METHOD FOR MANUFACTURING AN OPTICALLY VARIABLE SAFETY ELEMENT

DE502021005199D1Active Publication Date: 2024-10-02GIESECKE & DEVRIENT CURRENCY TECHNOLOGY GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502021005199
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-28
Filing Date
2021-07-22
Publication Date
2024-10-02
Estimated Expiration
2041-07-22

AI Technical Summary

Technical Problem

Existing methods for producing optically variable security elements lack a robust and efficient way to create security elements with independently selectable colors for relief structures, which are essential for advanced authentication and anti-replication features.

Method used

A method involving a production carrier with a partial embossing lacquer layer and selective coating application, where the first embossed lacquer layer prevents removal of the first coating in lacquer areas while allowing its removal in free areas, creating a combination structure with two height levels and differing adhesion properties to achieve distinct color effects.

Benefits of technology

This method enables the production of optically variable security elements with seamless binary color and motif changes, providing enhanced authentication and anti-replication capabilities by ensuring precise registration of color and effect differences.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a method for producing an optically variable security element.

[0002] Data storage devices, such as valuables or identification documents, as well as other valuable items such as branded goods, are often provided with security elements for security purposes. These elements allow verification of the authenticity of the data storage device and also serve as protection against unauthorized reproduction. These security elements can, for example, take the form of a security thread embedded in a banknote, a cover foil for a banknote with a hole, an applied security strip, a self-supporting transfer element, or even a feature area printed directly onto a valuable document.

[0003] Security elements with a viewing-angle-dependent or three-dimensional appearance play a special role in authenticity assurance, as these cannot be reproduced even with the most modern copying machines. For this purpose, the security elements are equipped with optically variable elements that convey a different image impression to the viewer at different viewing angles, for example, displaying a different color or brightness impression and / or a different graphic motif depending on the viewing angle. In the prior art, optically variable effects include, for example, motion effects, pump effects, depth effects, or flip effects, which are realized using holograms, microlenses, or micromirrors.

[0004] Some time ago, optically variable security elements were proposed that have two relief structures arranged at different heights, each provided with a colored coating (see WO 2020 / 011390 A1, WO 2020 / 011391 A1, and WO 2020 / 011391 A2). The colored coating of the higher relief structure is either structured as a grid or provided with recesses, so that when the security element is viewed from certain angles, the color of the colored coating of the lower relief structure appears in the spaces between the grids or recesses.

[0005] Furthermore, the following procedure is assumed to be familiar. An embossing lacquer layer is applied to a production substrate only in certain areas. The embossing lacquer layer is embossed – for example, with a hologram structure – and metallized over the entire surface. To create negative characters next to the hologram, the metallization is removed in certain areas by selectively applying another layer – before or after metallization. The resulting security element is then peeled off the production substrate.

[0006] EP 3 216 620 A1 relates to a security element with a plurality of reflective facets, some of which have a random orientation and some of which have an orientation for reflection in an angular range. WO 2020 / 126077 A2 describes a method for producing an optically variable security element in which a non-metal coating is selectively lifted off from a higher relief structure. EP 2 996 885 B1 shows the preamble of claim 1.

[0007] Based on this, the invention is based on the object of specifying a robust method for producing optically variable security elements, in particular optically variable security elements with two independently selectable colors of the relief structures.

[0008] This object is achieved by the features of the independent claim. Further developments of the invention are the subject of the dependent claims.

[0009] According to the invention, in the method for producing an optically variable security element, a production carrier is provided whose surface area defines a z-axis perpendicular thereto.

[0010] A first embossing lacquer layer is applied to the surface of the production substrate only in partial areas, creating lacquer areas with an embossing lacquer layer and free areas without an embossing lacquer layer. The applied first embossing lacquer layer is provided with a first embossing at a first height level.

[0011] The surface area is coated with a first coating in the free areas and in the painted areas. The surface area is then coated with a second layer in the free areas and optionally also in the painted areas. The first coating is removed again in the free areas. The production carrier is removed according to the invention.

[0012] According to the invention, the further layer is a second embossing lacquer layer, which is provided with a second embossing - on a second height level spaced from the first height level in the z-direction - so that a combination structure with the two embossings on two height levels is created.

[0013] According to the invention, the first embossing lacquer layer prevents removal of the first coating in the lacquer regions during or after the production carrier is removed from the combination structure. In the free regions, however, the first coating is removed during or after the production carrier is removed. In the free regions, the first coating is preferably removed with the production carrier and thus removed when the production carrier is removed. For this purpose, the first coating can have a higher adhesion to the production carrier than the first embossing lacquer layer to the production carrier. Alternatively or additionally, the first coating can have a higher adhesion to the production carrier than the first coating to an intermediate layer remaining in the combination structure, which intermediate layer can in particular be the second embossing lacquer layer, an adhesive layer, or a dielectric layer.

[0014] In the lacquer areas, the first embossing lacquer layer remains in the combination structure when the production carrier is removed, particularly since it has lower adhesion to the production carrier than the first coating.

[0015] The removal of the first coating in the free areas can alternatively or additionally also occur after stripping the production substrate. The first coating, or a residue of the first coating remaining after stripping, is then removed by etching. The intermediate layer remaining in the combination structure can advantageously exhibit a higher resistance to an etchant than the first coating. However, since it is generally thicker than the first coating, a similar or slightly lower resistance is theoretically also possible.

