Aluminum alloy and process for additive manufacture of lightweight components

JP2022087830A5Active Publication Date: 2024-12-06AIRBUS (SAS)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021193699
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-12-01
Filing Date
2021-11-30
Publication Date
2024-12-06
Estimated Expiration
2041-11-30

AI Technical Summary

Technical Problem

Existing aluminum alloys used in additive manufacturing, such as L-PBF, face challenges with process stability due to high vapor pressure metals like Mg and Zn, and require improved strength and corrosion resistance for lightweight aircraft components.

Method used

An aluminum alloy comprising Ti, Sc, and Zr with controlled contents, along with optional additional metals, is developed for additive manufacturing, utilizing rapid solidification to achieve a fine microstructure and precipitation hardening, enhancing strength and corrosion resistance.

Benefits of technology

The alloy provides improved process stability, strength, and corrosion resistance, enabling high-quality lightweight components suitable for aircraft construction through L-PBF.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide an improved aluminum alloy which is suitable for additive manufacturing with a sufficiently rapid cooling rate.SOLUTION: The invention relates to an alloy which consists of aluminum, titanium, scandium and zirconium, and other metals selected from hafnium, vanadium, niobium, chromium, molybdenum, silicon, iron, cobalt, nickel and calcium. The aluminum alloy is suitable for the additive manufacture of lightweight components for aircraft. In a first step, a powder of the aluminum alloy of the invention is made to a lightweight component precursor by additive manufacturing such as laser melting in an L-PBF (laser powder bed fusion) process. The precursor comprising titanium, scandium and zirconium in solid solution, as a result of rapid solidification of the laser melt. In a second step, the lightweight component precursor is hardened by precipitation of secondary phases at 250 to 400°C to give a lightweight component. 3D-printed lightweight components of high strength are obtained.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to an aluminium alloy, a method for additive manufacturing of lightweight components using powder from this aluminium alloy, and the lightweight components produced by this method. [Background technology]

[0002] Aluminum alloys are important materials for manufacturing lightweight components for aircraft. Reductions in the overall weight of aircraft, coupled with the incorporation of these lightweight components, can lead to reduced fuel costs. Aluminum alloys that can be used for this purpose must also possess high tensile strength, ductility, toughness, and corrosion resistance to ensure flight safety.

[0003] Examples of aluminum alloys that can be used in aircraft construction are the alloys designated AA2024, AA7349, and AA6061. These alloys contain, in addition to aluminum as the base metal, magnesium and copper as essential alloying partners, and also, necessarily or optionally, manganese, zirconium, chromium, iron, silicon, titanium, and / or zinc.

[0004] An important further development is represented by scandium-containing aluminum alloys, which are commercially available, for example, from APWorks GmbH under the product name Scalmalloy®. This alloy has higher strength, ductility, and corrosion resistance than the above-mentioned alloys. Among all transition metals, scandium exhibits the greatest increase in strength due to precipitation hardening of Al3Sc. Due to the low solubility of scandium in aluminum (about 0.3 wt. % at about 660°C), Scalmalloy® must be produced by rapid solidification of the melt, such as melt spinning, followed by precipitation hardening, which involves the formation of secondary Al3Sc precipitates in the aluminum matrix.

[0005] For more information on Scalmalloy®, please see the publication "Scalmalloy® - A unique, high-strength, corrosion-resistant AlMgScZr material concept" R - A unique high strength and corrosion insensitive AlMgScZr material concept” (AJ Bosch, R. Senden, W. Entelmann, M. Knuewer, F. Palm, “Proceedings of the 11th International Conference on Aluminum Alloys in: “Aluminum Alloys: Their physical and mechanical properties”, J. Hirsch, G. Gottstein, B. Skrotzki, Wiley-VCH) and “Metallurgical peculiarities in hyper-eutectic AlSc and AlMgSc engineering materials prepared by rapid solidification processing” (F. Palm, P. Vermeer, W. von Bestenbostel, D. Isheim, R. Schneider (cited above)).

[0006] Table 1 according to FIG. 1 shows the chemical compositions of the above-mentioned aluminum alloys that can be used to manufacture lightweight components for aircraft.

