Use of multi-block copolymers as a sacrificial material in a 3D printing process
Multi-block copolymers with tailored monomer compositions address the challenges of humidity and Tg matching in 3D printing, enabling stable support materials for high Tg polymers like PEEK, PEKK, PEI, and PPS, enhancing printing capabilities and stability.
Patent Information
- Application Number
- FR2021006675
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-06-23
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2041-06-23
AI Technical Summary
Existing 3D printing technologies face challenges in using support materials that are difficult to preserve in humid environments and require precise Tg matching with the printed polymer, limiting the choice of high Tg polymers like PEEK, PEKK, PEI, PAI, and PPS, and suffer from issues like filament massing and sticking due to ambient humidity.
Utilization of multi-block copolymers with specific monomer compositions and structures, allowing for adjustable solubility and mechanical properties, independent of the printed polymer's Tg, and improved stability in humid conditions.
Enables the printing of high Tg polymers like PEEK, PEKK, PEI, and PPS with improved storage stability and ease of solvent dissolution, overcoming humidity-related issues and expanding the range of printable materials.
Abstract
Description
Title of the invention: Use of multi-block copolymers as sacrificial material in a 3D printing process FIELD OF THE INVENTION
[0001] The present invention relates to the use of multi-block copolymers as sacrificial materials for 3D modeling by fused filament deposition. Only block copolymers are used in this invention. This excludes any other architectural polymer not in the form of block copolymers.
[0002] Such materials exhibit rapid solubilization or dispersibility in a variety of solvents while combining the ideal thermomechanical properties to make them into wires or rods usable in 3D printing (molten filament deposition modeling) to support polymers constituting the part to be manufactured, including polymers with a high glass transition temperature (Tg), before being removed by dissolution in a solvent.
[0003] Three-dimensional printing (or 3D printing) allows the additive manufacturing (AM) of a real object from a virtual object. It is based on cutting the 3D virtual object into very thin 2D strips. These thin strips are deposited one by one by fixing them on the previous ones, which reconstitutes the real object. Among the materials constituting the object, we find plastic materials (notably acrylonitrile butadiene styrene (or ABS) and polylactic acid (or PLA)), but also Polyaryletherectones (PAEK), Pole-theryimides (PEI), wax, metal or ceramics. Examples of additive techniques are fused filament fabrication (FFF) and laser sintering.
[0004] Fused filament deposition modeling is a technique that consists of melting a filament through an extrusion nozzle. From this nozzle comes out a molten filament, with a diameter of the order of a millimeter. This wire is deposited in line and is bonded by re-melting to what was previously deposited. This technique makes it possible to create parts in good material, with mechanical and thermal characteristics and stability identical to injected thermoplastic parts and often lighter. In the case of polymers, for reasons of mechanical consolidation, this technique requires a support for the production of the parts, also extruded jointly. This construction support is made of a material other than that constituting the created object, a support which is eliminated from said object, when the construction process of the latter is finished.
[0005] The construction support is generally a soluble polymeric composition or dispersible meeting a very precise specification. Among the properties sought, in addition to mechanical resistance, the glass transition temperature of the copolymer which must be close to the material to be printed, its thermal stability or its ease of implementation, the kinetics of solubilization or dispersion in a variety of solvents and in particular water is of prime importance. The material must also have good conservation, when the solubilization or dispersion solvent is water. This last characteristic is not always easy to establish because water-soluble or water-dispersible compositions and filaments in water can be difficult to store in a humid atmosphere. We observe caking of the granules or sticking of the filaments on the reels due to the presence of ambient humidity during storage. TECHNICAL BACKGROUND
[0006] This 3D printing technique requires support materials that allow the construction of complex parts, this is for example described in WO2010 / 045147. Other water-soluble support materials include:
[0007] - Polyvinyl alcohol - BVOH butenediol / vinyl alcohol copolymer. - (Meth)acrylic copolymers.
[0008] These carrier polymer compositions always comprise several copolymers, the role of which is to adjust solubility, mechanical properties or other parameters, resulting in more difficulties in development.
[0009] Among other support materials soluble in other solvents, we can cite for example impact polystyrene (HIPS), soluble in limonene.
[0010] It is known in the prior art that the support must have a glass transition temperature (Tg) relatively close to that of the polymer constituting the object to be printed within an order of magnitude 10°C lower than the Tg of the polymer constituting the object to be printed.
