Mo-containing niobium titanium oxide with a monoclinic structure addresses the limitations of titanium oxide electrodes by enhancing lithium insertion capacity and cycle life, resulting in secondary batteries with improved energy density and rapid charging capabilities.

JP2024132491AActive Publication Date: 2024-10-01KK TOSHIBA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023043275
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-10-01
Estimated Expiration
2043-03-17

AI Technical Summary

Technical Problem

Existing secondary batteries face challenges in achieving high energy density and stable rapid charging and discharging due to the limitations of titanium oxide negative electrodes, which have low capacity per weight and higher electrode potential, leading to issues like metallic lithium dendrite formation and internal short circuits.

Method used

The use of Mo-containing niobium titanium oxide with a monoclinic structure, characterized by specific peak intensity ratios in X-ray diffraction spectra, enhances lithium insertion capacity by partially replacing titanium with molybdenum, resulting in improved charge and discharge performance.

Benefits of technology

The Mo-containing niobium titanium oxide exhibits high theoretical capacity and maintains excellent cycle life performance, enabling secondary batteries to achieve higher energy density and stable rapid charging and discharging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132491000001_ABST
    Figure 2024132491000001_ABST
Patent Text Reader

Abstract

To provide an active material that can be used to achieve a secondary battery with a high capacity and excellent cycle life performance, an electrode containing the same, a secondary battery including the electrode, a battery pack including the secondary battery, and a vehicle mounted on the battery pack.SOLUTION: Provided is an active material containing a niobium-titanium oxide with a monoclinic crystal structure that contains molybdenum. In an X-ray diffraction spectrum of the active material, a ratio of I25 / I24 of the intensity of a first peak I24 appearing in a range of 2θ from 23.5° to 24.5° to the intensity of a second peak I25 appearing in a range of 2θ from 25.0° to 25.5° is 0.5 or more.SELECTED DRAWING: Figure 10
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THE DISCLOSURE Embodiments of the present invention relate to an active material, an electrode, a secondary battery, a battery pack, and a vehicle. [Background technology]

[0002] In recent years, research and development of secondary batteries such as non-aqueous electrolyte secondary batteries, such as lithium ion secondary batteries, as high energy density batteries, has been actively promoted. Secondary batteries such as non-aqueous electrolyte secondary batteries are expected to be used as power sources for vehicles such as hybrid electric vehicles and electric vehicles, and for uninterruptible power sources for mobile phone base stations. Therefore, in addition to high energy density, secondary batteries are also required to have excellent other performances such as rapid charge and discharge performance and long-term reliability. For example, secondary batteries capable of rapid charge and discharge not only significantly reduce charging time, but also improve the power performance of vehicles such as hybrid electric vehicles and efficiently recover regenerative energy from power.

[0003] In order to enable rapid charging and discharging, it is necessary that electrons and lithium ions can move quickly between the positive and negative electrodes. However, when a battery using a carbon-based negative electrode is repeatedly charged and discharged rapidly, dendrites of metallic lithium are precipitated on the electrode, which may cause heat generation or fire due to an internal short circuit.

[0004] Therefore, batteries that use metal composite oxides instead of carbonaceous materials for the anode have been developed. Among them, batteries that use titanium oxide for the anode are capable of stable rapid charging and discharging and have a longer life than batteries that use carbon-based anodes.

[0005] However, titanium oxide has a higher potential relative to metallic lithium than carbonaceous materials, i.e., it is more noble. Moreover, titanium oxide has a low capacity per weight. Therefore, batteries using titanium oxide in the negative electrode have a problem of low energy density.

[0006] For example, the electrode potential of titanium oxide is about 1.5 V (vs. Li / Li) based on metallic lithium.+ ), which is higher (more noble) than the potential of a carbon-based negative electrode. The potential of titanium oxide is the potential of Ti when electrochemically inserting and extracting lithium. 3+ and Ti 4+ The charge is electrochemically limited because it is caused by an oxidation-reduction reaction between the two. + It is also true that rapid charging and discharging of lithium ions can be performed stably at high electrode potentials of around 1000 kV. Therefore, it has been difficult to lower the electrode potential in order to improve the energy density.

[0007] On the other hand, in terms of capacity per unit weight, the theoretical capacity of titanium dioxide (anatase structure) is about 165 mAh / g, and Li4Ti5O 12 The theoretical capacity of spinel-type lithium titanium oxide such as the one shown in Fig. 1 is about 180 mAh / g. On the other hand, the theoretical capacity of general graphite-based electrode materials is 385 mAh / g or more. Thus, the capacity density of titanium oxide is significantly lower than that of carbon-based negative electrodes. This is because the crystal structure of titanium oxide has few sites for absorbing lithium and lithium is easily stabilized in the structure, resulting in a decrease in the actual capacity.

[0008] In view of the above, new electrode materials containing Ti and Nb are being investigated. Such niobium titanium oxide materials are expected to have high charge / discharge capacity. For example, an oxide represented by TiNb2O7 has a high theoretical capacity of more than 380 mAh / g. Therefore, niobium titanium oxide is Li4Ti5O 12 It is expected to be a high-capacity material to replace [Prior art documents] [Patent documents]

[0009] [Patent Document 1] China Patent Application Publication No. 105633456 [Patent Document 2] JP 2016-177972 A [Patent Document 3] JP 2019-169343 A [Patent Document 4] JP 2022-145421 A [Non-patent literature]

[0010] [Non-Patent Document 1] Chunfu Lin, et. al., Chem. Commun., 2015, 51, 8970-8973, “TiNb6O17: a new electrode material for lithium-ion batteries” [Non-Patent Document 2] Chunfu Lin, et. al., Small, 2017, 13, 1702903, “Intercalating Ti2Nb14O39 Anode Materials for Fast-Charging, High-Capacity and Safe Lithium-Ion Batteries” [Non-Patent Document 3] Aghamohammadi Hamed, et. al., J. Alloys Compd., 2022, 911, 165117, “A Comprehensive Review Study on Pure Titanium Niobium Oxide as the Anode Material for Li-ion Batteries” [Non-Patent Document 4] "Practice of Powder X-ray Analysis" First Edition (2002) Edited by the X-ray Analysis Research Roundtable of the Japan Society for Analytical Chemistry, edited by Izumi Nakai and Fujio Izumi (Asakura Publishing) Summary of the Invention [Problem to be solved by the invention]

[0011] The object is to provide an active material capable of realizing a secondary battery capable of exhibiting high capacity and excellent cycle life performance, an electrode containing this active material, a secondary battery equipped with this electrode, a battery pack equipped with this secondary battery, and a vehicle equipped with this battery pack. [Means for solving the problem]

[0012] According to an embodiment, an active material is provided. The active material includes a Mo-containing niobium titanium oxide having a monoclinic structure. In the X-ray diffraction spectrum of the active material, the intensity I of a first peak appearing within the 2θ range of 23.5° to 24.5° is 24 Intensity of the second peak appearing within the 2θ range of 25.0° to 25.5° for 25 Ratio I 25 / I 24 is 0.5 or more.

[0013] According to another embodiment, an electrode is provided that includes an active material according to the above embodiments.

[0014] According to another embodiment, there is provided a secondary battery comprising a positive electrode, a negative electrode and an electrolyte. The negative electrode is an electrode according to the above embodiment.

[0015] According to another embodiment, a battery pack including the secondary battery according to the above embodiment is provided.

[0016] According to another embodiment, a vehicle is provided that is equipped with a battery pack according to the above embodiment. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of a secondary battery according to an embodiment. [Diagram 2] 2 is an enlarged cross-sectional view of a portion A of the secondary battery shown in FIG. 1. [Diagram 3] FIG. 4 is a partially cutaway perspective view illustrating a schematic diagram of another example of a secondary battery according to an embodiment. [Figure 4] 4 is an enlarged cross-sectional view of a portion B of the secondary battery shown in FIG. 3. [Diagram 5] FIG. 1 is a perspective view illustrating an example of a battery pack according to an embodiment. [Figure 6] FIG. 1 is an exploded perspective view illustrating an example of a battery pack according to an embodiment. [Figure 7] 7 is a block diagram showing an example of an electric circuit of the battery pack shown in FIG. 6. [Figure 8] 1 is a cross-sectional view illustrating an example of a vehicle according to an embodiment. [Figure 9] 1 is a diagram illustrating an example of a control system for an electrical system in a vehicle according to an embodiment. [Figure 10] FIG. 2 is a diagram showing X-ray diffraction spectra of active materials according to Examples 1 to 4 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Ti can be reduced from 4 to 3 to 1. In contrast, Nb can be reduced from 5 to 3 to 2. Therefore, the higher the Nb stoichiometric ratio, the more lithium can be inserted theoretically, and the higher the capacity. For example, the Wadsley-Roth phase crystal structure and the general formula TiNb x O 2+2.5x The theoretical capacity of the niobium titanium oxide family, which can be expressed by the formula, is 403-5441 / (133x+80) mAh / g, and approaches the maximum theoretical value of 403 mAh / g as the subscript x, which represents the Nb stoichiometric ratio, increases. For example, the theoretical capacity of TiNb2O7 (x=2) calculated from the above formula is 387 mAh / g. Similarly, Ti2Nb6O 19 The theoretical capacity of (x=3) is 392 mAh / g, and Ti2Nb 14 O 39 The theoretical capacity for (x=7) is 398 mAh / g.

[0019] As mentioned above, the theoretical capacity of niobium titanium oxides with high Nb composition is high. However, the reported capacity of high Nb composition compounds does not reach that of TiNb2O7.

[0020] Hereinafter, the embodiments will be described with reference to the drawings. Note that the same reference numerals are used to designate common components throughout the embodiments, and duplicated descriptions will be omitted. Each figure is a schematic diagram for explaining the embodiments and for facilitating understanding thereof, and the shapes, dimensions, ratios, etc. may differ from those of the actual device, but these can be appropriately modified in design by taking into consideration the following explanation and known techniques.

