Polyolefin-based microporous films by sequential cold and hot stretching of unannealed polypropylene copolymer films.

JP2022551819A5Active Publication Date: 2024-11-15DDP SPECIALTY ELECTRONICS MATERIALS US LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022519544
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-09-16
Filing Date
2020-09-29
Publication Date
2024-11-15
Estimated Expiration
2040-09-29

AI Technical Summary

Technical Problem

Existing microporous films, particularly those used in housewraps and roof membranes, face challenges in achieving high water vapor permeability while maintaining a barrier to liquid water and ensuring good mechanical properties, often requiring complex manufacturing processes and inorganic fillers that can lead to inefficiencies and environmental impacts.

Method used

The development of microporous polypropylene copolymer films, composed of polypropylene homopolymer and ethylene-containing copolymer segments, which are produced through a cold and hot stretching process without annealing, creating a non-porous structure with tunable porosity and permeability, allowing for high water vapor transmission and liquid barrier properties.

Benefits of technology

The films achieve improved breathability, mechanical strength, and processability, suitable for applications like housewraps, roofing membranes, and medical packaging, with reduced environmental impact and cost-effective production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2021067270000001
    Figure 2021067270000001
  • Figure 2021067270000002
    Figure 2021067270000002
  • Figure 2021067270000003
    Figure 2021067270000003
Patent Text Reader

Abstract

A microporous polymer film and a method for making the same are disclosed. The microporous polymer film comprises one or more polypropylene copolymers including one or more polypropylene homopolymer chain segments and one or more ethylene-containing copolymer chain segments, wherein the microporous polymer film comprises (i) a total amount of the polypropylene homopolymer chain segments of 50 to 82 wt %, based on the weight of the microporous polymer film, and (ii) a total amount of the one or more ethylene-containing copolymer chain segments of 18 to 50 wt %, based on the weight of the microporous polymer film, wherein at least a portion of the ethylene-containing copolymer chain segments comprise polymerized units of ethylene in an amount of at least 45 wt %, based on the weight of the ethylene-containing copolymer chain segments.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] Embodiments of this disclosure generally relate to microporous films and applications of microporous films in various end uses such as house wraps, roofing membranes, active and medical packaging, and sanitary and medical articles.

[0002] The present invention provides microporous polymer films derived from specific polypropylene (PP) copolymers comprising polypropylene homopolymer chain segments and ethylene-containing copolymer chain segments. The PP copolymer microporous films disclosed herein are produced without the use of conventional means to achieve porosity, i.e., without the use of inorganic fillers, perforations, or extensive pre-annealing that cause voiding to produce good crystalline morphology, as performed with respect to homopolymer polyolefins. Instead, film porosity is achieved by the use of a specific type of PP copolymer to produce a non-porous film, followed by a continuous cold / hot stretching process that results in pore formation induced by microphase separation in the polyolefin-based films disclosed herein. One advantageous feature of the method disclosed herein is that the non-porous film does not require an annealing step before the cold / hot stretching process, nor does it require a thermosetting or annealing step after the cold / hot stretching process.

[0003] This specification describes compositions of PP copolymers and process steps and methods for producing and using them. In particular, these microporous films can be manufactured to provide water vapor permeability while maintaining an effective barrier against liquid water, and these permeability is adjustable. The balance of properties of the microporous films disclosed herein suggests that these films may find applications in applications such as house wraps, roofing membranes, and sanitary and medical articles, packaging (including active packaging and medical packaging), and filtration. [Background technology]

[0004] Microporous films, methods for manufacturing them, and their uses are described herein. The present invention provides cost-effective and environmentally friendly forms of creating microporous structures in polyolefin-based films by extrusion film casting / blow molding and dry stretching processes. The pore size and porosity of these microporous films can be adjusted to achieve optimized performance in various end-use applications (for example, with respect to applications in house wrap, the film can be manufactured to have porosity and permeability properties equivalent to commercially available products such as Tyvek® house wrap from DuPont de Nemours, Inc., Wilmington, DE, USA). Alternatively, smaller pore sizes can provide a barrier against air moving through walls. According to the U.S. Department of Energy, up to 40% of the energy consumed to heat or cool a building is lost due to air leakage.

[0005] Various end-use applications require or at least benefit from the use of breathable films. A breathable film can be described as a film that is relatively permeable to water vapor and relatively impermeable to liquids.

[0006] House wrap functions as a weather-resistant barrier, preventing rain from entering the wall assembly while allowing water vapor to pass through to the outside. Therefore, to be effective, house wrap must be water-repellent and have high water vapor permeability (permeability). Currently, house wrap can be classified into two categories: woven and perforated, and nonwoven and non-perforated. Generally, the less expensive perforated wrap is manufactured from polyethylene or polypropylene that has been microscopically perforated to make it permeable, while non-perforated wrap consists of a polyolefin layer that allows water vapor to pass through its nonwoven fiber mesh. Current technology generally involves multiple steps for the manufacturing process.

[0007] In addition, the present invention provides a polyolefin-based microporous film for roof membrane applications. There is a large market need for breathable roof membranes. Current non-permeable roof membranes made from polyvinyl chloride (PVC), thermoplastic polyolefin (TPO), or polymerized ethylene propylene diene monomer (EPDM) cannot meet this need, and polyolefin-based microporous films offer an opportunity to provide a low-cost alternative with high water vapor permeability compared to such current ones. The low / small water vapor permeability of current roof membranes leads to water accumulation under the roof membrane, which over time causes delamination of the roof membrane from the roof (e.g., lightweight concrete structures), and then damage to the roof structure. The higher water vapor permeability of thick polyolefin-based microporous films meets important requirements for roof membranes, such as high water vapor transmission (permeability), e.g., above 10 perms; and good water repellency (weather barrier). The weather resistance of polyolefin-based microporous films can be further enhanced by applying UV-resistant agents.

[0008] Polyethylene films are widely used in sanitary absorption products such as diaper backsheets. Diaper backsheets can be classified as breathable or non-breathable. Breathable backsheets typically use films filled with more than 50% by weight of CaCO3 (or other inorganic fillers) and / or micro-cavitated. However, due to the active competition in the sanitary absorption product market, film manufacturers are required to pursue differentiated technologies that enable enhanced product performance such as improved mechanical property performance while also allowing cost reduction, for example, from further down gauging (thinner films). SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION

[0009] Thus, in many end-use markets, there is a need for an improved breathable film that has a very thin gauge, high porosity that allows high water vapor transmission, while preventing leakage of water, which is a liquid, and ensuring good processability and mechanical properties. The non-interconnected micropores of the microporous films disclosed herein provide better barrier performance against air, water, bacteria, and blood, and such barrier performance is essential for applications such as housewrap, roofing membranes, air filtration, medical packaging, and medical backtable covers. Due to the relatively high melting temperature of the PP copolymer, its application in steam sterilization related to medical packaging is possible. Also, the wide range of adjustable breathability suggests that these microporous films are also possible for applications related to active packaging (sachets). Thus, there is a need for compositions containing the polypropylene copolymer compositions described herein, microporous films made therefrom, methods for preparing them, and methods for using them. The present invention disclosed herein addresses these and other important objectives and provides solutions to these market needs.

Means for Solving the Problems

[0010] In certain embodiments, the present invention as described herein comprises, consists of, or is essentially composed of, one or more polypropylene copolymers comprising one or more polypropylene homopolymer chain segments and one or more ethylene-containing copolymer chain segments, wherein (i) the polypropylene homopolymer chain segments comprise a total amount of 50 to 82% by weight based on the weight of the microporous polymer film or 43 to 79 mol% based on the molar content of propylene polymerization units in the polypropylene homopolymer chain segments as a percentage of the total molar content of polymerization monomer units in the microporous polymer film, and (ii) the ethylene-containing copolymer chain segments The present invention relates to a microporous polymer film comprising a total amount of ethylene-containing copolymer chain segments, comprising 18 to 50% by weight of the microporous polymer film or 21 to 57 mol% as a percentage of the total molar content of polymer monomer units in the microporous polymer film, and wherein at least a portion of the ethylene-containing copolymer chain segments contains polymer units of ethylene in an amount of at least 45% by weight of the ethylene-containing copolymer chain segments or at least 55 mol% as a percentage of the total molar content of polymer monomer units in the ethylene-containing copolymer chain segments, based on the molar content of polymer units of ethylene in the ethylene-containing copolymer chain segments.

[0011] In one embodiment, a method for forming a microporous polymer film, the method step comprising: (a) one or more polypropylene copolymers, (i) one or more polypropylene homopolymer chain segments, comprising one or more polypropylene homopolymer chain segments in a total amount of 50 to 82% by weight based on the weight of the polypropylene copolymer or 43 to 79 mol% based on the molar content of propylene polymerization units in the polypropylene homopolymer chain segments as a percentage of the total molar content of polymerization monomer units in the polypropylene copolymer; and (ii) one or more ethylene-containing copolymer chain segments, comprising one or more ethylene-containing copolymers in a total amount of 18 to 50% by weight based on the weight of the polypropylene copolymer or 21 to 57 mol% based on the molar content of polymerization monomer units in the ethylene-containing copolymer chain segments as a percentage of the total molar content of polymerization monomer units in the polypropylene copolymer. A method is disclosed comprising, or essentially comprising, one or more polypropylene copolymers, comprising a polymer chain segment, wherein at least a portion of the ethylene-containing copolymer chain segment contains polymer units of ethylene in an amount of at least 45% by weight based on the weight of the ethylene-containing copolymer chain segment or at least 55 mol% based on the molar content of polymer monomer units of ethylene in the ethylene-containing copolymer chain segment as a percentage of the total molar content of polymer monomer units in the ethylene-containing copolymer chain segment; (b) forming a non-porous film from the polypropylene copolymer; and (c) subjecting the non-porous film to a series of cold-stretching and hot-stretching steps, including (i) at least one cold-stretching step at a temperature in the range of -20°C to 50°C and (ii) at least one hot-stretching step at a temperature in the range of 50°C to 150°C, thereby producing a microporous polymer film.

[0012] In some embodiments, the method is a continuous process for producing a microporous polymer film. In particular, in some embodiments, the method proceeds without any annealing step after the formation of a non-porous film, and proceeds without any annealing or thermosetting step after the formation of a microporous polymer film, and is a continuous process for producing a microporous polymer film.

[0013] To provide a further understanding of the present invention, the accompanying drawings, which are included herein and constitute part of this specification, illustrate embodiments of the present invention and, together with the description, help to illustrate the principles of the present invention. [Brief explanation of the drawing]

[0014] [Figure 1A] This shows mercury intrusion porosimetry data for Tyvek® house wrap. [Figure 1B] This shows mercury intrusion porosimetry data for PP C7054-07NA microporous film after changing the range of heat stretching conditions. [Figure 2A] This image shows a SEM image of a cross-section of an unstretched PP C7054-07NA film, indicated by a 20-micron scale bar. [Figure 2B] The image shows a SEM cross-section of a stretched PP C7054-07NA film after 25% cold stretching at 100 mm / second (room temperature) and 50% hot stretching at 5 mm / second (100°C), indicated by a 20-micron scale bar. [Figure 2C] The image shows a SEM cross-section of a stretched PP C7054-07NA film after 25% cold stretching at 100 mm / second (room temperature) and 50% hot stretching at 5 mm / second (100°C), indicated by a 5-micron scale bar. [Figure 3A] This image shows a SEM image of the film surface of an unstretched PP C7054-07NA film, indicated by a 20-micron scale bar. [Figure 3B]This image shows a SEM image of the film surface of an unstretched PP C7054-07NA film, indicated by a 10-micron scale bar. [Figure 3C] The image shows SEM images of the film surface of a stretched PP C7054-07NA film after 25% cold stretching at 100 mm / second (room temperature) and 50% hot stretching at 5 mm / second (100°C), indicated by a 20-micron scale bar. [Figure 3D] The image shows SEM images of the film surface of a stretched PP C7054-07NA film after 25% cold stretching at 100 mm / second (room temperature) and 50% hot stretching at 5 mm / second (100°C), indicated by a 10-micron scale bar. [Figure 4A] The image shows a TEM image of the PP C7054-07NA film before stretching, indicated by a 1-micron scale bar. [Figure 4B] TEM images of PP C7054-07NA film after 25% cold stretching at 100 mm / second (room temperature) and 100% hot stretching at 5 mm / second (100°C), indicated by a 1-micron scale bar. [Figure 4C] The image shows a TEM image of the PP INSPIRE® 114 film before stretching, indicated by a 0.2 micron scale bar. [Figure 4D] TEM images of PP INSPIRE® 114 film after 25% cold stretching at 100 mm / second (room temperature) and 100% hot stretching at 5 mm / second (100°C), indicated by a 0.2 micron scale bar. [Figure 5A] The wide-angle X-ray dispersion (WAXS) data for the PP C7054-07NA film before stretching is shown. [Figure 5B] The wide-angle X-ray dispersion (WAXS) data for PP C7054-07NA microporous film after 25% cold stretching at 100 mm / second (room temperature) followed by 100% hot stretching at 5 mm / second (100°C) are shown. [Figure 5C] The wide-angle X-ray dispersion (WAXS) data for the PP TI4020N film before stretching is shown. [Figure 5D]The wide-angle X-ray dispersion (WAXS) data for PP TI4020N microporous film after 25% cold stretching at 100 mm / second (room temperature) followed by 100% hot stretching at 5 mm / second (100°C) is shown. [Figure 6A] The image shows a TEM image of a film from a 20 / 80 blend of homopolymer PP H314 (20%) and PP C7054-07NA (80%) before stretching, indicated by a 1-micron scale bar. [Figure 6B] TEM images of films from a 20 / 80 blend of homopolymer PP H314 (20%) and PP C7054-07NA (80%) after 25% cold stretching at 100 mm / sec (room temperature) and 100% hot stretching at 5 mm / sec (100°C), indicated by a 0.5 micron scale bar. [Figure 7A] This shows mercury intrusion porosimetry data for a PP C7054-07NA film with a thickness of 762 μm (30 mil) after 25% cold stretching at 100 mm / second (room temperature) and 100% hot stretching at 5 mm / second (100°C). [Figure 7B] This shows mercury intrusion porosimetry data for a PP C7054-07NA film with a thickness of 762 μm (30 mils) after 25% cold stretching at 100 mm / second (room temperature) followed by 150% hot stretching at 5 mm / second (100°C). [Figure 8] This describes one suitable multi-stage stretching process for either cold or hot longitudinal orientation (MDO) of a film using rolls. [Figure 9] This demonstrates one suitable multi-stage stretching process for transverse orientation (TDO) of films using an oven. [Modes for carrying out the invention]

[0015] The present invention can be more readily understood by referring to the following detailed description, examples, drawings, and claims, as well as the preceding and following descriptions thereof. However, it should be understood that the present invention is not limited to the specific compositions, articles, devices, systems, and / or methods disclosed unless otherwise specified, and is therefore naturally subject to change. While aspects of the present invention may be described and claimed in specific legal classifications, such as legal classifications of compositions, this is for convenience only, and those skilled in the art will understand that each aspect of the present invention may be described and claimed in any legal classification.

[0016] The following detailed description of the present invention is also provided as teachings enabling the best known embodiment of the invention. To achieve this objective, various modifications and adaptations of the embodiments of the invention described herein can be made, while those skilled in the art will recognize and understand that the beneficial results of the invention can still be obtained. It will also be understood that some of the benefits of the invention can be obtained by selecting some of the features of the invention without using other features. Accordingly, those skilled in the art will recognize that many modifications and adaptations of the invention are possible, and that under certain circumstances, many such modifications and adaptations may be even more desirable, and therefore, many such modifications and adaptations are also part of the invention.

[0017] While the present invention can be embodied in various forms, the following descriptions of some embodiments are made with the understanding that this disclosure is intended to be illustrative of the invention and that the invention is not intended to be limited to any particular embodiment illustrated. The headings are provided for convenience only and should not be construed as limiting the invention. Embodiments illustrated in any heading or part of this disclosure may be combined with embodiments illustrated in the same or any other heading or part of this disclosure.

[0018] In all possible variations thereof, any combination of the elements described herein is incorporated by the present invention unless otherwise specifically indicated herein or unless it is particularly evident in the context.

[0019] Unless otherwise explicitly stated, no method or embodiment described herein is ever intended to be construed as requiring its steps to be performed in a specific order. Therefore, if a claim for a method does not specifically state in the claims or description that the steps are limited to a specific order, no order is ever intended to be inferred in any sense. This applies to all possible non-expressive bases for interpretation, including logical matters relating to the arrangement or flow of operations of the steps, simple meanings derived from grammatical construction or punctuation, or the number or type of embodiments described herein. It should be understood that both the above summary and the following detailed description are illustrative and descriptive only, and not restrictive.

[0020] All publications referenced herein are incorporated herein by reference to disclose and explain methods and / or materials in connection with those cited in those publications.

[0021] It should be understood that the technical terms used herein are merely for the purpose of describing specific embodiments and are not intended to be limiting. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the invention pertains. Many of the terms defined herein will be referenced in this specification and in the subsequent claims.

[0022] As used herein and in the appended claims, the singular forms “a,” “an,” and “it” refer to multiple objects unless the context explicitly indicates otherwise.

[0023] As used herein, the term "and / or" means "and / or alternatively."

[0024] As used herein, the terms “optional” or “optional” mean that the events, conditions, components, or circumstances described below may or may not occur, and that the descriptions thereof include instances in which such events, conditions, components, or circumstances occur and instances in which they do not occur.

[0025] As used herein, any disclosure using the terms “contains” or “contains” includes similar disclosures, and instead, “contains” or “contains” shall be replaced by “consisting of” or “being made of,” or instead by “essentially being made of” or “essentially being made of.”

[0026] As used herein, the phrase “sufficient” (e.g., “sufficient conditions to…”) means such a value or condition that can perform a function or characteristic for a sufficient value or condition to be manifested. As noted below, the exact value or specific condition required may vary from embodiment to embodiment depending on widely accepted variables, such as the materials and / or processing conditions used.

[0027] The term "by weight," when used in combination with an ingredient, is based on the total weight of the compound or composition in which that ingredient is contained, unless otherwise specified. For example, if a particular element or ingredient in a composition or article is said to be present in an amount of 8 wt.% (also written as 8 wt.%), this percentage is understood to refer to 100% of the overall composition. The wt% of ingredient A in a composition is the weight of ingredient A expressed as a percentage of the total weight of the composition, and is traditionally written as "wt% of A based on the total weight of the composition." In some examples, the wt% of an ingredient is based on the total weight of the composition on a "dry basis," indicating the weight of the composition without water (e.g., less than about 1 wt%, less than about 0.5 wt%, less than about 0.1 wt%, less than about 0.05 wt%, or about 0 wt% water based on the total weight of the composition).