[0011] Otherwise, the construction of the part to be printed is not done correctly because the support material has too much fining. This is explained for example in US5866058.
[0012] Surprisingly, the applicant has found that when block copolymers are used alone or in combination as sacrificial support material, this condition of proximity of the Tg materials to be printed-support material is no longer necessary. This presents an advantage because the definition of the other characteristics of the support polymer presents many more possibilities. It is thus easier to adjust the other parameters such as mechanical or solubilization in aqueous medium without worrying about the Tg of the sacrificial support polymer, provided that they remain lower than that of the polymer constituting the object to be printed. Thus, with block copolymers whose highest Tg of one of the blocks is, for example, 50°C, such block copolymers can be used as a support material to construct objects made of material with a Tg ranging from 50°C to 200°C.
[0013] This offers new possibilities for printing objects made of poly aryl ether ketones (PAEK), polyether imides (PEI), polamide-imide (PAI), Polysulfone (PSU), poly(ethersulfone) (PES), poly(phenylene sulfide) (PPS) for which the choice of sacrificial support polymers is very limited and has other disadvantages. Summary of the invention
[0014] The invention relates to the use of at least one multi-block copolymer as a sacrificial material in a 3D printing process for polymers whose Tg is between 50 and 200°C, at least one multi-block copolymer(s) comprising at least one block consisting of i monomers M; linked together in a statistical manner, i being an integer ranging from 2 to 5, inclusive, and at least one block consisting of j monomers Mj linked together in a statistical manner, j being an integer ranging from 2 to 5, inclusive, Mj being selected from monomers A whose Tg of their homopolymers is less than 0°C and hydrophilic monomers B, the mass proportion of A varying from 80 to 95% and the mass proportion of B varying from 5 to 20%.
[0015] Mj being selected from monomers C whose Tg of their homopolymers is less than 0°C, monomers D whose Tg of their homopolymers is greater than 25°C and hydrophilic monomers E, the mass proportions of monomers C, D, E being respectively between 25-35%, 25-35%, 35-45%. Detailed description
[0016] There is every reason to believe that any type of monomers having the characteristics and the associated proportions in block copolymers as described in the summary of the invention lead to behavior favorable to the resolution of the technical problems as described in the technological background.
[0017] This does not prejudge the chemistry used.
[0018] Few chemistries allow the preparation of such block copolymer structures.
[0019] For example, reactive blocks can be prepared by polycondensation or ring opening so that other blocks can be linked in a second step, with choices and proportions of monomers according to the summary of the invention.
[0020] The blocks can also be prepared by radical or anionic polymerization in the same way, i.e. block by block, so that other blocks can be linked in stages with choices and proportions of monomers according to the summary of the invention.
[0021] Among the preferred techniques, controlled radical polymerizations will be used because they make it possible to obtain block copolymers in sequential steps within the same process operation.
[0022] We can cite RAFT (Radical Addition Fragmentation Transfer in English) or NMP (Nitroxide Mediated Polymerization, polymerization controlled by ni-troxides) in a non-limiting manner.
[0023] Preferably, NMP will be chosen, and preferably that using the counter radical N-tert-Butyl-1-diethylphosphono-2,2-dimethylpropyl Nitroxide. Such a counter radical is widely described and used in the literature and implemented through the alkoxyamine or polyalkoxyamines of 2-([tert-butyl[1-(diethoxyphosphoryl)-2,2-dimethylpropyl]amino]oxy)-2 methylpro-pionic acid.
[0024] With regard to the monomers as described in the summary of the invention, the monomers A will be chosen from the following:
[0025] Oxygenated or non-oxygenated alkyl (meth)acrylates with a C4-C18 chain, linear or substituted and in particular the following monomers: Butyl acrylate (Abu), 2-ethylhexyl acrylate (AE2H), methoxyethyl acrylate (AME), Lauryl methacrylate (MAlau), stearyl methacrylate (MAS).
[0026] The monomers B will be chosen from the following: acrylic acid (AA), methacrylate acid (AMA).
[0027] The monomers C will be chosen from the following:
[0028] Oxygenated or non-oxygenated alkyl (meth)acrylates with a C4-C18 chain, linear or substituted and in particular the following monomers: Butyl acrylate (Abu), 2-ethylhexyl acrylate (AE2H), methoxyethyl acrylate (AME), LAuryl methacrylate (MAlau), stearyl methacrylate (MAS).
