Method for manufacturing colored products and mobile phone cases
Patent Information
- Application Number
- JP2023519319
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-09-25
- Filing Date
- 2021-09-24
- Publication Date
- 2024-10-02
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for manufacturing color mobile phone cases are complicated and do not provide radiation protection, failing to achieve rich colors and simplicity in processing.
The method involves using tantalum, niobium, tantalum niobium alloy, titanium, or titanium alloy materials for the case base and applying anodic oxidation and/or molten salt electrochemical methods to form amorphous metal oxide and lithium-containing compound layers, achieving rich colors and radiation reduction.
The process results in mobile phone cases with vibrant colors, reduced radiation exposure, and a simplified manufacturing process, allowing for easy color repair and change.
Abstract
Description
[Technical Field]
[0001] The present invention relates to a method for producing a colored product, in particular a method for producing a colored mobile phone case, and to a colored product, in particular a colored mobile phone case, produced by the method. [Background technology]
[0002] People often prefer colorful products, and mobile phones with beautiful exterior colors are especially likely to attract people's attention. The mobile phone industry is evolving every day, and mobile phones themselves are becoming increasingly sophisticated. At the same time, more and more attention is being paid to the appearance of mobile phones, especially the color of the mobile phone case. In addition, since mobile phones emit a certain amount of radiation, there is growing interest in producing mobile phone cases with radiation protection functions.
[0003] Chinese Patent Publication No. 106067911 describes a method for manufacturing a plastic mobile phone case, which includes the following steps: (1) mixing a plastic base material, fluorescent powder, and dye in accordance with the ratio, feeding the mixture into an injection molding machine, and then forcing the mixture into a mobile phone case mold; (2) sequentially applying a primer and a color paint, followed by vacuum coating; (3) removing the vacuum coating in the area of the vacuum coating layer that needs to reveal the color paint layer by laser engraving; (4) sequentially forming an intermediate coating layer and a UV top coat layer on the surface of the coating after the vacuum coating.
[0004] The method described in the patent requires complicated processing steps, and the plastic mobile phone case does not have radiation protection function.
[0005] Chinese Patent Publication No. 105970270 describes a process for processing two kinds of aluminum anodized colors on an aluminum metal mobile phone case, which is characterized by the following steps: Step 1: Processing the aluminum case - Processing the aluminum case using CNC cutting; Step 2: Injecting PPS resin - injecting PPS resin into the corresponding position of the aluminum case manufactured in step 1; Step 3: Primary aluminum anodizing coloring - After completing the PPS resin injection in step 2, the entire aluminum case is subjected to primary aluminum anodizing coloring. Step 4: High-gloss edge processing - After the first aluminum anodizing coloring process in step 3 is completed, a uniform, high-gloss edge is machined on the edge of the aluminum case using a CNC machine. Step 5: Covering a portion of the high-gloss edge with photosensitive protective ink - applying photosensitive protective ink to the surface of a portion of the high-gloss edge, and then baking it at a certain temperature for a certain period of time before exposing it to light; Step 6: Secondary aluminum anodizing coloring - the high-gloss edge of the part not covered with the photosensitive protective ink is subjected to secondary aluminum anodizing coloring, wherein the color of the secondary aluminum anodizing coloring is the same as the color of the first aluminum anodizing coloring; Step 7: cleaning the photosensitive protective ink—using a cleaning solution to clean the photosensitive protective ink after exposure in step 5, thereby exposing a high-gloss edge; Step 8: Tertiary aluminum anodizing coloring - After the photosensitive protective ink is washed away after exposure in Step 7, the exposed high-gloss edge is subjected to a tertiary aluminum anodizing coloring, the color of which is different from the color of the primary aluminum anodizing coloring, i.e., a process of processing two types of aluminum anodizing color on an aluminum metal mobile phone case is completed.
[0006] The method described in the patent also requires cumbersome processing steps.
[0007] Chinese Patent Publication No. 107567217 describes a method for manufacturing a case, which includes the steps of: (1) providing a metal substrate and performing hard anodizing on the metal substrate to obtain a metal substrate having a metal hard anodic oxide outer shell; (2) forming a resin film layer on one surface of the metal substrate obtained in step (1); (3) alkali-etching the substrate obtained in step (2), thereby removing the metal hard anodic oxide outer shell on the surface of the substrate where the resin film layer is not formed; and (4) acid-etching the substrate obtained in step (3), thereby removing the remaining metal in the substrate.
[0008] In the patent, the holes or etchings formed in the surface may cause a change in the color of the surface. In addition, the method described in the patent is also cumbersome in processing steps. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Chinese Patent Application Publication No. 106067911 [Patent Document 2] Chinese Patent Application Publication No. 105970270 [Patent Document 3] Chinese Patent Application Publication No. 107567217 Summary of the Invention [Problem to be solved by the invention]
[0010] Therefore, there is still a need to find a method for manufacturing color products, especially color mobile phone cases, which is simple in process and can not only achieve rich colors, but also the manufactured mobile phone cases have radiation protection function. [Means for solving the problem]
[0011] (Summary of the Invention) For this reason, the present invention provides (1) providing a product substrate; and (2) performing a surface treatment on the product substrate by employing an anodic oxidation method and / or a molten salt electrochemical method; Including, wherein the product substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, titanium, and a titanium alloy, preferably the product substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, and titanium, more preferably the product substrate is made of a material selected from tantalum, niobium, and a tantalum-niobium alloy; A method for producing a color product is provided.
[0012] The present invention also provides (1) providing a case substrate; and (2) performing a surface treatment on the case substrate by employing an anodic oxidation method and / or a molten salt electrochemical method; Including, wherein the case base is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, titanium, and a titanium alloy, preferably the case base is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, and titanium, more preferably the case base is made of a material selected from tantalum, niobium, and a tantalum-niobium alloy; A method for manufacturing a color case is provided.
[0013] The present invention further comprises: (1) providing a mobile phone case substrate; and (2) performing a surface treatment on the mobile phone case substrate by adopting an anodic oxidation method and / or a molten salt electrochemical method; Including, Wherein, the mobile phone case substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, titanium, and a titanium alloy, preferably the mobile phone case substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, and titanium, more preferably the mobile phone case substrate is made of a material selected from tantalum, niobium, and a tantalum-niobium alloy; A method for manufacturing a colored mobile phone case is provided.
[0014] The present invention further comprises: (1) the product substrate, and (2) an amorphous metal oxide layer and / or a lithium-containing compound layer formed on the surface of the product substrate; Including, wherein the product substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, titanium, and a titanium alloy, preferably the product substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, and titanium, more preferably the product substrate is made of a material selected from tantalum, niobium, and a tantalum-niobium alloy; A color product produced by the method is provided.
[0015] The present invention further comprises: (1) a case base, and (2) an amorphous metal oxide layer and / or a lithium-containing compound layer formed on the surface of the case substrate; Including, wherein the case base is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, titanium, and a titanium alloy, preferably the case base is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, and titanium, more preferably the case base is made of a material selected from tantalum, niobium, and a tantalum-niobium alloy; A color case manufactured by the above method is provided.
