpropionic acid, dimethylolbutyric acid and hydroxypivalic acid or their salts.
[0043] Suitable non-ionic hydrophilizing compounds of component A4) are, for example, polyoxyalkylene ethers containing at least one hydroxy or amino group, preferably at least one hydroxy group.
[0044] Examples are the monohydroxy-functional polyalkylene oxide polyether alcohols, which on average contain 5 to 70, preferably 7 to 55 ethylene oxide units per molecule, and which can be accessed in a manner known per se by alkoxylation of suitable starter molecules (e.g. in Ullmann's Encyclopedia of Industrial Chemistry, 4th edition, Volume 19, Verlag Chemie, Weinheim, pp. 31-38).
[0045] These are either pure polyethylene oxide ethers or mixed polyalkylene oxide ethers, containing at least 30 mol%, preferably at least 40 mol% of ethylene oxide units based on all alkylene oxide units contained.
[0046] Preferred polyethylene oxide ethers of the type mentioned above are monofunctional mixed polyalkylene oxide polyethers comprising 40 to 100 mol% ethylene oxide and 0 to 60 mol% propylene oxide units.
[0047] Preferred nonionic hydrophilizing compounds of component A4) are those of the type mentioned above, wherein they are block (co)polymers prepared by block-wise addition of alkylene oxides to suitable starters.
[0048] Suitable starter molecules for such nonionic hydrophilizing agents are saturated monoalcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, the isomers pentanols, hexanols, octanols and nonanols, n-decanol, n-dodecanol, n-tetradecanol, n-hexadecanol, n-octadecanol, cyclohexanol, the isomers methylcyclohexanols or hydroxymethylcyclohexane, 3-ethyl-3-hydroxymethyloxetane or tetrahydrofurfuryl alcohol, diethylene glycol monoalkyl ethers, such as diethylene glycol monobutyl ether, unsaturated alcohols such as allyl alcohol, 1,1-dimethylallyl alcohol or oleic alcohol, aromatic alcohols such as phenol, the isomers cresols or methoxyphenols, and araliphatic alcohols such as benzyl alcohol. Anise alcohol or cinnamyl alcohol, secondary monoamines such as dimethylamine, diethylamine, dipropylamine, diisopropylamine, dibutylamine, bis-(2-ethylhexyl)amine, N-methyl- and N-ethylcyclohexylamine or dicyclohexylamine, and heterocyclic secondary amines such as morpholine,Pyrrolidine, piperidine, or 1H-pyrazole. Preferred starter molecules are saturated monoalcohols of the type mentioned above. Diethylene glycol monobutyl ether or n-butanol are particularly preferred as starter molecules.
[0049] Suitable alkylene oxides for the alkoxylation reaction are in particular ethylene oxide and propylene oxide, which can be used in any order or in a mixture in the alkoxylation reaction.
[0050] Component B1) can be di- or polyamines such as 1,2-ethylenediamine, 1,2- and 1,3-diaminopropane, 1,4-diaminobutane, 1,6-diaminohexane, isophorone diamine, isomeric mixture of 2,2,4- and 2,4,4-trimethylhexamethylenediamine, 2-methylpentamethylenediamine, diethylenetriamine, triaminononane, 1,3- and 1,4-xylylenediamine, α,α,α',α'-tetramethyl-1,3- and -1,4-xylylenediamine, and 4,4-diaminodicyclohexylmethane and / or dimethylethylenediamine. The use of hydrazine and hydrazides such as adipic acid dihydrazide is also possible, but less preferred.
[0051] Furthermore, compounds that, in addition to a primary amino group, also contain secondary amino groups, or OH groups in addition to an amino group (primary or secondary), can also be used as component B1). Examples include primary / secondary amines such as diethanolamine, 3-amino-1-methylaminopropane, 3-amino-1-ethylaminopropane, 3-amino-1-cyclohexylaminopropane, 3-amino-1-methylaminobutane, and alkanolamines such as N-aminoethylethanolamine, ethanolamine, 3-aminopropanol, and neopentanolamine.
[0052] Furthermore, monofunctional isocyanate-reactive amine compounds can also be used as component B1), such as methylamine, ethylamine, propylamine, butylamine, octylamine, laurylamine, stearylamine, isononyloxypropylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, N-methylaminopropylamine, diethyl(methyl)aminopropylamine, morpholine, piperidine, or suitable substituted derivatives thereof, amidamines from diprimary amines and monocarboxylic acids, monoketimes of diprimary amines, primary / tertiary amines such as N,N-dimethylaminopropylamine.
[0053] Preferred compounds of component B1) are 1,2-ethylenediamine, 1,4-diaminobutane, and isophoronediamine. Mixtures of the aforementioned diamines of component B1) are particularly preferred, especially mixtures of 1,2-ethylenediamine and isophoronediamine, as well as mixtures of 1,4-diaminobutane and isophoronediamine.
[0054] Anionic or potentially anionic hydrophilizing compounds of component B2) are understood to be all compounds that have at least one amino group and at least one functionality such as -COO -< M +< , -SO 3 -< M +< , -PO(O -< M +< ) 2 with M +< for example equal to metal cation, H +< , NH 4 +< , NHR 3 +< , where R can be a C1-C12 alkyl group, C5-C6 cycloalkyl group and / or a C2-C4 hydroxyalkyl group, which enters into a pH-dependent dissociation equilibrium upon interaction with aqueous media and can thus be negatively or neutrally charged.
[0055] Suitable anionic or potentially anionic hydrophilizing compounds are mono- and diaminocarboxylic acids, mono- and diaminosulfonic acids, and mono- and diaminophosphonic acids and their salts. Examples of such anionic or potentially anionic hydrophilizing agents are N-(2-aminoethyl)-β-alanine, 2-(2-aminoethylamino)ethanesulfonic acid, ethylenediaminepropyl or butylsulfonic acid, 1,2- or 1,3-propylenediamineβ-ethylsulfonic acid, glycine, alanine, taurine, lysine, 3,5-diaminobenzoic acid, and the addition product of IPDA and acrylic acid (EP-A 0 916 647, Example 1). Furthermore, cyclohexylaminopropanesulfonic acid (CAPS) from WO-A 01 / 88006 can be used as an anionic or potentially anionic hydrophilizing agent.
[0056] Mixtures of anionic or potentially anionic hydrophilizing agents and non-ionic hydrophilizing agents can also be used for hydrophilization.
[0057] In a preferred embodiment for the production of the special polyurethane dispersions (A), the components A1) to A4) and B1) to B2) are used in the following quantities, the individual quantities always adding up to 100 wt.%: 5 to 40 wt% component A1), 55 to 90 wt% A2), 0 to 20 wt% sum of components A3) and B1), 0.1 to 25 wt% sum of components A4) and B2), wherein, based on the total amounts of components A1) to A4) and B1) to B2), 0.1 to 10 wt% of anionic or potentially anionic hydrophilizing agents from A4) and / or B2) are used.
[0058] In a particularly preferred embodiment for the production of the special polyurethane dispersions (A), the components A1) to A4) and B1) to B2) are used in the following quantities, the individual quantities always adding up to 100 wt.%: 5 to 35 wt% component A1), 60 to 90 wt% A2), 0.5 to 15 wt% sum of components A3) and B1), 0.5 to 15 wt% sum of components A4) and B2), wherein, based on the total amounts of components A1) to A4) and B1) to B2), 0.5 to 7 wt% of anionic or potentially anionic hydrophilizing agents from A4) and / or B2) are used.
[0059] The production of the anionically hydrophilized polyurethane dispersions (A) can be carried out in one or more steps in a homogeneous phase or, in the case of multi-step reactions, partially in a dispersed phase. After complete or partial polyaddition from A1) to A4), a dispersion, emulsification, or dissolution step is performed. Subsequently, a further polyaddition or modification may be carried out in the dispersed phase.
[0060] All methods known from the prior art, such as prepolymer mixing processes, acetone processes, or melt dispersion processes, can be used. The acetone process is preferred.
[0061] For the production via the acetone process, components A2) to A4) and the polyisocyanate component A1) are typically added in whole or in part to produce an isocyanate-functional polyurethane prepolymer. This mixture is optionally diluted with a water-miscible solvent that is inert towards isocyanate groups and heated to temperatures in the range of 50 to 120°C. Catalysts known in polyurethane chemistry can be used to accelerate the isocyanate addition reaction.
[0062] Suitable solvents are the usual aliphatic, keto-functional solvents such as acetone and 2-butanone, which can be added not only at the beginning of the preparation but also, if necessary, in portions later on. Acetone and 2-butanone are preferred.
[0063] Other solvents such as xylene, toluene, cyclohexane, butyl acetate, methoxypropyl acetate, N-methylpyrrolidone, N-ethylpyrrolidone, and solvents containing ether or ester units can be added and distilled off completely or partially, or, in the case of N-methylpyrrolidone and N-ethylpyrrolidone, remain completely in the dispersion. However, preferably no solvents other than the aforementioned aliphatic, keto-functional solvents are used.
[0064] Subsequently, the components A1) to A4) that were not added at the beginning of the reaction are added.
[0065] In the production of the polyurethane prepolymer from A1) to A4), the stoichiometric ratio of isocyanate groups to isocyanate-reactive groups is 1.05 to 3.5; preferably 1.2 to 3.0 and particularly preferably 1.3 to 2.5.
[0066] The conversion of components A1) to A4) to the prepolymer is carried out partially or completely, but preferably completely. Polyurethane prepolymers containing free isocyanate groups are thus obtained in bulk or in solution.
[0067] In the neutralization step for the partial or complete conversion of potentially anionic groups into anionic groups, bases such as tertiary amines, e.g. trialkylamines with 1 to 12, preferably 1 to 6 C atoms, particularly preferably 2 to 3 C atoms in each alkyl group, or alkali metal bases such as the corresponding hydroxides are used.
[0068] Examples include trimethylamine, triethylamine, methyldiethylamine, tripropylamine, N-methylmorpholine, methyldiisopropylamine, ethyldiisopropylamine, and diisopropylethylamine. The alkyl groups can also bear hydroxyl groups, as in dialkylmonoalkanols, alkyldialkanols, and trialkanolamines. Inorganic bases, such as aqueous ammonia solution or sodium or potassium hydroxide, can also be used as neutralizing agents.
[0069] Preferred substances are ammonia, triethylamine, triethanolamine, dimethylethanolamine or diisopropylethylamine, as well as sodium hydroxide and potassium hydroxide; sodium hydroxide and potassium hydroxide are particularly preferred.
[0070] The amount of base is between 50 and 125 mol%, preferably between 70 and 100 mol%, of the amount of acid groups to be neutralized. Neutralization can also be carried out simultaneously with dispersion by using a dispersion solution that already contains the neutralizing agent.
[0071] Subsequently, in a further process step, if this has not already been done or has only been partially done, the resulting prepolymer is dissolved using aliphatic ketones such as acetone or 2-butanone.
[0072] In chain extension (step B), NH₂ and / or NH-functional components are partially or completely reacted with the remaining isocyanate groups of the prepolymer. Preferably, chain extension / termination is carried out before dispersion in water.
[0073] For chain termination, amines (B1) with a group reactive towards isocyanates such as methylamine, ethylamine, propylamine, butylamine, octylamine, laurylamine, stearylamine, isononyloxypropylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, N-methylaminopropylamine, diethyl(methyl)aminopropylamine, morpholine, piperidine, or suitable substituted derivatives thereof, amidamines from diprimary amines and monocarboxylic acids, monoketimes of diprimary amines, primary / tertiary amines such as N,N-dimethylaminopropylamine are usually used.
