Tires with a rubber compound containing a novel polysulfide coupling agent carrying nitrogen-containing associative groups
Patent Information
- Application Number
- DE602019061472
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-04-06
- Filing Date
- 2019-04-04
- Publication Date
- 2024-11-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Tires reinforced with inorganic fillers face challenges in achieving good rigidity for improved road behavior without increasing rolling resistance, as conventional coupling agents like TESPT are expensive and do not provide an optimal balance between rigidity and hysteresis properties.
A rubber composition using a polysulfide with nitrogen associative groups as a coupling agent between the isoprene elastomer and the inorganic filler, such as silica, to enhance the balance between rigidity and hysteresis, reducing production costs and improving tire performance.
The polysulfide coupling agent provides a cost-effective solution that enhances the rigidity and hysteresis properties of tires, improving road behavior and reducing rolling resistance, as demonstrated by increased complex dynamic shear modulus and reduced hysteresis values.
Description
[0001] The field of the present invention is that of tires, in particular tires comprising at least one rubber composition reinforced by an inorganic filler.
[0002] Since fuel savings and the need to protect the environment have become a priority, it has become necessary to produce tires with reduced rolling resistance, without penalizing their other performances.
[0003] This has been made possible in particular thanks to the discovery of new rubber compositions reinforced with specific inorganic fillers called "reinforcing", capable of competing from a reinforcing point of view with a conventional tire-grade carbon black, while offering these compositions a lower hysteresis, synonymous with lower rolling resistance for tires containing them. Rubber compositions filled with such highly dispersible silicas (denoted "HD" or "HDS" for "highly dispersible" or "highly dispersible silica"), usable in tires with low rolling resistance sometimes called "Green Tires" for the energy savings offered to the user ("Green Tire concept"), have been extensively described.Reference is made in particular to patent applications EP0501227, EP0692492, EP0692493, EP0735088, EP0767206, EP0786493, EP0881252, WO99 / 02590, WO99 / 02601, WO99 / 02602, WO99 / 06480, WO00 / 05300 and WO00 / 05301.
[0004] However, although these reinforcing inorganic fillers have high dispersibility, their implementation in a rubber composition nevertheless remains more difficult than for rubber compositions conventionally filled with carbon black.
[0005] Indeed, for reasons of reciprocal affinities, the particles of these inorganic fillers have an unfortunate tendency, in the elastomeric matrix, to agglomerate with each other. These interactions have the harmful consequence of limiting the dispersion of the filler and therefore of limiting the reinforcing properties to a level significantly lower than that which would theoretically be possible to achieve if all the elastomer-inorganic filler bonds likely to be created during the mixing operation were actually obtained. It is known to those skilled in the art that it is necessary to use a coupling agent, also called a bonding agent, which has the function of ensuring the connection between the surface of the inorganic filler particles and the elastomer, while facilitating the dispersion of this inorganic filler within the elastomeric matrix.
[0006] It is recalled here that by "coupling agent" (inorganic filler / elastomer), we mean, in a known manner, an agent capable of establishing a sufficient connection, of a chemical and / or physical nature, between the inorganic filler and the diene elastomer; such a coupling agent, at least bifunctional, has for example as a simplified general formula "YWX", in which: Y represents a functional group (function "Y") which is capable of physically and / or chemically bonding to the inorganic filler, such bonding being able to be established, for example, between a silicon atom of the coupling agent and the surface hydroxyl (OH) groups of the inorganic filler (for example the surface silanols in the case of silica); X represents a functional group (function "X") capable of physically and / or chemically bonding to the diene elastomer, for example via a sulfur atom; W represents a divalent group allowing Y and X to be connected.
[0007] Coupling agents should, in particular, not be confused with simple inorganic filler covering agents which, in a known manner, may comprise the Y function active with respect to the inorganic filler but are devoid of the X function active with respect to the diene elastomer.
[0008] Inorganic filler / elastomer coupling agents, in particular silica / elastomer, have been described in a large number of documents. The best known are bifunctional sulfurized silanes, in particular sulfurized alkoxysilanes, and more particularly, bis 3-triethoxysilylpropyl tetrasulfide (abbreviated TESPT), marketed by the company Evonik under the reference "Si69". Reference may be made in particular to documents FR2206330 and FR2149339 which describe such coupling agents and rubber compositions containing them. TESPT is the reference coupling agent for those skilled in the art for rubber compositions filled with reinforcing inorganic fillers such as silicas. It is generally considered today as the product providing for these compositions the best compromise in terms of safety during scorching, ease of processing and reinforcing power; However, it has the known disadvantage of being very expensive.
[0009] Tire manufacturers are always looking to improve the performance of their tires while reducing production costs, particularly the performance of tires comprising a rubber composition reinforced with a reinforcing inorganic filler and containing an agent for coupling the elastomer with this filler.
[0010] In particular, tire manufacturers want to improve the properties of the tire tread. As is well known, the tread must meet a large number of technical requirements, often contradictory, including high wear resistance, low rolling resistance, etc. In particular, it must provide the tire with good road behavior.
[0011] To improve road handling, it is known that greater rigidity of the top of the tire, particularly the tread, is desirable. Increasing rigidity can be achieved, for example, by increasing the reinforcing filler content or by incorporating certain reinforcing resins into the compositions comprising this tread (see, for example, WO02 / 10269).
[0012] EP3260304A1 describes tire compositions comprising a silane with a polar organic group containing urea for increasing stiffness.
[0013] However, as is known, such an increase in the rigidity of the top of the tire, particularly the tread, can penalize the hysteresis properties and therefore the rolling resistance of the tires.
[0014] The aim of the present invention is to provide a tire comprising at least one rubber composition reinforced by an inorganic filler having good rigidity, therefore good road behavior, without affecting the hysteresis, and therefore the rolling resistance.
[0015] This aim is achieved in that the Applicant has discovered that the compromise between good rigidity (in particular at low and high deformations) and good hysteretic properties could be obtained by using a polysulfide carrying nitrogenous associative groups as a cutting agent for the elastomer with the filler in a rubber composition reinforced by a reinforcing inorganic filler and comprising an isoprene elastomer as the majority elastomer. 1 - SUMMARY OF THE INVENTION
[0016] The subject of the invention is therefore a tire comprising at least one rubber composition based on at least one isoprene elastomer as the majority elastomer, an inorganic filler as the reinforcing filler, a crosslinking system and at least one polysulfide of general formula (I) as an agent for coupling the elastomer with the reinforcing inorganic filler. in which: A 1 and A 2 each represent an associative group comprising at least one nitrogen atom and corresponding to the formula (VII) shown below in which the symbol * represents the direct attachment of the groups A 1 and A 2 to the groups Q1 and Q2 respectively, Q 1 and Q 2 , identical or different, each represent a divalent linking group, x is a number greater than or equal to 2.
[0017] Groups A1 and A2 are identical and correspond to formula (VII) in which the symbol * represents the direct attachment of groups A 1 and A 2 to groups Q 1 and Q 2 respectively.
[0018] According to a preferred embodiment, the groups Q 1 and Q 2 , identical or different, each represent a linear or branched C 1 -C 24 divalent hydrocarbon radical, substituted or not, and optionally interrupted by one or more nitrogen or oxygen atoms, preferably represent a linear or branched C 1 -C 13 divalent hydrocarbon radical, substituted or not, and optionally interrupted by one or more nitrogen or oxygen atoms.
[0019] According to a preferred embodiment, x is a number in a range from 2 to 8, preferably from 2 to 6, more preferably still from 2 to 4.
[0020] According to a preferred embodiment, the coupling agent of the elastomer with the reinforcing inorganic filler is a mixture of polysulfides of general formula (I) with A 1 , A 2 , x, Q 1 and Q 2 as defined above.
[0021] According to a preferred embodiment, the mixture of polysulfides of general formula (I) comprises at least 20 mol% of polysulfides of general formula (I) with x ≥ 4, preferably comprises at least 20 mol% of polysulfides of general formula (I) with x included in a range from 4 to 8, more preferably from 4 to 6.
[0022] According to a preferred embodiment, the polysulfide of general formula (I) corresponds to formula (VIII) or to formula (IX) in which x is a number in a range from 2 to 8, preferably from 2 to 6, more preferably still from 2 to 4, even more preferably x=4.
[0023] According to a preferred embodiment, the coupling agent of the elastomer with the reinforcing inorganic filler is a mixture of polysulfides of formula (VIII) with x as defined previously.
[0024] According to a preferred embodiment, the mixture of polysulfides of general formula (VIII) comprises at least 20 mol% of polysulfides of general formula (I) with x ≥ 4, preferably comprises at least 20 mol% of polysulfides of general formula (VIII) with x included in a range from 4 to 8, more preferably from 4 to 6.
[0025] According to a preferred embodiment, the isoprene elastomer is selected from the group consisting of natural rubber, synthetic polyisoprenes, isoprene copolymers and mixtures thereof.
[0026] According to a preferred embodiment, the isoprene elastomer is a synthetic polyisoprene.
