Synthetic polyisoprene latex condoms with reduced nitrosamine
Patent Information
- Application Number
- JP2024023051
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-10-22
- Filing Date
- 2024-02-19
- Publication Date
- 2024-11-08
AI Technical Summary
Existing methods for manufacturing synthetic polyisoprene latex condoms result in the formation of carcinogenic nitrosamines during the vulcanization process, posing health risks to workers and users due to their release into the manufacturing environment and contact with the skin.
A method involving pre-vulcanization of synthetic polyisoprene latex using multiple accelerators activated at different temperatures to form bonds between polyisoprene molecules and sulfur, limiting sulfur availability to prevent over-curing and nitrosamine formation, with a controlled prevulcanization process at low temperatures.
The method produces highly elastic, tear-resistant condoms with minimal nitrosamine content, ensuring a safe manufacturing environment and reducing carcinogenic compound transfer to users, while maintaining high tensile strength and elasticity.
Smart Images

Figure 00000017_0000
Abstract
Description
[Technical field]
[0001] The present invention relates to the manufacture and method of highly stretchable, reduced nitrosamine synthetic polyisoprene latex condoms.
[0002] Technical Field The present invention relates to the manufacture of dip-molded synthetic polyisoprene condoms, which involves immersing condom formers in a pre-vulcanized synthetic polyisoprene latex emulsion at low temperature to reduce or prevent the formation of carcinogenic nitrosamines. See https: / / www.who.int / ipcs / publications / cicad / en / cicad38.pdf. The latex condom manufacturing environment is thereby free of nitrosamines, typically as described by Sen et al. 1984 (Sen NP, Seaman S, Clarkson S, Garrod F, Lalonde P (1984) Volatile N-nitrosamines in baby bottle rubber nipples and pacifiers. Analysis, occurrence and migration. IARC scientific npublications, 57:51-57). The nitrosamine contamination of the areas that come into contact with the user's skin is minimal or below the limit of detection. [Background technology]
[0003] In the dip molding process, most of the research with natural polyisoprene has focused on the development of polyisoprene condoms and gloves using the dip process. In this type of process, a former having the shape of a glove is first dipped into a coagulant solution known to destabilize latex formulations. The coagulant layer is then dried, after which the former is dipped into a bath of ready-mixed latex formulation. The coagulated wet latex gel is typically filtered in water to remove residual surfactants in the ready-mixed latex formulation. This is followed by drying at a relatively high temperature to complete the cross-linking of the rubber membrane. The condom former is dipped without the coagulant.
[0004] The use of vulcanizing or sulfur crosslinking agents in the manufacture of rubber products is well known. The effectiveness of sulfur crosslinking agents is improved by conventional accelerators such as dithiocarbamates, thiazoles, guanidines, thioureas, amines, disulfides, thiurams, xanthates, and sulfonamides. The use of vulcanizing agents in the manufacture of polyisoprene rubber is disclosed in U.S. Patent No. 5,744,552 by D'Sidocky et al. and U.S. Patent No. 6,114,469 by Rauchfuss et al.
[0005] Attempts have been made to use several accelerators in the vulcanization of polyisoprene latex.
[0006] U.S. Patent No. 4,695,609 to Stevenson discloses a vulcanizable rubber composition of xanthogen polysulfide and xanthate compounds containing less than 0.4 parts by weight of nitrosatable material per 100 parts by weight of rubber. The rubber composition includes a dihydrocarbyl xanthogen polysulfide and a xanthate selected from metal hydrocarbyl xanthates and dihydrocarbyl xanthates. Aqueous latex emulsion 9E contains sulfur, zinc oxide, and zinc diethyldithiocarbamate, and is only stable for 4 days and has low tensile strength at break, making it unsuitable for manufacturing processes.
[0007] U.S. Patent No. 5,254,635 to Stevenson discloses a rubber composition containing dibenzyl thiuram sulfide. Dibenzyl thiuram sulfides such as thiophene, in combination with dihydrocarbyl xanthogen polysulfides and / or xanthates provide compositions that crosslink natural rubber at 120-180°C without the formation of harmful nitrosable materials. However, these natural latex compositions do not contain sulfur and do not crosslink the intraparticle regions of the less stereoregular synthetic cis-1,4-polyisoprene. Thus, the use of these crosslinkers with natural polyisoprene latex results in a non-uniform product with poor properties.
[0008] U.S. Patents 6,653,380 and 7,048,977 to Dzikowicz disclose latex film compounds with improved tear resistance. The method enhances the tear resistance, tensile strength, and anti-aging properties of the latex product by adding an antioxidant synergist to the latex compound along with an antioxidant. The latex compound includes a polymer, a stabilizing system, a film surface conditioner, and a curing system including an activator, a crosslinker, and an accelerator. The antioxidant synergists include 2-mercaptobenzimidazole (MBI), 2-mercaptotoluimidazole (MTI), zinc 2-mercaptobenzimidazole (ZMBI), and zinc 2-mercaptotoluimidazole (ZMTI). The latex product that is molded can be a glove, but also includes threads, balloons, and other latex related products. The latex used with the addition of antioxidants does not prevulcanize the polyisoprene latex.
