Container and packaging bag for heating

JP2023121833A5Active Publication Date: 2024-12-05TOPPAN HOLDINGS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023108124
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-01-14
Filing Date
2023-06-30
Publication Date
2024-12-05
Estimated Expiration
2041-12-02

AI Technical Summary

Benefits of technology

【0026】 本開示によれば、デジタル印刷機による印刷が施された印刷面を有しつつも、製造過程で生じる屈曲部においても静電インク層とプライマー層との界面、及び静電インク層と接着剤層との界面におけるはく離が抑制された容器を提供できる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a container with restricted detachment at an interface between an electrostatic ink layer and a primer layer, and the interface between the electrostatic layer and an adhesive layer even at a bent part generated during a manufacturing process while having a printing surface on which the printing is applied by a digital printer.SOLUTION: A container according to one aspect of the disclosure comprises a body part having a bent part, the body part is composed of at least one laminate, the laminate comprises a substrate, a primer layer, an adhesive layer and a sealant layer in this order and has a printing surface composed of an electrostatic ink composition at least one part of a main surface at the sealant layer side of the primer layer, and the adhesive layer comprises at least either an adhesive composition including epoxy compound or its cured product.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure relates to containers and heat-packaging bags. The containers relating to this disclosure particularly relate to containers composed of at least one laminate and having a bendable portion. [Background technology]

[0002] Containers (e.g., packaging bags) for airtight storage of packaged goods such as food are well known. Many such containers use thin film or sheet packaging. These containers are printed with various information, including decorations, product names, brands, and manufacturer information. Digital printing using electrostatic ink compositions is a known method for applying such printing. Digital printing is performed using digital printing presses.

[0003] For example, Patent Document 1 proposes applying a primer resin to a first flexible substrate such as a PET film to obtain a coated surface, performing electrostatic printing on the coated surface using a digital printing press (HP Indigo20000 digital printing press for labels and packaging), and applying a crosslinking composition. After performing these predetermined steps, a technique is proposed to laminate the first flexible substrate coated with predetermined components and the second flexible substrate to obtain a laminate (packaging material for containers). [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] Japanese Patent Publication No. 2018-530478 [Overview of the project] [Problems that the invention aims to solve]

[0005] Digital printing using electrostatic ink compositions allows for small-lot production, and therefore, laminates with digital printing are used as materials for various containers. However, the electrostatic ink layer formed by the printed area created by the digital printing press may not have sufficient adhesive strength with the primer or adhesive layer, and delamination may occur between the electrostatic ink layer and the primer layer, or between the electrostatic ink layer and the adhesive layer, when external force is applied. In particular, when the laminate is bent and its deformation is large, the stress generated between the layers is large, and delamination may occur between the electrostatic ink layer and the primer or adhesive layer. In such situations, for example, the function of the container may be impaired, and misalignment of the printed surface may occur, making it difficult to read the printed information. While measures such as not providing a printed surface in the bent area can be considered, printing on the bent area is required to meet diverse demands. Therefore, a container that does not impair the function of the container or impair the printed information even when it has a bent area would be useful.

[0006] Furthermore, the electrostatic ink layer created by a digital printing press may not have sufficient adhesive strength with adjacent layers. Therefore, if packaging material created by the above method is used in packaging bags intended for heat treatment such as boiling and retorting, there was a possibility that the packaging bag would rupture during heating.

[0007] One of the objectives of this disclosure is to provide a container that has a printed surface printed by a digital printing press, while suppressing peeling at the interface between the electrostatic ink layer and the primer layer, and at the interface between the electrostatic ink layer and the adhesive layer, even in the bent parts that occur during the manufacturing process.

[0008] Another objective of this disclosure is to provide a heat-resistant packaging bag that has an electrostatic ink layer produced by a digital printing press while also having sufficient resistance to heat treatment. [Means for solving the problem]

[0009] One embodiment of the present disclosure provides a container comprising a body portion having a bent portion, wherein the body portion is composed of at least one laminate, the laminate comprising a base material, a primer layer, an adhesive layer, and a sealant layer in that order, the primer layer having a printed portion made of an electrostatic ink composition on at least a part of the main surface of the primer layer on the sealant layer side, and the adhesive layer comprising at least one of an adhesive composition containing an epoxy compound and a cured product thereof.

[0010] Since the adhesive layer of the above-mentioned container is composed of at least one of a specific adhesive composition and its cured product, sufficient adhesion can be maintained even in bent areas, and delamination at the interface between the electrostatic ink layer and the primer layer, and at the interface between the electrostatic ink layer and the adhesive layer, is suppressed. Furthermore, since the adhesion between each layer is maintained even in bent areas, the occurrence of misalignment of the printed area is suppressed, and the printed information on the body, including the bent areas, can be maintained in the initial state after printing. Even if new bends occur during the use of the container, for example, due to the container bending, the adhesion between each layer is maintained, so the function of the container (e.g., barrier properties) can be maintained throughout the period of use. Similarly, tearing of the container itself and deterioration of the printed information can be suppressed throughout the period of use.

[0011] The printed portion may be located in the bent portion. Since the body of the container according to this disclosure is made of the specific laminate described above, changes in the printed information are suppressed even when the printed portion is located in the bent portion.

[0012] The epoxy compound described above may include a bifunctional alicyclic epoxy compound. The bifunctional nature of the epoxy compound increases the number of crosslinking points with the electrostatic ink composition, thereby enabling stronger adhesion between the main surface (printing surface) of the primer layer and the adhesive layer.

[0013] The above adhesive composition further contains a polyol, the polyol includes an aliphatic polyester polyol, and the epoxy compound may include those having epoxy groups at both ends. Such an adhesive layer can exhibit high lamination strength particularly in a high-temperature environment.

[0014] The above adhesive composition further contains a polyisocyanate, and the polyisocyanate may include a xylylene diisocyanate derivative. Such a polyisocyanate and a polyol are excellent in reactivity. Thereby, the curability of the adhesive composition is improved, and peeling at the interface between the printing part (electrostatic ink layer) and the primer layer and at the interface between the printing part (electrostatic ink layer) and the adhesive layer can be further suppressed.

[0015] It may further include a stopper connected to the above body part.

[0016] The above stopper may have a cylindrical pouring outlet and a flange that spreads outward from the peripheral edge at the lower end of the above pouring outlet.

[0017] The above body part may be composed of one of the above laminates.

[0018] The above body part may be composed of two of the above laminates that become side sheets and one of the above laminates that becomes a bottom sheet.

[0019] Also, in order to achieve the above object, a heatable packaging bag according to one aspect of the present disclosure is a packaging bag for heat treatment, which is composed of a laminate having a base material, a primer layer, an electro-static ink layer, an adhesive layer, and a sealant layer in this order, wherein the adhesive layer contains at least one of an adhesive composition containing an epoxy compound and a cured product thereof.

[0020] The printed portion formed by printing an electrostatic ink composition using a digital printing machine tends to have inferior heat resistance and strength compared to when other inks are used. Therefore, when attempting to apply a laminate having a printed portion (electrostatic ink layer) derived from a conventional electrostatic ink composition to a heat treatment packaging bag, the adhesion near the printed surface is inferior, and thus damage to the packaging bag or the like may occur. On the other hand, according to the above configuration, since the deformation of the laminate due to heating or the like is suppressed by the curing of the adhesive composition containing an epoxy compound, a heat-resistant packaging bag having sufficient resistance to heat treatment can be obtained.

[0021] The primer layer may contain a polyethyleneimine resin. Since it has a primer layer containing a polyethyleneimine resin, the water resistance is also improved, and particularly sufficient resistance can be obtained even for heat treatment in an environment where there is a large amount of moisture, such as boiling heat treatment or retort heat treatment.

[0022] It may include a seal portion that adheres the sealant layers of the two laminates to each other at the outer peripheral portion, and the seal portion may be in an embodiment where the ink coverage rate of the electrostatic ink layer is 300% or less. Since the seal portion is an area where heat bonding such as heat sealing is performed, the possibility of damage is higher than in other areas. On the other hand, by setting the ink coverage rate of the electrostatic ink layer within the above range, more sufficient resistance to heat treatment can be ensured for the seal portion, and a heat-resistant packaging bag having stronger resistance to heat treatment can be obtained.

[0023] The epoxy compound can be in an embodiment that includes a bifunctional alicyclic epoxy compound. Such an epoxy compound, by being bifunctional, can increase the crosslinking points with the electrostatic ink composition and more firmly adhere the adhesive layer and the printed surface of the primer layer.

[0024] The above adhesive composition may further contain a polyol, the polyol may include an aliphatic polyester polyol, and the epoxy compound may include one having epoxy groups at both ends. Such an adhesive layer has high adhesive strength, especially in high-temperature environments. Therefore, even when the heat-treated packaging bag is subjected to heat treatment, the breakage of the electrostatic ink composition and damage to the packaging bag can be sufficiently suppressed.

[0025] The above adhesive composition may further contain a polyisocyanate, and the polyisocyanate may contain a xylylene diisocyanate derivative. Such polyisocyanates and polyols exhibit excellent reactivity. This improves the curability of the adhesive composition, thereby suppressing deformation of the heat-resistant packaging bag. [Effects of the Invention]

[0026] According to this disclosure, it is possible to provide a container that has a printed surface printed by a digital printing press, while suppressing peeling at the interface between the electrostatic ink layer and the primer layer, and at the interface between the electrostatic ink layer and the adhesive layer, even in the bent parts that occur during the manufacturing process.

[0027] According to this disclosure, a heat-resistant packaging bag is provided that has an electrostatic ink layer produced by a digital printing press and is sufficiently resistant to heat treatment. [Brief explanation of the drawing]

[0028] [Figure 1] Figure 1 is a perspective view showing an example of a container. [Figure 2] Figure 2 is a schematic cross-sectional view showing an example of a container equipped with a spout. [Figure 3] Figure 3 is a perspective view showing another example of a container. [Figure 4] Figure 4 is an end view along the line IV-IV in Figure 3. [Figure 5] Figure 5 is a cross-sectional view showing an example of a laminate. [Figure 6] Figure 6 is a cross-sectional view showing another example of a laminate. [Figure 7] Figure 7 is a plan view showing an example of a packaging bag. [Figure 8] Figure 8 is a plan view showing another example of a packaging bag. [Figure 9] Figure 9 is a reference diagram showing the results of the peeling suppression performance evaluation in the example. [Figure 10] Figure 10 is a reference diagram showing the results of the peeling suppression performance evaluation in the example. [Figure 11] Figure 11 is a reference diagram showing the results of the peeling suppression performance evaluation in the example. [Figure 12] Figure 12 illustrates the shape of the sealing portion of the packaging according to the examples and comparative examples. [Modes for carrying out the invention]

[0029] Embodiments of this disclosure will be described below with reference to the drawings, where applicable. However, the following embodiments are illustrative examples for illustrating this disclosure and are not intended to limit this disclosure to the following. In the description, the same reference numerals will be used for elements that are the same or have the same function, and redundant explanations will be omitted where applicable. Furthermore, positional relationships such as up, down, left, and right will be based on the positional relationships shown in the drawings unless otherwise specified. Moreover, the dimensional ratios in the drawings are not limited to those shown.

[0030] Unless otherwise specified, the materials exemplified herein may be used individually or in combination of two or more. The content of each component in a composition means the total amount of any multiple substances present in the composition, unless otherwise specified, if there are multiple substances corresponding to each component in the composition.

[0031] [container] One embodiment of the container is a container having a body portion with a bend, the body portion being composed of at least one laminate, the laminate comprising a base material, a primer layer, an adhesive layer, and a sealant layer in that order, and having a printed portion made of an electrostatic ink composition on at least a part of the main surface of the primer layer on the sealant layer side. The container may be, for example, a packaging bag, a tube container, and a standing pouch. The packaging bag is not limited to those used at room temperature, but may also be a packaging bag exposed to temperature changes such as heating and freezing. The container may be, for example, a container that is designed to be further folded during use. In the case of a tube container, when the packaged item is removed from the container by pressing and deforming the body portion, a new fold may be formed in the body portion. With the container of this disclosure, the adhesion between each layer is maintained even in such cases, so that the function of the container (e.g., barrier properties, etc.) can be maintained over the period of use.

[0032] Figure 1 shows an example of a container. Container 100 is made from a single sheet of laminate 300. Container 100 is obtained by first bonding two opposing sealant layers of a roughly rectangular laminate 300 together by a predetermined width to form a seal portion 101 and a cylindrical body, and then further bonding sealant layers together by a predetermined width at one of the openings of the cylindrical body to form a seal portion 103. Container 100 has a body portion 200 with a bent portion 60 and seal portions 101 and 103. The bent portion 60 is formed by bending the seal portion 101 along the side of the body portion 200 to improve handling when used as a container.