[0016] The present invention further comprises: (1) a mobile phone case base, and (2) an amorphous metal oxide layer and / or a lithium-containing compound layer formed on the surface of the mobile phone case substrate; Including, Wherein, the mobile phone case substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, titanium, and a titanium alloy, preferably the mobile phone case substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, and titanium, more preferably the mobile phone case substrate is made of a material selected from tantalum, niobium, and a tantalum-niobium alloy; A colored mobile phone case manufactured by the method is provided. [Effects of the Invention]
[0017] The method for producing a colored product, particularly a mobile phone case, of the present invention has one or more of the following advantageous effects: (1) a product, particularly a mobile phone case, with a wide variety of colors can be obtained; (2) the obtained colored mobile phone case has the effect of reducing the radiation dose of the mobile phone; (3) the production process is simple; and (4) color repair and color change are easy. [Brief explanation of the drawings]
[0018] [Figure 1] 1A-1C are colored tantalum foils produced under different process conditions according to an embodiment of the present invention. [Figure 2] 1A-1C are colored tantalum mobile phone cases manufactured under different process conditions according to an embodiment of the present invention. [Figure 3] 1A-1C are colored niobium foils produced under different process conditions according to an embodiment of the present invention. [Figure 4] 1A-1C are colored tantalum-niobium alloy foils produced under different process conditions according to an embodiment of the present invention. [Figure 5] 1A-1C are colored titanium foils produced under different process conditions according to an embodiment of the present invention. [Figure 6]1A-1C are colored titanium cell phone cases fabricated in molten lithium nitrate under different process conditions according to one embodiment of the present invention. [Figure 7] 10A-10C are colored titanium mobile phone cases fabricated in molten lithium nitrate under different process conditions according to another embodiment of the present invention. [Figure 8] 1A-1C are off-white and white tantalum, niobium, and tantalum-niobium alloy foils produced in molten lithium nitrate according to embodiments of the present invention. [Figure 9] 1 is a titanium cell phone case having a variety of patterns manufactured according to an embodiment of the present invention. [Figure 10] 1 is a tantalum mobile phone case with colorful patterns fabricated in a 0.05 wt % H3PO4 aqueous solution according to an embodiment of the present invention. [Figure 11] 1 is a niobium cell phone case with colorful patterns fabricated in a 0.05 wt % H3PO4 aqueous solution according to an embodiment of the present invention. [Figure 12] 1A-1C are colored tantalum, niobium, and tantalum-niobium alloy foils fabricated in lithium nitrate:potassium nitrate (1:1 weight ratio) according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE INVENTION
[0019] The method for producing colored products (e.g., mobile phone cases) of the present invention can employ anodizing and / or molten salt electrochemical processes. In particular, for tantalum, niobium, and tantalum-niobium alloys, anodizing alone can be employed, or a combination of anodizing and molten salt electrochemical processes can be employed to produce colored products, including colored mobile phone cases. For titanium and titanium alloys, anodizing is preferably employed to produce colored products, and molten salt anodizing is more preferably employed to produce colored products, including colored mobile phone cases.
[0020] Anodic oxidation method
[0021] Anodization is performed by using tantalum, niobium, tantalum-niobium alloy, titanium, or a titanium alloy product, such as a mobile phone case, as the anode and nickel, stainless steel, or other metal that is stable in the oxygen-containing electrolyte solution as the cathode in an oxygen-containing electrolyte solution at an appropriate temperature, applying an appropriate anodic voltage, and maintaining the voltage constant for an appropriate period of time.
[0022] In one embodiment, the method for producing the color product of the present invention comprises: (1) providing a product substrate; and (2) performing a surface treatment on the product substrate by anodizing; Including, The product substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, titanium, and a titanium alloy, preferably the product substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, and titanium, more preferably the product substrate is made of a material selected from tantalum, niobium, and a tantalum-niobium alloy, and also preferably the product substrate is made of a material selected from titanium and a titanium alloy.
[0023] In one embodiment, the method for producing the color case of the present invention includes the steps of: (1) providing a case substrate; and (2) performing a surface treatment on the case substrate by anodizing; Including, The case base is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, titanium, and a titanium alloy, preferably the case base is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, and titanium, more preferably the case base is made of a material selected from tantalum, niobium, and a tantalum-niobium alloy, and also preferably the case base is made of a material selected from titanium and a titanium alloy.
[0024] In one embodiment, the method for making the colored cell phone case of the present invention comprises: (1) providing a mobile phone case substrate; and (2) performing a surface treatment on the mobile phone case base by using an anodic oxidation method; Including, Wherein, the mobile phone case substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, titanium, and a titanium alloy, preferably the mobile phone case substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, and titanium, more preferably the mobile phone case substrate is made of a material selected from tantalum, niobium, and a tantalum-niobium alloy, and also preferably the mobile phone case substrate is made of a material selected from titanium and a titanium alloy.
[0025] In one preferred embodiment, the substrates, such as case substrates and cell phone case substrates, are made from tantalum.
[0026] In one preferred embodiment, the substrates, such as case substrates and cell phone case substrates, are made from niobium.
[0027] In one preferred embodiment, the substrates, such as case substrates and cell phone case substrates, are made from a tantalum-niobium alloy.
[0028] In one preferred embodiment, the substrates, such as case substrates and cell phone case substrates, are made from titanium.
[0029] In one preferred embodiment, the substrates, such as case substrates and mobile phone case substrates, are made from titanium alloys.
[0030] Preferably, the temperature of the electrolyte solution is 20°C-600°C, the anode voltage is 1V-800V, the voltage constant time is 0.01-2 hours, and the boost current density is 1-200mA / cm 2 The anodization is carried out under the condition that an amorphous metal oxide layer is formed on the surface of the substrate, such as a case substrate and a mobile phone case substrate.
[0031] The electrolyte solution includes aqueous solutions, mixtures of aqueous solutions and organic compounds, and non-aqueous solutions.
[0032] In one embodiment, the aqueous solution comprises an aqueous acid, base or salt solution, preferably an aqueous phosphoric acid solution, the concentration of which is preferably 0.01-1% by weight, more preferably 0.01-0.1% by weight, and even more preferably 0.01-0.05% by weight.
[0033] In one embodiment, in the mixture of an aqueous solution and an organic compound, the aqueous solution comprises an aqueous solution of an acid, a base, or a salt, and the organic compound comprises an alcohol organic compound, such as ethanol, ethylene glycol, n-butanol, or any combination thereof.
[0034] In one preferred embodiment, the mixture of an aqueous solution and an organic compound comprises a mixture of an aqueous solution of phosphoric acid having a concentration of 0.01-0.05 wt % and an alcohol, such as ethylene glycol, in a volume ratio of 1:1 to 1:3, preferably 1:1 to 2:1, more preferably 2:1. Preferably, the mixture of an aqueous solution and an organic compound comprises a mixture of an aqueous solution of phosphoric acid having a concentration of 0.05 wt % and an alcohol, such as ethylene glycol, in a weight ratio of 2:1.
[0035] Preferably, the non-aqueous solution includes concentrated anhydrous sulfuric acid, a molten salt, and a mixture of a molten salt and a base. Preferably, the molten salt includes molten lithium nitrate, molten sodium nitrate, molten potassium nitrate, or any combination thereof. Preferably, the base includes lithium hydroxide, sodium hydroxide, potassium hydroxide, or any combination thereof.
[0036] In one embodiment, the anodization method is carried out by placing a substrate, such as a case substrate or a mobile phone case substrate, in an aqueous electrolyte solution or a mixed solution of an aqueous electrolyte solution and an organic compound. Preferably, the temperature of the solution is 1-99°C, preferably 10-95°C, more preferably room temperature to 90°C, the anode voltage is 5-300V, the voltage holding time is 0.5-1.5 hours, and the boost current density is 5-25mA / cm. 2 is.
[0037] The solution temperature is preferably controlled between room temperature and 95°C. If the temperature is too high, the evaporation rate of water will be excessive. A relatively high solution temperature, a relatively high anodic voltage, and a relatively long constant voltage time will likely cause the amorphous metal oxide layer to crystallize. The crystallized metal oxide layer does not refract or transmit light, and therefore does not change color with film thickness (generally exhibiting a gray or off-white color).
[0038] In one embodiment, the method for manufacturing the colored mobile phone case comprises: (1) providing a mobile phone case substrate; and (2) performing a surface treatment on the mobile phone case substrate in an aqueous solution using an anodic oxidation method; Including, The mobile phone case substrate is made of tantalum.
[0039] The aqueous solution is preferably an aqueous phosphoric acid solution, more preferably an aqueous phosphoric acid solution having a concentration of 0.01-0.05% by weight.
[0040] In one preferred embodiment, a tantalum mobile phone case having a thickness of 0.01-0.3 mm is manufactured by anodizing the tantalum mobile phone case, preferably at room temperature (25°C) in a 0.01-0.05 wt% H3PO4 aqueous solution, by applying an anodic voltage of 28-32 V and maintaining the voltage constant for 0.5-1.5 hours, to obtain a blue mobile phone case.
[0041] In one preferred embodiment, a tantalum mobile phone case with a thickness of 0.01-0.3 mm is manufactured by anodizing the tantalum mobile phone case, preferably at room temperature (25°C) in a 0.01-0.05 wt% H3PO4 aqueous solution, by applying an anodic voltage of 72-84 V and maintaining the voltage constant for 0.5-1.5 hours, to obtain a gold-colored mobile phone case.
[0042] In one preferred embodiment, a tantalum mobile phone case with a thickness of 0.01-0.3 mm is manufactured by anodizing the tantalum mobile phone case, preferably at room temperature (25°C) in a 0.01-0.05 wt% H3PO4 aqueous solution, by applying an anodic voltage of 91-103 V and maintaining the voltage constant for 0.5-1.5 hours, to obtain a blue-purple mobile phone case.