[0074] If anionic or potentially anionic hydrophilizing agents according to definition B2) with NH2 or NH groups are used for partial or complete chain extension, the chain extension of the prepolymers preferably takes place before dispersion.
[0075] The amine components B1) and B2) can optionally be used individually or in mixtures in the process according to the invention in water- or solvent-diluted form, and in principle any sequence of addition is possible.
[0076] If water or organic solvents are used as a diluent, the diluent content in the component used in B) for chain elongation is preferably 70 to 95 wt.%.
[0077] Dispersal preferably takes place after chain elongation. For this purpose, the dissolved and chain-elongated polyurethane polymer is either introduced into the dispersing water, optionally under strong shearing, such as vigorous stirring, or conversely, the dispersing water is stirred into the chain-elongated polyurethane polymer solutions. Preferably, the water is added to the dissolved chain-elongated polyurethane polymer.
[0078] The solvent remaining in the dispersions after the dispersion step is usually subsequently removed by distillation. Removal during the dispersion process is also possible.
[0079] The residual content of organic solvents in the polyurethane dispersions (A) is typically less than 1.0 wt.%, preferably less than 0.5 wt.%, based on the total dispersion.
[0080] The pH value of the polyurethane dispersions (A) essential to the invention is typically less than 9.0, preferably less than 8.5; particularly preferably less than 8.0 and most preferably between 6.0 and 7.5.
[0081] The solids content of the polyurethane dispersions (A) is preferably 35 to 70 wt.%, particularly preferably 40 to 65 wt.%, most preferably 45 to 60 wt.% and particularly 45 to 55 wt.%.
[0082] The amount of anionic or potentially anionic groups on the particle surface, measured by acid-base titration, is generally 2 to 500 mmol, preferably 30 to 400 mmol per 100 grams of solid. Polyurethane dispersion (B)
[0083] In the production of polyurethane dispersion (B), an isocyanate-containing prepolymer is first formed, which is then chain-extended with amino groups. Due to the use of amino group-containing compounds in the production of polyurethane dispersion (B), urea groups can also be formed. Therefore, the polyurethane contained in polyurethane dispersion (B) is subsequently referred to as polyurethane urea, and consequently, polyurethane dispersion (B) is also called polyurethane urea dispersion (B).
[0084] In the context of polyurethane urea dispersion (B), ionogenic groups are understood to be functional groups that are able to form ionic groups, for example by neutralization with a base.
[0085] Component A can be any polyisocyanate that a person skilled in the art would use for this purpose. Particularly suitable polyisocyanates as component A are those aliphatic polyisocyanates known to a person skilled in the art with an average isocyanate functionality of ≥ 1.8 and ≤ 2.6. The term aliphatic also includes cycloaliphatic and / or araliphatic polyisocyanates.
[0086] The average isocyanate functionality refers to the average number of isocyanate groups per molecule.
[0087] Preferred polyisocyanates are those with a molecular weight in the range of 140 to 336 g / mol. Particularly preferred are those selected from the group consisting of... 1,4-Diisocyanatobutane (BDI), 1,5-Pentane diisocyanate (PDI), 1,6-Diisocyanatohexane (HDI), 1,3-Bis(isocyanatomethyl)benzene (1,3-Xylylene diisocyanate, XDI), 1,4-Bis(isocyanatomethyl)benzene (1,4-Xylylene diisocyanate, XDI), 1,3-Bis(1-isocyanato-1-methyl-ethyl)benzene (TMXDI), 1,4-Bis(1-isocyanato-1-methyl-ethyl)benzene (TMXDI), 4-Isocyanatomethyl-1,8-octanediisocyanate (Trisisocyanatononane (TIN)), 2-Methyl-1,5-diisocyanatopentane, 1,5-Diisocyanato-2,2-dimethylpentane, 2,2,4- or 2,4,4-Trimethyl-1,6-diisocyanatohexane 1,10-Diisocyanatodecane and the cycloaliphatic diisocyanates 1,3- and 1,3-diisocyanates.1,4-Diisocyanatocyclohexane, 1,4-Diisocyanato-3,3,5-trimethylcyclohexane, 1,3-Diisocyanato-2(4)-methylcyclohexane, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1-Isocyanato-1-methyl-4(3)isocyanato-methylcyclohexane, 1,8-diisocyanato-p-menthane, 4,4'-diisocyanato-1,1'-bi(cyclohexyl), 4,4'-diisocyanato-3,3'-dimethyl-1,1'-bi(cyclohexyl), 4,4'-Diisocyanato-2,2',5,5'-tetramethyl-1,1'-bi(cyclohexyl), 4,4' and / or 2,4'-Diisocyanatodicyclohexylmethane, 4,4' Diisocyanato-3,3'-dimethyldicyclohexylmethane, 4,4' Diisocyanato-3,3',5,5'-tetramethyldicyclohexylmethane, 1,3-Diisocyanatoadamantane, and 1,3-Dimethyl-5,7-diisocyanatoadamantane or any mixtures of such isocyanates.Particularly preferred are the polyisocyanates selected from 1,4-butylene diisocyanate, 1,5-pentamethylene diisocyanate (PDI), 1,6-hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), 2,2,4- and / or 2,4,4-trimethylhexamethylene diisocyanate, the isomeric bis-(4,4'-isocyanatocyclohexyl)methanes or mixtures thereof of any isomer content (H12-MDI), 1,4-cyclohexylene diisocyanate, 4-isocyanatomethyl-1,8-octane diisocyanate (nonane triisocyanate) and alkyl-2,6-diisocyanatohexanoates (lys diisocyanates) with C1-C8 alkyl groups.
[0088] In addition to the polyisocyanates mentioned above, modified diisocyanates with a mean isocyanate functionality ≥ 2 and ≤ 2.6, with uretdione, isocyanu-rate, urethane, allophanate, biuret, iminooxadiazindione or oxadiazintrione structure, as well as mixtures of these and / or the above, can also be used in proportion.
[0089] Preferably, these are polyisocyanates or polyisocyanate mixtures of the type mentioned above with exclusively aliphatic or cycloaliphatic bonded isocyanate groups or mixtures thereof and an average NCO functionality of the mixture of ≥ 1.8 and ≤ 2.6 and particularly preferably ≥ 2.0 and ≤ 2.4.
[0090] Particularly preferably, the organic polyisocyanate component A. contains an aliphatic or cycloaliphatic polyisocyanate selected from HDI, IPDI and / or H12-MDI or their modification products, most preferably selected from HDI and / or IPDI.
[0091] In a preferred variant, component A consists of IPDI and HDI in the mixture.
[0092] The weight ratio of IPDI:HDI is preferably in the range of 1.05 to 10, particularly preferably in the range of 1.1 to 5, and most preferably in the range of 1.1 to 1.5.
[0093] Preferably, ≥ 5 and ≤ 40 wt.% of component A. and particularly preferably ≥ 10 and ≤ 35 wt.% of component A., in each case based on the total mass of the polyurethane urea, are used to produce the polyurethane urea used according to the invention.
[0094] For the production of the polyurethane urea, component H., an aliphatic polyisocyanate component with a mean isocyanate functionality (mean number of isocyanate groups per molecule) of > 2.6 and ≤ 4, preferably ≥ 2.8 and ≤ 3.8, is preferably used. Component H. is preferably used in a mixture with component A.
[0095] Oligomeric diisocyanates with a functionality > 2.6 and ≤ 4, preferably ≥ 2.8 and ≤ 3.8, and with isocyanurate, urethane, allophanate, biuret, iminooxadiazindione, or oxadiazinetrione structures are particularly suitable as component H. Most preferably, H. contains isocyanurate structures.
[0096] Preferably, the organic polyisocyanate component H. consists of an aliphatic or cycloaliphatic polyisocyanate oligomer based on HDI, IPDI and / or H12-MDI, most preferably based on HDI.
[0097] The molar ratio of the NCO groups from component A to component H is preferably 100:0.5 to 100:50; particularly preferably 100:2 to 100:15 and most preferably 100:3 to 100:8.
[0098] Preferably, ≥ 0 and ≤ 10 wt.% of component H. and particularly preferably ≥ 0.1 and ≤ 3 wt.% of component H., in each case based on the total mass of the polyurethane urea, are used for the production of the polyurethane urea used according to the invention.
[0099] The polymeric polyether polyols used as component B according to the invention preferably have number-average molecular weights of ≥ 500 and ≤ 8000 g / mol, determined by gel permeation chromatography against a polystyrene standard in tetrahydrofuran at 23°C, more preferably ≥ 400 and ≤ 6000 g / mol, and particularly preferably ≥ 600 and ≤ 3000 g / mol, and / or OH functionalities of preferably ≥ 1.5 and ≤ 6, more preferably ≥ 1.8 and ≤ 3, and particularly preferably ≥ 1.9 and ≤ 2.1. The term "polymeric" polyether polyols here means in particular that the polyols mentioned have at least three, more preferably at least four, interconnected repeating units.
[0100] The number-mean molecular weight is determined in this application by gel permeation chromatography (GPC) in tetrahydrofuran at 23°C, unless otherwise specified. The procedure follows DIN 55672-1: "Gel permeation chromatography, Part 1 - Tetrahydrofuran as eluent" (SECurity GPC system from PSS Polymer Service, flow rate 1.0 ml / min; columns: 2 × PSS SDV linear M, 8 × 300 mm, 5 µm; RID detector). Polystyrene samples of known molar mass are used for calibration. The number-mean molecular weight is calculated using software. Baseline points and evaluation limits are defined according to DIN 55672 Part 1.
[0101] Suitable polyether polyols include, for example, the known addition products of styrene oxide, ethylene oxide, propylene oxide, butylene oxide, and / or epichlorohydrin to di- or polyfunctional starter molecules. In particular, polyalkylene glycols such as polyethylene, polypropylene, and / or polybutylene glycols are suitable, especially those with the preferred molecular weights mentioned above. Suitable starter molecules include all compounds known from the prior art, such as water, butyldiglycol, glycerol, diethylene glycol, trimethylpropane, propylene glycol, sorbitol, ethylenediamine, triethanolamine, and 1,4-butanediol.
[0102] The preferred component contains or consists of poly(tetramethylene glycol) polyether polyols.
[0103] Suitable poly(tetramethylene glycol)polyether polyols can be obtained, for example, by polymerization of tetrahydrofuran via cationic ring opening.
[0104] Preferably, component B contains or consists of a mixture of poly(tetramethylene glycol)polyether polyols, wherein the poly(tetramethylene glycol)polyether polyols differ in their number-average molecular weights.
[0105] According to the invention, an amino-functional chain extender component C. with at least 2 isocyanate-reactive amino groups, containing at least one amino-functional compound C 1. which has no ionic or ionogenic groups and / or an amino-functional compound C2. which has ionic or ionogenic groups, is used to produce the polyurethane urea.
[0106] The amino-functional compounds of component C are preferably selected from primary and / or secondary diamines. In particular, the amino-functional compounds of component C comprise at least one diamine.
[0107] Preferably, the amino-functional component C. comprises at least one amino-functional compound C2., which has ionic and / or ionogenic groups.