[0033] The container 100 shown in Figure 1 includes a storage section 102 for containing the packaged goods (e.g., food and beverages), which is formed by sealing sections 101 and 103 and an unsealed section (sheet section). In this specification, the sealed container containing the packaged goods is also referred to as a package. The sealing section 103 at the lower end may be sealed after the packaged goods are filled into the storage section 102. The sealing sections 101 and 103 are formed by heat-sealing the sealant layers of the laminate 300 together.

[0034] The container 100 may further include a spout connected to the body portion 200. Figure 2 is a schematic cross-sectional view showing an example of a container with a spout. Figure 2 shows an example of a container in which the body portion 200 of the container 100 and the spout are connected by placing the spout 70 on the unsealed upper end of the container 100 and heat-sealing a sealant layer to the spout 70. In this case, the container 100 comprises the body portion 200 and the spout 70, and the packaged goods can be removed from the spout by pressing the body portion 200. In this specification, such a container is also called a tube container.

[0035] The spout 70 shown in Figure 2 is an example consisting of a cylindrical spout 72 and a flange 74 that extends outward from the periphery of the lower end of the spout 72. The spout may have a cylindrical spout and a flange that extends outward from the periphery of the lower end of the spout, and may be, for example, a spout. The position in which the spout is provided is not particularly limited. If the spout is a spout, it may be a so-called center spout or a corner spout.

[0036] Figures 3 and 4 show another example of a container. The container 110 has a body 200 composed of two laminated bodies 300 that form the side sheets and one laminated body 306 that forms the bottom sheet. The container 110 is constructed by bonding the sealant layers of the two laminated bodies 300 that form the side sheets and the one laminated body 306 that forms the bottom sheet together. The container 110 has a sealed portion 122 obtained by bonding the two laminated bodies 300 that form the side sheets together, and a sealed portion 121 obtained by bonding the laminated body 306 that forms the bottom sheet together and the two laminated bodies 300 that form the side sheets together, thereby forming a bag-like shape. This configuration allows the volume of the storage section 102 to be expanded. The laminated body 306 that forms the bottom sheet has a bent portion 60 that occurs when manufacturing the container 110. The open, unsealed portion at the upper end of the container 110 may be sealed after the packaged goods are filled into the storage section 112. The sealing portions 122 and 121 are formed by heat-sealing the sealant layers of the laminate 300 together.

[0037] The three laminates constituting the container 110 do not necessarily have the same layer configuration; for example, they may have different layer configurations.

[0038] Containers 100, 110 may contain the packaged goods in an unsealed portion (sheet portion) surrounded by sealed portions 101, 121, 122. In this specification, a further sealed portion is also referred to as a package. The container may be provided with an opening means for easy opening. The opening means may have a pair of easy-open sections consisting of V-shaped notches formed in the unsealed portion at the side end or in the sealed portion 122 at the side end, and a half-cut line between the pair of easy-open sections that serves as a cutting trajectory. The half-cut line can be formed using a laser. The easy-open sections are not limited to V-shaped notches, but may be U-shaped or I-shaped notches, or a group of scratches.

[0039] The laminates constituting the above-mentioned containers 100 and 110 will now be described. Figure 5 is a schematic cross-sectional view showing an example of a laminate. Figure 5 shows a cross-section along the lamination direction (thickness direction) of the laminate. The laminate 302 has a base material 10, a primer layer 40, an adhesive layer 30, and a sealant layer 20 in this order. The base material 10, primer layer 40, adhesive layer 30, and sealant layer 20 may each be in the shape of a film. At least a part of the main surface (printed surface) of the primer layer 40 on the sealant layer 20 side may have a printed portion 52 made of an electrostatic ink composition. An electrostatic ink layer 50 made of one or more printed portions 52 is provided on the printed surface. In other words, an electrostatic ink layer 50 made of a printed portion 52 may be provided on at least a part of one of the pair of main surfaces of the primer layer 40 that is closer to the sealant layer 20.

[0040] The thickness of the laminate 302 may be, for example, 15 to 200 μm, or 18 to 120 μm.

[0041] The substrate 10 and the sealant layer 20 may be flexible substrates. Examples of flexible substrates include biaxially oriented polypropylene (BOPP), polyethylene terephthalate (PET), oriented polyamide (OPA), unoriented polypropylene (CPP), linear low-density polyethylene (LLDPE), and low-density polyethylene (LDPE).

[0042] The base material 10 may be, for example, a composite film in which a metal foil is laminated onto a flexible base material, or a vapor-deposited film in which metal or the like is vapor-deposited onto a flexible base material. The metal or the like may be, for example, a pure metal such as aluminum or a metal oxide such as aluminum oxide. From the viewpoint of improving gas barrier properties, the base material 10 may be a vapor-deposited film (transparent vapor-deposited film) in which aluminum or aluminum oxide is vapor-deposited onto a PET film. The thickness of the base material 10 may be, for example, 7 to 150 μm, 15 to 90 μm, or 20 to 80 μm.

[0043] Examples of sealant layers 20 include CPP film, LLDPE film, and OPP film. The thickness of the sealant layer 20 may be the same as or different from the thickness of the substrate 10, for example, 7 to 150 μm, 15 to 90 μm, or 20 to 80 μm.

[0044] The primer layer 40 may contain a resin. Examples of resins include polyvinyl alcohol resin, cellulose resin, polyester, polyamine, polyethyleneimine resin, polyamide resin, polyurethane, polyacrylic polymer hydroxyl-containing resin, carboxyl group-containing resin, and amine polymer. By providing the primer layer 40 on the substrate to be printed, printing of the electrostatic ink composition using a digital printing press can be performed smoothly. The amount of resin constituting the primer layer 40 is, for example, 0.01 to 1.5 g / m². 2 , or 0.05~1.0g / m 2 That's fine.

[0045] The laminate 302 has printed sections 52 on the main surface (printing surface) of the primer layer 40 opposite to the substrate 10. An electrostatic ink layer 50 composed of multiple printed sections 52 is provided on the printing surface. The electrostatic ink layer 50 is composed of an electrostatic ink composition and is provided by electrostatic printing using a digital printing press. In Figure 5, the multiple printed sections 52 may have the same composition or may have different compositions to have different colors. The printed sections 52 may be provided scattered on the primer layer 40 or may be provided to cover the entire surface of one side of the primer layer 40.

[0046] The printed area 52 in the electrostatic ink layer 50 is composed of circular halftone dots of the electrostatic ink composition. In other words, even though it appears uniform in a single color, there are plain areas between the halftone dots. When printing a predetermined area to be printed in a single color, the electrostatic ink layer 50 is generally configured such that the circular halftone dots are spaced apart from each other, and when printing in two or more colors, the circular halftone dots of the second and subsequent electrostatic ink compositions are arranged between the halftone dots printed in the first color or partially overlapping the halftone dots printed in the first color. The density of the color on the printed surface can be adjusted by changing the size of the halftone dots, and the color tone on the printed surface can also be adjusted by arranging halftone dots of different colors.

[0047] The ink coverage rate of each printed section 52 constituting the electrostatic ink layer 50 is 500% or less, but may be, for example, 450% or less, or 400% or less. By setting the ink coverage rate of the printed section 52 within the above range, the laminate strength of the laminate is improved, printing using multiple inks is possible, and it can accommodate a variety of printing methods. The lower limit of the ink coverage rate of the printed section 52 is not particularly limited, but may be, for example, 20% or more, 50% or more, 80% or more, or 100% or more. The ink coverage rate of the printed section 52 may be adjusted within the above range, for example, 20-500%, 50-400%, 100-400%, or 100-300%.

[0048] In this specification, ink coverage refers to the ratio of halftone dot area per unit area. It is defined as 100% ink coverage when a predetermined area to be printed is uniformly printed with a single color, and 0% ink coverage for areas that are not printed. When printing with multiple ink colors, the ink coverage is calculated for each color, and the sum of these values ​​represents the ink coverage of the target printed area and electrostatic ink layer. Ink coverage is set on the digital printing press and can be adjusted by specifying the desired value in the ink coverage setting. For example, HP's "Indigo20000 Digital Printing Press for Labels and Packaging" (product name) can be used as a digital printing press. Furthermore, the ink coverage of the electrostatic ink layer on the target laminate can also be confirmed by optical microscope observation of the printed surface of the container or laminate.

[0049] Furthermore, since the printed portion 52 is composed of circular halftone dots of the electrostatic ink composition, even when the ink coverage rate is 100%, the main surface of the primer layer 40 can be confirmed by observing the surface of the electrostatic ink layer 50 on the sealant layer 20 side with an optical microscope or the like. In other words, even with an ink coverage rate of 100%, the primer layer 40 and the adhesive layer 30 can be directly bonded. On the other hand, as the ink coverage rate increases, the proportion of the primer layer 40 at the bonding surface (interface) between the printed portion 52 and the adhesive layer 30 tends to decrease. When using conventional adhesives, as the ink coverage rate increases, the adhesive strength at the interface between the electrostatic ink layer and the primer layer, or between the electrostatic ink layer and the adhesive layer, decreases, and the laminate strength of the laminate may not be as expected. On the other hand, in the laminate according to this disclosure, sufficient laminate strength can be achieved even with a high ink coverage rate by using the adhesive composition described later. In the laminate according to this disclosure, by using the adhesive composition described later, expansion of the laminate 300, especially during heat treatment, can be prevented.

[0050] The amount of ink applied to the main surface (printing surface) of the primer layer 40 on the sealant layer 20 side is, for example, 0.5 g / m². 2More than 1.0g / m 2 More than 2.0g / m 2 Above, or 3.0 g / m² 2 The above amounts are acceptable. By keeping the above ink application amount within the above range, a variety of printed expressions composed of multiple colors can be obtained. For example, the ink application amount on the main surface of the primer layer 40 on the sealant layer 20 side is 8.0 g / m². 2 The following, or 6.0 g / m 2 The following is acceptable. By keeping the above ink application amount within the above range, the decrease in adhesive strength at the interface between the electrostatic ink layer 50 and the primer layer 40, or at the interface between the electrostatic ink layer 50 and the adhesive layer 30, can be more sufficiently suppressed. In this specification, the ink application amount means the total amount (solid content) of the ink composition used for printing, and in the case of multi-color printing, it means the sum of those amounts.

[0051] Figure 6 is a cross-sectional view showing another example of a laminate. Laminate 304 in Figure 6 differs from laminate 302 in Figure 5 in that the entire surface of one side of the primer layer 40 is covered with the electrostatic ink layer 51 (printed portion 52 formed over the entire printed surface). That is, in laminate 304, the coverage ratio of the main surface of the primer layer 40 by the electrostatic ink layer 51 is 100 area. By using the adhesive composition described later, even in a configuration like laminate 304 where it is difficult to secure a sufficient direct bonding area between the primer layer 40 and the adhesive layer 30, sufficient adhesive strength is achieved and interlayer delamination in laminate 304 is suppressed.

[0052] In laminates 302 and 304, the electrostatic ink compositions constituting the electrostatic ink layers 50 and 51 are ink compositions used in liquid electrophotographic printing, i.e., electrostatic printing, and are printed on substrates such as paper and plastic, or on a primer layer. The electrostatic ink compositions may contain colorants such as pigments and dyes, and resins. The electrostatic ink compositions may further contain a carrier fluid or carrier liquid. The electrostatic ink compositions may contain, for example, a charge director, a charge adjuvant, a surfactant, a viscosity modifier, an emulsifier, and other additives.

[0053] Examples of colorants include cyan pigment, magenta pigment, yellow pigment, and black pigment. From the viewpoint of facilitating digital printing, a resin with a relatively low melting point can be used. A relatively low melting point means, for example, 100°C or lower. Examples of resins include thermoplastic resins such as ethylene acrylic acid copolymer, propylene acrylic acid copolymer, ethylene methacrylic acid copolymer, propylene methacrylic acid copolymer, and ethylene vinyl acetate copolymer. Preferably, the resin contains at least one of ethylene acrylic acid copolymer and ethylene methacrylic acid copolymer.

[0054] Examples of carrier fluids and carrier liquids include hydrocarbons, silicone oils, and vegetable oils. Examples of hydrocarbons include aliphatic hydrocarbons, branched-chain aliphatic hydrocarbons, and aromatic hydrocarbons. The electrostatic ink composition may be substantially free of carrier fluids and carrier liquids when printed on a substrate. The carrier fluids and carrier liquids may be removed, for example, by an electrophoretic process during printing or by evaporation. By the above removal operation, substantially only the solid components are transferred onto the substrate or primer layer.

