Electrode, film-electrode joint, electrochemical cell, stack and electrolytic apparatus
The electrodes with a porous titanium base and titanium oxide coatings, combined with Ir and Ru catalysts, address durability issues in PEMEC, enabling efficient hydrogen and ammonia electrolysis with reduced noble metal consumption.
Patent Information
- Application Number
- JP2024003033
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-17
- Filing Date
- 2024-01-12
- Publication Date
- 2024-10-01
AI Technical Summary
Existing electrochemical cells, particularly polymer electrolyte membrane electrolysis cells (PEMEC), face challenges in achieving sufficient durability and electrolytic properties due to the use of noble metal catalysts like platinum and iridium, which are costly and may not be suitable for large-scale hydrogen generation or ammonia electrolysis.
The electrodes are designed with a porous titanium base material coated with alternating layers of electrolytic catalyst and titanium oxide coatings, where the first coating on the catalyst side and second coating on the opposite side have specific thickness relationships to enhance durability, using noble metal oxides like Ir and Ru for the catalyst layer.
The design provides high durability and maintains low cell voltage over extended operation times, ensuring efficient hydrogen generation and ammonia electrolysis with reduced noble metal usage.
Smart Images

Figure 2024132874000001_ABST
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE Embodiments of the invention relate to electrodes, membrane electrode assemblies, electrochemical cells, stacks and electrolyzers. [Background technology]
[0002] In recent years, electrochemical cells have been actively researched. For example, polymer electrolyte membrane electrolysis cells (PEMEC) are expected to be used to generate hydrogen in large-scale energy storage systems. To ensure sufficient durability and electrolytic properties, platinum (Pt) nanoparticle catalysts are generally used in the cathode of PEMEC, and precious metal catalysts such as iridium (Ir) nanoparticle catalysts are generally used in the anode. Methods of obtaining hydrogen from ammonia are also being investigated. They can also be used as the anode of electrolysis devices that electrolyze carbon dioxide to produce organic compounds such as methanol and ethylene, and carbon monoxide. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 3743472 [Patent Document 2] JP 2017-50542 A [Patent Document 3] JP 2009-256751 A [Patent Document 4] Japanese Unexamined Patent Publication No. 62-207855 [Patent Document 5] JP 2018-156798 A [Patent Document 6] International Publication No. 2022 / 210655 [Patent Document 7] JP 2012-204221 A [Non-patent literature]
[0004] [Non-Patent Document 1] Let's make colorful titanium plates using anodizing Akita University Faculty of Science and Technology, Department of Technology February 10, 2023 [Non-Patent Document 2] Relationship between Oxide Film and Corrosion of Porous Titanium Oita National College of Technology Bulletin No. 47 (November 2010) [Non-Patent Document 3] Thermal Oxidation and Anodizing of Titanium Kinki Aluminum Surface Treatment Research Association Journal No. 167 1994 [Non-Patent Document 4] Flash lamp annealing (Wikipedia URL: https: / / ja.wikipedia.org / wiki / %E3%83%95%E3%83%A9%E3%83%83%E3%82%B7%E3%83%A5%E3%83%A9%E3%83%B3%E3%83%97%E3%82%A2%E3%83%8B%E3%83%BC%E3%83%AB) Summary of the Invention [Problem to be solved by the invention]
[0005] The embodiments provide highly durable electrodes. [Means for solving the problem]
[0006] The electrode of the embodiment includes a porous titanium substrate and an electrolysis catalyst layer provided on the titanium substrate, the electrolysis catalyst layer being formed by alternatingly laminating sheet layers and gap layers. The titanium substrate includes a first coating containing titanium oxide on the electrolysis catalyst layer side. The titanium substrate includes a second coating containing titanium oxide on the side opposite to the electrolysis catalyst layer side. [Brief description of the drawings]
[0007] [Figure 1] FIG. 2 is a schematic diagram of an electrode according to an embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a catalyst layer according to an embodiment. [Diagram 3] 4 is an analysis spot of an embodiment. [Figure 4]Graph of an embodiment. [Diagram 5] 1 is a cross-sectional image of an electrode 100. [Figure 6] 1 is a cross-sectional image of an electrode 100. [Figure 7] 1 is a cross-sectional image of an electrode 100. [Figure 8] 1 is a cross-sectional image of an electrode 100. [Figure 9] 1 is a schematic diagram of a membrane electrode assembly according to an embodiment. [Figure 10] FIG. 1 is a schematic diagram of an electrochemical cell according to an embodiment. [Figure 11] FIG. 2 is a schematic diagram of a stack according to an embodiment. [Figure 12] FIG. 1 is a conceptual diagram of an electrolysis device according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In the following description, the same components will be given the same reference numerals, and the description of components that have already been described will be omitted as appropriate.
[0009] The physical properties in the specification are values at a temperature of 25°C and a pressure of 1 atom. The thickness of each component is the average value of the distance in the stacking direction.
[0010] (First embodiment) The first embodiment relates to an electrode. A schematic cross-sectional view of an electrode 100 according to the embodiment is shown in FIG.
[0011] In the embodiment, the catalyst layer 2 is used as an electrolytic catalyst. The electrolytic reaction produces, for example, hydrogen from water or ammonia. The electrolytic reaction produces, for example, carbon monoxide from carbon dioxide. The catalyst layer 2 is also used as an anode catalyst in the electrolytic production of ammonia.