[0027] According to a preferred embodiment, the level of reinforcing inorganic filler in the rubber composition is within a range from 10 to 200 phr, preferably from 30 to 150 phr.
[0028] According to a preferred embodiment, the reinforcing inorganic filler comprises silica.
[0029] According to a preferred embodiment, the silica has a BET specific surface area greater than or equal to 30 m 2 < / g.
[0030] According to a preferred embodiment, in which the level of coupling agent in the rubber composition is within a range of 1 to 20 phr.
[0031] According to a preferred embodiment, the rubber composition further comprises carbon black.
[0032] According to a preferred embodiment, the carbon black content in the rubber composition is within a range of 2 to 20 phr.
[0033] According to a preferred embodiment, the rubber composition further comprises at least one plasticizing agent chosen from extender oils, plasticizing resins and mixtures thereof.
[0034] The present invention overcomes the disadvantages of the prior art. More particularly, it provides tires comprising at least one rubber composition based on at least one isoprene elastomer as the major elastomer, an inorganic filler as the reinforcing filler, a crosslinking system and at least one polysulfide of general formula (I) as an agent for coupling the elastomer with the reinforcing inorganic filler, exhibiting a good compromise between rigidity and hysteretic properties. Advantageously, the new polysulfides of general formula (I) are obtained in a few steps compared to the synthesis of TESPT, with good yields, from inexpensive and readily available raw materials.In addition to improving the aforementioned properties, the use of these polysulfides of general formula (I) in rubber compositions comprising a reinforcing inorganic filler such as silica, and an isoprene elastomer as the majority elastomer, advantageously makes it possible to reduce the production costs of these tires. 2 - MEASUREMENT METHOD USED. Dynamic properties
[0035] The dynamic properties G* and tan(δ) max are measured on a viscoanalyzer (Metravib VA4000), according to the ASTM D 5992-96 standard. The response of a sample of vulcanized composition (cylindrical specimen 2 mm thick and 78 mm 2< in cross-section) is recorded, subjected to alternating sinusoidal shear stress at a frequency of 10 Hz, and at a temperature of 30°C, 60°C and 100°C. A strain amplitude sweep is carried out from 0.1% to 100% (forward cycle), then from 100% to 0.1% (return cycle). The results used are the loss factor tan(δ) and the complex dynamic shear modulus (G*). For the return cycle, the maximum value of tan(δ) observed between 0.1 and 10%, noted tan(δ) max, is indicated.
[0036] The G* values are representative of the stiffness at low strains when G* is measured at 0.1% strain (G* 0.1%) and of the stiffness at medium strains when G* is measured at 100% strain (G* 100%). The results are expressed on a base of 100; the arbitrary value 100 is assigned to the control rubber composition to calculate and then compare the G* 0.1% (respectively the G* 100%) with that of the different rubber compositions to be tested. The value on a base of 100 of the G* 0.1% (respectively the G* 100%) for the rubber composition to be tested is calculated according to the following operation: (measured value of G* 0.1% (respectively of G* 100%) of the rubber composition to be tested / measured value of G* 0.1% (respectively of G* 100%) of the control rubber composition) × 100.
[0037] In this way, a result greater than 100 indicates an increase in the complex dynamic shear modulus which corresponds to an improvement in the stiffness property (therefore an improvement in the behavior performance).
[0038] The tan(δ) max value is representative of the hysteresis of the compound, and in this case of the rolling resistance of the tire. The results are given in base 100; the arbitrary value 100 is assigned to the control to then calculate and compare tan(δ) max of the different samples tested. The value in base 100 for the sample to be tested is calculated according to the operation: (tan(δ)max value of the sample to be tested / tan(δ) max value of the control) × 100. In this way, a result lower than 100 indicates a decrease in hysteresis (therefore an improvement in hysteretic properties) which corresponds to an improvement in rolling resistance performance. Glass transition temperature Tg
[0039] The glass transition temperature Tg is measured in a known manner by DSC (Differential Scanning Calorimetry), according to the ASTM D3418 standard of 1999. 3 - DETAILED DESCRIPTION OF THE INVENTION
[0040] The invention and its advantages will be easily understood in light of the description and the examples of embodiment.
[0041] In this description, unless expressly indicated otherwise, all percentages (%) indicated are percentages by mass.
[0042] On the other hand, any interval of values designated by the expression "between a and b" represents the domain of values going from more than "a" to less than "b" (i.e., excluding the limits a and b) while any interval of values designated by the expression "from a to b" means the domain of values going from "a" up to "b" (i.e., including the strict limits a and b).
[0043] In the present application, "pce" (usually "phr" in English) means the part by weight of a constituent per hundred parts by weight of the elastomer(s), that is to say of the total weight of the elastomer(s).
[0044] When a “majority” compound is referred to, within the meaning of the present invention, this compound is the majority among the compounds of the same type in the composition, i.e. it is the one that represents the largest quantity by mass among the compounds of the same type. Thus, for example, a majority polymer is the polymer representing the largest mass relative to the total mass of the polymers in the composition. In the same way, a so-called majority filler is the one representing the largest mass among the fillers in the composition. For example, in a system comprising a single polymer, this is the majority within the meaning of the present invention; and in a system comprising two polymers, the majority polymer represents more than half of the mass of the polymers. On the contrary, a “minority” compound is a compound that does not represent the largest mass fraction among the compounds of the same type.
[0045] In the context of the invention, the carbon-containing products mentioned in the description may be of fossil or bio-sourced origin. In the latter case, they may be, partially or totally, derived from biomass or obtained from renewable raw materials derived from biomass. This includes in particular polymers, plasticizers, fillers, etc.
[0046] The tires according to the invention comprise at least one rubber composition based on at least one isoprene elastomer as the majority elastomer, an inorganic filler as the reinforcing filler, a crosslinking system and at least one polysulfide of general formula (I) as defined in claim 1 as an agent for coupling the elastomer with the reinforcing inorganic filler. Isoprenic diene elastomer
[0047] The rubber compositions usable in the tires in accordance with the invention comprise at least one isoprene elastomer as the majority elastomer.
[0048] The term "isoprene elastomer" is understood to mean, in a known manner, a homopolymer or a copolymer of isoprene.
[0049] Synthetic polyisoprenes and isoprene copolymers can have any microstructure which depends on the polymerization conditions used, in particular the presence or absence of a modifying and / or randomizing agent and the quantities of modifying and / or randomizing agent used. Isoprene diene elastomers can be, for example, block, random, sequenced, microsequenced.
[0050] According to an advantageous embodiment of the invention, the isoprene elastomer may be an isoprene styrenic thermoplastic elastomer. Isoprenic styrenic thermoplastic elastomers are, in a known manner, part of the family of thermoplastic elastomers (abbreviated as "TPE"). With an intermediate structure between thermoplastic polymers and elastomers, they consist of rigid polystyrene blocks connected by flexible isoprene elastomer blocks. They are often triblock elastomers with two rigid segments connected by a flexible segment. The rigid and flexible segments may be arranged linearly, in a star shape or branched. Typically, each of these segments or blocks contains at least more than 5, generally more than 10 basic units (for example styrene units and isoprene units for a styrene / isoprene / styrene block copolymer).
[0051] By styrene, should be understood in the present description any styrene-based monomer, unsubstituted or substituted; among the substituted styrenes that may be cited for example methylstyrenes (for example α-methylstyrene, β-methylstyrene, p -methylstyrene, tert -butylstyrene), chlorostyrenes (e.g. monochlorostyrene, dichlorostyrene), bromostyrenes.
[0052] The number-average molecular mass (Mn) of the isoprene styrenic thermoplastic elastomer is preferably between 30,000 and 500,000 g / mol, more preferably between 40,000 and 400,000 g / mol. Below the indicated minima, the cohesion between the elastomer chains, in particular due to the possible dilution of the latter by an extender oil, risks being affected; on the other hand, an increase in the operating temperature risks affecting the mechanical properties, in particular the breaking properties, with the consequence of reduced performance "when hot". Furthermore, too high a mass Mn can be detrimental. Thus, it has been found that a value in the range of 50,000 to 300,000 g / mol is particularly well suited, in particular for use in a composition in a tire.
[0053] The number-average molecular mass (Mn) of the styrenic isoprene thermoplastic elastomer is determined in a known manner by size exclusion chromatography (SEC). The sample is first solubilized in tetrahydrofuran at a concentration of approximately 1 g / l; then the solution is filtered through a 0.45 µm porosity filter before injection. The equipment used is a "WATERS alliance" chromatographic chain. The elution solvent is tetrahydrofuran, the flow rate is 0.7 ml / min, the system temperature is 35°C and the analysis time is 90 min. A set of four WATERS columns in series, with the trade names "STYRAGEL" ("HMW7", "HMW6E" and two "HT6E"), is used. The injected volume of the polymer sample solution is 100 µl. The detector is a "WATERS 2410" differential refractometer and its associated software for processing chromatographic data is the "WATERS MILLENIUM" system.The calculated average molar masses are relative to a calibration curve produced with polystyrene standards.
