battery

The battery design addresses the challenge of preventing short circuits during separation by directly connecting electrodes to current collectors without overlap and using insulators, facilitating easy separation and terminal formation for customized batteries.

JP2024132360AActive Publication Date: 2024-10-01MAXELL LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023043094
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-10-01
Estimated Expiration
2043-03-17

AI Technical Summary

Technical Problem

Conventional methods for separating power generation elements from batteries require additional processes or special cutting methods to prevent short circuits, making it difficult to obtain batteries with desired characteristics easily.

Method used

The battery design includes a configuration where positive and negative electrodes are directly connected to current collectors without overlap, with insulators placed between elements to allow easy separation and connection terminals, and ensures a minimum distance between current collectors to prevent short circuits.

Benefits of technology

This design effectively suppresses short circuits during separation and enables easy formation of connection terminals, allowing for batteries with varied characteristics to be obtained without specialized cutting methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132360000001_ABST
    Figure 2024132360000001_ABST
Patent Text Reader

Abstract

To provide a battery which has a plurality of power generation elements that can be used as a battery by being separated, can sufficiently suppress the generation of short circuit during separating the power generation elements, and allows a connection terminal for being connected to an applied apparatus to be easily formed on the separated power generation element, the battery being related to goals 3, 7, 11 and 12 of the SDGs.SOLUTION: In a battery of the present invention, a plurality of power generation elements each having a positive electrode, a negative electrode, and a solid-electrolyte layer arranged between the positive electrode and the negative electrode, are disposed on a substrate. In plan view, a collector connecting the positive electrodes of the power generation elements and a collector connecting the negative electrodes of the power generation elements do not overlap with one another at least in areas where there is no power generation element. In the plan view, the collector for the positive electrodes and the collector for the negative electrodes have a length of 0.5 mm or more in a direction perpendicular to a direction in which adjacent power generation elements are connected to one another. The substrate can be cut in an area where no power generation element is arranged and the insulator is arranged.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a battery having a plurality of power generating elements, which can be separated and used as a battery, which can effectively prevent the occurrence of a short circuit when the power generating elements are separated, and which can easily form connection terminals for connecting the separated power generating elements to applicable equipment. [Background technology]

[0002] In recent years, with the development of portable electronic devices such as mobile phones and notebook personal computers, and the practical application of electric vehicles, there has been a demand for small, lightweight batteries with high capacity and high energy density.

[0003] Currently, lithium batteries that can meet this demand, particularly lithium ion batteries, use lithium-containing composite oxides such as lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2) as the positive electrode active material, graphite or the like as the negative electrode active material, and an organic electrolyte solution containing an organic solvent and a lithium salt as the non-aqueous electrolyte.

[0004] Furthermore, with the further development of devices in which lithium-ion batteries are used, there is a demand for lithium-ion batteries with longer life, higher capacity and higher energy density, as well as a high demand for the reliability of these longer life, higher capacity and higher energy density lithium-ion batteries.

[0005] However, the organic electrolyte used in lithium-ion batteries contains an organic solvent, which is a flammable substance, and therefore the organic electrolyte may generate abnormal heat when an abnormality such as a short circuit occurs in the battery. In addition, with the recent trend toward higher energy density of lithium-ion batteries and an increasing amount of organic solvent in the organic electrolyte, there is a demand for even higher reliability in lithium-ion batteries.

[0006] In the above circumstances, all-solid-state lithium batteries that do not use organic solvents are also being considered. All-solid-state lithium batteries use a molded body of a solid electrolyte that does not use an organic solvent instead of the conventional organic solvent-based electrolyte, and are highly reliable without the risk of abnormal heat generation of the solid electrolyte. Therefore, there are high expectations for them, especially in the product field that requires a high-capacity secondary battery.

[0007] In addition, all-solid-state batteries are not only highly safe, but also highly reliable, highly environmentally resistant, and have a long lifespan, so they are expected to be maintenance-free batteries that can contribute to social development while also continuing to contribute to safety and security. By providing all-solid-state batteries to society, we can contribute to the achievement of Goal 3 (Ensure healthy lives and promote well-being for all at all ages), Goal 7 (Ensure access to affordable, reliable, sustainable and modern energy for all), Goal 11 (Make cities and human settlements inclusive, safe, resilient and sustainable), and Goal 12 (Ensure sustainable consumption and production patterns) out of the 17 Sustainable Development Goals (SDGs) established by the United Nations.

[0008] In addition, in the case of all-solid-state batteries, for example, attempts to increase the capacity are being made by arranging a plurality of battery elements (single cells) each having a positive electrode and a negative electrode with a small area.

[0009] For example, Patent Document 1 proposes an all-solid-state secondary battery in which a thin sheet-like battery element with a relatively small area, in which a positive electrode, a solid electrolyte, and a negative electrode are sequentially laminated, is arranged at specific intervals on a current collector to suppress deterioration of characteristics caused by expansion and contraction of the electrodes and brittle fracture due to impact.

[0010] Various techniques for constructing a battery by arranging multiple small-sized power generating elements (single cells) are being studied for batteries other than all-solid-state batteries. For example, Patent Document 2 proposes a flexible battery in which multiple small-sized batteries are arranged on a flexible substrate.

[0011] There are also proposals for technologies that separate individual power generating elements from a battery having multiple power generating elements and use them individually as batteries (Patent Documents 3 and 4). According to the technologies in Patent Documents 3 and 4, the number of power generating elements according to the desired characteristics can be selected and separated from a battery having many power generating elements, which has the advantage that battery manufacturers do not need to manufacture batteries with different characteristics for each user, and battery users have the advantage that batteries with various characteristics according to the application can be easily obtained from a single product.

[0012] Incidentally, Patent Document 3 describes that when cutting a battery having a required number of power generating elements from a battery having a large number of power generating elements, it is necessary to form an insulator protrusion by reheating and pressurizing the peripheral portion in order to prevent a short circuit due to contact between the positive electrode current collector and the negative electrode current collector in the cut battery.

[0013] On the other hand, Patent Document 4 discloses that separation of power generating elements is performed with laser light, making it possible to prevent short circuits caused by contact between the positive electrode current collector and the negative electrode current collector after separation. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] JP 2001-15153 A [Patent Document 2] JP 2015-15143 A [Patent Document 3] JP 6-215753 A (Patent Claims, paragraph

[0007] ) [Patent Document 4] Japanese Patent Application Publication No. 6-267581 Summary of the Invention [Problem to be solved by the invention]

[0015] As described above, in conventional technology, when some of the power generating elements are separated from a battery having multiple power generating elements and used individually as batteries, a separate process must be carried out after cutting to prevent short circuits after separation (cutting), or a special cutting method (a method using laser light) is required. Therefore, there is still room for improvement in terms of the ease of operation for users to obtain batteries with different characteristics as needed.

[0016] The present invention has been made in consideration of the above-mentioned circumstances, and its object is to provide a battery which has a plurality of power generating elements, which can be separated and used as a battery, which can effectively prevent the occurrence of a short circuit when the power generating elements are separated, and which can easily form connection terminals for connecting the separated power generating elements to an applicable device. [Means for solving the problem]

[0017] The battery of the present invention is configured by enclosing a plurality of power generating elements in an exterior body, the power generating elements having a positive electrode, a negative electrode, and a solid electrolyte layer disposed between the positive electrode and the negative electrode, the positive electrode having a positive electrode mixture layer and a sheet-shaped conductive substrate, the negative electrode having a negative electrode mixture layer and a sheet-shaped conductive substrate, the plurality of power generating elements are arranged on the substrate, and each positive electrode is directly connected to a current collector, thereby connecting the positive electrodes to each other via the current collector, and each negative electrode is directly connected to a current collector, thereby connecting the negative electrodes the positive electrode current collector and the negative electrode current collector do not overlap in a planar view at least in the areas where the power generating elements are not present, the positive electrode current collector and the negative electrode current collector have a length of 0.5 mm or more in a direction perpendicular to the direction connecting the adjacent power generating elements in a planar view, an insulator is disposed in at least a part of the area of ​​the base material where the power generating elements are not disposed, and the base material is cuttable at the areas where the insulator is disposed. Effect of the Invention

[0018] According to the present invention, it is possible to provide a battery having a plurality of power generating elements, which can be separated and used as a battery, which can effectively prevent the occurrence of a short circuit when the power generating elements are separated, and which can easily form connection terminals for connecting the separated power generating elements to an applicable device. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a plan view illustrating a schematic example of a battery of the present invention. [Diagram 2] FIG. 1 is a longitudinal sectional view illustrating a schematic diagram of an example of a battery of the present invention. [Diagram 3] 1 is a cutting example when the power generating element is separated from the battery of the present invention to form individual batteries. [Figure 4] 1 is a diagram for explaining the arrangement of a power generating element, current collectors connecting positive electrodes, and current collectors connecting negative electrodes in a battery of the present invention. [Diagram 5] 1 shows an example of attachment of connection terminals to a battery obtained by separating a power generating element. [Figure 6] 1 is a scanning electron microscope photograph of the surface of an example of a positive electrode having a positive electrode mixture layer and a sheet-like porous metal substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] 1 and 2 are drawings that show a schematic diagram of an example of the battery of the present invention, in which Fig. 1 is a plan view of the battery, and Fig. 2 is a longitudinal sectional view of the battery.