[0012] The electrode 100 of the first embodiment is used, for example, as an anode for water electrolysis. When the catalyst layer 2 further contains a catalyst for a fuel cell, the electrode 100 of the embodiment is also used as an oxygen electrode of a fuel cell. The electrode 100 of the embodiment can also be used as an anode for electrolytically generating ammonia. The electrode of the embodiment can be used as an anode for an electrolysis device for ammonia synthesis. In the following, the first embodiment and other embodiments will be described using water electrolysis as an example, but the electrode 100 of the embodiment can be used as the anode of a membrane electrode assembly used for electrolysis for ammonia synthesis, in which ultrapure water is supplied to the anode, water is decomposed at the anode to generate protons and oxygen, the protons generated in the electrolyte membrane pass through the electrolyte membrane, and nitrogen supplied to the cathode is combined with the protons and electrons to generate ammonia. The electrode 100 of the embodiment can also be used as a cathode for electrolyzing ammonia to generate hydrogen. The electrode of the embodiment can be used as a cathode for a hydrogen generating device. In the following, the first embodiment and other embodiments will be described taking water electrolysis as an example. However, the electrode 100 of the embodiment can be used as the cathode of a membrane electrode assembly used in electrolysis for ammonia decomposition, in which ammonia is supplied to the cathode, the ammonia is decomposed at the cathode to generate protons and nitrogen, the generated protons pass through an electrolyte membrane, and the protons and electrons combine at the anode to generate hydrogen.
[0013] A porous, highly conductive material is preferably used as the substrate 1. The substrate 1 is a porous member that allows gas and liquid to pass through. The electrode 100 is also used as an anode of a water electrolysis cell, for example, so a titanium substrate is preferred.
[0014] Highly durable Ti is preferable as the valve metal of the substrate 1. There are no particular limitations on the substrate 1 as long as it is a porous titanium substrate. For the substrate 1, for example, a Ti mesh or a cloth (non-woven fabric) made of Ti fibers is used.
[0015] Considering the movement of materials, the porosity of the substrate 1 should be 20% or more and 95% or less, and more preferably 40% or more and 90% or less.
[0016] For example, when the substrate 1 is a metal nonwoven fabric in which Ti fibers are entangled, the fiber diameter is preferably 1 μm or more and 500 μm or less, and more preferably 1 μm or more and 100 μm or less in consideration of reactivity and power supply. When the substrate 1 is a particle sintered body, the particle diameter is preferably 1 μm or more and 500 μm or less, and more preferably 1 μm or more and 100 μm or less in consideration of reactivity and power supply.
[0017] The substrate 1 has a first coating 1A containing titanium oxide on the catalyst layer 2 side thereof, and a second coating 1B containing titanium oxide on the side opposite to the catalyst layer 2 side thereof.
[0018] A case where the substrate 1 is a Ti mesh will be described. A first coating 1A which is an oxide coating is provided on the surface of the substrate 1 on the side where the catalyst layer 2 is provided. A second coating 1B which is an oxide coating is provided on the surface of the substrate 1 opposite to the side where the catalyst layer 2 is provided. For example, the first coating 1A is an oxide coating provided on the surface on the side where the catalyst layer 2 made of a cloth made of Ti mesh or Ti fibers is provided. For example, the second coating 1B is an oxide coating provided on the surface on the side opposite to the side where the catalyst layer 2 made of a cloth made of Ti mesh or Ti fibers is provided.
[0019] The case where the substrate 1 is a Ti cloth made of Ti fibers will be described. A first coating 1A, which is an oxide coating, is provided on the surface of the Ti fibers on the side of the substrate 1 where the catalyst layer 2 is provided. A second coating 1B, which is an oxide coating, is provided on the surface of the Ti fibers on the opposite side of the substrate 1 from the side where the catalyst layer 2 is provided. In this case, the first coating 1A is provided in a cylindrical shape on the surface of the Ti fibers on the catalyst layer 2 side. It is preferable that the first coating 1A is provided on the entire surface of the Ti fibers on the catalyst layer 2 side. In this case, the second coating 1B is provided in a cylindrical shape on the surface of the Ti fibers on the opposite side to the catalyst layer 2 side. It is preferable that the second coating 1B is provided on the entire surface of the Ti fibers on the opposite side to the catalyst layer 2 side. When an oxide coating is provided on the surface of the Ti fibers, the central portion of the Ti fibers (the region inside the first region 1A and the region inside the second region 1B) is Ti.
[0020] At least a portion of first coating 1A is preferably in direct contact with catalyst layer 2. First coating 1A is preferably in direct contact with Ti on the inside of first coating 1A and in direct contact with catalyst layer 2.
[0021] Second coating 1B is not in direct contact with catalyst layer 2.
[0022] The average thickness of the first coating 1A is 10 nm or more and 50 nm or less. Natural oxidation of Ti may cause a thin oxide coating to form on the surface of Ti. The average thickness of an unintentional oxide coating is less than 10 nm. The average thickness of the first coating 1A is preferably 10 nm or more and 45 nm or less, and more preferably 20 nm or more and 40 nm or less.
[0023] The average thickness of the second coating 1B is 10 nm or more and 50 nm or less. Natural oxidation of Ti may cause a thin oxide coating to form on the surface of Ti. The average thickness of an unintentional oxide coating is 10 nm or less. The average thickness of the second coating 1B is preferably 10 nm or more and 45 nm or less, and more preferably 20 nm or more and 40 nm or less. The average thickness of the second coating 1B is thinner than the average thickness of the first coating 1A. In other words, the average thickness of the first coating 1A is thicker than the average thickness of the second coating 1B.
[0024] The surface of the substrate 1 on which the catalyst layer 2 is provided is difficult to see due to the catalyst layer 2. The surface of the substrate 1 opposite to the side on which the catalyst layer 2 is provided is visible as the electrode 100 alone. The substrate 1 on the side on which the second coating 1B is provided preferably has a glossy yellow surface (yellowish color). The surface on the back side opposite to the catalyst layer 2 side is preferably yellow with metallic luster. The color of the surface of titanium changes depending on the thickness of the oxide coating. The surface on which the second coating 1B, which has an average thickness of 10 nm or more and 50 nm or less, is provided is yellow.