[0007] Another advantage of Scalmalloy® is its suitability for the additive manufacturing of lightweight components. It is particularly suited to processes such as wire arc additive manufacturing (WAAM = "Wire Arc Additive Manufacturing") as well as laser powder bed fusion (LPBF), also referred to below as the L-PBF process (LPBF = "Laser Powder Bed Fusion"). The number of alloys that can be used in this process is limited. According to WO 2018 / 144323, the alloys Scalmalloy®, AlSi10Mg, TiAl6V4, CoCr, and Inconel 718 can be reliably additively manufactured in the L-PBF process. However, the majority of the more than 5,500 alloys currently in use cannot be used in the L-PBF process or 3D printing. Summary of the Invention [Problem to be solved by the invention]

[0008] It is an object of the present invention to provide an improved aluminium alloy that is suitable for additive manufacturing at sufficiently fast cooling rates, for example in the L-PBF process.

[0009] This problem is solved by an aluminum alloy according to claim 1. Advantageous refinements are the subject matter of the subclaims.

[0010] According to a first aspect, the present invention provides an aluminum alloy comprising the following alloying elements: - Ti with a content of 0.1 to 15.0% by weight, - Sc with a content of 0.1-3.0% by weight, - Zr with a content of 0.1 to 3.0% by weight, - The rest of Al and unavoidable impurities.

[0011] The addition of Ti has many advantages. The LPB-F process is stable due to the absence of metals with high vapor pressures or low vaporization enthalpies, such as Mg or Zn. Ti enhances strength by refining the crystal grains. This is primarily due to the coherent precipitation of Al3X phases (X = Ti, Zr, Sc), which act as nucleation sites in combination with the high structural undercooling induced by the incorporation of Ti into the alloy. During subsequent heat and post-treatment, the secondary phases precipitation harden, increasing strength. AlSc alloys containing Ti also exhibit superior corrosion resistance.

[0012] Ti does not cause as large an increase in room temperature strength in aluminum alloys as Sc or Zr. Most of the Ti remains dissolved in solid solution during rapid solidification. Coarsening of precipitates is slower than expected. Fatigue and creep resistance are improved.

[0013] The chemical driving force for precipitation, ΔFch, is significantly greater for Al3Zr than for Al3Ti. The elastic strain energy ΔFel ("elastic strain energy for precipitation") of Al3Ti during precipitation prevents nucleation and is seven times that of Al3Zr. When rapidly cooled, up to 2 wt.% Ti can be forced to dissolve in the aluminum matrix.

[0014] The advantage of Ti in the additive manufacturing of lightweight components by the L-PBF process (or SLM process from "selective laser melting") of aluminum alloys is its low vapor pressure, or high heat of vaporization. The vapor pressure of Ti is lower than that of the base metal, aluminum. The vapor enthalpy of Ti is higher than that of the base metal, aluminum. As a result, the process stability is improved and a very calm and stable molten pool is created during remelting compared to aluminum alloys containing magnesium.

[0015] Ti ensures strong structural undercooling during solidification, which activates strong primary nucleation sites in the melt and refines the crystal grains. The fine microstructure is characterized by the Hall-Petch effect; the strength increase is due to the d -1 / 2 Increases the strength of aluminum alloys according to (inversely proportional to grain size).

[0016] In the molten state, Zr provides effective nucleation sites even at high temperatures, since Al3Zr precipitates already at about 900 °C and can therefore be activated by structural undercooling. In contrast, Al3Sc precipitates only shortly before the solidus temperature.

[0017] The aluminum alloy preferably contains Ti in an amount of 0.5 to 5.0% by weight, Sc in an amount of 0.2 to 1.5% by weight, and Zr in an amount of 0.2 to 1.5% by weight.

[0018] The aluminum alloy preferably contains Ti in an amount of 1.0 to 5.0% by weight, preferably 1.0 to 4.0% by weight, Sc in an amount of 0.5 to 1.0% by weight, and Zr in an amount of 0.2 to 0.8% by weight.