[0016] In the lacquer areas, the first embossing lacquer layer preferably prevents the removal of the first coating, even after the production substrate has been removed. It can optionally have a higher resistance to an etching agent than the first coating. However, since the embossing lacquer layer has a higher layer thickness than the first coating, a similar or slightly lower resistance is theoretically also usable.

[0017] In the lacquer areas, the first embossing lacquer layer lies directly on the surface of the production substrate, while in the free areas, the first coating lies directly on the surface of the production substrate. In the lacquer areas, one side of the first coating lies directly on the embossed surface of the first embossing lacquer layer. Preferably, an intermediate layer lies directly on the other side of the first coating in the free areas and optionally also in the lacquer areas, which remains in the combined structure. The intermediate layer can be, for example, the second embossing lacquer layer, an adhesive layer, or a dielectric layer.

[0018] A large difference in adhesion has proven advantageous for removal during peeling off the production carrier. The aforementioned adhesions preferably differ by at least a factor of 2, more preferably at least a factor of 3 or 5, in particular at least a factor of 10. In particular, the adhesion of the first coating to the production carrier is more than a factor of 2 (3, 5 or 10) greater than the adhesion of the first embossing lacquer layer to the production carrier. The adhesion of the first coating to the production carrier is more than a factor of 2 (3 or 5) greater than the adhesion of the first coating to the intermediate layer remaining in the combination structure. The adhesion of the first coating to the intermediate layer is generally selected to be greater than the adhesion of the embossing lacquer layer to the production carrier.

[0019] The first coating is preferably a (first) reflection-enhancing coating that follows the first embossing; preferably, a second reflection-enhancing coating follows the second embossing. Advantageously, both sides of the first and / or second reflection-enhancing coating follow their embossing.

[0020] In particular, the combination structure should comprise a first and a second relief structure with different colors, preferably reflective and / or transmissive. The first and second relief structures are formed by the first and second embossing lacquer layers, respectively, the first and second reflection-enhancing layers, respectively, and an optional first and second color layer.

[0021] In particularly advantageous embodiments, a product carrier of the combination structure is applied in one method step. Preferably, at least the first embossing lacquer layer, in particular either only the first embossing lacquer layer or both embossing lacquer layers, is arranged between the product carrier and the production carrier. The product carrier can be a final product carrier that forms part of the optically variable security element. Alternatively, the product carrier is a transfer product carrier on which the optically variable security element with its combination structure is detachably (i.e., only temporarily) arranged. The security element remains temporarily on the transfer product carrier, for example until a transfer from the transfer product carrier to an object to be secured.

[0022] In a first embodiment, the second embossing lacquer layer is applied and the second embossing is only applied on the production substrate. In a second embodiment, an already embossed second embossing lacquer layer is applied, in particular by means of an adhesive layer.

[0023] In the first embodiment, the second embossing lacquer layer can follow the second embossing with its first surface and the first embossing with its second surface. If, however, an intermediate layer - for example a colored one - is previously applied in the lacquer areas (and the free areas) to compensate for the first embossing, the second embossing lacquer layer does not follow the first embossing with its second surface. Additionally or alternatively, the embossed second embossing lacquer layer can be provided with the second reflection-enhancing coating. Additionally or alternatively, a product carrier can be provided and connected to the, in particular coated, embossed second embossing lacquer layer by means of an adhesive layer.

[0024] In the second embodiment, the second embossing lacquer layer on the product carrier can be provided with the second embossing beforehand. Alternatively or additionally, the embossed second embossing lacquer layer can be provided with the second reflection-enhancing coating beforehand. Alternatively or additionally, the adhesive layer can follow the second embossing with a first surface and the first embossing with a second surface. If, on the other hand, an intermediate layer - for example a colored one - is applied beforehand in the lacquer areas (and the free areas) to compensate for the first embossing, the adhesive layer does not follow the first embossing with the second surface. The same applies if the embossed second lacquer layer and the adhesive layer are arranged on different sides of the product carrier.

[0025] A viewer views the security element from a given viewing side. The two relief structures can differ in terms of effect type and / or viewing angle. The effect of the two relief structures from the given viewing side should appear different to the viewer in terms of color.

[0026] In initial variants, the first, preferably reflection-enhancing, coating and / or the second reflection-enhancing coating is a reflection-enhancing colored coating. The reflection-enhancing colored coating can be formed by a single layer, such as a colored metallization or a color-imparting HRI layer, or by a multilayer structure. The reflection-enhancing colored coating can be only reflective or transmissive and color-effective. For example, it can be formed by a color-imparting (transmissive and reflective) HRI multilayer structure, by a color-shifting multilayer structure (usually with three layers of absorber, dielectric, and reflector, for example, with a full-surface or partial reflector), or by a color-filtering, transmissive and reflective multilayer structure (usually with three layers of absorber, dielectric, and absorber).Preferably, it is formed by a reflection-enhancing partial layer which is provided with a partial layer of translucent and / or luminescent paint.

[0027] In second variants, the first coating, which is a reflection-enhancing coating, and / or the second reflection-enhancing coating, has a color-reflecting effect due to a substructure of its embossing, in particular a subwavelength structure, interference structure (for example as a nanostructure with a binary surface) or diffraction structure.

[0028] In third variants, exactly one first or second translucent color layer is provided for the first coating, which is a reflection-enhancing coating, and / or for the second reflection-enhancing coating, or a first or second color-imparting multilayer substructure (such as a dielectric and reflector / absorber) is provided, which only has a reflective and / or transmissive color effect together with the reflection-enhancing coating. In particular, a first or second translucent color layer can also be formed as an unstructured color layer, meaning that neither of its sides follows either of the two embossing patterns.