[0108] Preferably, the amino-functional component C. comprises both amino-functional compounds C2., which have an ionic and / or ionogenic group, and amino-functional compounds C1., which do not have an ionic or ionogenic group.
[0109] For example, component C1 may consist of organic di- or polyamines such as 1,2-ethylenediamine, 1,2- and 1,3-diaminopropane, 1,4-diaminobutane, 1,6-diaminohexane, isophorone diamine (IPDA), isomeric mixture of 2,2,4- and 2,4,4-trimethylhexamethylenediamine, 2-methylpentamethylenediamine, diethylenetriamine, 4,4-diaminodicyclohexylmethane and / or dimethylethylenediamine or mixtures of at least two of these.
[0110] The component C1 is preferably selected from the group consisting of 1,2-ethylenediamine, bis(4-aminocyclohexyl)methane, 1,4-diaminobutane, IPDA, ethanolamine, diethanolamine and diethylenetriamine or a mixture of at least two thereof.
[0111] The component preferably contains ≥ 75 mol%, particularly preferably ≥ 80 mol%, very preferably ≥ 85 mol%, further preferably ≥ 95 mol%, and more preferably 100 mol% of 1,2-ethylenediamine or IPDA, or a mixture of 1,2-ethylenediamine and IPDA, wherein the sum of the two amines in relation to the total amount of C1 preferably lies within the aforementioned ranges. The component preferably contains ≥ 75 mol%, particularly preferably ≥ 80 mol%, very preferably ≥ 85 mol%, further preferably ≥ 95 mol%, and more preferably 100 mol% of 1,2-ethylenediamine.
[0112] Preferably, the hydrophilizing component C2 comprises at least one anionically hydrophilizing compound. More preferably, the hydrophilizing component C2 comprises an anionically hydrophilizing compound comprising at least 80 wt.%, or preferably at least 90 wt.%, based on the total weight of component C2. Particularly preferably, component C2 consists exclusively of anionically hydrophilizing compounds.
[0113] Suitable anionically hydrophilizing compounds contain at least one anionic or ionogenic group that can be converted into an anionic group. Furthermore, suitable anionically hydrophilizing compounds preferably have at least two amino groups and particularly preferably two amino groups. Particularly preferably, the hydrophilizing component C2 comprises or consists of an anionically hydrophilizing compound having at least one anionic or ionogenic group and at least two amino groups.
[0114] Suitable anionically hydrophilizing compounds as component C2, hereinafter also referred to as hydrophilizing agents C2, preferably contain a sulfonic acid or sulfonate group, particularly preferably a sodium sulfonate group. Suitable anionically hydrophilizing compounds as component C2 are, in particular, the alkali metal salts of mono- and diaminosulfonic acids. Examples of such anionically hydrophilizing agents are salts of 2-(2-aminoethylamino)ethanesulfonic acid, ethylenediamine propylsulfonic acid, ethylenediamine butylsulfonic acid, or 1,2- or 1,3-propylenediamine β-ethylsulfonic acid, or mixtures of at least two of these.
[0115] Preferred anionic hydrophilizing agents C2 are those containing sulfonate groups as ionic groups and two amino groups, such as the salts of 2-(2-aminoethylamino)ethylsulfonic acid and 1,3-propylenediamine-β-ethylsulfonic acid. 2-(2-aminoethylamino)ethylsulfonic acid or its salts are particularly preferred as the anionic hydrophilizing agent C2.
[0116] Optionally, the anionic group in component C2 can also be a carboxylate or carboxylic acid group. Component C2 is then preferably selected from diaminocarboxylic acids. In this alternative embodiment, however, the carboxylic acid-based components C2 must be used in higher concentrations compared to those components C2 bearing sulfonate or sulfonic acid groups. Therefore, for the production of the polyurethane urea, it is particularly preferred that no hydrophilic compounds be used that exclusively bear carboxylate groups as the anionic groups of component C2.
[0117] Preferably, for the production of the polyurethane urea used according to the invention, component C2 is used in a range of ≥ 0.1 and ≤ 10 wt.% and particularly preferably in a range of ≥ 0.5 and ≤ 4 wt.% of component C2, in each case based on the total mass of the polyurethane urea.
[0118] For hydrophilization, mixtures of anionic hydrophilizing agents C2. and other hydrophilizing agents D., which are different from C2., can also be used.
[0119] Suitable additional hydrophilizing agents D are, for example, non-ionic hydrophilizing compounds D1 and / or hydroxy-functional ionic or ionogenic, preferably anionic, hydrophilizing agents D2. Preferably, component D is a non-ionic hydrophilizing component D1.
[0120] Suitable hydroxy-functional ionic or ionogenic hydrophilizing agents as component D2 are, for example, hydroxycarboxylic acids such as mono- and dihydroxycarboxylic acids, such as 2-hydroxyacetic acid, 3-hydroxypropanoic acid, 12-hydroxy-9-octadecanoic acid (ricinoleic acid), hydroxypivalic acid, lactic acid, dimethylolbutyric acid, and / or dimethylolpropionic acid, or mixtures of at least two thereof. Hydroxypivalic acid, lactic acid, and / or dimethylolpropionic acid are preferred; dimethylolpropionic acid is particularly preferred. Preferably, no hydroxy-functional ionic or ionogenic hydrophilizing agents D2 are used; in particular, preferably, no hydrophilizing agents containing carboxylate and hydroxy groups, such as dimethylolpropionic acid, are used. The amount of hydroxy-functional ionic or ionogenic hydrophilizing agent D2 is preferably in the range of 0 to 1 wt.%, or more preferably in the range of 0 to 0.5 wt.%.-%, based on the total mass of polyurethane urea contained in the polyurethane urea.
[0121] Suitable nonionically hydrophilizing compounds as component D1 are, for example, polyoxyalkylene ethers possessing isocyanate-reactive groups such as hydroxy, amino, or thiol groups. Preferably, monohydroxy-functional polyalkylene oxide polyether alcohols containing, on average, 5 to 70, preferably 7 to 55 ethylene oxide units per molecule are used. These can be obtained in a known manner by alkoxylation of suitable starter molecules (e.g., in Ullmann's Encyclopedia of Industrial Chemistry, 4th edition, Volume 19, Verlag Chemie, Weinheim, pp. 31–38). These are either pure polyethylene oxide ethers or mixed polyalkylene oxide ethers, containing at least 30 mol%, preferably at least 40 mol%, of ethylene oxide units based on all alkylene oxide units present.
[0122] Preferred nonionic compounds are monofunctional mixed polyalkylene oxide polyethers containing 40 to 100 mol% ethylene oxide and 0 to 60 mol% propylene oxide units.
[0123] Suitable starter molecules for such nonionic hydrophilizing agents include, in particular, saturated monoalcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, the isomeric pentanols, hexanols, octanols and nonanols, n-decanol, n-dodecanol, n-tetradecanol, n-hexadecanol, n-octadecanol, cyclohexanol, the isomeric methylcyclohexanols or hydroxymethylcyclohexane, 3-ethyl-3-hydroxymethyloxetane or tetrahydrofurfuryl alcohol, diethylene glycol monoalkyl ethers, such as diethylene glycol monobutyl ether, unsaturated alcohols such as allyl alcohol, 1,1-dimethylallyl alcohol or oleic alcohol, aromatic alcohols such as phenol, the isomeric cresols or methoxyphenols, and araliphatic alcohols. Benzyl alcohol, anise alcohol or cinnamyl alcohol, secondary monoamines such as dimethylamine, diethylamine, dipropylamine, diisopropylamine, dibutylamine, bis-(2-ethylhexyl)amine,N-methyl- and N-ethylcyclohexylamine or dicyclohexylamine, as well as heterocyclic secondary amines such as morpholine, pyrrolidine, piperidine, or 1H-pyrazole. Preferred starter molecules are saturated monoalcohols of the type mentioned above. Diethylene glycol monobutyl ether, methanol, or n-butanol are particularly preferred as starter molecules.
[0124] Suitable alkylene oxides for the alkoxylation reaction are in particular ethylene oxide and propylene oxide, which can be used in any order or in a mixture in the alkoxylation reaction.
[0125] Preferably, the polyurethane urea used to form the polyurethane urea dispersion (B) contains component D in a range of ≥ 0 and ≤ 20 wt.%, more preferably in a range of ≥ 0 and ≤ 10 wt.%, and most preferably in a range of ≥ 0 and ≤ 5 wt.%, in each case based on the total mass of the polyurethane urea. In a further preferred embodiment, component D is not used to produce the polyurethane urea.
[0126] Component E can optionally be polyols, in particular non-polymeric polyols, of the aforementioned molecular weight range of 62 to 399 mol / g with up to 20 carbon atoms, such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,3-butylene glycol, cyclohexanediol, 1,4-cyclohexanedimethanol, 1,6-hexanediol, neopentyl glycol, hydroquinone dihydroxyethyl ether, bisphenol A (2,2-bis(4-hydroxyphenyl)propane), hydrogenated bisphenol A (2,2-bis(4-hydroxycyclohexyl)propane), trimethylolpropane, trimethylolethane, glycerol, pentaerythritol, and any mixtures thereof.
[0127] Preferably, the polyurethane urea used to form the polyurethane urea dispersion (B) contains ≤ 10 wt.% of component E., preferably ≤ 5 wt.%, and particularly preferably 0 wt.% of component E., in each case based on the total mass of the polyurethane urea. More preferably, the polyurethane urea contains component E. in a range of 0.1 to 10 wt.%, more preferably in a range of 0.2 to 8 wt.%, and more preferably in a range of 0.1 to 5 wt.%, in each case based on the total mass of the polyurethane urea. In a further preferred embodiment, component E. is not used to produce the polyurethane urea.
[0128] Preferably, for the production of the polyurethane urea used according to the invention, in a range of ≥ 0.5 and ≤ 20 wt.% of the sum of components C1. and optionally E., or preferably in a range of ≥ 1 and ≤ 15 wt.% of the sum of components C1. and optionally E., in each case based on the total mass of the polyurethane urea, it is used.
[0129] Component F can be made from other polymeric polyols that differ from B.
[0130] Examples include polymeric polyols that do not fall under the definition of B. because they are not polyether polyols - for example, the polyester polyols, polyacrylate polyols, polyurethane polyols, polycarbonate polyols, , polyester polyacrylate polyols, polyurethane polyacrylate polyols, polyurethane polyester polyols, , polyurethane polycarbonate polyols and polyester polycarbonate polyols known in polyurethane coating technology per se.
[0131] Preferably, component F is not a polymeric polyol containing ester groups, and in particular not a polyester polyol.
[0132] According to the invention, components B and F together contain ≤ 30 wt.%, preferably ≤ 10 wt.%, and particularly preferably ≤ 5 wt.%, of component F, based on the total mass of components B and F. Most preferably, component F is not used in the production of the polyurethane urea.
[0133] Preferably, polyurethane urea used in the invention is used in a range of ≥ 55 and ≤ 90 wt.% of the sum of components B and optionally F, and particularly preferably in a range of ≥ 60 and ≤ 85 wt.% of the sum of components B and optionally F, in each case based on the total mass of the polyurethane urea.
[0134] Component G consists of compounds that have exactly one isocyanate-reactive group, or compounds that have more than one isocyanate-reactive group, where only one of the isocyanate-reactive groups reacts with the isocyanate groups present in the reaction mixture under the chosen reaction conditions.
