Waterproof fastener stringer and method of producing the same

Plasma treatment of the tape surfaces in the manufacturing process of waterproof fastener tapes enhances adhesion energy, addressing adhesion challenges and improving tape durability by creating hydrophilic functional groups and surface roughness, thus preventing element-turn.

GB2614648BActive Publication Date: 2024-11-06YKK CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
GB2023005354
Authority / Receiving Office
GB · GB
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-22
Filing Date
2020-10-22
Publication Date
2024-11-06
Estimated Expiration
2040-10-22

AI Technical Summary

Technical Problem

Existing methods for manufacturing waterproof fastener tapes face challenges in achieving strong adhesion between the waterproof layer and fastener elements, leading to issues like element-turn and reduced durability due to inadequate surface modification and roughness.

Method used

A process involving plasma treatment of the tape base fabric and fastener tape surfaces to create hydrophilic functional groups and surface roughness, followed by extrusion and injection molding to form a waterproof layer and attach fastener elements, enhancing adhesion energy and preventing element-turn.

Benefits of technology

The process significantly increases the adhesion energy between the fastener elements and the waterproof layer, reducing element-turn and improving the durability and performance of the waterproof fastener tapes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000001_0000
    Figure 00000001_0000
  • Figure 00000002_0000
    Figure 00000002_0000
  • Figure 00000003_0000
    Figure 00000003_0000
Patent Text Reader

Abstract

A penetration hole (9) penetrating a fastener tape (21, 31), in which a tape ground fabric (25) is coated with a waterproof layer (26), is formed at a constant pitch along a lateral edge part (23, 33) of the fastener tape (21, 31). On one side or both sides of the fastener tape (21, 31), the lateral edge part (23, 33) of the fastener tape (21, 31) is subjected to plasma treatment or corona treatment to form an activating region on a surface of the waterproof layer (26). A fastener element (29, 39) is injection molded to be attached to the lateral edge part (23, 33) of the fastener tape (21, 31). A molten resin that turns into the fastener element (29, 39) after curing adheres to the activating region and fills in the penetration hole (9).
Need to check novelty before this filing date? Find Prior Art

Description

[0039] The extrusion (S101) may be performed for example by using an extruder shown in Fig. 5. Specifically, a tape base fabric 25 and a melted or softened material 26’, which will solidify into the waterproof layer 26, are supplied to an extruder mold 111, and the sides of the tape base fabric 25 is coated by the melted or softened material 26’ which in turn solidify into the waterproof layer 26 on the sides of the tape base fabric 25.

[0040] The extruder mold 111 has a conveyance channel for the tape base fabric 25 conveyed from the upstream side to the downstream side, and a supply channel for supplying the melted or softened material 26’ to the both upper and lower surfaces of the tape base fabric 25 while being conveyed through the conveyance channel. The tape base fabric 25 is inserted into the conveyance channel of the extrusion mold 111 and moves from the upstream side to the downstream side through the conveyance channel. The supply channel of the extruder mold 111 is filled by the melted or softened material 26’ with high temperature and high pressure supplied from a feeder such as a screw. In such a manner, the melted or softened material 26’ is coated to be a layer on the upper and bottom surfaces of the tape base fabric 25. Viscosity and supply pressure of the melted or softened material 26’ would be adjusted appropriately for formation of layer with a target thickness. The melted or softened material 26’ is cooled (e.g. in air or in liquid) and solidified, and then adheres to the tape base fabric 25 as the waterproof layer 26. Note that, a conveyance system for the tape base fabric 25 such as grippers, rolls and so on may be employed, not illustrated in Fig. 5 though.

