METHOD FOR WELDING COATED STEEL SHEETS

DE502020009343D1Active Publication Date: 2024-10-10VOESTALPINE AUTOMOTIVE COMPONENTS LINZ GMBH & CO KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502020009343
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-26
Filing Date
2020-11-26
Publication Date
2024-10-10
Estimated Expiration
2040-11-26

AI Technical Summary

Technical Problem

Existing welding processes for coated steel sheets, particularly those with aluminum-silicon coatings, face challenges in achieving stable, reproducible weld seams with consistent mechanical properties due to the adverse effects of aluminum on martensite transformation and the complexity of system technology, leading to issues like brittleness, cracking, and poor corrosion protection.

Method used

A method involving a configuration of two laser beams that rotate around the weld pool, with a defined stirring effect and welding speed, using a filler wire with tailored chemistry to neutralize aluminum's effects, inhibit scale formation, and enhance high-temperature strength, ensuring homogeneous mixing and metallurgical bonding without removing the aluminum-silicon coating.

Benefits of technology

This approach results in reliable, reproducible weld seams with improved mechanical properties and high-temperature strength, preventing decarburization and scaling, and maintaining corrosion protection, even under poorer cooling conditions during hot forming.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a method for welding coated steel sheets according to the preamble of claim 1.

[0002] In automotive manufacturing, it is common practice to produce body parts from highly hardenable steel sheets to ensure sufficient stability of the passenger cell. High-strength steels offer the advantage that their high load-bearing capacity allows for reduced dimensions and therefore weight, thus saving fuel.

[0003] Examples of such high-strength steel grades are manganese-boron alloyed steels, such as the most commonly used steel for this purpose, 22MnB5.

[0004] These high-strength steel grades are processed using a method called press hardening, in which the steel is heated to such a high temperature that the originally ferritic-pearlitic structure is transformed into an austenitic microstructure. This high-temperature austenitic structure of the iron then allows it to be quenched at a rate exceeding the critical hardening rate, resulting in a martensitic microstructure. Due to the different carbon solubilities of austenite and martensite, this process leads to lattice distortion, enabling high hardness values ​​of over 1500 MPa. This hardening process has been known for a long time and is therefore frequently used.

[0005] In press hardening, there are basically two different ways to manufacture such components: the direct and the indirect method.

[0006] In the direct process, a flat blank is austenitized and then formed in a press hardening tool in one or more strokes and quenched. This process is relatively inexpensive, but does not always allow for the forming of highly complex geometries.

[0007] In the indirect process, a component is first cold-formed from a flat sheet, which also allows for complex geometries. The formed component is then austenitized and subsequently quenched in a press tool, typically without undergoing any further significant deformation. The forming tool thus has a contour corresponding to the already formed component and serves only for hardening.

[0008] Steel sheets used for press hardening can already be supplied as blanks with a corrosion protection coating. The most common corrosion protection coatings are zinc or zinc alloy coatings, or aluminum or aluminum alloy coatings.

[0009] Furthermore, it is known to use composite blanks, so-called tailored blanks, in which either different types of steel are welded together or the same types of steel, but with different thicknesses, are welded together.

[0010] Here too, coated starting circuit boards are of course possible, so that, for example, two sheets of 22MnB5 with different thicknesses and an aluminum-silicon coating can be welded together.

[0011] Particularly when welding aluminum-silicon coated sheets, it was observed that aluminum from the coating apparently migrates into the weld seam. This aluminum in the weld seam has a detrimental effect on martensitic transformation and martensite formation. Furthermore, aluminum causes the formation of intermetallic phases, which are relatively hard in themselves but also very brittle and can therefore serve as initiation points for cracking.

[0012] To circumvent the problem of welding tailored blanks, it is known to partially remove aluminium layers on both sides of a planned butt weld before welding, in order to prevent aluminium-silicon from penetrating the weld seam.

[0013] A disadvantage here is that in this case there is no corrosion protection in the area of ​​the weld seam, and especially during heating for the purpose of hardening, the weld seam and the edges bordering the weld seam can later become scaled and decarburized.

[0014] Furthermore, a disadvantage here is that these methods for removing the aluminum-silicon coatings represent an additional process step that is also not easy to control.

[0015] From DE 10 2012 111 118 B3, a method for laser welding one or more workpieces made of press-hardenable steel, in particular manganese-boron steel, is known, in which butt welding is performed and in which the workpiece(s) have a thickness of at least 1.8 mm and / or a thickness difference of at least 0.4 mm is created at the butt joint, wherein filler wire is fed into the molten pool generated by a laser beam during laser welding. To ensure that the weld seam can be reliably hardened to a martensitic microstructure during hot forming, this document provides for the addition of at least one alloying element from the group comprising manganese, chromium, molybdenum, silicon and / or nickel to the filler wire, which promotes the formation of austenite in the molten pool generated by the laser beam, wherein this alloying element has at least one alloying element with a thickness difference of at least 1.8 mm.0.1 percent greater mass fraction is present in the filler wire than in the press-hardenable steel of the workpiece(s).

