Copolymer, compression molded body, transfer molded body, and compressed member
Patent Information
- Application Number
- JP2022149284
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-09-30
- Filing Date
- 2022-09-20
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2041-09-30
AI Technical Summary
Existing fluororesins, such as tetrafluoroethylene/perfluoroalkyl vinyl ether copolymers, face challenges in maintaining sealing properties at high temperatures, resisting electrolyte leakage, and preventing fluorine ion elution, while also requiring excellent moldability and resistance to mold corrosion.
A copolymer with specific compositions of tetrafluoroethylene and perfluoro(propyl vinyl ether) units, within defined ranges of 2.0 to 2.7% PPVE content, melt flow rates of 0.8 to 7.0 g/10 minutes, and limited functional groups, enhancing glass transition temperature, moldability, and reducing water vapor and electrolyte permeability.
The copolymer achieves excellent sealing properties at high temperatures, low electrolyte permeability, and resistance to fluorine ion elution, with improved moldability and reduced mold corrosion, suitable for applications requiring high thermal and chemical resistance.
Smart Images

Figure 00000026_0000
Abstract
Description
[Technical Field]
[0001] This disclosure relates to copolymers, compression molded articles, transfer molded articles, and members to be compressed. [Background technology]
[0002] Tetrafluoroethylene / perfluoroalkyl vinyl ether copolymer (PFA) is known as a fluororesin that has excellent mechanical, chemical, and electrical properties, and is also melt-processable.
[0003] For example, Patent Document 1 describes a sealing material comprising a fluorine-containing polymer having polymerization units based on tetrafluoroethylene and polymerization units based on one or more types of perfluoro(alkyl vinyl ether), wherein the fluorine-containing polymer is characterized in that the polymerization units based on perfluoro(alkyl vinyl ether) are 4.0% by mass or less of the total polymerization units, and the melt flow rate is 0.1 to 100 g / 10 min. [Prior art documents] [Patent Documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 2013-177574 [Overview of the project] [Problems that the invention aims to solve]
[0005] The present disclosure aims to provide a copolymer that has a high glass transition temperature, is less likely to corrode molds used for molding, has excellent moldability and electrical properties, and furthermore has excellent low water vapor permeability and low electrolyte permeability, is less likely to leak electrolyte, maintains appropriate compression set properties, has extremely excellent sealing properties at high temperatures, and can produce a molded article that is less likely to leach fluoride ions into the electrolyte. [Means for solving the problem]
[0006] According to the present disclosure, there is provided a copolymer containing tetrafluoroethylene units and perfluoro(propyl vinyl ether) units, wherein the content of perfluoro(propyl vinyl ether) units is 2.0 to 2.7% by mass based on all monomer units, the melt flow rate at 372 °C is 0.8 to 7.0 g / 10 min, and the number of functional groups is 50 or less per 10 main chain carbon atoms. 6
[0007] Further, according to the present disclosure, there is provided a compression molded article containing the above copolymer.
[0008] Further, according to the present disclosure, there is provided an extruded molded article containing the above copolymer.
[0009] Further, according to the present disclosure, there is provided a transfer molded article containing the above copolymer.
[0010] Further, according to the present disclosure, there is provided a compressed member containing the above copolymer.
[0011] Further, according to the present disclosure, there is provided a film containing the above copolymer.
[0012] Further, according to the present disclosure, there is provided a tube containing the above copolymer.
[0013] Further, according to the present disclosure, there is provided a coated electric wire having a coating layer containing the above copolymer.
Advantages of the Invention
[0014] According to the present disclosure, there is provided a copolymer having a high glass transition temperature, being difficult to corrode the mold used for molding, excellent in moldability and electrical properties, further excellent in low water vapor permeability and low electrolyte permeability, being difficult to leak electrolyte, maintaining appropriate compression set properties, extremely excellent in sealing properties at high temperatures, and being difficult to elute fluoride ions into the electrolyte, and a molded article can be obtained. [Brief explanation of the drawing]
[0015] [Figure 1] Figure 1 is a schematic cross-sectional view of a test fixture used for electrolyte leakage testing. [Modes for carrying out the invention]
[0016] The following describes specific embodiments of this disclosure in detail, but this disclosure is not limited to the embodiments described below.
[0017] The copolymers of this disclosure contain tetrafluoroethylene (TFE) units and perfluoro(propyl vinyl ether) (PPVE) units.
[0018] Patent Document 1 states that in-vehicle secondary batteries are sometimes exposed to high temperatures of 85°C or higher in their operating environment, and in order to maintain airtightness and liquid tightness inside the battery, it is important that the sealing material maintains sufficient compressibility and recovery even under such harsh operating conditions, and that a high degree of adhesion between the battery case and the sealing body can be maintained.
[0019] However, there is a need for copolymers that can exhibit excellent sealing properties even in higher temperature environments. In particular, there is a need for copolymers that can exhibit excellent sealing properties even at temperatures exceeding the glass transition temperature of the copolymer.
[0020] It was found that by appropriately adjusting the PPVE unit content, melt flow rate (MFR), and number of functional groups of a copolymer containing TFE units and PPVE units, the glass transition temperature of the copolymer can be sufficiently increased, resulting in excellent heat resistance. This copolymer exhibits excellent moldability and is less corrosive to the mold used for molding, making it suitable for, for example, transfer molding. Furthermore, it was also found that molded articles containing such copolymers exhibit excellent low water vapor and electrolyte permeability, making them less prone to electrolyte leakage, maintaining appropriate compression set properties, and exhibiting extremely excellent sealing properties at high temperatures, while also being less likely to leach fluoride ions into the electrolyte. In addition, it was found that molded articles containing such copolymers also exhibit excellent electrical properties.
[0021] The copolymer of this disclosure is a melt-processable fluororesin. Melt-processability means that the polymer can be melted and processed using conventional processing equipment such as extruders and transfer molding machines.
[0022] The PPVE unit content of the copolymer is 2.0 to 2.7% by mass relative to the total monomer units. Preferably, the PPVE unit content of the copolymer is 2.1% by mass or more, more preferably 2.2% by mass or more, even more preferably 2.3% by mass or more, still more preferably 2.4% by mass or more, preferably 2.6% by mass or less, and more preferably 2.5% by mass or less. By having the PPVE unit content of the copolymer within the above range, it is possible to obtain a copolymer with an even higher glass transition temperature, which provides excellent low water vapor permeability and low electrolyte permeability, makes it difficult for the electrolyte to leak, maintains appropriate compression set properties, and provides a copolymer that gives an extremely good sealing performance at high temperatures.
[0023] The content of the TFE unit in the copolymer is preferably 97.3 to 98.0% by mass, more preferably 97.9% by mass or more, still more preferably 97.8% by mass or less, yet still more preferably 97.7% by mass or less, particularly preferably 97.7% by mass or less, most preferably 97.6% by mass or less, more preferably 97.4% by mass or more, and still more preferably 97.5% by mass or more, based on all monomer units. By having the content of the TFE unit in the copolymer within the above range, a copolymer with a higher glass transition temperature can be obtained, which is excellent in low water vapor permeability and low electrolyte permeability, difficult to leak electrolyte, and can provide a molded body that is extremely excellent in sealing property at high temperatures while appropriately maintaining the compression set property.
[0024] In the present disclosure, the content of each monomer unit in the copolymer is 19 measured by the F-NMR method.
[0025] The copolymer may also contain monomer units derived from monomers copolymerizable with TFE and PPVE. In this case, the content of the monomer units copolymerizable with TFE and PPVE is preferably 0 to 4.0% by mass, more preferably 0.05 to 0.7% by mass, and still more preferably 0.1 to 0.5% by mass, based on all monomer units of the copolymer.
[0026] Examples of the monomer copolymerizable with TFE and PPVE include hexafluoropropylene (HFP), CZ 1 Z 2 =CZ 3 (CF2) n Z 4 (where Z 1 , Z 2 and Z 3 are the same or different and represent H or F, Z 4 represents H, F or Cl, and n represents an integer of 2 to 10.) vinyl monomers represented by, and CF2=CF-OCH2-Rf 1 (where Rf 1represents a perfluoroalkyl group having 1 to 5 carbon atoms. Examples include alkyl perfluorovinyl ether derivatives represented by ). Among these, HFP is preferred.
[0027] As the copolymer, at least one selected from the group consisting of copolymers comprising only TFE units and PPVE units, and TFE / HFP / PPVE copolymers is preferred, and copolymers comprising only TFE units and PPVE units are more preferred.
[0028] The melt flow rate (MFR) of the copolymer is 0.8 to 7.0 g / 10 min. Preferably, the MFR of the copolymer is 1.0 g / 10 min or more, more preferably 1.2 g / 10 min or more, particularly preferably 1.5 g / 10 min or more, most preferably 1.8 g / 10 min or more, preferably 6.0 g / 10 min or less, more preferably 5.5 g / 10 min or less, even more preferably 5.0 g / 10 min or less, and particularly preferably 4.8 g / 10 min or less. By having the MFR of the copolymer within the above range, a copolymer is obtained that exhibits excellent low water vapor permeability and low electrolyte permeability, is less prone to electrolyte leakage, maintains appropriate compression set properties, and provides a molded article with extremely excellent sealing properties, especially at high temperatures. Furthermore, because the MFR of the copolymer is within the above range, the copolymer exhibits high moldability and can be molded by compression molding, transfer molding, extrusion molding, etc.
