AIRCRAFT TURBOMACHINE TURBINE TURBINE AND ASSOCIATED MANUFACTURING METHOD

A hybrid bonding layer with an adhesion underlayer and grip sub-layer enables thermal spraying of protective shields onto composite blades, simplifying assembly and improving adhesion and mechanical properties, addressing the complexity and repeatability issues in existing manufacturing processes.

FR3141965B1Active Publication Date: 2024-11-01SAFRAN SA +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022011789
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-11-14
Publication Date
2024-11-01
Estimated Expiration
2042-11-14

AI Technical Summary

Technical Problem

The manufacturing process of composite material blades for aircraft turbomachines, particularly the attachment of protective shields, is complex, tedious, and difficult to repeat with low tolerances, requiring manual precision to avoid defects.

Method used

A hybrid bonding layer comprising an adhesion underlayer and a grip sub-layer with embedded particles is used, allowing the protective shield to be thermally sprayed onto the blade, eliminating the need for separate shield manufacturing and pairing steps.

Benefits of technology

This method simplifies the assembly process, reduces defects, and ensures high adhesion and mechanical anchoring, achieving equivalent mechanical properties and adhesion to traditional gluing methods while enabling complex geometry coatings with improved repeatability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000017_0000
    Figure 00000017_0000
  • Figure 00000017_0001
    Figure 00000017_0001
  • Figure 00000018_0000
    Figure 00000018_0000
Patent Text Reader

Abstract

The invention relates to a blade (11) for an aircraft turbomachine (1), the blade (11) comprising: - a blade (12) comprising an extrados face (12e) and an intrados face (12i) connected by a leading edge (12a) and a trailing edge (12b), the blade (12) comprising a composite material, - a protective shield (14) arranged on the blade (12), and - a bonding layer (16) arranged between the blade (12) and the protective shield (14) and comprising an adhesion sub-layer (17) of polymeric material, characterized in that the bonding layer (16) further comprises a tack sub-layer (18) comprising particles (18a) embedded in the adhesion sub-layer (17), the tack sub-layer (18) being arranged between the adhesion sub-layer (17) and the protective shield (14). Abbreviated figure: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: BLADE FOR AN AIRCRAFT TURBOMACHINE AND ASSOCIATED MANUFACTURING METHOD Technical field of the invention

[0001] The invention relates to the field of blades for aircraft turbomachines. The invention relates more particularly to the field of blades comprising a blade made of composite material and a blade protection shield as well as the method of manufacturing these blades. Technical background

[0002] An aircraft turbomachine typically comprises an engine comprising, from upstream to downstream in the direction of gas flow, a fan rotatable about a longitudinal axis, a low-pressure compressor and a high-pressure compressor, a combustion chamber, a high-pressure turbine and a low-pressure turbine and a gas exhaust nozzle.

[0003] The blower allows the suction of an air flow dividing into a primary flow and a secondary flow. The primary flow passes through a primary vein of the turbomachine while the secondary flow is directed towards a secondary vein surrounding the primary vein.

[0004] The primary flow is compressed within the compressors. The compressed air is then mixed with a fuel and burned within the combustion chamber. The gases resulting from the combustion pass through the turbines and then escape through the nozzle, the cross-section of which allows the acceleration of these gases to generate propulsion.

[0005] Turbomachine components such as the fan, compressors or turbines comprise blades that act on the air flow. For example, compressor blades act to compress the primary air flow and fan blades act to compress the secondary air flow.

[0006] A blade comprises a blade which has an aerodynamic shape and thus comprises a pressure face and an extrados face connected to the pressure face by a leading edge and a trailing edge. To reduce the weight of the blade, the blade is made of a composite material. The composite material of the blade comprises reinforcing fibers embedded in a polymer matrix. In order to protect the blade, in particular a fan blade, from degradation caused by the impact of foreign bodies and from erosion, it is known to arrange a protective shield on the blade. The protective shield is generally metallic. It has a dihedral shape comprising a first lateral fin and a second lateral fin connected by a core. The core covers for example the leading edge of the blade and the first lateral fin extends over the pressure face and the second lateral fin extends over the extrados face. The protective shield protection is typically bonded to the blade. For this purpose, the blade further comprises a bonding layer arranged between the blade and the protective shield. The bonding layer typically comprises a polymeric material such as an epoxy resin.