[0025] When the first coating 1A and the second coating 1B are provided on the substrate 1, the durability of the electrode 100 is preferably improved.
[0026] The average thickness of the first coating 1A is defined as D1. The average thickness of the second coating 1B is defined as D2. It is preferable that D1 and D2 satisfy D2≧D1. By satisfying this relationship, it is preferable that the electrode 100 has high initial characteristics and high durability.
[0027] It is more preferable that D1 and D2 satisfy 1 [nm] ≦ D2 - D1 ≦ 20 [nm]. It is more preferable that D1 and D2 satisfy 1 [nm] ≦ D2 - D1 ≦ 10 [nm]. If there is a large difference between the average thickness of the first coating 1A and the average thickness of the second coating 1B, the oxide coating may become thick locally. If the oxide coating is thick, the electrical resistance of the substrate 1 is likely to be high. Therefore, an electrode 100 that satisfies these relationships is preferable.
[0028] From the viewpoint of suppressing deterioration of the electrode 100 during operation, it is preferable that D1 and D2 satisfy 1 [nm] ≦ D2 - D1 ≦ 20 [nm] or 1 [nm] ≦ D2 - D1 ≦ 10 [nm], and the average thickness D1 of the first coating 1A satisfies 1 [nm] to 50 [nm]. It is preferable that the average thickness D2 of the second coating 1B is within a range that satisfies 1 [nm] ≦ D2 - D1 ≦ 20 [nm] (or 1 [nm] ≦ D2 - D1 ≦ 10 [nm]) and 10 [nm] ≦ D1 ≦ 50 [nm].
[0029] From the viewpoint of suppressing deterioration during operation of the electrode 100, when D1 and D2 satisfy 1 [nm] ≦ D2 - D1 ≦ 20 [nm] or 1 [nm] ≦ D2 - D1 ≦ 10 [nm], the average thickness D1 of the first coating 1A is preferably 5 [nm] or more and less than 100 [nm], more preferably 5 [nm] or more and 50 [nm] or less, and even more preferably 10 [nm] or more and 45 [nm] or less. The average thickness D2 of the second coating 1B is preferably within a range that satisfies 1 [nm] ≦ D2 - D1 ≦ 20 [nm] (or 1 [nm] ≦ D2 - D1 ≦ 10 [nm]) and 10 [nm] ≦ D1 ≦ 50 [nm].
[0030] From the viewpoint of suppressing deterioration of the electrode 100 during operation, when D1 and D2 satisfy 1 [nm]≦D2-D1≦20 [nm] or 1 [nm]≦D2-D1≦10 [nm], the average thickness D2 of the second coating 1B is preferably 6 [nm] or more and less than 100 [nm], more preferably 6 [nm] or more and 50 [nm] or less, and even more preferably 6 [nm] or more and 45 [nm] or less.
[0031] From the viewpoint of suppressing deterioration of the electrode 100 during operation, it is more preferable that D1 and D2 satisfy 3 [nm] ≦ D2 - D1 ≦ 20 [nm]. It is more preferable that D1 and D2 satisfy 3 [nm] ≦ D2 - D1 ≦ 10 [nm]. It is preferable that the average thickness D2 of the second coating 1B is within a range that satisfies 3 [nm] ≦ D2 - D1 ≦ 20 [nm] (or 3 [nm] ≦ D2 - D1 ≦ 10 [nm]) and 10 [nm] ≦ D1 ≦ 50 [nm].
[0032] From the viewpoint of suppressing deterioration of the electrode 100 during operation, when D1 and D2 satisfy 3 [nm]≦D2-D1≦20 [nm] or 3 [nm]≦D2-D1≦10 [nm], the average thickness D1 of the first coating 1A is preferably 5 [nm] or more and less than 100 [nm], more preferably 5 [nm] or more and 50 [nm] or less, and even more preferably 5 [nm] or more and 45 [nm] or less.
[0033] From the viewpoint of suppressing deterioration of the electrode 100 during operation, when D1 and D2 satisfy 3 [nm]≦D2-D1≦20 [nm], the average thickness of the second coating 1B is preferably 8 [nm] or more and less than 100 [nm], more preferably 8 [nm] or more and 50 [nm] or less, and even more preferably 8 [nm] or more and 45 [nm] or less.
[0034] It is preferable that 90 [wt%] to 100 [wt%] of the first coating 1A is TiO2. It is preferable that 90 [wt%] to 100 [wt%] of the second coating 1B is TiO2. The oxide coating on the surface of the substrate 1 is preferably an oxide formed by oxidation of Ti, not an oxide layer that clearly contains other metal elements. Therefore, it is more preferable that 95 [wt%] to 100 [wt%] of the first coating 1A is TiO2. It is more preferable that 95 [wt%] to 100 [wt%] of the second coating 1B is TiO2. It is more preferable that 98 [wt%] to 100 [wt%] of the first coating 1A is TiO2. It is more preferable that 98 [wt%] to 100 [wt%] of the second coating 1B is TiO2.
[0035] From the same viewpoint as above, it is preferable that 95 atom % or more and 100 atom % or less of the metal elements contained in first coating 1A are Ti. From the same viewpoint as above, it is preferable that 95 atom % or more and 100 atom % or less of the metal elements contained in second coating 1B are Ti.
[0036] From the same viewpoint as above, it is preferable that 99 atom % or more and 100 atom % or less of the metal elements contained in first coating 1A are Ti. From the same viewpoint as above, it is preferable that 99 atom % or more and 100 atom % or less of the metal elements contained in second coating 1B are Ti.
