BALL-SHAPED MOLD, COPOLYMER BLOCK, RESIN COMPOSITION AND PRODUCTION METHOD FOR A COPOLYMER BLOCK

A block copolymer with tailored aromatic vinyl monomer units and molecular weight distribution addresses the hardness and crushability issues of conventional impact-resistant styrene-based resin balls, achieving easy handling and improved impact resistance and gloss.

FR3146901A1Pending Publication Date: 2024-09-27JAPAN ELASTOMER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2024002875
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-02-29
Filing Date
2024-03-22
Publication Date
2024-09-27

AI Technical Summary

Technical Problem

Conventional methods for producing impact-resistant styrene-based resins result in ball-shaped molded bodies with high hardness, leading to issues such as falling during transport and requiring intervals for positioning due to high load during grinding, without addressing hardness and crushability.

Method used

A block copolymer with specific compositions of aromatic vinyl monomer units, peak molecular weight, and molecular weight distribution is used to create a ball-shaped molded body with moderate hardness, allowing easy crushability and superior workability, achieved by controlling the content of aromatic vinyl monomer units, the proportion of the aromatic vinyl block fragment, peak molecular weight, and molecular weight distribution.

Benefits of technology

The solution results in a ball-shaped molded body with controlled hardness, enabling easy handling and grinding without deformation, and enhances impact resistance and gloss when used as a resin modifier.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a bullet-shaped molded body made of a block copolymer of moderate hardness, thus easily grindable and with superior workability. The bullet-shaped body of a block copolymer contains one unit of aromatic vinyl monomer and one unit of conjugated diene monomer, the block copolymer containing an aromatic vinyl block fragment, and the block copolymer satisfying the following conditions: the block copolymer has an aromatic vinyl monomer unit content of 10 to 30% by mass; the proportion between the aromatic vinyl block fragment and the total aromatic vinyl monomer unit content is 90 to 100% by mass; the aromatic vinyl block fragment has a peak molecular weight of 10,000 to 30,000; the ratio between the weight-average molecular weight, Mw, and the number-average molecular weight, Mn, in the aromatic vinyl block fragment (Mw / Mn) is between 1.15 and 1.40.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: BALL-SHAPED MOLDED BODY, BLOCK COPOLYMER, RESIN COMPOSITION AND METHOD FOR PRODUCING A BLOCK COPOLYMER Technical field

[0001] The present invention relates to a ball-shaped molded body, a block copolymer, a resin composition and a method for producing a block copolymer. Technological background

[0002] Styrene-based resins are widely used in various applications for their superior quality in terms of rigidity, transparency, gloss, etc., as well as their superior quality in terms of moldability, but they require the addition of a rubber-like polymer as a modifier due to their inferior quality in terms of impact resistance.

[0003] Methods of adding a rubber-like polymer to a styrene-based resin include a method of mechanically mixing a rubber-like polymer with a polystyrene-based resin and a method of subjecting a solution of a rubber-like polymer in styrene to bulk polymerization or bulk / suspension polymerization.

[0004] In particular, the mentioned methods of adding a rubber-like polymer to a styrene-based resin by various polymerization techniques give resin compositions having superior physical properties, and thus widely put into practice in the industry, and the resulting impact-resistant styrene-based resin compositions are used as materials of household appliances.

[0005] A known resin modification technique for acrylonitrile-butadiene-styrene (ABS) resins involves using a 5% by mass solution in styrene of a low viscosity conjugated diene-vinyl aromatic block copolymer to reduce the particle size of a rubber-like polymer used as a modifier.

[0006] For example, the following Patent Documents 1 and 2 each disclose a technique for producing a satisfactory impact-resistant styrene-based resin with a specified value of the peak-top molecular weight of a styrenic block moiety in a conjugated diene-aromatic vinyl block copolymer as a modifier.

[0007] Patent document 3 discloses a method for producing a conjugated diene polymer with a reduced amount of Li, and further discloses a technique to fix the viscosity of a 5% by mass solution in styrene of the conjugated diene polymer between 11 and 35 mPa-s and to use it to modify HIPS resins and ABS resins.

[0008] [List of quotes]

[0009] [Patent Document]

[0010] Patent Document 1: Japanese Patent No. 4029470

[0011] Patent Document 2: Japanese Patent No. 4029471

[0012] Patent Document 3: Japanese Patent No. 6646437 Summary of the invention

[0013] [Problem to be solved by the invention]

[0014] If prepared as a low viscosity solution in styrene, a conjugated diene-vinyl aromatic block copolymer as described above provides satisfactory ball moldability as a modifier.

[0015] However, even such a conjugated diene-aromatic vinyl block copolymer in a low-viscosity styrene solution may give rise to high hardness in a ball-shaped molded body produced by molding. In this case, when the ball-shaped molded body held by a conveying robot with its grippers is transferred in this state, the pressure of the grippers may release and disadvantageously cause the ball-shaped molded body to fall. In addition, such a hard ball-shaped molded body is subjected to a high load during crushing, which has the disadvantage of requiring intervals for placing the ball-shaped molded body.

[0016] The hardness of the ball-shaped molded body is affected by the structure of the conjugated diene-aromatic vinyl block copolymer. Although patent document 2 refers to the ball-shaped moldability, patent documents 1 to 3 do not refer to the hardness and grindability of the ball-shaped molded body.

[0017] A "ball-shaped molded body" is a cuboid having the shape of a 25 to 35 kg block produced by press molding a synthetic rubber.

[0018] In view of these circumstances, an object of the present invention is to provide: a ball-shaped molded body of moderate hardness made of a block copolymer, thus easily grindable and having superior workability; a block copolymer constituting the ball-shaped molded body; and a resin composition resulting from the polymerization of the block copolymer and a styrene-based resin.

[0019] [Means to solve the problem]

[0020] The inventors of the present invention have diligently sought to solve the problems inherent in the conventional techniques described above and have discovered that these problems could be solved by specifying the content of aromatic vinyl monomer units, the proportion of aromatic vinyl block moiety to the total content of aromatic vinyl monomer units, the peak top molecular weight of the aromatic vinyl block moiety and the molecular weight distribution of the aromatic vinyl block moiety, which finally resulted in the present invention.

[0021] More specifically, the present invention is as follows.

[0022] [1] Ball-shaped molded body of a block copolymer containing a unit of aromatic vinyl monomer and a conjugated diene monomer unit,

[0023] the block copolymer containing an aromatic vinyl block fragment, and

[0024] the block copolymer satisfying the<condition (a)> has<condition (d)> following:

[0025] <Condition (a)>

[0026] the block copolymer has a content of aromatic vinyl monomer units of 10 to 30% by mass;

[0027] <Condition (b)>

[0028] the proportion between the sequenced aromatic vinyl block fragment and the total content of aromatic vinyl monomer units is 90 to 100% by mass;

[0029] <Condition (c)>

[0030] the aromatic vinyl block fragment has a peak top molecular weight of 10,000 to 30,000; and [0031 ]<Condition (d)>

[0032] the ratio of the weight average molecular weight, Mw, to the number average molecular weight, Mn, in the aromatic vinyl block fragment (Mw / Mn) is between 1.15 and 1.40.

[0033] [2] Ball-shaped molded body according to [1], wherein a solution in the 5% by mass styrene block copolymer has a viscosity of 7 to 15 rnPa-s under a temperature condition of 25 °C.

[0034] [3] Ball-shaped molded body according to [1] or [2], wherein the copolymer block has a 1,2-vinyl bond content of 15 to 30 mol% in the conjugated diene monomer unit.

[0035] [4] Body molded in the form of a ball according to any one of points [1] to [3], having a hardness of 50 to 72 measured using a type E durometer according to JIS K6253.

[0036] [5] Block copolymer containing an aromatic vinyl monomer unit and a conjugated diene monomer unit,

[0037] the block copolymer containing an aromatic vinyl block fragment, and

[0038] the block copolymer satisfying the<condition (a)> has<condition (d)> following:

[0039] <Condition (a)>

[0040] the block copolymer has a content of aromatic vinyl monomer units of 10 to 30% by mass;

[0041] <Condition (b)>

[0042] the proportion between the aromatic vinyl block fragment and the total content of aromatic vinyl monomer units is 90 to 100% by mass;

[0043] <Condition (c)>

[0044] the aromatic vinyl block fragment has a peak top molecular weight of 10,000 to 30,000; and

[0045] <Condition (d)>

[0046] the ratio of the weight average molecular weight, Mw, to the number average molecular weight, Mn, in the aromatic vinyl block fragment (Mw / Mn) is between 1.15 and 1.40.