[0029] The monomers D will be chosen from the following:
[0030] Styrene (S); Methyl methacrylate (MMA), Acrylonitrile (AN)
[0031] The monomers E will be chosen from the following: acrylic acid (AA), methacrylate acid (AMA).
[0032] Preferably, A is butyl or 2-ethylhexyl acrylate, and more preferably butyl acrylate, B is acrylic acid or methacrylic acid, C is butyl or 2-ethylhexyl acrylate, and more preferably butyl acrylate, D is styrene, acrylonitrile or methyl methacrylate, and more preferably styrene, E is acrylic acid or methacrylic acid.
[0033] The polymers which can be printed using the sacrificial polymers of the invention have glass transition temperatures (Tg) greater than 50°C, among which we can cite, without limitation, polylactic acid (PLA), acrylonitrile butadiene styrene (ABS, acrylonitrile styrene acrylonitrile (ASA), polyamides (PA), polycarbonate (PC), polymethyl methacrylate (PMMA), copolyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyolefins (PE, PP), and for high Tg polymers between 140 and 200°C poly aryl ether ketones (PAEK), called PEEK, PEKK, PEK, PEKEKK, PEEKK, PEKK depending on the aryl-ether ketone chains, polyether imides (PEI), polamide-imide (PAI), Polysulfone (PSU), poly(ethersulfone) (PES), or poly(phenylene sulfide) (PPS).
[0034] The use of block copolymers as water-soluble support materials for high-temperature polymers such as PEEK, PEKK, PEI, PAI PSU, and PPS is particularly useful. The other lower Tg polymers mentioned can also be printed, but other solutions already exist.
[0035] Thus, the preferences of the invention are for the use of block copolymers as described in the summary of the invention for printing polymers whose Tg is between 50 and 200°C, and preferably whose Tg is between 140 and 200°C.
[0036] The block copolymers as described in the summary of the invention are preferably di or tri block copolymers, and more preferably di block copolymers. In the definition of these copolymers, i can take values between 2 and 5, preferably between 2 and 3, inclusive, and more preferably 2. In the definition of these copolymers, j can take values between 2 and 5, preferably between 2 and 3, inclusive, and preferably 3.
[0037] They have a mass proportion of the blocks consisting of monomers of family A and B varying from 5 to 40% (block 1), preferably between 10 and 30% and a mass proportion of the blocks consisting of monomers C, D, and E varying from 50 to 90% (block 2), preferably between 60 and 80%.
[0038] The balance of properties associated with the choices of monomers selected in the invention allows these copolymers to be soluble in solvents chosen from water, DMSO, alcohols, or even ketones in a non-limiting manner. Water is the preferred solvent in a pH range which can vary from 7 to 12 and preferably from 10 to 12.
[0039] When the dissolution or dispersion solvent is water, they exhibit very good solubilization at high pHs, 12 for example, and much less good solubilization at pH 7. This provides an advantage because the coils of wires manufactured with these copolymers exhibit better storage stability, particularly in a humid atmosphere.
[0040] The copolymers as described in the summary of the invention have a molecular mass by weight of between 80,000 and 150,000 g / mol and a dispersity index of between 1 and 3, and preferably between 1.5 and 2.5) measured by SEC using polystyrene standards.
[0041] They can be blended with other block copolymers to adjust certain properties.
[0042] Glass transition temperatures (Tg) are measured by DSC. Examples
[0043] Example 1 - Synthesis of a copolymer PfBA - AA) - b - PfBA - S - AMA)
[0044] In this example we are aiming at a di-block copolymer iMi-jMj, with i= 2 and j=3 represented mMnN-block-oOpPqQ.
[0045] Block 1:
[0046] M: Butyl acrylate (Abu), m= 9% of block 1
[0047] N: Acrylic acid (AA), n= 10% of block 1.
[0048] Block 2:
[0049] O: Abu, o=30% of block 2.
[0050] P: Styrene (S), p = 30% of block 2
[0051] Q: Methacrylic acid (AMA), q= 40% of block 2.
[0052] The synthesis of this di-block copolymer takes place in two stages:
[0053] 1st block P(BA - AA) in mass then stripping of the unreacted monomers.
