Scintillating hybrid material, method for its production, associated apparatus and method for measuring the scintillation

DE602018077072T2Active Publication Date: 2024-11-27COMMISSARIAT A LENERGIE ATOMIQUE ET AUX ENERGIES ALTERNATIVES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602018077072
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-12-24
Filing Date
2018-12-20
Publication Date
2024-11-27
Estimated Expiration
2038-12-20

AI Technical Summary

Technical Problem

Current plastic scintillators face challenges in separating scintillation pulses due to insufficient differences in fluorescence decay constants between fast and slow compartments, leading to erroneous values and underestimation of counting rates, especially at high ionizing particle or radiation intensities.

Method used

A hybrid plastic scintillator material with a polymer matrix and a fluorescent mixture comprising 95.6% to 99.1 molar% naphthalene and 0.9% to 4.4 molar% of an additional primary fluorophore with specific photophysical properties, optimizing the fluorescence decay constant between 10 ns and 90 ns, thereby improving pulse discrimination and scintillation efficiency.

Benefits of technology

The hybrid material enhances the separation of scintillation pulses, reduces saturation issues, and allows for precise measurement of ionizing radiation, offering improved detection accuracy and efficiency in high-counting rate scenarios.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention belongs to the field of measuring radioactivity by the plastic scintillation technique.

[0002] The invention relates more particularly to a material for measurement by plastic scintillation, a part comprising the material and its associated measuring device or apparatus, the associated manufacturing methods, as well as the method of measurement by plastic scintillation using the device. TECHNICAL BACKGROUND

[0003] Plastic scintillation measurement consists of determining the presence and / or quantity of one or more radioactive materials, particularly in physics, geology, biology, medicine, for dating, environmental monitoring or control of the non-proliferation of nuclear weapons.

[0004] In practice, radioactive material emitting ionizing radiation or an ionizing particle (alpha particle, electron, positron, photon, neutron, etc.) is exposed to a scintillating material called a "plastic scintillator" which converts the energy deposit resulting from the radiation / matter interaction into light radiation (called radioluminescent) measurable by a photon-electron gain converter, such as a photomultiplier.

[0005] The plastic scintillator has been known since the middle of the 20th century. It is described, for example, in the document "Moser, SW; Harder, WF; Hurlbut, CR; Kusner, MR; "Principles and practice of plastic scintillator design", Radiat. Phys. Chem., 1993, Vol. 41, No. l / 2, 31-36 »[reference 1] and "Bertrand, GHV; Hamel, M.; Sguerra, F.; "Current status on plastic scintillators modifications", Chem. Eur. J., 2014, 20, 15660-15685" [reference 2]. It generally comes in the form of a polymer matrix into which a primary fluorophore or even a secondary fluorophore is inserted. A fluorophore is a chemical compound capable of emitting visible fluorescence light after excitation by photons or other incident particles. The primary fluorophore and the secondary fluorophore consist of an aromatic molecule with fluorescent properties (molecule called fluorophore) allowing detection by scintillation.

[0006] The main function of the polymer matrix is ​​to be a support capable of receiving the energy of the ionizing radiation or the ionizing particle. After recombination of the excited and / or ionized species which are then formed, this energy is converted into radioluminescent radiation and then transferred to the primary fluorophore and possibly to the secondary fluorophore, which can increase the wavelength of the radiation emitted by the primary fluorophore in order to improve its detection.

[0007] A particular plastic scintillator of the phoswich type (Anglo-Saxon neologism resulting from the combination of the terms phosphorus and sandwich generally translated as meaning "sandwich scintillator") was proposed from the beginning of the development of plastic scintillators in the document "Wilkinson DH, "The Phoswich - A Multiple Phosphor", Rev. Sci. Instrum. 1952, 23, 414-417 . » [reference 3].

[0008] In order to obtain new scintillation properties, a phoswich scintillator combines at least two compartments: one compartment comprising a slow scintillator on the one hand (high fluorescence decay constant, generally between 200 ns and 1000 ns) and another compartment comprising a fast scintillator (much lower fluorescence decay constant, generally between 2 ns and 7 ns on the other hand).

[0009] Such a scintillator nevertheless poses at least one of the following problems: the difference between the fluorescence decay constant of the fast compartment and that of the slow compartment is too small: the separation of the scintillation pulses between these stages is then not possible electronically; the difference between the fluorescence decay constant of the fast compartment and that of the slow compartment is too large: the scintillation pulse of the slow scintillator can be partially or totally masked in the electronic background noise of the scintillation pulse acquisition device, which leads to obtaining erroneous values. the acquisition of the luminescent signal is carried out over a duration which is typically about 6 to 10 times the fluorescence decay constant of the slow compartment.In case of high counting rate due to the multiplicity of ionizing particles or the high intensity of ionizing radiation interacting with the phoswich scintillator, the probability of stacking (i.e. two pulses present in the same acquisition time window) of scintillation pulses becomes increasingly important. As a result, it is possible that several pulses appear in the same acquisition time window, which leads to a rejection of the stacks by saturation phenomenon of the acquisition electronics, and therefore an underestimation of the counting rate.

[0010] Furthermore, WO 2015 / 118533 A1 describes a formulation for 3D printing of scintillators, in particular plastic scintillators. Assuming, in the absence of explicit indication in this document, that the percentages indicated are percentages by weight, formulation (h) would comprise 94.52 mol% of naphthalene and 5.48 mol% of 2,5-diphenyloxazole (PPO) as an additional primary fluorophore relative to the total number of moles of primary fluorophore in the formulation, as well as the prepolymer TMPTA.

[0011] Document US 2014 / 332689 A1 aims to protect a plastic scintillator comprising a polymer matrix based on aromatic rings in which oxazole is incorporated. In an example intended to illustrate the principle of discrimination (PSD: Pulse Shape Discrimination) between gamma radiation and neutron, the inventors use a material for plastic scintillation not corresponding to the claimed invention. This material therefore does not comprise oxazole, but 10% naphthalene, 0.1% PPO and 0.1% 1,4-bis(5-phenyl-2-oxazolyl)benzene (POPOP) incorporated in a polystyrene polymer matrix. Again, provided that the assumption is made in the absence of explicit indication in this document that the percentages indicated are percentages by weight, the plastic scintillator material of the Figure 8 would comprise 99.42 mol% naphthalene and 0.58 mol% PPO relative to the total number of moles of primary fluorophore.

[0012] EP 2 655 546 A1 describes a solid organic scintillator comprising a polymer matrix, in which one or more fluorophore compounds and one or more chemical elements having an atomic number ranging from 40 to 83 (D2, abbreviated) are dispersed. It does not mention the use of naphthalene as the main primary fluorophore.

[0013] GB 1 377 703 A describes a scintillation composition comprising 0.05% to 10% of a compound of formula (I) dissolved in a transparent organic liquid or "plastic solvent"» made of polymers. A scintillation cocktail solution is made in Examples 1 and 2: it comprises 5 g / l of PPO as the primary fluorophore, 0.1 g / l of aminocoumarin as the secondary fluorophore and 120 g / l of naphthalene in dioxane as the solvent. Reported as a molar percentage, this is equivalent to a liquid fluorescent mixture comprising 97.64% naphthalene and 2.36% PPO. However, these solutions do not include monomers or oligomers intended to form a polymeric matrix, or the resulting polymers. STATEMENT OF THE INVENTION

[0014] One of the aims of the invention is therefore to avoid or mitigate one or more of the drawbacks described above, by proposing a new type of material constituting a plastic scintillator called a “hybrid material”.

[0015] The present invention relates to a hybrid material for plastic scintillation measurement comprising (or even consisting of): a polymeric matrix; and, a fluorescent mixture incorporated in the polymeric matrix and comprising in molar concentration relative to the total number of moles of primary fluorophore in the incorporated fluorescent mixture: i) 95.6% to 99.1% mol of a main primary fluorophore consisting of naphthalene; and ii) 0.9% to 4.4% mol of an additional primary fluorophore whose centroid of the light absorption spectrum and of the fluorescence emission spectrum respectively have a wavelength between 250 nm and 340 nm and between 330 nm and 380 nm, the fluorescence decay constant is between 1 ns and 10 ns, and the fluorescence quantum yield in an apolar solvent is between 0.2 and 1; preferably greater than 0.5, typically between 0.5 and 1.

[0016] The hybrid material of the invention may also exclude certain compounds, in particular when this material is implemented according to the invention described below, in particular for the part, the device, the apparatus and their associated processes. More particularly, it does not comprise one or more of the following compounds, in particular relative to the total weight of the material: a polymerization initiator, such as for example a photoinitiator, particularly TPO (2,4,6-Trimethylbenzoyl-diphenyl-phosphineoxide), more particularly 0.5% by weight of TPO. The use of a photoinitiator to initiate the polymerization can in fact lead to scintillators with a lower scintillation efficiency, or even containing fluorophores subject to photobleaching by the activating photonic source; and / or 15% naphthalene, 1.5% PPO, 0.08% POPOP, 0.5% TPO and the remainder TMPTA (ethoxylated trimethylolpropanetriacrylate); and / or 10% naphthalene, 0.1% PPO, 0.1% POPOP and the remainder polystyrene; and / or a metallic compound (i.e., an inorganic or organometallic compound) comprising a metallic element selected, for example, from lead, tin, bismuth, or mixtures thereof. Such a metallic element may decrease scintillation efficiency; and / or a secondary fluorophore.

[0017] One or more of the exclusions of these compounds may also apply to the polymerization composition and / or the ready-to-use kit according to the invention as described below.

[0018] A suitable non-polar solvent for fluorescence quantum yield measurement is, for example, cyclohexane, toluene, dichloromethane, xylene or any isomer of xylene.

[0019] The material for plastic scintillation measurement according to the invention may also be designated in the present description by the expression "plastic scintillator". It is called "hybrid" because its fluorescence decay constant is intermediate between that of a fast plastic scintillator and a slow plastic scintillator. Advantageously, the value of this constant may also be optimally chosen during the manufacture of the hybrid material in an intermediate range between 10 ns and 90 ns (preferably between 15 ns and 80 ns), among values ​​between these two extremes which, to the inventor's knowledge, are not obtained with the plastic scintillators currently on the market. It may particularly be chosen between 25 ns and 75 ns, more particularly between 28 ns and 70 ns.

[0020] This temporal tunability of the fluorescence decay constant of the hybrid material is made possible by the use of a specific fluorescent mixture. This mixture is characterized in particular by the combined choice of naphthalene as the main primary fluorophore and an additional primary fluorophore with specific photophysical properties, as well as by the choice of a defined concentration ratio between these two primary fluorophores.

[0021] Unexpectedly, as shown by the embodiments, the main primary fluorophore and the additional primary fluorophore act in synergy to vary very significantly, while using a reduced concentration range for the additional primary fluorophore, the fluorescence decay constant. In addition, the relative simplicity of this system which essentially requires this combination between these two primary fluorophores avoids the addition of an additional molecule which may be disruptive or expensive. These advantageous properties make the hybrid material of the invention a particularly effective material for plastic scintillation measurement and which can be easily produced on an industrial scale at a moderate cost.

[0022] Contrary to the improvement paths followed by the state of the art, the invention does not consist of the use of a new polymer matrix, the addition of an additive to the plastic scintillator or the development as primary fluorophore of new families of molecules ("quantum dots", organometallic complexes, nanoparticles, etc.) in order to overcome at least one of the aforementioned drawbacks, but identifies the fluorescent mixture of the invention which allows access to a hybrid material. All of the characteristics necessary for the material for measurement by plastic scintillation according to the invention can thus be essentially limited to a polymer matrix and the incorporated fluorescent mixture.The composition of the plastic scintillator is thus simplified by overcoming the difficulty of determining very precisely the appropriate proportion between a primary fluorophore and a secondary fluorophore in order to obtain optimized radioluminescence radiation and fluorescence decay constant. Thus, as indicated previously, according to a particular embodiment, the hybrid material of the invention does not comprise a secondary fluorophore.

[0023] At the molecular level, the plastic scintillator of the invention can be considered as a pseudo-liquid, because the chains of the polymers constituting all or part of the polymer matrix are labile and allow a certain freedom of movement to the different constituents of the plastic scintillator. At the macroscopic level, the plastic scintillator nevertheless retains sufficient mechanical strength to manufacture a part for scintillation detection.

[0024] The invention is completed by the following objects and / or characteristics, taken alone or in any of their technically possible combinations.