[0041] Prior to the extrusion, a plasma treatment is applied to one or both of the upper and lower surfaces of the tape base fabric 25. This enables the modification of surface of the side-edge portion of the tape base fabric 25, facilitating adhesion of the melted or softened material 26’ to the surface of the tape base fabric 25. Preferably, a region positioned between the left and right side-edges (e.g. a region positioned away from one side-edge by a predetermined distance (e.g. 5mm to 15 mm)), which extends along the elongation direction of the tape base fabric 25, is subjected to the 02 07 24 plasma treatment. Note that, the plasma treatment is a surface treatment based on discharge phenomenon. Plasma (plasma beam), where negatively charged electrons and positively charged cations fly around in space, is irradiated in the plasma treatment. Electrons emitted from electrode and associated negative ions are irradiated in corona treatment.

[0042] In Fig. 5, plasma emitters 121 and 122 are arranged at both upper and lower sides of the tape base fabric 25 in the upstream position of the extruder mold 111. The plasma emitter 121,122 emits a plasma generated by non-illustrated (common or separate) plasma source(s) to the surface of the side-edge portion of the tape base fabric 25. Typically, the plasma source has a gas channel and an electrode for exciting a plasma from a gas flowing through the gas channel. Air may be employed as the gas to be plasma-excited, for example. Once subjected to irradiation of plasma, hydrophilic functional groups are formed on the surfaces of threads of the tape base fabric 25, thus increasing its wettability. Moreover, the surfaces of the threads of the tape base fabric 25 are slightly roughened. Such modification on the surfaces of the threads of the tape base fabric 25 allows increased adhesion of the melted or softened material 26’ (in turn of the waterproof layer 26) to the threads of the tape base fabric 25.

[0043] Likewise the plasma treatment (S103) described below, a plasma-irradiated region (a plasma spot) is formed in a section corresponding to or limited to the side-edge portion of the tape base fabric 25. The spot diameter of the plasma-irradiated region may preferably be less than 2 times or less than 1.5 times of the width of the side-edge portion of the tape base fabric 25 in the left-right direction. Needless to say, the tape base fabric 25 may be subjected to the plasma treatment independently and separately to the extrusion. It should be noted that, the hydrophilic functional groups disappear as time progresses, and thus the extrusion is preferably performed without delay from the irradiation of plasma.

[0044] In perforation (S102), through-holes 9 piercing the fastener tape 21,31 are formed at a constant pitch along the side-edge portion of the fastener tape 21,31. Perforator illustrated in Fig. 6 may be used for example. The perforator has one or plural (in the illustrated case, three) vertically movable punches 131, a supporting stage 132 arranged beneath the punches 131, and rolls 134-137 for conveying the fastener tape 21,31. The fastener tape 21,31 is conveyed from upstream side to downstream side, and is stopped intermittently and perforated by the punches 131. The punches 131 are moved down to form the through-holes 9 piercing the fastener tape 21,31 and are moved to enter into the holes 132h in the supporting stage 132. Shred wastes caused by the tape base fabric 25 pierced by the punches would fall and would be collected by a collecting box 133.

[0045] Note that the bottom tip of the punch 131 should not be limited to a single-edge shape such as the illustrated one but might be shaped to be double-edge or other sharp shapes. The number of punches 131 should be arbitrary and may be one, two or three or more depending to cases. Through the perforation, the fastener tape 21,31 shifts from a condition illustrated in Fig. 8 to a condition illustrated in Fig. 9.

[0046] In plasma treatment (S103), the plasma treatment is applied to the side-edge portion of the fastener tape 21,31 on one or both surfaces of the fastener tape 21,31 so as to 02 07 24 form activation region(s) on the surface(s) of the waterproof layer 26. The activation region is an area where hydrophilic functional groups are formed on the surface of the waterproof layer 26 and / or an area where the surface of the waterproof layer 26 is roughened. The hydrophilic functional groups reduce as time progresses from a time point of irradiation of plasma. Thus, it would be preferable not to interpose a delay window between the plasma treatment (S103) and the injection molding (S104). In some cases, the injection molding (S104) is performed within one week or 48 hours from the completion of the plasma treatment (S103).

