AI Technical Summary
Existing electrophotographic photoreceptors face challenges in reducing frictional force with cleaning blades in low-temperature, low-humidity environments, leading to poor cleaning performance and increased torque, while also experiencing toner slip-through and transfer inefficiencies, particularly with spherical toners of small particle size.
The photoreceptor features a surface layer with an uneven shape and exposed inorganic particles in recesses, where the outer surface exhibits wrinkles and ridgelines facing various directions, reducing friction and enhancing transfer properties by promoting point contact with toner.
The solution effectively reduces frictional force with cleaning blades and improves cleaning and transfer performance, even in low-temperature, low-humidity conditions, ensuring high-quality image production.
Abstract
Description
[Technical Field]
[0001] The present invention relates to an electrophotographic photosensitive member, a process cartridge having the electrophotographic photosensitive member, and an electrophotographic apparatus having the electrophotographic photosensitive member. [Background technology]
[0002] As the electrophotographic photoreceptor mounted in a process cartridge and an electrophotographic apparatus, an organic electrophotographic photoreceptor (hereinafter simply referred to as "electrophotographic photoreceptor" or "photoreceptor") containing an organic photoconductive substance (charge generating substance) is used. In recent years, there has been a demand for electrophotographic apparatuses with longer life, and there has been a desire to provide an electrophotographic photoreceptor with improved image quality and wear resistance (mechanical durability).
[0003] Furthermore, in recent electrophotographic devices, in addition to the aforementioned need for longer life, there is also a demand for more efficient transfer processes to suppress toner scattering during transfer, thereby improving image quality and reducing waste toner.
[0004] As a method for improving the abrasion resistance of an electrophotographic photoreceptor, a technique has been proposed in which a radically polymerizable resin is used in the surface layer of the photoreceptor, making the surface layer of the photoreceptor a hardened layer, thereby increasing the mechanical strength of the surface layer.
[0005] Electrophotographic photoreceptors are generally used in an electrophotographic image forming process consisting of a charging step, an exposure step, a developing step, a transfer step, and a cleaning step. Among these steps, the cleaning step of removing residual toner on the electrophotographic photoreceptor after the transfer step is an important step in obtaining a clear image. A typical cleaning method in the cleaning step is to press a rubber cleaning blade against the electrophotographic photoreceptor and scrape off the toner.
[0006] However, in the above cleaning method, the frictional force between the cleaning blade and the electrophotographic photosensitive member is large, which causes chattering of the cleaning blade and easily leads to poor image quality due to poor cleaning. This problem in the cleaning process becomes more pronounced as the mechanical strength of the surface layer of the electrophotographic photosensitive member increases, that is, as the peripheral surface of the electrophotographic photosensitive member becomes less susceptible to wear. That is, this problem is more likely to occur when the surface layer of the electrophotographic photosensitive member is made a hardened layer as described above, thereby increasing the mechanical strength of the surface layer.
[0007] Furthermore, the surface layer of an organic electrophotographic photosensitive member is generally formed by a dip coating method, and the surface of the surface layer formed by the dip coating method (i.e., the outer surface of the electrophotographic photosensitive member) becomes very smooth, which increases the contact area between the cleaning blade and the peripheral surface of the electrophotographic photosensitive member, thereby increasing the frictional resistance between the cleaning blade and the peripheral surface of the electrophotographic photosensitive member, and making the above-mentioned problems more pronounced.
[0008] As a method for overcoming the above-mentioned problems, a method has been proposed in which an uneven shape is provided on the outer surface of the photosensitive member, thereby reducing the contact area between the outer surface of the electrophotographic photosensitive member and the cleaning blade, thereby reducing the frictional force and improving the cleaning performance.
[0009] Patent Document 1 describes a technology in which metal oxide fine particles are contained in the surface layer. By containing metal oxide fine particles in the surface layer, some of the metal oxide fine particles are exposed on the outer surface of the electrophotographic photosensitive member, forming an uneven shape, which is thought to reduce the friction force between the cleaning blade and the photosensitive member.
[0010] Furthermore, Patent Document 2 describes a technology for a photoreceptor having a groove shape along the circumferential direction of the outer peripheral surface of the photoreceptor. In the technology disclosed in Patent Document 2, by providing a groove shape along the circumferential direction on the outer surface of the photoreceptor, the contact area between the cleaning blade and the photoreceptor is reduced, thereby reducing frictional force. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Japanese Patent Application Laid-Open No. 2018-128515 [Patent Document 2] Japanese Patent Application Laid-Open No. 2010-250355 Summary of the Invention [Problem to be solved by the invention]
[0012] The technique disclosed in Patent Document 1 does not sufficiently reduce the frictional force between the cleaning blade and the photosensitive member, and there are cases where the torque becomes large when used in a low-temperature, low-humidity environment.
[0013] Furthermore, in the technology disclosed in Patent Document 2, in a low-temperature, low-humidity environment, cleaning failures may occur in which toner partially passes through the groove-shaped portion. Furthermore, the technology disclosed in Patent Document 2 leaves room for improvement in transferability.
[0014] The present invention has been made in view of the above problems, and an object of the present invention is to provide a photoreceptor that can reduce the frictional force with a cleaning blade when used in a low-temperature, low-humidity environment, exhibits high cleaning performance, and has excellent transferability. [Means for solving the problem]
[0015] The above object is achieved by the present invention as follows. That is, the electrophotographic photoreceptor according to the present invention comprises: An electrophotographic photoreceptor having a support, a photosensitive layer, and a surface layer in this order, The outer surface of the electrophotographic photosensitive member has an uneven shape and thus exhibits a wrinkled shape, A square observation area with a side length of 200 μm is placed at an arbitrary position on the outer surface, a line passing through the center point of the observation area and parallel to the circumferential direction of the electrophotographic photosensitive member is defined as a reference line L1, and 1799 reference lines obtained by rotating the reference line L1 in 0.1° increments around the center point are defined as reference lines L2 to L1800, respectively. Each of the reference lines L1 to L1800 intersects with the ridge lines of the convex portions of the uneven shape at a plurality of points, At least two locations selected from the plurality of locations have mutually different intersection angles between the reference lines L1 to L1800 and the ridge line, and the surface layer contains a binder resin and inorganic particles, At least some of the inorganic particles are exposed in the recesses of the uneven surface. [Effects of the Invention]
[0016] According to the present invention, when used in a low-temperature, low-humidity environment, the frictional force with a cleaning blade can be reduced, and an electrophotographic photoreceptor exhibiting high cleaning performance and excellent transferability can be provided. [Brief explanation of the drawings]
[0017] [Figure 1] 1A and 1B are diagrams showing an example of the uneven shape of the outer surface of an electrophotographic photosensitive member according to the present invention, in which FIG. 1A is a top view of the outer surface of the electrophotographic photosensitive member, and FIG. 1B is a graph showing height information of the uneven shape obtained by surface observation of the outer surface of the electrophotographic photosensitive member. [Figure 2] 1A and 1B are diagrams showing an example of results obtained by numerically analyzing an electrophotographic photosensitive member according to the present invention, in which (A) shows a two-dimensional power spectrum F(r, θ) obtained by frequency analysis of wrinkles on the outer surface of the electrophotographic photosensitive member, (B) shows a one-dimensional radial distribution function obtained by integrating the two-dimensional power spectrum F(r, θ) in the θ direction, and (C) shows the variation in power values over the entire θ range when the angular distribution q(θ) is calculated from the two-dimensional power spectrum F(r, θ) for the frequency rp at which the one-dimensional radial distribution function p(r) takes on a maximum value. [Figure 3] FIG. 2 is a schematic diagram showing a cross section of the outer surface of an electrophotographic photosensitive member. [Figure 4] FIG. 2 is a schematic diagram showing exposure of inorganic particles in recesses observed when the outer surface of an electrophotographic photosensitive member is viewed from above. [Figure 5]1 is a diagram showing a schematic configuration of an electrophotographic apparatus having a process cartridge equipped with an electrophotographic photosensitive member. [Figure 6] FIG. 2 is a diagram showing a polishing machine used to polish the outer surface of an electrophotographic photosensitive member in a comparative example. DETAILED DESCRIPTION OF THE INVENTION
[0018] The present invention will be described in detail below with reference to preferred embodiments. The technology described in Patent Document 1 does not sufficiently reduce the contact area between the photosensitive member and the cleaning blade, and therefore, it is thought that there are cases where the reduction in frictional force is insufficient when used in a low-temperature, low-humidity environment.