[0029] Preferably, the same variant is used for both embossings of the combination structure. Alternatively, two different variants of the three mentioned variants can be used in one security element.

[0030] The first coating and / or the second reflection-enhancing coating is particularly preferably a vapor-deposited layer, in particular a metal layer or an HRI layer.

[0031] The first and / or second embossed structure is advantageously molded in a transparent or translucently colored embossed lacquer layer. If an embossed lacquer layer is arranged between the viewer and the first and / or second reflection-enhancing coating, the color of the embossed lacquer layer can determine the color effect or modify a color effect of the first or second reflection-enhancing coating. When using transparent, i.e., uncolored, embossed lacquer layers, the color effect of the embossed structures is determined by the respective colored coating or color layer. By using translucently colored embossed lacquer layers, the color effect of the colored coating can be modified, so that, for example, different color effects of the embossed lacquer layers can be created despite using the same metallization, e.g., an aluminum metallization.

[0032] In an advantageous embodiment, the lacquer areas and free areas are formed, at least in a partial area of ​​the surface area, as a regular or irregular grid with grid elements and grid spaces, wherein the dimensions of the grid elements and / or the dimensions of the grid spaces in one or both lateral directions are below 140 µm, preferably between 20 µm and 100 µm, in particular between 20 µm and 60 µm. The observer does not perceive the grid. The dimensions of the grid elements or grid spaces are selected in particular so that they are below the resolution of the human eye.

[0033] In the grid areas formed by the lacquered and free areas, the security element advantageously displays an appearance when tilted or the viewing direction changes accordingly, suddenly jumping from a first to a second appearance (or from the second to the first appearance when tilted back). This involves a simultaneous and seamless change in the depicted motif (e.g., value number or coat of arms) and color (e.g., yellow or blue). Such an appearance, which changes seamlessly between two different motifs with two different colors, is referred to in this description as a binary color and motif change.A binary change of color, motif and effect is possible, especially since an optically variable effect of the motifs (flat / three-dimensional and / or lying in the substrate plane / floating above the substrate plane / floating below the substrate plane and / or stationary / moving ...) can also differ.

[0034] The grid formed by the lacquer areas and free areas is advantageously formed with a constant area coverage by the grid elements, which is expediently between 30% and 70%, preferably between 40% and 60%, in particular approximately 50%.

[0035] Alternatively or additionally, it is provided that the lacquer areas and free areas are formed as an effect area at least in a portion of the surface area, in which the lacquer areas and / or the free areas have lateral dimensions of more than 140 µm. The effect area is large enough to be perceived separately by the observer.

[0036] In these effect areas, the security element preferably displays two different effects (e.g., a three-dimensional motif and a moving effect such as a moving bar) that appear in two different colors. The areas of different color impressions and different effects are precisely matched to each other, which is also referred to as color-to-effect registration.

[0037] Advantageously, at least one lacquer area and / or at least one free area is formed with lateral dimensions of more than 250 µm, preferably of more than 500 µm and in particular of more than 1 mm.

[0038] The embossed structures are advantageously formed by micromirror arrangements with directed micromirrors. The micromirrors are particularly formed by non-diffractive mirrors and do not produce color separation. Preferably, flat mirrors, concave mirrors, and / or Fresnel-type mirrors can be used. The lateral dimensions of the micromirrors are expediently below 50 µm, advantageously below 20 µm, preferably approximately 10 µm, i.e., between 7 µm and 13 µm. On the other hand, the lateral dimensions of the micromirrors can also be above 2 µm, in particular above 3 µm, or even above 5 µm. The pitch of the micromirrors is preferably less than 10 µm, more preferably less than 5 µm.

[0039] In principle, other embossed relief structures, in particular Fresnel lenses, concave mirrors, hologram structures, nanostructures, or diffractive blazed gratings, can be used instead of micromirrors. Achromatic diffraction gratings, so-called matte structures, can be used particularly advantageously here. These essentially reflect white light and thus do not interfere with the color effect of the coating or any color layers by generating diffraction colors. To create bright colors in transmission and / or reflection, the relief structures can also have subwavelength structures, in particular subwavelength gratings, which, in combination with the respective reflection-enhancing coating, determine or at least co-determine its color.

[0040] In an advantageous embodiment, the first and second color coatings completely cover the respective embossed structure. If an embossed structure, such as the first embossed structure, is present only in partial areas of the surface area, complete coverage of the embossed structure refers to the complete coverage of those partial areas in which the embossed structure is present in the surface area.

[0041] Alternatively, negative markings can also be provided in the security element through recesses in the first and / or second reflection-enhancing coating, which form, for example, text, symbols or value numbers.

[0042] Transmissive negative markings, such as text, symbols, or value numbers, can be formed in the lacquered areas and / or in the free areas of the reflective surface area. This is particularly possible by creating congruent recesses in the first and second reflection-enhancing coatings in the lacquered areas and / or by creating recesses in the second reflection-enhancing coating in the free areas.

[0043] Negative marks can be provided in the halftone areas formed by the aforementioned lacquer areas and free areas. However, they generally appear less visually attractive there, as the line width of the negative marks is usually greater than the screen of the first embossing lacquer layer, so the viewer may be able to see the printing screen of the negative marks.