[0021] 1 and 2, a plurality of power generating elements 110 are arranged and enclosed in an exterior body 150. Each power generating element 110 has a positive electrode 120, a negative electrode 130, and a solid electrolyte layer 140 interposed between them.

[0022] The exterior body 150 is composed of base materials 160 and 170. The power generating elements 110 are arranged on the base materials 160 and 170.

[0023] The positive electrode 120 of each power generating element 110 is in contact with the current collector 161, thereby directly connecting the positive electrodes 120 to each other. Although not shown in Fig. 2, the negative electrode 130 of each power generating element 110 is also in contact with a current collector arranged on the lower side of the substrate 170 in the figure, thereby directly connecting the negative electrodes 130 to each other via this current collector.

[0024] In the battery 100 shown in FIG. 2, the positive electrode 120 has a positive electrode mixture layer 121 and a porous metal substrate 122 which is a sheet-like conductive substrate, and the entirety of the porous metal substrate 122, including the end on the positive electrode mixture layer 121 side, is embedded in the positive electrode mixture layer 121. That is, the entirety of the location of the porous metal substrate 122 corresponds to the region where the positive electrode mixture layer and the porous metal substrate coexist. In the positive electrode 120, the end of the porous metal substrate 122 on the opposite side to the positive electrode mixture layer 121 side (the end on the lower side in FIG. 2) is exposed. Note that the dotted line in the positive electrode 120 indicates the boundary between the region in the positive electrode mixture layer 121 where the porous metal substrate does not coexist and the region where the positive electrode mixture layer and the porous metal substrate coexist, and corresponds to the end of the porous metal substrate 122 on the positive electrode mixture layer 121 side.

[0025] Furthermore, in the battery 100 shown in FIG. 2, the negative electrode 130 has a negative electrode mixture layer 131 and a porous metal substrate 132 which is a sheet-like conductive substrate, and the entirety of the porous metal substrate 132, including the end on the negative electrode mixture layer 131 side, is embedded in the negative electrode mixture layer 131. That is, the entirety of the location of the porous metal substrate 132 corresponds to the region where the negative electrode mixture layer and the porous metal substrate coexist. In the negative electrode 130, the end of the porous metal substrate 132 on the opposite side to the negative electrode mixture layer 131 side (the upper end in FIG. 2) is exposed. Note that the dotted line in the negative electrode 130 indicates the boundary between the region in the negative electrode mixture layer 131 where the porous metal substrate does not coexist and the region where the negative electrode mixture layer and the porous metal substrate coexist, and corresponds to the end of the porous metal substrate 132 on the negative electrode mixture layer 131 side.

[0026] In the battery, as shown in FIG. 2, it is preferable that the positive electrode has a positive electrode mixture layer and a sheet-shaped porous metal substrate arranged on the surface of the positive electrode mixture layer, at least a portion of the porous metal substrate of the positive electrode, including the end portion on the positive electrode mixture layer side, is embedded in the positive electrode mixture layer to be integrated with the positive electrode mixture layer, and the other end of the porous metal substrate of the positive electrode is exposed on the surface of the positive electrode, and it is also preferable that the negative electrode has a negative electrode mixture layer and a sheet-shaped porous metal substrate arranged on the surface of the negative electrode mixture layer, at least a portion of the porous metal substrate of the negative electrode, including the end portion on the negative electrode mixture layer side, is embedded in the negative electrode mixture layer to be integrated with the negative electrode mixture layer, and the other end of the porous metal substrate of the negative electrode is exposed on the surface of the negative electrode.

[0027] In a battery (battery module) having multiple power generation elements (unit cells), if the electrodes of the power generation elements are directly connected to each other using current collectors, the electrical connections between the positive electrodes and the negative electrodes tend to become unstable.

[0028] However, when the positive electrode of the power generation element has a positive electrode mixture layer and a sheet-like porous metal substrate arranged on the surface of the positive electrode mixture layer, and at least a portion of the porous metal substrate of the positive electrode, including the end portion on the positive electrode mixture layer side, is embedded in the positive electrode mixture layer and integrated with the positive electrode mixture layer, and the other end portion of the porous metal substrate of the positive electrode is exposed on the surface of the positive electrode, it is possible to achieve good electrical connection between the sheet-like porous metal substrate that functions as a positive electrode current collector in the power generation element and the positive electrode mixture layer, and also good electrical connection between the sheet-like porous metal substrate and a current collector that connects the positive electrodes to each other. In addition, when the negative electrode of the power generation element has a negative electrode mixture layer and a sheet-shaped porous metal substrate arranged on the surface of the negative electrode mixture layer, and at least a part of the porous metal substrate of the negative electrode, including the end on the negative electrode mixture layer side, is embedded in the negative electrode mixture layer and integrated with the negative electrode mixture layer, and the other end of the porous metal substrate of the negative electrode is exposed on the surface of the negative electrode, the electrical connection between the sheet-shaped porous metal substrate that functions as a current collector of the negative electrode in the power generation element and the negative electrode mixture layer, and the electrical connection between the sheet-shaped porous metal substrate and the current collector that connects the negative electrodes together can be improved. Therefore, since the electrical connection between the power generation elements can be improved without individually packaging each power generation element, a battery can be obtained that has higher reliability of electrical connection and can exhibit better characteristics.

[0029] In addition, an insulator 180 is disposed in the region between the power generating elements 110. In the battery 100 shown in Fig. 1, each power generating element is disposed inside a portion indicated by a rectangle with curved corners, and insulators are disposed between the rectangles and inside portions of the exterior body 150 outside the rectangles. The portions of the insulator can be cut, which allows the power generating elements to be separated and used as individual batteries.

[0030] 3 shows an example of cutting when the power generating element is separated from the battery of the present invention to form individual batteries. In the battery, one power generating element can be cut and separated to form an individual battery 200 as shown in the upper left of the figure, or it can be cut and separated to include multiple power generating elements to form battery 201 having multiple power generating elements as shown in the upper right of the figure. In addition, the region including multiple power generating elements can be cut and separated in an L-shape in plan view as in the example in the lower left of the figure to form individual batteries 202, or cut and separated in a square shape in plan view as in the example in the lower right of the figure to form individual batteries 203. Note that in the example in the lower right of the figure, the power generating element cut from the center of the separated battery can also be used as individual batteries 200.

[0031] In this way, in the battery of the present invention, the portion containing one or more power generating elements can be cut at the location where the insulator is arranged inside, depending on the characteristics and shape required for the application device, thereby making it easy to obtain batteries with various characteristics and shapes.

[0032] However, when a portion containing a desired number of power generating elements is cut from a battery containing multiple power generating elements to obtain individual batteries, there is a risk that a short circuit will occur due to the current collector connecting the positive electrodes of the power generating elements and the current collector connecting the negative electrodes of the power generating elements coming into contact near the cut portions.

[0033] Therefore, in the battery of the present invention, the current collectors connecting the positive electrodes of multiple power generation elements and the current collectors connecting the negative electrodes are arranged so that they do not overlap in a planar view, at least in areas where no power generation elements are present.

[0034] Fig. 4 shows a diagram for explaining the arrangement of a plurality of power generating elements, current collectors connecting the positive electrodes of the power generating elements, and current collectors connecting the negative electrodes of the power generating elements. That is, Fig. 4 shows the battery 100 shown in Figs. 1 and 2, for example, with the substrate 170 on the upper side (negative electrode side) in the diagram, which constitutes the exterior body 150, removed so that the inside can be confirmed.

[0035] 4 shows a portion including four power generating elements 110, and insulators are disposed in the region between the dotted line and the end of the substrate 160, and in the region outside the dotted line where the power generating elements 110 are disposed. The region where the insulators are disposed is the portion that can be cut to obtain individual batteries.

[0036] 4, current collector 161 connecting the positive electrodes of multiple power generating elements 110 and current collector 171 connecting the negative electrodes overlap in a plan view only at the locations where power generating elements 110 are present, and do not overlap at locations where power generating elements 110 are not present. Therefore, even if cutting is performed at the location where the insulator is disposed so as to include one or more power generating elements 110, current collector 161 connecting the positive electrodes and current collector 171 connecting the negative electrodes do not overlap in the depth direction in the figure at the cut surface, so there is no risk of contact and short circuit.

[0037] As described above, in the battery of the present invention, the current collectors connecting the positive electrodes of a plurality of power generating elements and the current collectors connecting the negative electrodes of a plurality of power generating elements are arranged so as not to overlap in a planar view, at least in the areas where no power generating elements are present. Therefore, even if the battery is cut at the locations where the insulators are arranged to obtain individual batteries, the current collectors connecting the positive electrodes (the positive electrode side current collector in the case of battery 200 in FIG. 3) and the current collectors connecting the negative electrodes (the negative electrode side current collector in the case of battery 200 in FIG. 3) cannot come into contact with each other on the cut surface. Therefore, even if the battery is cut with a general-purpose cutting means such as a cutter or scissors, the occurrence of a short circuit can be suppressed, and no special operation is required to prevent a short circuit after cutting.