[0028] Where a number is disclosed herein, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, the following sentences typically follow such numbers: "Each of the aforementioned numbers may be used with the terms “about,” “at least about,” or “less than about,” and any of the aforementioned numbers may be used alone or in combination with a description of a restrictive range to state a non-restrictive range." This sentence means that each of the aforementioned numbers may be used alone (e.g., 4), preceded by the word “about” (e.g., about 8), preceded by the phrase “at least about” (e.g., at least about 2), preceded by the phrase “less than about” (e.g., less than about 7), or used in any combination or without any of the prefixing words or phrases for defining a range (e.g., 2 to 9, about 1 to 4, 8 to about 9, about 1 to about 10, etc.). Furthermore, where a range is described as “less than or equal to about X,” this phrase is equivalent to the range which is instead a combination of “about X” and “less than about X.” For example, “about 10 or less” is the same as “about 10 or less than about 10.” Such interchangeable range descriptions are intended herein. Other range forms are disclosed herein, but formal differences should not be construed as implying differences in substance.

[0029] As used herein, “continuous” means a process whose duration is continuous or one that is interrupted, stopped, or terminated only momentarily compared to the duration of the process. A process is “continuous” if the starting materials or reactants are supplied to the apparatus without interruption or substantially without interruption, or if the processing of the starting materials or reactants is not carried out in a batch process.

[0030] As used herein, the term “substantially free” means a composition having less than about 1% by weight of the indicated substance, for example, less than about 0.5% by weight, less than about 0.1% by weight, less than about 0.05% by weight, or less than about 0.01% by weight, based on the total weight of the composition.

[0031] As used herein, the term “substantially” means, when used in reference to a composition, at least about 60% by weight of a particular feature or component based on the total weight of the composition, for example, at least about 65% by weight, at least about 70% by weight, at least about 75% by weight, at least about 80% by weight, at least about 85% by weight, at least about 90% by weight, at least about 91% by weight, at least about 92% by weight, at least about 93% by weight, at least about 94% by weight, at least about 95% by weight, at least about 96% by weight, at least about 97% by weight, at least about 98% by weight, at least about 99% by weight, or about 100% by weight.

[0032] All molecular weights and other molecular weight-related values ​​disclosed herein (e.g., polydispersity index) are measured by gel permeation chromatography (GPC).

[0033] As used herein, the terms “molar mass distribution,” “MMD,” and “molecular weight distribution” are interchangeable, and each refers to the number of moles of a polymer species or the number of polymer chains (N). i ) and the molar mass of that kind (M i ) or the relationships between polymer chains are described. The molar mass distribution of the polymer may be altered by the polymer fraction. Depending on the statistical method applied, different mean values ​​may be defined and are described herein.

[0034] As used herein, the term "number-average molecular weight" (M n , or

number

number

[0035] As used herein, the term "weight average molecular weight" (M w or [Number] ) is defined by the following formula. [[ID=第十六]]

数

[0036] [[ID=第三十五]] As used herein, gel permeation chromatography (GPC) refers to a chromatographic separation method in which molecules in a solution are separated according to their size. Separation is achieved by differential exclusion of sample molecules as they pass through a layer of porous particles known as a separation column. GPC can be used to determine the substantially accurate molar mass distribution of polymer molecules. For example, a certain amount of the liquid fraction (eluent) that has passed through the column is collected. As the polymer elutes through the column, molecules that are too large to pass through the column's pores are excluded from the packed pore volume and elute with an earlier retention time, while smaller molecules enter the column's pores and elute with a slower retention time. The concentration of the eluted polymer can be measured by spectroscopic techniques such as refractive index (RI) and ultraviolet (UV). The flow of the eluent can also be continuously analyzed by RI, low-angle laser scattering (LALLS), multi-angle laser scattering (MALLS), UV, and / or viscosity measurement.

[0037] The use of numerical values ​​in the various quantitative values ​​specified herein, unless otherwise explicitly indicated, means that the minimum and maximum values ​​within a given range are described as approximations, as if both were preceded by the word “approximately”. Thus, slight differences from the indicated values ​​may be used to achieve substantially the same results as the indicated values. Furthermore, the disclosure of ranges is intended to be a continuous range including all values ​​between the enumerated minimum and maximum values, as well as any range that can be formed by such values. Also disclosed herein are any and all ratios (and any ranges of any such ratios) that can be formed by dividing the enumerated numerical values ​​into any other enumerated numerical values. Accordingly, those skilled in the art will understand that many such ratios, ranges, and ranges of ratios may clearly derive from the numerical values ​​presented herein, and in all examples, such ratios, ranges, and ranges of ratios represent various embodiments of the invention.

[0038] In this specification, “average pore diameter” refers to the “average pore diameter” measured by mercury intrusion porosimetry (4V / A according to UOP method 578-11 described below), which is known to those skilled in the art or known in the field of mercury intrusion porosimetry. The UOP method is available from ASTM International, West Conshohocken, PA, USA (or from www.astm.org). Since the mean is the median mean, this term may be referred to as “median pore diameter” in this specification.

[0039] As used herein, the term “polypropylene copolymer” means a copolymer comprising a polymer backbone, side chains, or chain segments of polypropylene, in particular, such backbone, side chains, or chain segments comprising 15 or more continuous polymerization units of propylene. Preferred PP copolymers, as disclosed herein, include polypropylene homopolymer chain segments (e.g., isotactic PP) and ethylene-containing copolymer chain segments. In some embodiments, the ethylene-containing copolymer chain segment is an ethylene-propylene (EP) copolymer chain segment, and such polypropylene copolymers may also be described herein as PP-EP copolymers.

[0040] In some embodiments, the present invention relates to a microporous polymer film comprising one or more polypropylene copolymers (PP copolymers). The PP copolymer may comprise one or more polypropylene homopolymer chain segments and one or more ethylene-containing copolymer chain segments.

[0041] In some embodiments, the PP copolymer comprises polypropylene homopolymer chain segments in an amount of at least about 50% by weight based on the total weight of the PP copolymer, and the maximum amount of polypropylene homopolymer chain segments is not particularly limited. In the same or other embodiments, the PP copolymer comprises polypropylene homopolymer chain segments in an amount up to about 95% by weight based on the total weight of the PP copolymer, and the minimum amount of polypropylene homopolymer chain segments is not particularly limited. For example, the PP copolymer may contain polypropylene homopolymer chain segments in amounts of 44, 46, 48, 50, 52, 54, 56, 58, 60, 62, 64, 65, 66, 68, 70, 72, 74, 76, 78, 80, 82, 84, 86, 88, 90, 95% (in weight percent based on the weight of the PP copolymer). Each of the aforementioned figures may be preceded by the words “about,” “at least about,” or “less than about,” and any of the aforementioned figures may be used alone to describe a non-limiting range or in combination to describe a limiting range. For example, but not limited to, the amount of polypropylene homopolymer chain segments in a PP copolymer may be at least about 50% by weight, about 50% to about 82% by weight, or about 60% to about 82% by weight, based on the total weight of the PP copolymer. In terms of mol%, the PP copolymer may contain polypropylene homopolymer chain segments in amounts of 40, 42, 43, 44, 45, 46, 47, 48, 49, 50, 52, 54, 55, 56, 58, 60, 62, 64, 66, 68, 70, 72, 74, 76, 78, 79, 80, 82, or 85% (in mol%) based on the molar content of propylene polymerization units in the polypropylene homopolymer chain segments as a percentage of the total molar content of polymerization monomer units in the PP copolymer. Each of the aforementioned numbers may precede the words “approximately,” “at least approximately,” or “less than approximately,” and any of the aforementioned numbers may be used alone to describe an unrestrictive range or in combination to describe a restrictive range.For example, but not limited to, the amount of polypropylene homopolymer chain segments in a PP copolymer may be at least about 43 mol%, about 43 mol% to about 79 mol%, or about 50 mol% to about 79 mol%, based on the molar content of propylene polymerization units in the polypropylene homopolymer chain segments, as a percentage of the total molar content of polymerization monomer units in the PP copolymer.

[0042] In some embodiments, the PP copolymer contains ethylene-containing copolymer chain segments in an amount of at least about 5% by weight based on the total weight of the PP copolymer, and the maximum amount of ethylene-containing copolymer chain segments is not particularly limited. In the same or other embodiments, the PP copolymer contains ethylene-containing copolymer chain segments in an amount up to about 50% by weight based on the total weight of the PP copolymer, and the minimum amount of ethylene-containing copolymer chain segments is not particularly limited. For example, the PP copolymer may contain ethylene-containing copolymer chain segments in amounts of 5, 10, 15, 17, 18, 19, 20, 22, 24, 26, 28, 30, 32, 34, 36, 38, 40, 42, 44, 46, 48, 50, 52, 54, or 55% (in weight percent based on the weight of the PP copolymer). Each of the aforementioned figures may be preceded by the words “approximately,” “at least approximately,” or “less than approximately,” and any of the aforementioned figures may be used alone to describe a non-limiting range or in combination to describe a limiting range. For example, but not limited to, the amount of ethylene-containing copolymer chain segments in a PP copolymer may be at least about 10% by weight, about 18% to about 50% by weight, or about 25% to about 40% by weight, based on the total weight of the PP copolymer. Preferably, the ethylene-containing copolymer chain segments in a PP copolymer are ethylene-propylene (EP) copolymer chain segments. In terms of mol%, a PP copolymer may contain ethylene-containing copolymer chain segments in amounts of 10, 15, 17, 18, 19, 20, 21, 22, 24, 26, 28, 30, 32, 34, 36, 38, 40, 42, 44, 46, 48, 50, 52, 54, 55%, 57, or 60% (in mol%) based on the molar content of polymerized monomer units in the ethylene-containing copolymer chain segments as a percentage of the total molar content of polymerized monomer units in the PP copolymer. Each of the aforementioned figures may be preceded by the words “about,” “at least about,” or “less than about,” and any of the aforementioned figures may be used alone to describe a non-limiting range or in combination to describe a limiting range.For example, but not limited to, the amount of ethylene-containing copolymer chain segments in a PP copolymer may be at least about 15 mol%, about 21 mol% to about 57 mol%, or about 21 mol% to about 45 mol%, based on the molar content of polymer monomer units in the ethylene-containing copolymer chain segments, as a percentage of the total molar content of polymer monomer units in the PP copolymer.

[0043] In some embodiments, the ethylene-containing copolymer chain segment in the PP copolymer contains at least 45% by weight of ethylene polymerization units based on the total weight of the ethylene-containing copolymer chain segment, and the maximum amount of ethylene in the ethylene-containing copolymer chain segment is not particularly limited. For example, the ethylene unit content in the ethylene-containing copolymer chain segment in the PP copolymer may be 40, 42, 44, 45, 46, 47, 48, 49, 50, 52, 54, 56, 58, 60, 62, 64, 66, 68, 70, 72, 75, or 80% (in weight percent based on the weight of the ethylene-containing copolymer chain segment). Each of the aforementioned figures may be preceded by the words “about,” “at least about,” or “less than about,” and any of the aforementioned figures may be used alone to describe a non-limiting range or in combination to describe a limiting range. For example, but not limited to, the amount of ethylene units in an ethylene-containing copolymer chain segment in a PP copolymer may be at least about 45% by weight, about 45% to about 80% by weight, or about 45% to about 60% by weight, based on the total weight of the ethylene-containing copolymer chain segment. In terms of mol%, the ethylene unit content in an ethylene-containing copolymer chain segment in a PP copolymer may be 50, 52, 54, 55, 56, 57, 58, 59, 60, 62, 64, 66, 68, 70, 72, 74, 76, 78, 80, 82, 85, or 90% (in mol%) based on the molar content of ethylene polymerization units in the ethylene-containing copolymer chain segment as a percentage of the total molar content of polymerization monomer units in the ethylene-containing copolymer chain segment. Each of the aforementioned figures may be preceded by the words “about,” “at least about,” or “less than about,” and any of the aforementioned figures may be used alone to describe a non-limiting range or in combination to describe a limiting range. For example, but not limited to, the amount of ethylene units in the ethylene-containing copolymer chain segment of a PP copolymer may be at least about 55 mol%, about 55 mol% to about 80 mol%, or about 55 mol% to about 69 mol%, based on the molar content of ethylene polymerization units in the ethylene-containing copolymer chain segment, as a percentage of the total molar content of polymerization monomer units in the ethylene-containing copolymer chain segment.Preferably, the ethylene-containing copolymer chain segment in the PP copolymer is an ethylene-propylene (EP) copolymer chain segment, in which case the above percentage refers to the ethylene unit content % in the EP copolymer chain segment (either by weight % or mol %) as described above.

[0044] The total ethylene content of the polymerization form in the PP copolymer is at least 10% by weight, for example, 10-30% by weight or more, 15-25% by weight, based on the weight of the PP copolymer, or at least 14 mol%, for example, 14-39 mol% or 15-25 mol%, based on the molar content of the polymerization units of ethylene in the PP copolymer, as a percentage of the total molar content of polymerization monomer units in the PP copolymer.

[0045] Microporous polymer films can essentially consist of one or more polypropylene copolymers (PP copolymers) comprising one or more polypropylene homopolymer chain segments and one or more ethylene-containing copolymer chain segments. Therefore, in at least some embodiments, the same amounts and ranges of polypropylene homopolymer chain segments and ethylene-containing copolymer chain segments outlined above in the PP copolymer are also suitable for the amounts and ranges of polypropylene homopolymer chain segments and ethylene-containing copolymer chain segments in the microporous polymer film.

[0046] In some embodiments, the microporous polymer film contains polypropylene homopolymer chain segments in an amount of at least about 50% by weight based on the total weight of the microporous polymer film, and the maximum amount of polypropylene homopolymer chain segments is not particularly limited. In the same or other embodiments, the microporous polymer film contains polypropylene homopolymer chain segments in an amount of up to about 95% by weight based on the total weight of the microporous polymer film, and the minimum amount of polypropylene homopolymer chain segments is not particularly limited. For example, the microporous polymer film may contain polypropylene homopolymer chain segments in amounts of 44%, 46%, 48%, 50%, 52%, 54%, 56%, 58%, 60%, 62%, 64%, 66%, 68%, 70%, 72%, 74%, 76%, 78%, 80%, 82%, 84%, 86%, 88%, 90%, and 95% (in weight percent based on the weight of the microporous polymer film). Each of the aforementioned figures may be preceded by the words “approximately,” “at least approximately,” or “less than approximately,” and any of the aforementioned figures may be used alone to describe an unrestrictive range or in combination to describe a restrictive range. For example, but are not limited to, the amount of polypropylene homopolymer chain segments in a microporous polymer film may be at least about 50% by weight, about 50% to about 82% by weight, or about 60% to about 82% by weight, based on the total weight of the microporous polymer film. In terms of mol%, a microporous polymer film may contain polypropylene homopolymer chain segments in amounts of 40, 42, 43, 44, 45, 46, 47, 48, 49, 50, 52, 54, 55, 56, 58, 60, 62, 64, 66, 68, 70, 72, 74, 76, 78, 79, 80, 82, or 85% (in mol%) based on the molar content of propylene polymerization units in the polypropylene homopolymer chain segments as a percentage of the total molar content of polymerization monomer units in the microporous polymer film. Each of the aforementioned figures may be preceded by the words “about,” “at least about,” or “less than about,” and any of the aforementioned figures may be used alone to describe a non-limiting range or in combination to describe a limiting range.For example, but not limited to, the amount of polypropylene homopolymer chain segments in a microporous polymer film may be at least about 43 mol%, about 43 mol% to about 79 mol%, or about 50 mol% to about 80 mol%, based on the molar content of propylene polymerization units in the polypropylene homopolymer chain segments, as a percentage of the total molar content of polymerization monomer units in the microporous polymer film.

[0047] Polypropylene homopolymer chain segments present in a microporous polymer film may be derived solely from the PP copolymer component, or they may be a combination of the PP copolymer component and polypropylene homopolymer chain segments derived from one or more other polymer components containing polypropylene homopolymer chain segments (a PP homopolymer containing polypropylene homopolymer chain segments or another copolymer). Preferably, the polypropylene homopolymer chain segments present in the microporous polymer film are derived solely from the PP copolymer component.

[0048] In some embodiments, the microporous polymer film contains ethylene-containing copolymer chain segments in an amount of at least about 5% by weight based on the total weight of the microporous polymer film, and the maximum amount of ethylene-containing copolymer chain segments is not particularly limited. In the same or other embodiments, the microporous polymer film contains ethylene-containing copolymer chain segments in an amount of up to about 60% by weight based on the total weight of the microporous polymer film, and the minimum amount of ethylene-containing copolymer chain segments is not particularly limited. For example, the microporous polymer film may contain ethylene-containing copolymer chain segments in amounts of 5, 10, 15, 17, 18, 19, 20, 22, 24, 26, 28, 30, 32, 34, 36, 38, 40, 42, 44, 46, 48, 50, 52, 54, 55, 56, 58, or 60% (in weight percent based on the weight of the microporous polymer film). Each of the aforementioned figures may be preceded by the words “approximately,” “at least approximately,” or “less than approximately,” and any of the aforementioned figures may be used alone to describe an unrestrictive range or in combination to describe a restrictive range. For example, but are not limited to, the amount of ethylene-containing copolymer chain segments in a microporous polymer film may be at least about 10% by weight, about 18% to about 50% by weight, or about 25% to about 40% by weight, based on the total weight of the microporous polymer film. In terms of mol%, a microporous polymer film may contain ethylene-containing copolymer chain segments in amounts of 10, 15, 17, 18, 19, 20, 21, 22, 24, 26, 28, 30, 32, 34, 36, 38, 40, 42, 44, 46, 48, 50, 52, 54, 55, 57, or 60% (in mol%) based on the molar content of polymerized monomer units in the ethylene-containing copolymer chain segments as a percentage of the total molar content of polymerized monomer units in the microporous polymer film. Each of the aforementioned figures may be preceded by the words “about,” “at least about,” or “less than about,” and any of the aforementioned figures may be used alone to describe a non-limiting range or in combination to describe a limiting range.For example, but not limited to, the amount of ethylene-containing copolymer chain segments in a microporous polymer film may be at least about 15 mol%, about 21 mol% to about 57 mol%, or about 20 mol% to about 45 mol%, based on the molar content of polymer monomer units in the ethylene-containing copolymer chain segments, as a percentage of the total molar content of polymer monomer units in the microporous polymer film.

