Nickel base alloy for powder and method for producing a powder

DE502020009444D1Active Publication Date: 2024-10-31VDM METALS INTERNATIONAL GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502020009444
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-26
Filing Date
2020-07-01
Publication Date
2024-10-31
Estimated Expiration
2040-07-01

AI Technical Summary

Technical Problem

Current methods for producing nickel-based powders for additive manufacturing lack cost-effectiveness and do not adequately meet requirements for particle size distribution, shape, and processability, while also being inefficient in terms of operating time and powder quality.

Method used

A nickel-based alloy powder with specific composition and production process involving Vacuum Induction Melting (VIM) followed by Vacuum Inert Gas Atomization (VIGA) or Electrode Induction Gas Atomization (EIGA), optimizing particle size, shape, and porosity, and using a protective argon atmosphere to ensure low residual porosity and high bulk density.

Benefits of technology

The process produces powders with optimized particle size, shape, and porosity, enhancing the quality for additive manufacturing, reducing operating time, and achieving cost-effectiveness while maintaining the advantageous properties of Ni and Ni-Co alloys.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a nickel-based alloy for powder.

[0002] WO 2015 / 110668 A2 describes a process for producing iron-based powders which are atomized using a centrifuge, with the following process steps: providing an alloy having a melting point above 1040°C, melting the composition, atomizing the molten composition using a centrifuge or a rotating atomizing device.

[0003] DE 10 2015 016 729 A discloses a process for producing metallic semi-finished products from an alloy with more than 50% nickel, comprising the following process steps: an electrode is produced by VIM, the electrode is subjected to a heat treatment in a furnace in order to reduce stresses and overaging in the temperature range between 400 and 1250°C for a period of 10 to 336 hours, the electrode is cooled in air or in the furnace, depending on the dimension, in particular depending on the diameter, to a temperature between room temperature and less than 1250°C, in particular less than 900°C, the cooled electrode is then remelted by VAR at a remelting rate of 3.0 to 10 kg / minute to form a VAR ingot, the VAR ingot is heat treated in a furnace in the temperature range between 400 and 1250°C for a period of 10 to 336 hours, the VAR ingot is cooled in air or in the furnace, depending on the dimension, in particular depending on the diameter, to a temperature between room temperature and less than 1.250°C, in particular less than 900°C, cooled, the VAR block is remelted again at a remelting rate of 3.0 to 10 kg / minute, the remelted VAR block is subjected to heat treatment in the temperature range between 400 and 1250°C for a period of 10 to 336 hours, the VAR block is then brought to the desired product shape and dimensions by hot and / or cold forming.

[0004] US 3,802,938 discloses a process for producing a nickel-based alloy which may have the following composition: Cr 5.0-25%, Co 5.0-25%, Mo up to 12%, W up to 15%, Nb up to 4%, Ti 0.5-6%, Al 1-7%, B up to 0.4%, Zr up to 0.3%, Ta up to 12%, Hf up to 5%, Re up to 1%. The alloy may consist of powder that is deformed by pressure and subjected to heat treatment, with one powder component consisting of a largely carbon-free nickel-based superalloy and another component consisting of a powdered carbide.

[0005] It is well known that Ni and Ni-Co alloys are used to produce components with special properties regarding corrosion resistance and good mechanical properties, such as strength, heat resistance and fracture toughness.

[0006] DE 10 2013 018 006 A1 discloses a nickel-chromium-molybdenum alloy which (in wt%) 20 - 23 % chrome 10 - 13 % cobalt 8 - 10 % molybdenum 0,03 - 0,10 % carbon 0,8 - 1,5 % aluminum 0,2 - 0,50 % titanium 0,005 - 0,10 % zirconium 0,008 - 0,02 % boron rest nickel and contains unavoidable impurities.

[0007] In addition, one or more of the elements Si, Mn, P, S, Nb, or Fe may be present. A product can be generated from the alloy, which may be a powder, granulate, plate, rod, wire, tube, cast product, forged product, rolled product, or welded product.