[0054] The polydispersity index Ip (reminder: Ip = Mw / Mn with Mw weight average molecular mass) of the isoprene styrenic thermoplastic elastomer is preferably less than 3; more preferably Ip is less than 2.
[0055] Preferably, the weight content of styrene in the styrenic isoprene thermoplastic elastomer is between 5% and 50%. Below the minimum indicated, the thermoplastic character of the elastomer risks decreasing significantly while above the recommended maximum, the elasticity of the composition may be affected. For these reasons, the styrene content is more preferably between 10% and 40%, in particular between 15 and 35%.
[0056] The elastomer blocks of the isoprene styrenic thermoplastic elastomer for the purposes of the invention may be any type of isoprene elastomer known to those skilled in the art. They generally have a Tg of less than 25°C, preferably less than 10°C, more preferably less than 0°C and very preferably less than -10°C. Also preferably, the elastomer block Tg of the isoprene styrenic thermoplastic elastomer is greater than -100°C.
[0057] The elastomer block of the isoprene styrenic thermoplastic elastomer is preferably composed predominantly of an isoprene elastomer portion. By predominantly, we mean a weight ratio of isoprene monomer that is the highest relative to the total weight of the elastomer block, and preferably a weight ratio of more than 50%, more preferably more than 75% and even more preferably more than 85%.
[0058] According to one variant, the isoprene monomers polymerized to form the isoprene elastomer part may be copolymerized, in a statistical manner, with at least one other monomer so as to form this elastomer block. According to this variant, the molar fraction of polymerized monomer other than an isoprene monomer, relative to the total number of units of the elastomer block, must be such that this block retains its elastomer properties. Advantageously, the molar fraction of this other co-monomer may range from 0 to 50%, more preferably from 0 to 45% and even more preferably from 0 to 40%.
[0059] By way of illustration, this other monomer capable of copolymerizing with the isoprene monomer may be chosen from ethylenic monomers such as ethylene, diene monomers, more particularly, conjugated diene monomers having 4 to 14 carbon atoms other than isoprene, vinylaromatic type monomers having from 8 to 20 carbon atoms as defined below or else, it may be a monomer such as vinyl acetate.Preferably, the conjugated diene monomers are selected from butadiene, piperylene, 2-methylbutadiene, 2,3-dimethyl-1,3-butadiene, 2,4-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 3-methyl-1,3-pentadiene, 4-methyl-1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 2,5-dimethyl-1,3-pentadiene, 2-methyl-1,4-pentadiene, 1,3-hexadiene, 2-methyl-1,3-hexadiene, 2-methyl-1,5-hexadiene, 3-methyl-1,3-hexadiene, 4-methyl-1,3-hexadiene, 5-methyl-1,3-hexadiene, 2,5-dimethyl-1,3-hexadiene, 2,5-dimethyl-2,4-hexadiene, 2-neopentyl-1,3-butadiene, 1,3-cyclopentadiene, methylcyclopentadiene, 2-methyl-1,6-heptadiene, 1,3-cyclohexadiene, 1-vinyl-1,3-cyclohexadiene or a mixture thereof. More preferably still, the diene monomer is butadiene.
[0060] Preferably, the styrenic isoprene thermoplastic elastomer may be chosen in particular from the group consisting of styrene / isoprene block copolymers (SI), styrene / butadiene / isoprene block copolymers (SBI), styrene / isoprene / styrene block copolymers (SIS), styrene / butadiene / isoprene / styrene block copolymers (SBIS) and mixtures of these copolymers.
[0061] According to another preferred embodiment, the isoprene elastomer is chosen from the group consisting of natural rubber (NR), synthetic polyisoprenes (IR), different isoprene copolymers and mixtures of these elastomers. Among the isoprene copolymers, mention will be made in particular of isobutene-isoprene (IIR), isoprene-styrene (SIR), isoprene-butadiene (BIR) or isoprene-butadiene-styrene (SBIR) copolymers.
[0062] More preferably according to this embodiment, the isoprene elastomer is natural rubber or a synthetic polyisoprene.
[0063] More preferably still, the isoprene elastomer is a synthetic polyisoprene.
[0064] Particularly suitable are synthetic polyisoprenes with a molar rate of cis-1,4 chains (units) greater than 90%, more preferably still greater than 95%.
[0065] The isoprene elastomer represents the majority elastomer of the rubber compositions usable in the tires according to the invention, that is to say that the mass fraction of the isoprene elastomer in these rubber compositions is greater than 50%, preferably greater than or equal to 60% relative to the total mass of the elastomers present in these rubber compositions. Preferably, the rate of the isoprene elastomer (preferably synthetic polyisoprene) is greater than 50 phr, more preferably still greater than or equal to 60 phr.
[0066] According to an advantageous embodiment, the isoprene elastomer (preferably synthetic polyisoprene) is the only diene elastomer of the rubber compositions usable in the tires according to the invention. It may be a single isoprene elastomer or a mixture of isoprene elastomers, for example a mixture of natural rubber and a synthetic polyisoprene.
[0067] According to another advantageous embodiment, the isoprene elastomer (preferably synthetic polyisoprene) is used in a blend (mixture) with at least one other diene elastomer, in particular different from the isoprene elastomer (preferably different from a synthetic polyisoprene).
[0068] By "diene elastomer (or indistinctly "rubber"; the two terms being considered synonymous)", whether natural or synthetic, must be understood in a known manner an elastomer derived at least in part (i.e., a homopolymer or a copolymer) from diene monomers (monomers carrying two carbon-carbon double bonds, conjugated or not).
[0069] Diene elastomers can be classified into two categories: those called "essentially unsaturated" and those called "essentially saturated". "Essentially unsaturated" is generally understood to mean a diene elastomer derived at least in part from conjugated diene monomers, having a content of units or motifs of diene origin (conjugated dienes) which is greater than 15% (mol %); thus, diene elastomers such as butyl rubbers or copolymers of dienes and alpha-olefins such as EPDM do not fall within the previous definition and can be described in particular as "essentially saturated" diene elastomers (low or very low content of motifs of diene origin, always less than 15% (mol %)).In the category of “essentially unsaturated” diene elastomers, a “highly unsaturated” diene elastomer is understood to mean in particular a diene elastomer having a content of units of diene origin (conjugated dienes) which is greater than 50% (mol %).
[0070] This other diene elastomer (or additional diene elastomer) may be chosen from polybutadienes (abbreviated as "BR"), butadiene copolymers and blends of these diene elastomers. Such butadiene copolymers are more preferably chosen from the group consisting of butadiene-styrene copolymers (abbreviated as "SBR") whether the latter are prepared by emulsion polymerization ("ESBR") or by solution polymerization ("SSBR"). These other aforementioned elastomers may have any microstructure which depends on the polymerization conditions used, in particular the presence or absence of a modifying and / or randomizing agent and the quantities of modifying and / or randomizing agent used. They may be coupled and / or star-shaped or even functionalized with a coupling and / or star-shaped or functionalizing agent.For coupling to carbon black, examples that may be mentioned are functional groups comprising a C-Sn bond or amine functional groups such as aminobenzophenone for example; for coupling to a reinforcing inorganic filler such as silica, examples that may be mentioned are silanol or polysiloxane functional groups having a silanol end (as described for example in FR 2 740 778 or US 6 013 718, and WO 2008 / 141702), alkoxysilane groups (as described for example in FR 2 765 882 or US 5 977 238), carboxylic groups (as described for example in WO 01 / 92402 or US 6 815 473, WO 2004 / 096865 or US 2006 / 0089445) or polyether groups (as described for example in EP 1127909 or US6503973, WO2009 / 000750 and WO2009 / 000752).
[0071] When an additional diene elastomer is present in the rubber compositions usable in the tires of the invention, its content is less than 50 pce, preferably less than or equal to 40 pce.
[0072] The isoprene elastomers of the composition can be used in combination with any type of synthetic elastomer other than diene, or even with polymers other than elastomers, for example thermoplastic polymers. Reinforcing charge
[0073] The rubber compositions usable in the tires of the invention comprise at least one inorganic filler as a reinforcing filler.
[0074] By "reinforcing inorganic filler" is meant here, as is known, any inorganic or mineral filler, whatever its color and origin (natural or synthetic), also called "white" filler, "light" filler or even "non-black" filler ( "non-blackfiller" ) as opposed to carbon black, this inorganic filler being capable of reinforcing on its own, without any other means than an intermediate coupling agent, a rubber composition intended for the manufacture of tires, in other words capable of replacing, in its reinforcing function, a conventional tire-grade carbon black; such a filler is generally characterized, in a known manner, by the presence of hydroxyl groups (-OH) on its surface.
[0075] Preferably, the reinforcing inorganic filler is a siliceous or aluminous type filler, or a mixture of these two types of fillers. Preferably, the reinforcing inorganic filler comprises silica. Even more preferably, the reinforcing inorganic filler consists of silica.