[0021] (First embodiment) According to a first embodiment, an active material is provided. The active material includes a Mo-containing niobium titanium oxide. The oxide has a monoclinic crystal structure. In the X-ray diffraction spectrum of the active material, a first peak appears in the 2θ range of 23.5° to 24.5° and a second peak appears in the 2θ range of 25.0° to 25.5°. The intensity I 24 Intensity of the second peak I 25 Ratio I 25 / I 24 is greater than or equal to 0.5.

[0022] The active material may be a battery active material. The active material may be, for example, an electrode active material used in an electrode of a secondary battery such as a lithium ion battery or a nonaqueous electrolyte battery. The active material may be, for example, a negative electrode active material used in a negative electrode of the secondary battery.

[0023] In an X-ray diffraction spectrum obtained by a wide-angle X-ray diffraction (XRD) method using CuKα radiation as an X-ray source, the peak intensity ratio I between the first peak appearing in the 2θ range of 23.5° to 24.5° and the second peak appearing in the 2θ range of 25.0° to 25.5° is 25 / I 24 Mo-containing niobium titanium oxides having a ratio of 0.5 or more can exhibit high capacity while maintaining cycle life performance equivalent to that of niobium titanium oxides having a high Nb composition. 25 / I 24 It is desirable that the ratio I be 0.9 or less. 25 / I 24 It is more preferable that the ratio is 0.85 or less.

[0024] The first peak has a peak top within the range of 23.5°≦2θ≦24.5° in the XRD spectrum. The first peak is observed in the XRD spectrum for various niobium titanium oxides regardless of the presence or absence of Mo. The second peak has a peak top within the range of 25.0°≦2θ≦25.5° in the XRD spectrum. The second peak is observed in niobium titanium oxides containing Mo.

[0025] A method for carrying out wide-angle X-ray diffraction is described below.

[0026] Niobium titanium oxide containing Mo can absorb more lithium ions (Li + ) can be stored. The upper limit of the valence of molybdenum (Mo) is +6, while the upper limit of the valence of titanium is +4 and that of niobium is +5. Therefore, by including Mo, which can change its valence more, the amount of Li that can be inserted into the oxide can be increased. + This increases the capacity of the electrode active material. 4+ Mo 6+ By replacing it with, a high capacity can be achieved.

[0027] The composition of the Mo-containing niobium titanium oxide is, for example, represented by the general formula Ti x-y Mo y Nb 12-x O 29+z The subscripts in the general formula are within the ranges of 1.5≦x≦2.2, 0<y≦0.7x, and −3≦z≦1. As can be seen from the general formula, the Mo-containing niobium titanium oxide can be a compound in which Ti in a niobium titanium oxide having a high Nb composition is partially substituted with Mo. As the upper limit of the subscript y indicates, the oxide can be a compound in which up to half of Ti is substituted with Mo.

[0028] Next, the morphology, particle size, and specific surface area of ​​the active material will be described.

[0029] <Form> The form of the active material according to the embodiment is not particularly limited. The active material can be, for example, the particles of the Mo-containing niobium titanate described above, or a powder composed of such particles. The particles of the Mo-containing niobium titanate can take the form of primary particles, for example, or can take the form of secondary particles formed by aggregation of primary particles. The particles of the Mo-containing niobium titanate may be a mixture of primary particles and secondary particles.

[0030] The particles of the Mo-containing niobium titanate may have a carbon-containing layer on the surface. The carbon-containing layer may adhere to the surface of the primary particles or may adhere to the surface of the secondary particles. Alternatively, the active material may contain secondary particles formed by aggregation of primary particles having a carbon-containing layer adhered to the surface. Since carbon exists between such primary particles, such secondary particles can exhibit excellent conductivity. An embodiment containing such secondary particles is preferable because the active material-containing layer containing the same can exhibit lower resistance.

[0031] <Particle size> The average particle size of the active material particles, which are primary particles or secondary particles containing Mo-containing niobium titanate, is not particularly limited. The average particle size of the active material particles is, for example, in the range of 0.1 μm or more and 50 μm or less. The average particle size can be changed according to the required battery performance. For example, in order to enhance the rapid charge and discharge performance, it is preferable to set the average particle size to 1.0 μm or less. By doing so, the diffusion distance of lithium ions in the crystal can be reduced, so that the rapid charge and discharge performance can be enhanced. The average particle size can be determined, for example, by the laser diffraction method.

[0032] <BET specific surface area> The BET (Brunauer, Emmett, Teller) specific surface area of the active material is not particularly limited. However, the BET specific surface area is preferably 5 m 2 / g or more and less than 200 m 2 / g.

[0033] When the specific surface area is 5 m 2When the specific surface area is 200 m / g or more, the contact area with the electrolyte can be secured when the material is used in a battery, good discharge rate performance can be easily obtained, and the charging time can be shortened. 2 When the molecular weight is less than 1 / g, the reactivity with the electrolyte is not too high, and the life performance can be improved. In addition, the coating property of a slurry containing an active material used in the production of an electrode described later can be improved.

[0034] Here, the specific surface area is measured by adsorbing molecules with known adsorption occupancy areas onto the powder particle surfaces at liquid nitrogen temperature, and then calculating the specific surface area of ​​the sample from the amount of adsorption. The most commonly used method is the BET method, which uses low-temperature, low-humidity physical adsorption of an inert gas. This BET method is based on the BET theory, which is the most famous method for calculating specific surface area, and which extends the Langmuir theory, a theory of monolayer adsorption, to multilayer adsorption. The specific surface area calculated in this way is called the BET specific surface area.

[0035] <Manufacturing method> The active material according to the embodiment can be produced by the synthesis method described below.

[0036] The starting materials, titanium, niobium and molybdenum sources, are dissolved in an acidic solution, the solution is neutralized and the resulting gel is dried to obtain a precursor, which is then heat-treated to obtain Mo-containing niobium titanium oxide.

[0037] The titanium source may be, for example, titanium tetraisopropoxide (C 12 H 28 O4Ti) can be used. As a niobium source, for example, ammonium niobium oxalate hydrate (C4H4NNbO9·xH2O) can be used. As a molybdenum source, for example, ammonium molybdate ((NH4)6Mo7O 244H2O) can be used. As the acidic solution for dissolving the Ti source, Nb source, and Mo source, for example, an aqueous solution of oxalic acid can be used. For the neutralization treatment, for example, ammonia water can be used. For drying the gel after neutralization, for example, a heating method in air, a spray drying method, etc. can be applied.

[0038] When the precursor is heat-treated to obtain an oxide, the precursor is densely packed in a container having an appropriate opening. Increasing the density in this way promotes sufficient oxidation of the precursor while suppressing the volatilization of Mo. In the heat treatment, preliminary firing (first firing) is performed before the main firing. Preliminary firing is preferably performed at a temperature of 200°C to 400°C for 1 hour to 12 hours. By performing preliminary firing, it is possible to remove trace amounts of impurity components (e.g., water, organic matter, etc.) adsorbed on the precursor. Preliminary firing may be omitted. The main firing (second firing) is preferably performed at a temperature of 900°C to 1500°C for 1 hour to 40 hours.

[0039] In addition to the above liquid phase synthesis method, the active material according to the embodiment can be obtained by, for example, a general solid phase reaction method. As a specific example, the active material according to the embodiment can be obtained by mixing titanium oxide (TiO2), niobium oxide (Nb2O5 or NbO2) and molybdenum oxide (MoO3 or MoO2) in a mortar or ball mill, and firing the mixture in air.

[0040] <Powder X-ray diffraction measurement and peak intensity ratio of active materials I 25 / I 24 Calculation of > The powder X-ray diffraction measurement of the active material can be carried out, for example, as follows.

[0041] First, the target sample is crushed until the average particle size is about 5 μm. The crushed sample is filled into the holder portion formed on the glass sample plate, with a depth of 0.2 mm. At this time, care is taken to ensure that the sample is filled sufficiently into the holder portion. Also, care is taken to fill the sample with just the right amount so that cracks, voids, etc. do not occur. Next, another glass plate is pressed from the outside to flatten the surface of the sample filled into the holder portion. Care is taken to ensure that the amount of filling is not too much or too little, resulting in unevenness compared to the reference surface of the holder.

[0042] Next, the glass plate filled with the sample is placed in a powder X-ray diffractometer, and a diffraction pattern (XRD pattern) is obtained using Cu-Kα radiation.

[0043] In addition, the orientation of the particles may become large depending on the particle shape of the sample. When the orientation of the sample is high, the peak position may shift or the intensity ratio may change depending on how the sample is filled. Samples with extremely high orientation are measured using a glass capillary. Specifically, the sample is inserted into a capillary, and the capillary is placed on a rotating sample stage for measurement. This measurement method can reduce the orientation. As the glass capillary, it is preferable to use a Lindemann glass capillary with a diameter of 1 mm to 6 mmφ.

[0044] When performing powder X-ray diffraction measurement on the active material contained in the electrode, it can be performed, for example, as follows.

[0045] First, in order to grasp the crystalline state of the active material, the active material is placed in a state in which lithium ions are completely removed. For example, when the active material is used in a negative electrode, the battery is placed in a completely discharged state. For example, the battery is discharged at a current of 0.1 C in a 25° C. environment until the rated end voltage or the battery voltage reaches 1.0 V, and the current value during discharge is set to 1 / 100 or less of the rated capacity, thereby placing the battery in a discharged state. Residual lithium ions may still be present even in the discharged state.