[0016] German patent DE 10 2014 001 979 A1 discloses a method for laser welding one or more workpieces made of hardenable steel in a butt joint, wherein the steel is in particular a manganese-boron steel and the workpieces have a thickness between 0.5 and 1.8 mm and / or a thickness difference of between 0.2 and 0.4 mm occurs at the butt joint, wherein a filler wire is introduced into the weld pool during laser welding, the weld pool being generated exclusively by the single laser beam. To ensure that the weld seam can be reliably hardened to a martenstic microstructure during hot forming, the patent specifies that the filler wire contains at least one alloying element from the group comprising manganese, chromium, molybdenum, silicon and / or nickel, thus promoting the formation of austenite.

[0017] From EP 2 737 971 A1, a tailor-welded blank and a method for its production are known, wherein the sheet is produced by joining sheets of different thicknesses or compositions together, thereby reducing quality problems in the weld zone. Here too, a filler wire is used, which is designed so that no ferrite forms in the temperature range of 800 to 950°C. This method is said to be particularly suitable for AlSi-coated sheets, and this wire is also said to have a higher content of austenite-stabilizing elements, consisting in particular of carbon or manganese.

[0018] From EP 1 878 531 B1, a method for hybrid laser-arc welding of surface-coated metallic workpieces is known, wherein the surface coating is said to contain aluminum. The laser beam is to be combined with at least one arc, such that melting of the metal and welding of the part(s) is effected, and that at least one of the parts, prior to welding, has deposits of the aluminum-silicon coating on one of its lateral cut surfaces to be welded.

[0019] From EP 2 942 143 B1, a method for joining two blanks is known, wherein the blanks are steel sheets with a coating comprising a layer of aluminum or an aluminum alloy, wherein the two parts are welded together using a laser beam and an electric arc, wherein the arc torch comprises a flux-cored electrode and the flux-cored electrode comprises stabilizing elements made of a steel alloy, wherein the laser and the arc are moved in a welding direction, wherein the arc welding torch and the laser beam are arranged downstream in the welding direction.

[0020] From EP 2 883 646 B1 a method for joining two blanks is known, wherein at least one of the blanks comprises a layer of aluminium or an aluminium alloy, wherein a metal powder is introduced into the welding zone during the welding process and the metal powder is an iron-based powder comprising gamma-stabilizing elements and the laser beam welding is a two-point laser beam welding.

[0021] From EP 2 007 545 B1, a method for producing a welded part with very good mechanical properties is known, wherein a steel sheet has a coating consisting of an intermetallic layer and a metal alloy layer located on the intermetallic layer. For the purpose of welding the sheets, the metal alloy layer on the intermetallic layer, which is an aluminum alloy layer, is to be removed at the periphery of the sheet, i.e., the areas to be welded. This coating is to be removed by a laser beam so that this layer, which forms an aluminum-silicon layer, is vaporized before welding in order to avoid harmful effects of the aluminum in the weld seam. At the same time, the intermetallic layer is to remain in place to potentially provide corrosion-inhibiting effects.

[0022] From WO 2017 / 103149 A1, a welding process is known in which two separately generated laser beams are guided along a planned weld seam. The first laser beam serves to melt a filler wire, while the second laser, through a rotating motion, ensures mixing of the weld pool. This is intended to ensure both the melting and the mixing of the filler material. Furthermore, a process is disclosed in which a leading laser beam is generated to melt the filler wire, while a lagging laser beam is split into two laser beams that are guided one after the other along the weld seam. It is stated that in this case, no movement of these laser beams is required.

[0023] From WO 2019 / 030249 A1 a welding process is known in which two aluminium-silicon coated sheets are joined together by means of a laser, wherein this laser rotates to mix a weld pool during the welding process.

[0024] The disadvantage of WO 2017 / 103149 A1 is that the plant technology is extremely complex, and it has been found that the specified serial double focus with wire does not provide sufficient homogenization.

[0025] From DE 10 2017 120 051 A1, a method for laser beam welding of one or more steel sheets made of press-hardenable manganese-boron steel is known, in which at least one of the steel sheets has an aluminum coating, wherein the laser beam welding is carried out by feeding a filler wire into the weld pool, which is generated exclusively by a laser beam. The filler wire is to contain at least one austenite-stabilizing alloying element. The aim of the method is to achieve, with relatively low energy consumption and high productivity, that the weld seam after hot forming has a strength comparable to that of the base material. For this purpose, it is proposed that the laser beam be set into oscillation such that it oscillates transversely to the welding direction, wherein the oscillation frequency of the laser beam is at least 200 Hz, preferably at least 500 Hz.This is intended to eliminate, in particular, the need to remove the aluminium coating from the edge of the sheet metal edges to be welded.

[0026] From JP 2004 000 1084 a welding process is known in which a laser welding process and an arc welding process are combined to improve gap bridging and depth welding, whereby it is possible to design the laser as a laser with two beams, wherein the welding device provides for the two beams to rotate around each other.

