Assembly method using friction stir welding, sacrificial shim and welding plate equipped with a sacrificial shim
The use of sacrificial wedges in friction stir welding prevents surface defects on the elements by guiding the welding tool through the wedges, enabling rapid and automated assembly with improved visual quality.
Patent Information
- Application Number
- FR2023002919
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-28
AI Technical Summary
Friction stir welding generates surface defects at both ends of the weld bead, which are prone to fracture and corrosion, requiring tedious manual correction that degrades the visual appearance of the assembled parts.
A method involving the use of sacrificial wedges positioned on the elements to be assembled, guiding a friction stir welding tool to penetrate and withdraw through these wedges, thereby forming surface defects only on the wedges rather than the elements, and optionally using a robotic arm for automation.
Rapidly forms a weld bead without surface defects on the elements, maintaining the visual appearance and allowing for automated assembly.
Smart Images

Figure 00000012_0000 
Figure 00000012_0001 
Figure 00000012_0002
Abstract
Description
Title of the invention: Friction stir welding assembly method, sacrificial wedge and welding plate provided with a sacrificial wedge Technical field
[0001] The technical field of the invention is friction stir welding assembly processes, also called “friction stir welding” in English terms.
[0002] In particular, the present invention relates to a method of assembling a first element with a second element, a sacrificial wedge for producing a friction stir weld bead and a welding plate comprising such a sacrificial wedge. Previous techniques
[0003] In industry, particularly in the aeronautical industry, it is common to assemble several elements together. It is, for example, known to assemble a stiffener on a structural panel of an aircraft in order to stiffen the structural panel.
[0004] This assembly can be carried out by friction stir welding using a tool equipped with a rotating pin adapted to knead together the materials of the elements to be assembled and thus form a weld bead between the elements.
[0005] However, friction stir welding causes surface defects at both ends of the weld bead, when the pin penetrates the material and / or withdraws from the material. These surface defects are prime locations for the initiation of fracture and / or for corrosion.
[0006] It is known to manually correct these surface defects, in particular by piercing the material at the two ends of the weld bead and then filling the holes thus pierced, in particular by using a rivet. Manually correcting these surface defects is a tedious operation. In addition, manually correcting these surface defects degrades the visual appearance of the part. Statement of the invention
[0007] The present invention therefore aims to overcome all or part of the aforementioned drawbacks and to propose a rapid assembly method reducing the appearance of surface defects.
[0008] The present invention relates to a method for assembling a first element with a second element comprising a step of positioning a sacrificial wedge against a surface of the first element, a step of producing a weld bead by friction stir welding of the first element with the second element, the step of producing the bead comprising guiding a tool provided with a pin of welding such that the pin penetrates the sacrificial wedge and then passes through the surface of the first member and / or passes through the surface of the first member and then withdraws from the sacrificial wedge, as well as a step of removing the sacrificial wedge.
[0009] Thus, a surface defect forms on the sacrificial wedge when the pin penetrates the sacrificial wedge and / or withdraws from the sacrificial wedge, the pin not forming the surface defect on the first element and / or on the second element.
[0010] Optionally, the positioning of the sacrificial shim comprises gluing and / or welding the shim to the first element and / or to the second element.
[0011] Advantageously, the assembly method comprises guiding the tool so that the pin is in contact only with the first element and the sacrificial wedge when the pin passes through the surface of the first element. Thus, the sacrificial wedge is not welded to the second element.
[0012] Optionally, the method comprises a step of sanding the surface of the first element and a step of applying mastic to a periphery of a contact surface between the first element and the second element.
[0013] Advantageously, the guiding of the tool comprises the use of a robotic arm programmed to guide the tool.
[0014] In one embodiment, the assembly method comprises the use of a sacrificial wedge provided with a cell, the step of positioning the wedge comprising the positioning of the cell opposite the surface of the first element, the guiding of the tool being carried out so that the pin penetrates the sacrificial wedge, is guided through the cell and then passes through the surface of the first element and / or so that the pin passes through the surface of the first element, is guided through the cell and then withdraws from the sacrificial wedge.