[0049] The ethylene-containing copolymer chain segments present in the microporous polymer film may be derived solely from the PP copolymer component, or from a combination of the PP copolymer component and one or more other polymer components (e.g., EP copolymers) containing ethylene-containing copolymer chain segments. Preferably, the ethylene-containing copolymer chain segments present in the microporous polymer film are derived solely from the PP copolymer component. Preferably, the ethylene-containing copolymer chain segments are ethylene-propylene (EP) copolymer chain segments.

[0050] In some embodiments, the ethylene-containing copolymer chain segments in the microporous polymer film contain at least 45% by weight of ethylene polymerization units based on the total weight of the ethylene-containing copolymer chain segments, and the maximum amount of ethylene in the ethylene-containing copolymer chain segments is not particularly limited. For example, the ethylene unit content in the ethylene-containing copolymer chain segments in the microporous polymer film may be 40, 42, 44, 45, 46, 47, 48, 49, 50, 52, 54, 56, 58, 60, 62, 64, 66, 68, 70, 72, 75, or 80% (in weight percent based on the weight of the ethylene-containing copolymer chain segments). Each of the aforementioned figures may be preceded by the words “about,” “at least about,” or “less than about,” and any of the aforementioned figures may be used alone to describe a non-limiting range or in combination to describe a limiting range. For example, but not limited to, the amount of ethylene units in an ethylene-containing copolymer chain segment in a microporous polymer film may be at least about 45% by weight, about 45% to about 80% by weight, or about 45% to about 60% by weight, based on the total weight of the ethylene-containing copolymer chain segment. In terms of mol%, the ethylene unit content in an ethylene-containing copolymer chain segment in a microporous polymer film may be 50, 52, 54, 55, 56, 57, 58, 59, 60, 62, 64, 66, 68, 70, 72, 74, 76, 78, 80, 82, 85, or 90% (in mol%) based on the molar content of ethylene polymerization units in the ethylene-containing copolymer chain segment as a percentage of the total molar content of polymerization monomer units in the ethylene-containing copolymer chain segment. Each of the aforementioned numbers may precede the words “approximately,” “at least approximately,” or “less than approximately,” and any of the aforementioned numbers may be used alone to describe an unrestrictive range or in combination to describe a restrictive range.For example, but not limited to, the amount of ethylene units in an ethylene-containing copolymer chain segment in a microporous polymer film may be at least about 55 mol%, about 55 mol% to about 80 mol%, or about 55 mol% to about 69 mol%, based on the molar content of ethylene polymerization units in the ethylene-containing copolymer chain segment, as a percentage of the total molar content of polymerization monomer units in the ethylene-containing copolymer chain segment. Preferably, the ethylene-containing copolymer chain segment in the PP copolymer is an ethylene-propylene (EP) copolymer chain segment, in which case the above percentage refers to the ethylene unit content % in the EP copolymer chain segment (either by weight % or mol%) as described above.

[0051] The total ethylene content of the polymerization form in the microporous polymer film is at least 10% by weight, for example 10-30% by weight or more precisely 15-25% by weight, based on the weight of the microporous polymer film, or at least 14 mol%, based on the molar content of ethylene polymerization units in the microporous polymer film, as a percentage of the total molar content of polymerization monomer units in the microporous polymer film, for example 14-39 mol%, 15-25 mol%, or 21-33 mol%.

[0052] In certain embodiments, these PP copolymers can be produced in a reactor from a PP homopolymer of one or more components and an ethylene-containing copolymer of one or more components. Preferably, the ethylene-containing copolymer is an ethylene-propylene (EP) copolymer. Accordingly, the present invention provides a microporous polymer film comprising a polypropylene copolymer produced from the reaction product of a polypropylene homopolymer and an ethylene-propylene copolymer.

[0053] In certain embodiments where the ethylene-containing copolymer is an ethylene-propylene (EP) copolymer, the microporous film may essentially consist of a PP-EP copolymer comprising one or more polypropylene homopolymer chain segments and one or more ethylene-propylene copolymer chain segments. In certain such embodiments, the weight ratio of the PP component to the EP component may be 50:50, 55:45, 60:40, 65:35, 67:33, 70:30, 72:28, 74:26, 76:24, 78:22, 79:21, 80:20, 81:19, 82:18, 84:16, 86:14, 88:12, 90:10, or 95:5. Each of the aforementioned figures may be preceded by the words “about,” “at least about,” or “less than about,” and any of the aforementioned figures may be used alone to describe a non-limiting range or in combination to describe a limiting range. For example, the weight ratio could be at least about 60:40, about 65:35 to about 85:15, or less than about 90:10.

[0054] Ethylene-containing copolymers may be random copolymers, alternating copolymers, or block copolymers, and ethylene-propylene copolymers may be random EP copolymers, alternating EP copolymers, or EP block copolymers. For example, a PP copolymer containing an EP copolymer main chain or chain segments may include a random EP copolymer main chain or chain segments, an alternating EP copolymer main chain or chain segments, or a diblock copolymer main chain or chain segments. For example, a diblock copolymer may include polypropylene blocks and polyethylene blocks, or polypropylene blocks and EP copolymer blocks, or polyethylene blocks and EP copolymer blocks. Other ethylene-containing copolymers may also be used.

[0055] The film can be produced from the PP copolymer or its polymer blend by heating to a temperature sufficient to obtain the PP copolymer (or its blend) in a molten form, most conveniently by any method known in the art, followed by extrusion or inflation molding. In some embodiments, the film can be a multilayer film. The multilayer film can be co-extruded, thereby co-extruding the first layer with the second layer.

[0056] Before stretching, a non-porous polymer film may have a morphology characterized by a majority polypropylene phase (or matrix) within the polymer film, a minority polymer region of ethylene-containing copolymers such as ethylene-propylene copolymer regions, and a phase containing the major polypropylene phase within the minority polymer region. This allows for effective transfer of stretching force from the major phase to the minority region, which is then divided, and subsequently, micropores are initiated and developed by stretching. Thus, the non-porous films disclosed herein may undergo the stretching process (as described herein) to produce a microporous film.

[0057] In one embodiment, the microporous film described herein is oriented in the machine direction. The microporous film may be oriented by cold stretching in the machine direction and by hot stretching in the machine direction after cold stretching. Alternatively, or in addition, one or more cold stretches and / or one or more hot stretches may be performed in any other direction, such as the transverse direction (across the machine direction). The cold stretch percentage may be 25% to 150%, and formula I:

number

[0058] Cold stretching can be performed at temperatures ranging from 10°C to 50°C, but is typically performed at room temperature. Unless otherwise explicitly stated, cold stretching is performed at room temperature. In this specification, “room temperature” is considered to be a temperature of 15°C to 25°C (and more typically 20°C to 23°C). The percentage of heat stretching can be 50% to 500%, and is given by Equation II:

number

[0059] Thermal stretching can be carried out at temperatures ranging from 90°C to 140°C.

[0060] In some embodiments, a method for producing a microporous film includes providing the microporous film described herein and cold-stretching the film in the mechanical direction to a cold-stretch percentage of 25% to 200% at a temperature in the range of -20°C to 50°C, preferably 10°C to 50°C. The cold-stretch percentage is determined using Formula I above. After cold-stretching, the film is subjected to thermal stretching in the mechanical direction to a thermal-stretch ratio of 50% to 500% at a temperature in the range of 50°C to 150°C, preferably 90°C to 140°C or 100°C to 140°C. The thermal-stretch percentage is determined using Formula II above.

[0061] In one embodiment, the stretching process comprises one or more cold stretching steps, followed by one or more hot stretching steps, optionally accompanied by one or more thermosetting steps. The process may optionally include a post-annealing step. Film uniformity is important, and therefore it is preferable to maintain the temperature below 150°C.

[0062] In one embodiment, the stretching process may be carried out as the film moves along a production line which may include a series of rollers. The degree of stretching in the mechanical direction may be controlled by using rollers of different speeds or by different diameters of rollers. Optionally, a degree of stretching in the transverse direction may be carried out, which may be controlled by stretching the film transversely between a series of clips that grip the ends of the web and traverse downwards a pair of adjustable branch rails. A polymer film at the front end of a production line may appear colorless and transparent (before stretching), but as it moves along the production line, such as along the area where the stretching process is carried out, it may appear to change so that its opacity increases, a white haze develops, and the film then turns white due to the formation of pores (and the associated light scattering effect from the void spaces).

[0063] Processes for stretching non-porous films to produce microporous films have been previously reported (see, for example, U.S. Patent No. 3,801,404 to Druin et al. and U.S. Patent No. 3,426,754 to Bierenbaum et al.), but these reported processes using polyethylene or polypropylene films require an annealing step before the stretching process (or at an intermediate point between separate film stretching stages), sometimes along with a separate thermosetting step after the stretching process. However, the extension of the annealing time is problematic from the viewpoint of the desired objective of running a continuous production line for producing microporous films. Ideally, a continuous extrusion and pore formation process in a single continuous production line that does not require a holding period related to the extension of the annealing step is preferred. Advantageously, films produced from PP copolymers (and their blends) described herein do not require any annealing or thermosetting steps to produce microporous films from the stretching process (in this case, the mechanism of pore formation differs from that of polyethylene and polypropylene films previously reported). Accordingly, the PP copolymers described herein can be heated and extruded to form non-porous films that can be stretched in a continuous production line for manufacturing microporous films.

[0064] In certain embodiments, the present invention as described herein is a microporous polymer film comprising one or more polypropylene copolymers comprising one or more polypropylene homopolymer chain segments and one or more ethylene-containing copolymer chain segments, wherein (i) the polypropylene homopolymer chain segments comprise a total amount of 50 to 82% by weight based on the weight of the microporous polymer film or 43 to 79 mol% based on the molar content of propylene polymerization units in the polypropylene homopolymer chain segments as a percentage of the total molar content of polymerization monomer units in the microporous polymer film, and (ii) the ethylene-containing copolymer chain segments comprised of one or more polypropylene copolymers comprising one or more polypropylene homopolymer chain segments The present invention relates to a microporous polymer film comprising 18 to 50% by weight of the film, or 21 to 57 mol% of the total molar content of polymer monomer units in the ethylene-containing copolymer chain segments, based on the molar content of polymer monomer units in the ethylene-containing copolymer chain segments, wherein at least a portion of the ethylene-containing copolymer chain segments contains polymer units of ethylene in an amount of at least 45% by weight of the ethylene-containing copolymer chain segments, or at least 55 mol% of the total molar content of polymer monomer units in the ethylene-containing copolymer chain segments, based on the molar content of polymer units of ethylene in the ethylene-containing copolymer chain segments.

[0065] In one embodiment, a method for forming a microporous polymer film, the method step comprising: (a) one or more polypropylene copolymers, (i) one or more polypropylene homopolymer chain segments, comprising one or more polypropylene homopolymer chain segments in a total amount of 50 to 82% by weight based on the weight of the polypropylene copolymer or 43 to 79 mol% based on the molar content of propylene polymerization units in the polypropylene homopolymer chain segments as a percentage of the total molar content of polymerization monomer units in the polypropylene copolymer; and (ii) one or more ethylene-containing copolymer chain segments, comprising one or more polypropylene homopolymer chain segments in a total amount of 18 to 50% by weight based on the weight of the polypropylene copolymer or 21 to 57 mol% based on the molar content of polymerization monomer units in the ethylene-containing copolymer chain segments as a percentage of the total molar content of polymerization monomer units in the polypropylene copolymer. A method is disclosed that provides one or more polypropylene copolymers comprising an ethylene-containing copolymer chain segment, wherein at least a portion of the ethylene-containing copolymer chain segment contains ethylene polymer units in an amount of at least 45% by weight based on the weight of the ethylene-containing copolymer chain segment or at least 55 mol% based on the molar content of ethylene polymer units in the ethylene-containing copolymer chain segment as a percentage of the total molar content of polymer monomer units in the ethylene-containing copolymer chain segment; (b) forming a non-porous film from the polypropylene copolymer; and (c) subjecting the non-porous film to a series of cold-stretching and hot-stretching steps, including (i) at least one cold-stretching step at a temperature in the range of -20°C to 50°C, and (ii) at least one hot-stretching step at a temperature in the range of 50°C to 150°C, thereby producing a microporous polymer film.

[0066] In some embodiments, the method is a continuous process for producing a microporous polymer film. In particular, in some embodiments, the method proceeds without any annealing step after the formation of a non-porous film, and proceeds without any annealing or thermosetting step after the formation of a microporous polymer film, and is a continuous process for producing a microporous polymer film.

[0067] The present invention relates to a microporous film manufactured by the method described herein, and further to an article manufactured from the microporous film described herein.

[0068] The total thickness of the microporous film is not particularly limited and may be less than 2.54 mm (100 mils) in some embodiments. Different end uses may require different film thicknesses, or conversely, different film thicknesses may be more appropriate for some end uses. For example, a microporous film suitable for use as a house wrap may have a thickness of 51 to 254 μm (2 to 10 mils), preferably 102 to 178 μm (4 to 7 mils). A microporous film suitable for use as a roofing membrane in Europe may have a thickness of 102 to 508 μm (4 to 20 mils), preferably 127 to 254 μm (5 to 10 mils), or a microporous film suitable for use as a roofing membrane in North America may have a thickness of 508 to 2032 μm (20 to 80 mils), preferably 1016 to 1524 μm (40 to 60 mils). Furthermore, microporous films suitable for medical applications, such as packaging wraps for surgical packs, can have thicknesses ranging from 51 to 508 μm (2 to 20 mils), for example, 127 to 254 μm (5 to 10 mils).

[0069] The film thickness may depend on the end use of the microporous film discussed herein, and all thicknesses and ranges of thickness are considered appropriate for the microporous film of the present invention. Accordingly, all individual values ​​and subranges less than 2540 μm (100 mil) are included and disclosed herein. For example, in some embodiments, the total thickness of the microporous film (in μm) may be 2540, 2032, 1524, 1270, 1016, 762, 508, 381, 254, 203, 178, 152, 127, 102, 51, 38, 25, 13, or 2.5 μm. Each of the aforementioned figures may be preceded by the words “about,” “at least about,” or “less than about,” and any of the aforementioned figures may be used alone to describe a non-limiting range or in combination to describe a limiting range. In further embodiments, the total thickness of the microporous film may be 2.5 to 152.4 μm (0.1 to 6 mils), 2.5 to 102 μm (0.1 to 4 mils), or 2.5 to 50.8 μm (0.1 to 2 mils). In further embodiments, the total thickness of the film may be 2.5 to 38.1 μm (0.1 to 1.5 mils).

[0070] The films described herein are microporous, having specific pore sizes and porosity, which can be modified to control desirable and useful barrier properties for the selected end application. For house wrap films and roof membranes, the same types of barrier properties are important, such as water vapor transmission rate (WVTR) and permeability. Water vapor transmission rate depends on the film thickness. Permeability is substantially the normalized water vapor transmission rate (assuming a constant pressure difference across the film when comparing different film samples), and the film thickness records the adjusted WVTR. All "perm" here refers to US perm. 1 US perm = 5.72 × 10⁻¹⁰ -8 g / Pa·s·m 2 For building wrap applications, the appropriate average pore diameter (nm) can be 30-300 nm, and the appropriate film porosity to achieve 10-100 perm water vapor permeability can be 25-55% (and WVTR 70-700 g / 24h·m). 2(This can be within this range). Also, regarding the roof film, the appropriate median mean pore diameter (nm) can be 30-250 nm, and the appropriate film porosity to achieve a transmission of 10-70 perm can be 25-45% (and WVTR can be 70-500 g / 24h·m). 2 (This may be within the range). In the field of medical packaging, the same barrier properties are important, but the focus on permeability is usually on air (or gaseous disinfectant) permeability, which is measured as Gurley permeability, and maximum penetration (calculated %P) in the ASTM F2638 test (for porous packaging as a microbial barrier). max This concerns the barrier against bacteria / microorganisms, as measured by ). For medical packaging, the appropriate average pore diameter (nm) can be 300-1,000 nm, and 1-100 s / 100 cm 3 Useful range of Garley breathability and calculation %P less than 10 max The appropriate film porosity to achieve the value can be 55-75% (P max (For this, the smaller the value, the better.)

[0071] In some embodiments, the microporous polymer film has at least about 20% porosity, and the maximum porosity is not particularly limited. In the same or other embodiments, the microporous polymer film has up to about 75% porosity, and the minimum porosity is not particularly limited. For example, the microporous polymer film may have porosity (%) of 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, or 80%. Each of the aforementioned figures may be preceded by the words “about,” “at least about,” or “less than about,” and any of the aforementioned figures may be used alone to describe a non-limiting range or in combination to describe a limiting range. For example, but not limited to, the microporous polymer film may have porosity of at least about 20%, about 20% to about 75%, or about 25% to about 70%.

[0072] In some embodiments, the microporous polymer film has a median mean pore diameter (by volume) of at least about 20 nm, and the maximum median pore diameter is not particularly limited. In the same or other embodiments, the microporous polymer film has a median pore diameter up to about 2000 nm, and the minimum median pore diameter is not particularly limited. For example, the microporous polymer film may have a median pore diameter (nm) of 10, 15, 20, 25, 30, 40, 50, 60, 70, 80, 90, 100, 150, 200, 250, 300, 350, 400, 450, 500, 600, 700, 800, 900, 1000, 1500, and 2000 nm. Each of the aforementioned figures may be preceded by the words “approximately,” “at least approximately,” or “less than approximately,” and any of the aforementioned figures may be used alone to describe a non-limiting range or in combination to describe a limiting range. For example, but are not limited to, a microporous polymer film may have a median pore diameter of at least approximately 20 nm, approximately 20 nm to approximately 1000 nm, or approximately 25 nm to approximately 1000 nm.

[0073] In some embodiments, the microporous polymer film has a permeability of at least about 1 perm, and the maximum permeability is not particularly limited. In the same or other embodiments, the microporous polymer film has a permeability up to about 150 perm, and the minimum permeability is not particularly limited. For example, the microporous polymer film may have a permeability (perm) of 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 110, 120, 130, 140, or 150 perm. Each of the aforementioned figures may be preceded by the words “about,” “at least about,” or “less than about,” and any of the aforementioned figures may be used alone to describe a non-limiting range or in combination to describe a limiting range. For example, but not limited to, a microporous polymer film may have permeability of at least about 10 perm, about 10 perm to about 100 perm, or about 20 perm to about 100 perm.

