Gas barrier multilayer film

A multilayer film with inorganic and ionic polymer layers enhances moisture barrier properties, addressing charge leakage issues in electronic devices by reducing moisture permeability, thereby ensuring device integrity.

JP2023030650A5Active Publication Date: 2024-10-18TOYO SEIKAN GRP HLDG LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021135891
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-08-23
Publication Date
2024-10-18
Estimated Expiration
2041-08-23

AI Technical Summary

Technical Problem

Existing gas barrier films for electronic devices, such as organic electroluminescent (EL) elements and solar cells, fail to provide sufficient moisture barrier properties, leading to charge leakage due to residual moisture in plastic substrates.

Method used

A multilayer film structure comprising a base layer with an inorganic barrier layer and a moisture trap layer, where the moisture trap layer is formed using an ionic polymer matrix with dispersed moisture absorbents, and optionally includes additional inorganic barrier layers and adhesive layers, enhancing moisture barrier properties.

Benefits of technology

The multilayer film achieves excellent moisture barrier properties, reducing moisture permeability to 1×10^-4 g/m^2/day or less at 40°C and 90% RH, effectively preventing charge leakage in electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a multilayer film which exhibits excellent moisture barrier properties.SOLUTION: There is provided a gas barrier multilayer film which comprises a base material layer (A1), a moisture trap layer (B1) and an outer layer (Q) in this order, wherein the base material layer (A1) has a layer selected from the group consisting of an inorganic barrier layer (a1) and an inorganic barrier layer (a2) on at least one surface of a plastic layer (x) and the base material layer (A1) has a moisture permeability (40°C, RH 90%) of less than 1×10-3 g / m2 / day.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gas barrier multilayer film used as a sealing material or substrate for electronic devices such as organic electroluminescence (EL) elements and solar cells. [Background technology]

[0002] Various electronic devices that have been developed and put to practical use in recent years, such as organic electroluminescence (organic EL), solar cells, touch panels, and electronic paper, require high moisture barrier properties to prevent charge leakage due to moisture.

[0003] Incidentally, as a means for improving the properties of various plastic substrates, particularly the gas barrier properties, it is known to form an inorganic thin film (inorganic barrier layer) made of silicon oxide or the like on the surface of the plastic substrate by vapor deposition (Patent Document 1), and films with such inorganic thin films are widely used as barrier films. Such barrier films are insufficient to satisfy the moisture barrier properties required for the above-mentioned electronic devices, and the residual moisture in the resin used in the plastic substrate significantly deteriorates the device.

[0004] To meet such demands, a moisture barrier laminate is also known that has a structure in which a moisture trapping layer having a hygroscopic ionic polymer as a matrix is ​​laminated (Patent Document 2).

[0005] The moisture trapping layer as described above is formed by applying a coating composition for forming a trapping layer, which contains an ionic polymer, onto an inorganic barrier layer formed on the surface of a plastic film by vapor deposition or the like, and then curing the composition. The formation of such a layer is said to provide excellent moisture barrier properties.

[0006] However, since the moisture barrier property of the inorganic barrier layer is insufficient, the moisture barrier property is not yet sufficient for use as a sealing material for electronic devices, and the problem remains unsolved. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2000-255579 A [Patent Document 2] JP 2015-96320 A Summary of the Invention [Problem to be solved by the invention]

[0008] It is therefore an object of the present invention to provide a multilayer film that exhibits sufficient moisture barrier properties as an encapsulant for electronic devices. [Means for solving the problem]

[0009] The present invention includes the following inventions. 1. A substrate layer (A1), a moisture-trapping layer (B1), and an outer layer (Q) in this order; The base layer (A1) has a layer selected from the group consisting of an inorganic barrier layer (a1) and an inorganic barrier layer (a2) on at least one surface of the plastic layer (x), The moisture permeability of the base layer (A1) (40°C, RH90%) is 1×10 -3 g / m 2 / day or less, Gas barrier multi-layer film. 2. The base layer (A1) is (α) having an inorganic barrier layer (a1) on the side opposite to the moisture-trapping layer (B1), (β) having an inorganic barrier layer (a2) on the surface on which the moisture-trapping layer (B1) is formed, or (γ) comprising the above (α) and (β); 2. The gas barrier multilayer film according to item 1 above. 3. The gas barrier multilayer film according to item 1 or 2 above, wherein the outer layer (Q) is a layer selected from the group consisting of a plastic layer (C), a base layer (A1) and a base layer (A2), and the base layer (A2) is a layer having an inorganic barrier layer (a4) on one side of the plastic layer (y). 4. The gas barrier multilayer film according to item 1 or 2 above, further comprising a moisture-trapping layer (B2) on the surface of the base layer (A1) opposite to the moisture-trapping layer (B1). 5. A gas barrier multilayer film according to the preceding item 4, further comprising an adhesive layer (D) and a base layer (A3) in this order on the side of the moisture-trapping layer (B2) opposite the base layer (A1), the base layer (A3) being a layer having an inorganic barrier layer (a5) on one side of the plastic layer (z). 6. The gas barrier multilayer film according to any one of items 1 to 5 above, further comprising an inorganic barrier layer (a3) ​​on the surface of the plastic layer (C) on the moisture-trapping layer (B1) side. 7. The gas barrier multilayer film according to any one of the above items 1 to 6, further comprising an adhesive layer (D) on the surface of the moisture-trapping layer (B1) on the outer layer (Q) side. 8. The gas barrier multilayer film according to any one of items 1 to 7 above, wherein the inorganic barrier layers (a1) to (a5) are metal oxide films. 9. The gas barrier multilayer film according to any one of items 1 to 8 above, wherein the plastic layers (x) to (z) contain an olefin resin, a polyester resin, a polyimide resin, a polyamide resin or a cyclic olefin resin. 10. The gas barrier multilayer film according to any one of items 1 to 9, wherein the moisture trapping layer (B1) and the moisture trapping layer (B2) both contain a resin composition in which a moisture absorbent (ii) is dispersed in an ionic polymer (i). 11. The gas barrier multilayer film according to any one of items 1 to 10 above, wherein the plastic layer (C) contains an olefin resin, a polyester resin, a polyimide resin, a polyamide resin or a cyclic olefin resin. Effect of the Invention

[0010] The gas barrier multilayer film of the present invention has excellent moisture barrier properties. [Brief description of the drawings]

[0011] [Figure 1] 1 is a schematic cross-sectional side view showing the layer structure of a multilayer film 1 of Example 1. FIG. [Diagram 2] FIG. 2 is a schematic cross-sectional side view showing the layer structure of a multilayer film 2 of Example 2. [Diagram 3] FIG. 4 is a schematic cross-sectional side view showing the layer structure of a multilayer film 3 of Example 3. [Figure 4] 1 is a schematic cross-sectional side view showing the layer structure of a multilayer film 4 of Example 4. FIG. [Diagram 5] 1 is a schematic cross-sectional side view showing the layer structure of a multilayer film 5 of Example 5. FIG. [Figure 6] 1 is a schematic cross-sectional side view showing the layer structure of a multilayer film 6 of Comparative Example 1. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The multilayer film of the present invention comprises a substrate layer (A1), a moisture-trapping layer (B1), and an outer layer (Q) in this order, The base layer (A1) has a layer selected from the group consisting of an inorganic barrier layer (a1) and an inorganic barrier layer (a2) on at least one surface of the plastic layer (x), The moisture permeability of the base layer (A1) (40°C, RH90%) is 1×10 -3 g / m 2 / day or less, It is a gas barrier multi-layer film.