[0019] Furthermore, in low-temperature, low-humidity environments, the toner and photoreceptor are easily charged, which increases the electrostatic adhesion between the toner and the photoreceptor. In the technology described in Patent Document 2, the grooves extend parallel to the rotational direction of the photoreceptor. Therefore, the inventors' investigations revealed that, particularly in low-temperature, low-humidity environments, residual toner on the outer surface of the photoreceptor may slip through the grooves and pass through the contact area with the cleaning blade, resulting in streak-like image defects. In particular, in recent years, due to the increasing demand for high-resolution, high-quality images, small-particle spherical toners have become mainstream. Small-particle spherical toners have a strong adhesive force to the outer surface of the photoreceptor, which makes it difficult for the cleaning blade to remove the toner. Therefore, it is believed that the technology described in Patent Document 2 is more likely to produce streak-like image defects when small-particle spherical toners are used.
[0020] Furthermore, as mentioned above, in a low-temperature, low-humidity environment, the adhesive force between the toner and the photoreceptor tends to be high, which tends to result in a large amount of residual toner remaining on the outer surface of the photoreceptor after the transfer process. To improve transferability, it is necessary to reduce the adhesive force between the toner and the electrophotographic photoreceptor, and reducing the contact area between the toner and the surface of the photoreceptor is effective. Therefore, one possible method is to reduce the contact area between the toner and the surface of the photoreceptor by providing an uneven surface to the outer surface of the photoreceptor. However, the uneven surface described in Patent Document 2 was not sufficient to improve transferability.
[0021] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by providing the outer surface of the photoreceptor with a predetermined uneven shape described below, and further exposing inorganic particles in the recesses of the uneven shape.
[0022] Specifically, the electrophotographic photoreceptor according to the present invention is An electrophotographic photoreceptor having a support, a photosensitive layer, and a surface layer in this order, The outer surface of the electrophotographic photosensitive member has an uneven shape and thus exhibits a wrinkled shape, A square observation area with a side length of 200 μm is placed at an arbitrary position on the outer surface, a line passing through the center point of the observation area and parallel to the circumferential direction of the electrophotographic photosensitive member is defined as a reference line L1, and 1799 reference lines obtained by rotating the reference line L1 in 0.1° increments around the center point are defined as reference lines L2 to L1800, respectively. Each of the reference lines L1 to L1800 intersects with the ridge lines of the convex portions of the uneven shape at a plurality of points, At least two points selected from the plurality of points have mutually different intersection angles between the reference lines L1 to L1800 and the ridge line, the surface layer contains a binder resin and inorganic particles, At least some of the inorganic particles are exposed in the recesses of the uneven surface.
[0023] Although the present inventors have not yet clarified the mechanism by which the electrophotographic photosensitive member according to the present invention has the above-described configuration and thus solves the problems in the prior art, they speculate as follows.
[0024] First, the outer surface of the electrophotographic photosensitive member has a predetermined number of convex portions within a certain range, thereby sufficiently reducing the contact area when the cleaning blade contacts the electrophotographic photosensitive member. It is presumed that this sufficiently reduces the frictional force between the cleaning blade and the electrophotographic photosensitive member, even in a low-temperature, low-humidity environment. Furthermore, the outer surface of the electrophotographic photosensitive member has an uneven shape, which gives it a wrinkled appearance, and the ridges of the convex portions of this uneven shape face in various directions. It is presumed that this also prevents toner from passing through the concave portions of the uneven shape when the electrophotographic photosensitive member rotates. It is believed that the above-mentioned features enable a high degree of both reduction in frictional force and prevention of toner from passing through.
[0025] Next, the reason why the electrophotographic photoreceptor according to the present invention has excellent transferability will be explained. According to the inventors' investigations, when the outer surface of the electrophotographic photoreceptor only has the above-described uneven shape and no inorganic particles are exposed in the recesses of the uneven shape, the effect of improving transferability is limited. This is thought to be because the toner is pressed into the recesses of the uneven shape, increasing the adhesive force between the toner and the surface of the photoreceptor. Therefore, as a result of further investigations, the inventors have found that excellent transferability can be obtained by incorporating inorganic particles into the surface layer of the electrophotographic photoreceptor and exposing the inorganic particles in the recesses of the uneven shape. This is presumably because the inorganic particles exposed in the recesses of the uneven shape come into point contact with the toner, increasing the distance between the toner and the surface of the photoreceptor and creating gaps, thereby reducing the adhesive force between the toner and the surface of the photoreceptor.
[0026] The irregular shape of the outer surface of the electrophotographic photosensitive member according to the present invention and the inorganic particles contained in the surface layer of the electrophotographic photosensitive member according to the present invention will be described in more detail below.
[0027] The unevenness on the outer surface of the electrophotographic photoreceptor according to the present invention has a certain level of fineness and a predetermined number of convex portions within a certain range. Specifically, first, on the outer peripheral surface of the photoreceptor, square observation areas with sides of 200 μm each are placed, each centered at 76 intersections of 19 line segments dividing the electrophotographic photoreceptor into 20 equal parts in the axial direction and four line segments dividing the electrophotographic photoreceptor into four equal parts in the circumferential direction, with each side parallel to the circumferential direction of the photoreceptor. Next, in each observation area, a line passing through the center of the observation area and parallel to the circumferential direction of the photoreceptor is designated as reference line L1. Furthermore, 1,799 reference lines obtained by rotating reference line L1 in 0.1° increments around the center point are designated as reference lines L2 to L1800. In this case, the unevenness in each observation area has a sufficient number of convex portions to intersect each of reference lines L1 to L1800 at multiple locations.
[0028] Furthermore, the uneven shape on the outer surface of the electrophotographic photosensitive member according to the present invention has a complex shape, with the ridges of the convex portions pointing in various directions. Specifically, for each of the reference lines L1 to L1800, at least two selected from a plurality of points at which the uneven shape intersects with the convex portions have different intersection angles. This causes the outer surface of the electrophotographic photosensitive member according to the present invention to exhibit a wrinkled shape.
[0029] FIG. 1 is a diagram showing an example of the uneven shape of the outer surface of an electrophotographic photosensitive member according to the present invention, in which FIG. 1(A) is a top view of the outer surface of the electrophotographic photosensitive member, and FIG. 1(B) is a graph showing height information of the uneven shape obtained by surface observation of the outer surface of the electrophotographic photosensitive member.
[0030] The uneven shape on the outer surface of the electrophotographic photosensitive member according to the present invention is a stripe-like uneven shape that can be observed on the outer surface of the electrophotographic photosensitive member, as shown in Fig. 1(A). The stripe shape is not distributed in a single direction but is composed of curved portions, straight portions, interrupted portions, branched portions, etc., and a plurality of stripes are present in a square observation area with one side of 200 µm.
[0031] Furthermore, the ridge line of the convex portions of the uneven shape refers to a straight line or curve obtained by connecting the highest points of the convex portions separating adjacent concave portions in the striped uneven shape when the outer surface of the electrophotographic photosensitive member is observed, as shown by a in Figure 1(A).
[0032] The method for identifying convex portions and obtaining ridgelines by surface observation of the outer surface of an electrophotographic photosensitive member is not particularly limited, but includes, for example, a method of performing image analysis on height information obtained by measurement using a confocal laser microscope. Figure 1(B) shows an example of height information obtained by this method plotted against the position on an arbitrary straight line placed on the outer surface of an electrophotographic photosensitive member. By identifying the vertex of the convex shape indicated by b in Figure 1(B), it is possible to obtain a curved ridgeline such as that indicated by a in Figure 1(A).
[0033] In the present invention, the ridge lines of the convex portions of the concave-convex shape have multiple curvatures within the ridge lines. Curvature is a quantity that represents the degree of curvature of a curve, and when the vicinity of an arbitrary point on the curve is approximated by a circle, the curvature χ is obtained as the reciprocal of the radius R of the circle, as shown in mathematical formula (I).
number
[0034] The electrophotographic photoreceptor according to the present invention preferably satisfies the following conditions. That is, in the observation region of the uneven shape, when the height information of the uneven shape is frequency analyzed to obtain a two-dimensional power spectrum F(r,θ) with the frequency component r and the angle component θ, a one-dimensional radial distribution function p(r) obtained by integrating the two-dimensional power spectrum F(r,θ) in the θ direction has at least one maximum value, and when the angular distribution q(θ) is calculated from the two-dimensional power spectrum F(r,θ) for the frequency rp at which the one-dimensional radial distribution function p(r) takes on the maximum value, the variation in power values over the entire θ range is 15% or less.
[0035] As a result of investigations by the present inventors, it has been found that the effects of the present invention can be highly obtained when the outer surface of the electrophotographic photosensitive member has an uneven shape and the uneven shape has a predetermined periodicity, as shown in FIG. 1(A).