[0074] In some embodiments, the microporous polymer film has a density of at least about 1 s / 100 cm3 The film has a Guarley Hill porosity (referred to herein as "Guarley permeability"), and the maximum Guarley permeability is not particularly limited. In the same or other embodiments, the microporous polymer film has a permeability of about 35,000 s / 100 cm 3 It has a Garley air permeability up to 1,5,10,15,20,25,30,35,40,45,50,55,60,65,70,75,80,85,90,95,100,110,120,130,140 or 150,200,300,400,500,600,700,800,900,1000,1500,2000,3000,400,500,600,700,800,900,1000,1500,2000,3000,4000,5000,6000,7000,8000,900,10000,15000,20000,25000,30000,35000 s / 100cm 3 Garley breathable (s / 100cm) 3 ) may have. Each of the aforementioned figures may be preceded by the words “about,” “at least about,” or “less than about,” and any of the aforementioned figures may be used alone to describe a non-limiting range or in combination to describe a limiting range. For example, but not limited to, a microporous polymer film may have at least about 1 s / 100 cm 3 , about 1s / 100cm 3 ~About 10000s / 100cm 3 , or approximately 10s / 100cm 3 ~About 5000s / 100cm 3 , or approximately 10s / 100cm 3 ~About 1000s / 100cm 3 , or approximately 10s / 100cm 3 ~About 100s / 100cm 3 Garley may have breathability.

[0075] In some embodiments, the microporous polymer film has a maximum penetration rate (%P) of less than approximately 10, calculated in the ASTM F2638-18 test. max ) has a barrier against microorganisms as measured by and has a minimum calculation %P maxThere are no particular restrictions. For example, microporous polymer films have a calculated %P of less than 10, 5, 2, 1, 0.5, 0.2, 0.1, 0.05, 0.03, 0.02, 0.015, 0.010, and 0.005. max It may have the following. Each of the aforementioned numbers may be preceded by the words “about,” “at least about,” or “less than about,” and any of the aforementioned numbers may be used alone to describe an unrestrictive range or in combination to describe a restrictive range. For example, but not limited to, a microporous polymer film may have a calculated %P of less than about 10, about 0 to about 10, or about 0 to about 1. max It may have. Ideally, the calculated %P max The value is zero, but the detection limit cannot be zero. Calculated %P max It can be approximately 0.005 or less to approximately 10, or approximately 0.005 or less to approximately 5, or approximately 0.005 or less to approximately 1.

[0076] The films described herein do not use the addition of fillers such as calcium carbonate, CaCO3, etc., to produce highly water vapor permeable films. Accordingly, the films described herein contain less than 5% by weight of fillers based on the total weight of polymers present in the film. Exemplary fillers, but not limited to, may include CaCO3, clay, silica, alumina, titania, zirconia, ceria, talc, magnesium carbonate, calcium sulfate, barium sulfate, porous glass beads, porous polymer beads, ceramic beads, aluminum trihydrate, magnesium trihydrate, wollastonite whiskers, wood flour, lignin, starch, clay, carbon black, graphite, graphene, carbon nanotubes, carbon fibers, carbon nanofibers, or combinations thereof. In further embodiments, the films described herein contain less than 3% by weight, less than 2% by weight, less than 1% by weight, or less than 0.5% by weight of fillers based on the total weight of polymers present in the film. In some embodiments, the films described herein contain no fillers (0% by weight). In many pharmaceutical applications, a 0% by weight filler is preferred to minimize the possibility of such particulate contamination of the film and the fragmentation of film particles.

[0077] The films described herein may incorporate UV stabilizers, especially if the intended use may include outdoor applications. Typical UV stabilizer additives include ultraviolet light absorbers, e.g., Tinuvin® 329 (BASF, Ludwigshafen, Germany) and hindered amine light stabilizers, e.g., Tinuvin® 770 or Chimassorb® 2020 (both BASF). For example, an effective UV stabilizer package for a microporous film of polypropylene copolymer PP C7054-07NA may include a combination of 0.75 wt% Chimassorb® 2020, 0.25 wt% Tinuvin® 770, 0.25 wt% Tinuvin® 329, and 0.15 wt% Irganox® B215 (antioxidant, BASF). PP C7054-07NA microporous film without UV additives turned into powder after an 8-week UV aging test at 50°C. In contrast, PP C7054-07NA microporous film with the above-mentioned UV additive package showed no visual defects such as cracking, yellowing, or deformation after an 8-week UV aging test at 50°C.

[0078] The films described herein may incorporate other additives, such as antioxidants (e.g., hindered phenolic resins, e.g., IRGANOX® 1010 or IRGANOX® 1076 (supplied by Ciba Geigy)), phosphates (e.g., IRGAFOS® 168 (supplied by Ciba Geigy)), processing aids, UV light stabilizers, heat stabilizers, pigments, colorants, antistatic additives, flame retardants, slip agents, antiblocking additives, biocides, antibiotics, and purifying / nucleation promoters (e.g., HYPERFORM® HPN-20E, MILLAD® 3988, MILLAD® NX 8000 (available from Milliken Chemical)). Other additives may be included in the films at concentrations typically used in the art to achieve their desired purposes. In some examples, one or more additives are included in amounts ranging from 0 to 10% by weight based on the total polymer weight of the film, or in amounts ranging from 0 to 5% by weight, 0.001 to 5% by weight, 0.001 to 3% by weight, 0.05 to 3% by weight, or 0.05 to 2% by weight based on the total polymer weight of the film. In embodiments herein where the fillers have other uses such as colorants or pigments, they are present in a total amount of less than 5% by weight.

[0079] Laminates also exist in this specification. Laminates include the microporous films described herein and a nonwoven substrate at least partially adhered to the films. As used herein, “nonwoven substrate” includes nonwoven webs, nonwoven fabrics, and any nonwoven structure in which fibers or threads are inserted in a manner other than regular or repeating. Nonwoven substrates described herein may be formed by various processes, such as carding processes, including, for example, airlaid processes, meltblown processes, spunbond processes, and bonded-carded web processes. Nonwoven webs may include single webs such as spunbond webs, carded webs, airlaid webs, spunlaced webs, or meltblown webs. However, due to the relative strengths and weaknesses associated with the various processes and materials used to manufacture nonwoven fabrics, composite structures of two or more layers may be used to achieve a better balance of properties. Such structures are often identified by letters indicating the various layers, for example, SM for a two-layer structure consisting of a spunbond layer and a meltblown layer, SMS for a three-layer structure, or more generally, an SXnS structure where S is the spunbond layer, and X can independently be the spunbond layer, carded layer, airlaid layer, spunlaced layer, or meltblown layer, and n can be any number, but practically generally less than 5. To maintain the structural integrity of such composite structures, the layers must be bonded together. Common bonding methods include thermal calendering, point bonding, adhesive lamination, ultrasonic bonding, and other methods known to those skilled in the art. All of these structures can be used in the present invention, particularly when incorporated with microporous films in the form of laminates.

[0080] The microporous films described herein should find applications in housing and construction, for example, as barrier layers for building coverings such as house wraps and roofing membranes.

[0081] Articles are also described herein. Articles include the films or laminates described herein. In some embodiments, the breathable backsheet includes the microporous films described herein. In other embodiments, the breathable backsheet includes laminates. Articles can be used in a variety of sanitary and medical applications. In some embodiments, articles may include diapers, training pants and adult incontinence articles or other similar absorbent clothing articles. In other embodiments, articles may include air masks, medical drapes, gowns, surgical gowns and protective clothing or other fabric (knitted or nonwoven) articles.

[0082] This embodiment is applicable to other technologies susceptible to problems similar to those described above. For example, the film may be used to manufacture cloth-like backsheets and medical backtable (or endtable) covers for operating rooms, as well as medical packaging (e.g., medical sterilization pouches and sterilization pouches for containing sterilized surgical instruments) and active packaging (e.g., sachets for containing desiccants in pharmaceutical tablet bottles). These are all within the scope of this embodiment. Unlike other candidates for breathable textile products in which the interstitial space between pores of the microporous polymer film described herein contains thin solid segments of PP homopolymer or PP homopolymer and E / P copolymer, where the interstitial space contains fibers that may or may not be bonded (typically by thermal bonding of the contact points they encounter). The advantage of the microporous polymer film of the present invention is that the stretching process of the present invention allows for better control of pore size and pore size distribution, resulting in pores formed by overlapping fibers and pore size and distribution with respect to the number density (fibers / cm²). 3This results in a narrower pore size distribution than other (fibrous) porous structures, which depend on the distribution of the number of fibers and fiber diameter. Furthermore, the microporous polymer films of the present invention have smaller pores with diameters in the nanometer range compared to fibrous materials with very large pore sizes in the range of several micrometers. Although fibrous structures can be manufactured from similar hydrophobic materials, the smaller pore size of PP-copolymer microporous polymer films can provide higher resistance to blood and body fluids, thereby making them suitable for use as breathable covers for operating room end tables. Another advantage of the microporous polymer films described herein compared to fibrous breathable films is that the possibility of fragmentation resulting from handling, cutting, conversion, and use of the microporous polymer films is much lower than with respect to fibrous structures. This makes the microporous polymer films suitable for use in ultra-clean spaces such as electronic processing, filtration, and sterile environments in medical and pharmaceutical applications.

[0083] Microporous films may also find applications in regular packaging (such as outer coverings, fruit packaging, powder packaging, and packaging for sensitive electronic components) and as filtration media (for gas or liquid separation). Films may be single-layer films or multilayer films. As used herein, “multilayer film” refers to a film having two or more layers that are at least partially adjacent, preferably but optionally identical in extent.

[0084] Some embodiments disclosed herein are described in the following clauses, and any combination of these clauses (or parts thereof) may be used to define an embodiment.

[0085] Clause A: In a particular embodiment, the present invention as described herein relates to a microporous polymer film comprising, consisting of, or essentially consisting of, one or more polypropylene copolymers comprising one or more polypropylene homopolymer chain segments and one or more ethylene-containing copolymer chain segments, wherein the microporous polymer film comprises (i) a total amount of polypropylene homopolymer chain segments of 50 to 82% by weight based on the weight of the microporous polymer film, and (ii) a total amount of ethylene-containing copolymer chain segments of 18 to 50% by weight based on the weight of the microporous polymer film, wherein at least a portion of the ethylene-containing copolymer chain segments comprises polymerization units of ethylene in an amount of at least 45% by weight based on the weight of the ethylene-containing copolymer chain segments.

[0086] Clause B: In certain embodiments, the present invention as described herein relates to a microporous polymer film comprising, consisting of, or essentially comprising one or more polypropylene copolymers, each comprising one or more polypropylene homopolymer chain segments and one or more ethylene-containing copolymer chain segments, wherein the microporous polymer film comprises (i) a polypropylene homopolymer chain segment comprising a total amount of 43 to 79 mol% of the polypropylene homopolymer chain segment based on the molar content of propylene polymerization units in the polypropylene homopolymer chain segment as a percentage of the total molar content of polymerization monomer units in the microporous polymer film, and (ii) an ethylene-containing copolymer chain segment comprising a total amount of 21 to 57 mol% of the ethylene-containing copolymer chain segment based on the molar content of polymerization monomer units in the ethylene-containing copolymer chain segment as a percentage of the total molar content of polymerization monomer units in the microporous polymer film, wherein at least a portion of the ethylene-containing copolymer chain segment comprises polymerization units of ethylene in an amount of at least 55 mol% based on the molar content of ethylene polymerization units in the ethylene-containing copolymer chain segment as a percentage of the total molar content of polymerization monomer units in the ethylene-containing copolymer chain segment.

[0087] Clause 1: In a particular embodiment, the present invention as described herein comprises, consists of, or is essentially composed of, one or more polypropylene copolymers comprising one or more polypropylene homopolymer chain segments and one or more ethylene-containing copolymer chain segments, wherein (i) the polypropylene homopolymer chain segments comprise a total amount of 50 to 82% by weight based on the weight of the microporous polymer film or 43 to 79 mol% based on the molar content of propylene polymerization units in the polypropylene homopolymer chain segments as a percentage of the total molar content of polymerization monomer units in the microporous polymer film, and (ii) the ethylene-containing copolymer chain segments The present invention relates to a microporous polymer film comprising a total amount of ethylene-containing copolymer chain segments, comprising 18 to 50% by weight of the microporous polymer film or 21 to 57 mol% as a percentage of the total molar content of polymerization monomer units in the microporous polymer film, wherein at least a portion of the ethylene-containing copolymer chain segments contains polymerization units of ethylene in an amount of at least 45% by weight of the ethylene-containing copolymer chain segments or at least 55 mol% as a percentage of the total molar content of polymerization monomer units in the ethylene-containing copolymer chain segments, based on the molar content of polymerization units of ethylene in the ethylene-containing copolymer chain segments.

[0088] Clause 2: The microporous polymer film of Clause 1, wherein at least a portion of the ethylene-containing copolymer chain segment contains ethylene polymer units in an amount of 45% to 80% by weight or 45% to 60% by weight based on the weight of the ethylene-containing copolymer chain segment, or 55 mol% to 86 mol% or 55 mol% to 69 mol% as a percentage of the total molar content of polymer monomer units in the ethylene-containing copolymer chain segment, based on the molar content of ethylene polymer units in the ethylene-containing copolymer chain segment.

[0089] Clause 3: The microporous polymer film according to Clause 1 or 2, wherein the total ethylene content of the polymerization form in the microporous polymer film is at least 10% by weight based on the weight of the microporous polymer film, or at least 14 mol% based on the molar content of the polymerization units of ethylene in the microporous polymer film as a percentage of the total molar content of polymerization monomer units in the microporous polymer film.

[0090] Clause 4: A microporous polymer film according to any one of Clauses 1 to 3, wherein the total ethylene content of the polymerization form in the microporous polymer film is 10 to 30% by weight or 15 to 25% by weight based on the weight of the microporous polymer film, or 14 to 39 mol% or 21 to 33 mol% as a percentage of the total molar content of polymerization monomer units in the microporous polymer film, based on the molar content of polymerization units of ethylene in the microporous polymer film.

[0091] Clause 5: The ethylene-containing copolymer chain segment is an ethylene-propylene copolymer chain segment, a microporous polymer film according to any one of Clauses 1-4.

[0092] Clause 6: The ethylene-propylene copolymer chain segments are random ethylene-propylene copolymer chain segments in the microporous polymer film of Clause 5.

[0093] Clause 7: The microporous polymer film of Clause 5, wherein the ethylene-propylene copolymer chain segment is an ethylene-propylene diblock copolymer chain segment comprising a polypropylene block and a polyethylene block, or a diblock copolymer chain segment comprising a polypropylene block and an ethylene-propylene copolymer block.

[0094] Clause 8: One or more ethylene-propylene copolymer chain segments are present in any one of the microporous polymer films according to Clauses 5, 6, or 7, in a total amount of 18 to 50% by weight based on the weight of the microporous polymer film or 21 to 57 mol% based on the molar content of polymer monomer units in the ethylene-propylene copolymer chain segments as a percentage of the total molar content of polymer monomer units in the microporous polymer film.

[0095] Clause 9: A microporous polymer film according to any one of Clauses 5, 6, or 7, wherein at least a portion of the ethylene-propylene copolymer chain segment contains polymerized ethylene in an amount of 45% to 80% by weight or 45% to 60% by weight based on the weight of the ethylene-propylene copolymer chain segment, or in an amount of 55 mol% to 86 mol% or 55 mol% to 69 mol% based on the molar content of polymerized ethylene polymerized units in the ethylene-propylene copolymer chain segment as a percentage of the total molar content of polymerized monomer units in the ethylene-propylene copolymer chain segment.

[0096] Clause 10: A microporous polymer film according to any one of Clauses 5, 6, 7, or 8, wherein the total ethylene content of the polymerization form in the microporous polymer film is at least 10% by weight based on the weight of the microporous polymer film, or at least 14 mol% based on the molar content of the polymerization units of ethylene in the microporous polymer film as a percentage of the total molar content of polymerization monomer units in the microporous polymer film.

[0097] Clause 11: A microporous polymer film according to any one of Clauses 5, 6, 7, or 8, wherein the total ethylene content of the polymerization form in the microporous polymer film is 10 to 30% by weight or 15 to 25% by weight based on the weight of the microporous polymer film, or 14 to 39 mol% or 21 to 33 mol% as a percentage of the total molar content of polymerization monomer units in the microporous polymer film, based on the molar content of polymerization units of ethylene in the microporous polymer film.

[0098] Clause 12: A microporous polymer film having at least 25% porosity and a median pore diameter of at least 25 nm (4V / A, according to UOP method 578-11), both of which are measured by mercury intrusion porosimetry, according to any one of Clauses 1 to 11.

[0099] Clause 13: A microporous polymer film having permeability according to ASTM E96 / E96M-16 in the range of 10 to 100 perm, conforming to any one of Clauses 1 to 12.

[0100] Clause 14: A microporous polymer film of any one of Clauses 1 to 13, further comprising a polypropylene homopolymer.

[0101] Clause 15: A microporous polymer film of any one of Clauses 1 to 14, further comprising an ethylene-containing copolymer.

[0102] Clause 16: A method for forming a microporous polymer film in one embodiment, the method step comprising: (a) one or more polypropylene copolymers, (i) one or more polypropylene homopolymer chain segments comprising one or more polypropylene homopolymer chain segments in a total amount of 50 to 82% by weight based on the weight of the polypropylene copolymer or 43 to 79 mol% based on the molar content of propylene polymerization units in the polypropylene homopolymer chain segments as a percentage of the total molar content of polymerization monomer units in the polypropylene copolymer; and (ii) one or more ethylene-containing copolymer chain segments comprising 18 to 50% by weight based on the weight of the polypropylene copolymer or 21 to 57 mol% based on the molar content of polymerization monomer units in the ethylene-containing copolymer chain segments as a percentage of the total molar content of polymerization monomer units in the polypropylene copolymer, wherein at least one of the ethylene-containing copolymer chain segments Disclosed are methods comprising, or essentially comprising, one or more polypropylene copolymers, each comprising at least 45% by weight of ethylene copolymer chain segments based on the weight of the ethylene copolymer chain segments, or at least 55 mol% based on the molar content of ethylene polymerization units in the ethylene copolymer chain segments as a percentage of the total molar content of polymerization monomer units in the ethylene copolymer chain segments; (b) forming a non-porous film from the polypropylene copolymer or a blend of polymers optionally comprising the polypropylene copolymer; and (c) subjecting the non-porous film to a series of cold-stretching and hot-stretching steps, including (i) at least one cold-stretching step at a temperature in the range of -20°C to 50°C, preferably 10°C to 30°C, and (ii) at least one hot-stretching step at a temperature in the range of 50°C to 150°C, preferably 90°C to 145°C or 100°C to 140°C, thereby producing a microporous polymer film. For example, the stretching in at least one cold-stretching step may be in the mechanical direction. Furthermore, the stretching in at least one heat stretching step may be in the mechanical direction and / or the transverse direction.