[0047] [6] Block copolymer according to [5], in which a solution in styrene at 5% in block copolymer mass has a viscosity of 7 to 15 mPa-s under a temperature condition of 25 °C.

[0048] [7] Block copolymer according to [5] or [6], the block copolymer having a content of 1,2-vinyl linkages of 15 to 30 mol% in the conjugated diene monomer unit.

[0049] [8] Resin composition resulting from the polymerization of:

[0050] 3 to 20 parts by mass of the block copolymer which constitutes the molded body in the form of ball according to any of points [1] to [4], and

[0051] 97 to 80 parts by mass of a styrene-based resin.

[0052] [9] Resin composition according to [8], wherein the styrene-based resin is a copolymer of a compound based on styrene and acrylonitrile.

[0053]

[10] Process for producing the block copolymer which constitutes the molded body in ball shape according to any one of points [1] to [4], the method comprising the steps of:

[0054] providing a conjugated diene compound into a reactor to polymerize the conjugated diene compound to reach a peak temperature of 91 to 100°C; and

[0055] providing and polymerizing an aromatic vinyl compound while maintaining a temperature of 90 to 100°C in the reactor.

[0056]

[11] Resin composition resulting from the polymerization of:

[0057] 3 to 20 parts by mass of the block copolymer according to any one of points [5] to [7] ; and

[0058] 97 to 80 parts by mass of a styrene-based resin.

[0059]

[12] Resin composition according to

[11] , wherein the styrene-based resin is a copolymer of a compound based on styrene and acrylonitrile.

[0060]

[13] Process for producing the block copolymer according to any one of points [5] to [7], the method comprising the steps of:

[0061] providing a conjugated diene compound into a reactor to polymerize the conjugated diene compound to reach a peak temperature of 91 to 100°C; and

[0062] providing and polymerizing an aromatic vinyl compound while maintaining a temperature of 90 to 100°C in the reactor.

[0063] [Advantageous effects of the invention]

[0064] The present invention can provide: a ball-shaped molded body made of a conjugated diene-aromatic vinyl block copolymer, which has moderate hardness and is therefore easily grindable and has superior workability; a block copolymer constituting the ball-shaped molded body; and a resin composition superior in gloss and impact resistance, resulting from the polymerization of the block copolymer and a styrene-based resin. Detailed description for carrying out the invention

[0065] Embodiments of the present invention (hereinafter referred to as "the present embodiment") will be described in detail below.

[0066] The present embodiment illustrated below is an example for describing the present invention, the present invention not being limited to the embodiments illustrated below. The present invention may be implemented with various modifications that fall within the scope of the present invention.

[0067] [Bullet-shaped molded body and block copolymer]

[0068] A ball-shaped molded body according to the present embodiment is a ball-shaped molded body of a block copolymer of the present embodiment containing a conjugated diene monomer unit and an aromatic vinyl monomer unit.

[0069] In the present invention, a monomer, which is a constituent element of a block copolymer, is referred to as a "monomer unit", and a monomer before being incorporated into a polymer is referred to as a "compound".

[0070] The block copolymer according to the present embodiment, which constitutes the ball-shaped molded body of the present embodiment, contains an aromatic vinyl block moiety and satisfies the<condition (a)> has<condition (d)> following: [0071 ]<Condition (a)>

[0072] the block copolymer has a content of aromatic vinyl monomer units of 10 to 30% by mass;

[0073] <Condition (b)>

[0074] the proportion between the aromatic vinyl block fragment and the total content of aromatic vinyl monomer units is 90 to 100% by mass;

[0075] <Condition (c)>

[0076] the aromatic vinyl block fragment has a peak top molecular weight of 10,000 to 30,000; and

[0077] cCondition (d)>

[0078] the ratio of the weight average molecular weight, Mw, to the number average molecular weight, Mn, in the aromatic vinyl block fragment (Mw / Mn) is between 1.15 and 1.40.

[0079] The configurations of the ball-shaped molded body and the block copolymer of the present embodiment make it possible to obtain a ball-shaped molded body having moderate hardness, thus being easily grindable and having superior workability.

[0080] In the present invention, a monomer which is used to produce a polymer is referred to as a "compound", and a constituent element of a polymer is referred to as a "monomer unit".

[0081] Examples of the conjugated diene compound forming each conjugated diene monomer unit in the block copolymer include, but are not limited to, 1,3-butadiene, 2-methyl-1,3-butadiene (i.e., isoprene), 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, and 1,3-pentadiene. Among them, 1,3-butadiene and 2-methyl-1,3-butadiene are preferable, and 1,3-butadiene is particularly preferable. Only one of these conjugated diene compounds may be used alone; alternatively, two or more of them may be used in combination.

[0082] Examples of the aromatic vinyl compound forming each aromatic vinyl monomer unit in the block copolymer include, but are not limited to, styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-diisopropylstyrene, 2,4-dimethylstyrene, 4-t-butylstyrene, 5-t-butyl-2-methylstyrene, monochlorostyrene, dichlorostyrene, and monofluorostyrene. Among them, styrene is preferable. Only one of these aromatic vinyl compounds may be used alone; another possibility is to use two or more of them in combination.

[0083] (cCondition (a) > Content of aromatic vinyl monomer units of the block copolymer)

[0084] The content of aromatic vinyl monomer units in the block copolymer which constitutes the ball-shaped molded body of the present embodiment and that in the block copolymer of the present embodiment are each 10 to 30% by mass, preferably 14 to 26% by mass and more preferably 17 to 23% by mass.

[0085] The content of conjugated diene monomer units in the block copolymer is 70 to 90% by mass, preferably 74 to 86% by mass and more preferably 77 to 83% by mass.

[0086] The configuration in which the content of aromatic vinyl monomer units in the block copolymer is greater than or equal to 10% by mass ensures the required hardness for the ball-shaped molded body, which enables the ball-shaped molded body of ball to be resistant to deformation under load. In addition, a rigidity-improving effect is exhibited when used as a curing agent for an aromatic vinyl resin. The configuration in which the content of aromatic vinyl monomer units is 30% by mass or less enables the ball-shaped molded body to have moderately high hardness and exhibit satisfactory grindability and solubility, and ensures impact resistance when used as a curing agent for an aromatic vinyl resin.

[0087] In the present invention, "the hardness of the ball-shaped molded body" refers to the hardness of the ball-shaped molded body produced by molding without adding oil to the block copolymer. In the present embodiment, controlling the hardness of the ball-shaped molded body in a so-called non-oil-extended state by virtue of the structure of the block copolymer enables the workability of the ball-shaped molded body to be improved, as well as an improvement effect, for example, for the degree of freedom in the design of a resin composition, since any accidental inclusion of oil is avoided in applications with the ball-shaped molded body.

[0088] The content of aromatic vinyl monomer units in the block copolymer can be controlled within the numerical range shown below by adjusting the amount of aromatic vinyl compound to be added and the polymerization time in the polymerization process.

[0089] (<Condition (b)> Ratio of the vinyl aromatic block fragment to the total content of vinyl aromatic monomer units in the block copolymer)

[0090] The proportion of the aromatic vinyl block moiety to the total content of aromatic vinyl monomer units in the block copolymer constituting the ball-shaped molded body of the present embodiment and that in the block copolymer of the present embodiment are each in the range of 90 to 100% by mass, preferably 93 to 100% by mass, and more preferably 95 to 99.9% by mass.

[0091] In the present invention, "aromatic vinyl block moiety" refers to a block moiety in which 10 or more aromatic vinyl monomer units are consecutively linked.

[0092] The configuration in which the proportion of the aromatic vinyl block moiety to the total content of aromatic vinyl monomer units in the block copolymer is 90% by mass or more enables the ball-shaped molded body to exhibit satisfactory solubility in styrene, styrene / acrylonitrile, styrene / methacrylate and the like after being ground, and provides improved resistance to shocks when used as a curing agent for aromatic vinyl resin.

