Pigment-coated glass substrate for a cooktop

DE502021005605D1Active Publication Date: 2024-11-21SCHOTT AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502021005605
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-22
Publication Date
2024-11-21
Estimated Expiration
2041-03-22

AI Technical Summary

Technical Problem

Existing pigment-coated glass substrates for hobs suffer from high image grain, which affects the visibility of displays, especially 7-segment displays, due to pigment agglomeration, leading to non-homogeneous surfaces and reduced visibility of high-resolution displays.

Method used

A pigment-coated glass substrate with a layer system comprising a matrix of silicon, carbon, and oxygen, incorporating organic or inorganic pigments and optionally graphite, where the image grain size is controlled to 35% or less, achieved through a specific method involving the preparation of a first component and a color paste with a controlled ratio of film former to silicone, applied to a glass substrate.

Benefits of technology

The solution provides a glass substrate with reduced image grain, ensuring good visibility of displays, maintaining transparency, and being cost-effective to produce, while preventing the view into the hob's interior.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a special pigment-coated glass substrate for a hob, a special method for producing a pigment-coated glass substrate, and a pigment-coated glass substrate for a hob which can be produced by the special method. State of the art

[0002] Semi-transparent coatings on glass and glass-ceramic are known from the prior art and are used, for example, in display areas on cooking surfaces. 7-segment displays are used particularly in cooktops. These display, for example, indicate the heating level or indicate with a dot which cooking zones have higher temperatures. Furthermore, displays can be arranged beneath the glass substrate to display complex information, such as graphics, images, or similar.

[0003] Due to the variety of possible color impressions and designs, the use of transparent glass substrates for cooking surfaces has become established in recent years. However, transparent glass ceramic has the disadvantage that the components beneath the cooking surface are visible. To ensure appropriate opacity, the glass substrate can be coated with a variety of layers, as is known from the prior art. Typically, the glass substrate is first coated with a color-imparting layer (hereinafter referred to as layer B) and then with a sealing layer. To ensure the visibility of a 7-segment display or other display mounted beneath the cooking surface, a semi-transparent layer (hereinafter referred to as layer A) is required in this area.This must ensure sufficient opacity, but allow the red light of the 7-segment display, for example, to pass through and have no scattering centers in the visible wavelength range.

[0004] Semitransparent layers with various colorants are known from the prior art. Colorants can be selected from pigments (insoluble) or dyes (at least partially soluble). However, dyes have the disadvantage that they are not very heat-resistant, and some effects can only be achieved with pigments. Since color-imparting layers with pigments are used under the heating elements due to their heat resistance and a homogeneous visible image is desired, these pigments should also be used in the semitransparent layer. The transparency can also be adjusted by adding graphite. Layers, both with colorants and pigments, can have a high light absorption capacity. In addition, the scattering of the layers impairs the visibility of the indication or display. Layers containing a pigment are known, for example, from EP 2 223 900 A1.Further special coated glass substrates are disclosed in WO 2004 / 085555 A2, WO 2011 / 144671 A1 and WO 2014 / 086619 A2.

[0005] One aspect that has received little attention to date is the image grain (also called granularity) of the layer. While in dye layers the dyes are homogeneously dissolved in the matrix, in layers containing solids, e.g. pigments, solids can clump together, causing evenly semi-transparent surfaces to become fragmented. The term image grain refers to local brightness fluctuations in a translucent or translucent surface. The effect of image grain is similar to the grain of film in photography or image noise in digital photography. 7-segment displays or displays arranged beneath layers with high image grain are less recognizable. As a result, details on high-resolution displays are no longer recognizable, and very small 7-segment displays are difficult to realize.

[0006] The object of the present invention is to provide a pigment-coated glass substrate for a hob which: enables good visibility of the display, has a defined transparency; and / or is inexpensive to manufacture. Description of the invention

[0007] The present invention comprises a pigment-coated glass substrate for a cooktop, comprising: i) a glass substrate, wherein the glass substrate comprises a glass or a glass ceramic, preferably consisting of a glass or a glass ceramic; and ii) a layer system comprising: a layer A containing: a) a matrix, wherein the matrix contains silicon, carbon and oxygen, b) a pigment, preferably an organic or inorganic pigment, more preferably an effect pigment, and c) optionally graphite, wherein the layer A has an image grain of 35% or less; and wherein the pigment-coated glass substrate is obtainable by a process wherein layer A is formed on the glass substrate by the following steps: i) preparing a first component by: 1) mixing a first mixture comprising: a) a compound of the formula Si(OR 4< ) x (OC=OR 5< ) y R 6< 4-xy , where x+y is 1 to 4, where R 4< to R 6< are independently selected from an organic radical having 1 to 20 carbon atoms, -OH and -H; b) a hydrolysis catalyst;c) water; and d) optionally silicone; 2) concentrating the first mixture under reduced pressure and optionally elevated temperature; and 3) optionally adding silicone; to obtain a first component; ii) preparing a color paste by mixing a second mixture containing: a) the first component; b) pigment; c) optionally graphite; d) solvent; and e) silicone; to obtain a color paste; and wherein the color paste contains a proportion of 10 to 60 wt.% silicone, and wherein the ratio of film former [wt.%] / silicone [wt.%] has a value of 0.2 or more and 0.8 or less, wherein the film former has the following formula: Si(OR 4< ) x (OC=OR 5< ) y R 6< 4-xy , where x, y and R 4< to R 6< are as defined above; iii) applying the color paste to a glass substrate; and iv) drying the applied color paste to obtain a pigment-coated glass substrate.

[0008] Also disclosed is a pigment-coated glass substrate for a cooktop, comprising: i) a glass substrate, wherein the glass substrate comprises a glass or a glass ceramic, preferably consists of a glass or a glass ceramic; and ii) a layer system comprising: a layer A containing: a) a matrix, wherein the matrix contains silicon, carbon and oxygen, b) a pigment, preferably an organic or inorganic pigment, more preferably an effect pigment, and c) optionally graphite, wherein the layer A has an image grain of 35% or less.

[0009] Furthermore, the invention relates to a method for producing a pigment-coated glass substrate, wherein a layer A is formed on the glass substrate by the following steps: i) Preparing a first component by: 1) mixing a first mixture containing: a) a compound of the formula Si(OR 4< ) x (OC=OR 5< ) y R 6< 4-xy , where x+y is 1 to 4, where R 4< to R 6< are independently selected from an organic radical having 1 to 20 carbon atoms, -OH and -H; b) a hydrolysis catalyst; c) water; and d) optionally silicone; 2) concentrating under reduced pressure and optionally elevated temperature the first mixture; and 3) optionally adding silicone; to obtain a first component; ii) Preparing a color paste by mixing a second mixture containing: a) the first component; b) pigment; c) optionally graphite; d) solvent; and e) silicone; to obtain a color paste; and wherein the color paste contains a proportion of 10 to 60 wt.% silicone, and wherein the ratio of film former [wt.%] / silicone [wt.-%] has a value of 0.2 or more and 0.8 or less, wherein the film former has the following formula: Si(OR 4< ) x (OC=OR 5< ) y R 6< 4-xy , wherein x, y and R 4< to R 6< are as defined above; iii) applying the color paste to a glass substrate; and iv) drying the applied color paste to obtain a pigment-coated glass substrate. .

[0010] Furthermore disclosed herein is a pigment-coated glass substrate obtainable by a method described herein.

[0011] A further embodiment of the invention is a cooking hob, an oven, a fireplace viewing window, a microwave, preferably a cooking hob, more preferably a cooking hob containing a 7-segment display or a display comprising a pigment-coated glass substrate as described herein. Definitions

[0012] Unless otherwise specified, all percentages refer to weight percent. The weight percent values ​​for the glass substrate refer to the oxide-based glass composition. Unless explicitly stated, all weight percents refer to the initial weights. The skilled person is aware that during the production of the color paste and during its curing, the weighed components react at least partially.