[0038] In addition, the current collectors connecting positive electrodes and the current collectors connecting negative electrodes do not necessarily always overlap in a planar view where the power generating elements are present. For example, in the case of a battery in which multiple power generating elements are arranged in a row, there is no overlapping portion in a planar view between the current collectors connecting positive electrodes and the current collectors connecting negative electrodes.

[0039] In order to use the power generating element separated from the battery as an individual battery, a connection terminal is usually attached to connect it to an applicable device. After the power generating element is separated, such a connection terminal is connected to, for example, the current collector 161 that connects the positive electrodes together, or the current collector 171 that connects the negative electrodes together, as shown in FIG. 4. However, if a thin conductor is used for such a current collector, the attachment point needs to be strictly controlled in order to reliably connect the connection terminal, and if the battery or the connection terminal is misaligned when the connection terminal is attached, there is a risk that the current collector and the connection terminal cannot be connected well. In addition, after the power generating element is separated, the connection terminal is connected from the outside to the current collector located inside the exterior body, which can cause problems such as difficulty in finely adjusting the connection position depending on the situation.

[0040] Therefore, in the battery of the present invention, the length in the direction perpendicular to the direction connecting adjacent power generating elements in a plan view of the current collector connecting the positive electrodes of the power generating elements and the current collector connecting the negative electrodes of the power generating elements is set to 0.5 mm or more, preferably 1 mm or more. The above length means the lengths a and b (in the case of the current collector 161 connecting the positive electrodes) and the lengths c and d (in the case of the current collector 171 connecting the negative electrodes) in FIG. 4. That is, in FIG. 4, the multiple power generating elements 110 are arranged in the horizontal and vertical directions in the figure, and the positive electrodes are connected to each other by the current collector 161, and the negative electrodes are connected to each other by the current collector 171. Therefore, in a plan view, the directions in which adjacent power generating elements are connected are the horizontal and vertical directions indicated by the arrows in the figure, and the lengths of current collectors 161, 171 in the direction perpendicular to the vertical direction are lengths a and c in the figure, and the lengths of current collectors 161, 171 in the direction perpendicular to the horizontal direction are lengths b and d in the figure.

[0041] In this way, when the lengths of the current collectors connecting the positive electrodes and the current collectors connecting the negative electrodes satisfy the above-mentioned values, the current collectors to which the connection terminals are attached have a certain width, so that even if some misalignment occurs, the connection terminals can be satisfactorily attached to the current collectors. This makes it easier to form the connection terminals when separating the power generating elements from the battery to form individual batteries.

[0042] The length of a current collector connecting the positive electrodes of multiple power generating elements and a current collector connecting the negative electrodes of multiple power generating elements in a direction perpendicular to the direction connecting adjacent power generating elements in a planar view depends on the area of ​​the power generating elements in a planar view and the spacing between the power generating elements, but if the length is too long, there is a risk that the effect of suppressing short circuits when the power generating elements are separated to form individual batteries will be reduced, so the length is preferably 40% or less of the width or diameter of the power generating element, and more preferably 30% or less of the width or diameter of the power generating element.

[0043] Fig. 5 shows an example of attachment of connection terminals in an individual battery obtained by separating a power generating element from a battery. In the battery 200 shown in Fig. 5, a connection terminal 190 for a positive electrode and a connection terminal 191 for a negative electrode are disposed outside the exterior body 150, and are joined by joining means 192, 192 to a current collector on the positive electrode side (a current collector that connects the positive electrodes together in the case of a battery having multiple power generating elements) and a current collector on the negative electrode side (a current collector that connects the negative electrodes together in the case of a battery having multiple power generating elements) in the battery 200, respectively.

[0044] As a joining means for joining the connection terminal for the positive electrode and the connection terminal for the negative electrode to the current collector connecting the positive electrodes and the current collector connecting the negative electrodes, for example, a metal needle, an alligator clip (having relatively sharp teeth), a staple, etc., can be used without any particular limitation as long as it can penetrate the exterior body of the battery to join the connection terminal and the current collector and electrically connect the two. In addition, the connection terminal and the current collector may be electrically connected by welding them with an output that is enough to break the exterior body of the part where the connection terminal is arranged.

[0045] In addition, even when the battery is used without separating some of the power generating elements, the connection terminals can be attached in the same manner as the method of attaching them to individual batteries. In addition, when it is planned to use the remaining part as a battery after separating some of the power generating elements, the connection terminals can be provided by connecting one end of the connection terminal to the current collector connecting the positive electrodes and the current collector connecting the negative electrodes inside the exterior body by welding or the like, and drawing the other end of the connection terminal out from the exterior body.

[0046] The battery of the present invention includes a primary battery (all-solid-state primary battery) and a secondary battery (all-solid-state secondary battery). The battery will be described in detail below.

[0047] <Power generation element> The power generating element has a positive electrode, a negative electrode, and a solid electrolyte layer interposed between them.

[0048] (positive electrode) The positive electrode has a positive electrode mixture layer containing a positive electrode active material and the like, and a sheet-like conductive substrate.

[0049] When the battery is a primary battery, the positive electrode active material may be the same as the positive electrode active material used in conventionally known non-aqueous electrolyte primary batteries. Specifically, for example, manganese dioxide, lithium-containing manganese oxide (e.g., LiMn3O6, or a composite oxide having the same crystal structure as manganese dioxide (e.g., β-type, γ-type, or a structure in which β-type and γ-type are mixed) and a Li content of 3.5% by mass or less, preferably 2% by mass or less, more preferably 1.5% by mass or less, and particularly preferably 1% by mass or less), Li a Ti 5 / 3 Examples include lithium-containing composite oxides such as O4 (4 / 3≦a<7 / 3); vanadium oxide; niobium oxide; titanium oxide; sulfides such as iron disulfide; graphite fluoride; silver sulfides such as Ag2S; and nickel oxides such as NiO2.

[0050] In addition, as the positive electrode active material when the battery is the positive electrode of a secondary battery, the same materials as those used in conventional positive electrode active materials for non-aqueous electrolyte secondary batteries and the like can be used. Specifically, LiM r Mn 2-r O4 (where M is at least one element selected from the group consisting of Li, Na, K, B, Mg, Ca, Sr, Ba, Ti, V, Cr, Zr, Fe, Co, Ni, Cu, Zn, Al, Sn, Sb, In, Nb, Ta, Mo, W, Y, Ru, and Rh, and 0 ≦ r ≦ 1), a spinel-type lithium manganese composite oxide represented by Li r Mn (1-s-r) Ni s M t O (2-u) F v (where M is at least one element selected from the group consisting of Co, Mg, Al, B, Ti, V, Cr, Fe, Cu, Zn, Zr, Mo, Sn, Ca, Sr, and W, 0.8 ≦ r ≦ 1.2, 0 < s < 0.5, 0 ≦ t ≦ 0.5, u + v < 1, -0.1 ≦ u ≦ 0.2, 0 ≦ v ≦ 0.1), a layered compound represented by LiCo 1-r M r O2 (where M is at least one element selected from the group consisting of Al, Mg, Ti, V, Cr, Zr, Fe, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, and Ba, and 0 ≦ r ≦ 0.5), a lithium cobalt composite oxide represented by LiNi 1-r M r O2 (where M is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Fe, Co, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, and Ba, and 0 ≦ r ≦ 0.5), a lithium nickel composite oxide represented by Li 1+s M 1-r N r PO4F s (where M is at least one element selected from the group consisting of Fe, Mn, and Co, and N is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, V, and Ba, and 0 ≦ r ≦ 0.5, 0 ≦ s ≦ 1), an olivine-type composite oxide represented by Li2M 1-r Nr Examples of the positive electrode active materials include one or more of various positive electrode active materials used in conventionally known nonaqueous electrolyte secondary batteries, such as a pyrophosphate compound represented by P2O7 (wherein M is at least one element selected from the group consisting of Fe, Mn, and Co, and N is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, V, and Ba, and 0≦r≦0.5).

[0051] In the case where the battery is a secondary battery, the average particle size of the positive electrode active material is preferably 1 μm or more, more preferably 2 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less. The positive electrode active material may be either primary particles or secondary particles formed by agglomeration of primary particles. When a positive electrode active material having an average particle size in the above range is used, a large interface with the solid electrolyte contained in the positive electrode can be obtained, and therefore the output characteristics of the battery are further improved.

[0052] The average particle diameter of various particles (positive electrode active material, solid electrolyte, etc.) in this specification is the 50% diameter value (D) in the volume-based integrated fraction when calculating the integral volume from small particles using a particle size distribution measurement device (such as the Microtrac particle size distribution measurement device "HRA9320" manufactured by Nikkiso Co., Ltd.). 50 )

[0053] When the battery is a secondary battery, the positive electrode active material preferably has a reaction suppression layer on its surface for suppressing reaction with the solid electrolyte contained in the positive electrode.

