Apparatus, system and method for manufacturing electrodes, electrode stacks and batteries

JP2023553115A5Active Publication Date: 2024-11-29ENOVIX CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023535005
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-12-09
Filing Date
2021-12-07
Publication Date
2024-11-29
Estimated Expiration
2041-12-07

AI Technical Summary

Technical Problem

Existing manufacturing techniques for three-dimensional secondary batteries face challenges in balancing improved capacity and longevity with reduced manufacturing costs and defects, often leading to increased productivity costs and reduced battery life.

Method used

A process involving the merging and separation of electrode webs using a receiving member with protrusions to align and overlap substrate components, along with a punch system to separate electrode subunits, enhancing precision and efficiency in electrode assembly.

Benefits of technology

This approach preserves or improves battery capacity and life while reducing manufacturing defects and costs, enabling faster production of high-quality electrode assemblies for secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The web merging process for manufacturing secondary battery electrode assemblies includes: moving a first web, the first web including a first component population for electrode subunits, the first components defined by corresponding weakening patterns, and a first transport feature population; moving a second web, the second component population for electrode subunits, the second components defined by corresponding weakening patterns, and a second transport feature population; conveying a receiving member, the receiving member including multiple protrusions; receiving the first web with the receiving member; and overlapping the second web with the first web so that the first component is aligned with the second component and the transport features of the second web are engaged by the multiple protrusions of the receiving member. The second web merge location is spaced from that of the first web.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] Cross-reference with related applications This application claims priority to U.S. Provisional Patent Application No. 63 / 123328, filed on 9 December 2020, which is incorporated herein by reference in its entirety.

[0002] U.S. Provisional Patent Application No. 63 / 115266 filed November 18, 2020, U.S. Provisional Patent Application No. 63 / 080345 filed September 18, 2020, and U.S. Provisional Patent Application No. 63 / 081686 filed September 22, 2020, U.S. Patent Application No. 16 / 533082 filed August 6, 2019, claiming priority to U.S. Provisional Patent Application No. 62 / 715233 filed August 6, 2018, and International Patent Application No. PCT / US2018 / 061245 filed November 15, 2018, claiming priority to U.S. Provisional Patent Application No. 62 / 586737 filed November 15, 2017, and U.S. Provisional Patent Application No. 62 / 715233 filed August 6, 2018. The contents of each of these applications are incorporated herein by reference in their entirety.

[0003] field The field of this disclosure generally relates to energy storage technologies, such as battery technologies. More specifically, the field of this disclosure relates to systems and methods for assembling energy storage systems, such as electrodes for use in secondary batteries, including lithium-based batteries. [Background technology]

[0004] background Lithium-based rechargeable batteries are a desirable energy source due to their relatively high energy density, output, and shelf life. Examples of lithium-based rechargeable batteries include non-aqueous batteries such as lithium-ion batteries and lithium polymer batteries.

[0005] Known energy storage devices such as batteries, fuel cells, and electrochemical capacitors typically have a two-dimensional laminar structure, such as a planar or helically wound (i.e., jelly roll) laminate structure, where the surface area of ​​each laminate is approximately equal to its geometric footprint (neglecting porosity and surface roughness).

[0006] Figure 1 is a cross-sectional view of a known layered secondary battery, generally denoted as 10. The battery 10 includes a positive electrode current collector 15 in contact with a positive electrode 20. The negative electrode 25 is separated from the positive electrode 20 by a separator layer 30. The negative electrode 25 is in contact with a negative electrode current collector 35. As shown in Figure 1, the battery 10 is formed in a stack. The stack may also be covered with another separator layer (not shown) on top of the negative electrode current collector 35, and then rolled up and placed in a can (not shown) to assemble the battery 10. During the charging process, carrier ions (typically lithium) leave the positive electrode 20 and move through the separator layer 30 to the negative electrode 25. Depending on the anode material used, the carrier ions either intercalate (e.g., settle into the matrix of the negative electrode material without forming an alloy) or form an alloy with the negative electrode material. During the discharging process, the carrier ions leave the negative electrode 25 and return to the positive electrode 20 through the separator layer 30.

[0007] Three-dimensional rechargeable batteries have the potential to offer improved capacity and lifespan compared to layered rechargeable batteries. However, manufacturing such three-dimensional batteries presents manufacturing and cost challenges. While existing precision manufacturing techniques can produce rechargeable batteries with improved cycle life, they come at the expense of productivity and manufacturing costs. However, increasing the speed of known manufacturing techniques may increase defects, reduce capacity, and shorten battery life.

[0008] Therefore, it is desirable to manufacture three-dimensional batteries while addressing the problems of publicly known technologies. [Overview of the project]

[0009] One embodiment is a process for merging webs to manufacture an electrode assembly for a secondary battery, in which, A step of moving a web of a first substrate along a first web merge path, wherein the web of the first substrate includes (i) a group of first components for an electrode subunit, the first components being a group of first components defined by a corresponding weakening pattern, and (ii) a group of first transport features. A step of moving a web of a second substrate along a second web merge path, wherein the web of the second substrate includes (iii) a group of second components for an electrode subunit, the second components being defined by a corresponding weakening pattern, and (iv) a group of second transport features; A process of transporting a receiving member in the web merging direction adjacent to a first web merging path and a second web merging path, wherein the receiving member comprises a plurality of protrusions configured to engage with a first transport feature of the web of the first substrate and a second transport feature of the web of the second substrate. The process includes receiving the web of the first substrate on a receiving member at a first web merge position such that the conveying features of the web of the first substrate are engaged by at least some of the multiple protrusions on the belt, A step of overlapping the web of the second substrate on the web of the first substrate on a receiving member at a second web merge position such that the first component is substantially aligned with the second component and the conveying features of the web of the second substrate are engaged by at least some of the multiple protrusions on the belt, wherein the second web merge position is spaced apart from the first web merge position in the down-web direction; include.

[0010] Another embodiment is a process for merging webs to manufacture an electrode assembly for a secondary battery, in which, A step of moving a web of a first substrate along a first web merge path, wherein the web of the first substrate includes (i) a group of first electrode components for an electrode subunit, the first electrode components being a group of first electrode components defined by a corresponding weakening pattern, and (ii) a group of first transport features, and the web of the first substrate includes a web of electrode material. A step of moving a web of a second substrate along a second web merge path, wherein the web of the second substrate includes (iii) a group of separator components defined by a corresponding weakening pattern, and (iv) a group of second transport features, and the web of the second substrate includes a web of separator material. A process of transporting a receiving member in the web merging direction adjacent to a first web merging path and a second web merging path, wherein the receiving member comprises a plurality of protrusions configured to engage with a first transport feature of the web of the electrode material and a second transport feature of the web of the separator material. A step of receiving one of the electrode material web and the separator material web on a belt at a first web merge position such that the respective transport features of the electrode material web and the separator material web are engaged by at least some of the multiple protrusions on the belt, A step of overlapping the web of the electrode material and the other web of the separator material at a second web merge position, such that the respective transport features of the web of the electrode material and the other web of the separator material are engaged by at least a portion of a plurality of protrusions on the belt, and the separator structure is substantially aligned with the first electrode structure, wherein the second web merge position is spaced down the web from the first web merge position. include.

[0011] Another embodiment is a process for separating electrode subunits from a group of electrode subunits in a layered arrangement of a laminated web, In this process, each electrode subunit is defined within the laminated web by a corresponding weakening pattern. The process is A step of positioning the layered electrode subunits of a laminated web at the punch position between a receiving unit and a punch head, wherein the receiving unit includes a base, alignment pins, and a movable platform, A process of positioning the alignment pins of the receiving unit through the fiducial features of the electrode subunit, A step of positioning the movable platform at a predetermined position between the lower surface of the electrode subunit and the base of the receiving unit, A step of applying force to an electrode subunit using a punch head, wherein the force is large enough to separate the electrode subunit from the array of the laminated web along a weakening pattern. Includes.

[0012] Another embodiment is a system for separating electrode subunits from a group of electrode subunits within an array of stacked webs, in which, The electrode subunit is defined by the corresponding weakening pattern. The system is A receiving unit having at least two alignment pins extending therefrom, the alignment pins being positioned to engage with corresponding fiducial features of an electrode subunit and facing a first surface of the electrode subunit, A movable punch head comprising at least two punch head holes, wherein the punch head holes are sized and positioned to receive one corresponding alignment pin, and the punch head is positioned to face the opposing surface of an electrode subunit, A controller is configured to cause the punch head to apply sufficient force to the opposing surface of the electrode subunit to separate the electrode subunit from the array of laminated web along the weakening pattern. Includes.

[0013] Another embodiment is a system for separating electrode subunits from a group of electrode subunits within an array of stacked webs, in which, The electrode subunit is defined by the corresponding weakening pattern. The system A receiving unit having a base and a movable platform, wherein the movable platform is selectively positionable at a predetermined position between the array of laminated webs and the base, A movable punch head positioned to face the opposing surface of the electrode subunit, A controller configured to cause a punch head to apply sufficient force to the opposing surface of an electrode subunit to separate the electrode subunit from the array of laminated webs along a weakening pattern, wherein the movable platform of the receiving unit is selectively positioned to receive the electrode subunit separated from the array of laminated webs, and Includes.

[0014] Another embodiment is a system for merging webs to manufacture electrode assemblies for secondary batteries, in which, A first merge zone configured to move a web of a first substrate along a first web merge path, the web of the first substrate comprising a group of first components for an electrode subunit and a group of first transport features, the first components being defined by a corresponding weakening pattern, the first merge zone and A second merge zone configured to move the web of a second substrate along a second web merge path, the web of the second substrate comprising a group of second components for an electrode subunit and a group of second transport features, the second components being defined by a corresponding weakening pattern, the second merge zone A receiving member comprising a plurality of protrusions, wherein the receiving member is positioned adjacent to a first web merge path and a second web merge path, and the plurality of protrusions are configured to engage with a first transport feature of the web of the first substrate and a second transport feature of the web of the second substrate. Includes, The first merge zone is adapted to transport the web of the first substrate onto the receiving member at the first web merge position such that the transport features of the web of the first substrate are engaged by at least some of the multiple protrusions on the belt. The second merge zone is adapted to transport the web of the second substrate onto the receiving member at the second web merge position such that the second component is substantially aligned with the first component and the transport features of the web of the second substrate are engaged by at least some of the multiple projections on the belt. The second merge zone is spaced down the web from the first merge zone. [Brief explanation of the drawing]

[0015] [Figure 1] Figure 1 is a cross-sectional view of an existing (prior art) layered battery. [Figure 2] Figure 2 is a schematic diagram of a preferred embodiment of the electrode manufacturing system according to the present disclosure. [Figure 3] Figure 3 is an enlarged schematic diagram of a preferred embodiment of the laser system according to this disclosure. [Figure 4] Figure 4 is an isometric view of a preferred embodiment of the cutting plenum according to the present disclosure. [Figure 5] Figure 5 is a cross-sectional top view of an exemplary web of a substrate formed on an electrode after processing through the electrode manufacturing system of the present disclosure. [Figure 6] Figure 6 is a top view of an exemplary substrate web having an electrode pattern formed thereon. [Figure 6A] Figure 6A is a perspective view of a portion of the web of a substrate used as an exemplary negative electrode. [Figure 6B]Figure 6B is a perspective view of a portion of the web of a substrate used as an exemplary cathode. [Figure 7] Figure 7 is an enlarged top view of a portion of the web of a substrate having an exemplary electrode pattern formed thereon. [Figure 8] Figure 8 is an isometric view of a substrate formed on a web of electrode material containing an electrode pattern after processing through the electrode manufacturing system of the present disclosure. [Figure 8A] Figure 8A is a top view of a portion of the web of the electrode material shown in Figure 8. [Figure 9] Figure 9 is an isometric view of a preferred embodiment of the winding roller of the electrode manufacturing system of the present disclosure. [Figure 10] Figure 10 is a top view of a preferred embodiment of the brushing station of the present disclosure. [Figure 11] Figure 11 is a side view of an exemplary brushing station shown in Figure 10. [Figure 12] Figure 12 is an isometric view of a preferred embodiment of the inspection station according to the present disclosure. [Figure 13] Figure 13 is a top view of a chuck according to a preferred embodiment of the present disclosure. [Figure 14] Figure 14 is a partial schematic diagram of the combined and stacked arrangement according to this disclosure. [Figure 14A] Figure 14A is a partial side view of the merge zone according to this disclosure. [Figure 14B] Figure 14B is a magnified detail view illustrating a portion of the unwinding section of the stacked device shown in Figure 14A. [Figure 14C1] Figures 14C1-14C3 are side, top, and front views of the merged configuration according to this disclosure. [Figure 14C2] Figures 14C1-14C3 are side, top, and front views of the merged configuration according to this disclosure. [Figure 14C3] Figures 14C1- are side, top, and front views of the merged configuration according to this disclosure. [Figure 14D] Figure 14D is an isometric view of the electrode material tensioning section of the electrode manufacturing system of the present disclosure. [Figure 14E1] Figures 14E1-14E4 include side and top views of a non-tapered projection (top) and a tapered projection (bottom) according to embodiments of the present disclosure. [Figure 14E2] Figures 14E1-14E4 include side and top views of a non-tapered projection (top) and a tapered projection (bottom) according to embodiments of the present disclosure. [Figure 14E3] Figures 14E1-14E4 include side and top views of a non-tapered projection (top) and a tapered projection (bottom) according to embodiments of the present disclosure. [Figure 14E4] Figures 14E1-14E4 include side and top views of a non-tapered projection (top) and a tapered projection (bottom) according to embodiments of the present disclosure. [Figure 14F1] Figures 14F1-14F3 show isometric (left), top (center), and side (right) views of a reverse-rotating brush according to an embodiment of the present disclosure. [Figure 14F2] Figures 14F1-14F3 show isometric (left), top (center), and side (right) views of a reverse-rotating brush according to an embodiment of the present disclosure. [Figure 14F3] Figures 14F1-14F3 show isometric (left), top (center), and side (right) views of a reverse-rotating brush according to an embodiment of the present disclosure. [Figure 14G] Figure 14G shows a magnified view of the initial contact point shown in Figure 14B of a web having a merged sprocket according to an embodiment of the present disclosure. [Figure 14H1] Figures 14H1-3 show three views of the web interacting with the merge sprocket according to embodiments of the present disclosure: a side view (i), a top view (ii), and an isometric view (iii). [Figure 14H2] Figures 14H1-3 show three views of the web interacting with the merge sprocket according to embodiments of the present disclosure: a side view (i), a top view (ii), and an isometric view (iii). [Figure 14H3] Figures 14H1-3 show three views of the web interacting with the merge sprocket according to embodiments of the present disclosure: a side view (i), a top view (ii), and an isometric view (iii). [Figure 15]Figure 15 is a cross-sectional view of a multilayer stack of electrodes according to this disclosure. [Figure 15A] Figure 15A is a partial top view of the web of the electrode material according to this disclosure. [Figure 16A] Figure 16A is a side view of a multilayer stack of electrode subunits according to this disclosure. [Figure 16B] Figure 16B is a partial top view of the multilayer stack of the electrode subunit shown in Figure 16A. [Figure 16C] Figure 16C is a partial top view of the multilayer stack in Figure 16A after the rupture of the second perforation. [Figure 17] Figure 17 is an isometric view of the stacked cell according to this disclosure. [Figure 18A] Figures 18A and 18B are serial isometric views of a stacked cell having a battery package placed on top of it. [Figure 18B] Figures 18A and 18B are serial isometric views of a stacked cell having a battery package placed on top of it. [Figure 19] Figure 19 is a side view of the merge section of the system of this disclosure. [Figure 20] Figure 20 is a side view of the high-capacity stacking system of this disclosure. [Figure 20A] Figure 20A is a partial close-up view of the toothed area below the large stacking system in Figure 20. [Figure 21] Figure 21 is a perspective view of the receiving unit according to this disclosure. [Figure 22] Figure 22 is a front view of the receiving unit shown in Figure 21. [Figure 23] Figure 23 is a schematic diagram of one embodiment of the punching stacking system of the present disclosure. [Figure 24A] Figures 24A, 24B, and 24C are top views of the merged material web highlighting the electrode subunit, electrode subunit, and series of stacked electrode subunits of the present disclosure, respectively. [Figure 24B]Figures 24A, 24B, and 24C are top views of the merged material web highlighting the electrode subunit, electrode subunit, and series of stacked electrode subunits of the present disclosure, respectively. [Figure 24C] Figures 24A, 24B, and 24C are top views of the merged material web highlighting the electrode subunit, electrode subunit, and series of stacked electrode subunits of the present disclosure, respectively. [Figure 24D] Figure 24D is a section view of an embodiment of a merged material web containing a group of electrode subunits. [Figure 24E] Figure 24E is an isometric view of the receiving unit of this disclosure. [Figure 24F] Figure 24F is a front view showing a receiving unit having a group of electrode subunits stacked on top of it. [Figure 25] Figure 25 is an isometric view of the demarg sprocket of the punched-out laminated system of the present disclosure. [Figure 26A] Figure 26A is a top view of a punch head during punching operations according to an embodiment of the present disclosure. [Figure 26B] Figure 26B is an isometric view of the punch head shown in Figure 26A. [Figure 26C] Figure 26C is a detailed view of a portion of Figure 26A, specifically part 26C. [Modes for carrying out the invention]

[0016] As used herein, “A,” “an,” and “the” (i.e., singular) refer to multiple references unless the context clearly indicates otherwise. For example, in one example, a reference to “electrode” includes both a single electrode and multiple similar electrodes.

[0017] As used herein, “approximately” and “about” refer to plus or minus 10%, 5%, or 1% of the stated value. For example, approximately 250 μm includes 225 μm to 275 μm. For another example, approximately 1,000 μm includes 900 μm to 1,100 μm. Unless otherwise indicated, all numerical values ​​used in this specification and in the claims, such as quantities (e.g., measured values), are understood in all cases to be modified by the term “approximately.” Therefore, unless otherwise indicated, the numerical parameters described in the following specification and in the appended claims are approximations. Each numerical parameter should be interpreted using common rounding techniques, taking into account at least the number of significant figures reported.

[0018] In this specification, the term "anode" as used in the context of secondary batteries refers to the negative electrode of a secondary battery.

[0019] As used herein, "anode material" or "anode activity" refers to a material suitable for use as the negative electrode of a secondary battery.

[0020] In the context of rechargeable batteries, "cathode" refers to the positive electrode of the battery.

[0021] As used herein, "cathode material" or "cathode activity" means a material suitable for use as the positive electrode of a secondary battery.

[0022] As used herein in the context of a secondary battery cycle between a charged state and a discharged state, “cycle” means charging and / or discharging the battery in order to move it within a cycle from a first state, which is either a charged state or a discharged state, to a second state which is the opposite of the first state (i.e., a charged state if the first state was a discharged state, or a discharged state if the first state was a charged state), and then returning the battery to the first state to complete the cycle. For example, a single cycle of a secondary battery between a charged state and a discharged state may include a charge cycle, which charges the battery from a discharged state to a charged state, and then returns it to a discharged state to complete the cycle. A single cycle may also include a discharge cycle, which discharges the battery from a charged state to a discharged state, and then charges it back to a charged state to complete the cycle.

[0023] As used herein, "electrochemically active material" means either an anode-active material or a cathode-active material.

[0024] As used herein, the term "electrode" may refer to the negative or positive electrode of a secondary battery unless the context clearly indicates otherwise.

[0025] As used herein, "electrode current collector layer" may refer to an anode (e.g., negative) current collector layer or a cathode (e.g., positive) current collector layer.

[0026] As used herein, “electrode material” may refer to either an anode material or a cathode material unless the context explicitly indicates otherwise.

[0027] As used herein, “electrode structure” may refer to an anode structure (e.g., negative electrode structure) or a cathode structure (e.g., positive electrode structure) adapted for use in a battery, unless the context explicitly indicates otherwise.

[0028] As used herein, “longitudinal axis,” “horizontal axis,” and “vertical axis” refer to mutually orthogonal axes (i.e., axes that are each orthogonal to each other). For example, as used herein, “longitudinal axis,” “horizontal axis,” and “vertical axis” are analogous to the Cartesian coordinate system used to define three-dimensional aspects or orientations. Thus, the descriptions of elements of the subject disclosed herein are not limited to any particular axis or axis used to describe the three-dimensional orientation of the element. Alternatively, the axes may be interchangeable when referring to the three-dimensional aspects of the disclosed subject.

[0029] A "weakened region" refers to a part of the web that has undergone processing operations such as scoring, cutting, or drilling, in which the local fracture strength of the weakened region is lower than that of the unweakened region.

[0030] Detailed explanation Embodiments of this disclosure relate to apparatus, systems, and methods for manufacturing electrode components for batteries, such as three-dimensional rechargeable batteries, which improve the manufacturing speed of battery components while maintaining or improving battery capacity and battery life and reducing the occurrence of defects during the manufacturing process.

[0031] An exemplary system for manufacturing electrode components, including electrodes and separators used in batteries, is described with reference to Figure 2. Generally, the electrode production (or manufacturing) system, represented by 100, includes numerous individual stations, systems, components, or devices that function to enable the efficient production of precision electrodes used in batteries. The manufacturing system 100 is first described in general terms with respect to Figure 2, then a more broad description of the manufacturing system 100 is presented, followed by further details of each component.

[0032] In the illustrated exemplary embodiment, the manufacturing system 100 includes a base unwinding roller 102 for holding and unwinding a base web 104. The base web 104 may be an electrode material suitable for manufacturing electrode assemblies for secondary batteries (i.e., a web of anode material or a web of cathode material), a separator material, and the like. The base web 104 is a thin sheet of material wound into a roll and has a central through-hole sized for placement on the base unwinding roller 102. In some embodiments, the base web 104 is a multilayer material including, for example, an electrode current collector layer (i.e., an anode current collector layer or a cathode current collector layer) and an electrochemically active material layer on at least one of its main faces (i.e., an anode active material layer or a cathode active material layer), while in other embodiments, the base web may be a single layer (e.g., a web of separator material). The base unwinding roller 102 may be formed from a metal, a metal alloy, a composite material, a plastic, or any other material that enables the manufacturing system 100 to function as described herein. In one embodiment, the rewind roller 102 is made of stainless steel and has a diameter of 3 inches (76.2 mm).

[0033] As shown in the embodiment of Figure 2, the substrate web 104 is passed across an edge guide 106 to facilitate the unwinding of the substrate web 104. In one embodiment, the edge guide 106 uses a through-beam type optical sensor to detect the position of one edge of the substrate web 104 relative to a fixed reference point. Feedback is sent from the edge guide 106 to a “web steering” roller, generally an unwinding roller 102, which moves in a direction perpendicular to the direction of movement of the substrate web 104. In this embodiment, the substrate web 104 then passes around an idler 108a and enters the splicing station 110. The idler 108a (sometimes called an idler roller) facilitates proper positioning and tension maintenance of the substrate web 104, as well as facilitating the reorientation of the substrate web 104. In the embodiment shown in Figure 2, idler 108a receives the substrate web 104 vertically and is partially wrapped around idler 108a such that the substrate web 104 moves away from idler 108a substantially 90 degrees from the input direction in the output direction. However, it should be understood that the input and output directions may vary without departing from the scope of this disclosure. In some embodiments, the manufacturing system 100 may use a plurality of idlers 108a-108x to change the orientation of the substrate web once or more times as the substrate web is transported through the manufacturing system 100. Idlers 108a-108x may be formed from metal, metal alloy, composite, plastic, rubber, or any other material that enables the manufacturing system 100 to function as described herein. In one embodiment, idlers 108a-108x are made of stainless steel and have dimensions of 1 inch (25.4 mm) in diameter and 18 inches (457.2 mm) in length.

[0034] The splicing station 110 is configured to facilitate the splicing of two separate webs together. In one preferred embodiment, the web 104 of the first substrate is unwound so that the trailing edge (not shown) of the substrate web 104 stops within the splicing station 110, and the leading edge (not shown) of the second substrate web 104 is unwound within the splicing station 110 so that the trailing edge of the first web and the leading edge of the second web are adjacent to each other. The user can then apply an adhesive, such as adhesive tape, to join the leading edge of the second web to the trailing edge of the first web, forming a seam between the two webs and creating a continuous substrate web. Such a process can be repeated for multiple substrate webs 104 at the user's direction. Thus, the splicing station 110 makes it possible to splice multiple substrate webs to form a single continuous web. In other embodiments, it should be understood that the user can, as desired, splice together webs of the same or different materials.

[0035] In one preferred embodiment, upon leaving the splicing station 110, the substrate web 104 is transported down the web direction WD to enter the nip roller 112. The nip roller 112 is configured to facilitate control of the speed at which the substrate web 104 is transported through the manufacturing system 100. In one embodiment, the nip roller 112 includes at least two adjacent rollers having a space between them that defines a nip. The nip is such that the substrate web 104 is pressed against each of the two adjacent rollers 114 (also called the “nip rollers”) with enough pressure to allow friction between the rollers to move the substrate web 104, but with enough pressure to avoid significant deformation or damage to the substrate web 104. In some preferred embodiments, the pressure exerted on the substrate web 104 by the nip roller 114 is such that the web cross-web span S WThe force is set between 0 and 210 pounds, such as 0 pounds, 5 pounds, 10 pounds, 15 pounds, 20 pounds, 25 pounds, 30 pounds, 35 pounds, 40 pounds, 45 pounds, 50 pounds, 55 pounds, 65 pounds, 70 pounds, 75 pounds, 80 pounds, 85 pounds, 90 pounds, 95 pounds, 100 pounds, 110 pounds, 120 pounds, 130 pounds, 140 pounds, 150 pounds, 160 pounds, 170 pounds, 180 pounds, 190 pounds, 200 pounds, or 210 pounds, across the web edge-to-edge distance (i.e., the distance from edge to edge of the web in the cross-web direction XWD) (Figures 6 and 8A).