[0036] The method for determining the periodicity of the uneven shape is not particularly limited, but an example thereof is a method in which height information is obtained from surface observation of the outer surface of an electrophotographic photosensitive member, and then the obtained results are analyzed using a two-dimensional Fourier transform.
[0037] Specifically, when height information of the uneven shape is obtained with the number of data N1 × N2, the height at any point (n, m) on the surface is expressed as h n,m Then, the two-dimensional power spectrum P(k,l) obtained by the discrete Fourier transform is given by the following equation (II).
number
[0038] where f k,l is given by the following formula (III):
number
[0039] Furthermore, the two-dimensional power spectrum P(k,l) obtained by formula (II) is transformed from the Cartesian coordinate system (k,l) to the polar coordinate system (r,θ) and expressed as the two-dimensional power spectrum F(r,θ), where r and θ satisfy the following formulas (IV) and (V), respectively.
number
number
[0040] In the present invention, in a square observation region with sides of 200 μm, height information obtained by measuring at regular intervals of 0.25 μm or less in two directions parallel to each side of the square is used for analysis.
[0041] 2A and 2B show an example of the results obtained by numerically analyzing the electrophotographic photosensitive member according to the present invention. Fig. 2A shows a two-dimensional power spectrum F(r,θ) obtained by frequency analysis of the uneven shape of the outer surface of the electrophotographic photosensitive member. Fig. 2B shows a one-dimensional radial distribution function obtained by integrating the obtained two-dimensional power spectrum F(r,θ) in the θ direction. Fig. 2C shows the variation in power values over the entire θ range when the angular distribution q(θ) is calculated from the two-dimensional power spectrum F(r,θ) for the frequency rp at which the one-dimensional radial distribution function p(r) takes a maximum value.
[0042] 2(B), the electrophotographic photosensitive member according to the present invention has at least one maximum value in the radial distribution function p(r) obtained by linearizing the two-dimensional power spectrum F(r, θ) in the radial direction, which means that the multiple concaves and convexes on the outer surface of the electrophotographic photosensitive member are distributed at regular intervals.
[0043] Furthermore, as shown in Figure 2(C), when calculating the angular distribution q(θ) of F(rp,θ) for the frequency rp at which the radial distribution function p(r) is maximized, it is preferable that the power value variation is within 15%, as this tends to prevent toner from slipping through. This indicates that when the power value variation is small, the ridges of the convex parts of the uneven shape face in various directions, making it isotropic.
[0044] The frequency rp at which the radial distribution function p(r) above takes a maximum value is 0.05 μm -1 More than 0.17μm -1 If the frequency rp is 0.05 μm or less, the toner is prevented from passing through, and the transferability is good, which is preferable. -1If the frequency rp is 0.17 μm or more, the contact area with the cleaning blade becomes small, and the effect of reducing the friction force with the cleaning blade can be obtained to a large extent. -1 If the amount is less than this, the inorganic particles exposed in the recesses and the toner tend to come into point contact with each other.
[0045] The depth of the uneven shape is preferably 1.0 μm or less, since this allows the inorganic particles to more easily come into point contact with the toner. More preferably, the depth of the uneven shape is 0.1 μm or more and 1.0 μm or less. If the depth of the uneven shape is 0.1 μm or more, the effect of reducing the friction force with the cleaning blade can be highly obtained. The method for measuring the depth of the uneven shape will be described later.
[0046] 3, the electrophotographic photoreceptor according to the present invention contains inorganic particles in the surface layer, and some of the inorganic particles in the surface layer are inorganic particles d that are partially exposed in the concave portions c of the uneven shape formed on the outer surface of the electrophotographic photoreceptor. Inorganic particles have low elasticity, which is advantageous because they can reduce the contact area between the toner surface and the particle surface when they come into contact with the toner.
[0047] Examples of inorganic particles contained in the surface layer include particles such as magnesium oxide, zinc oxide, lead oxide, tin oxide, tantalum oxide, indium oxide, bismuth oxide, yttrium oxide, cobalt oxide, copper oxide, manganese oxide, selenium oxide, iron oxide, zirconium oxide, germanium oxide, tin oxide, titanium oxide, niobium oxide, molybdenum oxide, vanadium oxide, copper aluminum oxide, antimony ion-doped tin oxide, and hydrotalcite. These particles can be used alone or in combination of two or more. Furthermore, silica particles are preferably used as the inorganic particles.
[0048] As the silica particles, known silica particles can be used, and may be either dry silica particles or wet silica particles. More preferably, the silica particles are wet silica particles obtained by a sol-gel method (hereinafter also referred to as "sol-gel silica").
[0049] The sol-gel silica may have a hydrophilic particle surface or may have a hydrophobic surface. Preferably, the sol-gel silica has a hydrophobic surface. By subjecting the surface of the silica particles to a hydrophobic treatment, the silica particles can be easily dispersed in the surface layer and easily exposed to the surface of the surface layer, which is preferable.
[0050] The hydrophobic treatment method includes a sol-gel method in which the solvent is removed from the silica sol suspension, the suspension is dried, and then the suspension is treated with a hydrophobic treatment agent, and a method in which the hydrophobic treatment agent is directly added to the silica sol suspension and the suspension is treated simultaneously with drying. From the viewpoint of controlling the half-value width of the particle size distribution and the saturated water adsorption amount, the method in which the hydrophobic treatment agent is directly added to the silica sol suspension is preferred.
[0051] Examples of hydrophobic treatment agents include the following. chlorosilanes such as methyltrichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, phenyltrichlorosilane, diphenyldichlorosilane, t-butyldimethylchlorosilane, and vinyltrichlorosilane; Tetramethoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, o-methylphenyltrimethoxysilane, p-methylphenyltrimethoxysilane, n-butyltrimethoxysilane, isobutyltrimethoxysilane, hexyltrimethoxysilane, octyltrimethoxysilane, decyltrimethoxysilane, dodecyltrimethoxysilane, tetraethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, diphenyldiethoxysilane, isobutyltrimethoxysilane, methyltriethoxysilane, methyltriethoxysilane, diphenyldiethoxysilane, isobutyltrimethoxysilane, methyltriethoxysilane, methyltriethoxysilane, diphenyldiethoxysilane, isobutyltrimethoxysilane, methyltriethoxysilane, methyltriethoxysilane, diphenyldiethoxysilane, isobutyltrimethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, isobutyltrimethoxy ... alkoxysilanes such as isobutyltriethoxysilane, decyltriethoxysilane, vinyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-chloropropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, and γ-(2-aminoethyl)aminopropyldimethoxysilane; silazanes such as hexamethyldisilazane, hexaethyldisilazane, hexapropyldisilazane, hexabutyldisilazane, hexapentyldisilazane, hexahexyldisilazane, hexacyclohexyldisilazane, hexaphenyldisilazane, divinyltetramethyldisilazane, and dimethyltetravinyldisilazane; Silicone oils such as dimethyl silicone oil, methyl hydrogen silicone oil, methyl phenyl silicone oil, alkyl-modified silicone oil, chloroalkyl-modified silicone oil, chlorophenyl-modified silicone oil, fatty acid-modified silicone oil, polyether-modified silicone oil, alkoxy-modified silicone oil, carbinol-modified silicone oil, amino-modified silicone oil, fluorine-modified silicone oil, and terminally reactive silicone oil; siloxanes such as hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, hexamethyldisiloxane, and octamethyltrisiloxane; Fatty acids and their metal salts include long-chain fatty acids such as undecylic acid, lauric acid, tridecylic acid, dodecylic acid, myristic acid, palmitic acid, pentadecylic acid, stearic acid, heptadecylic acid, arachidic acid, montanic acid, oleic acid, linoleic acid, and arachidonic acid, and salts of the above fatty acids with metals such as zinc, iron, magnesium, aluminum, calcium, sodium, and lithium.
[0052] Among these, alkoxysilanes, silazanes, and silicone oils are preferably used because they are easy to hydrophobize. These hydrophobizing agents may be used alone or in combination of two or more.
[0053] The volume average particle diameter of the inorganic particles is preferably 50 nm or more and 550 nm or less. By using inorganic particles with this volume average particle diameter, it is easy to expose them partially in the recesses of the uneven surface layer, and since the curvature is high, it is easy to reduce the contact area with the toner.
[0054] When the outer surface of the electrophotographic photosensitive member according to the present invention is viewed from above at a predetermined magnification using a scanning electron microscope, inorganic particles d exposed in the concave portions c of the uneven surface can be observed as shown in Fig. 4. Here, when the total area of the exposed portions of the inorganic particles in the concave portions is S1 and the total area of the portions of the concave portions other than the portions where the inorganic particles are exposed is S2, it is preferable that S1 / (S1+S2) (hereinafter also referred to as "coverage") is 0.20 or more and 0.80 or less.