[0007] A method of manufacturing the aforementioned blade typically comprises steps of manufacturing the blade and manufacturing the protective shield. The protective shield is for example manufactured by forging or bending a sheet metal.

[0008] The method then comprises a step of pairing and bonding the protective shield to the blade.

[0009] Such a manufacturing method is not entirely satisfactory. Indeed, the step of manufacturing the protective shield presents challenges because the configuration of the protective shield is complex. This step is therefore tedious. Furthermore, the manufacturing tolerances are small and it is difficult to ensure the repeatability of this step.

[0010] Furthermore, the step of pairing the protective shield which consists of attaching the protective shield to the blade is carried out manually so that, guaranteeing the precision of the assembly of the blade and the repeatability of this step, require perfect mastery of the manufacturing process to limit defects on the protective shield or the blade and therefore the scrap of these parts.

[0011] Therefore, there is a need to provide a blade comprising a composite material blade which is resistant to shock and erosion while being simple to manufacture. Summary of the invention

[0012] To this end, the invention proposes a blade for an aircraft turbomachine, the blade comprising:

[0013] - a blade comprising an extrados face and an intrados face connected by an edge leading edge and a trailing edge, the blade comprising a composite material,

[0014] - a protective shield arranged on the blade, and

[0015] - a bonding layer arranged between the blade and the protective shield and comprising an adhesion underlayer made of polymeric material.

[0016] The blade is remarkable in that the bonding layer further comprises a bonding sub-layer comprising particles embedded in the adhesion sub-layer, the bonding sub-layer being arranged between the adhesion sub-layer and the protective shield.

[0017] The blade according to the invention therefore comprises a hybrid bonding layer composed of a first layer called the adhesion sub-layer made of polymeric material and a second layer called the adhesion sub-layer comprising particles embedded in the adhesion sub-layer. The hybrid bonding layer makes it possible to protect the blade when forming the protective shield on the blade.

[0018] The adhesion undercoat ensures high adhesion between the substrate, i.e. the blade, and the adhesion undercoat.

[0019] The bonding underlay creates a surface favorable to the mechanical anchoring of the protective shield on the blade.

[0020] Therefore, the protective shield can be deposited on the blade for example by a thermal spraying process. Without such a hybrid bonding layer, such a process could not be implemented satisfactorily since the adhesion of the protective shield would be too weak and the blade would be severely degraded.

[0021] The thermal spraying method is particularly advantageous in that it allows complex geometry coatings to be formed in a precise and repeatable manner, thereby reducing the risks of defects in the protective shield and its scrapping. In addition, thanks to the thermal spraying method, it is possible to dispense with a step of manufacturing the protective shield in favor of a step of forming the protective shield directly on the blade. This also makes it possible to dispense with a step of pairing the shield on the blade, thus simplifying the step of assembling the protective shield and the blade, and reducing blade assembly defects.

[0022] The thermal spraying process also allows the implementation of a variability of materials for the protective shield which is not offered by other shield manufacturing processes.

[0023] Thanks to the combination of the bonding underlayer and the adhesion underlayer, it has also been found that the mechanical properties of the blade are improved or at least equivalent to those of a blade whose protective shield is added and then bonded by a layer of adhesive to the blade, that the adhesion of the protective shield is improved or at least equivalent to that of a protective shield added and then bonded by a layer of adhesive to the blade.

[0024] Thanks to the combination of the adhesion sub-layer and the adhesion sub-layer, it has also been found that the mechanical properties of the blade and the adhesion of the shield are improved or at least equivalent to those of a blade without an adhesion sub-layer and whose shield would be formed by thermal spraying.

[0025] The invention may comprise one or more of the following features, taken in isolation from one another or in combination with one another:

[0026] - the particles are particles of metal, ceramic, oxide or a mixture of these;

[0027] - the particles have a size less than or equal to 500 pm, advantageously less than or equal to 400 pm, preferably less than or equal to 300 pm;

[0028] - the adhesion sub-layer has a thickness of between 10 pm and 500 pm, advantageously between 50 pm and 500 pm or between 80 pm and 400 pm;

[0029] - the polymeric material of the adhesion sub-layer is chosen from among thermosetting polymers such as epoxy or thermoplastic polymers or a mixture thereof;

[0030] - the mass rate of particles in the bonding layer is between 20% and 90%, preferably between 50% and 90%;

[0031] - the adhesion sub-layer comprises a first polymeric layer and a second polymeric layer, the particles being embedded in the second layer which is arranged between the first layer and the bonding sub-layer;

[0032] - the first layer comprises a first polymeric material and the second layer comprises a second polymeric material different from the first polymeric material;

[0033] - the first layer has a first thickness and the second layer has a second thickness less than the first thickness.