[0103] Clause 17: The method of Clause 16, wherein at least a portion of the ethylene-containing copolymer chain segment contains ethylene polymer units in an amount of 45% to 80% by weight or 45% to 60% by weight based on the weight of the ethylene-containing copolymer chain segment, or 55 mol% to 86 mol% or 55 mol% to 69 mol% as a percentage of the total molar content of polymer monomer units in the ethylene-containing copolymer chain segment, based on the molar content of ethylene polymer units in the ethylene-containing copolymer chain segment.

[0104] Clause 18: The method of Clause 16 or 17, wherein the microporous polymer film has a total ethylene content of polymerized form of at least 10% by weight based on the weight of the microporous polymer film, or at least 14 mol% based on the molar content of polymerized units of ethylene in the microporous polymer film as a percentage of the total molar content of polymerized monomer units in the microporous polymer film.

[0105] Clause 19: The method of any one of Clauses 16 to 18, wherein the microporous polymer film has a total ethylene content of 10 to 30% by weight or 15 to 25% by weight based on the weight of the microporous polymer film, or a total ethylene content of 14 to 39 mol% or 21 to 33 mol% of the polymerized monomer units in the microporous polymer film, based on the molar content of ethylene polymerized units in the microporous polymer film.

[0106] Clause 20: The ethylene-containing copolymer chain segment is an ethylene-propylene copolymer chain segment, according to any one of the methods in Clauses 16-19.

[0107] Clause 21: The method of Clause 20, wherein the ethylene-propylene copolymer chain segment is a random ethylene-propylene copolymer chain segment.

[0108] Clause 22: The method of Clause 20, wherein the ethylene-propylene copolymer chain segment is an ethylene-propylene diblock copolymer chain segment comprising a polypropylene block and a polyethylene block, or a diblock copolymer chain segment comprising a polypropylene block and an ethylene-propylene copolymer block.

[0109] Clause 23: The ethylene-propylene copolymer chain segment is present in a total amount of 18 to 50% by weight based on the weight of the polypropylene copolymer or 21 to 57 mol% based on the molar content of polymerized monomer units in the ethylene-propylene copolymer chain segment, according to any one of the methods of Clauses 20, 21, or 22, as a percentage of the total molar content of polymerized monomer units in the polypropylene copolymer.

[0110] Clause 24: At least a portion of the ethylene-propylene copolymer chain segment contains polymerized ethylene units in an amount of 45% to 80% by weight or 45% to 60% by weight based on the weight of the ethylene-propylene copolymer chain segment, or in an amount of 55 mol% to 86 mol% or 55 mol% to 69 mol% based on the molar content of polymerized ethylene units in the ethylene-propylene copolymer chain segment as a percentage of the total molar content of polymerized monomer units in the ethylene-propylene copolymer chain segment.

[0111] Clause 25: The total ethylene content of the polymerized form in the microporous polymer film is at least 10% by weight based on the weight of the microporous polymer film, or at least 14 mol% based on the molar content of the polymerized units of ethylene in the microporous polymer film as a percentage of the total molar content of polymerized monomer units in the microporous polymer film, according to any one of the methods of Clauses 20, 21, 22, or 23.

[0112] Clause 26: The total ethylene content of the polymerization form in the microporous polymer film is 10 to 30% by weight or 15 to 25% by weight based on the weight of the microporous polymer film, or 14 to 39 mol% or 21 to 33 mol% based on the molar content of the polymerization units of ethylene in the microporous polymer film, as a percentage of the total molar content of polymerization monomer units in the microporous polymer film.

[0113] Clause 27: The polypropylene copolymer shall have a melt flow rate of 0.1 to 100 g / 10 min, measured at 230°C and 2.16 kg according to ASTM D-1238, condition L, and 0.9 g / cm³. 3 One of the methods of clauses 16 to 26 having a superdensity.

[0114] Clause 28: A polypropylene copolymer is blended with a polypropylene homopolymer to form a polymer blend before forming a non-porous film, in any one of the methods of Clauses 16 to 27.

[0115] Clause 29: The polypropylene copolymer is blended with an ethylene-containing copolymer, preferably an ethylene-propylene copolymer, to form a polymer blend before forming a non-porous film, according to any one of the methods of Clauses 16 to 28.

[0116] Clause 30: Forming a non-porous film is achieved by any one of the methods of Clauses 16 to 29, which is achieved by extruding a polypropylene copolymer or a polymer blend thereof in a molten state.

[0117] Clause 31: A non-porous polymer film having a morphology characterized by a majority polymer phase of polypropylene, a plurality of minority polymer regions of ethylene-containing copolymers within the majority polymer phase, and an inclusion phase of the major polypropylene phase within the minority polymer regions, according to any one of the methods of Clauses 16 to 30.

[0118] Clause 32: In some embodiments, any one of the methods of Clauses 16 to 31 is carried out without any annealing step after the formation of the non-porous film.

[0119] Clause 33: Any one of the methods of Clauses 16 to 32, wherein at least one cold stretching step stretches the film by at least 10% in at least one direction, and at least one hot stretching step stretches the film by at least 20% in at least one direction.

[0120] Clause 34: In some embodiments, any one of the methods of Clauses 16 to 33 is carried out without any annealing or thermosetting steps after the formation of the microporous polymer film.

[0121] Clause 35: In some embodiments, any one of the methods described in Clauses 16-34 is a continuous process for producing a microporous polymer film.

[0122] Clause 36: The microporous polymer film shall have at least 25% porosity and a median pore diameter of at least 25 nm (4V / A, according to UOP method 578-11), both of which shall be measured by any one of the methods of Clauses 16-351, by mercury intrusion porosimetry.

[0123] Clause 37: The microporous polymer film has permeability in the range of 10 to 100 perm, according to ASTM E96 / E96M-16, by any one of the methods of Clauses 16 to 36.

[0124] Clause 38: A microporous polymer film formed by any one of the methods described in Clauses 16 to 37.

[0125] Clause 39: A non-porous polymer film is a microporous polymer film formed by any one of the methods of Clauses 16 to 37, having a morphology characterized by a majority polymer phase of polypropylene, a plurality of minority polymer regions of ethylene-containing copolymers within the majority polymer phase, and an inclusion phase of the main polypropylene phase within the minority polymer regions. In one embodiment, the non-porous polymer film has a morphology characterized by a majority polymer phase of polypropylene, a plurality of minority polymer regions of ethylene-propylene copolymers within the majority polymer phase, and an inclusion phase of the main polypropylene phase within the minority polymer regions.

[0126] Clause 40: A microporous polymer film of any one of Clauses 1 to 15, which is either a roof membrane or a component thereof.

[0127] Clause 41: A microporous polymer film according to Clause 40, having a thickness of at least 100 μm or at least 250 μm.

[0128] Clause 42: A microporous polymer film of any one of Clauses 1 to 15, which is at least part of a medical packaging or active packaging article or a medical back table cover.

[0129] Clause 43: Medical packaging or active packaging articles or medical back table covers comprising any one of the microporous polymer films described in Clauses 1 to 15.

[0130] Clause 44: Medical packaging or active packaging articles or medical back table covers comprising a microporous polymer film comprising one or more polypropylene copolymers comprising one or more polypropylene homopolymer chain segments and one or more ethylene-containing copolymer chain segments, wherein the microporous polymer film comprises (i) polypropylene homopolymer chain segments comprising a total amount of polypropylene homopolymer chain segments of 50 to 82% by weight based on the weight of the microporous polymer film or 43 to 79 mol% based on the molar content of propylene polymerization units in the polypropylene homopolymer chain segments as a percentage of the total molar content of polymerization monomer units in the microporous polymer film, and (ii) ethylene-containing copolymer chain segments comprising a total amount of polypropylene homopolymer chain segments comprising a total amount of polypropylene homopolymer chain segments of 50 to 82% by weight based on the weight of the microporous polymer film A medical packaging or active packaging article or medical back table cover comprising 18-50% by weight of ethylene-containing copolymer chain segments, or 21-57 mol% of ethylene-containing copolymer chain segments based on the molar content of polymer monomer units in the ethylene-containing copolymer chain segments, wherein at least a portion of the ethylene-containing copolymer chain segments contains polymerized ethylene units in an amount of at least 45% by weight, such as 45-80% by weight, preferably 45-60% by weight, or at least 55 mol%, such as 55-86 mol%, based on the molar content of polymerized ethylene units in the ethylene-containing copolymer chain segments, based on the molar content of polymerized ethylene units in the ethylene-containing copolymer chain segments.

[0131] Clause 45: The microporous polymer film has a barrier against microorganisms, equal to <10%, preferably <5% or <1%, of the maximum penetration, calculated %Pmax, as defined by ASTM F2638-18, for medical packaging or active packaging articles or medical back table covers as specified in Clause 44.

[0132] Clause 46: Microporous polymer films shall have a curing time of 10-35,000 seconds / 100cm². 3 Medical packaging according to Clause 44 or 45, having a Gurley gauge breathability and controlling the inflow or outflow of air or one or more gases into or out of the package.

[0133] Clause 47: A microporous polymer film is thermoformable and heat-sealable, for use in any one of the medical packaging applications described in Clauses 44-46.

[0134] Clause 48: A microporous polymer film comprising a polypropylene copolymer produced from the reaction product of a polypropylene homopolymer and an ethylene-propylene copolymer.

[0135] The present invention is further defined in the following embodiments, where all parts and percentages are by weight unless otherwise specified. While these embodiments illustrate preferred embodiments of the present invention, it should be understood that they are provided merely as examples and should not be construed as limiting. From the foregoing discussion and these embodiments, those skilled in the art will be able to identify essential features of the present invention and make various modifications and alterations to suit various uses and conditions without departing from its spirit and scope. [Examples]

[0136] material Homopolymer polyethylene is referred to herein as PE. The homopolymer-PE used herein is HDPE 6400, a resin available from Dow Chemical Company, Midland, MI, USA.

[0137] Homopolymer polypropylene is referred to herein as PP. The homopolymer-PP used herein is PP H314, a resin available from Braskem, USA (Philadelphia, PA, USA).

[0138] Ethylene-propylene copolymers are referred to herein as EP. Numerous EP and PP-EP copolymers, as well as homopolymer-PP blends with EP or PP-EP copolymers, are described herein, for example, in detail in Examples 2 and 6.

[0139] The polypropylene copolymer resin used in this study is PP C7054-07NA, purchased from Braskem USA, which is a PP-EP copolymer containing PP chain segments and ethylene-propylene random copolymer chain segments. The PP C7054-07NA resin contains 32.9% by weight of ethylene-propylene copolymer (and 100-32.9=67.1% PP), but the ethylene content in the ethylene-propylene copolymer chain segments is 49.7% by weight. It is 0.9 g / cm³. 3 It has a density and a melt index of 7 g / 10 min at 230°C and 2.16 kg. Other PP copolymer resins are listed in Table 2.

[0140] The term "Tyvek®" itself refers to Tyvek® Housewrap (approximately 32% porosity; average pore diameter of 37 nm), while the term "Tyvek® 1073B" refers to a special grade of Tyvek® nonwoven fabric used as a medical packaging layer (approximately 65% ​​porosity; average pore diameter of 2500 nm).

[0141] Cast Film The PP C7054-07NA resin cast film was manufactured on a film casting line consisting of a 1.25-inch Killion uniscrew extruder and a 30-inch wide cast die with a die spacing of approximately 762 μm (30 mils). A typical temperature profile (for extruder areas 1-8) of a pilot-scale extrusion line using a 76.2 cm (30 inch) die used to manufacture the (co)polymer cast film described herein may be as follows (for example, for PP copolymer film): 180, 200, 210, 210, 210, 210, 210, 210°C.

[0142] Uniaxial and biaxial stretching of film on an Iwamoto twin-axis stretcher Uniaxial stretching (machine-directed orientation, MDO) procedure: The film was cut to predetermined dimensions. Adhesive tape was attached to both ends of the film (laterally), and it was fitted into a specially designed sample holder. The sample holder plate was secured together with five bolts. Next, the legs of the sample holder were attached to the back of the grip of an Iwamoto twin-axis stretcher (BIX-703, Iwamoto Seisakusho). Uniaxial cold stretching was performed on the film in the machine direction. Then, the door of the sample chamber was closed, the sample chamber was heated to 100°C, and then held at this temperature for 1 minute. After that, uniaxial hot stretching was performed on the film in the machine direction. The degree of cold stretching was:

number

number

[0143] After stretching, the film changed to white due to the formation of a microporous structure.

[0144] For biaxial stretching, a PP-based film was cut to predetermined dimensions (70mm x 70mm) and then loaded onto the grip of an Iwamoto biaxial stretcher. The film was simultaneously biaxially stretched in both directions at room temperature and then heated to 100°C. After being held at 100°C for 1 minute, the film was simultaneously biaxially stretched in both directions at the high temperature. The degree of stretching for biaxial stretching is defined in the same way as for uniaxial stretching.

[0145] Differential scanning calorimetry (DSC) A portion of the sample was weighed and placed in an aluminum sealed DSC pan (pan P / N 900793.901 and lid P / N 900794.901), which was then sealed. The sample weight was approximately 1–4 mg for each sample. The samples were scanned in a TA Instruments Q2000 DSC (Differential Scanning Calorimeter) (P / N 970001.901) (s / N 2000.0877) equipped with an automated sampler, 50 ml / min nitrogen purging, and mechanical cooling accessories. The running parameters for the heating-cooling heating cycle were -20°C to 200°C at 10°C / min, with a sampling interval of 0.1 seconds / pt. The scans were analyzed using Universal Analysis V4.7A TA Instruments software. The melting points obtained from the DSC scans are shown as output from the instrument software, corresponding to the peak temperature versus temperature plot in the heat flow for the second heating cycle.

[0146] Mercury intrusion porosimetry Mercury intrusion porosimetry analysis was performed on a Micromeritics Autopore IV 9520 according to ASTM D4404-10. Prior to mercury analysis, the sample was mechanically degassed under vacuum at room temperature to remove any physically adsorbed species (i.e., water) from the sample surface.

[0147] The test conditions included Hg filling pressure of 0.50 psia, Hg contact angle of 130°, Hg surface tension of 485 dynes / cm, Hg density of 13.53 g / mL, evacuation time of 30 minutes, a small-bore hardness tester with a 5 cm³ valve (solid type: 0.392 stem volume), an equilibrium time of 30 seconds, a 92-point pressure table (75 press-fit plus 17 extrusion pressure points), and mechanical evacuation <50 μm Hg. Low-to-high pressure intersections were collected at approximately 46 psia (3.8 μm). The pressure table used was designed to allow incremental pressure distribution on a logarithmic scale from 0.5 to 60,000 psia and was used to detect pore size (diameter) from 0.003 to 400 μm. As the pressure was gradually increased from vacuum to a maximum of approximately 60,000 psia, mercury was pushed into smaller pores. According to the UOP method 578-11, the average pore diameter (4V / A) is calculated based on the assumption that all pores are right cylindrical columns with length (l) and diameter (d). Total pore volume (V = πd 2 When l / 4) is divided by the total pore area (=πdl), the average pore diameter (d) is 4V / A.

[0148] To confirm that the instrument was functioning correctly, silica-alumina reference material, lot A-501-46, was analyzed. The reported (by volume) median pore diameter of the reference sample was 0.0072 ± 0.0005 μm. Autopore reported a (by volume) median pore diameter of 0.0072 μm.

[0149] Scanning electron microscopy (SEM) The samples were freeze-cut, mounted to the SEM stub with carbon tape, and then coated with 30 nm gold to reduce static charge. Using the FEI Nova NanoSEM Model 600 in secondary electron (TLD) imaging mode, the upper and cut surfaces of each sample were imaged at specific positions and at various magnifications ranging from 5,000x to 10,000x. To prevent beam damage to the samples, the acceleration voltage was set to within 3-5 kV with 3-4 spot diameters (size of the spot diameter knob) at a working distance of approximately 5 mm (distance from the final polarity of the lens to the sample when the image is in focus).

[0150] Transmission electron microscopy (TEM) The PP copolymer film was cut into small trapezoidal shapes so that portions could be collected. Using a diamond knife on a Leica EM UC7 microtome, portions approximately 100 nanometers thick were collected at ambient temperature and placed on a 400-mesh virgin TEM grid for observation. The microtome-collected films were stained with a 0.5 M (mol / L) osmium tetroxide aqueous solution in the gas phase for 3–5 minutes at ambient temperature. TEM images were collected on an FEI Tecnai 12 operated at an accelerating voltage of 120 kV using a Gatan MultiScan CCD camera.

[0151] X-ray diffraction technology Small-angle X-ray scattering (SAXS) and wide-angle X-ray diffraction (WAXD) studies were performed at the Advanced Photon Source (Argonne National Laboratory) using the DND-CAT (5-ID-D beamline). A standard APS Undulator A was used as the X-ray source with an X-ray energy setting of 17 keV (λ=0.7923 Å). All samples were processed in normal beam transmission mode. Detector calibration was performed using silver behenate and lanthanum hexaboride standard reference materials. The two-dimensional dispersion pattern was reduced to a one-dimensional dataset of dispersion intensity against dispersion vectors by radiative agglomeration of the two-dimensional image. The reduction and analysis of the one-dimensional pattern were performed using the commercially available software package JADE.

[0152] Water vapor transmission rate (WVTR) measurement (ASTM F1249) For this study, a Mocon 3 / 33 model MG module was used to evaluate WVTR. The test conditions were 37.8°C / 100%RH according to ASTM method F1249. 20.3cm 2To concentrate the test area to approximately 2 inches in diameter, a film sample was prepared using a 76.2 μm (3 mil) aluminum foil / acrylic adhesive mask. The film sample divided the test cell into two halves. The ends of the test cell were securely sealed to prevent outside air from leaking into the cell. This was achieved using silicone grease to assist in sealing the film to the cell (carrier gas side), and a rubber O-ring was used to seal the outer cell cover or water vapor side. The standard sample area was 50 cm². 2 During a typical test, water vapor (test gas) was continuously introduced into the outer half of the test cell. This gas could be generated by the instrument at 100% relative humidity (moist sponge) or 30-90% relative humidity. The water vapor permeated the film sample and was then transported to an IR sensor on a carrier gas (dry nitrogen), where a current was generated that was directly proportional to the amount of water vapor passing through the film. Data from the IR sensor was collected by a computer, and a final value explaining the water vapor permeation rate of the test material was calculated. WVTR data was expressed as grams / 24h·m 2 It is reported in units of g·cm / 24h·m. Normalized WVTR takes film thickness into account, 2 It is reported as such.