[0013] <Base material layer (A1)> The substrate layer (A1) has a layer selected from the group consisting of an inorganic barrier layer (a1) and an inorganic barrier layer (a2) on at least one surface of the plastic layer (x).

[0014] <Plastic layer (x)> The plastic layer (x) serves as a base for the inorganic barrier layer (a1) and the inorganic barrier layer (a2) described later, and is usually made of a thermoplastic or thermosetting resin, and is molded by injection or co-injection molding, extrusion or co-extrusion molding, film or sheet molding, compression molding, or the like according to its form. shape, It is molded by cast polymerization or the like.

[0015] The plastic layer (x) is preferably made of a thermoplastic resin from the viewpoints of moldability, cost, etc. Examples of such thermoplastic resins include low-density polyethylene, high-density polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, or α-olefins such as ethylene, propylene, 1-butene, and 4-methyl-1-pentene. Peer random or block copolymers of the above; cyclic olefin resins such as cyclic olefin copolymers and cyclic olefin polymers; ethylene-vinyl compound copolymers such as ethylene-vinyl acetate copolymers, ethylene-vinyl alcohol copolymers, and ethylene-vinyl chloride copolymers; styrene resins such as polystyrene, acrylonitrile-styrene copolymers, ABS, and α-methylstyrene-styrene copolymers; polyvinyl compounds such as polyvinyl chloride, polyvinylidene chloride, vinyl chloride-vinylidene chloride copolymers, polymethyl acrylate, and polymethyl methacrylate; polyamides such as nylon 6, nylon 6-6, nylon 6-10, nylon 11, and nylon 12; thermoplastic polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate (PEN); polycarbonate; polyphenylene oxide; and biodegradable resins such as polyimide resins, polyamide-imide resins, polyetherimide resins, fluororesins, allyl resins, polyurethane resins, cellulose resins, polysulfone resins, polyethersulfone resins, ketone resins, amino resins, and polylactic acid. Furthermore, blends of these resins and resins appropriately modified by copolymerization (eg, acid-modified olefin resins) may also be used. The plastic layer (x) preferably contains an olefin resin, a polyester resin, a polyimide resin, a polyamide resin or a cyclic olefin resin.

[0016] In addition, the plastic layer (x) is also preferably formed from a gas barrier resin having excellent oxygen barrier properties, such as an ethylene-vinyl alcohol copolymer, and may further have a multi-layer structure including a layer formed from such a gas barrier resin.

[0017] From the viewpoint that the plastic layer (x) is suitable as a base for the inorganic barrier layer (a) described below, it is more preferable to use a film of a polyester resin such as polyethylene terephthalate (PET), polybutylene terephthalate, or polyethylene naphthalene carboxylate, or a cyclic olefin resin such as a polyimide resin, a polyamide resin, or a cyclic olefin copolymer or a cyclic olefin polymer as the plastic layer (x).

[0018] Although the thickness of the plastic layer (x) is not particularly limited, if the thickness is too thick, the residual moisture content of the plastic layer (x) increases, and the flexibility of the gas barrier multilayer film is lost. Therefore, the thickness of the plastic layer (x) is preferably 200 μm or less, more preferably 125 μm or less, and even more preferably 45 μm or less.

[0019] <Inorganic Barrier Layer (a1), Inorganic Barrier Layer (a2)> The substrate layer (A1) has an inorganic barrier layer on at least one side of the plastic layer (x). The substrate layer (A1) may be any of the following modes α, β, and γ. The embodiment α is an embodiment in which the base layer (A1) has an inorganic barrier layer (a1) on the surface opposite to the moisture-trapping layer (B1). The embodiment β is an embodiment in which the base layer (A1) has an inorganic barrier layer (a2) on the surface on the moisture-trapping layer (B1) side. The embodiment γ is an embodiment that has the above (α) and (β), that is, in the base layer (A1), the inorganic barrier layer (a1) is on the side opposite the moisture trapping layer (B1), and the inorganic barrier layer (a2) is on the side facing the moisture trapping layer (B1).

[0020] The inorganic barrier layer (a1) and the inorganic barrier layer (a2) may be layers having the same characteristics and thickness, or may be layers having different characteristics and thicknesses.

[0021] In the present invention, the moisture permeability (40° C., RH90%) of the base layer (A1) is 1×10 -3 g / m 2 / day, preferably less than 8×10 -4 g / m 2 / day, preferably less than 5×10 -4 g / m 2 / day. When the base layer (A1) has an inorganic barrier layer (a1) or an inorganic barrier layer (a2) on one side of the plastic layer (x), the moisture permeability of the base layer (A1) (40° C., RH 90%) is preferably 1×10 -3 g / m 2 / day, more preferably less than 8×10 -4 g / m 2 / day, more preferably less than 5×10 -4 g / m 2 / day. When the base layer (A1) has an inorganic barrier layer (a1) on one side of the plastic layer (x) and an inorganic barrier layer (a2) on the other side, the moisture permeability (40° C., RH 90%) of the base layer (A1) is preferably 8×10 -4 g / m 2 / day, more preferably less than 5×10 -4 g / m 2 / day, more preferably less than 3×10 -4 g / m 2 / day.

[0022] The inorganic barrier layer (a1) and the inorganic barrier layer (a2) are layers formed on the plastic layer (x). The inorganic barrier layer (a) is preferably a film formed by vapor deposition or a film formed by wet coating. Vapor deposition includes inorganic or inorganic-organic hybrid vapor deposition films formed by physical vapor deposition such as sputtering, vacuum deposition, and ion plating, and chemical vapor deposition such as plasma CVD. Wet coating includes inorganic or inorganic-organic hybrid coating films formed by a sol-gel process. The inorganic barrier layer (a1) and the inorganic barrier layer (a2) are preferably films formed of various metals, metal oxides, or metal oxides containing organic substances, in that they can ensure high oxygen barrier properties. In particular, they are preferably formed by plasma CVD or a sol-gel process, in that they can be uniformly formed on uneven surfaces and exhibit excellent barrier properties not only against oxygen but also against moisture. The inorganic barrier layer (a1) and the inorganic barrier layer (a2) are preferably metal oxide films or metal oxides containing organic substances.