[0037] It is preferable that the region of the surface of the substrate 1 excluding the oxide film including the first region (first coating) 1A and the second region (second coating) 1B (including the region inside the first region (first coating) 1A and the region inside the second region (second coating) 1B) contains Ti. It is preferable that the region of the surface of the substrate 1 excluding the oxide film is 95 [wt%] to 100 [wt%] Ti. It is preferable that the region of the surface of the substrate 1 excluding the oxide film is 98 [wt%] to 100 [wt%] Ti. It is preferable that the region of the surface of the substrate 1 excluding the oxide film is 99 [wt%] to 100 [wt%] Ti.
[0038] The thickness of the inner region of the first coating 1A is preferably 980 nm or more and 50 μm (50,000 nm) or less. The thickness of the inner region of the first coating 1A is preferably 19.6 times or more and 5,000 times or less the thickness of the first coating 1A. It is preferable that the Ti region not provided with an oxide coating is relatively thick.
[0039] The thickness of the inner region of the second coating 1B is preferably 980 nm or more and 50 μm (50,000 nm) or less. The thickness of the inner region of the second coating 1B is preferably 19.6 times or more and 5,000 times or less the thickness of the second coating 1B. It is preferable that the Ti region not provided with an oxide coating is thick.
[0040] The catalytic layer 2 contains a precious metal oxide mainly composed of Ir and Ru and a non-precious metal oxide. An intermediate layer (not shown) may be provided between the catalytic layer 2 and the substrate 1. A configuration in which the catalytic layer 2 and the substrate 1 are in direct contact with each other is preferable.
[0041] The amount of precious metal in the catalyst layer 2 is 0.02 [mg / cm 2 ] or more 1.0[mg / cm 2 ] or less, and more preferably 0.05 [mg / cm 2 ] or more 0.5[mg / cm 2 This sum of masses can be measured by ICP-MS.
[0042] The porosity of the catalyst layer 2 is preferably 10% or more and 90% or less, and more preferably 30% or more and 70% or less.
[0043] The catalyst layer 2 has a structure in which sheet layers 2A and gap layers 2B are alternately laminated. The laminated structure of the catalyst layer 2 is shown in the schematic cross-sectional view of the catalyst layer 2 in Fig. 2. The sheet layers 2A and the gap layers 2B are laminated substantially parallel to each other. Most of the gap layers 2B are hollow, but some of the sheet layers 2A protrude and connect the sheet layers 2A. The sheet layers 2A are connected by pillars 2C present in the gap layers 2B, and the laminated structure is maintained.
[0044] The sheet layer 2A is a layer in which catalyst particles, which are particles of unsupported precious metal oxide aggregated into a sheet shape, are arranged. There are some voids in the sheet layer 2A. The sheet layer 2A is a dense layer containing a large amount of catalyst particles.
[0045] The gap layer 2B is a region sandwiched between the sheet layers 2A and contains catalyst particles, which are particles of unsupported precious metal oxide. Unlike the sheet layers 2A, the gap layer 2B does not have a regular structure of catalyst particles. The gap layer 2B is a region with a low density of catalyst particles.
[0046] The average thickness of one layer of the sheet layer 2A is preferably 6 nm or more and 50 nm or less. The average thickness of one layer of the gap layer 2B is preferably 6 nm or more and 50 nm or less. The average thickness of one layer of the sheet layer 2A is preferably thicker than the average thickness of one layer of the gap layer 2B. Some of the gap layers 2B may be thicker than some of the sheet layers 2A.
[0047] The catalytic layer 2 preferably contains Ir oxide or / and a composite oxide of Ir and Ru as a precious metal oxide, and optionally contains Ru oxide. The sum of the concentrations of Ir and Ru among the precious metals contained in the catalytic layer 2 is preferably 90 wt% or more and 100 wt% or less. The precious metals contained in the precious metal oxide of the catalytic layer 2 are not limited to Ir and Ru. Note that Ru may be replaced with other metals or alloys in some cases.
[0048] The catalytic layer 2 preferably contains, as the non-precious metal oxide, an oxide of one or more non-precious metals selected from the group consisting of Ni, Co, and Mn. The non-precious metals contained in the catalytic layer 2 preferably contain Ni, and optionally Co and / or Mn. When the amount of the non-precious metals contained in the catalytic layer 2 is taken as 100 [wt%], the total ratio of Ni, Co, and Mn among the non-precious metals contained in the catalytic layer 2 is preferably 80 [wt%] to 100 [wt%].
[0049] The catalyst layer 2 may contain one or more non-noble metals selected from the group consisting of Ni, Co, and Mn.
[0050] Each spot should be square and at least 1 mm 2 As shown in FIG. 3, when the length of the electrode 100 is D1 and the width of the electrode 100 is D2 (D1≧D2), imaginary lines are drawn from two opposing sides of the electrode 100 in the width direction at a distance of D3 (=D1 / 10) inward, and from two opposing sides of the electrode 100 in the length direction at a distance of D4 (=D2 / 10) inward. Furthermore, imaginary lines parallel to the width direction passing through the center of the electrode 100 are drawn, and imaginary lines parallel to the length direction passing through the center of the electrode 100 are drawn. The analysis spots A1 to A9 are areas centered on nine intersections of the imaginary lines. The cross section observed by SEM is perpendicular to the plane of FIG. 3 and parallel to the width direction. The thickness of each gap layer 2B of the analysis spots A1 to A9 is obtained at 50 [nm] intervals in the width direction of the SEM image. Then, the ratio of the gap layer 2B thickness less than 2 [nm] is obtained. The average thicknesses of the gap layer 2B and the sheet layer 2A are obtained in the same manner. A similar analysis using a similar SEM-EDX can be performed to observe the cross section of the substrate 1. By observing the cross section of the substrate 1, the thickness of the oxide film of the substrate 1 and the composition of the substrate 1 can be obtained.