[0025] In the present description of the invention, a verb such as "to understand", "to incorporate", "to include", "to contain" and its conjugated forms are open terms and therefore do not exclude the presence of element(s) and / or step(s)

[0026] More specifically, at least one monomer may be chosen from styrene, vinyltoluene, vinylxylene, 1-vinylbiphenyl, 2-vinylbiphenyl, 1-vinylnaphthalene, 2-vinylnaphthalene, 1-methylnaphthalene, N-vinylcarbazole, methyl (meth)acrylate, (meth)acrylic acid or 2-hydroxyethyl (meth)acrylate, or more generally an alkyl methacrylate whose linear or branched alkyl group comprises between 1 and 20 carbon atoms.

[0027] Preferably, the monomer is styrene or vinyltoluene in order to form the corresponding homopolymer.

[0028] Advantageously, the monomer may be chosen more particularly from a molecule with particular fluorescence properties, for example 1-vinylbiphenyl, 2-vinylbiphenyl, 1-vinylnaphthalene, 2-vinylnaphthalene, 1-methylnaphthalene, N-vinylcarbazole or mixtures thereof.

[0029] According to a particular embodiment, the polymer matrix of the hybrid material of the invention does not comprise, in whole or in part, at least one polymer comprising repeating units resulting from the polymerization of monomers or oligomers comprising a triacrylate and / or trimethylacrylate group; which excludes from the polymer matrix a polymer such as, for example, TMPTA (ethoxylated trimethylolpropanetriacrylate), in particular ethoxylated TMPTA (15). Advantageously, this makes it possible to exclude a polymer with brittle mechanical properties.

[0030] The polymer matrix may consist in whole or in part (preferably more than 10% by mass of polymer in the polymer matrix) of at least one crosslinked polymer (for example by means of a crosslinking agent) in which polymer chains are linked together by crosslinking bridges, in particular to improve the mechanical and / or scintillation properties. The crosslinking agent may be a monomer comprising at least two polymerizable functions capable, after polymerization, of forming a bridge between two polymer chains. It may be chosen from divinylbenzene, a diacrylate or an alkyl dimethacrylate, the hydrogenocarbon chain of the latter two containing between 2 and 20 carbon atoms.

[0031] Preferably, the crosslinking agent is 1,4-butanediyl dimethacrylate or divinylbenzene.

[0032] After polymerization of the crosslinked polymer, in addition to the aforementioned repeating units, the copolymer obtained may comprise repeating units resulting from the polymerization of the crosslinking agent.

[0033] Concerning one of the other main constituents of the hybrid material of the invention, which is the fluorescent mixture incorporated in the polymer matrix, the hybrid material may comprise 1% by mass to 25% by mass of the incorporated fluorescent mixture, or even 1% by mass to 5% by mass of the incorporated fluorescent mixture relative to the total mass of hybrid material. Beyond a mass concentration of 25%, exudation may occur, namely oozing of the fluorescent mixture out of the plastic scintillator.

[0034] The mass concentration of the fluorescent mixture incorporated into the hybrid material can be easily calculated by determining the mass of the polymer matrix.

[0035] One of the methods of the person skilled in the art is as follows: the molar concentration of the monomers and oligomers in the polymerization medium is known in advance or can be determined by a quantitative measurement method such as UV spectrophotometry. The corresponding mass concentration is then calculated from the molecular weights. However, the monomers, oligomers or their mixtures form the polymer matrix according to a polymerization yield which can be measured beforehand, but which is generally greater than 95%, or even 98%, or most often equal to 100%. Therefore, the mass proportion of the monomers and oligomers present in the polymer matrix is ​​equivalent to this reaction yield multiplied by the previously determined mass concentration.A person skilled in the art can therefore easily, using his general knowledge, convert a mass concentration into a molar concentration for all the constituents of the hybrid material.

[0036] The mass or molar percentages of the incorporated fluorescent mixture, the main primary fluorophore, the additional primary fluorophore, the secondary fluorophore or an additional compound can be determined a posteriori in the hybrid material by an analytical technique such as, for example, solid-state Nuclear Magnetic Resonance (NMR). Another technique consists of dissolving the plastic scintillator in dichloromethane, precipitating the polymer constituting the polymer matrix in methanol, filtering the mixture obtained to recover the molecule whose concentration is to be measured, then quantifying it by elemental analysis with detection of a specific atom constituting this molecule.

[0037] The incorporation of the fluorescent mixture into the polymer matrix can be carried out according to several embodiments. In particular, at least one fluorescent molecule selected from the main primary fluorophore, the additional primary fluorophore or their mixtures can be incorporated into the polymer matrix by dispersion or by grafting of this molecule into the polymer matrix. In the case of grafting, the fluorescent molecule (generally the additional primary fluorophore) is covalently bonded to the polymer matrix. This covalent bond is formed for example during the manufacture by polymerization of the polymer matrix, the fluorescent molecule comprising at least one polymerizable function.

[0038] Optionally, the hybrid material of the invention may contain one or more materials that do not have a significant impact on the plastic scintillation measurement with the hybrid material of the invention or that improve certain of its properties. Like the incorporated fluorescent mixture, these materials are generally dispersed homogeneously or not in the hybrid material.

[0039] The decay constant of the hybrid material of the invention is conferred by that of the incorporated fluorescent mixture. Thus, the incorporated fluorescent mixture, and therefore the hybrid material, may have a fluorescence decay constant of between 10 ns and 90 ns, or even between 15 ns and 80 ns, advantageously between 30 ns and 80 ns, particularly between 25 ns and 75 ns, more particularly between 28 ns and 70 ns.

[0040] The judiciously chosen concentration of the main primary fluorophore and the complementary concentration of the additional primary fluorophore give the incorporated fluorescent mixture, and thus the hybrid material, a desired fluorescence decay constant.

[0041] The incorporated fluorescent mixture comprises i) 95.6% to 99.1% mol of the main primary fluorophore consisting of naphthalene and ii) 0.9% to 4.4% mol of the additional primary fluorophore. Depending on this concentration range, the fluorescence decay constant of the hybrid material of the invention may be between 25 ns and 75 ns, more particularly between 28 ns and 70 ns.

[0042] These preferred ranges of primary fluorophore concentration can therefore give the hybrid material an increasingly high fluorescence decay constant: such a hybrid material can then advantageously be included in the composition of a hybrid plastic scintillator compartment, possibly combined with a fast plastic scintillator compartment in a phoswich-type plastic scintillation detection device to improve discrimination between beta particles and gamma radiation. They also represent a good compromise between scintillation efficiency and tunability of the hybrid material of the invention.

[0043] For example, varying molar concentrations of the main primary fluorophore in the incorporated fluorescent mixture (the remainder of the mixture being the additional primary fluorophore) can potentially impart the following fluorescence decay constants to the hybrid material: 86% molar concentration: 15 ns (not subject to the requested protection); 95.6% molar concentration: 28 ns; 96% molar concentration: 35 ns; 99% molar concentration: 80 ns; 100% molar concentration: 90 ns (not subject to the requested protection).

[0044] Preferably, the additional primary fluorophore has a fluorescence decay constant (generally designated "tau") of between 1 ns and 10 ns, has a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength of between 250 nm and 340 nm and of between 330 nm and 380 nm, and whose fluorescence quantum yield in an apolar solvent is between 0.5 and 1.

[0045] In this description, the centroid denotes the wavelength for the middle of the width at half maximum of the largest amplitude band of the radiation considered. A light absorption spectrum can be measured with a UV / visible spectrophotometer, and a fluorescence emission spectrum with a spectrofluorometer.

[0046] The fluorescence decay constant corresponds to the variation over time of the photoluminescence intensity. It is measured by time-resolved single-photon counting; as described for example in the document « M. Wahl, "Time-Correlated Single Photon Counting", M. Wahl, PicoQuant Company Technical Note, 2014" [reference 4], available online at the following Internet address: "https: / / www.picoquant.com / images / uploads / page / files / 7253 / t echnote_tcspc.pdf", as well as the book "DV O'Connor, D. Phillips, "Time Correlated Single Photon Counting", Academic Press, New York, 1984, pages 25 to 34" [reference 5].

[0047] The fluorescence quantum efficiency corresponds to the proportion of luminescence photons emitted per quantity of photons absorbed by the hybrid material. Preferably, its value is obtained using an absolute measurement method, i.e., one that does not involve a third-party compound and a calibration function. It is, for example, measured with an integrating sphere as a module of a spectrofluorometer. For a measurement of the absolute value, one can refer to the document “Rohwer, LS, Martin, JE; "Measuring the absolute quantum efficiency of luminescent materials", J. Lumin. 2005, 115, pages 77-90” [reference 6]).

[0048] The value of the fluorescence quantum yield can also be obtained by a relative measurement method whose principle is as follows: knowing the absolute fluorescence quantum yield of a third compound, the value of the absolute measurement is obtained by a simple rule of three. For example, without an integrating sphere, the fluorescence quantum yield can be determined by relative measurement of the sample (a reference solution of quinine sulfate as a third compound is for example used in the document “Velapoli, RA; Mielenz, KD, "A Fluorescence Standard reference Material: Quinine Sulfate Dihydrate", Appl. Opt., 1981, 20, 1718.” [reference 7] available online at the following Internet address: https: / / www.nist.gov / sites / default / files / documents / srm / SP260-64.PDF).

[0049] Generally, the values ​​obtained by the absolute and relative measurement method are the same or similar.

[0050] Advantageously, the additional primary fluorophore may have a fluorescence emission spectrum whose centroid is at a wavelength between 355 nm and 365 nm, typically centered around 360 nm, such that the interaction effect is optimal with the secondary fluorophore.

[0051] Time-resolved single-photon counting is a spectroscopy technique for measuring the fluorescence decay constant of photoluminescent compounds or their mixtures. It consists of exciting a fluorophore or a fluorescent mixture with a rapidly decaying light beam (relative to the luminescent radiation emitted in return to be observed), then observing the resulting photoluminescence using a monochromator coupled to a photomultiplier. The hybrid material of the invention is more particularly excited with a low frequency (typically up to 1 MHz) to avoid any stacking of scintillation pulses.

[0052] Preferably, the additional primary fluorophore is chosen from at least one compound such as: an oxazole (such as for example 2,5-diphenyloxazole (PPO)); and / or a polycyclic aromatic compound which is hydrogenated (i.e. without heteroatom) comprising from 3 to 6 phenyl rings of which at least one phenyl ring optionally comprises at least one substituent in the ortho, meta or preferably para position (for example a linear or branched alkyl substituent R, preferably saturated, preferably comprising from 1 to 10 carbon atoms, preferentially from 1 to 4 carbon atoms) such as for example [para]-terphenyl (pTP), [meta] -terphenyl (mTP), the [ para ]-quaterphenyl, biphenyl, 1-vinylbiphenyl, 2-vinylbiphenyl, 4-isopropylbiphenyl, [ para]-sexiphenyl), or mixtures thereof; and / or an oxadiazole, such as for example 2-phenyl-5-(4-biphenyl)-1,3,4-oxadiazole (PBD), 2-(4'-t-butylphenyl)-5-(4"-biphenylyl)-1,3,4-oxadiazole (Butyl-PBD) or mixtures thereof; and / or a compound from the anthracene family such as anthracene, 9-anthracenyl methacrylate or mixtures thereof; and / or a naphthalene substituted by a vinyl group (such as 1-vinylnaphthalene or 2-vinylnaphthalene), a naphthalene substituted by a substituent R as defined above (such as for example 1-methylnaphthalene) or mixtures thereof; and / or a carbazole such as for example N-vinylcarbazole, N -ethylcarbazole, the N -(2-ethylhexyl)carbazole or mixtures thereof; and / or tetraphenylbutadiene.

[0053] More specifically, the additional primary fluorophore is 2,5-diphenyloxazole (PPO), [ para ]-terphenyl (pTP), or even the [meta] -terphenyl (mTP) or mixtures thereof.

[0054] As previously indicated, the additional primary fluorophore may be covalently linked to the polymer matrix, for example via the polymerization of a vinyl, allylic, acrylic or methacrylic function carried by the additional primary fluorophore. For example, 1-vinylbiphenyl, 2-vinylbiphenyl, 1-vinylnaphthalene, 2-vinylnaphthalene, 1-methylnaphthalene, N -vinylcarbazole can be used to be covalently linked to form a copolymer with the polymer matrix.

[0055] The incorporated fluorescent mixture may further include a secondary fluorophore. The secondary fluorophore further improves the detection of radioluminescent radiation.

[0056] The mass concentration of the secondary fluorophore relative to the mass of the hybrid material may be between 0.002% and 0.5% by mass, preferably between 0.01% and 0.2% by mass, even more preferably between 0.01% and 0.1% by mass.