[0015] Optionally, the assembly method comprises the use of a sacrificial wedge provided with a wall forming a slope, the guiding of the tool being carried out so that the trajectory of the tool follows the slope of the sacrificial wedge when the pin crosses the surface of the first element.
[0016] Optionally, the assembly method comprises using a sacrificial shim bonded to the first element, a primer being formed in the bond of the sacrificial shim to the first element.
[0017] The present invention also relates to a sacrificial wedge for producing a weld bead by friction stir welding suitable for implementing an assembly method as defined above.
[0018] The present invention also relates to a welding plate comprising a first element intended to be assembled with a second element by implementing an assembly method as defined previously, the plate comprising a sacrificial shim bonded to a surface of the first element, a primer being formed in the connection of the sacrificial wedge to the first element. Brief description of the drawings
[0019] Other aims, characteristics and advantages of the invention will appear on reading the following description, given solely by way of non-limiting example and made with reference to the appended drawings in which:
[0020] [Fig-1] schematically illustrates an assembly method according to the invention;
[0021] [Fig.2] schematically illustrates the assembly of a first element with a second element according to a first embodiment of the invention;
[0022] [Fig.3] schematically illustrates the assembly of the first element with the second element according to a second embodiment of the invention;
[0023] [Fig.4] schematically illustrates the assembly of the first element with the second element according to a third embodiment of the invention;
[0024] [Fig.5] schematically illustrates the assembly of the first element with the second element according to a fourth embodiment of the invention;
[0025] [Fig.6] schematically illustrates a welding plate according to the invention arranged on the second element in perspective; and
[0026] [Fig.7] schematically illustrates a profile view of [Fig.6]. Detailed description
[0027] [Fig. 1] schematically represents the steps allowing the implementation of a method of assembling a first element 2 with a second element 4, for example the assembly of a stiffener on a structural panel of an aircraft.
[0028] The first element 2 comprises, for example, an aluminum alloy or any other alloy that can be welded by friction stir.
[0029] The second element 4 comprises, for example, an aluminum alloy or any other alloy that can be welded by friction stir.
[0030] [Fig. 2] schematically represents the assembly of the first element 2 with the second element 4, the first element 2 being arranged on the second element 4 so that the first element 2 covers the second element 4 on a contact surface 6.
[0031] Firstly, a step 8 is carried out for positioning at least one sacrificial wedge against the first element 2. For example, an input sacrificial wedge 10 is positioned against an input surface 12 of the first element 2 and an output sacrificial wedge 14 against an output surface 16 of the first element 2.
[0032] Advantageously, the sacrificial inlet wedge 10 is arranged on the second element 4 and comes to bear against the inlet surface 12 of the first element 2, the sacrificial outlet wedge 14 being arranged on the second element 4 and coming to bear against the outlet surface 16 of the first element 2.
[0033] In one embodiment, at least one of the sacrificial input or output shims 10, 14 is bonded to the first element 2 and / or to the second element 4, in particular by using a temporary adhesive 17a intended to be removed at the end of the assembly process. Alternatively, at least one of the sacrificial input or output shims 10, 14 is welded to the first element 2 and / or to the second element 4, in particular by producing a weld point 17b intended to be removed at the end of the assembly process.
[0034] A weld bead 20 is then produced by friction stir welding of the first element 2 with the second element using a friction stir welding tool 22 (step 18).
[0035] The tool 22 comprises, for example, a tubular portion 24 and a pin 26, in particular a rotary pin and adapted to knead together the materials of the first and second elements 2, 4 to be assembled, the pin 26 extending the tubular portion 24 so that the tubular portion 24 forms a shoulder 28. The length of the pin 26, taken along the longitudinal direction of the tubular portion 24, is adapted to the thickness of the first element 2. In particular, the length of the pin 26 is greater than the thickness of the first element 2 in order to allow the assembly by friction kneading of the first element 2 on the second element 4. Several positions of the tool 22 during the step 18 of producing the weld bead 20 are shown.