[0008] DE 10 2010 011 609 A1 describes a nickel-chromium-cobalt-molybdenum alloy consisting of (in wt%) Cr 20 - 24 % Fe ≤ 1,5 % C 0,03 - 0,1 % Mn ≤ 0,5 % Si ≤ 0,25 % Co 10 - 15 % Cu ≤ 0,1 % Mon 9,0 - 10,5 % Ti 0,1 - 0,8 % AI 0,3 - 2,0 % P < 0,012 % S < 0,05 % B > 0,02 - < 0,08 % Nb 0,2 - 2 % N ≤ 0,015 % Mg ≤ 0,006 % Ca ≤ 0,01 % V ≤ 0,05 % Ni Residue and melting-related impurities

[0009] This alloy can be used for pipes, sheets, wire, bars, forgings, strips, welded structures for gas turbines, in furnace and power plant construction, in the petrochemical industry and in the field of nuclear energy technology.

[0010] In the technical paper "Microstructure of Long-Term Aged IN617 Ni-Base Superalloy" by Quanyan Wu et al., Table 1 shows the chemical composition of the IN617 alloy, which contains the following elements: Ni rest Cr 22,0 % Co 12,5 % Mon 9,0 % Al 1,2 % Fe 1,0 % Mn 1,0 % Ti 0,4 % Si 0,1 % C 0,1 % Cu 0,5 % B 0,006 % S 0,015 %

[0011] The invention is based on the object of providing a powder for the additive manufacturing of components that exhibits the advantageous properties of Ni and Ni-Co alloys and is cost-effective to produce. It is important to meet the specific requirements regarding particle size distribution, particle shape, and flowability of the powder.

[0012] Furthermore, a process for producing such a powder is to be proposed.

[0013] This task is solved by a nickel-based alloy for powder, where the contents (in wt.%) are defined as follows: C 0,015 - 0,5 % S max. 0.15%, in particular max. 0.03% Cr 20 - 25 % Ni rest Mn max. 1% Si max. 1% Mon up to 10% Ti 0,25 - 0,6 % Nb up to 5.5% Cu up to 5%, especially up to 0.5% Fe up to 25% P max. 0.03%, in particular max. 0.02% Al 0,8 - 1,5 % V max. 0.6% Zr max. 0.12%, in particular max. 0.1% Co up to 15% B 0,006 - 0,125 % O >0,00001 - 0,1 % optional See max. 0.0005% Bi max. 0.00005% Pb max. 0.002% and manufacturing-related impurities, wherein the carbon to boron ratio C / B is between 4 and 25, wherein the sum C + B is between 0.156 and 0.625%, in particular in the range 0.16 and 0.6%, especially in the range 0.1875 and 0.530%, and wherein the sum Nb + Ta is max. 5.2%.

[0014] Advantageous further developments of the powder alloy according to the invention can be found in the associated subclaims.

[0015] The object is also achieved by a process for producing a powder from a nickel-based alloy by an alloy is melted in a VIM furnace, the liquid melt is kept for 5 minutes to 2 hours to homogenise, a closed atomisation system is set to a dew point of -10°C to -120°C with a supplied gas, the melt is blown through a nozzle into a gas stream with a gas flow rate of 2 m³ / min to 150 m³ / min, the solidified powder particles are collected in a gas-tight container, the particles have a particle size of 5 µm to 250 µm, the powder particles are spherical, the powder has gas inclusions of 0.0 to 4% pore area (pores > 1 µm) in relation to the total area of ​​the evaluated objects, the powder has a bulk density of 2 to the density of the alloy of approx. 8 g / cm³, the powder is hermetically packed under a protective gas atmosphere with argon.

[0016] Advantageous further developments of the method according to the invention can be found in the associated subclaims.

[0017] The following initial production steps are conceivable: A master alloy block with a defined chemical analysis is produced by melting in a VIM furnace. A master alloy block is cut into small pieces by sawing. The master alloy pieces are melted in a VIM furnace, or alloying elements of a defined weight are melted in a VIM according to the chemical analysis. The liquid melt is held for 5 minutes to 2 hours for homogenization.