[0046] Next, the battery is disassembled in a glove box filled with argon, and the electrodes are removed and washed with a suitable solvent. An example of a suitable solvent is ethyl methyl carbonate. If the electrodes are not sufficiently washed, lithium ions remaining in the electrodes may cause impurity phases such as lithium carbonate and lithium fluoride to be mixed in. In that case, it is recommended to use an airtight container in which the measurement atmosphere can be in an inert gas. The washed electrodes are cut to have an area approximately the same as the area of ​​the holder of the powder X-ray diffraction apparatus to prepare the measurement sample. This sample is directly attached to the glass holder and the measurement is performed.

[0047] At this time, the peaks originating from the metal foil, conductive agent, binder, etc., which is the current collector, are measured and understood in advance using XRD. Of course, if these are known in advance, this operation can be omitted. When the peak of the current collector and the peak of the active material overlap, it is desirable to peel off the active material-containing layer from the current collector and measure it. This is to separate the overlapping peaks when quantitatively measuring the peak intensity. The active material-containing layer may be physically peeled off, but it is easier to peel off by applying ultrasonic waves in a solvent. When ultrasonic treatment is performed to peel off the active material-containing layer from the current collector, the electrode body powder (including the active material, conductive agent, and binder) can be recovered by volatilizing the solvent. The recovered electrode body powder can be filled in, for example, a Lindemann glass capillary and measured to perform powder X-ray diffraction measurement of the active material. The electrode body powder recovered by ultrasonic treatment can also be subjected to various analyses other than powder X-ray diffraction measurement.

[0048] As an apparatus for powder X-ray diffraction measurement, for example, SmartLab manufactured by Rigaku Co., Ltd. is used. The measurement conditions are as follows: X-ray source: Cu target Output: 45kV, 200mA Soller slit: 5° for both incidence and reception Step width (2θ): 0.01 deg Scan speed: 2deg / min Semiconductor detector: D / teX Ultra 250 Sample plate holder: Flat glass sample plate holder (thickness 0.5 mm) Measurement range: 5°≦2θ≦90°.

[0049] When using other equipment, perform measurements using standard Si powder for powder X-ray diffraction. In order to obtain measurement results equivalent to those obtained by the above equipment, find conditions under which the same peak intensity, half-width, and diffraction angle measurement results as those obtained by the above equipment are obtained, and adjust the conditions to measure the sample.

[0050] The conditions of the powder X-ray diffraction measurement are such that an XRD pattern applicable to Rietveld analysis can be obtained. To collect data for Rietveld analysis, specifically, the step width is set to 1 / 3-1 / 5 of the minimum half-width of the diffraction peak, and the measurement time or X-ray intensity is appropriately adjusted so that the intensity at the peak position of the most intense reflection is 5000 cps or more. For example, Rietveld analysis can be performed based on the method detailed in Non-Patent Document 4.

[0051] By the above method, information about the crystal structure of the active material to be measured can be obtained. For example, when the active material according to the embodiment is measured as described above, it is found that the active material to be measured contains an oxide having a monoclinic structure. Furthermore, by measuring as described above, the crystallinity and symmetry of the crystal structure of the measurement target, such as the monoclinic system, can be investigated.

[0052] In the obtained diffraction spectrum, the peak intensity I of the first peak having a peak top within the range of 2θ from 23.5° to 24.5° is 24 In addition, in the diffraction spectrum, the peak intensity I of the second peak having a peak top within the range of 2θ from 25.0° to 25.5° is determined. 25 Then, the peak intensity ratio I 25 / I 24 Calculate.

[0053] <Method for measuring the composition of niobium titanium oxide> The composition of the niobium titanium oxide in the active material can be determined by inductively coupled plasma atomic emission spectroscopy (ICP-AES analysis).

[0054] First, the target sample is pulverized. It is then dissolved in acid and subjected to inductively coupled plasma atomic emission spectroscopy (ICP-AES). ICP-AES can measure the type and concentration of elements contained in the active material.

[0055] The composition of the active material contained in the electrode can be measured, for example, as follows. First, an active material from which Li has been completely removed is prepared using the same procedure as in the powder X-ray diffraction method described above. This is subjected to vacuum drying at a temperature of 140° C. for 24 hours. Next, the total weight of this active material is measured in a dry atmosphere. This is dissolved in acid and subjected to inductively coupled plasma atomic emission spectroscopy (ICP-AES analysis). The type and concentration of elements contained in the active material can be measured by ICP-AES.

[0056] According to the first embodiment, an active material containing Mo-containing niobium titanium oxide having a monoclinic structure is provided. In the X-ray diffraction spectrum obtained for the active material, the intensity I of the first peak at 2θ=23.5°-24.5° is 25 and the intensity of the second peak at 2θ=25.0°-25.5°, I 25 What is the ratio I 25 / I 24 is 0.5 or more. Such an active material can realize a secondary battery that can exhibit high capacity and excellent cycle life performance.

[0057] Second embodiment According to a second embodiment, an electrode is provided.

[0058] The electrode according to the second embodiment includes the active material according to the first embodiment. This electrode can be a battery electrode that includes the active material according to the first embodiment as a battery active material. The electrode as a battery electrode can be, for example, a negative electrode that includes the active material according to the first embodiment as a negative electrode active material.

[0059] Such an electrode may include a current collector and an active material-containing layer. The active material-containing layer may be formed on one or both sides of the current collector. The active material-containing layer may include an active material and, optionally, a conductive agent and a binder.

[0060] The active material-containing layer may contain the active material according to the first embodiment alone, or may contain two or more types of the active material according to the first embodiment. Furthermore, it may contain a mixture of one or more types of the active material according to the first embodiment and one or more types of other active materials. It is desirable that the content ratio of the active material according to the first embodiment with respect to the total mass of the active material according to the first embodiment (the above-mentioned Mo-containing niobium titanium oxide) and the other active materials is 10 mass % or more and 100 mass % or less.

[0061] For example, when the active material according to the first embodiment is contained as a negative electrode active material, examples of other active materials include lithium titanate having a ramsdellite structure (e.g., Li 2+y Ti3O7, 0≦y≦3), lithium titanates with spinel structure (e.g., Li 4+x Ti5O 12 , 0≦x≦3), titanium dioxide (TiO2), anatase type titanium dioxide, rutile type titanium dioxide, niobium pentoxide (Nb2O5), hollandite type titanium composite oxide, orthorhombic titanium composite oxide, and other monoclinic type niobium titanium oxides.

[0062] As an example of the above-mentioned orthorhombic titanium-containing composite oxide, Li 2+a M I 2-b Ti 6-c M II d O 14+σIn this case, the compound represented by M I is at least one selected from the group consisting of Sr, Ba, Ca, Mg, Na, Cs, Rb and K. II is at least one selected from the group consisting of Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni, and Al. The subscripts in the composition formula are 0≦a≦6, 0≦b<2, 0≦c<6, 0≦d<6, and -0.5≦σ≦0.5. Specific examples of orthorhombic titanium-containing composite oxides include Li 2+a Na2Ti6O 14 (0≦a≦6).

[0063] As an example of the monoclinic niobium titanium oxide, Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δ Here, M1 is at least one selected from the group consisting of Zr, Si, and Sn. M2 is at least one selected from the group consisting of V, Ta, and Bi. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3. Specific examples of monoclinic niobium titanium oxide include Li x Examples include Nb2TiO7 (0≦x≦5).

[0064] Another example of monoclinic niobium titanium oxide is Li x Ti 1-y M3 y+z Nb 2-z O 7-δ Here, M3 is at least one selected from Mg, Fe, Ni, Co, W, and Ta. Each subscript in the composition formula is 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3.

[0065] The conductive agent is blended to improve the current collecting performance and to reduce the contact resistance between the active material and the current collector. Examples of the conductive agent include carbonaceous materials such as vapor grown carbon fiber (VGCF), carbon black such as acetylene black, graphite, carbon nanotubes, and carbon nanofibers. One of these may be used as the conductive agent, or two or more may be used in combination as the conductive agent. Alternatively, instead of using a conductive agent, a carbon coating or an electronically conductive inorganic material coating may be applied to the surface of the active material particles.

[0066] The binder is blended to fill the gaps between the dispersed active materials and to bind the active materials and the current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene butadiene rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.

[0067] The mixing ratio of the active material, conductive agent and binder in the active material-containing layer can be appropriately changed depending on the application of the electrode. For example, when the electrode is used as a negative electrode of a secondary battery, it is preferable to mix the active material (negative electrode active material), conductive agent and binder at a ratio of 68% by mass or more and 96% by mass or less, 2% by mass or more and 30% by mass or less, and 2% by mass or more and 30% by mass or less, respectively. By making the amount of the conductive agent 2% by mass or more, the current collection performance of the active material-containing layer can be improved. In addition, by making the amount of the binder 2% by mass or more, the binding property between the active material-containing layer and the current collector becomes sufficient, and excellent cycle performance can be expected. On the other hand, it is preferable to make the conductive agent and the binder 30% by mass or less, respectively, in order to increase the capacity.

[0068] The current collector is made of a material that is electrochemically stable at the potential at which lithium (Li) is inserted and removed from the active material. For example, when the active material is used as a negative electrode active material, the current collector is preferably made of copper, nickel, stainless steel, or aluminum, or an aluminum alloy containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si. The thickness of the current collector is preferably 5 μm or more and 20 μm or less. A current collector having such a thickness can balance the strength and weight of the electrode.

[0069] The current collector may also include a portion on the surface of which the negative electrode active material-containing layer is not formed, and this portion can function as a negative electrode current collecting tab.

[0070] The electrode can be produced, for example, by the following method. First, an active material, a conductive agent, and a binder are suspended in a solvent to prepare a slurry. This slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate of an active material-containing layer and a current collector. After that, the laminate is pressed. In this manner, an electrode is produced.

[0071] Alternatively, the electrode may be prepared by the following method: first, the active material, the conductive agent, and the binder are mixed to obtain a mixture, then the mixture is formed into pellets, and then the pellets are placed on a current collector to obtain an electrode.