[0047] As illustrated in Fig. 6, plasma emitters 138 and 139 are arranged at the both upper and lower sides of the fastener tape 21,31 at the downstream side of the perforator (punches 131). The plasma emitter 138,139 emits a plasma generated by a plasma source to the surface of the fastener tape 21,31. As the plasma is irradiated, hydrophilic functional groups are generated on the surface of the waterproof layer 26, thus increasing its wettability. Moreover, the surface of the waterproof layer 26 is slightly roughened. Such modification on the surface of the waterproof layer allows increased adhesion of melted resin (in turn the fastener elements 29, 39) to the waterproof layer 26.

[0048] As illustrated in Fig. 9, a plasma-irradiated region (plasma spot) SP is formed on the surface of the waterproof layer in the side-edge portion of the fastener tape. In this setting, the fastener tape is conveyed from the upstream side to the downstream side, and an activation region is continuously formed along the elongation direction of the fastener tape. The plasma-irradiated region SP is formed corresponding to or limited to the side-edge portion 23, 33, suppressing the consumption of power required for the plasma generation. The spot diameter of the plasma-irradiated region SP may preferably be greater than the diameter of the through-hole 9. The spot diameter of the plasma-irradiated region SP may preferably be less than 2 times or less than 1.5 times of the width of the side-edge portion 23,33 in the left-right direction.

[0049] In the side-edge portion 23,33, the plasma-irradiated region SP is formed across a region (hereinafter referred to as an adhesion region) to which the fastener element 29,39 will adhere and a region (hereinafter referred to as a non-adhesion region) to which the fastener element 29,39 will not adhere. The same applied to the activation region. Note that, the non-adhesion region is a region interposed between the adhesion regions. The plasma treatment may be more suitable over a corona treatment for a purpose of suppressing the increased roughness of the non-adhesion region. Condition on irradiation of plasma may preferably be adjusted to lower the degree of surface roughness of the waterproof layer 26. Preferably, the flow rate of plasma irradiation gas is 1400 L / h to 1800 L / h; the type of gas is air; the conveyance speed of fastener tape is 5m / min to 15m / min; the distance between the plasma emitter and the fastener tape directly beneath the emitter is 5 mm to 50 mm; and the output power of plasma ranges from 300 W to 500 W.

[0050] The plasma treatment may be performed or not performed in a region to which a stop member such as front and rear stops adheres. For example, the plasma is emitted intermittently or shield is used to interrupt the emitted plasma. In this instance, the plasma is emitted to the adhesion region and the non-adhesion region of the fastener elements, and the plasma is not irradiated to the region to which the stop 02 07 24 member will adhere.

[0051] After the perforation (S102), there may be cases where threads or fibers are left in the through-hole 9. The threads or fibers in the through-hole 9 may be a part of thread of the tape base fabric 25 protruding into the through-hole 9, a thread waste cut from a thread of the tape base fabric 25 and left in the through-hole 9, or a fiber waste caused at the time of perforation of the tape base fabric 25. In some cases, the plasma treatment (S103) is performed not before the perforation (SI02) but after the perforation (S102). This allows to remove the threads or fibers in the through-hole 9. The threads or fibers in the through-hole 9 are suppressed from flowing to the surfaces of the fastener elements 29, 39 in the period of injection molding and are suppressed from appearing on the surfaces of the fastener elements 29,39 in visible manner. Note that this problem becomes particularly evident in case where the color of fastener element 29 and the color of the threads of the tape base fabric 25 are different, but should not be limited to such a case. We consider that the threads or fibers disappear or fall or are cut off as receiving energy from the plasma.

[0052] Separate plasma treatment device may be utilized which is provided independently to the perforator. In this case either, the plasma treatment device would emit the plasma to the side-edge portion of the fastener tape on its one or both sides to form the activation region on the surface of the waterproof layer. For example, the fastener tape supplied from the perforator is wound about a reel. The plasma treatment device unreels the fastener tape from the reel and performs the plasma treatment thereto.