[0019] The aluminum alloy preferably contains one or more metals selected from the group consisting of hafnium (Hf), vanadium (V), niobium (Nb), chromium (Cr), molybdenum (Mo), silicon (Si), iron (Fe), cobalt (Co), and nickel (Ni). The contents of each of these elements are as follows: - representing up to 100%, preferably at most 90%, preferably at most 70%, more preferably at most 50% of the Ti content, with the total content of these metals being at most 15% by weight, preferably at most 10% by weight, of the aluminum alloy of any one of claims 1 to 3, or - 0.1% to 2% by weight, provided that the total content of these metals in the aluminum alloy according to any one of claims 1 to 3 constitutes a maximum of 15% by weight, preferably a maximum of 10% by weight.

[0020] Preferably, the aluminum alloy contains, in addition to aluminum and unavoidable impurities, only metals that have a higher heat of vaporization or a lower vapor pressure than aluminum.

[0021] The aluminum alloy preferably contains calcium (Ca) in the range of 0.1 to 5 wt.%, preferably greater than 0.5 to 5 wt.%, and particularly preferably in the range of 0.7 to 3 wt.%, which forms a calcium oxide coating during laser melting and prevents undesired evaporation of the alloying elements.

[0022] The aluminum alloy is preferably free of magnesium and / or manganese.

[0023] The aluminum alloy preferably comprises a combination of the alloying elements previously described.

[0024] The aluminum alloy preferably consists of Al, Ti, Sc and Zr, except for unavoidable impurities, or consists of Al, Ti, Sc, Zr and one or more of the above metals.

[0025] The aluminum alloy preferably consists of Al, Ti, Sc, Zr and Cr, excluding unavoidable impurities, with the Cr content being in the range of 0.2 to 3.5 wt.%, preferably in the range of 0.5 to 3.0 wt.%.

[0026] The aluminum alloy preferably consists of Al, Ti, Sc, Zr and Ni, excluding unavoidable impurities, with the Ni content being in the range of 0.2 to 2.5 wt.%, preferably in the range of 0.5 to 2.0 wt.%.

[0027] The aluminum alloy preferably consists of Al, Ti, Sc, Zr and Mo, excluding unavoidable impurities, with the Mo content being in the range of 0.1 to 1.3 wt.%, preferably in the range of 0.5 to 1.0 wt.%.

[0028] The aluminum alloy preferably consists of Al, Ti, Sc, Zr and Fe, excluding unavoidable impurities, with the Fe content being in the range of 0.1 to 2.5% by weight, preferably in the range of 0.5 to 2.0% by weight.

[0029] The aluminum alloy preferably consists of Al, Ti, Sc, Zr and Ca, excluding unavoidable impurities, with the Ca content being in the range of 0.1 to 5% by weight, preferably in the range of more than 0.5 to 5% by weight, and particularly preferably in the range of 0.7 to 3% by weight.

[0030] According to a second aspect, the present invention creates a method for additively manufacturing precursors of lightweight structural members, comprising: a) The metals are melted together to form a molten aluminum alloy. b) The aluminum alloy melt is forced to cool or allowed to cool. b1) obtaining a solidified aluminum alloy, optionally in the form of a powder, containing scandium in solid solution by a rapid solidification process (e.g., melt spinning, powder atomization in gas or water, strip casting, or spray forming (in-situ compaction)) at a cooling rate of 1,000 K / s (K / second) to 10,000,000 K / s, in particular at a cooling rate of 100,000 K / s to 1,000,000 K / s, or b2) A cooling process is performed to obtain a solidified aluminum alloy. c) grinding the aluminum alloy of step b1) or b2) into powder;

[0031] In step b) or step b1), the cooling rate is preferably maintained at least in the temperature range from 1,800K to 500K.