[0051] The catalyst layer 2 is formed by alternately forming a sheet layer precursor, which is essentially a precursor of the sheet layer 2A and contains a precious metal oxide, and a gap layer precursor, which is essentially a precursor of the gap layer 2B and mainly contains a non-precious metal oxide, on the substrate 1 by sputtering. At this time, the sheet layer precursor and the gap layer precursor are formed in an oxidizing atmosphere. The non-precious metal oxide is eluted by an acid treatment such as sulfuric acid. After the non-precious metal is eluted, a heat treatment is performed in an oxidizing atmosphere. The heat treatment in the oxidizing atmosphere improves the adhesion between the catalyst layer 2 and the substrate 1.
[0052] For example, a titanium oxide coating of a desired thickness can be formed on any surface of the substrate 1 by heating, anodizing, or the like.
[0053] The average thickness of the oxide film (first film 1A and second film 1B) on the substrate 1, and the initial characteristics and characteristics after operation are described below. Here, the initial characteristics and durability of the electrode 100 are described using water electrolysis as an example. An electrochemical cell is fabricated using the electrode 100 as the anode and cathode, and the electrode 100 is evaluated. A current of 2 [A / cm2] is applied between the anode and cathode using a power source. 2 Water electrolysis is performed by applying a current at a current density of [0.015 V], and the cell voltages at the start of operation and 75 hours after the start of operation are compared. The vertical axis of FIG. 4 is the cell voltage. The values on the horizontal axis of FIG. 4 represent the average thickness of the oxide coating (first coating 1A and second coating 1B) on the substrate 1. The thickness of the oxide coating is adjusted by the oxidation conditions when the electrode 100 is produced. The actual thickness of the oxide coating falls within the range of the values shown on the horizontal axis.
[0054] Cross-sectional images of the electrode 100 showing the thickness of the first oxide film 1A are shown in Figs. 5 to 8. Figs. 5 to 8 show a cross section of a portion where a laminated catalyst layer having a laminated structure is formed on the surface of titanium (substrate 1). Figs. 5 and 6 are cross-sectional images of the electrode 100 corresponding to a comparative example. The first film 1A in Figs. 5 and 6 is unclear. The thickness of the first film 1A in Figs. 5 and 6 is less than 10 [nm]. Figs. 7 and 8 are cross-sectional images of the electrode 100 corresponding to an example. The first film 1A in Figs. 7 and 8 is slightly clearer than the first film 1A in Figs. 5 and 6. The thickness of the first film 1A in Fig. 7 is 11 [nm] or more and 13 [nm] or less. The thickness of the first oxide film 1A in Fig. 8 is 22 [nm] or more and 36 [nm] or less.
[0055] Fig. 4 shows a graph illustrating the relationship between the thickness of the oxide film (first film 1A and second film 1B) on the substrate 1 and the initial characteristics and the characteristics after operation. When the average thickness of the oxide film is 0 nm or more and less than 10 nm, the initial cell voltage is low, but the cell voltage increases after operation, and durability is not high. It is believed that the catalyst layer 2 has deteriorated due to the water electrolysis operation.
[0056] When the average thickness of the oxide film (first coating 1A) is less than 1 nm, the increase in cell voltage after operation when D2≧D1 is satisfied and the average thickness of the oxide film (first coating 1A) is 1 nm or more and 50 nm or less is suppressed compared to when the average thickness of the oxide film (first coating 1A) is 0 nm. Therefore, it is preferable that the average thickness of the oxide film (first coating 1A) is 1 nm or more and 50 nm or less, and 1 nm≦D2-D1≦20 nm. It is preferable that the average thickness D2 of the second coating 1B is within a range that satisfies 1 nm≦D2-D1≦20 nm and 10 nm≦D1≦50 nm.
[0057] When the thickness of the oxide film is 10 nm or more and 50 nm or less, the initial cell voltage is low and the cell voltage increases slightly after operation. The cell voltage hardly increases due to the water electrolysis operation, and it is found that the electrode 100 of the embodiment has high durability. When water electrolysis is performed using the electrode 100 of the embodiment, high water electrolysis characteristics can be maintained for a long time.
[0058] Compared to when the average thickness of the first coating D1 is less than 1 nm, when the average thickness of the oxide coating is greater than 50 nm and less than 100 nm, the increase in cell voltage after operation is suppressed compared to when the average thickness of the oxide coating is 0 nm. However, when the average thickness of the oxide coating is greater than 50 nm and less than 100 nm, the initial voltage is slightly higher.
[0059] The deterioration of the electrode 100 is suitably suppressed even after operation for more than 75 hours (e.g., 750 hours) from the start of operation. When the electrode 100 that satisfies 1 [nm] ≦ D2 - D1 ≦ 20 [nm] is used, the increase in the cell voltage can be suppressed even when the operation time is long.
[0060] The deterioration of the electrode 100 is suitably suppressed even after operation for more than 75 hours (e.g., 750 hours) from the start of operation. When the electrode 100 that satisfies 1 [nm] ≦ D2 - D1 ≦ 10 [nm] is used, the increase in the cell voltage can be suppressed even when the operation time is long.
[0061] By using an electrode 100 in which, after operation for more than 75 hours (e.g., 750 hours) from the start of operation, the average thickness D1 of the first coating 1A is 1 [nm] or more and 50 [nm] or less, and satisfies 1 [nm]≦D2-D1≦20 [nm], and the average thickness D2 of the second coating 1B is within the ranges that satisfy 1 [nm]≦D2-D1≦20 [nm] and 10 [nm]≦D1≦50 [nm] (preferably, 10 [nm]≦D1≦45 [nm]), an increase in cell voltage can be suppressed.