[0036] In one preferred embodiment, at least one of the adjacent rollers 114 may be a compliant roller, which may be a high-friction roller driven by an electric motor, and the other adjacent roller may be a low-friction passive roller. The compliant roller may have at least an outer surface made of rubber or polymer that can provide sufficient grip to the web 104 of the substrate and impart a pushing or pulling force to the web 104 of the substrate for transport through the manufacturing system 100. In one embodiment, at least one of the adjacent rollers 114 is a steel roller having a diameter of about 3.863 inches (98.12 mm). In another embodiment, at least one of the adjacent rollers 114 is a rubber roller having a diameter of about 2.54 inches (64.51 mm). In yet another embodiment, one or more of the adjacent rollers 114 include a rubber ring positioned above it, which is adjustable to be positioned at any position along the width of the roller, and each ring has an outer diameter of about 3.90 inches (99.06 mm). In one embodiment, one or more rubber rings are positioned on the rollers and contact the web 104 of the substrate with their continuous outer edges to drive the web 104 of the substrate in the down-web direction WD. Thus, the speed of the web 104 of the substrate is controlled by controlling the rotational speed of the high-friction rollers via the user interface 116. In an embodiment, the speed of the web in the web direction is controlled to be between 0.001 m / s and 10 m / s. In an embodiment, the maximum speed of the web in the web direction WD is directed by the inertia of the web and system components so that the web maintains proper alignment, flatness and tension as further described herein. In other embodiments, each of the adjacent rollers 114 may be made of any high-friction or low-friction material, enabling the manufacturing system 100 to function as described herein. It should be understood that one or both of the adjacent rollers 114 may be connected to a motor (not shown) for controlling the speed of the web 104 of the substrate as it passes through the nip.The manufacturing system 100 may include one or more additional nip rollers 122, 132 to facilitate control of the speed of the substrate web 104 being transported through the manufacturing system 100, which can be controlled via a user interface 116. If multiple nip rollers are used, each nip roller may be set to the same speed via the user interface 116 so that the substrate web 104 is transported smoothly through the manufacturing system 100. In the embodiment, the speed of the substrate web 104 in the web direction WD is controlled to be between 0.001 m / s and 10 m / s.

[0037] The manufacturing system 100 may also include a dancer 118. As shown in Figure 2, the illustrated dancer 118 includes a pair of rollers spaced apart from each other, but the pair of rollers of the dancer 118 are connected around a central axis. The pair of rollers of the dancer 118 can rotate around the central axis, thereby passively adjusting the tension of the web 104 of the substrate. For example, when the tension of the web 104 of the substrate exceeds a predetermined threshold, the pair of rollers of the dancer 118 rotate around the central axis to reduce the tension of the web. Thus, the dancer 118 may use, alone, the mass of the dancer (e.g., the mass of one or more of the pair of rollers), springs, torsion rods, or other bias / tensioning devices that may be adjustable or controllable by the user via the user interface 116 to ensure that the appropriate tension is consistently maintained on the web of the substrate. In one embodiment, the mass of the dancer 118 and the inertia of the dancer are reduced or minimized to allow web tension of 500 grams-force or less, for example by using hollow rollers made of aluminum. In other embodiments, the rollers of the Dansa 118 are made of other lightweight materials such as carbon fiber, aluminum alloy, magnesium, other lightweight metals and metal alloys, glass fiber, or any other suitable material that allows for a mass low enough to provide web tension at 500 grams or less. In yet another embodiment, the rollers of the Dansa 118 are counterbalanced to allow for tension on the web 104 of a substrate at 250 grams or less.

[0038] The manufacturing system 100 includes one or more laser systems 120a, 120b, 120c. The embodiment shown in Figure 2 includes three laser systems 120a-c, but it should be understood that any number of laser systems may be used to enable the manufacturing system 100 to function as described herein. Further description of the laser systems 120a-c is made with reference to Figure 3. In one preferred embodiment, at least one of the laser systems 120a-c includes a laser device 300 configured to emit a laser beam 302 toward a cutting plenum 304 (Figure 3). In the illustrated embodiment, the cutting plenum 304 includes a chuck 306 and a vacuum 308. Details of the chuck 306 are best shown in Figures 4 and 13 and will be further described below. In one preferred embodiment, as also illustrated in Figure 4, one or more inspection systems 310, 312 are provided adjacent to the laser system 120, which may be visual inspection devices such as cameras, or any other preferred inspection systems that enable the manufacturing system 100 to function as further described herein.

[0039] The exemplary manufacturing system 100 shown in Figure 2 includes one or more cleaning stations, such as a brushing station 124 and an air knife 126. Each cleaning station is configured to remove or otherwise facilitate the removal of debris (not shown) from the web 104 of the substrate, as will be further described herein.

[0040] The manufacturing system 100 in Figure 2 includes, as further described herein, an inspection device 128 for identifying defects and a related defect marking device 130 for marking the web 104 of the substrate to identify the location of the identified defects.

[0041] In one preferred embodiment, the base material web 104 is wound together with the web of the interleaf material 138 via the winding roller 134 and unwound via the interleaf material roller 136 to create a roll of electrodes 140 having layers of electrodes separated by the interleaf material 138. In some embodiments, the base material web 104 can be wound via the winding roller 134 without the web of the interleaf material 138.

[0042] It should be noted that the series of nip rollers 112, 122, 132, idlers 108a-x, and dancers 118a-x may be referred to together with the conveying system for conveying the web 104 of the substrate through the manufacturing system 100. As used herein, conveying system or conveying the web 104 of the substrate refers to intentionally moving the web 104 of the substrate in the web direction WD through the production system.

[0043] Referring to Figure 5, the substrate web 104 may be any material suitable for manufacturing electrode components for use in batteries as described herein. For example, the substrate web 104 may be an electrically insulating separator material 500, an anode material 502, or a cathode material 504. In one preferred embodiment, the substrate web 104 is an electrically insulating and ion-permeable polymer woven fabric material suitable for use as a separator in a secondary battery.

[0044] In another preferred embodiment, again referring to Figure 5, the substrate web 104 is a web of anode material 502 which may include an anode current collector layer 506 and an anode active material layer 508. The anode current collector layer 506 may consist of a conductive metal such as copper, a copper alloy, or another material suitable as a negative electrode current collector layer. The anode active material layer 508 can be formed as a first layer on a first surface of the anode current collector layer 506 and a second layer on a second opposing surface of the anode current collector layer 506. In another embodiment, the anode current collector layer 506 and the anode active material layer 508 may be mixed. The first surface and the second opposing surface may be referred to as the primary surface, or front and back surface, of the substrate web 104. As used herein, primary surface refers to a surface defined by a plane formed by the length of the substrate web in the down-web direction WD and the span of the substrate web 104 in the cross-web direction XWD.

[0045] Generally, when the substrate web 104 is a web of anode material, the anode active material layer has a thickness of at least about 10 μm each. For example, in one embodiment, the anode active material layer has a thickness of at least about 40 μm each. As a further example, in such an embodiment, the anode active material layer has a thickness of at least about 80 μm each. As a further example, in such an embodiment, the anode active material layer has a thickness of at least about 120 μm each. However, typically, the anode active material layer has a thickness of less than about 60 μm each, or less than about 30 μm each.

[0046] Exemplary anode-active materials include any of the following: graphite, carbon materials such as soft or hard carbon, or graphene (e.g., single-walled or multi-walled carbon nanotubes), or metals, metalloids, alloys, oxides, nitrides, and compounds that can intercalate lithium or form alloys with lithium. Specific examples of metals or metalloids that can constitute anode materials include graphite, tin, lead, magnesium, aluminum, boron, gallium, silicon, Si / C composites, Si / graphite blends, silicon oxide (SiOx), porous Si, intermetallic Si alloys, indium, zirconium, germanium, bismuth, cadmium, antimony, silver, zinc, arsenic, hafnium, yttrium, lithium, sodium, graphite, carbon, lithium titanate, palladium, and mixtures thereof. In one exemplary embodiment, the anode-active material consists of aluminum, tin, or silicon, or their oxides, nitrides, fluorides, or other alloys thereof. In another exemplary embodiment, the anode active material is silicon, or an alloy or oxide thereof.

[0047] In one embodiment, the anode active material is microstructured to provide a significant void volume fraction to accommodate the volume expansion and contraction that occur when lithium ions (or other carrier ions) are incorporated into or detached from the anode active material during the charging and discharging process. Generally, the void volume fraction of the anode active material layer is at least 0.1. However, typically, the void volume fraction of each anode active material layer is 0.8 or less. For example, in one embodiment, the void volume fraction of the anode active material layer is about 0.15 to about 0.75. As a further example, in one embodiment, the void volume fraction of each anode active material layer is about 0.2 to about 0.7. As a further example, in one embodiment, the void volume fraction of each anode active material layer is about 0.25 to about 0.6.

[0048] Depending on the composition and method of forming the microstructured anodic active material, the microstructured anodic active material may consist of macroporous, microporous, or mesoporous material layers, or combinations thereof, for example, a combination of microporous and mesoporous, or a combination of mesoporous and macroporous. Microporous materials are typically characterized by pore dimensions of less than 10 nm, wall dimensions of less than 10 nm, pore depths of 1 to 50 micrometers, and pore morphology generally characterized by a "spongy" and irregular appearance, uneven walls, and branched pores. Mesoporous materials are typically characterized by pore dimensions of 10 to 50 nm, wall dimensions of 10 to 50 nm, pore depths of 1 to 100 micrometers, and pore morphology generally characterized by somewhat distinct branched or dendritic pores. Macroporous materials are generally characterized by pore dimensions greater than 50 nm, wall dimensions greater than 50 nm, pore depths of 1 to 500 micrometers, and pore morphology that can be varied, linear, branched, dendritic, and smooth or rough-walled. Furthermore, the void volume may consist of open voids, closed voids, or a combination thereof. In one embodiment, the void volume consists of open voids, i.e., the anode active material contains voids having openings on the lateral surface of the anode active material, through which lithium ions (or other carrier ions) can enter and exit the anode active material. For example, lithium ions can exit the cathode active material and then enter the anode active material through the void openings. In another embodiment, the void volume consists of closed voids, i.e., the anode active material contains voids surrounded by the anode active material. Generally, open voids can provide a larger interfacial surface area for carrier ions, while closed voids tend to be less affected by the solid electrolyte interface, although each provides room for expansion of the anode active material as carrier ions enter. Therefore, in certain embodiments, it is preferable that the anode active material consists of a combination of open and closed voids.

[0049] In one embodiment, the anode active material consists of porous aluminum, tin, or silicon, or their alloys, oxides, or nitrides. The porous silicon layer can be formed, for example, by anodizing, by etching (for example, by depositing a noble metal such as gold, platinum, silver, or gold / palladium on the surface of single-crystal silicon and etching the surface with a mixture of hydrofluoric acid and hydrogen peroxide), or by other methods known in the art, such as patterned chemical etching. Furthermore, porous anode active materials generally have a porosity of at least about 0.1, less than 0.8 and a thickness of about 1 to about 100 micrometers. For example, in one embodiment, the anode active material consists of porous silicon and has a thickness of about 5 to about 100 micrometers and a porosity of about 0.15 to about 0.75. As a further example, in one embodiment, the anode active material consists of porous silicon and has a thickness of about 10 to about 80 micrometers and a porosity of about 0.15 to about 0.7. As a further example, in one such embodiment, the anode active material is made of porous silicon, having a thickness of about 20 to about 50 micrometers and a porosity of about 0.25 to about 0.6. As a further example, in one embodiment, the anode active material is made of a porous silicon alloy (such as nickel silicide), having a thickness of about 5 to about 100 micrometers and a porosity of about 0.15 to about 0.75.

[0050] In another embodiment, the anode active material layer consists of fibers of aluminum, tin, silicon, or alloys thereof. Individual fibers may have a diameter (thickness dimension) of about 5 nm to about 10,000 nm and a length that roughly corresponds to the thickness of the anode active material. Silicon fibers (nanowires) can be formed, for example, by chemical vapor deposition, or by other techniques known in the art, such as vapor-phase liquid-solid (VLS) deposition or solid-liquid-solid (SLS) deposition. Furthermore, the anode active material generally has a porosity of at least about 0.1 and less than 0.8, and a thickness of about 1 to about 200 micrometers. For example, in one embodiment, the anode active material consists of silicon nanowires, has a thickness of about 5 to about 100 micrometers, and a porosity of about 0.15 to about 0.75. As a further example, in one embodiment, the anode active material consists of silicon nanowires, has a thickness of about 10 to about 80 micrometers, and a porosity of about 0.15 to about 0.7. As a further example, in one such embodiment, the anode active material consists of silicon nanowires having a thickness of about 20 to about 50 micrometers and a porosity of about 0.25 to about 0.6. As a further example, in one embodiment, the anode active material consists of nanowires of a silicon alloy (such as nickel silicide) having a thickness of about 5 to about 100 micrometers and a porosity of about 0.15 to about 0.75.

[0051] Generally, an anode current collector has a conductivity of at least about 10³ siemens / cm. For example, in one such embodiment, the anode current collector has a conductivity of at least about 10⁴ siemens / cm. In a further example, in one such embodiment, the anode current collector has a conductivity of at least about 10⁵ siemens / cm. Exemplary conductive materials suitable for use as anode current collectors include metals such as copper, nickel, cobalt, titanium, and tungsten, and their alloys.

[0052] Referring again to Figure 5, in another preferred embodiment, the substrate web 104 is a web of cathode material 504 which may include a cathode current collector layer 510 and a cathode active material layer 512. The cathode current collector layer 510 of the cathode material may consist of aluminum, an aluminum alloy, titanium, or other material suitable for use as a cathode current collector layer. The cathode active material layer 512 may be formed as a first layer on a first surface of the cathode current collector layer 510 and as a second layer on a second opposing surface of the cathode current collector layer 510. The cathode active material layer 512 may be coated on one or both sides of the cathode current collector layer 510. Note that current collectors and conductors can be used interchangeably as described herein. Similarly, the cathode active material layer 512 may be coated on one or both main surfaces of the cathode current collector layer 510. In another embodiment, the cathode current collector layer 510 may be mixed with the cathode active material layer 512.

[0053] Generally, when the substrate web 104 is a cathode material web, the cathode active material layer has a thickness of at least about 20 μm. For example, in one embodiment, the cathode active material layer has a thickness of at least about 40 μm each. As a further example, in such an embodiment, the cathode active material layer(s)(one or more) has a thickness of at least about 60 μm each. As a further example, in such an embodiment, the cathode active material layer(s)(s)(s) has a thickness of at least about 100 μm each. However, typically, the cathode active material layer(s) has a thickness of less than about 90 μm each, or less than about 70 μm each.

[0054] Exemplary cathode active materials include any of a wide range of cathode active materials. For example, in the case of a lithium-ion battery, as the cathode active material, a cathode active material selected from transition metal oxides, transition metal sulfides, transition metal nitrides, lithium-transition metal oxides, lithium-transition metal sulfides, and lithium-transition metal nitrides can be selectively used. Examples of the transition metal elements of these transition metal oxides, transition metal sulfides, and transition metal nitrides include metal elements having a d-shell or f-shell. Specific examples of such metal elements include Sc, Y, lanthanoids, actinoids, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Tc, Re, Fe, Ru, Os, Co, Rh, Ir, Ni, Pb, Pt, Cu, Ag, Au, etc. Additional cathode active materials include LiCoO2, LiNi 0.5 Mn 1.5 O4, Li(Ni x Co y Al z )O2, LiFePO4, Li2MnO4, V2O5, molybdenum oxy sulfide, phosphates, silicates, vanadates, sulfur, sulfur compounds, oxygen (air), Li(Ni x Mn y Co z )O2, and combinations thereof are included.

[0055] Generally, the cathode current collector has an electrical conductivity of at least about 103 Siemens / cm. For example, in such an embodiment, the cathode current collector has a conductivity of at least about 104 Siemens / cm. As a further example, in such an embodiment, the cathode current collector has a conductivity of at least about 105 Siemens / cm. Exemplary cathode current collectors include metals such as aluminum, nickel, cobalt, titanium, tungsten, and alloys thereof.

[0056] Referring again to Figure 5, in another preferred embodiment, the substrate web 104 is a web of an electrically insulating but ion-permeable separator material. The electrically insulating separator material 500 is adapted to electrically isolate each member of the anode group from each member of the cathode group of the secondary battery. The electrically insulating separator material 500 typically includes a microporous separator material that can be permeated with a non-aqueous electrolyte. For example, in one embodiment, the microporous separator material includes pores having a diameter in the range of at least 50 Å, more typically about 2,500 Å, and a porosity in the range of about 25% to about 75%, more typically about 35% to 55%.

[0057] Generally, when the substrate web 104 is a web of an electrically insulating separator material, the electrically insulating separator material has a thickness of at least about 4 μm. For example, in one embodiment, the electrically insulating separator material has a thickness of at least about 8 μm. As a further example, in one such embodiment, the electrically insulating separator material has a thickness of at least about 12 μm. As a further example, in one such embodiment, the electrically insulating separator material has a thickness of at least about 15 μm. However, typically, the electrically insulating separator material has a thickness of less than about 12 μm, or less than about 10 μm.

[0058] In one embodiment, the microporous separator material consists of a particulate material and a binder and has a porosity (void ratio) of at least about 20 vol%. The pores of the microporous separator material have a diameter of at least 50 Å and are typically in the range of about 250 to 2500 Å. The microporous separator material typically has a porosity of less than about 75%. In one embodiment, the microporous separator material has a porosity (void ratio) of at least about 25 vol%. In one embodiment, the microporous separator material has a porosity of about 35 to 55%.

[0059] The binder for microporous separator materials can be selected from a wide range of inorganic or polymer materials. For example, in one embodiment, the binder is an organic material selected from the group consisting of silicates, phosphates, aluminates, aluminosilicates, and hydroxides such as magnesium hydroxide and calcium hydroxide. For example, in one embodiment, the binder is a fluoropolymer derived from monomers such as vinylidene fluoride, hexafluoropropylene, and tetrafluoropropene. In another embodiment, the binder is a polyolefin such as polyethylene, polypropylene, and polybutene, having any of a range of molecular weights and densities. In yet another embodiment, the binder is selected from the group consisting of ethylene diene propenterpolymer, polystyrene, polymethyl methacrylate, polyethylene glycol, polyvinyl acetate, polyvinyl butyral, polyacetal, and polyethylene glycol diacrylate. In another embodiment, the binder is selected from the group consisting of methylcellulose, carboxymethylcellulose, styrene rubber, butadiene rubber, styrene-butadiene rubber, isoprene rubber, polyacrylamide, polyvinyl ether, polyacrylic acid, polymethacrylic acid, and polyethylene oxide. In another embodiment, the binder is selected from the group consisting of acrylate, styrene, epoxy, and silicone. In yet another embodiment, the binder is a copolymer or blend of two or more of the aforementioned polymers.

[0060] The microporous separator material can also be selected from a wide range of materials. Generally, such materials have relatively low electronic and ionic conductivity at the operating temperature and do not corrode under the operating voltage of the battery electrodes or current collectors that come into contact with the microporous separator material. For example, in one embodiment, the microporous material is 1 × 10⁻¹⁶ -4 It has conductivity for carrier ions (e.g., lithium) of less than S / cm. As a further example, in one embodiment, the particulate material is 1 × 10 -5 It has a conductivity for carrier ions of less than S / cm. As a further example, in one embodiment, the particulate material is 1 × 10 -6It has a conductivity to carrier ions of less than S / cm. Exemplary particulate materials include particulate polyethylene, polypropylene, TiO2-polymer composites, silica aerogel, fumed silica, silica gel, silica hydrogel, silica xerogel, silica sol, colloidal silica, alumina, titania, magnesia, kaolin, talc, diatomaceous earth, calcium silicate, aluminum silicate, calcium carbonate, magnesium carbonate, or combinations thereof. For example, in one embodiment, the particulate material consists of particulate oxides or nitrides such as TiO2, SiO2, Al2O3, GeO2, B2O3, Bi2O3, BaO, ZnO, ZrO2, BN, Si3N4, and Ge3N4. See, for example, P. Arora and J. Zhang, “Battery Separators”, Chemical Reviews 2004, 104, 4419-4462. In one embodiment, the particulate material has an average particle size of about 20 nm to 2 micrometers, more typically 200 nm to 1.5 micrometers. In another embodiment, the particulate material has an average particle size of about 500 nm to 1 micrometer.

[0061] In alternative embodiments, particulate materials composed of microporous separator materials can be bonded by techniques such as sintering, bonding, and curing, while maintaining the porosity desired for electrolyte penetration to provide ionic conductivity for battery function.

[0062] In assembled energy storage devices, microporous separator materials impregnate non-aqueous electrolytes suitable for use as secondary battery electrolytes. Typically, non-aqueous electrolytes consist of lithium salts and / or mixtures of salts dissolved in organic solvents and / or solvent mixtures. Exemplary lithium salts include inorganic lithium salts such as LiClO4, LiBF4, LiPF6, LiAsF6, LiCl, LiBr, and LiB(C6H5)4, LiN(SO2CF3)2, LiN(SO2CF3)3, LiNSO2CF3, LiNSO2CF5, LiNSO2CF4F9, and LiNSO2CF5F 11 LiNSO2CF6F 13, and LiNSO2CF7F 15 Examples of organolithium salts include those shown above. Examples of organic solvents that dissolve lithium salts include cyclic esters, linear esters, cyclic ethers, and linear ethers. Specific examples of cyclic esters include propylene carbonate, butylene carbonate, γ-butyrolactone, vinylene carbonate, 2-methyl-γ-butyrolactone, acetyl-γ-butyrolactone, and γ-valerolactone. Specific examples of linear esters include dimethyl carbonate, diethyl carbonate, dibutyl carbonate, dipropyl carbonate, methyl ethyl carbonate, methyl butyl carbonate, methyl propyl carbonate, ethyl butyl carbonate, ethyl propyl carbonate, butyl propyl carbonate, alkylpropionate, dialkylmalonate, and alkyl acetate. Specific examples of cyclic ethers include tetrahydrofuran, alkyltetrahydrofuran, dialkyltetrahydrofuran, alkoxytetrahydrofuran, dialkoxytetrahydrofuran, 1,3-dioxolane, alkyl-1,3-dioxolane, and 1,4-dioxolane. Specific examples of linear ethers include 1,2-dimethoxyethane, 1,2-diethoxyethane, diethyl ether, ethylene glycol dialkyl ether, diethylene glycol dialkyl ether, triethylene glycol dialkyl ether, and tetraethylene glycol dialkyl ether.

[0063] In one embodiment, the web 104 of the substrate can have an adhesive tape layer (not shown) adhered to one or both surfaces of the anode-active material layer 508 or the cathode-active material layer 512. This adhesive layer can be removed after ablation or cutting (described later) to remove unwanted material or debris.

[0064] Embodiments of the laser systems 120a to c will be further described with reference to Figures 2 to 6. The substrate web 104 enters the laser system 120 in the web direction WD. In one embodiment, the substrate web 104 enters the laser system 120a in a first state 400, which has not yet been ablated or cut. Thus, the substrate web 104 in the first state 400 should have virtually no defects or changes from its initial state. The substrate web 104 passes over a chuck 306 which includes a plurality of vacuum holes 406. The vacuum holes 406 are in fluid communication with the vacuum 308 and apply vacuum pressure to the substrate web 104 as it passes through the vacuum holes 406. The vacuum holes 406 can be staggered or chamfered to allow the substrate web 104 to pass over them more easily without getting stuck. The cross-sectional area of ​​the holes must be small enough to prevent the substrate web 104 from being pulled into them, but large enough to allow a suitable airflow from the vacuum to pass through them. The vacuum pressure facilitates maintaining the substrate web 104 in a substantially flat / planar state as it is transported across the chuck 306. In some preferred embodiments, the laser system 120 is focus-sensitive, and in such embodiments, it is important to maintain the substrate web 104 at a substantially constant distance from the laser output 313 to ensure that the laser beam 302 is at focus when it contacts the substrate web 104 during the cutting or ablation process. Thus, the vacuum pressure through the vacuum hole 406 can be monitored and adjusted in real time, for example, via the user interface 116, to keep the substrate web 104 in a substantially flat state across the chuck 306 and prevent it from lifting or buckling during processing. The cross-sectional shape of the vacuum hole may be circular, square, rectangular, elliptical, or other shapes that allow the chuck 306 to function as described herein.

[0065] As shown in Figure 4, the chuck 306 includes an opening 410 defined by an upstream edge 412 and a downstream edge 414. The illustrated chuck 306 includes a chamfer 416 on the downstream edge 414. In this embodiment, the chamfer 416 facilitates the passage of the substrate web 104 over the downstream edge 414 without the substrate web 104 catching or snagging on the downstream edge 414. The angle α of the chamfer 416 may be between 1 and 90 degrees, for example, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85 degrees, or any other angle that allows the chamfer 416 to function as described herein. In the illustrated embodiment, for example, the angle α is approximately 25 degrees. It has been found that performance improves if the angle α of the chamfer 416 is greater than the deflection of the web 104 of the substrate passing over the chamfer 416. The upper edge 418 of the chamfer 416 can be radial to provide a smooth transition from the chamfer 416 to the surface of the chuck 306.

[0066] In one preferred embodiment, the chuck 306 is formed from aluminum. However, the chuck 306 may be formed from an aluminum alloy, a composite material, a metal or metal alloy, or any other suitable material that enables the chuck 306 to function as described herein.