[0055] When the coverage is 0.20 or more, the contact area between the toner and the portions of the outer surface of the photoreceptor where the inorganic particles are not exposed can be reduced, thereby reducing toner adhesion and improving the transferability of the photoreceptor. If the proportion of inorganic particles exposed in the recesses is too high, the distance between the contact points between the toner and the inorganic particles becomes shorter, resulting in a larger contact area between the toner and the inorganic particles exposed on the outer surface of the photoreceptor. This increases toner adhesion and limits the effect of improving transferability. When the coverage is 0.80 or less, the distance between the contact points between the toner and the inorganic particles can be maintained at an appropriate level, thereby improving the transferability of the photoreceptor. It is more preferable that the coverage is 0.25 or more and 0.60 or less.
[0056] The configuration of the electrophotographic photoreceptor according to the present invention will be described below. [Electrophotographic photoreceptor] The electrophotographic photoreceptor according to the present invention has a support, a photosensitive layer, and a surface layer in this order, and may further have a conductive layer and an undercoat layer between the support and the photosensitive layer.
[0057] The method for producing the electrophotographic photoreceptor according to the present invention includes a method in which a coating liquid for each layer is prepared, and the coating liquid is applied to a support in the desired layer order, followed by drying. In this case, the coating liquid can be applied by dip coating, spray coating, inkjet coating, roll coating, die coating, blade coating, curtain coating, wire bar coating, ring coating, etc. Among these, dip coating is preferred from the viewpoints of efficiency and productivity.
[0058] The support and each layer will be described below. <Support> In the present invention, the electrophotographic photoreceptor has a support. The support is preferably a support having electrical conductivity (conductive support). The support may have a cylindrical, belt-like, or sheet-like shape. Of these, a cylindrical support is preferred. The surface of the support may be subjected to electrochemical treatment such as anodization, blasting, cutting, or the like.
[0059] The support is preferably made of a metal, a resin, a glass, or the like. Examples of metals include aluminum, iron, nickel, copper, gold, stainless steel, and alloys thereof. Among these, an aluminum support using aluminum is preferred. Furthermore, the resin or glass may be made conductive by mixing or coating it with a conductive material.
[0060] <Conductive layer> In the present invention, a conductive layer may be provided on the support. By providing the conductive layer, scratches and irregularities on the surface of the support can be concealed and light reflection on the surface of the support can be controlled. The conductive layer preferably contains conductive particles and a resin.
[0061] Examples of materials for the conductive particles include metal oxides, metals, and carbon black. Examples of metal oxides include zinc oxide, aluminum oxide, indium oxide, silicon oxide, zirconium oxide, tin oxide, titanium oxide, magnesium oxide, antimony oxide, bismuth oxide, etc. Examples of metals include aluminum, nickel, iron, nichrome, copper, zinc, silver, etc. Among these, it is preferable to use metal oxides as the conductive particles, and it is particularly preferable to use titanium oxide, tin oxide, or zinc oxide. When a metal oxide is used as the conductive particles, the surface of the metal oxide may be treated with a silane coupling agent or the like, or the metal oxide may be doped with an element such as phosphorus or aluminum or an oxide thereof. The conductive particles may have a laminated structure including a core particle and a coating layer covering the core particle. Examples of the core particle include titanium oxide, barium sulfate, and zinc oxide. Examples of the coating layer include a metal oxide such as tin oxide. When metal oxide particles are used as the conductive particles, the volume average particle size thereof is preferably 1 nm or more and 500 nm or less, and more preferably 3 nm or more and 400 nm or less.
[0062] Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, and alkyd resin. The conductive layer may further contain silicone oil, resin particles, a masking agent such as titanium oxide, and the like.
[0063] The thickness of the conductive layer is preferably 1 μm or more and 50 μm or less, and particularly preferably 3 μm or more and 40 μm or less.
[0064] The conductive layer can be formed by preparing a coating solution for the conductive layer containing the above-mentioned materials and solvent, forming a coating film from this, and drying it. Examples of solvents used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Examples of dispersion methods for dispersing the conductive particles in the coating solution for the conductive layer include methods using a paint shaker, sand mill, ball mill, or liquid collision-type high-speed disperser.
[0065] <Undercoat layer> In the present invention, an undercoat layer may be provided on the support or the conductive layer. By providing an undercoat layer, the adhesion between layers can be improved and a charge injection blocking function can be imparted.
[0066] The undercoat layer preferably contains a resin. Alternatively, the undercoat layer may be formed as a cured film by polymerizing a composition containing a monomer having a polymerizable functional group. Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, acrylic resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinylphenol resin, alkyd resin, polyvinyl alcohol resin, polyethylene oxide resin, polypropylene oxide resin, polyamide resin, polyamic acid resin, polyimide resin, polyamideimide resin, and cellulose resin. Examples of the polymerizable functional group contained in the monomer having a polymerizable functional group include an isocyanate group, a blocked isocyanate group, a methylol group, an alkylated methylol group, an epoxy group, a metal alkoxide group, a hydroxyl group, an amino group, a carboxyl group, a thiol group, a carboxylic anhydride group, and a carbon-carbon double bond group.
[0067] Furthermore, for the purpose of improving electrical properties, the undercoat layer may further contain an electron transporting substance, a metal oxide, a metal, a conductive polymer, etc. Among these, it is preferable to use an electron transporting substance or a metal oxide. Examples of the electron transport substance include a quinone compound, an imide compound, a benzimidazole compound, a cyclopentadienylidene compound, a fluorenone compound, a xanthone compound, a benzophenone compound, a cyanovinyl compound, an aryl halide compound, a silole compound, a boron-containing compound, etc. An electron transport substance having a polymerizable functional group may be used as the electron transport substance, and the undercoat layer may be formed as a cured film by copolymerizing the electron transport substance with the above-mentioned monomer having the polymerizable functional group. Examples of metal oxides include indium tin oxide, tin oxide, indium oxide, titanium oxide, zinc oxide, aluminum oxide, silicon dioxide, etc. Examples of metals include gold, silver, aluminum, etc. The undercoat layer may further contain additives.
[0068] The thickness of the undercoat layer is preferably from 0.1 μm to 50 μm, more preferably from 0.2 μm to 40 μm, and particularly preferably from 0.3 μm to 30 μm.
[0069] The undercoat layer can be formed by preparing a coating solution for the undercoat layer containing the above-mentioned materials and solvent, forming a coating film from the coating solution, and drying and / or curing the coating film. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.
[0070] <Photosensitive layer> Photosensitive layers of electrophotographic photoreceptors are mainly classified into (1) multi-layer photosensitive layers and (2) single-layer photosensitive layers. (1) The multi-layer photosensitive layer has a charge generation layer containing a charge generation material and a charge transport layer containing a charge transport material. (2) The single-layer photosensitive layer has a photosensitive layer containing both a charge generation material and a charge transport material. The electrophotographic photoreceptor according to the present invention preferably has a multi-layer photosensitive layer.
[0071] (1) Laminated photosensitive layer The laminated photosensitive layer has a charge generating layer and a charge transport layer.
[0072] (1-1) Charge generation layer The charge generating layer preferably contains a charge generating material and a resin.
[0073] Examples of charge-generating materials include azo pigments, perylene pigments, polycyclic quinone pigments, indigo pigments, and phthalocyanine pigments. Among these, azo pigments and phthalocyanine pigments are preferred. Among phthalocyanine pigments, oxytitanium phthalocyanine pigments, chlorogallium phthalocyanine pigments, and hydroxygallium phthalocyanine pigments are preferred. The content of the charge generating material in the charge generating layer is preferably 40% by mass or more and 85% by mass or less, and more preferably 60% by mass or more and 80% by mass or less, based on the total mass of the charge generating layer.
[0074] Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, polyvinyl butyral resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinyl alcohol resin, cellulose resin, polystyrene resin, polyvinyl acetate resin, polyvinyl chloride resin, etc. Among these, polyvinyl butyral resin is more preferred.
[0075] The charge generating layer may further contain additives such as antioxidants and ultraviolet absorbers, etc. Specific examples include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, and benzophenone compounds.
[0076] The thickness of the charge generating layer is preferably 0.1 μm or more and 1 μm or less, and more preferably 0.15 μm or more and 0.4 μm or less.
[0077] The charge generating layer can be formed by preparing a coating solution for the charge generating layer containing the above-mentioned materials and solvent, forming a coating film from the coating solution, and drying the coating film. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.
[0078] (1-2) Charge transport layer The charge transport layer preferably contains a charge transport material and a resin.