[0029] Furthermore, by setting the MFR of the copolymer to 3.8 g / 10 min or less, preferably 3.4 g / 10 min or less, and even more preferably 3.0 g / 10 min or less, a copolymer that is less prone to deformation even in a molten state can be obtained. By using such a copolymer, large-diameter pipes with high dimensional accuracy can be easily obtained by extrusion molding.
[0030] In this disclosure, MFR is a value obtained in accordance with ASTM D1238 as the mass (g / 10 min) of polymer flowing out of a nozzle with an inner diameter of 2.1 mm and a length of 8 mm per 10 minutes using a melt indexer at 372°C and a load of 5 kg.
[0031] MFR can be adjusted by adjusting the type and amount of polymerization initiator and chain transfer agent used when polymerizing monomers.
[0032] In this disclosure, the main chain number of the copolymer is 10 6 The number of functional groups per molecule is 50 or less. The main chain number of the copolymer is 10 6 The number of functional groups per molecule is preferably 40 or less, more preferably 30 or less, even more preferably 20 or less, still more preferably 15 or less, particularly preferably 10 or less, and most preferably less than 6. By having the number of functional groups of the copolymer within the above range, the copolymer is less likely to corrode the mold during molding using a mold, and the electrical properties of the copolymer can be further improved. Furthermore, a copolymer can be obtained that provides a molded article that is less likely to leak electrolyte and less likely to dissolve fluoride ions into the electrolyte. In addition, by having the number of functional groups of the copolymer within the above range, it is possible to suppress the decomposition of functional groups of the copolymer, which generates gas and causes molding defects such as foaming.
[0033] Infrared spectroscopy can be used to identify the types of functional groups and measure their number.
[0034] The number of functional groups is specifically measured by the following method. First, the copolymer is molded by cold pressing to produce a film with a thickness of 0.25 to 0.3 mm. This film is analyzed by Fourier transform infrared spectroscopy to obtain the infrared absorption spectrum of the copolymer, and a difference spectrum is obtained from this spectrum to the base spectrum where the copolymer is completely fluorinated and no functional groups are present. From the absorption peaks of specific functional groups appearing in this difference spectrum, the number of carbon atoms in the copolymer (1 × 10) is determined according to the following formula (A). 6 Calculate the number of functional units N per individual.
[0035] N = I × K / t (A) I: Absorbance K: Correction coefficient t: Film thickness (mm)
[0036] For reference, Table 1 shows the absorption frequency, molar extinction coefficient, and correction factor for several functional groups. The molar extinction coefficient was determined from FT-IR measurement data of a small molecule model compound. [Table 1]
[0037] The absorption frequencies of -CH2CF2H, -CH2COF, -CH2COOH, -CH2COOCH3, and -CH2CONH2 are tens of kaiser (cm) from the absorption frequencies of -CF2H, -COF, -COOH free and -COOH bonded, -COOCH3, and -CONH2, respectively, as shown in the table. -1 ) It will become lower.
[0038] For example, the number of functional groups in -COF is the absorption frequency of 1883 cm⁻¹ due to -CF₂COF. -1 The number of functional groups determined from the absorption peak and the absorption frequency of 1840 cm² due to -CH2COF -1 This is the sum of the number of functional groups determined from the absorption peaks.
[0039] Functional groups are functional groups located at the ends of the main chain or side chains of the copolymer, and functional groups located within the main chain or side chains. The number of functional groups may be the total number of -CF=CF2, -CF2H, -COF, -COOH, -COOCH3, -CONH2, and -CH2OH.
[0040] The functional groups described above are introduced into the copolymer, for example, by chain transfer agents or polymerization initiators used in the production of the copolymer. For instance, if an alcohol is used as a chain transfer agent, or if a peroxide having the structure -CH2OH is used as a polymerization initiator, -CH2OH is introduced to the main chain ends of the copolymer. Alternatively, the functional groups can be introduced to the side chain ends of the copolymer by polymerizing monomers having the functional groups.
[0041] By fluorinating a copolymer having such functional groups, a copolymer having a number of functional groups within the above range can be obtained. That is, it is preferable that the copolymer of this disclosure is fluorinated. It is also preferable that the copolymer of this disclosure has a -CF3 terminal group.
[0042] The melting point of the copolymer is preferably 305 to 317°C, and more preferably 305 to 315°C. Having the melting point within this range makes it possible to obtain a copolymer that provides a molded article with even better sealing properties, especially at high temperatures.
[0043] In this disclosure, the melting point can be measured using a differential scanning calorimetry (DSC).
[0044] The glass transition temperature (Tg) of the copolymer is preferably 95.0°C or higher, more preferably 98.8°C or higher, more preferably 99.0°C or higher, preferably 110.0°C or lower, more preferably 105.0°C or lower, and even more preferably 103.0°C or lower. Because the copolymer of this disclosure can have such a high glass transition temperature, it is possible to obtain a copolymer that exhibits excellent heat resistance and provides a molded article with even better sealing properties, especially at high temperatures.
[0045] In this disclosure, the glass transition temperature can be measured by dynamic viscoelasticity measurement.
[0046] The water vapor permeability of the copolymer is preferably 11.0 g·cm / m 2 The following, and more preferably 10.0 g·cm / m 2 The following, and more preferably 9.8 g·cm / m 2 The following applies: The copolymer of the present disclosure has excellent low water vapor permeability because the content of PPVE units and the melt flow rate (MFR) of the copolymer containing TFE units and PPVE units are appropriately adjusted. Therefore, by using a molded body containing the copolymer of the present disclosure as, for example, a compressible component of a secondary battery, it is possible to effectively prevent the intrusion of moisture even under high temperature and high humidity conditions.
[0047] In this disclosure, water vapor transmission can be measured under conditions of 95°C for 30 days. Specific measurements of water vapor transmission can be performed by the method described in the examples.
[0048] The electrolyte permeability of the copolymer is preferably 8.8 g·cm / m 2 The following, and more preferably 8.6 g·cm / m 2 The following applies: The copolymer of this disclosure has excellent electrolyte low permeability because the content of PPVE units, melt flow rate (MFR), and number of functional groups of the copolymer containing TFE units and PPVE units are appropriately adjusted. Therefore, by using a molded body containing the copolymer of this disclosure as, for example, a compressible member of a secondary battery, the permeation of the electrolyte contained in the secondary battery can be effectively prevented.
[0049] In this disclosure, the specific measurement of electrolyte permeability can be performed by the method described in the examples.
[0050] The copolymer of this disclosure has an amount of eluted fluoride ions detected in an electrolyte immersion test that is preferably 1.0 ppm or less, more preferably 0.8 ppm or less, and even more preferably 0.7 ppm or less, on a mass basis. Having the amount of eluted fluoride ions within the above range can further suppress the generation of gases such as HF in non-aqueous electrolyte batteries, and further suppress the deterioration of battery performance and shortening of battery life of non-aqueous electrolyte batteries.
[0051] In this disclosure, the electrolyte immersion test can be performed by preparing a test piece using a copolymer with a weight equivalent to 10 molded bodies (15 mm × 15 mm × 0.2 mm), and placing a glass sample bottle containing the test piece and 2 g of dimethyl carbonate (DMC) in a constant temperature bath at 80°C for 144 hours.
[0052] The copolymers of this disclosure can maintain appropriate compression set properties, thereby providing molded articles with excellent sealing properties at low temperatures. The sealing properties at low temperatures can be evaluated by measuring the compression set rate at 65°C. Copolymers with a low compression set rate at 65°C can provide molded articles with excellent sealing properties at low temperatures.
[0053] The copolymer of this disclosure preferably has a compression set of 45 to 80%, more preferably 70 to 80%, and more preferably 72 to 77%, when measured after being left at 65°C for 72 hours under conditions of a 50% compressibility. Having a compression set within the above range at 65°C allows the molded article containing the copolymer to maintain sufficient rebound elasticity for a long period of time when used, for example, as a compressible member.
[0054] In this disclosure, the compression set can be measured in accordance with the method described in ASTM D395 or JIS K6262:2013.
[0055] As described above, the copolymers of this disclosure can provide molded articles with extremely excellent sealing properties at high temperatures while appropriately maintaining compression set properties. Sealing properties at high temperatures can be evaluated by measuring the storage modulus (E'), recovery amount at 150°C, and surface pressure at 150°C. Copolymers with a high storage modulus (E') and a large recovery amount at 150°C enable sufficient rebound elasticity to be maintained for a long period of time even at high temperatures. Furthermore, copolymers with a high surface pressure at 150°C can provide molded articles with excellent sealing properties at high temperatures. The copolymers of this disclosure can provide molded articles that exhibit extremely excellent sealing properties even at high temperatures exceeding the glass transition temperature of the copolymer.
[0056] The storage modulus (E') of the copolymer at 150°C is preferably 120 MPa or higher, more preferably 130 MPa or higher, even more preferably 135 MPa or higher, preferably 1000 MPa or lower, more preferably 500 MPa or lower, and even more preferably 300 MPa or lower. By having the storage modulus (E') of the copolymer at 150°C within the above range, sufficient rebound elasticity can be maintained for a long period even at high temperatures, resulting in a copolymer that provides a molded article with extremely excellent sealing properties at high temperatures.
[0057] The storage modulus (E') can be measured by dynamic viscoelasticity testing in the range of 30 to 250°C under conditions of a heating rate of 2°C / min and a frequency of 10 Hz. The storage modulus (E') at 150°C can be increased by adjusting the PPVE unit content and melt flow rate (MFR) of the copolymer.