[0067] In one preferred embodiment, the substrate web 104 is first ablated by a laser beam 302 (Figure 3) in order to form an ablation 404 (Figure 4) on the substrate web 104. In one embodiment, the substrate web 104 is an anode material 502, and the ablation 404 removes the anode active material layer 508 to expose the anode current collector layer 506 (Figure 5). In another embodiment, the substrate web 104 is a cathode material 504, and the ablation 404 removes the cathode active material layer 512 to expose the cathode current collector 510. In one embodiment, the ablation 404 is configured as an electrode tab 520 (adapted to electrically connect the cathode current collector and the anode current collector to the positive and negative terminals of a secondary battery, respectively). When the laser system 120a is used to form ablation 404 on the substrate web 104, the output of the laser beam 302 is set to a level that allows for substantially or completely removal of the coating layer, but without damaging or cutting the current collector layer. During use, the laser beam 302 is controlled, for example, via the user interface 116, to form the ablation 404 while the substrate web 104 is moving and being transported in the down-web direction WD. The ablation 404 is formed on both sides of the substrate web 104, as best shown in Figure 5. In one embodiment, after forming the ablation 404, the laser system 120a forms fiducial features 602 (such as holes), as further described herein. In another embodiment, multiple lasers can be used to ablate portions of the substrate web 104, each to form one or more ablation 404, thereby improving the throughput of the manufacturing system 100.

[0068] Referring further to Figures 2, 3, and 4, in another stage of the production process, the web 104 of the substrate is transported down the web direction WD toward the cutting area 408 of the laser system 120a. The cutting area 408 includes an opening 410 of the chuck 306. In one embodiment, the opening 410 is in fluid communication with a vacuum 308, applying vacuum pressure to the web 104 of the substrate as it passes over the opening 410. In a preferred embodiment, the opening 410 is wider in the cross-web direction XWD than the web 104 of the substrate, such that the entire width of the web 104 of the substrate is suspended over the opening 410 in the cross-web direction XWD. In one embodiment, a second vacuum may be present, configured to equalize the pressure on the web 104 of the substrate facing the chuck 306. In this embodiment, the pressure equalization makes it easier to keep the web 104 of the substrate substantially flat / planar and at a constant height as it passes over the opening 410, and makes it easier to maintain focus of the laser beam 302 onto the web 104 of the substrate. In one embodiment, a carrier web can be used to support the substrate web 104. In some embodiments, the carrier web is removably attached to the substrate web using a low-tack adhesive or electrostatic pinning. In such embodiments, the attachment has sufficient adhesive strength to remain attached to the substrate web during processing, but is removable without damaging the substrate web. In one embodiment, the carrier web is made of a material that does not absorb the laser wavelength used during processing of the substrate web 104, and the carrier web is not cut, vaporized, or ablated, and can therefore be reused on other substrate webs.

[0069] The laser system 120a is configured to cut one or more patterns (such as individual electrode patterns 800 (Figure 8) which may also be called electrode tier patterns) in the web 104 of the substrate while the web of the substrate is over the opening 410, each of which is a member of a group of electrode structures. Referring to Figure 6, the patterns may include one or more longitudinal edge cuts 600 which define the longitudinal edges of the electrodes in the cross-web direction XWD. The longitudinal edge cuts 600 are cut using a laser beam 302 which cuts the web 104 of the substrate in the cross-web direction XWD while the web of the substrate is being transported in the down-web direction WD. The cross-web direction XWD is perpendicular to the down-web direction WD. It should be noted that in one embodiment, in order to form a longitudinal edge cut 600 which is substantially perpendicular to the down-web direction WD, the laser beam 302 must be controlled to move at an angle with respect to the down-web direction WD, taking into account the movement of the web 104 of the substrate in the down-web direction WD. For example, as the substrate web 104 moves in the down-web direction WD, the path of the laser beam 302 is projected onto the substrate web 104 at the initial cut position 604 and then synchronized with the movement of the substrate web 104 in the web direction. Thus, the path of the laser beam 302 is controlled to move in both the cross-web direction XWD and the down-web direction WD until it reaches the end-cut position 606, forming a longitudinal edge cut 600. In this embodiment, a compensation factor is applied to the path of the laser beam 302 so that a cut can be made in the cross-web direction XWD while the substrate web is moving continuously in the web direction WD. It should be understood that the angle at which the laser beam 302 travels changes based on the velocity of the substrate web 104 in the down-web direction WD. In another embodiment, the substrate web 104 is temporarily stopped during the laser processing operation, and as such, the path of the laser beam 302 does not need to consider the movement of the substrate web in the down-web direction WD. Such embodiments may be called a step process or a step-and-repeat process.During laser processing, one or more of the laser systems 120a to c may use a repeating alignment feature, such as a fiducial feature 602, to adjust / align the laser beam 302 during the laser processing operation, for example, to compensate for possible variations in the position of the web 104 of the substrate.

[0070] The laser processing operation described herein is performed such that the longitudinal edge cut 600 is defined in the cross-web direction XWD, so that the repeating pattern of the electrode pattern is aligned in the cross-web direction XWD. However, it should be understood that in other embodiments, the laser processing operation described herein may be controlled so that the longitudinal edge cut 600 and all associated cutting, drilling, and ablation operations are oriented perpendicularly to each other. For example, the longitudinal edge cut 600 may be aligned in the down-web direction WD so that the group of electrode patterns 800 is aligned in the down-web direction WD rather than the cross-web direction XWD.

[0071] In one embodiment, the laser system 120a cuts a tie bar 614 between one or more electrode patterns. The tie bar 614 can be used to separate groups of electrode patterns. For example, in the embodiment shown in Figure 6, the tie bar 614 is cut between groups of five individual electrode patterns. However, in other embodiments, the tie bar 614 may be included after any number of individual electrode patterns, or it may not be present at all. The tie bar is defined by upstream and downstream tie bar edge cuts 616, 618, respectively. In some embodiments, the tie bar 614 is sized to provide additional structural rigidity to the web during processing.

[0072] Furthermore, in one preferred embodiment, the laser system 120a cuts one or more repeating alignment features, such as a plurality of fiducial features 602, in the web 104 of the substrate. In one embodiment, the fiducial feature 602 is a fiducial through-hole. The fiducial feature 602 is cut at a known location on the web 104 of the substrate. The fiducial feature 602 is shown as circular in Figure 6, but may be rectangular as shown in Figure 5, or may be any size or shape that allows the manufacturing system 100 to function as described herein. The fiducial feature 602 is tracked by one or more visual inspection systems 310, 312 that measure position and movement speed. The measurement of the fiducial feature 602 is then used to enable accurate front-to-back alignment of the pattern on the web 104 of the substrate in both the down-web direction WD and the cross-web direction XWD. The laser system 120a may also cut a plurality of tractor holes 612 that can be used for aligning the web 104 of the substrate or as holes that engage with a gear wheel 1210 (Figure 12) for transporting, positioning, and tension control of the web 104 of the substrate. The tractor holes 612 may be circular, square, or other shapes that allow the manufacturing system 100 to function as described herein. In another preferred embodiment, the web 104 of the substrate has a plurality of tractor holes 612 and / or fiducial features 602 pre-cut therein before being unwound and transported through the manufacturing system 100. In one embodiment, the ratio of fiducial features 602 to electrode patterns 800 is 1:1. In other embodiments, there may be two or more fiducial features for each electrode pattern 800.

[0073] Referring to Figures 2 and 6, in one preferred embodiment, the laser system 120a cuts a first perforation 608 and a second perforation 610 into the web 104 of the substrate as part of the electrode pattern. The first perforation 608 is located outside the electrode pattern in the cross-web direction XWD and may therefore be called the “outer perforation,” and the second perforation 610 is located inside the outer perforation in the cross-web direction XWD and may therefore be called the “inner perforation.” The perforations 608, 610 are best shown in Figure 7, which is an enlarged view of a portion 615 (Figure 6) of the web 104 of the substrate. The first perforation 608 is formed by laser cutting with the laser beam 302 while the web of the substrate is positioned over the opening 410 of the chuck 306. The first perforation 608 is formed as a linear slit (e.g., a through-cut) in a direction coinciding with the down-web direction WD. Importantly, the first perforation 608 is located on the electrode W e The outer tear strip 700 does not extend across the entire width. Instead, the outer tear strip 700 remains on both the upstream and downstream edges of the perforation 608, ensuring that the electrode pattern remains connected to the web 104 of the substrate.

[0074] Similarly, referring further to Figures 6 and 7, the second perforation 610 is formed inboard (in the cross-web direction XWD) from the first perforation 608. In a preferred embodiment, the second perforation 610 is formed as a line of slits in the down-web direction WD separated by the inner tear strip 702. In the illustrated embodiment, the second perforation 610 intersects with the through hole 704. In the illustrated embodiment, the inner tear strip 702 is at least twice the length of the outer tear strip 700, and the breaking force required to separate the outer tear strip is about half the breaking force required to separate the inner tear strip 702 from the web 104 of the substrate. In other embodiments, the ratio of the breaking strengths of the first and second tear strips may vary, but it is preferable that the outer tear strip 700 has a lower breaking strength than the inner tear strip 702, so that when a tensile or shear force is applied to the end of the web 104 of the base material, the outer tear strip 700 breaks before the inner tear strip 702.

[0075] Referring to Figures 3, 4, and 6, by performing laser cutting of the longitudinal edge cut 600, fiducial feature 602, and first and second perforations 608, 610 on the opening 410 of the chuck 306, the fragments can be dropped through the opening 410, and the vacuum 308 can collect the fragments formed during the laser cutting process.

[0076] In one preferred embodiment, the laser system 120a is configured as a first ablation station. In this embodiment, the laser system 120a forms ablation 404 on the first surface of the substrate web 104 as described above. Exiting the laser system 120a, the substrate web passes over an idler 108d that inverts the substrate web 104 in such a way that the second surface of the substrate web (facing the first surface) is positioned for processing by the laser system 120b, which in this embodiment is configured as a second ablation station. In this embodiment, the laser system 120b is configured to use fiducial features 602 to ensure alignment in the down-web direction WD and the cross-web direction XWD. Thus, the laser system 120b performs a second ablation process on opposing surfaces of the substrate web 104 so that the ablation 404 on each surface of the substrate web 104 is aligned in the down-web direction WD and the cross-web direction XWD. In one embodiment, the ablation 404 is configured as a current-collecting tab of an electrode.

[0077] In one embodiment, the laser system 120c shown in Figure 2 is configured as a laser cutting station. In this embodiment, the laser system 120c performs laser cutting such as longitudinal edge cutting 600 and first and second perforations 608 and 610.

[0078] In a preferred embodiment, one or more of the laser devices 300 in the laser systems 120a-c are 20-watt fiber lasers. In an embodiment, a preferred laser device 300 in the laser systems 120a-c has a laser output in the range of 10W to 5000W, for example, in the range of 10W to 100W, 100W to 250W, 250W to 1kW, 1kW to 2.5kW, or 2.5kW to 5kW. A suitable laser device 300 includes a laser beam having wavelengths from 150nm to 10.6μm, for example, 150nm to 375nm, 375nm to 750nm, 750nm to 1500nm, or 1500nm to 10.6μm. In an embodiment, the laser device 300 may have one or more laser pulse width types of continuous wave (CW), microsecond (μs), nanosecond (ns), picosecond (ps), and femtosecond (fs) pulse types. Any of these types of lasers can be used individually or in combination as the laser device 300 of the laser systems 120a-c. In other preferred embodiments, the laser device 300 is any other laser that can enable the laser systems 120a-c to operate as described herein.

[0079] In some embodiments, the substrate web 104 may include machine-punched or laser-cut fiducial features 602 before being loaded into the manufacturing system 100. In another preferred embodiment, the fiducial features 602 may be mechanically machine-punched following the formation of abrasions 404 on the first surface of the substrate web. In yet another preferred embodiment, the manufacturing system 100 may include one or more additional mechanical punches that can be used to form longitudinal edge cuts 600 and / or one or more of the first and second perforations 608, 610.

[0080] In one embodiment, one or more rollers in the conveyor system may not be perfectly circular, such that the rollers are eccentric. In such cases, especially if the eccentric roller is a nip roller, the web of the substrate may be conveyed so that the position of the web 104 of the substrate advances in different ways depending on which part of the eccentric roller is in contact with the web. For example, if the eccentric roller has a portion with a radius greater than the expected roller radius, the web may advance further down the web direction WD than expected when the larger radius portion of the roller is pushing / pulling the web. Similarly, if the eccentric roller has a smaller radius portion, the web may advance a reduced distance down the web direction WD than expected. Therefore, in one embodiment, the eccentric roller can be mapped to determine the radius-to-radial position. The laser system 120a-c can then be controlled to adjust the position of the laser beam 302 to account for the eccentricity based on the roller mapping. In one embodiment, the roller mapping is stored in the memory of the user interface 116.

[0081] After exiting one or more of the laser systems 120a-c, the substrate web may be transported to one or more cleaning stations, such as a brushing station 124 and an air knife 126. In a preferred embodiment, the brushing station 124 includes a brush 1000 (Figures 10 and 11) that moves in the cross-web direction XWD. The brush 1000 includes a pair of bristle 1002 held by a bristle holder 1004. The brush 1000 is configured such that the bristle 1002 can make delicate contact with the surface of the substrate web 104, removing or removing any debris therefrom. The contact pressure of the bristle 1002 against the surface of the substrate web 104 must be low enough to maintain the electrode pattern attached to the substrate web 104 without causing damage, rupture, or other defects to the electrode pattern. In one embodiment, the normal force between the bristle 1002 and the surface of the substrate web 104 is between 0 and 2 pounds, for example, 0.1 pound, 0.2 pound, 0.3 pound, 0.4 pound, 0.5 pound, 0.6 pound, 0.7 pound, 0.8 pound, 0.9 pound, 1.0 pound, 1.1 pound, 1.2 pound, 1.3 pound, 1.4 pound, 1.5 pound, 1.6 pound, 1.7 pound, 1.8 pound, 1.9 pound, or 2.0 pound. In other embodiments, the normal force may be greater than 2.0 pound.

[0082] In one embodiment, the length of the bristle 1002 is 3 / 4 inch (19.05 mm). In one embodiment, the bristle 1002 is inserted or clamped into the bristle holder 1004 by about 1 / 8 inch. The diameter of the bristle can be from 0.003 inches (0.076 mm) to 0.010 inches (0.254 mm), for example, 0.003 inches (0.076 mm), 0.004 inches (0.101 mm), 0.005 inches (0.127 mm), 0.006 inches (0.152 mm), 0.007 inches (0.177 mm), 0.008 inches (0.203 mm), 0.009 inches (0.228 mm), and 0.010 inches (0.254 mm). In a preferred embodiment, the bristle 1002 is a nylon bristles. However, in other embodiments, the bristle 1002 may be made of other natural or synthetic materials that enable the brush 1000 to function as described herein.

[0083] Referring further to Figures 10 and 11, in one preferred embodiment, in order to enable the movement of the brush 1000 in the cross-web direction XWD, the brush 1000 is connected to a crank arm 1006 via a rotatable coupling 1008 such as a bearing or bushing. The crank arm 1006 is rotatably coupled to a drive wheel 1010 via a second rotatable coupling 1012. The rotatable coupling is coupled to the drive wheel 1010 at an offset position from the center such that the crank arm 1006 causes the brush 1000 to reciprocate in the cross-web direction XWD. The drive wheel 1010 is coupled to a motor 1014 to enable the rotation of the drive wheel. A position sensor 1016 senses the position of a brush position marker 1018 coupled to the drive wheel 1010. Thus, the position sensor 1016 can measure the phase (e.g., angular position) and rotations per unit time of the drive wheel 1010. In one embodiment, the drive wheel 1010 is controlled to be within a range of 0 to 300 revolutions per minute ("rpm"), such as 0 rpm, 25 rpm, 50 rpm, 75 rpm, 100 rpm, 125 rpm, 150 rpm, 175 rpm, 200 rpm, 225 rpm, 250 rpm, 275 rpm, and 300 rpm (for example, 0 to 300 strokes per minute for the brush 1000). In other embodiments, the rpm of the drive wheel 1010 may be greater than 300 rpm. Note that if the rotational speed of the drive wheel 1010 is constant, sinusoidal speed fluctuations of the brush 1000 occur due to the connection of the crank arm 1006 to the drive wheel 1010.

[0084] In one preferred embodiment, a second brush (not shown) is positioned to contact the opposing surface of the web 104 of the substrate. In this embodiment, the second brush, which may be substantially the same as the first brush 1000, is configured to move in the opposite direction to the first brush, preferably with a 180-degree phase difference. The phases of the first and second brushes can be determined via position sensor 1016 and an equivalent position sensor for the second brush. In this embodiment, the contact pressure of the bristles of the first and second brushes together must be low enough to keep the electrode pattern attached to the web 104 of the substrate without causing damage, rupture, or other defects to the electrode pattern.

[0085] In one embodiment, the brush 1000 has a bristle width 1022 that is wider than the width of the web 104 of the substrate in the cross-web direction XWD. For example, in one embodiment, the bristle width 1022 is wide enough so that the bristle 1002 remains in contact with the surface of the web 104 of the substrate throughout the entire range of motion of the brush 1000 as the brush 1000 vibrates in the cross-web direction XWD. The vibration speed of the brush 1000 and the pressure exerted by the bristle 1002 on the surface of the web 104 of the substrate can be controlled by the user using the user interface 116.

[0086] The brushing station 124 may include a vacuum system configured to create a vacuum through the brushing station orifice 1020, thereby discharging brushed debris from one or more surfaces of the substrate web 104. In this embodiment, the debris may be brushed off and fall from the substrate web 104 or be sucked through the brushing station orifice 1020. The brushing station orifice 1020 is illustrated as circular, but may be of any shape that allows the brushing station 124 to function as described herein. Furthermore, the upper edge of the brushing station orifice 1020 may be chamfered and / or offset to allow the substrate web 104 to pass over it more easily without the edges of the substrate web catching therein. In one embodiment, the vacuum level can be controlled to range from 0 to 140 inches of H2O, for example, 0 inches of H2O, 10 inches of H2O, 20 inches of H2O, 30 inches of H2O, 40 inches of H2O, 50 inches of H2O, 60 inches of H2O, 70 inches of H2O, 80 inches of H2O, 90 inches of H2O, 100 inches of H2O, 110 inches of H2O, 120 inches of H2O, 130 inches of H2O, and 140 inches of H2O. In some embodiments, the vacuum flow rate is controlled to be approximately 0 to 425 cubic feet / minute ("cfm"), for example, 0 cfm, 25 cfm, 50 cfm, 75 cfm, 100 cfm, 125 cfm, 150 cfm, 175 cfm, 200 cfm, 225 cfm, 250 cfm, 275 cfm, 300 cfm, 325 cfm, 350 cfm, 375 cfm, 400 cfm, and 425 cfm. In other embodiments, the vacuum level and flow rate may be greater than 140 inches of H2O and 425 cfm, respectively. The vacuum level and flow rate are controlled to be within a range that allows the debris to be pulled away from the substrate web 104 without creating unwanted friction between the substrate web 104 and the transport system components. In some embodiments, such vacuum levels and flow rates are applicable to all other components of the system that use vacuum.

[0087] In another preferred embodiment, one or more of the first and second brushes may include a load sensor that measures or monitors the pressure the brush exerts on the web 802 of the electrode material. As shown in Figure 8, the web 802 of the electrode material refers to the web after it has been processed as described herein so that a cluster of electrode patterns 800 is formed therein. In this embodiment, the first and second brushes can be controlled via the user interface 116 to maintain a uniform brushing pressure on the web 802 of the electrode material based on wear of the brush bristles or variations in the thickness or surface roughness of the electrodes.

[0088] In another preferred embodiment, one or more of the first and second brushes are configured to move at least partially in the down-web direction WD at a speed equal to the speed of the electrode material web 802, so that the speed difference between the brush and the electrode material web 802 is kept substantially zero in the down-web direction WD.

[0089] In yet another preferred embodiment, the brushing station 124 may include a position sensor, which is a phase measuring sensor 1016 for determining the phases of the first and second brushes. In such an embodiment, the phase sensor may measure the position of the home sensor flags 1018 of the first and second brushes. In this embodiment, the phase measuring sensor 1016 determines whether the first and second brushes are out of phase by 180 degrees, 90 degrees, 0 degrees, or within a predetermined phase difference range, such as any other suitable phase difference that would enable the manufacturing system 100 to function as described herein. As used herein, “phase” of brushes refers to the angular position of the brushes such that the bristles of two separate brushes are aligned when they are “in phase”.

[0090] In yet another embodiment, an ultrasonic transducer (not shown) may be configured to apply ultrasonic vibrations to one or more of the first and second brushes in order to facilitate the removal of debris from the web 802 of the electrode material.

[0091] Referring further to Figure 2, in one preferred embodiment, the substrate web 104 is transported through an air knife 126. As used herein, the term air knife refers to a device that uses compressed air to blow onto the substrate web 104. The compressed air comes into contact with the surface of the substrate web 104 and removes debris from there. The air knife 126 is controlled to supply air at a pressure / velocity such that it does not cause defects such as damage or rupture to the electrode pattern, thus maintaining the electrode pattern attached to the substrate web 104. In another embodiment, a second air knife 126 is configured to blow air onto an opposing surface of the substrate web 104 to remove debris from there. In this embodiment, the second air knife may blow air in the same direction as the first air knife, or in a direction opposite to the first air knife, or in any other direction that allows the air knife 126 to function as described herein. In one embodiment, the air knife 126 station is equipped with a vacuum to facilitate the removal of debris removed by the air knife 126.

[0092] Referring to Figure 8, after being processed by laser systems 120a-c and cleaned by brushing station 124 and air knife 126, the substrate web 104 leaves the cleaning station as a web containing a cluster of electrode patterns 800 within the substrate web 104, collectively as a web 802 of electrode material.

[0093] Referring further to Figures 2, 8, and 12, in one embodiment, the web of electrode material 802 passes through an inspection device 128. The inspection device 128 is a device configured to analyze the electrode material 802 and identify its defects. For example, in one embodiment, the inspection device 128 is a visual inspection device that includes a camera 1200, which may be a digital camera such as a digital 3D camera, configured to analyze the electrode pattern on the web of electrode material 802. The camera 1200 is optically coupled to a lens 1202, which may be a wide-field lens. In one embodiment, the lens 1202 is a telecentric lens. The lens 1202 is held in place by a lens mount 1204 and, in one embodiment, may be adjustable in the vertical direction V to control the focus of the lens 1202. The lens 1202 is oriented to focus on the web of electrode material 802 as the web of electrode material 802 passes over the inspection plate 1206. In one embodiment, the inspection plate 1206 includes a transparent or translucent top 1208 that allows light from a light source (not shown) housed within the inspection plate 1206 to illuminate it to produce a backlight. In one preferred embodiment, the intensity and / or color of the light can be controlled via a user interface 116. In one embodiment, one or more additional light sources, such as an upstream light source and a downstream light source, illuminate the web of electrode material 802 while it is inside the inspection apparatus 128. In some embodiments, each of the illumination sources is independently controllable with respect to intensity and color. In one embodiment, the backlight includes a diffuse low-angle ring light. The web of electrode material 802 may be fixed and transported on the inspection plate 1206 by a gear wheel 1210 configured to engage with tractor holes 612 in the web of electrode material 802. In doing so, the web of electrode material 802 is held in a taught position relative to the inspection plate 1206 to substantially eliminate curling of the web of electrode material 802. The front edge 1214 and the rear edge 1216 of the inspection plate may each be chamfered (for example, at an angle similar to angle α) so that the web of electrode material can pass over it smoothly without getting caught.

[0094] Continuing to refer to Figure 12, in one embodiment, the inspection device 128 includes a trigger sensor 1212 that detects predetermined features of the web 802 of the electrode material, such as fiducial features 602, longitudinal edge cuts 600, or other features that enable the inspection device 128 to function as described herein. When the electrodes are imaged, the camera 1200 may be configured to detect one or more metrics, such as the height of the electrodes, the size or shape of the features cut by any of the laser devices 120a-120c (Figure 2), the pitch (distance) between the electrodes, or other features that enable the inspection device to function as described herein. For example, in one preferred embodiment, the inspection device 128 detects whether the ablation 404 (Figure 4), longitudinal edge cuts 600, fiducial features 602, tractor holes 612, the pitch between individual electrode structures, the cross-web and web-direction offsets of the tractor holes 612, and the first and second perforations 608, 610 (Figure 6) are within predefined tolerances for size, shape, arrangement and orientation. In a preferred embodiment, the user can use the user interface 116 to control which features are inspected.

[0095] In this embodiment, the flatness of the electrode material web 802 during inspection allows for more precise imaging and analysis of the electrode material web 802, resulting in higher quality error and defect detection. For example, the inspection device 128 can be configured to measure metrics such as web thickness, electrode pattern size, and shape while the web is being transported in the web-downward WD direction. These metrics are transmitted to the user interface 116 for display or memory storage, or used to adjust production parameters of the manufacturing system 100.

[0096] In one embodiment, if the inspection system determines that a defect exists on the electrode material web 802 (Figure 8), the marking device 130 (Figure 2) marks the electrode material web to identify such a defect. The marking device 130 may be a laser etching apparatus, a printer, a stamper, or any other marking device capable of placing a mark indicating the presence of a defect on the electrode material web 802. In another preferred embodiment, the marking device 130 is controllable to mark one or more of the identification number (ID) and known good electrodes (KGE) on the electrode material web 802, and may further mark the electrode material web 802 with grades such as Grade A, Grade B, Grade C, indicating a quality measurement of a particular electrode within the electrode material web 802 (such as the number or type of defects).