[0013] Herein, any expression in the singular is intended to include the plural, and any expression in the plural is intended to include the singular, unless otherwise stated. In particular, all limitations and preferred embodiments of one layer (e.g., layer A) also apply to another layer (e.g., layer B), unless otherwise stated. Furthermore, all limitations and preferred embodiments of the pigment-coated glass substrate also apply to the method for producing a pigment-coated glass substrate, and vice versa, unless otherwise stated. Preferred embodiments of a pigment-coated glass substrate described herein also apply to all pigment-coated glass substrates described herein, unless otherwise stated.

[0014] Herein, R 1< to R 6< are independently selected from an organic radical having 1 to 20 carbon atoms, -OH and -H.

[0015] Preferably, R 1< to R 6< are independently selected from a list consisting of alkyl, heteroalkyl, cycloalkyl, alkyl-cycloalkyl, heteroalkyl-cycloalkyl, heterocycloalkyl, alkyl-heterocycloalkyl, heteroalkyl-heterocycloalkyl, aryl, alkyl-aryl, heteroalkyl-aryl, heteroaryl, alkyl-heteroaryl, heteroalkyl-heteroaryl, -OH and H; more preferably from unsubstituted alkyl, heteroalkyl, alkyl-cycloalkyl, heteroalkyl-cycloalkyl, heterocycloalkyl, alkyl-heterocycloalkyl and heteroalkyl-heterocycloalkyl; more preferably unsubstituted alkyl; more preferably methyl and ethyl.

[0016] Each radical R 1< to R 6< can be independently substituted or unsubstituted, preferably unsubstituted. Possible substituents are, for example, halogens (e.g., F, Cl, Br, and / or I), an alkoxy group (e.g., methoxy or ethoxy), -NH 2 , and -OH. Furthermore, each radical R 1< to R 6< can independently be linear or branched; preferably, each radical is linear. Preferably, R 1< and R 2< are the same. Preferably, R 4< and R 5< are the same, more preferably, R 4< to R 6< are the same.

[0017] Herein, the variables x and y are independently selected from 1 to 4, preferably 2 to 4, more preferably 3 or 4. Preferably, x is 3 or 4 and y is 0 or 1, more preferably y is 0. Glass substrate

[0018] According to the invention, the glass substrate comprises a glass or a glass ceramic. Preferably, the glass substrate consists of a glass or a glass ceramic.

[0019] The glass is preferably a borosilicate glass or aluminosilicate glass, more preferably a borosilicate glass; more preferably comprising, more preferably consisting of, in wt.%: SiO2 50 - 90, preferably 60 - 74; B2O3 5 - 15, preferably 8 - 12; X 2 O 1 - 15, preferably 5 - 10, where X is selected from Na, K and / or Li; Al2O3 0 - 15, preferably 3 - 8; YO 0 - 15, preferably 1 - 5, where Y is selected from Ca, Sr and / or Mg; ZnO 0 - 5, preferably 0.1 to 2; TiO2 0 - 10, preferably 0.1 to 5; ZrO2 0 - 5, preferably 0.1 to 2; SnO2 0 - 1, preferably 0.01 to 0.05; P2O5 0 - 5, preferably 0.01 to 2; Moss 0 - 1, preferably 0.001 to 0.05; Fe 2 O 3 0 - 0.1, preferably 0.001 to 0.05; V2O5 0 - 0.1, preferably 0.001 to 0.05; Nd2O3 0 - 0.1, preferably 0.001 to 0.05; Additives 0 - 2; and unavoidable contamination.

[0020] The glass ceramic is preferably a LAS glass ceramic, more preferably a transparent, colored LAS glass ceramic, preferably containing as coloring components 0.003 - 0.5 wt.% MoO 5 and / or less than 0.2 wt.% Nd 2 O 3 and / or less than 0.015 wt.% V 2 O 5 . Preferably, the composition comprises, more preferably the composition of the glass ceramic consists of, in wt.%: Li2O 2,5 - 5,5; Σ Na 2 O + K 2 O 0,1 - 4; MgO 0 - 3; Σ CaO + SrO + BaO 0 - 5; ZnO 0 - 4; B2O3 0 - 3; Al2O3 16 - 26; SiO2 58 - 72; TiO2 1,5 - 5,5; ZrO2 0 - 2,5; SnO2 0,1 - 0,7; Σ TiO 2 + ZrO 2 + SnO 2 3 - 6,5; P2O5 0 - 5; MoO 3 0,003 - 0,5; Fe 2 O 3 0 - 0,25; V2O5 0 - 0,015; Nd2O3 0 - 0,02; Additives 0 - 2; and unavoidable contamination.

[0021] The glass substrate optionally contains additives such as chemical refining agents, e.g. As 2 O 3 , Sb 2 O 3 , CeO 2 , and / or refining additives, e.g. manganese oxide, sulfate, halide compounds (F, Cl, Br), in total contents of up to 2.0 wt.%. Compounds of a large number of elements such as the alkalis Rb, Cs or elements such as Mn, Hf are common impurities in batch raw materials used on an industrial scale. Other compounds such as those of the elements W, Nb, Ta, Y, rare earths, Bi, V, Cr, Ni can also be present as impurities in batch raw materials used on an industrial scale, typically in the ppm range. For reasons of environmental protection and occupational health and safety, the use of toxic or questionable raw materials is avoided wherever possible.Therefore, the glass substrate is preferably free of environmentally harmful substances such as arsenic (As), antimony (Sb), cadmium (Cd), lead (Pb), cesium (Cs), rubidium (Rb) halides and sulfur (S), apart from unavoidable impurities in the range of preferably 0 to less than 0.5 weight percent, more preferably less than 0.1 weight percent, most preferably less than 0.05 weight percent.

[0022] In general, either naturally occurring raw materials or chemically processed or synthetically produced raw materials can be used for production. Naturally occurring raw materials are generally more cost-effective than equivalent chemically processed or synthesized raw materials. However, the usability of natural raw materials is limited by the typically high levels of impurities they contain. Examples of naturally occurring raw materials are quartz sand, spodumene, and petalite. Chemically processed or synthetically produced raw materials generally contain very few impurities. Examples of commonly processed or synthesized raw materials are lithium carbonate or titanium dioxide powder.The upper limit of contamination by typical trace elements in the technical raw materials used is usually 30 ppm Cl, 1 ppm CoO, 3 ppm Cr 2 O 3 , 200 ppm Cs 2 O, 3 ppm CuO, 200 ppm F, 400 ppm HfO 2 , 3 ppm NiO, 500 ppm Rb 2 O, 5 ppm V 2 O 5 . Shift system

[0023] The pigment-coated glass substrate for a hob comprises a layer system comprising a layer A containing: a) a matrix, wherein the matrix contains silicon, carbon and oxygen, b) a pigment, preferably an organic or inorganic pigment, more preferably an effect pigment, and c) optionally graphite wherein layer A has an image grain of 35% or less.

[0024] Layer A is preferably produced from a color paste containing an at least partially hydrolyzed film former (first component), pigments, and optionally graphite and / or silicone. The time of addition of pigments and optionally graphite and / or silicone can, in principle, be freely chosen. However, it has proven more economical to first mix the film former, water, and optionally hydrolysis catalyst into a first mixture, then at least partially hydrolyze the film former to obtain a first component; and then subsequently add pigments and optionally graphite and / or silicone to this first component to obtain a color paste, from which layer A is then formed. matrix

[0025] According to the invention, layer A contains a matrix containing silicon, carbon, and oxygen. Preferably, the matrix is ​​a sol-gel matrix. The sol-gel matrix can be produced by a process described herein. The pigments and optionally graphite are held in or by the matrix.

[0026] Layer A is preferably produced from a color paste (see process below for details) comprising one or more at least partially hydrolyzed film formers, hydrolysis catalyst, solvent, pigments and optionally silicone, fillers and graphite. Preferably, a first component is first produced by mixing one or more film formers, hydrolysis catalyst, solvent, water, and optionally fillers and silicone to obtain a first mixture. This first mixture is concentrated to obtain a first component and then one or more pigments and optionally graphite, silicone, solvent and fillers are added and then mixed to obtain the color paste. It is also possible to mix all components at once and then concentrate the mixture to obtain the color paste.