[0076] The silica (SiO 2 ) used may be any reinforcing silica known to those skilled in the art, in particular any silica (in particular precipitated or pyrogenic) having a BET specific surface area greater than or equal to 30 m 2 < / g, preferably greater than or equal to 60 m 2 < / g. Preferably, the silica (SiO 2 ) used may be any reinforcing silica known to those skilled in the art, in particular any silica (in particular precipitated or pyrogenic) having a BET specific surface area less than 450 m 2 < / g, preferably within a range from 30 to 400 m 2 < / g.
[0077] More preferably still, the silica may be any silica, in particular precipitated or pyrogenic, having a BET specific surface area and a CTAB specific surface area both less than 450 m 2 < / g, preferably within a range from 30 to 400 m 2 < / g. Highly dispersible precipitated silicas (known as "HDS" for "highly dispersible" or "highly dispersible silica") are preferred, in particular for the manufacture of tires having low rolling resistance; Examples of such silicas include “Ultrasil 7000” silicas from Evonik, “Zeosil 1165 MP, 1135 MP, 1115 MP and Zeosil premium 200 MP” silicas from Solvay, “Hi-Sil EZ150G” silica from PPG, and “Zeopol 8715, 8745 or 8755” silicas from Huber.
[0078] The reinforcing alumina (Al 2 O 3 ) preferably used is a highly dispersible alumina having a BET surface area ranging from 30 to 400 m 2 < / g, more preferably between 60 and 250 m 2 < / g, an average particle size at most equal to 500 nm, more preferably at most equal to 200 nm. As non-limiting examples of such reinforcing aluminas, mention may in particular be made of the aluminas “Baikalox A125” or “CR125” (Baïkowski company), “APA-100RDX” (Condéa), “Aluminoxid C” (Evonik) or “AKP-G015” (Sumitomo Chemicals).
[0079] As other examples of inorganic filler capable of being used in the rubber compositions usable in the tires of the invention, mention may also be made of aluminum oxides, aluminum hydroxides, aluminosilicates, titanium oxides, silicon carbides or nitrides, all of the reinforcing type as described for example in applications WO99 / 28376-A2, WO00 / 73372-A1, WO02 / 053634-A1, WO2004 / 003067-A1, WO2004 / 056915-A2, US6610261-B1 and US6747087-B2.
[0080] The physical state in which the reinforcing inorganic filler is present is indifferent, whether in the form of powder, microbeads, granules, beads or any other suitable densified form. Of course, the term reinforcing inorganic filler also means mixtures of different reinforcing inorganic fillers, in particular highly dispersible siliceous and / or aluminous fillers as described above.
[0081] In this paper, the BET specific surface area is determined by gas adsorption using the Brunauer-Emmett-Teller method described in "The Journal of the American Chemical Society" (Vol. 60, page 309, February 1938), and more precisely according to a method adapted from the NF ISO 5794-1 standard, Annex E of June 2010 [multipoint volumetric method (5 points) - gas: nitrogen - vacuum degassing: one hour at 160°C - relative pressure range p / in: 0.05 to 0.2]. The CTAB specific surface area values were determined according to the NF ISO 5794-1 standard, Annex G of June 2010. The method is based on the adsorption of CTAB (N-hexadecyl-N,N,N-trimethylammonium bromide) on the "external" surface of the reinforcing filler.
[0082] Finally, a person skilled in the art will understand that, as a filler equivalent to the reinforcing inorganic filler described in this paragraph, a reinforcing filler of another nature, in particular organic, could be used, provided that this reinforcing filler is covered with an inorganic layer such as silica, or else comprises functional sites on its surface, in particular hydroxyl sites, requiring the use of a coupling agent to establish the bond between the filler and the elastomer. Examples of such organic fillers include functionalized polyvinylaromatic organic fillers as described in applications WO2006 / 069792-A1 and WO2006 / 069793-A1.
[0083] A person skilled in the art will be able to adapt the level of reinforcing inorganic filler according to the nature of the inorganic filler used and according to the type of tire concerned, for example for a motorcycle, for a passenger vehicle or for a utility vehicle such as a van or heavy goods vehicle. Preferably, the level of reinforcing inorganic filler (preferably the level of silica) in the rubber composition usable in the tires of the invention is within a range from 10 to 200 phr, more preferably from 30 to 150 phr, and even more preferably from 60 to 140 phr, the optimum being, in a known manner, different according to the particular applications targeted.
[0084] According to a preferred embodiment, the rubber compositions usable in the tires of the invention may further comprise carbon black.
[0085] Suitable carbon blacks are all carbon blacks, including blacks conventionally used in tires (so-called tire-grade blacks). Among the latter, we will mention in particular the reinforcing carbon blacks of the 100, 200, 300 series, or the 500, 600 or 700 series blacks (ASTM grades), such as for example blacks N115, N134, N234, N326, N330, N339, N347, N375, N550, N683, N772). These carbon blacks can be used in the isolated state, as commercially available, or in any other form, for example as a carrier for certain of the rubber additives used.
[0086] The quantity of carbon black present in the rubber compositions usable for the tires of the invention can vary within wide limits; it is preferably lower than that of the reinforcing inorganic filler. Advantageously, carbon black is used in a very small proportion, with a rate in a range from 2 to 20 phr and preferably at a rate of less than 10 phr in the rubber compositions usable for the tires of the invention. Within the ranges indicated, the coloring (black pigmenting agent) and anti-UV properties of carbon blacks are benefited from, without otherwise penalizing the typical performances provided by the reinforcing inorganic filler. Of course, the rubber compositions usable in the tires of the invention can be completely free of carbon black. Coupling agent for elastomer and reinforcing inorganic filler Polysulfide of general formula (I)
[0087] The polysulfide used in the rubber compositions usable in the tires of the invention therefore corresponds to the general formula (I) above. in which S is a sulfur atom, x is an integer or decimal number greater than or equal to 2, A 1 and A 2 each represent an associative group comprising at least one nitrogen atom and corresponding to formula (VII) defined above, and Q 1 and Q 2 , identical or different, each represent a divalent linking group. The polysulfide of general formula (I), thanks to its dual functionality, is used as an agent for coupling the elastomer with the reinforcing inorganic filler in the rubber compositions usable in the tires of the invention. In particular, it makes it possible to improve the compromise of stiffness / hysteresis properties (and therefore the compromise of behavior / rolling resistance performance) compared to tires comprising a rubber composition usually comprising TEPST as an agent for coupling the elastomer with the reinforcing inorganic filler.
[0088] By "associative groups" is meant groups capable of associating with each other in particular by hydrogen, ionic and / or hydrophobic bonds. According to a preferred embodiment of the invention, these are groups capable of associating with each other by hydrogen bonds.
[0089] When the associative groups are capable of associating by hydrogen bonds, each associative group preferably comprises at least one donor "site" and one acceptor site with respect to the hydrogen bond so that two identical associative groups are self-complementary and can associate with each other by forming at least two hydrogen bonds.
[0090] The associative groups according to the invention are also capable of associating by hydrogen, ionic and / or hydrophobic bonds with functions present on fillers, in particular on reinforcing fillers and in particular on inorganic reinforcing fillers, such as silica.
[0091] Groups A1 and A2 are identical and correspond to formula (VII) in which the symbol * represents the direct attachment of groups A 1 and A 2 to groups Q 1 and Q 2 respectively.
[0092] The linking groups Q 1 and Q 2 can be any divalent radical. They are preferably chosen so as not to interfere, or to interfere only slightly, with the associating groups A 1 and A2.
[0093] Said groups Q 1 and Q 2 are then considered as groups inert with respect to the associative groups A 1 and A 2 . By “group inert with respect to the associative groups A 1 and A 2”, we mean a group which does not comprise associative functions as defined according to the invention.
[0094] The groups Q 1 and Q 2 are preferably, independently of each other, a divalent, linear, branched or cyclic hydrocarbon radical. They may independently contain one or more aromatic radicals, and / or one or more heteroatoms such as the nitrogen atom, the sulfur atom, the oxygen atom. This divalent hydrocarbon radical may optionally be substituted, the substituents preferably being inert with respect to the associative groups A 1 and A 2 .
[0095] According to a preferred embodiment, the groups Q 1 and Q 2 , identical or different, each represent a linear or branched C 1 -C 24 divalent hydrocarbon radical, substituted or not, and optionally interrupted by one or more nitrogen or oxygen atoms. More preferably, Q 1 and Q 2 , identical or different, each represent a linear or branched C 1 -C 13 divalent hydrocarbon radical, substituted or not, and optionally interrupted by one or more nitrogen or oxygen atoms. Even more preferably, Q 1 and Q 2 , identical or different, each represent a linear C 1 -C 6 alkanediyl.
[0096] The groups Q 1 and Q 2 may be different or the same, but preferably Q 1 and Q 2 are the same.
[0097] In the general formula (I) above, the symbol x denotes a number, in particular an integer or a decimal number, x is a number greater than 2, more preferably a number in a range from 2 to 8, preferably in a range from 2 to 6, even more preferably in a range from 2 to 4.