[0097] When the substrate web 104 is processed into the electrode material web 802, the electrode material web 802 exhibits a 25% to 90% reduction in web strength in the down-web direction WD compared to the unprocessed substrate web 104. Referring to Figure 8A, a portion of the electrode material web 802 is shown. In this embodiment, the electrode material web 802 includes an electrode cluster EC consisting of five electrode patterns 800 separated by tie bars 614. However, it should be understood that in other embodiments, the electrode cluster EC may include one or more electrode patterns, such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 or any other number of electrode patterns 800 between tie bars 614. Distance L EC This is defined as the distance WD in the downweb direction between the center point of the first electrode pattern of electrode cluster EC and the center point of the first electrode of the second electrode cluster EC.

[0098] In an exemplary embodiment, the cross-web span S of the web W The width is 3X mm in the cross-web direction, and the width W of each electrode pattern is 800 in the down-web direction WD. EPThe width is X mm. In this embodiment, the decrease in web strength in the down web direction WD is 33% compared to the web 104 of the unprocessed substrate. The decrease in web strength is due to the width W EP Crosswebspan S W It is calculated as if divided by (i.e., Xmm / 3Xmm = 0.33).

[0099] In another exemplary embodiment, the cross-webspan S of the web W The width is 1.5X mm in the cross-web direction, and the width W of each electrode pattern is 800 in the down-web direction WD. EP It is 1.3X mm. In this embodiment, the decrease in web strength in the down web direction WD is 87 percent compared to the web 104 of the unprocessed substrate. The decrease in web strength is W EP / S w It is calculated as (i.e., 1.3X / 1.5X = 0.87). The web strength in the down web direction WD is verified and measured as the fracture strength of the web 802 of the electrode material using an electromechanical or hydraulic material testing machine with at least force feedback, which may include displacement feedback such as Instron brand testing machines.

[0100] In another exemplary embodiment, there is a decrease in strength in the cross-web direction XWD of the electrode material web 802 compared to the substrate web 104. In the first exemplary embodiment, the width W of the electrode cluster EC The width of the tie bar 614 is 6X mm ​​in the down-web direction WD, the width WTB is X mm in the down-web direction WD, and the width of the electrode pattern is W EP The length of the electrode pattern is X mm in the down-web direction WD, and L E The length is 1.7X mm in the cross-web direction XWD. In this embodiment, the decrease in strength of the electrode material web 802 in the cross-web direction XWD is about 77 percent compared to the web 104 of the unprocessed substrate. In another exemplary embodiment, the length L of the electrode cluster is 1.7X mm. ECThe width of the tie bar 614 is 10X mm, the width WTB is 0X mm (i.e., no tie bar), and the width of the electrode pattern is W EP It is 2X mm, and the length of the electrode pattern L E The thickness is 1.7X mm. In this embodiment, the reduction in strength of the electrode material web 802 in the cross-web direction XWD is approximately 92% compared to the web 104 of the unprocessed substrate. The web strength in the cross-web direction XWD is verified and measured as the fracture strength of the electrode material web 802 using an electromechanical or hydraulic material testing machine with at least force feedback, which may include displacement feedback such as an Instron brand testing machine.

[0101] Referring further to Figure 9, the electrode material web 802 is then transported to the winding roller 134, where it is wound together with the web of the interleaf material 138 to create a spool 900 having alternating layers of the electrode material web 802 and the web of the interleaf material 138.

[0102] In one preferred embodiment, the user interface 116 may include a processor and memory configured to store and execute instructions causing the manufacturing system 100 to function as described herein. The user interface 116 may further include a display device such as an LCD or LED display and a set of control devices, or virtual control devices, which enable the user to control and adjust parameters of the manufacturing system 100 and also display metrics such as web transport speed, tension, number of defects, and any other parameters that cause the manufacturing system 100 to function as described herein.

[0103] When in use, referring to Figure 2, the base unwinding roller 102 of the manufacturing system 100 is loaded with the base material web 104. The base material web 104 is passed across the edge guide 106 to facilitate the unwinding of the base material web 104. In this embodiment, the base material web 104 is then passed around an idler 108a and placed into the splicing station 110. The idler 108a is used to facilitate the proper positioning and tension maintenance of the base material web 104 and to change the orientation of the base material web 104. The idler 108a receives the base material web 104 vertically and is partially wound around the idler 108a such that the base material web 104 moves away from the idler 108a at a substantially 90-degree angle from the input direction in the output direction. However, it should be understood that the input and output directions may change without departing from the scope of this disclosure. In some embodiments, the manufacturing system 100 can use a plurality of idlers 108a to 108x to change the orientation of the substrate web once or more times as the substrate web is transported through the manufacturing system 100. In this embodiment, the user unwinds the substrate 104 through idlers 108a to 108x, for example, as shown in Figure 2.

[0104] In one embodiment, a splicing station 110 is used to splice two separate webs together. In this embodiment, the web 104 of the first substrate is unwound so that the trailing edge (not shown) of the substrate web 104 stops within the splicing station 110, and the leading edge (not shown) of the second substrate web 104 is unwound within the splicing station 110 so that the trailing edge of the first web and the leading edge of the second web are adjacent to each other. The user then applies an adhesive, such as adhesive tape, to join the leading edge of the second web to the trailing edge of the first web, forming a seam between the two webs and creating a continuous substrate web. Such a process may be repeated for multiple webs of the substrate 104 at the user's direction.

[0105] In a preferred embodiment, upon leaving the splicing station 110, the substrate web 104 is transported in the downweb direction WD to the nip roller 112. The nip roller 112 is controlled via a user interface 116 to regulate / maintain the speed at which the substrate web 104 is transported through the manufacturing system 100. The substrate web 104 is pressed against each of the two adjacent rollers 114 of the nip roller 112 with enough pressure to allow friction between the rollers to move the substrate web 104, but with enough pressure to avoid causing significant deformation or damage to the substrate web 104.

[0106] In one embodiment, during use, the speed of the substrate web 104 is controlled by controlling the rotational speed of the high-friction roller of the nip roller 112 via the user interface 116. In another embodiment, the manufacturing system 100 may include one or more additional nip rollers 122, 132 to facilitate control of the speed of the substrate web 104, through which the substrate web is conveyed. In this embodiment, the speeds of the additional nip rollers 122, 132 can be controlled via the user interface 116. If multiple nip rollers are used during use, the speed of each of the nip rollers 112, 122, 132 may be set to the same speed via the user interface 116, or may be set to different speeds as needed, so that the substrate web 104 is conveyed smoothly through the manufacturing system 100.

[0107] In use, in one embodiment, the web of the base material is unwound through the dancer 118. In this embodiment, a pair of rollers of the dancer 118 rotate about their central axis to passively adjust the tension of the web 104 of the base material.

[0108] Referring further to Figure 2, during use, the substrate web is transported through one or more laser systems 120a, 120b, and 120c. Although the embodiment shown in Figure 2 includes three laser systems 120a-c, it should be understood that any number of laser systems may be used to enable the manufacturing system 100 to function as described herein.

[0109] The use of the production system will be further described with reference to Figures 2-6. The substrate web 104 is transported through the laser systems 120a-c in the down-web direction WD. In one embodiment, the substrate web 104 is transported to the laser system 120a in a first state 400, before ablation or cutting. The substrate web 104 is transported over the chuck 306, and therefore over a plurality of vacuum holes 406. The vacuum holes 406 are in fluid communication with a vacuum 308, which is controlled via a user interface 116 to apply vacuum pressure to the substrate web 104 as it passes through the vacuum holes 406. The vacuum pressure is controlled to maintain a substantially flat / planar state as the substrate web 104 is transported across the chuck 306. In one embodiment of use, the vacuum pressure through the vacuum holes 406 is monitored and adjusted in real time via the user interface 116 to ensure that the substrate web 104 maintains a substantially flat state across the chuck 306 and does not lift or buckle during processing.

[0110] Referring to Figure 4, the web 104 of the substrate is transported over the opening 410 of the chuck 306 and further over the chamfered portion 416 of the downstream edge 414. In this embodiment, the chamfer 416 facilitates the passage of the web 104 of the substrate over the downstream edge 414 without the web 104 getting caught or snagged on the downstream edge 414.

[0111] Referring further to Figures 3-5, in one embodiment of use, the substrate web 104 is ablated by a laser beam 302 (Figure 3) to form an ablation 404 (Figure 4) on the substrate web 104. In one embodiment, the substrate web 104 is an anode material 502, and the ablation 404 removes the anode active material layer 508 to expose the anode current collector layer 506 (Figure 5). In another embodiment, the substrate web 104 is a cathode material 504, and the ablation 404 removes the cathode active material layer 512 to expose the cathode current collector 510.

[0112] During use, when the laser system 120a is used to form ablation 404 on the substrate web 104, the output of the laser beam 302 is controlled via the user interface 116 to a level that allows for substantially or completely removal of the coating layer, but without damaging or cutting the current collector layer. During use, the laser beam 302 is controlled, for example, via the user interface 116, to form ablation 404 while the substrate web 104 is moving and being transported in the web-downward WD direction. The laser beam 302 is controlled so that ablation 404 is formed on each side of the substrate web 104, as best shown in Figure 5. In one embodiment of use, after forming the ablation 404, the laser system 120a is controlled to cut fiducial features 602 in the substrate web 104, as further described herein. In some embodiments, multiple lasers are used, each to ablate a portion of the substrate web 104, each creating one or more ablation 404 to increase the throughput of the manufacturing system 100.

[0113] Referring further to Figures 2, 3, and 4, in another stage of the production process, the substrate web 104 is transported in the down-web direction WD toward the cutting area 408 of the laser system 120a. In this embodiment, the opening 410 is in fluid communication with a vacuum 308, which is controlled to draw vacuum pressure as the substrate web 104 passes over the opening 410. In another embodiment, a second vacuum is controlled to equalize the pressure on the substrate web 104 facing the chuck 306. In this embodiment, the pressure equalization is monitored and controlled to keep the substrate web 104 substantially flat / planar and at a constant height as it passes over the opening 410, facilitating the focusing of the laser beam 302 onto the substrate web 104.

[0114] In one embodiment of use, the laser system 120a is controlled to cut one or more patterns into the substrate web 104 while the substrate web is over the opening 410. Referring to Figure 6, the laser system is controlled to cut one or more longitudinal edge cuts 600 to define the longitudinal edge of the electrode in the cross-web direction XWD. The longitudinal edge cuts 600 are cut using the laser beam 302 by cutting the substrate web 104 in the cross-web direction XWD while the substrate web is being transported in the down-web direction WD. For example, in one embodiment, the path motion of the laser beam 302 is controlled and / or synchronized with the motion of the substrate web 104 in the down-web direction WD. Thus, the path of the laser beam 302 moves obliquely with respect to the down-web direction WD to account for the movement of the substrate web 104 in the down-web direction WD. In this embodiment, a compensation factor is applied to the path of the laser beam 302 so that cuts can be made in the cross-web direction XWD while the substrate web is moving continuously in the down-web direction WD. In this embodiment, as the substrate web 104 moves in the web direction WD, the laser is projected onto the substrate web 104 at an initial cut position 604, and then controlled to move in both the cross-web direction XWD and the web direction WD, forming a longitudinal edge cut 600 until it reaches the end-cut position 606. It should be understood that the angle at which the laser beam 302 is controlled to move varies based on the velocity of the substrate web 104 in the down-web direction WD. In another embodiment, the substrate web 104 is temporarily stopped during the laser processing operation, and therefore the path of the laser beam 302 does not need to take into account the moving motion of the substrate web 104. Such embodiments may be called a step process, or a step-and-repeat process. During laser processing, one or more of the laser systems 120a-c use a repeating alignment feature, such as a fiducial feature 602, to adjust and / or align the laser beam 302 during the laser processing operation, for example, to compensate for possible variations in the position of the substrate web 104.

[0115] Referring further to Figure 6, in one embodiment of use, the laser system 120a is controlled to cut one or more repeating alignment features, such as multiple fiducial features 602, in the web 104 of the substrate. The fiducial features 602 are cut at predetermined / known locations on the web 104 of the substrate. In one embodiment of use, the fiducial features 602 are tracked by one or more of the visual inspection systems 310, 312 to measure the position and moving speed of the web 104 of the substrate. The measurement of the fiducial features 602 is then used to accurately maintain the front-to-back alignment of the pattern on the web 104 of the substrate in both the down-web direction WD and the cross-web direction XWD. In some embodiments of use, the laser system 120a cuts multiple tractor holes 612 and / or fiducial features 602. In other embodiments, the fiducial features 602 are pre-formed on the web 104 of the substrate so that one or more of the laser systems 120a-c use them for positioning / alignment as described above.

[0116] Referring to Figures 2 and 6, in one preferred embodiment of use, the laser system 120a is controlled to cut a first perforation 608 and a second perforation 610 into the substrate web 104 as part of the electrode pattern when the substrate web is moving in the down-web direction WD. The first perforation 608 is formed by laser cutting with the laser beam 302 while the substrate web is positioned over the opening 410 of the chuck 306. The first perforation 608 is formed as a linear slit (e.g., a through-cut) in a direction consistent with the down-web direction WD. Importantly, the first perforation 608 is formed into the electrode W e The cutting is to be such that it does not extend across the entire width. Instead, the laser system 120a is controlled to cut the pattern so that the outer tear strip 700 remains on both the upstream and downstream edges of the perforation 608, so that the electrode pattern remains connected to the web 104 of the substrate.

[0117] Referring further to Figures 6 and 7, in use, the second perforation 610 is cut inboard (cross-web direction XWD) from the first perforation 608. In this embodiment of use, the second perforation 610 is cut as a line of slits in the down-web direction WD separated by the inner tear strip 702. In the illustrated embodiment, the second perforation 610 is cut so as to intersect with the through hole 704. In the illustrated embodiment, the inner tear strip 702 is cut to be at least twice the length of the outer tear strip 700, but it may be cut to different lengths so that the manufacturing system 100 functions as described herein.

[0118] During use, as shown in Figures 3, 4, and 6, fragments from the laser cut for the longitudinal edge cut 600, fiducial feature 602, and first and second perforations 608, 610 on the opening 410 of the chuck 306 are dropped through the opening 410, and the vacuum 308 is controlled to collect the fragments formed during the laser cutting process.

[0119] In one preferred embodiment of use, the laser system 120a is configured as a first ablation station. In this embodiment, the laser system 120a is controlled to form the ablation 404 described above on a first surface of the substrate web 104. Leaving the laser system 120a, the substrate web is transported on the idler 108d to invert the substrate web 104 in such a way that a second surface of the substrate web 104 (facing the first surface) is positioned for processing by the laser system 120b. In this embodiment, the laser system 120b is configured as a second ablation station and uses fiducial features 602 to ensure alignment of the ablation 404 in the down-web direction WD and the cross-web direction XWD. Thus, the laser system 120b is controlled to perform a second ablation process on opposing surfaces of the substrate web 104 so that the ablation 404 on each surface of the substrate web 104 is aligned in the web direction WD and the cross-web direction XWD.

[0120] In one embodiment of use, the laser system 120c shown in Figure 2 is configured as a laser cutting station. In this embodiment, the laser system 120c is controlled to perform laser cutting for longitudinal edge cuts 600 and for first and second holes 608 and 610.

[0121] Referring further to Figures 2, 10, and 11, in one embodiment of use, the substrate web is then transported through one or more cleaning stations, such as a brushing station 124 and an air knife 126, after exiting one or more laser systems 120a-c. In one preferred embodiment of use, the substrate web 104 is transported through the brushing station 124, where a bristle 1002 is controlled to make subtle contact with the surface of the substrate web 104, removing or dislodging any debris therefrom. The contact pressure of the bristle 1002 against the surface of the substrate web 104 is controlled to be low enough not to cause damage, rupture, or other defects to the electrode pattern, thus maintaining the electrode pattern attached to the substrate web 104.

[0122] Referring further to Figures 10 and 11, in one embodiment of a preferred use, the brush 1000 is controlled to move in the cross-web direction XWD by controlling the motor 1014 to cause rotation of the drive wheel 1010. A position sensor 1016 is controlled to sense the position of the brush position marker 1018 and to measure the phase (e.g., angular position) and rotations per unit time of the drive wheel 1010.

[0123] In one preferred embodiment of use, a second brush (not shown) is controlled to contact the opposing surface of the substrate web 104. In this embodiment, the second brush, which may be substantially the same as the first brush 1000, is controlled to move in the opposite direction to the first brush, preferably with a 180-degree phase difference. The phases of the first and second brushes can be monitored via position sensor 1016 and an equivalent position sensor on the second brush. In this embodiment, the contact pressure of the bristles of the first and second brushes together is controlled to be low enough not to cause damage, rupture, or other defects to the electrode pattern, and to maintain the electrode pattern in contact with the substrate web 104.

[0124] During use, the vibration speed of the brush 1000 and the pressure exerted by the bristle 1002 on the web 104 surface of the substrate can be controlled by the user using the user interface 116.

[0125] In one embodiment of use, the brushing station 124 is equipped with a vacuum system that creates a vacuum through the brushing station orifice 1020 and is controlled to discharge brushed debris from one or more surfaces of the substrate web 104. In this embodiment, the debris is either brushed off the substrate web 104 and falls, or sucked in through the brushing station orifice 1020.

[0126] In this embodiment, the first and second brushes are controlled via the user interface 116 to maintain a substantially uniform brushing pressure on the electrode material web 802 based on wear of the brush bristles, the thickness of the electrodes, or variations in surface roughness.

[0127] In another preferred embodiment of use, one or more of the first and second brushes are controlled to move at least partially in the down-web direction WD at a speed equal to the speed of the electrode material web 802, thereby maintaining a substantially zero speed difference between the brush and the electrode material web 802 in the down-web direction WD.

[0128] In yet another preferred embodiment of use, the brushing station 124 comprises a phase measuring sensor 1016 for determining the phases of a first brush and a second brush. In this embodiment, the phase sensor measures the positions of brush position markers 1018 (e.g., origin sensor flags) of the first brush and the second brush. In this embodiment, the phase measuring sensor 1016 determines whether the first brush and the second brush are out of phase by 180 degrees, 90 degrees, 0 degrees, or within a predetermined phase difference range, such as any other suitable phase difference that would allow the manufacturing system 100 to function as described herein, and allows for correction or warns the user via the user interface 116 or other warning device that the brushes are not properly phased.

[0129] In yet another preferred embodiment of use, the brushing station 124 comprises a phase measuring sensor 1016 for determining the phases of the first and second brushes. In this embodiment, the phase sensor measures the positions of brush position markers 1018 (e.g., home sensor flags) of the first and second brushes. In this embodiment, the phase measuring sensor 1016 determines whether the first and second brushes are out of phase by 180 degrees, 90 degrees, 0 degrees, or within a predetermined range of phase differences, such as any other suitable phase difference that would enable the manufacturing system 100 to function as described herein, and allows for correction or warns the user via the user interface 116 or other warning device that the brushes are not properly phased.

[0130] In yet another embodiment of use, an ultrasonic transducer (not shown) is activated to apply ultrasonic vibrations to one or more of the first and second brushes to facilitate the removal of debris from the electrode material web 802.

[0131] Referring further to Figure 2, in one preferred embodiment of use, the substrate web 104 is transported through an air knife 126. In this embodiment, high-pressure air is controlled to come into contact with the surface of the substrate web 104, removing debris therefrom. The air knife 126 is controlled, for example, via a user interface 116, to supply air at a pressure / velocity that does not cause defects such as damage or rupture to the electrode pattern, and to maintain the electrode pattern in contact with the substrate web 104. In another embodiment, a second air knife 126 is controlled to blow air onto an opposing surface of the substrate web 104, removing debris therefrom. In this embodiment, the second air knife is controlled to blow air in the same direction as the first air knife, or in a direction opposite to the first air knife, or in any other direction that allows the air knife 126 to function as described herein. In another embodiment, the air knife 126 station includes a vacuum controlled to facilitate the removal of debris removed by the air knife 126.

[0132] Referring to Figure 8, after being processed by laser systems 120a-c and cleaned by brushing station 124 and air knife 126, the substrate web 104 leaves the cleaning station as a web containing multiple electrode patterns 800 within the substrate web 104, collectively as a web of electrode material 802.

[0133] Referring further to Figures 2, 8, and 12, in one embodiment of use, the electrode material web 802 is transported through an inspection device 128. The inspection device 128 is controlled to analyze the electrode material 802 and identify its defects. For example, in one embodiment, the inspection device 128 is a visual inspection device including a camera 1200. The lens 1202 is directed to focus on the electrode material web 802 as it passes over an inspection plate 1206. In one embodiment of use, the inspection plate 1206 includes a transparent or translucent top 1208 that allows light from a light source (not shown) housed within the inspection plate 1206 to illuminate it. In one preferred embodiment, the intensity and / or color of the light is controlled via a user interface 116. The electrode material web 802 is then taught to the inspection plate 1206 to substantially eliminate curling of the electrode material web 802.

[0134] Referring further to Figure 12, in one embodiment of use, the inspection device 128 includes a trigger sensor 1212 controlled to detect predetermined features of the electrode material web 802, such as fiducial features 602, longitudinal edge cuts 600, or other features that enable the inspection device 128 to function as described herein. When the electrode is imaged, the camera 1200 is controlled to detect one or more metrics, such as the height of the electrode, the size or shape of a feature cut by one of the laser devices 120a-120c (Figure 2), the pitch (distance) between the electrodes, or other features that enable the inspection device to function as described herein. For example, in one preferred embodiment, the inspection device 128 is controlled to detect whether there is an ablation 404 (Figure 4), a longitudinal edge cut 600, a fiducial feature 602, and first and second perforations 608, 610 (Figure 6). 6) The system detects whether the cross-web direction XWD dimension of individual electrode structures, the down-web direction WD dimension of individual electrode structures, the individual electrode active area offset, and any other cuts or abrasions of the web 802 of the electrode material are within predefined tolerances for size, shape, arrangement, cross-machine direction pitch, machine direction pitch, and orientation, and presents this information to the user via the user interface 116. In one preferred embodiment, the user can use the user interface 116 to control which features are inspected. In yet another embodiment, the inspection device 128 may detect cluster identification codes of one or more electrode structures in the web 802 of the electrode material.

[0135] In this embodiment, the inspection device 128 is controlled to measure metrics such as the thickness of the web, the size and shape of the electrode pattern, while the web is being transported in the machine direction. These metrics are transmitted to the user interface 116 for display or memory storage, or used to adjust production parameters of the manufacturing system 100.

[0136] In one embodiment of use, if the inspection system determines that a defect exists on the web of electrode material 802 (Figure 8), the marking device 130 (Figure 2) is controlled to mark the web of electrode material 802 to identify such defect using a laser etching device, printer, stamper, or any other marking device capable of placing a mark indicating the presence of a defect on the web of electrode material 802. In another preferred embodiment of use, the marking device 130 is controlled to mark one or more of the identification number (ID) and known good electrode (KGE) on the web of electrode material 802, and allows for the possibility of further marking the web of electrode material 802 with grades such as Grade A, Grade B, Grade C, indicating a quality measurement of a particular electrode within the web of electrode material 802 (such as the number or type of defects).

[0137] Referring further to Figure 9, the electrode material web 802 is then transported to the winding roller 134, where it is wound together with the interleaf material web 138 to create a spool 900 having alternating layers of electrode material web 802 and interleaf material web 138.

[0138] In one preferred embodiment of use, the base material web 104 is wound together with the web of the interleaf material 138 via the winding roller 134 and unwound via the interleaf material roller 136 to create a roll of electrodes 140 having layers of electrodes separated by the interleaf material 138. In some embodiments, the base material web 104 is wound via the winding roller 134 without the web of the interleaf material 138.

[0139] In one embodiment, the web 104 of the substrate has an adhesive tape layer (not shown) bonded to one or both surfaces of the anode active material 508 or the cathode active material layer 512. In this embodiment, during use, the adhesive layer is removed following ablation and cutting (as described above) to remove any unwanted material or debris.

[0140] In one embodiment of use, one or more rollers in the conveyor system are not perfectly circular, such that the rollers are eccentric. In such embodiments, the eccentric rollers are mapped to determine their radial-to-radial position. The laser systems 120a-c are controlled to adjust the position of the laser beams 302 to account for the eccentricity based on the roller mapping.

[0141] Referring to Figures 14-16, the electrode material web 802 is used to manufacture a battery. In this embodiment, the individual spools of electrode material web from spools 1402, 1404, and 1406A, 1406B are each unwound, merged in merge zone 1408, and stacked in punching and lamination zone 1410 in an alternating configuration including at least one layer of cathode material web from spool 1402 and anode material web from spool 1404, and separated by separator material web from spool 1406. It should be understood that the electrode material spools from spools 1402, 1404, and 1406A, 1406B are manufactured as electrode material web 802 as described herein.

[0142] Refer to Figures 14A and 15A to describe additional details of the merge zone 1408 and the merging process. In the merge zone 1408, the spools of electrode material webs from spools 1402, 1404, and 1406A, 1406B are individually unwound in the direction indicated by arrow U. In one embodiment, the spools of electrode material from spools 1402, 1404, and 1406A, 1406B are the rolls of electrodes 140 described above. In the embodiment shown in Figure 14A, spool 1406 is a spool of wound web separator material having a cluster of individual electrode separators 1506 formed therein, each surrounded by an outer perforation 608 and a longitudinal edge cut 600. Spool 1402 is a spool of wound web cathode material having a cluster of individual cathode electrodes 1502 formed therein, each surrounded by an outer perforation 608 and a longitudinal edge cut 600. The spool 1404 is a spool of anode material for a wound web, having a cluster of individual anode electrodes 1504 formed therein, surrounded by an outer perforation 608 and a longitudinal edge cut 600.