[0034] The invention also relates to a method of manufacturing a blade for an aircraft turbomachine, the method comprising the following steps:

[0035] (a) providing a blade comprising an extrados face and an intrados face connected by a leading edge and a trailing edge, the blade comprising a composite material,

[0036] (b) arranging a bonding layer on the blade, the bonding layer comprising a polymeric material adhesion undercoat,

[0037] (c) forming a protective shield on the blade.

[0038] The method is remarkable in that in step (b) the bonding layer further comprises a bonding sub-layer comprising particles embedded in the adhesion sub-layer, the bonding sub-layer being arranged between the adhesion sub-layer and the protective shield.

[0039] The invention may comprise one or more of the following features, taken in isolation from one another or in combination with one another:

[0040] - step (b) comprises the following sub-steps:

[0041] (bO) deposit the adhesion undercoat on the blade,

[0042] (b2) depositing the bonding undercoat on the adhesion undercoat,

[0043] (b3) heat treating the bonding layer;

[0044] - step (b) further comprises between steps (b0) and (b2) the following sub-step:

[0045] (bl) heat pretreating the adhesion sub-layer;

[0046] - step (b) comprises the following sub-steps:

[0047] (bi) depositing a first polymeric layer on the blade,

[0048] (bii) depositing a second polymeric layer and the particles on the first sub-layer;

[0049] - step (b) comprises, after sub-step (bii), the following sub-step:

[0050] (biii) heat treating the first layer;

[0051] - sub-step (bi) is carried out by thermal projection;

[0052] - sub-step (bii) is carried out by thermal projection of the particles previously impregnated with a polymer matrix forming the second layer;

[0053] - step (c) is carried out by thermal projection;

[0054] - thermal projection is carried out with a powder comprising grains of which at at least 90% of these grains have a size (d90) between 5 pm and 200 pm, advantageously between 10 pm and 150 pm;

[0055] - at most 10% of the grains have a size (dlO) between 0.05 pm and 50 pm, advantageously between 0.1 pm and 20 pm;

[0056] - the material of the powder is identical to that of the particles of the undercoat of hook;

[0057] - the method comprises, after step (c), a step (d) of machining the shield of protection. Brief description of the figures

[0058] Other characteristics and advantages will emerge from the following description of a non-limiting embodiment of the invention with reference to the appended drawings in which:

[0059] [Fig.l] is a schematic view in longitudinal section of a half aircraft turbomachine,

[0060] [Fig.2] is a schematic perspective view of a blade equipping the turbomachine of [Fig.l],

[0061] [Fig.3] is a cross-sectional view of the blade of [Fig.2],

[0062] [Fig.4] is a schematic sectional view of the bonding layer arranged on the blade and coated with the protective shield, according to the invention,

[0063] [Fig.4a] is a schematic sectional view of the bonding layer arranged on the blade and coated with the protective shield, according to one embodiment of the invention,

[0064] [Fig.5] is a schematic view of a manufacturing method according to the invention,

[0065] [Fig.6] is a schematic view of the manufacturing process according to a first mode of realization,

[0066] [Fig.7] is a schematic view of the manufacturing method according to a second embodiment. Detailed description of the invention

[0067] An example of an aircraft turbomachine 1 according to the invention is shown in [Fig.l]. The turbomachine 1 extends around and along a longitudinal axis A.

[0068] In the present application, the terms "axial", "axially", "radial" and "radially" are defined with respect to the longitudinal axis A.

[0069] The terms “upstream” and “downstream” are defined in relation to the direction of circulation of the gases in the turbomachine 1 along the longitudinal axis A.

[0070] The terms “internal”, “interior”, “external”, “exterior”, “externally” are defined in relation to the distance from the longitudinal axis X along a radial axis perpendicular to the longitudinal axis A.