[0032] When the molten aluminum alloy is cooled in step b), provided the cooling rate is not too rapid, as when the melt is cast into a crucible, an aluminum matrix is ​​formed in which the alloying elements Ti, Sc, and Zr are present primarily in large primary precipitates. If the aluminum alloy is cooled very rapidly, at rates ranging from 1,000 K / s to 10,000,000 K / s, the solidified aluminum alloy contains these alloying elements essentially in solid solution. The precipitation of primary phases is suppressed by rapid cooling. The faster the melt is cooled, the lower the content of primary precipitates. During subsequent precipitation solidification at temperatures between approximately 250 and 450°C, nanoscale coherent Al3X phases (X = Ti, Zr, Sc) precipitate, ensuring a significant increase in the strength of the aluminum alloy.

[0033] In step e), the powder is melted by the laser beam followed by very rapid cooling in which the alloying elements solidify substantially into solid solution, a process step which generally involves remelting into the desired alloy.

[0034] According to a third aspect, the present invention provides a method for additively manufacturing a precursor of a lightweight component from an aluminium alloy as described above, the method comprising: d) producing a powder bed from the powder obtained in step c) of claim 10. e) Additive manufacturing of three-dimensional lightweight component precursors in a powder bed laser melting process by locally laser melting the powder and forcing the locally melted areas to cool or be cooled, resulting in a lightweight component precursor from an aluminum alloy with scandium in solid solution.

[0035] According to a fourth aspect, the present invention provides a method for producing a lightweight component, comprising heat treating a lightweight component precursor obtained by the method described above at a temperature at which the lightweight component precursor hardens by precipitation hardening.

[0036] According to a fifth aspect, the present invention provides a lightweight component precursor obtainable by the additive manufacturing process described above.

[0037] According to a sixth aspect, the present invention provides a lightweight component obtainable by the curing process described above.

[0038] According to a seventh aspect, the present invention provides the use of an aluminium alloy as described above, or a powder obtainable by the method described above, for the manufacture of a lightweight component by selective laser melting to produce a lightweight component precursor followed by selective laser melting and subsequent precipitation hardening (use of the powder).

[0039] Exemplary embodiments are described in more detail below with reference to the accompanying drawings. [Brief explanation of the drawings]

[0040] [Figure 1] Table 1 shows the chemical compositions of common aluminum alloys used in lightweight aircraft components. [Figure 2] Table 2 shows the physical properties of the most important alloying elements. [Figure 3] 1 shows the vapor pressure as a function of temperature for the constituent elements of Scalmalloy®. [Figure 4] 1 shows the vapor pressure as a function of temperature for the constituent elements of an alloy according to the present invention. DETAILED DESCRIPTION OF THE INVENTION

[0041] Figure 1 shows in Table 1 the compositions of aluminum alloys used in the manufacture of lightweight components for aviation. Alloys AA2024, AA7349, AA7010 and AA6061 contain magnesium and copper, as does duralumin. Duralumin is an aluminum alloy developed in 1906 by Alfred Wilms, who recognized that precipitation hardening could significantly increase the strength of the alloy. The increased strength thus achieved has made it possible to use aluminum in alloy form in aviation.

[0042] The strength of aluminum can be further improved significantly by adding scandium, as in Scalmalloy®. Due to the low solubility of scandium in aluminum at room temperature, scandium must first be forced into solution in the aluminum in a rapid solidification process such as melt spinning before precipitation hardening can be achieved at temperatures in the range of 250°C to 450°C.

[0043] The characteristics of the two aluminum alloys in Table 1, AlSi10Mg and Scalmalloy®, make them suitable for laser melting in the L-PBF process, and therefore these two alloys can be processed by additive manufacturing into lightweight components for aircraft.

[0044] Figure 2 shows the physical properties of various alloying elements in Table 2. All alloying elements above aluminum have a higher enthalpy of vaporization than aluminum. All below aluminum have a lower enthalpy of vaporization than aluminum.

[0045] FIG. 3 is a diagram showing the temperature dependence of vapor pressure for the alloy components (elements that make up the alloy) of Scalmalloy®.

[0046] FIG. 4 is a diagram showing the temperature dependence of the vapor pressure of an aluminum alloy according to the present invention.

[0047] The aluminum alloy, the lightweight member precursor, and the method for manufacturing the lightweight member will be described below.