[0027] From DE 10 2014 107 716 B3 a welding process is known in which, to reduce weld spatter during welding, the laser beam that performs the welding is superimposed with a spatially oscillating movement during the feed movement, wherein the oscillating movement is carried out parallel or perpendicular to the joint.

[0028] A disadvantage of the aforementioned methods is that, in practice, stable load-bearing welds cannot be reliably achieved, and for inexplicable reasons, large differences in the final strength of the welds are repeatedly observed.

[0029] The object of the invention is to make a welding process more reliable and to produce welds with reproducible mechanical properties.

[0030] The problem is solved by a method having the features of claim 1.

[0031] Advantageous further training courses are indicated in the dependent sub-claims.

[0032] According to the invention, it was found that in processes in which a laser beam melts the wire while two lagging laser beams introduce additional energy into the melt pool, the welds repeatedly exhibit very different properties for unexplained reasons.

[0033] In a process where a single laser stirs but wire is used, it was found according to the invention that even with optimal mixing of the aluminum from the coating in the melt pool, there is theoretically so much aluminum available that the welds, especially with thin sheet thicknesses, cannot be sufficiently hardened. Furthermore, it was found that oscillating single-spot lasers are clearly not capable of ensuring consistent weld quality.

[0034] According to the invention, the naturally occurring melt pool flow is superimposed by an additional forced flow, which is generated by the rotation of a double laser beam, in order to distribute the filler wire and the aluminum from the coating homogeneously in the weld seam.

[0035] According to the invention, it was recognized that there is a relationship between the rotation frequency and the welding speed, without which a desired stirring effect cannot be achieved.

[0036] Furthermore, it has been shown that it is advantageous to define both the spot diameter and the spot distance in order to further improve the desired effects.

[0037] According to the invention, at least two laser beams, in particular two partial laser beams, are provided which rotate in the weld pool. The welding lasers can, for example, rotate symmetrically around the center of the weld pool or rotate asymmetrically around the center of the weld pool, wherein one welding beam or laser beam rotates in a smaller radius around the center of the weld pool, while a second welding beam or laser beam rotates in a larger radius around the center of the weld pool.

[0038] In another possible embodiment, a laser beam moves along the center of the weld pool, while a second welding beam or laser beam orbitally oscillates or rotates around the first welding beam. According to the invention, it has been found that the feed rate and the stirring action must be precisely coordinated. An incorrect combination of feed rate and stirring action can lead to negative effects such as humping, excessive spatter formation, and even weld penetration. Insufficient feed rate can negatively impact the process's efficiency. The stirring action is defined here as the number of revolutions achieved by the feed.

[0039] In addition to the homogenization of the weld pool by physical means according to the invention, the sheets to be coated are also welded together metallurgically without completely or partially removing the respective aluminum-silicon layer, whereby the negative influence of the aluminum on the mechanical properties of the weld joint is neutralized by the use of filler material. Furthermore, according to the invention, decarburization and scaling of the weld are prevented, the hot strength of the weld is increased, and the weld is also made suitable for subsequent hot forming processes in such a way that the poorer cooling conditions prevailing at the weld due to the tooling are compensated for.

[0040] For the metallurgical neutralization of aluminum or its negative effects according to the invention, welding is carried out with a special filler material whose chemistry or alloy composition is specifically designed to counteract the effects of the aluminum. The filler material can be powder, wire, or a combination thereof. A welding wire is preferably chosen as the filler material because it can offer process-related advantages with regard to handling and feeding.

[0041] In particular, the welding wire has a defined chromium content that strongly inhibits scale formation and edge decarburization.

[0042] Accordingly, unlike the state of the art, no gamma stabilization is performed; instead, welding is carried out with low levels of nickel and manganese. Surprisingly, it has been found that a high-strength weld is still produced.

[0043] This makes it possible to weld without ablation and to suppress the negative influence of aluminum on the mechanical properties of the weld joint, while also virtually avoiding decarburization and scaling of the weld seam and increasing its hot strength. This is achieved, among other things, by welding with a higher chromium content, which improves hardenability. This is important because, according to the invention, it was recognized that during the hot forming process, tool-related factors often result in poorer cooling conditions at the weld seam, which is reflected in a decrease in the weld's hardness after the press hardening process.

[0044] Overall, the use of a filler wire specifically matched to the material largely neutralizes the aluminum, and the chromium content in the weld seam strongly inhibits scale formation and decarburization. A suitable filler wire has a carbon content of 0.80 to 2.28 times the carbon content of the base material, preferably 0.88 to 1.51 times the carbon content of the base material, particularly preferably 0.90 to 1.26 times the carbon content of the base material, and even more preferably 0.90 to 1.17 times the carbon content of the base material, with a chromium content of 8 to 20%, a nickel content of less than 5%, preferably less than 1%, a silicon content of 0.2 to 3%, a manganese content of 0.2 to 1%, and optionally a molybdenum content of up to 2%, preferably 0.5 to 2%.