[0027] Whether the cured layer A contains the above-mentioned components depends on the boiling points or decomposition temperatures of the components, as well as the heating temperature and heating duration (see procedure below) of the color paste.

[0028] Preferably, layer A contains only traces (1 wt% or less, preferably 0.1 wt% or less) of solvent, more preferably layer A and / or B contains no solvent.

[0029] In a preferred embodiment, the matrix contains one or more of the following binding motifs: i) [OSiR 1< R 2< ]; where R 1< and R 2< are independently selected from an organic radical having 1 to 20 carbon atoms, -OH and -H, preferably where R 1< and R 2< are the same; ii) [Si-O-Si]; and iii) [O 3 SiR 3< ]; where R 3< is independently selected from an organic radical having 1 to 20 carbon atoms, -OH and -H. This ensures good crosslinking.

[0030] Preferred R 1< to R 3< are defined above. filmmaker

[0031] Suitable film formers include alkyl silicates such as orthosilicic acid, polysilicic acids, esters of orthosilicic acid, or esters of polysilicic acids, optionally containing one or more organic, non-hydrolyzable radicals that are soluble in organic solvents and at least partially hydrolyzable with water. Hydrolysis can be catalyzed by a hydrolysis catalyst (see below). A sol is produced by the reaction of the film former with water. After curing, sols form a solid sol-gel matrix in which the monomers are (cross-)linked. Curing can be accelerated by heating (e.g., 200 °C for 1 h).

[0032] Preferably, layer A is produced from a color paste comprising a film former having the following formula: Si(OR 4< ) x (OC=OR 5< ) y R 6< 4-xy , where x, y and R 4< to R 6< are as defined above.

[0033] Particularly suitable film formers are described in DE 043 38 360 A1 and EP 1 611 067 B1. The film formers methyltriethoxysilane and tetraethoxysilane are particularly preferred.

[0034] Layer A is preferably produced by a color paste which contains 15 wt.% or more, preferably 20 wt.% or more, more preferably 25 wt.% or more, more preferably 30 wt.% or more, more preferably 32 wt.% or more, more preferably 35 wt.% or more, more preferably 40 wt.% or more, more preferably 45 wt.% or more, more preferably 50 wt.% or more; and / or, preferably and, 80 wt.% or less, preferably 75 wt.% or less, more preferably 70 wt.% or less, more preferably 65 wt.% or less, more preferably 60 wt.% or less, more preferably 55 wt.% or less, more preferably 53 wt.% or less, more preferably 50 wt.% or less, more preferably 45 wt.% or less, more preferably 40 wt.% or less; film former. If the ink paste contains a high film-forming agent, the processability of the ink paste is improved and the layer thickness is increased. A low image grain can be achieved particularly well with a low film-forming agent content.The inventors have surprisingly found that if the color paste contains a proportion of 10 to 60 wt.%, preferably 15 to 50 wt.%, more preferably 18 to 40 wt.%, more preferably 20 to 45 wt.%, more preferably 25 to 35 wt.%, of film former, a very low image grain can be achieved. silicone

[0035] The color paste preferably contains a silicone, more preferably a silicone resin. A silicone resin is a viscous silicone. Silicones differ from a dried film-forming agent in a dried color paste in their composition. While a dried color paste (= coating) is solid, silicones are usually clear, colorless, neutral, odorless, hydrophobic liquids.

[0036] Preferably, the molecular mass of the silicone is 100 to 250,000 g / mol, the density is 0.7 to 1.1 g / cm 3 (25°C), and / or the viscosity is 0.5 to 1*10 6 mPa s, preferably 500 to 10,000 mPa s, more preferably 1,000 to 8,000 mPa s, preferably 1,500 to 5,000 mPa s (25°C). A silicone resin has a viscosity of 2,000 mPa s (25°C) or more.

[0037] The silicone can be selected from a cyclic polysiloxane, a linear polysiloxane, a (partially) crosslinked polysiloxane, and a branched polysiloxane, and mixtures thereof. The silicone is preferably a linear polysiloxane. The silicone can be functionalized with various groups, e.g., methoxy or ethoxy. The silicone is preferably a silicone-polyester resin, more preferably an ethoxy-functional silicone-polyester resin. If the silicone contains crosslinkable functional groups, the scratch resistance of the coating can be increased. Therefore, layer A can preferably be produced using a color paste containing a silicone containing crosslinkable functional groups, preferably crosslinkable at 200°C or less.

[0038] According to the invention, the color paste contains a proportion of 10 to 60 wt.% silicone. Furthermore, it is disclosed herein that layer A is preferably produced by a color paste which contains 0.4 wt.% or more, preferably 1 wt.% or more, more preferably 5 wt.% or more, more preferably 10 wt.% or more, more preferably 15 wt.% or more, more preferably 18 wt.% or more, more preferably 20 wt.% or more, more preferably 25 wt.% or more, more preferably 30 wt.% or more, more preferably 31 wt.% or more, more preferably 32 wt.% or more, more preferably 33 wt.% or more, more preferably 35 wt.% or more, more preferably 40 wt.% or more, more preferably 45 wt.% or more, more preferably 50 wt.-% or more; and / or, preferably and, 80 wt% or less, preferably 75 wt% or less, more preferably 70 wt% or less, more preferably 65 wt% or less, more preferably 60 wt% or less, more preferably 55 wt% or less, more preferably 53 wt% or less, more preferably 50 wt% or less, more preferably 45 wt% or less, more preferably 40 wt% or less; more preferably 35 wt% or less; more preferably 30 wt% or less; more preferably 20 wt% or less; more preferably 15 wt% or less; more preferably 10 wt% or less; more preferably 5 wt% or less; silicone. The inventors have surprisingly found that if the color paste contains a proportion of 10 to 60 wt.%, preferably 15 to 50 wt.%, more preferably 18 to 40 wt.%, more preferably 20 to 45 wt.%, more preferably 25 to 35 wt.%, of silicone, a very low image grain can be achieved.To achieve relatively good scratch resistance, a proportion of 50 wt% or less is advantageous.

[0039] The inventors have also recognized that the ratio of film former to silicone in the color paste plays an important role in the image grain. Particularly low values ​​for the image grain could be achieved when the ratio of film former to silicone, ie film former [wt.%] / silicone [wt.%], has a value of 0.2 or more, preferably 0.3 or more, more preferably 0.4 or more, more preferably 0.42 or more, more preferably 0.44 or more, more preferably 0.46 or more, more preferably 0.48 or more, more preferably 0.5 or more; and / or, preferably and; 0.8 or less, preferably 0.7 or less, more preferably 0.6 or less, more preferably 0.58 or less, more preferably 0.56 or less, more preferably 0.54 or less, more preferably 0.52 or less, more preferably 0.5 or less. According to the invention, the ratio of film former [wt%] / silicone [wt%] has a value of 0.2 or more and 0.8 or less. hydrolysis catalyst

[0040] Layer A is preferably produced using a color paste containing a hydrolysis catalyst. The hydrolysis catalyst catalyzes the hydrolysis of the film former. The hydrolysis catalyst is preferably an organic acid or base, preferably an acid, more preferably a sulfonic acid, more preferably p-toluenesulfonic acid.

[0041] Layer A is preferably produced by a color paste which contains 0.001 wt% or more, preferably 0.01 wt% or more, more preferably 0.1 wt% or more, more preferably 0.5 wt% or more, more preferably 1 wt% or more, more preferably 2 wt% or more, more preferably 5 wt% or more; and / or, preferably and, 10 wt% or less, preferably 6 wt% or less, more preferably 2 wt% or less, more preferably 0.2 wt% or less, more preferably 0.02 wt% or less, more preferably 0.002 wt% or less; hydrolysis catalyst. solvent

[0042] Suitable solvents, particularly for producing a screen-printable ink paste, are low-volatility solvents such as C3-C20 glycol ethers, C4-C20 alcohols, C7-C12 alkanes, C5-C20 ethers, e.g. diethylene glycol monomethyl ether, butyl carbitol acetate, terpineol, methoxypropanol (VD = 38), butyl glycol (VD = 165) or butyl diglycol (VD > 1200); preferably with an evaporation number (VD) above 35 and a boiling point above 120 °C (VD diethyl ether = 1). The low-volatility, high-boiling solvents have the task of keeping the ink paste liquid in the screen, i.e. processable. Secondly, it is important that the concentration in the ink paste remains constant during processing so that reproducible layer thicknesses and, as a result, constant transmission of the coating can be achieved.A constant concentration of the ink during the processing can only be achieved with sufficient amounts of low-volatility solvents in the ink paste, because highly volatile (VD < 10) or medium-volatile (VD = 10 - 35) solvents would evaporate during the printing of the ink paste and thus the concentration of the ink paste would change unacceptably.