[0058] The copolymer has a very high surface pressure at 150°C. The surface pressure of the copolymer at 150°C is preferably 1.80 MPa or higher, more preferably 1.85 MPa or higher, and even more preferably 1.99 MPa or higher, and there is no particular upper limit, but it may be 3.0 MPa or lower. The surface pressure at 150°C can be increased by adjusting the PPVE unit content, melt flow rate (MFR), and number of functional groups of the copolymer.
[0059] The surface pressure can be calculated by measuring the height of the specimen (height of the specimen after compression deformation) after deforming the specimen obtained from the copolymer to a compression deformation rate of 50%, leaving it at 150°C for 18 hours, releasing the compression, leaving it at room temperature for 30 minutes, and then using the following formula from the height of the specimen after compression deformation and the storage modulus of elasticity (MPa) at 150°C. Surface pressure at 150℃ (MPa) = (t2-t1) / t1 × E' t1: Original height of the test specimen before compression deformation (mm) × 50% t2: Height of the test specimen after compression deformation (mm) E': Storage modulus at 150°C (MPa)
[0060] The amount of recovery of a copolymer at 150°C can be measured using the same method as for measuring surface pressure. The amount of recovery of a molded body at 150°C is the difference (t2-t1) between the height of the test specimen after compression deformation (t2) and the original height of the test specimen before compression deformation (t1), when the test specimen is deformed at a compression deformation rate of 50%. The amount of recovery of a molded body at 150°C can be increased by adjusting the PPVE unit content, melt flow rate (MFR), and number of functional groups of the copolymer.
[0061] The dielectric loss tangent of the copolymer of this disclosure at 6 GHz is preferably 6.0 × 10⁻⁶. -4 The following, more preferably 5.0 × 10 -4 The following, and more preferably 4.0 × 10 -4 The following is the case. In recent years, with the increasing amount of information to be transmitted, there has been a growing tendency to use radio waves in the higher frequency range. For example, microwaves in the 3-30 GHz range are used in high-frequency wireless LANs, satellite communications, and mobile phone base stations. Materials with a low dielectric loss tangent (tanδ) are required for materials used in communication equipment that uses such high frequencies. It is preferable that the dielectric loss tangent of the copolymer of this disclosure is within the above range, as this greatly reduces the attenuation rate of high-frequency signals.
[0062] In this disclosure, the dielectric loss tangent is a value obtained by measuring the changes in resonant frequency and electric field strength using an Agilent Technologies network analyzer and cavity resonator under a temperature range of 20 to 25°C.
[0063] The copolymers of this disclosure can be produced by polymerization methods such as suspension polymerization, solution polymerization, emulsion polymerization, and bulk polymerization. Emulsion polymerization or suspension polymerization is preferred as the polymerization method. In these polymerizations, various conditions such as temperature and pressure, polymerization initiators, and other additives can be appropriately set according to the composition and amount of the copolymer.
[0064] As polymerization initiators, oil-soluble radical polymerization initiators or water-soluble radical polymerization initiators can be used.
[0065] The oil-soluble radical polymerization initiator may be a known oil-soluble peroxide, for example, Dialkyl peroxycarbonates such as dinormal propyl peroxydicarbonate, diisopropyl peroxydicarbonate, disec-butyl peroxydicarbonate, and di-2-ethoxyethyl peroxydicarbonate; Peroxy esters such as t-butyl peroxyisobutyrate and t-butyl peroxypivalate; Dialkyl peroxides such as di-t-butyl peroxide; Di[fluoro(or fluorochloro)acyl]peroxides; These are some typical examples.
[0066] Examples of di[fluoro(or fluorochloro)acyl]peroxides include diacylperoxides represented as [(RfCOO)-]2 (where Rf is a perfluoroalkyl group, an ω-hydroperfluoroalkyl group, or a fluorochloroalkyl group).
[0067] Examples of di[fluoro(or fluorochloro)acyl]peroxides include di(ω-hydro-dodecafluorohexanoyl)peroxide, di(ω-hydro-tetradecafluoroheptanoyl)peroxide, di(ω-hydro-hexadecafluorononanoyl)peroxide, di(perfluoropropionyl)peroxide, di(perfluorobutyryl)peroxide, di(perfluoropareryl)peroxide, di(perfluorohexanoyl)peroxide, di(perfluoroheptanoyl)peroxide, di(perfluorooctanoyl)peroxide, di(perfluorononanoyl)peroxide, di(ω-chloro-hexafluorobutyryl)peroxide, and di(ω-chloro-decafluorohexa Examples include (noyl) peroxide, di(ω-chloro-tetradecafluorooctanoyl) peroxide, ω-hydro-dodecafluoroheptanoyl-ω-hydrohexadecafluorononanoyl-peroxide, ω-chloro-hexafluorobutyryl-ω-chloro-decafluorohexanoyl-peroxide, ω-hydrododecafluoroheptanoyl-perfluorobutyryl-peroxide, di(dichloropentafluorobutanoyl) peroxide, di(trichlorooctafluorohexanoyl) peroxide, di(tetrachloroundecafluorooctanoyl) peroxide, di(pentachlorotetradecafluorodecanoyl) peroxide, and di(undecachlorotriacontafluorodocosanoyl) peroxide.
[0068] The water-soluble radical polymerization initiator may be a known water-soluble peroxide, such as ammonium salts, potassium salts, and sodium salts of persulfuric acid, perboric acid, perchloric acid, superphosphate, and percarbonate; organic peroxides such as disuccinate peroxide and diglutaric acid peroxide; t-butyl permalate; and t-butyl hydroperoxide. A reducing agent such as sulfites may also be used in combination with the peroxide, and the amount used may be 0.1 to 20 times the amount of the peroxide.
[0069] In polymerization, surfactants, chain transfer agents, and solvents can be used, and conventionally known surfactants can be used for each of these.
[0070] As the surfactant, known surfactants can be used, such as nonionic surfactants, anionic surfactants, and cationic surfactants. Among these, fluorine-containing anionic surfactants are preferred, and linear or branched fluorine-containing anionic surfactants having 4 to 20 carbon atoms are more preferred, which may contain ether-bonded oxygen (i.e., oxygen atoms may be inserted between carbon atoms). The amount of surfactant added (relative to polymerization water) is preferably 50 to 5000 ppm.
[0071] Examples of chain transfer agents include hydrocarbons such as ethane, isopentane, n-hexane, and cyclohexane; aromatics such as toluene and xylene; ketones such as acetone; acetic acid esters such as ethyl acetate and butyl acetate; alcohols such as methanol and ethanol; mercaptans such as methyl mercaptan; and halogenated hydrocarbons such as carbon tetrachloride, chloroform, methylene chloride, and methyl chloride. The amount of chain transfer agent added may vary depending on the magnitude of the chain transfer constant of the compound used, but it is usually used in the range of 0.01 to 20% by mass relative to the polymerization solvent.
[0072] Examples of solvents include water and mixed solvents of water and alcohol.
[0073] In suspension polymerization, a fluorinated solvent may be used in addition to water. Examples of fluorinated solvents include hydrochlorofluoroalkanes such as CH3CClF2, CH3CCl2F, CF3CF2CCl2H, and CF2ClCF2CFHCl; chlorofluoroalkanes such as CF2ClCFClCF2CF3 and CF3CFClCFClCF3; hydrofluoroalkanes such as CF3CFHCFHCF2CF2CF3, CF2HCF2CF2CF2CF2H, and CF3CF2CF2CF2CF2CF2CF2H; and CH3OC2F5 and CH3OC3F5. Examples include hydrofluoroethers such as CF3CF2CH2OCHF2, CF3CHFCF2OCH3, CHF2CF2OCH2F, (CF3)2CHCF2OCH3, CF3CF2CH2OCH2CHF2, and CF3CHFCF2OCH2CF3; and perfluoroalkanes such as perfluorocyclobutane, CF3CF2CF2CF3, CF3CF2CF2CF2CF3, and CF3CF2CF2CF2CF2CF3, with perfluoroalkanes being preferred. The amount of fluorinated solvent used is preferably 10 to 100% by mass relative to the aqueous medium, from the standpoint of suspension and economy.
[0074] The polymerization temperature is not particularly limited and may be between 0 and 100°C. The polymerization pressure is determined appropriately depending on the type and amount of solvent used, its vapor pressure, the polymerization temperature, and other polymerization conditions, but is usually between 0 and 9.8 MPaG.
[0075] If the polymerization reaction yields an aqueous dispersion containing the copolymer, the copolymer can be recovered by coagulating, washing, and drying the copolymer contained in the aqueous dispersion. Alternatively, if the polymerization reaction yields the copolymer as a slurry, the copolymer can be recovered by removing the slurry from the reaction vessel, washing, and drying it. Drying allows the copolymer to be recovered in powder form.
[0076] The copolymer obtained by polymerization may be formed into pellets. There are no particular limitations on the molding method for forming pellets, and conventionally known methods can be used. For example, one method involves melt-extruding the copolymer using a single-screw extruder, twin-screw extruder, or tandem extruder, and then cutting it to a predetermined length to form pellets. The extrusion temperature during melt-extrusion needs to be varied depending on the melt viscosity of the copolymer and the manufacturing method, and is preferably between the melting point of the copolymer + 20°C and the melting point of the copolymer + 140°C. There are no particular limitations on the method of cutting the copolymer, and conventionally known methods such as strand cutting, hot cutting, underwater cutting, and sheet cutting can be used. The obtained pellets may be heated to remove volatile components (degassing treatment). The obtained pellets may also be treated by contacting them with hot water at 30-200°C, steam at 100-200°C, or hot air at 40-200°C.