[0048] A) Aluminum alloy manufacturing process Example 1: Production of aluminum alloy powder In an inert crucible, 0.75 wt% Sc, 0.35 wt% Zr, 1.0 wt% Ti, and 97.9 wt% Al are melted. The melt may be homogenized before further processing.

[0049] A first fraction of the melt is poured into an inert crucible where it cools and solidifies. Upon cooling, primary Al3Sc, Al3Zr, and Al3Ti phases precipitate. The resulting material is ground into a powder that can be used for selective laser melting in a powder bed.

[0050] A second fraction of the melt is poured onto a rotating, water-cooled copper roller in a melt-spinning process. The melt is cooled at a rate of 1,000,000 K / s to form a strip. The melt is cooled so rapidly that the formation of Al3Sc, Al3Zr, and Al3Ti is completely or substantially suppressed. The strip is cut into short flakes.

[0051] The alloy material obtained from the two cooling processes can be ground into powder and used for selective laser melting in a powder bed.

[0052] Example 2: Production of aluminum alloy powders with different titanium contents The above procedure is repeated, except that the Ti content is increased to 3.0 wt%, 5.0 wt%, 10.0 wt%, and 15.0 wt%, and the Al content is decreased accordingly, while the Sc and Zr contents remain unchanged.

[0053] Example 3: Preparation of vanadium-containing aluminum alloy in powder form The process of Example 1 is repeated except that 2.0 wt. % vanadium is additionally placed in the crucible, and the Ti, Sc, and Zr contents are kept constant.

[0054] Example 4: Preparation of powdered aluminum alloy containing nickel The process of Example 1 is repeated except that 1.2 wt. % nickel is additionally placed in the crucible, and the Ti, Sc, and Zr contents are kept constant.

[0055] Example 5: Preparation of powdered aluminum alloy containing chromium vanadium The process of Example 1 is repeated except that 1.0 wt.% vanadium and 2.0 wt.% chromium are additionally added to the crucible, the titanium content is increased to 5 wt.%, and the Zr content remains unchanged.

[0056] B) Manufacturing process of lightweight component precursors using the L-PBF process Each aluminum alloy powder from each of Examples 1-5 above is placed in a selective laser melting additive manufacturing facility to form a powder bed. A laser beam moves over the three-dimensional powder bed according to digital information. During this process, the powder bed is gradually lowered in height and covered with a new powder layer. The point-shaped molten aluminum alloy is cooled very rapidly so that scandium, zirconium, and titanium are completely, substantially, or predominantly frozen (solidified) into a solid solution, regardless of the other components of the aluminum alloy and regardless of whether the powder was produced by normal cooling or rapid cooling (e.g., cooling at a rate of 1,000,000 K / s). After the scanning process is completed, the aluminum alloy component precursor is separated from the powder bed.

[0057] C) Manufacturing methods for lightweight components The component precursor produced in step B) is heated to a temperature in the range of 250°C to 450°C, preferably 300°C to 400°C, and more preferably 325°C to 350°C. This results in the precipitation of various Al3X phases (X = Ti, Zr, Sc, or any desired non-stoichiometric mixture of the individual elements). Al3Ti is also precipitated, but compared to Al3Sc and Al3Zr, the titanium component remains predominantly or predominantly in solid solution.

Claims

1. Aluminum alloys containing the following alloying elements: - titanium (Ti) with a content of 0.1% to 15.0% by weight, - scandium (Sc) with a content of 0.1% to 3.0% by weight, - zirconium (Zr) with a content of 0.1% to 3.0% by weight, and The balance is aluminum (Al) and unavoidable impurities.

2. Ti with a content of 0.5% to 5.0% by weight, Sc with a content of 0.2% to 1.5% by weight, and 2. An aluminum alloy according to claim 1, characterized in that it contains Zr in a content of 0.2 to 1.5% by weight.

3. Ti with a content of 1.0 to 5.0% by weight, preferably 1.0 to 4.0% by weight, Sc with a content of 0.5% to 1.0% by weight, and 3. An aluminum alloy according to claim 1, characterized in that it contains Zr in a content of 0.2 to 0.8% by weight.