[0044] On the other hand, negative markings can be very well integrated into the effect areas with color-to-effect registration due to the larger dimensions of the lacquer areas and free areas, whereby the following variants are preferred: a) The negative marks can be created in the overlap area of ​​the two embossed structures, i.e., in the aforementioned lacquer areas of the surface area. In this case, maintaining the register presents a particular challenge, as the two relief structures have a certain register tolerance with each other, and the demetallization also has a certain register tolerance. Since both reflection-enhancing coatings must be partially removed in this variant, the register tolerances add up.

[0045] Transparent, colorless negative markings require that both embossing lacquer layers (first process variant) or the first embossing lacquer layer and the laminating adhesive (second process variant) be colorless. If one or both embossing lacquer layers or the laminating adhesive are colored, colored negative markings are produced with the color effect of the colored layers or the subtractive color effect of both colored layers. b) The negative markings can be created in the free areas of the surface area where only the second embossing lacquer layer is present. In this case, maintaining register is easier because only the reflection-enhancing coating of the second relief structure needs to be removed / demetallized.

[0046] Transparent, colorless negative markings require the color effect of the second embossed structure to be created by a metal layer removed in the recesses. If the second embossing lacquer layer (first process variant) or the laminating adhesive (second process variant) is colored, colored negative markings are produced.

[0047] In all process variants, it is preferred that both embossed structures are constructed on the same side of the production carrier or the final product carrier in order to have as few work steps as possible in the production of the security element and to reliably achieve the desired visual effects.

[0048] The described reflective surface area of ​​the security element can be combined with other security features, for example with holograms, in particular true-color holograms, with subwavelength gratings or other subwavelength structures, with micromirror arrangements without diffractive gratings, or with security features based on special material properties, such as electrical conductivity, magnetic properties, luminescence, fluorescence or the like, as are known from the prior art.

[0049] The optically variable security element can be provided with additional layers, such as a protective, covering, or additional functional layer, a primer layer, or a heat-sealing lacquer layer. However, these are not essential to the present invention and are therefore not described in detail.

[0050] Further embodiments and advantages of the invention are explained below with reference to the figures, in which a true-to-scale and true-to-proportion reproduction has been omitted in order to increase clarity.

[0051] They show: Fig. 1 a schematic representation of a banknote with an optically variable security element produced according to the invention, Fig. 2 a security element produced according to the invention in cross section, Fig. 3 in (a) to (c) intermediate steps in the production of the primary structure of a security element, Fig. 4 in (a) to (e) intermediate steps in the completion of the primary structure of the Fig. 3 with a secondary structure according to a first process variant according to the invention, Fig. 5in (a) to (d) intermediate steps in the completion of the primary structure of the Fig. 3 with a secondary structure according to a second process variant according to the invention, Fig. 6 a security element produced according to the first process variant with additionally introduced negative markings, and Fig. 7 a security element produced according to the second process variant with additionally introduced negative markings.

[0052] The invention will now be explained using the example of security elements for banknotes. Figur 1 shows a schematic representation of a banknote 10 with an optically variable security element 12 produced according to the invention in the form of an adhesive-applied transfer element. However, it is understood that the invention is not limited to transfer elements and banknotes, but can be used for all types of security elements, for example, labels on goods and packaging or for securing documents, ID cards, passports, credit cards, health cards, and the like. For banknotes and similar documents, in addition to transfer elements (such as patches with or without their own carrier layer), security threads or security strips, for example, are also possible.

[0053] The security element 12 itself is very flat, but nevertheless gives the observer the three-dimensional impression of a motif 14 that appears to bulge out from the plane of the banknote 10 and appears in a first color. In practice, the motif 14 can, for example, represent a value number, a portrait, or another graphic motif. Within the motif 14, a movement effect in a second color is visible in a partial area 16. For example, when the banknote 10 is tilted, a light-colored bar can move back and forth along the curved partial area 16, creating a so-called rolling bar effect. The areas of different colors (first and second colors) and different effects (three-dimensional motif or moving bar) are precisely registered to one another. This registration is also referred to below as color-to-effect registration.

[0054] For further explanation, the security element 12 contains with reference to the cross section of the Fig. 2 a flat end-product carrier 18, the surface area of ​​which defines an xy plane and a z-axis perpendicular thereto. Arranged on the end-product carrier 18 is a multicolored reflective surface region 20 containing two embossed structure regions 24, 34 arranged in the z-direction at two specific, different heights relative to the flat carrier 18. In the exemplary embodiment, the different heights of the embossed structure regions 24, 34 are defined by the different heights of the base surfaces of the micromirror arrangements 24, 34 above the carrier 18.

[0055] In the exemplary embodiment, the two embossed structure regions each represent micromirror embossments or micromirror arrangements 24, 34, which are formed from a plurality of micromirrors inclined relative to the xy plane. The local inclination angles of the micromirrors are selected precisely so that the relief structure of the micromirror arrangements 24, 34, together with the respective color coating, create a desired optical appearance, such as the bulging three-dimensional impression of motif 14 or the rolling bar effect of subregion 16.

[0056] To create the desired appearance of the security element 12 with two independently selectable colors, the micromirror arrays 24, 34 are each provided with a reflection-enhancing color coating 26, 36, which creates the different color impression of the micromirror arrays in reflection for an observer. In the exemplary embodiment shown, the micromirror arrays 24, 34 are coated with differently colored reflective metals 26, 36, for example, aluminum and copper. However, the different color impression can also be created in other ways, for example by combining a metallization (for example, made of aluminum or silver) that reflects essentially uniformly across the entire visible spectral range with a translucent color, as explained in more detail elsewhere.