[0043] However, the tests also showed that highly volatile solvents such as ethanol (VD = 8.3) or medium-volatile solvents such as butyl acetate (VD = 11) may be present in certain quantities without causing excessively high transmission changes due to solvent evaporation and the associated increase in concentration during the screen printing process. In particular, the proportion of highly volatile solvents should not be higher than the proportion of less volatile solvents.

[0044] Layer A is preferably produced by a color paste which contains 2 wt.% or more, preferably 4 wt.% or more, more preferably 8 wt.% or more, more preferably 12 wt.% or more, more preferably 16 wt.% or more, more preferably 20 wt.% or more, more preferably 25 wt.% or more; and / or, preferably and, 30 wt.% or less, preferably 25 wt.% or less, more preferably 20 wt.% or less, more preferably 16 wt.% or less, more preferably 12 wt.% or less, more preferably 8 wt.% or less; solvent. A color paste which is very easy to process and is suitable for producing a coating with a low image grain preferably contains 10 to 30 wt.%, preferably 15 to 25 wt.%, solvent. Fillers

[0045] Fillers, also called additives, include thickeners and thixotropic agents, defoamers, wetting and leveling agents.

[0046] Suitable thickeners and thixotropic agents that do not change the color or transmittance include polyacrylates, pyrogenic silica, or cellulose derivatives. Silica is particularly suitable for increasing viscosity (cellulose derivatives decompose in acidic sols, and the color paste would only be stable for a few days). The silica content (based on the baked layer) should not, however, exceed 15 wt.%; the unusually high content of 4-10 wt.% for color pastes is ideal. With a silica content higher than 15 wt.%, the viscosity of the color paste is too high, meaning that a continuous film is no longer achieved, i.e., small, uncoated areas appear in the coating. In these places, the luminous elements would shine disproportionately brightly through the cooking surface, which would impair the aesthetic impression. With a content lower than 1 wt.%, the viscosity of the color paste is too high and a continuous film is no longer achieved.-% the viscosity of the color paste is too low, so that the color paste drips through the screen mesh.

[0047] To optimize the print image, defoamers, wetting agents and leveling agents can also be added to the ink paste.

[0048] Layer A is preferably produced by a color paste which contains 0.001 wt% or more, preferably 0.1 wt% or more, more preferably 0.2 wt% or more, more preferably 0.3 wt% or more, more preferably 0.4 wt% or more, more preferably 0.5 wt% or more, more preferably 0.6 wt% or more; and / or, preferably and, 15 wt% or less, more preferably 10 wt% or less, more preferably 5 wt% or less, more preferably 1 wt% or less, more preferably 0.5 wt% or less, more preferably 0.4 wt% or less, more preferably 0.3 wt% or less, more preferably 0.2 wt% or less, more preferably 0.1 wt% or less; of fillers. A color paste which is very easy to process and has a low image grain preferably contains 0.1 to 0.5 wt.%, preferably 0.2 to 0.4 wt.%, of fillers. pigment

[0049] The matrix itself is almost colorless after drying or firing. To reduce the transmission of the coating and achieve the desired effect, the addition of pigments is necessary. The type and quality of the pigments can influence the image grain. Suitable pigments are those that are thermally stable up to 200°C, at least for a short time (1-10 minutes). Layer A does not normally have to withstand higher temperatures. This is partly because the 7-segment displays or LCD screens arranged underneath it do not tolerate higher temperatures, and such display areas are therefore located in the cold area of ​​the cooking surface. Furthermore, touch switches are usually located near the display areas, and the cooking surface must be cooler than 60°C in the area of ​​the switches to prevent the user from burning their fingers when operating the cooking surface.

[0050] In addition to the thermally very stable inorganic pigments, organic pigments are also suitable. Due to legal regulations for electrical and electronic equipment, the pigments should not contain lead, hexavalent chromium (especially Cr VI< ), cadmium, or mercury. Suitable materials include inorganic colored pigments and black pigments such as iron oxide pigments, chromium oxide pigments, or mixed-phase oxide pigments with a rutile or spinel structure, as well as inorganic white pigments (oxides, carbonates, sulfides). Examples of suitable pigments are iron oxide red pigments made from hematite (α-Fe 2 O 3 ), iron oxide black pigments with the approximate composition Fe 3 O 4 and the mixed phase pigments cobalt blue CoAlO 4 , zinc iron brown (Zn,Fe)FeO 4 , chromium iron brown (Fe,Cr) 2 O 4 , iron manganese black (Fe,Mn)(Fe,Mn) 2 O 4 , spinel black Cu(Cr,Fe) 2 O 4 and also white pigments such as TiO 2 and ZrO 2 .

[0051] To achieve special color effects, inorganic luster pigments (metallic effect pigments, pearlescent pigments, and interference pigments) can also be used, so-called effect pigments. Platelet-shaped particles made of aluminum, copper, or copper-zinc alloys are suitable as effect pigments.

[0052] Azo pigments (e.g. naphthol AS, dipyrazolone), polycyclic pigments (e.g. quinacridone, perylene) or metal complex pigments (e.g. copper phthalocyanine pigments) can be used as organic pigments.

[0053] In principle, there are no particular restrictions on the size and shape of the pigments. The average particle diameter of the pigments is preferably in the range of 1-25 µm (preferably 5-10 µm). D90 should be below 40 µm (preferably 6-15 µm), D50 below 25 µm (preferably 6-8 µm), and D10 below 12 µm (preferably 2-5 µm). Platelet-shaped pigments should have a maximum edge length of 60-100 µm (preferably 5-10 µm) so that the color paste can be printed smoothly with screen mesh sizes of 140-31 (corresponding to a mesh size of 36 µm) or 100-40 (corresponding to a mesh size of 57 µm) and a low image grain can be achieved. Coarser pigments result in layers that appear inhomogeneous, making the illuminated display less clearly visible. The finer the pigments, the more homogeneous the layer appears, and the image grain is also reduced.For the grain sizes mentioned, a scattering of 5–40% (wavelength range: 400–800 nm) typically occurs (see EP 1 867 613 A1). In addition to scattering, the shape and size of the pigments can influence the image grain.

[0054] The above-mentioned effect is particularly pronounced when using pigments with particle sizes below 1 µm. However, the effort required to disperse the nanoparticles and stabilize the color paste, and the associated costs, are disproportionate to the gain in display quality achieved with such low-scattering layers.

[0055] Layer A is preferably produced using a color paste which contains 2% by weight or more, preferably 4% by weight or more, more preferably 8% by weight or more, more preferably 12% by weight or more, more preferably 16% by weight or more, more preferably 20% by weight or more, more preferably 25% by weight or more; and / or, preferably and, 45% by weight or less, preferably 30% by weight or less, more preferably 20% by weight or less, more preferably 16% by weight or less, more preferably 12% by weight or less, more preferably 8% by weight or less; pigment. If the pigment content is too low, the transmission of the coating is too high, so that the view into the interior of the cooktop is not sufficiently prevented. If the pigment content is too high, the transmission of the coating is too low, so that the illuminated displays can no longer be perceived clearly enough.

[0056] Layer A can also contain a dye in addition to a pigment. However, layer A preferably does not contain any dyes so that they are more temperature-stable. Very high temperatures do not normally arise under a 7-segment display during operation. However, the color paste is hardened by heating, which can lead to a change in the color of dye-containing layers. Furthermore, the same colorants are preferably used in layer A and layer B, and since the cooking plates are usually arranged beneath layer B, the color of layer B, if it contains a dye, can change over time. Therefore, layer A, and preferably layers A and B, do not contain any dyes. graphite

[0057] The color paste used to create Layer A preferably contains graphite. Graphite is used to adjust the transmittance of the layers and also acts as a lubricant. In addition to pigments, graphite is also believed to have a significant influence on image grain.