[0093] The proportion of the vinyl aromatic block moiety to the total content of vinyl aromatic monomer units in the block copolymer can be controlled within this numerical range by adjusting the timing of addition of the vinyl aromatic compound in the polymerization process.

[0094] (<Condition (c)> Peak molecular weight of the aromatic vinyl block fragment)

[0095] In the ball-shaped molded body of the present embodiment and the block copolymer constituting the block copolymer of the present embodiment, the vinyl aromatic block moiety constituting each block copolymer has a peak top molecular weight of 10,000 to 30,000.

[0096] In particular, the peak top molecular weight of the vinyl aromatic block moiety on a molecular weight distribution curve for an ozonolysis product of the block copolymer, as a value in terms of standard monodisperse polystyrene as measured by gel permeation chromatography (hereinafter also referred to as "GPC"), is in the range of 10,000 to 30,000, preferably in the range of 11,000 to 27,000 and more preferably in the range of 12,000 to 25,000.

[0097] The configuration in which the peak-top molecular weight of the aromatic vinyl block moiety is 10,000 or higher ensures the required hardness for the ball-shaped molded body of the present embodiment, thereby enabling the ball-shaped molded body to be resistant to deformation under load when stacked. The configuration in which the peak-top molecular weight on a molecular weight distribution curve for the aromatic vinyl block moiety is 30,000 or lower enables the ball-shaped molded body of the present embodiment to have moderately high hardness with satisfactory workability, whereby the increase in load during crushing is successfully prevented.The configuration in which the peak-top molecular weight of the aromatic vinyl fragment is in the range of 10,000 to 30,000 provides a satisfactory balance between impact strength and gloss when used as a curing agent for an aromatic vinyl resin.

[0098] The peak top molecular weight of the aromatic vinyl fragment can be controlled within this numerical range by adjusting the amount of polymerization initiator to be added and the amount of aromatic vinyl compound to be added in the polymerization process.

[0099] (<Condition (d)> Ratio of weight average molecular weight, Mw, to number average molecular weight, Mn, in the vinyl aromatic block fragment)

[0100] The ratio of the weight average molecular weight to the number average molecular weight in the block copolymer which constitutes the ball-shaped molded body of the present embodiment (Mw / Mn) (hereinafter referred to as the molecular weight distribution) and that in the block copolymer of the present embodiment are each between 1.15 and 1.40.

[0101] In particular, the molecular weight distribution (Mw / Mn) acquired in a molecular measurement for the vinyl aromatic block moiety of an ozonolysis product of the block copolymer is in the range of 1.15 to 1.40. For the adjustment of the hardness of the ball-shaped molded body of the present embodiment, the molecular weight distribution is preferably in the range of 1.15 to 1.35, more preferably in the range of 1.15 to 1.30, even more preferably in the range of 1.15 to 1.25, more preferably in the range of 1.18 to 1.35, even more preferably in the range of 1.18 to 1.30, and particularly preferably in the range of 1.20 to 1.30.

[0102] The configuration in which the molecular weight distribution in the aromatic vinyl block moiety is within this range enables the hardness of the ball-shaped molded body to be controlled so as to achieve a value satisfactory for practical use. In the present invention, the hardness of the ball-shaped molded body is that measured using an E-type durometer according to JIS K 6253 and can, in particular, be measured by a method described below in the examples.

[0103] The configuration in which the molecular weight distribution (Mw / Mn) in the aromatic vinyl block fragment is 1.15 or greater enables the hardness of the ball-shaped molded body to be adjusted to 72 or less with ease, and while the ball-shaped molded body held by a robot or the like with its grippers is transferred in this state, it is possible to successfully prevent the ball-shaped molded body from falling by the pressure of the grippers. The configuration in which the molecular weight distribution (Mw / Mn) in the aromatic vinyl block fragment is 1.40 or less enables the hardness of the ball-shaped molded body to be set to 50 or less with ease, and it is possible to successfully prevent the ball-shaped molded body from being deformed under a load when ball-shaped molded bodies each being the ball-shaped molded body are stacked.

[0104] The molecular weight distribution in the aromatic vinyl block fragment can be controlled within this numerical range by adjusting the temperature in a reactor when the aromatic vinyl compound is added.

[0105] The above-described hardness of the ball-shaped molded body of the block copolymer of the present embodiment, particularly its hardness as measured using an E-type durometer according to JIS K 6253, is preferably between in the range of 50 to 72, more preferably in the range of 53 to 70 and even more preferably in the range of 55 to 68. The configuration in which the hardness of the ball-shaped molded body is 50 or higher enables, when a plurality of ball-shaped molded bodies each being the ball-shaped molded body are stacked, to prevent the lower ball-shaped molded bodies from being deformed under a load. The configuration in which the hardness of the ball-shaped molded body is 72 or lower ensures the maneuverability of the ball-shaped molded body by robotic arms and does not cause a high load for crushing the ball-shaped molded body, thereby enabling the ball-shaped molded body to be continuously placed in a crusher without intervals and ensuring satisfactory crushing efficiency.

[0106] The hardness of the ball-shaped molded body of the block copolymer can be controlled within this numerical range by adjusting the molecular weight distribution (Mw / Mn) in the aromatic vinyl block moiety that constitutes the block copolymer. In particular, the hardness of the ball-shaped molded body can be controlled to reach 72 or less by adjusting the molecular weight distribution (Mw / Mn) to 1.15 or more, and the hardness of the ball-shaped molded body can be controlled to reach 50 or more by adjusting the molecular weight distribution (Mw / Mn) to 1.40 or less.

[0107] The molecular weight distribution in the aromatic vinyl block fragment can be controlled within this numerical range by adjusting the temperature in a reactor when the aromatic vinyl compound is added in the polymerization process.

[0108] In the block copolymer constituting the ball-shaped molded body of the present embodiment as well as in the block copolymer of the present embodiment, the vinyl aromatic block moiety is preferably disposed at one end of the block copolymer. In this way, the ball-shaped molded body exhibits satisfactory solubility in styrene, styrene / acrylonitrile, styrene / methacrylate or the like in an application in which the ball-shaped molded body is ground and then dissolved in such a solvent.

[0109] A 5 mass% styrene solution of the block copolymer which constitutes the ball-shaped molded body of the present embodiment as well as the block copolymer of the present embodiment has a viscosity of 7 to 15 mPa-s, preferably a viscosity of 8 to 13 mPa-s and even more preferably a viscosity of 9 to 12 mPa-s under a temperature condition of 25°C.

[0110] When the viscosity of the solution in styrene at 5% by mass of the block copolymer is greater than or equal to 7 mPa-s, it is likely to obtain a better impact resistance when used as a curing agent for aromatic vinyl resin.

[0111] When the viscosity of the 5% by mass styrene solution of the block copolymer is less than or equal to 15 mPa-s, it is likely to achieve sufficient reduction in the rubber particle size of an aromatic vinyl resin when used as a curing agent for an aromatic vinyl resin, as well as a satisfactory balance between impact strength, gloss and rigidity.

[0112] The viscosity of the solution in 5% by mass styrene of the block copolymer can be controlled within this numerical range by adjusting the peak top molecular weight of the block copolymer.

[0113] The block copolymer constituting the ball-shaped molded body of the present embodiment and the block copolymer of the present embodiment each preferably have a 1,2-vinyl bond content of 15 to 30 mol%, more preferably 16 to 28%, even more preferably 17 to 25% in the conjugated diene monomer unit. The configuration in which the 1,2-vinyl bond content is 30 mol% or less makes it possible, when using the ball-shaped molded body of the present embodiment or the block copolymer of the present embodiment as a reinforcing agent for an impact-resistant aromatic vinyl resin, to easily control the corresponding amount to be grafted so as to give the rubber particles in the impact-resistant aromatic vinyl resin the shape of salami-like particles, and the particle sizes can also be easily controlled.The configuration in which the content of 1,2-vinyl bonds is 15 mol% or more enables, when using the ball-shaped molded body of the present embodiment or the block copolymer of the present embodiment as a reinforcing agent for an impact-resistant aromatic vinyl resin, easy reduction in the size of rubber particles, particularly those in an acrylonitrile-butadiene-styrene (ABS) resin, as well as improved impact resistance of a resin composition resulting from the polymerization of such an impact-resistant aromatic vinyl resin and the block copolymer of the present embodiment.