[0055] A charge director has the function of maintaining a sufficient electrostatic charge on the particles contained in the electrostatic ink composition. Examples of charge directors include ionic compounds such as metal salts of fatty acids, metal salts of sulfosuccinates, metal salts of oxyphosphates, metal salts of alkylbenzenesulfonic acids, metal salts of aromatic carboxylic acids, and metal salts of aromatic sulfonic acids, as well as dual ionic and nonionic compounds such as polyoxyethylene-derived alkylamines, lecithin, polyvinylpyrrolidone, and organic acid esters of polyhydric alcohols.

[0056] Charge adjuvants have the effect of increasing or stabilizing the charge of particles contained in the electrostatic ink composition. Examples of charge adjuvants include barium petrolate, calcium petrolate, cobalt naphthenate, calcium naphthenate, copper naphthenate, manganese naphthenate, nickel naphthenate, zinc naphthenate, iron naphthenate, barium stearate, cobalt stearate, pearl stearate, zinc stearate, aluminum stearate, copper stearate, iron stearate, and metal carboxylates.

[0057] The electrostatic ink layers 50 and 51 may contain a crosslinked material formed by a component contained in at least one of the adhesive layer 30 and the primer layer 40. By including a crosslinked material, the strength of the electrostatic ink layers 50 and 51 themselves, as well as the adhesive strength between the printed surface of the primer layer 40 and the electrostatic ink layer 50, and the adhesive strength between the electrostatic ink layer 50 and the adhesive layer 30 can be further improved.

[0058] The printed portion 52 of the electrostatic ink composition and the adhesive layer 30 are bonded to each other. That is, the printed portion 52 serves as the bonding surface with the adhesive layer 30, and the electrostatic ink composition and the adhesive composition are in direct contact.

[0059] The adhesive composition contains an epoxy compound. The epoxy compound reacts with the components constituting the electrostatic ink composition, the adhesive layer, and the primer layer and hardens, thereby firmly bonding the printed surfaces of the adhesive layer and the primer layer. The epoxy compound may harden itself to form a cured product. The adhesive composition may further contain at least one selected from the group consisting of polyols and polyisocyanates, or it may further contain a polyol, or it may further contain a polyisocyanate, or it may further contain a polyol and a polyisocyanate. The adhesive composition may contain a polyol, a polyisocyanate, and an epoxy compound. At least a portion of these three components (polyol, polyisocyanate, and epoxy compound) may react with each other and harden to form a cured product. That is, the adhesive composition may consist of at least one of an adhesive composition containing a polyol, a polyisocyanate, and an epoxy compound and its cured product, and the adhesive layer 30 may consist of the adhesive composition, its cured product, or a mixture thereof. Polyols and polyisocyanates react as the main agent and curing agent, respectively, to produce polyurethane (polyurethane adhesive).

[0060] The epoxy compound may be a compound having one or more epoxy groups in one molecule. From the viewpoint of further increasing the adhesive strength of the adhesive layer 30 in a high-temperature environment, it may have epoxy groups at both ends. Examples of epoxy compounds include glycidyl ether type epoxy compounds, glycidylamine type epoxy compounds, glycidyl ester type epoxy compounds, and alicyclic epoxy compounds (cyclic aliphatic epoxy compounds).

[0061] The epoxy compound in the adhesive composition can penetrate layers adjacent to the adhesive layer (e.g., primer layer, electrostatic ink layer, and sealant layer). This penetration can further improve the adhesion between each layer after the epoxy compound has cured. In this case, the primer layer, electrostatic ink layer, and sealant layer each contain at least one of the epoxy compound and its cured product (e.g., epoxy resin). The molecular weight of the epoxy compound may be, for example, 500 or less, 450 or less, or 400 or less. Having the molecular weight of the epoxy compound within the above range allows the epoxy compound to penetrate more sufficiently into the electrostatic ink composition constituting the electrostatic ink layer. The lower limit of the molecular weight of the epoxy compound may be, for example, 98 or more.

[0062] Examples of alicyclic epoxy compounds include epoxycyclohexylmethyl-epoxycyclohexanecarboxylate and bis(epoxycyclohexyl)adipate.

[0063] Examples of monofunctional alicyclic epoxy compounds having one epoxy group per molecule include 3,4-epoxycyclohexylmethyl methacrylate and 1,2-epoxy-4-vinylcyclohexane. Examples of bifunctional epoxy compounds having two epoxy groups per molecule include 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexane carboxylate, bis(3,4-epoxycyclohexylmethyl) adipate, and 4-vinylcyclohexene dioxide. Furthermore, an example of an epoxy compound having one or more epoxy groups per molecule is the 1,2-epoxy-4-(2-oxyranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, represented by the following general formula (I).

[0064] [ka]

[0065] In the general formula (I) above, n may be an integer between 1 and 4.

[0066] The epoxy compound preferably contains a bifunctional alicyclic epoxy compound. Being bifunctional increases the number of crosslinking points with the electrostatic ink composition and the primer resin, promoting the curing reaction of the adhesive and making it easier to cure. Furthermore, if the adhesive composition further contains polyisocyanate, the alicyclic nature of the epoxy compound can suppress the reaction with the polyisocyanate due to steric hindrance. As a result, it is possible to achieve stable curing and sufficiently excellent adhesion at the interface between the printed portion 52 and the adhesive layer 30.

[0067] A polyol may have two or more hydroxyl groups in one molecule, and for example, its number-average molecular weight may be 400 or more. The number-average molecular weight of a polyol may be 10,000 or less.

[0068] The polyol may contain at least one selected from the group consisting of, for example, polyester polyols and polyether polyols. Of these, from the viewpoint of sufficiently increasing the adhesive strength of the adhesive layer 30 in a high-temperature environment, the polyol may include polyester polyols or aliphatic polyester polyols.

[0069] Polyester polyols can be obtained, for example, by condensation reactions or transesterification reactions between a polyhydric alcohol and a polybasic acid, an alkyl ester of a polybasic acid, an acid anhydride of a polybasic acid, or an acid halide of a polybasic acid.

[0070] Examples of polyhydric alcohols include low molecular weight diols, low molecular weight triols, and low molecular weight polyols having four or more hydroxyl groups.

[0071] Examples of low molecular weight diols include ethylene glycol, propylene glycol, trimethylene glycol, 1,4-butylene glycol, 1,3-butylene glycol, 1,2-butylene glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 2,2-dimethyl-1,3-propanediol, neopentyl glycol, 1,6-hexanediol, 2,2-diethyl-1,3-propanediol, 3,3-dimethylolheptane, and 2-ethyl-2-butyl-1,3-propanediol.

[0072] Examples of low molecular weight triols include glycerin, 2-methyl-2-hydroxymethyl-1,3-propanediol, 2,4-dihydroxy-3-hydroxymethylpentane, 1,2,6-hexanetriol, trimethylolethane, trimethylolpropane, 2-methyl-2-hydroxymethyl-1,3-propanediol, 2,4-dihydroxy-3-(hydroxymethyl)pentane, and 2,2-bis(hydroxymethyl)-3-butanol.

[0073] Examples of low molecular weight polyols having four or more hydroxyl groups include tetramethylolmethane, pentaerythritol, dipentaerythritol, D-sorbitol, xylitol, D-mannitol, and D-mannitol.

[0074] Examples of alkyl esters of polybasic acids include methyl esters and ethyl esters of polybasic acids. Examples of acid anhydrides of polybasic acids include acid anhydrides derived from polybasic acids. More specifically, examples of acid anhydrides of polybasic acids include oxalic anhydride, succinic anhydride, maleic anhydride, phthalic anhydride, 2-alkyl (12-18 carbon atoms) succinic anhydride, tetrahydrophthalic anhydride, and trimellitic anhydride.

[0075] Examples of polybasic acid halides include the alkyl esters of the polybasic acids mentioned above, or acid halides derived from the acid anhydrides of polybasic acids. More specifically, examples of polybasic acid halides include oxalic acid dichloride, adipic acid dichloride, and sebatic acid dichloride.

[0076] Examples of polyether polyols include polyalkylene oxides. Polyether polyols may be obtained, for example, by adding an alkylene oxide such as ethylene oxide and / or propylene oxide to a low molecular weight polyol as an initiator. More specifically, examples of polyether polyols include polyethylene glycol, polypropylene glycol, and polyethylene-polypropylene glycol (random or block copolymer). Other examples of polyether polyols include polytetramethylene ether glycol obtained by ring-opening polymerization of tetrahydrofuran.

[0077] Polyisocyanates have two or more isocyanate groups in a single molecule. Examples of polyisocyanates include polyisocyanate monomers, polyisocyanate derivatives, and isocyanate-terminated prepolymers. The adhesive composition may contain multiple different types of polyisocyanates. The molar ratio (NCO / OH) of isocyanate groups in the polyisocyanate to the hydroxyl groups in the polyol may be, for example, 0.5 to 10. Such an adhesive composition can form a cured product that has high adhesive strength while exhibiting excellent flexibility.

[0078] Examples of polyisocyanate monomers include aliphatic polyisocyanates, aromatic polyisocyanates, aromatic aliphatic polyisocyanates, and alicyclic polyisocyanates.

[0079] Examples of aliphatic polyisocyanates include trimethylene diisocyanate, 1,2-propylene diisocyanate, butylene diisocyanate (tetramethylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate), 1,5-pentamethylene diisocyanate (PDI), hexamethylene diisocyanate (HDI), 2,4,4-trimethylhexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and 2,6-diisocyanate methyl capeate.

[0080] Examples of aromatic aliphatic polyisocyanates include xylylene diisocyanate derivatives. Examples of xylylene diisocyanate derivatives include xylylene diisocyanate (1,3-xylylene diisocyanate or 1,4-xylylene diisocyanate) (XDI), tetramethyl xylylene diisocyanate (1,3-tetramethyl xylylene diisocyanate or 1,4-tetramethyl xylylene diisocyanate) (TMXDI), ω,ω'-diisocyanate-1,4-diethylbenzene, and polyol-modified xylylene diisocyanates obtained by the reaction of xylylene diisocyanate with trimethylolpropane.

[0081] The content of xylylene diisocyanate derivative relative to the total polyisocyanate may be, for example, 10% by mass or more, 20% by mass or more, 30% by mass or more, or 40% by mass or more, from the viewpoint of improving reactivity with the main component (e.g., polyol). By setting the content of xylylene diisocyanate derivative relative to the total polyisocyanate to 30% by mass or more, the reactivity can be further increased.

[0082] Examples of alicyclic polyisocyanates include 1,3-cyclopentane diisocyanate, 1,3-cyclopentene diisocyanate, cyclohexane diisocyanate (1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate), 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (isoholodiisocyanate) (IPDI), methylcyclohexane diisocyanate (methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate), and norbornane diisocyanate (NBDI).

[0083] Examples of polyisocyanate derivatives include polymers of the polyisocyanate monomers mentioned above, allophanate-modified derivatives, polyol-modified derivatives, polyol-modified derivatives produced by the reaction of monomers with alcohols, biuret-modified derivatives, urea-modified derivatives, oxadiazinetrione-modified derivatives, carbodiimide-modified derivatives, uretdione-modified derivatives, and uretonimine-modified derivatives.

[0084] An isocyanate-terminated prepolymer is a urethane prepolymer having at least two isocyanate groups at its molecular ends. An isocyanate-terminated prepolymer can be obtained by urethane-forming a polyol with at least one selected from the group consisting of polyisocyanate monomers, polyisocyanate derivatives, and isocyanate-terminated prepolymers. In this case, the molar ratio (NCO / OH) of isocyanate groups contained in the polyisocyanate to the hydroxyl groups of the polyol may be, for example, 0.5 or more, 0.6 or more, 0.8 or more, 1 or more, or 1.5 or more. The above molar ratio (NCO / OH) may also be 10 or less, 5 or less, 4 or less, or 3 or less. Examples of numerical ranges for the molar ratio (NCO / OH) include, for example, 0.5 to 10, 0.5 to 5, 0.8 to 4, and 0.6 to 3.

[0085] In the adhesive composition, the content of the epoxy compound per 100 parts by mass of polyol may be, for example, 3 to 25 parts by mass, 6 to 25 parts by mass, or 8 to 20 parts by mass, from the viewpoint of achieving both high adhesive strength and excellent shear suppression. If the content of the epoxy compound is too high, the excellent shear suppression tends to be impaired. That is, when the adhesive layer 30 is formed, the adhesive surface may shift or the adhesive composition may overflow. If the amount of epoxy compound is too low, the adhesive strength under high-temperature hot water treatment conditions tends to decrease.