[0072] The electrode according to the second embodiment includes the active material according to the first embodiment, and therefore the electrode can exhibit high capacity and excellent life performance.

[0073] (Third embodiment) According to the third embodiment, a secondary battery including a negative electrode, a positive electrode, and an electrolyte is provided. This secondary battery includes the electrode according to the second embodiment as the negative electrode. That is, the secondary battery according to the third embodiment includes an electrode including the active material according to the first embodiment as a battery active material as the negative electrode.

[0074] The secondary battery may further include a separator disposed between the positive electrode and the negative electrode. The negative electrode, the positive electrode, and the separator may constitute an electrode group. The electrolyte may be held in the electrode group.

[0075] Moreover, such a secondary battery can further include an exterior member that houses the electrode group and the electrolyte.

[0076] Furthermore, such a secondary battery may further include a negative electrode terminal electrically connected to the negative electrode and a positive electrode terminal electrically connected to the positive electrode.

[0077] Such a secondary battery may be, for example, a lithium secondary battery. The secondary battery also includes a non-aqueous electrolyte secondary battery that contains a non-aqueous electrolyte.

[0078] The negative electrode, the positive electrode, the electrolyte, the separator, the exterior member, the negative electrode terminal, and the positive electrode terminal will be described in detail below.

[0079] 1) Negative electrode The negative electrode may include a negative electrode current collector and a negative electrode active material-containing layer. The negative electrode current collector and the negative electrode active material-containing layer may be the current collector and the active material-containing layer that can be included in the electrode according to the second embodiment, respectively. The negative electrode active material-containing layer includes the active material according to the first embodiment as a negative electrode active material.

[0080] Among the details of the negative electrode, those parts that overlap with the details explained in the second embodiment will be omitted.

[0081] The density of the negative electrode active material-containing layer (excluding the current collector) is 1.8 g / cm 3 More than 2.8g / cm 3 A negative electrode having a density of the negative electrode active material-containing layer within this range is excellent in energy density and electrolyte retention. The density of the negative electrode active material-containing layer is preferably 2.1 g / cm or less. 3 More than 2.6g / cm 3 It is more preferable that:

[0082] The negative electrode can be produced, for example, by the same method as the electrode according to the second embodiment.

[0083] 2) Positive electrode The positive electrode can include a positive electrode current collector and a positive electrode active material-containing layer. The positive electrode active material-containing layer can be formed on one or both sides of the positive electrode current collector. The positive electrode active material-containing layer can contain a positive electrode active material, and optionally a conductive agent and a binder.

[0084] As the positive electrode active material, for example, an oxide or a sulfide can be used. The positive electrode may contain one type of compound alone as the positive electrode active material, or may contain a combination of two or more types of compounds. Examples of the oxide and the sulfide include compounds into which Li or Li ions can be inserted and desorbed.

[0085] Examples of such compounds include manganese dioxide (MnO2), iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide (e.g., Li x Mn2O4 or Li x MnO2; 0 < x ≦ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≦ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≦ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≦ 1, 0 < y < 1), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≦ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≦ 1, 0 < y < 2), lithium phosphate having an olivine structure (e.g., Li x FePO4; 0 < x ≦ 1, Li x Fe 1-y Mn y PO4; 0 < x ≦ 1, 0 < y ≦ 1, Li xCoPO4; 0 < x ≦ 1), iron sulfate (Fe2(SO4)3), vanadium oxide (e.g., V2O5), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≦ 1, 0 < y < 1, 0 < z < 1, y + z < 1) are included.

[0086] Among the above, examples of more preferable compounds as the positive electrode active material include lithium manganese composite oxide having a spinel structure (e.g., Li x Mn2O4; 0 < x ≦ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≦ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≦ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≦ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≦ 1, 0 < y < 2), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≦ 1, 0 < y < 1), lithium iron phosphate (e.g., Li x FePO4; 0 < x ≦ 1), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≦ 1, 0 < y < 1, 0 < z < 1, y + z < 1) are included. When these compounds are used as the positive electrode active material, the positive electrode potential can be increased.

[0087] When a room temperature molten salt is used as the electrolyte of the battery, lithium iron phosphate, Li xIt is preferable to use a positive electrode active material containing VPO4F (0≦x≦1), lithium manganese composite oxide, lithium nickel composite oxide, lithium nickel cobalt composite oxide, or a mixture thereof. These compounds have low reactivity with room temperature molten salts, so that the cycle life can be improved. Details of the room temperature molten salt will be described later.

[0088] The primary particle size of the positive electrode active material is preferably 100 nm or more and 1 μm or less. A positive electrode active material with a primary particle size of 100 nm or more is easy to handle in industrial production. A positive electrode active material with a primary particle size of 1 μm or less can smoothly diffuse lithium ions in the solid.

[0089] The specific surface area of ​​the positive electrode active material is 0.1 m 2 / g or more 10m 2 / g or less. 2 A positive electrode active material having a specific surface area of ​​10m / g or more can secure sufficient sites for absorbing and releasing Li ions. 2 A positive electrode active material having a specific surface area of ​​100 / g or less is easy to handle in industrial production and can ensure good charge-discharge cycle performance.

[0090] The binder is blended to fill the gaps between the dispersed positive electrode active material and to bind the positive electrode active material and the positive electrode current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.

[0091] The conductive agent is blended to improve current collection performance and reduce contact resistance between the positive electrode active material and the positive electrode current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, and carbonaceous materials such as graphite. One of these may be used as the conductive agent, or two or more may be combined and used as the conductive agent. The conductive agent may also be omitted.

[0092] In the positive electrode active material-containing layer, the positive electrode active material and the binder are preferably mixed in an amount of 80% by mass to 98% by mass and 2% by mass to 20% by mass, respectively.

[0093] By making the amount of binder 2% by mass or more, sufficient electrode strength can be obtained. In addition, the binder can function as an insulator. Therefore, by making the amount of binder 20% by mass or less, the amount of insulator contained in the electrode is reduced, and the internal resistance can be reduced.

[0094] When a conductive agent is added, the positive electrode active material, the binder, and the conductive agent are preferably mixed in proportions of 77% by mass or more and 95% by mass or less, 2% by mass or more and 20% by mass or less, and 3% by mass or more and 15% by mass or less, respectively.

[0095] By making the amount of the conductive agent 3% by mass or more, the above-mentioned effects can be achieved. Also, by making the amount of the conductive agent 15% by mass or less, the ratio of the conductive agent in contact with the electrolyte can be reduced. If this ratio is low, decomposition of the electrolyte during high-temperature storage can be reduced.

[0096] The positive electrode current collector is preferably an aluminum foil or an aluminum alloy foil containing one or more elements selected from Mg, Ti, Zn, Ni, Cr, Mn, Fe, Cu, and Si.

[0097] The thickness of the aluminum foil or aluminum alloy foil is preferably 5 μm or more and 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99 mass% or more. The content of transition metals such as iron, copper, nickel, and chromium contained in the aluminum foil or aluminum alloy foil is preferably 1 mass% or less.

[0098] The positive electrode current collector may also include a portion on the surface of which the positive electrode active material-containing layer is not formed, and this portion can function as a positive electrode current collecting tab.

[0099] The positive electrode can be produced, for example, by using a positive electrode active material in the same manner as in the electrode according to the second embodiment.

[0100] 3) Electrolytes The electrolyte may be, for example, a liquid nonaqueous electrolyte or a gel nonaqueous electrolyte. The liquid nonaqueous electrolyte is prepared by dissolving an electrolyte salt as a solute in an organic solvent. The concentration of the electrolyte salt is preferably 0.5 mol / L or more and 2.5 mol / L or less.

[0101] Examples of the electrolyte salt include lithium salts such as lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), and lithium bistrifluoromethylsulfonylimide (LiN(CF3SO2)2), and mixtures thereof. The electrolyte salt is preferably one that is difficult to oxidize even at high potentials, and LiPF6 is most preferred.

[0102] Examples of organic solvents include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyl tetrahydrofuran (2MeTHF), and dioxolane (DOX); chain ethers such as dimethoxyethane (DME) and diethoxyethane (DEE); γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These organic solvents can be used alone or as a mixed solvent.

[0103] The gelled non-aqueous electrolyte is prepared by combining a liquid non-aqueous electrolyte with a polymeric material, such as polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyethylene oxide (PEO), or a mixture thereof.

[0104] Alternatively, as the nonaqueous electrolyte, in addition to liquid nonaqueous electrolytes and gel nonaqueous electrolytes, room temperature molten salts containing lithium ions (ionic melts), polymer solid electrolytes, inorganic solid electrolytes, and the like may be used.

[0105] Room temperature molten salts (ionic melts) refer to organic salts consisting of a combination of organic cations and anions that can exist as a liquid at room temperature (15°C or higher and 25°C or lower). Room temperature molten salts include room temperature molten salts that exist as a liquid by themselves, room temperature molten salts that become liquid when mixed with an electrolyte salt, room temperature molten salts that become liquid when dissolved in an organic solvent, and mixtures of these. In general, the melting point of room temperature molten salts used in secondary batteries is 25°C or lower. In addition, organic cations generally have a quaternary ammonium skeleton.

[0106] The polymer solid electrolyte is prepared by dissolving an electrolyte salt in a polymer material and solidifying it.

[0107] The inorganic solid electrolyte is a solid substance that has Li-ion conductivity. Here, Li-ion conductivity is defined as having a Li-ion conductivity of 1×10 at 25°C. -6 It means that the inorganic solid electrolyte has a lithium ion conductivity of 1.0 S / cm or more. Examples of the inorganic solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes. Specific examples of the inorganic solid electrolyte are as follows.

[0108] The oxide-based solid electrolyte has a NASICON (Sodium (Na) Super Ionic Conductor) type structure and is represented by the general formula Li 1+x It is preferable to use a lithium phosphate solid electrolyte represented by Mα2(PO4)3. In the above general formula, Mα is, for example, one or more selected from the group consisting of titanium (Ti), germanium (Ge), strontium (Sr), zirconium (Zr), tin (Sn), aluminum (Al), and calcium (Ca). The subscript x is within the range of 0≦x≦2.