[0036] When producing the weld bead 20, the pin 26 gradually penetrates the sacrificial entry wedge 10 in the direction of the second element 4 and the first element 2, then crosses the entry surface 12 of the first element 2, here a lateral entry surface of the first element 2.
[0037] In the example shown, the inlet sacrificial wedge 10 is of the same thickness as the first element 2, the pin 26 of the tool 22 penetrating the inlet sacrificial wedge 10 until the shoulder 28 of the tool 22 is in contact with a flat upper surface 30 of the inlet sacrificial wedge 10. The tool 22 is then translated along a trajectory for producing the weld bead 20 through the inlet surface 12 of the first element 2, here in the direction of the outlet sacrificial wedge 14. The shoulder 28 of the tool 22 being here in contact with the inlet sacrificial wedge 10 before crossing the inlet surface 12 of the first element 2, the weld bead 20 is formed at the interface between the first element 2 and the second element 4 up to the surface input 12 of the first element 2.
[0038] The shoulder 28 of the tool 22 then travels over an upper surface 32 of the first element 2 towards the sacrificial outlet wedge 14 in order to continue the formation of the weld bead 20 at the interface between the first element 2 and the second element 4.
[0039] The tool 22 does not directly penetrate the upper surface 32 of the first element 2, no surface defect is formed on the upper surface 32 of the first element 2.
[0040] Alternatively, the pin 26 of the tool 22 penetrates the sacrificial entry wedge 10 so that the pin 26 is only in contact with the first element 2 and the sacrificial wedge when the pin 26 passes through the entry surface 12 of the first element 2. Since the pin 26 is not in contact with the second element 4 when the pin 26 passes through the entry surface 12 of the first element 2, the weld bead 20 is not formed at the interface between the first element 2 and the second element 4 up to the entry surface 12 of the first element 2, the sacrificial entry wedge 10 then not being welded with the second element 4.
[0041] Advantageously, when producing the weld bead 20 (step 18), a programmed robotic arm (not shown) is used to guide the tool 22 provided with the pin 26. Thus, the assembly process is rapid and automated. At least one of the sacrificial input and output wedges 10, 14 comprises, for example, markings to facilitate the guidance of the robotic arm.
[0042] Preferably, at least one of the sacrificial input and output shims 10, 14 comprises an aluminum alloy or any other alloy constituting the first element 2 or the second element 4, in particular in order to facilitate friction stir welding.
[0043] The guiding of the tool 22 continues until the pin 26 passes through the exit surface 16 of the first element 2, here a lateral exit surface of the first element 2. The tool 22 then gradually withdraws from the sacrificial exit wedge 14 so that the pin 26 of the tool 22 moves away from the second element 4 and from the first element 2. The shoulder 28 of the tool 22 being in contact with the sacrificial exit wedge 14 after having passed through the exit surface 16 of the first element 2, the weld bead 20 is formed at the interface between the first element 2 and the second element 4 up to the exit surface 16. The weld bead 20 is here formed at the interface between the first element 2 and the second element 4 from the entry surface 12 to the exit surface 16.
[0044] Alternatively, the shoulder 28 of the tool 22 breaks contact with the first element 2 before the pin 26 of the tool 22 passes through the exit surface 16 so that the pin 26 is only in contact with the first element 2 and the sacrificial exit wedge 14 when the pin 26 passes through the exit surface 16. Thus the weld bead 20 is not formed at the interface between the first element 2 and the second element 4 up to the exit surface 16 of the first element 2, the sacrificial exit wedge 14 then not being welded with the second element 4.
[0045] Since the tool 22 is not directly removed from the upper surface 32 of the first element 2, no surface defect is formed on the upper surface 32 of the first element 2.
[0046] The sacrificial shim is so named because the surface defects 34 are formed in the sacrificial shim and not in the first and second elements 2, 4.