[0058] Layer A is preferably produced using a color paste which contains 0.01 wt.% or more, preferably 1 wt.% or more, more preferably 3 wt.% or more, more preferably 8 wt.% or more, more preferably 10 wt.% or more, more preferably 12 wt.% or more, more preferably 16 wt.% or more, more preferably 20 wt.% or more, more preferably 25 wt.% or more; and / or, preferably and, 45 wt.% or less, preferably 30 wt.% or less, more preferably 20 wt.% or less, more preferably 16 wt.% or less, more preferably 12 wt.% or less, more preferably 10 wt.% or less, more preferably 8 wt.% or less; more preferably 4 wt.% or less; graphite. If the graphite content is too low, the transmission of the coating is too high, so that the view into the interior of the cooking hob is not sufficiently prevented.If the graphite content is too high, the coating's transmission is too low, meaning the LED indicators are no longer clearly visible. Furthermore, as the graphite content increases, electrical conductivity increases, which can lead to undesirable electrical contacts in electronics.

[0059] Layer A is preferably produced using a color paste which contains 0.01 wt.% or more, preferably 1 wt.% or more, more preferably 3 wt.% or more, more preferably 8 wt.% or more, more preferably 10 wt.% or more, more preferably 15 wt.% or more, more preferably 20 wt.% or more, more preferably 25 wt.% or more, more preferably 30 wt.% or more, more preferably 35 wt.% or more; and / or, preferably and, 45 wt.% or less, preferably 40 wt.% or less, more preferably 35 wt.% or less, more preferably 30 wt.% or less, more preferably 25 wt.% or less, more preferably 20 wt.% or less; pigment and graphite. If the graphite and pigment content is too low, the transmission of the coating is too high, so that the view into the interior of the cooking hob is not sufficiently prevented.If the graphite and pigment content is too high, the transmission of the coating is too low, so that the illuminated displays can no longer be perceived clearly enough. composition

[0060] The composition of layer A consists of the cured film former, the optionally crosslinked silicone, the hydrolysis catalyst, and the unreacted filler(s) remaining virtually unchanged. If curing occurs by heating, the solvent is largely evaporated, and only traces may remain, preferably no longer present.

[0061] Since the color paste used to produce the coating preferably contains approximately 20% by weight of solvent, which largely evaporates, preferred ranges for the film former, silicone, hydrolysis catalyst, solvent, and fillers can be calculated by multiplying the above values ​​by a factor of approximately 1.2. However, differentiating the individual components in the cured layer proves difficult.

[0062] The pot life of the color paste used to make Layer A can also influence the image grain. If the pot life is 6 months or less, preferably 2 months or less, more preferably 1 month or less, more preferably 2 weeks or less, more preferably 1 week or less, more preferably 1 day or less, a low image grain can be achieved.

[0063] The scratch resistance of layer A plays a minor role, as the layer is preferably applied to the side of the glass plate facing the interior of the cooktop. However, the scratch resistance is preferably 50 g or more, more preferably 75 g or more, more preferably 100 g or more, more preferably 200 g or more. Image grain

[0064] The term image grain refers to the local brightness fluctuation of a translucent surface with a size of 1 mm². The effect of image grain is similar to the grain of film in photography or image noise in digital photography.

[0065] If a pigment-coated glass substrate has low image grain, good visibility of the display is possible. Image grain is completely independent of scattering and transmission. The inventors have discovered through intensive testing that it is possible to produce layers that have low image grain but high transmission and / or scattering, as well as layers that have high image grain but also high transmission and / or scattering. Likewise, it is possible to produce layers that have low image grain but also low transmission and / or scattering, as well as layers that have high image grain but also low transmission and / or scattering.

[0066] To achieve very good visibility of the indicator or display, an image grain of 35% or less is necessary. The lower the image grain value, the better the underlying displays and indicators can be seen. Therefore, the image grain is preferably 34% or less, more preferably 33% or less, more preferably 32% or less, more preferably 31% or less, more preferably 30% or less, more preferably 29% or less, more preferably 28% or less, more preferably 27% or less, more preferably 26% or less, more preferably 25% or less, more preferably 24% or less, more preferably 23% or less, more preferably 22% or less, more preferably 21% or less, more preferably 20% or less, more preferably 15% or less, more preferably 10% or less.

[0067] However, very low values ​​are difficult to achieve, and costs, e.g., for very small pigments, increase. Therefore, the image grain is preferably 5% or more, more preferably 10% or more, more preferably 12% or more, more preferably 14% or more, more preferably 16% or more, more preferably 18% or more, more preferably 20% or more, more preferably 22% or more, more preferably 24% or more, more preferably 26% or more, more preferably 28% or more, more preferably 30% or more.

[0068] A range of image grain that can be realized cost-effectively and allows displays and / or indicators located under the pigment-coated glass substrate to be clearly seen is when layer A has an image grain of 10 to 30%, preferably 15 to 28%, preferably 17 to 27%, more preferably 19 to 25%. Light transmittance and transmission at 630 nm of layer A

[0069] If the light transmittance or transmission at 630 nm of layer A is too low, the display or indicator beneath the glass substrate cannot be sufficiently seen. If the value is too high, the display is clearly visible even when the device is turned off, and the pigment-coated glass substrate presents an irregular overall appearance.

[0070] Therefore, the light transmittance of layer A is preferably 0.5% or more, preferably 1% or more, more preferably 2% or more, more preferably 3% or more, more preferably 4% or more, more preferably 5% or more, more preferably 6% or more; and / or, preferably and, 50% or less, preferably 40% or less, more preferably 30% or less, more preferably 20% or less, more preferably 15% or less, more preferably 10% or less, more preferably 8% or less, more preferably 7% or less, more preferably 6% or less, more preferably 5% or less, more preferably 4% or less, more preferably 3% or less, more preferably 2% or less.

[0071] Likewise, the transmittance at 630 nm of layer A is preferably 0.5% or more, preferably 1% or more, more preferably 2% or more, more preferably 3% or more, more preferably 4% or more, more preferably 5% or more, more preferably 6% or more; and / or, preferably and, 50% or less, preferably 40% or less, more preferably 30% or less, more preferably 20% or less, more preferably 15% or less, more preferably 12% or less, more preferably 10% or less, more preferably 9% or less, more preferably 8% or less, more preferably 7.5% or less, more preferably 7.0% or less, more preferably 6% or less, more preferably 5% or less, more preferably 4% or less, more preferably 3% or less, more preferably 2% or less.

[0072] A value at which the display is very easy to see when switched on, but hardly visible when switched off is 1-8%, preferably 4-6%. Layer B

[0073] Preferably, the layer system comprises a layer B containing: a) a matrix, wherein the matrix contains silicon, carbon and oxygen; and b) a pigment, preferably an effect pigment; and c) optionally graphite; wherein at least a region of the glass substrate is coated with layer B and preferably layer A and layer B at least partially overlap; and wherein layer A and layer B preferably contain at least one identical pigment, wherein layer A and layer B more preferably contain the same pigments.

[0074] Preferably, the area of ​​the glass substrate coated with layer B has a light transmittance and / or a transmission at 630 nm that is lower than layer A and / or less than 5%, preferably less than 1%, more preferably less than 0.1%.

[0075] In a preferred form, layer A was printed into a recess of layer B. This means that in the overlapping area, layer B is preferably arranged between layer A and the glass substrate.

[0076] Preferably, all limitations and / or preferred embodiments of layer A described herein also apply to layer B, unless otherwise stated. Dimensions

[0077] The area of ​​layer A is not particularly limited. Layer A is preferably 1 (e.g., 1 mm x 1 mm) mm 2 or more, more preferably 4 (e.g., 2 mm x 2 mm) - 30,000 mm 2 , more preferably 10 - 15,000 mm 2 , more preferably 15 - 500 mm 2 , more preferably 20 - 250 mm 2 . A glass substrate may have one or more, e.g., 2 or more, 3 or more, or 4 or more, layers A and / or B, preferably layers A.