[0023] The deposition film by plasma CVD is obtained by disposing a plastic layer (x) in the form of a film that serves as the base for the inorganic barrier layer (a1) and the inorganic barrier layer (a2) in a plasma processing chamber maintained at a predetermined vacuum level, supplying a gas (reactive gas) of the metal to be used to form the film or a compound containing the metal and an oxidizing gas (usually oxygen or NOx gas) together with a carrier gas such as argon or helium, as appropriate, using a gas supply pipe into the plasma processing chamber that is shielded by a metal wall and has been reduced in pressure to a predetermined vacuum level, and generating a glow discharge in this state using a microwave electric field or a high-frequency electric field, generating plasma using the electrical energy generated, and depositing the decomposition reaction products of the above compounds on the surface of the plastic layer (x) to form a film.

[0024] As the above-mentioned reactive gas, it is generally preferable to use a gas of an organometallic compound, for example, an organoaluminum compound such as trialkylaluminum, an organotitanium compound, an organozirconium compound, an organosilicon compound, or the like, from the viewpoint of being able to form a film having a flexible region containing a carbon component at the interface with the underlying plastic layer (x) and having a region thereon with a high degree of oxidation and excellent barrier properties. In particular, an organosilicon compound is most preferable from the viewpoint of being able to relatively easily and efficiently form the inorganic barrier layer (a1) or inorganic barrier layer (a2) with high barrier properties against oxygen.

[0025] Examples of such organic silicon compounds include organic silane compounds such as hexamethyldisilane, vinyltrimethylsilane, methylsilane, dimethylsilane, trimethylsilane, diethylsilane, propylsilane, phenylsilane, methyltriethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, tetramethoxysilane, tetraethoxysilane, phenyltrimethoxysilane, methyltrimethoxysilane, and methyltriethoxysilane, and organic siloxane compounds such as octamethylcyclotetrasiloxane, 1,1,3,3-tetramethyldisiloxane, and hexamethyldisiloxane. In addition to these, aminosilane, silazane, and the like can also be used. The above-mentioned organic metal compounds can be used alone or in combination of two or more kinds.

[0026] The thicknesses of the inorganic barrier layer (a1) and the inorganic barrier layer (a2) are set so as to satisfy a predetermined moisture permeability depending on the thickness of the underlying plastic layer (x), and generally have a thickness of about 4 to 500 nm, particularly about 30 to 400 nm.

[0027] Furthermore, the inorganic barrier layer (a1) and the inorganic barrier layer (a2) can also be formed on the plastic layer (x) by coating or the like instead of a technique such as vapor deposition.

[0028] The inorganic barrier layer (a) formed by coating is typically formed by using an organic solvent solution containing polysilazane, a polycondensable silane compound (e.g., alkoxysilane), or a polycondensable alumina compound (e.g., alkoxyaluminum) as a film-forming component, and optionally mixed with inorganic particles such as silica or alumina, which is then applied to a specified surface, heated, and the organic solvent is evaporated to form a film.

[0029] The inorganic barrier layer (a) may have an anchor coat layer and a top coat layer. The anchor coat layer and the top coat layer can be formed by using known techniques. For example, acrylic resin, epoxy resin, acrylic urethane resin, polyester polyurethane resin, and polyether polyurethane resin can be used for the anchor coat layer. From the viewpoint of adhesion and heat resistance, polyester polyurethane resin and acrylic urethane resin are preferable. For example, polyvinyl alcohol, polyvinylpyrrolidone, methyl cellulose, carboxymethyl cellulose, starch, sodium alginate, or a mixture thereof can be used for the top coat layer. For the top coat layer, the above resin can be mixed with an inorganic oxide.

[0030] <Outer layer (Q)> The outer layer (Q) is a layer on the side opposite to the electronic device when the multilayer film of the present invention is attached to an electronic device. The outer layer (Q) is a layer selected from the group consisting of a plastic layer (C), a substrate layer (A1) and a substrate layer (A2). In the present invention, there is an embodiment in which the same layer as the substrate layer (A1) is used as the outer layer (Q). That is, there is an embodiment in which two layers of the same substrate layer (A1) are used. The substrate layer (A2) and the plastic layer (C) will be described later.

[0031] <Base material layer (A2)> The base layer (A2) has an inorganic barrier layer (a4) on one side of the plastic layer (y). In the present invention, as shown in (7) and (8) of embodiment γ described below, the moisture-trapping layer (B1) may further include an adhesive layer (D) and a base layer (A2) in this order on the side opposite the base layer (A1). The material and thickness of the plastic layer (y) can be the same as those described in the section on the plastic layer (x). The material and thickness of the plastic layer (y) may be the same as or different from those of the plastic layer (x). The characteristics, material, thickness, and manufacturing method of the inorganic barrier layer (a4) can be the same as those described for the inorganic barrier layer (a1) and the inorganic barrier layer (a2). The characteristics, material, thickness, and manufacturing method of the inorganic barrier layer (a4) may be the same as or different from those of the inorganic barrier layer (a1) or the inorganic barrier layer (a2). The moisture permeability (40°C, RH90%) of the inorganic barrier layer (a4) is not necessarily 1×10 -3 g / m 2 It does not have to be less than / day.

[0032] <Base material layer (A3)> The base layer (A3) has an inorganic barrier layer (a5) on one side of the plastic layer (z). In the present invention, as shown in (5) to (8) and (11) to (12) of the embodiment γ described later, the surface of the moisture-trapping layer (B2) opposite to the substrate layer (A1) further includes an adhesive layer (D) and a substrate layer (A3) in this order, and the substrate layer (A3) can have an inorganic barrier layer (a5) on one side of the plastic layer (z). (6) of the embodiment γ is an embodiment in which the substrate layer (A3) in (5) is inverted. (8) of the embodiment γ is an embodiment in which the substrate layer (A3) in (7) is inverted.

[0033] The material and thickness of the plastic layer (z) can be the same as those described in the section on the plastic layer (x). The material and thickness of the plastic layer (z) may be the same as or different from those of the plastic layer (x). The characteristics, material, thickness, and manufacturing method of the inorganic barrier layer (a5) can be those described in the sections on the inorganic barrier layer (a1) and the inorganic barrier layer (a2). The characteristics, material, thickness, and manufacturing method of the inorganic barrier layer (a5) may be the same as or different from those of the inorganic barrier layer (a1) or the inorganic barrier layer (a2). The moisture permeability (40° C., RH90%) of the inorganic barrier layer (a5) is not necessarily 1×10 -3 g / m2 It does not have to be less than / day.

[0034] <Inorganic Barrier Layer (a3)> The multilayer film of the present invention may have an embodiment containing an inorganic barrier layer (a3), an inorganic barrier layer (a4) and an inorganic barrier layer (a5) other than the inorganic barrier layer (a1) and the inorganic barrier layer (a2) constituting the base layer (A1). The inorganic barrier layer (a3) ​​is a layer formed on the plastic layer (C) as a base. The inorganic barrier layer (a3) ​​can be formed on the surface of the plastic layer (C) on the moisture-trapping layer (B1) side.