[0143] As is most commonly seen in Figure 15A, each spool of electrode material from spools 1402, 1404, and 1406 is formed by a web having a continuous outer edge 1508 in which tractor holes 612 are formed, and a web edge boundary 1510 defining the outer circumference of the web. In other embodiments, it should be understood that the order and arrangement of the spools of electrode material from spools 1402, 1404, and 1406 during the merging process may differ, as long as separator material is placed between any adjacent layers of anode and cathode material to prevent short circuits.

[0144] In one embodiment, as each spool of electrode material is unwound from spools 1402, 1404, and 1406, the unwound webs of each spool 1402, 1404, and 1406 are controlled to form a catenary curve 1412 before engagement with the merge sprocket 1414, as shown, for example, in Figure 14B. In embodiments using the catenary curve 1412, the catenary curve 1412 facilitates the self-alignment and / or tensioning of the webs from spools 1402, 1404, and 1406 to the merge sprocket 1414 without the use of steering rollers or dancers. In another embodiment, as an alternative to, or in addition to, the catenary curve 1412, web steering rollers and dancers (similar to, for example, dancer 118) precisely control the position of the unwound webs when they engage with the merge sprocket 1414. In embodiments, the merge sprocket 1414 may have a radius Rs of 19 mm or more (Figures 14H1-3), such as 38 mm, 51 mm, 76 mm, 114 mm, 152 mm, or any other radius that enables the system to function as described herein. It should be noted that any or all of the other sprockets, spools, and rollers described herein may have the same or similar radii that enable the system to function as described herein. From a practical standpoint, in some embodiments, it is desirable to reduce the size of the merge sprocket 1414 (and any other sprockets, spools, or rollers) so that it takes up less space, and therefore the system can be made smaller accordingly. In addition, it should be noted that by using smaller sprockets, spools, and rollers, the total path length over which the web travels while being processed in the system can be shortened, as described herein, thereby promoting waste reduction and improved web alignment. Each of the merge sprockets 1414 includes a group of teeth 1416 (e.g., pins or projections) of a size, shape and arrangement such that they engage or align precisely with the tractor holes 612 of the web. For example, if the tractor holes 612 have a square cross-sectional shape, the teeth 1416 will have a corresponding square cross-sectional shape.However, the size and shape of the tractor holes 612 and teeth 1416 may be any size and shape, including any taper, that allows the system to function as described herein, for example, the following cross-sectional shapes: square, rectangular, circular, elliptical, triangular, polygonal, or a combination thereof.

[0145] Referring to Figures 14A, 14B, and 14H1-3, the webs of electrode material from the spools 1402, 1404, and 1406 are moved in a circular path around each merge sprocket 1414 until they engage with the reversing tooth sprocket 1418. In embodiments, the radius of the reversing tooth sprocket 1418 is 19 mm or greater, and is, for example, 38 mm, 51 mm, 76 mm, 114 mm, 152 mm, or any other radius that allows the system to function as described herein. Each of the reversing tooth sprockets 1418 includes a group of reversing teeth 1420 configured to engage with the teeth 1416 of the merge sprocket 1414 while one of the webs from each of the spools 1402, 1404, and 1406 is positioned between them, in order to facilitate proper positioning and tension maintenance of the webs of electrode material from the spools 1402, 1404, and 1406 during the unwinding procedure. In one preferred embodiment, the merge sprocket 1414 is driven by a motor, and its speed is controlled to ensure proper tension in the web of electrode material from the spools 1402, 1404, and 1406. In another embodiment, the merge sprocket 1414 rotates freely, and the speed of the spools of electrode material from the spools 1402, 1404, and 1406 is controlled to ensure proper tension in the web of electrode material from the spools 1402, 1404, and 1406. In yet another embodiment, the merge sprocket 1414 is controlled to rotate at a fixed speed, mechanically or electronically keyed to match the speed of the pin plate 1424. In this embodiment, the pin plate 1424 acts as a master component for speed control, and the merge sprocket 1414 is driven as a slave component to match the speed of the pin plate 1424. In this embodiment, the speed of the electrode material spools from spools 1402, 1404, and 1406 can also be controlled to ensure proper tension of the web of electrode material from spools 1402, 1404, and 1406.In one such embodiment, a loop sensor 1422, such as an optical or physical sensor, determines the amount of sag (curvature) of the catenary curve 1412, which is then used to calculate the tension of the web from the spools of electrode material from spools 1402, 1404, and 1406. For example, if it is determined that the sag is too large (i.e., the tension is too low), the speed of the merge sprocket 1414 is increased or the speed of the spools of electrode material from spools 1402, 1404, and 1406 is decreased in order to reduce the sag to within a predetermined range (i.e., increase the tension). Alternatively, if it is determined that the sag is too small (i.e., the tension is too high), the speed of the merge sprocket 1414 is decreased or the speed of the spools of electrode material from spools 1402, 1404, and 1406 is increased in order to increase the sag to within a predetermined range (i.e., decrease the tension). In one embodiment, sag is targeted to control the angle αCL at which the webs of the electrode material spools 1402, 1404, and 1406 contact the merge sprocket 1414. In such an embodiment, αCL is from 0° to 90°, measured counterclockwise from the vertical, and for example, in an embodiment, αCL is 0°, 5°, 10°, 15°, 20°, 25°, 30°, 35°, 40°, 45°, 50°, 55°, 60°, 65°, 70°, 75°, 80°, 85°, or 90°. In another embodiment, αCL is controlled to be within ±5° from the vacuum tensioner 1442. In the embodiment shown in Figure 14H1, αCL may also be indicated using clock positions, where 12:00 refers to the upper vertical position and each hour in the clockwise direction refers to a movement of 30 degrees. Therefore, in the embodiment shown in Figure 14H1, the webs from spools 1402, 1404, and 1406 contact the merge sprocket 1414 at the 10:30 position on the merge sprocket 1414, and the brush 1440 is positioned at the 11:00 position.

[0146] After the webs of electrode material from spools 1402, 1404, and 1406 are unwound onto the reversing tooth sprocket 1418, each web is then guided and transported onto a pin plate 1424 at a transport position 1426. In one embodiment, the tension of the webs of electrode material from spools 1402, 1404, and 1406 is controlled so that each web is transported onto the pin plate 1424 at the 6 o'clock position (e.g., vertically downward). The pin plate 1424 includes a series of pins 1428 that are sized and shaped to precisely engage with the tractor holes 612 of the webs of electrode material from spools 1402, 1404, and 1406, as well as with the reversing teeth 1420 of the reversing tooth sprocket 1418. Therefore, each of the webs of electrode material from spools 1402, 1404, and 1406 is sandwiched between the pin plate 1424 and the reversing tooth sprocket 1418 as it is transferred onto the pin plate 1424, while the pin 1428 extends into the reversing tooth 1420 through the tractor hole 612 to facilitate the alignment of the webs of electrode material from spools 1402, 1404, and 1406 onto the pin plate 1424.

[0147] In one embodiment, the reversing tooth sprocket 1418 is positioned at a suitable height above the pin plate 1424 in the Z direction, for example, between 0 μm and 3000 μm, i.e., 0 μm, 1 μm, 5 μm, 10 μm, 20 μm, 50 μm, 100 μm, 200 μm, 300 μm, 500 μm, 1000 μm, 1250 μm, 1500 μm, 2000 μm, 2500 μm, 3000 μm, or other distances that allow the system to operate as described herein. In one embodiment, the reversing tooth sprocket 1418 is positioned at a suitable height above the pin plate 1424 in the Z direction, based on the height of the web on the pin plate 1424. For example, in the embodiment, the reversing tooth sprocket 1418 is positioned at an appropriate height above the pin plate 1424 in the Z direction, up to a height of no more than 10 times the height of the web on the pin plate 1424. In this context, "float" refers to a portion of the web that is not in contact with either the reversing tooth sprocket 1418 or the pin plate 1424, so that the web has some slack to facilitate the self-alignment of the tractor hole 612 with respect to the pin 1428. In the embodiment, the height of the reversing tooth sprocket 1418 above the pin plate 1424 may be automatically or manually adjustable to ensure the self-alignment of the tractor hole 612 with respect to the pin 1428.

[0148] In another embodiment, the height of the reversing tooth sprocket 1418 on the pin plate 1424 may vary depending on which of the webs of electrode material from spools 1402, 1404, and 1406 is transferred to the pin plate 1424. In this embodiment, small possible misalignments of each web of electrode material from spools 1402, 1404, and 1406 are reduced or eliminated by allowing the webs of electrode material from spools 1402, 1404, and 1406 to have enough slack (i.e., a web not in contact with either the reversing tooth sprocket 1418 or the pin plate 1424) to self-adjust, and thus allow each tractor hole 612 to align with the pin plate 1424. In one preferred embodiment, the slack is sufficient to form an S-shaped curve in the web of electrode material from spools 1402, 1404, and 1406 between the reversing tooth sprocket 1418 and the pin plate 1424. As each layer of the electrode material web from spools 1402, 1404, and 1406 is positioned on the pin plate 1424, it should be understood that the subsequent (i.e., downstream) nip formed between the reversing tooth sprocket 1418 and the pin plate 1424 will increase in size in consideration of the preceding layer of the electrode material web from spools 1402, 1404, and 1406 positioned on it. In one preferred embodiment, the nip distance increases by an amount equal to the thickness of the preceding layer of the electrode material web from spools 1402, 1404, and 1406 positioned on the pin plate 1424.

[0149] In one embodiment, as shown in Figure 14A, there are four spools of electrode material webs from spools 1402, 1406, 1404, and 1406. In this embodiment, spools 1402, 1406, 1404, and 1406 are arranged so that they can be sequentially unwound and joined onto a pin plate 1424. In this embodiment, the pin plate 1424 extends from a pre-merge position 1430 located upstream of the first transfer position 1426. The pin plate 1424 extends to a downstream position past the last transfer position 1426X (Figure 14A). In this embodiment, each of the four spools of electrode material webs from spools 1402, 1406A, 1404, and 1406B has its own transfer positions 1426, 1426A, 1426B, and 1426X, respectively. In other embodiments, additional spools of electrode material may be unwound and combined, and therefore additional transfer positions may be included for each additional spool.

[0150] Referring to Figures 14A, 14B, 14C1, 14C2, and 14C3, the individual layers of the electrode material web from spools 1402, 1406A, 1404, and 1406B are merged (e.g., sequentially stacked) to form the merged material web 1432. Each layer of the electrode material web from spools 1402, 1406A, 1404, and 1406B is, for example, aligned along the longitudinal axis A of each electrode pattern. E(Figure 7), each layer of the merge material web is merged so that it is vertically aligned, such that one or more of the tractor holes 612, fiducial features 602 and longitudinal edge cuts 600 and the perforations 608, 610 of the electrode patterns of each layer (Figure 6) are aligned in both the web direction and the cross-web direction XWD. Variations in web alignment can lead to defects in subsequent operations such as punching and stacking, and therefore maintaining web alignment when merging webs from spools 1402, 1406A, 1404, and 1406B is important in some embodiments. Note that the spools of separator material 1406A and 1406B may be the same separator material or different separator materials. When used herein, when describing spools of separator material webs in general, 1406A and 1406B may be referred to as spools of separator material webs from spool 1406 in general.

[0151] Each layer of the merge material web 1432 is transported sequentially layer by layer, as described in the steps above, so that it is aligned vertically. That is, the first layer in this embodiment, consisting of the separator material web from spool 1406, is transported to the pin plate 1424 at transport position 1426. Then, at transport position 1426A, located downstream of transport position 1426, the cathode material web from spool 1402 is transported on top of the separator material web from spool 1406. Next, a second layer of separator material from spool 1406 (via another spool) is transported on top of the layer of separator material from spool 1406 at transport position 1426B, located downstream of transport position 1426A. In this embodiment, a layer of anode material web from spool 1404 is transported on top of the second layer of separator material web from spool 1406 at transport position 1426X. When all four layers are stacked or joined, the four-layer laminated web is called a merged material web 1432. While each layer is being transported onto the pin plate 1424, the target downweb tension for each layer of the merged material web 1432 is zero. In one embodiment, the downweb tension for each layer of the merged material web 1432 is determined by the mass of the web from each spool 1402, 1404, 1406 and the amount of slack in such webs between the merge sprocket 1414 and the pin 1428 of the pin plate 1424, respectively.

[0152] During the transfer of each layer, it should be understood that the pins 1428 of the pin plate 1424 extend through each layer of material into the reversing teeth 1420 of the reversing tooth sprocket 1418, and are sized to maintain the alignment of each layer relative to one another. At each transfer position, a nip (i.e., gap) is formed at the transfer position 1426 between each reversing tooth sprocket 1418 and the pin plate 1424, and this nip is set to a fixed gap distance of 100 to 1000 μm across the web. In one embodiment, the nip is set to about three times the thickness of the web. For example, if the thickness of the web in the Z direction is 100 microns, the nip gap will be about 300 microns in the Z direction. It should be understood that the actual gap distance between each reversing tooth sprocket 1418 and the pin plate 1424 is increased at each downstream transfer position 1426 to account for the added thickness of each previous layer transferred onto the pin plate 1424. In one embodiment, the increase in gap distance at each subsequent downstream transfer position is approximately equal to the height of the added layer in the Z direction. In one embodiment, the nip gap is approximately three times the height of the merge material web at each transfer position 1426. As shown in Figures 14E1 to 14E4, the pins 1428 of the pin plate 1424 may have a constant cross-sectional area in the Z direction, as shown in the upper diagrams of Figures 14E1 to 12E4, or they may be tapered to have a larger cross-sectional area proximal to the pin plate 1424 in the Z direction. In embodiments where the pins 1428 have such a taper, the merge material web is preferably located above the pin plate 1424, approximately midway between the pins 1428 in the Z direction. Furthermore, in other embodiments, the order of the layers may vary depending on the desired result, and accordingly, the positioning of each of the spools 1402, 1404, and 1406 may be placed at the corresponding transfer position to facilitate proper lamination of the web from the spools of electrode material from spools 1402, 1404, and 1406. Additional spools of electrode material may be included, and a corresponding number of transfer positions may be used to facilitate the lamination of additional webs.

[0153] Figure 15 shows a cross-sectional view 1500 of one embodiment of the merged material web 1432, which can also represent a cross-section of a multilayer electrode substack. In this embodiment, the merged material web 1432 is formed by laminating a central anode current collector layer 506, an anode active material layer 508, an electrically insulating separator material 500, a cathode active material layer 512, and a cathode conductor layer 510. Additional layers can be merged to form a desired number of layers of the merged material web 1432 by alternately laminating the web layers from the spools of anode 1404, separator 1406, and cathode 1402. In one embodiment, the spools of anode 1404, separator 1406, and cathode 1402 may be rolls of electrode 140, as described above.

[0154] In some embodiments, the pin plate 1424 comprises a group of individual separate pin plates (each similar to the pin plate 1424) that are abutted against and indexed to each other to form a continuous flow of pin plates. In this embodiment, it is important that the individual pin plates are precisely positioned relative to each other so that proper registration of the layers of the merge material web 1432 is maintained as each layer is transferred onto the pin plate. Thus, in some embodiments, each pin plate 1424 may be held by fixtures or other alignment devices such as pins, magnets, projections, etc., to maintain proper registration of the pin plate 1424. The pin plate 1424 is transported in the web direction via a conveyor mechanism 1436 controlled to move at the same speed as a reversing tooth sprocket 1418 so that the layers of the merge material web 1432 are properly aligned with the pins 1428 of the pin plate 1424. In one embodiment, the engagement of the pins 1428 with the reversing teeth 1420 propels the pin plate 1424 down the web direction WD. Therefore, in such embodiments, an appropriate speed is maintained between the pin plate 1424 and the reverse-tooth sprocket 1418.

[0155] In one embodiment, the electrode defect sensor 1434 is positioned such that at one or more transfer positions 1426, 1426A-X, the web of electrode material from spools 1402, 1404, and 1406 passes adjacent to the defect sensor 1434. Note that, as used herein, 1426X is used to refer to any number of additional transfer positions as described herein. The defect sensor 1434 is configured to detect defects in the web of electrode material from spools 1402, 1404, and 1406. For example, the defect sensor 1434 may be configured to detect missing electrodes from the web, misalignment or absence of tractor holes 612, fiducial features 602, excision, cut, perforation, or other weakened areas in the web of electrode material from spools 1402, 1404, and 1406. If the defect sensor 1434 detects a defect in the web of electrode material from spools 1402, 1404, and 1406, the web can be marked to indicate the defect using a marking device working in conjunction with the defect sensor 1434. The defect marking may be used in subsequent process steps to ensure that the defective portion of the web of electrode material from spools 1402, 1404, and 1406 is not used in the lamination stage described further below, or is disposed of in other ways before becoming part of the lamination cell 1704.

[0156] Referring to Figure 14D, one embodiment of the manufacturing system includes an electrode material tensioning unit 1438 configured to flatten the webs of electrode material from spools 1402, 1404, and 1406 before they enter the transfer position 1426. In one embodiment, the webs of electrode material from spools 1402, 1404, and 1406 may tend to curl or cup so that the web becomes U-shaped. It is hypothesized that this curl may be caused by weakening of the web structure by the longitudinal edge cuts 600, which cause the central portion of the web to sag. Furthermore, if electricity or static electricity accumulates along the longitudinal edges of the webs of electrode material from spools 1402, 1404, and 1406, such edges may curl inward. If the webs of electrode material from spools 1402, 1404, and 1406 have such curls, the position of the tractor holes 612 and the spacing between opposing tractor holes 612 will not be aligned with respect to the merge sprocket 1414.

[0157] Therefore, to improve curl, the tensioning unit 1438 may include at least one of the reverse-rotating brushes 1440 (Figures 14D, 14F1-14F3, 14G, 14H1-14H3) and a vacuum tensioner 1442. In one embodiment, the reverse-rotating brush 1440 is driven by an electric motor (not shown) in the opposite direction Wb in the cross-web direction XWD. In one embodiment, the reverse-rotating brush has an outer diameter Db of 25 mm to 150 mm and an inner diameter Da of 10 mm to 50 mm. In one embodiment, the reverse-rotating brush has a central through hole 1441 having a diameter of 5 mm to 25 mm, the center of which defines the axis on which the reverse-rotating brush 1440 rotates. Each reverse-rotating brush 1440 has a thickness TB of 2 mm to 20 mm. The reverse-rotating brush comprises several bristle 1443 which may be made of natural or synthetic materials such as animal hair, nylon, carbon fiber, high-density polyethylene, high-temperature nylon, PEEK, polyester, polyethylene, polypropylene, polystyrene, polyvinyl chloride, metal, metal alloy, and plastic. In a preferred embodiment, the bristle 1443 is made of nylon. The bristle material should be appropriately selected so that the brush functions as described herein without abrasive or otherwise damaging the web. The reverse-rotating brush 1440 is positioned adjacently and adjustablely to flatten the web of electrode material from spools 1402, 1404, and 1406 so as to contact the web at a brush pitch angle αbp (Figure 14G) with sufficient pressure to uncurl and flatten the longitudinal ends of the web of electrode material from spools 1402, 1404, and 1406 before engaging with the merge sprocket 1414. In some embodiments, the rotational speed and contact pressure of the reverse-rotating brush 1440 may be monitored and adjusted to ensure that sufficient flatness of the web of electrode material from spools 1402, 1404, and 1406 is obtained. In one embodiment, as shown, for example, in Figure 14H2, the brush speed is referred to as a velocity vector Vbs having a velocity component Vb in the cross-web direction XWD and a velocity component Vs in the down-web direction WD.In the embodiment, the velocity component Vb is 50 mm / sec, 60 mm / sec, 70 mm / sec, 80 mm / sec, 90 mm / sec, 100 mm / sec, 110 mm / sec, 120 mm / sec, 130 mm / sec, 140 mm / sec, 150 mm / sec, 160 mm / sec, 170 mm / sec, 180 mm / sec, 190 mm / sec, 200 mm / sec, 210 mm / sec, 220 mm / sec, 230 mm / sec, 240 mm / sec, or 250 mm / sec, or any of these velocities, which can be set (for example by adjusting the rotational speed of the brush (e.g., rpm)). In an embodiment, the velocity component Vs can be set to 10 mm / s to 100 mm / s, e.g., 10 mm / s, 20 mm / s, 30 mm / s, 40 mm / s, 50 mm / s, 60 mm / s, 70 mm / s, 80 mm / s, 90 mm / s, 100 mm / s, or any velocity within that range (for example, by adjusting the speed of the web in the web direction WD). Thus, the speed of the brush tip across the web is V. bs =sqrt(V b 2 +V s 2 ) can be calculated as V bs This can be within the range of 51 mm / second to 270 mm / second.

[0158] In one embodiment, the tension adjustment unit includes a deionization device 1447 configured to reduce or remove static charge on the web of electrode material from spools 1402, 1404, and 1406. In such embodiments, the deionization device 1447 is located upstream, immediately before the vacuum tensioner 1442 and the reverse-rotating brush 1440. In some embodiments, the deionization device 1447 is configured to neutralize the charge on components such as the vacuum tensioner 1442, which may be formed from a plastic pipe such as PVC. For example, if a deionization device is not used, static charge may accumulate on the vacuum tensioner 1442 as separator material from spool 1406 passes over the vacuum tensioner, or as small particles are carried through the vacuum tensioner by airflow. Therefore, the deionization device 1447 can be used to neutralize the charge on the vacuum tensioner 1442, thus allowing the webs of electrode material from spools 1402, 1404, and 1406 to pass through the vacuum tensioner 1442 without being electrically attracted to it. Although the deionization device has been described in relation to the vacuum tensioner 1442, it should be noted that one or more deionization devices 1447 can be used in any component in a system that is affected by charge and would benefit from charge neutralization, such as any component that is in contact with or adjacent to the webs of electrode material from spools 1402, 1404, and 1406. In some embodiments, the deionization device 1447 is a DC ionization bar. In some embodiments, the deionization device 1447 is capable of pulsed DC ionization for short-distance applications such as 20 mm to 200 mm. In some embodiments, the pulse frequency can be controlled automatically or by the user to set it to 1 Hz to 20 Hz in order to adjust the effect of the deionization device 1447 on the affected components. In some embodiments, the deionization device 1447 consists of metal pins, such as titanium pins, used as ionizer emitters.Such pins can have an output of -3kV to +7.5kV in pulsed DC mode, which facilitates the enabling of a positive-negative charge-ion ratio of 80:20 to 20:80. Thus, in other embodiments, the order of the deionization device 1447, vacuum tensioner 1442, and reverse-rotating brush 1440 may be different. In another embodiment, charge accumulation can be prevented by grounding the affected component. In this embodiment, a grounding strap or grounding wire (not shown) is electrically connected to the affected device, such as the vacuum tensioner 1442, to prevent charge accumulation by providing a path for the charge to ground. In yet another embodiment, charge accumulation of the component can be prevented by coating the affected device with a conductive coating to prevent charge accumulation.

[0159] In one preferred embodiment, the rotational speed of the reverse-rotating brush 1440 is kept low enough to reduce or eliminate excessive wear or heat buildup caused by friction of the reverse-rotating brush 1440 in contact with the web of electrode material from spools 1402, 1404, and 1406. In one embodiment, the reverse-rotating brush 1440 is configured to smooth or otherwise reduce wrinkles present in the web of electrode material from spools 1402, 1404, and 1406. In one embodiment, the reverse-rotating brush 1440 is configured to reduce or remove micro-wrinkles in the web of electrode material from spools 1402, 1404, and 1406. In such an embodiment, micro-wrinkles are web wrinkles that are too small to be removed by the deionization device 1447 or the vacuum tensioner 1442. In such an embodiment, micro-wrinkles are defined as wrinkles that are about 20 percent the size of macro-wrinkles that are removed by the deionization device 1447 or the vacuum tensioner 1442. In a preferred example, if the macro-level wrinkles are approximately 100 mm in size in the Z direction, the micro-wrinkles are 20 mm or less in size in the Z direction. In other embodiments, the macro-wrinkles can be 1 mm to 250 mm in size, and the micro-wrinkles can be 0.2 mm to approximately 50 mm in size.

[0160] In another embodiment, in addition to, or instead of, the reverse-rotating brush 1440, the material tensioning unit 1438 includes a vacuum tensioner 1442, which includes a plurality of vacuum orifices 1444 positioned on the surface of the vacuum tensioner 1442 adjacent to the web of electrode material from spools 1402, 1404, and 1406. In this embodiment, a vacuum is drawn through the vacuum tensioner 1442, and suction occurs through the vacuum orifices 1444. The vacuum tensioner 1442 is positioned at an angle αvac (Figure 14G) with respect to the vertical. The suction from the vacuum orifices 1444 creates a fluid flow (typically an air flow) across the surface of the web of electrode material from spools 1402 facing the vacuum orifices 1444. Because the fluid flow is faster across the surface of the web of electrode material from spools 1402, 1404, and 1406 facing the vacuum orifice 1444 than on the opposite side of the web of electrode material from spools 1402, 1404, and 1406, its effect (i.e., the Bernoulli effect) pulls the web of electrode material from spools 1402, 1404, and 1406 taught to the vacuum tensioner 1442, facilitating alignment between the tractor hole 612 and the teeth 1416 of the merge sprocket 1414.