[0098] According to particular embodiments, x is a number ranging from 2 to 5, or x is a number ranging from 2 to 4, or x is a number ranging from 3 to 8, or x is a number ranging from 3 to 5 or x is a number equal to 2 or 3, or x is a number equal to 3 or 4.
[0099] According to other particular embodiments, x is 2, or 3, or 4, or 5 or 6.
[0100] Preferably, the agent for coupling the elastomer with the reinforcing inorganic filler is a polysulfide of general formula (I) above in which A 1 and A 2 are identical and each represent an associative group of formula (VII), Q 1 and Q 2 are identical and each represent a linear C 1 -C 13 alkanediyl, preferably C 1 -C 6 , and x is a number greater than 2, more preferably a number in a range from 2 to 8, preferably in a range from 2 to 6, even more preferably in a range from 2 to 4.
[0101] More preferably still, the agent for coupling the elastomer with the reinforcing inorganic filler used in the rubber compositions for the tires of the invention is a polysulfide chosen from the following polysulfides of formula (VIII) or (IX): in which x is a number greater than or equal to 2, preferably within a range from 2 to 8, preferably from 2 to 6, more preferably still from 2 to 4, even more preferably x = 4.
[0102] More preferably still, the polysulfide coupling agent used in the rubber compositions usable in the tires of the invention is a polysulfide of the following formula (X) or (XI):
[0103] The synthesized polysulfides of general formula (I) may be mixtures of polysulfides (for example from x = 2 to x = 8) with consequently an average value for x which may possibly be different from an integer value. The average value for x is preferably in a range from 2 to 6, preferably from 3 to 5, more preferably still from 3.5 to 4.5.
[0104] The chemical nature of the polysulfides of formula (I) can be determined by any technique well known to those skilled in the art, in particular by 1< H NMR. In the case of a mixture, it may be necessary, in certain cases, to separate the different species of the mixture by any technique well known to those skilled in the art before carrying out a 1< H NMR analysis.
[0105] Advantageously, the agent for coupling the elastomer with the reinforcing inorganic filler is a mixture of polysulfides of general formula (I), said mixture comprising at least 20 mol% of polysulfide of general formula (I) with x≥4 (preferably with x within a range from 4 to 8, more preferably from 4 to 6).
[0106] More preferably still, the synthesized polysulfides of general formula (VIII) may be mixtures of polysulfides (for example from x = 2 to x = 8) with consequently an average value for x which may possibly be different from an integer value. The average value for x is preferably within a range from 2 to 6, preferably from 3 to 5, more preferably still from 3.5 to 4.5.
[0107] Advantageously, the agent for coupling the elastomer with the reinforcing inorganic filler is a mixture of polysulfides of general formula (VIII), said mixture comprising at least 20 mol% of polysulfide of general formula (VIII) with x≥4 (preferably with x included in a range from 4 to 8, more preferably from 4 to 6).
[0108] A person skilled in the art knows how to adapt the quantity of coupling agent, i.e. the level of polysulfide of general formula (I) or of the mixture of polysulfides of general formula (I) (preferably the level of polysulfide of formula (VIII) or of the mixture of polysulfides of formula (VIII)) as a function of the level of reinforcing inorganic filler of the rubber compositions which can be used in the tires according to the invention. The polysulfides of general formula (I) or the mixture of polysulfides of general formula (I) (preferably those of formula (VIII)) have proven to be sufficiently effective on their own for coupling an elastomer and a reinforcing inorganic filler, such as silica, and can be used at a preferential level greater than 1 pce (part by weight per hundred parts of elastomers).Advantageously, the level of polysulfide(s) of general formula (I) (preferably of formula (VIII)) in the rubber compositions which can be used for the tires of the invention is within a range from 1 to 20 phr, preferably from 1 to 10 phr.
[0109] The polysulfides of general formula (I) (preferably the polysulfides of formula (VIII)) can advantageously constitute the only coupling agent of the elastomer with the reinforcing inorganic filler present in the rubber compositions usable in the compositions of the invention. However, according to a particular embodiment, the rubber compositions usable in the tires according to the invention can comprise an additional coupling agent different from the polysulfide of general formula (I), in particular the polysulfide of formula (VIII) or the mixture of polysulfides of general formula (I), in particular the mixture of polysulfides of formula (VIII).
[0110] This additional coupling agent may be chosen from the group consisting of polysulfurized organosilanes (symmetrical or asymmetrical) such as bis(3-triethoxysilylpropyl) tetrasulfide, abbreviated to TESPT, marketed under the name “Si69” by the company Evonik, or bis-(triethoxysilylpropyl) disulfide, abbreviated to TESPD, marketed under the name “Si75” by the company Evonik, polyorganosiloxanes, mercaptosilanes, blocked mercaptosilanes, such as “NXT-Silane” marketed by the company Momentive.
[0111] In this particular embodiment, the weight fraction of the additional coupling agent is in the minority. It is preferably less than 50% by weight relative to the total weight of the coupling agents (total weight of the coupling agents = weight of the polysulfide(s) of general formula (I), in particular of formula (VIII), + weight of the additional coupling agent).
[0112] When the rubber compositions usable in the tires of the invention comprise an additional coupling agent, the total level of coupling agents in the rubber compositions is within a range from 1 to 20 phr, preferably from 1 to 10 phr. Processes for the preparation of polysulfides of general formula (I)
[0113] Polysulfides of general formula (I) may be prepared by a process generally comprising a step of reacting a sulfur compound with a compound of formula (XII) A 1 - Q 1 - Z (XII) and a compound of formula (XIII) A 2 - Q 2 - Z (XIII), in which A 1 , A 2 , Q 1 and Q 2 have the meanings defined above, and Z represents a Cl atom or an SH group.
[0114] The compound of formula (XII) and the compound of formula (XIII) may be different or the same; preferably they are the same. In this case, the process provides for the reaction of a certain amount of sulfur compound with a certain amount of the single compound of formula (XII).
[0115] The sulfur compound may be any sulfur compound known to those skilled in the art capable of reacting with the compounds of formula (XII) and the compounds of formula (XIII). For example, the sulfur compound may be chosen from sulfur, sodium tetrasulfide and sulfur monochloride.
[0116] According to a particular embodiment, the polysulfides of general formula (I), in particular those with x= 4, are prepared by a process comprising a step of reacting sodium tetrasulfide with a compound of formula A 1 - Q 1 - Cl and a compound of formula A 2 - Q 2 - Cl, in which A 1 , A 2 , Q 1 and Q 2 have the meanings defined above.
[0117] A 1 and A 2 are a group of formula (VII), in which the symbol * represents the direct attachment of groups A 1 and A 2 to groups Q 1 and Q 2 respectively.
[0118] Preferably Q 1 and Q 2 are independently a linear or branched C 1 -C 13 divalent hydrocarbon radical, more preferably a linear C 1 -C 6 divalent hydrocarbon radical, preferably a linear C 2 divalent hydrocarbon radical.
[0119] The compound of formula A 1 - Q 1 - Cl and the compound of formula A 2 - Q 2 - Cl may be different or the same. Preferably, they are the same. In this case, the process involves reacting a certain amount of sodium tetrasulfide with a certain amount of the single compound of formula A 1 - Q 1 - Cl.
[0120] Sodium tetrasulfide can be prepared, for example, by reacting sulfur with anhydride sodium sulfide; the latter can be prepared by reacting sodium ethoxide with hydrogen sulfide. Sodium tetrasulfide is preferably prepared in situ by adding sulfur to an ethanolic solution of sodium sulfide. The final nucleophilic substitution is preferably carried out in the solvent used for the preparation of sodium tetrasulfide, i.e., ethanol. The temperature of this step can be between room temperature (23°C) and the reflux temperature of the solvent. Preferably, this step is carried out at the reflux temperature of the solvent. The salt formed can be removed by filtration and the final product can be isolated by evaporation of the solvent.
[0121] This process can be applied in particular to the preparation of the polysulfide of formula (X), according to the following synthetic scheme: Na + EtOH → NaOEt + 1 / 2 H 2 2NaOEt + H 2 S → Na 2 S + EtOH Na 2 S + 3S → Na 2 S 4
[0122] According to another particular embodiment, the polysulfides of general formula (I), in particular those with x= 4, are prepared by a process comprising a step of reacting sulfur monochloride S 2 Cl 2 with a compound of formula A 1 - Q 1 - SH and a compound of formula A 2 - Q 2 - SH, in which A 1 , A 2 , Q 1 and Q 2 have the meanings defined above.
[0123] A 1 and A 2 are a group of formula (VII) in which the symbol * represents the direct attachment of groups A 1 and A 2 to groups Q 1 and Q 2 .
[0124] Preferably Q 1 and Q 2 are independently a linear or branched C 1 -C 13 divalent hydrocarbon radical, more preferably a linear C 1 -C 6 divalent hydrocarbon radical, preferably a linear C 2 divalent hydrocarbon radical.