[0057] The micromirror arrays 24, 34 each represent embossed structures that are embossed into a previously applied embossed lacquer layer 22, 32. Depending on the desired color effects, the embossed lacquer layers 22, 32 can be colorless, transparent, or colored.

[0058] The security element 12 is designed for viewing from above (or in reflection), in this case from the side facing away from the carrier 18. The micromirror arrangement 24 further away from the observer is therefore also referred to as the lower micromirror arrangement, and the micromirror arrangement 34 closer to the observer is referred to as the higher micromirror arrangement.

[0059] The two micromirror arrangements 24, 34 of the embodiment are arranged one above the other, wherein the higher micromirror arrangement 34 has at least one large-area recess 42, for example in the form of a 5 mm wide and 2 cm long curved strip ( Fig. 1 ). In the area of ​​the recess 42, the observer looks at the lower micromirror arrangement 24 with its colored coating 26, while the visual impression of the surface area 20 in the area 44 outside the recess 42 is determined by the higher micromirror arrangement 34 with the colored coating 36.

[0060] When viewing the security element 12 in reflection, the observer perceives the motif 14 generated by the micromirror arrangement 34 in the areas 44 outside the recess 42 with a first color, which is determined by the color of the color coating 36 and the color or colorlessness of the embossing lacquer layer 32.

[0061] Within the recess 42, a movement effect occurs, in which, for example, when the banknote 10 is tilted, a bright bar of a second color appears within the curved partial area 16 ( Fig. 1 ) appears to run back and forth. The second color is determined by the color of the color coating 26 and the color or colorlessness of the embossing lacquer layer 22. The height difference between the two micromirror arrangements 24, 34 is in the range of a few micrometers or a few tens of micrometers and is therefore imperceptible to the observer. The two differently colored motifs and the different effects 14, 16 therefore appear to the observer to be arranged in exact registration with one another.

[0062] The inventive production of such security elements will now be described with reference to the Figuren 3 bis 5 described in more detail, wherein intermediate steps of a first advantageous process with reference to the Fig. 3(a)-(c) and Fig. 4(a)-(e) and intermediate steps of a second advantageous procedure with reference to the Fig. 3(a)-(c) and Fig. 5(a)-(d) be described.

[0063] First, with reference to Fig. 3(a) A production substrate 30 is provided whose surface exhibits low adhesion to embossing lacquer and high adhesion to metal. The surface area of ​​the production substrate 30 defines an xy plane and a z axis perpendicular to it. The production substrate 30 is preferably a plastic film. In particular, it exhibits a smooth surface or a surface with reduced adhesion.

[0064] In a surface area 20 of the production carrier 30, a first embossing lacquer layer 32 is applied to the surface in the desired partial areas and a first embossing in the form of the desired micromirror embossing 34 is embossed into the embossing lacquer layer 32, as in Fig. 3b shown. In the surface area 20, on the one hand, lacquer areas 52 with an embossed embossing lacquer layer 32, 34 and, on the other hand, free areas 54 without an embossing lacquer layer are created, wherein the free areas 54 correspond to the desired recesses 42 in the finished security element ( Fig. 2 ) and the lacquer areas 52 correspond to the desired areas 44 outside the recesses 42. To ensure that the desired free areas 54 are created on the surface in addition to the lacquer areas 52, the wetting properties of the embossing lacquer are selected or adjusted accordingly both on the production carrier 30 and on the embossing tool itself (not shown).

[0065] The embossing lacquer layer 32 can be applied, in particular, by screen printing, offset printing, flexographic printing, or gravure printing. The embossing lacquer can be, in particular, UV lacquer, a thermoplastic lacquer, or a dual-cure system, i.e., a combination of UV embossing lacquer and thermoplastic lacquer.

[0066] After applying and embossing the first embossing lacquer layer 32, the surface area 20 is metallized over its entire surface, for example, with an aluminum layer. Metallization is preferably carried out by vapor deposition (PVD, CVD). Through the full-surface metallization, the metal layer 36 is applied in the free areas 54 on the surface of the production carrier 30, and in the lacquer areas 52 on the first embossed embossing lacquer layer 32, 34, so that a first reflective embossed structure is created in the lacquer areas 52 at a first height level H1, as shown in Fig. 3(c) The printed and / or cured first embossing lacquer layer 32 in the lacquer region 52 adheres approximately 10 times worse to the production carrier 30 than the vapor-deposited first reflection-enhancing layer 36 (4 to 8 N / m compared to 50 to 90 N / m).

[0067] The structure formed in this way in the surface area 20 is referred to here as the primary structure, which is subsequently supplemented with a structure referred to as the secondary structure, which in turn has a second, embossed and metallized embossing lacquer layer located inside the finished product and an external (end) product carrier.

[0068] In the first described variant of the Fig. 4 For this purpose, a full-surface second embossing lacquer layer 22 is applied to the primary structure of the Fig. 3(c) applied, as in Fig. 4(a) shown, and this second embossing lacquer layer 22 is then provided with the second embossing in the form of the desired micromirror embossing 24, as shown in Fig. 4(b) shown.

[0069] Subsequently, the surface area 20 is metallized again over its entire surface, for example with a copper layer, and thereby a second metal layer 26 is applied over its entire surface to the embossed second embossing lacquer layer 22, 24, so that a second reflective embossed structure is created there at a second height level H2, as in Fig. 4(c) shown.