[0109] A specific example of a lithium phosphate solid electrolyte having a NASICON structure is Li 1+x Al x Ti 2-x LATP compound represented by (PO4)3, where 0.1≦x≦0.5; Li 1+x Al y Mβ 2-yA compound represented by (PO4)3, where Mβ is one or more selected from the group consisting of Ti, Ge, Sr, Zr, Sn, and Ca, 0 ≦ x ≦ 1, and 0 ≦ y ≦ 1; Li 1+x Al x Ge 2-x A compound represented by (PO4)3, where 0 ≦ x ≦ 2; and Li 1+x Al x Zr 2-x A compound represented by (PO4)3, where 0 ≦ x ≦ 2; Li 1+x+y Al x Mγ 2-x Si y P 3-y O 12 A compound represented by, where Mγ is one or more selected from the group consisting of Ti and Ge, 0 < x ≦ 2, and 0 ≦ y < 3; Li 1+2x Zr 1-x Ca x Examples of compounds represented by (PO4)3, where 0 ≦ x < 1, can be given.

[0110] In addition, as the oxide-based solid electrolyte, in addition to the above lithium phosphate solid electrolyte, Li x PO y N z An amorphous LIPON compound represented by, where 2.6 ≦ x ≦ 3.5, 1.9 ≦ y ≦ 3.8, and 0.1 ≦ z ≦ 1.3 (for example, Li 2.9 PO 3.3 N 0.46 ); A garnet-type structure La 5+x A x La 3-x Mδ2O 12 A compound represented by, where A is one or more selected from the group consisting of Ca, Sr, and Ba, Mδ is one or more selected from the group consisting of Nb and Ta, and 0 ≦ x ≦ 0.5; Li3Mδ 2-x L2O 12 A compound represented by, where Mδ is one or more selected from the group consisting of Nb and Ta, L may contain Zr, and 0 ≦ x ≦ 0.5; Li 7-3x Al x A compound represented by La3Zr3O 12 where 0 ≦ x ≦ 0.5; Li 5+x La3Mδ 2-x Zr x O12 where Mδ is at least one selected from the group consisting of Nb and Ta, and 0≦x≦2. LLZ compounds (e.g., Li7La3Zr2O 12 ); and La 2 / 3-x Li x Examples of such compounds include those represented by TiO3, where x is 0.3≦x≦0.7.

[0111] One or more of the above compounds can be used as the solid electrolyte. Two or more of the above solid electrolytes can also be used.

[0112] Alternatively, instead of the non-aqueous electrolyte, a liquid aqueous electrolyte or a gel aqueous electrolyte can be used as the electrolyte. The liquid aqueous electrolyte is prepared by dissolving, for example, the above-mentioned electrolyte salt as a solute in an aqueous solvent. The gel aqueous electrolyte is prepared by compounding the liquid aqueous electrolyte with the above-mentioned polymer material. As the aqueous solvent, a solution containing water can be used. The solution containing water may be pure water or a mixed solvent of water and an organic solvent.

[0113] 4) Separator The separator is formed, for example, from a porous film containing polyethylene (PE), polypropylene (PP), cellulose, or polyvinylidene fluoride (PVdF), or a synthetic resin nonwoven fabric. From the viewpoint of safety, it is preferable to use a porous film formed from polyethylene or polypropylene. This is because these porous films melt at a certain temperature and are capable of cutting off electric current.

[0114] 5) Exterior materials As the exterior member, for example, a container made of a laminate film or a metal container can be used.

[0115] The thickness of the laminate film is, for example, 0.5 mm or less, preferably 0.2 mm or less.

[0116] The laminate film is a multi-layer film including a plurality of resin layers and a metal layer interposed between the resin layers. The resin layers include polymeric materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably made of aluminum foil or aluminum alloy foil for weight reduction. The laminate film can be molded into the shape of the exterior member by sealing it by heat fusion.

[0117] The thickness of the wall of the metal container is, for example, 1 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less.

[0118] The metal container is made of, for example, aluminum or an aluminum alloy. The aluminum alloy preferably contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains transition metals such as iron, copper, nickel, and chromium, the content of the transition metals is preferably 100 ppm by mass or less.

[0119] The shape of the exterior member is not particularly limited. The shape of the exterior member may be, for example, flat (thin), rectangular, cylindrical, coin-shaped, or button-shaped. The exterior member can be appropriately selected depending on the battery dimensions and the application of the battery.

[0120] 6) Negative terminal The negative electrode terminal can be made of a material that is electrochemically stable at the Li absorption / release potential of the negative electrode active material and has electrical conductivity. Specifically, the material of the negative electrode terminal can be copper, nickel, stainless steel, aluminum, or an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The material of the negative electrode terminal is preferably aluminum or an aluminum alloy. The negative electrode terminal is preferably made of the same material as the negative electrode current collector in order to reduce the contact resistance with the negative electrode current collector.

[0121] 7) Positive terminal The positive electrode terminal has a potential range of 3V to 4.5V with respect to the redox potential of lithium (vs. Li / Li + ) and can be formed from a material that is electrically stable and conductive. Examples of the material for the positive electrode terminal include aluminum and an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The positive electrode terminal is preferably formed from the same material as the positive electrode current collector in order to reduce the contact resistance with the positive electrode current collector.

[0122] Next, the secondary battery according to the embodiment will be described more specifically with reference to the drawings.

[0123] Fig. 1 is a cross-sectional view showing an example of a secondary battery, and Fig. 2 is an enlarged cross-sectional view of part A of the secondary battery shown in Fig. 1.

[0124] The secondary battery 100 shown in Figures 1 and 2 includes a bag-shaped exterior member 2 shown in Figure 1, an electrode group 1 shown in Figures 1 and 2, and an electrolyte (not shown). The electrode group 1 and the electrolyte are stored in the bag-shaped exterior member 2. The electrolyte (not shown) is held in the electrode group 1.

[0125] The bag-shaped exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.

[0126] As shown in Fig. 1, the electrode group 1 is a flat wound-type electrode group. As shown in Fig. 2, the flat wound-type electrode group 1 includes a negative electrode 3, a separator 4, and a positive electrode 5. The separator 4 is interposed between the negative electrode 3 and the positive electrode 5.

[0127] The negative electrode 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b. In the negative electrode 3, in a portion located at the outermost shell of the wound-type electrode group 1, the negative electrode active material-containing layer 3b is formed only on the inner surface side of the negative electrode current collector 3a as shown in Fig. 2. In the other portions of the negative electrode 3, the negative electrode active material-containing layer 3b is formed on both sides of the negative electrode current collector 3a.

[0128] The positive electrode 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b formed on both sides of the positive electrode current collector 5a.

[0129] As shown in FIG. 1, the negative electrode terminal 6 and the positive electrode terminal 7 are located near the outer peripheral end of the wound electrode group 1. The negative electrode terminal 6 is connected to a portion located at the outermost shell of the negative electrode current collector 3a. The positive electrode terminal 7 is connected to a portion located at the outermost shell of the positive electrode current collector 5a. The negative electrode terminal 6 and the positive electrode terminal 7 extend to the outside from an opening of the bag-shaped exterior member 2. A thermoplastic resin layer is provided on the inner surface of the bag-shaped exterior member 2, and the opening is closed by heat sealing.

[0130] The secondary battery according to the embodiment is not limited to the secondary battery having the configuration shown in FIGS. 1 and 2, but may be a battery having the configuration shown in FIGS.

[0131] Fig. 3 is a partially cutaway perspective view showing a schematic diagram of another example of a secondary battery, and Fig. 4 is an enlarged cross-sectional view of part B of the secondary battery shown in Fig. 3.

[0132] The secondary battery 100 shown in Figures 3 and 4 includes an electrode group 1 shown in Figures 3 and 4, an exterior member 2 shown in Figure 3, and an electrolyte (not shown). The electrode group 1 and the electrolyte are housed in the exterior member 2. The electrolyte is held in the electrode group 1.

[0133] The exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.

[0134] The electrode group 1 is a laminated type electrode group, as shown in Fig. 4. The laminated type electrode group 1 has a structure in which negative electrodes 3 and positive electrodes 5 are alternately laminated with separators 4 interposed therebetween.

[0135] The electrode group 1 includes a plurality of negative electrodes 3. Each of the plurality of negative electrodes 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b supported on both sides of the negative electrode current collector 3a. The electrode group 1 also includes a plurality of positive electrodes 5. Each of the plurality of positive electrodes 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b supported on both sides of the positive electrode current collector 5a.

[0136] The negative electrode current collector 3a of each negative electrode 3 includes a portion on one side where the negative electrode active material-containing layer 3b is not supported on any surface. This portion serves as a negative electrode current collector tab 3c. As shown in FIG. 4, the negative electrode current collector tab 3c does not overlap with the positive electrode 5. The negative electrode current collector tabs 3c are electrically connected to a belt-shaped negative electrode terminal 6. The tip of the belt-shaped negative electrode terminal 6 is pulled out to the outside of the exterior member 2.

[0137] Although not shown, the positive electrode current collector 5a of each positive electrode 5 includes a portion on one side where the positive electrode active material-containing layer 5b is not supported on any surface. This portion serves as a positive electrode current collector tab. The positive electrode current collector tab does not overlap with the negative electrode 3, similar to the negative electrode current collector tab 3c. The positive electrode current collector tab is located on the opposite side of the electrode group 1 to the negative electrode current collector tab 3c. The positive electrode current collector tab is electrically connected to a strip-shaped positive electrode terminal 7. The tip of the strip-shaped positive electrode terminal 7 is located on the opposite side of the negative electrode terminal 6 and is drawn out to the outside of the exterior member 2.