[0047] Alternatively, a single sacrificial wedge is used, with the pin 26 of the tool 22 penetrating the single sacrificial wedge and withdrawing from the single sacrificial wedge such that both ends of the weld bead 20 are formed in the single sacrificial wedge.
[0048] Finally, a step 36 is carried out for removing the sacrificial input wedge 10 and the sacrificial output wedge 14.
[0049] Optionally, following the removal step 36, a sanding step 38 of the entry surface 12 of the first element 2 and of the entry surface 12 of the first element 2 is carried out.
[0050] Advantageously, a step of applying mastic 40 is finally carried out on a periphery of the contact surface 6 between the first element 2 and the second element 4 in order to guarantee the sealing of the assembly of the first element 2 with the second element 4.
[0051] [Fig. 3] schematically represents the use of an inlet sacrificial wedge 10 provided with a cell 42 and an outlet sacrificial wedge 14 provided with a cell 42.
[0052] Step 8 of positioning the wedge comprises positioning the cell 42 of the sacrificial input wedge 10 opposite the input surface 12 of the first element 2 and positioning the cell 42 of the sacrificial output wedge 14 opposite the output surface 16 of the second element 4.
[0053] The guiding of the tool 22 is carried out so that the pin 26 of the tool 22 penetrates the sacrificial entry wedge 10, is guided through the cell 42 of the sacrificial entry wedge 10 and then passes through the entry surface 12 of the first element 2. Then, the shoulder 28 of the tool 22 travels on the upper surface 32 of the first element 2, then the pin 26 of the tool 22 passes through the exit surface 16 of the first element 2, is guided through the cell 42 of the sacrificial exit wedge 14 and then withdraws from the sacrificial exit wedge 14.
[0054] The cell 42 of the input sacrificial wedge 10 makes it possible not to weld the input sacrificial wedge 10 to the first element 2 during the step 18 of producing the weld bead 20. The cell 42 of the output sacrificial wedge 14 makes it possible not to weld the output sacrificial wedge 14 to the first element 2 during the step 18 of producing the weld bead 20.
[0055] [Fig.4] schematically represents the use of an inlet sacrificial wedge 10 provided with an upper wall forming a slope 44 with respect to the flat upper surface 32 of the first element 2. The outlet sacrificial wedge 14 is also provided with an upper wall forming a slope 44 with respect to the flat upper surface 32 of the first element 2.
[0056] Step 8 of positioning the shim comprises positioning the inlet sacrificial shim 10 such that the thickness of the inlet sacrificial shim 10 increases away from the inlet surface 12, as well as positioning the outlet sacrificial shim 14 such that the thickness of the outlet sacrificial shim 14 increases away from the outlet surface 16.
[0057] The guiding of the tool 22 is carried out so that the tool 22 follows the slope 44 of the sacrificial entry wedge 10 when the pin 26 passes through the entry surface 12 of the first element 2, the shoulder 28 of the tool 22 bearing against the slope 44 of the sacrificial entry wedge 10.
[0058] The guiding of the tool 22 is carried out so that the tool 22 follows the slope 44 of the sacrificial output wedge 14 when the pin 26 passes through the output surface 16 of the first element 2, the shoulder 28 of the tool 22 bearing against the slope 44 of the sacrificial output wedge 14.
[0059] The slope 44 of the sacrificial entry wedge 10 makes it possible, together with the height of the pin 26 of the tool 22, to determine the positioning of the weld bead 20 on the side of the entry surface 12 at the interface between the first element 2 and the second element 4 and optionally not to weld the sacrificial entry wedge 10 to the first element 2 during the step 18 of producing the weld bead 20.
[0060] The slope 44 of the sacrificial output wedge 14 makes it possible, together with the height of the pin 26 of the tool 22, to determine the positioning of the weld bead 20 on the side of the output surface 16 at the interface between the first element 2 and the second element 4 and optionally not to weld the sacrificial output wedge 14 to the first element 2 during the step 18 of producing the weld bead 20.