[0153] Water vapor permeability (ASTM E96 / E96M-16) Water vapor permeability was determined according to ASTM E96 / E96M-16, Standard Test Method for Water Vapor Permeability of Materials, Desiccant Method. The test specimen was cut into a circular disc with a diameter of 90.3 mm. Calcium chloride was filled into the pocket of the dish to within 6.4 mm (1 / 4 inch) of the test specimen. The test specimen was then fitted onto the dish just above the pocket, with a metal plate protruding 76.1 mm in diameter, exposing the specimen to the environment. The test specimen was prepared with the outer surface of the product facing the desiccant. The assembly was then placed in a control chamber operating at a temperature of 23 ± 2°C and a relative humidity (RH) of 50 ± 5%, respectively. The weight of the assembly was then measured periodically. Water vapor permeability data was reported in units of "perm," in grams / 24h·m². 2It is possible to convert permeation to water vapor permeation in units of 10. In this specification, any use of the unit "perm" refers to US perm. 1 US perm = 5.72 × 10 -8 g / (Pa·s·m 2 ).

[0154] Garley Hill porous (Garley breathable) To measure the Gurley flow value of microporous films, a Genuine Gurley Instruments Densometer and a Lorentzen & Wettre L&W Model 121D Densometer were used. The densometer was used to measure the gas (e.g., the conventionally used 100 cm³ in this test). 3 The time required for a given volume of air to pass through a 1-inch diameter area of ​​the film (and a specific pressure gradient, conventionally, approximately 4.9 inches of water) is recorded. The test procedure conformed to the TAPPI T-460 OM-11 method. Prior to the test, a confirmation test was performed using a calibration plate with a known value for Gurley air permeability (19.2 seconds). The calibration plate allowed 100 cm³ to pass through within 19.2 seconds. 3 It was possible for air to pass through. Once confirmed, the microporous film sample was tested. Even though the permeability depends on the area and pressure of the test sample, these values ​​are standardized with respect to the instrument, so the results are as usual in s / 100cm 3 It is reported, or sometimes (100cm of air) 3 (Since the samples are also standardized, they are simply reported as seconds, s.) In this specification, Guarley Hill porosity is described as Guarley permeability and is expressed as s / 100cm as is common in the art. 3 It will be reported.

[0155] Grab tensile test Grab tensile tests were performed on an Instron Tester. The test procedure followed ASTM D 5034-09 (2013). The grab specimen was gripped at the center of its width to ensure that the upper and lower portions were not equally gripped. The crosshead speed was 12 inches / min for all experiments. The Instron recorded the tensile strength (Newtons per unit width) and elongation (%) at peak load.

[0156] Nuclear magnetic resonance (NMR) spectroscopy Approximately 0.25 g of the sample was cut into small pieces and placed in a 10 mm NMR tube. 2.6 ml of tetrachloroethane-d2 (TCEd2) containing 10 mM mitigating agent was added. The sample was then heated to 115°C. Using the following parameters, an NMR spectrum was obtained on a Bruker 600 MHz spectrometer equipped with a 10 mm cryogenic probe. 13 13C NMR and diffusion measurements (translational diffusion) were performed to confirm whether the material was a homopolymer or a blend. Repeat time: 15 seconds Number of scans: 1536 90° pulse: 12ms Spectral width: 240 ppm Temperature: 115℃ Spectral center: 90 ppm

[0157] Gel permeation chromatography (GPC) The sample was dissolved in a carrier liquid at a concentration of 1 mg / ml by shaking in 1,2,4-trichlorobenzene (TCB) containing 200 ppm butylhydroxytoluene (BHT) at 160°C for 2 hours. GPC was performed on a PolymerChar high-temperature LC system operated in GPC mode. The injection volume was 300 μl. The flow rate was 1 ml / min. The eluent was TCB containing 200 ppm BHT. Separation was performed on two 7.5 × 300 mm PL-Gel mixed B columns (Agilent). An integrated IR5 detector was used for detection in PolymerChar HTLC (high-temperature liquid chromatography). A series of 16 polystyrene (PS) narrow molecular weight distribution standards (Agilent Corporation) was used for molecular weight calibration. The calibration range was 0.58 to 3750 kg / mol, and the calibration curve was least squares fitted to a cubic polynomial. Therefore, the reported molecular weight is the PS equivalent molecular weight value. Once confirmed, the microporous film sample was tested.

[0158] Microbial barrier test (ASTM F2638-18) The microbial barrier test (ASTM F2638-18) uses aerosol filtration to measure the performance of porous packaging materials as surrogate microbial barriers and is applicable to porous materials used to package devices for end-user sterilization medical applications. The aerosol filtration performance of porous packaging materials is measured by generating a defined aerosol of 1.0 μm particles and evaluating the filtration efficiency of the material using a single or double particle counter. The test results are calculated as %P max This is recorded as the highest percentage concentration of particles in the filtrate aerosol (particles that remain aerosolized after passing through the test specimen) when the test specimen is tested over a range of pressure differences or airflow velocities. max A lower value indicates better barrier protection against particulate matter or microorganisms.

[0159] Example 1 This example investigates the effect of pre-stretch annealing on homopolymer PP films. Table 1 shows the stretching conditions and corresponding porosity and pore size (median pore diameter) of homopolymer polypropylene, PP H314, both with and without pre-stretch annealing. The notation CSXX-HSYY indicates that the film was subjected to XX% cold stretching followed by YY% hot stretching.

[0160] [Table 1]

[0161] Table 1 shows that prolonged annealing at temperatures near the melting point of PP is required to achieve the desired pore size and porosity. PP H314 samples that were not annealed did not turn white after stretching, and correspondingly, as shown in Table 1, the films exhibited very low porosity (2-4%). ​​In contrast, when annealing was performed at 150°C for 24 hours, the films immediately turned white after the same stretching conditions, and porosity of 20-24% was achieved. Similar results were obtained for homopolymer PE (HDPE 6400) films.

[0162] Furthermore, to determine whether polymer incompatibility aids pore formation when the film is not pre-annealed, blends of homopolymer PE (HDPE 6400) and homopolymer PP (PP H314) were investigated. Blends of homopolymer polypropylene and homopolymer polyethylene were prepared in a twin-screw extruder and extruded into films. Extruded films with blend ratios of 100:0, 90:10, 80:20, 70:30, 50:50, 30:70, 20:80, 10:90, and 0:100 (homopolymer polyethylene to homopolymer polypropylene) were prepared as described above without performing the annealing step, and then subjected to continuous cold (CS) and hot (HS) uniaxial stretching (25% cold stretching at room temperature and 100 mm / sec, followed by 100% hot stretching at 100°C and 5 mm / sec). Again, when annealing was not performed, no pore formation was observed with respect to these PP / PE homopolymer blend films.

[0163] Long annealing times present problems in terms of running a continuous production line to produce microporous films for the desired purpose. Ideally, a continuous extrusion and pore formation process in a single continuous production line is preferred, which does not require a holding period related to the extension of the annealing step.

[0164] Example 2 One of the objectives of the present invention is to produce a film that can form pores during film stretching without requiring any heat annealing step before or after film stretching. Eliminating the annealing step in the conventional process enables a continuous manufacturing process. In this embodiment, pore formation in homopolymer polypropylene induced by microphase separation was investigated in order to reduce the required annealing time or, preferably, to completely eliminate the annealing step from a similar manufacturing process for polyethylene or polypropylene homopolymers. For this reason, a PP copolymer consisting of homopolymer polypropylene (PP) chain segments and ethylene-propylene (EP) copolymer chain segments was prepared and extruded into a film.

[0165] To define the effective parameters and range of the present invention, PP copolymers of four different reactor grades were evaluated. The characteristics of the various PP copolymers are shown in Table 2 (melt flow rate, EP copolymer content (isotactic PP content is 100-EP content), and ethylene and propylene content in the EP copolymer chain segments).

[0166] [Table 2]

[0167] These PP copolymer films were prepared as described above and then subjected to continuous cold (CS) and hot (HS) uniaxial stretching (25% CS at 100 mm / sec, followed by 100% HS at 100°C and 5 mm / sec). The film characteristics (average pore size, porosity, and WVTR) are shown in Table 3.

[0168] [Table 3]

[0169] The comparative examples, PP TI4020N and PP INSPIRE film® 114, had very low average pore diameters (8-12 nm) and very low film porosity (7-10%), and these film characteristics were found to correspond to very low water vapor transmission rates and very low water vapor permeability. Both samples were unsuitable for their intended purpose as breathable films. On the other hand, the PP C700-35N and PP C7054-07NA films of the examples of the present invention had average pore diameters and film porosity in a target range similar to commercially available Tyvek®, and film characteristics such as water vapor transmission rates and water vapor permeability that suggest both samples are suitable as breathable films.

[0170] Example 3 PP copolymers, including PP C7054-07NA resin, homopolymerized polypropylene chain segments, and ethylene-propylene copolymer chain segments, were selected for further research to optimize stretching conditions in order to investigate the range of microporous film characteristics available through this approach. The initial thickness of the PP C7054-07NA resin film before stretching was 203 μm.

[0171] As described above, films were prepared from PP C7054-07NA and subjected to continuous cold and hot uniaxial stretching under various process conditions listed in Table 4. Subsequently, film characteristics (pore size and porosity) were evaluated to confirm practical process parameters.

[0172] [Table 4]

[0173] Table 4 shows that the stretching conditions can be optimized to adjust the desired porosity and average pore diameter. Numerous comparisons can be performed with respect to specific stretching variables (cold stretching (%), hot stretching (%), and hot stretching temperature (°C)) (by controlling two of the three variables to remain constant while changing a third variable). For example, one such series is illustrated by samples 1-4, which show the effect of hot stretching temperature (°C) when the range of room temperature cold stretching and hot stretching is kept constant (25% and 50%, respectively). As the hot stretching temperature increases in the temperature range of 60-120°C, porosity and pore diameter (median pore diameter) increase. Another such series is illustrated by samples 11-16, which show the effect of hot stretching at 100°C after 25% room temperature cold stretching. Again, as the degree of thermal stretching increases in the 25-100% range, porosity and pore size (median pore diameter) increase, but this trend recedes at higher degrees of thermal stretching (200 or 300%).

[0174] Example 4 This example investigates the performance of uniaxially oriented microporous films made of PP copolymer. Example 3 demonstrated the effect of film stretching conditions on pore formation (in terms of porosity (%) and average pore diameter (nm)). As Table 4 above clearly shows that the degree of thermal stretching has a significant effect on porosity and average pore diameter, this series (samples 11-14) was selected for further study, including physical properties and performance data.

[0175] PP C7054-07NA resin microporous films were subjected to the same cold stretching degree (25%) at 25°C, but the range of heat stretching degree at 100°C was 25% to 100%. The initial thickness of the PP C7054-07NA resin film before stretching was 203 μm, and the final film thickness after stretching under various stretching conditions is listed in Table 5.

[0176] Mercury porosimetry was used to measure the average pore diameter and porosity of the stretched PP C7054-07NA films in this series, and the results are summarized in Tables 4 and 5. The pore distribution of the PP C7054-07NA microporous films in this series is illustrated in Figure 1B and compared with that of Tyvek® in Figure 1A. Note that the y-axis scale is different in Figure 1A compared to that shown in Figure 1B.

[0177] [Table 5]

[0178] Table 5 and Figures 1A and 1B show that, under appropriate stretching conditions, PP C7054-07NA microporous film can exhibit larger pore sizes and porosity than Tyvek® Housewrap.

[0179] [Table 6]

[0180] As shown above (Table 4, Example 3), both porosity and pore size (average pore diameter) increase as the thermal stretching range increases in the 25-100% thermal stretching range. Furthermore, it is expected that an increase in both porosity and average pore diameter will lead to an increase in water vapor permeability ("perm") (Table 6). As shown in Table 6, by adjusting the pore diameter of the PP C7054-07NA microporous film, water vapor permeability can be varied from 14 perms to 82 perms (ASTM E96). Note that the water vapor permeability for Tyvek® house wrap of similar thickness is approximately 60 perms. Table 6 also shows the Guarley permeability of the PP C7054-07NA microporous film, which indicates that the C7054-07NA microporous film may have a better barrier to airflow and therefore may be a better option for improving the energy efficiency of a house than, for example, Tyvek®.

[0181] Example 5 This example considers the morphology of PP copolymer films. Conventional blends of homopolymer polypropylene and a small number of homopolymer polyethylene components produce films (PP / PE) with microphase separation resulting in incompatible regions of polyethylene within the polypropylene matrix. The polypropylene copolymers disclosed herein were cast as films and investigated for the purpose of generating microphase separation within the incompatible EP regions of the polymer film. Such microphase separation generates an inclusion phase within the incompatible region. The morphology of these films before and after stretching was investigated by SEM and TEM.

[0182] Figure 2 shows SEM images of the film cross-section. Figure 2A shows a cross-section of an unstretched PP C7054-07NA film (indicated by a 20-micron scale bar), while Figures 2B and 2C show stretched PP C7054-07NA films by 25% cold stretching and 50% hot stretching (100°C). Figure 2B is shown with a 20-micron scale bar compared to the 5-micron scale bar in Figure 2C. In the unstretched PP C7054-07NA film in Figure 2A, microphase separation and associated region formation can be observed in regions ranging in diameter from several hundred nanometers to approximately 3 microns. In Figures 2B and 2C, the PP C7054-07NA films were not annealed and were directly subjected to cold stretching (25%) at a stretching rate of 100 mm / sec, followed by hot stretching at a stretching rate of 5 mm / sec and a temperature of 100°C. As can be seen from the SEM images of the film cross-section in Figures 2B and 2C, many pores are formed by 25% cold stretching and 50% hot stretching.

[0183] Figure 3 shows SEM images of the film surface. Figures 3A and 3B show unstretched PP C7054-07NA film, with Figure 3A indicated by a 20-micron scale bar compared to the 10-micron scale bar in Figure 3B. Figures 3C and 3D show PP C7054-07NA film stretched by 25% cold stretching at a stretching speed of 100 mm / sec followed by 50% hot stretching at a stretching speed of 5 mm / sec (100°C), with Figure 3C indicated by a 20-micron scale bar compared to the 10-micron scale bar in Figure 3D. Before stretching, the film surface is very smooth (Figures 3A and 3B). In contrast, pores can be clearly observed on the surface of the stretched PP C7054-07NA film (Figures 3C and 3D).

[0184] Figure 4 shows TEM images of the film before and after stretching. Figures 4A and 4B show the PP C7054-07NA film before and after stretching (25% CS; 50% HS, as described above), and both Figures 4A and 4B are indicated by a 1-micron scale bar. Figures 4C and 4D show the PP INSPIRE® 114 film before and after stretching (25% CS; 50% HS, as described above), and both Figures 4C and 4D are indicated by a 0.2-micron scale bar.

[0185] In the unstretched PP C7054-07NA film shown in Figure 4A, microphase separation and associated region formation can be easily observed in regions ranging in diameter from several hundred nanometers to approximately 3 microns. The TEM images in Figures 4A and 4B suggest that the cavitation process in the ethylene-propylene (EP) region is nucleated in the PP C7054-07NA film. While we do not wish to be constrained by theory, it is thought that the inclusion morphology of the PP microphase within the EP region of the PP matrix allows for the effective transfer of stretching force to the microphase region, thereby dividing the microphase region into small fragments and initiating pore formation and growth. In contrast, after stretching the PP INSPIRE® 114 film, the EP region of the PP INSPIRE® 114 film only showed elongation along the stretching direction (Figures 4E and 4F). No pore formation occurred.

[0186] Further evidence of the different responses to stretching between films of PP C7054-07NA or PP C700-35N compared to PP TI4020N or PP INSPIRE® 114 was observed in wide-angle X-ray dispersion (WAXS) studies. The WAXS patterns were correlated with the Bragg diffraction of X-rays by the polypropylene crystalline lattice, providing information on the relative amounts of crystal composition, crystal orientation, and crystallinity.

[0187] Figure 5 shows the WAXS patterns of films made from two different PP copolymers, PP C7054-07NA and PP TI4020N. Samples for each copolymer included unstretched films and samples stretched by 25% cold stretching at room temperature and 100% hot stretching at 100°C. No significant changes in crystal structure were observed between the pre- and post-stretching stages for the PP C7054-07NA resin film (Figures 5A and 5B, respectively). The same observations were made for the PP C700-35N resin film (not shown). As shown in Figures 5C and 5D, significant orientation was observed in the PP TI4020N resin film due to rotation and reorganization of the crystal structure into a filamentous structure, caused by the emission of strong diffraction intensities in the (110), (040), (130), and (131) planes. Similar observations were made for the PP INSPIRE® 114 resin film (not shown). From the WAXS results above, it was inferred that while the stretching force was applied to the crystalline polypropylene structure of PP TI4020N resin film and PP INSPIRE® 114 resin film, during the stretching process of PP C7054-07NA resin and PP C700-35N resin film, the stretching force was transferred to the EP phase to initiate and grow pores. This discrepancy results in high porosity for both PP C7054-07NA resin and PP C700-35N resin microporous films, but low porosity for both PP TI4020N resin film and PP INSPIRE® 114 resin microporous film.

[0188] Example 6 Pore ​​formation after stretching of films that have not been annealed has been previously demonstrated using PP copolymers (see PP C7054-07NA microporous film above) (Examples 2-4 above). Further blending of this PP copolymer as the main component with homopolymer-PP, PP H314 (as a minor component) was also investigated (Table 7). Films were prepared as described above and stretched under the following conditions: 25% cold stretching at a stretching speed of 100 mm / sec (room temperature), followed by 100% hot stretching at a stretching speed of 5 mm / sec (100°C).

[0189] [Table 7]

[0190] By increasing the amount of homopolymer-PP and blending it with PP C7054-07NA copolymer, followed by cold and hot stretching processes, progressively lower porosity and lower average pore diameter were obtained in the stretched microporous film until pore formation was no longer achieved with an additional 40% of homopolymer-PP.

[0191] Similarly, pore formation after stretching of films that have not been annealed has been previously demonstrated using another PP copolymer (see PP C700-35N microporous film, Table 3) (Example 2). Further blending of this PP copolymer as the main component with homopolymer-PP, PP H314 (as a minor component) was also investigated (Table 8).