[0079] Examples of charge transport materials include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, and resins having groups derived from these materials. Among these, triarylamine compounds and benzidine compounds are preferred, and compounds represented by formula (1) are preferably used. [ka] (In formula (1), R 1 ~R10 each independently represents a hydrogen atom or a methyl group.
[0080] Examples of the structure represented by formula (1) are shown in formulas (1-1) to (1-10). Among these, the structures represented by formulas (1-1) to (1-6) are more preferred. [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka]
[0081] The resin used is a thermoplastic resin, such as polyester resin, polycarbonate resin, acrylic resin, or polystyrene resin. Among these, polycarbonate resin and polyester resin are preferred. As the polyester resin, polyarylate resin is particularly preferred.
[0082] The content of the charge transport material in the charge transport layer is preferably 25% by mass to 70% by mass, and more preferably 30% by mass to 55% by mass, based on the total mass of the charge transport layer.
[0083] The content ratio (mass ratio) of the charge transport material to the resin is preferably 4:10 to 20:10, and more preferably 5:10 to 12:10.
[0084] The charge transport layer may also contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, and abrasion resistance improvers. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, and boron nitride particles.
[0085] The thickness of the charge transport layer is preferably from 5 μm to 50 μm, more preferably from 8 μm to 40 μm, and particularly preferably from 10 μm to 30 μm.
[0086] (2) Single-layer photosensitive layer The single-layer photosensitive layer can be formed by preparing a coating solution for the photosensitive layer containing a charge generating material, a charge transport material, a resin, and a solvent, forming the coating film, and drying the coating. The charge generating material, charge transport material, and resin are the same as those exemplified in "(1) Multilayer Photosensitive Layer" above.
[0087] <Protective layer> The electrophotographic photoreceptor according to the present invention has a protective layer as a surface layer on a photosensitive layer. The protective layer contains a binder resin and, as described above, inorganic particles. The protective layer is formed as a cured film by polymerizing a compound having a polymerizable functional group in a composition containing the compound having a polymerizable functional group. Here, the binder resin contained in the protective layer contains a polymer of the compound having a polymerizable functional group.
[0088] Examples of the polymerizable functional group contained in the monomer having a polymerizable functional group include an acryloyloxy group and a methacryloyloxy group.
[0089] A material having charge transport capability may be used as the monomer having a polymerizable functional group. As the charge transport structure, a triarylamine structure is preferred in terms of charge transport. As the polymerizable functional group of the material having charge transport capability, an acryloyloxy group or a methacryloyloxy group is preferred.
[0090] The number of polymerizable functional groups possessed by the monomer having a polymerizable functional group may be one or more. Among these, it is particularly preferred to form a cured film by polymerizing a composition containing both a compound having a plurality of polymerizable functional groups and a compound having one polymerizable functional group, since this makes it easy to eliminate distortion caused by polymerization of the plurality of functional groups.
[0091] Examples of the compound having one polymerizable functional group are shown in (2-1) to (2-6). [ka] [ka] [ka] [ka] [ka] [ka]
[0092] Examples of the compound having a plurality of polymerizable functional groups are shown in (3-1) to (3-7). [ka] [ka] [ka] [ka] [ka] [ka] [ka]
[0093] The protective layer preferably further contains conductive particles and / or a charge transport material, and a resin.
[0094] Examples of conductive particles include particles of metal oxides such as titanium oxide, zinc oxide, tin oxide, and indium oxide.
[0095] Examples of the charge transport material include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, and resins having groups derived from these materials. Among these, triarylamine compounds and benzidine compounds are preferred.
[0096] Examples of the resin include polyester resin, acrylic resin, phenoxy resin, polycarbonate resin, polystyrene resin, phenol resin, melamine resin, epoxy resin, etc. Among these, polycarbonate resin, polyester resin, and acrylic resin are preferred.
[0097] The protective layer may further contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slippage imparting agents, abrasion resistance improvers, etc. Specific examples of the additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, and boron nitride particles.
[0098] The thickness of the protective layer is preferably 0.2 μm to 5.0 μm in order to form a fine and uniform uneven shape, more preferably 0.2 μm to 4.0 μm inclusive, and even more preferably 0.2 μm to 3.0 μm inclusive.
[0099] The protective layer can be formed by preparing a coating solution for the protective layer containing the above-mentioned materials and solvent, forming a coating film from this, and drying and / or curing the coating film. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, sulfoxide-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.
[0100] <Method for forming unevenness on the outer surface of an electrophotographic photosensitive member> Methods for forming a textured shape on the outer surface of an electrophotographic photoreceptor include, for example, (1) laminating and compressing films with different Young's moduli, and (2) forming a structure by embossing. Method (1) requires a structure in which a relatively hard thin film is adhered to the surface of a relatively soft object. In this structure, the surface layer buckles (bends) due to compressive stress in the surface direction. Method (2) involves pressing a metal mold or other material against the outer surface of the photoreceptor to form a pattern, and is widely known as a technique for imparting a surface shape to a photoreceptor. Other methods, such as laser ablation, can also be used.
[0101] The method for forming the uneven shape (1) will be explained below. In the case of a laminated photosensitive layer, a protective layer is formed on a charge transport layer whose main component is a thermoplastic resin, or in the case of a single-layer photosensitive layer, on a single-layer photosensitive layer whose main component is a thermoplastic resin. The protective layer is a cured film formed by polymerizing a crosslinkable monomer. The composition (protective layer coating solution) containing a compound having a polymerizable functional group used to form the protective layer contains inorganic particles. After the protective layer is formed, a heat treatment is performed to form a concave-convex shape.
[0102] The mechanism by which the unevenness is formed is thought to be that during heat treatment, compressive stress is applied in the surface direction due to the difference in deformation between the protective layer and the charge transport layer or single-layer photosensitive layer, causing the protective layer to buckle, resulting in the formation of unevenness on the outer surface of the photoreceptor.Since the entire surface of the photoreceptor attempts to buckle uniformly, the ridges of the convex parts of the unevenness are formed randomly and isotropically, as shown in the example in Figure 1, and the outer surface of the electrophotographic photoreceptor appears wrinkled.
[0103] The heating temperature for forming the unevenness is preferably a temperature exceeding the boiling point of the residual solvent contained in the photosensitive layer. Furthermore, depending on the boiling point of the solvent used, a temperature of 140°C or higher and 230°C or lower is more preferable. When the heating temperature exceeds the boiling point of the residual solvent, the residual solvent in the photosensitive layer rapidly evaporates, and this portion tends to become the starting point for buckling due to compressive stress, making it easier to form a fine and uniform unevenness.
[0104] The photosensitive layer is formed by applying the photosensitive layer coating liquid to form a photosensitive layer coating film, heating the film, and drying it. Examples of solvents for the photosensitive layer coating liquid include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Specific examples include toluene, xylene (including at least one selected from the group consisting of o-xylene, m-xylene, and p-xylene), methyl benzoate, cyclohexanone, diethylene glycol monoethyl ether acetate, tetrahydrofuran, and dimethoxymethane. It is preferable to combine a solvent with a boiling point of 140°C or higher with a solvent with a boiling point lower than 140°C, as this allows an appropriate amount of solvent to remain in the photosensitive layer before heating to form the textured pattern. The amount of residual solvent can be measured by a known method, for example, gas chromatography.
[0105] The coating liquid for the protective layer contains a compound having a chain-polymerizable functional group. The protective layer is formed as a hardened film by applying this protective layer coating liquid onto the photosensitive layer and polymerizing the compound having a chain-polymerizable functional group.
[0106] Examples of polymerization reactions for a composition containing a monomer having a polymerizable functional group include polymerization methods using heat, light (such as ultraviolet light), or radiation (such as an electron beam). Among these, radiation is preferred, and among radiation, electron beams are more preferred. Electron beam irradiation is preferably carried out in a low-oxygen atmosphere to prevent deactivation of radicals in the polymerizable functional group. Furthermore, a relatively high temperature is required to sufficiently promote polymerization in a short period of time and form a cured film. Heating is preferably carried out in a low-oxygen atmosphere to prevent deactivation of radicals and promote rapid polymerization. The heating temperature should not exceed the boiling point of the residual solvent in the photosensitive layer, and specifically, a temperature between 90°C and 130°C is preferred.
[0107] [Process cartridges, electrophotographic devices] The process cartridge according to the present invention is characterized in that it integrally supports the electrophotographic photosensitive member described above and at least one means selected from the group consisting of a charging means, a developing means, and a cleaning means, and is detachably mountable to the main body of the electrophotographic apparatus.
[0108] The electrophotographic apparatus according to the present invention is characterized by having the electrophotographic photosensitive member described above, as well as a charging means, an exposing means, a developing means, and a transferring means.