[0062] By using an electrode 100 in which, after operation for more than 75 hours (e.g., 750 hours) from the start of operation, the average thickness D1 of the first coating 1A is 3 [nm] or more and 50 [nm] or less, and satisfies 3 [nm] <= D2 - D1 <= 20 [nm], and the average thickness D2 of the second coating 1B is within the ranges satisfying 3 [nm] <= D2 - D1 <= 20 [nm] and 10 [nm] <= D1 <= 50 [nm] (preferably, 10 [nm] <= D1 <= 45 [nm]), an increase in cell voltage can be suppressed.
[0063] When the oxide film thickness is 100 nm or more, the cell voltage is high from the initial stage, and the cell voltage increases slightly after operation. Although the increase in voltage due to water electrolysis operation is small, the cell voltage is high from the initial stage, and the water electrolysis characteristics are poor.
[0064] Second embodiment The second embodiment relates to a membrane electrode assembly (MEA). Fig. 9 shows a schematic diagram of a membrane electrode assembly 200 of the embodiment. The membrane electrode assembly 200 has a first electrode 11, a second electrode 12, and an electrolyte membrane 13. The first electrode 11 is preferably an anode electrode, and the second electrode 12 is preferably a cathode electrode. The electrode 100 of the first embodiment is preferably used for the first electrode 11. The membrane electrode assembly 200 of the embodiment is preferably used in an electrochemical cell or stack that generates hydrogen or oxygen.
[0065] It is preferable to use the electrode 100 of the first embodiment as the first electrode 11. The catalyst layer 2 of the electrode 100 used as the first electrode 11 is provided on the electrolyte membrane 13 side. It is preferable that the catalyst layer 2 is in direct contact with the electrolyte membrane 13.
[0066] The second electrode 12 has a second substrate 12B and a second catalyst layer 12A. The second catalyst layer 12A is provided on the second substrate 12B. The second catalyst layer 12A is provided on the electrolyte membrane 13 side. The second catalyst layer 12A is preferably in direct contact with the electrolyte membrane 13.
[0067] The second substrate 12B is preferably made of a porous material having high conductivity. The second substrate 12B is a porous member that allows gas and liquid to pass through. The second substrate 12B is, for example, carbon paper or a metal mesh. As the metal mesh, a porous substrate made of a valve metal is preferable. As the porous substrate made of a valve metal, a porous substrate containing one or more metals selected from the group consisting of titanium, aluminum, tantalum, niobium, hafnium, zirconium, zinc, tungsten, bismuth, and antimony, or a porous substrate made of one metal selected from the group consisting of titanium, aluminum, tantalum, niobium, hafnium, zirconium, zinc, tungsten, bismuth, and antimony is preferable. The second substrate 12B has a carbon layer (MPL layer) containing carbon fine particles and a water-repellent resin (fluororesin such as PTFE or Nafion). The carbon layer is provided, for example, between the carbon paper and the second catalyst layer 12A.
[0068] The second catalytic layer 12A has a catalytic metal. The second catalytic layer 12A is preferably a catalytic metal particle, and the catalytic metal is not supported on a carrier. The second catalytic layer 12A is preferably a porous catalytic layer. The catalytic metal is not particularly limited, but includes, for example, one or more selected from the group consisting of Pt, Rh, Os, Ir, Pd, and Au. It is preferable to include one or more selected from the group consisting of such catalytic materials. The catalytic metal is preferably a metal, an alloy, or a metal oxide. The second catalytic layer 12A preferably has a plurality of catalytic units in which, for example, sheet-like catalytic layers and gap layers are alternately laminated.
[0069] The amount of metal per area of the second catalyst layer 12A is 0.02 [mg / cm 2] or more 1.0[mg / cm 2 ] or less, and more preferably 0.05 [mg / cm 2 ] or more 0.5[mg / cm 2 This sum of masses can be measured by ICP-MS.
[0070] The porosity of the second catalyst layer 12A is preferably 10% or more and 90% or less, and more preferably 30% or more and 70% or less.
[0071] The electrolyte membrane 13 is preferably a proton conductive membrane. The electrolyte membrane 13 is preferably a fluorine-based polymer or an aromatic hydrocarbon-based polymer having one or more selected from the group consisting of a sulfonic acid group, a sulfonimide group, and a sulfate group. The electrolyte membrane 13 is preferably a fluorine-based polymer having a sulfonic acid group. Examples of the fluorine-based polymer having a sulfonic acid group that can be used include Nafion (trademark, manufactured by DuPont), Flemion (trademark, manufactured by Asahi Kasei), Selemion (trademark, manufactured by Asahi Kasei), Aquivion (trademark; Solvay Specialty Polymers), and Aciplex (trademark, manufactured by Asahi Glass). Note that instead of the proton conductive membrane, various conductive membranes such as anion exchange membranes and porous membranes can be used in some cases.
[0072] The thickness of the electrolyte membrane 13 can be appropriately determined in consideration of the membrane's properties such as permeability and durability. From the viewpoints of strength, dissolution resistance, and MEA output properties, the thickness of the electrolyte membrane 13 is preferably 20 μm to 500 μm, more preferably 50 μm to 300 μm, and even more preferably 80 μm to 200 μm.
[0073] The electrolyte membrane 13 preferably includes a precious metal region on the first electrode 11 side. The precious metal region includes precious metal particles. The precious metal region is preferably present on the surface of the electrolyte membrane 13. The precious metal region is preferably composed of one region, but may be composed of multiple separate regions.