[0125] Preferably, again the groups Q 1 and Q 2 are identical.
[0126] Preferably, the compound of formula A 1 - Q 1 - SH is obtained by the reaction of a compound of formula A 1 - Q 1 - Cl with sodium hydrogen sulfide NaSH. It can also be obtained by an esterification or amidation reaction from compounds of type A 1 -OH or A 1 -NH 2 with a compound of type HOOC-Q 1 -SH.
[0127] Preferably, the compound of formula A 2 - Q 2 - SH is obtained by the reaction of a compound of formula A 2 - Q 2 - Cl with sodium hydrogen sulfide NaSH. It can also be obtained by an esterification or amidation reaction from compounds of type A 2 -OH or A 2 -NH 2 with a compound of type HOOC-Q 2 -SH.
[0128] The compound of formula A 1 - Q 1 - SH and the compound of formula A 2 - Q 2 - SH may be different or the same, preferably the compound of formula A 1 - Q 1 - SH and the compound of formula A 2 - Q 2 - SH are the same. In this case, the process provides for the reaction of a certain amount of sulfur monochloride with a certain amount of the single compound of formula A 1 - Q 1 - SH.
[0129] This process can be carried out in a solvent medium, preferably tetrahydrofuran, at a temperature between -10°C and 30°C, preferably at approximately 0°C.
[0130] The polysulfide of formula (X) can thus be prepared from an imidazolidinone mercaptan and sulfur monochloride according to the following synthetic scheme:
[0131] According to another particular embodiment, the polysulfides of general formula (I) with x ranging from 2 to 8, preferably from 2 to 6, and more particularly from 2 to 4, are prepared by a process comprising a step of reacting the sulfur with a compound of formula A 1 - Q 1 - SH and a compound of formula A 2 - Q 2 - SH, in which A 1 , A 2 , Q 1 and Q 2 have the meanings defined above.
[0132] A 1 and A 2 are a group of formula (VII) in which the symbol * represents the direct attachment of groups A 1 and A 2 to groups Q 1 and Q 2 .
[0133] Preferably, the groups Q 1 and Q 2 are independently a linear or branched C 1 -C 13 divalent hydrocarbon radical, more preferably a linear C 1 -C 6 divalent hydrocarbon radical, preferably a linear C 2 divalent hydrocarbon radical. Preferably the groups Q 1 and Q 2 are identical.
[0134] Preferably, the compound of formula A 1 - Q 1 - SH is obtained by the reaction of a compound of formula A 1 - Q 1 - Cl with sodium hydrogen sulfide NaSH. It can also be obtained by an esterification or amidation reaction from compounds of type A 1 -OH or A 1 -NH 2 with a compound of type HOOC-Q 1 -SH.
[0135] Preferably, the compound of formula A 2 - Q 2 - SH is obtained by the reaction of a compound of formula A 2 - Q 2 - Cl with sodium hydrogen sulfide NaSH. It can also be obtained by an esterification or amidation reaction from compounds of type A 2 -OH or A 2 -NH 2 with a compound of type HOOC-Q 2 -SH.
[0136] The compound of formula A 1 - Q 1 - SH and the compound of formula A 2 - Q 2 - SH may be different or the same, preferably they are the same.
[0137] In this case, the process involves the reaction of a certain amount of sulfur with a certain amount of the unique compound of formula A 1 - Q 1 - SH.
[0138] Preferably, the reaction is catalytic. The reaction step may be carried out in the presence of a catalyst, which may in particular consist of a combination of a mercaptan with an alkene oxide, preferably ethylene oxide, and an alkali base, preferably sodium hydroxide.
[0139] A reaction solvent may be used in particular if the melting point of the polysulfide of general formula (I) is greater than 100°C.
[0140] The implementation of such a method according to this embodiment generally makes it possible to obtain a mixture of polysulfides of general formula (I) whose average value for x is within a range from 2 to 6, preferably from 3 to 5, more preferably still from 3.5 to 4.5.
[0141] In particular, the polysulfide of formula (VIII) with x ranging from 2 to 8, preferably from 2 to 6, more particularly from 2 to 5, and mainly from 2 to 4, can be prepared from an imidazolidinone mercaptan and sulfur according to the following synthetic scheme:
[0142] Even more preferably, this process generally allows the production of a mixture of polysulfides of formula (VIII) whose average value for x is within a range from 2 to 6, preferably from 3 to 5, even more preferably from 3.5 to 4.5.
[0143] According to another advantageous embodiment of the invention, the mixtures of polysulfides of general formula (I) having an average value for x in a range from 2 to 6, preferably from 3 to 5, more preferably still from 3.5 to 4.5, can be prepared by a process comprising a step of reacting a sodium polysulfide Na 2 S x of average rank x with a compound of formula A 1 - Q 1 - Cl and a compound of formula A 2 - Q 2 - Cl, in which A 1 , A 2 , Q 1 and Q 2 have the meanings defined above.
[0144] The compound of formula A 1 - Q 1 - Cl and the compound of formula A 2 - Q 2 - Cl may be different or identical. Preferably they are identical. In this case, the process provides for the reaction of a certain amount of sodium polysulfide with a certain amount of the single compound of formula A 1 - Q 1 - Cl.
[0145] Sodium polysulfide of average rank x can be prepared by reaction in a solvent between sodium sulfide and sulfur by adapting their respective molar proportions according to the following equation: Na 2 S + (x-1) S → Na 2 S x
[0146] The reaction for preparing sodium polysulfide Na 2 S x of average rank x and its reaction with a compound of formula A 1 - Q 1 - Cl and a compound of formula A 2 - Q 2 - Cl are preferably carried out in one or more solvents. A wide choice of solvents is possible among the solvents known to those skilled in the art to promote nucleophilic substitutions. For example, the following solvents can be used, alone or in mixture: an alcohol such as methanol, ethanol, 1-propanol, 2-propanol, butanol, an aromatic such as toluene, xylene, an ether such as isopropyl ether, methyl t-butyl ether, dioxane and tetrahydrofuran.
[0147] The reaction of sodium polysulfide with a compound of formula A 1 - Q 1 - Cl and a compound of formula A 2 - Q 2 - Cl can be carried out by adding the compounds of formulas A 1 - Q 1 - Cl and A 2 - Q 2 - Cl to a sodium polysulfide solution or by adding a sodium polysulfide solution to a solution of the compounds of formulas A 1 - Q 1 - Cl and A 2 - Q 2 - Cl. Alternatively, the sodium polysulfide solution and the solution of the compounds of formulas A 1 - Q 1 - Cl and A 2 - Q 2 - Cl can be added simultaneously in a semi-continuous or continuous reactor. The temperature of the reaction step can be between room temperature, for example 20°C, and 150°C and preferably between room temperature, for example 20°C, and 100°C. Preferably, this step is carried out at the reflux temperature of the solvent at atmospheric pressure.
[0148] The molar ratio between sodium polysulfide Na 2 S x of average rank x and the compounds of formulas A 1 - Q 1 - Cl and A 2 - Q 2 - Cl is from 0.95 to 1.5, preferably from 1 to 1.2 and more preferably from 1 to 1.1.
[0149] According to a particular embodiment, the reactions are carried out in an anhydrous environment, with anhydrous sodium polysulfide and anhydrous solvents.
[0150] The salt formed during the reaction (NaCl) can be removed by filtration and the final product can be isolated by evaporation of the solvent. According to a particular embodiment, a water washing step can be implemented to remove inorganic residues from the product.
[0151] The implementation of such a method according to this embodiment generally makes it possible to obtain a mixture of polysulfides of general formula (I) whose average value for x is within a range from 2 to 6, preferably from 3 to 5, more preferably still from 3.5 to 4.5.
[0152] Even more preferably, this embodiment generally makes it possible to obtain a mixture of polysulfides of formula (VIII) whose average value for x is within a range from 2 to 6, preferably from 3 to 5, even more preferably from 3.5 to 4.5. Crosslinking system
[0153] The crosslinking system is preferably a vulcanization system, that is to say a system based on sulfur (or a sulfur-donating agent) and a primary vulcanization accelerator. To this basic vulcanization system are added, incorporated during the first non-productive phase and / or during the productive phase as described later, various known secondary accelerators or vulcanization activators such as zinc oxide, stearic acid or equivalent compounds, guanidine derivatives (in particular diphenylguanidine).
[0154] Sulphur is used at a preferential rate within a range of 0.5 to 12 pce, in particular 1 to 10 pce. The primary vulcanisation accelerator is used at a preferential rate of 0.5 to 10 pce, more preferably 0.5 to 5.0 pce.
[0155] Any compound capable of acting as an accelerator (primary or secondary) for the vulcanization of diene elastomers in the presence of sulfur can be used, in particular thiazole-type accelerators and their derivatives, thiuram-type accelerators, zinc dithiocarbamates. Other additives in the composition
[0156] The rubber compositions as described above alone make it possible to respond to the technical problem posed, in particular they make it possible to have an excellent compromise of rigidity / hysteresis properties.