[0109] FIG. 5 shows an example of the schematic configuration of an electrophotographic apparatus having a process cartridge equipped with the electrophotographic photosensitive member according to the present invention.
[0110] A cylindrical electrophotographic photoreceptor 1 is rotated around an axis 2 in the direction of the arrow at a predetermined peripheral speed. The surface of the electrophotographic photoreceptor 1 is charged to a predetermined positive or negative potential by a charging unit 3. While FIG. 5 shows a roller charging method using a roller-type charging member, other charging methods, such as corona charging, proximity charging, and injection charging, may also be used. An exposure unit (not shown) irradiates the charged surface of the electrophotographic photoreceptor 1 with exposure light 4, forming an electrostatic latent image corresponding to the desired image information. The electrostatic latent image formed on the surface of the electrophotographic photoreceptor 1 is developed with toner contained in a developing unit 5, forming a toner image on the surface of the electrophotographic photoreceptor 1. The toner image formed on the surface of the electrophotographic photoreceptor 1 is transferred to a transfer material 7 by a transfer unit 6. The transfer material 7 to which the toner image has been transferred is transported to a fixing unit 8, where the toner image is fixed and printed out from the electrophotographic device. The electrophotographic device may also have a cleaning unit 9 for removing toner and other deposits remaining on the surface of the electrophotographic photoreceptor 1 after transfer. Furthermore, a so-called cleanerless system may be used in which the deposits are removed by the developing unit 5 or the like without providing a separate cleaning unit 9. The electrophotographic apparatus may have a charge-removing mechanism that performs a charge-removing process on the surface of the electrophotographic photosensitive member 1 with pre-exposure light 10 from pre-exposure unit (not shown). Furthermore, guide unit 12 such as a rail may be provided in order to mount and remove the process cartridge 11 to and from the main body of the electrophotographic apparatus.
[0111] The electrophotographic photoreceptor according to the present invention can be used in laser beam printers, LED printers, copying machines, facsimiles, and combination machines thereof.
[0112] [Evaluation method for uneven surface shape and inorganic particles] The method for evaluating the irregularities on the outer surface of the electrophotographic photosensitive member according to the present invention and the inorganic particles contained in the surface layer will be described below.
[0113] <Method for evaluating the unevenness of the outer surface of a photoreceptor and measuring the depth of the unevenness> The outer surface of the electrophotographic photosensitive member is magnified and observed using a laser microscope (Keyence Corporation VK-X200) to obtain height information about the uneven shape. The observation points are square observation areas with sides of 200 μm, each centered at one of 76 intersections between 19 line segments that divide the electrophotographic photosensitive member into 20 equal parts in the axial direction and 4 line segments that divide the electrophotographic photosensitive member into 4 equal parts in the circumferential direction, and one side is set parallel to the circumferential direction of the electrophotographic photosensitive member. The height information is subjected to surface tilt correction to flatten the cylindrical photosensitive member.
[0114] Next, a reference line L1 that passes through the center point of the observation area and is parallel to the circumferential direction of the electrophotographic photosensitive member is set on the image including the uneven shape obtained by observation. Furthermore, reference lines L1 to L1800 are set by rotating the reference line L1 in 0.1° increments around the center point of the observation area.
[0115] Then, it is confirmed that each of the reference lines L1 to L1800 intersects with the ridge lines of the convex portions of the uneven shape at multiple points, and that the intersection angles between each of the reference lines L1 to L1800 and the ridge lines at at least two points selected from the multiple intersection points have mutually different values.
[0116] The depth of the unevenness was measured by analyzing the line roughness (JIS B 0601-2001) of the reference line L1 set in the observation area from the height information to determine the maximum valley depth Rv. The arithmetic mean value of Rv determined for each of the 76 observation areas was taken as the depth of the unevenness.
[0117] <Method for measuring the frequency rp of the unevenness of the outer surface of the photoconductor and the variation in power value> The height information of the uneven shape obtained above is subjected to frequency analysis to obtain a two-dimensional power spectrum F(r,θ). Next, the two-dimensional power spectrum F(r,θ) is made one-dimensional in the radial direction to calculate the radial distribution function p(r), and the frequency rp at which p(r) is maximized is determined. Furthermore, for the frequency rp at which p(r) is maximized, the angular distribution q(θ) of F(rp, θ) is calculated, and the variation in power values over the entire θ range is calculated.
[0118] <Method for measuring volume average particle size of inorganic particles> The volume average particle size is measured using a Zetasizer Nano-ZS (manufactured by MALVERN). This device can measure particle size by dynamic light scattering. First, the inorganic particles to be measured are diluted and adjusted to a solid-liquid ratio of 0.10% by mass (±0.02% by mass), then collected in a quartz cell and placed in the measurement unit. Water or a methyl ethyl ketone / methanol mixed solvent is used as the dispersion medium. Measurement conditions are entered into the control software Zetasizer software 6.30, including the refractive index of the inorganic particles, the refractive index of the dispersion solvent, viscosity, and temperature. Dn is used as the number average particle size. The refractive index of inorganic particles is taken from "Refractive Index of Solids" on page 517 of Volume II of the Chemical Handbook, Basics, 4th Revised Edition (edited by the Chemical Society of Japan, Maruzen Co., Ltd.). The refractive index, viscosity, and temperature of the dispersion solvent are selected from the values stored in the control software. In the case of mixed solvents, the weight average of the dispersion media to be mixed is taken.
[0119] <Method for checking the exposed state of inorganic particles in the recesses of the uneven surface and method for measuring the coverage rate> From the height information of the 200 μm square observation area obtained above, the total height H, which is the height from the highest point to the lowest point of the uneven shape, is determined. As shown in Figure 3, the part with a height equal to or less than half of the total height H is set as the recess c of the uneven shape. The recess c of the uneven shape is set for each of the above observation areas.
[0120] When the outer surface of the electrophotographic photosensitive member is viewed from above, it is determined whether inorganic particles are exposed in the concave portions of the uneven surface. The coverage rate is determined by calculating S1 / (S1+S2), where S1 is the total area of the portions of the concave portions of the uneven surface occupied by the exposed inorganic particles, and S2 is the total area of the concave portions of the uneven surface other than the portions occupied by the exposed inorganic particles.
[0121] The observation points for checking the exposed state of the inorganic particles and measuring the coverage rate were chosen from 19 points in the same axial direction out of the 76 points that are the center points of the observation area, and every other point from the edge was chosen (10 points in total). Each of the 10 points used was used as the center, and a 15 μm square area with one side parallel to the circumferential direction of the electrophotographic photosensitive member was observed using a scanning electron microscope (SEM) ("S-4800", manufactured by JEOL Ltd.).
[0122] Next, a photographic image of the photoreceptor taken using a scanning electron microscope is scanned. Image analysis is performed using image processing software (Image J (available from https: / / imagej.nih.gov / ij / )), and the particles in the photographic image are binarized. The concave portions of the uneven surface are identified in advance using a laser microscope. The total area of the portions where the particles are exposed in the concave portions of the uneven surface is defined as S1, and the total area of the portions other than the portions where the particles are exposed is defined as S2, and the coverage rate S1 / (S1+S2) is calculated. The coverage rate is calculated as described above for a total of 10 locations, and the arithmetic mean value of the obtained coverage rates is taken as the coverage rate of the particles in the concave portions of the uneven surface of the photoreceptor. [Example]
[0123] The present invention will be described in more detail below using examples and comparative examples. The present invention is not limited in any way by the following examples, provided that the gist of the invention is not exceeded. In the following description of the examples, "parts" are based on mass unless otherwise specified. The film thickness of each layer of the electrophotographic photoreceptor in the examples and comparative examples was determined using an eddy current film thickness meter (Fischerscope, manufactured by Fisher Instruments) or by converting the mass per unit area into specific gravity.
[0124] (particle) Particles 1 to 7 used to form the protective layer (surface layer) in the examples and comparative examples are shown in Table 1. Particles 1 to 6 are silica particles (inorganic particles), and particle 7 is a silicone resin particle. Particles 4 to 6 are particles whose surfaces have been hydrophobized.
[0125] [Table 1]
[0126] (Preparation of surface-treated particles 1) The following materials were prepared: 10 parts methanol 5 parts of particle 1 (listed in Table 1) These were mixed and dispersed at room temperature for 30 minutes using a US homogenizer. Next, 0.25 parts by mass of n-propyltrimethoxysilane ("KBM-3033" manufactured by Shin-Etsu Chemical Co., Ltd.), a reactive surface treatment agent, and 10 parts by mass of toluene were added, and the mixture was stirred at room temperature for 60 minutes. After removing the solvent using an evaporator, the mixture was heated at 140°C for 60 minutes to produce surface-treated particles 1, which were surface-treated with the reactive surface treatment agent.