[0114] The 1,2-vinyl bond content of the block copolymer can be controlled within this numerical range by adjusting the amount of polar substance to be added and the polymerization temperature in the polymerization process.

[0115] The block copolymer that constitutes the ball-shaped molded body of the present embodiment and the block copolymer of the present embodiment each have a configuration such that the block copolymer has a content of aromatic vinyl monomer units of 10 to 30 mass%, the proportion between the aromatic vinyl block fragment and the total content of aromatic vinyl monomer units is 90-100% by mass, the aromatic vinyl block fragment has a peak top molecular weight of 10,000-30,000, and the molecular weight distribution (Mw / Mn) in the aromatic vinyl block fragment is in the range of 1.15-1.40.

[0116] The block copolymer having such a configuration is obtained by a process consisting of: supplying a conjugated diene compound into a reactor with adjustment of the amount of a catalyst to be added in order to polymerize the conjugated diene compound so as to reach a maximum temperature of 91 to 100°C; then supplying and polymerizing an aromatic vinyl compound while maintaining a temperature of 90 to 100°C in the reactor.

[0117] An example of such methods involves providing and polymerizing an aromatic vinyl compound, preferably maintaining a temperature of 91 to 99°C in the reactor, more preferably maintaining a temperature of 92 to 98°C in the reactor.

[0118] If the reactor temperature is below 90°C, the molecular weight distribution (Mw / Mn) in the aromatic vinyl block fragment will likely be less than 1.15. If the reactor temperature is above 100°C, the molecular weight distribution in the aromatic vinyl block fragment (Mw / Mn) will likely be broad and sometimes bimodal, corresponding to a dispersed molecular weight distribution.

[0119] (Process for producing a block copolymer)

[0120] The block copolymer which constitutes the ball-shaped molded body of the present embodiment contains an aromatic vinyl monomer unit and a conjugated diene monomer unit and contains an aromatic vinyl block moiety.

[0121] The block copolymer can be produced by polymerization in a hydrocarbon solvent with an organolithium compound as a polymerization initiator.

[0122] Examples of the organolithium compound include, but are not limited to, a compound with one or more lithium atoms bonding in the molecule. Examples of the compound include ethyllithium, n-propyllithium, isopropyllithium, n-butyllithium, sec-butyllithium, tert-butyllithium, rhexamethylenelithium, butadienyldilithium, and isoprenyldilithium. One of these may be used alone; another possibility is to use two or more of them in combination.

[0123] Examples of the hydrocarbon solvent for producing the block copolymer include, but are not limited to, hydrocarbon solvents from among: aliphatic hydrocarbons such as butane, pentane, hexane, isopentane, heptane, octane and isooctane; alicyclic hydrocarbons such as cyclopentane, methylcyclopentane, cyclohexane, methylcyclohexane and ethylcyclohexane; and aromatic hydrocarbons such as benzene, toluene, ethylbenzene and xylene.

[0124] One of them can be used alone; another possibility is to use two or more of them in combination.

[0125] Exemplary methods of adjusting the content of 1,2-vinyl bonds in the conjugated diene monomer unit of the block copolymer include a method of adding a polar substance such as dimethyl ether, diethyl ether, diphenyl ether, tetrahydrofuran, diethylene glycol dimethyl ether, diethylene glycol dibutyl ether, trimethylamine, triethylamine, tetramethylethylenediamine, triphenylphosphine and hexamethylphosphoramide to a polymerization system containing an organolithium compound as a polymerization initiator.

[0126] One of them can be used alone; another possibility is to use two or more of them in combination.

[0127] In particular, it is preferable to supply a conjugated diene compound to a polymerization system containing an organolithium compound and a polar substance in a reactor so as to reach a maximum temperature of 91 to 100°C, and then supply and polymerize an aromatic vinyl compound while maintaining a temperature of 90 to 100°C in the reactor.

[0128] Although the polymerization time is longer, the molecular weight distribution (Mw / Mn) in the aromatic vinyl block fragment can be controlled in the range of 1.15 to 1.40 by applying a method of adding an aromatic vinyl compound over a longer period or a method of adding an aromatic vinyl compound in portions.

[0129] It is preferable to use a method of supplying a conjugated diene compound into a reactor to polymerize the conjugated diene compound to reach a peak temperature of 91 to 100°C, and then supplying and polymerizing an aromatic vinyl compound while maintaining a temperature of 90 to 100°C in the reactor to obtain a block copolymer, this method giving the best polymerization rate, which makes it efficient.

[0130] Furthermore, it is preferable to use an inert gas atmosphere such as nitrogen gas as the atmosphere for the polymerization system.

[0131] The polymerization pressure is not limited and only needs to be within a pressure range sufficient to maintain the monomers and solvent in the liquid phase within the polymerization temperature range.

[0132] (Additive)

[0133] After quenching by adding water, an alcohol, an organic acid or the like to a solution of the block copolymer described above, a stabilizer such as a phenolic stabilizer, a phosphorus-containing stabilizer, a sulfur-containing stabilizer and an amine stabilizer or any other known additive may be added to the solution of the block copolymer.

[0134] As disclosed in Japanese Patent No. 6646437, catalysis residues, if necessary, can be removed from the block copolymer of the present embodiment, and the latter can be separated from the block copolymer solution. Solvent separation can be carried out by placing the block copolymer solution in hot water with stirring and removing the solvent by steam extraction. After the solvent removal process, e.g., by steam extraction, the block copolymer is extruded using an extruder and then dried with hot air or under vacuum, and the resulting block copolymer, in the form of flakes, is molded using a ball-shaped molding machine, thereby obtaining a ball-shaped molded body.

[0135] Since the hardness of the ball-shaped molded body of the present embodiment, which has been produced as described above, can be adjusted so as to obtain superior workability, resulting in superior quality in terms of workability and grindability for robots, and since the size of rubber particles in an aromatic vinyl resin such as ABS can also be reduced, it is possible to obtain a resin composition superior in terms of gloss and impact resistance. Thus, the block copolymer of the present embodiment can be used as a resin modifier (curing agent) capable of improving gloss and impact resistance.

[0136] [Resin composition]

[0137] A resin composition according to the present embodiment results from the polymerization of: 3 to 20 parts by mass of the above-described block copolymer which constitutes the ball-shaped molded body of the present embodiment or the block copolymer of the present embodiment; and 97 to 80 parts by mass of a styrene-based resin.

[0138] For the styrene-based resin, it is possible to use a styrene-based compound used for the production of resin compositions. It should be noted that the styrene-based compound can be in any polymer, monomer and oligomer state.

[0139] Examples of the styrene-based compound include, but are not limited to, styrenes and / or derivatives thereof, such as styrene, α-methylstyrene, vinyltoluene and chlorostyrene. Among them, styrene is preferable.

[0140] Only one of these styrene-based compounds can be used alone; another possibility is to use two or more of them used in combination.

[0141] The styrene-based compound may be a homopolymer of the compound or a copolymer of styrene and a compound copolymerizable with another compound.

[0142] Examples of the compound copolymerizable with the styrene-based compound include vinyl monomers, including unsaturated nitrile compounds such as acrylonitrile and methacrylonitrile, acrylates such as methyl acrylate, and methacrylates such as methyl methacrylate, with acrylonitrile being particularly preferable.

[0143] The block copolymer content of the resin composition of the present embodiment with respect to the block copolymer of the present embodiment is preferably 5 to 18 parts by mass, and more preferably 8 to 15 parts by mass.

[0144] The styrene-based resin content is preferably 95 to 82 parts by mass, and more preferably 92 to 85 parts by mass.

[0145] The resin composition of the present embodiment can be produced by polymerizing the styrene-based resin and the block copolymer, and the polymerization can be carried out by mixing monomers of the styrene-based resin and the block copolymer. In particular, the resin composition of the present embodiment can be produced by a method described below in the examples. Examples

[0146] The present embodiment will be described in more detail below with the aid of specific examples and comparative examples; however, the present invention is in no way limited to the following examples and comparative examples.