[0035] The inorganic barrier layer (a3) ​​may be made of the same material as the inorganic barrier layer (a1) or the inorganic barrier layer (a2) and may have the same thickness. The inorganic barrier layer (a3) ​​can be formed by the same method as the inorganic barrier layer (a1) or the inorganic barrier layer (a2). a3 ) may have an anchor coat layer and a top coat layer. The anchor coat layer and the top coat layer can be formed using known techniques. For the anchor coat layer, for example, acrylic resin, epoxy resin, acrylic urethane resin, polyester polyurethane resin, and polyether polyurethane resin can be used. From the viewpoint of adhesion and heat resistance, polyester polyurethane resin and acrylic urethane resin are preferable. For the top coat layer, for example, polyvinyl alcohol, polyvinylpyrrolidone, methyl cellulose, carboxymethyl cellulose, starch, sodium alginate, or a mixture thereof can be used. For the top coat layer, the above resin can be mixed with an inorganic oxide.

[0036] <Moisture trapping layer (B1)> In the present invention, the moisture-trapping layer (B1) serves to block moisture from flowing in the thickness direction of the gas barrier multi-layer film.

[0037] <Ionic polymer> The moisture trapping layer (B1) is preferably formed from an ionic polymer. The moisture trapping layer (B1) is preferably formed by using an ionic polymer as a matrix and dispersing a moisture absorbent having a lower humidity level than the ionic polymer in the matrix. Such a layer having an ionic polymer as a matrix has excellent moisture capturing properties, and a layer having a moisture absorbent having a lower humidity level dispersed therein can transfer the moisture absorbed by the ionic polymer to the moisture absorbent, thereby trapping the absorbed moisture within the moisture absorbent, and completely trapping the permeated moisture within the trapping layer. capture In addition, deformation such as swelling caused by moisture absorption in the trap layer can be effectively avoided.

[0038] Ionic polymers that are preferably used to form the moisture-trapping layer (B1) include cationic polymers and anionic polymers.

[0039] A cationic polymer is a polymer having, in the molecule, a cationic group that can become positively charged in water, such as a primary to tertiary amino group, a quaternary ammonium group, a pyridyl group, an imidazole group, a quaternary pyridinium group, etc. In such cationic polymers, the cationic group has a strong nucleophilic action and can attract water by hydrogen bonding. capture Therefore, a hygroscopic matrix can be formed. The amount of cationic groups in the cationic polymer may generally be such that the water absorption rate (JISK-7209-1984) of the polymer is 20% or more, particularly 30 to 45%, in an atmosphere at a humidity of 80% RH and a temperature of 30°C.

[0040] As the cationic polymer, at least one cationic monomer represented by amine monomers such as allylamine, ethyleneimine, vinylbenzyltrimethylamine, [4-(4-vinylphenyl)-methyl]-trimethylamine, vinylbenzyltriethylamine, etc.; nitrogen-containing heterocyclic monomers such as vinylpyridine, vinylimidazole, etc.; and salts thereof; is polymerized or copolymerized with other copolymerizable monomers, and if necessary, is partially neutralized by acid treatment to obtain the polymer. As such a cationic polymer, polyallylamine is preferable from the viewpoint of film-forming properties, etc.

[0041] On the other hand, an anionic polymer is a polymer having an anionic functional group that can become negatively charged in water, such as a carboxylic acid group, a sulfonic acid group, a phosphonic acid group, or an acidic base formed by partially neutralizing these groups in the molecule. In an anionic polymer having such a functional group, the functional group is capable of attracting water by hydrogen bonding. capture Therefore, a hygroscopic matrix can be formed. The amount of anionic functional groups in the anionic polymer varies depending on the type of functional group, but similar to the cationic polymer described above, it is sufficient that the water absorption rate of the polymer (JISK-7209-1984) is 20% or more, particularly 30 to 45%, at a humidity of 80% RH and an atmosphere of 30°C.

[0042] As the anionic polymer having the above-mentioned functional group, for example, at least one of anionic monomers represented by carboxylic acid monomers such as methacrylic acid, acrylic acid, maleic anhydride, etc.; sulfonic acid monomers such as α-halogenated vinyl sulfonic acid, styrene sulfonic acid, vinyl sulfonic acid, etc.; phosphonic acid monomers such as vinyl phosphoric acid, etc.; and salts of these monomers; is polymerized or copolymerized with other copolymerizable monomers as appropriate, and further, if necessary, is partially neutralized by alkali treatment to obtain the polymer. As the anionic polymer, poly(meth)acrylic acid and its partially neutralized product (for example, a part of which is a Na salt) are preferable.

[0043] <Moisture absorbent> The moisture absorbent can transfer the moisture absorbed by the ionic polymer to the moisture absorbent and trap the absorbed moisture in the moisture absorbent. In addition, deformation due to swelling of the ionic polymer can be prevented. The moisture absorbent preferably has a lower humidity level than the ionic polymer. Examples of such moisture absorbents include those that have a humidity level of 6% or less under environmental conditions of 80% RH and 30°C. That is, if the humidity level of the moisture absorbent is higher than that of the ionic polymer, the moisture absorbed in the matrix is ​​not sufficiently trapped, and moisture is easily released. However, when a moisture absorbent with a lower humidity level than the ionic polymer is blended in the ionic polymer, not only can moisture be effectively trapped even in a low humidity atmosphere, but the moisture absorbed in the ionic polymer can be captured by the moisture absorbent, so that moisture release can be suppressed and high moisture barrier properties can be exhibited.

[0044] Moreover, the above-mentioned moisture absorbents generally have a water absorption rate (JISK-7209-1984) of 50% or more in an atmosphere with a humidity of 80% RH and a temperature of 30° C., and are classified into inorganic and organic types. Examples of inorganic moisture absorbents include zeolite, alumina, activated carbon, clay minerals such as montmorillonite, silica gel, calcium oxide, and magnesium sulfate. Examples of organic moisture absorbents include crosslinked anionic polymers or partially neutralized products thereof. Examples of the anionic polymer include those obtained by polymerizing or copolymerizing at least one of anionic monomers represented by carboxylic acid monomers (e.g., (meth)acrylic acid, maleic anhydride, etc.), sulfonic acid monomers (e.g., halogenated vinyl sulfonic acid, styrene sulfonic acid, vinyl sulfonic acid, etc.), phosphonic acid monomers (e.g., vinyl phosphoric acid), and salts of these monomers with other monomers. In particular, organic moisture absorbents are effective in applications where transparency is required. For example, fine particles of crosslinked sodium poly(meth)acrylate are typical organic moisture absorbents.

[0045] Among the above moisture absorbents, those with small particle size are preferred from the viewpoint of increasing the specific surface area and exhibiting high moisture absorption properties (for example, an average primary particle size of 100 nm or less, particularly 80 nm or less), and organic polymer moisture absorbents with small particle size are particularly suitable. That is, the organic polymer moisture absorbent has extremely good dispersibility in the ionic polymer matrix, and can be uniformly dispersed. Furthermore, by adopting emulsion polymerization or suspension polymerization as the polymerization method for producing the organic polymer moisture absorbent, the particle shape can be made fine and uniformly spherical, and by blending a certain amount of this, it is possible to ensure extremely high transparency.