[0077] The copolymer obtained by polymerization may be subjected to fluorination treatment. Fluorination treatment can be carried out by contacting an unfluorinated copolymer with a fluorine-containing compound. Fluorination treatment can convert thermally unstable functional groups such as -COOH, -COOCH3, -CH2OH, -COF, -CF=CF2, and -CONH2, as well as thermally relatively stable functional groups such as -CF2H, into the thermally extremely stable -CF3. As a result, the total number of -COOH, -COOCH3, -CH2OH, -COF, -CF=CF2, -CONH2, and -CF2H (number of functional groups) in the copolymer can be easily adjusted to the range described above.
[0078] The fluorine-containing compound is not particularly limited, but examples include fluorine radical sources that generate fluorine radicals under fluorination treatment conditions. Examples of the above fluorine radical sources include F2 gas, CoF3, AgF2, UF6, OF2, N2F2, CF3OF, and halogenated fluorides (e.g., IF5, ClF3).
[0079] Fluorine radical sources such as F2 gas may be at 100% concentration, but for safety reasons, it is preferable to mix them with an inert gas and dilute them to 5-50% by mass, and more preferably to 15-30% by mass. Examples of the inert gas include nitrogen gas, helium gas, and argon gas, but nitrogen gas is preferred for economic reasons.
[0080] The conditions for the fluorination treatment are not particularly limited, and the copolymer may be brought into contact with a fluorine-containing compound in a molten state. However, it is usually carried out at a temperature below the melting point of the copolymer, preferably 20 to 240°C, and more preferably 100 to 220°C. The above fluorination treatment is generally carried out for 1 to 30 hours, preferably 5 to 25 hours. The fluorination treatment is preferably carried out by bringing the unfluorinated copolymer into contact with fluorine gas (F2 gas).
[0081] A composition may be obtained by mixing the copolymer of the present disclosure with other components as needed. Examples of other components include fillers, plasticizers, processing aids, mold release agents, pigments, flame retardants, lubricants, light stabilizers, weather stabilizers, conductive agents, antistatic agents, ultraviolet absorbers, antioxidants, foaming agents, fragrances, oils, softeners, and hydrofluoricating agents.
[0082] Examples of fillers include silica, kaolin, clay, organic clay, talc, mica, alumina, calcium carbonate, calcium terephthalate, titanium dioxide, calcium phosphate, calcium fluoride, lithium fluoride, cross-linked polystyrene, potassium titanate, carbon, boron nitride, carbon nanotubes, and glass fibers. Examples of conductive agents include carbon black. Examples of plasticizers include dioctyl phthalate and pentaerythritol. Examples of processing aids include carnauba wax, sulfone compounds, low molecular weight polyethylene, and fluorine-based aids. Examples of dehydrofluoridating agents include organonium and amidines.
[0083] Other polymers besides the copolymers described above may be used as the other components. Examples of other polymers include fluororesins, fluororubbers, and non-fluorinated polymers other than the copolymers described above.
[0084] Examples of methods for producing the above composition include a method of dry mixing the copolymer and other components, or a method of pre-mixing the copolymer and other components in a mixer and then melt-kneading them in a kneader, melt extruder, etc.
[0085] The copolymers or compositions described herein can be used as processing aids, molding materials, etc., but are preferably used as molding materials. Aqueous dispersions, solutions, suspensions, and copolymer / solvent systems of the copolymers described herein are also available and can be applied as coatings, or used for sealing, impregnation, and film casting. However, since the copolymers described herein have the properties described above, they are preferably used as molding materials.
[0086] A molded article may be obtained by molding the copolymer of the present disclosure or the above composition.
[0087] The method for molding the above copolymer or composition is not particularly limited and includes compression molding, transfer molding, extrusion molding, blow molding, roto molding, roto lining molding, etc. Among the molding methods, compression molding, extrusion molding, or transfer molding is preferred, extrusion molding and transfer molding are more preferred due to their ease of production, and transfer molding is even more preferred because it allows for easy production of multiple pieces and produces uniform molded products, resulting in high productivity. In other words, the molded product is preferably an extruded product, a compression product, or a transfer product, and is even more preferred because it can be produced with high productivity.
[0088] The shape of the molded body is not particularly limited and may be, for example, a hose, pipe, tube, wire insulation, sheet, seal, gasket, packing, film, tank, roller, bottle, container, etc.
[0089] The copolymers, compositions, or molded articles of this disclosure can be used, for example, in the following applications: Food packaging films, lining materials for fluid transfer lines used in food manufacturing processes, packings, sealing materials, sheets, and other fluid transfer components for food manufacturing equipment; Chemical stoppers, packaging films, lining materials, packings, sealing materials, sheets, and other chemical liquid transfer components used in pharmaceutical manufacturing processes; Internal lining material for chemical tanks and piping in chemical plants and semiconductor factories; O-rings, tubes, gaskets, valve cores, hoses, seals, etc. used in the fuel systems and peripheral equipment of automobiles; fuel transfer components such as hoses and seals used in the automatic transmission systems of automobiles; Carburetor flange gaskets, shaft seals, valve stem seals, sealing materials, hoses, etc. used in automobile engines and peripheral equipment; other automotive components such as automobile brake hoses, air conditioning hoses, radiator hoses, and wire insulation materials; Chemical transfer components for semiconductor equipment, such as O-rings, tubes, packings, valve cores, hoses, sealing materials, rolls, gaskets, diaphragms, and fittings for semiconductor manufacturing equipment; Painting and ink-related components for painting equipment, such as paint rolls, hoses, tubes, and ink containers; Tubes or hoses for food and beverages, belts, gaskets, fittings and other components for transporting food and beverages, food packaging materials, glass cooking equipment; Tubes, hoses, and other components for transporting waste liquids; Components for transporting high-temperature liquids, such as tubes and hoses; Steam piping components such as tubes and hoses for steam piping; Corrosion-preventive tapes for pipes, such as tapes used to wrap around pipes on ship decks; Various coating materials such as wire coatings, optical fiber coatings, transparent surface coatings and backing materials for the light incident side surface of photovoltaic elements in solar cells; Sliding components of diaphragm pumps, such as diaphragms and various packings; Agricultural films, weather-resistant covers for various roofing materials and side walls; Interior materials used in the construction field, and coatings for glass such as non-combustible fire-resistant safety glass; Lining materials such as laminated steel sheets used in the home appliance sector;
[0090] Other fuel transfer components used in the fuel system of the above-mentioned automobile include fuel hoses, filler hoses, and evaporator hoses. These fuel transfer components can also be used as fuel transfer components for sour-resistant gasoline, alcohol-resistant fuels, and fuels containing gasoline additives such as methyl tert-butyl ether and amines.
[0091] The chemical stoppers and packaging films for the above-mentioned chemicals have excellent chemical resistance to acids and other substances. Furthermore, corrosion-resistant tapes wrapped around chemical plant piping can also be used as chemical liquid transfer components.
[0092] Examples of the above-mentioned molded products include automobile radiator tanks, chemical tanks, bellows, spacers, rollers, gasoline tanks, waste liquid transport containers, high-temperature liquid transport containers, and fishing and aquaculture tanks.
[0093] The above-mentioned molded products also include components used in automobiles such as bumpers, door trims, instrument panels, food processing equipment, cooking equipment, water- and oil-repellent glass, lighting-related equipment, display panels and housings for office automation equipment, illuminated signs, displays, liquid crystal displays, mobile phones, printed circuit boards, electrical and electronic components, general merchandise, trash cans, bathtubs, unit baths, ventilation fans, and lighting frames.
[0094] The molded article containing the copolymer of this disclosure has excellent heat resistance and moldability, can be manufactured without corroding the mold when using a mold, has excellent low water vapor permeability and low electrolyte permeability, is less likely to leak electrolyte, maintains appropriate compression set properties, has extremely excellent sealing properties at high temperatures, and is less likely to leach fluoride ions into the electrolyte, making it suitable for use as a compressible member containing the copolymer. A transfer molding method is suitable as the molding method using the above-mentioned mold.
[0095] The compressible member of this disclosure exhibits an appropriate compression set and high surface pressure even when deformed at a high compression deformation rate. The compressible member of this disclosure can be used in a state of compression deformation at a compression deformation rate of 10% or more, and can be used in a state of compression deformation at a compression deformation rate of 20% or more or 25% or more. By using the compressible member of this disclosure in a state of compression deformation at such a high compression deformation rate, a certain rebound elasticity can be maintained for a long period of time, and sealing properties and insulation properties can be maintained for a long period of time.
[0096] The compressible member of this disclosure exhibits a high storage modulus, high recovery amount, and very high surface pressure even when deformed at high temperatures and with a high compressive deformation rate. The compressible member of this disclosure can be used in a state of compression deformation of 10% or more at 150°C or above, and can be used in a state of compression deformation of 20% or more or 25% or more at 150°C or above. By using the compressible member of this disclosure deformed at such high temperatures and with a high compressive deformation rate, a certain rebound elasticity can be maintained for a long period of time even at high temperatures, and sealing and insulating properties at high temperatures can be maintained for a long period of time.