[0053] In the injection molding (SI04), the fastener elements are injection molded, and the fastener elements are attached to the side-edge portion of the fastener tape. Before solidifying into the fastener element, the melted resin adheres to the activation region of the waterproof layer 26 and fills the through-hole 9 in the side-edge portion 23,33. The fastener element is attached to the activation region formed on the surface of the waterproof layer 26 by the irradiation of plasma, thus enhancing the adhesion strength of the fastener element to the waterproof layer 26.

[0054] The injection molding (S104) is performed using an injection molding apparatus where upper mold 141 and lower mold 142 are attached to a mold-clamping device. As illustrated in Fig. 7, the fastener tape 21,31 is supplied and sandwiched between the lower mold 142 and the upper mold 141. The lower mold 142 and the upper mold 141 define a molding cavity 146, and the through-hole 9 in the side-edge portion 23,33 is positioned in this molding cavity 146. Melted resin is supplied into the molding cavity 146 through a channel (sprue, runner and gate) in the mold and the molding cavity 146 is filled with the melted resin. The melted resin adheres to the activation region of the surface of the waterproof layer 26, and flows into the through-hole 9 formed in the side-edge portion. As the upper and lower molds 141 and 142 are cooled, the melted resin is solidified and the fastener element is attached to the side-edge portion 23,33. The melted resin, having flowed into the molding cavity 146, is solidified to include the filling portion 71 (corresponding to the through-hole 9), the upper portion 72 (corresponding to the upper space of cavity), and the lower portion 73 (corresponding to the lower space of cavity). Note that detail descriptions on the injection molding apparatus, e.g. extruder, mold clamping device or the like are omitted. 02 07 24

[0055] One through-hole 9 is associated with one fastener element 29,39. The diameter of the through-hole 9 is appropriately set to allow the melted resin to flow into the through-hole 9 and / or to flow between the upper space and the lower space via the through-hole 9. In the case where the diameter of the through-hole 9 is too small, unfilled spaces may possibly be formed. In the case where the diameter of the through-hole 9 is too large, the contact area between the fastener element 29, 39 and the fastener tape 21,31 would be smaller. Note that, from a viewpoint of enlarged contact area or from other viewpoints, the upper portion 72 and the lower portion 73 may preferably have the shoulders 74 and / or fins 75 additionally to the head 76, the neck 77 and the body 78.

[0056] In the present embodiment, the plasma treatment is applied to the surface of the waterproof layer to which the fastener elements will adhere before the fastener elements is injection molded to adhere to the fastener tape. As a result of this, adhesion energy of the fastener element to the surface of the waterproof layer 26 is increased notably, thus reducing the occurrence of the element-turn remarkably. Furthermore, by performing the plasma treatment after the perforation, the threads or fibers in the through-hole 9 may be removed as being irradiated by the plasma, thus avoiding or suppressing the appearance of the threads or fibers on the surfaces of the fastener elements.

[0057] One may envision that two through-holes are associated with one fastener element so that the element-turn would be suppressed. However in this case, the contact area between the fastener element and the waterproof layer may be reduced as the number of through-hole increases. Moreover, the diameter of through-hole may be obliged to be smaller, inviting possible short shot.

[0058] The sliders 4 of the waterproof slide fasteners 1 have a higher sliding resistance. There may be a case where a lubricant (e.g. grease) which is other than recommended lubricants is applied to the left and right lines of the fastener elements 29, 39 in order to smoothly move the slider 4. When operation of opening and closing of slide fastener with sufficient force is repeated in such an unusual circumstance, there is a possibility of facilitated removal of fastener element off the waterproof layer as the grease enters between the fastener element and the waterproof layer. In the present embodiment, the element-turn would be effectively hindered even if the fastener elements were placed in a chemically severe environment as noted above, which is demonstrated by the example described below.

[0059] Note that in a case where the side-edge portion 23,33 of the fastener tape 21, 31 is a smooth surface, there is a higher likelihood for the melted resin to enter into a clearance between the fastener tape 21,31 and the lower or upper mold.