[0135] Component G differs in at least one property from the other isocyanate-reactive groups, in particular component B, used to produce the polyurethane dispersion (B). Preferably, component G differs from the other isocyanate-reactive groups, in particular component B, due to its chemical composition.
[0136] The isocyanate-reactive groups of component G can be any functional group that can react with an isocyanate group, such as hydroxy groups, thiol groups, or primary and secondary amino groups.
[0137] Isocyanate-reactive groups within the meaning of the invention are preferably primary or secondary amino groups that react with isocyanate groups to form urea groups. In addition to the amino group, the compounds of component G can also have other isocyanate-reactive groups, such as OH groups, wherein only one of the isocyanate-reactive groups reacts with the isocyanate groups present in the reaction mixture under the selected reaction conditions. This can be achieved, for example, by reacting corresponding amino alcohols at relatively low temperatures, for example, at 0 to 60°C, preferably at 20 to 40°C. Preferably, the reaction is carried out in the absence of catalysts that would catalyze the reaction of isocyanate groups with alcohol groups.
[0138] Examples of suitable compounds of component G are primary / secondary amines such as methylamine, ethylamine, propylamine, butylamine, octylamine, laurylamine, stearylamine, isononyloxypropylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, N-methylaminopropylamine, diethyl(methyl)aminopropylamine, morpholine, piperidine, diethanolamine, 3-amino-1-methylaminopropane, 3-amino-1-ethylaminopropane, 3-amino-1-cyclohexylaminopropane, 3-amino-1-methylaminobutane, ethanolamine, 3-aminopropanol, or neopentanolamine.
[0139] Suitable monofunctional compounds also include ethanol, n-butanol, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monomethyl ether, dipropylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monobutyl ether, 2-ethylhexanol, 1-octanol, 1-dodecanol, 1-hexadecanol.
[0140] Preferably, ≥ 0.1 and ≤ 20 wt.% of component G. and particularly preferably ≥ 0.3 and ≤ 10 wt.% of component G., in each case based on the total mass of the polyurethane urea, are used to produce the polyurethane urea used according to the invention.
[0141] Component H is preferably used and the molar ratio of component G to component H is preferably 5:1 to 1:5, particularly preferably 1.5:1 to 1:4 and most preferably 1:1 to 1:3.
[0142] For the production of the polyurethane ureas used according to the invention, components A to H are preferably used in the following quantities, wherein the individual quantities always add up to 100 wt.%: 5 to 40 wt.% component A, 55 to 90 wt.% sum of components B and, if applicable, F, 0.5 to 20 wt.% sum of components C1 and, if applicable, E, 0.1 to 10 wt.% component C2, 0 to 20 wt.% component D, 0.1 to 20 wt.% component G and 0 to 10 wt.% component H.
[0143] Preferably, the foamed article comprises a polyurethane urea obtainable by reacting at least A. an aliphatic polyisocyanate component with an average isocyanate functionality of ≥ 1.8 and ≤ 2.6, selected from HDI, IPDI and / or H12-MDI or their modification products, preferably a mixture of IPDI and HDI; B. a polymeric polyether-polyol component consisting of poly(tetramethylene glycol)polyether polyols (such as (HO-(CHz-CH2-CH2-CH2-O)x-H)), preferably a polymeric polyether-polyol component being a mixture of at least two poly(tetramethylene glycol)polyether polyols, wherein the poly(tetramethylene glycol)polyether polyols differ in their number-average molecular weights; C. an amino-functional chain extender component with at least two isocyanate-reactive primary and / or secondary amino groups, containing at least one amino-functional compound C1, which does not contain ionic or has ionogenic groups and / or an amino-functional compound C2., which has ionic or ionogenic groups, D. optionally further hydrophilizing components which are different from C2., wherein the components D1. are preferably nonionic hydrophilizing components, E. optionally hydroxy-functional compounds with a molecular weight of 62 to 399 mol / g, F. optionally further polymeric polyols which are different from B., G. a compound which has exactly one isocyanate-reactive group, or a compound which has more than one isocyanate-reactive group, wherein only one of the isocyanate-reactive groups reacts with the isocyanate groups present in the reaction mixture under the selected reaction conditions, wherein the isocyanate-reactive group is preferably a primary and / or secondary amino and / or hydroxy group, and H. optionally an aliphatic polyisocyanate component with an average isocyanate functionality of > 2.6 and ≤ 4, wherein the component H.consisting of an aliphatic or cycloaliphatic polyisocyanate oligomer having an isocyanurate, urethane, allophanate, biuret, iminooxadiazindione or oxadiazintrione structure, preferably based on HDI, IPDI and / or H12-MDI, . wherein components B and F together contain ≤ 30 wt.%, preferably ≤ 20 wt.%, or preferably ≤ 10 wt.% of component F, based on the total mass of components B and F.
[0144] The number-average molecular weight of the polyurethane ureas preferably used according to the invention is preferably ≥ 2000 to ≤ 300000 g / mol, preferably ≥ 5000 to ≤ 150000 g / mol.
[0145] The polyurethane urea used to produce the foamed article, as the basis for the polyurethane urea dispersion (B), is preferably present in a physiologically acceptable medium. Particularly preferably, the medium is water, and most preferably, the polyurethane urea is present as an aqueous dispersion (B). Generally, water, along with any other liquid media optionally present, such as solvents, constitutes the main component (> 50 wt%) of the dispersing medium, based on the total amount of the liquid dispersing medium, and optionally, it may even be the sole liquid dispersing medium.
[0146] The foamed article itself contains the polyurethane urea, which contains no or only residual amounts of this medium.
[0147] Preferably, the polyurethane urea used is therefore dispersible in water, which in the context of this invention means that the polyurethane urea can form a sedimentation-stable dispersion in water, in particular deionized water, at 23°C.
[0148] The polyurethane ureas used to form the polyurethane urea dispersion (B) are preferably obtained by producing isocyanate-functional polyurethane prepolymers a) from components A., B. and optionally D. and / or C2., as well as optionally compounds E. and / or H. (step a) and subsequently reacting their free NCO groups wholly or partially with the amino-functional chain extender component C., as well as component G. and optionally components D. and H. (step b).
[0149] Whereas if component H is only used in step b), it is preferably added before the addition of component C and reacted with the prepolymer A.
[0150] Preferably in step b) the reaction is carried out with one or more diamines (component C. with chain elongation, in which the monofunctional component G. is also added as a chain terminator for molecular weight control.
[0151] Components A to H are defined as above. The preferred embodiments mentioned above also apply.
[0152] Preferably, in step b) of the reaction of the prepolymer a) to produce the polyurethane urea, a mixture of components C1, C2, and G is reacted. The use of component C1 allows for the production of a high molar mass without increasing the viscosity of the previously prepared isocyanate-functional prepolymer to a degree that would impede processing. The combination of components C1, C2, and G enables an optimal balance between hydrophilicity and chain length.
[0153] Preferably, the polyurethane prepolymer used has a) terminal isocyanate groups, i.e., the isocyanate groups are located at the chain ends of the prepolymer. Particularly preferably, all chain ends of the prepolymer have isocyanate groups.
[0154] The hydrophilicity of the prepolymer can be controlled via the hydrophilizing components C2 and / or D. Of course, other components, especially the hydrophilicity of component B, also play a role in the hydrophilicity of the prepolymer.
[0155] Preferably the isocyanate-functional polyurethane prepolymers are a) insoluble in water and not dispersible in water.
[0156] Within the scope of the invention, the term "water-insoluble, non-water-dispersible polyurethane prepolymer" means, in particular, that the water solubility of the prepolymer used according to the invention at 23°C is less than 10 g / liter, preferably less than 5 g / liter, and that the prepolymer does not form a sedimentation-stable dispersion in water, especially deionized water, at 23°C. In other words, the prepolymer settles when an attempt is made to disperse it in water. The water insolubility or lack of dispersibility in water refers to deionized water without the addition of surfactants.
[0157] Furthermore, the polyurethane prepolymer used a) preferably has essentially neither ionic nor ionogenic (capable of forming ionic groups) groups. Within the scope of the present invention, this means that the proportion of ionic and / or ionogenic groups, such as, in particular, anionic groups like carboxylate or sulfonate, or cationic groups, is less than 15 milliequivalents per 100 g of polyurethane prepolymer a), preferably less than 5 milliequivalents, particularly preferably less than 1 milliequivalent, and most preferably less than 0.1 milliequivalents per 100 g of polyurethane prepolymer a).
[0158] In the case of acidic ionic and / or ionogenic groups, the acid number of the prepolymer is expediently below 30 mg KOH / g prepolymer, preferably below 10 mg KOH / g prepolymer. The acid number indicates the mass of potassium hydroxide in mg required to neutralize 1 g of the sample under investigation (measurement according to DIN EN ISO 211). The neutralized acids, i.e., the corresponding salts, naturally have no or a reduced acid number. According to the invention, the acid number of the corresponding free acid is decisive in this case.
[0159] The water-insoluble, non-water-dispersible, isocyanate-functional polyurethane prepolymers A. are preferably exclusively obtainable from components A., B. and optionally D., E. and / or H.
[0160] The components are defined as specified above. The preferred embodiments mentioned above also apply.
[0161] In an alternative, less preferred embodiment of the invention, the prepolymers a) used to produce the polyurethane urea according to the invention are water-soluble or water-dispersible. In this embodiment, the hydrophilizing component D. and / or C2. are used in the production of prepolymer a) in an amount sufficient to make the prepolymer water-soluble or water-dispersible. The prepolymer a) preferably has ionic or ionogenic groups.
[0162] Suitable hydrophilizing components D and C2 for this embodiment of the invention are the compounds mentioned above for D and C2. Preferably, at least the compounds mentioned above under D1 and / or C2 are used as hydrophilizing components.
[0163] The polyurethane ureas used to produce the foamed article are preferably dispersed in water before, during, or after step b), particularly preferably during or after step b). This yields a dispersion of the polyurethane ureas, the polyurethane urea dispersion (B).
[0164] The production of the polyurethane urea dispersions (B) can be carried out in one or more steps in a homogeneous phase or, in the case of multi-step reactions, partially in a dispersed phase. After the preparation of the prepolymer (a), a dispersion, emulsification, or dissolution step is preferably carried out. Subsequently, a further polyaddition or modification may optionally take place in the dispersed phase. The solvent or dispersant suitable for the respective prepolymer, such as water or acetone or mixtures thereof, is selected in each case.
[0165] All methods known from the prior art, such as prepolymer mixing processes, acetone processes, or melt dispersion processes, can be used. The acetone process is preferred.
[0166] For the production via the acetone process, components B, optionally D and E, and the polyisocyanate component A, possibly in combination with component H, are typically prepared wholly or partially to produce an isocyanate-functional polyurethane prepolymer. This is optionally diluted with a water-miscible solvent that is inert towards isocyanate groups and heated to temperatures in the range of 50 to 120°C. Catalysts known in polyurethane chemistry can be used to accelerate the isocyanate addition reaction.
[0167] Suitable solvents are the usual aliphatic, keto-functional solvents such as acetone and 2-butanone, which can be added not only at the beginning of the preparation but also, if necessary, in portions later on. Acetone and 2-butanone are preferred, with acetone being particularly preferred. The addition of other solvents without isocyanate-reactive groups is also possible, but not preferred.
[0168] Subsequently, the components of A, B and, if applicable, H, D and E that were not added at the beginning of the reaction can be dosed.