[0057] For example, the secondary fluorophore may be chosen from 1,4-di[2(5-phenyloxazolyl)]benzene, 1,4-bis-(2-methylstyryl)-benzene, 1,4-bis(4-methyl-5-phenyl-2-oxazolyl)benzene, 9,10-diphenylanthracene or mixtures thereof. The polymer matrix then comprises, relative to the mass of the hybrid material, 0.002% by mass to 0.2% by mass of the secondary fluorophore.

[0058] According to a first embodiment, the secondary fluorophore may be chosen such that it has a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength between 330 nm and 380 nm and between 405 nm and 460 nm, and whose fluorescence quantum yield in an apolar solvent is between 0.5 and 1. The secondary fluorophore may thus be chosen from 1,4-bis(5-phenyl-2-oxazolyl)benzene (POPOP), 1,4-bis(4-methyl-5-phenyl-2-oxazolyl)benzene (dimethylPOPOP), bis-methylstyrylbenzene (bis-MSB), 9,10-diphenylanthracene (9,10-DPA) or mixtures thereof. The molecular structures of these secondary fluorophores are illustrated below.

[0059] According to a second embodiment, the secondary fluorophore may be chosen such that it has a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength between 330 nm and 380 nm and between 460 nm and 550 nm, and whose fluorescence quantum yield in an apolar solvent is between 0.5 and 1. The secondary fluorophore may then be chosen from coumarin 6, coumarin 7, coumarin 30, coumarin 102, coumarin 151, coumarin 314, coumarin 334, 3-hydroxyflavone or mixtures thereof. The molecular structures of these secondary fluorophores are illustrated below.

[0060] According to a third embodiment, the secondary fluorophore may be chosen such that it has a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength between 330 nm and 380 nm and between 550 nm and 630 nm, and whose fluorescence quantum yield in an apolar solvent is between 0.5 and 1. The secondary fluorophore may then be chosen from Nile red, rhodamine B or one of its salts, 4-(dicyanomethylene)-2-methyl-6-(4-dimethylaminostyryl)-4H-pyran (DCM), pyrromethene 580, any molecule of N-alkyl or N-alkyl or N-aryl-perylenediimide type (such as for example N,N'-bis(2,5-di-tert-butylphenyl)-3,4,9,10-perylenedicarboximide). The molecular structures of these secondary fluorophores are illustrated below. R = alkyl or aryl R' = alkyl, aryl, H, F, CI, Br, I

[0061] The invention also relates to a manufacturing method by polymerization, via a polymerization medium, of the hybrid material of the invention which may be as defined in the present description, in particular according to one or more of the variants described for this material.

[0062] The process for manufacturing a hybrid material by polymerization includes the following successive steps: a) having a polymerization medium comprising: monomers, oligomers or their mixtures intended to form at least one polymer constituting the polymer matrix which may be as defined in the present description, in particular according to one or more of the variants described for this polymer matrix;a liquid fluorescent mixture comprising in molar concentration relative to the total number of moles of primary fluorophore in the liquid fluorescent mixture i) 95.6% to 99.1% mol of a main primary fluorophore consisting of naphthalene and ii) 0.9% to 4.4% mol of an additional primary fluorophore whose centroid of the light absorption spectrum and of the fluorescence emission spectrum respectively have a wavelength between 250 nm and 340 nm and between 330 nm and 380 nm, the fluorescence decay constant is between 1 ns and 10 ns, and the fluorescence quantum yield in an apolar solvent is between 0.2 and 1, preferably between 0.5 and 1; b) polymerizing the polymerization medium in order to obtain the hybrid material. ;

[0063] During step b) of polymerization of a precursor of the polymer (namely a precursor such as the aforementioned monomers and / or oligomers), the main and additional primary fluorophores, as well as any other compound present in the polymerization medium, are generally trapped and distributed homogeneously in the polymer matrix being formed.

[0064] Therefore, in the present description, the “liquid fluorescent mixture” is the fluorescent mixture comprising the main primary fluorophore and the additional primary fluorophore and which is contained in the polymerization medium before carrying out step b).

[0065] “Incorporated fluorescent mixture” means the fluorescent mixture comprising the main primary fluorophore and the additional primary fluorophore and which is incorporated into the hybrid material after polymerization step b), for example by grafting or dispersion.

[0066] “Fluorescent extrusion mixture” means the fluorescent mixture comprising the main primary fluorophore and the additional primary fluorophore which is contained in the extrusion mixture further containing polymerized ingredients intended to form a polymer matrix.

[0067] The polymerization medium generally does not contain a solvent. The manufacturing process is then a so-called “mass polymerization” process.

[0068] However, optionally, the polymerization medium may further comprise a polymerization solvent. The manufacturing process is then generally carried out at reflux of the solvent. The solvent of the polymerization medium may be chosen from xylene, chloroform, dichloromethane, chlorobenzene, benzene, tetrachloromethane or mixtures thereof.

[0069] The monomers or oligomers may comprise at least one aromatic, (meth)acrylic or vinyl group. At least one monomer may be selected from styrene, vinyltoluene, vinylxylene, 1-vinylbiphenyl, 2-vinylbiphenyl, 1-vinylnaphthalene, 2-vinylnaphthalene, vinylbiphenyl, 1-vinylnaphthalene, 2-vinylnaphthalene, 1-methylnaphthalene, N-vinylcarbazole, methyl (meth)acrylate, (meth)acrylic acid or 2-hydroxyethyl (meth)acrylate.

[0070] The polymerization medium can comprise 1% by mass to 25% by mass (or even 1% by mass to 5% by mass) of the liquid fluorescent mixture.

[0071] The liquid fluorescent mixture comprises i) 95.6% to 99.1% mol of the main primary fluorophore consisting of naphthalene and ii) 0.9% to 4.4% mol of the additional primary fluorophore.

[0072] The polymerization medium may further comprise at least one chemical species intended to be incorporated into the hybrid material to give it or improve particular properties (for example a secondary fluorophore), and / or at least one species intended to be consumed or modified during step b) of polymerization (for example a crosslinking agent, a polymerization initiator).

[0073] The polymerization medium may include: a secondary fluorophore, typically in a mass concentration of between 0.002% and 0.5% by mass, or even 0.002% by mass to 0.2% by mass; and / or a crosslinking agent, typically in a mass concentration of between 0.1% and 20% (more precisely 20.0%) by mass, or even 0.001% by mass to 1% by mass; and / or a polymerization initiator, typically in a concentration of 0.001% by mass to 1% by mass. a polymerization initiator, typically in a concentration of 0.001% by mass to 1% by mass.

[0074] The additional primary fluorophore, secondary fluorophore and / or crosslinking agent may also be as defined in one or more of the variations described herein.

[0075] The polymerization reaction according to step b) can be carried out according to the conditions usually used by those skilled in the art.

[0076] Thus, it can be started with a polymerization initiator, in particular a photoinitiator for initiating radical polymerization. Preferably, the photoinitiator is not a photoinitiator activatable under UV radiation, such as for example TPO. A UV photoinitiator can produce residual compounds or modify other compounds of the plastic scintillation material, which results in photobleaching of this material detrimental to good scintillation efficiency.

[0077] Preferably, in order to best avoid such a problem, the photoinitiator used in the invention is activatable under visible light radiation. For example, as indicated in patent application WO 2013076281 [reference 8], the polymerization initiator may be selected from a peroxide compound (e.g. benzoyl peroxide), a nitrile compound (e.g. azo(bis)isobutyronitrile (AIBN)) or mixtures thereof.

[0078] When the polymerization reaction is carried out in particular with methacrylate monomers, it can be induced by heating the polymerization medium to a suitable temperature (generally between 40 °C and 140 °C), or by doping the polymerization medium with 2,2-dimethoxy-2-phenylacetophenone as a polymerization initiator and then carrying out UV irradiation (for example, at a wavelength of 355 nm). The polymerization reaction in the presence of styrenic monomers can be induced thermally, typically by heating between 40 °C and 140 °C.

[0079] The process for manufacturing the hybrid material by polymerization of the invention may be such that, during polymerization step b), the polymerization medium is heated to a polymerization temperature of between 100°C and 140°C (for a time sufficient for the polymerization to be complete, generally for 24 hours), then cooled at a rate of 10°C to 20°C per day (generally to reach room temperature, typically 20°C) until the hybrid material is obtained.

[0080] For example, the polymerization medium can be heated for 24 hours at 140°C, then cooled at a rate of 20°C per day until it returns to 20°C.

[0081] Steps a) and b) of the manufacturing process by polymerization via a polymerization medium of the invention can be carried out in a mold in order to obtain a part as defined in the present description, or a blank of this part.

[0082] The manufacturing method of the invention by polymerization via a polymerization medium may further comprise a step c) during which the hybrid material or the blank of the part is machined in order to obtain the part as defined in the present description. This machining step consists, for example, of grinding the faces (for example on a lathe), then polishing them.

[0083] The invention also relates to a hybrid material obtained or capable of being obtained by the manufacturing process by polymerization of a hybrid material via a polymerization medium, in particular according to one or more of the variants described for this process.

[0084] The invention also relates to a part for plastic scintillation detection comprising a hybrid material which may be as defined according to one or more of the variants described in the present description for this material.

[0085] Generally speaking, the part for plastic scintillation detection is thus composed in whole or in part of a hybrid material comprising: a polymeric matrix; and, a fluorescent mixture incorporated in the polymeric matrix and comprising in molar concentration relative to the total number of moles of primary fluorophore in the incorporated fluorescent mixture i) 95.6% to 99.1% mol of a main primary fluorophore consisting of naphthalene and ii) 0.9% to 4.4% mol of an additional primary fluorophore whose centroid of the light absorption spectrum and of the fluorescence emission spectrum respectively have a wavelength between 250 nm and 340 nm and between 330 nm and 380 nm (or even between 355 nm and 365 nm), the fluorescence decay constant is between 1 ns and 10 ns, and the fluorescence quantum yield in an apolar solvent is between 0.2 and 1 (or even between 0.5 and 1).

[0086] This part can be a unit (such as for example an optical fiber) or a subunit of a device for plastic scintillation detection (for example the hybrid compartment of a phoswich type detector).

[0087] The polymer matrix of the hybrid material making up all or part of the part may be composed in whole or in part of at least one polymer comprising repeating units resulting from the polymerization of monomers comprising at least one aromatic, (meth)acrylic or vinyl group and / or it may be composed in whole or in part of at least one crosslinked polymer.

[0088] At least one monomer intended to form the polymer matrix is ​​selected from styrene, vinyltoluene, vinylxylene, 1-vinylbiphenyl, 2-vinylbiphenyl, 1-vinylnaphthalene, 2-vinylnaphthalene, 1-methylnaphthalene, N-vinylcarbazole, methyl (meth)acrylate, (meth)acrylic acid or 2-hydroxyethyl (meth)acrylate. Preferably, the monomer is styrene or vinyltoluene.

[0089] The part for plastic scintillation detection of the invention can be presented according to the following variants, possibly combined: the hybrid material comprises 1% by mass to 25% by mass (or even 1% by mass to 5% by mass) of the incorporated fluorescent mixture, and / or; the incorporated fluorescent mixture comprises 95.6% to 99.1% by mass of the main primary fluorophore consisting of naphthalene and ii) 0.9% to 4.4% by mass of the additional primary fluorophore. the additional primary fluorophore is covalently bonded to the polymer matrix, and / or; the additional primary fluorophore is selected from 2,5-diphenyloxazole (PPO), [ para ]-terphenyl (pTP), the [meta] -terphenyl (mTP), biphenyl, 2-phenyl-5-(4-biphenyl)-1,3,4-oxadiazole (PBD), 2-(4'-t-butylphenyl)-5-(4"-biphenylyl)-1,3,4-oxiadiazole (Butyl-PBD), anthracene, [ para ]-quaterphenyl, tetraphenylbutadiene, N -ethylcarbazole, the N -(2-ethylhexyl)carbazole, 4-isopropylbiphenyl, [ para]-sexiphenyl, 1-vinylbiphenyl, 2-vinylbiphenyl, 1-vinylnaphthalene, 2-vinylnaphthalene, 1-methylnaphthalene, N -vinylcarbazole, 9-anthracenyl methacrylate or mixtures thereof; the additional primary fluorophore preferably being 2,5-diphenyloxazole (PPO), [ para ]-terphenyl (pTP), or even the [meta]- terphenyl (mTP) or mixtures thereof.

[0090] The incorporated fluorescent mixture of the hybrid material of the part may further comprise a secondary fluorophore, for example at a mass concentration relative to the mass of the hybrid material which is between 0.002% and 0.5% by mass, or even 0.01% by mass to 0.2% by mass of the secondary fluorophore.

[0091] The primary fluorophore may be selected from 1,4-di[2(5-phenyloxazolyl)]benzene, 1,4-bis-(2-methylstyryl)-benzene, 1,4-bis(4-methyl-5-phenyl-2-oxazolyl)benzene, 9,10-diphenylanthracene or mixtures thereof.