[0043] In one preferred embodiment, a tantalum mobile phone case having a thickness of 0.01-0.3 mm is manufactured by anodizing the tantalum mobile phone case, preferably at room temperature (25°C) in a 0.01-0.05 wt% H3PO4 aqueous solution, by applying an anodic voltage of 150-160 V and maintaining the voltage constant for 0.5-1.5 hours, to obtain a pink mobile phone case.
[0044] In one preferred embodiment, a tantalum mobile phone case with a thickness of 0.01-0.3 mm is manufactured by anodizing the tantalum mobile phone case, preferably at room temperature (25°C) in a 0.01-0.05 wt% H3PO4 aqueous solution, by applying an anodic voltage of 203-210 V and maintaining the voltage constant for 0.5-1.5 hours, to obtain a green mobile phone case.
[0045] In another embodiment, the method for manufacturing the colored mobile phone case comprises: (1) providing a mobile phone case substrate; and (2) performing a surface treatment on the mobile phone case substrate in an aqueous solution using an anodic oxidation method; Including, The mobile phone case substrate is made of niobium.
[0046] The aqueous solution is preferably an aqueous phosphoric acid solution, more preferably an aqueous phosphoric acid solution having a concentration of 0.01-0.05% by weight.
[0047] In one preferred embodiment, a niobium mobile phone case having a thickness of 0.01-0.3 mm is manufactured by anodizing the niobium mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 21-29 V, and maintaining the voltage constant for 0.5-1.5 hours to obtain a blue mobile phone case.
[0048] In one preferred embodiment, a niobium mobile phone case having a thickness of 0.01-0.3 mm is manufactured by anodizing the niobium mobile phone case, preferably at room temperature (25°C) in a 0.01-0.05 wt% H3PO4 aqueous solution, by applying an anodic voltage of 31-38 V and maintaining the voltage constant for 0.5-1.5 hours, to obtain a silver-white mobile phone case.
[0049] In one preferred embodiment, a niobium mobile phone case having a thickness of 0.01-0.3 mm is manufactured by anodizing the niobium mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 40-48 V, and maintaining the voltage constant for 0.5-1.5 hours to obtain a gold-colored mobile phone case.
[0050] In one preferred embodiment, a niobium mobile phone case having a thickness of 0.01-0.3 mm is manufactured by anodizing the niobium mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 71-78 V, and maintaining the voltage constant for 0.5-1.5 hours to obtain a green mobile phone case.
[0051] In one preferred embodiment, a niobium mobile phone case having a thickness of 0.01-0.3 mm is manufactured by anodizing the niobium mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 105-113 V, and maintaining the voltage constant for 0.5-1.5 hours to obtain a fuchsia-colored mobile phone case.
[0052] In yet another embodiment, the method for manufacturing a colored mobile phone case comprises: (1) providing a mobile phone case substrate; and (2) performing a surface treatment on the mobile phone case substrate in an aqueous solution using an anodic oxidation method; Including, The mobile phone case substrate is made of a tantalum-niobium alloy.
[0053] The aqueous solution is preferably an aqueous phosphoric acid solution, more preferably an aqueous phosphoric acid solution having a concentration of 0.01-0.05% by weight.
[0054] In one preferred embodiment, a tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is manufactured by anodizing the tantalum-niobium alloy mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 8-18 V, and maintaining the voltage constant for 0.5-1.5 hours to obtain a chocolate-colored mobile phone case.
[0055] In one preferred embodiment, a tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is manufactured by anodizing the tantalum-niobium alloy mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 27-28 V, and maintaining the voltage constant for 0.5-1.5 hours to obtain a sky blue mobile phone case.
[0056] In one preferred embodiment, a tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is manufactured by anodizing the tantalum-niobium alloy mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 38-46 V, and maintaining the voltage constant for 0.5-1.5 hours to obtain a silver-gray mobile phone case.
[0057] In one preferred embodiment, a tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is manufactured by anodizing the tantalum-niobium alloy mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 97-102 V, and maintaining the voltage constant for 0.5-1.5 hours to obtain a marine green mobile phone case.
[0058] In one preferred embodiment, a tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is manufactured by anodizing the tantalum-niobium alloy mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 138-145 V, and maintaining the voltage constant for 0.5-1.5 hours to obtain a violet-colored mobile phone case.
[0059] In one preferred embodiment, a tantalum-niobium alloy mobile phone case with a thickness of 0.01-0.3 mm is manufactured by anodizing the tantalum-niobium alloy mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), preferably by applying an anodic voltage of 246-251 V and maintaining the voltage constant for 0.5-1.5 hours, to obtain a dark brown mobile phone case.
[0060] In one embodiment, the method for manufacturing the colored mobile phone case comprises: (1) providing a mobile phone case substrate; and (2) performing a surface treatment on the mobile phone case substrate in an aqueous solution using an anodic oxidation method; Including, The mobile phone case body is made of titanium.
[0061] The aqueous solution is preferably an aqueous phosphoric acid solution, more preferably an aqueous phosphoric acid solution having a concentration of 0.01-0.05% by weight.
[0062] In one preferred embodiment, a titanium mobile phone case with a thickness of 0.01-0.3 mm is manufactured by anodizing the titanium mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 44-54 V, and maintaining the voltage constant for 0.5-1.5 hours to obtain a white-green mobile phone case.
[0063] In one preferred embodiment, a titanium mobile phone case with a thickness of 0.01-0.3 mm is manufactured by anodizing the titanium mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 72-84 V, and maintaining the voltage constant for 0.5-1.5 hours to obtain a gold-colored mobile phone case.
[0064] In one preferred embodiment, a titanium mobile phone case having a thickness of 0.01-0.3 mm is manufactured by anodizing the titanium mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 92-109 V, and maintaining the voltage constant for 0.5-1.5 hours to obtain a fuchsia-colored mobile phone case.
[0065] In one preferred embodiment, a titanium mobile phone case with a thickness of 0.01-0.3 mm is manufactured by anodizing the titanium mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 121-133 V, and maintaining the voltage constant for 0.5-1.5 hours to obtain a green mobile phone case.
[0066] In one preferred embodiment, a titanium mobile phone case having a thickness of 0.01-0.3 mm is manufactured by anodizing the titanium mobile phone case in a 0.01-0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 159-180 V, and maintaining the voltage constant for 0.5-1.5 hours to obtain a brownish gray mobile phone case.
[0067] The anodization method can also be carried out by placing the case substrate in a non-aqueous electrolyte solution. The temperature of the electrolyte solution is from the melting point of the electrolyte solution to 500°C, the anode voltage is 3V-66V, and the voltage holding time is 0.1-80 minutes. Preferably, the temperature of the electrolyte solution is 250-380°C, the anode voltage is 10-40V, and the voltage holding time is 3 seconds-40 minutes.
[0068] In one embodiment, the method for producing the color case, in particular the mobile phone case, comprises the steps of: (1) providing a case substrate; and (2) performing a surface treatment on the case substrate in a non-aqueous solution using an anodic oxidation method; Including, The case substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium, and titanium alloy.
[0069] The oxide film formed in non-aqueous solution is porous, and its thickness, i.e., color, during the formation process of the oxide film is correlated not only with the temperature and the anodic voltage, but also with the time at which the voltage is maintained. On the other hand, in the case of anodic oxidation in aqueous solution, it is not correlated with the time at which the voltage is maintained.
[0070] The non-aqueous solution includes concentrated anhydrous sulfuric acid, molten salt, and a mixture of molten salt and a base. Preferably, the molten salt includes molten lithium nitrate, molten sodium nitrate, molten potassium nitrate, and any combination thereof. Preferably, the base includes lithium hydroxide, sodium hydroxide, potassium hydroxide, and any combination thereof.
[0071] The non-aqueous solution is preferably a molten salt, including molten potassium nitrate, molten sodium nitrate, molten lithium nitrate, and any combination thereof. Preferably, the molten salt is molten lithium nitrate.
[0072] In one embodiment, the method for producing the color case, in particular the mobile phone case, comprises the steps of: (1) providing a case substrate; and (2) performing a surface treatment on the case substrate in a non-aqueous solution using an anodic oxidation method; Including, The case body is made of titanium.
[0073] As shown in Figures 6 and 7, in one preferred embodiment, a case substrate made of titanium is anodized in lithium nitrate at 460°C under a voltage of 10V for 5 minutes to obtain a gold-colored case.
[0074] In one preferred embodiment, a case substrate made of titanium is anodized in lithium nitrate at 482° C. under a voltage of 12 V for 10 minutes to obtain a purple case.