[0097] The above compression deformation rate is the compression deformation rate of the part with the greatest compression deformation rate when the compressed member is used in a compressed state. For example, if a flattened member is used in a compressed state in the thickness direction, it is the compression deformation rate in the thickness direction. Also, for example, if only a part of the member is used in a compressed state, it is the compression deformation rate of the part with the greatest compression deformation rate among the compressed parts.
[0098] The size and shape of the compressible member of this disclosure may be set as appropriate depending on the application and are not particularly limited. The shape of the compressible member of this disclosure may be, for example, annular. Furthermore, the compressible member of this disclosure may have a circular, oval, or rounded-corner quadrilateral shape in plan view and have a through hole in its center.
[0099] The compressible member of this disclosure is preferably used as a component for constituting a non-aqueous electrolyte battery. The compressible member of this disclosure is particularly suitable as a component used in contact with the non-aqueous electrolyte in a non-aqueous electrolyte battery because it exhibits excellent low water vapor permeability and low electrolyte permeability, is less likely to leak electrolyte, maintains appropriate compression set properties, has extremely excellent sealing properties at high temperatures, and is less likely to dissolve fluoride ions into the electrolyte. In other words, the compressible member of this disclosure may have a liquid-contacting surface with the non-aqueous electrolyte in a non-aqueous electrolyte battery.
[0100] The compressible member of this disclosure does not easily dissolve fluoride ions into the non-aqueous electrolyte. Therefore, by using the compressible member of this disclosure, it is possible to suppress the increase in fluoride ion concentration in the non-aqueous electrolyte. As a result, by using the compressible member of this disclosure, it is possible to suppress the generation of gases such as HF in non-aqueous electrolyte batteries, and to suppress the deterioration of battery performance and shortening of the lifespan of non-aqueous electrolyte batteries.
[0101] The compressible member of this disclosure can further suppress the generation of gases such as HF in non-aqueous electrolyte batteries, and can further suppress the deterioration of battery performance and shortening of battery life of non-aqueous electrolyte batteries. Therefore, the amount of eluted fluoride ions detected in the electrolyte immersion test is preferably 1.0 ppm or less, preferably 0.8 ppm or less, and more preferably 0.7 ppm or less by mass. The electrolyte immersion test can be performed by preparing a test piece with a weight equivalent to 10 molded bodies (15 mm × 15 mm × 0.2 mm) using the compressible member, and placing a glass sample bottle containing the test piece and 2 g of dimethyl carbonate (DMC) in a constant temperature bath at 80°C for 144 hours.
[0102] The compressible member of this disclosure exhibits excellent liquid-tightness and low electrolyte permeability, making it difficult for the electrolyte to leak or permeate. Therefore, by using the compressible member of this disclosure, it is possible to suppress poor battery performance and shortened lifespan of non-aqueous electrolyte batteries.
[0103] The amount of electrolyte leakage from the compressed member in this disclosure is preferably 0.0030 g / 1000 hrs or less, and more preferably 0.0025 g / 1000 hrs or less, in order to further suppress poor battery performance and shortened lifespan of non-aqueous electrolyte batteries. The amount of electrolyte leakage from the compressed member can be measured by the method described in the examples.
[0104] The compressible member of this disclosure is impermeable to water vapor. Therefore, by using the compressible member of this disclosure, it is possible to suppress the permeation of water vapor into the secondary battery from the outside. As a result, by using the compressible member of this disclosure, it is possible to suppress the deterioration of the battery performance and shortening of the lifespan of a non-aqueous electrolyte battery.
[0105] The water vapor permeability of the compressible member in this disclosure is preferably 11.0 g·cm / m², as this can further suppress the deterioration of battery performance and shortening of the battery life of non-aqueous electrolyte batteries. 2 The following, and more preferably 10.0 g·cm / m 2 The following, and more preferably 9.8 g·cm / m 2 The following applies: Water vapor transmission can be measured under conditions of 95°C for 30 days.
[0106] Non-aqueous electrolyte batteries are not particularly limited as long as they contain a non-aqueous electrolyte, and examples include lithium-ion secondary batteries and lithium-ion capacitors. Furthermore, components constituting a non-aqueous electrolyte battery include sealing members and insulating members.
[0107] The above non-aqueous electrolyte is not particularly limited, but one or more known solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, γ-butyl lactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate can be used. The non-aqueous electrolyte battery may further include an electrolyte. The above electrolyte is not particularly limited, but LiClO4, LiAsF6, LiPF6, LiBF4, LiCl, LiBr, CH3SO3Li, CF3SO3Li, cesium carbonate, etc. can be used.
[0108] The compressible members of this disclosure can be suitably used, for example, as sealing members such as sealing gaskets and sealing packings, and insulating members such as insulating gaskets and insulating packings. Sealing members are members used to prevent leakage of liquid or gas or intrusion of liquid or gas from the outside. Insulating members are members used to insulate electricity. The compressible members of this disclosure may be members used for both sealing and insulating purposes.
[0109] The compressible member of this disclosure has excellent heat resistance and extremely good sealing properties at high temperatures, making it suitable for use in high-temperature environments. For example, the compressible member of this disclosure is suitable for use in environments where the maximum temperature is 40°C or higher. For example, the compressible member of this disclosure is suitable for use in environments where the maximum temperature is 150°C or higher. Situations in which the compressible member of this disclosure may reach such high temperatures include, for example, when the compressible member is attached to a battery in a compressed state and then other battery components are attached to the battery by welding, or when a non-aqueous electrolyte battery generates heat.
[0110] The compressible member of this disclosure exhibits excellent low water vapor permeability and low electrolyte permeability, making it difficult for the electrolyte to leak out, maintaining appropriate compression set properties, and exhibiting extremely excellent sealing properties at high temperatures. Because it is also difficult for fluoride ions to leach into the electrolyte, it can be suitably used as a sealing member or insulating member for non-aqueous electrolyte batteries. For example, during charging of batteries such as non-aqueous electrolyte secondary batteries, the battery temperature may temporarily exceed 40°C, and particularly temporarily exceed 150°C. Even when used in batteries such as non-aqueous electrolyte secondary batteries, deformed at high temperatures with a high compression deformation rate, and even when in contact with non-aqueous electrolyte at high temperatures, the compressible member of this disclosure maintains its high rebound elasticity. Therefore, when the compressible member of this disclosure is used as a sealing member, it exhibits excellent sealing properties, and these sealing properties are maintained for a long period even at high temperatures. Furthermore, because the compressible member of this disclosure contains the above-mentioned copolymer, it also possesses excellent insulating properties. Therefore, when the compressible member of this disclosure is used as an insulating member, it adheres firmly to two or more conductive members, preventing short circuits over a long period of time.
[0111] Since the copolymer of this disclosure has a low dielectric loss tangent at 6 GHz, it can be suitably used as a material for high-frequency signal transmission products.
[0112] The above-mentioned high-frequency signal transmission products are not particularly limited as long as they are products used for transmitting high-frequency signals, and include (1) molded boards such as insulating boards for high-frequency circuits, insulating materials for connecting components, and printed circuit boards, (2) molded bodies such as bases for high-frequency vacuum tubes and antenna covers, and (3) insulated wires such as coaxial cables and LAN cables. The above-mentioned high-frequency signal transmission products can be suitably used in equipment that utilizes microwaves, particularly microwaves in the 3 to 30 GHz range, such as satellite communication equipment and mobile phone base stations.
[0113] In the above-mentioned high-frequency signal transmission product, the copolymer of this disclosure can be suitably used as an insulator due to its low dielectric loss tangent.
[0114] As the molded plate in (1) above, a printed circuit board is preferred because it provides good electrical characteristics. The printed circuit board is not particularly limited, but examples include printed circuit boards for electronic circuits in mobile phones, various computers, communication equipment, etc. As the molded body in (2) above, an antenna cover is preferred because it has low dielectric loss.
[0115] As the coated wire described in (3) above, a coated wire having a coating layer containing the copolymer of the present disclosure is preferred. That is, a molded article containing the copolymer of the present disclosure can be suitably used as a coating layer.
[0116] Commercially available tetrafluoroethylene / fluoro(alkyl vinyl ether) copolymers are known to have a continuous operating temperature of 260°C. The continuous operating temperature refers to the maximum operating temperature that the polymer can continuously withstand. In recent years, there has been a growing need for copolymers that can be used in more demanding working environments, in other words, copolymers with continuous operating temperatures exceeding 260°C. Numerous real-world industrial applications in oil and gas fields are creating a need for melt-workable polymer materials with continuous operating temperatures exceeding 260°C to withstand the extremely high operating temperatures encountered during construction work and other operations. For example, during deep drilling, data communication cables can be exposed to temperatures exceeding 280°C within downhole wells. A molded article containing the copolymer of this disclosure can have a continuous operating temperature of 280°C. Even at the extremely high temperature of 280°C, the molded article containing the copolymer of this disclosure does not melt, and the coating layer formed by the molded article maintains its coating without forming rupture or cracks due to thermal load, allowing for continuous use. Therefore, the molded article containing the copolymer of this disclosure is suitable for use as a coating layer in coated electric wires used in environments where the maximum temperature exceeds 280°C.