[0138] The secondary battery according to the third embodiment contains in its negative electrode the active material according to the first embodiment, and therefore the secondary battery can exhibit high capacity and excellent life performance.

[0139] (Embodiment 4) According to a fourth embodiment, there is provided a battery pack including a plurality of secondary batteries according to the third embodiment.

[0140] In such a battery pack, the individual cells may be electrically connected in series or parallel, or may be arranged in a combination of series and parallel connections.

[0141] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.

[0142] Fig. 5 is a perspective view showing an example of a battery pack. The battery pack 200 shown in Fig. 5 includes five cells 100a to 100e, four bus bars 21, a positive electrode lead 22, and a negative electrode lead 23. Each of the five cells 100a to 100e is a secondary battery according to the third embodiment.

[0143] The bus bar 21 connects, for example, the negative electrode terminal 6 of one cell 100a and the positive electrode terminal 7 of the adjacent cell 100b. In this way, the five cells 100 are connected in series by the four bus bars 21. That is, the battery pack 200 in FIG. 5 is a five-series battery pack. Although no example is shown, in a battery pack including a plurality of cells electrically connected in parallel, for example, the plurality of negative electrode terminals are connected to each other by a bus bar and the plurality of positive electrode terminals are connected to each other by a bus bar, so that the plurality of cells are electrically connected to each other.

[0144] The positive electrode terminal 7 of at least one of the five cells 100a to 100e is electrically connected to a positive electrode lead 22 for external connection. Also, the negative electrode terminal 6 of at least one of the five cells 100a to 100e is electrically connected to a negative electrode lead 23 for external connection.

[0145] The battery pack according to the fourth embodiment includes the secondary battery according to the third embodiment, and therefore can exhibit high capacity and excellent life performance.

[0146] Fifth embodiment According to a fifth embodiment, there is provided a battery pack. The battery pack includes the battery assembly according to the fourth embodiment. The battery pack may include a single secondary battery according to the third embodiment, instead of the battery assembly according to the fourth embodiment.

[0147] Such a battery pack may further include a protection circuit. The protection circuit has a function of controlling charging and discharging of the secondary battery. Alternatively, a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source may be used as the protection circuit for the battery pack.

[0148] The battery pack may further include an external terminal for current flow. The external terminal for current flow is for outputting current from the secondary battery to the outside and / or inputting current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, current is supplied to the outside through the external terminal for current flow. When the battery pack is charged, a charging current (including regenerative energy from the power of an automobile or the like) is supplied to the battery pack through the external terminal for current flow.

[0149] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.

[0150] Fig. 6 is an exploded perspective view showing an example of a battery pack, and Fig. 7 is a block diagram showing an example of an electric circuit of the battery pack shown in Fig. 6.

[0151] The battery pack 300 shown in Figs. 6 and 7 includes a container 31, a lid 32, a protective sheet 33, a battery pack 200, a printed wiring board 34, wiring 35, and an insulating plate (not shown).

[0152] 6 is a bottomed, square container having a rectangular bottom. The container 31 is configured to be able to accommodate a protective sheet 33, a battery pack 200, a printed wiring board 34, and wiring 35. The lid 32 has a rectangular shape. The lid 32 covers the container 31 to accommodate the battery pack 200 and the like. Although not shown, the container 31 and the lid 32 are provided with openings or connection terminals for connection to an external device or the like.

[0153] The battery pack 200 includes a plurality of cells 100, a positive electrode lead 22, a negative electrode lead 23, and an adhesive tape 24.

[0154] At least one of the plurality of unit cells 100 is a secondary battery according to the third embodiment. Each of the plurality of unit cells 100 is electrically connected in series as shown in FIG. 7. The plurality of unit cells 100 may be electrically connected in parallel, or may be connected in a combination of series and parallel connections. When the plurality of unit cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.

[0155] The adhesive tape 24 fastens the plurality of unit cells 100. The plurality of unit cells 100 may be fixed using heat shrink tape instead of the adhesive tape 24. In this case, the protective sheets 33 are disposed on both side surfaces of the battery pack 200, the heat shrink tape is wrapped around the battery pack 200, and the heat shrink tape is then thermally shrunk to bind the plurality of unit cells 100 together.

[0156] One end of the positive electrode lead 22 is connected to the battery pack 200. One end of the positive electrode lead 22 is electrically connected to the positive electrode of one or more cells 100. One end of the negative electrode lead 23 is connected to the battery pack 200. One end of the negative electrode lead 23 is electrically connected to the negative electrode of one or more cells 100.

[0157] The printed wiring board 34 is disposed along one of the short side surfaces of the inner surface of the container 31. The printed wiring board 34 includes a positive connector 342, a negative connector 343, a thermistor 345, a protection circuit 346, wiring 342a and 343a, an external terminal 350 for supplying electricity, a positive wiring (positive wiring) 348a, and a negative wiring (negative wiring) 348b. One main surface of the printed wiring board 34 faces one side of the battery pack 200. An insulating plate (not shown) is interposed between the printed wiring board 34 and the battery pack 200.

[0158] The other end 22a of the positive electrode lead 22 is electrically connected to the positive electrode connector 342. The other end 23a of the negative electrode lead 23 is electrically connected to the negative electrode connector 343.

[0159] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each of the cells 100, and transmits a detection signal to the protection circuit 346.

[0160] The external terminal 350 for current supply is fixed to the other main surface of the printed wiring board 34. The external terminal 350 for current supply is electrically connected to a device present outside the battery pack 300. The external terminal 350 for current supply includes a positive terminal 352 and a negative terminal 353.

[0161] The protection circuit 346 is fixed to the other main surface of the printed wiring board 34. The protection circuit 346 is connected to the positive terminal 352 via a positive wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via a negative wiring 348b. The protection circuit 346 is also electrically connected to the positive electrode connector 342 via a wiring 342a. The protection circuit 346 is electrically connected to the negative electrode connector 343 via a wiring 343a. Furthermore, the protection circuit 346 is electrically connected to each of the plurality of single cells 100 via the wiring 35.

[0162] The protective sheet 33 is disposed on both inner surfaces in the long side direction of the container 31 and on the inner surface in the short side direction that faces the printed wiring board 34 via the battery pack 200. The protective sheet 33 is made of, for example, resin or rubber.

[0163] The protection circuit 346 controls charging and discharging of the multiple cells 100. In addition, the protection circuit 346 cuts off electrical connection between the protection circuit 346 and external terminals 350 (positive terminal 352, negative terminal 353) for supplying electricity to an external device, based on a detection signal transmitted from the thermistor 345, or a detection signal transmitted from each of the cells 100 or the battery pack 200.

[0164] An example of the detection signal transmitted from the thermistor 345 is a signal that detects that the temperature of the cell 100 is equal to or higher than a predetermined temperature. An example of the detection signal transmitted from each cell 100 or the battery pack 200 is a signal that detects overcharging, overdischarging, and overcurrent of the cell 100. When detecting overcharging or the like for each cell 100, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 100.

[0165] The protection circuit 346 may be a circuit included in a device (such as an electronic device or an automobile) that uses the battery pack 300 as a power source.

[0166] As described above, the battery pack 300 includes the external terminal 350 for current supply. Therefore, the battery pack 300 can output a current from the assembled battery 200 to an external device and input a current from the external device to the assembled battery 200 via the external terminal 350 for current supply. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 is supplied to the external device through the external terminal 350 for current supply. When the battery pack 300 is charged, a charging current from the external device is supplied to the battery pack 300 through the external terminal 350 for current supply. When the battery pack 300 is used as an in-vehicle battery, regenerative energy of the vehicle's power can be used as the charging current from the external device.

[0167] The battery pack 300 may include a plurality of assembled batteries 200. In this case, the assembled batteries 200 may be connected in series, in parallel, or in a combination of series and parallel connections. The printed wiring board 34 and the wiring 35 may be omitted. In this case, the positive electrode lead 22 and the negative electrode lead 23 may be used as a positive terminal 352 and a negative terminal 353, respectively, of the external terminal 350 for current supply.

[0168] Such a battery pack is used in applications that require excellent cycle performance, for example, when a large current is drawn. Specifically, the battery pack is used, for example, as a power source for electronic devices, a stationary battery, or an on-board battery for various vehicles. An example of the electronic device is a digital camera. The battery pack is particularly suitable for use as an on-board battery.

[0169] The battery pack according to the fifth embodiment includes the secondary battery according to the third embodiment or the battery pack according to the fourth embodiment, and therefore can exhibit high capacity and excellent life performance.

[0170] Sixth embodiment According to a sixth embodiment, a vehicle is provided. The vehicle is equipped with the battery pack according to the fifth embodiment.

[0171] In such a vehicle, the battery pack, for example, recovers regenerative energy of the vehicle's motive power. The vehicle may include a mechanism (regenerator) that converts the kinetic energy of the vehicle into regenerative energy.

[0172] Examples of vehicles include, for example, two to four wheel hybrid electric vehicles, two to four wheel electric vehicles, power assisted bicycles, and rail vehicles.

[0173] The mounting position of the battery pack in the vehicle is not particularly limited. For example, when the battery pack is mounted in an automobile, the battery pack can be mounted in the engine compartment, the rear of the vehicle body, or under the seat of the vehicle.

[0174] The vehicle may be equipped with a plurality of battery packs. In this case, the batteries included in each battery pack may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. For example, when each battery pack includes a battery pack, the battery packs may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. Alternatively, when each battery pack includes a single battery, the batteries may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections.

[0175] Next, an example of a vehicle according to an embodiment will be described with reference to the drawings.

[0176] FIG. 8 is a partially see-through view that illustrates a schematic example of a vehicle.

[0177] A vehicle 400 shown in Fig. 8 includes a vehicle body 40 and a battery pack 300 according to the fifth embodiment. In the example shown in Fig. 8, the vehicle 400 is a four-wheeled automobile.