[0075] In one preferred embodiment, a case substrate made of titanium is anodized in lithium nitrate at 460° C. under a voltage of 10 V for 60 minutes to obtain a royal blue case.
[0076] In one preferred embodiment, a case substrate made of titanium is anodized in lithium nitrate at 300-350° C. under a voltage of 10 V for 2 minutes to obtain a sky blue case.
[0077] In one preferred embodiment, a case substrate made of titanium is anodized in lithium nitrate at 482° C. under a voltage of 12 V for 10 minutes to obtain a purple case.
[0078] In one embodiment, the present invention provides a method for producing a pharmaceutical composition comprising: (1) Forming a kind of color pattern on the product substrate according to the intended pattern by anodizing and / or molten salt electrochemical methods; and (2) masking the formed color pattern, and then forming another kind of color pattern by anodizing and / or molten salt electrochemical method; Including, To provide a method for manufacturing a color product having a variety of color patterns, particularly a color mobile phone case.
[0079] In one preferred embodiment, a method for producing a color product with multiple color patterns, particularly a color mobile phone case, involves first protecting a portion of the mobile phone case with an adhesive tape having a specific pattern, then anodizing the mobile phone case to form a color pattern, then peeling off the adhesive tape, and protecting the color pattern formed on the mobile phone case with another adhesive tape, followed by further anodizing the mobile phone case to form another color pattern. Naturally, multiple adhesive tapes can be used to protect the mobile phone case during anodizing, thereby producing a mobile phone case with multiple colors, for example, three or more colors. The adhesive tape used is typically waterproof and resistant to the anodizing conditions used.
[0080] In one preferred embodiment, a method for producing a color product having various color patterns, particularly a color mobile phone case, includes the steps of: (1) Determine the metal material and specific pattern on the mobile phone case; (2) Determine the colors of any patterns on the phone case; (3) Determine the surface treatment sequence for achieving each pattern color of the mobile phone case. This sequence should follow the principle of gradually decreasing oxide film thickness, i.e., the thickness of the film corresponding to the pattern color that is first surface treated (or anodized) should be greater than the thickness of the film of the color that is subsequently treated; and (4) First, use waterproof, acid-resistant adhesive tape to protect the area other than the pattern to be anodized first, and peel it off after the first oxidation treatment is completed. Then, use the same adhesive tape protection method to anodize the next pattern until all patterns are finally treated. Including, The waterproof adhesive tape should also meet the resistance requirements of the anodizing conditions used, such as temperature, acid resistance, etc.
[0081] Molten Salt Electrochemistry
[0082] In one embodiment, the method for producing the color case, in particular the mobile phone case, comprises the steps of: (1) providing a case substrate; and (2) performing a surface treatment on the case substrate using a molten salt electrochemical method; Including, The case substrate is made of a material selected from tantalum, niobium, and a tantalum-niobium alloy.
[0083] Preferably, the molten salt electrochemistry is a molten lithium salt electrochemistry.
[0084] Preferably, the molten salt electrochemical method involves placing the case substrate in a molten mixture of an oxygen-containing inorganic lithium salt, a molten mixture of an oxygen-containing inorganic lithium salt and lithium hydroxide, a molten mixture of a salt and lithium hydroxide, or a molten mixture of a lithium salt and an oxygen-containing salt at 200°C to 650°C, applying an anode voltage of 1 to 66 V, and keeping the voltage constant for 3 seconds to 60 hours, for example, 0.1 to 90 minutes, during which the boost current density is 1 to 1000 mA / cm. 2 and obtaining a white or off-white case. Preferably, an ultrasonic generator is placed in the mixed melt or the mixed molten liquid.
[0085] Preferably, the temperature of the mixed melt or the mixed melt is 250°C-520°C, the applied anode voltage is 5-25V, and the boosted current density is 5-20mA / cm 2 is.
[0086] In one preferred embodiment, the oxygen-containing inorganic lithium salt is LiNO3.
[0087] In one preferred embodiment, the molten mixture of a lithium salt and an oxygen-containing salt is a molten mixture of LiNO3 and KNO3.
[0088] In one preferred embodiment, the mixed molten liquid of the lithium salt and the oxygen-containing salt is a mixed molten liquid of LiNO3 and KNO3 in a weight ratio of 1:2 to 2:1, preferably 1:1.
[0089] For the mixed melt or mixed melt, such as nitrates such as LiNO3, NaNO3, and KNO3, the thickness of the amorphous metal oxide film (layer) formed at a relatively high temperature increases with increasing anodization time. After reaching a certain thickness, the amorphous metal oxide film can electrochemically react with the nitrates, thereby forming a white or off-white lithium tantalate film, lithium niobate film, or a mixed lithium tantalate and lithium niobate film, especially at a relatively high temperature and a relatively high anodization voltage.
[0090] In one embodiment, the method for producing the color case, in particular the mobile phone case, comprises the steps of: (1) providing a case substrate; and (2) performing a surface treatment on the case substrate using a molten salt electrochemical method; Including, The case substrate is made of tantalum.
[0091] In one embodiment, a case substrate made of tantalum is immersed in lithium nitrate at 440° C.-650° C. under a constant voltage of 5-50 V for 3 seconds-5 hours to obtain a white case.
[0092] In one preferred embodiment, a case substrate made of tantalum is immersed in lithium nitrate at 570°C-585°C under a constant voltage of 8-50V for 2 minutes to 5 hours to obtain a white case.
[0093] In one embodiment, a case substrate made of niobium is subjected to a constant voltage of 5-48V for 2 seconds to 2 hours in a lithium nitrate:potassium nitrate mixture (weight ratio of 1:2 to 2:1, preferably 1:1) at 380°C-550°C to obtain a white case.
[0094] In one preferred embodiment, a case substrate made of niobium is immersed in a mixture of lithium nitrate and potassium nitrate (weight ratio of 1:2 to 2:1, preferably 1:1) at 450°C-480°C under a constant voltage of 5-28V for 2-30 minutes to obtain a white case.
[0095] In one embodiment, the method for producing the color case, in particular the mobile phone case, comprises the steps of: (1) providing a case substrate; and (2) performing a surface treatment on the case substrate by using an anodic oxidation method and a molten salt electrochemical method; Including, The case substrate is made of a material selected from tantalum, niobium, and tantalum-niobium alloys.
[0096] In one preferred embodiment, a case substrate made of a tantalum-niobium alloy is subjected to a constant voltage of 135-145 V for 1-2 hours in a 0.01-0.05 wt % HPO aqueous solution, and then subjected to a constant voltage of 25-32 V for 1-3 hours in a lithium nitrate:potassium nitrate (weight ratio 1:2 to 2:1, preferably 1:1) solution at 460-585°C, to obtain a white case.
[0097] Additionally, a combination of anodizing and molten salt electrochemical processes can be used to form white or other color combination patterns on a mobile phone case. For example, a mobile phone case made of tantalum, niobium, or a tantalum-niobium alloy can be electrochemically reacted with an appropriate anodic voltage in a molten oxygen-containing lithium salt, such as lithium nitrate, or a mixture of lithium nitrate and potassium nitrate or sodium nitrate, to form a corresponding white lithium tantalate film, lithium niobate film, or a mixture of lithium tantalate and lithium niobate. If the desired pattern is white and the contrasting background color is a colorful anodic oxide film, mechanical polishing or HF acid etching can be used to remove the white film outside the pattern until the metallic tantalum, niobium, or tantalum-niobium alloy is exposed. The desired color anodic oxide film can then be formed by anodizing in a dilute aqueous solution or molten salt.
[0098] The color product produced by the method of the present invention is (1) the product substrate, and (2) an amorphous metal oxide layer and / or a lithium-containing compound layer, preferably an amorphous metal oxide layer, formed on the surface of the substrate; Including, The article substrate is made from a material selected from tantalum, niobium, tantalum-niobium alloys, titanium and titanium alloys, preferably the article substrate is made from a material selected from tantalum, niobium, tantalum-niobium alloys and titanium, preferably the article substrate is made from a material selected from tantalum, niobium and tantalum-niobium alloys.
[0099] The color case manufactured by the method of the present invention is (1) a product case base, and (2) an amorphous metal oxide layer and / or a lithium-containing compound layer, preferably an amorphous metal oxide layer, formed on the surface of the housing substrate; Including, The case substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, titanium, and a titanium alloy, preferably the case substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, and titanium, more preferably the case substrate is made of a material selected from tantalum, niobium, and a tantalum-niobium alloy.