[0054] In the positive electrode mixture layer, if the positive electrode active material and the solid electrolyte come into direct contact with each other, the solid electrolyte may be oxidized to form a resistance layer, which may reduce the ionic conductivity in the positive electrode mixture layer. By providing a reaction suppression layer that suppresses the reaction with the solid electrolyte on the surface of the positive electrode active material and preventing direct contact between the positive electrode active material and the solid electrolyte, it is possible to suppress the reduction in the ionic conductivity in the positive electrode mixture layer due to the oxidation of the solid electrolyte.

[0055] The reaction suppression layer may be made of a material that has ion conductivity and can suppress the reaction between the particles of the electrode active material (positive electrode active material) and the solid electrolyte. Examples of materials that can form the reaction suppression layer include oxides containing Li and at least one element selected from the group consisting of Nb, P, B, Si, Ge, Ti, Zr, Ta, and W, more specifically, Nb-containing oxides such as LiNbO3, Li3PO4, Li3BO3, Li2SO4, Li4SiO4, Li4GeO4, LiTiO3, LiZrO3, and Li2WO4. The reaction suppression layer may contain only one of these oxides, or may contain two or more of them, and further, a plurality of these oxides may form a composite compound. Among these oxides, it is preferable to use an Nb-containing oxide, and it is more preferable to use LiNbO3.

[0056] The reaction suppression layer is preferably present on the surface in an amount of 0.1 to 1.0 part by mass per 100 parts by mass of the positive electrode active material, in order to effectively suppress the reaction between the positive electrode active material and the solid electrolyte.

[0057] Methods for forming a reaction suppression layer on the surface of a positive electrode active material include the sol-gel method, the mechanofusion method, the CVD method, the PVD method, and the ALD method.

[0058] The content of the positive electrode active material in the positive electrode mixture is preferably 60 to 85 mass % from the viewpoint of increasing the energy density of the battery.

[0059] The positive electrode mixture may contain a conductive assistant. Specific examples include carbon materials such as graphite (natural graphite, artificial graphite), graphene, carbon black, carbon nanofibers, and carbon nanotubes. For example, when Ag2S is used as the active material, conductive Ag is generated during the discharge reaction, so the conductive assistant may not be included. When the positive electrode mixture contains a conductive assistant, the content is preferably 1.0 part by mass or more, preferably 7.0 parts by mass or less, and more preferably 6.5 parts by mass or less, when the content of the positive electrode active material is 100 parts by mass.

[0060] The positive electrode mixture may contain a binder. Specific examples of such binders include fluororesins such as polyvinylidene fluoride (PVDF). In addition, the positive electrode mixture may not contain a binder if good moldability can be ensured in forming the positive electrode mixture layer without using a binder, such as when a sulfide-based solid electrolyte is contained in the positive electrode mixture (described in detail later).

[0061] When the positive electrode mixture requires a binder, the content is preferably 15% by mass or less, and more preferably 0.5% by mass or more. On the other hand, when the positive electrode mixture requires no binder and can obtain moldability, the content is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and even more preferably 0% by mass (i.e., no binder is contained).

[0062] The positive electrode mixture may contain a solid electrolyte.

[0063] The solid electrolyte contained in the positive electrode mixture is not particularly limited as long as it has lithium ion conductivity. For example, a sulfide-based solid electrolyte, a hydride-based solid electrolyte, a halide-based solid electrolyte, an oxide-based solid electrolyte, etc. can be used.

[0064] Examples of sulfide-based solid electrolytes include particles of Li2S-P2S5, Li2S-SiS2, Li2S-P2S5-GeS2, and Li2S-B2S3-based glass. In addition, thio-LISICON-type electrolytes [Li 10 GeP2S 12 , Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 Li 12-12a-b+c+6d-e M 1 3+a-b-c-d M 2 b M 3 c M 4 d M 5 12-e X e (However, M 1 is Si, Ge or Sn, M 2 is P or V, M 3 is Al, Ga, Y or Sb, M 4 is Zn, Ca, Ba, M 5 is either S or S and O, and X is F, Cl, Br or I, 0≦a<3, 0≦b+c+d≦3, 0≦e≦3], or those having an argyrodite type crystal structure can also be used.

[0065] Examples of hydride-based solid electrolytes include LiBH4, solid solutions of LiBH4 and the following alkali metal compounds (for example, those in which the molar ratio of LiBH4 to the alkali metal compound is 1:1 to 20:1), etc. Examples of the alkali metal compounds in the solid solutions include at least one selected from the group consisting of lithium halides (LiI, LiBr, LiF, LiCl, etc.), rubidium halides (RbI, RbBr, RbF, RbCl, etc.), cesium halides (CsI, CsBr, CsF, CsCl, etc.), lithium amide, rubidium amide, and cesium amide.

[0066] Examples of halide-based solid electrolytes include monoclinic LiAlCl4, defective spinel-type or layered-structured LiInBr4, and monoclinic Li 6-3m Y m X6 (where 0 < m < 2 and X = Cl or Br), etc. In addition, for example, known ones described in International Publication No. 2020 / 070958 and International Publication No. 2020 / 070955 can also be used.

[0067] Examples of oxide-based solid electrolytes include Li2O-Al2O3-SiO2-P2O5-TiO2-based glass ceramics, Li2O-Al2O3-SiO2-P2O5-GeO2-based glass ceramics, Li3PO4-Li3BO3-Li2SO4-based glass, garnet-type Li7La3Zr2O 12 、NASICON-type Li 1+O Al 1+O Ti 2-O (PO4)3, Li 1+p Al 1+p Ge 2-p (PO4)3, perovskite-type Li 3q La 2 / 3-q TiO3, inverse perovskite-type Li3HX (X = O, S, Se, Te), etc.

[0068] Among these solid electrolytes, sulfide-based solid electrolytes are preferred because of their high lithium ion conductivity. Sulfide-based solid electrolytes containing Li and P are more preferred. Sulfide-based solid electrolytes having an argyrodite-type crystal structure are even more preferred because they have higher lithium ion conductivity and higher chemical stability.

[0069] Examples of sulfide-based solid electrolytes having an argyrodite-type crystal structure include those represented by the following general composition formula (1) or the following general composition formula (2), such as Li6PS5Cl, which are particularly preferred.

[0070] Li 7-x+y PS 6-x Cl x+y (1)

[0071] In the general composition formula (1), 0.05≦y≦0.9 and −3.0x+1.8≦y≦−3.0x+5.7.

[0072] Li 7-a P.S. 6-a Cl b Br c (2)

[0073] In the general composition formula (2), a=b+c, ​​0 <a≦1.8、0.1≦b / c≦10.0である。

[0074] The average particle size of the solid electrolyte is preferably 0.1 μm or more, and more preferably 0.2 μm or more, from the viewpoint of reducing grain boundary resistance, while it is preferably 10 μm or less, and more preferably 5 μm or less, from the viewpoint of forming a sufficient contact interface between the active material and the solid electrolyte.

[0075] The content of the solid electrolyte in the positive electrode mixture is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, when the content of the positive electrode active material is 100 parts by mass, from the viewpoint of further increasing the ion conductivity in the positive electrode and further improving the output characteristics of the battery. However, if the amount of the solid electrolyte in the positive electrode mixture is too large, the amount of other components may be reduced, and the effects of these components may be reduced. Therefore, the content of the solid electrolyte in the positive electrode mixture is preferably 65 parts by mass or less, more preferably 60 parts by mass or less, when the content of the positive electrode active material is 100 parts by mass.

[0076] The sheet-shaped conductive substrate of the positive electrode functions as a current collector for the positive electrode. As the sheet-shaped conductive substrate of the positive electrode, a mesh, foil, expanded metal, punched metal, or carbon sheet or mesh can be used, but a sheet-shaped porous metal substrate is preferably used.

[0077] It is preferable to use a foamed metal porous body as the sheet-like porous metal substrate in the positive electrode. A specific example of a foamed metal porous body is "Celmet (registered trademark)" by Sumitomo Electric Industries, Ltd. In addition, such a porous metal substrate usually has a thickness before use in a positive electrode that is greater than the above-mentioned thickness (thickness in the positive electrode) (for example, the thickness before compression is preferably 0.1 mm or more, more preferably 0.3 mm or more, and particularly preferably 0.5 mm or more, while it is preferably 3 mm or less, more preferably 2 mm or less, and particularly preferably 1.5 mm or less), and is compressed in the thickness direction during the production of a power generating element described later, so that the thickness becomes a value described later.

[0078] The porosity of the porous metal substrate before compression is preferably 80% or more, more preferably 90% or more, and particularly preferably 95% or more, so that the porous metal substrate and the positive electrode mixture layer can be easily integrated in the process of pressing the porous metal substrate and the positive electrode mixture, while the amount of the substrate is kept constant or more to increase the conductivity, the porosity is preferably 99.5% or less, more preferably 99% or less, and particularly preferably 98.5% or less.