[0071] The turbomachine 1 extends around a longitudinal axis A. It comprises from upstream to downstream in the direction of flow of the gases F along the longitudinal axis A, a fan 2, at least one compressor such as a low pressure compressor 3 and a high pressure compressor 4, a combustion chamber 5, at least one turbine 6 such as a high pressure turbine and a low pressure turbine, and a nozzle (not shown).

[0072] The rotor of the low pressure turbine is connected to the fan 2 and to the rotor of the low pressure compressor 3 by a low pressure shaft (not shown). The rotor of the high pressure turbine is connected to the rotor of the high pressure compressor 4 by a high pressure shaft (not shown).

[0073] The turbomachine 1 further comprises a rectifier 10. The rectifier 10 makes it possible to straighten the flow at the outlet of a rotor located upstream in order to provide maximum thrust at the outlet of the turbomachine 1. In the particular example of [Fig.l], the rectifier 10 is located downstream of the fan 2 and makes it possible to straighten the secondary flow F2.

[0074] The blower 2 allows the suction of an air flow dividing into a primary flow F1 and a secondary flow F2. The primary flow F1 passes through a primary vein of the turbomachine 1 while the secondary flow F2 is directed towards a secondary vein surrounding the primary vein.

[0075] The primary flow F1 is compressed within the low-pressure compressor 3 and then the high-pressure compressor 4. The compressed air is then mixed with a fuel and burned within the combustion chamber 5. The gases formed by the combustion pass through the high-pressure turbine and the low-pressure turbine. The gases finally escape through the nozzle, the cross-section of which allows the acceleration of these gases to generate propulsion. The secondary flow F2 passes through the rectifier 10, which accelerates the circulation speed of the secondary flow F2 to generate propulsion.

[0076] The fan 2 or the rectifier 10 comprise vanes 11. The vanes 11 equipping the rectifier 10 are known by the English term “Outlet Guide Vane” (OGV). The vanes 11 are movable or fixed in rotation about the longitudinal axis A. Typically, the vanes 11 of the fan 11 are movable in rotation. The vanes 11 of the rectifier 10 are fixed.

[0077] The blades 11 extend radially relative to the longitudinal axis A.

[0078] With reference to [Fig.2], each blade 11 comprises a blade 12 and a protective shield 14 arranged on the blade 12.

[0079] The blade 12 extends along an elongation axis X. The elongation axis X of the blade 12 extends radially relative to the longitudinal axis A of the turbomachine 1 after mounting the blade 11 on the turbomachine 1. The blade 12 has an aerodynamic profile. The blade 12 thus comprises an extrados face 12e and a intrados face 12i connected by a leading edge 12a and a trailing edge 12b. The blade 12 thus extends along a transverse axis Y between the leading edge 12a and the trailing edge 12b.

[0080] The blade 12 also extends longitudinally along the elongation axis X between a first end and a second end opposite the first end.

[0081] The blade 12 comprises a composite material. The composite material comprises a polymer matrix and a fibrous reinforcement embedded in the matrix. The composite material is for example an organic matrix composite (OMC). The matrix is ​​for example a thermoplastic or thermosetting polymer matrix. The thermosetting material is for example an epoxy polymer. The fibrous reinforcement comprises fibers which are for example carbon fibers or glass fibers. The fibers are organized for example in the form of a fibrous preform.

[0082] The protective shield 14 is advantageously arranged on the leading edge 12a. It advantageously extends along the entire length of the leading edge 12a. The protective shield 14 is advantageously made of a metallic material. The metallic material is, for example, titanium or an alloy such as a steel, for example a stainless steel or a nickel and cobalt alloy (NiCo), an aluminum, silver, zinc, nickel, copper or a mixture thereof.

[0083] The protective shield 14 is, according to another example, made of ceramic material.

[0084] It is intended to protect the leading edge 12a from external impacts. The shield of The protection shield 14 has an elongated dihedral shape. As best seen in [Fig. 3], the protection shield 14 has a V-shaped or U-shaped cross-section. The protection shield 14 comprises a first lateral fin 14a and a second lateral fin 14b connected to the first lateral fin 14a by a web 14j. The first and second lateral fins 14a, 14b define between them a cavity in which the leading edge 12a is arranged.