[0100] The colored mobile phone case produced by the method of the present invention is (1) a product mobile phone case base; and (2) an amorphous metal oxide layer and / or a lithium-containing compound layer, preferably an amorphous metal oxide layer, formed on the surface of the mobile phone case substrate; Including, The mobile phone case substrate is made from a material selected from tantalum, niobium, a tantalum-niobium alloy, titanium, and a titanium alloy, preferably the mobile phone case substrate is made from a material selected from tantalum, niobium, a tantalum-niobium alloy, and titanium, more preferably the mobile phone case substrate is made from a material selected from tantalum, niobium, and a tantalum-niobium alloy.
[0101] In one embodiment, the amorphous metal oxide comprises amorphous tantalum pentoxide, amorphous niobium pentoxide, amorphous titanium dioxide, and mixtures thereof.
[0102] In one preferred embodiment, the lithium-containing compound includes lithium tantalate, lithium niobate, and mixtures thereof.
[0103] In one preferred embodiment, the case substrate has a thickness of 0.01-0.5 mm, preferably 0.02-0.3 mm.
[0104] The case base of the present invention can be manufactured by techniques known in the art, such as cutting, casting, rolling, etc., and there are no particular limitations.
[0105] In the context of the present invention, the mobile phone case includes a mobile phone body case, a mobile phone decorative case, a mobile phone protective case, and so on.
[0106] In the context of the present invention, color products include cases such as mobile phone cases and computer cases, accessories such as rings, bracelets, necklaces and watch bands, pendants such as Buddha statues, human figures and animal figures, etc.
[0107] In one embodiment, a transparent plastic case may be added to the exterior of the mobile phone case of the present invention, thereby protecting the mobile phone from damage in the event of an accidental collision. By fitting the mobile phone case of the present invention into the transparent plastic case, the objectives of scratch resistance and deformation resistance can be achieved, while the transparent plastic case allows the vivid colors of the colored mobile phone case to be appreciated. Additionally, the mobile phone decorative case or mobile phone protective case fitted into the transparent plastic case can be easily converted to other colors.
[0108] In another embodiment, the mobile phone case of the present invention, such as a decorative mobile phone case or a protective mobile phone case, can be integrally bonded to a plastic transparent case, for example, by placing the metal mobile phone case of the present invention inside the transparent plastic case, thereby ensuring that when the plastic mobile phone case is removed, careless handling will not cause scratches, abrasions, or deformations to the metal mobile phone case.
[0109] In the context of the present invention, "color" should be construed to include, but not be limited to, red, green, blue, yellow, purple, gold, white, silver-white, gray, and the like.
[0110] Unless otherwise specified, all % or percentages herein are calculated on a weight basis.
[0111] The present invention can be easily understood by those skilled in the art through the following preferred embodiments, but these preferred embodiments are not intended to limit the scope of the present invention.
[0112] 1. (1) providing a product substrate; and (2) performing a surface treatment on the product substrate by employing an anodic oxidation method and / or a molten salt electrochemical method; Including, The article substrate is made from a material selected from tantalum, niobium, tantalum-niobium alloys, titanium, and titanium alloys; A method for producing a color product.
[0113] 2. (1) providing a case substrate; and (2) performing a surface treatment on the case substrate by employing an anodic oxidation method and / or a molten salt electrochemical method; Including, The case substrate is made of a material selected from tantalum, niobium, a tantalum-niobium alloy, titanium, and a titanium alloy. 2. The method of embodiment 1.
[0114] 3. (1) providing a mobile phone case substrate; and (2) performing a surface treatment on the mobile phone case substrate by adopting an anodic oxidation method and / or a molten salt electrochemical method; Including, The mobile phone case substrate is made of a material selected from tantalum, niobium, tantalum-niobium alloy, titanium, and titanium alloy; 3. The method of embodiment 2.
[0115] 4. Step (2) is - forming a kind of color pattern on the substrate according to the intended pattern by anodizing and / or molten salt electrochemical methods; and - masking the formed color pattern, and then forming another kind of color pattern by anodizing and / or molten salt electrochemical method; 4. The method of any one of embodiments 1-3, comprising:
[0116] 5. The temperature of the electrolyte solution is 20°C-600°C, the anode voltage is 1V-800V, the voltage constant time is 3 seconds-5 hours, preferably 30 seconds-1.5 hours, and the boost current density is 1-200mA / cm 2 4. The method of any one of embodiments 1-3, wherein the anodization is carried out under conditions where:
[0117] 6. The method of embodiment 5, wherein the electrolyte solution comprises an aqueous solution, a mixture of an aqueous solution and an organic compound, and a non-aqueous solution.
[0118] 7. The method of embodiment 6, wherein the aqueous solution comprises an aqueous solution of an acid, base or salt, preferably an aqueous phosphoric acid solution, and the concentration of the aqueous phosphoric acid solution is 0.01-1% by weight, preferably 0.01-0.05% by weight.
[0119] 8. The method of embodiment 6, wherein in the mixture of aqueous solution and organic compound, the aqueous solution comprises an aqueous solution of an acid, base or salt, and the organic compound comprises an alcohol, such as ethanol, ethylene glycol, n-butanol, or any combination thereof.
[0120] 9. The method of embodiment 6, wherein the mixture of aqueous solution and organic compound comprises a mixture of aqueous H3PO4 solution with a concentration of 0.01-0.05 wt % and ethylene glycol in a weight ratio of 1:1 to 3:1, preferably 1:1 to 2:1.
[0121] 10. The method of embodiment 6, wherein the non-aqueous solution comprises concentrated anhydrous sulfuric acid, molten salt, and a mixture of molten salt and a base-like substance.
[0122] 11. The method of embodiment 10, wherein the molten salt comprises molten lithium nitrate, molten sodium nitrate, molten potassium nitrate, and any combination thereof.
[0123] 12. The method of embodiment 10, wherein the base-like substance comprises lithium hydroxide, sodium hydroxide, potassium hydroxide, and any combination thereof.
[0124] 13. The method of embodiment 6, wherein the electrolyte solution is an aqueous solution or a mixture of an aqueous solution and an organic compound, the anodization is performed under the following conditions: the temperature of the electrolyte solution is 1-99°C, the anode voltage is 5V-600V, and the voltage constant time is 90 minutes or less; preferably, the temperature of the electrolyte solution is from room temperature to 95°C, the anode voltage is 10-200V, and the voltage constant time is 30-60 minutes.
[0125] 14. The method of embodiment 13, wherein a tantalum mobile phone case having a thickness of 0.01-0.3 mm is manufactured, and the tantalum mobile phone case is subjected to an anodizing method, preferably at room temperature (25°C) in a 0.01-0.05 wt% H3PO4 aqueous solution, at an anodic voltage of 72-84 V, and the voltage is kept constant for 0.5-1.5 hours, to obtain a gold-colored mobile phone case.
[0126] 15. The method of embodiment 13, wherein a niobium mobile phone case having a thickness of 0.01-0.3 mm is manufactured, and the niobium mobile phone case is subjected to an anodizing method, preferably at room temperature (25°C) in a 0.01-0.05 wt% H3PO4 aqueous solution, at an anodic voltage of 40-48 V, and the voltage is kept constant for 0.5-1.5 hours, to obtain a gold-colored mobile phone case.
[0127] 16. The method of embodiment 13, wherein a tantalum-niobium alloy mobile phone case having a thickness of 0.01-0.3 mm is manufactured, and the tantalum-niobium alloy mobile phone case is subjected to an anodic oxidation method, preferably at room temperature (25°C) in a 0.01-0.05 wt% H3PO4 aqueous solution, at an anodic voltage of 27-28 V, and the voltage is kept constant for 0.5-1.5 hours, to obtain a sky blue mobile phone case.
[0128] 17. The method of embodiment 13, wherein a titanium mobile phone case having a thickness of 0.01-0.3 mm is manufactured, and the titanium mobile phone case is subjected to an anodizing method, preferably at room temperature (25°C) in a 0.01-0.05 wt% H3PO4 aqueous solution, by applying an anodic voltage of 72-84 V, and maintaining the voltage constant for 0.5-1.5 hours, to obtain a gold-colored mobile phone case.
[0129] 18. The method of embodiment 6, wherein the anodizing method is performed under the following conditions: when the electrolyte solution is a non-aqueous solution, the temperature of the electrolyte solution is from the melting point of the electrolyte solution material to 500°C, the anode voltage is 3V-66V, and the voltage constant time is within 60 minutes; preferably, the temperature of the electrolyte solution is 250-350°C, the anode voltage is 5-40V, and the voltage constant time is 3-30 minutes.