[0079] In the positive electrode, the thickness of the portion of the porous metal substrate that is embedded in the positive electrode mixture layer is preferably 10% or more, and more preferably 20% or more, of the thickness of the porous metal substrate (the thickness of the entire porous metal substrate, including the thickness of the portion where the positive electrode mixture layer coexists; unless otherwise specified, the same applies hereinafter to the thickness of the porous metal substrate) from the viewpoint of more reliably integrating the porous metal substrate and the positive electrode mixture layer.

[0080] In addition, in order to reduce the resistance when the positive electrode is in contact with a current collector for connecting the positive electrodes of a plurality of power generating elements, it is desirable that the end of the porous metal substrate opposite to the positive electrode mixture layer side is not embedded in the positive electrode mixture layer, and the end of the positive electrode (the surface of the positive electrode) is composed only of the porous metal substrate. That is, when the porous metal substrate is compressed in the thickness direction during the production of the power generating element described later, it is desirable that the pores at the end of the porous metal substrate are crushed and disappear, and only the porous metal substrate is exposed on the surface of the positive electrode. However, some of the pores at the end of the porous metal substrate may not be crushed and may be filled with the positive electrode mixture, and a part of the positive electrode mixture may be exposed on the surface of the positive electrode together with the end of the porous metal substrate, as long as it does not significantly affect the contact resistance with the current collector.

[0081] A scanning electron microscope (SEM) photograph of the surface of an example of a positive electrode is shown in Fig. 6. In the surface of the positive electrode shown in Fig. 6, the end of the porous metal substrate 122 is exposed, and a part of the positive electrode mixture 121a is also exposed on the surface of the positive electrode by entering into the pores present at the end of the porous metal substrate.

[0082] However, since the greater the proportion (area ratio) of the positive electrode mixture exposed on the surface of the positive electrode, the greater the contact resistance between the porous metal substrate and the current collector for connecting the positive electrodes of multiple power generating elements to each other, it is desirable to set the proportion of the area of ​​the exposed positive electrode mixture on the positive electrode surface to 50% or less in a plan view, more desirably 25% or less, even more desirably 15% or less, and particularly desirably 10% or less.

[0083] In the positive electrode, when at least a part of the porous metal substrate is embedded in the positive electrode mixture layer, from the viewpoint of more reliably integrating the porous metal substrate and the positive electrode mixture layer, the thickness of the porous metal substrate is preferably 1% or more, more preferably 2% or more, and particularly preferably 3% or more of the total thickness of the positive electrode mixture layer (including the thickness of the portion coexisting with the porous metal substrate. In the following, when the positive electrode has a sheet-shaped porous metal substrate, unless otherwise specified, the "thickness of the positive electrode mixture layer" means the "total thickness of the positive electrode mixture layer" here.) of the total thickness of the positive electrode mixture layer. In addition, from the viewpoint of improving the filling property of the positive electrode mixture layer in the positive electrode, the thickness of the porous metal substrate is preferably 30% or less, more preferably 20% or less, and particularly preferably 10% or less of the thickness of the positive electrode mixture layer.

[0084] In the positive electrode, the thickness of the porous metal substrate is preferably 10 μm or more, more preferably 20 μm or more, and particularly preferably 30 μm or more, while it is preferably 300 μm or less, more preferably 200 μm or less, and particularly preferably 100 μm or less.

[0085] The thickness of the positive electrode mixture layer is preferably 0.2 mm or more, more preferably 0.5 mm or more, and particularly preferably 0.7 mm or more, while it is preferably 3 mm or less, more preferably 2.5 mm or less, and particularly preferably 2 mm or less.

[0086] The thickness of the porous metal substrate, the thickness of the positive electrode mixture layer, and the thickness of the negative electrode mixture layer described later are determined by the maximum width in the thickness direction of the region where the porous metal substrate can be confirmed and the region where the positive electrode mixture or the negative electrode mixture can be confirmed in an image obtained by observing the cross section of the thickness direction of the positive electrode or the negative electrode by SEM at a magnification of 50 to 1000 times. The thickness of the part of the porous metal substrate embedded in the positive electrode mixture layer or the negative electrode mixture layer is determined by the maximum width in the thickness direction of the part where the region where the porous metal substrate can be confirmed overlaps with the region where the positive electrode mixture or the region where the negative electrode mixture can be confirmed (each value in the examples described later is determined by these methods).

[0087] The proportion (area ratio) of the positive electrode mixture exposed on the surface of the positive electrode and the proportion (area ratio) of the negative electrode mixture exposed on the surface of the negative electrode are determined by the ratio (A / B) of the total area A of the exposed parts of the positive electrode mixture or the negative electrode mixture to the area B of the entire positive electrode or negative electrode in an image obtained by observing the surface of the positive electrode or the negative electrode with an SEM at a magnification of 50 to 200 times (the values ​​in the examples described later are determined by this method).

[0088] (Negative electrode) The negative electrode has, for example, a negative electrode mixture layer containing a negative electrode active material and the like, and a sheet-like conductive substrate.

[0089] Examples of the negative electrode active material include carbon materials such as graphite, lithium titanium oxides (lithium titanate, etc.), simple substances containing elements such as Si and Sn, compounds (oxides, etc.), and alloys thereof, etc. In addition, lithium metal and lithium alloys (lithium-aluminum alloys, lithium-indium alloys, etc.) can also be used as the negative electrode active material.

[0090] The content of the negative electrode active material in the negative electrode mixture is preferably 40 to 80 mass % from the viewpoint of increasing the energy density of the battery.

[0091] The negative electrode mixture may contain a conductive assistant. Specific examples thereof include the same conductive assistants as those exemplified above as those that may be contained in the positive electrode mixture. The content of the conductive assistant in the negative electrode mixture is preferably 10 to 30 parts by mass when the content of the negative electrode active material is 100 parts by mass.

[0092] In addition, the negative electrode mixture may contain a binder. Specific examples thereof include the same binders as those exemplified above as those that may be contained in the positive electrode mixture. Note that, for example, in the case where a sulfide-based solid electrolyte is contained in the negative electrode mixture (described later), if good moldability can be ensured in forming the negative electrode mixture layer without using a binder, the negative electrode mixture may not contain a binder.

[0093] In the case where the negative electrode mixture requires a binder, the content is preferably 15% by mass or less, and more preferably 0.5% by mass or more. On the other hand, in the case where the negative electrode mixture requires no binder and can obtain moldability, the content is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and even more preferably 0% by mass (i.e., no binder is contained).

[0094] The negative electrode mixture can contain a solid electrolyte. Specific examples thereof include the same solid electrolytes as those exemplified above as those that can be contained in the positive electrode mixture. Among the above-mentioned solid electrolytes, it is preferable to use a sulfide-based solid electrolyte because it has high lithium ion conductivity and also has a function of increasing the moldability of the negative electrode mixture, and it is more preferable to use a sulfide-based solid electrolyte having an argyrodite-type crystal structure, and it is even more preferable to use one represented by the general composition formula (1) or the general composition formula (2).

[0095] For the same reasons as in the case of the positive electrode mixture, the average particle size of the solid electrolyte in the negative electrode mixture is preferably 0.1 μm or more, and more preferably 0.2 μm or more, and is preferably 10 μm or less, and more preferably 5 μm or less.

[0096] The content of the solid electrolyte in the negative electrode mixture is preferably 30 parts by mass or more, more preferably 35 parts by mass or more, when the content of the negative electrode active material is 100 parts by mass, from the viewpoint of further increasing the ion conductivity in the negative electrode and further improving the output characteristics of the battery. However, if the amount of the solid electrolyte in the negative electrode mixture is too large, the amount of other components may be reduced, and the effects of these components may be reduced. Therefore, the content of the solid electrolyte in the negative electrode mixture is preferably 130 parts by mass or less, more preferably 110 parts by mass or less, when the content of the negative electrode active material is 100 parts by mass.

[0097] The sheet-like conductive substrate of the negative electrode functions as a current collector for the negative electrode. As the sheet-like conductive substrate of the negative electrode, a metal mesh, foil, expanded metal, punched metal, or carbon sheet or mesh can be used, but a sheet-like porous metal substrate is preferably used.

[0098] For the sheet-like porous metal substrate in the negative electrode, it is preferable to use a foamed metal porous body, as in the positive electrode. A specific example of a foamed metal porous body is "Celmet (registered trademark)" by Sumitomo Electric Industries, Ltd. In addition, such a porous metal substrate usually has a thickness before being used for a negative electrode that is larger than the thickness (thickness in the negative electrode) (for example, the thickness before being compressed is preferably 0.1 mm or more, more preferably 0.3 mm or more, and particularly preferably 0.5 mm or more, while it is preferably 3 mm or less, more preferably 2 mm or less, and particularly preferably 1.5 mm or less). During the manufacture of the negative electrode described later, it is compressed in the thickness direction, and the thickness becomes the value described later.