[0161] Referring further to Figure 14B, in one preferred embodiment, the teeth 1416 of the merge sprocket 1414 are tapered in such a manner that the outer edges of the tractor holes 612 in the cross-web direction XWD are pulled apart when the tractor holes 612 seat on the teeth 1416. For example, the teeth 1416 may have a larger cross section at the proximal end (proximal to the center of the merge sprocket 1414) and be tapered so that the cross section changes continuously and becomes smaller in the distal direction (i.e., distal to the center of the merge sprocket 1414). Thus, the tapering of the teeth 1416 applies sufficient cross-web tension to the web of electrode material from spools 1402, 1404 and 1406, eliminating web slack and curl in the cross-web direction XWD. In this embodiment, the vacuum orifice 1444 of the vacuum tensioner 1442 is positioned only near the merge point of the electrode material webs from spools 1402, 1404, and 1406 or the merge point to the teeth 1416 of the merge sprocket 1414, because beyond that point, the electrode material webs from spools 1402, 1404, and 1406 seat against the merge sprocket 1414 via the tension applied to the electrode material webs from spools 1402, 1404, and 1406 by the taper of the teeth 1416.

[0162] In one embodiment, the reverse-rotating brush 1440 is positioned downstream of the vacuum tensioner 1442 in the web direction WD. However, in other embodiments, the reverse-rotating brush is positioned at the same location as the vacuum tensioner 1442, or upstream of the vacuum tensioner 1442. In one embodiment, each transfer position 1426, 1426A-X includes the reverse-rotating brush 1440 and the vacuum tensioner. In another embodiment, only the transfer station that transfers the web of separator material includes the reverse-rotating brush 1440, but all transfer stations include the vacuum tensioner 1442.

[0163] Referring to Figure 19, in one embodiment, the alignment feature detection system 1900 is located downstream of the merge zone 1408. In this embodiment, the alignment of the layers of the merge material web is within 1 mm when measured from the center point of the layers in each of the web direction WD and cross-web direction XWD. The alignment feature detection system 1900 includes an optical sensor 1902 and a backlight 1904. The optical sensor may be a digital camera or other photosensitive device that can make the apparatus function as described herein. In this embodiment, the optical sensor 1902 is positioned to capture light from the backlight 1904 after such light has passed through the merge material web 1432, so that the silhouette of the merge material web 1432 is captured by the optical sensor 1902. The silhouette of the merge material web 1432 is analyzed by the optical sensor 1902 to precisely determine the location of the fiducial features 602. The position of the fiducial feature 602, positioned by the optical sensor 1902, is stored by the user interface 116 (Figure 1) and can be used to ensure that the merged material web 1432 is precisely positioned for subsequent processing. Therefore, precise positioning refers to, for example, the longitudinal axis A of each electrode pattern. E(Figure 7), this means that each layer of the merged material web is vertically aligned so that the tractor holes 612, fiducial features 602, and the edges of the electrode patterns of each layer (lengthwise edge cuts 600, perforations 608, 610) (Figure 6) are aligned in both the web direction and the cross-web direction XWD. In one embodiment, as will be further described below, the fiducial feature 602 is positioned by an optical sensor 1902, and the position of the receiving unit 2010 and alignment pins 2012 is used to control the position of the receiving unit 2010 and alignment pins 2012 so as to align with the fiducial feature 602. It is therefore important that the fiducial features of each layer are aligned. In one embodiment, the receiving unit 2010 is controlled to center the alignment pins within ±10 μm to 50 μm from the center of the fiducial feature 602 in the web direction WD. In another embodiment, the receiving unit 2010 is a controller that controls the center of the alignment pin 2012 to align with the fiducial feature 602 within ±10 μm to 50 μm in the cross-web direction XWD.

[0164] Referring to Figures 20 and 20A, in one embodiment, a high-capacity lamination system 2000 is used. In this embodiment, the merge zone 1408 is similar to that described above. However, in this embodiment, a toothed belt 2002 (shown by dashed lines) is utilized. In one embodiment, the toothed belt 2002 is made of stainless steel and includes a group of conveying teeth 2038 (Figure 20A) having a size, shape and position to engage with one or more tractor holes 612 or fiducial features 602 of the spools 1402, 1404 and 1406, and subsequently the merging material web 1432. The toothed belt 2002 is configured to operate in an endless configuration through the merge zone 1408 and the lamination / punching zone 2004. The toothed belt 2002 is conveyed using one or more synchronous sprockets 2006 that engage with the drive portion of the toothed belt 2002 to control its speed, which is synchronized with the process in the merge zone 1408 described above.

[0165] Referring further to Figure 20, the mass stacking system includes an automated jig loading assembly 2008 within the punching and stacking zone 1410. The automated jig loading assembly includes one or more receiving units 2010. In the embodiment shown in Figure 20, there are four receiving units 2010 aligned sequentially along the path of the toothed belt 2002. In one embodiment, each of the receiving units 2010 may be driven by the same actuator to produce simultaneous motion of all receiving units 2010, which may be a cam that drives the motion of the receiving unit 2010. In other embodiments, each of the receiving units 2010 may be controlled or driven independently.

[0166] Referring to Figures 21 and 22, each receiving unit 2010 comprises one or more alignment pins 2012 extending from a receiving base 2014. The alignment pins 2012 are configured to engage with one or more of the fiducial features 602 or tractor holes 612. Each receiving unit 2010 may be coupled to a two-axis motion control device, such as a servo or motor, which enables the receiving unit 2010 to move in the cross-web direction XWD and the down-web direction WD. In one embodiment, the motion control device is controlled based on the position of the fiducial feature 602 positioned by an optical sensor 1902. In this embodiment, the position of the fiducial feature 602 is used to control the motion control device to position the receiving unit 2010 so that its alignment pins 2012 are properly positioned to pass through the corresponding fiducial feature 602 of the merged material web 1432. The motion control device is controlled to properly position the receiving unit 2010 for each punching operation performed in the punching and lamination zone 1410, as will be further described below.

[0167] The punching and stacking operations will be further illustrated with reference to Figures 23 and 26A-C. In this embodiment, the merge material web 1432 is transported from the merge zone 1408 to the punching and stacking zone 1410. The merge material web 1432 passes under the punch head 2016 and over the receiving unit 2010 while being transported by a toothed belt 2002 which is carried by one or more synchronous sprockets 2006. In one embodiment, the punch head 2016 is controlled to move up and down in the Z direction (e.g., vertically) as indicated by the double-headed arrow. In one embodiment, the receiving unit 2010 is controlled to move up and down in the Z direction (e.g., vertically) as indicated by the double-headed arrow.

[0168] Referring to Figures 24A-C, in one embodiment, each receiving unit 2010 has a pair of alignment pins 2012 as described above, sized and spaced to correspond to the fiducial feature 602 of each electrode subunit 2018. In one embodiment, the alignment pins 2012 are configured to engage with only a portion of the inner circumference of the fiducial feature 602. For example, in one embodiment, the fiducial feature 602 has a substantially rectangular inner circumference, and the alignment pins 2012 are configured to contact only the outer edge 2400, down-web edge 2402, and up-web edge 2404 of the fiducial feature 602, but not the inner edge 2406 (Figure 24D). During a single punching operation, a single electrode subunit 2018 is punched out and loaded into the receiving unit 2010. In another embodiment, the alignment pin 2012 and the fiducial feature 602 are positioned to the corresponding size and location such that there is clearance between the alignment pin 2012 and all edges of the fiducial feature 602 (outer edge 2400, down web edge 2402, up web edge 2404, and inner edge 2406). In this embodiment, there may be a clearance of about 50 micrometers between the alignment pin 2012 and each of the outer edge 2400, down web edge 2402, up web edge 2404, and inner edge 2406.In other embodiments, the clearance between the alignment pin 2012 and each of the outer edge 2400, down web edge 2402, up web edge 2404, and inner edge 2406 is 0 micrometers, 50 micrometers, 100 micrometers, 150 micrometers, 200 micrometers, 250 micrometers, 300 micrometers, 350 micrometers, 400 micrometers, 450 micrometers, 500 micrometers, 550 micrometers, 600 micrometers, 650 micrometers, 700 micrometers, 750 micrometers, 800 micrometers, 850 micrometers, 900 micrometers, The clearances may be within the range of 0 to 2000 micrometers, such as 950 micrometers, 1000 micrometers, 1050 micrometers, 1100 micrometers, 1150 micrometers, 1200 micrometers, 1250 micrometers, 1300 micrometers, 1350 micrometers, 1400 micrometers, 1450 micrometers, 1500 micrometers, 1550 micrometers, 1600 micrometers, 1650 micrometers, 1700 micrometers, 1750 micrometers, 1800 micrometers, 1850 micrometers, 1900 micrometers, 1950 micrometers, and 2000 micrometers. In one embodiment, the clearances between the alignment pin 2012 and the down web edge 2402 and up web edge 2404 are in the range of 50 to 2000 micrometers, respectively. In yet another embodiment, the clearances between the alignment pin 2012 and each of the outer edge 2400, down web edge 2402, up web edge 2404, and inner edge 2406 may be the same or different in order to enable the system to function as described herein.

[0169] As shown in Figure 24E, the receiving unit 2010 may include a movable platform 2034 that moves in the Z direction and maintains a force in the Z direction toward the punch head 2016. The movable platform 2034 may also be referred to herein as an elevator. The movable platform 2034 is controlled to move in close proximity to the merge material web 1432 during the punching process to prevent uneven movement of the electrode subunit 2018 as the electrode subunit 2018 is separated from the merge material web 1432, as shown in 2018'. It should also be understood that any misalignment of the layers of the electrode subunit 2018 may cause further friction on the alignment pins 2012, resulting in uneven shifts of the electrode subunit, as shown in 2018', if, for example, the fiducial features 602 of each layer are not precisely aligned in the web direction WD and the cross-web direction XWD (e.g., causing a reduction in cross-sectional area). In one embodiment, the movable platform 2034 is controlled to contact the electrode subunit 2018 of the merged material web 1432 (e.g., zero clearance). In other embodiments, the movable platform 2034 is controlled to be within a range of 0 to 1000 micrometers of the merged material web 1432, for example, 0 micrometers, 50 micrometers, 100 micrometers, 150 micrometers, 200 micrometers, 250 micrometers, 300 micrometers, 350 micrometers, 400 micrometers, 450 micrometers, 500 micrometers, 550 micrometers, 600 micrometers, 650 micrometers, 700 micrometers, 750 micrometers, 800 micrometers, 850 micrometers, 900 micrometers, 950 micrometers, or 1000 micrometers. In one embodiment, the movable platform 2034 is mounted on a ball-bearing slide mechanism that allows movement in the Z direction. In one embodiment, the movable platform 2034 may be coupled to a gear drive mechanism driven by a stepping motor, which is actuated to move immediately before and / or immediately after each punching operation.

[0170] In some embodiments, the punch head 2016 is made of a metal or metal alloy such as stainless steel, aluminum, titanium, steel, other metals, and alloys thereof. In other embodiments, the punch head 2016 may be made of any material that can enable the system to function as described herein, such as plastic, carbon fiber, or wood. The punch head should have sufficient strength and rigidity so as not to deform when force is applied to the electrode subunit 2018. Referring to Figures 26A-C, in one embodiment, the punch head 2016 has a punch surface 2017 having a size and shape that substantially covers the entire surface of the electrode subunit 2018 facing the punch surface 2017. In one embodiment, the punch surface 2017 includes a fiducial bore 2019 that is the same size and shape as, or substantially the same as, the fiducial feature 602. Thus, the alignment pin 2012 can pass through the fiducial bore 2019 during the punching operation. In one embodiment, the punch head 2016 has a punch surface 2017 that is slightly smaller in size than the electrode subunit 2018 in the cross-web direction. For example, in one embodiment, the electrode subunit 2018 may have a portion 2023 that extends 0 to 100 micrometers beyond the distal end 2021 of the punch surface 2017 in the cross-web direction XWD, as shown, for example, in Figure 26C. In one embodiment, the punch surface 2017 may be slightly larger than the electrode subunit 2018 in the web direction WD, extending 0 to 100 micrometers beyond the longitudinal end 2025 to the longitudinal edge cut 600 in the web direction WD. In one embodiment, the punch surface 2017 does not have a sharp cutting edge for cutting the electrode subunit 2018, which may, in some cases, cause contamination of the layer of the electrode subunit 2018. Rather, the punch surface 2017 has a blunt edge and separates the electrode subunit 2018 from the web using a downward force to rupture the perforation, as described herein.

[0171] In one embodiment, the punch head 2016 applies a force in the Z direction to the electrode subunit 2018 and transmits that force to the movable platform 2034, which applies a counteracting force (for example, by controlling a stepping motor to generate a holding torque). In one embodiment, these counteracting forces cause a slight compression of the electrode subunit, which facilitates overcoming static friction between the alignment pin and the fiducial feature 602 of the electrode subunit 2018, thereby facilitating the maintenance of parallelism of the electrode subunit 2018 to an ideal plane perpendicular to the alignment pin 2012. In one embodiment, the force applied to the movable platform 2034 by the punch head 2016 causes the movable platform 2034 to move in the Z direction by a distance equal to the height of the electrode subunit 2018, and thus rupture the weakened region along the path formed by the longitudinal edge cut 600 and perforation 608, and thus prepare to receive the next electrode subunit 2018. In another embodiment, the movable platform 2034 may be controlled, for example by using a stepping motor, to move away from the punch head 2016 in the Z direction by a predetermined distance equal to the Z-direction dimension of the electrode subunit 2018 after each electrode subunit 2018 has been punched by the punch head 2016. In this way, the movable platform 2034 facilitates maintaining the electrode subunits perpendicular to the alignment pins 2012 during the punching operation.

[0172] As shown in Figure 24C, for example, the merge material web 1432 may then advance to position additional electrode subunits 2018 to be punched out and stacked, and this process may continue until a predetermined number of electrode subunits 2018 are loaded into the receiving unit 2010. In the embodiment shown in Figure 24C, there are three stacked electrode subunits 2018, but it should be understood that any number of electrode subunits can be stacked into the receiving unit 2010. In the embodiment, the number of electrode subunits 2018 to be stacked may be in the range of 1 to 300. In this embodiment, each electrode subunit consists of four layers, but it may consist of any number of layers according to the present disclosure.

[0173] In one embodiment, before initiating the punching operation, the system 2000 verifies that the electrode subunits 2018 are free of defects (as determined by the electrode defect sensor 1434), and if a defect is detected, the system is controlled to avoid punching and laminating the defective electrode subunit 2018. In one embodiment, if multiple receiving units 2010 and corresponding punch heads 2016 are used, if a defect is detected in one of the electrode subunits 2018, all of the receiving units 2010 and corresponding punch heads 2016 are controlled to skip the punching and lamination operation, and the merge material web 1432 is transported forward to a position where all of the receiving units 2010 and corresponding punch heads 2016 are aligned below the defect-free electrode subunits 2018.

[0174] In one embodiment, to separate each of the electrode subunits 2018 from the merge material web 1432, the punch head 2016 is moved in the Z direction toward the merge material web 1432, for example, within a range of about 0.15 mm to about 0.50 mm from the surface of the merge material web. The alignment pin 2012 of the receiving fixture is controlled to move in the Z direction toward the opposing surface of the merge material web 1432. The alignment of the alignment pin 2012 and the punch head 2016 can be verified using an optical sensor 1902. If it is determined that the alignment pin 2012 is not properly aligned with the punch head 2016, one or more of the punch head 2016, receiving unit 2010, or merge material web 1432 may be moved in the web direction WD until satisfactory alignment is achieved. In such embodiments, one or more of the receiving unit 2010 and the punch head 2016 may be configured to translate in the web direction via an electric carriage assembly (not shown). Once satisfactory alignment of the alignment pin 2012 and the punch head 2016 is achieved, the receiving unit is moved in the Z direction so that the alignment pin 2012 moves through the fiducial feature 602 to the corresponding punch head hole 2020 of the punch head 2016. In one embodiment, the alignment pin 2012 enters the punch head hole 2020 at least 2 mm. In one embodiment, the punch head hole 2020 is sized and shaped to closely match the outer diameter of the alignment pin 2012 to minimize any misalignment or displacement during punching and lamination operations.

[0175] Next, the punch head 2016 is controlled to move in the Z direction toward the receiving unit 2010, for example, past the opposing surface of the merge material web 1432 by at least 5 mm. As the punch head 2016 moves, the electrode subunit 2018 is separated from the merge material web 1432 along a weakening region that forms the outer periphery of the electrode subunit 2018. For example, the weakening region can constitute a path along the longitudinal edge cuts 600 and perforations 608 (Figure 6) of the electrode pattern in each layer. In such embodiments, the perforations 608 rupture, releasing the electrode subunit 2018 from the merge material web 1432. The web downstream of such punched electrode subunit 2018 is called the used web 2022. In one embodiment, the layers of the merge material web 1432 are arranged so that the web of anode material from the spool 1404 is on top (i.e., in contact with the punch head 2016). In another embodiment, the layer of merge material web 1432 is positioned such that the cathode material web from spool 1402 is on top (i.e., in contact with the punch head 2016). In yet another embodiment, the layer of merge material web 1432 is positioned such that the separator material web from spool 1406 is on top (i.e., in contact with the punch head 2016). In some embodiments, it is preferable that either the anode material web from spool 1404 or the cathode material web from spool 1402 has a greater mass than the separator material web from spool 1406 and is therefore in contact with the punch head 2016. Thus, in such embodiments, the anode material web from spool 1404 and the cathode material web from spool 1402 are less likely to be pulled back in the Z direction away from the merge material web 1432 when the punch head 2016 retracts after the punching operation. For example, in embodiments where the web of separator material from spool 1406 has low mass, under certain conditions, it may be pulled together with the punch head 2016 as the punch head 2016 retracts due to the vacuum effect.In such embodiments, therefore, in order to avoid such effects, it is desirable that the merge material web 1432 has an uppermost layer that is either an anode material web from spool 1404 or a cathode material web from spool 1402.

[0176] After the electrode subunit is separated from the merged material web 1432, the punch head 2016 moves in the Z direction away from the receiving unit 2010, and the receiving unit moves in the Z direction away from the punch head 2016. In one embodiment, both the punch head 2016 and the receiving unit 2010 move simultaneously. In other embodiments, the punch head 2016 and the receiving unit 2010 are controlled to move sequentially. In one embodiment, the punch head 2016 and the receiving unit 2010 are moved approximately 0.5 mm away from their respective surfaces in the Z direction.

[0177] Although Figure 23 illustrates only a single punch head 2016 and receiving unit 2010, it should be understood that in other embodiments, a group of corresponding punch heads 2016 and receiving units 2010 may be used simultaneously to increase the number of electrode subunits separated from the merge material web 1432 during a unit of time. For example, in one embodiment as shown in Figure 20, a series of four punch heads 2016 and receiving units 2010 are used. In yet another embodiment, there may be 1 to 100 punch heads 2016 and receiving units 2010 each operating simultaneously. Furthermore, it should be noted that in some embodiments, the punching and stacking operations described above are performed intermittently (i.e., while the merge material web is stopped). However, in other embodiments, the system may be configured so that the punching and stacking operations are performed continuously, in which case the merge material web remains in motion in the web direction WD during the punching and stacking operations.

[0178] After the electrode subunits are separated from the merge material web 1432, the web remaining downstream is called the spent web 2022 and is transported in the web direction WD using a demerging sprocket 2024 (Figure 25) that engages with the tractor holes 612 of the spent web 2022. For example, as shown in Figure 25, the spent web 2022 includes portions of the web having tractor holes 612 and tie bars 614. The spent web may also include unpunched electrode subunits 2027 that were not punched out due to misalignment or other defects in one or more of the unpunched electrode subunits 2027. In one embodiment, the spent web 2022 is wound onto a spent web winding roller 2026. Thus, the spent web 2022 is cleanly removed from the toothed belt 2002, which facilitates the toothed belt 2002 to advance in the web direction WD in a continuous loop manner to receive the merge material web 1432 to be processed.

[0179] In one embodiment, the high-capacity stacking system 2000 includes one or more cross-web belt tensioners 2028. The cross-web belt tensioners 2028 are configured to engage with a secondary set of teeth 2032 (Figure 20A) of the toothed belt 2002. The secondary set of teeth 2032 is located on the opposite side of the toothed belt 2002 from the position where the sprocket 2006 engages with the toothed belt 2002. The cross-web belt tensioners 2028 function to provide tension to the merge material web 1432 in the cross-web direction to facilitate the alignment and positioning of the fiducial feature 602. In one embodiment, the cross-web belt tensioners 2028 include a set of reversed teeth that engage with the secondary set of teeth 2032. The cross-web belt tensioners may be mounted on a servo, motor, or other motion control device to move the cross-web belt tensioners 2028 in the cross-web direction XWD. As the cross-web belt tensioner 2028 is moved outward (away from the center of the web) in the cross-web direction XWD, the cross-web tension on the merge material web 1432 increases. Similarly, as the cross-web belt tensioner 2028 is moved inward (towards the center of the web) in the cross-web direction, a decrease in cross-web tension acts on the merge material web 1432. Each of the cross-web belt tensioners 2028 can be individually controlled to apply different amounts of cross-web tension to the merge material web 1432 at different points along the movement path of the merge material web 1432. Thus, the cross-web belt tensioners 2028 function to promote the flattening of the merge material web 1432 (e.g., de-wrinkling, de-curling, de-sagging, etc.). In some embodiments, the cross-web belt tension provided by the cross-web belt tensioner 2028 is in the range of 0 to 50 percent of the breaking strength of the outer perforation 608. In one embodiment, the cross-web belt tensioner 2028 is useful in preventing displacement of the fiducial feature 602 due to deformation caused by sagging, wrinkling, or curvature by flattening the merged material web 1432.

[0180] In some embodiments, when sufficient downweb tension is applied to the merge material web 1432 by the synchronous sprocket 2006, the merge material web 1432 may stretch in the downweb direction, causing the fiducial features 602 to be further spaced apart than intended in the downweb direction. In such embodiments, the toothed belt 2002 is controlled to decrease its speed, thereby reducing the downweb tension on the merge material web 1432 in the web direction WD accordingly, or the toothed belt 2002 is controlled to increase its speed, thereby increasing the tension on the merge material web 1432 in the web direction WD accordingly.

[0181] During the punching operation, the electrode subunit 2018 is configured to separate from the merge material web 1432 in a predetermined manner defined by the strength of the outer perforation 608 and the inner perforation 610 (Figure 15A). In one embodiment, the outer perforation has a lower breaking strength (i.e., is more prone to breaking) than the inner perforation 610. In this embodiment, the electrode subunit 2018 separates from the merge material web along a path defined by the outer perforation 608 and the longitudinal edge cut 600.

[0182] In one embodiment, a predetermined number of electrode subunits 2018 are stacked on a receiving unit 2010 to form a multi-unit electrode stack 2030 (Figure 24C). It should be understood that each of the stacked electrode subunits 2018 is aligned such that its respective fiducial feature 602, longitudinal edge cut 600, and perforations 608, 610 are aligned in the web direction WD and the cross-web direction XWD. The multi-unit electrode stack 2030 is then placed within a pressurizing restraint 1602 having pressure plates 1604, 1606 that apply pressure to the multi-unit electrode stack 2030 in the direction indicated by the pressure arrow P. The pressure applied to the multi-unit electrode stack 2030 may be adjustable using a user interface 116 to control the pressure P applied to the multi-unit electrode stack 2030 by the pressure plates 1604, 1606. Once sufficient pressure P is applied to the multi-unit electrode stack 2030, the alignment pin 1600 can be moved in the removal direction R, which causes the second perforation 610 to rupture along its length so that the ablation 404 (e.g., electrode tab 520) becomes the outer edge of the multi-unit electrode stack 2030, as shown in Figure 16C.

[0183] After the perforation 610 bursts, the multi-unit electrode stack 2030 proceeds to the tab welding station, where busbars 1700 and 1702 are welded to the ablation 404 to form a laminated cell 1704. Prior to welding, the busbars 1700 and 1702 are positioned through the busbar openings 1608 of their respective electrodes. In one embodiment, once the busbars 1700 and 1702 are positioned through the busbar openings 1608, the ablation 404 is folded toward the busbars 1700 and 1702, respectively, prior to welding. In this embodiment, busbar 1700 is a copper busbar welded to the ablation 404 (anode tab) of the anode current collector layer 506, and busbar 1702 is an aluminum busbar welded to the ablation 404 (cathode tab) of the cathode conductor 510. However, in other embodiments, the busbars 1700 and 1702 may be made of any suitable conductive material to enable the battery 1804 to function as described herein. Welding can be performed using a laser welding machine, friction welding, ultrasonic welding, or any suitable welding method for welding the busbars 1700 and 1702 to the electrode tabs 520. In one embodiment, each of the busbars 1700 and 1702 is in electrical contact with all of the electrode tabs 520 for the anode and cathode, respectively.

[0184] Once the laminated cell 1704 is formed, it proceeds to the packaging station 1800. At the packaging station 1800, the laminated cell 1704 is covered with an insulating packaging material such as a multilayer aluminum polymer material or plastic to form a battery package 1802. In one embodiment, the battery package 1802 is evacuated using a vacuum and filled with an electrolyte material through an opening (not shown). The insulating packaging material may be sealed around the laminated cell 1704 using heat sealing, laser welding, adhesive, or any suitable sealing method. The busbars 1700 and 1702 are left exposed and not covered by the battery package 1802 so that a user can connect the busbars to a powered device or a battery charger. Once the battery package 1802 is placed on the laminated cell 1704, the finished battery 1804 is defined. In this embodiment, the finished battery is a three-dimensional lithium-ion battery. In other embodiments, the finished battery may be any battery type suitable for manufacture using the apparatus and methods described herein.