[0178] The vehicle 400 may be equipped with a plurality of battery packs 300. In this case, the batteries (e.g., single cells or assembled batteries) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series and parallel connections.

[0179] 8 illustrates an example in which the battery pack 300 is mounted in an engine room located in the front of the vehicle body 40. As described above, the battery pack 300 may be mounted, for example, in the rear of the vehicle body 40 or under a seat. This battery pack 300 can be used as a power source for the vehicle 400. In addition, this battery pack 300 can recover regenerative energy for the motive power of the vehicle 400.

[0180] Next, an embodiment of a vehicle according to the present embodiment will be described with reference to FIG.

[0181] Fig. 9 is a diagram illustrating an example of a control system for an electrical system in a vehicle. The vehicle 400 illustrated in Fig. 9 is an electric vehicle.

[0182] The vehicle 400 shown in FIG. 9 comprises a vehicle body 40, a vehicle power supply 41, a vehicle ECU (ECU: Electric Control Unit) 42 which is a higher-level control device of the vehicle power supply 41, an external terminal (terminal for connecting to an external power supply) 43, an inverter 44, and a drive motor 45.

[0183] The vehicle 400 has a vehicle power supply 41 mounted, for example, in an engine compartment, the rear of the vehicle body, or under a seat. Note that in the vehicle 400 shown in Fig. 9, the mounting location of the vehicle power supply 41 is shown diagrammatically.

[0184] The vehicle power supply 41 includes a plurality of (eg, three) battery packs 300a, 300b, and 300c, a battery management unit (BMU) 411, and a communication bus 412.

[0185] The battery pack 300a includes an assembled battery 200a and an assembled battery monitoring device 301a (for example, VTM: Voltage Temperature Monitoring). The battery pack 300b includes an assembled battery 200b and an assembled battery monitoring device 301b. The battery pack 300c includes an assembled battery 200c and an assembled battery monitoring device 301c. The battery packs 300a to 300c are battery packs similar to the above-mentioned battery pack 300, and the assembled batteries 200a to 200c are assembled batteries similar to the above-mentioned battery pack 200. The assembled batteries 200a to 200c are electrically connected in series. The battery packs 300a, 300b, and 300c can be removed independently and replaced with another battery pack 300.

[0186] Each of the assembled batteries 200a to 200c includes a plurality of unit cells connected in series. At least one of the plurality of unit cells is the secondary battery according to the third embodiment. Each of the assembled batteries 200a to 200c is charged and discharged via a positive terminal 413 and a negative terminal 414.

[0187] The battery management device 411 communicates with the assembled battery monitoring devices 301a to 301c, and collects information on the voltage, temperature, and the like of each of the cells 100 included in the assembled batteries 200a to 200c included in the vehicle power supply 41. In this way, the battery management device 411 collects information on the maintenance of the vehicle power supply 41.

[0188] The battery management unit 411 and the assembled battery monitoring units 301a to 301c are connected via a communication bus 412. In the communication bus 412, one set of communication lines is shared by a plurality of nodes (the battery management unit 411 and one or more assembled battery monitoring units 301a to 301c). The communication bus 412 is a communication bus configured based on, for example, the CAN (Control Area Network) standard.

[0189] The battery pack monitoring devices 301a to 301c measure the voltage and temperature of each of the cells constituting the battery packs 200a to 200c based on commands communicated from the battery management device 411. However, the temperature can be measured at only a few points per battery pack, and it is not necessary to measure the temperatures of all the cells.

[0190] The vehicle power supply 41 may also have an electromagnetic contactor (for example, a switch device 415 shown in FIG. 9) that switches between the presence and absence of an electrical connection between the positive terminal 413 and the negative terminal 414. The switch device 415 includes a pre-charge switch (not shown) that is turned on when the assembled batteries 200a-200c are charged, and a main switch (not shown) that is turned on when the output from the assembled batteries 200a-200c is supplied to a load. Each of the pre-charge switch and the main switch includes a relay circuit (not shown) that is switched on or off by a signal supplied to a coil disposed in the vicinity of the switch element. The electromagnetic contactor such as the switch device 415 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 that controls the operation of the entire vehicle 400.

[0191] The inverter 44 converts the input DC voltage into a three-phase alternating current (AC) high voltage for driving the motor. The three-phase output terminals of the inverter 44 are connected to the three-phase input terminals of the drive motor 45. The inverter 44 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 for controlling the operation of the entire vehicle. By controlling the inverter 44, the output voltage from the inverter 44 is adjusted.

[0192] The drive motor 45 rotates by electric power supplied from the inverter 44. A driving force generated by the rotation of the drive motor 45 is transmitted to the axles and drive wheels W via, for example, a differential gear unit.

[0193] Although not shown, the vehicle 400 is also equipped with a regenerative braking mechanism (regenerator). The regenerative braking mechanism rotates the drive motor 45 when the vehicle 400 is braked, and converts kinetic energy into regenerative energy as electrical energy. The regenerative energy recovered by the regenerative braking mechanism is input to the inverter 44 and converted into a direct current. The converted direct current is input to the vehicle power source 41.

[0194] One terminal of a connection line L1 is connected to the negative terminal 414 of the vehicle power supply 41. The other terminal of the connection line L1 is connected to a negative input terminal 417 of the inverter 44. A current detection unit (current detection circuit) 416 in the battery management device 411 is provided between the negative terminal 414 and the negative input terminal 417 on the connection line L1.

[0195] One terminal of a connection line L2 is connected to the positive electrode terminal 413 of the vehicle power supply 41. The other terminal of the connection line L2 is connected to a positive electrode input terminal 418 of the inverter 44. A switch device 415 is provided in the connection line L2 between the positive electrode terminal 413 and the positive electrode input terminal 418.

[0196] The external terminal 43 is connected to the battery management unit 411. The external terminal 43 can be connected to, for example, an external power source.

[0197] In response to operational inputs from the driver or the like, the vehicle ECU 42 coordinates with other management devices and control devices including the battery management device 411 to control the vehicle power supply 41, the switch device 415, the inverter 44, etc. Through the coordinated control of the vehicle ECU 42, etc., the output of power from the vehicle power supply 41 and the charging of the vehicle power supply 41 are controlled, and the entire vehicle 400 is managed. Data relating to the maintenance of the vehicle power supply 41, such as the remaining capacity of the vehicle power supply 41, is transferred between the battery management device 411 and the vehicle ECU 42 via a communication line.

[0198] The vehicle according to the sixth embodiment is equipped with the battery pack according to the fifth embodiment, and therefore can exhibit high performance and high reliability. EXAMPLES

[0199] The above embodiment will now be described in more detail with reference to examples.

[0200] <Synthesis method> Example 1 The molybdenum-containing niobium titanium oxide was synthesized as follows.

[0201] Oxalic acid was dissolved in water to prepare a 1M oxalic acid solution. Titanium tetraisopropoxide (C 12 H 28 O4Ti) was dissolved in a solution, and ammonium niobium oxalate hydrate (C4H4NNbO9 xH2O) and ammonium molybdate ((NH4)6Mo7O 24 4H2O) was dissolved in these Ti sources (C 12 H 28 O4Ti), Nb source (C4H4NNbO9·xH2O) and Mo source ((NH4)6Mo7O 24 The ratios of ammonium hydroxide, ammonium hydroxide, and ammonium hydroxide (4H2O) were 7.4 mass%, 91.6 mass%, and 1 mass%, respectively. The solution was then neutralized by dropping aqueous ammonia into it to obtain a white gel. This gel was dried using a spray dryer to obtain a precursor. This precursor was placed in a cylindrical alumina crucible with an aspect ratio of about 1 up to the top, and densely packed by tapping. Using an electric furnace, calcination was performed in air at 300°C for 1 hour and heat treatment was performed at 900°C for 4 hours in succession to obtain the active material of Example 1.

[0202] Example 2 An active material of Example 2 was obtained by carrying out synthesis in the same manner as in Example 1, except that the proportions of the Ti source, the Nb source, and the Mo source were changed to 5.3 mass %, 92.1 mass %, and 2.6 mass %, respectively.

[0203] Example 3 An active material of Example 3 was obtained by carrying out synthesis in the same manner as in Example 1, except that the proportions of the Ti source, the Nb source, and the Mo source were changed to 3.5 mass %, 92.6 mass %, and 3.9 mass %, respectively.

[0204] Example 4 An active material of Example 4 was obtained by carrying out synthesis in the same manner as in Example 1, except that the proportions of the Ti source, the Nb source, and the Mo source were changed to 8.1 mass %, 90.7 mass %, and 1.2 mass %, respectively.

[0205] Example 5 An active material of Example 5 was obtained by carrying out synthesis in the same manner as in Example 1, except that the proportions of the Ti source, the Nb source, and the Mo source were changed to 9.1 mass %, 88.9 mass %, and 2.0 mass %, respectively.

[0206] Example 6 An active material of Example 6 was obtained by carrying out synthesis in the same manner as in Example 1, except that the proportions of the Ti source, the Nb source, and the Mo source were changed to 8.0 mass %, 89.2 mass %, and 2.8 mass %, respectively.

[0207] Comparative Example 1 An active material of Comparative Example 1 was obtained by carrying out synthesis in the same manner as in Example 1, except that the proportions of the Ti source, the Nb source, and the Mo source were changed to 7.8 mass %, 92.2 mass %, and 0 mass %, respectively.

[0208] The results of measuring the composition of the active materials synthesized in Examples 1 to 6 and Comparative Example 1 are summarized in Table 1 below. In Table 1, the active material compositions are shown together with the compositions of the general formula Ti x-y Mo y Nb 12-x O 29+z The subscripts x, y, and z represent the active material compositions shown in Table 1 when the active material compositions are expressed by the general formula, but when converted to fit the general formula, the subscripts represent the active material compositions shown in Table 1.