[0085] The first lateral fin 14a has a first free longitudinal end and the second lateral fin 14b has a second free longitudinal end which are opposite the core 14j. The free longitudinal ends extend along the blade 12. The free longitudinal ends extend respectively on the intrados face 12i and the extrados face 12b of the blade 12.

[0086] Advantageously, the thickness of the protective shield 14 is variable. The thickness of the core 14j is greater than the thicknesses of the first and second lateral fins 14a, 14b. Advantageously, the thickness of the first and second lateral fins 14a, 14b decreases towards the trailing edge 12b of the blade 12. The first and second lateral fins 14a, 14b are tapered towards the trailing edge 12b of the blade 12.

[0087] Alternatively, and in a manner not shown, the protective shield 14 is arranged on the trailing edge 12b. According to yet another alternative not shown, the blade 11 comprises two protective shields 14 arranged respectively on the leading edge 12a and the trailing edge 12b.

[0088] The protective shield 14 is very advantageously formed on the blade 12 by thermal projection.

[0089] The blade 11 further comprises a bonding layer 16 arranged between the blade 12 and the protective shield 14. The bonding layer 16 ensures the adhesion and mechanical anchoring of the protective shield 14 on the blade 12 without damaging the blade 12.

[0090] As best seen in [Fig.4], the bonding layer 16 is a hybrid layer. It comprises an adhesion sub-layer 17 and a bonding sub-layer 18.

[0091] The adhesion sub-layer 17 is arranged between the blade 12 and the adhesion sub-layer 18. The adhesion sub-layer 17 is made of polymeric material. The polymeric material is advantageously chosen from thermosetting polymers such as an epoxy, silicone or polyurethane polymer or thermoplastic polymers chosen for example from the family of polyaryletherketones such as a polyetheretherketone (PEEK) or a mixture thereof. The epoxy polymer is for example the commercial material Redux® 322 from the company HEXCEL.

[0092] The adhesion sub-layer 17 is in the form of a film based on one of the materials mentioned. The film is for example the commercial film AF191 or AF3109 from the company 3M. According to another particularly preferred example, the adhesion sub-layer 17 is in the form of a coating produced by thermal spraying. According to this example, the adhesion sub-layer 17 is made of a polymer material based on PEEK for example or any polymer compatible with the thermal spraying process.

[0093] Advantageously, the adhesion sub-layer 17 has a thickness of between 10 μm and 500 μm, even more advantageously between 50 μm and 500 μm and even more advantageously between 80 μm and 400 μm.

[0094] According to an embodiment of the invention shown in [Fig.4], the adhesion sub-layer 17 is single-layer.

[0095] According to another embodiment of the invention shown in [Fig.4a], the adhesion sub-layer 17 is multi-layer. It comprises a first layer 17a having a first thickness and a second layer 17b having a second thickness. The first layer 17a is arranged between the blade 12 and the second layer 17b. The first and second layers 17a, 17b are polymeric. Preferably, the first layer 17a comprises a first polymeric material and the second layer 17b comprises a second polymeric material different from or identical to the first material. Advantageously, the first and second polymeric materials are different, which makes it possible to adapt the properties of the bonding layer 16. Advantageously, the first and second materials are chosen from thermosetting polymers such as an epoxy, silicone or polyurethane polymer or thermoplastic polymers chosen, for example, from the family of polyaryletherketones such as a polyetheretherketone (PEEK) or a mixture thereof.

[0096] The second thickness of the second layer 17b is greater than 50 μm, greater than 80 μm. Preferably, the second thickness of the second layer 17b is less than the first thickness of the first layer 17a.

[0097] The first and second layers 17, 17b are preferably produced by thermal spraying.

[0098] The bonding sub-layer 18 is arranged between the adhesion sub-layer 17 and the protective shield 14. The bonding sub-layer 18 comprises particles 18a embedded in the adhesion sub-layer 17. By embedded in the adhesion sub-layer 17, it is understood that the particles 18a are partially embedded in the adhesion sub-layer 17 and that a portion of the surface of the particles is not embedded in the adhesion sub-layer 17 in order to create a surface condition favorable to the mechanical attachment of the protective shield 14. Thus, according to the invention, the particles 18a are embedded in a depth of the adhesion sub-layer 17 which is less than the thickness of the adhesion sub-layer 17.