[0045] When welding with such an additional wire, it is possible to strongly inhibit scale formation and edge decarburization during the subsequent hardening process and to "neutralize" the effect of the aluminum from the description.

[0046] The invention thus relates to a method for welding coated steel sheets, in particular steel sheets coated with an aluminum-silicon metallic coating layer, wherein a configuration of two laser beams is present, wherein the laser beams act on a weld pool to be formed, wherein at least one laser beam rotates about an axis of rotation so that the laser beams perform a relative movement to each other, wherein the laser beams are guided along a welding axis, wherein, for the purpose of welding pool mixing, a defined stirring effect and a defined welding speed are maintained in relation to each other, wherein the following applies to the stirring effect: η = frot Vw , where f rot is the rotation frequency and vw is the welding speed and where: 4 ≤ η ≤ 120 Vw 1 mm 4 ≤ η ≤ 120 Vw 1 mm 4 ≤ Vw ≤ 14 m min where a welding filler wire is used when welding the sheets, the welding filler wire consisting of the following composition: C= 0.80 - 2.28 × %C Base material Cr= 8 - 20% Ni< 5% Si= 0,2 - 3% Mn= 0,2 - 1% Optional Mo< 2% Optional V and / or W in total < 1% Residual iron and unavoidable impurities resulting from smelting, all values ​​given in mass %.

[0047] In a further embodiment of the invention, the laser beams are arranged symmetrically around an axis of rotation and rotate diametrically opposite each other around the axis of rotation, or one laser beam is guided along a welding axis and the other welding beam rotates around the first laser beam, or a first laser beam rotates with a first smaller radius around the axis of rotation while the second laser beam rotates with a larger radius around the axis of rotation (5), or a mixture of these forms of movement.

[0048] In one embodiment, with a symmetrical rotation of the laser beams or their projection surfaces or spots, the laser beams are each spaced apart from the center by the spot distance X df, wherein the spot diameter or diameter of the laser beam df is 0.1 mm to 1 mm, wherein the total overlap width of the laser beams is the distance between the spot centers plus a spot diameter, the amount being between 0.5 mm and 2.5 mm.

[0049] In this embodiment, it is particularly advantageous if the following applies to the spot spacing X df. X df ≥ 0,8 ∗ d f .

[0050] In another embodiment, in a laser beam configuration, two laser beams are arranged orbitally, wherein a first laser beam remains along the welding progress direction on a central axis of the weld pool, namely the welding axis, while the second laser beam or second spot rotates around a rotation axis (5), wherein the rotation axis (5) lies on the welding axis (4) or oscillates around the welding axis (4) and represents the center point of the first spot (2).

[0051] In this embodiment, it is particularly advantageous if the spot diameter is between 0.1 and 1 mm, whereby: X df ≥ 0,8 ∗ d f und 0,45 mm ≤ x df + d f 2 ≤ 1,5 mm

[0052] In yet another embodiment, in a laser beam configuration, two laser beams or two laser spots rotate around a rotation axis, wherein a first laser beam or first laser spot rotates around the rotation axis with a first radius and the second laser beam or second laser spot rotates around the rotation axis with a second radius, one of the radii being larger than the other, wherein the following conditions apply: X df ≥ 0,8 ∗ d f 0,45 mm ≤ x df − xoff + d f 2 ≤ 1,5 mm 0 < xoff < x df 2

[0053] Where Xoff corresponds to the distance of the first laser beam from the axis of rotation and therefore defines the eccentricity of the laser beams to each other.

[0054] In the aforementioned embodiments, it is advantageous to weld with a laser power between 2 and 10 kW, in particular 3 to 8 kW, preferably 4 to 7 kW.

[0055] It is also advantageous if the stirring action η in mm -1< is between 4 and 30 mm -1<.

[0056] In another embodiment, the welding speed Vw is between 5 and 12, in particular 6 and 10 m / min.

[0057] The optimal process window for the stirring effect also depends on the welding speed V w .

[0058] It is advantageous to use a welding wire whose nickel content is less than 1% by mass.

[0059] It is also advantageous if the welding wire contains 0.5 to 2% molybdenum by mass.

[0060] Advantageously, gap widths of 0 to 0.3 mm, and in particular 0 to 0.2 mm, are set. Setting a "technical zero gap," i.e., sheets without any deliberate gap adjustment, can be particularly advantageous, as this can offer process-related benefits. In another embodiment, setting the gap to 0.2 mm can be advantageous for reducing the aluminum content in the weld.

[0061] Furthermore, it is advantageous if the carbon content of the filler wire is equal to C= 0.88 to 1.51 × C base material preferably C= 0.90 to 1.26 × C base material particularly preferably C= 0.90 to 1.17 × C base material is set.

[0062] Advantageously, the base material used is a boron-manganese steel which can be hardened to a tensile strength of greater than 900 MPa by an austenitizing and quenching process, and in particular a steel from the group of CMnB steels such as 22MnB5 or 20MnB8 is used.