[0018] The following further processing steps can follow the alternative initial production steps: the closed atomization system is set with argon gas to a dew point of -10°C to -120°C, preferably in the range of -30°C to -100°C, the melt is blown through a nozzle into an argon gas stream with a gas flow rate of 2 m³ / min to 150 m³ / min, the solidified powder particles are collected in a gas-tight container, the particles have a particle size of 5µm to 250µm, with preferred ranges being between 5 and 150µm, or 10 and 150µm, the powder particles are spherical, the powder has gas inclusions of 0.0 to 4% pore area (pores > 1µm) in relation to the total area of ​​​​evaluated objects, with preferred ranges being 0.0 to 2%. The amount of gas inclusions in the powder allows for minimal residual porosity in the manufactured parts. The powder has a bulk density of 2 to the alloy density of approximately.8 g / cm 3< , with preferred ranges being values ​​of 4 to 5 g / cm 3<, the powder is packaged hermetically under a protective gas atmosphere with argon. .

[0019] The powder according to the invention is preferably produced in a vacuum inert gas atomization system (VIGA). In this system, the alloy is melted in a vacuum induction melting furnace (VIM) and fed into a pouring funnel leading to a gas nozzle, in which the molten metal is atomized into metal particles using inert gas at high pressures of 5 to 100 bar. The melt is heated in the crucible at temperatures between 5 and 400°C above the melting point. The metal flow rate during atomization is 0.5 to 80 kg / min and the gas flow rate is 2 to 150 m³ / min. Due to the rapid cooling, the metal particles solidify into spherical particles. The inert gas used during atomization can contain 0.01 to 100% nitrogen if required. The gas phase is then separated from the powder in a cyclone, and the powder is subsequently packaged.

[0020] Alternatively, the powder according to the invention can be produced using the so-called EIGA process instead of VIGA. In this process, a prefabricated alloy block in the form of a rotating electrode is melted contactlessly by an induction coil. The melt drips from the electrode directly into the gas stream of a gas nozzle.

[0021] The alloy ingot for EIGA can be produced using the VIM, ESR, VAR, VOD, or VLF melting processes, and combinations thereof, and can optionally undergo hot forming processes such as forging and rolling. It is advantageous to clean the ingot's surface by treatment such as grinding and / or peeling before use in the EIGA process.

[0022] The inert gas used in powder production can be either argon or a mixture of argon with 0.01 to 100% nitrogen. Possible limitations of the nitrogen content may include: 0.01 to 80% 0.01 to 50% 0.01 to 30% 0.01 to 20% 0.01 to 10% 0.01 to 10% 0.1 to 5% 0.5 to 10% 1 to 5% 2 to 3%

[0023] Alternatively, the inert gas can be helium.

[0024] The inert gas preferably has a purity of at least 99.996 vol.%. In particular, the nitrogen content should be between 0.0 and 10 ppmv, the oxygen content between 0.0 and 4 ppmv, and the H2O content should be ≤ 5 ppmv.

[0025] In particular, the inert gas preferably has a purity of at least 99.999 vol.%. In particular, the nitrogen content should be between 0.0 and 5 ppmv, the oxygen content between 0.0 and 2 ppmv, and the H2O content should be ≤ 3 ppmv. The dew point in the system is in the range of -10 to -120°C. It is preferably in the range of -30 to -100°C.

[0026] The pressure during powder atomization can preferably be 10 to 80 bar.

[0027] The parts and components, or layers on parts and components, manufactured using additive manufacturing are constructed from layer thicknesses ranging from 5 to 500 µm and, immediately after production, have a textured microstructure with grains elongated in the build direction and an average grain size of 2 µm to 1000 µm. The preferred range is between 5 µm and 500 µm.

[0028] Parts and components, or coatings on parts and components, produced using additive manufacturing can optionally be subjected to solution annealing in the temperature range from 700°C to 1250°C for 0.1 min to 70 h, optionally under a protective gas such as argon or hydrogen, followed by cooling in air, in a moving annealing atmosphere, or in a water bath. The surface can then be cleaned or machined by pickling, blasting, grinding, turning, peeling, or milling. This machining can be carried out partially or entirely even before annealing.