[0130] 19. The method of embodiment 18, wherein the case substrate is made of titanium and is anodized in lithium nitrate at 460° C. under a voltage of 10 V for 5 minutes to obtain a gold-colored case.
[0131] 20. The molten salt electrochemical method includes placing a substrate in a molten oxygen-containing inorganic lithium salt, a mixed melt of an oxygen-containing inorganic lithium salt and lithium hydroxide, a mixed melt of a salt and lithium hydroxide, or a mixed melt of a lithium salt and an oxygen-containing salt at 250°C-650°C, applying an anode voltage of 1-66 V, and maintaining the voltage constant for 0.01-60 hours, wherein the boost current density is 1-1000 mA / cm. 2 and obtaining a white or off-white mobile phone case.
[0132] 21. The temperature of the mixed melt or the mixed melt is 300°C-520°C, the applied anode voltage is 5-25V, and the boost current density is 5-20mA / cm 2 21. The method of embodiment 20, wherein
[0133] 22. The method of embodiment 20, wherein the oxygen-containing inorganic lithium salt is LiNO3.
[0134] 23. The method of embodiment 20, wherein a case substrate made of tantalum is subjected to a constant voltage of 8-50V in lithium nitrate at 440-650°C for 2 minutes to 5 hours to obtain a white case.
[0135] 24. The method of embodiment 20, wherein a case substrate made of niobium is subjected to heating at 380-550°C in a lithium nitrate / potassium nitrate mixture in a weight ratio of 1:2 to 2:1, preferably 1:1, at a constant voltage of 5-28 V for 2-30 minutes to obtain a white case.
[0136] twenty five. (1) providing a case substrate; and (2) performing a surface treatment on the case substrate by using an anodic oxidation method and a molten salt electrochemical method; Including, The case substrate is made of a material selected from tantalum, niobium, and a tantalum-niobium alloy. 4. The method of embodiment 2 or 3.
[0137] 26. The method of embodiment 25, wherein a case substrate made of a tantalum-niobium alloy is subjected to constant voltage application at 135-145 V for 1-2 hours in an aqueous solution of 0.01-0.05 wt % H3PO4, and then subjected to constant voltage application at 25-32 V for 1-3 hours in a mixture of lithium nitrate and potassium nitrate in a weight ratio of 1:2 to 2:1, preferably 1:1, at 400-585°C, to obtain a white case.
[0138] 27. (1) the product substrate, and (2) an amorphous metal oxide layer and / or a lithium-containing compound layer, preferably an amorphous metal oxide layer, formed on the surface of the substrate; Including, the product substrate is made from a material selected from tantalum, niobium, a tantalum-niobium alloy, titanium, and a titanium alloy, preferably the product substrate is made from a material selected from tantalum, niobium, a tantalum-niobium alloy, and titanium, more preferably the product substrate is made from a material selected from tantalum, niobium, and a tantalum-niobium alloy; 27. A color product produced by the method of any one of embodiments 1-26.
[0139] 28. The color product of embodiment 27, wherein the amorphous metal oxide comprises amorphous tantalum pentoxide, amorphous niobium pentoxide, amorphous titanium dioxide, and mixtures thereof.
[0140] 29. The color product of embodiment 27 or 28, wherein the lithium-containing compound comprises lithium tantalate, lithium niobate, and mixtures thereof.
[0141] 30. The color product according to embodiment 27 or 28, wherein the color product includes cases such as mobile phone cases and computer cases, accessories such as rings, bracelets, necklaces and watch bands, pendants such as Buddha statues, human figures and animal figures.
[0142] 31. The color product of embodiment 30, wherein the mobile phone case includes a mobile phone body case, a mobile phone decorative case, and a mobile phone protective case. [Example]
[0143] Certain exemplary embodiments are described below with reference to the accompanying drawings. As will be recognized by those skilled in the art, the described embodiments may be modified in various ways without departing from the spirit or scope of the invention. Accordingly, the accompanying drawings and descriptions are to be regarded as illustrative in nature, rather than restrictive.
[0144] Example 1 Tantalum mobile phone cases with a thickness of 0.28 mm were manufactured using an anodization method. The tantalum mobile phone cases were placed in a 0.05 wt % H3PO4 aqueous solution at room temperature and subjected to anodic voltages of 1-286 V. The voltage was kept constant for 40 minutes to obtain colorful tantalum mobile phone cases. Among these, blue tantalum mobile phone cases were obtained at 30 V, gold tantalum mobile phone cases at 78 V, purple tantalum mobile phone cases at 95 V, green tantalum mobile phone cases at 125 V, yellow tantalum mobile phone cases at 142 V, and rose red tantalum mobile phone cases at 168 V, as shown in Figure 1.
[0145] Example 2 A tantalum mobile phone case with a thickness of 0.03 mm was manufactured by anodizing the tantalum mobile phone case in a 0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 30 V, and maintaining the voltage constant for 40 minutes to obtain a blue tantalum mobile phone case, as shown in Figure 2.
[0146] Example 3 A tantalum mobile phone case with a thickness of 0.03 mm was manufactured by anodizing the tantalum mobile phone case in a 0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 75 V, and maintaining the voltage constant for 40 minutes to obtain a gold-colored tantalum mobile phone case, as shown in Figure 2.
[0147] Example 4 A tantalum mobile phone case with a thickness of 0.02 mm was manufactured by anodizing the tantalum mobile phone case in a 0.05 wt % H3PO4 aqueous solution at room temperature (25°C), and an anodic voltage of 100 V was applied to the tantalum mobile phone case, and the voltage was kept constant for 40 minutes, resulting in a blue-purple tantalum mobile phone case, as shown in Figure 2.
[0148] Example 5 A tantalum mobile phone case with a thickness of 0.075 mm was manufactured by anodizing the tantalum mobile phone case in a 0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 110 V, and maintaining the voltage constant for 40 minutes to obtain a blue-green tantalum mobile phone case, as shown in Figure 2.
[0149] Example 6 A tantalum mobile phone case with a thickness of 0.03 mm was manufactured by anodizing the tantalum mobile phone case in a 0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 120 V, and maintaining the voltage constant for 40 minutes to obtain a light green tantalum mobile phone case, as shown in Figure 2.
[0150] Example 7 A tantalum mobile phone case with a thickness of 0.05 mm was manufactured by anodizing the tantalum mobile phone case in a 0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 154 V, and maintaining the voltage constant for 40 minutes to obtain a light pink tantalum mobile phone case, as shown in Figure 2.
[0151] Example 8 A tantalum mobile phone case with a thickness of 0.1 mm was manufactured by anodizing the tantalum mobile phone case in a 0.05 wt % H3PO4 aqueous solution at room temperature (25°C), and an anodic voltage of 160 V was applied to the tantalum mobile phone case, and the voltage was kept constant for 40 minutes to obtain a pink tantalum mobile phone case, as shown in Figure 2.
[0152] Example 9 A tantalum mobile phone case with a thickness of 0.03 mm was manufactured by anodizing the tantalum mobile phone case in a 0.05 wt % H3PO4 aqueous solution at room temperature (25°C), and an anodic voltage of 178 V was applied to the tantalum mobile phone case, and the voltage was kept constant for 40 minutes to obtain a purple tantalum mobile phone case, as shown in Figure 2.
[0153] Example 10 A tantalum mobile phone case with a thickness of 0.03 mm was manufactured by anodizing the tantalum mobile phone case in a 0.05 wt % H3PO4 aqueous solution at room temperature (25°C), applying an anodic voltage of 205 V, and maintaining the voltage constant for 40 minutes to obtain a green tantalum mobile phone case, as shown in Figure 2.
[0154] Example 11 Niobium mobile phone cases with a thickness of 0.03 mm were fabricated using an anodization method. The niobium mobile phone cases were immersed in a 0.05 wt% H3PO4 aqueous solution at room temperature and subjected to anodic voltages of 1-210 V. The voltage was maintained constant for 40 minutes to obtain colorful niobium mobile phone cases. Among these, blue niobium cases were obtained at 25 V, silver-white niobium cases at 36 V, gold niobium cases at 44 V, jewel green niobium cases at 73 V, and fuchsia niobium cases at 108 V, as shown in Figure 3.