[0063] It is particularly advantageous if the base material is a steel of the general alloy composition (in mass-%). Carbon (C) 0,03-0,6 Manganese (Mn) 0,3-3,0 Aluminum (Al) 0,01-0,07 Silicon (Si) 0,01-0,8 Chromium (Cr) 0,02-0,6 Nickel (Ni) <0,5 Titanium (Ti) 0,01-0,08 Niobium (Nb) <0,1 Nitrogen (N) < 0,02 Boron (B) < 0,02 Phosphorus (P) < 0,01 Sulfur (S) < 0,01 Molybdenum (Mo) < 1

[0064] Residual iron and impurities resulting from the smelting process are used.

[0065] Furthermore, a steel of the general alloy composition (in mass-%) can be advantageously used as the base material. Carbon (C) 0,03-0,36 Manganese (Mn) 0,3-2,00 Aluminum (Al) 0,03-0,06 Silicon (Si) 0,01-0,20 Chromium (Cr) 0,02-0,4 Nickel (Ni) <0,5 Titanium (Ti) 0,03-0,04 Niobium (Nb) <0,1 Nitrogen (N) < 0,007 Boron (B) < 0,006 Phosphorus (P) < 0,01 Sulfur (S) < 0,01 Molybdenum (Mo) < 1

[0066] Residual iron and impurities resulting from the smelting process are used.

[0067] It is also advantageous if the additional wire has a carbon content in the range of 0.024 to 1.086 wt%, particularly preferably 0.186 to 0.5082 wt%, and even more preferably between 0.20 and 0.257 wt%.

[0068] In one embodiment, it is advantageous if the steel sheets have a different alloy composition.

[0069] It is particularly advantageous if the aforementioned circuit board is subjected to hot forming or cold forming followed by press hardening.

[0070] The invention is explained by way of example with the aid of a drawing. The drawing shows: Figure 1: schematically depicts the symmetrical, asymmetrical, and orbital rotation of the welding laser beams; Figure 2: the process window according to the invention with respect to the stirring effect; Figure 3: the representation according to Figure 2with the significance of the outside areas; Figure 4: a table showing 16 different tests comparing embodiments according to the invention and those that are not; Figure 5: a representation of a symmetrical stirring arrangement with the functions of spot spacing and spot diameter relative to each other; Figure 6: the process window for a symmetrical stirring arrangement; Figure 7: a schematic representation of an orbital stirring arrangement with the functions of spot spacing and spot diameter; Figure 8: the process window of the orbital stirring arrangement; Figure 9: the representation of an asymmetrical stirring arrangement with the functions of spot spacing, spot diameter, and eccentricity; Figure 10: a hardened weld seam in a cross-sectional view according to test V1 in the table; Figure 11: a cross-sectional view according to test V2 in the table; Figure 12: a cross-sectional view of the weld seam according to test V4 in the table;Figure 13: A cross-sectional view of a weld seam according to test V16 as shown in the table.

[0071] In Figure 1 Three different, fundamentally possible and combinable laser beam configurations are shown, with the laser beam configurations shown being in a symmetrical configuration ( Fig. 1a ), the laser beams are arranged symmetrically to an axis of rotation and are rotated diametrically opposite each other around the axis of rotation.

[0072] The symmetrical configuration can advantageously achieve the highest stirring effect.

[0073] In an asymmetric arrangement ( Fig. 1b One laser beam is positioned closer to the axis of rotation than the other, thus creating an eccentricity. This asymmetrical arrangement advantageously allows for precise control over the desired weld geometry.

[0074] In the orbital arrangement ( Fig. 1c ) a central laser beam is present, which is moved along a welding progress direction, while the second laser beam rotates away from this one around it and the axis of rotation.

[0075] The orbital arrangement can advantageously compensate for any differences in sheet thickness.

[0076] In Figure 5 The symmetrical stirring arrangement is shown in more detail.

[0077] In this laser beam configuration 1, two laser beams 2, 3 are present, each located approximately equidistant from an idealized weld pool center 4. Preferably, the rotation axis 5 is also located at the ideal weld pool center 4, around which the two laser beams 2, 3 rotate according to the rotation directions 6, 7.

[0078] Accordingly, exemplary subsequent positions 2', 3' offset by 90° are shown. The laser beams 2, 3 and their projection area (spot) have a given diameter df corresponding to the extension arrows 8, 9.

[0079] The two laser beams 2 and 3, or rather their projection surfaces (spots), are each spaced apart from the center by the spot distance X df. The theoretical weld pool width is therefore the spot distance plus half the spot diameter.

[0080] The welding progress takes place along the idealized weld pool center 4 according to arrow 10 at a welding progress rate V w.

[0081] In this configuration of a symmetrical rotating arrangement, the spot diameter df is preferably located within a range of 0.1 to 1 mm.

[0082] The distance between the centers of the spots plus the spot diameter is preferably between 0.5 mm and 3 mm, in particular between 0.9 mm and 2.5 mm, where preferably for the spot spacing x df x df ≥ 0.8 * df.

[0083] A suitable process window for the symmetrical stirring arrangement regarding the relationship between spot spacing and diameter can be seen in Figure 6 As already stated, it is a general rule that the spot diameter df is between 0.1 and 1 mm.