[0009] U.S. Patent No. 6,828,387 to Wang et al. discloses a polyisoprene product and a method for its manufacture. The polyisoprene product produced by this method exhibits tensile strength properties similar to those of the solvent-based process using natural rubber latex. In this process, a synthetic latex is combined in a pre-cure step with sulfur, zinc oxide, and an accelerator composition including dithiocarbamate, thiazole, and guanidine compounds (all three must be present). In a preferred embodiment, the accelerator composition includes zinc diethyldithiocarbamate (ZDEC), zinc 2-mercaptobenzothiazole (ZMBT), and diphenylguanidine (DPG), along with a stabilizer that is primarily a milk protein salt such as sodium caseinate. Polyisoprene latex (typically 60% solids) and the stabilizer (such as sodium caseinate) are mixed at ambient temperature (approximately 20-25°C). After mixing for a period of time, the mixture is diluted with water to 40% solids. Wingstay L is then added and the mixture is stirred for about 15 minutes. At this point, the pH can be adjusted to a range of about 8.5 to 9.0. Zinc oxide is added, followed by sulfur and accelerator compounds. The elastomeric polyisoprene product produced by this method is a surgical glove in which a coagulant-coated former is dipped. The aqueous latex emulsion has minimal stability, with a maximum stability of 8 days. The resulting surgical glove product has a tensile strength of only about 3000 psi, or 20.6 MPa. The accelerator is added to the latex emulsion, but is maintained at low temperatures for up to 8 days. The stability of this aqueous latex composition is better than that of Stevenson (U.S. Pat. No. 4,695,609), but is still not suitable for manufacturing processes. Glove formers are dipped into a coagulant solution containing calcium nitrate, which is not suitable for dipping condoms without a coagulant.
[0010] U.S. Patent No. 7,041,746 to Dzikowicz discloses an accelerator system for synthetic polyisoprene latex. The accelerator system includes a dithiocarbamate and a thiourea and is capable of producing synthetic polyisoprene films with tensile strengths of about 3000 psi to about 5000 psi at low cure temperatures. There is no suggestion of pre-vulcanizing the polyisoprene particles with these accelerators, and the latex products produced have an extremely low modulus of 1.5 MPa at 300% elongation.
[0011] U.S. Patent Application Publication No. 2002 / 0173563 describes a method for making dipped products from latex that involves the use of an accelerator system containing zinc diethyldithiocarbamate ("ZDEC"), zinc 2-mercaptobenzothiazole ("ZMBT"), and diphenylguanidine ("DPG"). ZDEC in combination with ZMBT is a common accelerator system for natural rubber latex. To achieve a cured film with a tensile strength of greater than 3000 psi (20 MPa), DPG must be added to the accelerator system.
[0012] British Patent Application Publication No. 2,436,566 to Attrill et al. discloses minimizing pre-vulcanization of polyisoprene latex. The method for producing polyisoprene latex involves compounding synthetic polyisoprene latex with compounding ingredients and maturing the latex at low temperatures to minimize pre-vulcanization. Dipping of condoms is also typically performed at low temperatures, below 15°C to 20°C. To ensure that pre-vulcanization has not occurred, the strength of the rings produced is confirmed to have a prevulcanisate relaxed modulus of less than 0.1 MPa, which is indicative of no pre-vulcanization. The latex emulsion may contain accelerators such as dithiocarbamates. The teachings of the '566 patent application preclude pre-vulcanization prior to dipping of the latex product.
[0013] When rubber latex is vulcanized at high temperatures, nitrites react with secondary amines to produce nitrosamines.
[0014] U.S. Patent No. 6,495,065 to Lou et al. discloses a nitrosamine inhibiting composition for terminating free radical emulsion polymerization. This method of terminating free radical emulsion polymerization inhibits the formation of nitrosamines. The composition includes a combination of a nitrosamine inhibitor with a conventional alkylhydroxyamine polymerization terminator. Such nitrosamine inhibitors are based on primary amines, amine-containing polymers, pyrroles, hydroquinones, some phenols, ascorbic acid, and other well-known nitrosation inhibitors, which may be used individually or in mixtures. The composition is of interest for application in emulsion processes for rubber latex production and rubber product creation.
[0015] In WO 97 / 32927 to Gibbs et al., inhibition of nitrosamine formation in rubber is disclosed. This method for reducing or inhibiting nitrosamine formation in vulcanizable rubber involves the incorporation of alkaline earth metal carboxylates or phenates. These compounds have melting points below 130°C.