[0046] Furthermore, organic fine moisture absorbents not only exhibit high moisture absorption properties with an extremely low ultimate humidity, but also minimize volumetric changes due to swelling through crosslinking. Therefore, they are optimal for reducing the humidity of the environmental atmosphere to an absolute dry state or close to an absolute dry state while suppressing volumetric changes. As such organic moisture absorbent particles, for example, cross-linked sodium polyacrylate particles (average particle size: about 70 nm) are sold in the form of a colloidal dispersion (pH=10.4) by Nippon Exlan Kogyo Co., Ltd. under the product name Tuftic HU-820E.

[0047] In the present invention, the amount of the moisture absorbent as described above is set according to the type of ionic polymer, from the viewpoint of fully exhibiting its properties, significantly improving the moisture barrier property and effectively suppressing dimensional changes due to swelling, while at the same time ensuring a moisture barrier property for a long period of time that is higher than the barrier property exhibited by all of the inorganic barrier layers in the gas barrier laminate. For example, when the moisture-trapping layer (B1) is formed by dispersing the above-mentioned moisture absorbent in a cationic polymer, it is generally present in an amount of 50 parts by weight or more, particularly 100 to 900 parts by weight, and more preferably 200 to 600 parts by weight, per 100 parts by weight of the cationic polymer. When the moisture absorbent is dispersed in an anionic polymer, it is generally present in an amount of 50 parts by weight or more, particularly 100 to 1300 parts by weight, and more preferably 150 to 1200 parts by weight, per 100 parts by weight of the anionic polymer.

[0048] <Crosslinking agent> In addition, in the moisture-trapping layer (B1) formed by using the above-mentioned ionic polymer, it is preferable that a crosslinked structure is introduced into the ionic polymer. That is, if a crosslinked structure is introduced into the ionic polymer, when the ionic polymer absorbs water, the molecules of the ionic polymer are bound to each other by the crosslinks, suppressing the volume change due to swelling (moisture absorption), and improving the mechanical strength and dimensional stability. Such a crosslinked structure can be introduced by incorporating a crosslinking agent into the coating composition for forming the moisture-trapping layer (B1). In particular, in the case of an anionic polymer, unlike a cationic polymer, the water-trapping structure is formed by hydrogen bonding. capture Therefore, by introducing a network structure (crosslinked structure) with spaces suitable for moisture absorption into the matrix, the moisture absorption can be greatly increased.

[0049] The crosslinking agent for introducing such a crosslinked structure differs slightly between when a crosslinked structure is introduced into a cationic polymer and when a crosslinked structure is introduced into an anionic polymer.

[0050] As the crosslinking agent for the cationic polymer, a compound having a crosslinkable functional group (e.g., an epoxy group) capable of reacting with a cationic group and a functional group (e.g., an alkoxysilyl group) capable of forming a siloxane structure in the crosslinked structure through hydrolysis and dehydration condensation can be used. Specifically, a silane compound represented by the following formula (1) is preferably used. X-SiR1 n (OR 2 ) 3-n (1) In the formula, X is an organic group having an epoxy group at the end, and R 1 and R 2 are each independently a methyl group, an ethyl group, or an isopropyl group, and n is 0, 1, or 2.

[0051] Such a silane compound has an epoxy group and an alkoxysilyl group as functional groups, and the epoxy group undergoes an addition reaction with the functional group (e.g., NH2) of the cationic polymer. Meanwhile, the alkoxysilyl group generates a silanol group (SiOH group) by hydrolysis, and grows by forming a siloxane structure through a condensation reaction, ultimately forming a crosslinked structure between the cationic polymer chains. As a result, a crosslinked structure having a siloxane structure is introduced into the matrix of the cationic polymer. Moreover, the cationic polymer is alkaline. As a result, it is difficult to form a moisture trapping layer ( B1 When the silanol group is formed, the addition reaction between the cationic group and the epoxy group and the dehydration condensation between the silanol groups are rapidly promoted, making it possible to easily introduce a crosslinked structure.

[0052] In the present invention, the organic group X having an epoxy group in the above formula (1) is typically a γ-glycidoxyalkyl group, and for example, γ-glycidoxypropyltrimethoxysilane or γ-glycidoxypropylmethyldimethoxysilane is preferably used as a crosslinking agent. In addition, the epoxy group in the above formula (1) is also preferably an alicyclic epoxy group such as an epoxycyclohexyl group. For example, when a compound having an alicyclic epoxy group such as β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane is used as a crosslinking agent, an alicyclic structure is introduced into the crosslinked structure of the matrix together with the siloxane structure. The introduction of such an alicyclic structure can more effectively exert the function of the matrix, which is to form a network structure of spaces suitable for moisture absorption.

[0053] Furthermore, in order to introduce an alicyclic structure into the above-mentioned crosslinked structure, a compound having a plurality of epoxy groups and an alicyclic group, for example, a diglycidyl ester represented by the following formula (2), can be used as a crosslinking agent. GO(C=O)-A-(C=O)OG (2) In the formula, G is a glycidyl group, and A is a divalent hydrocarbon group having an aliphatic ring, such as a cycloalkylene group.

[0054] A representative example of such a diglycidyl ester is represented by the following formula (2-1). [ka]

[0055] That is, the diglycidyl ester of formula (2) does not have an alkoxysilyl group, but introduces an alicyclic structure into the crosslinked structure, and is therefore effective in forming a network structure of spaces suitable for moisture absorption in the matrix.

[0056] The above-mentioned crosslinking agent is desirably used in an amount of 5 to 60 parts by weight, particularly 15 to 50 parts by weight, per 100 parts by weight of the cationic polymer, and it is desirable that at least 70% by weight, preferably 80% by weight or more of such a crosslinking agent is the silane compound of the above-mentioned formula (1).

[0057] In addition, as a crosslinking agent for introducing a crosslinked structure into an anionic polymer, a compound having two or more crosslinkable functional groups (e.g., epoxy groups) capable of reacting with an ionic group possessed by an anionic polymer can be used, as described in JP 2015-96320 A, etc. For example, a diglycidyl ester represented by formula (2), which is also mentioned in the coating composition for cationic matrices, is preferably used. GO(C=O)-A-(C=O)OG (2) In the formula, G is a glycidyl group, and A is a divalent hydrocarbon group having an aliphatic ring, such as a cycloalkylene group.。

[0058] That is, in the diglycidyl ester of the above formula (2), the epoxy group reacts with the anionic group, and a crosslinked structure containing an alicyclic structure is formed in the matrix by the divalent group A. The formation of such a crosslinked structure containing an alicyclic structure leads to the suppression of swelling. In particular, among the above diglycidyl esters, the preferred ones have been mentioned above, and from the viewpoint of being able to form a network structure of spaces suitable for moisture absorption, the diglycidyl ester represented by the above formula (2-1) is the most preferred. The moisture-trapping layer (B1) may have an anchor coat layer and a top coat layer. The anchor coat layer and the top coat layer can be formed by known techniques. The layer forming the anchor coat layer is, for example, an organic layer made of at least one selected from urethane resin, polyester resin, polyether resin, epoxy resin, acrylic resin, phenol resin, and melamine resin, and is preferably formed from urethane resin, epoxy resin, and acrylic resin. A crosslinked structure may be introduced into these resins. Furthermore, it may be an organic layer to which an inorganic filler or a silane compound that improves the barrier properties is added. The layer forming the top coat layer is, for example, an organic layer made of at least one selected from urethane resin, polyester resin, polyether resin, epoxy resin, acrylic resin, phenol resin, and melamine resin, and is preferably formed from urethane resin, epoxy resin, and acrylic resin. A crosslinked structure may be introduced into these resins. Furthermore, it may be an organic layer to which a metal oxide that adjusts the refractive index, an inorganic filler that improves the barrier properties, and a silane compound are added.