[0078] The area of ​​layer B is not particularly limited. Preferably, the area of ​​layer B is 30% or more, preferably 40% or more, more preferably 50% or more, more preferably 60% or more, more preferably 70% or more, more preferably 80% or more, more preferably 90% or more, more preferably 95% or more, of the area of ​​one side of the glass substrate.

[0079] The thickness of layer A is not particularly limited. The thickness of layer A is preferably 1-15 µm, preferably 2-10 µm, more preferably 4 to 8 µm, more preferably 5 to 7 µm, more preferably about 6 µm. If layer A has a thickness of 4 to 8 µm, preferably 5 to 7 µm, more preferably about 6 µm, the transparency of the layer can be very well adjusted, while very low values ​​for image grain can be achieved.

[0080] In one embodiment, layer A has the following formula: F = B / D , where B is the image grain of layer A in % and D is the thickness of layer A in µm; a value F [1 / µm] of 8 or less, preferably 7 or less, more preferably 6 or less, more preferably 5 or less, more preferably 4 or less, more preferably 3 or less, more preferably 2 or less; and / or, preferably and, 1 or more, preferably 2 or more, more preferably 3 or more, more preferably 4 or more, more preferably 5 or more, more preferably 6 or more; If the value is between 3 and 7, a very cost-effective layer with low image grain is obtained, the light transmittance of which can be adjusted very well. Proceedings

[0081] A method according to the invention is a method for producing a pigment-coated glass substrate, wherein a layer A is formed on the glass substrate by the following steps: i) Preparing a first component by: 1) mixing a first mixture containing: a) a compound of the formula Si(OR 4< ) x (OC=OR 5< ) y R 6< 4-xy , where x+y is 1 to 4, where R 4< to R 6< are independently selected from an organic radical having 1 to 20 carbon atoms, -OH and -H; b) a hydrolysis catalyst; c) water; and d) optionally silicone; 2) concentrating under reduced pressure and optionally elevated temperature the first mixture; and 3) optionally adding silicone; to obtain a first component; ii) preparing a color paste by mixing a second mixture containing: a) the first component; b) pigment; c) optionally graphite; d) solvent; and e) silicone; and wherein the color paste contains a proportion of 10 to 60 wt.% silicone, and wherein the ratio of film former [wt.%] / silicone [wt.-%] has a value of 0.2 or more and 0.8 or less, wherein the film former has the following formula: Si(OR 4< ) x (OC=OR 5< ) y R 6< 4-xy , wherein x, y and R 4< to R 6< are as defined above; to obtain a color paste; iii) applying the color paste to a glass substrate; and iv) drying the applied color paste to obtain a pigment-coated glass substrate. .

[0082] Preferably, silicone is added to either the first component and / or the color paste, preferably the color paste, more preferably 10 to 60 wt.%, preferably 15 to 50 wt.%, more preferably 18 to 40 wt.%, more preferably 20 to 45 wt.%, more preferably 25 to 35 wt.%, of silicone is added to the color paste.

[0083] The solvent is preferably diethylene glycol monomethyl ether and / or, preferably, and the hydrolysis catalyst is preferably paratoluenesulfonic acid.

[0084] The color paste for layer A and / or B can be applied independently to the recessed area by spraying, dipping, pouring, brushing, screen printing, pad printing, or other stamping processes. The screen printing process offers the advantage that the thickness of the layer can be precisely defined using the fabric thickness, allowing consistent layer thicknesses to be produced with high precision during the manufacturing process, even over large, flat areas. This aspect is particularly important for layer A because it allows the transmission of the light from the luminous elements to be defined and remains constant across the entire layer A. Suitable layer thicknesses after screen printing, but before curing, are in the range of 2 - 20 µm, preferably 5 - 12 µm. At layer thicknesses lower than 2 µm, the cured layer A is no longer sufficiently opaque, and its scratch resistance is below 100 g.At layer thicknesses above 20 µm, the transmission of layer A for visible light is too low, and scattering effects increase significantly, making the illuminated display less visible. Adhesion problems can also occur at higher layer thicknesses.

[0085] Suitable screen mesh sizes for applying the color paste to a glass substrate are e.g. 140 - 31 (corresponding to a mesh size of 36 µm) or 100 - 40 (corresponding to a mesh size of 57 µm).

[0086] The concentration of the first mixture is preferably carried out at 20 to 100 °C and 50 to 1000 mbar.

[0087] The drying of the applied color paste is preferably carried out at 50°C or more, preferably at 100°C or more, more preferably at 150°C or more, more preferably at 180°C or more and / or, preferably and, 500°C or less, more preferably at 300°C or less, more preferably at 220°C or less, and / or preferably for 10 min or more, more preferably at 30 min or more and / or, preferably and, 500 min or less, preferably 180 min or less, more preferably 60 min or less. Measurement method

[0088] The measurement methods used here are described below: Image grain

[0089] The image grain can be determined for both emitting and transmitting samples.

[0090] To determine image grain, a black-and-white photograph of a sample is taken with a digital camera and analyzed on a computer. Each pixel in the image corresponds to a gray value between 0 (black) and 100% (white).

[0091] For evaluation, a 1 x 1 mm2 region of interest (ROI) is defined within the illuminated area. Only pixels within the ROI are used to calculate image grain. Of these pixels, those whose measured values ​​correspond to the lowest 10% of the measured values ​​and the highest 10% of the measured values ​​are excluded. This eliminates measurement artifacts such as dust particles on the surface, pinholes in any coatings, or hotspots in illuminants. From the remaining pixels within the ROI, the lowest measured value M min and the highest measured value M max are determined, and the image grain G is calculated as follows: G = M max − M min / M max + M min .

[0092] For example, if the highest and lowest measured values ​​are identical, the image grain is 0%. If the highest measured value is twice as high as the lowest, the image grain is approximately 33%.

[0093] If the illuminated area is sufficiently large, several ROIs, each measuring 1 x 1 mm², can be defined within the illuminated area. The image grain can then be determined for each ROI as described above. This allows the average image grain to be calculated from all individual ROI values, thus increasing statistical measurement accuracy.

[0094] The measurement setup and method are described in more detail below.

[0095] The measurement setup includes a darkroom containing at least the sample to be measured, and in the case of transmissive samples, a light source, and a digital camera. In the case of a transmissive sample, the sample must be positioned between the light source and the digital camera.

[0096] The darkroom serves to exclude extraneous light and thus enable appropriate exposure of the photograph.

[0097] Light-emitting surfaces often have a decreasing brightness at their edges. Therefore, the sample to be measured preferably has a light-emitting surface that is large enough to accommodate a square with an edge length of at least 2 x 2 mm². This makes it possible to position the ROI in such a way that the measurement of the image grain is little or not at all influenced by edge effects. In the case of transmissive samples, the light source preferably has a light-emitting surface that is large enough to accommodate a square with an edge length of at least 2 x 2 mm². At the same time, the light-emitting surface of the light source must be smaller than the transmissive sample. This ensures that the sample completely covers the light-emitting surface. If this is not the case, this may result in, for example, overexposure of the image or underexposure of the ROI.

[0098] In the case of transmitting samples that have a one-sided coating, the coating is arranged on the side facing the light source.

[0099] The light source used to measure transmissive samples must itself have an image grain of less than 3% to avoid interfering with the sample measurement results. Those skilled in the art know how to create a sufficiently homogeneous illuminated surface with low image grain using commercially available means, particularly white LEDs and diffusers.

[0100] For example, one or more cool white LEDs with a color temperature of 6500 to 8000 K, especially 6500 K, can be used as LEDs. One such LED is the Cree LED of the type XTEAWT-00-000000000HHE1 with 6500 K and a color rendering index of at least 80.

[0101] To homogenize the light with low image grain, suitable diffusers, such as LEXAN film 8B28, type 82728, opal smooth / structured, 250 µm, can be placed between the light source and the sample. If necessary, masking can be used to shape the illuminated area. Opaque plates or films with a suitably shaped cutout, e.g., a square, of the required size are suitable for this purpose. Such masking can be made of metal, for example.