[0099] The porosity of the porous metal substrate before compression is preferably 80% or more, more preferably 90% or more, and particularly preferably 95% or more, so that the porous metal substrate and the negative electrode mixture layer can be easily integrated in the process of pressing the porous metal substrate and the negative electrode mixture, while the amount of the substrate is kept constant or more to increase the conductivity, the porosity is preferably 99.5% or less, more preferably 99% or less, and particularly preferably 98.5% or less.

[0100] In the negative electrode, the thickness of the portion of the porous metal substrate that is embedded in the negative electrode mixture layer is preferably 10% or more, and more preferably 20% or more, of the thickness of the porous metal substrate (the thickness of the entire porous metal substrate, including the thickness of the portion where the negative electrode mixture layer coexists; unless otherwise specified, the same applies hereinafter to the thickness of the porous metal substrate) from the viewpoint of more reliably integrating the porous metal substrate and the negative electrode mixture layer.

[0101] In addition, in order to reduce the resistance when the negative electrode is in contact with a current collector for connecting the negative electrodes, it is desirable that the end of the porous metal substrate opposite to the negative electrode mixture layer side is not embedded in the negative electrode mixture layer, and the end of the negative electrode (surface of the negative electrode) is composed only of the porous metal substrate. That is, when the porous metal substrate is compressed in the thickness direction during the production of the negative electrode described later, it is desirable that the pores at the end of the porous metal substrate are crushed and disappear, and only the porous metal substrate is exposed on the surface of the negative electrode. However, some of the pores at the end of the porous metal substrate may not be crushed and may be filled with the negative electrode mixture, and a part of the negative electrode mixture may be exposed on the surface of the negative electrode together with the end of the porous metal substrate, as long as it does not significantly affect the contact resistance with the current collector.

[0102] However, since the greater the proportion (area ratio) of the negative electrode mixture exposed on the surface of the negative electrode, the greater the contact resistance between the porous metal substrate and the current collector for connecting the negative electrodes to each other, it is desirable to set the proportion of the area of ​​the exposed negative electrode mixture on the negative electrode surface to 50% or less in a plan view, more desirably 25% or less, even more desirably 15% or less, and particularly desirably 10% or less.

[0103] In the negative electrode, when at least a part of the porous metal substrate is embedded in the negative electrode mixture layer, from the viewpoint of more reliably integrating the porous metal substrate and the negative electrode mixture layer, the thickness of the porous metal substrate is preferably 1% or more, more preferably 2% or more, and particularly preferably 3% or more of the total thickness of the negative electrode mixture layer (including the thickness of the portion coexisting with the porous metal substrate. In the following, when the negative electrode has a sheet-shaped porous metal substrate, unless otherwise specified, the "thickness of the negative electrode mixture layer" means the "total thickness of the negative electrode mixture layer" here.) of the total thickness of the negative electrode mixture layer. In addition, from the viewpoint of increasing the filling property of the negative electrode mixture layer in the negative electrode, the thickness of the porous metal substrate is preferably 30% or less, more preferably 20% or less, and particularly preferably 10% or less of the thickness of the negative electrode mixture layer.

[0104] In the negative electrode, the thickness of the porous metal substrate is preferably 10 μm or more, more preferably 20 μm or more, and particularly preferably 30 μm or more, while it is preferably 300 μm or less, more preferably 200 μm or less, and particularly preferably 100 μm or less.

[0105] The thickness of the negative electrode mixture layer is preferably 0.2 mm or more, more preferably 0.5 mm or more, and particularly preferably 0.7 mm or more, while it is preferably 4 mm or less, more preferably 3.5 mm or less, and particularly preferably 3 mm or less.

[0106] (solid electrolyte layer) In the power generating element, a solid electrolyte layer is interposed between the positive electrode and the negative electrode. Specific examples of the solid electrolyte constituting the solid electrolyte layer include the same solid electrolytes as those exemplified above as those that can be contained in the positive electrode mixture. Among the above-mentioned solid electrolytes, it is preferable to use a sulfide-based solid electrolyte because it has high lithium ion conductivity and has a function of improving moldability, and it is more preferable to use a sulfide-based solid electrolyte having an argyrodite-type crystal structure, and it is even more preferable to use one represented by the general composition formula (1) or the general composition formula (2).

[0107] The solid electrolyte layer may have a porous body such as a resin nonwoven fabric as a support.

[0108] The thickness of the solid electrolyte layer is preferably 10 to 200 μm.

[0109] (Manufacturing method of power generating element) The power generating element can be manufactured by a manufacturing method including, for example, a step of press-molding a powdered positive electrode mixture to form the positive electrode mixture layer, a step of press-molding a powdered solid electrolyte to form a solid electrolyte layer, and a step of press-molding a powdered negative electrode mixture to form the negative electrode mixture layer.

[0110] For example, in the case of a power generating element having a positive electrode and a negative electrode each having a sheet-like porous metal substrate, a more specific manufacturing method includes, for example, a manufacturing method including the following first to third steps.

[0111] In the first step, a powdered electrode mixture (positive electrode mixture or negative electrode mixture) is charged into a metal mold and pressure-molded. The surface pressure of the pressure molding in the first step is preferably, for example, 30 to 500 MPa.

[0112] In the next step 2, a porous metal substrate is placed on the electrode mixture formed by pressure molding in step 1, and then in the next step 3, the electrode mixture and the porous metal substrate are pressed together. By pressing in this step 3, the electrode mixture is further compressed while the porous metal substrate is embedded in the electrode mixture from the end on the electrode mixture side, and the porous metal substrate is compressed in the thickness direction, so that the electrode mixture layer (positive electrode mixture layer or negative electrode mixture layer) and the porous metal substrate are integrated to form an electrode (positive electrode or negative electrode).

[0113] As described above, in this third step, the porous metal substrate is compressed in the thickness direction, and the degree of compression is preferably 30% or less, more preferably 20% or less, and particularly preferably 10% or less of the thickness before compression from the viewpoint of more reliably bonding the porous metal substrate and the electrode mixture layer. Also, from the viewpoint of retaining a certain amount or more of the electrode mixture in the voids of the porous metal substrate and increasing the bonding strength between the porous metal substrate and the electrode mixture layer, the thickness of the porous metal substrate compressed in the third step is preferably 1% or more, more preferably 2% or more of the thickness before compression.

[0114] The surface pressure during the pressurization in the third step is preferably 800 MPa or more, more preferably 1000 MPa or more, and particularly preferably 1200 MPa or more, for example, in order to compress and mold the electrode mixture and sufficiently increase the density of the electrode mixture layer. Although the upper limit of the surface pressure during the pressurization in the third step is not particularly specified, the upper limit is usually about 2000 MPa in a general pressurization device.

[0115] By going through the first to third steps, it is possible to obtain an electrode (positive or negative electrode) in which at least a portion of the porous metal substrate, including the end thereof on the electrode mixture layer side (a certain range in the thickness direction from the end of the porous metal substrate), is embedded in the electrode mixture layer and integrated with the electrode mixture layer, and the other end of the porous metal substrate is exposed on the surface of the electrode.

[0116] In addition, if the surface pressure during the application of pressure in the third step becomes too high, cracks may occur when the porous metal substrate is compressed. However, even if the substrate is broken into pieces, these pieces can contribute to reducing the contact resistance as long as the ends of the pieces are exposed on the surface of the electrode.

[0117] The positive and negative electrodes are prepared through the above-mentioned first, second and third steps, and are then arranged on both sides of the solid electrolyte layer, and if necessary, pressurized to form a power generating element.

[0118] Furthermore, before the first step, a preliminary step of putting a powdered solid electrolyte into a die and pressure-molding it can be provided, and an electrode mixture (positive electrode mixture or negative electrode mixture) can be placed on the solid electrolyte pressure-molded in this preliminary step. Then, the first step, the second step, and the third step can be carried out in sequence to produce an integrated product of the solid electrolyte layer and the electrode (positive electrode or negative electrode), which can be used as a power generation element.

[0119] The surface pressure during pressure molding in the preliminary step is preferably, for example, 30 to 120 MPa.

[0120] In addition, a power generating element can also be manufactured by forming one of a positive electrode and a negative electrode on one side of a solid electrolyte layer through a preliminary step, a first step, a second step, and a third step, and then sequentially carrying out the first step, the second step, and the third step on the other side of the solid electrolyte layer to form the other electrode (negative electrode or positive electrode).

[0121] (Layer structure of power generating element) The power generating element may have one positive electrode and one negative electrode, which are laminated with a solid electrolyte layer interposed therebetween, or may have a plurality of positive electrodes and a plurality of negative electrodes. In the case of a power generating element having a plurality of positive electrodes and a plurality of negative electrodes, for example, a plurality of unit laminate bodies, each having one positive electrode and one negative electrode laminated with a solid electrolyte layer interposed therebetween, may be laminated. When laminating the unit laminate bodies, for example, a method of laminating the positive electrode of one unit laminate body and the negative electrode of the other unit laminate body with a current collector such as a metal foil may be employed. In addition, a power generating element having a plurality of positive electrodes and a plurality of negative electrodes may be formed by using a bipolar electrode in which a positive electrode and a negative electrode are laminated with a metal foil or the like, laminating a negative electrode on the positive electrode side of this bipolar electrode with a solid electrolyte layer interposed therebetween, and laminating a positive electrode on the negative electrode side of the bipolar electrode with a solid electrolyte layer interposed therebetween.