[0086] In the adhesive composition, the amount of polyisocyanate per 100 parts by mass of polyol may be, for example, 10 to 50 parts by mass, 15 to 35 parts by mass, or 20 to 30 parts by mass, from the viewpoint of sufficiently increasing the seal strength and adhesive strength under high-temperature hot water treatment conditions.

[0087] The molar ratio of epoxy groups in the epoxy compound to isocyanate groups in the polyisocyanate may be, for example, 0.5 to 10, 1.5 to 9, or 2.0 to 6.5. This allows for maintaining a sufficiently high adhesive strength under high-temperature hot water treatment conditions.

[0088] The adhesive composition constituting the adhesive layer 30 may contain optional components such as additives in addition to the components described above. Examples of additives include antioxidants, ultraviolet absorbers, light stabilizers, fillers, silane coupling agents, epoxy resins, catalysts, coating properties improvers, leveling agents, nucleating agents, lubricants, mold release agents, defoamers, plasticizers, surfactants, pigments, dyes, organic fine particles, inorganic fine particles, antifungal agents, and flame retardants. The adhesive composition may contain solvents such as organic solvents.

[0089] The adhesive composition adheres the printed portion 52, on which the electrostatic ink composition is printed, to the sealant layer 20. An arbitrary layer may be provided between the adhesive layer 30 and the sealant layer 20. The laminates 302 and 304 may further have, for example, a barrier layer between the adhesive layer 30 and the sealant layer 20. In this case, the adhesive composition adheres the printed portion 52 to the arbitrary layer (e.g., a barrier layer). If the adhesive composition contains a polyol and a polyisocyanate, the polyol and polyisocyanate react to form a urethane bond, allowing the adhesive to function more fully. Even in the presence of an epoxy compound, the formation of the urethane bond proceeds smoothly, allowing the printed portion 52 to be bonded to the sealant layer 20 or any other layer with a sufficiently high adhesive strength.

[0090] The adhesive composition may also have the function of crosslinking the electrostatic ink composition that forms the electrostatic ink layers 50 and 51 along with the formation of urethane bonds. This can further improve the adhesive strength between the printed surface and the sealant layer 20 or any other layer.

[0091] When the coverage ratio of the primer layer 40 by the electrostatic ink layer 50 on the main surface (printed surface) is high, or when the ink coverage rate in the printed area 52 (electrostatic ink layers 50, 51) is high, the adhesive strength between the electrostatic ink layer 50 and the adhesive layer 30 generally tends to decrease. However, in the case of the adhesive composition described above, sufficient adhesive strength can be achieved. Furthermore, when the coverage ratio of the primer layer 40 by the electrostatic ink layer 50 on the main surface, or the ink coverage rate in the printed area 52 (electrostatic ink layers 50, 51) is high, the epoxy compound content in the adhesive composition can be increased accordingly, allowing the epoxy compound to sufficiently penetrate the electrostatic ink layers 50, 51 composed of the electrostatic ink composition, thereby further suppressing the decrease in adhesive strength. The penetrated epoxy compound has the effect of increasing the strength of the electrostatic ink composition (electrostatic ink layers 50, 51) by crosslinking the electrostatic ink composition. For this reason, even when the ink coverage rate in the printed area 52 is high and heat treatment such as retort heat treatment is applied, the decrease in adhesive strength can be sufficiently suppressed.

[0092] The adhesive composition maintains high adhesive strength even after heat treatment while also exhibiting excellent pot life. Therefore, it offers excellent workability for coating and lamination processes when bonding a printed surface to a substrate. The adhesive composition may contain an epoxy compound, and may also contain a polyol and polyisocyanate that form a urethane, along with the epoxy compound. At least a portion of these may harden to form an adhesive layer. This reduces the number of layers constituting the laminate 300 compared to providing separate adhesive layers containing only polyurethane and epoxy coating layers. Therefore, for example, when manufacturing a laminate using a roll-to-roll method, meandering of the roll after aging and the occurrence of wrinkles due to blocking can be suppressed. Furthermore, the aging process after coating can be reduced, improving manufacturing efficiency.

[0093] In laminates 302 and 304 where the electrostatic ink layers 50 and 51 on the printed surface are in direct contact with the adhesive layer 30, the epoxy compound contained in the adhesive composition, and in some cases components such as the epoxy compound and / or polyisocyanate, penetrates sufficiently into the electrostatic ink layers 50 and 51. This crosslinks the electrostatic ink composition constituting the electrostatic ink layers 50 and 51, improving the strength of the electrostatic ink composition (electrostatic ink layers 50 and 51). It also improves the adhesive strength between each layer. Furthermore, even when the printed surface includes blank areas (transparent areas) where there is no electrostatic ink layer 50, as shown in Figure 5, the epoxy compound is contained in the adhesive layer, thus eliminating stickiness. On the other hand, if an epoxy coating layer is provided separately from the adhesive layer 30, when the printed surface includes blank areas, the epoxy compound becomes excessive near the blank areas, making stickiness more likely to occur. Thus, the laminate 300 can bond the printed surface, including blank areas where the printed portion 52 is not formed, with high adhesive strength while eliminating stickiness.

[0094] As described above, laminates 302 and 304 can ensure sufficient adhesive strength between the electrostatic ink layers 50 and 51 and the substrate 10, primer layer 40, and adhesive layer 30. Therefore, a container can be constructed in which delamination between the electrostatic ink layers 50 and 51 and the substrate 10, primer layer 40, and adhesive layer 30 is suppressed even in the bent portion 60. In such a container, the adhesive state between each layer is maintained even in the bent portion 60, which suppresses the occurrence of misalignment of the printed surface, and the printed information on the body portion 200, including the bent portion 60, can be maintained in the initial state after printing. Even during the use of the container, for example, even if a new bend is created due to the container bending, the adhesive state between each layer is maintained, so that the function of the container (e.g., barrier properties) can be maintained throughout the period of use. Similarly, the tearing of the container itself and deterioration of the printed information can be suppressed throughout the period of use. In such containers, even when the curved portion has a printed surface, the occurrence of delamination between layers is suppressed, making the information printed on the surface legible. This makes them useful as containers for food and beverages and hygiene products where appearance is important. However, the uses are not limited to these. For example, because it exhibits excellent adhesive strength and seal strength even after high-temperature hot water treatment and retort heat treatment, it may be used as a material for retort containers, microwave-safe containers, and boiling containers.

[0095] In the modified laminate, a primer layer 40 may be provided on each of the opposing surfaces of the substrate 10 and the sealant layer 20. Furthermore, from the viewpoint of improving the gas barrier and water vapor barrier properties of the laminates 302, 304, at least one of a metal layer such as aluminum foil and a resin layer such as nylon film may be provided between the substrate 10 and the primer layer 40, and / or between the sealant layer 20 and the adhesive layer 30.

[0096] Specific examples of the layered structure of the laminate are shown below. In each example, the left end corresponds to the base material 10 and the right end to the sealant layer 20, and it means that each layer is laminated in order from left to right. The first adhesive layer is adhesive layer 30, and the second and third adhesive layers may be conventional adhesive layers.

[0097] (1) Transparent vapor-deposited PET film / primer layer / electrostatic ink layer / first adhesive layer / nylon layer / second adhesive layer / CPP film (unstretched polypropylene film) (2) PET film / primer layer / electrostatic ink layer / first adhesive layer / aluminum layer / second adhesive layer / nylon layer / third adhesive layer / CPP film (unoriented polypropylene film) (3) PET film / primer layer / electrostatic ink layer / first adhesive layer / nylon layer / second adhesive layer / CPP film (unoriented polypropylene film) (4) PET film / primer layer / electrostatic ink layer / first adhesive layer / aluminum layer / second adhesive layer / polyethylene film

[0098] In each of the above specific examples, any layer may be provided at any position between the first adhesive layer and the sealant layer 20. (1) and (2) are preferably used as laminates for retort packaging, (3) as a laminate for microwave packaging, and (4) as a laminate containing supplements or face masks. However, the applications are not limited to those described above.

[0099] The laminate described above can be prepared, for example, by the following method. One embodiment of the method for manufacturing the laminate is described below. In one example of the method for manufacturing the laminate, the laminate 302 shown in Figure 5 is manufactured. The method includes the steps of first forming a primer layer 40 on one side of a film-like substrate 10, printing an electrostatic ink composition onto the primer layer 40 to form an electrostatic ink layer 50 composed of printed parts 52, and bonding the electrostatic ink layer 50 and one side of the sealant layer 20 using the specific adhesive composition described above.

[0100] The primer layer 40 may be formed on one surface of the substrate 10 by flexographic printing or gravure printing, etc. The primer layer 40 may also be formed by crosslinking the resin raw material with a crosslinking agent. Crosslinking may be performed by irradiation with ultraviolet light, heating, ionizing radiation such as an electron beam, and non-ionizing radiation such as microwave radiation.

[0101] The electrostatic ink composition can be printed using electrostatic printing with a digital printing press.

[0102] Bonding of the electrostatic ink layer 50 and one side of the sealant layer 20 with an adhesive composition can be performed by lamination. Lamination can be performed using any apparatus. The epoxy compound contained in the adhesive composition may, optionally, penetrate the electrostatic ink composition and / or polyisocyanate that constitute the electrostatic ink layer 50 and the primer layer 40, and crosslink with the components contained in the electrostatic ink composition and the primer layer 40. This improves the strength of the electrostatic ink layer 50 and allows for the production of a laminate 300 in which the interfaces of each layer are sufficiently bonded. During lamination, at least a portion of the adhesive composition may harden and become a cured product. In this way, a laminate 302 comprising the base material 10, primer layer 40, electrostatic ink layer 50, adhesive layer 30, and sealant layer 20 in this order can be produced. Laminate 304 and laminates according to modified examples can be produced in the same manner as laminate 302.

[0103] The laminates 302 and 304 manufactured in this manner have the configuration and properties as described in these embodiments. The descriptions of the laminates 302 and 304 and their modified forms also apply to the description of the embodiments of the manufacturing method described above.

[0104] [Heating packaging bag] Figure 7 is a plan view showing an example of a packaging bag 120 (heat-resistant packaging bag) according to one embodiment. As shown in Figure 7, the packaging bag 120 is composed of a laminate 300 having a base material, a primer layer, an electrostatic ink layer, an adhesive layer, and a sealant layer in that order. The structure of the laminate 300 will be described later. The packaging bag 120 may be, for example, a bag that is sealed while containing the packaged item, such as food or beverages. The packaging bag 120 may or may not have a bent portion.

[0105] Furthermore, packaging bag 120 is a packaging bag for heating. A packaging bag for heating is a packaging bag intended to be heated while containing the packaged items. Heat treatments include "retort heat treatment," "boil heat treatment," and "microwave heating treatment." Retort heat treatment is a process in which the contents are heated under pressure at a temperature of 100°C or higher, and a steam method may be used, for example. Boil heat treatment is a process in which the packaging bag is heated in heated water (hot water), and is heated to a temperature of up to 100°C. Microwave heating treatment is a heating process using a microwave oven, which generates heat in water-containing substances by vibrating and rotating water molecules with electromagnetic waves (microwaves). All of these treatments are often performed for the purpose of sterilizing the packaging bag or the packaged items.

[0106] The packaging bag 120 is constructed by bonding the sealant layers of a pair of laminates 300 together. The packaging bag 120 comprises a sealed portion 101 formed by bonding (sealing) the periphery of a pair of substantially rectangular, film-like laminates 300, and a storage portion 124 formed between the pair of laminates 300 by the sealed portion 101. The sealed portion 101 is formed at a pair of side ends, a bottom end, and a top end of the rectangular packaging bag 120. Thus, in a plan view, the packaging bag 120 has a sealed portion 101 formed around the entire circumference of each of the pair of laminates 300 with their sealant layers overlapping. The storage portion 124 can contain, for example, the packaged goods (e.g., food and beverages). In the following embodiments, the sealed package containing the packaged goods may be specifically referred to as the packaging body 400. The sealed portion 101 at the bottom end may be sealed after the packaged goods have been filled into the storage portion 124. The seal portion 101 is formed by heat-sealing the sealant layers of the laminate 300 together.

[0107] Furthermore, it is not necessary for the pair of laminates 300 constituting the packaging bag 120 to have the same layer configuration; for example, the pair of laminates may have different layer configurations.

[0108] The packaging bag 120 may be provided with an opening means 140 for easy opening. The opening means 140 has a pair of easy-open sections 144 consisting of V-shaped notches formed in the seal portion 101 at the side end, and a half-cut line 141 between the pair of easy-open sections 144 that serves as a cutting trajectory. The half-cut line 141 can be formed, for example, using a laser. The easy-open sections 144 are not limited to V-shaped notches, but may be U-shaped or I-shaped notches, or a group of scratches.