[0185] In one embodiment, each member of the anode group has a bottom, a top, and a longitudinal axis A E (Figure 7) It has a longitudinal axis A. E It extends from its bottom to its top in the cross-web direction XWD. In an alternative embodiment, the longitudinal axis A E It extends down the web direction WD from its bottom to its top. In one embodiment, the members of the anode group are formed from the web 104 of the substrate, which is the anode material 502. Furthermore, each member of the anode group is aligned with the longitudinal axis (A) of the electrode. E Length (L) measured along ) E (Figure 6A) and the width (W) measured in the direction in which the alternating sequence of the negative electrode structure and the positive electrode structure progresses (i.e., the web direction WD). E ) and length (L E ) and width (W E The height (H) measured in the direction perpendicular to each of the measurement directions ("Z direction") E)(having (FIG. 6A)). Each member of the anode population also has a perimeter (P E ) corresponding to the sum of the side lengths of the projection of the electrode in a plane perpendicular to its longitudinal axis.

[0186] The length (L E ) of the members of the anode population varies depending on the energy storage device and its intended use. However, generally, the members of the anode population typically have a length (L E ) in the range of about 5 mm to about 500 mm. For example, in one such embodiment, the members of the anode population have a length (L E ) of about 10 mm to about 250 mm. As a further example, in one such embodiment, the members of the anode population have a length (L E ) of about 25 mm to about 100 mm.

[0187] The width (W E ) of the members of the anode population also varies depending on the energy storage device and its intended use. However, generally, each member of the anode population typically has a width (W E ) within the range of about 0.01 mm to about 2.5 mm. For example, in one embodiment, the width (W E ) of each member of the anode population is within the range of about 0.025 mm to about 2 mm. As a further example, in one embodiment, the width (W E ) of each member of the anode population is within the range of about 0.05 mm to about 1 mm.

[0188] The height (H E ) of the members of the anode population also varies depending on the energy storage device and its intended use. However, generally, the members of the anode population typically have a height (H E ) within the range of about 0.05 mm to about 10 mm. For example, in one embodiment, the height (H E ) of each member of the anode population is within the range of about 0.05 mm to about 5 mm. As a further example, in one embodiment, the height (H E) is in the range of about 0.1 mm to about 1 mm. According to one embodiment, the members of the anode population include one or more first electrode members having a first height and one or more second electrode members having a second height other than the first height. In yet another embodiment, the different heights for the one or more first electrode members and the one or more second electrode members are selected to correspond to a predetermined shape for the electrode assembly (e.g., the multi-layer electrode sub-stack 1500 (FIG. 15)), such as an electrode assembly shape having different heights along one or more of the vertical axis and / or the horizontal axis, and / or to provide a predetermined performance characteristic for the secondary battery.

[0189] Generally, the members of the anode population have a length (L E ) that is substantially greater than each of its width (W E ) and its height (H E ). For example, in one embodiment, for each member of the anode population, the ratio of L E to W E and the ratio of L E to H E are each at least 5:1 (i.e., the ratio of L E to W E is each at least 5:1, and the ratio of L E to H E are each at least 5:1). As a further example, in one embodiment, the ratio of L E to each of W E and H E is at least 10:1. As a further example, in one embodiment, the ratio of L E to each of W E and H E is at least 15:1. As a further example, in one embodiment, for each member of the anode population, the ratio of L E to each of W E and H

[0190] In one embodiment, the height (H E ) and width (WE ) The ratio of each is at least 0.4:1. For example, in one embodiment, for each member of the anode population, H E to W E The ratio of each is at least 2:1. As a further example, in one embodiment, H E to W E The ratio of each is at least 10:1. As a further example, in one embodiment, H E to W E The ratio of each is at least 20:1. However, typically, the ratio of H E to W E will generally be less than 1,000:1 for each. For example, in one embodiment, the ratio of H E to W E is less than 500:1 for each. As a further example, in one embodiment, the ratio of H E to W E is less than 100:1 for each. As a further example, in one embodiment, the ratio of H E to W E is less than 10:1 for each. As a further example, in one embodiment, the ratio of H E to W E is in the range of about 2:1 to about 100:1 for each member of the anode population.

[0191] In one embodiment, the members of the cathode population are formed from a web 104 of a substrate that is the cathode material 504. Referring now to FIG. 6B, each member of the cathode population has a longitudinal axis (A CE ) that extends generally perpendicular to the direction in which the alternating sequence of the negative electrode structure and the positive electrode structure progresses, in a direction from the bottom to the top in the bottom, top, and cross-web direction XWD. Further, each member of the cathode population has a length (L CE ) measured along a longitudinal axis (A CE ) that is parallel to the cross-web direction XWD, a width (W CE ) measured in the down-web direction WD in which the alternating sequence of the negative electrode structure and the positive electrode structure progresses, and a length (L CE ) and a width (W CEThe height (H) measured in a direction perpendicular to each of the measurement directions of ) CE ) has.

[0192] Length of members in the cathode group (L CE ) varies depending on the energy storage device and its intended use. However, generally, each member of the cathode group typically has a length (L) ranging from about 5 mm to about 500 mm. CE ) has. For example, in one such embodiment, each member of the cathode group has a length (L) of about 10 mm to about 250 mm. CE ) has. As a further example, in one such embodiment, each member of the cathode group has a length (L) of about 25 mm to about 100 mm. CE ) has.

[0193] Width of the cathode group member (W CE ) also varies depending on the energy storage device and its intended application. However, generally, the members of the cathode group typically have a width (W) in the range of about 0.01 mm to about 2.5 mm. CE ) has. For example, in one embodiment, the width (W) of each member of the cathode group is CE The width (W) of each member of the cathode group is in the range of approximately 0.025 mm to approximately 2 mm. As a further example, in one embodiment, the width (W) of each member of the cathode group is CE ) is within the range of approximately 0.05 mm to approximately 1 mm.

[0194] Height of the cathode group members (H CE ) also varies depending on the energy storage device and its intended application. However, generally, the height (H) of the cathode group members is typically in the range of about 0.05 mm to about 10 mm. CE ) has. For example, in one embodiment, the height (H) of each member of the cathode group is CE The height (H) of each member of the cathode group is in the range of approximately 0.05 mm to approximately 5 mm. As a further example, in one embodiment, the height (H) of each member of the cathode group is CEThe height is in the range of about 0.1 mm to about 1 mm. According to one embodiment, the members of the cathode group include one or more first cathode members having a first height and one or more second cathode members having a second height other than the first height. In yet another embodiment, the different heights for one or more first cathode members and one or more second cathode members may be selected to correspond to a predetermined shape for an electrode assembly, such as an electrode assembly shape having different heights along one or more of the longitudinal and / or transverse axes, and / or to provide predetermined performance characteristics for a secondary battery.

[0195] Generally, each member of the cathode group has a width (W CE It is substantially larger than ) and has a height (H CE (L) is effectively larger than CE ) has. For example, in one embodiment, each member of the cathode group has W CE and H CE L for each of CE The ratios of each are at least 5:1 (i.e., W CE L CE The ratios of each are at least 5:1, and H CE L CE The ratios of each are at least 5:1). As a further example, in one embodiment, for each member of the cathode group, W CE and H CE L for each of CE The ratio is at least 10:1. As a further example, in one embodiment, W CE and H CE L for each of CE The ratio is at least 15:1 for each member of the cathode group. As a further example, in one embodiment, WCE and H CE L for each of CE The ratio is at least 20:1 for each member of the cathode group.

[0196] In one embodiment, the width (W) of the members of the cathode group CEHeight (H) CE The ratios of ) are at least 0.4:1, respectively. For example, in one embodiment, H CE vs W CE The ratio is at least 2:1 for each member of the cathode group. As a further example, in one embodiment, H CE vs W CE The ratio is at least 10:1 for each member of the cathode group. As a further example, in one embodiment, H CE vs W CE The ratio is at least 20:1 for each member of the cathode group. However, typically, H CE vs W CE The ratio is generally less than 1,000:1 for each member of the anode group. For example, in one embodiment, H CE vs W CE The ratio is less than 500:1 for each member of the cathode group. As a further example, in one embodiment, H CE vs W CE The ratios of each are less than 100:1. As a further example, in one embodiment, H CE vs W CE The ratios of each are less than 10:1. As a further example, in one embodiment, H CE vs W CE The ratios for each member of the cathode group range from approximately 2:1 to approximately 100:1.

[0197] In one embodiment, the anode current collector 506 also has an electrical conductance substantially greater than that of the negative electrode active material layer. For example, in one embodiment, the ratio of the electrical conductance of the anode current collector 506 to the electrical conductance of the negative electrode active material layer is at least 100:1 when there is an applied current to store energy in the device or an applied load to discharge the device. As a further example, in some embodiments, the ratio of the electrical conductance of the anode current collector 506 to the electrical conductance of the negative electrode active material layer is at least 500:1 when there is an applied current to store energy in the device or an applied load to discharge the device. As a further example, in some embodiments, the ratio of the electrical conductance of the anode current collector 506 to the electrical conductance of the negative electrode active material layer is at least 1000:1 when there is an applied current to store energy in the device or an applied load to discharge the device. As a further example, in some embodiments, the ratio of the electrical conductance of the anode current collector 506 to the electrical conductance of the negative electrode active material layer is at least 5000:1 when there is an applied current to store energy in the device or an applied load to discharge the device. As a further example, in some embodiments, the ratio of the electrical conductance of the anode current collector 506 to the electrical conductance of the negative electrode active material layer is at least 10000:1 when there is an applied current to store energy in the device or an applied load to discharge the device.

[0198] Generally, the cathode current collector 510 may be composed of a metal such as aluminum, carbon, chromium, gold, nickel, NiP, palladium, platinum, rhodium, ruthenium, an alloy of silicon and nickel, titanium, or a combination thereof (see "Current collectors for positive electrodes of lithium-based batteries" by AH Whitehead and M. Schreiber, Journal of the Electrochemical Society, 152(11)A2105-A2113 (2005)). As a further example, in one embodiment, the cathode current collector 510 is composed of gold or an alloy thereof such as gold silicide. As a further example, in one embodiment, the cathode current collector 510 is composed of nickel or an alloy thereof such as nickel silicide.

[0199] The following embodiments are provided to illustrate aspects of the present disclosure, but the embodiments are not intended to be limiting, and other embodiments and / or forms may also be provided.

[0200] Embodiment 1. In a process of merging webs to manufacture an electrode assembly for a secondary battery, A step of moving a web of a first substrate along a first web merge path, wherein the web of the first substrate includes (i) a group of first components for an electrode subunit, the first components being a group of first components defined by a corresponding weakening pattern, and (ii) a group of first transport features. A step of moving a web of a second substrate along a second web merge path, wherein the web of the second substrate includes (iii) a group of second components for an electrode subunit, the second components being defined by a corresponding weakening pattern, and (iv) a group of second transport features; A process of transporting a receiving member in the web merging direction adjacent to a first web merging path and a second web merging path, wherein the receiving member comprises a plurality of protrusions configured to engage with a first transport feature of the web of the first substrate and a second transport feature of the web of the second substrate. The process includes receiving the web of the first substrate on a receiving member at a first web merge position such that the conveying feature of the web of the first substrate is engaged by at least some of the multiple protrusions on the belt, A step of overlapping the web of the second substrate on the web of the first substrate on a receiving member at a second web merge position such that the first component is substantially aligned with the second component and the conveying features of the web of the second substrate are engaged by at least some of the multiple protrusions on the belt, wherein the second web merge position is spaced apart from the first web merge position in the down-web direction; Including the process.

[0201] Embodiment 2. The process of Embodiment 1, wherein the web of the first substrate consists of a web of electrode material, and the web of the second substrate consists of a web of separator material.

[0202] Embodiment 3. The process of Embodiment 1, wherein the web of the first substrate is made of a separator material web, and the web of the second substrate is made of an electrode material web.

[0203] Embodiment 4. In a process of merging webs to manufacture an electrode assembly for a secondary battery, A step of moving a web of a first substrate along a first web merge path, wherein the web of the first substrate includes (i) a group of first electrode components for an electrode subunit, the first electrode components being a group of first electrode components defined by a corresponding weakening pattern, and (ii) a group of first transport features, and the web of the first substrate includes a web of electrode material. A step of moving a web of a second substrate along a second web merge path, wherein the web of the second substrate includes (iii) a group of separator components defined by a corresponding weakening pattern, and (iv) a group of second transport features, and the web of the second substrate includes a web of separator material. A process of transporting a receiving member in the web merging direction adjacent to a first web merging path and a second web merging path, wherein the receiving member comprises a plurality of protrusions configured to engage with a first transport feature of the web of the electrode material and a second transport feature of the web of the separator material. A step of receiving one of the electrode material web and the separator material web on a belt at a first web merge position such that the respective transport features of the electrode material web and the separator material web are engaged by at least some of the multiple protrusions on the belt, A step of overlapping the web of the electrode material and the other web of the separator material at a second web merge position, such that the respective transport features of the web of the electrode material and the other web of the separator material are engaged by at least a portion of a plurality of protrusions on the belt, and the separator structure is substantially aligned with the first electrode structure, wherein the second web merge position is spaced down the web from the first web merge position. Including the process.

[0204] Embodiment 5. The process according to Embodiment 4, wherein the web of the electrode material is received at a first web position and the web of the separator material is received at a second web position.

[0205] Embodiment 6. The process according to Embodiment 4, wherein a web of separator material is received at a first web position and a web of electrode material is received at a second web position.

[0206] Embodiment 7. The process according to any one of the preceding embodiments, wherein the first web merge path consists of a first catenary curve and the second merge path consists of a second catenary curve.

[0207] Embodiment 8. The process according to embodiment 7, further comprising the step of analyzing the first catenary curve and the step of adjusting the speed of the web of the first substrate traveling along the first web merge path based on the analysis of the first catenary curve so that the first conveying feature aligns with adjacent ones of the plurality of protrusions on the receiving member.

[0208] Embodiment 9. The process according to embodiment 8, further comprising the step of analyzing the second catenary curve and the step of adjusting the speed of the web of the second substrate traveling along the second web merge path based on the analysis of the second catenary curve so that the second conveying feature aligns with adjacent ones of the plurality of protrusions on the receiving member.

[0209] Embodiment 10. The process according to any one of the preceding embodiments, including conveying the web of the first substrate or the web of the second substrate on a merge sprocket having teeth that align with the respective first conveying feature or the second conveying feature of the web of the first substrate and the web of the second substrate, respectively.

[0210] Embodiment 11. The process according to any one of the preceding embodiments, wherein moving at least one of the web of the first substrate and the web of the second substrate along the respective first web merge path and the second web merge path includes conveying the web of the first substrate and / or the web of the second substrate between a merge sprocket and a reverse tooth sprocket.

[0211] Embodiment 12. The process according to embodiment 11, wherein the teeth of the merge sprocket pass through the respective first or second conveying feature of the web of the first substrate and / or the web of the second substrate and enter the corresponding recesses of the reverse tooth sprocket.

[0212] Embodiment 13. The process according to any of the prior embodiments, further comprising merging at least one of the webs of the first substrate and the web of the second substrate at the point where the projection of the receiving member engages with the reverse-tooth sprocket.

[0213] Embodiment 14. The process according to any of the preceding embodiments, further comprising the step of using a rotating brush to increase the flatness of at least one of the webs of a first substrate and a web of a second substrate, in the vicinity of the first contact point of each web with the merge sprocket.

[0214] Embodiment 15. The process according to Embodiment 14, further comprising the step of using a counter-rotating brush that rotates in the opposite direction to the rotating brush, wherein the counter-rotating brush is positioned across the web from the rotating brush.

[0215] Embodiment 16. The process according to any of the preceding embodiments, further comprising the step of using a vacuum device to increase the flatness of at least one of the webs of a first substrate and a web of a second substrate near the first contact point of each web with the merge sprocket.

[0216] Embodiment 17. The process according to Embodiment 16, wherein the vacuum apparatus comprises a base having a plurality of vacuum holes for drawing in air.

[0217] Embodiment 18. The process according to any of the prior embodiments, further comprising the step of reducing the web-direction tension of at least one of the web-directions of the web of the first substrate or the web of the second substrate at the first point of contact of the web of the web of the first substrate or the web of the second substrate with the merge sprocket by controlling the unwinding speed of the web of the web of the web of the web of the web of the web of the web of the web of the web of the first substrate or

[0218] Embodiment 19. The process according to any of the preceding embodiments, further comprising the step of using a deionizer to reduce the electrostatic charge on at least one of the first substrate webs or the second substrate webs near the first contact point of the first substrate webs or the second substrate webs with respect to the merge sprocket.

[0219] Embodiment 20. The process according to Embodiment 17, wherein the deionizer is positioned in front of at least one of the rotating brush and the vacuum tensioner in the web direction.

[0220] Embodiment 21. The process according to any of the preceding embodiments, further comprising the step of controlling the initial contact point between the web of the first substrate and the web of the second substrate and the merge sprocket to be within 0 to 90 degrees from the vertical.

[0221] Embodiment 22. The process according to any of the prior embodiments, further comprising the step of applying tension in the cross-web direction to at least one of the webs of a first substrate and a second substrate using a cross-web belt tensioner.

[0222] Embodiment 23. The process according to any of the preceding embodiments, wherein the teeth of the merge sprocket are tapered such that the base of the teeth has a larger cross-sectional area than the distal portion of the projection.

[0223] Embodiment 24. The process according to any of the preceding embodiments, wherein the projection of the receiving member is tapered such that the base of the projection has a larger cross-sectional area than the distal portion of the projection.

[0224] Embodiment 25. The process according to any of the prior embodiments, further comprising the step of controlling the web transverse tension of the receiving member such that the projection of the receiving member contacts only a portion of the conveying features of at least one of the webs of the first substrate and the web of the second substrate.

[0225] Embodiment 26. The process according to any of the prior embodiments, wherein the step of detecting a defect using a sensor further includes the step of detecting a defect in at least one of the webs of a first substrate and a web of a second substrate.

[0226] Embodiment 27. The process according to Embodiment 26, wherein the step of detecting defects using a sensor is performed before merging at least one of the webs of the first substrate and the web of the second substrate onto the receiving member.

[0227] Embodiment 28. The process according to Embodiment 26 or 27, further comprising the step of marking the detected defect on at least one of the webs of the first substrate or the webs of the second substrate.

[0228] Embodiment 29. The process according to any of the preceding embodiments, further comprising the step of controlling the web-direction tension of at least one of the webs of the first substrate and the web of the second substrate to be different at the point of initial contact with the merge sprocket and at the point of transfer to the receiving member.

[0229] Embodiment 30. The process according to any of the preceding embodiments, further comprising the step of positioning a reversing tooth roller perpendicular to the belt at a distance sufficient to allow slack in at least one of the webs of the first and / or the second substrate, in order to align the web of the first substrate and / or the web of the second substrate with the belt.

[0230] Embodiment 31. The process according to any of the preceding embodiments, further comprising the step of positioning a subsequent reversing tooth sprocket such that the nip distance between the reversing tooth sprocket and the receiving member is greater than the nip distance between the preceding reversing tooth sprocket and the receiving member.

[0231] Embodiment 32. The process according to any of the preceding embodiments, wherein the teeth of the merge sprocket are configured to allow at least one of the webs of the first substrate and the web of the second substrate to be positioned above the base of the teeth.

[0232] Embodiment 33. The process according to any of the preceding embodiments, further comprising: (a) moving a web of a third substrate along a third web merge path, wherein the web of the third substrate includes (i) a group of third components for an electrode subunit, defined by a corresponding weakening pattern, and (ii) a group of third transport features; and (b) superimposing the web of the third substrate onto the web of the second substrate at a third web merge position such that the transport features of the web of the third substrate are engaged by at least a portion of a plurality of projections on a receiving member, and the third components are substantially aligned with the second components, wherein the third web merge position is spaced down the web from the first and second web merge positions.

[0233] Embodiment 34. The process of Embodiment 33, wherein the web of the third substrate is made of a web of the counter electrode material, and the web of the second substrate is made of a web of the separator material.

[0234] Embodiment 35. The process of Embodiment 33, wherein the web of the third substrate is made of a separator material web and the web of the second substrate is made of an electrode material web.

[0235] Embodiment 36. The process according to Embodiment 33, 34, or 35, further comprising: moving the web of a fourth substrate along a fourth web merge path, wherein the web of the fourth substrate is a group of fourth components for an electrode subunit, the fourth components including a group of fourth components and a group of fourth transport features, defined by a corresponding weakening pattern; and superimposing the web of the fourth substrate onto the web of the third substrate at a fourth web merge position such that the transport features of the web of the fourth substrate are engaged by at least a portion of a plurality of projections on a receiving member and the fourth components are substantially aligned with the third components, the fourth web merge position being spaced down the web from the first web merge position, the second web merge position, and the third merge position.

[0236] Embodiment 37. The process of Embodiment 36, wherein the web of the fourth substrate is made of a web of counter electrode material, and the web of the third substrate is made of a web of separator material.

[0237] Embodiment 38. The process of Embodiment 36, wherein the web of the fourth substrate is made of a separator material web and the web of the third substrate is made of a counter electrode material web.

[0238] Embodiment 39. The process according to any of the preceding embodiments, wherein the receiving member consists of a continuous belt.

[0239] Embodiment 40. The process according to any of the preceding embodiments, wherein the receiving member consists of a plurality of pin plates.

[0240] Embodiment 41. The process according to any of the preceding embodiments, further comprising the step of rotating the merge sprocket in the opposite direction to the reverse-tooth sprocket.

[0241] Embodiment 42. The process according to any of the preceding embodiments, further comprising the step of analyzing either the first or second catenary curve using an optical sensor.

[0242] Embodiment 43. The process according to any of the preceding embodiments, further comprising increasing the web-direction tension on either the web of the first substrate or the web of the second substrate when the slack in the catenary curve is outside a predetermined threshold.

[0243] Embodiment 44. The process according to any of the preceding embodiments, wherein the unwinding speeds of the web of the first substrate and the web of the second substrate are key-set to the speed of the receiving member.

[0244] Embodiment 45. The process according to any of the preceding embodiments, wherein each of the first or second catenary curves facilitates the self-alignment of the transport features of the web of the first or second substrate and the teeth of the merge sprocket.

[0245] Embodiment 46. A process for separating electrode subunits from a group of electrode subunits arranged in a layered web, wherein each electrode subunit is defined within the layered web by a corresponding weakening pattern, in a process, The process is A step of positioning the layered electrode subunits of a laminated web at the punch position between a receiving unit and a punch head, wherein the receiving unit includes a base, alignment pins, and a movable platform, A process of positioning the alignment pins of the receiving unit through the fiducial features of the electrode subunit, A step of positioning the movable platform at a predetermined position between the lower surface of the electrode subunit and the base of the receiving unit, A step of applying force to an electrode subunit using a punch head, wherein the force is large enough to separate the electrode subunit from the array of the laminated web along a weakening pattern. A process that includes this.

[0246] Embodiment 47. The process of Embodiment 46, further comprising the step of receiving the separated electrode subunits onto a movable platform.

[0247] Embodiment 48. The process of Embodiment 46, further comprising the step of maintaining the receiving unit in a stationary position while a force is applied to the electrode subunit.

[0248] Embodiment 49. The processes of embodiments 46-48, further comprising the step of maintaining the punch head in a stationary position while positioning the alignment pins of the receiving unit through the fiducial features of the electrode subunit.

[0249] Embodiment 50. The process of embodiments 46-49, further comprising the step of maintaining the punch head in a stationary position while moving the alignment pins to corresponding punch head holes formed in the punch head.

[0250] Embodiment 51. The process of Embodiments 46-50, wherein separating an electrode subunit from the layered arrangement of the laminated web includes rupturing a first perforation defining a first outer edge of the electrode subunit and rupturing a second perforation defining a second outer edge of the electrode subunit.

[0251] Embodiment 52. The process of Embodiment 51, wherein the first outer edge and the second outer edge are located on opposing sides of the electrode subunit.

[0252] Embodiment 53. The processes of embodiments 46-52, further comprising the step of applying cross-web tension to the electrode subunit using alignment pins.

[0253] Embodiment 54. The process of Embodiments 46-53, further comprising the step of bringing only a portion of each fiducial feature of the electrode subunit into contact with the alignment pin.

[0254] Embodiment 55. The process of Embodiments 46-54, further comprising the steps of defining a defective electrode subunit in a group of electrode subunits and controlling the punch head so as not to separate the defective electrode subunit from the layered arrangement of the laminated web.

[0255] Embodiment 56. The processes of embodiments 46-55, further comprising the step of positioning the fiducial features of an electrode subunit using an optical device.

[0256] Embodiment 57. The process of Embodiments 46-56, further comprising the step of marking the layered arrangement of the laminated web to indicate defective electrode subunits.

[0257] Embodiment 58. The process of Embodiments 46-57, further comprising the step of applying a compressive force to an electrode subunit between a punch head and a receiving unit.

[0258] Embodiment 59. The process according to Embodiment 58, wherein the compression is sufficient to maintain the electrode subunit substantially parallel to the surface of the receiving unit.

[0259] Embodiment 60. The processes of Embodiments 46-59, further comprising the step of using a vacuum apparatus to flatten the layered arrangement of the laminated webs.

[0260] Embodiment 61. The process of Embodiments 46-60, further comprising the step of using one or more rotating brushes to flatten the array of laminated webs.

[0261] Embodiment 62. The process of Embodiments 46-61, wherein the layered arrangement of the laminated webs comprises a web of anode material, a web of cathode material, and a web of separator material positioned between the webs of anode material and cathode material.