[0122] (Shape of power generating element) The shape of the power generating element in a plan view is not particularly limited and may be any of a circle, an ellipse, a rectangle, a hexagon, or other polygon, but is usually a circle or a rectangle.

[0123] (Layout and number of power generating elements) In a battery, depending on the planar shape of the exterior body, multiple power generating elements can be arranged in a single linear row, or as shown in Figure 1, in multiple vertical and horizontal rows, in a single circular row, or in multiple concentric circular rows.

[0124] The number of power generating elements to be placed in the battery is not particularly limited as long as it is multiple, i.e., two or more, and can be selected appropriately depending on the characteristics required for the application of the battery; for example, it is possible to have 10, 100, 1000 or more.

[0125] <Substrate, current collector and exterior body> The substrate on which the power generating elements are arranged may be an insulating sheet-like material (such as a film, woven fabric, or nonwoven fabric that is substantially free of pores). The substrate is preferably flexible. By using a flexible substrate, a so-called flexible battery can be obtained. For example, the battery can be wound into a roll for storage or transportation, or can be used as a battery that can be deformed to fit the application location, such as a battery that can be placed on a curved surface.

[0126] Examples of materials for such substrates include resins such as nylon (eg, nylon 66), polyester (eg, polyethylene terephthalate (PET)), polyolefin (eg, polypropylene, polyethylene), polyurethane, epoxy, and polyimide.

[0127] The thickness of the substrate is preferably 1 to 100 μm.

[0128] The current collectors connecting the positive electrodes of the power generating elements and the current collectors connecting the negative electrodes of the power generating elements must have a shape in plan view that prevents them from overlapping at least in areas where the power generating elements are not present when the battery is viewed from above. For example, the shape of the current collector in plan view may be a shape in which a part is cut out of a foil (plate), such as a lattice shape as shown in Fig. 4. Alternatively, the current collector may be a lattice shape in which elongated foil (plate) pieces are arranged horizontally and vertically.

[0129] For the current collectors that connect positive electrodes together and the current collectors that connect negative electrodes together, metal foils (plates) such as stainless steel, nickel, aluminum, iron, copper, clad materials that combine these, and materials obtained by plating these materials with nickel, chrome, nickel chrome, etc. can be used.

[0130] The thickness of the current collector made of a metal foil (plate) is preferably 10 to 100 μm.

[0131] In addition, a battery may use a substrate having an insulating layer and a conductive layer, and the conductive layer may function as a current collector that connects the positive electrodes and the negative electrodes of a plurality of power generating elements to each other.

[0132] The insulating layer in the substrate having an insulating layer and a conductive layer may be an insulating sheet-like material (such as a substantially pore-free film, woven fabric, or nonwoven fabric) made of the material exemplified above as the substrate on which the power generating elements are arranged. The thickness of the insulating layer is preferably 1 to 100 μm.

[0133] In addition, the conductive layer in the base material having an insulating layer and a conductive layer may be a metal foil that can be used for the current collector, etc. The thickness of the conductive layer is preferably 10 to 100 μm.

[0134] In a base material having an insulating layer and a conductive layer, the insulating layer and the conductive layer may simply be stacked on top of each other, but it is preferable that the insulating layer and the conductive layer are bonded to each other.

[0135] When the positive electrode of the power generating element has a porous metal substrate, the porous metal substrate and the current collector connecting the positive electrodes may simply be in contact with each other or may be welded to each other. When the negative electrode of the power generating element has a porous metal substrate, the porous metal substrate and the current collector connecting the negative electrodes may simply be in contact with each other or may be welded to each other.

[0136] With regard to the exterior body of the battery, from the viewpoint of being able to cut at the location where the internal insulating layer is located, an exterior body that can be easily cut, such as one made of a resin film or one made of a laminate film having a metal layer on the surface of a resin film, is used.

[0137] In the case of an exterior body made of a resin film, the resin film can be the same as a film having substantially no pores among resin sheet-like materials usable as an insulating layer in a base material having an insulating layer and a conductive layer. Also, the laminate film constituting the exterior body can be the same as the base material having an insulating layer and a conductive layer.

[0138] The exterior body can also be formed from a base material having an insulating layer and a conductive layer. That is, the exterior body can be formed by sealing the outer periphery edges of two base materials on which the power generating elements are arranged by bonding them together.

[0139] The substrates for forming the exterior body can be bonded together by heat fusion via an ionomer resin, etc. As the ionomer resin, for example, "Himilan (ethylene-based ionomer resin, product name)" manufactured by Dow Mitsui Polychemicals can be used.

[0140] There are no particular limitations on the shape of the exterior body in a plan view, and it may be a polygon such as a rectangle, a circle, or the like.

[0141] <Connection terminal> The connection terminal for connecting the battery to the applicable device can be made of a metal plate such as stainless steel, nickel, aluminum, iron, copper, a clad material combining these materials, or a material obtained by plating these materials with nickel, chrome, nickel chrome, etc. The thickness of the connection terminal is preferably 10 to 300 μm.

[0142] <Insulator> Examples of insulators to be placed in areas where the power generating elements are not placed include ionomer resins (such as the same as those exemplified above for bonding substrates to form the outer casing), polyolefins (polypropylene, polyethylene, etc.), polyurethane, epoxy, polyimide, and other resins.

[0143] In addition, in a battery, from the viewpoint of facilitating cutting at the location where the insulator is arranged, it is preferable that the thickness of the location where the insulator is arranged is small, and for example, it is more preferable that the thickness of the location where the insulator is arranged is smaller than the thickness of the location where the power generating element is arranged, as shown in Fig. 2. Although the thickness of the location where the power generating element is arranged varies depending on the thickness of the power generating element, it is usually preferable that the thickness of the location where the insulator is arranged is 0.2 to 1.0 mm, and if it is of this thickness, it can be cut relatively easily.

[0144] The battery of the present invention can be used in the same applications as conventionally known primary batteries and secondary batteries, but since it has a solid electrolyte instead of an organic electrolyte, it has excellent heat resistance and can be preferably used in applications where it is exposed to high temperatures. EXAMPLES

[0145] The present invention will be described in detail below with reference to examples, although the present invention is not limited to the following examples.

[0146] Example 1 Lithium titanate (Li4Ti5O 12 A negative electrode mixture was prepared by mixing a sulfide-based solid electrolyte (Li6PS5Cl) having an average particle size of 0.7 μm and graphene (conductive additive) in a mass ratio of 50:41:9.

[0147] In addition, a positive electrode mixture was prepared by mixing LiCoO2 (positive electrode active material) with an average particle size of 5 μm and a LiNbO3 coating layer formed on the surface, a sulfide-based solid electrolyte (Li6PS5Cl) with an average particle size of 0.7 μm, and graphene in a mass ratio of 65:30.7:4.3.

[0148] Next, a powder of sulfide-based solid electrolyte (Li6PS5Cl) with an average particle size of 0.7 μm was placed in a powder molding die, and pressure molding was performed at a surface pressure of 70 MPa using a press machine to form a provisionally molded layer of the solid electrolyte layer. Furthermore, the negative electrode mixture was placed on the upper surface of the provisionally molded layer of the solid electrolyte layer, and pressure molding was performed at a surface pressure of 50 MPa to further form a provisionally molded layer of the negative electrode on the provisionally molded layer of the solid electrolyte layer.

[0149] Next, a nickel foamed metal porous body (nickel "Celmet" (registered trademark)) made by Sumitomo Electrochemical Industries, Ltd., cut into a circle with a diameter of 8 mm (thickness: 1.2 mm, porosity: 98%) was placed on the provisionally molded layer of the negative electrode formed on the provisionally molded layer of the solid electrolyte layer, and pressure molding was performed with a surface pressure of 300 MPa to form an integrated body of the solid electrolyte layer and the negative electrode.

[0150] Furthermore, after the mold was turned upside down, the positive electrode mixture was placed on the upper surface of the solid electrolyte layer in the mold (the surface opposite to the surface having the negative electrode), and pressure molding was performed at a surface pressure of 50 MPa to form a provisionally molded layer of the positive electrode on the solid electrolyte layer.

[0151] Next, a cut piece of foamed nickel metal porous body, the same as that used for the negative electrode, was placed on top of the provisionally molded layer for the positive electrode formed on the solid electrolyte layer, and pressure molding was performed with a surface pressure of 1,400 MPa to obtain a power generating element having a circular shape with a diameter of 8 mm in plan view and a thickness of 1.4 mm.