[0127] (Preparation of surface-treated particles 2) Surface-treated particles 2 were prepared in the same manner as in the preparation of surface-treated particles 1, except that particles 1 were replaced with particles 2.
[0128] (Preparation of surface-treated particles 3) Surface-treated particles 3 were prepared in the same manner as in the preparation of surface-treated particles 1, except that particles 1 were replaced with particles 3.
[0129] <Production of Electrophotographic Photoreceptor> Example 1 An aluminum cylinder (JIS-A3003, aluminum alloy) having a diameter of 24 mm and a length of 257.5 mm was used as a support (conductive support).
[0130] Next, the following materials were prepared: 214 parts of titanium oxide (TiO2) particles (average primary particle size 230 nm) coated with oxygen-deficient tin oxide (SnO2) as metal oxide particles 132 parts of phenolic resin (phenolic resin monomer / oligomer) as a binder (product name: Plyofen J-325, manufactured by DIC Corporation, resin solid content: 60% by mass) 98 parts of 1-methoxy-2-propanol as solvent These were placed in a sand mill using 450 parts of 0.8 mm diameter glass beads and dispersed at 2000 rpm for 4.5 hours with a cooling water temperature of 18°C to obtain a dispersion. The glass beads were removed from this dispersion using a mesh (mesh opening: 150 μm). Silicone resin particles (product name: Tospearl 120, manufactured by Momentive Performance Materials, Inc., average particle size: 2 μm) were added to the resulting dispersion as a surface roughening agent. The amount of silicone resin particles added was 10% by mass of the metal oxide particles and binder material in the dispersion after removing the glass beads. Silicone oil (product name: SH28PA, manufactured by Dow Corning Toray Co., Ltd.) was also added as a leveling agent to the dispersion at 0.01% by mass of the metal oxide particles and binder material in the dispersion. Next, a mixed solvent of methanol and 1-methoxy-2-propanol (mass ratio 1:1) was added to the dispersion so that the total mass of the metal oxide particles, binder material, and surface roughening agent in the dispersion (i.e., the mass of the solid content) was 67 mass% relative to the mass of the dispersion. The mixture was then stirred to prepare a conductive layer coating solution. This conductive layer coating solution was dip-coated onto a support and heated at 140°C for 1 hour to form a conductive layer with a thickness of 30 μm.
[0131] Next, the following materials were prepared: 4 parts of an electron transport material represented by the following formula E-1 5.5 parts blocked isocyanate (trade name: Duranate SBN-70D, manufactured by Asahi Kasei Chemicals Corporation) Polyvinyl butyral resin (S-LEC KS-5Z, manufactured by Sekisui Chemical Co., Ltd.) 0.3 parts 0.05 parts zinc(II) hexanoate (Mitsuwa Chemical Co., Ltd.) as a catalyst These were dissolved in a mixed solvent of 50 parts tetrahydrofuran and 50 parts 1-methoxy-2-propanol to prepare a coating solution for an undercoat layer. The conductive layer was dip-coated with this coating solution and heated at 170°C for 30 minutes to form an undercoat layer with a thickness of 0.7 µm. [ka]
[0132] Next, the following materials were prepared: 10 parts of crystalline hydroxygallium phthalocyanine having peaks at 7.5° and 28.4° in a chart obtained by CuKα characteristic X-ray diffraction 5 parts polyvinyl butyral resin (product name: S-LEC BX-1, manufactured by Sekisui Chemical Co., Ltd.) These were added to 200 parts of cyclohexanone and dispersed for 6 hours using a sand mill with 0.9 mm diameter glass beads. This was further diluted with 150 parts of cyclohexanone and 350 parts of ethyl acetate to obtain a coating solution for the charge generating layer. The resulting coating solution was dip-coated onto the undercoat layer and dried at 95°C for 10 minutes to form a charge generating layer with a thickness of 0.20 μm.
[0133] The X-ray diffraction measurements were carried out under the following conditions. [Powder X-ray diffraction measurement] Measuring equipment used: Rigaku Electric Co., Ltd., X-ray diffraction equipment RINT-TTRII X-ray tube:Cu Tube voltage: 50KV Tube current: 300mA Scanning method: 2θ / θ scan Scan speed: 4.0° / min Sampling interval: 0.02° Starting angle (2θ): 5.0° Stop angle (2θ): 40.0° Attachment: Standard sample holder Filter: Not used Incident Monochrome:Use Counter monochromator: Not used Divergence slit: open Divergence vertical limit slit: 10.00 mm Scattering slit: open Receiving slit: open Flat plate monochromator: used Counter: Scintillation counter
[0134] Next, the following materials were prepared: 5 parts of a charge transport material (hole transport material) represented by the above formula (1-2) 5 parts of a charge transport material (hole transport material) represented by the above formula (1-3) 10 parts polycarbonate (product name: Iupilon Z400, manufactured by Mitsubishi Engineering Plastics Corporation) 0.02 parts of a polycarbonate resin having a copolymerization unit composed of a structure represented by the following formula (C-4) and a structure represented by the following formula (C-5) (x / y=0.95 / 0.05: viscosity average molecular weight=20,000) These were dissolved in a mixed solvent of 60 parts toluene, 20 parts methyl benzoate, and 20 parts dimethoxymethane to prepare a coating solution for the charge transport layer. The coating solution for the charge transport layer was dip-coated onto the charge generation layer to form a coating film for the charge transport layer, and the coating film was dried at 120°C for 30 minutes to form a charge transport layer with a thickness of 16 μm. [ka] [ka]
[0135] Next, the following materials were prepared: ·436 parts of particles 14 parts of the compound represented by the above formula (2-2) 10 parts of the compound represented by the above formula (3-1) 0.1 parts of siloxane-modified acrylic compound (Simac US270, manufactured by Toagosei Co., Ltd.) These were mixed with 58 parts of cyclohexane and 25 parts of 1-propanol and stirred to prepare a coating solution for the protective layer.
[0136] This protective layer coating solution was dip-coated onto the charge transport layer to form a protective layer coating film, and the resulting coating film was dried at 40°C for 5 minutes. Subsequently, under a nitrogen atmosphere, the coating film was irradiated with an electron beam for 1.6 seconds while rotating the support (irradiation target) at a speed of 300 rpm under conditions of an acceleration voltage of 70 kV and a beam current of 5.0 mA. The dose at the outermost surface layer was 15 kGy. Subsequently, under a nitrogen atmosphere, the first heating was performed by raising the temperature from 25°C to 100°C over 20 seconds to form a cured film with a thickness of 1.5 μm. The oxygen concentration from the electron beam irradiation to the subsequent first heating treatment was 10 ppm or less. Next, the coating film was naturally cooled in the atmosphere until the temperature reached 25°C, and then subjected to a second heating in the atmosphere at 160°C for 15 minutes to form a protective layer with an uneven surface and a wrinkled appearance. In this manner, an electrophotographic photoreceptor according to Example 1 was prepared.
[0137] The shape of the unevenness on the outer surface of the electrophotographic photosensitive member, the depth of the unevenness, frequency rp, power value variation, the presence or absence of exposed inorganic particles in the recesses of the unevenness, and the coverage of the inorganic particles were measured by the methods described above. The results are shown in Table 3.
[0138] Regarding the shape of the unevenness, if the following conditions were met, it was judged as A, and if the following conditions were not met, it was judged as B. Condition: Each of the reference lines L1 to L1800 intersects with the ridge lines of the convex portions of the uneven shape at multiple locations, and at least two locations selected from the multiple intersecting locations, the intersection angles between each of the reference lines L1 to L1800 and the ridge lines are different from each other.
[0139] In addition, for the frequency rp at which p(r) is maximized, the angular distribution q(θ) of F(rp,θ) was calculated, and a rating of A was given when the variation in power values over the entire θ range was 15% or less, and a rating of B was given when the variation was greater than 15%. In addition, the case where exposed inorganic particles were present in the recesses of the uneven shape was judged as A, and the case where no exposed inorganic particles were present was judged as B.
[0140] Examples 2 to 16 In forming the protective layer in Example 1, the type and amount of each compound used, the type and amount of particles, the film thickness, and the second heating treatment conditions were changed as shown in Table 2. Otherwise, electrophotographic photoreceptors according to Examples 2 to 16 were produced in the same manner as in Example 1. The obtained electrophotographic photoreceptors were subjected to various measurements and evaluations in the same manner as in Example 1. The results are shown in Table 3.