[0016] The IARC Sci Publ 1982;(41):231-43 article discusses nitrosamines and rubber. Occupational exposure to N-nitrosamines in the rubber industry was first reported by Fajen et al. (1979). Chemical and industrial products, as well as the air in various work areas, were analyzed to study the origin and formation of nitrosamines in this industry (Spiegelhalder et al., 1980). All chemicals used in rubber compounds contain nitrosamines if they are derivatives of secondary amines such as tetramethylthiuram, zinc diethyldithiocarbamate, or N-oxydiethylenebenzothiazolylsulfenamide. In all rubber products containing these dialkylamine derivatives, the corresponding nitrosamines were found in significant amounts. As a result, airborne nitrosamines were detected in various concentrations in areas where rubber products were manufactured or stored. The nitrosamines found correspond to the compounding chemicals. Natural nitrosamine concentrations in rubber chemicals are not high enough to explain the amounts found in rubber products and in the air. nitrosation must have occurred. The responsible nitrosating agents are described. Preliminary results indicate that in most cases, elimination of the nitrosating agents or the use of alternative rubber chemicals can significantly reduce nitrosamine concentrations in rubber products and work areas.
[0017] Thus, there is a need for highly extensible stretchable latex products, such as synthetic polyisoprene condoms, made by dipping formers into a stable polyisoprene latex emulsion composition that does not agglomerate or clump and has a suitable emulsion shelf life for use. The manufacture of these condoms involves no release of nitrosamines into the manufacturing environment and minimal concentrations of nitrosamines in the condoms, thus preventing the release of carcinogenic compounds to the consumer. The composition should achieve intra- and inter-particle crosslinking in the final product. Such compositions allow for the dip molding of products with or without the use of coagulants, resulting in products with thinner, continuous, defect-free layers, high strength and improved stretchability. Such products do not deteriorate and maintain their physical integrity over time. The present invention aims to provide such compositions, methods for preparing such compositions and their use in dip molding synthetic polyisoprene products, such as condoms and gloves, and the products made thereby. These and other objects and advantages, as well as further inventive features, will become apparent from the detailed description provided herein. Summary of the Invention [Problem to be solved by the invention]
[0018] The present invention relates to the manufacture and method of highly stretchable, reduced nitrosamine synthetic polyisoprene latex condoms. [Means for solving the problem]
[0019] The method for producing high quality condoms from synthetic polyisoprene includes using multiple accelerators that are effectively activated at different temperatures to form bonds between polyisoprene molecules and provided sulfur, where all of the provided sulfur is depleted in forming physical bonds with the polyisoprene molecules and does not cause over curing of the bonds at each temperature that forms the chemical bonds between the sulfur and the polyisoprene.
[0020] The amount of available sulfur is limited, and as the mix temperature increases from 20°C to 40°C, different accelerators provided in the latex bath activate the sulfur and pre-vulcanize the polyisoprene latex until all bonding sites are exhausted. This pre-vulcanization physically positions the sulfur atoms at suitable sites on the polyisoprene polymer molecule to react completely while forming chemical bonds during the vulcanization cycle.
[0021] Nitrosamines are not produced because the pre-vulcanization temperature is low and vulcanization is carried out in the temperature range of 90°C to 120°C. The raw material composition of the manufactured condoms is tested for nitrosamines.
[0022] The latex condom has controlled pre-vulcanized particles of synthetic polyisoprene latex that are pre-vulcanized with multiple accelerators that are individually activated as the temperature of the latex increases from 20° C. to 40° C. The pre-vulcanized aqueous latex emulsion is used to dip mold thin latex condoms and vulcanized at low temperatures of 90° C. to 120° C. for a short period of time. The cured latex condom is a highly stretchable synthetic rubber body that exhibits elongation of approximately 900% and is extremely tear resistant.
[0023] The manufacture of latex products by vulcanization at high temperatures results in the formation of carcinogenic nitrosamines. Nitrosamines are commonly present in latex manufacturing sites and are a potential hazard to workers. The latex products produced in this manner are potentially harmful. In addition, the latex products produced in this manner contain carcinogenic nitrosamines which can migrate to the skin of the user where they come into contact with the user. Thus, a need exists for a method of producing synthetic polyisoprene products which minimizes the formation of nitrosamines in both the work environment and the latex products produced in this manner.
[0024] The products thus produced have several distinguishing features that make this prevulcanization procedure impressive. The synthetic polyisoprene films of the latex are cured with improved crosslink density, resulting in low molecular weights between crosslinks. The zinc complexes of dithiocarbamates are converted to sulfur S.8 It catalytically cleaves the rings, allowing for reuse as a catalyst, and furthermore, due to its large molecular size, does not easily penetrate synthetic polyisoprene. The molecular size of zinc dibutyldithiocarbamate is larger than that of zinc diethyldithiocarbamate, which has a larger molecular size than zinc dimethyldithiocarbamate. Zinc dibenzyldithiocarbamate and zinc diphenyldithiocarbamate are larger molecules and are believed to be resistant to penetration into natural polyisoprene latex particles. Thus, the preferred zinc complexes of dithiocarbamate for pre-vulcanization of synthetic latex particles in latex emulsions are zinc dibutyldithiocarbamate (ZDBC) or zinc diethyldithiocarbamate (ZDEC). There is an accumulation of zinc-containing compounds surrounding each original synthetic polyisoprene particle, and this microstructural feature can be easily observed by microprobe elemental analysis using an electron microscope. The resulting synthetic polyisoprene membranes typically have acceptable tensile strength, high tensile modulus, and elongation at break, with fracture surfaces passing through both the interparticle and intraparticle regions, indicating that the intraparticle and interparticle regions within the resulting natural latex membrane are of substantially equal strength.