[0152] In the obtained power generating element, the thickness of the negative electrode mixture layer of the negative electrode, the thickness of the porous metal substrate, and the thickness of the portion of the porous metal substrate embedded in the negative electrode mixture layer were 740 μm, 50 μm (4% of the thickness of the porous metal substrate before use in the negative electrode), and 10 μm (20% of the total thickness of the porous metal substrate), respectively. In addition, the area ratio of the portion of the negative electrode mixture exposed on the surface of the negative electrode was 7%.

[0153] In the obtained power generating element, the thickness of the positive electrode mixture layer of the positive electrode, the thickness of the porous metal substrate, and the thickness of the portion of the porous metal substrate embedded in the positive electrode mixture layer were 420 μm and 50 μm (4% of the thickness of the porous metal substrate before use in the positive electrode), and 10 μm (20% of the total thickness of the porous metal substrate), respectively. The area ratio of the portion of the positive electrode mixture exposed on the surface of the positive electrode was 7%.

[0154] Thirty-six power generating elements obtained as described above were arranged in a lattice pattern of 6 columns by 6 columns with a spacing of 10 mm between the power generating elements, and a current collector made of nickel foil with a thickness of 20 μm and a width of 2 mm was placed on top of the power generating element at a position 2 mm shifted from the center of the power generating element in one horizontal direction (to the right in FIG. 4) on the positive electrode side of the power generating element, and the porous metal substrate embedded in the positive electrode mixture layer and the current collector were connected by resistance welding. In addition, a current collector made of the same nickel foil as above was placed on top of the power generating element at a position 2 mm shifted from the center of the power generating element in one vertical direction (to the bottom in FIG. 4) on the positive electrode side of the power generating element, and the porous metal substrate embedded in the positive electrode mixture layer and the current collector were similarly connected. Furthermore, on the negative electrode side of the power generating element, a current collector made of the same nickel foil as above was superimposed at a position shifted 2 mm from the center of the power generating element in the other horizontal direction (left direction in FIG. 4), and the porous metal substrate embedded in the negative electrode mixture layer and the current collector were welded and connected by resistance welding. Also, on the negative electrode side of the power generating element, a current collector made of the same nickel foil as above was superimposed at a position shifted 2 mm from the center of the power generating element in the other vertical direction (upward direction in FIG. 4), and the porous metal substrate embedded in the negative electrode mixture layer and the current collector were similarly connected, and a group of power generating elements connected in a lattice shape by the current collector was obtained. In this embodiment, the current collector connecting the power generating element in the vertical direction and the current collector connecting the power generating element in the horizontal direction were composed of separate current collectors made of nickel foil, but a lattice-shaped current collector in which the vertical current collector and the horizontal current collector are integrated may be used.

[0155] Next, two laminate films each having a three-layer structure of nylon / aluminum / CPP (non-oriented polypropylene) (thicknesses of 25 μm / 40 μm / 40 μm, respectively) were prepared.

[0156] A group of power generating elements connected in a grid pattern with current collectors as described above was placed on the CPP layer side of one of the laminate films, with the positive electrodes facing each other, and a 0.1 mm-thick ionomer resin (Himilan (product name) manufactured by Dow Mitsui Polychemicals) was placed in the areas where no power generating elements were present.

[0157] The other laminate film was then placed on top of this with the CPP layer side facing the negative electrode side of the power generation element group, and heat pressed along the ionomer resin to fuse the ionomer resin to the upper and lower laminate films.

[0158] A nickel connection terminal with a thickness of 50 μm, width of 3 mm, and length of 15 mm was placed on the laminate film on the nickel foil current collector at the outer periphery of the positive electrode side, and connected with a stainless steel staple. A connection terminal was similarly connected to the negative electrode side, obtaining a flexible all-solid-state battery (hereafter referred to as flexible battery).

[0159] Comparative Example 1 Two laminate films (insulating layer thickness 45 μm, conductive layer thickness 40 μm) having an insulating layer made of nylon 66 and a conductive layer made of stainless steel foil were prepared, and nickel connection terminals (3 mm × 15 mm, thickness 50 μm) were attached to each end.

[0160] Next, 36 power generating elements prepared in the same manner as in Example 1 were arranged on the conductive layer of one of the laminate films in 6 columns and 6 rows with the positive electrode sides facing each other and with a spacing of 10 mm between the power generating elements, and the same ionomer resin as in the Example was placed to a thickness of 0.1 mm in the areas where no power generating elements were present.

[0161] Then, the other laminate film was placed on top of that with the conductive layer facing the negative electrode side of the power generation element, and the whole was heat-pressed to fuse the ionomer resin with the upper and lower laminate films, and the outer edges of the four sides were further sealed by heat pressing to obtain a flexible battery.

[0162] The flexible batteries of Example 1 and Comparative Example 1 were subjected to the following evaluations.

[0163] For each of the flexible batteries of Example 1 and Comparative Example 1, constant current charging was performed at a current value of 200 mA equivalent to 1 C, equivalent to 0.5 C, until the voltage reached 2.6 V, and then constant voltage charging was performed at a voltage of 2.6 V until the current value reached 0.01 C.

[0164] For ten flexible batteries each of Example 1 and Comparative Example 1, the portions in which the ionomer resin was disposed inside were cut using ceramic scissors so as to include the portions with the connection terminals attached in three vertical rows and two horizontal rows. At this time, the short circuit occurrence rates of the individual batteries (power generation elements) cut out from the flexible batteries of Example 1 and Comparative Example 1 were 0 / 10 and 8 / 10, respectively.

[0165] For ten flexible batteries each of Example 1 and Comparative Example 1, a nickel connection terminal having a thickness of 50 μm and a width of 3 mm was placed on the laminate film on the nickel foil current collector at the outer peripheral end of the positive electrode side, and connected with a stainless steel staple. A connection terminal was similarly connected on the negative electrode side. At this time, the short circuit occurrence rates in the flexible batteries of Example 1 and Comparative Example 1 were 0 / 10 and 10 / 10, respectively.

[0166] As described above, in the flexible battery of Example 1, the occurrence of a short circuit when some of the multiple power generating elements are cut and separated is effectively suppressed, and it was found that even when attaching connection terminals to use the separated power generating elements as individual batteries, attachment can be performed by simple means without causing a short circuit. [Explanation of symbols]

[0167] 100 batteries 110 Power generation element 120 positive electrode 121 Positive electrode mixture layer 121a Positive electrode mixture 122 Sheet-shaped porous metal substrate 130 negative electrode 131 Negative electrode mixture layer 132 Sheet-shaped porous metal substrate 140 Solid electrolyte layer 150 Exterior body 160, 170 base material 161 Current collector connecting positive electrodes 171 Current collector connecting negative electrodes 180 Insulator 190, 191 Connection terminal 192 Joining means 200, 201, 202, 203 Separated battery (power generating element)

Claims

1. A battery in which a plurality of power generating elements are enclosed in an exterior body, the power generating element has a positive electrode, a negative electrode, and a solid electrolyte layer disposed between the positive electrode and the negative electrode, The positive electrode has a positive electrode mixture layer containing a positive electrode active material and a sheet-like conductive substrate, The negative electrode has a negative electrode mixture layer containing a negative electrode active material and a sheet-like conductive substrate, the plurality of power generating elements are arranged on a substrate, and each positive electrode is directly connected to a current collector, thereby connecting the positive electrodes to each other via the current collector, and each negative electrode is directly connected to a current collector, thereby connecting the negative electrodes to each other via the current collector; In a plan view, the positive electrode current collector and the negative electrode current collector do not overlap at least in a portion where the power generating element is not present, the positive electrode current collector and the negative electrode current collector have a length of 0.5 mm or more in a direction perpendicular to a direction in which adjacent power generating elements are connected to each other in a plan view; A battery characterized in that an insulator is disposed in at least a portion of the region of the substrate where the power generating element is not disposed, and the substrate can be cut at the location where the insulator is disposed.

2. 2. The battery according to claim 1, wherein after cutting at the location where the insulator is disposed, external connection terminals can be attached to the positive electrode current collector and the negative electrode current collector.

3. the conductive substrate of the positive electrode is a porous metal substrate, at least a portion of which including an end portion on the positive electrode mixture layer side is embedded in the positive electrode mixture layer and is integrated with the positive electrode mixture layer, and the other end portion of the porous metal substrate of the positive electrode is exposed on a surface of the positive electrode, 2. The battery according to claim 1, wherein the conductive substrate of the negative electrode is a porous metal substrate, at least a portion of which including an end portion on the negative electrode mixture layer side is embedded in the negative electrode mixture layer and integrated with the negative electrode mixture layer, and the other end portion of the porous metal substrate of the negative electrode is exposed on the surface of the negative electrode.

4. 2. The battery of claim 1, wherein the substrate is flexible.

Citation Information

Patent Citations

  • Method for manufacturing battery

    WO2021131095A1

  • Method for manufacturing battery

    WO2022270042A1

  • Battery and battery manufacturing method

    WO2022270141A1

  • Battery

    JP1994215753A

  • Manufacture of cell

    JP1994267581A