[0060] Working example 1 The side-edge portion of the tape base fabric woven from polyester threads was irradiated by plasma on its both surfaces (which may be referred to as a first plasma irradiation hereinafter). Next, a waterproof layer made of polyurethane was formed onto the both surfaces of the tape base fabric through extrusion. Thickness of the waterproof layer at the one side was about 0.2 mm. Next, the through-holes were formed at a pitch of 5 mm in the side-edge portion along the elongation direction of 02 07 24 the fastener tape. The through-hole pierces the tape base fabric of the fastener tape and pierces the waterproof layer formed onto the upper and lower surfaces of the tape base fabric. Next, the side-edge portion of the fastener tape was irradiated by the plasma on its both surfaces (which may be referred to as a second plasma irradiation hereinafter). Next, the fastener elements of polyamide were formed through injection molding and were attached to the side-edge portion of the fastener tape. Two fastener stringers were prepared following such processes, and were coupled by a slider in a separable manner. Note that the extrusion was performed within 48 hours after the first plasma irradiation. Similarly, the injection molding was performed within 48 hours after the second plasma irradiation.

[0061] Next, a test was conducted to evaluate the adhesion strength of the fastener element to the waterproof layer. We now refer to Figs. 11 and 12 for further description. Firstly, we removed one of the upper and lower portions of one fastener element S29 which is an object to be measured and is located at a middle (substantially middle) position between the both ends of the fastener stringer. We inserted a blade of a cutting tool such as a nipper or the like between the fastener tape and the upper portion 72 or the lower portion 73 to cut the filling portion 71. Note that, the lower portion 73 of the fastener element S29 was removed in Fig. 11, but it could be the upper portion 72 that is removed alternatively.

[0062] Next, a load curve was generated by measuring a load (unit: Newton (N)) required for displacement of the remainder of the upper portion 72 or the lower portion 73 of the fastener element S29 while moving the remainder of the upper portion 72 or the lower portion 73 of the fastener element S29 away from an overlap of the ends of the waterproof fastener stringer. As illustrated in Fig. 12, the upper grippers 120 gripped the remainder of the upper portion 72 or the lower portion 73 of the fastener element S29. Also, the lower grippers 130 gripped the overlap of the both ends of the fastener stringer. As the upper grippers 120 moved upwardly, the fastener element S29 was moved upwardly and was finally removed off the fastener tape (the waterproof layer). The load curve was generated by measuring the upward load (unit: Newton (N)) applied to the upper grippers 120 for the upward movement (unit: millimeter (mm)) of the upper grippers 120. Note that, the illustration of fastener elements between the grippers 120 and 130 is omitted in Fig. 12.

[0063] Fig. 13 shows a load curve of working example 1. In the load curve shown in Fig. 13, an interval can be set between a start line and an end line by setting the start line orthogonal to the displacement axis and at a position corresponding to an initial maximum value (about 61.5 N) of the measured load value, and by setting the end line orthogonal to the displacement axis and at a position corresponding to “measured load value = zero”. In a time window between the initial value and the maximum value, the waterproof layer is pulled away from the tape base fabric and at the maximum value, the waterproof layer is separated locally from the tape base fabric. After passing the maximum value, the fastener element (the remainder of the upper and lower portions) is pulled away from the waterproof layer. The area of the load curve (unit: N*mm) in the above interval reflects an adhesion energy of the fastener element to the waterproof layer. The adhesion energy (N*mm) is proportional to the area of the load curve after passing the initial maximum value of the measured load value, and reflects the adhesion energy of the fastener element to the waterproof layer. 02 07 24

[0064] The adhesion energy can be calculated by integrating the load curve in the abovedescribed interval. In detail, the load curve is plotted based on measurements of load applied to the upper grippers 120 by each 0.1 mm displacement of the upper grippers 120. The start point for the integration is set to a load value at which the measured load value is maximum. The end point for the integration is set to a load value at which the measured load value is zero. Small areas are calculated based on continuously measured values of load and this calculation repeatedly continues from the start point of integration toward the end point of integration. The small area can be calculated based on a formula = ((First value of load + Second value of load) / 2)*0.1. By summing the small areas calculated as such, the area of the load curve can be determined. Note that, software available from INSTRON can be used for this calculation, not necessarily limited to this though.