[0102] The digital camera must meet various requirements to be suitable for carrying out the measurement.

[0103] The specialist will select the camera optics based on the space available in the darkroom and the size and number of pixels of the camera sensor. The image scale ensures that the ROI is imaged with at least 49 pixels. An image with fewer than 49 pixels may result in increased measurement inaccuracy. A number of more than 49 pixels is not necessary, but is advantageous. A higher number of pixels improves measurement accuracy.

[0104] For example, a digital camera of the type acA1920 - 40 um from Basler AG with a Sony Pregius IMX249 CMOS sensor and a lens with a 35 mm focal length of the type LM35HC-SW from Kowa GmbH can be used.

[0105] The Sony Pregius IMX249 sensor is a black-and-white sensor with a pixel size of 5.86 x 5.86 µm² at a resolution of 1936 x 1216 pixels (2.35 MP) and a sensor size of approximately 11.3 x 7.1 mm². With a magnification of 1:1, an object with a length of 1 mm would be imaged on approximately 170 pixels. An ROI with an area of ​​1 mm² would accordingly be imaged on approximately 28,900 pixels. Imagery of an object with a length of 1 mm on 7 pixels (7 x 5.86 µm = 41.02 µm ~ 1 / 24 mm) would correspond to a magnification of approximately 1:24. Therefore, for this sensor, a magnification of 1:24 or more should be selected to image an ROI with an area of ​​1 × 1 mm 2< on at least 49 pixels.

[0106] The aforementioned lens has a minimum focusing distance of 30 cm. According to the data sheet, the image scale at this distance is 1:9. This combination of digital camera, lens, and distance to the sample ensures that an ROI of 1 × 1 mm2< is imaged on approximately 360 pixels, significantly more than 49 pixels.

[0107] The focus of the digital camera must always be adjusted for the measurement so that the surface of the sample to be measured is as close as possible to the focal plane of the digital camera. For transparent samples with a single-sided coating, the focus should generally be set to the underside of the coated sample. An incorrectly adjusted focus leads to a systematic underestimation of the image grain value. If in doubt, the measurement can be repeated with several different focus settings. The highest measured value will then be closest to the actual image grain value.

[0108] The electronic signal amplification of digital cameras, adjustable, for example, in the form of (analog) gain or ISO values, leads to increased image noise. This image noise systematically distorts the image grain value toward higher values. Therefore, the digital camera must be operated at the lowest adjustable signal amplification, preferably without signal amplification. If in doubt, the signal amplification for the measurement should be set so that the camera measures an image grain of no more than 3% for the light source.

[0109] The image must not be overexposed or underexposed. Underexposure distorts the result because the minimum value M min cannot be reliably determined. Overexposure affects the maximum value M max accordingly. As long as the image is neither overexposed nor underexposed, the exposure does not affect the grain measurement result. Professionals know how to adjust the exposure appropriately, for example, using the camera aperture, exposure time, suitable optical filters in front of the camera, or the brightness of the light source.

[0110] The captured image is transferred to a computer for processing. Saving and editing the image is preferably done in RAW format. Compressive file formats such as JPEG can lead to undesirable measurement inaccuracies. Therefore, they should not be used.

[0111] The analysis of the images and the calculation of image grain can be performed on the computer using commercially available image processing software. Suitable software includes Halcon SDK Industry 12 from MVTec Software GmbH or MATLAB from MathWorks. Light transmittance

[0112] The light transmittance was measured according to DIN EN 410. The light transmittance here was measured in an area of ​​layer A and / or layer B that does not overlap with any other layer. Transmission at 630 nm

[0113] The transmission at 630 nm was measured with a clamp photometer ZPM-RGB from Opsytec Dr. Gröbel GmbH. Scratch resistance

[0114] Scratch resistance was measured by placing a hard metal tip (tungsten carbide tip; tip radius: 0.5 mm) loaded with the respective weight (50 g, 100 g, 200 g, 300 g) vertically onto the coating and moving it over a distance of approximately 30 cm at a speed of 20–30 cm / s (ERICHSEN Universal Scratch Tester Model 413). The assessment was performed from the user's perspective through the glass substrate. The test is considered passed at the selected load if no damage is visible from a distance of 60–80 cm against a white background and D65 daylight. Drawings

[0115] Figure 1 shows a hob according to an embodiment of the invention. Figure 2 shows a section of a hob according to an embodiment of the invention in cross section. Figure 3 shows a block diagram of the method. List of reference symbols

[0116] 1Cooking surface 2Glass substrate 37-segment display 4Display 5Marking of the position of the cooking plates 6Layer A 7Layer B Description of the drawings

[0117] Figure 1 shows a top view of a cooktop 1 according to an embodiment of the invention. The glass substrate 2 extends flat in the plane of the paper. The glass plate has markings 5 ​​that indicate the positions of the cooking plates. These markings 5 ​​can be arranged either on or under the glass substrate 2. In the lower area of ​​the glass substrate 2, a 7-segment display 3 and a display 4 can be seen as an example. However, the cooktop 1 can also have only one 7-segment display 3 or one display 4, as well as multiple 7-segment displays 3 and / or multiple displays 4. Figure 2shows a section of a hob 1 according to an embodiment of the invention in cross section. On one side of the glass substrate 2, the layer A 6 is arranged, which is surrounded by a layer B 7. The layer A 6 usually overlaps slightly with the layer B 7 (not shown), so that in the plan view (see Fig. 1 ) no gap can be seen between layer A 6 and layer B 7. A 7-segment display 3 or a display 4 is arranged beneath layer A 6, which is either in direct contact with layer A 6 or slightly spaced apart (not shown). Figure 3 shows a block diagram of the process. The process is used to produce the pigment-coated glass substrate. First, a first component is prepared (i), then the color paste is prepared (ii). The color paste is then applied to a glass substrate (iii) and finally dried (iv) to obtain a pigment-coated glass substrate. Examples

[0118] To prepare the first component, 40.01 wt% MTEOS (methyltriethoxysilane, Sigma Aldrich) and 11.69 wt% TEOS (tetraethoxysilane, Sigma Aldrich) were placed in a vessel and reacted with 5.66 wt% deionized water, in which 1.43 wt% PTSH (paratoluenesulfonic acid, Sigma Aldrich) was dissolved, for 30 minutes at room temperature. 32.97 wt% terpineol (Sigma Aldrich) and 8.24 wt% n-butyl acetate (Sigma Aldrich) were added to this mixture, and the resulting ethanol was then removed by distillation at 200 mbar and 40 °C to obtain the first component.

[0119] The remaining substances were added to this first component (see table for proportions). The silicone used in each example was 0.30 wt.% polydimethylsiloxane (M 1000 from Carl Roth GmbH & Co. KG), and in Examples 2 and 3, a specific amount (see table) of ethoxy-functional silicone-polyester resin (Silikoftal HTT from Evonik) was also used. Diethylene glycol monoethyl ether was used as the solvent. The pigments used were 12.84 wt.% Iriodin 103 from Merck and 0.94 wt.% Iriodin 305 from Merck (= 13.78 wt.%). The filler was 2.18 wt.% fumed silica (Aerosil A300 from Evonik). The graphite used was Timrex SFG6 from TimCal. The substances were stirred with a mixer (IKA Labortechnik, stirrer RW 28 basic) for about 10 min until a homogeneous color paste was obtained.