[0147] The measurement of physical properties and the evaluation of characteristics of the examples and comparative examples were carried out as follows.

[0148] ((1) Content of aromatic vinyl monomer units of the block copolymer)

[0149] To determine the content of aromatic vinyl monomer units of a block copolymer, a chloroform solution of a block copolymer sample was prepared as a sample, and the UV absorption by the phenyl group of the aromatic vinyl at 254 nm was measured using a measuring apparatus (manufactured by JASCO Corporation: V-550) to determine the content of aromatic vinyl monomer units (mass%).

[0150] ((2) Proportion between the content of aromatic vinyl block fragment and the total content in aromatic vinyl monomer units in the block copolymer)

[0151] The ratio of the vinyl aromatic block fragment content to the total vinyl aromatic monomer unit content in a block copolymer was measured according to an osmate decomposition process described in LM Kolthoff, et al., J. Polym. Sci., 1, 429 (1948).

[0152] In particular, 0.05 g of a block copolymer was dissolved in 10 ml of chloroform, 16 ml of a 69% aqueous solution of tert-butyl hydroperoxide and 4 ml of a 0.05% chloroform solution of osmium tetroxide were added, and the result was refluxed in a 90°C bath for 12 minutes for an oxidative decomposition reaction. After the reaction was completed, the reaction solution was cooled and 200 ml of methanol was added to the reaction solution with stirring to precipitate an aromatic vinyl block fragment component, which was separated by filtration through a 5 µm glass filter, and the aromatic vinyl block fragment content of the block copolymer was measured. Then, the proportion between the aromatic vinyl block fragment and the total content of aromatic vinyl monomer units in the block copolymer, the value of which was obtained during the measurement in (1), was calculated.

[0153] ((3) Peak top molecular weight of the block copolymer)

[0154] The peak top molecular weight of a block copolymer was measured by gel permeation chromatography (hereinafter also referred to as "GPC").

[0155] A chromatogram was acquired by GPC (device: HLC-8320GPC EcoSEC manufactured by Tosoh Corporation, column: PL MiniMIX-C 4.6 mm gel column <p x 300 mm x trois colonnes, solvant : tétrahydrofurane, conditions de mesure : température de la colonne de 40 °C, débit de 0,4 ml / min, concentration de l’échantillon de 0,1 % en masse, volume d’injection de 50 pl).

[0156] A calibration curve was prepared with commercially available standard monodisperse polystyrenes having known molecular weights, and the peak top molecular weight was determined using this calibration curve from the acquired GPC chromatogram.

[0157] GPC: HLC-8320GPC EcoSEC (manufactured by Tosoh Corporation)

[0158] Detector: IR

[0159] Column: PL 5 pm MiniMIX-C 4.6 mm gel column <p x 300 mm x trois colonnes

[0160] Solvant : tétrahydrofurane

[0161] Flow rate: 0.4 ml / min

[0162] Concentration: 0.1% by mass

[0163] Column temperature: 40°C

[0164] Injection volume: 50 μl

[0165] ((4) Peak top molecular weight of the aromatic vinyl block fragment and molecular weight distribution (Mw / Mn) in the block copolymer)

[0166] In a solution of 0.1 g of a block copolymer dissolved in 100 ml of dichloromethane, oxygen with an ozone concentration of 1.5% was passed at 150 ml / min for oxidative decomposition, and the resulting ozonide was added dropwise into diethyl ether with lithium aluminum hydride mixed therewith for reduction.

[0167] Then, pure water was added dropwise for hydrolysis, potassium carbonate was added for salt removal, and the result was filtered to give the aromatic vinyl block fragment component. This aromatic vinyl block fragment was subjected to GPC measurement.

[0168] A chromatogram was acquired by GPC (device: HLC-8320GPC EcoSEC manufactured by Tosoh Corporation, column: Shodex KF-803L and KF-801 x two columns, solvent: tetrahydrofuran, measurement conditions: column temperature of 40 °C, flow rate of 0.8 ml / min, sample concentration of 0.1 mass%, injection volume of 50 μl), and the peak top molecular weight was determined.

[0169] A calibration curve was prepared with commercially available standard monodisperse polystyrenes having known molecular weights, the weight average molecular weight, Mw, and number average molecular weight, Mn, were determined using this calibration curve from the acquired GPC chromatogram, and the molecular weight distribution (Mw / Mn) was calculated.

[0170] GPC: HLC-8320GPC EcoSEC (manufactured by Tosoh Corporation)

[0171] Detector: UV

[0172] Column: Shodex K-803L, K801, K801, three columns

[0173] Solvent: tetrahydrofuran

[0174] Flow rate: 0.8 ml / min

[0175] Concentration: 0.1% by mass

[0176] Column temperature: 40°C

[0177] Injection volume: 50 μl

[0178] ((5) Content of 1,2-vinyl bonds in the conjugated diene monomer unit of the block copolymer)

[0179] The content of 1,2-vinyl bonds in the conjugated diene monomer unit was determined by infrared spectrometry according to "Hampton, Anal. Chem. 21, 923 (1941)".

[0180] ((6) Viscosity of a solution in styrene at 5% by mass of the block copolymer under a temperature condition of 25°C)

[0181] For the viscosity of a 5 mass% styrene solution of a block copolymer at a temperature of 25°C, 5 g of a block copolymer was dissolved in 95 g of styrene, and the viscosity was measured using a Cannon-Fenske viscometer (manufactured by Kusano Science Instrument Mill Co., Ltd., product name: Cannon-Fenske No. 200) at a measuring temperature of 25°C.

[0182] ((7) Hardness of the ball-shaped molded body of the block copolymer)

[0183] In a mold for ball-shaped molding (length: 70 cm, width: 35 cm), 35 kg of flakes of a block copolymer were placed and molded into a ball shape under conditions of compression pressure: 200 kg / cm2, compression time: 50 seconds, and compression temperature: 60°C, and a “Type E Durometer JIS K 6253” manufactured by Kobunshi Keiki Co., Ltd. (ASKER) was pressed onto smooth parts of the obtained ball-shaped molded body to determine the hardness of the ball-shaped molded body, and each maximum value was recorded.

[0184] The ball-shaped molded body was turned over and five smooth parts were subjected to measurement; the average value was determined as the hardness of the ball-shaped molded body.

[0185] ((8) Peak current during grinding of the ball-shaped molded body of the block copolymer)

[0186] In a Rietz cutter (HOSOKAWA MICRON CORPORATION, Rietz rubber cutter model PB15H), 35 kg of a ball-shaped molded body of a block copolymer was placed in the vertical direction, and the Rietz cutter was then started to rotate the screw. A peak current value was measured before the ball-shaped molded body was completely attacked in the vertical direction by the rotating screw of the Rietz cutter, and was used as an index of the loads when crushing the ball-shaped molded body.

[0187] In some cases, a current value greater than the upper limit was instantaneously generated at the start of a bullet attack when the Rietz cutter was turned on; however, the current was only an instantaneous phenomenon and therefore was not considered a peak current value.

[0188] ((9) Grinding time of the ball-shaped molded body of the block copolymer)

[0189] A 35 kg ball-shaped body was introduced vertically into the Rietz cutting device, then the ball-shaped molded body was sheared between a screw hammer and a fixed blade, and the resulting ground product was extruded through a diaphragm by the movement of the screw and was cut using a rotating knife. The time from the start of the initial setting of the ball-shaped molded body to the return to the current value before the setting of the next ball-shaped molded body, when the discharge of ground product through the diaphragm ceased, was defined as the grinding time of one ball.

[0190] The current value of the Rietz cutting device when no ball-shaped molded body was placed was 19 amperes.

[0191] [Polymerization of block copolymer and production of ball-shaped molded body]

[0192] [Example 1]

[0193] (Polymerization of block copolymer (SBR1) and molding into a ball shape)

[0194] A polymerization tank with a capacity of 100 1, equipped with a rotating stirring blade and a jacket, was charged with 79 parts by mass of 1,3-butadiene with 100 ppm of 1,2-butadiene and 600 parts by mass of a cyclohexane solution with 150 ppm of tetrahydrofuran (THF), 0.016 parts by mass of tetramethylethylenediamine (TMEDA) was added as an adjuvant of the 1,2-vinyl bond content, and the polymerization was carried out with the addition of 0.095 parts by mass of the polymerization initiator n-butyllithium under stirring at a polymerization initiation temperature of 43.2 °C. The maximum reaction temperature of 1,3-butadiene was 96.1 °C. One minute after the maximum reaction temperature was reached, 21 parts by mass of styrene were added. The reactor temperature at the time of styrene addition was 95.2 °C.