[0092] According to a first embodiment, the secondary fluorophore has a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength between 330 nm and 380 nm and between 405 nm and 460 nm, and whose fluorescence quantum yield in an apolar solvent is between 0.5 and 1.

[0093] In this case, the secondary fluorophore may be selected from 1,4-bis(5-phenyl-2-oxazolyl)benzene (POPOP), 1,4-bis(4-methyl-5-phenyl-2-oxazolyl)benzene (dimethylPOPOP), bis-methylstyrylbenzene (bis-MSB), 9,10-diphenylanthracene (9,10-DPA) or mixtures thereof.

[0094] According to a second embodiment, the secondary fluorophore has a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength between 330 nm and 380 nm and between 460 nm and 550 nm, and whose fluorescence quantum yield in an apolar solvent is between 0.5 and 1.

[0095] In this case, the secondary fluorophore may be chosen from coumarin 6, coumarin 7, coumarin 30, coumarin 102, coumarin 151, coumarin 314, coumarin 334, 3-hydroxyflavone or mixtures thereof.

[0096] According to a third embodiment, the secondary fluorophore has a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength between 330 nm and 380 nm and between 550 nm and 630 nm, and whose fluorescence quantum yield in an apolar solvent is between 0.5 and 1.

[0097] In this case, the secondary fluorophore may be chosen from Nile red, rhodamine B or one of its salts, 4-(Dicyanomethylene)-2-methyl-6-(4-dimethylaminostyryl)-4 H -pyrane, pyrromethene 580, or a N -alkyl or N -aryl-perylenediimide.

[0098] Due to the possibility of varying the relative proportion between the main primary fluorophore and the additional primary fluorophore, the hybrid material (and therefore the part for plastic scintillation detection) can have a fluorescence decay constant between 10 ns and 90 ns (or even between 15 ns and 80 ns); particularly between 25 ns and 75 ns, more particularly between 28 ns and 70 ns.

[0099] The part can have a wide variety of shapes, for example a parallelepiped or cylindrical shape.

[0100] The parallelepiped-shaped part is, for example, a plastic scintillator compartment capable of being incorporated into a device for detection by plastic scintillation.

[0101] When the part has a cylindrical shape, and is used for example in the composition of a plastic scintillator pillar, it can have a square or rectangular section.

[0102] When the cylindrical-shaped part is, for example, a scintillating optical fiber (in which case the hybrid material comprises a polymer matrix consisting entirely or partly of at least one polymer which is not crosslinked), it may have a circular, elliptical or hexagonal section.

[0103] An optical fiber is a waveguide that exploits the refractive properties of light. It usually consists of a core surrounded by a cladding. The fiber core has a slightly higher refractive index (a difference of a few thousandths) than the cladding. The light is therefore entirely reflected multiple times at the interface between the inner fiber material constituting the core and the cladding material by total internal reflection.

[0104] The scintillating optical fiber as part of the invention 10 may comprise a polymer fiber 11 composed in whole or in part of the hybrid material and provided or not with a sheath 12 covering the polymer fiber and composed in whole or in part of a sheathing material for optical fiber whose refractive index is lower than that of the hybrid material, the hybrid material comprising a polymer matrix consisting in whole or in part of at least one polymer which is not crosslinked.

[0105] Several scintillating optical fibers can be joined into a fiber bundle.

[0106] The presence of a cladding is not mandatory. For example, when the part is intended to detect an alpha particle, the scintillating optical fiber is composed only of an internal polymer fiber without a cladding to prevent the energy of the incident radiation from being mainly absorbed by the cladding.

[0107] However, most often, the scintillating optical fiber comprises a sheath whose sheathing material is a material usually used for an optical fiber, in particular a scintillating one. For example, the sheathing material is chosen from poly(methyl methacrylate), poly(benzyl methacrylate), poly(trifluoromethyl methacrylate), poly(trifluoroethyl methacrylate) or mixtures thereof.

[0108] The invention also relates to a method of manufacturing by extrusion a part for detection by plastic scintillation and composed in whole or in part of a hybrid material, the part being able to be as defined according to one or more of the variants described in the present description, the method comprising the following successive steps: a') having an extrusion mixture comprising: polymerized ingredients intended to form a polymer matrix as defined in the present description, in particular according to one or more of the variants described, with the exception of the case where the polymer matrix consists in whole or in part (preferably more than 10% by mass of polymer in the polymer matrix) of at least one crosslinked polymer; a fluorescent mixture for extrusion comprising in molar concentration relative to the total number of moles of primary fluorophore in the fluorescent mixture for extrusion: i) 95.6% to 99.1% mol of a main primary fluorophore consisting of naphthalene;and ii) 0.9% to 4.4% mol of an additional primary fluorophore whose centroid of the light absorption spectrum and fluorescence emission spectrum have a wavelength of between 250 nm and 340 nm and between 330 nm and 380 nm, respectively, the fluorescence decay constant is between 1 ns and 10 ns, and the fluorescence quantum yield in a non-polar solvent is between 0.2 and 1; b') under an extrusion atmosphere at an extrusion temperature of between 170°C and 200°C, extruding the extrusion mixture through a die to obtain the part composed in whole or in part of a hybrid material. ;

[0109] An extrusion manufacturing process is essentially a process for transforming polymerized ingredients which, once softened or molten by heat, are continuously pushed through a die which gives its geometry to the polymer-based profile obtained at the end of the process. The extrusion process is well known to those skilled in the art: it is described for example in the document "Techniques de l'ingénieur, Extrusion - extrusion monovis (part 1), Reference AM3650, publication of 2002" [reference 9].

[0110] The polymerized ingredients that can be used are formed from one or more polymers that have thermal stability such that the polymer is not degraded at the temperature required for extrusion, which depends on the glass transition temperature. Their chemical composition is identical to that of the polymer matrix.

[0111] Polymerized ingredients are usually in solid form, especially in the form of granules.

[0112] Extrusion step b') can be carried out using an extruder (for example a single-screw, twin-screw, or multi-screw extruder) or a co-kneader. Typically, the die is positioned at the outlet of the extruder.

[0113] The extrusion atmosphere may be chemically inert to the extrusion mixture. Such an atmosphere limits or prevents oxidation of the resulting polymer matrix. It may include, for example, nitrogen or a rare gas, such as argon.

[0114] Typically, the extrusion process of the invention is carried out at an extrusion temperature below 218°C which is the evaporation temperature of naphthalene at atmospheric pressure, but at a temperature high enough to soften or melt the polymerized ingredients, for example at an extrusion temperature between 170°C and 200°C.

[0115] Extrusion step b') can be carried out using an extruder (for example single-screw, twin-screw or multi-screw type) or a co-kneader.

[0116] The invention also relates to a method of manufacturing by polymerization a part for detection by plastic scintillation and composed in whole or in part of a hybrid material, the part being able to be as defined according to one or more of the variants described in the present description, the method comprising at least one polymerization via a polymerization medium according to the following successive steps: a) in a first mold, having a first polymerization medium comprising: monomers, oligomers or their mixtures intended to form at least one polymer constituting a polymer matrix as defined according to one or more of the variants described in the present description (in particular the case where the polymer matrix is ​​constituted in whole or in part of at least one crosslinked polymer; a liquid fluorescent mixture comprising in molar concentration relative to the total number of moles of primary fluorophore in the liquid fluorescent mixture: i) 95.6% to 99.1% mol of a main primary fluorophore constituted of naphthalene;and ii) 0.9% to 4.4% mol of an additional primary fluorophore whose centroid of the light absorption spectrum and fluorescence emission spectrum have a wavelength of between 250 nm and 340 nm and between 330 nm and 380 nm respectively, the fluorescence decay constant is between 1 ns and 10 ns, and the fluorescence quantum yield in an apolar solvent is between 0.2 and 1; b) polymerizing the first polymerization medium in order to directly obtain the part or a blank of the part which is then modified (for example machined, in particular by drawing the blank) to obtain the part. ;

[0117] In the process of manufacturing a part by polymerization, the fluorescent mixture is liquid, because it is mixed in the first polymerization medium with monomers and / or oligomers.

[0118] The internal volume of the mold can have a parallelepiped or cylindrical shape. The cylindrical shape can be circular, elliptical, hexagonal, square or rectangular in section.

[0119] When the internal volume of the mold has a parallelepiped shape, the manufacturing process by polymerization can be such that the parallelepiped-shaped part obtained at the end of step b) is a plastic scintillator compartment as defined in the present description and capable of being incorporated into a device for detection by plastic scintillation.

[0120] In this case, the parallelepiped-shaped plastic scintillator compartment can be obtained directly at the end of the manufacturing process by polymerization, after an optional rectification step if necessary.

[0121] When the internal volume of the mold has a cylindrical shape, the polymerization manufacturing method may be such that the part is a scintillating optical fiber 10 without a sheath which may be as defined in the present description according to one or more of its variants, such that a cylindrical bar as a blank of the part is obtained at the end of step b), the method comprising the following additional step carried out after step b) of polymerization: c) in a fiberizing tower, softening by heating then drawing the blank of the part in order to obtain a polymer fiber 11 composed in whole or in part of the hybrid material as a scintillating optical fiber 10 without a sheath.

[0122] Alternatively, when the internal volume of the mold has a cylindrical shape, the polymerization manufacturing method may be such that the part is a scintillating optical fiber 10 provided with a sheath 12 which may be as defined in the present description according to one or more of its variants, such that a cylindrical bar as a first blank of the part is obtained at the end of step b), the method comprising the following additional step carried out after step b): b1) placing the first blank of the part in a second cylindrical mold, then filling the free volume delimited by the internal face of the second cylindrical mold and the external face of the first blank of the part with a second polymerization medium comprising a precursor of a cladding material for optical fiber for which the refractive index of the cladding material is lower than that of the hybrid material; b2) polymerizing the second polymerization medium in order to form the cladding material which covers the first blank of the part, in order to obtain a second blank of the part (constituting a preform); c) in a fiberizing tower, soften by heating and then draw the second blank of the part in order to obtain, as a scintillating optical fiber 10 provided with a sheath 12, a polymer fiber 11 composed in whole or in part of the hybrid material and provided with the sheath 12 covering the polymer fiber 11.

[0123] In both of these alternatives, the internal volume of the cylindrical mold has, for example, a circular cross-section. The mold can then have an internal diameter of between 2 cm and 10 cm (typically 5 cm) and / or a longitudinal length of between 10 cm and 100 cm (typically 50 cm). These dimensions generally correspond to those of the cylindrical bar as a preform or blank of the part.

[0124] The precursor of the sheathing material is for example chosen from methyl methacrylate, benzyl methacrylate, trifluoromethyl methacrylate, trifluoroethyl methacrylate or mixtures thereof.

[0125] The blank of the part or preform is generally placed vertically on the fiberizing tower. At the end of step c), the scintillating optical fiber, with or without a sheath, is most often recovered by gravimetric spinning.

[0126] During the polymerization step b) and / or b1), the first polymerization medium may be heated to a first polymerization temperature of between 100°C and 140°C (for example for a period of 12 h to 24 h, in particular one day at 140°C), then cooled according to a reduction in the polymerization temperature of 10°C to 20°C per day until the part or the blank of the part is obtained. Cooling is generally continued until the ambient temperature of 20°C is reached.

[0127] During polymerization step b2), the second polymerization medium may be heated to a second polymerization temperature of between 50°C and 70°C (for example for a period of 8 to 10 days, in particular 10 days at 60°C), then cooled by decreasing the polymerization temperature by 10°C to 20°C per day until the part or the blank of the part is obtained. Cooling is generally continued until the ambient temperature of 25°C is reached.

[0128] The heating operation for softening can be carried out during step c) at a temperature between 150°C and 190°C.

[0129] The blank of the part can be ground just before carrying out step c) of drawing. For example, the cylindrical bar is ground by cutting its upper and lower part over a short length. The upper face of a parallelepiped-shaped part, namely the face which is in light contact with the ambient air, can also be ground by cutting the upper part over a short length and then polishing.

[0130] At the end of the polymerization manufacturing process, the scintillating optical fiber can be such that: the diameter of the polymer fiber 11 is between 50 µm and 1 mm, and / or; the thickness of the cladding 12 is between 1 µm and 20 µm, and / or; the length of the scintillating optical fiber is between 0.1 and 2 km.

[0131] The first polymerization medium and / or the second polymerization medium may comprise a polymerization solvent chosen for example from xylene, chloroform, dichloromethane, chlorobenzene, benzene, tetrachloromethane or mixtures thereof.