[0262] Embodiment 63. The processes of embodiments 46-62, further comprising the step of applying cross-web tension to a conveyor belt that engages with a transport feature of the laminated web array in order to flatten the web.

[0263] Embodiment 64. The processes of embodiments 46-63, further comprising the step of using a two-axis moving device to move an alignment pin so that it aligns with a fiducial feature.

[0264] Embodiment 65. The process of Embodiments 46-64, further comprising the step of moving a movable platform a distance equal to the thickness of the electrode subunit after separating the electrode subunit from the layered arrangement of the laminated web.

[0265] Embodiment 66. Processes of embodiments 46 to 65, wherein the electrode subunit comprises an anode material, a cathode material, and a separator material.

[0266] Embodiment 67. The array of stacked webs downstream of the punch head is an array of used webs, The processes of embodiments 46 to 66 further include the step of winding an array of used webs onto a roller.

[0267] The process of Embodiments 46 to 67, wherein the electrode subunits of Embodiments 68.100 to 300 are stacked on a receiving unit.

[0268] Embodiment 69. A battery assembly including an electrode subunit formed by a process of any of the preceding embodiments.

[0269] Embodiment 70. The processes of Embodiments 46-68, further comprising the step of stopping the web-direction movement of the layered arrangement of the laminated web while force is applied.

[0270] Embodiment 71. The process of Embodiment 70, wherein the force is applied in a direction substantially perpendicular to both the cross-web direction and the web direction.

[0271] Embodiment 72. The process of Embodiments 46-68, wherein the punch head contacts the anode material while force is applied.

[0272] Embodiment 73. The punch head is in contact with the cathode material while force is being applied, in the process of Embodiments 46-68.

[0273] Embodiment 74. The process of Embodiments 46-68, wherein the punch head contacts the separator material while applying force.

[0274] Embodiment 75. The processes of Embodiments 46-68, further comprising the step of applying cross-web tension to the layered arrangement of the laminated web within the range of 0-50 percent of the breaking strength of the perforations outside the weakening pattern.

[0275] Embodiment 76. A system for separating electrode subunits from a group of electrode subunits within an array of stacked webs, The electrode subunit is defined by the corresponding weakening pattern. The system is A receiving unit having at least two alignment pins extending therefrom, the alignment pins being positioned to engage with corresponding fiducial features of an electrode subunit and facing a first surface of the electrode subunit, A movable punch head comprising at least two punch head holes, wherein the punch head holes are sized and positioned to receive one corresponding alignment pin, and the punch head is positioned to face the opposing surface of an electrode subunit, A controller is configured to cause the punch head to apply sufficient force to the opposing surface of the electrode subunit to separate the electrode subunit from the array of laminated web along the weakening pattern. A system that includes this.

[0276] Embodiment 77. A system for separating electrode subunits from a group of electrode subunits within an array of stacked webs, The electrode subunit is defined by the corresponding weakening pattern. The system A receiving unit having a base and a movable platform, wherein the movable platform is selectively positionable at a predetermined position between the array of laminated webs and the base, A movable punch head positioned to face the opposing surface of the electrode subunit, A controller configured to cause a punch head to apply sufficient force to the opposing surface of an electrode subunit to separate the electrode subunit from the array of laminated webs along a weakening pattern, wherein the movable platform of the receiving unit is selectively positioned to receive the electrode subunit separated from the array of laminated webs, and A system that includes this.

[0277] Embodiment 78. The system according to Embodiment 76 or 77, wherein the receiving unit comprises a base, alignment pins, and a movable platform.

[0278] Embodiment 79. The system according to Embodiment 78, wherein the movable platform is configured to move by a distance equal to the thickness of the electrode subunit.

[0279] Embodiment 80. The system according to embodiments 76-79, wherein the controller is configured to move the movable platform.

[0280] Embodiment 81. The system according to embodiments 76-80, wherein the punch head has punch head holes for receiving each of the alignment pins.

[0281] Embodiment 82. The system according to embodiments 76-81, wherein the alignment pins of the receiving unit are adapted to apply cross-web tension to the electrode subunit.

[0282] Embodiment 83. The system according to embodiments 76-82, wherein the alignment pins of the receiving unit are adapted to receive each fiducial feature of the electrode subunit.

[0283] Embodiment 84. The system according to embodiments 76 to 83, further comprising a defect detection system for detecting defects in electrode subunits.

[0284] Embodiment 85. The system according to embodiments 76-84, wherein the controller is configured to operate the punch head so as not to separate defective electrode subunits from the array of laminated webs.

[0285] Embodiment 86. The system according to embodiments 76 to 85, further comprising an optical device for locating the fiducial features of an electrode subunit.

[0286] Embodiment 87. The system according to embodiments 76-86 further comprises a marking system for marking an array of laminated webs to indicate a defective electrode subunit.

[0287] Embodiment 88. The system according to embodiments 76-87, further comprising a vacuum device for planarizing an array of laminated webs.

[0288] Embodiment 89. The system according to embodiments 76-88, further comprising one or more rotating brushes for planarizing an array of laminated webs.

[0289] Embodiment 90. The system according to Embodiments 76 to 89, wherein the array of laminated webs comprises a web of anode material, a web of cathode material, and a web of separator material disposed between the web of anode material and the web of cathode material.

[0290] Embodiment 91. The system according to Embodiments 76 to 90, wherein the electrode subunit comprises an anode material, a cathode material, and a separator material.

[0291] Embodiment 92. A system for merging webs to manufacture electrode assemblies for secondary batteries, A first merge zone configured to move a web of a first substrate along a first web merge path, the web of the first substrate comprising a group of first components for an electrode subunit and a group of first transport features, the first components being defined by a corresponding weakening pattern, the first merge zone and A second merge zone configured to move the web of a second substrate along a second web merge path, the web of the second substrate comprising a group of second components for an electrode subunit and a group of second transport features, the second components being defined by a corresponding weakening pattern, the second merge zone A receiving member comprising a plurality of protrusions, wherein the receiving member is positioned adjacent to a first web merge path and a second web merge path, and the plurality of protrusions are configured to engage with a first transport feature of the web of the first substrate and a second transport feature of the web of the second substrate. Includes, The first merge zone is adapted to transport the web of the first substrate onto the receiving member at the first web merge position such that the transport features of the web of the first substrate are engaged by at least some of the multiple protrusions on the belt. The second merge zone is adapted to transport the web of the second substrate onto the receiving member at the second web merge position such that the second component is substantially aligned with the first component and the transport features of the web of the second substrate are engaged by at least some of the multiple projections on the belt. The second merge zone is spaced down the web from the first merge zone. system.

[0292] Embodiment 93. The process of Embodiment 92, wherein the web of the first substrate consists of a web of electrode material, and the web of the second substrate consists of a web of separator material.

[0293] Embodiment 94. The process of Embodiment 92, wherein the web of the first substrate is made of a separator material web, and the web of the second substrate is made of an electrode material web.

[0294] Embodiment 95. The system according to embodiments 92 to 94, wherein the first merge zone comprises a first merge sprocket having teeth for aligning with transport features on the web of the first substrate, and the second merge zone comprises a second merge sprocket having teeth for aligning with transport features on the web of the second substrate.

[0295] Embodiment 96. The system according to Embodiment 95, wherein the first merge zone consists of a first reverse-tooth sprocket, the second merge zone consists of a second reverse-tooth sprocket, and each of the first and second reverse-tooth sprockets consists of a plurality of recesses configured to engage with the teeth of the first and second merge sprockets, respectively.

[0296] Embodiment 97. The system according to Embodiment 96, wherein a first reverse-tooth sprocket is positioned between the first merge sprocket and the receiving member along a first web merge path, and a second reverse-tooth sprocket is positioned between the second merge sprocket and the receiving member along a second web merge path.

[0297] Embodiment 98. The system according to Embodiment 97, wherein the teeth of a first merge sprocket are positioned to pass through a first transport feature of the web of a first substrate and enter into a recess of a first reverse tooth sprocket, and the teeth of a second merge sprocket are positioned to pass through a second transport feature of the web of a second substrate and enter into a recess of a second reverse tooth sprocket.

[0298] Embodiment 99. The system according to Embodiment 97, wherein a first reversing tooth sprocket and receiving member define a first nip, and a second reversing tooth sprocket and receiving member define a second nip, the second nip having a larger gap than the first nip.

[0299] Embodiment 100. The system according to embodiments 92-99, wherein the first merge sprocket and the second merge sprocket have the same radius.

[0300] Embodiment 101. The system according to embodiments 92-100, wherein the first reverse-tooth sprocket and the second reverse-tooth sprocket have the same radius.

[0301] Embodiment 102. The system according to Embodiment 101, wherein the radii of the first and second merge sprockets are greater than the radii of the first and second reverse tooth sprockets.

[0302] Embodiment 103. The system according to embodiments 92-102, wherein the first merge zone further comprises a first unwinding roller for unwinding a spool of a web of a first substrate, and the second merge zone further comprises a second unwinding roller for unwinding a spool of a web of a second substrate.

[0303] Embodiment 104. The system according to Embodiments 92 to 103, wherein the first web merge path consists of a first catenary curve and the second merge path consists of a second catenary curve.

[0304] Embodiment 105. The system according to Embodiment 104, further comprising a sensor for detecting at least one characteristic of the first catenary curve.

[0305] Embodiment 106. The system according to Embodiment 105, further comprising a sensor for detecting at least one characteristic of a second catenary curve.

[0306] Embodiment 107. The system according to embodiments 92 to 106, further comprising a rotating brush for increasing the flatness of at least one of the webs of the first substrate and the web of the second substrate.

[0307] Embodiment 108. The system according to Embodiment 107, wherein the rotating brush is positioned in the web direction in front of at least one of the first merge sprocket and the second merge sprocket.

[0308] Embodiment 109. The system according to Embodiment 107, further comprising a counter-rotating brush that rotates in the opposite direction to the rotating brush, the counter-rotating brush being positioned across the web from the rotating brush.

[0309] Embodiment 110. The system according to embodiments 92-109, further comprising a vacuum device for increasing the flatness of at least one of the webs of the first substrate and the web of the second substrate.

[0310] Embodiment 111. The system according to Embodiment 110, wherein the vacuum device comprises a base having a plurality of vacuum holes for drawing in air.

[0311] Embodiment 112. The system according to embodiments 90 to 107, further comprising a deionizer configured to reduce the electrostatic charge of at least one of the webs of the first substrate or the web of the second substrate.

[0312] Embodiment 113. The system according to embodiments 107-112, wherein the deionizer is positioned in the web direction in front of at least one of the rotating brush and the vacuum tensioner.

[0313] Embodiment 114. The system according to embodiments 92 to 113, wherein the teeth of the first merge sprocket and the teeth of the second merge sprocket are tapered such that the base of the teeth has a larger cross-sectional area than the distal portion of the projection.

[0314] Embodiment 115. The system according to Embodiments 92 to 114, wherein the projection of the receiving member is tapered such that the base of the projection has a larger cross-sectional area than the distal portion of the projection.

[0315] Embodiment 116. The system according to embodiments 92 to 115, further comprising a sensor for detecting defects in at least one of the webs of the first substrate and the web of the second substrate.

[0316] Embodiment 117. The system according to Embodiment 116, wherein the sensor is positioned to detect a defect before at least one of the webs of the first substrate and the web of the second substrate is merged onto the receiving member.

[0317] Embodiment 118. The system according to Embodiment 116 or 117, further comprising a marking device for marking detected defects on at least one of the webs of the first substrate and the web of the second substrate.

[0318] Embodiment 119. The system according to Embodiments 92-118, further comprising a third merge zone configured to move a web of a third substrate along a third web merge path, wherein the web of the third substrate is a group of third components for an electrode subunit, the third components comprising a group of third components defined by a corresponding weakening pattern and a group of third transport features, the third merge zone is adapted to transport the web of the third substrate onto a receiving member at the merge position of the third web such that the third components are substantially aligned with the first and second components and the transport features of the web of the third substrate are engaged by at least some of a plurality of projections on the belt, and the third merge zone is spaced down the web from the first and second merge zones.

[0319] Embodiment 120. The process of Embodiment 119, wherein the web of the third substrate is made of a web of the counter electrode material, and the web of the second substrate is made of a web of the separator material.

[0320] Embodiment 121. The process of Embodiment 119, wherein the web of the third substrate is made of a separator material web and the web of the second substrate is made of an electrode material web.

[0321] Embodiment 122. The system according to Embodiments 119-121, further comprising a fourth merge zone configured to move a web of a fourth substrate along a fourth web merge path, wherein the web of the fourth substrate is a group of fourth components for an electrode subunit, the fourth components comprising a group of fourth components defined by a corresponding weakening pattern and a group of fourth transport features, the fourth merge zone is adapted to transport the web of the fourth substrate onto a receiving member at the merge position of the fourth web such that the fourth components are substantially aligned with the first, second, and third components and the transport features of the web of the fourth substrate are engaged by at least some of the protrusions on the belt, and the fourth merge zone is spaced down the web from the first, second, and third merge zones.

[0322] Embodiment 123. The process of Embodiment 122, wherein the web of the fourth substrate is made of a web of counter electrode material and the web of the third substrate is made of a web of separator material.

[0323] Embodiment 124. The process of Embodiment 122, wherein the web of the fourth substrate is made of a separator material web and the web of the third substrate is made of a counter electrode material web.

[0324] Embodiment 125. The system according to Embodiments 92 to 124, wherein the receiving member consists of a continuous belt.

[0325] Embodiment 126. The system according to Embodiments 92 to 124, wherein the receiving member consists of a plurality of pin plates.

[0326] Embodiment 127. An electrode subunit manufactured using the system described in any of Embodiments 92-126 or 129-154.

[0327] Embodiment 128. The electrode subunit according to Embodiment 119, wherein the electrode subunit comprises an anode material, a cathode material, and a separator material.

[0328] Embodiment 129. A process or system according to any of the prior embodiments, wherein the web of the electrode material comprises an electrode active material.

[0329] Embodiment 130. The process or system according to Embodiment 129, wherein the electrode active material is an anode active material.

[0330] Embodiment 131. The process or system according to Embodiment 129, wherein the electrode active material is a cathode active material.

[0331] Embodiment 132. A process or system according to any of the prior embodiments, wherein the web of the counter electrode material comprises a counter electrode active material.

[0332] Embodiment 133. The process or system according to Embodiment 132, wherein the counter electrode active material is an anode active material.

[0333] Embodiment 134. The process or system according to Embodiment 132, wherein the counter electrode active material is a cathode active material.

[0334] Embodiment 135. A process or system according to any of the preceding embodiments, wherein one of the electrode active material and the counter electrode active material is an anode active material selected from the group consisting of the following. (a) Silicon (Si), germanium (Ge), tin (Sn), lead (Pb), antimony (Sb), bismuth (Bi), zinc (Zn), aluminum (Al), titanium (Ti), nickel (Ni), cobalt (Co), and cadmium (Cd); (b) Alloys or intermetallic compounds of Si, Ge, Sn, Pb, Sb, Bi, Zn, Al, Ti, Ni, Co, or Cd with other elements; (c) Oxides, carbides, nitrides, sulfides, phosphides, selenides, tellurides of Si, Ge, Sn, Pb, Sb, Bi, Zn, Al, Ti, Fe, Ni, Co, V, Cd, and mixtures thereof, composites, lithium-containing composites; (d) Salts and hydroxides of Sn; (e) Lithium titanate, lithium manganate, lithium aluminate, lithium-containing titanium oxide, lithium transition metal oxide, ZnCo2O4; (f) Graphite and carbon particles; (g) Lithium metal; A combination of (h)(a)~(G).

[0335] Embodiment 136. A process or system according to any of the preceding embodiments, wherein one of the electrode active material and the counter electrode active material is an anode active material selected from the group consisting of silicon (Si), germanium (Ge), tin (Sn), lead (Pb), antimony (Sb), bismuth (Bi), zinc (Zn), aluminum (Al), titanium (Ti), nickel (Ni), cobalt (Co), and cadmium (Cd).

[0336] Embodiment 137. A process or system according to any of the preceding embodiments, wherein one of the electrode active material and the counter electrode active material is an anode active material selected from the group consisting of alloys and intermetallic compounds of Si, Ge, Sn, Pb, Sb, Bi, Zn, Al, Ti, Ni, Co, or Cd with other elements.

[0337] Embodiment 138. A process or system according to any of the preceding embodiments, wherein one of the electrode active material and the counter electrode active material is an anode active material selected from the group consisting of oxides, carbides, nitrides, sulfides, phosphides, selenides, and tellurides of Si, Ge, Sn, Pb, Sb, Bi, Zn, Al, Ti, Fe, Ni, Co, V, and Cd.

[0338] Embodiment 139. A process or system according to any of the preceding embodiments, wherein one of the electrode active material and the counter electrode active material is an anode active material selected from the group consisting of oxides, carbides, nitrides, sulfides, phosphides, selenides, and tellurides of Si.

[0339] Embodiment 140. The process or system according to any of the preceding embodiments, wherein one of the electrode active material and the counter electrode active material is an anode active material selected from the group consisting of silicon and silicon oxides and carbides.

[0340] Embodiment 141. The process or system according to any of the preceding embodiments, wherein one of the electrode active material and the counter electrode active material is an anode active material made of lithium metal.

[0341] Embodiment 142. The process or system according to any of the preceding embodiments, wherein one of the electrode active material and the counter electrode active material is an anode active material selected from the group consisting of graphite and carbon.

[0342] Embodiment 143. A process or system according to any of the prior embodiments, wherein the web of the separator material comprises a polymer electrolyte.

[0343] Embodiment 144. A process or system according to any of the prior embodiments, wherein the web of the separator material comprises a solid electrolyte.

[0344] Embodiment 145. A process or system according to any of the preceding embodiments, wherein the web of the separator material comprises a solid electrolyte selected from the group consisting of sulfide-based electrolytes.

[0345] Embodiment 146. The web of the separator material is lithium tin sulfide (Li 10 SnP2S 12 ), lithium phosphate sulfide (β-Li3PS4) and lithium phosphorus sulfur iodide chloride (Li6PS5Cl) 0.9 I0.1 ) A process or system according to any of the preceding embodiments, comprising a solid electrolyte selected from the group consisting of

[0346] Embodiment 147. A web of separator material includes an electrolyte separator having an upper surface, a lower surface, and a bulk therebetween, the bulk having a thickness, the length or width of the upper surface or the lower surface being at least 10 times greater than the thickness of the bulk, the thickness of the bulk being from about 10 nm to about 100 μm, the bulk being characterized by the chemical formula LiALaBM′CM″DZrEOF, where 4 < A < 8.5, 1.5 < B < 4, 0 ≤ C ≤ 2, 0 ≤ D ≤ 2; 0 ≤ E < 2, 10 < F < 13, M′ is Al, and M″ is selected from Al, Mo, W, Nb, Sb, Ca, Ba, Sr, Ce, Hf, Rb, and Ta; where either the upper surface or the lower surface consists of lithium carbonate, lithium hydroxide, lithium oxide, lithium peroxide, their hydrates, their oxides, or a combination thereof, A process or system according to any of the preceding embodiments.

[0347] Embodiment 148. A web of separator material includes a polymer electrolyte selected from the group consisting of a PEO-based polymer electrolyte, a polymer-ceramic composite electrolyte (solid), a polymer-ceramic composite electrolyte, and a polymer-ceramic composite electrolyte, a process or system according to any of the preceding embodiments.

[0348] Embodiment 149. A web of separator material includes a solid electrolyte selected from the group consisting of an oxide-based electrolyte, a process or system according to any of the preceding embodiments. [[ID=***]]

[0349] Embodiment 150. A web of separator material is lithium lanthanum titanate (Li 0.34 La 0.56 TiO3), aluminum-doped lanthanum zirconate (Li 6.24 La3Zr2Al 0.24 O 11.98), Ta-doped zirconium lanthanum (Li 6.4 La3Zr 1.4 Ta 0.6 O 12 ) and lithium aluminum titanium phosphate (Li 1.4 Al 0.4 Ti 1.6 A process or system according to any of the preceding embodiments, comprising a solid electrolyte selected from the group consisting of (PO4)3).

[0350] Embodiment 151. The process or system according to any of the preceding embodiments, wherein one of the electrode active material and the counter electrode active material is a cathode active material selected from the group consisting of an intercalation chemical cathode and a conversion chemical cathode.

[0351] Embodiment 152. The process or system according to any of the prior embodiments, wherein one of the electrode active material and the counter electrode active material is a cathode active material consisting of an intercalation chemical cathode material.

[0352] Embodiment 153. A process or system according to any of the prior embodiments, wherein one of the electrode active material and the counter electrode active material is a cathode active material comprising a conversion chemical cathode active material.

[0353] Embodiment 154. One of the electrode active material and the counter electrode active material is S (or Li2S in a lithium state), LiF, Fe, Cu, Ni, FeF2, FeOdF 3.2 A process or system according to any of the preceding embodiments, wherein d is a cathode-active material selected from the group consisting of FeF3, CoF3, CoF2, CuF2, and NiF2, where 0 ≤ d ≤ 0.5.

[0354] This specification discloses the present invention, including best embodiments, using examples, enabling anyone skilled in the art to carry out the invention, including the manufacture and use of any device or system, and the execution of any method incorporating the invention. The patentable scope of the present invention is defined by the claims and may include other embodiments that a person skilled in the art can conceive. Such other embodiments are intended to be included in the claims if they have structural elements that are not different from the language of the claims, or if they include equivalent structural elements that are substantially different from the language of the claims.

Claims

1. 1. A system for merging webs to manufacture an electrode assembly for a secondary battery, comprising: a first merge zone configured to move a first web of substrate along a first web merge path, the first web of substrate including a first population of components for electrode subunits and a first population of transport features, the first components being defined by a corresponding weakening pattern; a second merge zone configured to move a web of a second substrate along a second web merge path, the web of the second substrate including a population of second components for the electrode subunits and a population of second transport features, the second components being defined by a corresponding weakening pattern; a receiver member including a plurality of protrusions disposed adjacent the first web merge path and the second web merge path, the plurality of protrusions configured to engage a first transport feature of the web of the first substrate and a second transport feature of the web of the second substrate; Including, the first merge zone is adapted to convey the first substrate web onto the receiver member at a first web merge location such that first conveying features of the first substrate web are engaged by at least a portion of the plurality of protrusions on the receiver member; the second merge zone is adapted to convey the second substrate web onto the receiver member at a second web merge location such that the second component is substantially aligned with the first component and a second conveying feature of the second substrate web is engaged by at least a portion of the plurality of protrusions on the receiver member; the second merge zone is spaced in a downweb direction from the first merge zone; system.

2. the first substrate web comprises a web of electrode material and the second substrate web comprises a web of separator material; The system of claim 1 .

3. the first substrate web comprises a web of separator material and the second substrate web comprises a web of electrode material; The system of claim 1 .

4. the first merging zone includes a first merging sprocket having teeth for aligning with a transport feature on the web of the first substrate, and the second merging zone includes a second merging sprocket having teeth for aligning with a transport feature on the web of the second substrate; A system according to any one of claims 1 to 3.

5. the first merging zone includes a first inverted tooth sprocket and the second merging zone includes a second inverted tooth sprocket, each of the first and second inverted tooth sprockets including a plurality of recesses configured to engage teeth of the first and second merging sprockets, respectively; The system of claim 4.

6. The first inverted tooth sprocket and the backing member define a first nip, and the second inverted tooth sprocket and the backing member define a second nip, the second nip having a larger spacing than the first nip. The system of claim 5.

7. the first web merge path includes a first catenary curve and the second merge path includes a second catenary curve; A system according to any one of claims 1 to 6.

8. a first sensor for detecting at least one characteristic of the first catenary curve; and a second sensor for detecting at least one characteristic of the second catenary curve. The system of claim 7 further comprising:

9. the teeth of the first merge sprocket and the teeth of the second merge sprocket are tapered such that a base of the tooth has a larger cross-sectional area than a distal portion of the lug; A system according to any one of claims 5 to 8.

10. the projection of the receiver member is tapered such that a base of the projection has a larger cross-sectional area than a distal portion of the projection; A system according to any one of claims 1 to 9.

11. The system of any one of claims 1 to 10, further comprising a defect sensor for detecting defects in at least one of the first substrate web and the second substrate web.

12. a third merging zone configured to move the web of the third substrate along a third web merging path; a third substrate web including a third population of components for the electrode subunits and a third population of transport features; the third component is defined by a corresponding weakening pattern; The third merge zone is a third component adapted to convey a third web of substrate onto the receiver member at a third web merge location such that the third component is substantially aligned with the first and second components and a third conveying feature of the third web of substrate is engaged by at least a portion of the plurality of protrusions on the receiver member; the third merging zone is spaced in a downweb direction from the first merging zone and the second merging zone; A system according to any one of claims 1 to 11.

13. further comprising a fourth merging zone configured to move the fourth web of substrate along a fourth web merge path; a fourth substrate web including a fourth population of components for the electrode subunits and a fourth population of transport features, the fourth components being defined by corresponding weakening patterns; a fourth merge zone adapted to convey a fourth substrate web onto the receiving member at a fourth web merge location such that the fourth component is substantially aligned with the first, second, and third components and conveying features of the fourth substrate web are engaged by at least a portion of the plurality of protrusions on the receiving member; the fourth merging zone is spaced in a downweb direction from the first merging zone, the second merging zone, and the third merging zone; The system of claim 12.

14. the fourth substrate web comprises a web of counter electrode material and the third substrate web comprises a web of separator material; The system of claim 13.

15. the fourth substrate web comprises a web of separator material and the third substrate web comprises a web of counter electrode material; The system of claim 13.