[0029] The parts and components, or coatings on parts and components, produced using additive manufacturing have an average grain size of 2 µm to 2000 µm after annealing. The preferred range is between 20 µm and 500 µm.

[0030] The parts and components, or coatings on parts and components, produced by additive manufacturing from the powder produced according to the invention are preferably intended for use in areas where the material is also used as a wrought or cast alloy with a related analytical method. Additive manufacturing also includes terms such as generative manufacturing, rapid technology, rapid tooling, rapid prototyping, and the like.

[0031] In addition, the powder described above can also be used to manufacture components using hot isostatic pressing (HIP) or conventional sintering and extrusion processes. A combination of additive manufacturing and subsequent HIP treatment is also possible. The post-processing steps for HIP components described below for additive manufacturing can be applied.

[0032] In general, a distinction is made between: 3D printing with powders, selective laser sintering and selective laser melting, laser cladding and selective electron beam welding.

[0033] The abbreviations used here are defined as follows: VIM Vacuum Induction Melting VIGA Vacuuminert gas atomization system VAR Vacuum Arc Remelting VOD Vaccum Oxygen Decaburization VLF Vaccum Ladle Furnace EIGA Electrode Induction Melting Gas Atomization

[0034] Advantageous further developments of the method according to the invention can be found in the subclaims.

[0035] The particle size range of the powder is between 5 and 250 µm, with preferred ranges being between 5 and 150 µm, or 10 and 150 µm.

[0036] The powder has gas inclusions of 0.0 to 4% pore area (pores > 1 µm) in relation to the total area of ​​evaluated objects, with preferred ranges being 0.0 to 2% 0.0 to 0.5% 0.0 to 0.2% 0.0 to 0.1% 0.0 to 0.05%

[0037] The powder has a bulk density of 2 to the density of the alloy of approximately 8 g / cm 3< , whereby preferred ranges can be the following values: 4-5 g / cm 3< 2-8 g / cm 3< 2-7 g / cm 3< 3-6 g / cm 3<

[0038] The amount of gas inclusions in the powder allows for low residual porosity in the manufactured parts.

[0039] The powder produced using this process, as well as components manufactured from this powder (3D-printed samples), are free of nitrides, carbides, and / or carbonitriding. If nitrides or carbides are present, they have a particle size of < 100 nm, particularly < 50 nm.

[0040] After heat treatment of components manufactured from this powder (3D-printed samples) for homogenization and diffusion annealing at temperatures above 900°C, especially above 1000°C, ideally above 1100°C, for more than 1 hour, nitrides, carbides, and / or carbonitrides may appear in the manufactured components (3D-printed samples). These have particle sizes of < 8µm or < 5µm, respectively, and ideally < 1µm.

[0041] Compared to the state of the art, the centrifuge process is omitted, thus optimizing the plant's operating time. The subsequent refining processes optimize the quality of the powder for additive manufacturing.

[0042] It can be advantageous if the block is subjected to surface treatment (e.g., brushing, grinding, pickling, cutting, peeling, etc.) before cutting. This can remove defects that cannot be eliminated by further remelting and could be detrimental to later applications.

[0043] The process according to the invention can be applied to any Ni or Ni-Co base alloy.

[0044] The following presents an alloy composition that can be produced as a powder using the process parameters according to the invention. This carbon-containing alloy composition can be processed into components as a powder with a particle size preferably between 15 µm and 53 µm or between 45 µm and 150 µm using a fusion welding process such as laser or electron beam welding. The alloy composition is characterized by particularly good processability in the form of a particularly low tendency to hot cracking when the carbon to boron ratio (C / B ratio) in the powder is between > 4 and < 25 and the sum of B+C is > 0.1875% and < 0.525%.

[0045] The components produced by welding from this alloy composition are preferably used in high-temperature applications (operating temperature > 550°C) with simultaneous mechanical stress (creep rupture stress > 10,000h).