[0132] Regarding respectively the process for manufacturing a part by extrusion or the process for manufacturing a part by polymerization, the fluorescent mixture for extrusion or the liquid fluorescent mixture (both comprising i) 95.6% to 99.1% mol of the main primary fluorophore consisting of naphthalene and therefore ii) 0.9% to 4.4% mol of the additional primary fluorophore) may be such that: the additional primary fluorophore has a fluorescence quantum yield in an apolar solvent of between 0.5 and 1, and / or; it comprises a secondary fluorophore as defined in the present description, in particular according to one or more of the variants described.

[0133] The invention also relates to a device for plastic scintillation detection comprising a part for plastic scintillation detection (which may be as defined according to one or more of the variants described in the present description) as a hybrid plastic scintillator element, the part being generally composed in whole or in part of a hybrid material comprising: a polymeric matrix; and, a fluorescent mixture incorporated in the polymeric matrix and comprising in molar concentration relative to the total number of moles of primary fluorophore in the incorporated fluorescent mixture: i) 95.6% to 99.1% mol of a main primary fluorophore consisting of naphthalene; and ii) 0.9% to 4.4% mol of an additional primary fluorophore whose centroid of the light absorption spectrum and of the fluorescence emission spectrum respectively have a wavelength between 250 nm and 340 nm and between 330 nm and 380 nm, the fluorescence decay constant is between 1 ns and 10 ns, and the fluorescence quantum yield in an apolar solvent is between 0.2 and 1 (or even between 0.5 and 1);the part being coupled to an electronic acquisition module such that the module is capable of collecting the radioluminescent radiation emitted by the part when the latter is brought into contact with ionizing radiation or an ionizing particle.;

[0134] The polymer matrix of the hybrid material making up all or part of the part may be composed in whole or in part of at least one polymer comprising repeating units resulting from the polymerization of monomers comprising at least one aromatic, (meth)acrylic or vinyl group and / or it may be composed in whole or in part of at least one crosslinked polymer.

[0135] At least one monomer intended to form the polymer matrix may be chosen from styrene, vinyltoluene, vinylxylene, 1-vinylbiphenyl, 2-vinylbiphenyl, 1-vinylnaphthalene, 2-vinylnaphthalene, 1-methylnaphthalene, N-vinylcarbazole, methyl (meth)acrylate, (meth)acrylic acid or 2-hydroxyethyl (meth)acrylate. Preferably, the monomer is styrene or vinyltoluene.

[0136] The hybrid material making up all or part of the part integrated into the device for detection by plastic scintillation of the invention may be presented according to the following variants, possibly combined: the hybrid material comprises 1% by mass to 25% by mass (or even 1% by mass to 5% by mass) of the incorporated fluorescent mixture, and / or; the additional primary fluorophore is covalently bonded to the polymer matrix, and / or; the additional primary fluorophore is chosen from 2,5-diphenyloxazole (PPO), [ para ]-terphenyl (pTP), the [meta] -terphenyl (mTP), biphenyl, 2-phenyl-5-(4-biphenyl)-1,3,4-oxadiazole (PBD), 2-(4'- t- butylphenyl)-5-(4"-biphenylyl)-1,3,4-oxiadiazole (Butyl-PBD), anthracene, [ para ]-quaterphenyl, tetraphenylbutadiene, N -ethylcarbazole, the N -(2-ethylhexyl)carbazole, 4-isopropylbiphenyl, [ para ]-sexiphenyl, 1-vinylbiphenyl, 2-vinylbiphenyl, 1-vinylnaphthalene, 2-vinylnaphthalene, 1-methylnaphthalene, N-vinylcarbazole, 9-anthracenyl methacrylate or mixtures thereof; the additional primary fluorophore preferably being 2,5-diphenyloxazole (PPO), [ para ]-terphenyl (pTP), or even the [meta]- terphenyl (mTP) or mixtures thereof.

[0137] The incorporated fluorescent mixture of the hybrid material of the part may further comprise a secondary fluorophore, for example at a mass concentration relative to the mass of the hybrid material which is between 0.002% and 0.5% by mass, or even 0.01% by mass to 0.2% by mass of the secondary fluorophore.

[0138] The primary fluorophore may be selected from 1,4-di[2(5-phenyloxazolyl)]benzene, 1,4-bis-(2-methylstyryl)-benzene, 1,4-bis(4-methyl-5-phenyl-2-oxazolyl)benzene, 9,10-diphenylanthracene or mixtures thereof.

[0139] According to a first embodiment, the secondary fluorophore has a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength between 330 nm and 380 nm and between 405 nm and 460 nm, and whose ratio to the mass of the hybrid material is between 0.002% and 0.5% by mass, or even 0.01% by mass to 0.2% by mass of the secondary fluorophore.

[0140] The primary fluorophore may be selected from 1,4-di[2(5-phenyloxazolyl)]benzene, 1,4-bis-(2-methylstyryl)-benzene, 1,4-bis(4-methyl-5-phenyl-2-oxazolyl)benzene, 9,10-diphenylanthracene or mixtures thereof.

[0141] According to a first embodiment, the secondary fluorophore has a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength between 330 nm and 380 nm and between 405 nm and 460 nm, and whose fluorescence quantum yield in an apolar solvent is between 0.5 and 1.

[0142] In this case, the secondary fluorophore may be selected from 1,4-bis(5-phenyl-2-oxazolyl)benzene (POPOP), 1,4-bis(4-methyl-5-phenyl-2-oxazolyl)benzene (dimethylPOPOP), bis-methylstyrylbenzene (bis-MSB), 9,10-diphenylanthracene (9,10-DPA) or mixtures thereof.

[0143] According to a second embodiment, the secondary fluorophore has a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength between 330 nm and 380 nm and between 460 nm and 550 nm, and whose fluorescence quantum yield in an apolar solvent is between 0.5 and 1.

[0144] In this case, the secondary fluorophore may be chosen from coumarin 6, coumarin 7, coumarin 30, coumarin 102, coumarin 151, coumarin 314, coumarin 334, 3-hydroxyflavone or mixtures thereof.

[0145] According to a third embodiment, the secondary fluorophore has a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength between 330 nm and 380 nm and between 550 nm and 630 nm, and whose fluorescence quantum yield in an apolar solvent is between 0.5 and 1.

[0146] In this case, the secondary fluorophore may be chosen from Nile red, rhodamine B or one of its salts, 4-(Dicyanomethylene)-2-methyl-6-(4-dimethylaminostyryl)-4 H -pyrane, pyrromethene 580, or a N- alkyl or N -aryl-perylenediimide.

[0147] Due to the possibility of varying the relative proportion between the main primary fluorophore and the additional primary fluorophore, the hybrid material (and therefore the part for plastic scintillation detection and the device which integrates it) can have a fluorescence decay constant between 10 ns and 90 ns (or even between 15 ns and 80 ns); particularly between 25 ns and 75 ns, more particularly between 28 ns and 70 ns.

[0148] The device part can have a wide variety of shapes, for example, a parallelepiped or cylindrical shape.

[0149] The parallelepiped-shaped part is, for example, a plastic scintillator compartment capable of being incorporated into a device for detection by plastic scintillation.

[0150] When the part has a cylindrical shape, and is used for example in the composition of a plastic scintillator pillar, it can have a square or rectangular section.

[0151] When the cylindrical-shaped part is, for example, a scintillating optical fiber (in which case the hybrid material comprises a polymer matrix consisting entirely or partly of at least one polymer which is not crosslinked), it may have a circular, elliptical or hexagonal section.

[0152] The scintillating optical fiber as part of the invention 10 may comprise a polymer fiber 11 composed in whole or in part of the hybrid material and provided or not with a sheath 12 covering the polymer fiber and composed in whole or in part of a sheathing material for optical fiber whose refractive index is lower than that of the hybrid material, the hybrid material comprising a polymer matrix consisting in whole or in part of at least one polymer which is not crosslinked.

[0153] Several scintillating optical fibers can be joined into a fiber bundle.

[0154] The presence of a cladding is not mandatory. For example, when the part is intended to detect an alpha particle, the scintillating optical fiber is composed only of an internal polymer fiber without a cladding to prevent the energy of the incident radiation from being mainly absorbed by the cladding.

[0155] However, most often, the scintillating optical fiber comprises a sheath whose sheathing material is a material usually used for an optical fiber, in particular a scintillating one. For example, the sheathing material is chosen from poly(methyl methacrylate), poly(benzyl methacrylate), poly(trifluoromethyl methacrylate), poly(trifluoroethyl methacrylate) or mixtures thereof.

[0156] The coupling between the part as a plastic scintillator element and the acquisition module is generally achieved by bringing the acquisition module into contact with a portion of the part from which the radioluminescent radiation emerges from the part.

[0157] According to a first embodiment, the device for detection by plastic scintillation is such that the hybrid plastic scintillator element is a first hybrid plastic scintillator element 1, the device further comprising a second fast plastic scintillator element 2 whose fluorescence decay constant is lower than that of the first hybrid plastic scintillator element 1, these plastic scintillator elements 1 and 2 forming a plastic scintillator assembly.The first hybrid plastic scintillator element 1 is preferably composed in whole or in part of a hybrid material whose fluorescence decay constant is included in one of the above-mentioned ranges for the hybrid material (for example between 10 ns and 90 ns, or even between 15 ns and 80 ns, advantageously between 30 ns and 80 ns, particularly between 70 ns and 80 ns; or between 25 ns and 75 ns or even between 28 ns and 70 ns when the molar concentration of the main primary fluorophore consisting of naphthalene is between 95.6% and 99.1%. The device is preferably a phoswich type device, in which, for example, each plastic scintillator element is a plastic scintillator compartment.

[0158] The invention described is not, however, limited to the incorporation of the hybrid material into a phoswich-type plastic scintillation detector. It is of interest when the person skilled in the art needs a plastic scintillator with a determined and optimized fluorescence decay constant.

[0159] The first hybrid plastic scintillator element 1 may be in direct contact with the second fast plastic scintillator element 2.

[0160] According to another alternative, the first hybrid plastic scintillator element 1 is in contact with the second fast plastic scintillator element 2 via a bonding layer 5. The plastic scintillator assembly therefore further comprises a bonding layer.

[0161] In the case where the plastic scintillator elements are parallelepipedal in shape, the first hybrid plastic scintillator element and the second fast plastic scintillator element are typically in contact with each other via one of their faces, preferably their face with the largest surface area or the same surface area.

[0162] In the case where the plastic scintillator elements are cylindrical in shape, the first hybrid plastic scintillator element and the second fast plastic scintillator element are typically in contact with each other via their circular faces, which are generally of identical surfaces at the location of their contact.

[0163] Taking as a reference the direction of propagation of the ionizing radiation or of the ionizing particle with respect to the device for detection by plastic scintillation, the first hybrid plastic scintillator element can be indifferently the upstream plastic scintillator element or the downstream plastic scintillator element, in which case the second fast plastic scintillator element is respectively the downstream or upstream plastic scintillator element.

[0164] With reference to the direction of propagation of the ionizing radiation or the ionizing particle with respect to the device, the first hybrid plastic scintillator element 1 is preferably the upstream plastic scintillator element and the second fast plastic scintillator element 2 is the downstream plastic scintillator element.

[0165] The plastic scintillator elements 1 and 2 can have different thicknesses, so that the device comprises a thin plastic scintillator element and a thick fast scintillator element. Both configurations are therefore possible: the first hybrid plastic scintillator element can be the thin plastic scintillator element or the thick plastic scintillator element.

[0166] Preferably, the thickness of the first hybrid plastic scintillator element is less than that of the second fast plastic scintillator element. Thus, according to a preferred embodiment of the invention with a view to promoting beta / gamma discrimination, the device may comprise a first thin hybrid plastic scintillator element 1 and a second thick fast plastic scintillator element 2. Preferably, the device then comprises the first thin hybrid plastic scintillator element 1 upstream and the second thick fast plastic scintillator element 2 downstream, with reference to the direction R of propagation of the ionizing radiation or the ionizing particle with respect to the device.

[0167] The thin plastic scintillator element may have a thickness of 10 µm to 1 mm, for example 50 µm to 1 mm, preferably 100 µm to 500 µm; and the thick plastic scintillator element may have a thickness ranging from 1 mm to several centimeters, for example 1 mm to 10 cm, preferably 3 mm to 5 cm.

[0168] The second fast plastic scintillator element 2 may have a fluorescence decay constant between 1 ns and 7 ns.