[0109] The procedure for manufacturing a packaging bag 120 and a packaging body 400 using a laminate 300 is described below. A pair of laminates 300 molded into a predetermined shape are prepared. The sealant layers provided on one side of each laminate 300 are placed facing each other and the sealant layers are bonded together. At this time, a seal portion 101 is formed on a pair of side ends and on the lower end (or upper end), so that a seal portion 101 is formed in which three of the four sides are closed, and an unsealed portion is formed on the inside. As a result, a packaging bag 130 is obtained in which only the upper end (or only the lower end) is not sealed, as shown in Figure 8.

[0110] Next, the contents to be packaged are filled into the storage section 132 of the packaging bag 130 from the unsealed upper (or lower) end. Then, the sealant layers of the laminate 300 are bonded together at the unsealed upper (or lower) end to form a sealed section 101 at the upper (or lower) end. As a result, a package 400 comprising the packaging bag 120 and the contents to be packaged can be manufactured.

[0111] As described above, the packaging bag 120 is a packaging bag that can be used when it is expected that the packaged goods will be heated, i.e., when the packaged goods will be heated as a whole 400. Due to the heat treatment described above, the packaging bag 120 itself will be heated, so heat resistance is required. In addition, in all heat treatments, water molecules are present in the surrounding environment at high temperatures, so water resistance at high temperatures is required. Furthermore, since the packaging bag 120 is heat-treated with the goods inside, the seal portion 101 is considered to be particularly susceptible to the effects of the heat treatment. To meet these requirements, the packaging bag 120 improves the water resistance and heat resistance of the laminate by constructing each layer constituting the laminate 300 with a combination of specific materials. In addition, the packaging bag 120 prevents damage to the packaging bag 120, especially at the seal portion 101, by ensuring that a part of the composition of the laminate 300 at the seal portion 101 meets specific conditions.

[0112] Next, the laminate 300 that constitutes the packaging bag 120 can use the laminates 302 and 304 described as the constituent materials of the above-mentioned container, and the description can be applied unless otherwise specified. For example, materials and the like constituting each layer can use the materials and the like exemplified in the description of the corresponding layer in the description regarding the above-mentioned container. Hereinafter, an example using the above-mentioned laminate 302 as the laminate 300 will be described.

[0113] The primer layer 40 may contain a resin. When the packaging bag 120 is used for heating, the resin preferably contains a polyethyleneimine resin. In addition to the polyethyleneimine resin, the primer layer 40 may further contain, for example, a polyvinyl alcohol resin, a cellulose-based resin, a polyester, a polyamine, a polyamide resin, a polyurethane, a polyacrylic polymer hydroxyl group-containing resin, a carboxyl group-containing resin, and an amine-based polymer. By providing the primer layer 40 containing a polyethyleneimine resin on the substrate to be printed, the water resistance is improved, and the laminate 302 suitable for heat treatment can be produced. The content of the polyethyleneimine resin in the primer layer 40 may be 80% by mass or more, 90% by mass or more, or 97% by mass or more. The coating amount of the resin constituting the primer layer 40 is, for example, 0.01 to 1.5 g / m 2 or 0.05 to 1.0 g / m 2 and may be.

[0114] The laminate 302 includes a printing portion 52 on one main surface (printing surface) closer to the sealant layer 20 among the pair of main surfaces of the primer layer 40. An electrostatic ink layer 50 is provided on the printing surface. The electrostatic ink layer 50 is composed of an electrostatic ink composition and is provided by electrostatic printing using a digital printing machine. The plurality of printing portions 52 in FIG. 5 may have the same composition or may have different colors by having different compositions from each other. The electrostatic ink layer 50 may be composed of the printing portions 52 provided so as to be scattered on the primer layer 40, or may be composed of the printing portions 52 provided so as to cover the entire one surface of the primer layer 40.

[0115] When the packaging bag 120 is used for heating, the ink coverage of each printed section 52 constituting the electrostatic ink layer 50 may be 100 to 400%. By setting the ink coverage of the printed section 52 within the above range, the laminate strength of the laminate is excellent, printing with multiple inks is possible, and it can accommodate a variety of printing methods.

[0116] As described above, the laminate 300 (302, 304) can ensure sufficient adhesive strength between the electrostatic ink layers 50, 51 and the substrate 10, primer layer 40, and adhesive layer 30. Therefore, when the laminate 300 is used as a heat-treated packaging bag and heat treatment is performed, delamination between the electrostatic ink layers 50, 51 and the substrate 10, primer layer 40, and adhesive layer 30 is suppressed.

[0117] When the packaging bag 120 is used for heating, specific examples of the layered structure of the laminate are shown below. In each example, the left end corresponds to the base material 10 and the right end to the sealant layer 20, and it means that each layer is laminated in order from left to right. The first adhesive layer is the adhesive layer 30, and the second and third adhesive layers may be conventional adhesive layers.

[0118] (5) Transparent vapor-deposited PET film / primer layer / electrostatic ink layer / first adhesive layer / nylon layer / second adhesive layer / CPP film (unoriented polypropylene film) (6) PET film / primer layer / electrostatic ink layer / first adhesive layer / aluminum layer / second adhesive layer / nylon layer / third adhesive layer / CPP film (unstretched polypropylene film) (7) Nylon layer / Primer layer / Electrostatic ink layer / First adhesive layer / LLDPE (Linear low-density polyethylene) film (8) PET film / primer layer / electrostatic ink layer / first adhesive layer / nylon layer / second adhesive layer / CPP film

[0119] In each of the above specific examples, any layer may be provided at any position between the first adhesive layer and the sealant layer 20. (5) and (6) above are mainly used for packaging bags that are expected to undergo retort heat treatment, (7) is mainly used for packaging bags that are expected to undergo boil heat treatment, and (8) is mainly used for packaging bags that are expected to undergo microwave heating treatment. However, the applications are not limited to those described above.

[0120] The laminate described above can be prepared based on the same manufacturing method as the laminate used as a component material for the container described above.

[0121] [Effect] As described in the above embodiment, the packaging bag 120 (heat-resistant packaging bag) according to this embodiment is composed of a laminate 300 in which a base material 10, a primer layer 40, an adhesive layer 30, and a sealant layer 20 are laminated in this order. The adhesive layer 30 contains at least one of an adhesive composition containing an epoxy compound and a cured product of the adhesive composition. Furthermore, from the viewpoint of improving water resistance, the primer layer 40 may contain polyethyleneimine resin.

[0122] Electrostatic ink compositions produced by digital printing presses tend to have inferior heat resistance and strength compared to other inks. Therefore, when attempting to apply a laminate containing an electrostatic ink layer derived from an electrostatic ink composition to a packaging bag for heat treatment, there was a possibility of damage to the packaging bag. In contrast, with the above configuration, the deformation of the laminate due to heating is suppressed as the adhesive composition containing the epoxy compound hardens, resulting in a heat-resistant packaging bag with sufficient resistance to heat treatment. Furthermore, if a primer layer containing polyethyleneimine resin is included, water resistance is also improved, and more sufficient resistance is obtained, especially to heat treatment in environments with high moisture content, such as boiling or retort heat treatment.

[0123] Furthermore, the packaging bag 120 (heat-resistant packaging bag) includes a sealing portion 101 on its outer periphery that adheres the sealant layers 20 of the two laminated bodies 300 together. The ink coverage of the electrostatic ink layer 50 in the sealing portion 101 may be 300% or less. The sealing portion 101 is an area where heat-based bonding processes such as heat sealing are performed, and therefore is more susceptible to damage than other areas. In contrast, by setting the ink coverage of the electrostatic ink layer within the above range, more sufficient resistance to heat treatment can be ensured in the sealing portion as well, resulting in a heat-resistant packaging bag with stronger resistance to heat treatment.

[0124] The epoxy compound may include a bifunctional alicyclic epoxy compound. Such an epoxy compound, being bifunctional, increases the number of crosslinking points with the electrostatic ink composition, resulting in strong adhesion to the printed surface.

[0125] Furthermore, the adhesive composition may further contain a polyol, the polyol may include an aliphatic polyester polyol, and the epoxy compound may include one having epoxy groups at both ends. Such an adhesive layer 30 has high adhesive strength, especially in high-temperature environments. Therefore, when the laminates 300 are combined to produce a packaging bag, it is possible to sufficiently suppress the rupture of the electrostatic ink composition or the damage to the packaging bag.

[0126] The above adhesive composition may further contain a polyisocyanate, and the polyisocyanate may contain a xylylene diisocyanate derivative. Such polyisocyanates and polyols exhibit excellent reactivity. This improves the curability of the adhesive composition, thereby suppressing deformation of the laminate 300 and the packaging bag.

[0127] The laminates 300 (302, 304) and packaging bags manufactured in this manner have the configuration and properties as described in these embodiments. The descriptions of the laminates 300, packaging bags and their modified forms also apply to the description of the embodiments of the manufacturing method described above.

[0128] Although several embodiments have been described above, the descriptions of common configurations can be applied to each other. Furthermore, this disclosure is not limited in any way to the embodiments described above. [Examples]

[0129] The contents of this disclosure will be described in more detail with reference to examples, comparative examples, and reference examples, but this disclosure is not limited to the following examples.

[0130] (Example I-1) [Fabrication of laminates] As a substrate, an alumina-deposited PET film (manufactured by Toppan Printing Co., Ltd., product name: GLARH12, thickness: 12 μm) was prepared. An aqueous primer resin (resin containing polyethyleneimine, manufactured by Michelman, product name: DP050) was applied to this alumina-deposited surface to form a primer layer. The amount of aqueous polyethyleneimine applied was 0.10 to 0.18 g / m². 2 It was applied in this manner.

[0131] A predetermined print was performed on the surface of the primer layer using a digital printing press (HP Indigo 20000 label and packaging digital printing press). The electrostatic ink composition used was an electrostatic ink composition containing a thermoplastic resin containing a copolymer of ethylene acrylic acid and ethylene methacrylic acid (HP Indigo Electroink). The colors used for the electrostatic ink composition were yellow (Y), magenta (M), and cyan (C), as shown in Table 1. Multiple samples with different colors and ink coverage rates were prepared. The ink coverage rates were as shown in Table 1. Each ink coverage rate was adjusted according to the settings of the digital printing press. The total ink coverage rate was 200%.

[0132] An adhesive composition with a solid content of 36.5% by mass was prepared by combining an aliphatic polyester polyol (manufactured by Mitsui Chemicals, Inc., trade name: Takelac A626, sometimes referred to as "(A)") as the main agent, a polyisocyanate (manufactured by Mitsui Chemicals, Inc., trade name: Takenate A50, sometimes referred to as "(B)") as the curing agent, 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate (sometimes referred to as "C") as the epoxy compound, and ethyl acetate as the solvent. The structure of this epoxy compound is shown in formula (1) below. The mass-based mixing ratio (by mass) of each component was (A):(B):(C) = 8:1:0.28.

[0133] An adhesive layer was formed on the printed surface, which had been printed with an electrostatic ink composition, by applying the adhesive composition prepared as described above using a dry laminating apparatus. The amount of adhesive composition applied was 4.0 g / m². 2 That's what I decided.

[0134] [ka]

[0135] A laminated film was prepared by bonding a nylon film and an unoriented polypropylene film with a commercially available adhesive. Using the dry laminating apparatus described above, the nylon film and the adhesive layer were bonded together with the adhesive layer on the substrate facing each other to obtain a laminate. The curing time (aging) was 2 days at 40°C.

[0136] (Comparative example I-1) The laminate was prepared in the same manner as in Example I-1, except that the epoxy compound (component (C)) was not incorporated when preparing the adhesive composition.

[0137] <Evaluation of the delamination suppression performance of the laminate, Part 1> The delamination suppression performance during heating was evaluated for each of the laminates prepared in Example I-1 and Comparative Example I-1. Specifically, the laminate was folded in half to form a bent portion and secured with a clip to serve as an evaluation sample. The evaluation sample was heated for 45 minutes at the heating temperature listed in Table 1, and the condition of the bent portion of the evaluation sample after heating was observed using an optical microscope. The evaluation was performed according to the following criteria. The results are shown in Table 1. A: No delamination is observed. B: Slight voids are visible between the layers. C: Delamination is observed between the layers.