[0059] Like this Anionic Polymers The crosslinking agent for the above-mentioned polymerization is desirably used in an amount of 1 to 50 parts by weight, particularly 10 to 40 parts by weight, per 100 parts by weight of the anionic polymer.

[0060] The moisture-trapping layer (B1) is formed by applying a coating composition in which a specific hygroscopic polymer or hygroscopic agent is dissolved or dispersed in an organic solvent, heating the composition to form a film, and then maintaining the film under reduced pressure in a dry atmosphere to release moisture present in the layer formed. Alternatively, the moisture-trapping layer (B1) can be formed by applying the above-mentioned coating composition to another organic film in the same manner, and then bonding the moisture-trapping layer (B1) to the base layer (A1) using a dry lamination adhesive or the like.

[0061] <Moisture trapping layer (B2)> In the present invention, as shown in (3), (4), (6), and (8) of embodiment α described below, (3), (4), (6), and (8) of embodiment β described below, and (3) to (8), (11) to (12) of embodiment γ described below, the base layer (A1) may further include a moisture-trapping layer (B2) on the surface opposite to the moisture-trapping layer (B1). The moisture trapping layer (B2) is not particularly limited as long as it exhibits moisture blocking properties, and may be a layer known per se, such as a layer in which a moisture absorbent such as zeolite is dispersed in a specific resin layer. The moisture trapping layer (B2) may also be a layer made of the same material as the moisture trapping layer (B1). Both the moisture trapping layer (B1) and the moisture trapping layer (B2) preferably contain a resin composition in which a moisture absorbent (ii) is dispersed in a cationic polymer (i).

[0062] The moisture-trapping layer (B2) may have an anchor coat layer and a top coat layer. The anchor coat layer and the top coat layer may be formed by known techniques. The layer forming the anchor coat layer may be, for example, an organic layer made of at least one selected from urethane resin, polyester resin, polyether resin, epoxy resin, acrylic resin, phenol resin, and melamine resin, and is preferably formed from urethane resin, epoxy resin, or acrylic resin. A crosslinked structure may be introduced into these resins. Furthermore, it may be an organic layer to which an inorganic filler or a silane compound that improves the barrier properties is added. The layer forming the top coat layer may be, for example, an organic layer made of at least one selected from urethane resin, polyester resin, polyether resin, epoxy resin, acrylic resin, phenol resin, and melamine resin, and is preferably formed from urethane resin, epoxy resin, or acrylic resin. A crosslinked structure may be introduced into these resins. Furthermore, it may be an organic layer to which a metal oxide that adjusts the refractive index, an inorganic filler that improves the barrier properties, or a silane compound is added.

[0063] <Plastic layer (C)> The plastic layer (C) may be a layer of the material and thickness described in the section on the plastic layer (x) above. The plastic layer (C) may be made of the same material as the plastic layer (x) above or a different material. The plastic layer (C) may be made of the same thickness as the plastic layer (x) above or a different thickness. The plastic layer (C) preferably contains an olefin resin, a polyester resin, a polyimide resin, a polyamide resin, or a cyclic olefin resin.

[0064] <Adhesive layer (D)> The multilayer film of the present invention preferably further comprises an adhesive layer (D) on the surface of the moisture-trapping layer (B1) facing the plastic layer (C).

[0065] As the adhesive layer (D), known adhesives such as (meth)acrylic adhesives and urethane adhesives can be used, and these adhesives can be used to form an adhesive layer (D) of a certain thickness or less (for example, 30 μm or less). Ethylene-vinyl acetate copolymers (EVA), soft polyolefins (LLDPE), metallocene polyolefin elastomers, etc. can also be used as adhesives.

[0066] The adhesive is preferably adjusted so that the adhesive strength to the surface of the moisture-trapping layer (B1) is 0.3 N / 25 mm or more. The adhesive strength can be adjusted by introducing a crosslinked structure into the polymer forming the adhesive depending on the material of the surface of the moisture-trapping layer (B1). The adhesive strength can also be adjusted by adding a lubricant or the like to the adhesive.

[0067] <Manufacturing of multi-layer films> The multilayer film of the present invention is (1) a step of forming a layer selected from the group consisting of an inorganic barrier layer (a1) and an inorganic barrier layer (a2) by vapor deposition on at least one surface of a plastic layer (x) to form a substrate layer (A1); (2) coating the substrate layer (A1) with a resin composition for forming the moisture-trapping layer (B1), and then curing the composition; and (3) coating the resulting multilayer film with an adhesive that forms the adhesive layer (D) and then laminating the outer layer (Q); It can be produced by The plastic layer (x), vapor deposition, inorganic barrier layer (a), substrate layer (A1), moisture trapping layer (B1), adhesive layer (D), and outer layer (Q) are as described above.

[0068] <Application> The multilayer film of the present invention is used as a sealant for electronic devices. For example, the multilayer film is attached to a device using a pressure-sensitive adhesive or the like to seal the device, thereby keeping the inside of the device dry. Alternatively, the multilayer film of the present invention is used as a substrate for electronic devices, for example, by directly laminating an electronic device on the multilayer film of the present invention. The electronic device to which the multilayer film of the present invention is applied is not particularly limited, and the multilayer film can be applied to various electronic devices, such as organic EL elements, solar cells, touch panels, electronic panels, and other organic devices that are particularly susceptible to charge leakage due to moisture.

[0069] <Layer configuration> The substrate layer (A1) has the following aspects. Mode α: This mode has an inorganic barrier layer (a1) on the side opposite to the moisture-trapping layer (B1). Mode β: An embodiment having an inorganic barrier layer (a2) on the moisture-trapping layer (B1) side. Mode γ: A mode that incorporates the above modes (α) and (β), i.e., has an inorganic barrier layer (a1) on the side opposite the moisture trapping layer (B1), and has an inorganic barrier layer (a2) on the side facing the moisture trapping layer (B1).