[0117] The insulated wire comprises a core wire and a coating layer provided around the core wire and containing the copolymer of the present disclosure. For example, the coating layer can be an extruded body obtained by melt-extruding the copolymer of the present embodiment onto the core wire. Because the coating layer has excellent heat resistance and a low dielectric loss tangent, the insulated wire is suitable for high-frequency transmission cables, flat cables, heat-resistant cables, etc., and is particularly suitable for high-frequency transmission cables.
[0118] For the core wire material, metal conductor materials such as copper and aluminum can be used. The core wire is preferably 0.02 to 3 mm in diameter. The core wire diameter is more preferably 0.04 mm or more, even more preferably 0.05 mm or more, and particularly preferably 0.1 mm or more. The core wire diameter is more preferably 2 mm or less.
[0119] Specific examples of core wires include, for instance, AWG-46 (solid copper wire with a diameter of 40 micrometers), AWG-26 (solid copper wire with a diameter of 404 micrometers), AWG-24 (solid copper wire with a diameter of 510 micrometers), AWG-22 (solid copper wire with a diameter of 635 micrometers), etc.
[0120] The thickness of the coating layer is preferably 0.1 to 3.0 mm. A thickness of 2.0 mm or less is also preferable.
[0121] Examples of high-frequency transmission cables include coaxial cables. Coaxial cables generally have a structure in which an inner conductor, an insulating coating layer, an outer conductor layer, and a protective coating layer are laminated in order from the core to the outer periphery. The molded article containing the copolymer of this disclosure can be suitably used as an insulating coating layer containing the copolymer. The thickness of each layer in the above structure is not particularly limited, but typically the inner conductor has a diameter of about 0.1 to 3 mm, the insulating coating layer has a thickness of about 0.3 to 3 mm, the outer conductor layer has a thickness of about 0.5 to 10 mm, and the protective coating layer has a thickness of about 0.5 to 2 mm.
[0122] The coating layer may contain air bubbles, and it is preferable that the air bubbles are uniformly distributed within the coating layer.
[0123] The average bubble diameter is not limited, but is preferably 60 μm or less, more preferably 45 μm or less, even more preferably 35 μm or less, even more preferably 30 μm or less, particularly preferably 25 μm or less, and especially preferably 23 μm or less. Furthermore, the average bubble diameter is preferably 0.1 μm or more, and more preferably 1 μm or more. The average bubble diameter can be determined by taking an electron microscope image of the wire cross-section, calculating the diameter of each bubble through image processing, and averaging the results.
[0124] The coating layer may have a foaming rate of 20% or more. More preferably 30% or more, even more preferably 33% or more, and even more preferably 35% or more. There is no particular upper limit, but for example, it is 80%. The upper limit of the foaming rate may be 60%. The foaming rate is calculated as ((specific gravity of the wire coating material - specific gravity of the coating layer) / specific gravity of the wire coating material) × 100. The foaming rate can be appropriately adjusted according to the application, for example by adjusting the amount of gas inserted into the extruder as described later, or by selecting the type of gas to dissolve.
[0125] The insulated wire may have another layer between the core wire and the insulated layer, and may have yet another layer (outer layer) around the insulated layer. If the insulated layer contains air bubbles, the wire of this disclosure may have a two-layer structure (skin-foam) with a non-foamed layer inserted between the core wire and the insulated layer, a two-layer structure (foam-skin) with a non-foamed layer covering the outer layer, or a three-layer structure (skin-foam-skin) with a non-foamed layer covering the outer layer of the skin-foam. The non-foamed layer is not particularly limited and may be a resin layer made of TFE / HFP copolymer, TFE / PAVE copolymer, TFE / ethylene copolymer, vinylidene fluoride polymer, polyolefin resin such as polyethylene [PE], or resin such as polyvinyl chloride [PVC].
[0126] Insulated wires can be manufactured, for example, by using an extruder to heat a copolymer, extrude the molten copolymer onto a core wire, and form an insulated layer.
[0127] In forming the coating layer, the copolymer can be heated, and while the copolymer is molten, a gas can be introduced into the copolymer to form a coating layer containing bubbles. Examples of gases that can be used include chlorodifluoromethane, nitrogen, carbon dioxide, or mixtures thereof. The gas may be introduced as a pressurized gas into the heated copolymer, or it may be generated by mixing a chemical blowing agent into the copolymer. The gas dissolves in the molten copolymer.
[0128] Since the molded article containing the copolymer of this disclosure has excellent heat resistance, it can be suitably used as a film or tube containing the copolymer.
[0129] Copolymers of tetrafluoroethylene and fluoro(alkyl vinyl ether) are useful as release films and surface materials for rolls used in office automation equipment because they have excellent chemical and heat resistance and can be melt-molded. In recent years, the manufacturing of thin-film products has required high heat resistance to withstand thermal lamination, and in the field of office automation equipment, the increasing use of color and higher speeds have created a demanding situation where even higher heat resistance is required for the surface materials of the fixing part rolls.
[0130] The copolymers of this disclosure have appropriate adjustments to the content of PPVE units and melt flow rate (MFR) of the copolymers containing TFE units and PPVE units, and the films or tubes formed from these copolymers have high heat resistance. In the heat lamination process described above, it is necessary to be able to withstand a wide range of temperature conditions, from around 100 to 300°C, and because the copolymers of this disclosure have the above configuration, they can be suitably used even under harsh temperature conditions. Films containing the copolymers of this disclosure do not melt even at extremely high temperatures of 280°C, and due to their high glass transition temperature, they can withstand softening down to nearly 100°C. Therefore, films and tubes containing the copolymers of this disclosure are suitable for use as heat-resistant films in environments where the maximum temperature is 280°C or higher.
[0131] The above-mentioned release film can be manufactured by molding the copolymer of this disclosure by extrusion molding, calendering, press molding, compression molding, casting, etc. From the viewpoint of obtaining a uniform thin film, the release film can be manufactured by melt extrusion molding.
[0132] The copolymer of this disclosure can be formed into sheets, films, or tubes by extrusion molding, compression molding, press molding, or other methods to create the desired shape, and can be used as a surface material for OA equipment rolls or OA equipment belts. In particular, thin-walled tubes and films can be manufactured by extrusion molding.
[0133] The copolymer of this disclosure can be easily formed into a film of uniform thickness by extrusion molding. A molded article containing the copolymer of this disclosure can be suitably used as a film or sheet.
[0134] Although embodiments have been described above, it should be understood that various modifications to the form and details are possible without departing from the spirit and scope of the claims. [Examples]
[0135] Next, embodiments of the present disclosure will be described with reference to examples, but the present disclosure is not limited to such embodiments.
[0136] The numerical values for each example and comparative example were measured by the following method.
[0137] (Content in monomer units) The content of each monomer unit was measured using an NMR analyzer (e.g., Bruker BioSpin AVANCE300 high-temperature probe).
[0138] (Melt Flow Rate (MFR)) In accordance with ASTM D1238, the mass (g / 10 min) of polymer flowing out of a nozzle with an inner diameter of 2.1 mm and a length of 8 mm per 10 minutes was determined using a melt indexer G-01 (manufactured by Toyo Seiki Seisakusho Co., Ltd.) at 372°C under a 5 kg load.
[0139] (Number of functional groups) Copolymer pellets were molded by cold pressing to produce films with a thickness of 0.25-0.30 mm. These films were scanned 40 times using a Fourier transform infrared spectrometer (FT-IR, Spectrum One, PerkinElmer) to obtain infrared absorption spectra, and the difference spectrum from the base spectrum, which is completely fluorinated and lacks functional groups, was obtained. From the absorption peaks of specific functional groups appearing in this difference spectrum, the carbon atoms in the sample (1 × 10⁶) were analyzed according to the following formula (A). 6 The number of functional cards N per individual was calculated. N = I × K / t (A) I: Absorbance K: Correction coefficient t: Film thickness (mm) For reference, Table 2 shows the absorption frequency, molar extinction coefficient, and correction factor for the functional groups in this disclosure. The molar extinction coefficient was determined from FT-IR measurement data of a small molecule model compound.
[0140] [Table 2]
[0141] (Melting point) Using a differential scanning calorimeter (product name: X-DSC7000, manufactured by Hitachi High-Tech Science Corporation), the temperature was increased from 200°C to 350°C at a heating rate of 10°C / min, followed by cooling from 350°C to 200°C at a cooling rate of 10°C / min. A second heating was then performed from 200°C to 350°C at a heating rate of 10°C / min, and the melting point was determined from the melting curve peak generated during the second heating process.
[0142] (Glass transition temperature (Tg)) The glass transition temperature was determined by dynamic viscoelasticity measurements using a DVA-220 dynamic viscoelasticity analyzer (manufactured by IT Measurement Control Co., Ltd.). Measurements were taken at a heating rate of 2°C / min and a frequency of 10 Hz, and the temperature at the peak of the tanδ value was determined as the glass transition temperature.
[0143] Example 1 53.8 L of pure water was added to a 174 L autoclave, and after thorough nitrogen purging, 41.7 kg of perfluorocyclobutane, 0.51 kg of perfluoro(propyl vinyl ether) (PPVE), and 0.93 kg of methanol were charged, and the system temperature was maintained at 35°C and the stirring speed at 200 rpm. Next, tetrafluoroethylene (TFE) was injected under pressure to 0.5 MPa, and then 0.112 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate was added to start polymerization. As polymerization progressed, the system pressure decreased, so TFE was continuously supplied to keep the pressure constant, and 0.026 kg of PPVE was added for every 1 kg of TFE supplied, and polymerization was continued for 9 hours. After releasing the TFE and returning the autoclave to atmospheric pressure, the resulting reaction product was washed with water and dried to obtain 30 kg of powder.