[0099] According to the embodiment of [Fig.4a], the particles 18a are embedded in the second layer 17b of the adhesion layer 17.

[0100] Preferably, the surface coverage rate of the particles 18a is greater than or equal to 70%, greater than or equal to 80%, greater than or equal to 90% and even more preferably 100%. The surface coverage rate corresponds to the surface of the adhesion sub-layer 17 coated by the particles 18a divided by the total surface of the adhesion sub-layer 17, the surface being that opposite the blade 12.

[0101] Advantageously, the mass content of particles 18a in the bonding layer 16 is between 20% and 90%, advantageously between 50% and 90%.

[0102] Advantageously, the particles 18a are metal particles such as aluminum, silver, zinc, nickel, titanium, copper, an iron alloy or ceramic particles such as silicon carbide, or oxide particles such as than an aluminum oxide, a zirconium oxide, a silicon oxide, or a mixture of the particles. Advantageously, the material of the particles 18a is identical to the material of the protective shield 14. This makes it possible to increase the adhesion strength of the protective shield 14 on the blade 12.

[0103] Advantageously, the particles 18a have a size less than or equal to 500 pm, even more advantageously less than or equal to 400 pm and preferably less than or equal to 300 pm. Even more advantageously, at least 90% of the particles have a size (d90) of between 10 pm and 200 pm, advantageously of between 40 pm and 120 pm and at most 10% of the particles have a size (d10) of between 0.5 pm and 50 pm, advantageously of between 5 pm and 40 pm.

[0104] Advantageously, the particles 18a have a general spherical or acicular morphology.

[0105] The particle size distributions of the particles are for example grades F220, F80.

[0106] The adhesion sub-layer 17 makes it possible to ensure high adhesion between the substrate, i.e. the blade 12 and the adhesion sub-layer 18 while participating in the adhesion of the protective shield 14 to the blade 12. The adhesion sub-layer 18 makes it possible to create a surface favorable to the mechanical anchoring of the protective shield 14 to the blade 12. The protective shield 14 can then be formed by thermal spraying, a process which makes it possible to form coatings of complex shapes with low tolerances and in a repeatable manner.

[0107] Thanks to such a hybrid bonding layer 16, it has also been found that the mechanical properties of the blade 11 are improved.

[0108] A method of manufacturing the blade 11 according to the invention will now be described with reference to [Fig.5].

[0109] The method comprises the following chronological steps:

[0110] (a) providing the blade 12,

[0111] (b) arranging the bonding layer 16 on the blade 12,

[0112] (c) forming the protective shield 14 on the blade 12,

[0113] (d) optionally, machine the protective shield 14.

[0114] Step (a) may be carried out by molding such as resin transfer molding known by the acronym RTM for “Resin Transfer Molding” in English or draping.

[0115] Optionally, before step (b), the blade 12 may undergo mechanical or chemical surface preparation to improve the adhesion of the bonding layer 16.

[0116] Preferably, step (c) is carried out by thermal spraying. The thermal spraying process is, for example, flame spraying, for example by high velocity oxygen flame (HVOF), arc wire, suspension, plasma, cold spray, flame process or any other applicable thermal projection process.

[0117] The thermal projection is carried out with a powder comprising grains of which at least 90% of these grains have a size (d90) of between 5 pm and 200 pm, advantageously of between 10 pm and 150 pm and preferably of which at most 10% of the particles have a size (d10) of between 0.05 pm and 50 pm, advantageously of between 0.1 pm and 20 pm.

[0118] In particular, in the case of atmospheric pressure plasma projection (APS), the powder comprises particles of which at least 90% of these particles have a size (d90) of 110 pm and of which at most 10% of the particles have a size (d10) of 10 pm.

[0119] In the case of plasma projection of suspensions (SPS), the powder is in the form of a suspension comprising particles of which at least 90% of these particles have a size (d90) of 10 pm and of which at most 10% of the particles have a size (d10) of 0.1 pm.

[0120] Advantageously, the material of the powder is identical to that of the particles 18a of the bonding sub-layer 18.

[0121] The machining step (d) may be chemical machining or mechanical machining such as cutting.