[0120] The color paste was then applied by screen printing (screen thickness: 100-40) within 4 hours of production and then dried at 200°C for 45 min. Example First component silicone solvent Pigments graphite Fillers # % by weight % by weight % by weight % by weight % by weight % by weight 1* 65,28 0,30 13,13 13,78 5,33 2,18 2° 48,96 16,62 13,13 13,78 5,33 2,18 3° 32,64 32,94 13,13 13,78 5,33 2,18 Example Image grain Scratch resistance Transmission at 630 nm # % 9 % 1* 39,7 200 9,0 2° 31,7 500 7,0 3° 25,2 400 7,5 *Reference example ° Example according to the invention

[0121] The table shows that Example 1 has a very high image grain (39.7%). Starting from Example 1, there are a variety of conceivable ways to reduce the image grain. Increasing the proportion of one substance within the mixture simultaneously requires a reduction in the percentage of another substance. The inventors have discovered through intensive testing that, surprisingly, adding a silicone to the mixture and simultaneously reducing the proportion of film former, while all other proportions of the substances remain the same, leads to a reduction in image grain. The overall impression of the layer is only slightly influenced by the addition of silicone. For example, with a mixture containing 48.96 wt.% film former and 16.32 wt.% silicone, a layer was obtained which had an image grain of 31.7%. Increasing the silicone proportion to 32.64 wt.-% and a further reduction of the film former to also 32.64 wt.% in the mixture resulted in an image grain of 25.2 being measured in the resulting layer.

Claims

1. A pigment-coated glass substrate for a cooktop, comprising: i) a glass substrate, wherein the glass substrate comprises a glass or a glass-ceramic, preferably consists of a glass or a glass-ceramic; and ii) a layer system comprising: a layer A containing: a) a matrix, wherein the matrix contains silicon, carbon and oxygen, b) a pigment, preferably an organic or inorganic pigment, more preferably an effect pigment, and c) optionally graphite, wherein layer A has image graining of 35% or less; and wherein the pigment-coated glass substrate is obtainable by a method wherein layer A is formed on the glass substrate by the following steps: i) producing a first component by: 1) mixing a first mixture comprising: a) a compound of the formula         Si(OR4)x(OC=OR5)yR64-x-y where x + y is 1 to 4, where R4 to R6 are independently selected from an organic radical having 1 to 20 carbon atoms, -OH and -H; b) a hydrolysis catalyst; c) water; and d) optionally silicone; 2) concentrating under reduced pressure and optionally elevated temperature of the first mixture; and 3) optionally adding silicone; in order to obtain a first component; ii) producing a colour paste by mixing a second mixture comprising: a) the first component; b) pigment; c) optionally graphite; d) solvent; and e) silicone; in order to obtain a colour paste; and wherein the colour paste contains a proportion of 10% to 60% by weight of silicone, and wherein the ratio of film former [wt%] / silicone [wt%] has a value of 0.2 or more and 0.8 or less, wherein the film former has the following formula:         Si(OR4)x(OC=OR5)yR64-x-y where x, y and R4 to R6 are as defined above; iii) applying the colour paste to a glass substrate; and iv) drying the colour paste applied in order to obtain a pigment-coated glass substrate.

2. The coated glass substrate according to Claim 1, wherein layer A has image graining of 10% to 30%, preferably 15% to 28%, preferably 17% to 27%, more preferably 19% to 25%.

3. The coated glass substrate according to any of the preceding claims, wherein layer A has transmittance of 1-5%, preferably 2-4%; and / or wherein layer A has transmittance at 630 nm of 1-10%, preferably 5-8%.

4. The coated glass substrate according to any of the preceding claims, wherein the layer system comprises a layer B containing: a) a matrix, wherein the matrix contains silicon, carbon and oxygen; and b) a pigment, preferably an effect pigment; and c) optionally graphite; wherein at least a region of the glass substrate has been coated with layer B, and layer A and layer B preferably overlap at least partly; and wherein layer A and layer B preferably contain at least one identical pigment, where layer A and layer B more preferably contain the same pigments.

5. The coated glass substrate according to any of the preceding claims, wherein the region of the glass substrate coated with layer B has transmittance less than that of layer A and / or less than 5%, preferably less than 1%, more preferably less than 0.1%.

6. The coated glass substrate according to any of the preceding claims, wherein the thickness of layer A and / or layer B is 1-15 pm, preferably 2-10 pm, more preferably 4 to 8 µm, more preferably 5 to 7 µm, more preferably about 6 µm.

7. The coated glass substrate according to any of the preceding claims, wherein the pigment contains Al, Si, Cr, Fe, Cu, Mn, Co or Ti, preferably Al, Si, Cr, Fe, Cu, Mn or Co; and / or wherein layer A and / or B contains graphite, preferably 0.01% to 12% by weight, preferably 1% to 10% by weight, more preferably 3% to 8% by weight, of graphite; and / or wherein layer A, preferably layer A and layer B, do(es) not contain any dyes.

8. The coated glass substrate according to any of the preceding claims, wherein layer A and / or B comprises 0.4% by weight or more, preferably 0.4% to 60% by weight, more preferably 1% to 60% by weight, more preferably 15% to 50% by weight, more preferably 180 to 40% by weight, more preferably 20% to 45% by weight, more preferably 25% to 35% by weight, of silicone, preferably functionalized silicone, more preferably functionalized silicone resin, preferably wherein the functionalized silicone, preferably the functionalized silicone resin, is in crosslinked form.

9. The coated glass substrate according to any of the preceding claims, wherein the matrix contains one or more of the following binding motifs: i) [OSiR1R2]; where R1 and R2 is independently selected from an organic radical having 1 to 20 carbon atoms, -OH and -H, preferably where R1 and R2 are the same; ii) [Si-O-Si]; and iii) [O3SiR3]; where R3 is independently selected from an organic radical having 1 to 20 carbon atoms, -OH and -H.

10. The coated glass substrate according to any of the preceding claims, wherein 15% to 50% by weight, preferably 18% to 40% by weight, more preferably 20% to 45% by weight, more preferably 25% to 35% by weight, of silicone is added to the colour paste.

11. The coated glass substrate according to any of the preceding claims, wherein silicone is added to the first component.

12. The coated glass substrate according to any of the preceding claims, wherein the solvent is diethylene glycol monomethyl ether; and / or wherein the hydrolysis catalyst is paratoluenesulfonic acid; and / or wherein the silicone is a functionalized silicone, preferably an ethoxy-functional silicone, more preferably an ethoxy-functional silicone polyester resin.

13. The coated glass substrate according to any of the preceding claims, wherein R1 to R6 is independently selected from a list consisting of substituted or unsubstituted and / or linear or branched alkyl, heteroalkyl, cycloalkyl, alkylcycloalkyl, heteroalkylcycloalkyl, heterocycloalkyl, alkyl-heterocycloalkyl, heteroalkylheterocycloalkyl, aryl, alkylaryl, heteroalkylaryl, heteroaryl, alkyl-heteroaryl, heteroalkylheteroaryl, -OH and H; preferably respectively unsubstituted alkyl, heteroalkyl and alkylcycloalkyl, alkylcycloalkyl, heteroalkylcycloalkyl, heterocycloalkyl, alkyl-heterocycloalkyl and heteroalkylheterocycloalkyl; more preferably methyl and ethyl; and / or where x + y is 3 or 4, preferably x is 3 or 4 and y is 0 or 1.

14. Process for producing a pigment-coated glass substrate, wherein layer A on the glass substrate is formed by the following steps: i) producing a first component by: 1) mixing a first mixture comprising: a) a compound of the formula         Si(OR4)x(OC=OR5)yR64-x-y where x + y is 1 to 4, where R4 to R6 are independently selected from an organic radical having 1 to 20 carbon atoms, -OH and -H; b) a hydrolysis catalyst; c) water; and d) optionally silicone; 2) concentrating under reduced pressure and optionally elevated temperature of the first mixture; and 3) optionally adding silicone; in order to obtain a first component; ii) producing a colour paste by mixing a second mixture comprising: a) the first component; b) pigment; c) optionally graphite; d) solvent; and e) silicone; in order to obtain a colour paste; and wherein the colour paste contains a proportion of 10% to 60% by weight of silicone, and wherein the ratio of film former [wt%] / silicone [wt%] has a value of 0.2 or more and 0.8 or less, wherein the film former has the following formula:         Si(OR4)x(OC=OR5)yR64-x-y where x, y and R4 to R6 are as defined above; iii) applying the colour paste to a glass substrate; and iv) drying the colour paste applied in order to obtain a pigment-coated glass substrate.

15. A cooktop, a baking oven, a stove sightglass or a microwave, preferably a cooktop, more preferably a cooktop containing a 7-segment display or another kind of display, comprising a pigment-coated glass substrate according to any of Claims 1 to 13.