[0157] However, they may further comprise various usual additives usually used in elastomer compositions intended for the manufacture of tires, in particular treads, such as for example plasticizers, such as resins or extender oils, whether the latter are of aromatic or non-aromatic nature, pigments, protective agents such as anti-ozone waxes, chemical anti-ozonants, antioxidants, anti-fatigue agents, reinforcing resins, acceptors (for example phenolic novolak resin) or methylene donors (for example HMT or H3M) as described for example in application WO 02 / 10269
[0158] The rubber compositions as described above may further comprise at least one plasticizing agent chosen from extender oils, plasticizing resins or mixtures thereof.
[0159] In particular, the rubber compositions usable for the tires of the invention may comprise one or more so-called plasticizing resins corresponding, by definition here, to compounds which are solid at room temperature (23°C) (as opposed to a liquid plasticizing compound such as an oil).
[0160] Hydrocarbon resins are polymers well known to those skilled in the art, miscible by nature in diene elastomer compositions when they are also described as “plasticizers”. They have been described for example in the work entitled « Hydrocarbon Resins » by R. Mildenberg, M. Zander and G. Collin (New York, VCH, 1997, ISBN 3-527-28617-9) of which chapter 5 is devoted to their applications, notably in pneumatic rubber (5.5. "Rubber Tires and Mechanical Goods "). They can be aliphatic, aromatic or aliphatic / aromatic, i.e. based on aliphatic and / or aromatic monomers. They can be natural or synthetic, petroleum-based or not (if this is the case, also known as petroleum resins). They are preferably exclusively hydrocarbon-based, i.e. they only contain carbon and hydrogen atoms.
[0161] The softening point is measured according to ISO 4625 (Ring and Ball method). The glass transition temperature Tg is measured in a known manner by DSC ( Differential Scanning Calorimetry ), according to ASTM D3418
[0162] (1999). The macrostructure (Mw, Mn and Ip) of the hydrocarbon resin is determined by size exclusion chromatography (SEC): tetrahydrofuran solvent; temperature 35°C; concentration 1 g / l; flow rate 1 ml / min; solution filtered through a 0.45 µm porosity filter before injection; Moore calibration with polystyrene standards; set of 3 "WATERS" columns in series ("STYRAGEL" HR4E, HR1 and HR0.5); detection by differential refractometer ("WATERS 2410") and its associated operating software ("WATERS EMPOWER").
[0163] It is known to use in rubber compositions for tires hydrocarbon plasticizing resins having at least one of the following characteristics: a Tg greater than 20°C, more preferably greater than 30°C; a number-average molecular mass (Mn) between 400 and 2000 g / mol, a polymolecularity index (Ip) less than 4, preferably less than 3 (reminder: Ip = Mw / Mn with Mw weight-average molecular mass).
[0164] And in particular, whatever the type of plasticizing resins mentioned above, it is known to choose them from the group consisting of cyclopentadiene (abbreviated CPD) or dicyclopentadiene (abbreviated DCPD) homopolymer or copolymer resins, terpene homopolymer or copolymer resins, C5 cut homopolymer or copolymer resins, and mixtures of these resins.
[0165] Preferably, the level of plasticizing resins in the rubber compositions usable in the tires in accordance with the invention is within a range from 10 to 90 pce.
[0166] The rubber compositions may also contain agents for covering the reinforcing inorganic filler, making it possible to improve their processability in the raw state. These coating agents are well known (see for example patent applications WO2006 / 125533-A1, WO2007 / 017060-A1 and WO2007 / 003408-A1), examples of which are hydrolyzable silanes such as hydroxysilanes (see for example WO2009 / 062733-A2), alkylalkoxysilanes, polyols (for example diols or triols), polyethers (for example polyethylene glycols), primary, secondary or tertiary amines, hydroxylated or hydrolyzable polyorganosiloxanes (for example α,ω-dihydroxy-poly-organosilanes (see for example EP0784072-A1)).
[0167] According to another advantageous embodiment, the rubber compositions usable for the tires of the invention may comprise one or more extender oils (or plasticizing oils) liquid at 20°C, known as “low Tg”, that is to say which by definition has a Tg lower than -20°C, preferably lower than -40°C.
[0168] Any extender oil, whether aromatic or non-aromatic, known for its plasticizing properties towards elastomers, can be used. At room temperature (20°C), these oils, more or less viscous, are liquids (that is to say, as a reminder, substances having the capacity to eventually take the shape of their container), in particular unlike high Tg hydrocarbon resins which are by nature solid at room temperature.
[0169] Particularly suitable are plasticizing oils chosen from the group consisting of naphthenic oils (low or high viscosity, in particular hydrogenated or not), paraffinic oils, MES oils (Medium Extracted Solvates), TDAE oils (Treated Distillate Aromatic Extracts), RAE oils (Residual Aromatic Extract oils), TRAE oils (Treated Residual Aromatic Extract) and SRAE oils (Safety Residual Aromatic Extract oils), mineral oils, vegetable oils, ether plasticizers, ester plasticizers, phosphate plasticizers, sulfonate plasticizers and mixtures of these compounds.
[0170] According to a particular embodiment of the invention, the liquid plasticizer is a petroleum oil, preferably non-aromatic. A liquid plasticizer is described as non-aromatic when it has a content of polycyclic aromatic compounds, determined with the extract in DMSO according to the IP 346 method, of less than 3% by weight, relative to the total weight of the plasticizer. For this purpose, a liquid plasticizer chosen from the group consisting of MES oils, TDAE oils, naphthenic oils (low or high viscosity, in particular hydrogenated or not), paraffinic oils and mixtures of these oils may be used. Also suitable as petroleum oil are RAE oils, TRAE oils and SRAE oils or mixtures of these oils, which contain low contents of polycyclic compounds.
[0171] According to another advantageous embodiment, the rubber compositions usable for the tires of the invention may further comprise one or more plasticizing resins as described above in a mixture with one or more extending oils described above. Manufacture of rubber compounds and tires
[0172] The rubber compositions usable in the tires of the invention are manufactured in suitable mixers, using two successive preparation phases well known to those skilled in the art: a first thermomechanical working or mixing phase (so-called "non-productive" phase), which can be carried out in a single thermomechanical step during which all the necessary constituents are introduced into a suitable mixer such as a conventional internal mixer (for example of the "Banbury" type), in particular the non-isoprene diene elastomer as the major elastomer (and possibly the other elastomers), the inorganic filler as the reinforcing filler, the polysulfide of general formula (I) (preferably the polysulfide of formula (VIII)) and any other various additives, with the exception of the crosslinking system. The incorporation of the inorganic filler into the elastomer can be carried out in one or more stages by thermomechanical mixing.The non-productive phase is carried out at high temperature, up to a maximum temperature of between 110°C and 200°C, preferably between 130°C and 185°C, for a duration generally of between 2 and 10 minutes, a second phase of mechanical work (so-called "productive" phase), which is carried out in an external mixer such as a cylinder mixer, after cooling the mixture obtained during the first non-productive phase to a lower temperature, typically below 120°C, for example between 40°C and 100°C. The crosslinking system is then incorporated, and everything is then mixed for a few minutes, for example between 5 and 15 min.
[0173] The final composition thus obtained is then calendered, for example, in the form of a sheet or plate, in particular for characterization in the laboratory, or extruded in the form of a semi-finished (or profiled) rubber usable for the production of tires according to the invention. The profiled part may, for example, be a tread.
[0174] The tire according to the invention is manufactured by any technique well known to those skilled in the art, for example by successively stacking the different profiles on a building drum in order to form a blank, then by shaping the blank so that it takes a toric shape and can be introduced into a mold where it will be cured (or crosslinked). This crosslinking can be carried out in a manner known to those skilled in the art, for example at a temperature between 130°C and 200°C, under pressure, for a sufficient time which can vary for example between 5 and 90 min depending in particular on the curing temperature, the vulcanization system adopted, the vulcanization kinetics of the rubber composition considered or the size of the tire.
[0175] The tire according to the invention is intended to equip all types of motor vehicles, such as for example passenger vehicles, SUVs (“Sport Utility Vehicles”), two-wheelers, airplanes, as well as industrial vehicles such as vans, heavy goods vehicles and other transport or handling vehicles.
[0176] Preferably, the rubber composition as described above is that of a tire layer chosen from the group consisting of all or part of the tread of the tire of the invention.
[0177] The invention relates to tires as previously described, both in the raw state (i.e. before curing) and in the cured state (i.e. after curing). 4 - EXAMPLES
[0178] The following examples illustrate the invention without, however, limiting it. 4.1 - Summary of product A:
[0179] 1-(2-Chloroethyl)-imidazolidin-2-one is prepared according to Example 1b of WO2012 / 007684.
[0180] In a 1 liter glass reactor, equipped with a condenser, and purged with nitrogen, 28.7 g of anhydrous sodium sulfide (0.37 mol) and 723 g of anhydrous ethanol are introduced. While stirring at room temperature, 20.0 g of sulfur (0.62 mol) are added and the mixture is refluxed at atmospheric pressure for 2 hours.