[0025] The method for producing the synthetic polyisoprene condom includes the use of a synthetic latex emulsion, which is a pre-vulcanized composition. Preferably, the synthetic polyisoprene particles are cis-1,4-polyisoprene and have a diameter in the range of about 0.2 to 2 micrometers and are maintained in the aqueous medium of the latex emulsion. The pre-vulcanized composition includes sulfur, including sulfur extracted from an amorphous sulfur source by ZDBC catalysis, which is typically S. 8 S cleaved by dithiocarbamate zinc promoter destroys the sulfur ring structure 8It is of ring structure. A combination of surfactants such as Hostapur SAS is used to deliver the cleaved sulfur molecules to the latex. Pre-vulcanization of the synthetic latex particles in the synthetic latex emulsion occurs over a period of 12 hours in the mixing process plus 12-24 hours in the maturation tank, depending on the temperature of the latex emulsion, which generally ranges from 20°C to 40°C. The degree of pre-vulcanization of the synthetic latex particles is measured using a swelling index test, measuring the change in diameter of the dried film on toluene over a period of 20 minutes.
[0026] A typical synthetic polyisoprene latex emulsion composition is provided per 100 parts by weight of dry rubber (phr): sulfur crosslinker in the range of 0.6-1.8 wt%; ZDEC and / or ZDBC accelerator in the range of 0.3-1.0 wt%; SDBC accelerator in the range of 0.05-0.5 wt%; DXP accelerator in the range of 0.2-0.8 wt%; reactive zinc oxide activator in the range of 0-0.5 wt%; Hostapur SAS in the range of 0.1-0.5 wt%; SDBS surfactant in the range of 0.1-0.35 wt%; polyoxyethylene cetyl / stearyl ether surfactant in the range of 0.1-0.5 wt%; Winsgtay L or butylated reaction product of p-cresol and dicyclopentadiene antioxidant preservative in the range of 0.3-1 wt%; and ammonium hydroxide in the range of 0-0.36 wt%. As previously mentioned, the pre-vulcanization composition of the synthetic polyisoprene latex composition includes sulfur extracted from amorphous sulfur by ZDEC and / or ZDBC accelerators, Hostapur SAS and / or potassium caprylate surfactant, SDBS surfactant, and polyoxyethylene cetyl / stearyl ether surfactant. The post-vulcanization composition provides sulfur availability to the synthetic polyisoprene latex particles in the post-vulcanization emulsion, which then crosslinks the entire particle of synthetic polyisoprene during the vulcanization cure cycle. The post-vulcanization composition provides the ability to crosslink the regions between the particles of synthetic polyisoprene, thereby ensuring a high quality, substantially uniformly cured, synthetic polyisoprene product.
[0027] The method is effective for producing synthetic polyisoprene condoms, but can also be used to produce probe covers. The probes are similar to condoms, but do not have the reservoir at the tip of a condom. Being nitrosamine-free, the probes do not transfer any carcinogenic compounds to the user. [Brief description of the drawings]
[0028] [Figure 1] FIG. 1 shows the steps used in the present method for making condoms from synthetic polyisoprene. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] The condoms are made from synthetic polyisoprene rubber with a combination of accelerators that cure at different successively increasing temperatures, so that the sulfur vulcanizing agent is depleted at each site, ensuring full cure of the polyisoprene condom without any over-vulcanization of the accelerator cured polyisoprene.
[0030] The vulcanization temperature is low, so the formation of nitrosamines is limited. Nitrosamines are formed by the reaction of nitrites with secondary amines and are highly temperature dependent. Of the nitrosamines, N-nitrosodiethylamine (NDEA) is the most potent carcinogen.
[0031] The synthetic polyisoprene condoms are manufactured as follows: First, 15% Hostapur SAS anionic surfactant is prepared by mixing it in deionized water at 50° C. Then, a 10% potassium oleate solution is prepared.
[0032] The chemicals used in this method and their functions are detailed below. Sulfur: Vulcanizing agent Activated Zinc Oxide: Activator Butylated reaction products of p-cresol and dicyclopentadiene: antioxidants. Zinc diethyldithiocarbamate (ZDEC): Accelerator Zinc dibenzyldithiocarbamate (ZBEC): Accelerator Zinc dibutyldithiocarbamate (ZDBC): Accelerator Potassium hydroxide: Stabilizer The detailed procedure for adding these chemicals is as follows: 600 kg of polyisoprene latex is transferred to a mixing tank and stirred for 15 minutes. 7.8 kg of colloidal sulfur is stirred for 15 minutes. Add 6.48 kg of 15% Hostapur SAS surfactant solution. Add 3.78 kg of a 10% potassium oleate solution. Add 7.68 kg of 15% Eumulgin solution. 0.36 kg of zinc oxide activator is added over 15 minutes. 3.89 kg of antioxidant is added over 15 minutes. 3.89 kg of ZDEC is added over 15 minutes. 0.79 kg of ZBEC is added over 15 minutes. Add 1.2 kg of a 15% Hostapur SAS solution. 0.72 kg of ZDBC is added over 15 minutes. Add 28.8 kg of 1.23% potassium hydroxide solution in water + 0.38 kg of KOH. Stir for 12 hours.