[0169] In the production of the polyurethane prepolymer from A., B. and optionally H., D. and E., the stoichiometric ratio of isocyanate groups to isocyanate-reactive groups is preferably 1.05 to 3.5, particularly preferably 1.1 to 3.0 and most particularly preferably 1.1 to 2.5.
[0170] The conversion of components A, B, and optionally H, D, and E to form the prepolymer can be partial or complete, but preferably complete. Polyurethane prepolymers containing free isocyanate groups can thus be obtained in bulk or in solution.
[0171] If ionic groups, such as carboxyl groups, are present in the prepolymer, they can be converted into ionic groups in a further step by neutralization.
[0172] In the neutralization step for the partial or complete conversion of potentially anionic groups into anionic groups, bases such as tertiary amines, e.g. trialkylamines with 1 to 12, preferably 1 to 6 C atoms, particularly preferably 2 to 3 C atoms in each alkyl group, or, most preferably, alkali metal bases such as the corresponding hydroxides can be used.
[0173] Preferably, inorganic bases such as aqueous ammonia solution or sodium or potassium hydroxide can be used as neutralizing agents; sodium hydroxide and potassium hydroxide are particularly preferred.
[0174] The amount of base is preferably 50 to 125 mol%, particularly preferably between 70 and 100 mol% of the amount of acid groups to be neutralized. Neutralization can also be carried out simultaneously with dispersion, in which the dispersing water already contains the neutralizing agent.
[0175] Following neutralization, in a further process step, if this has not already been done or has only been partially done, the resulting prepolymer is dissolved using aliphatic ketones such as acetone or 2-butanone.
[0176] In the chain extension / termination step b), components C, G, and optionally D react with the remaining isocyanate groups of the prepolymer. Preferably, the chain extension / termination is carried out before dispersion in water.
[0177] Suitable components C. for chain extension and G. for chain breakage are already listed above. The preferred embodiments mentioned above also apply analogously.
[0178] If anionic hydrophilizing agents according to definition C2. with NH 2 - or NH groups are used for chain extension, the chain extension of the prepolymers in step b) preferably takes place before dispersion in water.
[0179] The equivalent ratio of NCO-reactive groups of the compounds used for chain elongation and chain termination to free NCO groups of the prepolymer is generally between 40 and 150%, preferably between 50 and 110%, and particularly preferably between 60 and 100%.
[0180] The components C1, C2 and G, can optionally be used individually or in mixtures in water- or solvent-diluted form in the process according to the invention, whereby in principle any sequence of addition is possible.
[0181] If water or organic solvents are used as diluents in step b), the respective diluent content in the components C1, C2 and G used is preferably 40 to 95 wt.%.
[0182] The dispersion is preferably carried out following chain elongation and chain termination. For this purpose, the dissolved polyurethane polymer (e.g., in acetone) reacted with the amine is added, optionally under strong shear, such as vigorous stirring, either to the dispersing water or, conversely, the dispersing water is stirred into the chain-elongated polyurethane polymer solutions. Preferably, the water is added to the dissolved polyurethane polymer. In this way, the polyurethane urea dispersion (B) is obtained.
[0183] The solvent remaining in the dispersions after the dispersion step is usually subsequently removed by distillation. Removal during the dispersion process is also possible.
[0184] The resulting aqueous polyurethane urea dispersions (B) preferably have a volatile organic compound (VOC) content, such as volatile organic solvents, of less than 10 wt.%, more preferably less than 3 wt.%, and even more preferably less than 1 wt.%, based on the aqueous polyurethane urea dispersion. VOCs within the meaning of this invention are, in particular, organic compounds with an initial boiling point of no more than 250 °C at a standard pressure of 101.3 kPa.
[0185] The determination of the content of volatile organic compounds (VOCs) is carried out in the context of the present invention in particular by gas chromatographic analysis.
[0186] The pH value of the aqueous polyurethane urea dispersion (B) used according to the invention is typically less than 9.0, preferably less than 8.5 and is particularly preferably between 5.5 and 8.0.
[0187] To achieve good sedimentation stability, the number-mean particle size of the special polyurethane urea dispersions is preferably less than 750 nm, particularly preferably less than 500 nm, determined by laser correlation spectroscopy after dilution with deionized water (instrument: Malvern Zetasizer 1000, Malvern Inst. Limited).
[0188] The solids content of the polyurethane urea dispersions (B) is preferably 10 to 70 wt.%, particularly preferably 20 to 60 wt.%, and most preferably 40 to 60 wt.%. The solids content is determined by heating a balanced sample to 125°C until a constant weight is reached. Once the weight is constant, the solids content is calculated by reweighing the sample.
[0189] Preferably, these polyurethane urea dispersions (B) contain less than 5 wt.%, particularly preferably less than 0.2 wt.%, based on the mass of the dispersions (B), of unbound organic amines.
[0190] The polyurethane urea dispersion (B) used to produce the foamed articles preferably has a viscosity of ≥ 1 and ≤ 10,000 mPa s, or more preferably ≥ 10 and ≤ 5,000 mPa s, and particularly preferably ≥ 10 and ≤ 4,000 mPa s, at 23°C and a constant shear rate of 10 s⁻¹. The viscosity is determined as described in the methods section.
[0191] Preferably, the two polyurethane dispersions (A) and (B) are not chemically or physically identical. The two polyurethane dispersions (A) and (B) preferably differ in the molecular masses of the polyurethanes contained in (A) and (B). The difference in the mean molecular weight Mw (determined by GPC with DMAc as the mobile phase) of the polyurethanes of (A) and (B) is preferably in the range of 20:1 to 1.2:1, particularly preferably from 10:1 to 1.3:1, and most preferably from 5:1 to 1.5:1. The polyurethane polymer of the polyurethane dispersion (A) preferably has a mean molecular weight Mw in the range of 150,000 to 1,000,000 g / mol, or more preferably from 170,000 to 700,000 g / mol, and most preferably from 180,000 to 500,000 g / mol. The polyurethane polymer of the polyurethane dispersion (B) preferably has a mean molecular weight Mw in the range of 10,000 to 170,000 g / mol, or preferably from 20,000 to 150,000 g / mol.
[0192] In addition to the polyurethane dispersions (A) and (B), additives in the form of auxiliary and additive substances can also be used in the foamed article.
[0193] Examples of such auxiliary and additive substances include foaming agents such as foaming agents and stabilizers, thickeners or thixotropic agents, antioxidants, light stabilizers, emulsifiers, plasticizers, pigments, fillers, dyes, container stabilizing additives, biocides, pH regulators, dispersions, and / or leveling agents. Depending on the desired properties and intended use of the foamed articles, the final product may contain ≤ 30 wt.%, preferably ≤ 20 wt.%, or preferably ≤ 10 wt.% of such fillers, based on the total dry matter of the foamed article. Preferably, no dyes or pigments are used, resulting in preferably white foams and thus white foamed articles.
[0194] Preferably, foaming agents such as foam formers and stabilizers are included as auxiliary and additive substances. Foam stabilizers are additives that extend the lifespan of foams by increasing the interfacial viscosity and elasticity of the foam lamellae, as described in "spektrum.de," the lexicon of chemistry. Generally, all surface-active amphiphilic substances can be used as foam stabilizers. Particularly suitable are, for example, commercially available compounds such as fatty acid amides, sulfosuccinamides, hydrocarbon sulfonates, sulfates, or fatty acid salts, where the lipophilic residue preferably contains 12 to 24 carbon atoms, amphiphilic organosilicon copolymers, and alkyl polyglycosides, which can be obtained by reacting longer-chain monoalcohols (4 to 22 carbon atoms in the alkyl residue) with mono-, di-, or polysaccharides using methods known to those skilled in the art (see, e.g., [reference]).Kirk-Othmer, Encyclopedia of Chemical Technology, John Wiley & Sons, Vol. 24, p. 29). Particularly suitable foaming agents are EO / PO block copolymers, which can be obtained by methods known to those skilled in the art by adding ethylene oxide and propylene oxide to OH- or NH-functional starter molecules (see, e.g., Kirk-Othmer, Encyclopedia of Chemical Technology, John Wiley & Sons, Vol. 24, p. 28). To improve foam formation, foam stability, or the properties of the resulting polyurethane foam, other additives can be included in the mixture in addition to or as an alternative to the EO / PO block copolymers. Such other additives can, in principle, be any anionic, nonionic, or cationic surfactants known per se; anionic and nonionic surfactants are preferred, and nonionic surfactants are particularly preferred. Surfactants are substances that reduce the surface tension of a liquid or the interfacial tension between two phases.Certain compounds can therefore act as both surfactants and foam stabilizers. However, amphiphilic, nonionic EO / PO block copolymers are particularly preferred as foam-forming additives. Preferably, 0.5 to 5 wt%, or more preferably 1 to 4 wt%, and most preferably 1.5 to 3.4 wt% of foam stabilizer are used, based on the total mass of the polyurethane dispersions (A) and (B). As will be explained in detail later, foam stabilizers are preferred that exhibit the lowest possible to no cytotoxic activity, which can be determined by measuring cell viability in a cytotoxicity test. Preferably, the foam stabilizers exhibit a cell viability of ≥70% or a classification of 0-2 (no to mild cytotoxicity) in a cytotoxicity test according to DIN ISO 10993-5.
[0195] Commercially available thickeners can be used, such as dextrin, starch, and polysaccharide derivatives like guar gum or cellulose derivatives like cellulose ethers or hydroxyethylcellulose, fully synthetic organic thickeners based on polyacrylic acids, polyvinylpyrrolidones, poly(meth)acrylic compounds, or polyurethanes (associative thickeners), as well as inorganic thickeners such as bentonite or silica. Associative polyurethane thickeners are particularly preferred. The amount of thickener is preferably ≤ 5 wt%, or more preferably in the range of 0.1 to 5 wt%, and further preferably from 0.2 to 2 wt%, based on the total mass of the sum of dispersions (A) and (B). Thickeners exhibiting the lowest possible to no cytotoxic activity are preferred, which can be determined by measuring cell viability in a cytotoxicity test.
[0196] Furthermore, it is preferable to use certain crosslinking agents in the production of the foamed article to improve, for example, the chemical resistance of the foamed article to bases, acids, or solvents. Examples include polyisocyanate-based crosslinking agents such as Bayhydur® < 3100 and Baymedix® < FP520. The foamed article preferably contains crosslinking agents in amounts ranging from 0 to 5 wt%, or more preferably from 0.1 to 4.5 wt%, or more preferably from 0.5 to 3 wt%, based on the total mass of the foamed article. It is also possible to add, incorporate, or coat the foamed article with antimicrobial or biological agents, which have a positive effect, for example, on wound healing and the prevention of microbial contamination.The addition or incorporation of these active ingredients can be carried out by adding them to the polyurethane dispersion (A) and / or to the polyurethane urea dispersion (B).
[0197] Preferred active substances of the aforementioned type are those from the group of antiseptics, growth factors, protease inhibitors and non-steroidal anti-inflammatory drugs / opiates, or also active substances such as thrombin alfa for local hemostasis.
[0198] Preferably, the active ingredient comprises at least a bacteriostatic agent or a bactericide, most preferably an antiseptic biguanide and / or its salt, preferably the hydrochloride.