[0070] Examples of layer configurations of the multilayer film of the present invention when using the base layer (A1) of embodiment α are as follows: The outer layer (Q) may be, for example, the plastic layers (C) (1) to (4), the base layer (A1) (5) to (6), i.e., a1 / x, or the base layer (A2) (7) to (8), i.e., a4 / y. (1) a1 / x / B1 / D / C (2) a1 / x / B1 / D / a3 / C (3) B2 / a1 / x / B1 / D / C (4) B2 / a1 / x / B1 / D / a3 / C (5) a1 / x / B1 / D / a1 / x (6) B2 / a1 / x / B1 / D / a1 / x (7) a1 / x / B1 / D / a4 / y (8) B2 / a1 / x / B1 / D / a4 / y

[0071] Examples of layer configurations of the multilayer film of the present invention when using the base layer (A1) of embodiment β are as follows: The outer layer (Q) may be, for example, the plastic layers (C) (1) to (4), the base layer (A1) (5) to (6), i.e., a1 / x, or the base layer (A2) (7) to (8), i.e., a4 / y. (1) x / a2 / B1 / D / C (2) x / a2 / B1 / D / a3 / C (3) B2 / x / a2 / B1 / D / C (4) B2 / x / a2 / B1 / D / a3 / C (5) x / a2 / B1 / D / a1 / x (6) B2 / x / a2 / B1 / D / a1 / x (7) x / a2 / B1 / D / a4 / y (8) B2 / x / a2 / B1 / D / a4 / y

[0072] An example of the layer structure of the multilayer film of the present invention when the base layer A of embodiment γ is used is as follows. The outer layer (Q) is made up of the plastic layers (C) (1) to (6) and the base layer (A2) (7) to (8), i.e., a4 / y, (9) to (10), 12 ) as the base layer (A1), that is, a1 / x, is used. (1) a1 / x / a2 / B1 / D / C (2) a1 / x / a2 / B1 / D / a3 / C (3) B2 / a1 / x / a2 / B1 / D / C (4) B2 / a1 / x / a2 / B1 / D / a3 / C (5) a5 / z / D / B2 / a1 / x / a2 / B1 / D / C (6) z / a5 / D / B2 / a1 / x / a2 / B1 / D / C (7) a5 / z / D / B2 / a1 / x / a2 / B1 / D / a4 / y (8)z / a5 / D / B2 / a1 / x / a2 / B1 / D / a4 / y (9) a1 / x / a2 / B1 / D / a1 / x (10) B2 / a1 / x / a2 / B1 / D / a1 / x (11)a5 / z / D / B2 / a1 / x / a2 / B1 / D / a1 / x (12)z / a5 / D / B2 / a1 / x / a2 / B1 / D / a1 / x

[0073] In the above layer structure, the abbreviations are as follows. A1: Base layer (a1 / x, x / a2 or a1 / x / a2) A2: Base material layer (A4 / Y) A3: Base layer (a5 / z or z / a5) x: Plastic layer y: Plastic layer z: plastic layer a1: inorganic barrier layer A2: Inorganic barrier layer A3: Inorganic barrier layer A4: Inorganic barrier layer A5: Inorganic barrier layer B1: Moisture trapping layer B2: Moisture trapping layer C: Plastic layer

[0074] The multi-layer film of the present invention is not limited to the above-mentioned layer structure, and for example, a plurality of multi-layer films having the above-mentioned layer structure may be bonded to each other. EXAMPLES

[0075] The excellent performance of the gas barrier multilayer film (multilayer film) of the present invention is as follows: Working Example This is explained below.

[0076] < Moisture permeability (g / m 2 / day) Measurement The water vapor permeability measurement device "HiBarSens 2.0 (SEMPA, Germany)" was used to measure the water vapor permeability under conditions of a temperature of 40°C and a relative humidity of 90%. The device switches between modes depending on the barrier performance of the sample being measured. -4 g / m 2 / day or more water vapor transmission rate was measured using the Carrier Gas mode, with a rate of 1×10 -4 g / m 2 / day, measurements were performed in Combination mode, which is suitable for more sensitive measurements, in order to accurately evaluate high barrier performance.

[0077] <Coating solution A preparation > Polyallylamine (manufactured by Nittobo Medical, PAA-15C, aqueous solution, solid content 15%) was used as an ionic polymer, and diluted with water to a solid content of 5% by weight to obtain a polymer solution. Meanwhile, γ-glycidoxypropyltrimethoxysilane was used as a crosslinking agent, and dissolved in water to a solid content of 5% by weight to prepare a crosslinking agent solution. Next, the polymer solution and the crosslinking agent solution were mixed so that γ-glycidoxypropyltrimethoxysilane was 15 parts by weight per 100 parts by weight of polyallylamine, and further, a crosslinked product of sodium polyacrylate (manufactured by Nippon Exlan Kogyo, Tuftic HU-820E, aqueous dispersion, solid content 13%, average particle size D 50 400 parts by weight of polyallylamine was added to the polyallylamine, and the solid content was adjusted to 5% with water, followed by thorough stirring to prepare coating solution A for the moisture-trapping layer.

[0078] <Example 1> A biaxially stretched PET (polyethylene terephthalate) film with a thickness of 100 μm was used as the plastic layer (x) (x in FIG. 1), and an inorganic barrier layer (a1) (a1 in FIG. 1) of silicon oxide was formed on one side of the film using a plasma CVD apparatus to obtain a base layer (A1) (A1 in FIG. 1). The film formation conditions are shown below.

[0079] Frequency 27.12MHz High Frequency Oscillator A CVD apparatus was used, which had a matching box, a metal cylindrical plasma processing chamber with a diameter of 300 mm and a height of 450 mm, and an oil rotary vacuum pump for evacuating the processing chamber. A plastic substrate was placed on parallel flat plates in the processing chamber, and 3 sccm of hexamethyldisiloxane and 45 sccm of oxygen were introduced. After that, high frequency waves were generated at an output of 50 W by the high frequency oscillator, and film formation was performed for 2 seconds to form an adhesive layer. Next, high frequency waves were generated at an output of 500 W by the high frequency oscillator, and film formation was performed for 30 seconds to form an inorganic barrier layer (a1). The obtained inorganic barrier layer-coated PET film, the substrate layer (A1) (A1 in Figure 1), was measured in an atmosphere of 40°C and 90% RH. Moisture permeability But 2×10 -4 g / m 2 It was / day.

[0080] Under the conditions mentioned above preparation The coating solution A was applied by a bar coater onto the PET surface of the base layer (A1) (A1 in Fig. 1) having the inorganic barrier layer (a1) previously prepared. The film after application was heat-treated in a box-type electric oven under conditions of a peak temperature of 120°C and a peak temperature holding time of 10 seconds to form a moisture-trapping layer (B1) (B1 in Fig. 1) with a thickness of 4 μm, and a coating film (i) (11 in Fig. 1) was obtained.

[0081] The obtained coating film (i) was then quickly transferred into a glove box in which the nitrogen concentration was adjusted to 99.95% or more. A 12 μm thick industrial PET film was used as the plastic layer (C) (C in FIG. 1), which was dry laminated onto the moisture trapping layer (B1) (B1 in FIG. 1) of the coating film (i) via a 4 μm thick urethane adhesive layer (D) (D in FIG. 1). In order to harden the adhesive layer (D) so as not to absorb moisture, aging was performed under vacuum at 50°C for 3 days, and a multilayer film 1 (12 in FIG. 1) with a layer structure as shown in FIG. 1 was obtained.