[0155] Example 12 Tantalum-niobium alloy (6:4 weight ratio) mobile phone cases with thicknesses of 0.1 mm or 0.28 mm were fabricated using an anodization method. The tantalum-niobium alloy cases were subjected to anodic voltages of 1-260 V in a 0.05 wt % H3PO4 aqueous solution at room temperature (25°C) and maintained at a constant voltage for 40 minutes to obtain colorful tantalum-niobium alloy cases. Among these, sky blue tantalum-niobium alloy cases were obtained at 0.1 mm and 28 V, gray tantalum-niobium alloy cases at 0.1 mm and 43 V, marine green tantalum-niobium alloy cases at 0.28 mm and 100 V, violet tantalum-niobium alloy cases at 0.1 mm and 141 V, and dark brown tantalum-niobium alloy cases at 0.28 mm and 249 V, as shown in Figure 4.
[0156] Example 13 Titanium mobile phone cases with a thickness of 0.02 mm were fabricated using an anodization method. The titanium mobile phone cases were then immersed in a 0.05 wt % H3PO4 aqueous solution at room temperature (25°C) and subjected to anodic voltages of 1-197 V. The voltage was maintained constant for 40 minutes to obtain colorful titanium mobile phone cases. Among these, silver-gray niobium cases were obtained at 16 V, silver-white niobium cases at 24 V, gold niobium cases at 82 V, rose-red niobium cases at 98 V, and rose-brown niobium cases at 175 V, as shown in Figure 5.
[0157] Example 14 A 0.02 mm thick titanium mobile phone case was fabricated, and then an anodic voltage of 10 V was applied to the titanium mobile phone case in a molten lithium nitrate solution at 300°C, and the voltage was kept constant for 2 minutes to obtain a blue titanium mobile phone case, as shown in Figure 6.
[0158] Example 15 A titanium mobile phone case with a thickness of 0.02 mm was manufactured, and then an anodic voltage of 10 V was applied to the titanium mobile phone case in a molten lithium nitrate solution at 350°C, and the voltage was kept constant for 2 minutes, resulting in a sky blue titanium mobile phone case, as shown in Figure 6.
[0159] Example 16 A titanium mobile phone case with a thickness of 0.02 mm was fabricated, and then an anodic voltage of 12 V was applied to the titanium mobile phone case in a molten lithium nitrate solution at 482°C, and the voltage was kept constant for 0.5 minutes, resulting in a rose-red titanium mobile phone case, as shown in Figure 6.
[0160] Example 17 A titanium mobile phone case with a thickness of 0.02 mm was manufactured, and then an anodic voltage of 12 V was applied to the titanium mobile phone case in a molten lithium nitrate solution at 482°C, and the voltage was kept constant for 10 minutes, resulting in a purple titanium mobile phone case, as shown in Figure 6.
[0161] Example 18 A titanium mobile phone case with a thickness of 0.02 mm was fabricated, and then an anodic voltage of 10 V was applied to the titanium mobile phone case in a molten lithium nitrate solution at 460°C, and the voltage was kept constant for 1 minute, resulting in a light yellow titanium mobile phone case, as shown in Figure 7.
[0162] Example 19 A titanium mobile phone case with a thickness of 0.02 mm was fabricated, and then an anodic voltage of 10 V was applied to the titanium mobile phone case in a molten lithium nitrate solution at 460°C, and the voltage was kept constant for 2 minutes, resulting in a light yellow titanium mobile phone case, as shown in Figure 7.
[0163] Example 20 A titanium mobile phone case with a thickness of 0.02 mm was fabricated and then immersed in a molten lithium nitrate solution at 460°C, at which an anodic voltage of 10 V was applied, and the voltage was kept constant for 5 minutes to obtain a gold-colored titanium mobile phone case, as shown in Figure 7.
[0164] Example 21 A titanium mobile phone case with a thickness of 0.02 mm was fabricated and then immersed in a molten lithium nitrate solution at 460°C, at which an anodic voltage of 10 V was applied, and the voltage was kept constant for 15 minutes to obtain a titanium mobile phone case with a Kyoto purple color, as shown in Figure 7.
[0165] Example 22 A titanium mobile phone case with a thickness of 0.02 mm was manufactured, and then an anodic voltage of 10 V was applied to the titanium mobile phone case in a molten lithium nitrate solution at 460°C, and the voltage was kept constant for 20 minutes, resulting in a light purple titanium mobile phone case, as shown in Figure 7.
[0166] Example 23 A 0.02 mm thick titanium mobile phone case was fabricated and then placed in a molten lithium nitrate solution at 460°C, at which an anodic voltage of 10 V was applied, and the voltage was kept constant for 30 minutes to obtain a purple titanium mobile phone case, as shown in Figure 7.
[0167] Example 24 A titanium mobile phone case with a thickness of 0.02 mm was manufactured, and then an anodic voltage of 10 V was applied to the titanium mobile phone case in a molten lithium nitrate solution at 460°C, and the voltage was kept constant for 35 minutes, resulting in a maroon-colored titanium mobile phone case, as shown in Figure 7.
[0168] Example 25 A titanium mobile phone case with a thickness of 0.02 mm was fabricated, and then an anodic voltage of 10 V was applied to the titanium mobile phone case in a molten lithium nitrate solution at 460°C, and the voltage was kept constant for 60 minutes, resulting in a jewel blue titanium mobile phone case, as shown in Figure 7.
[0169] Example 26 A tantalum mobile phone case with a thickness of 0.05 mm was manufactured, and an anodic voltage of 10 V was applied to the tantalum mobile phone case in molten lithium nitrate at 580°C, and the voltage was kept constant for 3 seconds and 60 seconds, resulting in an off-white tantalum mobile phone case, as shown in Figure 8.
[0170] Example 27 A 0.28 mm thick mobile phone case was manufactured, and an anode voltage of 10 V was applied to the tantalum mobile phone case in molten lithium nitrate at 580°C, and the voltage was kept constant for 3 seconds to 10 minutes to react, resulting in a gray or white tantalum mobile phone case, as shown in Figure 8.
[0171] Example 28 A tantalum-niobium alloy mobile phone case with a thickness of 0.05 mm was manufactured by first immersing the tantalum-niobium alloy mobile phone case in a 0.05 wt% H3PO4 aqueous solution at 90°C and maintaining a constant voltage of 143 V for 1.5 hours, then applying a voltage of 28 V to the tantalum-niobium alloy mobile phone case in a molten lithium nitrate:potassium nitrate (1:1 weight ratio) solution at 482°C, and carrying out a constant voltage electrochemical reaction for 3 hours to obtain a white tantalum-niobium alloy mobile phone case, as shown in Figure 8.
[0172] Example 29 A tantalum-niobium alloy mobile phone case with a thickness of 0.28 mm was manufactured by first immersing the tantalum-niobium alloy mobile phone case in a 0.05 wt% H3PO4 aqueous solution at 90°C and maintaining a constant voltage of 143 V for 1.5 hours, then applying a voltage of 28 V to the tantalum-niobium alloy mobile phone case in a molten lithium nitrate:potassium nitrate (1:1 weight ratio) solution at 482°C, and carrying out a constant voltage electrochemical reaction for 3 hours to obtain a white tantalum-niobium alloy mobile phone case, as shown in Figure 8.
[0173] Example 30 A niobium mobile phone case with a thickness of 0.05 mm was manufactured, and a voltage of 10 V was applied to the niobium mobile phone case in molten lithium nitrate:potassium nitrate (1:1 weight ratio) at 460°C, and the voltage was kept constant for 20 minutes to obtain a white niobium mobile phone case, as shown in Figure 8.
[0174] Example 31 A niobium mobile phone case with a thickness of 0.28 mm was manufactured, and a voltage of 10 V was applied to the niobium mobile phone case in molten lithium nitrate:potassium nitrate (1:1 weight ratio) at 460°C, and the voltage was kept constant for 20 minutes to obtain a white niobium mobile phone case, as shown in Figure 8.
[0175] Example 32 A 0.03 mm thick titanium foil was prepared and protected with adhesive tape. A voltage of 15 V was applied to the titanium foil in molten lithium nitrate at 268°C, and the voltage was held constant for 5 minutes, resulting in a blue background pattern. The stripe pattern was then protected with adhesive tape. A voltage of 10 V was then applied to the titanium foil in molten lithium nitrate at 268°C, and the voltage was held constant for 5 minutes, resulting in a purple stripe pattern. This is shown in Sample 1 in Figure 9.