[0199] Examples of mixtures for the production of the article according to the invention are listed below, wherein the sum of the values in wt.% is ≤ 100 wt.%. These mixtures typically comprise, based on the total mass of the mixture, ≥ 80 to ≤ 100 wt.% of dispersions (A) and (B) in total, ≥ 0 to ≤ 10 wt.% foaming agent, ≥ 0 to ≤ 10 wt.% crosslinker, and ≥ 0 to ≤ 10 wt.% thickener.
[0200] Preferably, the mixture comprises, based on the total mass of the mixture, ≥ 85 to ≤ 100 wt.% of the dispersions (A) and (B) in total, ≥ 0 to ≤ 7 wt.% foaming aids, ≥ 0 to ≤ 5 wt.% crosslinking agents, ≥ 0 to ≤ 10 wt.% antiseptics or biocides and ≥ 0 to ≤ 5 wt.% thickeners.
[0201] Particularly preferably, the mixture comprises, based on the total mass of the mixture, ≥ 89 to ≤ 100 wt.% of the dispersions (A) and (B) in total, ≥ 0 to ≤ 6 wt.% foaming agent, ≥ 0 to ≤ 4 wt.% crosslinker and ≥ 0 to ≤ 4 wt.% thickener.
[0202] Preferably, the foamed article is crack-free. According to the invention, "crack-free" means that at least one, preferably at least two, and particularly preferably all of the following criteria are met for the foamed article: i. the foamed article has no cracks with a width of ≥ 10 mm, preferably ≥ 5 mm, more preferably ≥ 2 mm, and particularly preferably ≥ 0.5 mm; ii. the foamed article has no cracks on its surface that are deeper than 0.4 mm; iii. the foamed article has a crack area of ≤ 6%, preferably ≤ 3% or preferably ≤ 0.5%, based on the total surface area of the foamed article;
[0203] The crack width under i., the crack depth under ii. and the crack area under iii. are each determined according to the method described below in the measurement methods.
[0204] In a preferred embodiment of the foamed article, the foamed article has at least one, preferably at least two, or preferably all of the following properties i. to xiii.: i. the foamed article has no cracks with a width of ≥ 2 mm, preferably ≥ 1 mm, more preferably ≥ 0.5 mm, and particularly preferably ≥ 0.1 mm, the crack width being determined according to the method under measurement methods; ii. the foamed article has no cracks on its surface deeper than 0.4 mm, preferably deeper than 0.2 mm, or more preferably deeper than 0.1 mm, the crack depth being determined according to the method under measurement methods; iii. the foamed article has a crack area of ≤ 6%, preferably ≤ 3%, or more preferably ≤ 0.5%, based on the total surface area of the foamed article; iv. the foamed article has a cell viability of ≥ 70% or classification as 0-2 (no to mild cytotoxicity) in a cytotoxicity test according to DIN ISO 10993-5; v. the foamed article has a density in the range of 80 to 500 g / L, preferably 100 to 400 g / L, or preferably 120 to 300 g / L; vi.the foamed article has a thickness (D) in the range of 0.1 to 100 mm, preferably in the range of 0.5 to 50 mm, more preferably in the range of 1 to 10 mm; vii. the foamed article has a tensile strength in the range of 100 to 1100 kPa, preferably in the range of 200 to 500 kPa, measured according to DIN EN ISO 527-2:2012-06; viii. the foamed article has an elongation at break in the range of 100 to 500%, preferably in the range of 150 to 400%, measured according to DIN EN ISO 527-2:2012-06; ix. that the polyurethane urea formed from the polyurethane dispersion (B) is amorphous and has a Tg ≤ - 25 °C, preferably ≤ - 40 °C, or preferably ≤ - 50 °C, determined by differential dynamic calorimetry in accordance with DIN EN 61006, method A; x.The foamed article has a melting or softening range of ≤ 180°C, preferably ≤ 150°C, at a maximum pressure of 4 bar and is fully thermoplastically processable within this range; xi. the foamed article has a mean pore size in the range of 200 to 750 µm, preferably in the range of 300 to 600 µm; xii. the foamed article has a top layer, preferably containing a thermoplastic polyurethane or a thermoplastic polyethylene, on at least one surface of the foamed article; xiii. that the foamed article is part of a composite material.
[0205] Preferably, the foamed article has at least the properties i. and ii., and particularly preferably the properties i., ii. and iii. It is further preferred if the foamed article has at least the properties i. and iv., or ii. and iv., or iii. and iv., or most preferably the properties i., ii., iii. and iv.
[0206] The term "thermoplastically processable" means that the material can be deformed when heated or processed, such as by lamination, without destroying the basic structure of the underlying polymer, since with thermoplastic materials, moderate heating only results in the structure melting out and subsequent crystallization upon cooling.
[0207] For the purposes of this invention, amorphous means that the polyurethane urea forms no or only such small crystalline components in the temperature range described in the measurement method below that only one or more glass transition points Tg, but no melting ranges with a fusion enthalpy ≥ 20J / g, can be found in the temperature range described using the DSC measurements.
[0208] Within the scope of this invention, the glass transition temperature Tg is determined by means of dynamic differential calorimetry in accordance with DIN EN 61006, Method A, wherein a DSC instrument is used which is calibrated for the determination of Tg with indium and lead and wherein three immediately successive cycles of heating from -100°C to +150°C, at a heating rate of 20 K / min, with subsequent cooling at a cooling rate of 320 K / min are carried out and the third heating cycle is used to determine the values and wherein Tg is determined as the temperature at half the height of a glass transition stage.
[0209] If the polyurethane urea is in dispersion form, special procedures are required for sample preparation for DSC measurements. When determining the glass transition temperature (Tg) of dispersions using DSC, the Tg of the polymer can be masked by the caloric effects of the dispersant (water, neutralizing agents, emulsifiers, co-solvents, etc.) or significantly lowered due to miscibility with the polymer. Therefore, the dispersant is preferably completely removed by suitable drying before DSC measurement, as even small residual amounts of dispersant act as plasticizers and can thus lower the glass transition temperature. The dispersion is therefore preferably spread onto a glass plate with a wet film thickness (WFT) of 100 µm, allowed to evaporate, and then dried for two days in a drying chamber at room temperature and 0% relative humidity (RH).After this sample preparation, residual moisture in the film can still create a broad endothermic evaporation range during the first heating of the DSC measurement. Therefore, to obtain the determined values as free as possible from such influences, the third heating curve is evaluated.
[0210] In a preferred embodiment of the foamed article, the weight ratio of the polyurethane dispersion (A) to the polyurethane dispersion (B) is in a range of 1:1 to 5:1, preferably in a range of 1:1 to 4:1, or preferably in a range of 1:1 to 3:1, based on the total mass of the masses of the dispersions (A) and (B).
[0211] In a preferred embodiment of the foamed article, a film formed from the dispersion (B) by drying has a tensile strength of ≤ 5 MPa, preferably ≤ 3.5 MPa, and particularly preferably ≤ 2.5 MPa. The film formed from the dispersion (B) preferably has an elongation at break of ≥ 1750%, more preferably ≥ 2000%, more preferably in the range of ≥ 1750% to 3000%, and more preferably from 2000% to 4000%. The 500% modulus of the film formed from the dispersion (B) is preferably ≤ 2 MPa, or more preferably ≤ 1.5 MPa, or more preferably ≤ 1.0 MPa, and more preferably in the range of 0.1 to 2 MPa.
[0212] To produce the required films from dispersion (A), dispersion (B) or a mixture of dispersions (A) and (B), the respective dispersion is applied to a polyolefin-coated release paper using a hand squeegee with a gap width of 200 µm and dried for 20 min at 40°C and then for 10 min at 130°C in a circulating air drying oven.
[0213] Preferably the polyurethane urea formed from the polyurethane dispersion (B) is amorphous and has a Tg ≤ - 25 °C, preferably ≤ - 40 °C, or preferably ≤ - 50 °C, determined by differential dynamic calorimetry according to DIN EN 61006, method A.
[0214] Surprisingly, it has been found that by appropriately mixing a foaming dispersion (A) with a dispersion (B) from which films can be formed that can be described as very soft, a foamed article can be produced that is crack-free.
[0215] A film formed from dispersion (A) preferably exhibits an elongation at break in the range of 400% to 700%, a tensile strength of 20 to 50 MPa, and a 100% modulus of preferably ≤ 7 MPa, preferably in the range of 2 to 7 MPa. The process for producing the film from dispersion (A) will be described in detail later.
[0216] Preferably, a film formed from dispersion (A) has an elongation at break that is in the range of 1 to 50% of the elongation at break of a film formed from dispersion (B). Preferably, a film formed from dispersion (A) has a tensile strength that is in the range of 5 to 40% of the tensile strength of a film formed from dispersion (B). Preferably, a film formed from dispersion (A) has a 100% modulus that is in the range of 10 to 50% of the 100% modulus of a film formed from dispersion (B).
[0217] The modulus values and elongations for determining the fracture stress and the fracture strain were determined in a tensile test procedure in accordance with DIN 53504:2009-10 with a test speed of 200 mm / min and a pre-force of 0.05 N / mm 2<.
[0218] In a preferred embodiment of the foamed article, hydrophilizing agents containing sulfone groups are used as B2). Preferably, the sodium or potassium salt of hydroxyethanesulfonic acid is used as the hydrophilizing agent containing sulfone groups.
[0219] In a preferred embodiment of the foamed article, the dispersion (A) has a solid polyurethane content of 52 to 65 wt.%, preferably 55 to 63 wt.%, or preferably 57 to 62 wt.%, based on the total mass of the dispersion (A).
[0220] In a preferred embodiment of the foamed article, component A. or A1) is isophorone diisocyanate (IPDI) and / or hexamethylene diisocyanate (HDI). More preferably, component A. or A1) is a mixture of IPDI and HDI, preferably in a ratio ranging from 2:1 to 1:2, or more preferably in a ratio ranging from 1.5:1 to 1:1.5.
[0221] In a preferred embodiment of the foamed article, component B contains or consists of poly(tetramethylene glycol) polyether polyols.
[0222] In a preferred embodiment of the foamed article, component B contains or consists of a mixture of at least two poly(tetramethylene glycol)polyether polyols, wherein the at least two poly(tetramethylene glycol)polyether polyols differ in their number-average molecular weights. Preferably, component B comprises a mixture of poly(tetramethylene glycol)polyether polyols I with a number-average molecular weight M n in the range of ≥ 400 and ≤ 1500 g / mol, particularly preferably in the range of ≥ 600 and ≤ 1200 g / mol, most preferably in the range of 1000 g / mol and poly(tetramethylene glycol)polyether polyols II with a number-average molecular weight M n in the range of ≥ 1500 and ≤ 8000 g / mol, particularly preferably in the range of ≥ 1800 and ≤ 3000 g / mol, most preferably 2000 g / mol.
[0223] The weight ratio of the poly(tetramethylene glycol)polyether polyols I to the poly(tetramethylene glycol)polyether polyols II is preferably in the range of 0.1 to 10, particularly preferably in the range of 0.2 to 10, and most preferably in the range of 1 to 6.
[0224] In a preferred embodiment of the foamed article, component D comprises nonionically hydrophilizing components D1. Preferably, nonionically hydrophilizing components D1 are nonionically monofunctional mixed polyalkylene oxide polyethers, comprising 40 to 100 mol% ethylene oxide and 0 to 60 mol% propylene oxide units, as previously described.
[0225] In a preferred embodiment of the foamed article, component H is used and the molar ratio of component G to component H is 5:1 to 1:5, or preferably 4.5:1 to 1:4.5, or preferably 4:1 to 1:4.