[0138] [Table 1]

[0139] As shown in Table 1, in the laminate of Example I-1, it was confirmed that sufficient delamination suppression performance was exhibited even in the bent portion by using the specified adhesive composition. In the laminate of Comparative Example I-1, it is presumed that the resin component of the electrostatic ink layer melted, causing delamination. Furthermore, in Comparative Example I-1, it was confirmed that this tendency became more pronounced as the heating temperature increased. On the other hand, in the laminate of Example I-1, it was confirmed that sufficient delamination suppression performance was maintained even at high temperatures. The laminate of Example I-1 is expected to exhibit a similarly sufficient delamination suppression effect even at non-heated temperatures (e.g., room temperature) when the resin component is solidified.

[0140] <Evaluation of the delamination suppression performance of the laminate, Part 2> For each of the laminates prepared in Example I-1 and Comparative Example I-1, the delamination suppression performance during heating was evaluated in the same manner as in "Evaluation of Delamination Suppression Performance of Laminates Part 1" described above, except that the heating temperature and heating time were changed. The results are shown in Table 2.

[0141] [Table 2]

[0142] As shown in Table 2, the same trend as in "Evaluation of Laminate Delamination Suppression Performance Part 1" was observed even when the heating temperature and heating time were changed. As the results for the laminate of Example I-1 show, it was confirmed that the container according to this disclosure has sufficient resistance to retort heat treatment at 120°C or higher (for example, heat and pressurized sterilization treatment at 120°C for 30 minutes).

[0143] <Thermal sealing test at bent sections: Evaluation of peeling suppression performance, part 3> Next, the effect of sealing with a bent section was evaluated. Three laminates were prepared in each of Example I-1 and Comparative Example I-1, and a standing pouch (a container with the same configuration as the containers shown in Figures 3 and 4) was prepared using these three laminates. Specifically, a sheet to be the bottom sheet was folded in half and placed between two laminates to be the side sheets. A thermal gradient tester was used to apply a pressure of 0.2 MPa to the laminate, and it was treated for 1 second at the temperatures shown in Table 3 to seal it. The laminate that would become the bottom sheet of the standing pouch was positioned so that the sealant layer side faced the inside of the container when folded. The thermal gradient tester used was the "HG-100" (product name) manufactured by Toyo Seiki Seisakusho Co., Ltd. After preparation, a cross-section including the bottom sheet of the standing pouch was observed with an optical microscope. The evaluation criteria were the same as those used in "Evaluation of Laminate Delamination Suppression Performance Part 1" above. The results are shown in Table 3. For reference, Figure 9 shows the appearance of the bent portion of the laminate that forms the bottom sheet of Example I-1 and Comparative Example I-1, both before sealing and after sealing at 210°C.

[0144] [Table 3]

[0145] As shown in Table 3, even during heat treatment under pressure, such as when bonding sealant layers together, delamination was sufficiently suppressed in the laminate prepared in Example I-1.

[0146] <Thermal sealing test at bent sections: Evaluation of peeling suppression performance, part 4> The pressure conditions applied during sealing, or the sealing time, were changed, and the same evaluation as in "Thermal sealing test at a bent section: Evaluation of delamination suppression performance, part 3" was performed. The results are shown in Tables 4 and 5, and Figures 10 and 11.

[0147] [Table 4]

[0148] [Table 5]

[0149] As shown in Tables 4 and 5, and Figures 10 and 11, it was confirmed that with the laminate of Example I-1, delamination was sufficiently suppressed even under heat sealing conditions, under general sealing conditions when manufacturing a container by sealing the laminate.

[0150] From the results of Example I-1 and Comparative Example I-1 described above, it was confirmed that using an adhesive composition containing an epoxy compound effectively suppresses delamination between the layers constituting the laminate. This delamination suppression effect is thought to be due to improvements in the strength of the electrostatic ink composition and the adhesive strength between the layers. For reference, examples of adjusted adhesive composition compositions are shown below.

[0151] (Reference example I-1) [Fabrication of laminates] Laminates were prepared in the same manner as in Example I-1, except that the mass-based mixing ratios of each component in the adhesive composition (A):(B):(C) were changed as shown in Table 5. The laminate strength of the obtained laminate was measured by the method described later. The results are shown in Table 6.

[0152] <Evaluation of the lamination strength of the laminate> The laminate strength of the laminate prepared in Reference Example I-1 was measured in accordance with JIS K 6854-1:1999. Specifically, the prepared laminate was first cut into 15 mm wide strips to serve as measurement samples. After delaminating the interlayers at the ends of the measurement samples, the delamination strength between the layers of the laminate was measured using a tensile testing machine under the conditions of an angle of 90°, a tensile speed of 300 mm / min, and room temperature. This delamination strength was defined as the laminate strength at room temperature (20°C). The measurement results are shown in Table 6.

[0153] (Reference example I-2) A two-component adhesive was prepared, consisting of a first liquid made of aliphatic polyester polyol (A) (manufactured by Mitsui Chemicals, Inc., trade name: Takelac A626) and a second liquid made of polyisocyanate (B) (manufactured by Mitsui Chemicals, Inc., trade name: Takenate A50) and an epoxy compound (C), each contained separately in containers. The first and second liquids were mixed to prepare adhesive compositions with the formulations shown in Table 6. Laminates were prepared in the same manner as in Reference Example I-1, except for the use of this adhesive composition, and the adhesive strength was measured. The measurement results are shown in Table 6.

[0154] (Comparative example I-2) A laminate was prepared in the same manner as in Reference Example I-1, except that epoxy compound (C) was not incorporated when preparing the adhesive composition, and the adhesive strength was measured. The measurement results are shown in Table 6.

[0155] (Comparative example I-3) A laminate was prepared in the same manner as in Reference Example I-1, except that an epoxy compound of formula (1) was applied to a printed surface printed with an electrostatic ink composition to form an epoxy coating layer, and the adhesive composition of Comparative Example I-2 was applied to this epoxy coating layer. The adhesive strength was then measured. The amount of epoxy coating layer applied was equivalent to 0.53 parts by mass in the formulation shown in Table 5. The measurement results are shown in 6.

[0156] [Table 6]

[0157] The column [(B) / (A)]×100 in Table 6 shows the amount of polyisocyanate blended per 100 parts by mass of aliphatic polyester polyol (parts by mass). The column [(C) / (A)]×100 in Table 6 shows the amount of epoxy compound blended per 100 parts by mass of aliphatic polyester polyol (parts by mass). The column "Epoxy Group / Isocyanate Group" in Table 6 shows the molar ratio of epoxy groups in epoxy compound (C) to isocyanate groups in polyisocyanate (B).

[0158] As shown in Table 6, the laminates of Reference Examples I-1 to I-2, in which an adhesive layer containing an epoxy compound was bonded to the printed surface, were found to have higher adhesive strength than the laminate of Comparative Example I-2, in which an adhesive layer without an epoxy compound was bonded to the printed surface. In Comparative Example I-3, relatively high adhesive strength was obtained, but the number of steps increased because an epoxy coating layer was formed in addition to the adhesive layer. The curing (aging) of the epoxy coating layer took two days, resulting in decreased productivity.

[0159] In the laminate of Comparative Example I-2, delamination occurred near the interface between the electrostatic ink layer and the primer layer. In the laminate of Comparative Example I-3, cohesive failure of the electrostatic ink layer occurred. On the other hand, the laminates of Reference Examples I-1 and I-2 exhibited sufficient lamination strength, and when a load was deliberately applied, delamination occurred at the interface between the electrostatic ink layer and the adhesive layer, but cohesive failure of the electrostatic ink layer was not observed. This suggests that the cohesive strength of the electrostatic ink layer has improved. In Reference Examples I-1 and I-2, the molar ratio of isocyanate groups contained in polyisocyanate (B) to hydroxyl groups of aliphatic polyester polyol (A) was in the range of 0.5 to 10.

[0160] Next, in addition to the laminate strength, the hot water lamination strength and seal strength were measured for the laminates of Reference Example I-1 and Comparative Example I-3. For the measurements, we used laminates with a total ink coverage of 500% and 200%. The details of the measurement procedure are as follows.

[0161] [Measurement of hot water lamination strength] The laminates of Reference Example I-1 and Comparative Example I-3 were each cut to a width of 15 mm to obtain measurement samples. After delaminating the interlayers at the edges of the measurement samples, the peel strength was measured using a tensile testing machine while immersed in 90°C hot water. Specifically, the peel angle was free and the tensile speed was 300 mm / min. This peel strength is shown in Table 7 as the hot water lamination strength.

[0162] [Measurement of seal strength (before heat treatment)] Using a pair of laminates from Reference Example I-1, heat sealing was performed so that the unoriented polypropylene films overlapped to form a sealed section. This heat-welded the unoriented polypropylene films together, and a 15 mm wide measurement sample was prepared. The seal strength of the sealed section of the prepared measurement sample was measured in accordance with JIS K 7127:1999. The peel strength between the heat seals was measured using a tensile testing machine under the conditions of a peel angle of 90°, a tensile speed of 300 mm / min, and room temperature (20°C). This peel strength was defined as the seal strength "before heat treatment". The measurement results are shown in Table 7. A similar measurement sample was prepared using the laminate from Comparative Example I-3, and the same measurement was performed. The measurement results are shown in Table 7.

[0163] [Measurement of seal strength (after boiling)] The sample prepared in the "Measurement of seal strength (before heat treatment)" described above was heated in 100°C water for 30 minutes. Afterward, the seal strength was measured using the same procedure as described in the "Measurement of seal strength (before heat treatment)" described above. The measurement results are shown in the "After boiling" column of Table 7.

[0164] [Measurement of seal strength after retorting (120°C)] The measurement samples prepared in the "Measurement of Seal Strength (Before Heat Treatment)" described above were subjected to retort heat treatment (120°C for 30 minutes). The peel strength was measured using a tensile testing machine in the same manner as in the "Measurement of Seal Strength (Before Heat Treatment)". The measurement results are shown in the "120°C x 30 minutes" column of Table 7.

[0165] [Measurement of seal strength after retorting (130°C)] The measurement samples prepared in the "Measurement of Seal Strength (Before Heat Treatment)" described above were subjected to retort heat treatment (130°C for 30 minutes). The peel strength was measured using a tensile testing machine in the same manner as in the "Measurement of Seal Strength (Without Heat Treatment)". The measurement results are shown in the "130°C x 30 minutes" column of Table 7.

[0166] [Table 7]

[0167] As shown in Table 7, the hot water lamination strength of Reference Example I-1 was significantly higher than that of Comparative Example I-3. Furthermore, the seal strength of Reference Example I-1 was also confirmed to be superior to that of Comparative Example I-3. In particular, the seal strength of Reference Example I-1 remained sufficiently high even after boiling, while the seal strength of Comparative Example I-3 decreased significantly after boiling. It was confirmed that the laminate of Comparative Example I-3 experienced a significant decrease in both lamination strength and seal strength when heated in the presence of moisture.

[0168] (Example II-1) [Fabrication of laminates] A nylon film (thickness: 15 μm) was prepared as the substrate. A water-based primer resin (resin containing polyethyleneimine, manufactured by Michelman, product name: DP050) was applied to one main surface of this nylon film to form a primer layer. The amount of water-based polyethyleneimine applied was 0.10 to 0.18 g / m². 2 It was applied in this manner.

[0169] A digital printing press (HP Indigo 20000 label and packaging digital printing press) was used to print the desired result onto the surface of the primer layer. The electrostatic ink composition used was an electrostatic ink composition containing a thermoplastic resin containing a copolymer of ethylene acrylic acid and ethylene methacrylic acid (HP Indigo Electroink). As shown in Table 8, white (W) and cyan (C) were used as the colors of the electrostatic ink composition. Multiple samples with different colors and ink coverage rates were prepared. The ink coverage rates were as shown in Table 8. Each ink coverage rate was adjusted according to the settings of the digital printing press. As shown in Table 8, the total ink coverage rate ranged from 100% to 300%.

[0170] An adhesive composition with a solid content of 36.5% by mass was prepared by combining an aliphatic polyester polyol (manufactured by Mitsui Chemicals, Inc., trade name: Takelac A626, sometimes referred to as "(A)") as the main agent, a polyisocyanate (manufactured by Mitsui Chemicals, Inc., trade name: Takenate A50, sometimes referred to as "(B)") as the curing agent, 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate (sometimes referred to as "C") as the epoxy compound, and ethyl acetate as the solvent. The structure of this epoxy compound is shown in formula (1) below. The mass-based mixing ratio (by mass) of each component was (A):(B):(C) = 8:1:0.28.

[0171] An adhesive layer was formed on the printed surface, which had been printed with an electrostatic ink composition, by applying the adhesive composition prepared as described above using a dry laminating apparatus. The amount of adhesive composition applied was 4.0 g / m². 2 That's what I decided.