[0144] The obtained powder was melt-extruded at 360°C using a screw extruder (product name: PCM46, manufactured by Ikegai Co., Ltd.) to obtain TFE / PPVE copolymer pellets. The PPVE content of the obtained pellets was measured using the method described above. The results are shown in Table 3.
[0145] The obtained pellets were placed in a vacuum vibration reactor VVD-30 (manufactured by Okawara Seisakusho Co., Ltd.) and heated to 210°C. After vacuuming, F2 gas diluted to 20% by volume with N2 gas was introduced to atmospheric pressure. 0.5 hours after the introduction of F2 gas, the reactor was vacuumed and F2 gas was introduced again. After another 0.5 hours, the reactor was vacuumed again and F2 gas was introduced again. Thereafter, the above operations of introducing F2 gas and vacuuming were continued once every hour, and the reaction was carried out at a temperature of 210°C for 10 hours. After the reaction was completed, the reactor was thoroughly replaced with N2 gas to terminate the fluorination reaction. Various physical properties were measured using the fluorinated pellets by the method described above. The results are shown in Table 3.
[0146] Example 2 Fluorinated pellets were obtained in the same manner as in Example 1, except that 0.55 kg of PPVE and 0.31 kg of methanol were used, with an additional 0.028 kg of PPVE added for every 1 kg of TFE supplied, the polymerization time was changed to 10 hours, the heating temperature of the vacuum vibrating reactor was changed to 160°C, and the reaction was changed to 5 hours at 160°C. The results are shown in Table 3.
[0147] Example 3 Fluorinated pellets were obtained in the same manner as in Example 1, except that 0.46 kg of PPVE was used, 0.100 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate was added without methanol, 0.024 kg of PPVE was added for every 1 kg of TFE supplied, and the polymerization time was changed to 8 hours. The results are shown in Table 3.
[0148] Example 4 Fluorinated pellets were obtained in the same manner as in Example 1, except that 0.40 kg of PPVE was used, 0.070 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate was added without methanol, 0.020 kg of PPVE was added for every 1 kg of TFE supplied, and the polymerization time was changed to 10 hours. The results are shown in Table 3.
[0149] Comparative Example 1 Pellets (non-fluorinated pellets) were obtained in the same manner as in Example 1, except that the amount of methanol was changed to 1.05 kg. The results are shown in Table 3.
[0150] Comparative Example 2 51.8 L of pure water was added to a 174 L autoclave, and after thorough nitrogen purging, 40.9 kg of perfluorocyclobutane, 0.37 kg of perfluoro(propyl vinyl ether) (PPVE), and 5.80 kg of methanol were charged, and the system temperature was maintained at 35°C and the stirring speed at 200 rpm. Next, tetrafluoroethylene (TFE) was injected under pressure to 0.64 MPa, and then 0.026 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate was added to start polymerization. As polymerization progressed, the system pressure decreased, so TFE was continuously supplied to keep the pressure constant, and 0.017 kg of PPVE was added for every 1 kg of TFE supplied. Polymerization was stopped when the amount of TFE added reached 40.9 kg. After releasing the unreacted TFE and returning the autoclave to atmospheric pressure, the resulting reaction product was washed with water and dried to obtain 41.1 kg of powder. The obtained powder was used to carry out a fluorination reaction in the same manner as in Example 1 to obtain fluorinated pellets. The results are shown in Table 3.
[0151] Comparative Example 3 Fluorinated pellets were obtained in the same manner as in Comparative Example 2, except that 0.67 kg of PPVE, 3.81 kg of methanol, 0.013 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate, and 0.022 kg of PPVE were added for every 1 kg of TFE supplied. The results are shown in Table 3.
[0152] Comparative Example 4 Fluorinated pellets were obtained in the same manner as in Comparative Example 2, except that 1.10 kg of PPVE and 3.90 kg of methanol were added, and an additional 0.030 kg of PPVE was added for every 1 kg of TFE supplied, resulting in 41.0 kg of powder. The results are shown in Table 3.
[0153] [Table 3]
[0154] In Table 3, the notation "<6" means that the number of functional groups is less than 6.
[0155] Next, the following characteristics were evaluated using the obtained pellets. The results are shown in Table 4.
[0156] (Water vapor transmission rate) Sheet-like test specimens with a thickness of approximately 0.2 mm were prepared using pellets and a heat press molding machine. (Test cup with a permeation area of 12.56 cm²) 2 18g of water was placed inside the container, covered with a sheet-like test piece, and sealed with a PTFE gasket. The sheet-like test piece was kept in contact with the water and maintained at 95°C for 30 days. After removal, it was left at room temperature for 2 hours and the mass loss was measured. The water vapor transmission rate (g·cm / m³) was calculated using the following formula. 2 ) was measured. Water vapor transmission rate (g·cm / m 2 ) = Mass loss (g) × Thickness of sheet-like test specimen (cm) / Permeation area (m²) 2 )
[0157] (Electrolyte leakage test) Copolymer pellets were placed in a mold (300mm x 300mm), preheated in an electric furnace at 350°C for 1 hour, and then pressurized at 1 MPaG for 1 minute to form a sheet of 300mm x 300mm x 25mm thickness. The sheet was then allowed to cool to room temperature to obtain a sample sheet (indicated as "HP" (heat press) in Table 4). The sample sheet was then machined to an outer diameter of Φ17.7mm, an inner diameter of Φ14.3mm, and a thickness of 1.6mmt to obtain a gasket.
[0158] As shown in Figure 1, 2 g of electrolyte 2 was placed in an aluminum alloy cup 1. The electrolyte contained ethylene carbonate (EC) and diethyl carbonate (DEC), with a volume ratio of EC to DEC (EC / DEC) of 30 / 70 (vol %). A gasket 7 was placed between cup 1 and gasket compression jig 3, and the lid 4 was tightened with bolts 5 to compress the gasket 7. A spacer 6 was placed between lid 4 and cup 1 to adjust the compression deformation rate of the gasket 7 to 50%. The mass of the test jig 10 obtained in this way was measured. The test jig 10 was placed in a constant temperature bath heated to 60°C, left for 1000 hours, removed, and its mass was measured after being left at room temperature for 2 hours. The amount of electrolyte leakage was calculated using the following formula. This operation was repeated 5 times, and the average amount of electrolyte leakage was calculated. The average values are listed in Table 4. Electrolyte leakage rate (g / 1000h) = (Mass of test fixture before heating) - (Mass of test fixture after heating)
[0159] (Compression set (CS)) The compression set was measured according to the methods described in ASTM D395 or JIS K6262:2013.
[0160] Approximately 2g of the above pellets was placed in a mold (inner diameter 13mm, height 38mm), melted at 370°C for 30 minutes using a hot plate press, and then water-cooled under pressure of 0.2MPa (resin pressure) to produce a molded body with a height of approximately 8mm. Subsequently, a test specimen with an outer diameter of 13mm and a height of 6mm was prepared by cutting the obtained molded body. The prepared test specimen was compressed at room temperature using a compression device to a compression deformation rate of 50% (i.e., the test specimen with a height of 6mm was compressed to a height of 3mm).
[0161] Next, the compressed specimen was left in the electric furnace, fixed to the compression device, and left at 65°C for 72 hours. The compression device was removed from the electric furnace, cooled to room temperature, and the specimen was removed. After leaving the recovered specimen at room temperature for 30 minutes, the height of the recovered specimen was measured, and the compression set was calculated using the following formula. Compression set (%) = (t0-t2) / (t0-t1) × 100 t0: Original height of the test specimen (mm) t1: Spacer height (mm) t2: Height of the test specimen removed from the compression device (mm) In the above test, t0 = 6 mm and t1 = 3 mm.
[0162] (Amount of restoration) The test specimens were prepared in the same manner as for measuring the compression set. The prepared test specimens were compressed to a compression deformation rate of 50% at room temperature using a compression device (i.e., a test specimen with a height of 6 mm was compressed to a height of 3 mm). The compressed test specimens were left in the compression device in an electric furnace and left at 150°C for 18 hours. The compression device was removed from the electric furnace, cooled to room temperature, and the test specimens were removed. After leaving the recovered test specimens at room temperature for 30 minutes, the height of the recovered test specimens was measured, and the amount of restoration was calculated using the following formula. Restoration amount (mm) = t2 - t1 t1: Spacer height (mm) t2: Height of the test specimen removed from the compression device (mm) In the above test, t1 = 3 mm.
[0163] (Storage modulus (E')) Dynamic viscoelasticity measurements were performed using a DVA-220 (manufactured by IT Measurement Control Co., Ltd.). As sample test pieces, heat-pressed sheets measuring 25 mm in length, 5 mm in width, and 0.2 mm in thickness were used. Measurements were taken in the range of 30°C to 250°C under conditions of a heating rate of 2°C / min and a frequency of 10 Hz, and the storage modulus (MPa) at 150°C was read.