[0192] [Table 8]

[0193] The inclusion morphology was also reduced by compounding 20% ​​by weight of homopolymer PP H314 with PP C7054-07NA using a twin-screw extruder, followed by film production. As a result, during stretching, most of the microphase regions were extended only along the stretching direction (see, for example, TEM in Figures 6A and 6B).

[0194] The results for films from a blend of PP C700-35N with homopolymer-PP were similar to those for films from a blend of PP C7054-07NA with homopolymer-PP.

[0195] As described above, pore formation after stretching of an unannealed film has been demonstrated for PP copolymers (see PPC7054-07NA microporous film above). It has also been demonstrated that this copolymer can be further blended with PP copolymer and PP TI4020N (as a minor component) to form pores after stretching of an unannealed film (Table 9).

[0196] [Table 9]

[0197] A blend of PP C700-35N and PP TI4020N can also be used to form a film that can be stretched (without prior annealing) to produce a microporous film.

[0198] Other polymer blends were evaluated as follows: VERSIFY® 2000 resin (melt flow rate = 2g / 10 min at 230°C, 2.16 kg) is an ethylene-propylene random copolymer with a composition of 94% P / 6% E (propylene-rich). VERSIFY® 2400 resin (melt flow rate = 2g / 10 min at 230°C, 2.16 kg) is also an ethylene-propylene random copolymer with a composition of 86% P / 14% E (propylene-rich). In each case, two blend ratios (85:15 and 70:30) with homopolymer PP (PP H314) were prepared. PP H314 was the main component in all blends. Films of these blends that had not been annealed were subjected to CS25-HS100 stretching conditions (described above). None of these PP / EP blends formed pores after the stretching process. This may be due to the high content of propylene segments in VERSIFY® 2000 and VERSIFY® 2400 resins. Propylene segments have good compatibility with the PP matrix and therefore cannot induce sufficient phase separation in the PP H314 resin.

[0199] The 13C04R21 experimental resin (melt flow rate = 18 g / 10 min at 230°C, 2.16 kg) is an isotactic PP diblock copolymer having a 50:50 ratio of PP:EP components in the copolymer, and the EP copolymer block contains 14 wt% E and 86 wt% P (total ethylene content of the resin is 7 wt%). Blends of homopolymer PP (PP H314) with this diblock copolymer were prepared in ratios of 85:15, 80:20, 70:30 and 60:40 (main PP), and films that had not been annealed were subjected to CS25-HS100 stretching conditions (as described above). None of these PP / EP blends formed pores after the stretching process. The EP block in this experimental grade resin contains only 14 wt% ethylene, producing a PP-rich EP block. As a result, EP blocks and iPP blocks exhibit good compatibility with homopolymer PP resin, and therefore, it is considered that EP blocks cannot initiate sufficient phase separation within the film.

[0200] INTUNE® D5545.00 (melt flow rate = 9.5 g / 10 min at 230°C, 2.16 kg) is another isotactic PP diblock block copolymer having a 50:50 ratio PP:EP copolymer, but the EP copolymer block is ethylene-rich, containing 92% E and 8% P by weight (total ethylene content of the resin is 46% by weight). By stretching a film that has not been annealed (CS25-HS100 stretching conditions of Example 6 above), only minimal pore formation is achieved: 13.6% porosity and an average pore diameter of 14.1 nm. Films of diblock copolymers are not suitable for the desired purpose as house wrap material. Blends of homopolymer PP (PP H314) and this diblock copolymer were prepared in ratios of 85:15, 80:20, 70:30, and 60:40 (main PP), and films that had not been annealed were subjected to the CS25-HS100 stretching conditions of Example 6 (described above). None of these PP / EP copolymer blends formed pores after the stretching process.

[0201] NORDELL® 3722P is an EPDM (ethylene-propylene diene monomer) copolymer having a composition of 28.5% by weight propylene, 71% by weight ethylene, and 0.5% by weight ENB (ethylidene norbornene). Blend ratios of 90:10, 80:20, and 70:30 (polypropylene-rich), and the blend of PP-H314:NORDELL® 3722P with the main homopolymer PP were investigated. Films that had not been annealed were subjected to CS25-HS100 stretching conditions (described above). None of these PP / EP copolymer blends formed pores after the stretching process.

[0202] In addition, ethylene acrylic acid (PRIMACOR® 1410 resin: 90.3% E, 9.7% acrylic acid) was evaluated (melt flow rate = 1.5 g / 10 min at 230°C, 2.16 kg). The blend consisted of 85% PP H314 resin and 15% PRIMACOR® 1410 resin. Under the same stretching conditions, this blend did not show pore formation. PRIMACOR® 1410 resin was incompatible with PP H314 resin and therefore formed a completely separated interface between the two phases.

[0203] Example 7 This example examines the aging performance of an unheat-cured microporous film. Many conventional microporous films have been observed to suffer property degradation after thermal aging (see, for example, Table 1 of U.S. Patent No. 3,801,404, showing progressive nitrogen flux loss in polypropylene microporous films at 65°C for 1 to 281 hours; and Table 2 of U.S. Patent No. 3,843,761, showing airflow loss rates of polypropylene microporous films after 1 hour at 90°C). Thermal curing (high-temperature annealing of polyolefin films after stretching) has been frequently used in the prior art (e.g., U.S. Patent No. 3,679,538) to prevent loss of water vapor permeability during aging (e.g., at 65°C). Unheat-cured PP C7054-07NA MDO microporous films (uniaxially oriented, mechanically oriented) were aged at 65°C for various times ranging from 1 to 168 hours (Table 10).

[0204] [Table 10]

[0205] As shown in Table 10, the water vapor permeability data did not change much over a long period of time. In the present invention, as indicated by the slight change in wide-angle X-ray (WAXS) data of the uniaxially oriented (MDO) PP C7054-07NA microporous film before and after stretching (Figures 5A and 5B), the stretching force was consumed to move to the microphase rubber-like (ethylene-propylene copolymer) region and create a microporous structure. In contrast, with respect to a comparative film, e.g., PP TI4020N resin film, the crystalline structure rotated and rearranged into a filamentous structure, and a significant orientation was observed in the WAXS data after stretching, due to the emission of strong diffraction intensities in the (110), (040), (130), and (131) planes (Figure 5D after stretching compared to Figure 5C before stretching). This aging performance of the permeable film disclosed herein distinguishes it from other homopolymer polyolefin microporous films reported in the prior art, which always require thermosetting.

[0206] Apart from the perspective of breathability, U.S. Patent No. 3,843,761 investigated the same phenomenon of performance degradation after the thermosetting step. In U.S. Patent No. 3,843,761, a film obtained from the thermosetting step was compared to a control film that did not undergo the thermosetting step. This reference document concluded that the flow velocity loss due to the thermosetting step ranges from 44 to 88% for conventional cold-drawn / single-stage thermo-drawn processes, and that the flow velocity loss due to the thermosetting step ranges from 24 to 37% for those novel cold-drawn / multiple-stage thermo-drawn processes.

[0207] For comparison with the thermosetting results disclosed in U.S. Patent No. 3,843,761, PP C7054-07NA microporous films having the same elongation as disclosed in U.S. Patent No. 3,843,761 (see Table 11) were prepared. In particular, the first sample, PP C7054-07NA-CS20-HS95, was stretched by 20% cold stretching at 100 mm / sec followed by 95% hot stretching at 5 mm / sec and 100°C. The second sample, PP C7054-07NA-CS40-HS75, was stretched by 40% cold stretching at 100 mm / sec followed by 75% hot stretching at 5 mm / sec and 100°C.

[0208] [Table 11]

[0209] Next, these microporous films were subjected to the same thermosetting step (1 hour at 90°C) as in the reference patent. The relative air permeability is calculated by the following formula.

number

[0210] Table 12 shows the relative air permeability (as defined above) of microporous films comparing the Gurley air permeability before and after thermosetting at 90°C for 1 hour (for each film type, there are four samples at four locations for each sample; each relative air permeability entry in the table is the average of four ratios determined from four measurements at four locations before and after thermosetting).

[0211] [Table 12]

[0212] Table 12 shows that the average relative air permeability is approximately 1.5 for both stretched films, indicating that, with respect to the films of the present invention, the (normal) air permeability increases by approximately 50% after thermosetting, unlike the 24-88% flow loss disclosed in U.S. Patent No. 3,843,761. The porous structure of the polyolefin-based microporous films disclosed in the present invention can withstand the thermosetting process.

[0213] The breathable film of the present invention can be prepared without an annealing step before stretching to produce a microporous film, and furthermore, no thermosetting step is required after pore formation. Moreover, if a thermosetting step is desirable for any reason, the film of the present invention does not suffer any loss of permeability compared to a film without a thermosetting step.

[0214] Example 8 This example demonstrates the performance of a biaxially oriented microporous film made of PP copolymer.

[0215] PP C7054-07NA copolymer films were subjected to simultaneous biaxial stretching, specifically 25% cold stretching at a speed of 100 mm / sec at room temperature and 50% hot stretching at 5 mm / sec at 100°C. As shown in Table 13, the biaxially oriented microporous film of PP C7054-07NA has a porosity of 34.7% and an average pore diameter of 44 nm. Correspondingly, the water vapor permeability for this microporous film was approximately 42 perm (Table 14), and after aging at 65°C for 168 hours, the water vapor permeability increased to 60 perm (Table 14).

[0216]

Table 13

[0217]

Table 14

[0218] This example shows that biaxial stretching can also be used to produce the microporous film.

[0219] Example 9 To conduct a proof-of-concept study of the roof film, a 762 μm (30 mil) thick PP C7054-07NA film was subjected to 25% cold stretching (CS) at 100 mm / sec at room temperature and then 100% (150% for the second film) hot stretching (HS) at 5 mm / sec at 100 °C. Pore distribution data in the range of several tens of nanometers to several microns are shown in Fig. 7. From Table 15, it can be seen that PP C7054-07NA-CS25-HS100 with a thickness of about 660 μm (25.5 mils) has 42.5% porosity and provides 58 perm of water vapor transmission, and PP C7054-07NA-CS25-HS150 with a thickness of about 533 μm (20.6 mils) has a higher porosity of 55% and provides 62 perm of water vapor transmission.

[0220] <00009​​​​​​​​​​​​​​Stretched microporous PP copolymer films were evaluated for medical packaging films and active packaging, where various combinations or degrees of air or water vapor permeability or microbial barrier may be required for each end use. Table 16 shows the film thickness, basis weight, porosity, and pore size (average pore diameter) for microporous films obtained under various stretching conditions.

[0223] [Table 16]

[0224] Further investigations were conducted regarding the permeability characteristics (Table 17), physical properties (Table 18), and gas filling / emptying rates (Table 19) of films from the same series when used as medical packaging.

[0225] Table 17 shows the important barrier properties (Gurley permeability, water vapor permeability, and F2638 barrier against microorganisms) obtained for the same microporous films as those shown in Table 16.

[0226] [Table 17]

[0227] Table 17 shows data for uniaxially oriented PP copolymer films, demonstrating that permeability properties can be modified and controlled by changing the stretching conditions. While target ranges for various properties can be estimated by comparison with existing commercial products for these applications (e.g., Tyvek® 1073B or medical-grade paper), these are not strict targets due to the existence of various end applications for films with different property balances (and one or more properties of commercial products may significantly exceed the minimum target range required for that property). By using optimized stretching conditions or biaxially oriented films, (F2638 P maxThe barrier against microorganisms (as indicated by the values) is already within a commercially viable target range, and targets for Guarley permeability (perhaps around 10–100 seconds for some applications) must also be available. Some applications may require specific hydrohead values ​​(resistance to water pressure). As shown in Table 16, porosity and uniform pore diameter were measured for films 4–9, with porosity being relatively stable (43%–53%) and pore diameters ranging from 70 nm to 108 nm. Although not shown in the table, films 1–9 had hydrohead values ​​higher than 500 cmwc (cm in water column), easily exceeding the hydrohead value of Tyvek® 1073B (hydrohead value of Tyvek® 1073B, approximately 150 cmwc).

[0228] In addition to permeability, breathable films for medical and active packaging also require appropriate physical properties related to film strength, such as tensile strength, tear strength, and elongation percentage. Table 18 summarizes such properties for the same series of breathable PP copolymer microporous films.

[0229] [Table 18]

[0230] The stretching process conditions can be modified to control the film thickness / basis weight and other physical properties (e.g., tensile strength, tear strength, and elongation). These physical properties are important for maintaining the integrity of the package during transport, sterilization, and storage, and for ensuring that the packaging structure does not tear when the package is peeled open.

[0231] Compared to current technologies, the tensile strength of these films appears to be sufficient for most medical and active packaging applications.

[0232] Medical packages are currently finding use as container packages that can be filled with a sterilizing agent gas (such as steam or ethylene oxide) to sterilize package contents (such as medical devices or instruments). The package is filled with the sterilizing agent, and then the contents remain with the sterilizing agent gas for the residence time for the sterilization process, and then the gas is evacuated and the package is sealed with the sterilized device inside. The package material provides a barrier against bacteria, microorganisms, and particulate matter so as to maintain the sterility of the medical device within the package after sterilization until such a device is ready for use.

[0233] Table 19 examines how the stretching process conditions can affect the fill / empty time of the PP copolymer film.

[0234]

Table 19

[0235] In Table 19 above, the improvement in Gurley air permeability between the comparative film (immediately after cold stretching) and the film of the present invention ranges from 45,200 to 860 seconds, which represents a 20% improvement in the time for filling (or emptying) a medical package with gas. Even when the relatively modest improvement in Gurley air permeability does not match that of Tyvek® 1073B, Table 19 includes breathable film (1) and breathable film (2), which are hypothetical films having Gurley air permeabilities of 300 seconds and 100 seconds, respectively, to show that it can translate into significant cost savings when such medical packages are used for the sterilization of medical equipment and devices, corresponding to a significant % improvement in the time for filling (or emptying) a medical package with gas.

[0236] The PP copolymer microporous films described herein are well suitable for medical packaging. Compared to current polyethylene technology, sterilization processes can be performed at higher temperatures due to the higher melting temperature of PP copolymer films compared to polyethylene films (for example, the typical melting temperature of high-density polyethylene is about 125-130°C according to DSC, while the typical melting temperature of the PP-EP copolymer of the present invention disclosed herein is about 168°C according to DSC). Furthermore, PP copolymer films are readily thermoformable (enabling easily customizable packaging for various medical devices and equipment) and heat-sealable (for easily sealing sterilized packs).

[0237] When the term "range" is used herein with respect to physical properties such as temperature ranges and pressure ranges, or chemical properties such as monomer or copolymer content, it is intended to include all combinations and partial combinations of ranges, as well as specific embodiments within them.

[0238] Any patents, patent applications, and publications cited or mentioned herein are incorporated herein by reference in their entirety.

[0239] Those skilled in the art will understand that many variations and modifications can be made to preferred embodiments of the present invention, and that such variations and modifications can be made without departing from the spirit of the invention. Accordingly, the appended claims are intended to cover all such equivalent variations that fall within the true spirit and scope of the invention.

[0240] Reference example Numerous PP copolymer films of varying thicknesses were extruded and cast onto chill rolls set to 80°C using a 2.5-inch uniscrew extruder and 24-inch wide cast die manufactured by Davis-Standard, LLC, producing films with smooth surfaces. The base resin was PP C7054-07NA (product code C7054-07NA), a polypropylene copolymer available from Braskem American, Inc. The extruder was maintained at a constant temperature profile of 460°F (238°C), and the chill roll temperature was heated by heating oil. The thicknesses of the resulting films are summarized in Table 20.

[0241] [Table 20]

[0242] Example 11 Next, using a multi-stage cold stretching process as shown in Figure 8, individual film samples from Table 20 were stretched in the machine direction (MDO - machine direction orientation). Each sample of PP copolymer film from Table 20 was mounted on the unwinding section 20 and guided by 11 stretching rollers (1-11), including a pre-stretching section 23, a stretching section 24, and an annealing section 25, and then rewound onto the winding section 21. Pressure was then applied to the film to close the nip rollers to prevent slippage during stretching. The roller speeds of rollers 3-7 were slowly increased, and the film was stretched to 50% or 100% at 25°C. During the stretching process, the film changed from translucent to white, indicating initial pore formation. Next, in the annealing section 25, the cold-stretched film was heated at 140°C on rollers 9-11 to fix the pore structure induced by the cold stretching step. The film was then cooled and rewound onto the winding machine. The characteristics of the final film measured are summarized in Table 21. Cold stretching is defined as (total roller speed ratio - 1) × 100%, and the total roll speed ratio is the result of multiplying all roller speed ratios (from roller 2 / roller 1 to roller 8 / roller 7) together.

[0243] [Table 21]

[0244] Next, the MDO cold-stretched film was further heat-stretched in the machine direction (MDO) using the same multi-stage process as shown in Figure 8, however, with respect to the heat stretching, the process included a pre-heat-stretching section 23, a heat-stretching section 24, and an annealing section 25. Each MDO cold-stretched film was mounted on the unwinding section, guided by 11 stretching rollers, and rewound onto the other winding section 21. In this process, the first eight rollers were set to a heat-stretching temperature of 135°C. Pressure was applied to the film to prevent slippage during stretching by closing the nip rollers, and then the roller speed of rollers 5-8 was slowly increased to stretch the film to 50% or 100% at 135°C. After the completion of the heat-stretching step, the film was annealed on rollers 9-11 at 140°C to reduce film shrinkage. The film was then cooled on the winding equipment section 22 and rewound into a roll. The degree of thermal stretching is defined as (total roller speed ratio - 1) × 100%, and the total roller speed ratio is the result of multiplying all roller speed ratios (from roller 5 / roller 4 to roller 8 / roller 7) together. Table 22 shows that upon completion of MDO thermal stretching, the porosity and average pore diameter of the PP film increased. This results in higher water vapor permeability and lower Gurley permeability.

[0245] [Table 22]

[0246] Example 12 To illustrate that thermal stretching may adversely affect pore formation and air and water vapor permeability, the above cold and thermal stretching processes were applied to a sample of Film 1 that was cold-stretched to 122% in the mechanical direction at 25°C, followed by thermal stretching to 103%–405% in the mechanical direction. As shown in Table 23, the porosity and permeability of the film deteriorated with stretching at higher temperatures. Consequently, biaxial stretching was proposed to further increase porosity and pore size, thereby achieving higher water vapor permeability and lower Gurley permeability.