[0209] [Table 1]

[0210] <Powder X-ray diffraction measurement and peak intensity ratio I 25 / I 24 Calculation of > The active material powders obtained in Examples 1 to 6 and Comparative Example 1 were subjected to the powder X-ray diffraction measurement described in the first embodiment under the conditions of a sampling interval of 0.01° and a scan speed of 2° / min. In the obtained diffraction spectrum, the peak intensity ratio I 25 / I 24 was calculated.

[0211] As an example, the diffraction spectra obtained by powder X-ray diffraction for the active materials according to Examples 1 to 4 and Comparative Example 1 are shown in FIG. 10. As shown in the figure, for each of the active materials according to Examples 1 to 4, the X-ray diffraction curve included both the first peak P1 in the range of 23.5° to 24.5° and the second peak P2 in the range of 25.0° to 25.5°. For the active material according to Comparative Example 1, the first peak P1 was observed, but no peak was observed in the range of 25.0° to 25.5°. The diffraction curve for Comparative Example 1 also included a peak P0 on the wider angle side than the first peak P1, but the peak top of the peak P0 was at a position of 2θ<25.0°.

[0212] <Electrochemical measurements> First, 100% by mass of the active material powder obtained in each example, 10% by mass of acetylene black as a conductive agent, 5% by mass of carbon nanofiber, 10% by mass of polyvinylidene fluoride (PVdF) as a binder, and N-methylpyrrolidone (NMP) were added and mixed to obtain a slurry. This slurry was applied to one side of a current collector made of aluminum foil with a thickness of 15 μm, dried, and pressed to obtain an electrode density of 2.4 g / cm. 3 The electrodes were prepared as follows.

[0213] Next, an electrolyte solution was prepared by dissolving LiPF6 supporting salt at a concentration of 1 mol / L in a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:2.

[0214] The obtained electrode was used as a working electrode, and Li metal was used as a counter electrode and a reference electrode. A glass cell was prepared using an electrolyte to evaluate the electrochemical performance.

[0215] In this embodiment, the glass cell for measurement uses lithium metal as the counter electrode, so that the electrode potentials of the embodiment and comparative example are nobler than the counter electrode and operate as positive electrodes. Therefore, the definitions of charge and discharge are reversed when the electrodes of the embodiment and comparative example are used as negative electrodes. Here, to avoid confusion, in this embodiment, the direction in which lithium ions are inserted into the electrode is unified as charge, and the direction in which they are removed is unified as discharge. The active material of this embodiment operates as a negative electrode when combined with a known positive electrode material.

[0216] The electrochemical measurement cell thus fabricated was charged and discharged in the potential range of 0.7 V to 3.0 V based on the metallic lithium electrode. The charge and discharge current value was set to 0.2 C (time discharge rate), and the 0.2 C discharge capacity was confirmed at room temperature. The 0.2 C discharge capacity value is an index of energy density.

[0217] Next, a life test was performed at room temperature on each cell by repeatedly charging and discharging at 1C in a potential range of 0.7V to 3.0V based on the metallic lithium electrode. 100 cycles of charging and discharging were repeated under these conditions (one cycle is one charge and one discharge), and the 0.2C discharge capacity was measured again. The cycle capacity retention rate was calculated by dividing the discharge capacity after 100 cycles by the discharge capacity before the cycles (cycle capacity retention rate = (0.2C discharge capacity after 100 cycles / 0.2C discharge capacity before 100 cycles) × 100%).

[0218] The above results are summarized in Table 2. Specifically, the peak intensity ratio I 25 / I 24 , 0.2C discharge capacity, and cycle capacity retention rate after 100 charge / discharge cycles, respectively.

[0219] [Table 2]

[0220] As shown in Table 2, in the XRD spectra of Examples 1 to 6, the peak intensity ratio I 25 / I 24 was 0.5 or more. In contrast, in Comparative Example 1, no second peak appeared within the range of diffraction angles 2θ of 25.0° to 25.5°. As a result of the electrochemical measurement, the electrochemical measurement cells according to Examples 1 to 6 exhibited cycle capacity retention rates equal to or higher than that of the cell according to Comparative Example 1, while achieving higher discharge capacity. From these results, it can be seen that the peak intensity ratio I 25 / I 24 It can be seen that in the Mo-containing niobium titanium oxide, in which both are 0.5 or more, the capacity is improved while maintaining excellent cycle life performance.

[0221] According to at least one of the above-described embodiments and examples, an active material is provided. The active material includes a Mo-containing niobium titanium oxide having a monoclinic structure. In the X-ray diffraction spectrum of the active material, the intensity I of a first peak appearing within the range of 23.5°≦2θ≦24.5° is 24 Intensity of the second peak appearing within the range of 25.0°≦2θ≦25.5° for 25 Ratio I 25 / I 24 is 0.5 or more. This active material can realize a secondary battery that can exhibit high capacity and excellent cycle life performance.

[0222] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims.

[0223] Several embodiments according to the present invention will be described below. [1] Contains Mo-containing niobium titanium oxide having a monoclinic crystal structure, Intensity I of the first peak appearing in the range of 2θ from 23.5° to 24.5° in the X-ray diffraction spectrum 24 Intensity of the second peak appearing within the 2θ range of 25.0° to 25.5° for 25 Ratio I 25 / I 24 is 0.5 or more. [2] Ratio I 25 / I 24 The active material according to [1], wherein [3] The Mo-containing niobium titanium oxide has the general formula Ti x-y Mo y Nb 12-x O 29+z The active material according to [1] or [2], having a composition represented by the formula: 1.5≦x≦2.2, 0<y≦0.7x, and −3≦z≦1. [4] An electrode comprising the active material according to any one of [1] to [3]. [5] The electrode according to [4], wherein the electrode includes an active material-containing layer that contains the active material. [6] A positive electrode; A negative electrode; and an electrolyte, The negative electrode is the electrode according to [4] or [5]. [7] A battery pack comprising the secondary battery described in [6]. [8] An external terminal for supplying current; Protection circuit and The battery pack according to [7], further comprising: [9] A battery comprising a plurality of the secondary batteries, The battery pack according to [7] or [8], wherein the secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.

[10] A vehicle equipped with a battery pack described in any one of [7] to [9].

[11] A vehicle as described in

[10] , including a mechanism for converting kinetic energy of the vehicle into regenerative energy. [Explanation of symbols]

[0224] 1...electrode group, 2...exterior member, 3...negative electrode, 3a...negative electrode current collector, 3b...negative electrode active material-containing layer, 3c...negative electrode current collector tab, 4...separator, 5...positive electrode, 5a...positive electrode current collector, 5b...positive electrode active material-containing layer, 6...negative electrode terminal, 7...positive electrode terminal, 21...bus bar, 22...positive electrode side lead, 22a...other end, 23...negative electrode side lead, 23a...other end, 24...adhesive tape, 31...container, 32...lid, 33...protective sheet, 34...printed wiring board, 35...wiring, 40...vehicle body, 41...vehicle power source, 42...electrical control device, 43...external terminal, 44...inverter, 45...driving motor, 100...secondary battery, 200...battery pack, 200a...battery pack, 200b...battery pack, 200c...battery pack, 300...battery pack, 30 0a...battery pack, 300b...battery pack, 300c...battery pack, 301a...assembled battery monitoring device, 301b...assembled battery monitoring device, 301c...assembled battery monitoring device, 342...positive connector, 343...negative connector, 345...thermistor, 346...protection circuit, 342a...wiring, 343a...wiring, 350...external terminal for energization, 352...positive terminal, 353...negative terminal, 348a...positive wiring, 348b...negative wiring, 400...vehicle, 411...battery management device, 412...communication bus, 413...positive terminal, 414...negative terminal, 415...switch device, 416...current detection unit, 417...negative input terminal, 418...positive input terminal, L1...connection line, L2...connection line, W...drive wheel.

Claims

1. The present invention includes a Mo-containing niobium titanium oxide having a monoclinic crystal structure, Intensity I of the first peak appearing in the range of 2θ from 23.5° to 24.5° in the X-ray diffraction spectrum 24 Intensity I of the second peak appearing within the range of 2θ from 25.0° to 25.5° 25 Ratio I 25 / I 24 is 0.5 or more.

2. The ratio I 25 / I 24 The active material according to claim 1 , wherein n is 0.9 or less.

3. The Mo-containing niobium titanium oxide has the general formula Ti x-y Mo y Nb 12-x O 29+z 2. The active material of claim 1 having a composition represented by the formula: where 1.5≦x≦2.2, 0<y≦0.7x, and −3≦z≦1.

4. An electrode comprising the active material according to claim 1 .

5. The electrode according to claim 4 , wherein the electrode comprises an active material-containing layer that contains the active material.

6. A positive electrode and A negative electrode; and an electrolyte, A secondary battery, wherein the negative electrode is the electrode according to claim 4 .

7. A battery pack comprising the secondary battery according to claim 6.

8. An external terminal for supplying electricity; Protection circuit and The battery pack of claim 7 further comprising:

9. A battery comprising a plurality of the secondary batteries, The battery pack according to claim 7 , wherein the secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.

10. A vehicle equipped with the battery pack according to claim 7.

11. The vehicle according to claim 10, further comprising a mechanism for converting kinetic energy of the vehicle into regenerative energy.

Citation Information

Patent Citations

  • Active material for batteries, method for manufacturing the same, nonaqueous electrolyte battery, and battery pack

    JP2015084321A

  • Active material for batteries, nonaqueous electrolyte battery and battery pack

    JP2016177972A

  • Nonaqueous electrolyte battery, battery pack and vehicle

    JP2017168318A

  • Li / Na-ion battery anode materials

    JP2023501077A

  • Preparation method of lithium ion battery negative material titanium niobate

    CN105633456A