[0169] The second fast plastic scintillator element 2 may comprise a polymeric matrix which may be as defined in the present description, in particular according to one or more of the variants described for this polymeric matrix, and / or a fast primary fluorophore chosen from 2,5-diphenyloxazole (PPO), [ para ]-terphenyl (pTP), the [meta] -terphenyl (mTP), biphenyl, 2-phenyl-5-(4-biphenyl)-1,3,4-oxadiazole (PBD), 2-(4'- t-butylphenyl)-5-(4"-biphenylyl)-1,3,4-oxadiazole (butyl-PBD), anthracene or mixtures thereof. Preferably, the fast primary fluorophore is 2,5-diphenyloxazole (PPO), [ para ]-terphenyl (pTP), or even the [meta]- terphenyl (mTP) or mixtures thereof.

[0170] The second fast plastic scintillator element 2 may comprise a secondary fluorophore which may be as defined in the present description, in particular according to one or more of the variants described.

[0171] According to a second embodiment, the device for detection by plastic scintillation according to the invention may comprise a single hybrid plastic scintillator element (so-called "single-compartment" plastic scintillation device). Such a single-compartment device is advantageous when coupled to an electronic acquisition module whose sampling frequency is less than 250 MHz: in accordance with the Niquist-Shannon theorem, a long pulse as obtained with a single hybrid plastic scintillator is better described with such an acquisition module for which the electronics are limited in number of points per nanosecond.

[0172] Generally speaking, whatever the embodiment, the part can be coupled to the electronic acquisition module by an optical interface layer 6, namely by optical coupling.

[0173] The optical interface layer has in particular the properties of allowing the radiation emerging from the plastic scintillator element to pass through, in particular in the downstream position. This layer may be composed in whole or in part of a material known to those skilled in the art, for example chosen from greases, glues, gels, cements, elastomeric compounds, silicone compounds or their mixtures.

[0174] The coupling between the part and the electronic acquisition module can be achieved directly or indirectly via the hybrid plastic scintillator element.

[0175] For example, this coupling is usually for the single hybrid plastic scintillator element.

[0176] The coupling with the hybrid plastic scintillator element is, on the other hand, indirect in the case of the phoswich scintillator: the downstream fast plastic scintillator element is interposed between these two parts, and it is the only one to be in direct contact with the electronic acquisition module.

[0177] Concerning the electronic acquisition module, it may comprise a photodetector 3, chosen for example from a photomultiplier, a photodiode, a CCD charge transfer camera or a CMOS sensor.

[0178] The electronic acquisition module may be placed downstream, with reference to the direction of propagation of the ionizing radiation or the ionizing particle with respect to the device, of the part as a hybrid plastic scintillator element, of the single hybrid plastic scintillator element, of the first hybrid plastic scintillator element 1 or of the second fast plastic scintillator element 2.

[0179] It can be energy calibrated using standard glitter materials.

[0180] The invention also relates to an apparatus for detection by plastic scintillation comprising a device as defined in the present description according to one or more of its variants, consisting of a portable apparatus for the detection of ionizing radiation, a detection portal or a CCD detector (English acronym for " Charge Coupled Device ”) .

[0181] The invention also relates to a method of manufacturing a device for plastic scintillation detection as defined in the present description according to one or more of its variants, in which the part as a hybrid plastic scintillator element is coupled (directly or indirectly) to the electronic acquisition module, such that the module is capable of collecting the radioluminescent radiation emitted by the part when the latter is brought into contact with ionizing radiation or an ionizing particle.

[0182] The manufacturing method may be such that the device comprises a plastic scintillator assembly, the method comprising the following successive steps: a") having a first hybrid plastic scintillator element 1 as a part and a second fast plastic scintillator element 2 whose fluorescence decay constant is lower than that of the first hybrid plastic scintillator element 1; each of these plastic scintillator elements further having a polished surface of the same dimension as that of the other plastic scintillator element; b") coupling, via their polished surface, the first hybrid plastic scintillator element 1 and the second fast plastic scintillator element 2 in order to obtain the plastic scintillator assembly; c") coupling the plastic scintillator assembly comprising the part to the electronic acquisition module, such that the module is capable of collecting the radioluminescent radiation emitted by the plastic scintillator assembly when the latter is brought into contact with ionizing radiation or an ionizing particle.

[0183] According to a first embodiment, the method of manufacturing the device is an autogenous coupling method by thermobonding: step b") of coupling bonding can be carried out by heating the polished surface of the first hybrid plastic scintillator element 1 and of the second rapid plastic scintillator element 2 in order to soften these surfaces which are then pressed against each other in order to couple them.

[0184] According to a second embodiment, the method of manufacturing the device comprising a plastic scintillator assembly is a molecular autogenous coupling method (namely autogenous in situ), the method comprising the following successive steps: a‴) a plastic scintillator element, consisting of a first hybrid plastic scintillator element 1 as a part or of a second fast plastic scintillator element 2 whose fluorescence decay constant is lower than that of the first hybrid plastic scintillator element 1, is manufactured in situ by polymerization on the other plastic scintillator element which constitutes a polymerization support, in order to obtain a plastic scintillator assembly at the end of step a‴); b‴) the plastic scintillator assembly comprising the part is coupled to the electronic acquisition module, such that the module is capable of collecting the radioluminescent radiation emitted by the plastic scintillator assembly when the latter is brought into contact with ionizing radiation or an ionizing particle.

[0185] The coupling between the plastic scintillator elements 1 and 2 according to step b"), and / or the coupling according to which the electronic acquisition module is coupled with the plastic scintillator assembly according to step c") or step b‴) or with the single hybrid plastic scintillator element as defined in the present description according to one or more of its variants, can be achieved by means of an optical interface layer 6.

[0186] The optical interface layer 6 may be an optical cement (for example of the EJ-500 type), a so-called “coupling” solvent (generally an alcohol, such as for example isopropanol or 1-butanol) or preferably an optical grease (for example of the RTV141A type).

[0187] This interface layer is typically 1 µm to 10 µm thick.

[0188] The invention also relates to a method of measuring by plastic scintillation, the method comprising the following successive steps: i) a device for plastic scintillation detection as defined in the present description, in particular according to one or more of its variants, is brought into contact with ionizing radiation or an ionizing particle so that the part (thanks to the hybrid material it contains) included in the device emits radioluminescent radiation; and ii) the radioluminescent radiation is measured with the electronic acquisition module of the device.

[0189] Preferably, the duration of the decay of the measured radioluminescent radiation is between 10 ns and 90 ns, even more preferably between 15 ns and 80 ns, even more preferably between 30 ns and 80 ns, particularly between 25 ns and 75 ns, more particularly between 28 ns and 70 ns.

[0190] The ionizing radiation or ionizing particle may originate from a radioactive material emitting gamma rays, X-rays, beta particles, alpha particles or neutrons. Where appropriate, the radioactive material may emit several types of ionizing radiation or ionizing particles. Thus, advantageously, discrimination by virtue of the shape of the different pulses between gamma rays and beta particles can be carried out during measurement step b) with the scintillation measurement method of the invention.

[0191] The radioluminescent radiation resulting from this exposure can be measured according to step ii) with a photodetector, such as for example a photodetector chosen from a photomultiplier, a photodiode, a charge-coupled device camera (CCD for “Charge-Coupled Device camera” in English), a CMOS sensor (for “Complementary Metal-Oxide Semiconductor” in English), or any other photon detector whose capture is converted into an electrical signal.

[0192] According to a preferred embodiment of the invention, the measurement method may comprise a step iii) in which the presence and / or quantity of the radioactive material is determined from the measurement of the radioluminescent radiation according to step ii), as is usually practiced in plastic scintillation. By way of example, step iii) of qualitative and / or quantitative measurement is described by making an analogy with plastic scintillation from the document “Techniques de l'ingénieur, Mesures de radioactivité par scintillation liquide, Référence p2552, publication dated 10 / 03 / 2004 » [reference 10].

[0193] Quantitative determination can in particular measure the activity of the radioactive source. It can be carried out from a calibration curve.

[0194] This curve is for example such that the number of photons from the radioluminescent radiation emitted for a known radioactive material is correlated with the energy of the incident radiation for this radioactive material. From the solid angle, the distance between the radioactive source and the plastic scintillator, and the activity detected by the measuring method using the plastic scintillator of the invention, it is then possible to quantify the activity of the radioactive source.

[0195] Not being the subject of the requested protection, a polymerization composition for manufacturing a hybrid material (as defined in the present description, according to one or more of its variants) for detection by plastic scintillation comprises: monomers, oligomers or their mixtures intended to form at least one polymer constituting a polymer matrix as defined in the present description according to one or more of the variants; a liquid fluorescent mixture comprising in molar concentration relative to the total number of moles of primary fluorophore in the liquid fluorescent mixture: i) 95.6% to 99.1% mol of a main primary fluorophore consisting of naphthalene; and ii) 0.9% to 4.4% mol of an additional primary fluorophore whose centroid of the light absorption spectrum and fluorescence emission spectrum have a wavelength of between 250 nm and 340 nm and between 330 nm and 380 nm, respectively, the fluorescence decay constant is between 1 ns and 10 ns, and the fluorescence quantum yield in an apolar solvent is between 0.2 and 1 (or even between 0.5 and 1).

[0196] The monomers, oligomers or their mixtures may comprise at least one aromatic, (meth)acrylic or vinyl group.

[0197] The liquid fluorescent mixture may comprise a secondary fluorophore, as defined in the present description, according to one or more of its variants.

[0198] Thus, according to some of these variants, the secondary fluorophore can have: a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength between 330 nm and 380 nm and between 405 nm and 460 nm, and whose fluorescence quantum yield in an apolar solvent is between 0.5 and 1, or; a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength between 330 nm and 380 nm and between 460 nm and 550 nm, and whose fluorescence quantum yield in an apolar solvent is between 0.5 and 1, or; a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength between 330 nm and 380 nm and between 550 nm and 630 nm, and whose fluorescence quantum yield in an apolar solvent is between 0.5 and 1, or;a light absorption spectrum and a fluorescence emission spectrum whose centroid is respectively at a wavelength between 330 nm and 380 nm and between 550 nm and 630 nm, and whose fluorescence quantum yield in an apolar solvent is between 0.5 and 1.;

[0199] The secondary fluorophore may be at a mass concentration relative to the mass of the polymerization composition which is between 0.002% and 0.5% by mass.

[0200] The polymerization composition may comprise 1% by mass to 25% by mass of the liquid fluorescent mixture.

[0201] It may also further comprise a polymerization solvent.

[0202] The polymerization composition can be implemented in the manufacturing processes of the hybrid material or the part as described previously.

[0203] Other objects, characteristics and advantages of the invention will now be specified in the following description of particular embodiments of the invention, given for illustrative and non-limiting purposes, with reference to Figures 1 to 8 annexed. BRIEF DESCRIPTION OF THE FIGURES

[0204] There Figure 1 represents a table in which the fluorescence decay constant is measured for hybrid materials that differ in the proportion between the main primary fluorophore and the additional primary fluorophore and by the possible addition of a secondary fluorophore, as well as for comparison for a material not containing an additional primary fluorophore. Figure 2A represents the evolution of the median monoexponential tau fluorescence decay constant as a function of the molar proportion between the main primary fluorophore and the additional primary fluorophore according to the data of the Figure 1. It may represent an abacus appearing in a notice supplied with a ready-to-use kit. For comparison, the Figure 2B represents the evolution of the median monoexponential tau fluorescence decay constant as a function of the molar proportion between a main primary fluorophore different from that of the invention and an additional primary fluorophore. The Figure 3 represents the pulse profile for different plastic scintillators, namely the evolution of their responses in number of counts / second as a function of time expressed in nanoseconds. A pulse recording profile is superimposed on these profiles. The Figure 4 represents the energy spectra of a plastic scintillator of the invention and a commercial slow plastic scintillator. The Figures 5 and 6represent a cross-sectional view of a “phoswich” type device for plastic scintillation detection according to the invention, respectively without and with a bonding layer. The Figure 7 represents a variant of the device of the Figure 6 . There Figure 8 represents the schematic view of a scintillating optical fiber provided with a sheath. PRESENTATION OF SPECIAL EMBODIMENTS

[0205] Unless otherwise stated, examples are performed at atmospheric pressure and room temperature. 1. Production of a hybrid material for plastic scintillation measurement according to the invention. 1.1. Example 1 of manufacturing a plastic scintillator with secondary fluorophore.

[0206] A liquid mixture comprising fluorescent molecules (5% by mass (3.624 g) of naphthalene as the main primary fluorophore + 0.2% by mass (183 mg) of 2,5-diphenyloxazole (PPO) as an additional primary fluorophore and 0.02% by mass (15.2 mg) of 9,10-diphenylanthracene (DPA) as a secondary fluorophore) to which styrene (80 mL or 94.78% by mass) is then added is introduced into a single-necked flask previously dried under an inert argon atmosphere.