4. 4. The aluminum alloy according to claim 1, comprising one, two, or more metals selected from the group consisting of hafnium (Hf), vanadium (V), niobium (Nb), chromium (Cr), molybdenum (Mo), silicon (Si), iron (Fe), cobalt (Co), and nickel (Ni), wherein the respective contents of these elements are individually as follows: - representing up to 100%, preferably at most 90%, preferably at most 70% and even more preferably at most 50% of the Ti content, with the total content of these metals never exceeding 15% by weight, preferably at most 10% by weight, of the aluminium alloy of any one of claims 1 to 3, or - 0.1 to 2% by weight, provided that the total content of these metals in the aluminium alloy of any one of claims 1 to 3 constitutes at most 15% by weight, preferably at most 10% by weight.

5. 5. An aluminum alloy according to claim 1, characterized in that it contains calcium (Ca) in a content ranging from 0.1% to 5% by weight, preferably in the range of more than 0.5% to 5% by weight, particularly preferably in the range of 0.7% to 3% by weight.

6. 6. An aluminum alloy according to claim 1, characterized in that it contains, in addition to aluminum and inevitable impurities, only metals having a higher vaporization enthalpy or a lower vapor pressure than aluminum.

7. 7. An aluminum alloy according to claim 1, which is free of magnesium and / or manganese.

8. An aluminum alloy comprising the alloy components set forth in claim 1.

9. An aluminum alloy according to any one of claims 1 to 8, characterized in that, excluding inevitable impurities, it consists of the following: Al, Ti, Sc, Zr and one, two or more metals according to claim 4. - Al, Ti, Sc, Zr and Cr. The Cr content is in the range of 0.2 to 3.5 wt %, preferably 0.5 to 3.0 wt %. Al, Ti, Sc, Zr and Ni, the Ni content being in the range of 0.2 to 2.5% by weight, preferably 0.5 to 2.0% by weight. Al, Ti, Sc, Zr and Mo. The Mo content is in the range of 0.1 to 1.3% by weight, preferably 0.5 to 1.0% by weight. Al, Ti, Sc, Zr and Fe, the Fe content being in the range of 0.1 to 2.5% by weight, preferably 0.5 to 2.0% by weight. - Al, Ti, Sc, Zr and Ca. The Ca content is in the range of 0.1 to 5% by weight, preferably in the range of more than 0.5 to 5% by weight, particularly preferably in the range of 0.7 to 5% by weight.

10. 10. A method for additively manufacturing a lightweight component precursor from an aluminium alloy according to any one of claims 1 to 9, comprising: a) The metals are melted together to form a melt of aluminum alloy. b) forcibly cooling or allowing the aluminum alloy melt to cool, b1) by a rapid solidification process at a cooling rate of 1,000 K / s to 10,000,000 K / s, in particular 100,000 K / s to 1,000,000 K / s, for example by melt spinning, powder atomization in gas or water, strip casting or spray forming, to obtain a solidified aluminum alloy, optionally in powder form, containing scandium in solid solution, or b2) A cooling process results in a solidified aluminum alloy. c) grinding the aluminum alloy of step b1) or b2) into powder;

11. 10. A method for additively manufacturing a lightweight component precursor from an aluminium alloy according to any one of claims 1 to 9, comprising: d) producing a powder bed from the powder obtained in step c) of claim 10. e) Additive manufacturing of three-dimensional lightweight component precursors in a powder bed laser melting process by locally laser melting the powder and forcing or causing the locally melted areas to cool, resulting in a lightweight component precursor from an aluminum alloy with scandium in solid solution.

12. A method for producing a lightweight member, comprising heat treating a precursor of the lightweight member obtained by the method according to claim 11 at a temperature at which the precursor of the lightweight member hardens by precipitation hardening.

13. A lightweight component precursor obtainable by the method according to claim 11.

14. A lightweight component obtainable by the method according to claim 12.

15. 11. Use of an aluminum alloy according to any one of claims 1 to 9 or a powder obtainable by the method according to claim 10 for producing a lightweight component precursor by selective laser melting followed by selective laser melting and subsequent precipitation hardening.