[0084] In another advantageous laser beam configuration 11 ( Figure 7 ) two laser beams 2, 3 are arranged orbitally, which means that a first spot 2 remains on the welding axis 4 according to the welding progress direction 10, while a second spot 3 rotates around a rotation axis 5 which lies on the welding axis 4 and represents the center point of the first spot 2.

[0085] The rotation of the second spot 3 accordingly occurs along the rotation direction 7, which is arranged at a specific radius around the rotation axis 5. The different positions of the second laser spot 3 are described in Figure 7 The example shows the position rotated 180° to position 3'. However, complete rotations are performed during welding along the welding progress 10.

[0086] The welding axis 4 is also the idealized weld pool center 4.

[0087] In this advantageous embodiment, the spot diameter is also between 0.1 and 1 mm, whereby the following applies: 0,45 mm ≤ x df + d f 2 ≤ 1,5 mm

[0088] Here too, x df ≥ 0.8 * df . In Figure 8The process window for the orbital stirring arrangement, which is applicable according to the aforementioned framework conditions, is specified, wherein the function of the spot spacing is specified via the spot diameter in the process window and the corresponding area according to the invention is located within the closed area.

[0089] In a further advantageous embodiment of a laser beam configuration 1 (shown in Figure 9 ) Two laser spots 2, 3 rotate around a rotation axis 5, but a first rotation direction 6 of a first laser beam 2 or first laser spot 2 is arranged closer to the rotation axis than the second rotation direction 7 of the second laser beam 2. The spot spacing center is thus located away from or offset from the weld pool center 4.

[0090] In this advantageous embodiment, the spot diameter df is again between 0.1 and 1 mm, and the following condition is also met: X df ≥ 0,8 ∗ d f 0,45 mm ≤ x df − xoff + d f 2 ≤ 1,5 mm 0 < x off < xdf 2

[0091] In Figure 2 The process window according to the invention with respect to the stirring effect is illustrated. This shows Figure 3 the respective effects when carrying out the process with unsuitable parameters, i.e., parameters lying outside the process window.

[0092] Choosing an excessively high stirring action in combination with a high welding speed can lead to humping (unstable welding process), increased spattering, and even laser weld penetration.

[0093] Surprisingly, even with insufficient stirring, the tendency to splash can increase significantly.

[0094] A laser welding speed (vw ) of less than 4 m / min is technically possible but no longer economically viable.

[0095] In the table according to Figure 4 Sixteen welding tests are presented, performed with varying welding rates, stirring conditions, and power outputs. After hardening, the welds were inspected and classified according to weld homogeneity and process stability. "Nb" indicates that a stable weld could not be assessed, as no stable weld could be achieved in these tests.

[0096] In Figure 10 A weld structure after hardening is shown (example V1 from the table). Fig. 4) where the parameters according to the invention were not adhered to. The weld structure after hardening is already visually perceptible as inhomogeneous, with a welding progress rate of 6 m per minute. The spot diameter was 0.3 mm, but with a spot spacing of 0, which means that only a single laser was used. It is evident that a qualitatively satisfactory result cannot be achieved with this conventional method.

[0097] In Figure 11 is the result of an embodiment according to the invention (example V2 from the table from Fig. 4 ) can be seen, with the polished surface being homogeneous after hardening. The spot diameter was 0.3 mm, using a symmetrical stirring arrangement with a spot spacing of 0.9 mm.

[0098] The laser power was 4.3 kW, the welding progress speed was 6 m per minute. The stirring effect η was 4.125 mm -1< , where the stirring effect is the quotient of the rotation frequency and the welding speed or welding progress.

[0099] The distance from the center of the spot to the axis of rotation was 0.45 mm, which means that the spots orbited the axis of rotation on a radius.

[0100] In Figure 12 Experiment 4 is shown, which is not in accordance with the invention. While the spot diameter and spot spacing are within the range of the invention, as is the welding progress speed, which at 6 m per minute corresponds to that of experiment 2, and the distance of the spot center to the axis of rotation is also the same, the stirring effect, as the quotient of the rotation frequency and welding progress speed, is too low, so that the polished section after hardening shows a significant inhomogeneity.

[0101] In Figure 13 Figure 16 shows the result of the experiment according to the invention. It can be seen that a homogeneous weld structure is present. The spot spacing is 0.4 mm with a spot diameter of 0.3 mm, and the progress rate corresponded to that of the other experiments. The stirring effect η is 4.125 mm⁻¹, within the range specified by the invention, with the distance of the spot center to the axis of rotation being 0.2 mm.

[0102] The invention has the advantage that reliably homogeneous weld seams can be achieved when welding aluminium silicon coated sheets through a targeted selection of parameters and a corresponding process control.

[0103] According to the invention, the welding of two sheets of different thicknesses, preferably CMn steels, in particular a hardenable CMnB steel, especially 22MnB5 steel materials, is accomplished by using a welding filler wire. In particular, according to the invention, aluminum-silicon coated steel sheets with a tensile strength > 900 MPa after hardening are joined by welding without ablation.