[0070] Then the final product carrier 18 is provided and bonded to the metallized embossing lacquer layer 22 by means of an adhesive layer 19, as shown in Fig. 4(d) The final product carrier 18 and the adhesive layer 19 are selected such that the adhesion between the target substrate 18, the adhesive layer 19, and the metallization 26 is greater than the adhesion between the production carrier 30 and the embossing lacquer layer 32 or metallization 36.

[0071] Subsequently, the production carrier 30 is subtracted from the combination structure thus formed 56, see Fig. 4(d) . Due to the high adhesion of the production carrier 30 to the vapor-deposited metal and the low adhesion of the production carrier to the embossing lacquer, the metal located in the free areas 54 is removed together with the production carrier during stripping 56, while the embossing lacquer 32 and thus also its metallization 36 remains in the lacquer areas 52 in the combination structure, as in Fig. 4(e) shown. The embossing lacquer 32 of the lacquer areas 52 thus forms a lift-off protection for the embossing lacquer metallization and ensures partial demetallization of the metal layer 36 only in the free areas 54.

[0072] After removing the production carrier 30, an optional etching step is carried out in which any metal residues on the exposed surface are removed.

[0073] The first reflection-enhancing coating 36 has so far been described as a colored metal layer, which is therefore also referred to as a colored coating. However, as already indicated in this and the subsequent embodiments, the reflection-enhancing coating(s) 36 (36, 26) can also be designed differently. Instead of a metal layer, a color-imparting HRI layer can also be used. Likewise, the (or one of the) reflection-enhancing coatings 26, 36 can be formed by an achromatic reflection-enhancing partial layer, such as a metal layer or HRI layer, and a translucent colored partial layer (located above it as seen from the viewer).

[0074] Also not separately depicted are designs in which a first reflection-enhancing layer only creates a color effect in conjunction with additional layers. When the production substrate is removed, at least one of the additional layers remains in the combination structure with its two embossed structures. Alternatively or additionally, one of the additional layers is not removed when the first reflection-enhancing layer is removed by etching. Fig. 3c the further layers would lie (in the free areas 54 and the lacquer areas 52) on the first reflection-enhancing layer 36, in Fig. 4c i.e., between the first reflection-enhancing layer 36 and the second embossing lacquer layer 22. The first reflection-enhancing layer can serve as a reflector or as an absorber of a color-imparting multilayer structure, which, for example, creates a colored effect as an absorber-dielectric-absorber or reflector-dielectric-absorber. Likewise, the reflection-enhancing layer could be an HRI layer of a color-imparting refractive index-based multilayer structure consisting of transparent sublayers with different refractive indices. By removing the first reflection-enhancing layer, the multilayer structure loses its colored effect. The color of the multilayer structure and the reflectivity of the reflection-enhancing layer can thus be removed simultaneously (and in register) in the free areas 42.

[0075] The different color effects of the first and / or the second relief structure of the combination structure could - in all embodiments also of the other figures, which in turn also comprise color-imparting embossing lacquer or adhesive layers - be achieved in one of the ways mentioned or in different ways of the ways mentioned.

[0076] The aforementioned etching step may be mandatory in other embodiments in which the metal layer 36 remains on the embossing resist in the exposed areas 54 during stripping. In the other embodiments, the reflection-enhancing layer in the exposed areas is only removed by etching.

[0077] Subsequently, the surface exposed by removing the production carrier 30 can be coated with a protective lacquer layer 48 ( Fig. 2 ) or a thin, transparent (PET) film can be laminated on. Depending on the intended use of the security element, for example, as a security thread for embedding in security paper, further conventional production steps may be required for completion, such as coating with a heat-sealing varnish.

[0078] As explained above, the terms "deeper relief structure" and "higher relief structure" refer to the position of the relief structures in the finished security element ( Fig. 2 ) relative to an observer. The designations therefore do not reflect the order in which the relief structures are applied during production. Since the security element is designed specifically for viewing from the side of the later-removed production substrate, the (later) higher-lying relief structure is first created on the production substrate during the described production process, followed by the (later) lower-lying relief structure.

[0079] Returning to the primary structure of the Fig. 3(c) This can also be done in the Fig. 5 shown type can be supplemented with a secondary structure.

[0080] In this process variant, a final product carrier 18 is first provided and printed over its entire surface with a second embossing lacquer layer 22. The second embossing lacquer layer 22 is then provided with the second embossing in the form of the desired micromirror embossing 24 and metallized over its entire surface, for example with a copper layer, in order to apply the second metal layer 26, as in Fig. 5(a) shown.

[0081] Then, a laminating lacquer 60 is applied to the metallization 36 of the production carrier 30 or to the metallization 26 of the final product carrier 18 or to both metallizations 26, 36. The laminating lacquer can be clear transparent or colored transparent. Fig. 5(b) As an example, the variant of applying the laminating varnish 60 only to the metallization 36 of the production carrier 30 is shown.

[0082] Subsequently, the primary structure of the Fig. 5(b) and the secondary structure of the Fig. 5(a) registered laminated together so that the two metallizations 26, 36 are separated by the laminating adhesive 60, as in Fig. 5(c) shown.

[0083] Here, too, care is taken to ensure that the adhesion between the final product carrier 18, the second embossing lacquer layer 22 and the metallization 26 is greater than the adhesion between the production carrier 30 and the embossing lacquer layer 32 or metallization 36. The production carrier 30 can, in particular, be provided with a roughened surface so that the upper surface of the metallization 36 to the laminating lacquer 60 is smoother than the lower surface of the metallization 36.