[0074] The precious metal particles are preferably particles of one or more precious metals selected from the group consisting of Pt, Re, Rh, Ir, Pd, and Ru. The precious metal particles may include alloy particles containing one or more selected from the group consisting of Pt, Re, Rh, Ir, Pd, and Ru. The precious metal particles are preferably particles of one precious metal selected from the group consisting of Pt, Re, Rh, Ir, Pd, and Ru. The precious metal particles are preferably Pt particles. The precious metal particles are preferably Re particles. The precious metal particles are preferably Rh particles. The precious metal particles are preferably Ir particles. The precious metal particles are preferably Pd particles. The precious metal particles are preferably Ru particles.
[0075] The precious metal particles oxidize hydrogen that is generated on the cathode side and passes through the electrolyte membrane 13. The precious metal particles can suppress hydrogen leakage. Because the precious metal particles are present on the anode side, they do not easily oxidize hydrogen discharged from the cathode side. The region where the precious metal particles are present may also be present in the electrolyte membrane 13 on the second electrode 12 (cathode) side.
[0076] The average circumscribed circle diameter of the precious metal particles is preferably 0.5 nm or more and 50 nm or less, more preferably 1 nm or more and 10 nm or less, and even more preferably 1 nm or more and 5 nm or less.
[0077] By using the highly durable electrode 100 as the anode of the membrane electrode assembly 200, long-term operation with high activity becomes possible.
[0078] Third embodiment The third embodiment relates to an electrochemical cell. Fig. 10 shows a cross-sectional view of an electrochemical cell 300 according to the third embodiment. The electrochemical cell 300 will be described below using water electrolysis as an example, but hydrogen can also be generated by decomposing ammonia or the like other than water.
[0079] 10, an electrochemical cell 300 of the third embodiment includes a first electrode (anode) 11, a second electrode (cathode) 12, an electrolyte membrane 13, a gasket 21, a gasket 22, a separator 23, and a separator 24. A sealing material for the first electrode 11 may be used as the gasket 21. A sealing material for the second electrode 12 may be used as the gasket 22.
[0080] It is preferable to use a membrane electrode assembly 200 in which a first electrode (anode) 11, a second electrode (cathode) 12, and an electrolyte membrane 13 are joined together. An anode power supply may be provided separately from the separator 23. A cathode power supply may be provided separately from the separator 24.
[0081] In the electrochemical cell 300 of FIG. 10, a power source (not shown) is connected to the separator 23 and the separator 24, and a reaction occurs at the anode 11 and the cathode 12. For example, water is supplied to the anode 11, and the water is decomposed into protons, oxygen, and electrons at the anode 11. The electrode support and the power supply are porous, and this porous body functions as a flow path plate. The generated water and unreacted water are discharged, and the protons and electrons are used in the cathode reaction. In the cathode reaction, the protons and electrons react to generate hydrogen. Either or both of the generated hydrogen and oxygen are used, for example, as fuel for the fuel cell.
[0082] (Fourth embodiment) The fourth embodiment relates to a stack. Fig. 11 is a schematic cross-sectional view showing a stack 400 of the fourth embodiment. The stack 400 of the fourth embodiment shown in Fig. 11 has a plurality of MEAs 200 or electrochemical cells 300 connected in series. Clamping plates 31 and 32 are attached to both ends of the MEA or electrochemical cell.
[0083] Since the amount of hydrogen produced in an electrochemical cell 300 consisting of one MEA 200 is small, a large amount of hydrogen can be obtained by forming a stack 400 in which a plurality of MEAs 200 or a plurality of electrochemical cells 300 are connected in series.
[0084] Fifth embodiment The fifth embodiment relates to an electrolysis device. Fig. 12 shows a conceptual diagram of the electrolysis device of the fifth embodiment. An electrolysis device 500 uses an electrochemical cell 300 or a stack 400. The electrolysis device 500 in Fig. 12 is for water electrolysis. An electrolysis device for water electrolysis will be described. For example, when hydrogen is generated from ammonia, it is preferable to adopt a device with a different configuration using the electrode 100. The electrodes of the embodiment can also be used in an electrolysis device that electrolyzes carbon dioxide to generate organic substances such as methanol and ethylene, and carbon monoxide.
[0085] As shown in FIG. 12, a stack 400 is formed by stacking unit cells for water electrolysis in series. A power source 41 is attached to the stack 400, and a voltage is applied between the anode and the cathode. A gas-liquid separator 42 for separating the generated gas from unreacted water and a mixing tank 43 are connected to the anode side of the stack 400. Water is sent from an ion-exchanged water production device 44, which supplies water, to the mixing tank 43 by a pump 46, and mixed in the mixing tank 43 through a check valve 47 from the gas-liquid separator 42 and circulated to the anode. Oxygen generated at the anode passes through the gas-liquid separator 42 to obtain oxygen gas. On the other hand, a hydrogen purifier 49 is connected to the gas-liquid separator 48 on the cathode side to obtain high-purity hydrogen. Impurities are discharged through a path having a valve 50 connected to the hydrogen purifier 49. In order to stably control the operating temperature, the stack and the mixing tank can be heated, and the current density during pyrolysis can be controlled.
[0086] In the specification, some elements are represented only by their element symbols.