[0104] The preferred chemical alloy of the filler wire or cored wire consists of the following elements: C= 0.80 - 2.28 × C base material Cr= 8 - 20% by mass Ni≤ 5, preferably ≤ 1 wt% Si= 0.2 - 3 mass % Mn= 0.2 - 1 mass % Optional Mo=< 2, preferably 0.5 - 2.5 wt% Optional V and / or W in total < 1% mass %

[0105] Residual iron and unavoidable impurities resulting from the smelting process

[0106] Preferably, the carbon of the filler wire is adjusted as follows, or the filler wire has the following composition: C= 0.88 to 1.51 × C base material Cr= 10 - 18% by mass Ni= ≤ 1 mass % Si= 0.3 - 1 mass % Mn= 0.4 - 1 mass % Mo= 0.5 - 1.3 mass % V = 0.1 - 0.5 mass % W= 0.1 - 0.5 mass %

[0107] Residual iron and unavoidable impurities resulting from the smelting process

[0108] Especially preferred: C= 0.90 to 1.26 × C base material

[0109] Even more especially preferred: C= 0.90 to 1.17 × C base material

[0110] As previously stated, the materials used are aluminum-silicon coated sheets with a coating thickness of 60 g / m² per side, made from 22MnB5. For tensile testing purposes, sheets with a thickness of 1.5 mm were joined. These sheets were prepared with weld edges and welded together using a Trumpf 4006 welding laser (4.4 kW) with a focal diameter of 0.6 mm.

[0111] The base material is a steel of the general alloy composition (in mass-%). Carbon (C) 0,03-0,6 Manganese (Mn) 0,3-3,0 Aluminum (Al) 0,01-0,07 Silicon (Si) 0,01-0,8 Chromium (Cr) 0,02-0,6 Nickel (Ni) <0,5 Titanium (Ti) 0,01-0,08 Niobium (Nb) <0,1 Nitrogen (N) < 0,02 Boron (B) 0,002-0,02 Phosphorus (P) < 0,01 Sulfur (S) < 0,01 Molybdenum (Mo) < 1

[0112] Residual iron and impurities resulting from the smelting process.

[0113] This means that the carbon content of the filler wire can range from 0.024 to 1.086 wt%.

[0114] In production, the carbon content of the filler wire is of course specifically selected based on the carbon content of the base material.

[0115] Preferably, the base material can have the following alloy composition: Carbon (C) 0,03-0,36 Manganese (Mn) 0,3-2,00 Aluminum (Al) 0,03-0,06 Silicon (Si) 0,01-0,20 Chromium (Cr) 0,02-0,4 Nickel (Ni) <0,5 Titanium (Ti) 0,03-0,04 Niobium (Nb) <0,1 Nitrogen (N) < 0,007 Boron (B) 0,002-0,006 Phosphorus (P) < 0,01 Sulfur (S) < 0,01 Molybdenum (Mo) < 1

[0116] Residual iron and impurities resulting from the smelting process.

[0117] Specifically, 22MnB5 can, for example, have the following composition: C=0.22 Si=0.19 Mn=1.22 P=0.0066 S=0.001 AI=0.053 Cr=0.26 Ti=0.031 B=0.0025 N=0.0042,

[0118] Residual iron and impurities resulting from smelting, all values ​​given in mass %.

[0119] With this specific composition of the base material, the carbon content of the filler wire can be in the range of 0.186 to 0.5082 wt% or, particularly preferably, between 0.216 and 0.257 wt%.

Claims

1. A method for welding coated steel sheets, particularly steel sheets that are coated with an aluminum-silicon-based metallic coating layer, wherein a configuration (1, 11, 12) of two laser beams (2, 3) is provided, wherein the laser beams act on a weld pool that is to be formed, wherein at least one laser beam (3) rotates around a rotation axis (5) so that the laser beams (2, 3) execute a movement relative to each other, wherein the laser beams (2, 3) are guided along a welding axis (4), wherein in order to achieve a mixing of the weld pool, a defined stirring effect and a defined welding speed in relation to each other are adhered to, wherein the following condition applies to the stirring effect: η = f rot v w where frot is the rotation frequency and vw is the welding speed and wherein the following conditions apply: 4 ≤ η ≤ 120 v w 1 mm 4 ≤ η ≤ 120 v w 4 ≤ v w ≤ 14 m min wherein in the welding of the sheets, a supplementary material, in particular welding filler wire, is used, wherein the supplementary material, in particular the welding filler wire, is of the following composition: C = 0.80 - 2.28 × % of the C in the base material Cr = 8 - 20% Ni < 5% Si = 0.2 - 3% Mn = 0.2 - 1% optionally Mo < 2% optionally V and / or W totaling < 1% residual iron and inevitable smelting-related impurities, all amounts expressed in % by mass.