[0033] During this time, the catalytic activity of the ZDBC reacts with the colloidal sulfur, breaking the S8 ring and generating linear sulfur chains, which are then transported by the Hostapur SAS surfactant into the interior of the intertwined synthetic polyisoprene chains, where the sulfur atoms attach to the synthetic polyisoprene chains within the polyisoprene particles, resulting in pre-vulcanization.
[0034] As all the accelerators are mixed and added to the synthetic polyisoprene, they all react based on the processing temperature conditions. At low temperatures, e.g. 20°C, the ZDBC catalytically reacts with colloidal sulfur to break the S8 ring and form linear sulfur chains, which enter the intertwined synthetic polyisoprene particles with the assistance of the surfactants present. The ZDEC also allows for the attachment of sulfur from the linear sulfur chains to active sites within the polyisoprene molecules, resulting in pre-vulcanization. When the temperature of the polyisoprene bath is raised to approximately 20°C to 40°C, all the accelerators react with the outer surface of the polyisoprene particles, attaching sulfur atoms to the outer surface of the synthetic polyisoprene particles, providing pre-vulcanization.
[0035] Prior to condom immersion, the degree of pre-vulcanization is measured by the swelling index of the latex in toluene. Measurements are made by preparing a dry disk of latex rubber film 20 mm in diameter and immersing it in toluene for 20 minutes to expand the disk. Unvulcanized rubber expands to 160% of its original size. Lightly vulcanized rubber swells from 100% to 160%. Moderately vulcanized rubber swells from 80% to 100%. Fully vulcanized rubber swells to 75%. In our method, a swelling index of 130% indicates that the latex is mature and ready for condom immersion.
[0036] Immersion tank 1 Latex temperature <40℃
[0037] Immersion tank 2 latex temperature <40℃
[0038] Latex soaking temperature 20℃~30℃
[0039] Vulcanization oven 90℃~120℃
[0040] The present invention uses sulfur S 8The present invention is based on the discovery that amorphous sulfur such as rings, catalyzed by a zinc complex of dithiocarbamate in combination with Hostapur SAS surfactant, produces pre-vulcanized synthetic polyisoprene particles in a latex composition. This latex composition allows for the production of condom latex film products by dipping a coagulant-free former into the latex composition. The surfactant package inhibits agglomeration and clumping of the synthetic polyisoprene particles. The latex-dipped film has synthetic polyisoprene particles that are crosslinked and the regions between the particles crosslink during vulcanization cure, resulting in intra- and inter-particle crosslinks. The resulting product contains a high quality, uniform latex film.
[0041] The latex stabilizing composition keeps the synthetic polyisoprene particles separated from one another in an aqueous medium. The polyisoprene particles do not come into contact with one another and therefore cannot agglomerate or clump together. This is important because if the particles begin to agglomerate, van der Waals forces may prevent them from separating from one another. Preferably, the latex stabilizing composition includes a Hostapur SAS surfactant package. Anionic surfactants are preferred, especially those that remain stable for periods significantly greater than one month, up to two months or more. An example of such a surfactant is sodium dodecylbenzene sulfonate (SDBS). Other examples include other alkyl aryl sulfonates, alkyl sulfonates (e.g., C14 aryl sulfonates sold under the tradename Calsoft AOS-40 (Pilot Chem. Co., Red Bank, NJ)). Examples of suitable surfactants include, but are not limited to, olefin sulfonates, olefin sulfonates, and alcohol sulfonates (e.g., sodium lauryl sulfate). The SDBS or other alkylaryl sulfonate is preferably present in an amount of about 0.1-0.35 wt% based on the dry weight of the polyisoprene. The SDBS or other alkylaryl sulfonate may be combined with one or more other surfactants, such as potassium caprylate and polyoxyethylene cetyl / stearyl ether. For example, the SDBS or other alkylaryl sulfonate may be combined with potassium caprylate alone or with polyoxyethylene cetyl / stearyl ether. When the SDBS or other alkylaryl sulfonate is used in combination with one or more other surfactants, each surfactant is preferably present in an amount of about 0.05-1.2 wt% based on the dry weight of the synthetic polyisoprene, with the total surfactant package being about 0.4-1.2 wt% based on the dry weight of the polyisoprene. When SDBS or other alkylaryl sulfonates are used in combination with potassium caprylate and polyoxyethylene cetyl / stearyl ether, preferably the polyoxyethylene cetyl / stearyl ether is present in an amount of about 0.1-0.5 wt % based on the dry weight of polyisoprene.