[0181] A mixture of 100.9 g of 1-(2-chloroethyl)-imidazolidin-2-one (0.68 mol) in 206 g of anhydrous ethanol is then added and left at reflux for 4 hours.
[0182] The reaction mixture is cooled to room temperature and then filtered. The precipitate is washed with 50 g of ethanol. The filtrates are combined and evaporated under vacuum. The crude product is taken up in 500 g of dichloromethane and washed in a separating funnel with successively 100 g and then 2 times 50 g of water. The organic phase is evaporated under vacuum. A solid product is recovered. NMR analysis, performed on a Bruker AVIII HD 500 spectrometer equipped with a 5 mm BBI probe, indicates that the solid product contains 95 mol% of polysulfides of formula (VIII) with x in the range 2 to 8 (including 26.5 mol% of compounds of formula (VIII) with x ≥ 4), 3 mol% of 1-(2-chloroethyl)-imidazolidin-2-one, 0.5 mol% of residual solvents and 1.5% of 1,1'-(thiobis(ethane-2,1-diyl))bis(imidazolidin-2-one). 4.2 - Preparation of rubber compositions
[0183] The following tests are carried out as follows: the isoprene diene elastomer (or the mixture of diene elastomers, if applicable), the reinforcing inorganic filler, the coupling agent, and then the various other ingredients, with the exception of the vulcanization system, are introduced into an internal mixer, filled to 70% and with an initial tank temperature of approximately 90°C. Thermomechanical work is then carried out (non-productive phase) in one or two stages (total mixing time of approximately 7 min), until a maximum "fall" temperature of approximately 165°C is reached. The mixture thus obtained is recovered, cooled, and then sulfur and sulfenamide accelerator are added to an external mixer (homo-finisher) at 30°C, mixing everything (productive phase) for 5 to 8 minutes.
[0184] The compositions thus obtained are then calendered in the form of plates (thickness of 2 to 3 mm) or thin sheets of rubber for the measurement of their physical or mechanical properties. 4.3 - Test 1
[0185] The purpose of this example is to demonstrate the improved performance of a rubber composition according to the invention compared to a conventional rubber composition.
[0186] Two rubber compositions are thus prepared in accordance with the process explained in the previous paragraph, based on a synthetic polyisoprene, reinforced mainly with silica. These compositions are distinguished from each other by the nature of the cutting agent used, these compositions comprising the same molar rate of coupling agents: the control composition T1 not in accordance with the invention is a conventional composition which comprises, as a coupling agent for TESPT, the composition C1, in accordance with the invention, is distinguished from the control composition T1 by the nature of the coupling agent which is product A.
[0187] It should be remembered that TESPT is bis(3-triethoxysilylpropyl) tetrasulfide, with the formula marketed for example by the company Evonik under the name “Si69”. The commercial product is a mixture of polysulfides S x with an average value for x which is close to 4). The developed formula of TESPT is:
[0188] Tables I and II give respectively the formulation of these two compositions (rates of the different products expressed in pce), and their properties after cooking for 30 min at 150°C. Tableau I Composition T1 Cl1 Isoprenic elastomer (1) 100,0 100,0 Carbon black (2) 3 3 Reinforcing inorganic filler (3) 60 60 Elastomer coupling agent (4) 6,0 Elastomer coupling agent (5) 3,9 Antioxidant (6) 1,5 1,5 Zinc oxide (7) 2,7 2,7 Stearic acid (8) 2,5 2,5 Accelerator (9) 1,3 1,3 Sulfur 1,6 1,6 (1) Synthetic polyisoprene “Nipol IR 2200” marketed by Nippon Zeon. This polyisoprene has 98 mol% cis-1,4 bond and a Tg = -62°C measured according to the method described in paragraph 2. (2) Carbon black N234 marketed by Cabot Corporation, (3) Silica “Zeosil 1165MP” marketed by Solvay, (4) TESPT (“Si69”) marketed by Evonik, (5) Product A synthesized according to the protocol described in paragraph 4.1, (6) Antioxidant: N-1,3-dimethylbutyl-N-phenyl-para-phenylenediamine marketed by Flexys under the reference “Santoflex 6-PPD” (7) Industrial grade zinc oxide marketed by Umicore, (8) Stearin “Pristerene 4931” marketed by Uniqema, (9) N-cyclohexyl-2-benzothiazyl-sulfenamide: “Santocure CBS” marketed by Flexsys, Table II Temperature T1 C1 G* 0.1% (MPa) (base 100) à 30°C 100 172 à 60°C 100 157 à 100°C 100 166 G* 100% (MPa) (base 100) à 30°C 100 128 à 60°C 100 116 à 100°C 100 117 tan(δ) max (base 100) à 30°C 100 97 à 60°C 100 85 à 100°C 100 80
[0189] In view of Table II, it is surprisingly noted that the composition Cl according to the invention has at 30°C a complex dynamic shear modulus at low deformation (G*0.1%) and at medium deformation (G*100%) significantly improved compared to the control composition T1, as well as an improvement in the hysteretic properties (tan(δ) max).
[0190] Furthermore, when measuring the complex dynamic shear modulus and tan(δ) max at 60°C and 100°C, it is surprisingly observed that both the modulus and the hysteretic properties are significantly improved compared to those of the control composition, whether at low or medium strains.
[0191] In summary, the improvement in the rolling resistance / stiffness property compromise at low and medium deformations is significant and unexpected given the properties observed with a rubber composition based on a predominantly isoprene diene elastomer comprising a sulfurized coupling agent carrying nitrogenous associative groups compared to conventional rubber compositions comprising a TESPT.
Claims
1. Tire comprising at least a rubber composition based on at least an isoprene elastomer as predominant elastomer, an inorganic filler as reinforcing filler, a crosslinking system and at least one polysulphide of general formula (I) as coupling agent of the elastomer to the reinforcing inorganic filler in which : - A1 and A2, each represent an associative group comprising at least one nitrogen atom and correspond to the formula (VII) in which the symbol * represents the direct attachment of the A1 and A2 groups to the Q1 and Q2 groups respectively, - Q1 and Q2, identical or different, each represent a divalent bonding group, - x is a number greater than or equal to 2.
2. Tire according to claim 1, wherein the groups Q1 and Q2, identical or different, each represent a linear or branched divalent hydrocarbon radical in C1-C24, substituted or not, and optionally interrupted by one or more nitrogen or oxygen atoms, preferably represent a divalent hydrocarbon radical in C1-C13, linear or branched, substituted or not, and optionally interrupted by one or more nitrogen or oxygen atoms.
3. Tire according to any one of the preceding claims, wherein x is a number within a range extending from 2 to 8, preferably from 2 to 6, more preferably from 2 to 4.
4. Tire according to any one of the preceding claims, wherein the coupling agent of the elastomer to the reinforcing inorganic filler is a mixture of polysulfides of general formula (I) with A1, A2, x, Q1 and Q2 as defined in claims 1 to 3.
5. Tire according to claim 4, wherein the mixture of polysulfides of general formula (I) comprises at least 20 mole% of polysulfides of general formula (I) with x ≥ 4, preferably comprises at least 20 mole% of polysulfides of general formula (I) with x included in a range from 4 to 8, more preferably from 4 to 6.
6. Tire according to any one of claims 1 to 5, wherein the polysulphide of general formula (I) corresponds to formula (VIII) or to formula (IX) in which x is a number within a range extending from 2 to 8, preferably from 2 to 6, even more preferably from 2 to 4, even more preferably x=4.
7. Tire according to claim 6, wherein the coupling agent of the elastomer to the reinforcing inorganic filler is a mixture of polysulphides of formula (VIII) with x as defined in claim 6.
8. Tire according to claim 7, wherein the mixture of polysulfides of general formula (VIII) comprises at least 20 mole% of polysulfides of general formula (I) with x ≥ 4, preferably comprises at least 20 mole% of polysulfides of general formula (VIII) with x included in a range from 4 to 8, more preferably from 4 to 6.
9. Tire according to any one of the preceding claims, wherein the isoprene elastomer is chosen from the group consisting of natural rubber, synthetic polyisoprenes, the copolymers of isoprene, and mixtures thereof.
10. Tire according to claim 9, wherein the isoprene elastomer is a synthetic polyisoprene.
11. Tire according to any one of the preceding claims, wherein the content of the reinforcing inorganic filler in the rubber composition is within a range extending from 10 to 200 phr, preferably from 30 to 150 phr.
12. Tire according to any one of the preceding claims, wherein the reinforcing inorganic filler comprises silica.
13. Tire according to any one of the preceding claims, wherein the content of the coupling agent in the rubber composition is within a range extending from 1 to 20 phr.
14. Tire according to any one of the preceding claims, wherein the rubber composition further comprises carbon black.
15. Tire according to any one of the preceding claims, wherein the rubber composition further comprises at least one plasticizing agent chosen among extension oils, plasticizing resins and mixtures thereof.