[0065] Note that, we confirmed dispersion of maximum value among the samples. Chart 1 shows values of maximum value for respective samples which were produced based on the working example 1. The average value of the maximum values was 58.24 N. As understood from the Chart 1, if the adhesion energy (N'mm) is denoted by S, S>200 is satisfied, and preferably S>300 or S>400 is satisfied. This is a result of the above-described feature, i.e. the irradiation of plasma to the surface of the waterproof layer, to which the fastener element will adhere, before the injection molding through which the fastener elements are attached to the fastener tape. [Chart 1]________________________________________________________________________ Sample number Maximum value (N) Adhesion energy (N'mm) 1 61.1 412.5 2 58.2 470.2 3 57.5 441.3 4 56.9 483.2 5 58.6 437.2 6 56.9 445.5 7 58.7 473.5 8 59.1 456.4 9 57.6 519.4 10 57.8 432.6

[0066] Comparative example 1 Fastener stringers were produced and evaluated in the same condition as in the working example 1 except that the first and second irradiations of plasma were omitted. Fig. 14 shows the load curve of the comparative example 1. In this comparative example, S<200 is satisfied when the adhesion energy is denoted by S. Therefore, sufficient adhesion energy was not obtained compared with that of the working example 1.

[0067] Note that, we confirmed dispersion of maximum value among the samples also in the comparative example. Chart 2 shows maximum values of respective samples produced based on the comparative example 1. The average value of the maximum value is 37.3 N. The adhesion energy (N'mm) shown in Chart 2 corresponds to the area of the load curve in the interval equivalent to that in the working example 1, and reflects the adhesion energy of the fastener element to the waterproof layer. [Chart 21_______________________________________________________________ Sample number Maximum value (N) Adhesion energy (N'mm) 1 41.2 101.9 2 42.7 92.1 3 42.8 83.4 4 38.7 83.7 5 35.1 75.2 6 31.7 41.1 7 35.6 80.1 8 30.6 54.3

[0068] 02 07 24 Working example 2 Fastener stringers were produced and evaluated in the same condition as in the working example 1 except that the first irradiation of plasma was omitted. Fig. 15 shows the load curve of the working example 2. In this working example 2, S>200 was satisfied similar to the working example 1. The maximum value was about 54 N.

[0069] Further, opening-closing test was conducted for the working example 1 and the comparative example 1. In the opening-closing test, the slider is reciprocated in the front-rear direction in the slide fastener, and it is determined if the number of reciprocating of the slider reaches a target number without causing the elementturn. If the element-turn occurred before reaching the reciprocation target number, the opening-closing test was terminated. In this opening-closing test, a grease was applied to the fastener elements in order to facilitate the element-turn. Further, the distance of movement of slider was set to 600 mm, and the speed of its movement was set to 900 mm / s. Still further, the test was conducted in a condition where a force of 3 kgf is constantly applied to the slide fastener in its elongation direction, and a force of 0.1 kgf is constantly applied thereto in its width direction (i.e. the test was conducted while the slide fastener was stretched to the front, rear, left and right sides). As seen in the result of the opening-closing test of Chart 3, remarkably beneficial outcome was obtained in the working example 1 compared with the comparative example 1. [Chart 3]  ___________________________________________________________________ Working example 1 Comparative example 1 Result No element-turn even up to 20,000 times Element-turn occurred at 650 times

[0070] Figs. 16 and 17 show conditions where a thread or fiber inside the through-hole is removed by the second irradiation of plasma in the working example 1.

[0071] Note that, fastener elements of the same or equivalent size were used in the load test and in the opening-closing test. In the load test and the opening-closing test described above, the area of the surface of the waterproof layer to which a fastener element adheres at one side of the fastener stringer is 17.08mm2 ±0.2mm2 (more accurately, 17.08mm2 ±0.1mm2 in the above-described working and comparative examples). Note that, the area of through-hole (the area defined by inner wall surface of through-hole) is not included in this area.