2. The method according to claim 1, characterized in that the laser beams (2, 3) are positioned symmetrically around a rotation axis (5) and rotate around the rotation axis in diametrically opposed positions or one laser beam (2) is guided along a welding axis (4) and the other laser beam (3) rotates around the first laser beam (2) or a first laser beam (2) rotates with a first smaller radius around the rotation axis (5) while the second welding beam (3) rotates with a larger radius around the rotation axis (5) or a mixture of these forms of movement.

3. The method according to one of the preceding claims, characterized in that with a symmetrical rotation of the laser beams (2, 3) or more precisely of their projected areas or spots, the laser beams (2, 3) are each spaced apart from the center by the spot spacing xdf, wherein the spot diameter or the diameter of the laser beam df is 0.1 mm to 1 mm, wherein the total coverage width of the laser beams (2, 3) is the sum of the spacing of the spot centers from each other plus one spot diameter, wherein the total is between 0.5 mm and 2.5 mm.

4. The method according to claim 3, characterized in that for the spot spacing xdf, the following condition applies: xdf ≥ 0.8 * df.

5. The method according to claim 2, characterized in that in a laser beam configuration (11), two laser beams (2, 3) are positioned orbitally, wherein a first laser beam (3) remains along the weld advancing direction (10) on a central axis of the weld pool, namely the welding axis (4), while the second laser beam (3) or second spot (3) rotates around a rotation axis (5), wherein the rotation axis (5) lies on the welding axis (4) or oscillates around the welding axis (4) and constitutes the center point of the first spot (2).

6. The method according to claim 5, characterized in that the spot diameter is between 0.1 and 1 mm, wherein the following conditions apply: x df ≥ 0.8 * d f and 0.45 mm ≤ x df + d f 2 ≤ 1.5 mm7. The method according to claim 2, characterized in that in a laser beam configuration (12), two laser beams (2, 3) or two laser spots (2, 3) rotate around a rotation axis (5), wherein a first laser beam (2) or first laser spot (2) rotates with a first radius around the rotation axis (5) and the second laser beam (3) or second laser spot (3) rotates with a second radius around the rotation axis (5), wherein one of the radii is greater than the other, wherein the following conditions apply: 0.45 mm ≤ x df − x off + d f 2 ≤ 1.5 mm x df ≥ 0.8 * d f 0 < x off < x df 2 8. The method according to one of the preceding claims, characterized in that the welding is performed with a laser power of between 2 and 10 kW, in particular from 3 to 8 kW, and preferably from 4 to 7 kW.

9. The method according to one of the preceding claims, characterized in that the stirring effect η in mm-1 is between 4 and 30 mm-1.

10. The method according to one of the preceding claims, characterized in that the welding speed vw is between 5 and 12, in particular between 6 and 10 m / min.

11. The method according to claim 1, characterized in that a welding wire is used, whose nickel content is less than 1% by mass.

12. The method according to claim 1, characterized in that a molybdenum content of 0.5 to 2% by mass is present in the welding wire.

13. The method according to one of the preceding claims, characterized in that gap widths of 0 to 0.3 mm, in particular 0 to 0.1 mm, are set.

14. The method according to one of the preceding claims, characterized in that the carbon content of the filler wire is set to C = 0.88 to 1.51 × the C in the base material preferably C = 0.90 to 1.26 × the C in the base material particularly preferably C = 0.90 to 1.17 × the C in the base material.

15. The method according to one of the preceding claims, characterized in that a steel that is a boron-manganese steel is used as the base material, which can be hardened by means of an austenitization and quenching process, particularly preferably to a tensile strength of greater than 900 MPa and in particular, a steel is used that belongs to the group of CMnB steels, for example a 22MnB5 or 20MnB8 steel.

16. The method according to one of the preceding claims, characterized in that a steel of the following general alloy composition (in % by mass) is used as the base material: carbon (C)0.03-0.6manganese (Mn)0.3-3.0aluminum (Al)0.01-0.07silicon (Si)0.01-0.8chromium (Cr)0.02-0.6nickel (Ni)< 0.5titanium (Ti)0.01-0.08niobium (Nb)< 0.1nitrogen (N)< 0.02boron (B)< 0.02phosphorus (P)< 0.01sulfur (S)< 0.01molybdenum (Mo)< 1 residual iron and smelting-related impurities.

17. The method according to one of the preceding claims, characterized in that a steel of the following general alloy composition (in % by mass) is used as the base material: carbon (C)0.03-0.36manganese (Mn)0.3-2.00aluminum (Al)0.03-0.06silicon (Si)0.01-0.20chromium (Cr)0.02-0.4nickel (Ni)< 0.5titanium (Ti)0.03-0.04niobium (Nb)< 0.1nitrogen (N)< 0.007boron (B)< 0.006phosphorus (P)< 0.01sulfur (S)< 0.01molybdenum (Mo)< 1 residual iron and smelting-related impurities.

18. The method according to one of the preceding claims, characterized in that the filler wire has a carbon content in the range from 0.024 to 1.086% by mass, particularly preferably 0.186 to 0.5082% by mass, even more particularly preferably between 0.20 and 0.257% by mass.