[0172] [ka]

[0173] An LLDPE film (manufactured by Futamura Chemical Co., Ltd., product name: XMTN, thickness: 60 μm) was prepared, and a laminate was obtained by bonding the adhesive layer on the substrate to the LLDPE film using the dry laminating apparatus described above. The curing time (aging) was set to 2 days at 40°C.

[0174] (Examples II-2, II-3) The laminate was prepared in the same manner as in Example II-1, except that the color and ink coverage of the electrostatic ink composition were changed as shown in Table 8.

[0175] (Comparative Examples II-1 to II-3) The laminates were prepared in the same manner as in Examples II-1 to II-3, except that the epoxy compound (component (C)) was not incorporated when preparing the adhesive composition.

[0176] [Creating packaging] For each of the above Examples II-1 to II-3 and Comparative Examples II-1 to II-3, two rectangular laminates measuring 150 mm x 200 mm were prepared. In this case, for Examples II-1 and Comparative Example II-1, the laminates were prepared without the electrostatic ink composition applied to the outer circumference with a width of 10 mm, while for Examples II-2 to II-3 and Comparative Examples II-2 to II-3, the laminates were prepared with the electrostatic ink composition applied to the outer circumference as well. The two laminates were stacked with their main surfaces facing each other on the LLDPE film side, and by heat sealing, a pair of ends along the longitudinal direction and one end along the short direction were bonded together to form sealed portions on three of the four sides of the laminate. Figure 12 shows the main surface of the laminate 310. First, sealed portions 111 were formed on three sides of the laminate 310 by the initial heat sealing, creating a packaging bag with three sides closed. The width T of the sealed portion 111 at this time (see Figure 12) was 10 mm. On the side where the seal portion 111 was not formed, a seal portion 114 was formed by bonding two laminates together by heat sealing. The width T of the seal portion 114 was also set to 10 mm. In other words, when using the laminates of Example II-1 and Comparative Example II-1, packaging bags were prepared in which the electrostatic ink composition was not printed inside the laminate at the seal portions 111 and 114.

[0177] Before completely sealing the seal portion 114 to create an airtight state inside, 500 ml of water was introduced as the contents of the packaging bag. This created the packaging bodies according to Examples II-1 to II-3 and Comparative Examples II-1 to II-3. As described above, the inside of the packaging body was filled with 500 ml of water.

[0178] <Evaluation of laminate strength (before boiling)> For each of the packaging materials according to Examples II-1 to II-3 and Comparative Examples II-1 to II-3, the laminate strength was measured in accordance with the description in JIS K 6854-1:1999. Specifically, instead of the prepared packaging materials according to Examples II-1 to II-3 and Comparative Examples II-1 to II-3, the laminates according to Examples II-1 to II-3 and Comparative Examples II-1 to II-3 before water filling were cut to a width of 15 mm to be used as measurement samples. After delaminating the interlayers at the ends of the measurement samples, the delamination strength between the layers of the laminate was measured using a tensile testing machine under the conditions of angle: 90°, tensile speed: 300 mm / min, and room temperature. This delamination strength was defined as the laminate strength at room temperature (20°C). The measurement results are shown in Table 8.

[0179] <Evaluation of laminate strength (after boiling)> Each of the packaging materials for Examples II-1 to II-3 and Comparative Examples II-1 to II-3 was heated in water at 90°C for 30 minutes (boiling heat treatment). Subsequently, a portion of the packaging material was cut out using the same procedure as described above for <Evaluation of Laminate Strength (Before Boiling)>, and the laminate strength was measured. The measurement results are shown in Table 8.

[0180] [Table 8]

[0181] From the results above, it was confirmed that the presence of the electrostatic ink layer reduces the laminate strength compared to the case without the electrostatic ink layer (Example II-1, Comparative Example II-1), and that the laminate strength decreases as the ink coverage rate increases. In particular, when the ink coverage rate reached 300%, the laminate strength of Comparative Example II-3 fell to 2 or less in both the packaging (laminated body) before and after boiling, indicating that it may not be suitable for use as a packaging bag for heat treatment. It should be noted that in all of Examples II-1 to II-3 and Comparative Examples II-1 to II-3, the laminate strength increased after boiling. This is presumed to be due to the reaction of the isocyanate, which acts as a curing agent in the adhesive composition, during boiling.

[0182] <Evaluation of seal strength (before boiling)> For each of the packaging materials in Examples II-1 to II-3 and Comparative Examples II-1 to II-3, a 15 mm wide measurement sample was prepared by cutting out a section including the seal portion before filling with water (before completely sealing the seal portion 114 and sealing the interior). The seal strength at the seal portion of the prepared measurement sample was measured in accordance with JIS K 7127:1999. The measurement was performed using a tensile testing machine under the conditions of peel angle: 90°, tensile speed: 300 mm / min, and room temperature (20°C) to measure the peel strength between the heat seals. This peel strength was defined as the seal strength "before heat treatment". The measurement results are shown in Table 9.

[0183] <Evaluation of seal strength (after boiling)> Each of the packaging materials for Examples II-1 to II-3 and Comparative Examples II-1 to II-3 was heated in 90°C water for 30 minutes (boiling heat treatment). After that, the packaging was opened, the water that had been filled inside was removed, and the seal strength was measured using the same procedure as described above for "evaluation of seal strength (before boiling)". The measurement results are shown in Table 9.

[0184] In Table 9, "film rupture" indicates that the measurement was completed when the film was ruptured. "Triangular delamination" indicates that delamination occurred between layers in at least one of the pair of laminates. "Edge breakage" indicates that damage occurred at the boundary between the heat-sealed area and the inside of the bag.

[0185] [Table 9]

[0186] From the results above, it was confirmed that the presence of the electrostatic ink layer reduces the seal strength compared to the case without the electrostatic ink layer (Example II-1, Comparative Example II-1), and that the seal strength decreases as the ink coverage increases. For Comparative Examples II-2 and II-3, the seal strength before and after boiling was 40 N / 15 mm or less, indicating that they may not be suitable for use as packaging bags for heat treatment.

[0187] <Aerated boiling test> For each of the above Examples II-1 to II-3 and Comparative Examples II-1 to II-3, two rectangular laminates measuring 150 mm x 200 mm were prepared, and packaging for the air-boiled test was manufactured using the same method as described above for preparing the packaging.

[0188] Furthermore, this differs from the packaging used for lamination strength and seal strength in that, before completely sealing the seal portion 114 and creating an airtight state inside, 300 ml of water was introduced as the contents of the packaging bag, and then 100 ml of air was added. This resulted in the creation of packaging for the air-filled boil test in Examples II-1 to II-3 and Comparative Examples II-1 to II-3. As described above, the inside of the packaging was filled with 300 ml of water and 100 ml of air.

[0189] Three packages were prepared for each of Examples II-1 to II-3 and Comparative Examples II-1 to II-3, and each was heated in water at 100°C for 60 minutes. The surface of the heated packages was visually inspected to check for any lifting of the printed surface due to the electrostatic ink composition on the surface of the laminate. The measurement results are shown in Table 10.

[0190] [Table 10]

[0191] From the results of the above-described examples and comparative examples, it was confirmed that adhesive compositions containing polyols, polyisocyanates, and epoxy compounds are resistant to heat treatment. This improvement in heat resistance is thought to be due to improvements in the strength of the electrostatic ink composition and the adhesive strength between each layer. The following experiments were conducted to verify these improvements.

[0192] (Reference Example II-1) [Preparation of adhesive compositions and laminates] A polyethylene terephthalate film (PET film, thickness: 12 μm) was prepared as the base material. The same aqueous primer resin as in Example II-1 was applied to one side of this PET film to form a primer layer. The amount of aqueous polyethyleneimine applied was also the same as in Example II-1.

[0193] Using the digital printing press used in Example II-1, a predetermined print was applied to the surface of the primer layer. The electrostatic ink composition used was an electrostatic ink composition (HP Indigo Electroink) containing a thermoplastic resin with a copolymer of ethylene acrylic acid and ethylene methacrylic acid. The colors used for the electrostatic ink composition were white (W), yellow (Y), magenta (M), and cyan (C), as shown in Table 11. Multiple samples with different colors and ink coverage rates were prepared. The ink coverage rates for each color and their total are shown in Table 11. As shown in Table 11, the total ink coverage rate ranged from 200% to 500%.

[0194] The same adhesive composition as in Example II-1 was prepared, and the adhesive composition was applied to the printed surface using the same procedure as in Example II-1 to form an adhesive layer. The amount of adhesive composition applied was 4.0 g / m². 2 That's what I decided.

[0195] A laminated film was prepared having aluminum foil (manufactured by Toyo Aluminum Co., Ltd., thickness: 7 μm), nylon film, and unoriented polypropylene film in that order. Using the same dry laminating apparatus as in Example II-1, the aluminum foil and the adhesive layer were bonded together with the adhesive layer on the substrate facing each other to obtain a laminate. The curing time (aging) was 2 days at 40°C.

[0196] [Measurement of adhesive strength (at room temperature)] The adhesive strength of the prepared laminate was measured in accordance with JIS K 6854-1:1999. Specifically, the prepared laminate was cut into 15 mm wide strips to serve as measurement samples. After delaminating the interlayers at the ends of the measurement samples, the delamination strength between the laminate layers was measured using a tensile testing machine under the conditions of an angle of 90°, a tensile speed of 300 mm / min, and room temperature. This delamination strength was defined as the adhesive strength at room temperature (20°C). The measurement results are shown in Table 11.

[0197] (Reference examples II-2 to II-6) Laminates were prepared in the same manner as in Reference Example II-1, except that the composition of the adhesive was changed as shown in Tables 11 and 12, and the adhesive strength was measured. The measurement results are shown in Tables 11 and 12.

[0198] (Reference Example II-7) A two-component adhesive was prepared, consisting of a first liquid made of aliphatic polyester polyol (A) (manufactured by Mitsui Chemicals, Inc., trade name: Takelac A626) and a second liquid made of polyisocyanate (B) (manufactured by Mitsui Chemicals, Inc., trade name: Takenate A50) and an epoxy compound (C), each contained separately in containers. The first and second liquids were mixed to prepare adhesive compositions with the formulations shown in Table 12. Laminates were prepared in the same manner as in Reference Example II-1, except for the use of this adhesive composition, and the adhesive strength was measured. The measurement results are shown in Table 12.

[0199] (Comparative Example II-4) A laminate was prepared in the same manner as in Reference Example II-1, except that epoxy compound (C) was not incorporated when preparing the adhesive composition, and the adhesive strength was measured. The measurement results are shown in Table 12.

[0200] (Comparative Example II-5) A laminate was prepared in the same manner as in Reference Example II-1, except that an epoxy compound of formula (1) was applied to a printed surface printed with an electrostatic ink composition to form an epoxy coating layer, and the adhesive composition of Comparative Example II-4 was applied to this epoxy coating layer. The adhesive strength was then measured. The amount of epoxy coating layer applied was equivalent to 0.53 parts by mass in the formulations shown in Table 11. The measurement results are shown in Table 12.

[0201] [Table 11]

[0202] [Table 12]

[0203] The column "[(B) / (A)] × 100" in Tables 11 and 12 shows the amount of polyisocyanate blended per 100 parts by mass of aliphatic polyester polyol (parts by mass). The column "[(C) / (A)] × 100" in Tables 11 and 12 shows the amount of epoxy compound blended per 100 parts by mass of aliphatic polyester polyol (parts by mass). The "Epoxy Group / Isocyanate Group" column in Tables 11 and 12 shows the molar ratio of epoxy groups in the epoxy compound (C) to isocyanate groups in the polyisocyanate (B).

[0204] As shown in Tables 11 and 12, the laminates of Reference Examples II-1 to II-7, in which an adhesive layer containing an epoxy compound was bonded to the printed surface, were found to have higher adhesive strength than the laminate of Comparative Example II-4, in which an adhesive layer without an epoxy compound was bonded to the printed surface. In Comparative Example II-5, relatively high adhesive strength was obtained, but the number of steps increased because an epoxy coating layer was formed in addition to the adhesive layer. The curing (aging) of the epoxy coating layer took two days, resulting in decreased productivity.

[0205] In the laminate of Comparative Example II-4, delamination occurred near the interface between the electrostatic ink layer and the primer layer. In the laminate of Comparative Example II-5, cohesive failure of the electrostatic ink layer was observed. On the other hand, in the laminates of Reference Examples II-1 to II-7, delamination occurred at the interface between the electrostatic ink layer and the adhesive layer, and no cohesive failure of the electrostatic ink layer was observed. This suggests that the cohesive strength of the electrostatic ink layer has improved. In Reference Examples II-1 to II-7, the molar ratio of isocyanate groups contained in polyisocyanate (B) to hydroxyl groups of aliphatic polyester polyol (A) was in the range of 0.5 to 10.