[0046] An advantageous composition of the powder according to the invention is given below (all data are in wt.%): C 0,15 - 0,50% S max. 0.150%, in particular max. 0.03% Cr 22 - 25 % Ni rest Mn max. 1% Si max. 1% Mon 8 - 10% Ti 0,25 - 0,5 % Nb max. 5.5% Cu max. 5%, in particular max. 0.5% Fe max. 25% Al 0,80 - 1,50 % V max. 0.6% Zr max. 0.12%, in particular max. 0.1% Co 11 - 13% O 0,00001-0,1 % B 0,0060 - 0,125 % and manufacturing-related impurities, where the carbon to boron ratio (C / B) is between 4 and 25 and the sum of B+C is > 0.1875% and < 0.525%.

[0047] The optimal carbon to boron ratio is between 4 and 25, and the sum of B+C is between > 0.1875% and < 0.525%. This is justified as follows: in melting, casting, and welding processes, the solidification interval—i.e., the temperature range between the liquidus temperature and the solidus temperature—determines the formation of solidification-related defects such as hot cracks or internal shrinkage cavities. The addition of the element boron broadens the solidification interval. It was found that increasing the boron content from 0.005% to 0.020% broadens the solidification interval from 127°C to 141°C. However, with increased addition of the element carbon, it combines with the element boron and effectively narrows the solidification interval. For example, an increase in the carbon content from 0.055% to 0.500% with a boron content of 0.005% leads to a reduction in the solidification interval from 127K to 99K.With a boron content of 0.020%, a carbon content of 0.350% leads to a solidification interval of 123K, but with a carbon content of 0.500%, the solidification interval is only 113K (see Table 1). Table 1 alloy B C incipient liquids dT C / B C+B FM 617B 0.0023 0.056 1255 1372 117 24 0,058 FM 617 0.0050 0.055 1245 1372 127 11 0,060 Var 1 0.0200 0.350 1236 1359 123 17,5 0,37 Var 2 0.0200 0.500 1240 1353 113 25 0,52 Var 3 0.0250 0.500 1240 1353 113 20 0,525 Var 4 *)< 0.0050 0.500 1255 1354 99 100 0,505 Var 5 *)< 0.0200 0.055 1230 1371 141 2,75 0,075 *) Control variants with B < 0.0060% or C / B < 4 or > 25

[0048] This means that increasing the boron content will not lead to an unacceptable deterioration in processing properties during the melting phase, such as welding or selective laser melting, if the carbon content is increased simultaneously. The ideal ratio between C and B was determined to be 14.8. This means that the solidification interval remains constant even with boron addition if the carbon to boron ratio is increased by a factor of 14.8.

[0049] The increase in boron combined with a simultaneous increase in carbon content also leads to a predominant occurrence of M23C6 primary carbides and a simultaneous reduction in the occurrence of M6C carbides. The advantage of M23C6 carbides over M6C carbides is that they do not dissolve again during annealing treatments such as solution annealing and remain stably distributed within the microstructure, and thus also within the grain, rather than primarily at the energetically favorable grain boundaries.

[0050] In addition, it was found that a higher carbon content reduces or even completely suppresses the formation of the sigma phase.

[0051] Optionally, the oxygen content of the produced alloy can be 0.00001 - 0.1%, 0.0001 - 0.1%, 0.001 - 0.1%, 0.001 - 0.002% or 0.0015 - 0.002%.

[0052] Alternatively, the oxygen content can be adjusted as follows: 0.00001 - 0.1 0.00002 - 0.1 0.00005 - 0.1 0.00008 - 0.1 0.0001 - 0.1 0.0002 - 0.1 0.0005 - 0.1 0.0008 - 0.1 0.001 - 0.1 0.002 - 0.1 0.005 - 0.1 0.008 - 0.1 0.010-0.1 0.00001 - 0.10 0.00001 - 0.08 0.00001 - 0.05 0.00001 - 0.03 0.00001 - 0.02

[0053] The following elements can be adjusted if required - depending on the application - within the following ranges: Co > 11 - < 15% Mn > 0,001 - < 0,3% Mon > 8,4 - < 10% Ti > 0,25 - < 0,35%

[0054] A favorable ratio: C / B is between > 12 and < 18.