[0207] After five cold degassings under vacuum (known as the “freeze-pump-thaw” method in English), the polymerization medium obtained, returned to room temperature, is poured into a mold capable of giving the final shape to the plastic scintillator.

[0208] After five days of heating the sealed mold to 140°C under an inert argon atmosphere, the plastic scintillator is removed from the mold, ground and then polished. 1.2. Example 2 of manufacturing a plastic scintillator with secondary fluorophore.

[0209] A liquid mixture comprising fluorescent molecules (5% by mass of naphthalene (3.624 g) + 0.2% by mass of 2,5-diphenyloxazole (PPO, 183 mg) as primary fluorophores and 0.02% by mass of 1,4-bis(4-methyl-5-phenyl-2-oxazolyl)benzene (dimethylPOPOP, 15.2 mg) as secondary fluorophore) to which styrene (80 mL, 94.78% by mass) is then added is introduced into a single-necked flask previously dried under an inert argon atmosphere.

[0210] After five cold degassings under vacuum, the polymerization medium obtained, returned to room temperature, is poured into a mold.

[0211] After five days of heating the sealed mold to 140°C under an inert argon atmosphere, the plastic scintillator is removed from the mold, ground and then polished. 1.3. Example 3 of manufacturing a plastic scintillator with crosslinked polymer matrix and secondary fluorophore.

[0212] A liquid mixture comprising fluorescent molecules (5% by mass of naphthalene (3.624 g) + 0.2% by mass of 2,5-diphenyloxazole (PPO, 183 mg) as primary fluorophores and 0.02% by mass of 9,10-diphenylanthracene (DPA, 15.2 mg) as secondary fluorophore) to which are then added 80% by mass of styrene (64 mL) then 14.78% by mass of 1,4-butanediyl dimethacrylate (10.3 mL) as crosslinking agent is introduced into a single-necked flask previously dried under an inert argon atmosphere.

[0213] After five cold degassings under vacuum, the polymerization medium obtained, returned to room temperature, is poured into a mold.

[0214] After ten days of heating the sealed mold to 65°C under an inert argon atmosphere, the plastic scintillator is removed from the mold, ground and then polished. 2. Manufacture of a range of plastic scintillators with variable proportion between the primary fluorophores.

[0215] Plastic scintillators are manufactured according to the characteristics specified in the table of Figure 1 according to a manufacturing process similar to that disclosed in the previous examples.

[0216] They differ in the chemical composition of the polymer matrix (St = polystyrene; St / 1,4 = mixture of styrene and 1,4-butanediyl dimethacrylate polymerized in a mass proportion between the two monomers of 5 to 1 respectively) and in the molar ratio between the main primary fluorophore (naphthalene) and the additional primary fluorophore (2,5-diphenyloxazole = PPO). The mass concentration of each primary fluorophore is indicated as a percentage of the total mass of the plastic scintillator, the remainder being therefore made up of the mass percentage of the polymer matrix, of the other primary fluorophore, as well as a constant concentration of 0.02% by mass of 9,10-diphenylanthracene (9,10-DPA) added as a secondary fluorophore not indicated in the table of Figure 1 .

[0217] The fluorescence decay constant tau is measured by time-resolved single-photon counting as previously described. It is generally obtained here by biexponential fitting of the obtained values, with weighting factors for each exponential component being indicated as a percentage in parentheses. To facilitate comparison between different plastic scintillators, the biexponential tau is converted to a median monoexponential tau according to the equation below, for which the quality of the fit of the measurement to the light pulse is assessed by the chi-square, which should ideally be as close as possible to 1. Alternatively, commercial time-resolved single-photon counting equipment automatically calculates the median monoexponential rate or even the biexponential rate from the recorded data.

[0218] The median fluorescence decay monoexponential tau constant can be calculated from the following formula: τ médian = τ rapide × % rapide + τ lent × % lent

[0219] The percentages "% fast" and "% slow" represent the respective weights of fast and slow decay. They are adjusted to best describe the median decay. Their sum is equal to 100%.

[0220] So, the Figure 2Arepresents the evolution of the median monoexponential tau fluorescence decay constant (median monoexponential tau) as a function of the naphthalene / PPO molar ratio. It clearly shows the continuous evolution of the fluorescence decay constant as a function of the molar ratio between the main primary fluorophore and the additional primary fluorophore. This evolution has the form of a decreasing exponential which is the signature of a synergy between the main primary fluorophore and the additional primary fluorophore. In the absence of such a synergy, the evolution of the time constant as a function of the molar ratio would be in the form of a linear line which would directly connect the value at 100% and at 0% reflecting the simple progressive replacement of one primary fluorophore by another.

[0221] For comparison, the main primary fluorophore according to the Figure 2Aof the naphthalene / PPO combination according to the invention has been replaced by pyrene, a compound which belongs to the family of condensed aromatic compounds just like naphthalene, as shown by the molecular structures below:

[0222] The evolution of the median monoexponential tau fluorescence decay constant (median monoexponential tau) is studied as a function of the pyrene / PPO molar ratio in a similar manner to the study of the Figure 2A . The result is illustrated by the Figure 2B which shows that this evolution absolutely does not have the form of a decreasing exponential: there is therefore no synergistic effect between pyrene and PPO, unlike the combination of the main primary fluorophore and the additional primary fluorophore according to the invention.

[0223] Another advantage of using a hybrid material for plastic scintillation measurement is demonstrated by the Figure 3which illustrates the type of response pulse obtained for a plastic scintillator referenced by an index in the figure: fast (index a): reference scintillator “Eljen EJ-200” marketed by the company Eljen Technology; slow (index b): reference scintillator “Eljen EJ-240” marketed by the company Eljen Technology; hybrid (index c): comprising the hybrid material according to the invention.

[0224] The recording profile used (500 ns with a noise of 10 counts / second) is superimposed on the pulses of these three plastic scintillators.

[0225] There Figure 3demonstrates the advantages of a phoswich plastic scintillator comprising a fast compartment and a hybrid compartment according to the invention compared to a phoswich plastic scintillator comprising a fast compartment and a slow compartment: for an electronic noise for example estimated at 10 counts per second, the hybrid pulse of the hybrid compartment has a better signal-to-noise ratio than the slow pulse of the slow compartment, thanks to the higher amplitude of the hybrid pulse.

[0226] Acquisition is performed by opening a time gate for recording these pulses. As previously indicated, the duration of this recording is generally chosen to be 6 to 10 times greater than the highest fluorescence decay constant, this decay constant corresponding for each pulse to the abscissa width of the pulse expressed in nanoseconds. In the case of high counting rates, such as when a high activity radioactive source is placed in the presence of the phoswich device, the use of a slow compartment therefore implies using a much longer recording window: several pulses can then coexist in the same time window (stacking phenomenon), which then results in acquisition errors in the absence of discrimination of these pulses.

[0227] These properties of a hybrid compartment are therefore particularly advantageous for beta particle discrimination in a gamma radiation environment with a "phoswich" device comprising a hybrid compartment (in particular when it is the compartment of the smallest thickness) and a fast compartment, each of these two compartments detecting the beta particle and the gamma radiation respectively. 3. Example of qualitative or quantitative measurement of a radioactive material in plastic scintillation according to the measuring method of the invention. 3.1. Measurement protocol.

[0228] A plastic scintillator comprising the hybrid material of the invention in which a secondary fluorophore is incorporated is connected by means of optical grease to a photomultiplier tube which fulfills the function of photodetector of an electronic acquisition module.

[0229] Following exposure to radioactive material, the plastic scintillator emits scintillation photons which are converted into an electrical signal by the high-voltage photomultiplier tube.

[0230] The electrical signal is then acquired and analyzed using an oscilloscope, spectrometry software, or an electronic acquisition card. The data collected is then processed by computer.

[0231] This analysis results in an energy spectrum histogram representing the channels (derived from an output energy) on the abscissa and the number of counts / second on the ordinate. After calibration with a gamma emitting source of known energy, the energy of the radioactive material to be measured is determined. 3.2. Quantitative measurement with scintillator.

[0232] Based on this measurement protocol, a quantitative measurement is carried out with a radioactive source of beta chlorine-36 with an activity on 4 π equal to 6 kBq. This source is placed on the upper part of the plastic scintillator.

[0233] A cylindrical plastic scintillator with a circular section, 49 mm in diameter and 35 mm high (reference F30B in the table of Figure 1 ) is coupled with Rhodorsil RTV141A optical grease to the photocathode of a photomultiplier (Hamamatsu H1949-51 model) powered by a high voltage (Ortec 556 model). The signal coming out of the photomultiplier is recovered and then digitized by an electronic card specific to the inventor. This card can be replaced by another equivalent electronic card (for example, CAEN DT5730B model) or an oscilloscope (for example, Lecroy Waverunner 640Zi model).

[0234] First, an energy calibration of the system (scintillator + photomultiplier) is carried out using two radioactive sources: one emitting gamma rays in the [0 - 200 keV] region and the other in the [500 - 1.3 MeV] region. This energy calibration is carried out by identifying the channel corresponding to 80% of the Compton front amplitude. For example, if the ordinate of the Compton front corresponds to 100 counts per second, the abscissa on the descent of the Compton front at 80 counts per second associates the Compton front energy (in keV) with the channel.

[0235] In a second step, this calibration carried out, the chlorine-36 beta source is attached to the upper face of the plastic scintillator. The analysis of the energy spectrum gives a read activity of 2.1 kBq (and therefore an intrinsic efficiency according to which 70% of the incident radiation is measured) and a photoelectric peak centered around 250 keV.

[0236] The energy spectrum of the obtained hybrid plastic scintillator is shown in the Figure 4 (index (c')). For comparison, it is superimposed on that of a slow plastic scintillator ("Eljen EJ-240 slow" marketed by the company Eljen Technology - index (b') on the Figure 4 ) whose measured intrinsic efficiency is 54%. 4. Geometries of a device for plastic scintillation detection according to the invention.

[0237] Such a device is described with reference to Figures 5 and 6 which represent, along a longitudinal axis with reference to the radiation R, sections of a plastic scintillator of parallelepiped shape of the “phoswich” type. Thus, unless otherwise indicated, each part of the device represented here is of parallelepiped shape. The same numerical references designate the same elements in these two figures. 4.1. Device with bonding layer.

[0238] According to a first embodiment illustrated by the Figure 5, the plastic scintillation detection device D of the invention comprises a part according to the invention which is a first hybrid plastic scintillator element 1 made entirely or partly of the hybrid material of the invention, and a second fast plastic scintillator element 2. These elements are respectively located upstream and downstream with respect to the direction R of propagation of the incident radiation (or of the incident particle) on the phoswich scintillator. By convention, they are therefore designated in the remainder of the description by “upstream hybrid scintillator 1” and “downstream fast scintillator 2”. In the configuration illustrated by the Figure 5, the upstream hybrid scintillator 1 is called "thin", because it has a smaller longitudinal thickness than the downstream fast scintillator 2 called "thick". The device for plastic scintillation detection of the invention having all these characteristics shows improved discrimination between gamma rays and beta particles.

[0239] The upstream hybrid scintillator 1 and the downstream fast scintillator 2 are optionally contained in an envelope 8 which may constitute the housing or the frame of the device. They are fixed to each other with an optical interface layer forming a bonding layer 5.

[0240] The bonding layer 5 is generally a layer separate from the upstream hybrid scintillator 1 and the downstream fast scintillator 2, for example an adjunct layer. However, it may be a layer composed of an intermediate material resulting from the fusion of the material of the upstream hybrid scintillator 1 and the downstream fast scintillator 2, as for plastic scintillation detectors comprising two scintillators bonded to each other by thermomechanical pressing.

[0241] The bonding layer 5 may be an optical layer which is transparent to luminescent radiation. It may be composed of a bonding material chosen from greases, glues, gels, optical cements, elastomeric compounds, silicone compounds usually used in the optical field. Such a material allows the light radiation leaving the downstream scintillator to pass through.

[0242] A photodetector 3 (such as for example a photomultiplier) is fixed on the downstream fast scintillator 2 with an optical interface layer 6. It is capable of collecting the radioluminescent radiation resulting from the contact of an ionizing particle or ionizing radiation with the scintillators 1 and 2.

[0243] The face of the upstream hybrid scintillator 1 which first receives the incident radiation in the direction of propagation R to be detected is covered with a metal layer 4 which is here thin. This metal layer 4 constitutes an entry window with which the incident radiation (or the incident particle) comes into contact, while preventing the ambient light from also coming into contact with the upstream scintillator by isolating it from the light. The lateral faces of the upstream and downstream scintillators are covered with a reflector or light diffuser 7 composed of a reflective material comprising for example aluminum (aluminized mylar, aluminum foil, ...) or composed of a diffusing material comprising for example Teflon, a paint based on titanium oxide Ti0 2 , a paint based on magnesium oxide MgO, Millipore filter paper. 4.2. Device without bonding layer.