[0042] Accordingly, the present invention provides a surfactant stabilized, prevulcanized synthetic polyisoprene latex composition, wherein a cast and dried film of the synthetic polyisoprene has an expansion of about 130% when immersed in toluene for 20 minutes. The consistency of the coagulum indicates the degree of prevulcanization of the latex. As the latex prevulcanizes, the coagulum becomes less tacky and more brittle. An expansion of about 130% indicates that the synthetic polyisoprene is ready for condom immersion. The prevulcanized synthetic polyisoprene can be stored indefinitely at 20°C to 30°C.
[0043] The pre-vulcanization composition includes potassium caprylate and SDBS or other alkylaryl sulfonate surfactants along with zinc dithiocarbamate and amorphous sulfur extracted by ZDBC. The surfactant-containing latex emulsion wets the synthetic polyisoprene particles, and the catalytic action of the zinc dithiocarbamate extracts the amorphous sulfur. 8 The molecular rings are broken to form linear sulfur chains, which pre-vulcanize the synthetic polyisoprene particles. The post-vulcanization composition has sulfur and other accelerators that cause interparticle crosslinking during the vulcanization cure. Such crosslinking results in a more uniform latex film with higher strength, elongation properties, and crosslink density.
[0044] Preferably, the pre-vulcanization composition comprises (i) a crosslinking package comprising zinc diethyldithiocarbamate or zinc dibutyldithiocarbamate accelerator and sulfur; and (ii) a wetting agent. During pre-vulcanization, sulfur having a ring structure is cleaved by the catalytic action of zinc dithiocarbamate accelerator. The accelerator penetrates into polyisoprene particles and first interacts with the isoprene double bonds therein. Details of the catalytic reactivity of zinc dithiocarbamate are described in the paper "The Mechanism of Zinc(II)-Dithiocarbamate-Accelerated Vulcanization Uncovered; Theoretical and Experimental Evidence" by Nieuwenhuizen, et al., published in J. Am. Chem. Soc., 121 (1), 163-168, 1999. Another publication by Nieuwenhuizen entitled "Zinc accelerator complexes. Versatile homogeneous catalysts in sulfur vulcanization" was published in Applied Catalysis A: General 207 (2001) 55-68. These two publications are related to the use of dithiocarbamate subcomplexes. The mechanism of catalytic action of lead, especially zinc dimethyldithiocarbamate, on sulfur is discussed. The sulfur is captured by four zinc atoms in the promoter molecule and is transferred in and out by catalytic action. In chapter 2.3.1.1 of the book by Professor Garry R. Hamed of the University of Akron, chapter 2 of which is available at the web address files.hanser.de / hanser / docs / 20040401_244515439-6683_3-446-21403-8.pdf, it is stated that for sulfur to be soluble, S 8 It is stated that the sulfur must have a ring structure in order to be soluble. Amorphous or polymeric sulfur is insoluble. In order for the sulfur to diffuse into the synthetic polyisoprene particles, it must be soluble. The same chapter also shows that with ZDBC, only small amounts of sulfur are needed because ZDBC is an ultrafast accelerator. Zhong et al., "Effect of adding pyridine ligand on the structure and properties of complex Zn(S 2 CNBz 2 ) 2 In a web article entitled "Zinc dibenzyldithiocarbamate and zinc dipyridinedithiocarbamate" at http: / / www.chemistrymag.org / cji / 2007 / 097032pe.htm, it is shown that zinc dibenzyldithiocarbamate and zinc dipyridinedithiocarbamate also have similar catalytic activity functionality for sulfur. The wetting agent promotes wetting of polyisoprene particles, and allows the soluble sulfur, whose ring structure has been cleaved by the catalytic action of zinc dithiocarbamate, to contact the surface of the polyisoprene particles, where the penetration of sulfur occurs during a given treatment time. The pre-vulcanized structure of the aqueous latex emulsion is stable at the aqueous latex emulsion holding temperature for a long period of time, for example, for two months, without causing problems of coagulation or instability of the latex emulsion, in contrast to the "pre-curing" procedure of U.S. Patent No. 6,828,387 to Wang, which provides a latex emulsion that is stable for only a maximum of eight days and is unsuitable for condom manufacture.
[0045] Sulfur is preferably present in the synthetic polyisoprene latex emulsion in an amount of about 0.8-1.8 wt% based on the dry weight of polyisoprene. When zinc oxide is used, it is preferably present in an amount of about 0-0.5 wt% based on the dry weight of polyisoprene, while when zinc diethyldithiocarbamate or zinc dibutyldithiocarbamate is used, it is preferably present in an amount of about 0.3-1.0 wt%, more preferably about 0.3-0.45 wt%, based on the dry weight of polyisoprene.