[0164] (Surface pressure at 150°C) Based on the results of the compression set test at 150°C and the storage modulus measurement at 150°C, the surface pressure at 150°C was determined using the following formula. Surface pressure at 150℃ (MPa) = (t2-t1) / t1 × E' t1: Spacer height (mm) t2: Height of the test specimen removed from the compression device (mm) E': Storage modulus at 150°C (MPa)
[0165] (Electrolyte immersion test) Approximately 5g of the above pellets was placed in a mold (inner diameter 120mm, height 38mm), melted at 370°C for 20 minutes using a hot plate press, and then water-cooled under pressure of 1MPa (resin pressure) to produce a molded body with a thickness of approximately 0.2mm. Subsequently, a 15mm square test piece was prepared using the obtained molded body.
[0166] Ten test specimens and 2 g of electrolyte (dimethyl carbonate (DMC)) were placed in a 20 mL glass sample bottle, and the bottle cap was closed. The sample bottle was placed in an 80°C constant temperature bath and left for 144 hours to immerse the test specimens in the electrolyte. After that, the sample bottle was removed from the constant temperature bath and allowed to cool to room temperature before the test specimens were removed from the sample bottle. The electrolyte remaining in the sample bottle was air-dried in a room controlled at 25°C for 24 hours, and 2 g of ultrapure water was added. The resulting aqueous solution was transferred to the measurement cell of an ion chromatography system, and the amount of fluoride ions in this aqueous solution was measured using an ion chromatography system (Thermo Fisher Scientific Dionex ICS-2100).
[0167] (Mold corrosion test) 20g of pellets were placed in a glass container (50ml screw-top tube), and a metal column (5mm square, 30mm long) made of HPM38 (Cr plating) or HPM38 (Ni plating) was suspended from the glass container so as not to touch the pellets. The glass container was then covered with aluminum foil. The glass container was placed in an oven in this state and heated at 380°C for 3 hours. After that, the heated glass container was removed from the oven and allowed to cool to room temperature, and the degree of corrosion on the surface of the metal column was visually observed. The degree of corrosion was judged according to the following criteria. ○: No corrosion observed △: Slight corrosion is observed. ×: Corrosion is observed.
[0168] (Dielectric loss tangent) Cylindrical test specimens with a diameter of 2 mm were fabricated by melt molding pellets. The fabricated test specimens were placed in a 6 GHz cavity resonator manufactured by Kanto Electronics Applied Development Co., Ltd., and measured using a network analyzer manufactured by Agilent Technologies. The dielectric loss tangent (tanδ) at 20°C and 6 GHz was determined by analyzing the measurement results using "CPMA," analysis software manufactured by Kanto Electronics Applied Development Co., Ltd., on a PC connected to the network analyzer.
[0169] (Film heat resistance) Using the pellets obtained in each example, films were fabricated using a φ14mm extruder (manufactured by Imoto Seisakusho) with a T-die. The extrusion molding conditions were as follows. a) Winding speed: 1m / min b) Roll temperature: 120℃ c) Film width: 70mm d) Thickness: 0.10mm e) Extrusion conditions: • Single-screw extruder with cylinder shaft diameter = 14mm and L / D = 20 Extruder temperature settings: Barrel section C-1 (330°C), Barrel section C-2 (350°C), Barrel section C-3 (370°C), T-die section (380°C) The obtained film was cut into 10 cm lengths, stacked in groups of 10, wrapped in aluminum foil, and left in a 280°C oven for 24 hours. After heat treatment, the film was removed from the aluminum foil and observed to confirm that it had not fused together. This is indicated by a circle in the table.
[0170] (Tube moldability) Using the pellets obtained in each example, tubes with an outer diameter of 10.0 mm and a wall thickness of 1.0 mm were extruded using a φ30 mm extrusion molding machine (manufactured by Tanabe Plastics Machinery). The extrusion molding conditions are as follows: a) Die inner diameter: 20mm b) Mandrel outer diameter: 13mm c) Sizing die inner diameter: 10.5 mm d) Pickup speed: 0.4 m / min e)Outer diameter: 10.0mm f) Wall thickness: 1.0mm g) Extrusion conditions: • Single-screw extruder with cylinder shaft diameter = 30mm and L / D = 22 Extruder temperature settings: Barrel section C-1 (330°C), Barrel section C-2 (365°C), Barrel section C-3 (380°C), Head section H-1 (380°C), Die section D-1 (390°C), Die section D-2 (390°C) The obtained tubes were cut to a length of 20 cm, bundled in groups of 10, wrapped in aluminum foil, and left in a 280°C oven for 24 hours. After heat treatment, the tubes were removed from the aluminum foil and observed to confirm that they had not fused together. This is indicated by a circle in the table.
[0171] (Wire insulation characteristics) Using the pellets obtained in each example, coated wires were obtained by extruding them onto copper conductors with a conductor diameter of 0.812 mm using a 30 mmφ wire coating molding machine (manufactured by Tanabe Plastic Machinery Co., Ltd.) with the following coating thickness. The wire coating extrusion molding conditions are as follows. a) Core conductor: Mild steel wire, conductor diameter 0.812 mm (AWG20) b) Coating thickness: 0.9 mm c) Insulated wire diameter: 2.6mm d) Wire pulling speed: 3m / min) e) Extrusion conditions: • Single-screw extruder with cylinder shaft diameter = 30mm and L / D = 22 Die (inner diameter) / Tip (outer diameter) = 26.0mm / 8.0mm Extruder temperature settings: Barrel section C-1 (330°C), Barrel section C-2 (350°C), Barrel section C-3 (370°C), Head section H (380°C), Die section D-1 (380°C), Die section D-2 (380°C). Core wire preheating was set to 80°C.
[0172] The obtained insulated wires were cut into 20cm lengths, bundled in groups of 10, wrapped in aluminum foil, and left in a 280°C oven for 24 hours. After heat treatment, the wires were removed from the aluminum foil and observed to confirm that the coating layer remained intact without fusing. This is indicated by a circle in the table.
[0173] (Electrolyte permeability) Sheet-like test specimens with a thickness of approximately 0.2 mm were prepared using pellets and a heat press molding machine. (Test cup with a permeation area of 12.56 cm²) 2 10 g of dimethyl carbonate (DMC) was placed inside the container, covered with a sheet-like test piece, and sealed with a PTFE gasket. The sheet-like test piece and DMC were in contact, and the container was kept at 60°C for 30 days. After removal, the mass loss was measured after being left at room temperature for 1 hour. The DMC transmittance (g·cm / m³) was calculated using the following formula. 2 ) was sought. Electrolyte permeability (g cm / m 2 ) = Mass loss (g) × Thickness of sheet-like test specimen (cm) / Permeation area (m²) 2 )
[0174] (Extrusion pressure) Extrusion pressure was measured using a twin capillary rheometer RHEOGRAPH 25 (Goettfert). The main die had an inner diameter of 1 mm and an L / D ratio of 16, and the sub-die had an inner diameter of 1 mm and an L / D ratio of <1. Measurements were taken at a temperature of 390°C, with a preheating time of 10 minutes after pellet loading and a shear rate of 20 seconds. -1 The extrusion pressure was determined by applying a Burgray correction to the cylinder pressure value after extrusion for 10 minutes. Copolymers with low extrusion pressure exhibit excellent moldability, including extrusion and injection molding properties.
[0175] (Self-weight deformation test during melting) A molded body with a diameter of 13 mm and a height of approximately 6.5 mm was produced using a pellet and heat press molding machine. The obtained molded body was cut to produce a test specimen with a height of 6.3 mm. The prepared test specimen was placed in a stainless steel petri dish and heated in an electric furnace at 330°C for 30 minutes, after which the petri dish containing the test specimen was cooled with water. The diameter of the surface (bottom) of the removed test specimen that was in contact with the petri dish was measured with calipers, and the bottom area increase rate was calculated using the following formula. Base area increase rate (%) = {Base area of test piece after heating (mm²) 2 )―Bottom surface area of test piece before heating (mm²) 2 )} / Bottom area of test piece before heating (mm 2 ) × 100 A lower base area increase rate means that the molded body is less likely to deform due to its own weight during melting. Copolymers that yield molded bodies with a low base area increase rate are advantageous because, even when the copolymer is molded by extrusion molding to produce thick sheets or large pipes, the molten molded body is less likely to deform, and the desired shape can be obtained after cooling and solidification.
[0176] [Table 4] [Explanation of symbols]
[0177] 10 Test fixtures 1 cup 2 Electrolyte 3. Gasket compression jig 4 Lid 5 volts 6 Spacers 7 Gasket
Claims
1. A copolymer consisting of only tetrafluoroethylene units and perfluoro(propyl vinyl ether) units, The content of perfluoro(propyl vinyl ether) units is 2.0 to 2.7 mass% based on the total monomer units; The content of tetrafluoroethylene units is 97.3 to 98.0 mass% based on the total monomer units, The melt flow rate at 372°C is 0.8 to 7.0 g / 10 min. The total number of functional groups, which is the total number of --CF.dbd.CF.sub.2, --CF.sub.2H, --COF, --COOH, --COOCH.sub.3, --CONH.sub.2 and --CH.sub.2OH, is 10 or more when the number of carbon atoms in the main chain is 10. 6 Each piece is 50 or less Copolymer.
2. A compression molded product comprising the copolymer according to claim 1.
3. An extruded article comprising the copolymer of claim 1.
4. A transfer molding comprising the copolymer according to claim 1.
5. A compressed member comprising the copolymer according to claim 1.
6. A film comprising the copolymer according to claim 1.
7. A tube comprising the copolymer of claim 1.
8. A coated electric wire comprising a coating layer containing the copolymer according to claim 1.
9. A pellet containing the copolymer described in claim 1.