[0141] [Table 2]
[0142] Comparative Example 1 In forming the protective layer in Example 1, the film thickness and the second heating treatment conditions were changed as shown in Table 2. Otherwise, an electrophotographic photoreceptor according to Comparative Example 1 having no irregularities on the outer surface was produced in the same manner as in Example 1. The obtained electrophotographic photoreceptor was subjected to various measurements and evaluations in the same manner as in Example 1. The results are shown in Table 3.
[0143] Comparative Example 2 An electrophotographic photosensitive member having no irregularities on its outer surface was produced in the same manner as in Comparative Example 1. The outer surface of this photosensitive member was polished under the following conditions using the polishing machine shown in Fig. 6. In this way, an electrophotographic photosensitive member according to Comparative Example 2 was produced, having a plurality of grooves extending in the circumferential direction and parallel to one another on its outer surface. Polishing sheet feed speed: 400mm / min Electrophotographic photoreceptor rotation speed: 240 rpm Abrasive grain: silicon carbide Average grain size of abrasive grains: 3 μm Polishing time: 20 seconds The polishing method involved feeding an abrasive sheet 1-1, which was made of a sheet-like substrate and had a layer of abrasive grains dispersed in a binder resin, in the direction of the arrow while rotating an electrophotographic photoreceptor 1-7 in the direction of the arrow for 20 seconds to roughen the surface. Here, 1-2 to 1-5 are guide rollers, 1-6 is a backup roller, 1-8 is a feed roller, and 1-9 is a take-up roller. The obtained electrophotographic photoreceptor was subjected to various measurements and evaluations in the same manner as in Example 1. The results are shown in Table 3.
[0144] Comparative Examples 3 to 5 In forming the protective layer in Example 1, the type and amount of each compound used, the type and amount of inorganic particles, the film thickness, and the second heating treatment conditions were changed as shown in Table 2. Otherwise, electrophotographic photoreceptors according to Comparative Examples 3 to 5 were produced in the same manner as in Example 1. The obtained electrophotographic photoreceptors were subjected to various measurements and evaluations in the same manner as in Example 1. The results are shown in Table 3.
[0145] [Table 3]
[0146] <Evaluation> The electrophotographic photoreceptors produced in Examples 1 to 16 and Comparative Examples 1 to 5 were used to carry out the following evaluations. [Torque rating] The electrophotographic device used was a modified Hewlett-Packard laser beam printer, product name HP LaserJet Enterprise Color M553dn. The modifications included the ability to measure the drive current of the photoreceptor rotation motor. The device was also modified to allow adjustment and measurement of the voltage applied to the charging roller, the amount of image exposure light, and the voltage applied during the transfer process. The photoreceptors according to the examples and comparative examples were mounted in a cyan cartridge of an image forming apparatus.
[0147] Next, in a low-temperature, low-humidity environment of 15°C and 10% RH, 100 sheets of A4-size plain paper were printed with a test chart with a print ratio of 5%. The charging conditions were a dark potential of -500V, and the exposure conditions were an image exposure light amount of 0.25 μJ / cm. 2 The drive current value (current value A) was read when 100 sheets were output. The larger the obtained current value, the greater the frictional force between the electrophotographic photosensitive member and the cleaning blade.
[0148] Furthermore, an electrophotographic photoreceptor serving as a control for the torque relative value was prepared as follows. An electrophotographic photoreceptor was prepared in the same manner as in Example 1, except that particle 4 was removed from Example 1, the second heating step was performed at 100°C for 10 minutes, and no irregularities were formed. In this way, a control electrophotographic photoreceptor was prepared that did not have an irregularity on its outer surface and whose surface layer did not contain inorganic particles. Using the prepared control electrophotographic photoreceptor, the drive current value (current value B) of the rotary motor of the electrophotographic photoreceptor was measured in the same manner as in Example 1.
[0149] The ratio of the drive current value (current value A) to the drive current value (current value B) of the rotary motor for the electrophotographic photosensitive member thus obtained was calculated. The obtained values of (current value A) / (current value B) were compared as relative torque values. A smaller relative value indicates a greater reduction in the frictional force between the electrophotographic photosensitive member and the cleaning blade. The results are shown in Table 4.
[0150] [Evaluation of cleaning ability] The modified machine was placed in a low-temperature, low-humidity environment of 15°C and 10% RH, and 500 sheets of A4-sized plain paper were printed with a 5% print ratio. The charging conditions were a dark potential of -500V, and the exposure conditions were an image exposure light intensity of 0.25μJ / cm. 2 Next, 10 solid white images were printed out in succession, and then 10 solid black images were printed out, and evaluation was performed using the halftone images immediately after that. Specifically, the number of streaks in the halftone images caused by toner passing through due to poor cleaning was visually counted and evaluated according to the following criteria. A: There are no streaks in the image quality and the image quality is good. B: Very slight streaks occur. C: Slight streaks occur. D: Lines appear in part of the image. E: Streaks appear across the entire image. The results are shown in Table 4.
[0151] [Evaluation of transferability] The modified machine was placed in a low-temperature, low-humidity environment of 15°C and 10% RH, and 500 sheets of A4-sized plain paper were printed with a 5% print ratio. The charging conditions were a dark potential of -500V, and the exposure conditions were an image exposure light intensity of 0.25μJ / cm. 2 For evaluation, a solid black image was output after printing 500 sheets, and the residual toner remaining on the outer surface of the photoreceptor during the formation of the solid black image was taped off with a transparent polyester adhesive tape. The density difference was calculated by subtracting the density of the paper with only the adhesive tape attached from the density of the paper with the peeled adhesive tape attached. Density measurements were performed at five locations, and the arithmetic average value was calculated. The transferability was evaluated based on the density difference (referred to as the residual transfer density) according to the following criteria. The density was measured using an X-Rite color reflection densitometer (X-rite 500 Series, manufactured by X-rite). (Evaluation criteria) A: Transfer residual density is less than 0.2 B: Transfer residual density is 0.2 or more and less than 0.5 C: Transfer residual density is 0.5 or more and less than 1.0 D: Transfer residual density is 1.0 or more The results are shown in Table 4.
[0152] [Table 4]
Claims
1. An electrophotographic photoreceptor having a support, a photosensitive layer, and a surface layer in this order, The outer surface of the electrophotographic photoreceptor has an uneven shape and thus exhibits a wrinkled shape, A square observation area with sides of 200 μm is placed at an arbitrary position on the outer surface, a line passing through the center point of the observation area and parallel to the circumferential direction of the electrophotographic photosensitive member is defined as a reference line L1, and 1799 reference lines obtained by rotating the reference line L1 about the center point in increments of 0.1° are defined as reference lines L2 to L1800, Each of the reference lines L1 to L1800 intersects with the ridges of the convex portions of the uneven shape at a plurality of points, At least two points selected from the plurality of points have mutually different intersection angles between the reference lines L1 to L1800 and the ridge line, In the observation region, when height information of the uneven shape is frequency-analyzed to obtain a two-dimensional power spectrum F(r, θ) with a frequency component of r and an angle component of θ, a one-dimensional radial distribution function p(r) obtained by integrating the two-dimensional power spectrum F(r, θ) in the θ direction has at least one maximum value, When an angular distribution q(θ) is calculated from the two-dimensional power spectrum F(r,θ) for a frequency rp at which the one-dimensional radial distribution function p(r) takes the maximum value, the variation in power value over the entire θ range is 15% or less, The surface layer contains a binder resin and inorganic particles, At least a part of the inorganic particles is exposed in the concave portions of the concave-convex shape.
2. The frequency rp is 0.05 μm -1 0.17 μm or more -1 2. The electrophotographic photoreceptor according to claim 1, wherein:
3. 3. The electrophotographic photoreceptor according to claim 1, wherein the depth of the uneven shape is 1.0 [mu]m or less.
4. 4. The electrophotographic photoreceptor according to claim 1, wherein the inorganic particles have a volume average particle size of 50 nm or more and 550 nm or less.
5. 5. The electrophotographic photoreceptor according to claim 1, wherein when the outer surface is viewed from above, a total area of the exposed portions of the inorganic particles in the recesses is S1, and a total area of the recesses other than the portions where the inorganic particles are exposed is S2, S1 / (S1+S2) is 0.20 or more and 0.80 or less.
6. 6. The electrophotographic photoreceptor according to claim 1, wherein the surfaces of the inorganic particles have been subjected to a hydrophobic treatment.
7. 7. A process cartridge which integrally supports the electrophotographic photosensitive member according to claim 1 and at least one means selected from the group consisting of a charging means, a developing means, and a cleaning means, and is detachably mountable to a main body of an electrophotographic apparatus.
8. 7. An electrophotographic apparatus comprising the electrophotographic photoreceptor according to claim 1, a charging means, an exposing means, a developing means, and a transferring means.