[0061] [Fig. 5] schematically represents an alternative embodiment of the sacrificial inlet and outlet wedges 10, 14 of [Fig. 4]. The sacrificial inlet wedge 10 here comprises an angular portion 46 configured to match the inlet surface 12 of the first element 2, the inlet surface 12 here being constituted by the lateral inlet surface of the first element 2 and a portion of the upper surface 32 of the first element 2. The sacrificial outlet wedge 14 here comprises an angular portion 46 configured to match the outlet surface 16 of the first element 2, the outlet surface 16 here being constituted by the lateral outlet surface of the first element 2 and a portion of the upper surface 32 of the first element 2.
[0062] Step 8 of positioning the wedge comprises positioning the sacrificial inlet wedge 10 so that the angular portion 46 of the sacrificial inlet wedge 10 matches the inlet surface 12 of the first element 2, the slope 44 of the sacrificial inlet wedge 10 extending the upper surface 32 of the first element 2 so that the thickness of the sacrificial inlet shim 10 increases away from the inlet surface 12.
[0063] Step 8 of positioning the shim also comprises positioning the sacrificial outlet shim 14 so that the angular portion 46 of the sacrificial outlet shim 14 matches the outlet surface 16 of the first element 2, the slope 44 of the sacrificial outlet shim 14 extending the upper surface 32 of the first element 2 so that the thickness of the sacrificial outlet shim 14 increases away from the outlet surface 16.
[0064] The angular portion 46 of the sacrificial inlet wedge 10 comprises a first wall intended to come into contact with the inlet side wall of the first element 2 and a second wall intended to come into contact with the upper surface 32 of the first element 2. The angular portion 46 of the sacrificial outlet wedge 14 comprises a first wall intended to come into contact with the outlet side wall of the first element 2 and a second wall intended to come into contact with the upper surface 32 of the first element 2.
[0065] Advantageously, the thickness of the sacrificial inlet wedge 10, taken in the extension of the first wall of the angular portion 46 of the sacrificial inlet wedge 10, between the second wall of the angular portion 46 of the sacrificial inlet wedge 10 and the surface of the wall forming a slope 44 of the sacrificial inlet wedge 10, is greater than the height of the pin 26 of the tool 22. Thus, when the angular portion 46 of the sacrificial inlet wedge 10 matches the inlet surface 12, guiding the tool 22 so that the shoulder 28 of the tool 22 travels on the slope 44 of the sacrificial inlet wedge 10 makes it possible to guarantee that the pin 26 of the tool 22 is in contact only with the sacrificial inlet wedge 10 and the first element 2 when the pin 26 of the tool 22 passes through the entry surface 12, and therefore to guarantee that the sacrificial entry wedge 10 is not welded with the second element 4.
[0066] Advantageously, the thickness of the sacrificial output wedge 14, taken in the extension of the first wall of the angular portion 46 of the sacrificial output wedge 14, between the second wall of the angular portion 46 of the sacrificial output wedge 14 and the surface of the slope 44 of the sacrificial output wedge 14, is greater than the height of the pin 26 of the tool 22. Thus, when the angular portion 46 of the sacrificial output wedge 14 matches the output surface 16, guiding the tool 22 so that the shoulder 28 of the tool 22 travels on the slope 44 of the sacrificial output wedge 14 makes it possible to guarantee that the pin 26 of the tool 22 is in contact only with the sacrificial output wedge 14 and the first element 2 when the pin 26 of the tool 22 passes through the output surface 16, and thus to ensure that the sacrificial output wedge 14 is not welded with the second element 4.
[0067] [Fig.6] schematically represents a welding plate 48 arranged on the second element 4, for example a structural panel of an aircraft.
[0068] The welding plate 48 comprises the first element 2, for example a stiffener, as well as an input sacrificial wedge 10 linked to the first element 2 and an output sacrificial wedge 14 linked to the first element 2.