[0247] [Table 23]

[0248] Example 13 Next, the MDO cold and hot-stretched films of Example 11 were further heat-stretched transversely using a process as shown in Figure 9, which included a multi-zone oven 50 having an unwinding section 41, a preheating section 43, a TDO (transverse orientation) stretching section 44, an annealing section 45, and a cooling section 46. The TDO line had a feed width range of 127 mm to 1,016 mm between clips and an exit width range of 203 mm to 2,184 mm between clips for stretching the film transversely. The TDO clips were able to hold a wide range of materials having a film thickness range of 25 μm to 2.54 mm. Following the heated sections (43, 44, and 45), there was a 1.5 m long cooling section 46 with circulating outside air. After the TDO oven was preheated to the target temperature (135°C), the MDO-stretched film was attached to the unwinding machine and guided through the feed section of the TDO line. The film was gradually gripped with clips and pulled through the preheating area at a constant width. The film was then stretched transversely until the TDO target elongation was reached. Upon completion of stretching, the film was passed through the annealing section 45 at 140°C, followed by quenching with circulating ambient air in the cooling section 46. The stretched film was then guided through a stack of rolls and rewound onto the winding machine section 42. To simplify the experiment, the line speed was fixed at 2 m / min. The TDO elongation was varied from 50% to 400%. Table 24 shows the stretching conditions and properties of biaxially oriented PP permeable films prepared by MDO cold stretching, MDO hot stretching, and TDO hot stretching. All samples had a hydrohead of greater than 300. These experiments demonstrated that biaxial stretching is highly effective in creating additional openings in the pores within the film. Table 24 shows that most biaxially oriented films have a porosity of nearly 70% and an average pore diameter greater than 200 nm. Correspondingly, most samples have a Gurley permeability of less than 100 sec / 100 cc, some samples are in the range of 20-30 sec / 100 cc, but many samples have water vapor permeability greater than 100 perm. At the same time, although not shown in the table, all films have a hydrohead greater than 300 cm, indicating good water resistance. Furthermore, the microbial barrier (%Pmax) measured by F2638 shows very good results (well within the target range).

[0249] [Table 24]

[0250] Example 14 Table 25 shows the stretching conditions and properties of biaxially oriented PP permeable films prepared by MDO cold stretching followed by TDO hot stretching. Very high porosity can be achieved even without MDO hot stretching. Furthermore, porosity and average pore diameter continued to increase with increasing TDO stretching. Correspondingly, these PP permeable films exhibit comparable water vapor permeability, Gurley permeability, and microbial barrier properties.

[0251] [Table 25]

[0252] Example 15 A key characteristic for waterproof and breathable roof membranes is that they must pass a hydrohead test, resisting water from a depth of 30 meters for at least 30 minutes. Stretched films for use as roof membranes were selected and tested. As can be seen from Table 26, all samples were manufactured by cold and hot stretching and passed the hydrohead test. These MDO samples had film thicknesses ranging from 0.19 mm to 0.53 mm and exhibited water vapor transmission rates (WVTR) ranging from 29.1 perm to 76.7 perm. Biaxially oriented samples manufactured by cold MDO stretching followed by hot TDO stretching did not pass the hydrohead test due to the increased number of interconnected pores resulting from the biaxial stretching process.

[0253] [Table 26]

[0254] Example 16 Polypropylene (PP) film samples were prepared by cold and hot MDO stretching and tested for use as roof underlayment. All samples shown in Table 27 passed water resistance (W1), aging durability (EN 1297 and EN 1296), low-temperature flexibility (≤-20°C), and lateral drop test (TU Berlin). However, Table 27 shows that samples 16a and 16b had low nail tear strength characteristics due to the low film thickness after stretching. Samples 16c and 16d show that acceptable nail tear strength can be achieved by increasing the film thickness. Samples 16e, 16f, and 16g demonstrate other possible solutions, such as laminating thinner films with grids or nonwoven films. 16e was laminated to a D&L grid, 16f was laminated with Thermanet®, and 16g was laminated to a spunbond PP nonwoven fabric. The characteristic data for these laminates are shown in Table 27. These laminated films demonstrated a significant improvement in nail tear strength.

[0255] [Table 27]

[0256] Example 17 Microbial barrier testing was collected in the selection of films from Examples 13 and 14 according to ASTM F2638, along with additional particulate barrier testing using the TSI-8130 automated filter testing machine. The obtained data are shown in Table 28. Biaxial stretching allows for an increase in porosity and average pore diameter, thus enabling 100 sec / 100 cm. 3 Lower Gurley permeability values ​​of less than 5 mph were derived. All biaxially oriented samples showed very good microbial barrier (<0.25% Pmax) within the target range. Furthermore, the burst pressure measured by the hydrohead test was higher than 5 mph for all biaxially oriented PP permeable films.

[0257] [Table 28]

Claims

1. 1. A microporous polymeric film comprising one or more polypropylene copolymers comprising one or more polypropylene homopolymer chain segments and one or more ethylene-containing copolymer chain segments, (i) polypropylene homopolymer chain segments in a total amount of 50 to 82 wt % based on the weight of the microporous polymer film or 43 to 79 mol % based on the molar content of polymerized units of propylene in the polypropylene homopolymer chain segments as a percentage of the total molar content of polymerized monomer units in the microporous polymer film; (ii) ethylene-containing copolymer chain segments in a total amount of 18 to 50 weight percent based on the weight of said microporous polymer film or 21 to 57 mole percent based on the molar content of polymerized monomer units in said ethylene-containing copolymer chain segments as a percentage of the total molar content of polymerized monomer units in said microporous polymer film; at least a portion of the ethylene-containing copolymer chain segment comprises polymerized units of ethylene in an amount of at least 45 wt %, based on the weight of the ethylene-containing copolymer chain segment, or at least 55 mol %, based on the molar content of polymerized units of ethylene in the ethylene-containing copolymer chain segment as a percentage of the total molar content of polymerized monomer units in the ethylene-containing copolymer chain segment; A microporous polymer film having a porosity of at least 25% and a median pore diameter, 4 V / A, by UOP method 578-11 of at least 25 nm, both characteristics measured by mercury intrusion porosimetry.

2. 2. The microporous polymer film of claim 1, wherein at least a portion of the ethylene-containing copolymer chain segment comprises polymerized units of ethylene in an amount of 45% to 80% by weight based on the weight of the ethylene-containing copolymer chain segment or 55 mol % to 86 mol % based on the molar content of polymerized units of ethylene in the ethylene-containing copolymer chain segment as a percentage of the total molar content of polymerized monomer units in the ethylene-containing copolymer chain segment.

3. 2. The microporous polymer film of claim 1, wherein the total ethylene content in polymerized form in the microporous polymer film is at least 10 wt. %, based on the weight of the microporous polymer film, or at least 14 mol. %, based on the molar content of polymerized units of ethylene in the microporous polymer film, as a percentage of the total molar content of polymerized monomer units in the microporous polymer film.

4. 2. The microporous polymer film of claim 1, wherein the total ethylene content in polymerized form in the microporous polymer film is 10 to 30 weight percent based on the weight of the microporous polymer film, or 14 to 39 mole percent based on the molar content of polymerized units of ethylene in the microporous polymer film as a percentage of the total molar content of polymerized monomer units in the microporous polymer film.

5. 2. The microporous polymeric film of claim 1, wherein the ethylene-containing copolymer chain segment is an ethylene-propylene copolymer chain segment.

6. 6. The microporous polymer film of claim 5, wherein the ethylene-propylene copolymer chain segments are random ethylene-propylene copolymer chain segments.

7. 6. The microporous polymer film of claim 5, wherein the ethylene-propylene copolymer chain segment is an ethylene-propylene diblock copolymer chain segment comprising a polypropylene block and a polyethylene block, or a diblock copolymer chain segment comprising a polypropylene block and an ethylene-propylene copolymer block.

8. The microporous polymer film of any one of claims 5 to 7, wherein the one or more ethylene-propylene copolymer chain segments are present in a total amount of 18 to 50 wt % based on the weight of the microporous polymer film or 21 to 57 mol % based on the molar content of polymerized monomer units in the ethylene-propylene copolymer chain segments as a percentage of the total molar content of polymerized monomer units in the microporous polymer film.

9. 8. The microporous polymer film of any one of claims 5 to 7, wherein at least a portion of the ethylene-propylene copolymer chain segments comprise polymerized units of ethylene in an amount of 45% to 80% by weight based on the weight of the ethylene-propylene copolymer chain segment or 55 mol% to 86 mol% based on the molar content of polymerized units of ethylene in the ethylene-propylene copolymer chain segment as a percentage of the total molar content of polymerized monomer units in the ethylene-propylene copolymer chain segment.

10. The microporous polymer film of any one of claims 5 to 8, wherein the total ethylene content in polymerized form in the microporous polymer film is at least 10 wt% based on the weight of the microporous polymer film, or at least 14 mol% based on the molar content of polymerized units of ethylene in the microporous polymer film as a percentage of the total molar content of polymerized monomer units in the microporous polymer film.

11. The microporous polymer film of any one of claims 5 to 8, wherein the total ethylene content in polymerized form in the microporous polymer film is 10 to 30 wt% based on the weight of the microporous polymer film, or 14 to 39 mol% based on the molar content of polymerized units of ethylene in the microporous polymer film as a percentage of the total molar content of polymerized monomer units in the microporous polymer film.

12. 10. The microporous polymeric film of claim 1 having a permeation according to ASTM E96 / E96M-16 in the range of 10 to 150 perms.

13. 10. The microporous polymeric film of claim 1 further comprising a polypropylene homopolymer.

14. 10. The microporous polymeric film of claim 1 further comprising an ethylene-containing copolymer.

15. 1. A method of forming a microporous polymeric film, the method steps comprising: (a) one or more polypropylene copolymers, (i) one or more polypropylene homopolymer chain segments in a total amount of from 50 to 82 wt % based on the weight of the polypropylene copolymer or from 43 to 79 mol % based on the molar content of polymerized units of propylene in said polypropylene homopolymer chain segments as a percentage of the total molar content of polymerized monomer units in said polypropylene copolymer; (ii) one or more ethylene-containing copolymer chain segments in a total amount of from 18 to 50% by weight based on the weight of the polypropylene copolymer or from 21 to 57 mol % based on the molar content of polymerized monomer units in the ethylene-containing copolymer chain segments as a percentage of the total molar content of polymerized monomer units in said polypropylene copolymer; providing one or more polypropylene copolymers comprising: at least a portion of said ethylene-containing copolymer chain segments comprising polymerized units of ethylene in an amount of at least 45 wt %, based on the weight of said ethylene-containing copolymer chain segment, or at least 55 mol %, based on the molar content of polymerized units of ethylene in said ethylene-containing copolymer chain segment as a percentage of the total molar content of polymerized monomer units of said ethylene-containing copolymer chain segment; (b) forming a non-porous film from the polypropylene copolymer or a blend of polymers including the polypropylene copolymer; (c) the non-porous film, (i) at least one cold drawing step at a temperature in the range of -20°C to 50°C; and (ii) at least one hot stretching step at a temperature in the range of 50° C. to 150° C. and subjecting the resulting film to successive cold and hot stretching steps, thereby producing a microporous polymer film. A method comprising:

16. 16. The method of claim 15, wherein at least a portion of the ethylene-containing copolymer chain segment comprises polymerized units of ethylene in an amount of from 45% to 80% by weight based on the weight of the ethylene-containing copolymer chain segment or from 55 mol % to 86 mol % based on the molar content of polymerized units of ethylene in the ethylene-containing copolymer chain segment as a percentage of the total molar content of polymerized monomer units in the ethylene-containing copolymer chain segment.

17. 16. The method of claim 15, wherein the microporous polymer film has a total ethylene content in polymerized form of at least 10 weight percent based on the weight of the microporous polymer film, or at least 14 mole percent based on the molar content of polymerized units of ethylene in the microporous polymer film as a percentage of the total molar content of polymerized monomer units in the microporous polymer film.

18. 16. The method of claim 15, wherein the microporous polymer film has a total ethylene content in polymerized form of 10 to 30 weight percent based on the weight of the microporous polymer film, or 14 to 39 mole percent based on the molar content of polymerized units of ethylene in the microporous polymer film as a percentage of the total molar content of polymerized monomer units in the microporous polymer film.

19. The method of claim 15, wherein the ethylene-containing copolymer chain segment is an ethylene-propylene copolymer chain segment.

20. 20. The method of claim 19, wherein the ethylene-propylene copolymer chain segments are random ethylene-propylene copolymer chain segments.

21. 20. The method of claim 19, wherein the ethylene-propylene copolymer chain segment is an ethylene-propylene diblock copolymer chain segment comprising a polypropylene block and a polyethylene block, or a diblock copolymer chain segment comprising a polypropylene block and an ethylene-propylene copolymer block.

22. 22. The method of any one of claims 19 to 21, wherein the ethylene-propylene copolymer chain segments are present in a total amount of 18 to 50 weight % based on the weight of the polypropylene copolymer or 21 to 57 mole % based on the molar content of polymerized monomer units in the ethylene-propylene copolymer chain segments as a percentage of the total molar content of polymerized monomer units in the propylene copolymer.

23. 23. The method of any one of claims 19 to 22, wherein at least a portion of the ethylene-propylene copolymer chain segments comprise polymerized units of ethylene in an amount of from 45% to 80% by weight, based on the weight of the ethylene-propylene copolymer chain segment, or from 55 mol % to 86 mol %, based on the molar content of polymerized units of ethylene in the ethylene-propylene copolymer chain segment, as a percentage of the total molar content of polymerized monomer units in the ethylene-propylene copolymer chain segment.

24. 23. The method of any one of claims 19 to 22, wherein the total ethylene content in polymerized form in the microporous polymer film is at least 10 wt%, based on the weight of the microporous polymer film, or at least 14 mol%, based on the molar content of polymerized units of ethylene in the microporous polymer film, as a percentage of the total molar content of polymerized monomer units in the microporous polymer film.

25. 23. The method of any one of claims 19 to 22, wherein the total ethylene content in polymerized form in the microporous polymer film is 10 to 30 wt%, based on the weight of the microporous polymer film, or 14 to 39 mol%, based on the molar content of polymerized units of ethylene in the microporous polymer film, as a percentage of the total molar content of polymerized monomer units in the microporous polymer film.

26. The polypropylene copolymer has a melt flow rate, measured according to ASTM D-1238, Condition L at 230° C. and 2.16 kg, of 0.1 to 100 g / 10 min, and a melt flow rate of 0.9 g / cm 3 The method of claim 15, wherein the granular material has a density greater than 100%.

27. 16. The method of claim 15, wherein the polypropylene copolymer is blended with a polypropylene homopolymer to form a polymer blend prior to forming the non-perforated film.

28. 16. The method of claim 15, wherein the polypropylene copolymer is blended with an ethylene-containing copolymer to form a polymer blend prior to forming the non-perforated film.

29. 16. The method of claim 15, wherein forming the non-porous film is accomplished by extruding the polypropylene copolymer or polymer blend thereof in a melt state.

30. 16. The method of claim 15, wherein the non-porous polymeric film has a morphology characterized by a majority polymer phase of polypropylene, a plurality of minor polymer domains of an ethylene-containing copolymer within the majority polymer phase, and inclusions of a predominant polypropylene phase within the minor polymer domains.

31. The method of claim 15 , performed without any annealing step after formation of the non-porous film.

32. 16. The method of claim 15, wherein the at least one cold stretching step stretches the film by at least 10% in at least one direction and the at least one hot stretching step stretches the film by at least 20% in at least one direction.

33. 16. The method of claim 15, carried out without any annealing or heat setting step after forming the microporous polymeric film and before step (c).

34. 16. The method of claim 15 which is a continuous process for producing a microporous polymeric film.

35. 16. The method of claim 15, wherein the microporous polymer film has a porosity of at least 25% and a median pore diameter of at least 25 nm (4V / A, by UOP method 578-11), both characteristics measured by mercury intrusion porosimetry.

36. The method of claim 15, wherein the microporous polymeric film has a permeability according to ASTM E96 / E96M-16 ranging from 10 to 150 perms.

37. A microporous polymeric film formed by the method of any one of claims 15 to 36.

38. 37. A microporous polymer film formed by the method of any one of claims 15 to 36, wherein the non-porous polymer film has a morphology characterized by a majority polymer phase of polypropylene, a plurality of minor polymer domains of an ethylene-containing copolymer within the majority polymer phase, and inclusion phases of a predominant polypropylene phase within the minor polymer domains.

39. 10. The microporous polymeric film of claim 1 which is or is a component of a roof membrane.

40. 40. The microporous polymeric film of claim 39 having a thickness of at least 100 μm.

41. 10. The microporous polymeric film of claim 1, which is at least a portion of a medical packaging or active packaging article or a medical back table cover.

42. A medical packaging or active packaging article or a medical back table cover comprising the microporous polymeric film of any one of claims 1 to 14.

43. A medical packaging or active packaging article or medical back table cover comprising a microporous polymeric film, the microporous polymeric film comprising one or more polypropylene copolymers comprising one or more polypropylene homopolymer chain segments and one or more ethylene-containing copolymer chain segments, the microporous polymeric film comprising: (i) polypropylene homopolymer chain segments in a total amount of 50 to 82 wt % based on the weight of the microporous polymer film or 43 to 79 mol % based on the molar content of polymerized units of propylene in the polypropylene homopolymer chain segments as a percentage of the total molar content of polymerized monomer units in the microporous polymer film; (ii) ethylene-containing copolymer chain segments in a total amount of 18 to 50 weight percent based on the weight of said microporous polymer film or 21 to 57 mole percent based on the molar content of polymerized monomer units in said ethylene-containing copolymer chain segments as a percentage of the total molar content of polymerized monomer units in said microporous polymer film; wherein at least a portion of said ethylene-containing copolymer chain segments comprise polymerized units of ethylene in an amount of at least 45% by weight, based on the weight of said ethylene-containing copolymer chain segment, or at least 55 mol %, based on the molar content of polymerized units of ethylene in said ethylene-containing copolymer chain segment as a percentage of the total molar content of polymerized monomer units in said ethylene-containing copolymer chain segment.

44. 44. The medical packaging or active packaging article or medical back table cover of claim 43, wherein the microporous polymeric film has a barrier to microorganisms equivalent to the maximum penetration, calculated %Pmax, defined by ASTM F2638-18, of <10%.

45. The microporous polymer film has a viscosity of 1 to 35,000 seconds / 100 cm 3 44. The medical packaging or active packaging article or medical back table cover of claim 43, having a Gurley Gauge Air Permeability of at least 100% and controlling the inflow or outflow of air or one or more gases into or out of the package.

46. 46. ​​The medical packaging or active packaging article or medical back table cover of claim 45, wherein said microporous polymeric film is thermoformable and heat sealable.