[0055] It is also advantageous if the sum C + B is between 0.156 and 0.625%, in particular in the range 0.16 and 0.6%, especially in the range 0.1875 and 0.530%.

[0056] The following are preferred areas of application of the powder according to the invention: Additive manufacturing of components or parts Additive manufacturing of layers on components or parts Manufacturing of components for turbines Manufacturing of components for the oil and gas industry Manufacturing of fans and flanges.

[0057] Powders with a particle size of 5µm to 250µm are achieved.

[0058] A particle size that is too small below 5 µm impairs the flow behavior and should therefore be avoided; a particle size that is too large above 250 µm impairs the behavior during additive manufacturing.

[0059] A bulk density that is too low, less than 2 g / cm², impairs the performance during additive manufacturing. The maximum possible bulk density of approximately 8 g / cm³ is determined by the density of the alloy.

[0060] The oxygen content must be less than or equal to 0.100% to ensure the manufacturability and usability of the alloy. An oxygen content that is too low increases costs. Therefore, the oxygen content is ≥ 0.0001%.

[0061] The powders produced using this process can be used in additive manufacturing to build components that exhibit the properties of the underlying alloys.

[0062] The process according to the invention is explained by way of example as follows: Table 2 shows exemplary chemical compositions (Var 1 to Var 3) of the powder variants possible with the process according to the invention: Table 2 Var 1 Var 2 Var 3 Batch #185855 Mass% C 0,350 0,500 0,500 0,055 S 0,002 0,002 0,002 0,002 N <0,01 <0,01 <0,01 <0,01 Cr 21,5 21,5 21,5 21,80 Ni Bal Bal Bal 55,82 Mn 0-1 0-1 0-1 0,15 Si 0-1 0-1 0-1 0,12 Mon 9,0 9,0 9,0 8,86 Ti 0,30 0,30 0,30 0,33 Nb 0,3 0,3 0,3 0,01 Cu 0,01 0,01 0,01 0,01 Fe 1,5 1,5 1,5 0,32 P 0,002 0,002 0,002 0,002 Al 1,35 1,35 1,35 1,32 Mg 0,002 0,002 0,002 0,002 Ca 0,001 0,001 0,001 0,001 Co 11,15 11,15 11,15 11,16 B 0,020 0,020 0,025 0,002 C / B 17,5 25 20 27,5 C+B 0,37 0,52 0,525 0,057

[0063] Table 3 documents creep rupture values ​​to fracture, measured on FM 617B weld metal from batch #185855 with a C / B ratio of (0.055 / 0.002) = 27.5 and the sum of C + B of 0.057. Due to the C / B ratio of > 25 and the low sum of C + B, a sufficiently weldable weldability can be achieved using common arc welding processes. However, the creep rupture values ​​(time t to fracture) are limited and only reach the required creep rupture values ​​of > 10,000 h in the temperature range between 650°C and 800°C at static loads of Sigma < 83 MPa. Table 3 Sample No. Blank No. T [°C] Sigma [MPa] Time t to fracture [h] 21.1C C1 650 458 634 21.1D D1 650 398 3357 21.1E E1 650 368 7712 21.1F F1 650 330 17742 21.1C C2 700 362 530 21.1D D2 700 302 2465 21.1E E2 700 261 6460 21.1F F2 700 214 28567 21.1C C3 750 261 322 21.1D D3 750 192 3594 21.1E E3 750 154 10921 21.1C C4 800 161 409 21.1D D4 800 107 4977 21.1F F4 800 83 26442