[0069] [Fig.7] schematically illustrates the connection of the sacrificial output wedge 14 with the first element 2. The sacrificial output wedge 14 is made of the same material as the first element 2, a primer 50 being formed in the connection of the sacrificial output wedge 14 to the first element 2.
[0070] Step 8 of positioning the sacrificial wedge 10, 14 is done naturally when positioning the first element 2 on the second element 4.
[0071] The primer 50 makes it possible to facilitate the step 36 of removing the sacrificial wedge 10, 14, in particular by making it possible to bend the welding plate 48 at the level of the initiated connection between the first element 2 and the sacrificial wedge 10, 14.
Claims
Claims
1. Method for assembling a first element (2) with a second element (4), characterized in that it comprises a step of positioning (8) a sacrificial wedge (10, 14) against a surface (12, 16) of the first element (2), a step of producing (18) a weld bead (20) by friction stir welding of the first element (2) with the second element (4), the step of producing (18) the bead (20) comprising guiding a tool (22) provided with a welding pin (26) so that the pin (26) penetrates the sacrificial wedge (10, 14) then passes through the surface (12, 16) of the first element (2) and / or passes through the surface (12, 16) of the first element (2) then withdraws from the sacrificial wedge (10, 14), as well as a step of removing (36) the sacrificial wedge (10, 14).
2. An assembly method according to claim 1, wherein the positioning of the sacrificial shim (10, 14) comprises gluing and / or welding the shim to the first element (2) and / or to the second element (4).
3. Assembly method according to one of claims 1 and 2, comprising guiding the tool (22) so that the pin (26) is in contact only with the first element (2) and the sacrificial wedge (10, 14) when the pin (26) passes through the surface (12, 16) of the first element (2).
4. Assembly method according to any one of claims 1 to 3, comprising a step of sanding (38) the surface (12, 16) of the first element (2) and a step of applying mastic (40) on a periphery of a contact surface (6) between the first element (2) and the second element (4).
5. An assembly method according to any one of claims 1 to 4, wherein guiding the tool (22) comprises using a robotic arm programmed to guide the tool (22).
6. An assembly method according to any one of claims 1 to 5, comprising the use of a sacrificial wedge (10, 14) provided with a cell (42), the step (8) of positioning the wedge comprising the positioning of the cell (42) opposite the surface (12, 16) of the first element (2), the guiding of the tool (22) being carried out so that the pin (26) penetrates the sacrificial wedge (10, 14), is guided through the cell (42) and then passes through the surface (12, 16) of the first element (2) and / or so that the pin (26) passes through the surface (12, 16) of the first element (2) element (2), is guided through the cell (42) then withdraws from the sacrificial wedge (10, 14).
7. Assembly method according to any one of claims 1 to 6, comprising the use of a sacrificial wedge (10, 14) provided with a wall forming a slope (44), the guiding of the tool (22) being carried out so that the trajectory of the tool (22) follows the slope (44) of the sacrificial wedge (10, 14) when the pin (26) crosses the surface (12, 16) of the first element (2).
8. An assembly method according to any one of claims 1 to 7, comprising the use of a sacrificial shim (10, 14) bonded to the first element (2), a primer being formed in the bond of the sacrificial shim (10, 14) to the first element (2).
9. Welding plate (48) comprising a first element (2) intended to be assembled with a second element (4) by implementing an assembly method according to any one of claims 1 to 8, the plate (48) comprising a sacrificial shim (10, 14) bonded to a surface (12, 16) of the first element (2), a primer (50) being formed in the bond of the sacrificial shim (10, 14) to the first element (2).
Citation Information
Patent Citations
Joint method
JP2016215267A
Method of joining together two planar members by friction stir welding, and tab plate used in the same method
US20040084506A1
Joining method and joining tool
US20120181324A1
Friction-stir welded structure
US20150175207A1
Repair of Pipeline Welds Using Friction Stir Processing
US20180221984A1