[0072] A skilled person in the art would be able to add various modifications to the respective embodiments based on the above teachings. Reference signs in Claims are added just for a purpose of reference and should not be referred to for narrowly construing the scope of Claims.

[0073] The fastener tape is not limited to be produced through extrusion, but may be produced by attaching the waterproof layer onto the tape base fabric by pressure. [List of signs]

[0074] 1 Slide fastener 2 Fastener stringer 3 Fastener stringer 21 Fastener tape 23 Side-edge portion 25 Tape base fabric 26 Waterproof layer 29 Fastener element 31 Fastener tape 33 Side-edge portion 39 Fastener element 07 24 CXI

Claims

[Claims]1. A method of producing a waterproof fastener stringer, the method comprising: forming through-holes (9) at a constant pitch along a side-edge portion (23,33) of a fastener tape (21,31) where a tape base fabric (25) is covered by a waterproof layer (26), the through-holes (9) piercing the fastener tape (21,31);applying a plasma treatment to the side-edge portion (23,33) of the fastener tape (21,31) so as to form an activation region on a surface of the waterproof layer (26) on one or both sides of the fastener tape (21,31); andperforming an injection molding of fastener elements (29,39) to attach the fastener elements (29,39) to the side-edge portion (23,33) of the fastener tape (21,31), a melted resin adhering to the activation region and filling the through-hole (9) before solidifying into the fastener element (29,39).

2. The method of producing a waterproof fastener stringer of Claim 1, wherein the plasma treatment is applied to the side-edge portion (23,33) of the fastener tape (21,31) after the through-holes (9) are formed in the side-edge portion (23,33) of the fastener tape (21,31).

3. The method of producing a waterproof fastener stringer of Claim 2, wherein the plasma treatment is applied to the side-edge portion (23,33) of the fastener tape (21,31) so as to remove a thread or fiber of the tape base fabric (25) in the through-hole (9).

4. The method of producing a waterproof fastener stringer of any one of Claims 1-3, wherein said applying a plasma treatment to the side-edge portion (23,33) of the fastener tape (21,31) so as to form an activation region on a surface of the waterproof layer (26) on one or both sides of the fastener tape (21,31) includes: forming a plasma-irradiated region on the surface of the waterproof layer (26) in the side-edge portion (23,33) of the fastener tape (21,31); and conveying the fastener tape (21,31) from an upstream side to a downstream side, whereinthe activation region is formed continuously along an elongation direction of the fastener tape (21,31).

5. The method of producing a waterproof fastener stringer of Claim 4, wherein a spot diameter of the plasma-irradiated region is greater than a diameter of the through-hole (9).

6. The method of producing a waterproof fastener stringer of Claim 4 or 5, wherein a spot diameter of the plasma-irradiated region is less than 2 times or 1.5 times of a width of the side-edge portion (23,33).

7. The method of producing a waterproof fastener stringer of any one of Claims 1-6, wherein said applying a plasma treatment to the side-edge portion (23,33) of the fastener tape (21,31) so as to form an activation region on a surface of the waterproof layer (26) on one or both sides of the fastener tape (21,31) is performed to skip a portion where a stop member is to be formed in the side-edge portion (23,33) of the fastener tape (21,31).02 07 248. The method of producing a waterproof fastener stringer of any one of Claims 1-7, further comprising: applying a plasma treatment to the tape base fabric (25) before the tape base fabric (25) is covered by the waterproof layer (26).

9. The method of producing a waterproof fastener stringer of Claim 8, wherein said applying a plasma treatment to the tape base fabric (25) before the tape base fabric (25) is covered by the waterproof layer (26) includes:forming a plasma-irradiated region on a surface of the tape base fabric (25); andconveying the tape base fabric (25) from an upstream side toward a downstream side.