[0122] According to a first embodiment shown in [Fig.6], step (b) comprises the following chronological sub-steps:

[0123] (bO) deposit the adhesion sub-layer 17 on the blade 12,

[0124] (bl) optionally, heat pretreat the adhesion sub-layer 17,

[0125] (b2) deposit the adhesion sub-layer 18 on the adhesion sub-layer 17,

[0126] (b3) heat treating the bonding layer 16 thus obtained,

[0127] (b4) optionally, mechanically treating the bonding layer 16.

[0128] Sub-step (b0) can be carried out by draping the film, or by manual application of the material of the adhesion underlayer 17 or even by spraying.

[0129] Sub-step (bl) can be carried out by heating the adhesion sub-layer 17. This heat pretreatment aims to increase the tack, so that the particles 18a adhere better in the adhesion sub-layer 17. This step can be carried out by heating the adhesion sub-layer 17 to a temperature below 100°C. Step (bl) is preferably carried out for a duration of less than or equal to 1 h, for example in an oven or furnace.

[0130] Sub-step (b2) is advantageously carried out by gravity deposition of the particles 18a, for example using a sieve manually or automatically.

[0131] Sub-step (b3) allows the polymerization of the adhesion layer 17 and the conso ligation of the bonding layer 16. It can be carried out by heating to a temperature between 100°C and 200°C, advantageously between 120°C and 190°C, even more advantageously between 140°C and 190°C.

[0132] Sub-step (b3) is preferably carried out for a duration greater than 10 min, greater than 15 min, greater than 20 min, greater than 30 min, even more preferably between 45 min and 200 min. The blade 11 is for example placed in an oven or a furnace.

[0133] Sub-step (b4) can be carried out by vibrations in order to remove the excess particles on the bonding layer (16) and achieve a surface rate advantageously of 100%. The blade 11 can for example be placed on a vibrating pot.

[0134] Sub-step (b4) can be carried out by sandblasting, plasma sanding or laser. This step makes it possible to release at least part of the particles from the adhesion layer 17 in order to create a surface condition favorable to the adhesion of the protective shield 14.

[0135] These mechanical treatments can be carried out in combination.

[0136] According to a second embodiment shown in [Fig.7], step (b) of the method comprises the following sub-steps:

[0137] (bi) depositing the first layer 17a on the blade 12,

[0138] (bii) depositing the second layer 17b and the particles 18a on the first layer 17a,

[0139] (biii) optionally heat treating the first layer 17a.

[0140] Step (bi) can be carried out after or simultaneously with step (a) in the case of draping the film, or by manual application of the material of the first layer 17a or by spraying, dipping, removal or any suitable process.

[0141] According to a particularly preferred embodiment, step (bi) is preferably carried out after step (a) by thermal spraying. The thermal spraying method is for example by high velocity oxygen flame (HVOF for "High Velocity Oxy-Fuel" in English), by arc-wire, by arc plasma, by cold spray, by flame process or any other applicable thermal spraying method.

[0142] Sub-step (bii) is carried out by thermal spraying of the particles 18a included in a polymer matrix forming the second layer 17b. The thermal spraying method is for example a high velocity oxygen flame (HVOF) method, arc-wire, arc plasma, cold spray, flame method or any other thermal spraying method applicable to the first layer 17a.

[0143] Sub-step (biii) is carried out by heating the bonding layer 16. It is optional in that the thermal spraying processes allow the polymerization of the adhesion layer 17 as soon as it is deposited on the blade 12.

[0144] This second variant is particularly advantageous since it allows the bonding layer 16 to be formed by the well-controlled method of thermal spraying. It also makes it possible to select different polymer matrices for the first and second layers 17a, 17b in order to adapt the properties of the bonding layer 16 and facilitate the manufacturing process of the blade 11.

Claims

Claims

1. A blade (11) for an aircraft turbomachine (1), the blade (11) comprising: - a blade (12) comprising an extrados face (12e) and an intrados face (12i) connected by a leading edge (12a) and a trailing edge (12b), the blade (12) comprising a composite material, - a protective shield (14) arranged on the blade (12), and - a bonding layer (16) arranged between the blade (12) and the protective shield (14) and comprising an adhesion sub-layer (17) made of polymeric material, characterized in that the bonding layer (16) further comprises an adhesion sub-layer (18) comprising particles (18a) embedded in the adhesion sub-layer (17), the adhesion sub-layer (18) being arranged between the adhesion sub-layer (17) and the protective shield (14).