[0176] Example 33 A 0.03 mm thick titanium foil was prepared and protected with adhesive tape. A voltage of 10 V was applied to the titanium foil in molten lithium nitrate at 268°C, and the voltage was held constant for 5 minutes, resulting in a purple background pattern. The stripe pattern was then protected with adhesive tape. A voltage of 5 V was then applied to the titanium foil in molten lithium nitrate at 268°C, and the voltage was held constant for 5 minutes, resulting in a gold stripe pattern. This is shown in Sample 2 in Figure 9.
[0177] Example 34 A 0.03mm thick titanium foil was prepared and protected with adhesive tape. A voltage of 15V was applied to the titanium foil in molten lithium nitrate at 268°C, and the voltage was held constant for 5 minutes, resulting in a blue background pattern. The bull pattern was then protected with adhesive tape. A voltage of 5V was then applied to the titanium foil in molten lithium nitrate at 268°C, and the voltage was held constant for 5 minutes, resulting in a bull pattern. This is shown in Sample 3 in Figure 9.
[0178] Example 35 Tantalum foils with thicknesses of 0.05 mm or 0.075 mm were prepared and protected with adhesive tape in a 0.05 wt % H3PO4 aqueous solution. A constant voltage was applied for 30 minutes for each of the various colors in the order shown in the figure, resulting in tantalum foils with various color patterns, as shown in Figure 10. In Sample 1, Background 1 is purple, Stripe 2 is blue, and Stripe 3 is gold. In Sample 2, the five-pointed star and Chinese pattern are gold, and the background is purple. In Sample 3, the five-pointed star and Chinese pattern are gold, and the background is blue-purple. In Sample 4, the bull pattern is gold, and the background is blue. In Sample 5, the bull pattern is gold, and the background is purple.
[0179] Example 36 Niobium foils with a thickness of 0.05 mm were prepared and protected with adhesive tape in a 0.05 wt% H3PO4 aqueous solution. The voltages were kept constant for 20 minutes for each of the colors under the voltages corresponding to the numbers in the figure, resulting in various color patterns of niobium foils, as shown in Figure 11.
[0180] Table 1 below shows the measured mobile phone radiation in various directions when a mobile phone is attached to a mobile phone case of the present invention and making a call. Tested at Tsinghua University Electromagnetic Testing Center.
[0181] [Table 1] The results in Table 1 show that the mobile phone case of the present invention has a certain radiation protection effect. Compared to a mobile phone not equipped with the mobile phone case of the present invention, a mobile phone equipped with the case of the present invention had reduced radiation in all directions during a call.
[0182] While specific embodiments of the present invention have been shown and described, other modifications, alternatives, and options will be apparent to those skilled in the art. Such modifications, alternatives, and optional embodiments may be made without departing from the spirit and scope of the present invention, which is determined by the appended claims. Various features of the present invention are set forth in the appended claims.
Claims
1. (1) providing a product substrate; and (2) performing a surface treatment on the product substrate by adopting anodizing and / or molten salt electrochemical methods; Including, The article substrate is made from a material selected from the group consisting of tantalum, niobium, tantalum-niobium alloys, titanium, and titanium alloys; A method for producing a color product.
2. (1) providing a mobile phone case substrate; and (2) carrying out a surface treatment on the mobile phone case substrate by adopting anodizing and / or molten salt electrochemical methods; Including, The mobile phone case substrate is made of a material selected from the group consisting of tantalum, niobium, tantalum-niobium alloys, titanium, and titanium alloys; The method of claim 1.
3. The temperature of the electrolyte solution is 20°C-600°C, the anode voltage is 1V-800V, the voltage constant time is 3 seconds-5 hours, and the boost current density is 1-200mA / cm 2 2. The method of claim 1, wherein the anodization process is carried out under conditions whereby an amorphous metal oxide layer and / or a lithium-containing compound layer is formed on the surface of the substrate.
4. The method of claim 3 , wherein the electrolyte solution comprises an aqueous solution, a mixture of an aqueous solution and an organic compound, and a non-aqueous solution.
5. The method according to claim 4, wherein when the electrolyte solution is an aqueous solution or a mixture of an aqueous solution and an organic compound, the anodization is performed under the conditions that the temperature of the electrolyte solution is 1-99°C, the anode voltage is 5V-600V, and the voltage constant time is within 90 minutes.
6. A tantalum mobile phone case having a thickness of 0.01-0.3 mm was manufactured, and the tantalum mobile phone case was anodized by adding 0.01-0.05 wt % H at room temperature (25° C.) using an anodizing method. 3 P.O. 4 The method according to claim 5, wherein an anodic voltage of 72-84V is applied in the aqueous solution, and the voltage is kept constant for 0.5-1.5 hours to obtain a gold-colored mobile phone case.
7. A niobium mobile phone case having a thickness of 0.01-0.3 mm is manufactured, and the niobium mobile phone case is anodized by anodizing at room temperature (25° C.) with 0.01-0.05 wt % H 3 P.O. 4 The method according to claim 5, wherein an anodic voltage of 40-48V is applied in the aqueous solution, and the voltage is kept constant for 0.5-1.5 hours to obtain a gold-colored mobile phone case.
8. A tantalum-niobium alloy mobile phone case having a thickness of 0.01-0.3 mm is manufactured, and the tantalum-niobium alloy mobile phone case is subjected to anodization at room temperature (25° C.) with 0.01-0.05 wt % H. 3 P.O. 4 The method according to claim 5, wherein an anodic voltage of 27-28V is applied in the aqueous solution, and the voltage is kept constant for 0.5-1.5 hours to obtain a sky blue mobile phone case.
9. A titanium mobile phone case having a thickness of 0.01-0.3 mm was manufactured, and the titanium mobile phone case was anodized by adding 0.01-0.05 wt % H at room temperature (25° C.) using an anodizing method. 3 P.O. 4 The method according to claim 5, wherein an anodic voltage of 72-84V is applied in the aqueous solution, and the voltage is kept constant for 0.5-1.5 hours to obtain a gold-colored mobile phone case.
10. 5. The method according to claim 4, wherein the anodization is performed under the conditions that when the electrolyte solution is a non-aqueous solution, the temperature of the electrolyte solution is from the melting point of the electrolyte solution material to 500° C., the anode voltage is 3V-66V, and the voltage constant time is within 60 minutes.
11. 11. The method according to claim 10, wherein the case body made of titanium is subjected to an anodizing process in lithium nitrate at 460° C. under a voltage of 10 V for 5 minutes to obtain a gold-colored case.
12. The molten salt electrochemical method includes disposing a substrate in an oxygen-containing inorganic lithium salt, a mixed melt of an oxygen-containing inorganic lithium salt and lithium hydroxide, a mixed melt of a salt and lithium hydroxide, or a mixed melt of a lithium salt and an oxygen-containing salt at 250°C to 650°C, applying an anode voltage of 1 to 66 V, and keeping the voltage constant for 0.01 to 60 hours, wherein the boost current density is 1 to 1000 mA / cm 2 13. The method of claim 1, wherein the cell phone case is white or off-white in color.
13. The oxygen-containing inorganic lithium salt is LiNO 3 The method of claim 12, wherein
14. The method according to claim 12, wherein the case body is made of tantalum, and the voltage is kept constant at 8-50V for 2 minutes to 5 hours in lithium nitrate at 440-650°C to obtain a white case.
15. The method according to claim 12, wherein the case substrate is made of niobium, and the white case is obtained by subjecting the case substrate to a constant voltage of 5-28V in a lithium nitrate / potassium nitrate mixture having a weight ratio of 1:2 to 2:1 at 380-550°C for 2-30 minutes.
16. (1) a product substrate; and (2) an amorphous metal oxide layer and / or a lithium-containing compound layer formed on the surface of the product substrate; Including, The article substrate is made of a material selected from the group consisting of tantalum, niobium, tantalum-niobium alloys, titanium, and titanium alloys; A color product produced by the method of claim 1.
17. 17. The color product of claim 16, wherein the amorphous metal oxide comprises amorphous tantalum pentoxide, amorphous niobium pentoxide, amorphous titanium dioxide, and mixtures thereof.
18. 17. The color product of claim 16, wherein the lithium-containing compounds include lithium tantalate, lithium niobate, and mixtures thereof.
19. 17. The color product of claim 16, wherein the color products include mobile phone cases and computer cases, finger rings, bracelets, necklaces and watch bands, Buddha statues, human figures and animal figures.
20. 20. The color product of claim 19, wherein the mobile phone cases include a mobile phone body case, a mobile phone decorative case and a mobile phone protective case.