[0195] Then, 5 minutes after the maximum reaction temperature of styrene was reached, methanol in an amount in moles 0.8 times higher than that of the polymerization initiator n-butyllithium was added for quenching, terminating the polymerization reaction of a block copolymer (SBR1).

[0196] Then, 0.15% by mass of 2,4-bis(octylthiomethyl)-o-cresol relative to the mass of the block copolymer was added as a stabilizer.

[0197] Similarly, the polymerization was carried out four times, followed by methanol quenching and subsequent addition of the stabilizer, and the resulting four rubber-like block copolymer solutions were mixed.

[0198] Further, the resulting rubber-like block copolymer solution was placed in hot water with stirring, the solvent was removed by steam extraction with pure water, and then said solution was dried under vacuum to give a block copolymer in the form of flakes.

[0199] A 35 kg portion of the resulting flakes was taken and fed into a ball molding machine (mold for ball molding: 70 cm in length, 35 cm in width), yielding a ball molded body of the block copolymer (SBR1).

[0200] Table 1 shows the details of the polymerization of the block copolymer (SBR1), the physical properties of the block copolymer, the result of the adjustment of the hardness of the ball-shaped molded body and the grindability of the ball-shaped molded body.

[0201] [Examples 2, 3 and comparative examples 1, 2, 3]

[0202] Ball-shaped molded bodies of block copolymers (SBR2, SBR3, SBR13, SBR14, SBR15) were produced according to the same procedure as in Example 1, except that the polymerization initiation temperature was changed and the maximum reaction temperature of 1,3-butadiene and the temperature in the reactor when styrene was added were modified, particularly under the conditions shown as polymerization details in Tables 1 and 3.

[0203] The details of the polymerization of the block copolymers of Examples 2 and 3 and Comparative Examples 1, 2 and 3 (SBR2 and SBR3, and SBR13, SBR14 and SBR15), the physical properties of the block copolymers, the results of the adjustment of the hardness of the ball-shaped molded bodies and the grindability of the ball-shaped molded bodies are shown in Tables 1 and 3.

[0204] In the case of SBR15 (comparative example 3), the amount of ground product partially adhering to the Rietz cutting device after bale grinding was slightly higher than that of SBR2 and SBR3 (examples) and SBR13 and SBR14 (comparative examples).

[0205] [Example 4 and comparative example 4]

[0206] Ball-shaped molded bodies of the SBR4 and SBR16 block copolymers were produced according to the same procedure as in Example 1, except that the amount of tetramethylethylenediamine (TMEDA) to be added to adjust the 1,2-vinyl linkage content was increased.

[0207] The details of the polymerization of the SBR4 and SBR16 block copolymers (Example 4 and Comparative Example 4), the physical properties of the block copolymers, the results of the adjustment of the hardness of the ball-shaped molded bodies and the grindability of the ball-shaped molded bodies are shown in Tables 1 and 3.

[0208] [Examples 5, 6 and comparative example 5]

[0209] Ball-shaped molded bodies of a block copolymer having an aromatic vinyl monomer unit content of 16.2 mass% (SBR5), a block copolymer having an aromatic vinyl monomer unit content of 24.8 mass% (SBR6), and a block copolymer having an aromatic vinyl monomer unit content of 34.8 mass% (SBR17) were produced under the conditions shown as polymerization details in Tables 1 and 3. The physical properties of the block copolymers of Examples 5 and 6 and Comparative Example 5, the results of adjusting the hardness of the ball-shaped molded bodies, and the grindability of the ball-shaped molded bodies are shown in Tables 1 and 3.

[0210] It was found that Comparative Example 5 (SBR17) gave a ball-shaped molded body with a hardness of up to 78, which caused a peak current of 47 A during grinding, and thus a high load for the grinder.

[0211] [Examples 7, 8 and comparative example 6]

[0212] The polymerization was carried out under the conditions indicated as polymerization details in Tables 2 and 3, in which the styrene was added in a phase after the reaction of 1,3-butadiene exceeded 90 °C but before the reaction peak. The styrene was added at 90.3 °C for Example 7 (SBR7), at 95.2 °C for Example 8 (SBR8) and at 92.0°C for Comparative Example 6 (SBR18). The resulting proportions between the content of aromatic vinyl block fragment and the content of aromatic vinyl monomer units were 90.8% by mass, 90.5% by mass and 91.4% by mass, respectively.

[0213] In Comparative Example 6 (SBR18), the peak top molecular weight of the aromatic vinyl block fragment exceeded 30,000 due to the increase in molecular weight due to the decrease in the amount of catalyst to be added, and thus the ball-shaped molded body had a hardness above 80, which caused a high load during grinding, resulting in a deterioration in grindability.

[0214] [Comparative Example 7]

[0215] The polymerization was carried out under the conditions shown as polymerization details in Table 3, wherein, before the initiation of the polymerization, a polymerization tank was charged with 6.3 parts by mass of styrene with 79 parts by mass of 1,3-butadiene, and 14.7 parts by mass of the residual part of styrene was added after a maximum reaction temperature of 1,3-butadiene was reached. As a result, a block copolymer (SBR19) whose proportion between the content of the aromatic vinyl block fragment and the content of the aromatic vinyl monomer units was 73.1% by mass was obtained.

[0216] The hardness of the ball was only 42, which resulted in a low load when grinding the ball, while adhesion due to heat generation during grinding was found in the mill, as in the case of Comparative Example 3 (SBR15). In addition, it was found that the ball-shaped molded body was susceptible to deformation when another ball was stacked on it due to its low hardness.

[0217] [Example 9]

[0218] A ball-shaped molded body of a block copolymer (SBR9) was produced according to the same procedure as in Example 1, except that the amount of n-BuLi polymerization initiator to be added was increased.

[0219] The peak top molecular weight of the block copolymer was lower than that of Example 1 due to the increase in the amount of polymerization initiator, and the ball hardness was 49.

[0220] Table 2 shows the details of the polymerization of the block copolymer (SBR9), the physical properties of the block copolymer, the result of the adjustment of the hardness of the ball-shaped molded body and the grindability of the ball-shaped molded body.

[0221] [Example 10]

[0222] A ball-shaped molded body of a block copolymer (SBR10) was produced according to the same procedure as in Example 1, except that the amount of n-BuLi polymerization initiator to be added was decreased.

[0223] The peak top molecular weight of the block copolymer was higher than that of Example 1 due to the decrease in the amount of polymerization initiator, and the ball hardness was 69.

[0224] The details of the polymerization of the block copolymer (SBR10), the physical properties of the block copolymer, the result of the adjustment of the hardness of the ball-shaped molded body and the grindability of the ball-shaped molded body are shown in Table 2.

[0225] [Example 11]

[0226] A ball-shaped molded body of a block copolymer having a 1,2-vinyl bond content of 13.3 mass% (SBR11) was produced according to the same procedure as in Example 1, except that tetramethylethylenediamine (TMEDA) for adjusting the 1,2-vinyl bond content was not added and the amount of tetrahydrofuran (THF) to be added was increased. The details of the polymerization of the block copolymer (SBR11), the physical properties of the block copolymer, the result of adjusting the hardness of the ball-shaped molded body, and the grindability of the ball-shaped molded body are shown in Table 2.

[0227] [Example 12]

[0228] A ball-shaped molded body of a block copolymer having a 1,2-vinyl bond content of 31.2% (SBR12) was produced according to the same procedure as in Example 1, except that the amount of tetramethylethylenediamine (TMEDA) to be added to adjust the 1,2-vinyl bond content was increased.