[0226] In a preferred embodiment of the foamed article, the polyurethane dispersion (B) is obtained by producing isocyanate-functional polyurethane prepolymers a) from components A., B. and optionally D. and / or C2., as well as optionally compounds E. and / or H., and subsequently reacting their free NCO groups wholly or partially with the amino-functional chain extender component C., as well as component G. and optionally components D. and H.
[0227] Another object of the invention is a method for producing a foamed article according to the invention, wherein the method comprises at least the following steps: (V1) Mixing the polyurethane dispersion (A) and the polyurethane dispersion (B) to obtain a mixture (M1), (V2) optionally adding to (M1) at least one surfactant, such as a foam stabilizer, preferably non-cytotoxic, (V3) optionally adding to (M1) at least one surfactant (liquid / liquid or liquid / air), preferably non-cytotoxic, (V4) optionally adding to (M1) a thickener, preferably an associative PU thickener, preferably non-cytotoxic, (V5) foaming the mixture (M1) to form a foam, preferably by introducing air into the mixture (M1), (V6) optionally ripening the foam from step (V2), (V7) optionally applying the foam formed in step (V5) or (V6) to a substrate, (V8) drying the foam to form the foamed article.
[0228] The mixing of dispersions (A) and (B) in step (V1) can be carried out with any device and in any conceivable manner that a person skilled in the art would use to homogeneously mix polyurethane dispersions to obtain a mixture (M1). Preferably, the mixing in step (V1) is carried out in a stainless steel container. The mixing in step (V1) preferably takes place over a period of time in the range of 30 seconds to 60 minutes, or more preferably in the range of 1 to 30 minutes.
[0229] The optional addition of at least one surface-active substance, such as a foam stabilizer in step (V2), as well as optionally a surfactant in step (V3) and optionally a thickener in step (V4), can be carried out by any means and in any manner that the person skilled in the art would choose for adding such additives as have already been described previously for the foamed article according to the invention to polyurethane dispersions and mixtures thereof.
[0230] Preferably, the addition of the at least one surface-active substance in step (V2) is carried out by adding this substance to one or both of the dispersions (A) or (B) before step (V1). Similarly, the optional addition of the surfactant (V3) and the optional addition of the thickener in step (V4) can be carried out in one or both of the dispersions (A) or (B) before step (V1).
[0231] Alternatively or additionally, the addition of at least one surfactant or the surfactant (V3) and the optional addition of the thickener (V4) can take place during mixing in step (V1) or after mixing in step (V1). Several surfactants and / or several surfactants and / or several thickeners can also be introduced into the mixture from (V1) in steps (V2), (V3) and / or (V4).
[0232] Preferably, the surfactants are selected from the group of additives previously described for the foamed article according to the invention. The amounts of these surfactants used are also preferably in the ranges described above for the foamed article according to the invention.
[0233] Preferably, the surfactants are selected from the group of additives as previously described for the foamed article according to the invention. The amounts of these surfactants used are also preferably in the ranges described above for the foamed article according to the invention.
[0234] Preferably, the thickeners are selected from the group of additives previously described for the foamed article according to the invention. The amounts of these thickeners used are also preferably within the ranges described above for the foamed article according to the invention.
[0235] After completing steps (V1) and optionally (V2), V3, and / or (V4), the mixture (M1) is foamed in step (V5). This is preferably done by introducing air into the mixture (M1). This is typically achieved by vigorous stirring or whipping of the mixture (analogous to the production of whipped cream). In mixing units, a mixing blade is preferably used, and an air pressure in the range of 3 to 10 bar, preferably 4 to 8 bar, is applied. The foam formed in step (V5) is then allowed to mature for a suitable period of time in step (V6). A suitable maturation period is preferably in the range of 1 second to 60 minutes, or more preferably in the range of 5 seconds to 30 minutes, or more preferably 1 to 10 minutes.The ripening process in step (V6) is preferably carried out at room temperature, preferably at 23 °C, or preferably at an elevated temperature, preferably in the range of 25 to 50 °C, or preferably from 30 to 40 °C. The ripening process in step (V6), in which the foam acquires its final properties, is preferably carried out in the same container in which the mixing in step (V1) and the foaming in step (V5) also take place. Alternatively, the ripening process in step (V6) can also be achieved via a longer connecting hose from the mixer to the application unit before the mixture (M1) is applied to a substrate. Such a measure ensures a continuous process in the mixer and during application. A combination of both process steps (V6) and (V7) is also possible.
[0236] The substrate onto which the foam can optionally be applied in step (V7) can comprise any material that a person skilled in the art would use as a coating substrate for a foam from step (V5). Preferably, the substrate is selected from the group consisting of a paper, for example, a release paper; a belt, for example, a conveyor belt made of rubber or a polymer; a metal; a wood surface; a nonwoven fabric; a stone surface; a polymer surface; or a glass surface; and a combination of at least two of these. Preferably, a release paper, a film, or a nonwoven fabric is used.
[0237] After foaming in step (V5) and optionally also after maturing in step (V6) and / or application to a substrate in step (V7), the foam is dried in step (V8). Drying in step (V8) preferably takes place on the substrate from step (V7). For particularly effective drying, the foam is applied to the substrate with a metal squeegee to a layer thickness of 100 µm to 10 mm, preferably 300 µm to 7 mm, and most preferably 1 to 5 mm. The drying process can preferably take place at an elevated temperature, preferably in the range of 50 to 130 °C, or more preferably from 60 to 100 °C. Typically, a rising temperature ramp is used on a coating system with different oven zones. The foam is preferably dried for a period of 1 to 60 minutes, or for a period of 10 to 50 minutes, or more preferably for a period of 3 to 10 minutes.To accelerate the drying process, for example, air heated to the temperature mentioned above can be passed over the foam, or a microwave oven or an infrared heater can be used. The foam preferably has a water content of 0 to 3 wt.%, or more preferably 0.2 to 2 wt.%, after step (V8). The foam dried in this way constitutes the foamed article according to the invention.
[0238] Another object of the invention is the use of the foamed article according to the invention or of a foamed article produced according to the inventive method as a wound dressing, as a hygiene article or as a wearable patch.
[0239] A further object of the invention is a kit of parts, comprising at least a polyurethane dispersion (A) as described above and a polyurethane dispersion (B) as described above, wherein the polyurethane dispersion (A) or the polyurethane dispersion (B) comprises an additive material (C), wherein the dispersion (A) or (B) comprising the additive material (C) exhibits a cell viability of ≥ 70%, preferably ≥ 75%, or preferably ≥ 80%, in a cytotoxicity test according to DIN ISO 10993-5:2009-10. Measurement methods Thickness measurement:
[0240] The layer thickness was determined using a pneumatic probe and a display from Heidehain (MT25P) connected to output the layer thickness. Density measurement:
[0241] To determine the density, a sample piece with dimensions of 5 × 5 cm² (with rounded corners, where the corners have a radius of 3 mm) was punched out using a die. The height was determined from the average of five measurements taken using the thickness measurement method described above. To subsequently calculate the density, the mass of the sample piece was determined using a Mettler Toledo XS603S balance, and together with the determined volume of the sample piece, the density [g / l] of the sample piece could be calculated. Crack area:
[0242] To determine crack areas in a foam, the surface of a foam sample measuring approximately 100 cm² was scanned using a flatbed scanner (Epson Perfection V370). For very light-colored foams, the scan was performed with the lid open to highlight the contrast differences more clearly. For dark foams, the scan was performed with the lid closed to create a white background for contrast. To ensure the cracks were adequately illuminated during scanning, the foam thickness ranged from 0.1 to 5 mm. The scan was then binarized using the software ImageJ (Standard Binarization -> Image - Adjust - Threshold - Default (0, 172)). This means that areas above a grayscale threshold, set to a value greater than 0.172, were classified as part of a crack, while areas below 0.172 were classified as smooth.To prevent even small pores from being detected as cracks, the threshold for the base area of a crack was set to > 0.4 mm². To calculate the percentage of the crack area, the detected crack area was compared to the total area. Crack width:
[0243] To determine the crack area of a foam, the surface of the foam sample, with an area of approximately 100 cm², was scanned using a flatbed scanner (Epson Perfection V370). Areas containing cracks were then identified based on the grayscale threshold value, as described above, and the crack width was measured every 2 mm along the crack length using the ImageJ software. Finally, the average of the measured values along the crack was calculated. Crack depth:
[0244] The layer thickness was measured as described above using a pneumatic probe with a tip that has a diameter of 3.5 mm. For cracks with a width of less than 3.5 mm, one side of the crack was cut off before measurement so that one flank was accessible for measuring the crack depth with the pneumatic probe. Pore size:
[0245] The determination of the mean pore size in the foam cross-section was carried out in accordance with the scientific article "Methods for Cell Structure Analysis of Polyurethane Foams" (Polyurethanes Expo; 2005; pages 453-465; Landers, R., Venzmer J., Boinowitz, T.). The following modifications were made for the determination of the pore size: Scanner type: Epson Perfection V39, resolution: 9600 dpi, 8-bit grayscale, Edding 390 black ink pen, software: ImageJ version 1.51n, plugin MorpholibJ. Example 1: Production of the polyurethane dispersion (A)
[0246] 1077.2 g of PolyTHF® < 2000, 409.7 g of PolyTHF® < 1000, 830.9 g of Desmophen® < C2200 and 48.3 g of polyether LB 25 were heated to 70 °C in a standard stirring apparatus. Subsequently, at 70 °C, a mixture of 258.7 g of hexamethylene diisocyanate and 341.9 g of isophorone diisocyanate was added over 5 min and stirred at 120 °C until the theoretical NCO value was reached or slightly below. The finished prepolymer was dissolved in 4840 g of acetone and cooled to 50 °C. A solution of 27.4 g of ethylenediamine, 127.1 g of isophoronediamine, 67.3 g of diaminosulfonate, and 1200 g of water was then added over 10 minutes. The mixture was stirred for 10 minutes. Dispersal was then achieved by adding 654 g of water. The solvent was subsequently removed by vacuum distillation.