[0084] Finally, the production carrier 30 is subtracted 56 from the combination structure thus formed, as in Fig. 5(c) shown. Due to the high adhesion of the production carrier 30 to metal and the low adhesion of the production carrier to embossing lacquer, the metal located in the free areas 54 is removed together with the production carrier during stripping 56, while the embossing lacquer 32 and thus also its metallization 36 remains in the lacquer areas 52 in the combination structure, as shown in Fig. 5(d) shown. In this process variant, the embossing lacquer 32 of the lacquer areas 52 also forms a lift-off protection for the embossing lacquer metallization and ensures partial demetallization of the metal layer 36 only in the free areas 54.

[0085] In the second process variant, an etching step can also be carried out after the removal of the production carrier 30. In this etching step, in the embodiment according to Fig. 5 Any metal residue on the exposed surface must be removed. Analogous to Fig. 4 However, in other designs with laminating adhesive, removal of the first reflection-enhancing layer would only be conceivable by etching.

[0086] The surface exposed by removing the production carrier 30 can be further coated with a protective lacquer layer to improve the circulation resistance of the security element, or a thin, transparent (PET) film can be laminated onto it. Depending on the intended use of the security element, for example, as a security thread for embedding in security paper, further, conventional production steps can be carried out for completion, again for example, the application of heat-sealing lacquer.

[0087] For additional security, the designs described may be provided with negative markings, for example, in the form of text, symbols, or value numbers. The negative markings are intended for viewing in a transparent manner.

[0088] Figur 6 shows a security element 70 which, like the security element of the Fig. 2 according to the first process variant, but with additionally introduced negative markings 72, 74. The first negative markings 72 are provided in the free areas 54 of the surface area 20, in which only the second embossed structure 22, 24, 26 is present, and are formed by a partial demetallization of the second color coating 26. If the second embossing lacquer layer 22 is colorless and transparent, the negative markings 72 also appear colorless and transparent, whereas in the case of a colored second embossing lacquer layer 22, the negative markings 72 appear with the transparent color of the embossing lacquer layer 22.

[0089] The second negative markings 74 are provided in the lacquer regions 52 of the surface region 20 where the two embossed structures overlap, and are formed by partial demetallization of both the first color coating 36 and the second color coating 26. If both embossing lacquer layers 22, 32 are colorlessly transparent, the negative markings 74 also appear colorlessly transparent. If one of the two embossing lacquer layers 22, 32 is colored and the other is colorlessly transparent, the negative markings 74 appear with the transparent color of the colored embossing lacquer layer. If both embossing lacquer layers 22, 32 are colored, the negative markings 74 appear with a transparent color resulting from subtractive color mixing of the colors of the embossing lacquer layers 22, 32.

[0090] Figur 7 shows a security element 80 which is produced according to the second method variant of Fig. 5 , but with additionally introduced negative markings 82, 84. The first negative markings 82 are provided in the free areas 54 of the surface area 20, in which only the second embossed structure 22, 24, 26 is present, and are formed by a partial demetallization of the second color coating 26. If the laminating varnish 60 is colorless and transparent, the negative markings 82 also appear colorless and transparent. In the case of a colored laminating varnish 60, the negative markings 82 appear with the transparent color of the laminating varnish 60.

[0091] The second negative markings 84 are provided in the lacquer regions 52 of the surface region 20 in which the two embossed structures overlap, and are formed by partial demetallization of both the first color coating 36 and the second color coating 26. If the embossing lacquer layer 32 and the laminating lacquer 60 are colorless and transparent, the negative markings 84 also appear colorless and transparent. If one of the two layers (embossing lacquer layer 32, laminating lacquer 60) is colored and the other is colorless and transparent, the negative markings 84 appear with the transparent color of the colored layer. If both the embossing lacquer layer 32 and the laminating lacquer 60 are colored, the negative markings 84 appear with a transparent color resulting from subtractive color mixing of the colors of the two layers 32, 60. Bezugszeichenliste

[0092] 10 Banknote 12 Security element 14 Motif 16 Partial area 18 End product carrier 20 Reflective surface area 22 Second embossing lacquer layer 24 Second embossing structure 26 Second coating 30 Production carrier 32 First embossing lacquer layer 34 First embossing structure 36 First coating 42 Cutout 44 Area outside the cutout 48 Protective lacquer layer 52 Lacquer areas 54 Free areas 60 Laminating lacquer 70 Security element 72, 74 Negative mark 80 Security element 82, 84 Negative mark

Claims

1. Method for producing an optically variable security element (12), wherein - a production carrier (30) is provided, the planar extent of which defines a z-axis perpendicular thereto; - one area (20) on the surface of the production carrier sees the application of a first embossing varnish layer (32) only in portions, with the result that varnish regions (52) with an embossing varnish layer and clear regions (54) without embossing varnish layer are created in the area; - the applied first embossing varnish layer (32) is provided with a first embossing (34) at a first height; - a first coating (36) is applied to the area (20) in the clear regions (54) and in the varnish regions (52); - a further layer is applied to the area (20) in the clear regions (54) and optionally in the varnish regions (52); and - the first coating (36) is removed from the clear regions (54) again; characterized in that - the production carrier (30) is stripped away; - the further layer is a second embossing varnish layer (22) provided with a second embossing (24) - at a second height spaced apart from the first height in the z-direction - with the result that a combination structure having the two embossings (34, 24) at two heights is created; and - the first embossing varnish layer (32) prevents a removal of the first coating (36) in the varnish regions (52) during or after the stripping of the production carrier (30) from the combination structure.