[0229] The details of the polymerization of the block copolymer (SBR12), the physical properties of the block copolymer, the result of the adjustment of the hardness of the ball-shaped molded body and the grindability of the ball-shaped molded body are shown in Table 2. [Tables 1] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Conjugated diene - aromatic vinyl block copolymer SBR1 SBR2 SBR3 SBR4 SBR5 SBR6 Details of the polymerization of a Cyclohexane g 57000 57000 57000 57000 57000 57000 THF g 8.6 8.6 8.6 8.6 8.6 8.6 TMEDA g 1.5 1.5 1.5 4.6 1.5 1.5 1,3-butadiene block copolymer g 7500 7500 7500 7500 7970 7120 Polymerization initiation temperature °C 41.5 39.8 43.2 42.6 40.7 43.8 n-BuLi g 9.0 9.2 9.1 9.1 8.9 9.2 Maximum reaction temperature of 1,3-butadiene °c 96.1 92.5 97.9 96.4 94.3 97.8 Styrene g 2000 2000 2000 2000 1530 2380 Temperature in the reactor at the time of addition of styrene °c 95.2 91.3 97.0 95.4 93.1 96.8 Physical properties of the block copolymer (1) Content of aromatic vinyl monomer units % by mass 20.9 20.8 21.0 20.9 16.2 24.8 (2) Content of aromatic vinyl block fragments % by mass 20.7 20.6 20.8 20.1 16.0 24.3 Proportion of the content of aromatic vinyl block fragments to the content of aromatic vinyl monomer units ((2) / (1)) x 100 % by mass 98.9 99.0 99.0 96.2 98.8 98.0 Peak top molecular weight of the block copolymer x 100 00 13.5 13.1 13.4 13.2 14.0 12.8 Peak molecular weight of aromatic vinyl block fragment x 100 00 1.44 1.42 1.43 1.45 1.21 1.53 Weight average molecular weight of aromatic vinyl block fragment (Mw) x 100 00 1.31 1.28 1.29 1.29 1.12 1.41 Number average molecular weight of aromatic vinyl block fragment (Mn) x 100 00 1.09 1.09 1.04 1.11 0.92 1.18 Molecular weight distribution in aromatic vinyl block fragment (Mw / Mn) 1.20 1.17 1.24 1.16 1.22 1.20 1,2-Vinyl bond content % by mass 19.6 21.8 18.2 28.1 20.4 19.2 Viscosity of a solution in styrene at 5% by mass mPa.s 10.7 10.3 10.6 10.2 12.2 9.5 Characteristics of the molded body so Fit Dur nt of the du ty d rety to the ball - 58 65 59 68 54 70 us ball shape Suitability for Cutting crest grinding ration 1 ors d ampere 32 34 31 36 30 38 b ale grinding Second grinding time from 174 178 169 188 160 192 [Tables 2] Example 7 Example 8 Example 9 Example 10 Example 11 Example 12 Conjugated diene - aromatic vinyl block copolymer SBR 7 SBR 8 SBR 9 SBR 10 SBR 11 SBR 12 Details of the polymerization of a block copolymer Cyclohexane g 5700 0 5700 0 5700 0 5700 0 5700 0 5700 0 THF g 8.6 8.6 8.6 8.6 10 8.6 TMEDA g 1.5 1.5 1.5 1.5 0 5.0 1,3-butadiene g 7500 8450 7500 7500 7500 7500 Initiation temperature of polymerization °C 40.3 44.2 38.8 43.5 41.6 42.8 n-BuLi g 9.2 5.6 11.8 7.3 8.9 8.7 Maximum reaction temperature of 1,3-butadiene °C - - 97.5 97.9 97.3 98.3 Styrene g 2000 1050 2000 2000 2000 2000 0 Temperature in the reactor at the time of addition of styrene °C 90.3 95.2 96.5 97.0 96.4 97.2 Physical properties of (1) Content of aromatic vinyl monomer units % by mass 20.8 14.8 20.8 20.9 21.0 20.8 block copolymer (2) Content of block aromatic vinyl fragments % by mass 18.8 13.4 20.6 20.6 20.9 20.5 Ratio of block aromatic vinyl fragment content to aromatic vinyl monomer unit content ((2) / (1)) x 100 % by mass 90.8 90.5 99.0 98.6 99.5 98.6 Peak and peak molecular weight of block copolymer x 100 00 13.1 28.1 9.4 17.9 13.6 13.8 Peak and peak molecular weight of block aromatic vinyl fragment x 100 00 1.09 2.51 1.02 1.86 1.46 1.43 Weight average molecular weight of fragment aromatic vinyl block (Mw) x 100 00 1.02 2.33 0.93 1.73 1.34 1.33 Number average molecular weight of aromatic vinyl block fragment (Mn) x 100 00 0.88 1.93 0.81 1.43 1.11 1.12 Molecular weight distribution in aromatic vinyl block fragment (Mw / Mn) - 1.16 1.21 1.15 1.21 1.21 1.18 1,2-vinyl bond content % by mass 20.6 17.8 16.3 16.8 13.3 31.2 Viscosity of a solution in styrene at 5% by mass mPa.s 10.1 20.7 6.8 15.6 9.6 11.0 Characteristics of the body cast in the form of a ball Hardness adjustment Ball hardness - 58 71 49 69 57 68 Grinding suitability Peak current during ball grinding ampere 31 38 29 37 29 37 . Grinding time sec of 166 186 194 178 163 187 [Tables 3] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 Conjugated Diene - Vinyl Aromatic Block Copolymer SBR13 SBR14 SBR15 SBR16 SBR17 SBR18 SBR19 Details of the Polymerization of a Block Copolymer Cyclohexane g 57000 57000 57000 57000 57000 57000 57000 THF g 8.6 8.6 8.6 8.6 8.6 8.6 8.6 TMEDA g 1.5 1.5 1.5 7.5 1.5 1.5 1.5 1,3-Butadiene g 7500 7500 7500 7500 6175 7500 7500 Styrene 600 Polymerization initiation temperature °C 37.2 38.1 46.4 38.8 44.2 44.5 40.5 n-BuLi g 9.2 9.0 9.2 8.9 9.2 5.5 9.0 Maximum reaction temperature of 1,3-butadiene °C 88.7 79.3 108.8 93.8 94.8 - 94.3 Styrene g 2000 2000 2000 2000 3325 2000 1400 Temperature in the reactor at the time of styrene addition °C 86.3 77.5 107.2 92.6 93.9 92.0 93.2 Physical properties of copolymer (1) Content of aromatic vinyl monomer units % by mass 20.9 21.0 20.9 20.9 34.8 20.9 20.8 (2) Content of aromatic vinyl fragments block % in mass 20.5 20.8 20.6 20.2 34.3 19.1 15.2 , block copolymer Ratio of block aromatic vinyl fragment content to aromatic vinyl monomer unit content ((2) / (1)) x 100% by mass 98.1 99.0 98.6 96.7 98.6 91.4 73.1 Peak molecular weight of block copolymer x 10,000 13.0 13.2 13.1 13.6 12.1 30.3 13.4 Peak molecular weight of aromatic vinyl block fragment x 10,000 1.58 1.62 1.38 1.57 2.09 3.20 1.39 Weight average molecular weight of vinyl block fragment aromatic vinyl block fragment (Mw) x 10,000 1.41 1.44 1.31 1.43 1.93 2.97 1.29 Number average molecular weight of aromatic vinyl block fragment (Mn) x 10,000 1.25 1.34 0.93 1.30 1.62 2.43 1.03 Molecular weight distribution in aromatic vinyl block fragment (Mw / Mn) 1.13 1.07 1.41 1.10 1.19 1.22 1.25 1,2-Vinyl bond content % by mass 22.1 22.9 16.2 36.1 17.1 16.2 18.1 Viscosity of a 5% by mass solution in styrene mP a. s 10.3 10.3 10.1 9.8 9.6 25.2 10.1 Characteristics of the molded body in the form of a ball Hardness adjustment Ball hardness - 72 76 46 75 78 86 42 Grinding suitability Peak current during ball grinding ampere 43 46 28 44 47 50 27 Grinding time sec ond 213 235 208 228 213 223 202

[0230] Tables 1 to 3 show that the block copolymers SBR1 to SBR12 (Examples 1 to 12) allow optimum adjustment of the hardness of the ball-shaped molded bodies for grinding, and that the resulting ball-shaped molded bodies are satisfactory because they cause low loads (current values) during grinding and can be set up continuously, and because a short grinding time is required for a ball-shaped molded body.