10. The method of producing a waterproof fastener stringer of any one of Claims 1-9, wherein the waterproof layer (26) is formed onto both upper and lower surfaces of the tape base fabric (25) through the injection molding.

11. The method of producing a waterproof fastener stringer of any one of Claims 1-10, wherein the waterproof layer (26) is made of polyurethane, and the fastener element (29,39) is made of polyamide.

12. The method of producing a waterproof fastener stringer of any one of Claims 1-11, wherein the fastener element (29,39) includes: a filling portion (71) that fills the through-hole (9); an upper portion (72) connected to an upper end of the filling portion (71); and a lower portion (73) connected to a lower end of the filling portion (71), each of the upper and lower portions (72, 73) has a head (76), a neck (77) and a body (78), andan end face of the side-edge portion (23,33) of the fastener tape (21,31) is positioned in a groove between the head (76) of the upper portion (72) and the head (76) of the lower portion (73).

13. The method of producing a waterproof fastener stringer of Claim 12, further comprising:removing one of the upper portion (72) and the lower portion (73) of one fastener element (29,39) positioned at a middle between both ends of the waterproof fastener stringer (2,3);moving a remainder of the upper portion (72) and the lower portion (73) away from an overlap of the both ends of the waterproof fastener stringer (2,3) and measuring a load required for displacement of the remainder to generate a load curve; andcalculating an area of the load curve in an interval in which a measured load value changes from an initial maximum value to zero, whereinS>200 is satisfied where S denotes the area (unit: N*mm) of the load curve in the interval.

14. The method of producing a waterproof fastener stringer of any one of Claims 1-13, wherein said forming through-holes (9), said applying a plasma treatment to the side-edge portion (23,33) of the fastener tape (21,31), and said performing an injection molding of fastener elements (29,39) are performed in this order at different02 07 24locations.

15. The method of producing a waterproof fastener stringer of any one of Claims 1-13, the method further comprising: conveying the fastener tape (21,31), whereinsaid forming through-holes (9) at a constant pitch along a side-edge portion (23,33) of a fastener tape (2 1,31) and said applying a plasma treatment to the sideedge portion (23,33) of the fastener tape (21,31) are performed in this order at different locations along a direction that the fastener tape (21,31) is conveyed, and said performing an injection molding of fastener elements (29,39) is performed at a different location from said forming through-holes (9) at a constant pitch along a side-edge portion (23,33) of a fastener tape (21,31) and said applying a plasma treatment to the side-edge portion (23,33) of the fastener tape (21,31).

16. A waterproof fastener stringer (2,3) comprising:a fastener tape (21,31) where a tape base fabric (25) is covered by a waterproof layer (26); andresin-made fastener elements (29,39) adhering to the fastener tape (21,31), each of the fastener elements (29,39) including at least one filling portion (71) that fills a through-hole (9) piercing the fastener tape (21,31), an upper portion (72) connected to an upper end of the at least one filling portion (71), and a lower portion (73) connected to a lower end of the at least one filling portion (71), whereinS>200 is satisfied where S denotes an area (unit: N*mm) of a load curve in an interval,said load curve generated based on measurement of load required for displacement of a remainder of the upper portion (72) and the lower portion (73) away from an overlap of the both ends of the waterproof fastener stringer (2,3) after one of the upper portion (72) and the lower portion (73) of one fastener element (29,39) positioned at a middle between both ends of the waterproof fastener stringer (2,3) is removed, andsaid area of the load curve is calculated in the interval in which a measured load value changes from an initial maximum value to zero.

17. The waterproof fastener stringer of Claim 16, wherein the maximum value is equal to or greater than 50N or the maximum value is equal to or greater than 58N.

Citation Information

Patent Citations

  • Waterproof slide fastener

    GB2512792A

  • Decorative sheet for three-dimensional processing

    JP2012116200A

  • Method for producing water-blocking fastener tape, and water-blocking fastener tape

    WO2016157536A1

  • Fastener stringer, production method for same, and mold