[0247] The resulting polyurethane dispersion had the following properties: Solid content: 61,6 % Particle size (LKS): 528 nm pH (23°C): 7,5 Example 2: Production of the polyurethane dispersion (B)
[0248] 75 g of PolyTHF® < 1000 and 350 g of PolyTHF® < 2000 were heated to 70°C. A mixture of 33.9 g hexamethylene diisocyanate, 49.7 g isophorone diisocyanate, and 8.7 g Desmodur N 3300 (HDI trimerisate with an NCO content of approximately 21.8% according to DIN EN ISO 11909) was then added and stirred at 100–115°C until the theoretical NCO value was reached. The finished prepolymer was dissolved in 920 g acetone at 50°C, and then a solution of 3.2 g ethylenediamine, 12.9 g diaminosulfonate, 11.7 g diethanolamine, and 145 g water was added. The stirring time was 15 minutes. Afterwards, the mixture was dispersed by adding 1080 g of water. The solvent was then removed by vacuum distillation, resulting in a storage-stable dispersion; the solids content was adjusted by adding more water. Solid content: 52 % Particle size (LKS): 307 nm Viscosity: 105 mPa s Tg polyurethane urea: -78,0 °C Thermoplastic foam made from two special polyurethane dispersions (examples)
[0249] All foams described here are white and contain no dyes or pigments. Production of polyurethane foam (comparative example 1):
[0250] 2 kg of the aqueous polyurethane dispersion (A) described above were mixed with 0.155 kg of a 40 wt% aqueous Pluronic PE6800 solution (BASF SE, Germany) containing 3.45 wt% citric acid (Bernd Kraft, Germany) using a disperser from VMA-Getzmann GmbH. The mixture was then whipped into a foam with a density of 200 g / l in a Pico-Mix from Hansa-Mixer. The whipped foam was poured onto a 30 cm wide polyolefin-coated release paper (Felix Schoeller Y05200) with a doctor blade setting of 3000 µm. This foam was dried at 120°C for 30 minutes. Table 1: Foam properties of comparison example 1 Parameter: Unit Result: thickness mm 1,1 Foam density (dry) g / L 222 cracked area % 5,3 Crack width mean mm 2,46 Standard deviation mm 1,44 Lowest value mm 0,54 Greatest value mm 7,97 Crack depth mean mm 0,39 Standard deviation mm 0,12 Viability % 75 Fracture stress kPa 1095 Elongation at break % 239 Medium pore size µm 427 Production of polyurethane foam (comparative example 2):
[0251] 4.5 kg of the aqueous polyurethane dispersion (A) described above were mixed with 0.349 kg of a 40 wt% aqueous Pluronic PE6800 solution (BASF SE, Germany) containing 3.45 wt% citric acid (Bernd Kraft, Germany) and 0.225 kg of Niax L6889 (Momentive Performance Materials Inc., USA) using a disperser from VMA-Getzmann GmbH. The mixture was then whipped into a foam with a density of 200 g / l in a Pico-Mix from Hansa-Mixer. The whipped foam was poured onto a 30 cm wide polyolefin-coated release paper (Felix Schoeller Y05200) with a doctor blade setting of 3000 µm. The foam was dried at 130 to 140 °C for 7 minutes. Table 2: Foam properties of comparison example 2 Parameter: Unit Result: thickness mm 2,4 Foam density (dry) g / L 128 cracked area % - Crack width mean mm - Standard deviation mm - Lowest value mm - Greatest value mm - Crack depth mean mm - Standard deviation mm - Viability % 18 Fracture stress kPa 334 Elongation at break % 208 Medium pore size µm 431 Production of the polyurethane foam (example according to the invention 1):
[0252] 3.19 kg of the aqueous polyurethane dispersion (A) described above were mixed with 1.367 kg of polyurethane dispersion (B), consisting of 0.91 kg of a 10 wt% aqueous Rheolate 208 dispersion (Elementis Specialties, Germany) and 0.353 kg of a 40 wt% aqueous Pluronic PE6800 solution (BASF SE, Germany) containing 3.45 wt% citric acid (Bernd Kraft, Germany), using a dispersant from VMA-Getzmann GmbH. The mixture was then whipped to a foam with a density of 200 g / l in a Pico-Mix from Hansa-Mixer. The whipped foam was poured onto a 30 cm wide polyolefin-coated release paper (Felix Schoeller Y05200) with a doctor blade setting of 3000 µm. The foam was then dried at 130 to 140 °C for 7 minutes. Table 3: Foam properties of example 1 according to the invention Parameter: Unit Result: thickness mm 1,8 Foam density (dry) g / L 159 cracked area % 0,0 Crack width mean mm - Standard deviation mm - Lowest value mm - Greatest value mm - Crack depth mean mm - Standard deviation mm - Viability % 85 Fracture stress kPa 377 Elongation at break % 248 Medium pore size µm 467
[0253] No detectable cracks were found in the foam produced according to Example 1 of the invention; therefore, no information on crack width and crack depth is provided in Table 3. Furthermore, a comparison of the results from Tables 1 to 3 shows that the inventive mixture of dispersions (A) and (B) yields a foamed article that is free of cracks yet exhibits high viability. The foamed articles according to the comparative examples either exhibit low viability or cracks.
Claims
1. Foamed article produced by mixing a first polyurethane dispersion (A) with at least one second polyurethane dispersion (B), optionally with addition of further additives, foaming and subsequently drying the mixture, wherein the polyurethane dispersion (A) is obtainable by preparing A) isocyanate-functional prepolymers from A1) organic polyisocyanates A2) polymeric polyols having number-average molecular weights of 400 to 8000 g / mol and OH functionalities of 1.5 to 6 and A3) optionally hydroxyl-functional compounds having molecular weights of 62 to 399 g / mol and A4) optionally isocyanate-reactive, anionic or potentially anionic and optionally nonionic hydrophilizing agents, and B) the free NCO groups thereof are then wholly or partly reacted B1) optionally with amino-functional compounds having molecular weights of 32 to 400 g / mol and B2) with amino-functional, anionic or potentially anionic hydrophilizing agents by chain extension and the prepolymers are dispersed in water before, during or after step B), and wherein the second polyurethane dispersion (B) is obtainable by reactive conversion of at least the following components: A. an aliphatic polyisocyanate component having an average isocyanate functionality of ≥ 1.8 and ≤ 2.6, B. a polymeric polyether polyol component; C. an amino-functional chain extender component having at least 2 isocyanate-reactive amino groups, comprising at least one amino-functional compound C1. that does not have any ionic or ionogenic groups and / or an amino-functional compound C2. that has ionic or ionogenic groups, D. optionally further hydrophilizing components other than C2., E. optionally hydroxyl-functional compounds having a molecular weight of 62 to 399 mol / g, F. optionally further polymeric polyols other than B. , G. a compound having exactly one isocyanate-reactive group or a compound having more than one isocyanate-reactive group where only one of the isocyanate-reactive groups reacts with the isocyanate groups present in the reaction mixture under the reaction conditions chosen, and H. optionally an aliphatic polyisocyanate component having an average isocyanate functionality of > 2.6 and ≤ 4, where components B. and F. together contain ≤ 30% by weight of component F., based on the total mass of components B. and F..
2. Foamed article according to Claim 1, wherein the foamed article has at least one, preferably at least two, or preferably all, of the following properties i. to xiii.: i. the foamed article has no cracks having a width of ≥ 2 mm, preferably of ≥ 1 mm, more preferably of ≥ 0.5 mm, especially preferably of ≥ 0.1 mm; ii. the foamed article has no surface cracks deeper than 0.4 mm, preferably deeper than 0.2 mm or preferably deeper than 0.1 mm; iii. the foamed article has a crack area of ≤ 6%, preferably ≤ 3% or preferably ≤ 0.5%, based on the total area of the foamed article; iv. the foamed article has a cell viability of ≥ 70% or a classification of 0 to 2 in a cytotoxicity test to DIN ISO 10993-5:2009-10; v. the foamed article has a density within a range from 80 to 500 g / l, preferably 100 to 400 g / l, or preferably 120 to 300 g / l; vi. the foamed article has a thickness (D) within a range from 0.1 to 100 mm, preferably within a range from 0.5 to 50 mm, preferably within a range from 1 to 10 mm; vii. the foamed article has a tensile stress at break within a range from 100 to 1100 kPa, preferably within a range from 200 to 500 kPa, measured to DIN EN ISO 527-2:2012-06; viii. the foamed article has an elongation at break within a range from 100% to 500%, preferably within a range from 150% to 400%, measured to DIN EN ISO 527-2: 2012-06; ix. the polyurethaneurea formed from the polyurethane dispersion (B) is amorphous and has a Tg ≤ - 25°C, preferably ≤ -40°C, or preferably ≤ -50°C, or preferably ≤ -70°C, determined by means of differential scanning calorimetry in accordance with DIN EN 61006, Method A; x. the foamed article has a melting or softening range of ≤ 180°C, preferably ≤ 150°C, at a maximum pressure of 4 bar and has full thermoplastic processibility within this range; xi. the foamed article has an average pore size within a range from 200 to 750 pm, preferably within a range from 300 to 600 µm; xii. the foamed article has an outer layer, preferably containing a thermoplastic polyurethane or a thermoplastic polyethylene, at least on one surface of the foamed article; xiii. the foamed article is part of a composite material.
3. Foamed article according to Claim 1 or 2, wherein the weight ratio of the polyurethane dispersion (A) to the polyurethane dispersion (B) is within a range from 1:1 to 5:1, based on the total mass of the masses of dispersions (A) and (B).
4. Foamed article according to any of the preceding claims, wherein a film formed from the dispersion (B) has a tensile strain at break of ≤ 5 MPa, preferably ≤ 3.5 MPa or preferably ≤ 2.5 MPa, combined with an elongation at break of ≥ 1750%, preferably ≥ 2000%.
5. Foamed article according to any of the preceding claims, wherein the hydrophilizing agents B2) used are hydrophilizing agents containing sulfone groups.
6. Foamed article according to any of the preceding claims, wherein the dispersion (A) has a solids content of polyurethane of 52% to 65% by weight, preferably 55% to 63% by weight, or preferably 57% to 62% by weight, based on the total mass of the dispersion (A).
7. Foamed article according to any of the preceding claims, wherein component A. or A1) is isophorone diisocyanate and / or hexamethylene diisocyanate.
8. Foamed article according to any of the preceding claims, wherein component B. comprises or consists of poly(tetramethylene glycol) polyether polyols.
9. Foamed article according to any of the preceding claims, wherein component B. comprises or consists of a mixture of at least two poly(tetramethylene glycol) polyether polyols, wherein the at least two poly(tetramethylene glycol) polyether polyols are of different number-average molecular weight.
10. Foamed article according to any of the preceding claims, characterized in that component D. comprises nonionically hydrophilizing components.
11. Foamed article according to any of the preceding claims, characterized in that component H. is used and the molar ratio of component G. to component H. is 5:1 to 1:5.
12. Foamed article according to any of the preceding claims, characterized in that the polyurethane dispersion (B) is obtainable by preparing isocyanate-functional polyurethane prepolymers a) from components A., B. and optionally D. and / or C2., and optionally compounds E. and / or H., and the free NCO groups thereof are then wholly or partly reacted with the amino-functional chain-extender component C., and also component G. and optionally components D. and H..
13. Process for producing a foamed article according to Claim 1, wherein the process comprises at least the following steps: (V1) mixing the polyurethane dispersion (A) and the polyurethane dispersion (B) to obtain a mixture (M1), (V2) optionally adding to (M1) at least one interface-active substance, such as a foam stabilizer, that is preferably non-cytotoxic, (V3) optionally adding to (M1) at least one surfactant that is preferably non-cytotoxic, (V4) optionally adding to (M1) a thickener, preferably an associative PU thickener, that is preferably non-cytotoxic, (V5) foaming the mixture (M1) to give a foam, preferably by introducing air into the mixture (M1), (V6) optionally maturing the foam from step (V2), (V7) optionally applying the foam formed in step (V2) or (V3) to a substrate, (V8) drying the foam to form the foamed article.
14. Use of the foamed article according to any of Claims 1 to 12 or produced according to Claim 13 as wound dressing, a hygiene article or a wearable patch.
15. Kit of parts at least including a polyurethane dispersion (A) as described in Claim 1 and a polyurethane dispersion (B) as described in Claim 1, wherein the polyurethane dispersion (A) or the polyurethane dispersion (B) includes an added material (C), wherein the dispersion (A) or (B) including the added material (C) has a cell viability of ≥ 70% in a cytotoxicity test or a classification of 0 to 2 according to DIN ISO 10993-5:2009-10.