[0231] [Characteristics of the impact-resistant aromatic vinyl resin composition]

[0232] As shown below in [Examples 13 to 19] and [Comparative Examples 8 and 9], impact-resistant aromatic vinyl resin compositions were produced, and the characteristics shown below were determined and evaluated.

[0233] <Taille moyenne des particules des particules de caoutchouc>

[0234] An impact-resistant aromatic vinyl resin composition was dissolved in dimethylformamide to dissolve only a polystyrene-based resin fragment forming the matrix of the resin composition, and a portion of the solution was dispersed in a liquid of the dimethylformamide solvent in a measuring cell of the particle size distribution analyzer (laser diffraction / diffusion), model LA-920, manufactured by HORIBA, Ltd. for measurement, and the acquired volume average particle size was defined as the rubber particle size.

[0235] <brillance>

[0236] Gloss was measured in accordance with JIS Z8742 (angle of incidence: 60°).

[0237] <Résistance aux chocs>

[0238] Izod impact resistance was measured in accordance with JIS K7110 (notched).

[0239] [Examples 13 to 19]

[0240] In a nitrogen-purged stirred-type polymerization tank, 20 parts by mass of ethylbenzene and 12 parts by mass of a block copolymer (shown in Table 4) were dissolved in 100 parts by mass of a monomer mixture having a styrene content of 75% by mass and an acrylonitrile content of 25% by mass; 0.15 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl) propionate and 200 ppm by mass of 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane relative to 100 parts by mass of the monomer mixture and 1500 ppm by mass of t-dodecyl mercaptan relative to 100 parts by mass of the monomer mixture were also added;the polymerization was continued under stirring at 150 rpm and 100°C for 7 hours, then under stirring at 15 rpm at successively increased temperatures, in particular at 120°C for 1 hour, at 135°C for 2 hours, at 150°C for 2 hours and at 170°C for 2 hours, and finally a heat treatment was carried out at 230°C for 30 minutes; then, the pressure in the polymerization tank was returned to atmospheric pressure, and an impact-resistant aromatic vinyl resin composition was taken during heating as a polymerization product and cooled in pure water. ;

[0241] To remove unreacted styrene, acrylonitrile and ethylbenzene, 1000 ml of dichloromethane was added per 100 g of polymerization product after cooling, and the polymerization product was dissolved by stirring.

[0242] The solution was added dropwise into isopropyl alcohol in a volume 10 times greater than that of the solution for reprecipitation.

[0243] The precipitated impact-resistant aromatic vinyl resin composition was vacuum dried to obtain an impact-resistant aromatic vinyl resin composition (ABS resin composition).

[0244] This was hot pressed at 200°C, then cooled and then ground into 5 mm0, the ground product was injection molded and the physical properties of the ABS resin composition were measured.

[0245] Table 4 shows the measurement results.

[0246] [Comparative Example 8, Comparative Example 9]

[0247] ABS test samples were produced in the same manner as in Example 13 with the block copolymers SBR14 and SBR15.

[0248] The results of the physical property measurements are shown in Table 4. [Tables 4] Example 13 Example 14 Example 15 Example 16 Example 17 Example 18 Example 19 Comparative Example 8 Comparative Example 9 Block copolymer used SBR 1 SBR 3 SBR 5 SBR 6 SBR 7 SBR 8 SBR 9 SBR1 4 SBR 15 Physical properties of ABS resin composition average particle size of rubber particles UC pm 0.46 0.45 0.45 0.42 0.46 0.48 0.41 0.44 0.47 Gloss % 94 94 95 95 93 90 94 94 91 Impact resistance s kg.cm / cm 9.1 9.3 9 9.4 8.9 8.9 9.2 9.3 8.2

[0249] With reference to Table 4, the comparison of the physical properties of the ABS resin compositions with block copolymers (SBR) differing in terms of molecular weight distribution (Mw / Mn) in the vinyl aromatic block moiety of the block copolymer revealed that the physical properties of the ABS resin composition with SBR1 of Example 13 where Mw / Mn = 1.20 and those of the ABS resin composition with SBR14 of Comparative Example 8 where Mw / Mn = 1.07 were comparable and satisfactory, and that the ABS with SBR15 of Comparative Example 9 where Mw / Mn = 1.41 exhibited poor impact resistance. Industrial application

[0250] The ball-shaped molded body of the block copolymer of the present embodiment has industrial application as a modifier for styrene-based resins.< / brillance>

Claims

Claims

1. A ball-shaped molded body of a block copolymer comprising an aromatic vinyl monomer unit and a conjugated diene monomer unit, the block copolymer comprising an aromatic vinyl block moiety, and the block copolymer satisfying the<condition (a)> has<condition (d)> following:<Condition (a)> the block copolymer has a content of aromatic vinyl monomer units of 10 to 30% by mass;<Condition (b)> a proportion between the aromatic vinyl block fragment and a total content of aromatic vinyl monomer units is 90 to 100% by mass;<Condition (c)> the aromatic vinyl block fragment has a peak molecular weight of 10,000 to 30,000; and<Condition (d)> a ratio of the weight average molecular weight, Mw, to the number average molecular weight, Mn, in the vinyl aromatic block fragment (Mw / Mn) is between 1.15 and 1.

40.

2. A ball-shaped molded body according to claim 1, wherein a 5% by mass styrene solution of the block copolymer has a viscosity of 7 to 15 mPa-s under a temperature condition of 25°C.

3. The ball-shaped molded body according to claim 1, wherein the block copolymer has a 1,2-vinyl bond content of 15 to 30 mol% in the conjugated diene monomer unit.

4. A ball-shaped molded body according to claim 1, having a hardness of 50 to 72 measured using a type E durometer according to JIS K6253.

5. A block copolymer comprising an aromatic vinyl monomer unit and a conjugated diene monomer unit, the block copolymer comprising an aromatic vinyl block moiety, and the block copolymer satisfying the<condition (a)> has<condition (d)> following:<Condition (a)> the block copolymer has a content of aromatic vinyl monomer units of 10 to 30% by mass;<Condition (b)> a proportion between the aromatic vinyl block fragment and a total content of aromatic vinyl monomer units is 90 to 100% by mass;<Condition (c)> the aromatic vinyl block fragment has a peak molecular weight of 10,000 to 30,000; and<Condition (d)> a ratio of the weight average molecular weight, Mw, to the number average molecular weight, Mn, in the vinyl aromatic block fragment (Mw / Mn) is between 1.15 and 1.

40.

6. A block copolymer according to claim 5, wherein a 5% by mass styrene solution of the block copolymer has a viscosity of 7 to 15 mPas under a temperature condition of 25 or

7. The block copolymer of claim 5, the block copolymer having a 1,2-vinyl bond content of 15 to 30 mol% in the conjugated diene monomer unit.

8. A resin composition resulting from the polymerization of: 3 to 20 parts by mass of the block copolymer which constitutes the ball-shaped molded body according to any one of claims 1 to 4, and 97 to 80 parts by mass of a styrene-based resin.

9. The resin composition of claim 8, wherein the styrene-based resin is a copolymer of a styrene-based compound and acrylonitrile.

10. A method of producing the block copolymer which constitutes the ball-shaped molded body according to any one of claims 1 to 4, the method comprising the steps of: supplying a conjugated diene compound to a reactor to polymerize the conjugated diene compound so as to reach a peak temperature of 91 to 100°C; and

11.

12.

13. supply and polymerize an aromatic vinyl compound while maintaining a temperature of 90 to 100°C in the reactor. Resin composition resulting from the polymerization of: 3 to 20 parts by mass of the block copolymer according to any one of claims 5 to 7; and 97 to 80 parts by mass of a styrene-based resin. The resin composition of claim 11, wherein the styrene-based resin is a copolymer of a styrene-based compound and acrylonitrile. A process for producing the block copolymer according to any one of claims 5 to 7, the process comprising the steps of: providing a conjugated diene compound into a reactor to polymerize the conjugated diene compound to reach a peak temperature of 91 to 100°C; and supply and polymerize an aromatic vinyl compound while maintaining a temperature of 90 to 100°C in the reactor.