[0054] 2nd block P(BA - S - AMA) in solvent 1.1. Synthesis of the P(BA - AA) block
[0055] The synthesis of this first block is carried out by a mass polymerization process using an Engineer Büro type reactor.
[0056] Reagents:
[0057] - butyl acrylate (BA) 208.7 g - acrylic acid (AA) 22.9 g - BlocBuilder® 2.51 g
[0058] A number-average molecular mass of 27,000 g / mol at 70% conversion is targeted.
[0059] The reagents are weighed and then mixed under magnetic stirring, they are introduced then into the reactor by vacuum. The reactor is stirred (250 rpm). The medium is degassed by alternating three nitrogen pressures and vacuum. The polymerization is carried out in three temperature stages: 105°C for 60 min then 110°C for 90 min. The polymerization time is 300 min. The conversion is monitored by dry extracts, samples are taken every hour (thermobalance 150°C and vacuum oven 125°C).
[0060] When the target conversion is reached, the temperature is lowered to 80°C. Once the set point is reached, the equipment will gradually be placed under vacuum, the unreacted monomers will be distilled (recovery in liquid nitrogen traps). We remain at 80°C and under maximum vacuum for approximately 90 minutes, when the distillation is finished, lower the set point to 40°C, once this set point is reached, 160g of toluene is introduced (by depression) in order to dilute the medium. Leave for a few hours under stirring and at 40°C in order to homogenize the solution well. This solution is then recovered. 1.2. Synthesis of the P(BA - S - AMA) block
[0061] We work in a solvent process, using an ethanol / toluene mixture having a mass ratio of 60 / 40. We work with 45% of solvent relative to the total charge.
[0062] A BA / S / AMA mixture with a mass ratio of 30 / 30 / 40 is introduced.
[0063] We are aiming at a P(BA - AA) - b - P(BA - S- AMA) copolymer of mass composition 30 / 70 with a 2nd block conversion of 70%.
[0064] The charge is prepared as indicated below:
[0065] 1st block diluted in ethanol: 154.8 g
[0066] BA / S / AMA: 154.8 / 154.8 / 206.4 (g)
[0067] Ethanol / Toluene: 329 / 219.5 (g)
[0068] The molar masses (PS equivalent) of this copolymer are as follows:
[0069] Mp=95000 g / mom
[0070] Mn=53000 g / mol
[0071] Mw=95000 g / mom
[0072] Ip=1.81
[0073] In Examples 2 to 4 (inventions 2 to 4) di-block copolymers iMi-jMj are prepared, with i= 2 and j=3 represented mMnN-block-oOpPqQ with the same block ratio and the same proportions of monomers under the same synthesis conditions as for Example 1. In Table 1 the following monomers are selected:
[0074] [Tables 1] b A >5 w .1 Abu ,.s, i pÿ ; j.ïïV'&At AA A ÀMà "A <<• ] ïnwst AA A £2 £ % AMA ..."""K........ J., b XW 4 s®. AU AM AMA .2. AA
[0075] The proportions m, n, o, p, q remaining identical to those of example 1. The polymers obtained have similar molecular mass characteristics not varying more than 10% in comparison with those obtained in example 1.
[0076] Example 5: dissolution tests.
[0077] The tests are carried out until a pellet of support material of the invention and of the Aquasis® 120 and 180 products available on the market is completely dissolved.
[0078] The pellets are prepared by compression at 200°C. The dissolution of the pellets is carried out at pH=7 and pH=12 at a temperature of 60°C.
[0079] Example 6: Extrusion of filaments:
[0080] Coils have been formed directly from the materials of the inventions.
[0081] Spinning is carried out on a Labtech LBE20-30 / C single-screw extruder (screw diameter: 20mm). A caterpillar puller is used to drive the rod at a constant speed (9.1-9.4m / min).
[0082] The extruder and gear pump are set at 190°C.
[0083] The screw speed of the extruder is 30-34 rpm, with a pressure P=55 bar.
[0084] The commercial control products Aquasis® 120 and Aquasis® 180 are available in the form of spools of wire that can be used directly in a 3D printing device.
[0085] Example 7: 3D Printing
[0086] The parts were printed on an “Original Prusa i3 MK3S+” 3D printer. Other available printers can be used. The sacrificial resin in the form of filament according to the invention or the Aquasis® 180 control are printed at a temperature of 250°C on a plate at 122°C for the first layer then 120°C for the following layers at a speed of 40mm / s. The layer heights are 0.2mm and the filling is 100% concentric.