[0046] Examples of suitable wetting agents include, but are not limited to, anionic salts of fatty acids (such as sodium or potassium salts), such as sodium stearate, sodium oleate, and potassium caprylate. Potassium caprylate is advantageously used with salts of short chain fatty acids, SDBS, and polyoxyethylene cetyl / stearyl ether. Potassium caprylate is used in an amount of 0.1 to 0.5 wt % based on the dry weight of polyisoprene.
[0047] The penetration of the components of the pre-vulcanization composition into the polyisoprene particles is strongly related to the particle size and size distribution of the polyisoprene. Typically, small particles have a larger surface area, and the components of the pre-vulcanization composition penetrate these small particles more quickly. However, this large surface area causes the interparticle area to increase compared to the intraparticle area, because the small particles tend to be pre-vulcanized more quickly than the larger particles. That is, the larger particles are not only large particles, but also aggregates of small particles, and are less likely to be pre-vulcanized. On the other hand, the larger particles have a smaller surface area, and the components of the pre-vulcanization composition penetrate these large particles more slowly. The smaller the surface area, the less the interparticle area. Therefore, a delicate balance must be made in the selection of the size and size range distribution of the polyisoprene particles to produce optimal strength properties with a balance of pre-vulcanization intraparticle crosslinking and post-vulcanization interparticle crosslinking. As mentioned above, particles in the range of about 0.2 to 2 micrometers provide optimal results. The penetration of the components of the prevulcanization composition into the polyisoprene particles is also related to the diffusion process itself, which is a linear function of time and reflects a thermal activation process. It is also an exponential function of temperature. Thus, a small increase in temperature during the pre-vulcanization step significantly increases the pre-vulcanization rate. For example, pre-vulcanization at room temperature requires about 12 hours of aging after the mixing process. However, more rapid pre-vulcanization is typically avoided because pre-vulcanization would occur only around large aggregates, compromising the final strength properties of the film, i.e., preventing surface-hardening reactions. The use of potassium caprylate has shown that it promotes the transport of the hardener into the particles and accelerates pre-vulcanization.
[0048] The method includes adding a latex stabilizing composition, such as a composition including a surfactant package of at least one surfactant, such as 15% Hostapur anionic surfactant, present in an amount of about 0.1-0.5 wt %, based on the dry weight of the synthetic polyisoprene. During addition of the latex stabilizing composition, the emulsion is stirred, such as for about 12 hours, to keep the synthetic polyisoprene particles from contacting each other.
[0049] The method further includes adding a post-vulcanization composition to the synthetic polyisoprene latex emulsion along with an accelerator selected from the group consisting of reactive zinc oxide, zinc-containing accelerators: ZDEC, ZBEC, and ZDBC. When reactive zinc oxide is present, it is preferably present in an amount of about 0-0.5 wt %, based on the dry weight of the synthetic polyisoprene. The composition thus produced is stable for up to about 60 days at 25° C. and can be used on the manufacturing line.
[0050] The method also allows for the production of synthetic polyisoprene probe covers that do not contain any nitrosamines, thus minimizing the risk of cancer by preventing transfer of carcinogenic agents to the user.
[0051] Table 1 below shows an example of a pre-vulcanization composition. A typical mixing sequence for the aqueous synthetic latex emulsion is shown. Each step and the time it takes are listed in the table. [Table 1]
[0052] As mentioned above, the present invention further provides a method for forming a synthetic polyisoprene latex condom product. The mold may be any suitable mold known in the art. The method comprises immersing a condom mold in a pre-vulcanized synthetic polyisoprene aqueous latex emulsion composition having a solids content of 40-60% and a viscosity of 20-30 seconds as described above, forming a thin layer of latex film 25-35 microns thick on the surface of the mold in which the individual particles of pre-vulcanized synthetic polyisoprene contact each other. The swelling index in toluene is 100-130% after exposure of a cast disk of synthetic polyisoprene for 20 minutes.
[0053] The first layer of latex membrane is typically 25-35 microns thick and not too soft. The condom former is then dipped again into a pre-vulcanized synthetic polyisoprene emulsion to form a thicker composite latex layer, approximately 45-80 microns thick. This increased thickness of the latex layer helps prevent the condom from tearing when worn.
[0054] The tensile properties of the condoms produced are shown in Table 2 below. [Table 2]
[0055] The nitrosamine content was measured in several samples and is shown in Tables 3A and B below. [Table 3A] [Table 3B]
[0056] FIG. 1 shows the steps involved in the production of nitrosamine-free synthetic polyisoprene latex. It shows a process flow chart for the manufacture of a dip-cured synthetic polyisoprene condom. The process begins with stripping off a previously prepared condom mold. The mold is immersed in a nitric acid bath and then in two acid baths. The mold is then dried in an oven. The mold is then immersed in pre-vulcanized synthetic latex #1 at 20-30° C. and having a total solids content of about 50-55%. The viscosity of said latex is about 18-22 seconds using a Ford cup #4. The thickness of the latex layer formed is about 25-35 microns. The mold coated with the latex layer is dried to ensure that the latex is not too soft. Next, The latex-coated condom former is then dipped into a second pre-vulcanized synthetic latex solution having a solids content of 50-55% and a viscosity of 25-30 seconds on a Ford Cup #6. The second latex dip produces a thicker synthetic latex layer, typically 45-80 microns in total thickness. This thicker layer helps prevent the condom from tearing.