[0244] According to a second embodiment illustrated by the Figure 6, the plastic scintillation detection device D of the invention has a structure as described in document WO 2013076279 [reference 11]. It therefore does not comprise a bonding layer such as the optical interface layer 5 described in Figure 5 The device for detection by plastic scintillation without a bonding layer of the invention nevertheless differs from that described in reference [8] by the fact that it comprises a first hybrid plastic scintillator element consisting entirely or partly of the hybrid material of the invention.

[0245] The plastic scintillation detection device D of the invention without a bonding layer illustrated by the Figure 6comprises a first hybrid plastic scintillator element 1 made entirely or partly of the hybrid material of the invention, and a second fast plastic scintillator element 2. These elements are respectively located upstream and downstream with respect to the direction R of propagation of the incident radiation (or of the incident particle) on the phoswich scintillator. In the configuration illustrated by the Figure 5 , the upstream hybrid scintillator 1 is called "thin", because it has a smaller longitudinal thickness than the downstream fast scintillator 2 called "thick". The device for plastic scintillation detection of the invention having all these characteristics shows improved discrimination between gamma rays and beta particles.

[0246] The upstream hybrid scintillator 1 and the downstream fast scintillator 2 are in direct contact and fixed to each other by an autogenous coupling process. In this coupling process, a first cross-linked plastic scintillator is prepared and then polymerized. After this first solid formulation, the monomer solution containing the fluorescent mixture to manufacture the second scintillator is poured onto the first scintillator, the assembly is then heated.

[0247] The scintillators 1 and 2 are possibly contained in an envelope 8 which can constitute the housing or the frame of the device.

[0248] A photodetector 3 (such as for example a photomultiplier) is fixed on the downstream fast scintillator 2 with an optical interface layer 6. It is capable of collecting the radioluminescent radiation resulting from the contact of an ionizing particle or ionizing radiation with the scintillators 1 and 2.

[0249] The face of the upstream hybrid scintillator 1 which first receives the incident radiation (or the incident particle) in the direction of propagation R to be detected is covered with a light-opaque layer 9. This opaque layer 9 constitutes an entrance window with which the incident radiation comes into contact, while limiting the contact of ambient light with the upstream scintillator.

[0250] The side faces of the upstream and downstream scintillators are covered with a light reflector or diffuser 7. The light-opaque layer 9 is permeable to the passage of beta and gamma radiation. It is composed of an opaque material such as Mylar.

[0251] As previously indicated, the upstream hybrid scintillator 1 may have a smaller thickness than the downstream fast scintillator 2. Such a configuration is represented on the Figure 7 . 4.3. Shimmering optical fiber.

[0252] There Figure 8represents a scintillating optical fiber 10 of cylindrical section. It comprises a polymer fiber 11 composed in whole or in part of the hybrid material of the invention. The polymer fiber 11 constituting the internal core of the fiber is covered with a sheath 12 covering the polymer fiber and composed in whole or in part of a sheathing material.

[0253] The invention is applicable to fields where scintillators are used, in particular: in the industrial field, for example for the measurement of physical parameters of parts during manufacture, for non-destructive inspection of materials, for the control of radioactivity at site entry and exit points and for the control of radioactive waste. in the geophysical field, for example for the evaluation of natural radioactivity in soils. in the field of fundamental physics and, in particular, nuclear physics. in the field of the safety of goods and people, for example for the security of critical infrastructures, the control of goods in circulation (luggage, containers, vehicles, etc.) as well as for the radiation protection of workers in the industrial, nuclear and medical sectors. in the field of medical imaging. REFERENCES CITED

[0254] [1] Moser, S. W.; Harder, W. F.; Hurlbut, C. R.; Kusner, M. R. "Principles and practice of plastic scintillator design", Radiat. Phys. Chem., 1993, Vol. 41, No. 1 / 2, 31-36. [2] Bertrand, G. H. V.; Hamel, M.; Sguerra, F. "Current status on plastic scintillators modifications", Chem. Eur. J., 2014, 20, 15660-15685. [3] Wilkinson, D. H. "The Phoswich - A Multiple Phosphor", Rev. Sci. Instrum. 1952, 23, 414-417. [4] M. Wahl, "Time-Correlated Single Photon Counting", note technique de la société PicoQuant, 2014. [5] D. V. O'Connor, D. Phillips, Time Correlated Single Photon Counting, Academic Press, New York, 1984, pages 25 à 34. [6] Rohwer, L. S., Martin, J. E.; "Measuring the absolute quantum efficiency of luminescent materials", J. Lumin. 2005, 115, pages 77-90. [7] Velapoli, R. A.; Mielenz, K. D. "A Fluorescence Standard Reference Material: Quinine Sulfate Dihydrate", Appl. Opt., 1981, 20, 1718. [8] WO 2013076281.[9] Engineering Techniques, Extrusion - single-screw extrusion (part 1), Reference AM3650, published in 2002.

[10] Engineering Techniques, Radioactivity measurements by liquid scintillation, Reference p2552, published on 03 / 10 / 2004.

[11] WO 2013076279.

Claims

1. Hybrid material for plastic scintillation measurement comprising: - a polymeric matrix; and - a fluorescent mixture incorporated in the polymeric matrix and comprising, in a molar concentration with respect to the total number of moles of primary fluorophore in the incorporated fluorescent mixture: i) from 95.6 molar% to 99.1 molar% of a main primary fluorophore consisting of naphthalene; and ii) from 0.9 molar% to 4.4 molar% of an additional primary fluorophore, the centroid of the light absorption spectrum and of the fluorescence emission spectrum of which have respectively a wavelength comprised between 250 nm and 340 nm and comprised between 330 nm and 380 nm, the fluorescence decay constant of which is comprised between 1 ns and 10 ns and the fluorescence quantum yield in a nonpolar solvent of which is comprised between 0.2 and 1.

2. Hybrid material according claim 1, wherein the incorporated fluorescent mixture comprises from 96 molar% to 99.1 molar% of the main primary fluorophore.

3. Hybrid material according to claim 1 or 2, wherein the incorporated fluorescent mixture further comprises a secondary fluorophore at a concentration by weight with respect to the weight of the hybrid material which is comprised between 0.002% and 0.5% by weight.

4. Process for the manufacture of a hybrid material as defined by any one of claims 1 to 3, by polymerization via a polymerization medium, the process comprising the following successive steps: a) having available a polymerization medium comprising: - monomers, oligomers or their mixtures intended to form at least one constituent polymer of a polymeric matrix as defined in any one of claims 1 to 3; - a liquid fluorescent mixture comprising, in a molar concentration with respect to the total number of moles of primary fluorophore in the liquid fluorescent mixture: i) from 95.6 molar% to 99.1 molar% of a main primary fluorophore consisting of naphthalene; and ii) from 0.9 molar% to 4.4 molar% of an additional primary fluorophore, the centroid of the light absorption spectrum and of the fluorescence emission spectrum of which have respectively a wavelength comprised between 250 nm and 340 nm and comprised between 330 nm and 380 nm, the fluorescence decay constant of which is comprised between 1 ns and 10 ns, and the fluorescence quantum yield in a nonpolar solvent of which is comprised between 0.2 and 1; b) polymerizing the polymerization medium in order to obtain the hybrid material.

5. Part for plastic scintillation detection composed, completely or partially, of a hybrid material as defined by any one of claims 1 to 3.

6. Part for plastic scintillation detection according to claim 5, wherein the part has a : - parallelepipedal shape and is a plastic scintillator compartment capable of being incorporated in a device for plastic scintillation detection, or - cylindrical shape and is a scintillating optical fiber (10) comprising a polymer fiber (11) composed, completely or partially, of the hybrid material and provided or not provided with a sheath (12) covering the polymer fiber and composed, completely or partially, of a sheathing material for an optical fiber, the refractive index of which is less than that of the hybrid material, the hybrid material comprising a polymeric matrix constituted, completely or partially, of at least one polymer which is not crosslinked.

7. Process for the manufacture by extrusion of a part for plastic scintillation detection and composed, completely or partially, of a hybrid material, the part being as defined according to claim 5 or 6, the process comprising the following successive steps: a') having available an extrusion mixture comprising: - polymerized ingredients intended to form a polymeric matrix as defined according to claim 5 ; - a fluorescent mixture for extrusion comprising, in a molar concentration with respect to the total number of moles of primary fluorophore in the fluorescent mixture for extrusion: i) from 95.6 molar% to 99.1 molar% of a main primary fluorophore consisting of naphthalene; and ii) from 0.9 molar% to 4.4 molar% of an additional primary fluorophore, the centroid of the light absorption spectrum and of the fluorescence emission spectrum of which respectively have a wavelength comprised between 250 nm and 340 nm and comprised between 330 nm and 380 nm, the fluorescence decay constant of which is comprised between 1 ns and 10 ns and the fluorescence quantum yield in a nonpolar solvent of which is comprised between 0.2 and 1; b') under an extrusion atmosphere at an extrusion temperature comprised between 170°C and 200°C, extruding the extrusion mixture through a die in order to obtain the part composed, completely or partially, of a hybrid material.

8. Process for the manufacture by polymerization of a part for plastic scintillation detection and composed, completely or partially, of a hybrid material, the part being as defined by claim 5 or 6, the process comprising at least one polymerization via a polymerization medium according to the following successive steps: a) in a first mold, having available a first polymerization medium comprising: - monomers, oligomers or their mixtures intended to form at least one constituent polymer of a polymeric matrix as defined in claim 1 ; - a liquid fluorescent mixture comprising, in a molar concentration with respect to the total number of moles of primary fluorophore in the liquid fluorescent mixture: i) from 95.6 molar% to 99.1 molar% of a main primary fluorophore consisting of naphthalene; and ii) from 0.9 molar% to 4.4 molar% of an additional primary fluorophore, the centroid of the light absorption spectrum and of the fluorescence emission spectrum of which respectively have a wavelength comprised between 250 nm and 340 nm and comprised between 330 nm and 380 nm, the fluorescence decay constant of which is comprised between 1 ns and 10 ns and the fluorescence quantum yield in a nonpolar solvent of which is comprised between 0.2 and 1; b) polymerizing the first polymerization medium in order to directly obtain the part or a preform of the part which is subsequently modified in order to obtain the part.

9. Device for plastic scintillation detection comprising a part as defined according to claim 5 or 6 for plastic scintillation detection as hybrid plastic scintillator element, the part being composed, completely or partially, of a hybrid material as defined according to any one of claims 1 to 3, and the part being coupled to an electronic acquisition module so that the module is capable of collecting the radio-luminescent radiation emitted by the part when the latter is brought into contact with ionizing radiation or an ionizing particle.

10. Device for plastic scintillation detection according to claim 9, wherein the hybrid plastic scintillator element is a first hybrid plastic scintillator element (1), the device further comprising a second fast plastic scintillator element (2), the fluorescence decay constant of which is less than that of the first hybrid plastic scintillator element (1), these plastic scintillator elements (1) and (2) forming a plastic scintillator assembly, the device being for example a device of phoswich type.

11. Device for plastic scintillation detection according to claim 9 or 10, wherein the plastic scintillator elements (1) and (2) have different thicknesses, so that the device comprises a thin plastic scintillator element and a thick fast scintillator element ; the thin first hybrid plastic scintillator element (1) being upstream and the thick second fast plastic scintillator element (2) being downstream, with reference to the direction R of propagation of the ionizing radiation or of the ionizing particle with regard to the device.

12. Device for plastic scintillation detection according to any one of the preceding claims 9 to 11, wherein the part comprises a single hybrid plastic scintillator element.

13. Item of equipment for plastic scintillation detection comprising a device as defined according to any one of claims 9 to 12, constituted by a portable instrument for the detection of ionizing radiation, a walk-through scanner or a CCD detector.

14. Process for the manufacture of a device for plastic scintillation detection as defined by any one of claims 9 to 12, wherein the part as hybrid plastic scintillator element is coupled to the electronic acquisition module, so that the module is capable of collecting the radioluminescent radiation emitted by the part when the latter is brought into contact with an ionizing radiation or an ionizing particle.

15. Plastic scintillation measurement method, the method comprising the following successive steps: i) a device as defined according to any one of claims 9 to 12 or an item of equipment as defined according to claim 13, is brought into contact with an ionizing radiation or an ionizing particle in order for the part comprised in the device to emit radioluminescent radiation; and ii) the radioluminescent radiation is measured with the electronic acquisition module of the device.