2. Method according to Claim 1, characterized in that the first embossing varnish layer (32) remains in the combination structure in the varnish regions (52) when the production carrier (30) is stripped away, in particular since the said first embossing varnish layer adheres less to the production carrier (30) than the first coating (36); and / or the first coating (36) is stripped off with the production carrier (30) in the clear regions (54) and thus removed, in particular since the first coating (36) adheres more to the production carrier (30) than the embossing varnish layer (32) adheres to the production carrier (30) and / or the first coating (36) adheres to the second embossing varnish layer (22).

3. Method according to Claim 1 or 2, characterized in that the first embossing varnish layer (32) prevents the removal of the first coating (36) in the varnish regions (52) after the production carrier has been stripped off, in particular by virtue of having greater resistance to an etching means than the first coating (36); and / or the first coating (36) or a residue of the first coating (36) is removed by etching from the clear regions (54) after the production carrier has been stripped off.

4. Method according to any of Claims 1 to 3, characterized in that the first coating (36) is a reflection-enhancing coating which follows the first embossing (34); wherein, preferably, a second reflection-enhancing coating (26) follows the second embossing (24).

5. Method according to any of Claims 1 to 4, characterized in that the combination structure comprises a first and a second relief structure (32, 36; 22, 26) which have different colour effects and are preferably reflective, in particular formed in each case by the first and, respectively, second embossing varnish layer, the first and, respectively, second reflection-enhancing layer and an optional colour layer.

6. Method according to any of Claims 1 to 5, characterized in that a product carrier (18) of the combination structure (24, 34) is applied, with, preferably, at least the first embossing varnish layer (32), in particular only the first or both embossing varnish layers (32, 22), being arranged between the product carrier (18) and the production carrier (30).

7. Method according to Claim 6, characterized in that the product carrier (18) is a final product carrier which forms part of the optically variable security element (12), or the product carrier (18) is a transfer product carrier on which the optically variable security element (12) is detachably arranged.

8. Method according to any of Claims 1 to 7, characterized in that the second embossing varnish layer (22) is applied and then provided with the second embossing (24); with preferably the second embossing varnish layer (22) following the second embossing (24) with one surface and following the first embossing (34) with the second surface, and / or the embossed second embossing varnish layer being provided with the second reflection-enhancing coating and / or a product carrier (18) being provided and connected via an adhesive layer (19) to the embossed second embossing varnish layer (22), which has been coated in particular.

9. Method according to any of Claims 1 to 7, characterized in that an embossed second embossing varnish layer (22) is provided, in particular on a product carrier (18), and applied by means of an adhesive layer (60), in particular a laminating adhesive layer; with in particular the second embossing varnish layer (22) on the product carrier (18) being provided with the second embossing in advance and / or the embossed second embossing varnish layer being provided with the second reflection-enhancing layer in advance and / or the adhesive layer (60) following the second embossing (24) with one surface and following the first embossing (34) with the second surface.

10. Method according to any of Claims 1 to 9, characterized in that the first embossing varnish layer (32) and / or the second embossing varnish layer (22) is a transparent embossing varnish layer or an embossing varnish layer with a glazed colouration.

11. Method according to any of Claims 1 to 10, characterized in that the first coating (36) and / or the second reflection-enhancing coating (26) is a reflection-enhancing colour coating, in particular formed by a coloured metallization, by a colour-giving HRI layer, by a colourtilting or colour-filtering reflective multi-layer construction or by a glazed and / or luminescent colour deposited on a reflective structure; or the first coating (36), which is a reflection-enhancing coating, and / or the second reflection-enhancing coating (26) reflects in colour by way of a substructure, in particular a sub-wavelength structure or interference structure, of its embossing (34, 24); or a separate first and, respectively, second glazed colour layer are provided for the first coating (36), which is a reflection-enhancing coating, and / or for the second reflection-enhancing coating (26).

12. Method according to any of Claims 1 to 11, characterized in that the varnish regions (52) and clear regions (54) are formed as a regular or irregular grid with grid elements and grid interspaces, at least in a portion of the area, with the dimensions of the grid elements in one or both lateral directions being less than 140 µm, preferably between 20 µm and 100 µm and in particular between 20 µm and 60 µm, with, preferably, the grid formed by the varnish regions (52) and clear regions (54) being formed by the grid elements with a constant area coverage which is expediently between 30% and 70%, preferably between 40% and 60% and in particular at approximately 50%.

13. Method according to any of Claims 1 to 12, characterized in that the varnish regions (52) and clear regions (54) are formed as an effect region in at least a portion of the area (20), in which effect region the varnish regions and / or the clear regions have lateral dimensions of more than 140 µm, with, preferably, at least one varnish region (52) and / or at least one clear region (54) being formed with lateral dimensions of more than 250 µm, preferably more than 500 µm and in particular more than 1 mm.

14. Method according to any of Claims 1 to 13, characterized in that the embossings (24, 34) of the combination structure provided with reflection-enhancing coatings (26, 36) form micromirror arrangements with directed micromirrors, in particular with plane mirrors, concave mirrors and / or Fresnel-like mirrors, with the lateral dimensions of the micromirrors advantageously being less than 50 µm, preferably less than 20 µm and particularly preferably less than 10 µm.

15. Method according to any of Claims 1 to 14, characterized in that transmissive negative features (72, 74) are formed in the varnish regions (52) and / or in the clear regions (54) of the reflective area (20), in particular by virtue of congruent cutouts being created in the first and second reflection-enhancing coating in the varnish regions and / or cutouts being created in the second reflection-enhancing coating in the clear regions.