[0206] Next, the adhesive strength, hot water adhesive strength, and seal strength of the laminates of Reference Example II-5 and Comparative Example II-5 were measured. For the measurements, laminates with a total ink coverage of 500% and 200% were used. The details of the measurement procedure are as follows.

[0207] [Measurement of hot water adhesion strength] The laminates of Reference Example II-5 and Comparative Example II-5 were each cut to a width of 15 mm to obtain measurement samples. After delaminating the interlayers at the edges of the measurement samples, the peel strength was measured using a tensile testing machine while immersed in 90°C hot water. Specifically, the peel angle was free and the tensile speed was 300 mm / min. This peel strength is shown as the hot water adhesion strength in Table 13.

[0208] [Measurement of seal strength (before heat treatment)] Using a pair of laminates from Reference Example II-5, heat sealing was performed so that the unoriented polypropylene films overlapped to form a sealed section. This heat-welded the unoriented polypropylene films together, and a 15 mm wide measurement sample was prepared. The seal strength of the sealed section of the prepared measurement sample was measured in accordance with JIS K 7127:1999. The peel strength between the heat seals was measured using a tensile testing machine under the conditions of peel angle: 90°, tensile speed: 300 mm / min, and room temperature (20°C). This peel strength was defined as the seal strength "before heat treatment". The measurement results are shown in Table 13. Using the laminate from Comparative Example II-5, a similar measurement sample was prepared and the same measurement was performed. The measurement results are shown in Table 13.

[0209] [Measurement of seal strength (after boiling)] The sample prepared in the "Measurement of seal strength (before heat treatment)" described above was heated in 100°C water for 30 minutes. Afterward, the seal strength was measured using the same procedure as in the "Measurement of seal strength (without heat treatment)" described above. The measurement results are shown in the "After boiling" column of Table 13.

[0210] [Measurement of seal strength after retorting (120°C)] The measurement samples prepared in the "Measurement of Seal Strength (Before Heat Treatment)" described above were subjected to retort heat treatment (120°C for 30 minutes). The peel strength was measured using a tensile testing machine in the same manner as in the "Measurement of Seal Strength (Before Heat Treatment)". The measurement results are shown in the "120°C x 30 minutes" column of Table 13.

[0211] [Measurement of seal strength after retorting (130°C)] The measurement samples prepared in the "Measurement of seal strength (before heat treatment)" described above were subjected to retort heat treatment (130°C for 30 minutes). The peel strength was measured using a tensile testing machine in the same manner as in the "Measurement of seal strength (without heat treatment)". The measurement results are shown in the "130°C x 30 minutes" column of Table 13.

[0212] [Table 13]

[0213] As shown in Table 13, the hot water bonding strength of Reference Example II-5 was significantly higher than that of Comparative Example II-5. Furthermore, the seal strength of Reference Example II-5 was also confirmed to be superior to that of Comparative Example II-5. In particular, the seal strength of Reference Example II-5 remained sufficiently high even after boiling, while the seal strength of Comparative Example II-5 decreased significantly after boiling. It was confirmed that the laminate of Comparative Example II-5 experienced a significant decrease in both bonding strength and seal strength when heated in the presence of moisture.

[0214] (Reference Example II-8) [Preparation of adhesive compositions and laminates] A polyethylene terephthalate film (PET film, thickness: 12 μm) was prepared as the base material. The same aqueous primer resin as in Example II-1 was applied to one side of this PET film to form a primer layer. The amount of aqueous polyethyleneimine applied was also the same as in Example II-1.

[0215] Using the digital printing press used in Example II-1, a predetermined print was made on the surface of the primer layer. The electrostatic ink composition used was white (W), yellow (Y), magenta (M), and cyan (C). Two ink coverages were prepared: one with W200% and another with C100%+M100%+Y100%+W200%. In Table 14, the former was labeled "Ink Coverage (1)" and the latter "Ink Coverage (2)". In this way, two types of samples with different ink coverages of the electrostatic ink composition were prepared.

[0216] An adhesive composition was prepared as in Example II-1, and the adhesive composition was applied to the printed surface using the same procedure as in Example II-1 to form an adhesive layer. The amount of adhesive composition applied was 4.0 g / m². 2 That's what I decided.

[0217] A laminated film (a laminated film obtained by bonding a nylon film and an unoriented polypropylene film with a commercially available adhesive), used in Example II-1, was bonded to the adhesive layer of the substrate in the same manner as in Example II-1 to obtain a laminate. The curing time (aging) was 40°C for 2 days.

[0218] The seal strength (before heat treatment) and seal strength (after boiling) of the laminate obtained in this manner were measured. The measurement results are shown in Table 14. In addition, the adhesive strength (before heat treatment) and hot adhesive strength (120°C) were measured using the following procedure.

[0219] Using a pair of laminates from Reference Example II-8, a three-sided bag with a sealed portion was fabricated by heat sealing the unstretched polypropylene films so that they overlapped. Water was sealed inside this three-sided bag. Subsequently, retort heat treatment (120°C for 30 minutes) was performed using a retort processing device (manufactured by Hisaka Works). After the retort heat treatment, the bag was cut to a width of 15 mm, and a sample of the sealed portion was taken. The interlayer strength between the electrostatic ink layer and the layer in contact with the electrostatic ink layer was measured. The measured peel strength is shown in the "Hot Adhesion Strength (120°C)" column of Table 14. Table 14 also shows the adhesion strength before the retort heat treatment.

[0220] (Reference examples II-9 to II-12) The laminate was prepared in the same manner as in Reference Example II-8, except that the amount of polyisocyanate (B) was changed as shown in Table 14 when preparing the adhesive composition. The prepared laminate was evaluated in the same manner as in Reference Example II-8. The evaluation results are shown in Table 14.

[0221] (Comparative Example II-6) A laminate was prepared in the same manner as in Comparative Example II-4, except that the lamination of the printed surface with the electrostatic ink composition was performed using a hand laminator instead of a dry laminating device. The color and ink coverage of the electrostatic ink composition were as shown in Table 14. The prepared laminate was evaluated in the same manner as in Reference Example II-8. The evaluation results are shown in Table 14.

[0222] [Table 14]

[0223] As shown in Table 14, it was confirmed that high adhesive strength and seal strength could be obtained even under heating conditions in each reference example. Furthermore, it was confirmed that the hot adhesive strength (120°C) and seal strength (before heat treatment and after boiling) could be sufficiently increased by adjusting the blending ratio of polyisocyanate (B) to aliphatic polyester polyol (A). On the other hand, in Comparative Example II-6, which did not use epoxy compound (C), it was confirmed that the adhesive strength and seal strength decreased significantly when exposed to high-temperature hot water treatment conditions. In Reference Examples II-8 to II-12, the molar ratio of isocyanate groups in polyisocyanate (B) to hydroxyl groups in aliphatic polyester polyol (A) was in the range of 0.5 to 10.

[0224] (Reference examples II-13 to II-17) An adhesive composition was prepared by blending an aliphatic polyester polyol (A1) (Takelac A525, manufactured by Mitsui Chemicals, Inc.), a polyisocyanate (B1) (Takenate A52, manufactured by Mitsui Chemicals, Inc.), and 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate as the epoxy compound (C). The blending ratios are shown in Table 15. Laminates were prepared and evaluated in the same manner as in Reference Examples II-8 to II-12, except for the use of this adhesive composition. The evaluation results are shown in Table 15.

[0225] (Comparative Example II-7) Adhesive compositions were prepared by blending aliphatic polyester polyol (A1) (Takelac A525, manufactured by Mitsui Chemicals, Inc.) and polyisocyanate (B1) (Takenate A52, manufactured by Mitsui Chemicals, Inc.) as polyols. The blending ratios are shown in Table 15. Laminates were prepared and evaluated in the same manner as in Comparative Example II-4, except for the use of these adhesive compositions. The evaluation results are shown in Table 15.

[0226] [Table 15]

[0227] As shown in Table 15, it was confirmed that high adhesive strength and seal strength could be obtained in each reference example even when the combination of aliphatic polyester polyol and polyisocyanate was changed. Furthermore, it was confirmed that the hot adhesive strength (120°C) and seal strength (without heat treatment and after boiling) could be sufficiently increased by adjusting the blending ratio of polyisocyanate (B1) to aliphatic polyester polyol (A1). On the other hand, in Comparative Example II-7, which did not use epoxy compound (C), it was confirmed that the adhesive strength and seal strength decreased significantly when exposed to high-temperature hot water treatment conditions. In Reference Examples II-13 to II-17, the molar ratio of isocyanate groups in polyisocyanate (B1) to hydroxyl groups in aliphatic polyester polyol (A1) was in the range of 0.5 to 10. [Industrial applicability]

[0228] According to this disclosure, it is possible to provide a container that has a printed surface printed by a digital printing press, while suppressing peeling at the interface between the electrostatic ink layer and the primer layer, and at the interface between the electrostatic ink layer and the adhesive layer, even in the bent parts that occur during the manufacturing process.

[0229] According to this disclosure, it is possible to provide a packaging bag that has an electrostatic ink layer produced by a digital printing machine and has sufficient resistance to heat treatment. [Explanation of symbols]

[0230] 10...Substrate, 20...Sealant layer, 30...Adhesive layer, 40...Primer layer, 50, 51...Electrostatic ink layer, 52...Printed section, 60...Bend section, 70...Stop, 72...Pouring spout, 74...Flange, 100, 110...Container, 101, 103, 111, 114, 121, 122...Seal section, 102, 112, 124, 132...Storage section, 120, 130...Packaging bag, 140...Opening means, 141...Half-cut line, 144...Easy-open processing section, 200...Body section, 300, 302, 304, 306, 310...Laminate, 400...Packaging body.

Claims

1. A container having a body portion having a bent portion, The body portion is composed of at least one laminate, the laminate includes a substrate, a primer layer, an adhesive layer, and a sealant layer in this order, and has a printed portion formed of an electrostatic ink composition on at least a part of a main surface of the primer layer on the sealant layer side, the printed portion being in direct contact with the adhesive layer; The bent portion has the printed portion, The ink coverage rate in the printed portion is 100% or more and 300% or less, The adhesive layer comprises at least one of an adhesive composition containing an epoxy compound having a molecular weight of 500 or less and a cured product thereof.

2. The container of claim 1 , wherein the epoxy compound comprises a difunctional cycloaliphatic epoxy compound.

3. The adhesive composition further comprises a polyol; 3. The container according to claim 1, wherein the polyol comprises an aliphatic polyester polyol, and the epoxy compound comprises one having epoxy groups at both ends.

4. the adhesive composition further comprises a polyisocyanate; The container of claim 3 , wherein the polyisocyanate comprises a xylylene diisocyanate derivative.

5. The container according to any one of claims 1 to 4, further comprising a plug connected to the body portion.

6. 6. The container according to claim 5, wherein the spout has a cylindrical spout and a flange extending outwardly from a periphery of a lower end of the spout.

7. The container according to any one of claims 1 to 6, wherein the body portion is formed from one sheet of the laminate.

8. The container according to any one of claims 1 to 7, wherein the body portion is composed of two of the laminates serving as side sheets and one of the laminates serving as a bottom sheet.

9. A packaging bag for heat treatment, comprising a laminate having a substrate, a primer layer, an electrostatic ink layer, an adhesive layer, and a sealant layer in this order, The packaging bag has a bent portion, The electrostatic ink layer is provided at the bent portion, The ink coverage rate of the electrostatic ink layer is 100% or more and 300% or less, the electrostatic ink layer is in direct contact with the adhesive layer; The packaging bag for heating, wherein the adhesive layer comprises at least one of an adhesive composition containing an epoxy compound and a cured product thereof.

10. The heating packaging bag according to claim 9 , wherein the primer layer comprises a polyethyleneimine resin.

11. a seal portion that bonds the sealant layers of the two laminates to each other on the outer periphery, The heating packaging bag according to claim 9 or 10, wherein the ink coverage of the electrostatic ink layer in the sealed portion is 300% or less.

12. The heating packaging bag according to any one of claims 9 to 11, wherein the epoxy compound comprises a difunctional alicyclic epoxy compound.

13. The adhesive composition further comprises a polyol; The heating packaging bag according to any one of claims 9 to 12, wherein the polyol includes an aliphatic polyester polyol, and the epoxy compound includes one having epoxy groups at both ends.

14. the adhesive composition further comprises a polyisocyanate; The heating packaging bag according to claim 13, wherein the polyisocyanate comprises a xylylene diisocyanate derivative.