2. Blade according to the preceding claim, characterized in that the particles (18a) are particles of metal, ceramic, oxide or a mixture thereof.

3. Blade according to any one of the preceding claims, characterized in that the particles (18a) have a size less than or equal to 500 pm, advantageously less than or equal to 400 pm, preferably less than or equal to 300 pm.

4. Blade according to any one of the preceding claims, characterized in that the adhesion sub-layer (17) has a thickness of between 10 pm and 500 pm, advantageously of between 50 pm and 500 pm or of between 80 pm and 400 pm.

5. Blade according to any one of the preceding claims, characterized in that the polymeric material of the adhesion sub-layer (17) is chosen from thermosetting polymers such as an epoxy or thermoplastic polymers or a mixture thereof.

6. Blade according to any one of the preceding claims, characterized in that the mass content of particles (18a) in the bonding layer (16) is between 20% and 90%, advantageously between 50% and 90%.

7. Blade according to any one of the preceding claims, characterized in that the adhesion sub-layer (17) comprises a first polymeric layer (17a) and a second polymeric layer (17b), the particles (18a) being embedded in the second layer (17b) which is arranged between the first layer (17a) and the bonding sub-layer (18).

8. Blade according to the preceding claim, characterized in that the first layer (17a) comprises a first polymeric material and the second layer (17b) comprises a second polymeric material different from the first polymeric material.

9. Blade according to one of claims 7 or 8, characterized in that the first layer (17a) has a first thickness and the second layer (17b) has a second thickness less than the first thickness.

10. A method of manufacturing a blade (11) for an aircraft turbomachine (1), the method comprising the following steps: (a) providing a blade (12) comprising an extrados face (12e) and an intrados face (12i) connected by a leading edge (12a) and a trailing edge (12b), the blade (12) comprising a composite material, (b) arranging a bonding layer (16) on the blade (12), the bonding layer (16) comprising an adhesion sub-layer (17) made of polymeric material, (c) forming a protective shield (14) on the blade (12), characterized in that in step (b) the bonding layer (16) further comprises an adhesion sub-layer (18) comprising particles (18a) embedded in the adhesion sub-layer (17), the adhesion sub-layer (18) being arranged between the adhesion undercoat (17) and the protective shield (14).

11. Method according to the preceding claim, characterized in that step (b) comprises the following sub-steps: (b0) depositing the adhesion sub-layer (17) on the blade (12), (b2) depositing the adhesion sub-layer (18) on the adhesion sub-layer (17), (b3) heat-treating the bonding layer (16).

12. Method according to the preceding claim, characterized in that step (b) further comprises between steps (b0) and (b2) the following sub-step: (bl) heat-pretreating the adhesion sub-layer (17).

13. Method according to claim 10, characterized in that step (b) comprises the following sub-steps:

14.

15.

16.

17.

18.

19.

20.

21. (bi) depositing a first polymeric layer (17a) on the blade (12), (bii) depositing a second polymeric layer (17b) and the particles (18a) on the first sub-layer (17a). Method according to the preceding claim, characterized in that step (b) comprises, after sub-step (bii), the following sub-step: (biii) heat-treating the first layer (17a). Method according to one of claims 13 to 14, characterized in that sub-step (bi) is carried out by thermal projection. Method according to one of claims 13 to 15, characterized in that sub-step (bii) is carried out by thermal projection of the particles (18a) previously impregnated with a polymer matrix forming the second layer (17b). Method according to any one of claims 10 to 16, characterized in that step (c) is carried out by thermal projection. Method according to the preceding claim, characterized in that the thermal projection is carried out with a powder comprising grains of which at least 90% of these grains have a size (d90) of between 5 pm and 200 pm, advantageously of between 10 pm and 150 pm. Method according to the preceding claim, characterized in that at most 10% of the grains have a size (d10) of between 0.05 pm and 50 pm, advantageously of between 0.1 pm and 20 pm. Method according to one of claims 18 to 19, characterized in that the material of the powder is identical to that of the particles (18a) of the bonding sub-layer (18). Method according to any one of claims 10 to 20, characterized in that it comprises, after step (c), a step (d) of machining the protective shield (14).