Claims

1. Nickel-based alloy for powder, wherein the contents (in % by weight) are defined as follows: C0.015 - 0.5%Smax. 0.15%, in particular max. 0.03%Cr20 - 25%NiremainderMnmax. 1%Simax. 1%Moup to 10%Ti0.25 - 0.6%Nbup to 5.5%Cuup to 5%, particularly up to 0.5%Feup to 25%Pmax. 0.03%, particularly max. 0.02%Al0.8 - 1.5%Vmax. 0.6%Zrmax. 0.12%, particularly max. 0.1%Coup to 15%B0.006 - 0.125%O> 0.00001 - 0.1% optionally Semax. 0.0005%Bimax. 0.00005%Pbmax. 0.002% and production-related impurities, wherein the carbon to boron ratio (C / B) is between 4 and 25, wherein the total C + B is between 0.156 and 0.625%, particularly in the range from 0.16 to 0.6%, most particularly in the range from 0.1875 to 0.530%, and wherein the total for Nb + Ta is max. 5.2%.

2. Alloy according to Claim 1, wherein Co content in % by weight is > 11% to < 15%.

3. Alloy according to Claim 1 or 2, wherein Mn content in % by weight is > 0.001 to < 0.30%.

4. Alloy according to any one of Claims 1 to 3, wherein Mo content in % by weight is > 8.4% - < 10%.

5. Alloy according to any one of Claims 1 to 4, wherein Ti content in % by weight is > 0.25% - < 0.35%.

6. Alloy according to any one of Claims 1 to 5, wherein C content in % by weight is > 0.15% - 0.5%.

7. Alloy according to any one of Claims 1 to 6, wherein B content in % by weight is > 0.010% and < 0.05%.

8. Alloy according to any one of Claims 1 to 7, wherein C / B is > 10 - 25.

9. Alloy according to any one of Claims 1 to 8, wherein the creep strength achieved at 750°C and a load of 261 MPa is greater than 322 h.

10. Method for producing a powder from a nickel-based alloy according to any one of Claims 1 to 9 by - melting an alloy in a VIM furnace, i.e. vacuum induction melting furnace, - retaining the liquid melt for 5 min to 2 hours for homogenisation, - setting a closed atomisation plant with a supplied gas to a dew point from -10°C to -120°C, - blowing the melt through a nozzle into a gas stream with a gas flow rate from 2 m3 / min to 150 m3 / min, - collecting the solidified powder particles in a gas-tight sealed container, wherein - particles having a particle size from 5 µm to 250 um and spherical shape are used, - powder is provided with gas inclusions from 0.0 to 4% porous area, for pores > 1 µm, relative to the total area of evaluated objects, - powder with a bulk density from 2 to the density of the alloy of approx. 8g / cm3 is used, - powder is packed airtight under the protective gas atmosphere with argon.

11. Method according to Claim 10, wherein the alloy is first produced as a master alloy block with defined chemical analysis by melting in the VIM furnace, - the master alloy block is separated into small pieces by sawing, - the pieces of the master alloy are melted in a VIM furnace.

12. Method according to Claim 10 or 11, characterized in that an inert gas is used as the supplied gas.

13. Method according to any of claims 10 or 11, characterized in that argon is used as the supplied gas.

14. Method according to any one of Claims 10 to 13, characterized in that the gas stream into which atomisation takes place consists of argon.

15. Method according to any one of Claims 10 to 14, characterized in that the gas stream into which atomisation takes place consists of nitrogen.

16. Method according to any one of Claims 10 to 15, characterized in that the gas stream into which t atomisation takes place consists of a mixture of nitrogen and argon.

17. Method according to any one of Claims 10 to 16, characterized in that the atomisation of the melt takes place at a rate of 0.5 to 80 kg / min.

18. Use of a powder produced by a method according to any one of Claims 10 to 17 for the additive manufacturing of components or parts.

19. Use of a powder produced by a method according to any one of Claims 10 to 17 for the additive manufacturing of layers on components or parts.

20. Use of a powder produced by a method according to any one of Claims 10 to 17 for the production of turbine components.

21. Use of a powder produced by a method according to any one of claims 10 to 17 for the production of components for the oil and gas industry.

22. Use of a powder produced by a method according to any one of Claims 10 to 17 for the production of valves or flanges.