[0057] All references cited herein, including publications, patent applications, and patents, are hereby incorporated by reference to the same extent as if each reference was individually and specifically indicated to be incorporated by reference in its entirety.
[0058] In the context of describing the present invention, the use of "a," "an," and "the" and similar referents (particularly in the context of the claims below) is intended to encompass both the singular and the plural, unless otherwise indicated or clearly contradicted by the context. References to ranges of values herein are intended merely to serve as a shorthand method for referring to each separate value falling within the range, unless otherwise indicated, and each separate value is to be incorporated herein as if it were individually set forth herein. All methods described herein may be performed in any suitable order, unless otherwise indicated herein or clearly contradicted by the context. The use of any and all examples or exemplary language (such as "e.g.," etc.) provided herein is intended merely to further clarify the invention, and is not intended to limit the scope of the invention, unless otherwise indicated. No language in this specification should be construed as indicating that any non-claimed element is essential to the practice of the invention.
Claims
1. A synthetic polyisoprene latex condom product having high stretch and tear resistance, synthesized from a pre-vulcanized synthetic latex emulsion; a. polyisoprene latex particles having a diameter in the range of 0.2 to 2 micrometers; b. sulfur; c. zinc diethyldithiocarbamate; d. zinc dibenzyldithiocarbamate; e. zinc dibutyldithiocarbamate; f. an anionic surfactant selected from the group consisting of alkyl sulfonates, alkylaryl sulfonates, olefin sulfonates, and alcohol sulfonates; and g. water; Including, the pre-vulcanized synthetic latex emulsion has a swelling index of 100% to 130%; The synthetic polyisoprene latex condom has high strength and high stretchability, and emits less than 10 ppb of nitrosamines. Synthetic polyisoprene latex condom products.
2. the anionic surfactant is selected from the group consisting of sodium dodecylbenzenesulfonate, sodium alkyl (C14-17) s-sulfonate, and mixtures thereof; 10. The synthetic polyisoprene latex condom product of claim 1, wherein said pre-vulcanized synthetic latex emulsion comprises said anionic surfactant in an amount of 0.1-0.35 wt %, based on the dry weight of polyisoprene latex particles.
3. 10. The synthetic polyisoprene latex condom product of claim 1, wherein the pre-vulcanized synthetic latex emulsion has a viscosity of 18-22 seconds using a Ford Cup #4, or a viscosity of 25-30 seconds using a Ford Cup #6.
4. 4. The synthetic polyisoprene latex condom product of claim 3, wherein said pre-vulcanized synthetic latex emulsion has a solids content of 40-60%.
5. 5. The pre-vulcanized synthetic latex emulsion according to claim 4, wherein the pre-vulcanized synthetic latex emulsion has a solids content of 50-55%.
2. The synthetic polyisoprene latex condom product according to claim 1 .
6. 10. The synthetic polyisoprene latex condom product of claim 1, wherein said pre-vulcanized synthetic latex emulsion has a Swell Index of 130%.
7. 3. The synthetic polyisoprene latex condom product of claim 2, wherein said pre-vulcanized synthetic latex emulsion comprises sulfur in an amount of 0.8-1.8 wt %, based on the dry weight of polyisoprene latex particles.
8. 8. The synthetic polyisoprene latex condom product of claim 7, wherein said pre-vulcanized synthetic latex emulsion comprises sulfur in an amount of 1.3 wt.%, based on the dry weight of the polyisoprene latex particles.
9. 9. The synthetic polyisoprene latex condom product of claim 8, wherein said pre-vulcanized synthetic latex emulsion comprises zinc diethyldithiocarbamate in an amount of 0.3-1.0 wt % based on the dry weight of polyisoprene latex particles.
10. 10. The synthetic polyisoprene latex condom product of claim 9, wherein said pre-vulcanized synthetic latex emulsion comprises zinc diethyldithiocarbamate in an amount of 0.3-0.45 wt %, based on the dry weight of polyisoprene latex particles.
11. 10. The synthetic polyisoprene latex condom product of claim 9, wherein said pre-vulcanized synthetic latex emulsion comprises zinc dibutyldithiocarbamate in an amount of 0.3-1.0 wt % based on the dry weight of polyisoprene latex particles.
12. 11. The synthetic polyisoprene latex condom product of claim 10, wherein said pre-vulcanized synthetic latex emulsion comprises zinc dibutyldithiocarbamate in an amount of 0.3-0.45 wt %, based on the dry weight of polyisoprene latex particles.
13. 5. The synthetic polyisoprene latex condom product of claim 4 having a thickness of 45 to 80 microns.
14. 14. The synthetic polyisoprene latex condom product of claim 13 having a stretchability of 900%.
15. 10. The synthetic polyisoprene latex condom product of claim 1 having less than 1 ppb nitrosamine emissions.