[0082] <Example 2> A substrate layer (A1) having an inorganic barrier layer (a2) was prepared under the same conditions as in Example 1, except that the high-frequency output of the film-forming conditions shown in Example 1 was changed to 300 W. The obtained substrate layer (A1) (A1 in FIG. 2) was measured in an atmosphere of 40° C. and 90% RH. Moisture permeability But 8 x 10 -4 g / m 2 Instead of the coating film (i) shown in Example 1, a coating film (ii) (21 in FIG. 2) was used in which the coating liquid A was applied by a bar coater onto the inorganic barrier layer (a2) on the side opposite to the PET of the base layer (A1), and a multilayer film 2 (22 in FIG. 2) was obtained in the same manner as in Example 1.

[0083] <Example 3> A biaxially stretched PET film having a thickness of 100 μm was used for the plastic layer (x), and an inorganic barrier layer (a1) of silicon oxide was formed on both sides of the film using a plasma CVD apparatus under the film forming conditions of Example 1, and an inorganic barrier layer (a2) of silicon oxide was formed under the film forming conditions of Example 2, to obtain a substrate layer (A1). The obtained substrate layer (A1) (A1 in FIG. 3) was measured in an atmosphere of 40° C. and 90% RH. Moisture permeability But 9×10 -5 g / m 2 Using a coating film (iii) (31 in FIG. 3) in which the coating liquid A was applied onto the inorganic barrier layer (a2) with a bar coater to form a moisture-trapping layer (B1), a 12 μm-thick PET film was dry-laminated onto the moisture-trapping layer (B1) (B1 in FIG. 3) as a plastic layer (C) via an adhesive layer (D) in the same manner as in Example 1 to obtain a multilayer film 3 (32 in FIG. 3).

[0084] <Example 4> In Example 1, instead of the 12 μm thick PET film used for the plastic layer (C), a 40 ℃9 Under 0% RH atmosphere Moisture permeability is 0.15g / m 2 The inorganic barrier layer (a4) side of a commercially available barrier film (Techbarrier LS, manufactured by Mitsubishi Chemical) having a coating film (i) of 1000 μm / day was (41 in Fig. 4) A multilayer film 4 (42 in FIG. 4) was obtained in the same manner as in Example 1, except that the above-mentioned was dry-laminated onto the moisture-trapping layer (B1).

[0085] <Example 5> Two substrate layers (A1) obtained in Example 1 were used, and one of them was placed on the inorganic barrier layer (a1) side instead of the 12 μm-thick PET film used in the plastic layer (C) in Example 1. adhesive layer (D) through the coating film (i) (51 in Fig. 5) A multilayer film 5 (52 in FIG. 5) was obtained in the same manner as in Example 1, except that the above-mentioned was dry-laminated onto the moisture-trapping layer (B1).

[0086] <Comparative Example 1> The base layer (A1) (A1 in FIG. 6) was prepared under the same conditions as in Example 1, except that the high-frequency output of the film-forming conditions shown in Example 1 was changed to 300 W. Moisture permeability is 2.1×10 -3 g / m 2 A multilayer film 6 (62 in FIG. 6) was obtained in the same manner as in Example 1, except that the drying time was changed to 10 min / day.

[0087] <Evaluation test> The laminated samples prepared above were heated at 40℃ 90% RH Under the atmosphere Moisture permeability The results are shown in Table 1. In Examples 1 to 5, unlike Comparative Example 1, the multilayer film was heated at 40° C. under 90% RH. Moisture permeability is 1×10 -6 g / m 2 / day.

[0088] [Table 1] [Explanation of symbols]

[0089] 11 Coating film (i) 12 Gas barrier multilayer film 1 21 Coating film (ii) 22 Gas barrier multilayer film 2 31 Coating film (iii) 32 Gas barrier multilayer film 3 41 Coating film (iv) 42 Gas barrier multilayer film 4 51 Coating Film (v) 52 Gas barrier multilayer film 5 61 Coating films (vi) 62 Gas barrier multilayer film 6 A1 Base material layer A2 base material layer x Plastic layer y Plastic layer a1 Inorganic barrier layer a2 Inorganic barrier layer a4 Inorganic barrier layer B1 Moisture trapping layer C Plastic layer D Adhesive layer

Claims

1. The sheet comprises a substrate layer (A1), a moisture-trapping layer (B1), and an outer layer (Q) in this order, The substrate layer (A1) has a layer selected from the group consisting of an inorganic barrier layer (a1) and an inorganic barrier layer (a2) on at least one surface of the plastic layer (x), The moisture permeability of the substrate layer (A1) (40°C, RH 90%) is 1 x 10 -3 g / m 2 / day, Gas barrier multilayer film.

2. The substrate layer (A1) is (α) having an inorganic barrier layer (a1) on the surface opposite to the moisture-trapping layer (B1), (β) having an inorganic barrier layer (a2) on the moisture-trapping layer (B1) side, or (γ) Comprises the above (α) and (β), The gas barrier multilayer film according to claim 1 .

3. 3. The gas barrier multilayer film according to claim 1 or 2, wherein the outer layer (Q) is a layer selected from the group consisting of a plastic layer (C), a base layer (A1) and a base layer (A2), and the base layer (A2) is a layer having an inorganic barrier layer (a4) on one side of the plastic layer (y).

4. 3. The gas barrier multilayer film according to claim 1, further comprising a moisture-trapping layer (B2) on the surface of the substrate layer (A1) opposite to the moisture-trapping layer (B1).

5. 5. The gas barrier multilayer film according to claim 4, further comprising an adhesive layer (D) and a substrate layer (A3) in this order on a surface of the moisture-trapping layer (B2) opposite to the substrate layer (A1), and the substrate layer (A3) is a layer having an inorganic barrier layer (a5) on one surface of the plastic layer (z).

6. 6. The gas barrier multilayer film according to claim 1, further comprising an inorganic barrier layer (a3) ​​on the surface of the plastic layer (C) on the moisture-trapping layer (B1) side.

7. 7. The gas barrier multilayer film according to claim 1, further comprising an adhesive layer (D) on the surface of the moisture-trapping layer (B1) on the side of the outer layer (Q).

8. The gas barrier multilayer film according to any one of claims 1 to 7, wherein the inorganic barrier layers (a1) to (a5) are metal oxide films.

9. The gas barrier multilayer film according to any one of claims 1 to 8, wherein the plastic layers (x) to (z) contain an olefin resin, a polyester resin, a polyimide resin, a polyamide resin, or a cyclic olefin resin.

10. The gas barrier multilayer film according to any one of claims 1 to 9, wherein the moisture-trapping layer (B1) and the moisture-trapping layer (B2) both contain a resin composition in which a moisture absorbent (ii) is dispersed in an ionic polymer (i).

11. The gas barrier multilayer film according to any one of claims 1 to 10, wherein the plastic layer (C) contains an olefin resin, a polyester resin, a polyimide resin, a polyamide resin, or a cyclic olefin resin.

Citation Information

Patent Citations

  • Plastic container and manufacture thereof

    JP2000255579A

  • Gas barrier laminate good in moisture barrier properties

    JP2015096320A