[0087] The sacrificial resin in the form of filament according to the invention or the Aquasis® 120 control are printed at a temperature of 220°C on a plate at 120°C for the first layer then 105°C for the following layers at a speed of 10 mm / s. The layer heights are 0.2 mm and the filling is 100% concentric.
[0088] The resins of the polymers of the parts to be built are printed under the following conditions:
[0089] ABS, 3DFilTech: 250°C; lOmm / s.
[0090] PLA, eMotion TECH: 210°C; lOmm / s.
[0091] PEI: ThermaX PEI - Ultem 9085: 360°C; lOmm / s.
[0092] PEKK, ThermaX PEKK 3DXTech: 360°C; lOmm / s.
[0093] The constructed parts are 4cm X 1cm X 0.5cm bars of a sacrificial polymer bar (invention and control) on which a bar of identical dimension is constructed using the target polymer (PLA, ABS, PEKK, PEI, etc.).
[0094] Example 8:
[0095] Once the parts have been constructed, when possible using the control sacrificial resins or those of the invention with a given polymer to be printed, the assembly is immersed in water at 60°C at a pH of 7 or 12, then the time taken for all of the sacrificial material to dissolve is noted. When the test is deemed impossible, this means that the part to be constructed does not conform to the desired 3D digital model.
[0096] The results of dissolution and 3D printing tests are given in Table 2:
[0097] [Tables2] polymers to be printed Table 2 Tl T2 PLA ABS PEKK PEI Invention 1 > 120 70 possible possible possible possible Invention 2 > 120 80 possible possible possible possible Invention 3 > 120 80 possible possible possible possible Invention 4 > 120 85 possible possible possible possible Aquasis® 120 40 75 possible possible impossible impossible Aquasis® 180 60 120 impossible impossible possible possible
[0098] Tl: Time in minutes, total dissolution at 60°C, water pH 7
[0099] T2: Time in minutes, total dissolution at 60°C, water pH 12
[0100] It can be seen that whatever the polymer to be printed in Table 2, the sacrificial resins of the invention make it possible to support the polymer to be printed.
Claims
Claims
1. Use of at least one multi-block copolymer as a sacrificial material in a 3D printing process for polymers whose Tg is between 140 and 200°C, chosen from PEEK, PEKK, PEK, PEKEKK, PEEKK, PEKK, PEI, PAI, PSU, and PPS, at least one multi-block copolymer(s) comprising at least one block consisting of i monomers Mi linked together in a statistical manner, i being an integer ranging from 2 to 5, inclusive, and at least one block consisting of j monomers Mj linked together in a statistical manner, j being an integer ranging from 2 to 5, inclusive, M; being selected from monomers A whose Tg of their homopolymers is less than 0°C and hydrophilic monomers B, the mass proportion of A varying from 80 to 95% and the mass proportion of B varying from 5 to 20%.Mj being selected from C monomers whose Tg of their homopolymers is less than 0°C, D monomers whose Tg of their homopolymers is greater than 25°C and hydrophilic E monomers, the mass proportions of the C, D, E monomers being respectively between 25-35%, 25-35%, 35-45%.
2. Use according to claim 1 wherein the at least one block copolymer is a di-block copolymer or a tri-block copolymer.
3. Use according to claim 2 wherein the block copolymer is a di-block copolymer.
4. Use according to claim 3 in which the di-block copolymer has a mass proportion of the blocks consisting of monomers from family A and B varying from 5 to 40% (block 1) and a mass proportion of the blocks consisting of monomers C, D, and E varying from 50 to 90% (block 2).
5. Use according to claim 1 in which the block copolymer(s) are prepared by controlled radical polymerization.
6. Use according to claim 5 in which the block copolymers are prepared by radical polymerization controlled by nitroxides.
7. Use according to claim 6 in which the block copolymers are prepared by radical polymerization controlled by N-tert-Butyl-l-diethylphosphono-2,2-dimethylpropyl Nitroxide.
8. Use according to claim 6 in which at least one block copolymer consists of blocks 1 using acrylate of butyl and acrylic acid and 2-blocks using butyl acrylate, styrene and methacrylic acid.
9. Use according to claim 1 in which at least one block copolymer has a molecular mass by weight of between 80,000 g / mol and 150,000 g / mol.