[0087] Below, technical proposals of the embodiments are added. The configurations added to the technical proposals are configurations using a preferred electrode 100. The configurations combining a plurality of the requirements added to the technical proposals are configurations using a preferred electrode 100. Technical proposal 1 A porous titanium substrate; an electrolysis catalyst layer provided on the titanium substrate and having sheet layers and gap layers alternately laminated thereon; having a first coating film containing titanium oxide on the electrolytic catalyst layer side of the titanium substrate; a second coating film containing titanium oxide on the opposite side of the titanium substrate to the electrolytic catalyst layer side; The average thickness of the first coating is D1, The average thickness of the second coating is D2, The electrodes have D1 and D2 satisfying 1 [nm]≦D2−D1≦20 [nm]. Technical proposal 2 An electrode as described in Technical Proposal 1, wherein D1 is 10 [nm] or more and 50 [nm] or less. Technical proposal 3 The D2 is 10 [nm] or more and 50 [nm] or less, The electrode according to Technical Scheme 1 or 2, wherein the titanium substrate has a shiny yellow (or yellowish) surface on the side opposite to the electrolytic catalyst layer. Technical proposal 4 An electrode described in any one of technical proposals 1 to 3, wherein D1 and D2 satisfy 3 [nm]≦D2-D1≦20 [nm]. Technical proposal 5 Any of the electrodes described in Technical Schemes 1 to 4, wherein D2 is within the ranges satisfying 1 [nm] ≦ D2 - D1 ≦ 20 [nm] and 10 [nm] ≦ D1 ≦ 50 [nm]. Technical proposal 6 An electrode described in any one of technical proposals 1 to 5, wherein D1 and D2 satisfy 1 [nm]≦D2-D1≦10 [nm]. Technical proposal 7 The D1 and the D2 satisfy 1 [nm] ≦ D2 - D1 ≦ 10 [nm], D1 is 10 [nm] or more and 50 [nm] or less, Any of the electrodes described in Technical Schemes 1 to 6, wherein D2 is within the ranges satisfying 1 [nm]≦D2-D1≦10 [nm] and 10 [nm]≦D1≦50 [nm]. Technical proposal 8 The D1 and the D2 satisfy 3 [nm] ≦ D2 - D1 ≦ 10 [nm], D1 is 10 [nm] or more and 50 [nm] or less, Any of the electrodes described in Technical Schemes 1 to 7, wherein D2 is within the ranges satisfying 3 [nm] ≦ D2 - D1 ≦ 10 [nm] and 10 [nm] ≦ D1 ≦ 50 [nm]. Technical proposal 9 D1 is equal to or greater than 10 [nm] and equal to or less than 45 [nm], Any of the electrodes described in Technical Schemes 1 to 8, wherein D2 is within the ranges satisfying 1 [nm] ≦ D2 - D1 ≦ 10 [nm] and 10 [nm] ≦ D1 ≦ 45 [nm]. Technical proposal 10 D1 is equal to or greater than 10 [nm] and equal to or less than 45 [nm], Any of the electrodes described in Technical Schemes 1 to 9, wherein D2 is within the ranges satisfying 3 [nm] ≦ D2 - D1 ≦ 10 [nm] and 10 [nm] ≦ D1 ≦ 45 [nm]. Technical proposal 11 The first coating contains TiO2 at 90 wt% or more and 100 wt% or less. An electrode described in any one of Technical Proposals 1 to 10, in which 90% by weight or more and 100% by weight or less of the second coating is TiO2. Technical proposal 12 The first coating contains 95 wt% or more and 100 wt% or less of TiO2, An electrode described in any one of Technical Proposals 1 to 11, in which 95% by weight or more and 100% by weight or less of the second coating is TiO2. Technical proposal 13 Among the metal elements contained in the first coating, 95 atom % or more and 100 atom % or less is Ti, An electrode according to any one of Technical Schemes 1 to 12, wherein 95 atom % or more and 100 atom % or less of the metal elements contained in the second coating is Ti. Technical proposal 14 Among the metal elements contained in the first coating, 99 atom % or more and 100 atom % or less is Ti, An electrode according to any one of Technical Schemes 1 to 13, wherein 99 atom % or more and 100 atom % or less of the metal elements contained in the second coating is Ti. Technical proposal 15 the inner region of the first coating contains Ti; The thickness of the inner region of the first coating is 980 nm or more and 50 μm or less, an inner region of the second coating includes Ti; An electrode described in any one of technical proposals 1 to 14, wherein the thickness of the inner region of the second coating is 980 nm or more and 50 μm or less. Technical proposal 16 the inner region of the first coating contains Ti; the thickness of the inner region of the first coating is 19.6 times or more and 5000 times or less than the thickness of the first coating; an inner region of the second coating includes Ti; An electrode described in any one of technical proposals 1 to 15, wherein the thickness of the inner region of the second coating is 19.6 times or more and 5000 times or less than the thickness of the first coating. Technical proposal 17 A membrane electrode assembly using the electrode described in any one of Technical Solutions 1 to 16. Technical proposal 18 An electrochemical cell using the membrane electrode assembly described in Technical Proposal 17. Technical proposal 19 A stack using the membrane electrode assembly described in Technical Proposal 18. Technical proposal 20 An electrolysis device using the stack described in Technical Proposal 19.
[0088] Although several embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. Although a PEMEC has been given as a water electrolysis cell, the present invention can be similarly applied to other electrolysis cells. These novel embodiments described above can be embodied in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and modifications thereof are included within the scope and gist of the invention, and are included within the scope of the invention and its equivalents as described in the claims. For example, "yellow" can be replaced with the expression "yellowish color." [Explanation of symbols]
[0089] 1 Base material 1A 1st coating 1B 2nd coating 2 Catalyst layer 11 1st electrode 12 2nd electrode 13 Electrolyte membrane 21 Gasket 22 Gasket 23 Separator 24 Separator 31 Clamping plate 32 Clamping plate 41 Power supply 42 Gas-liquid separation equipment 43 Mixing Tank 44 Ion exchange water production equipment 46 Pump 47 Check valve 48 Gas-liquid separation equipment 49 Hydrogen purification equipment 50 valves 100 electrodes 200 Membrane electrode assembly 300 Electrochemical Cells 400 Stack 500 Electrolyzer
Claims
1. A porous titanium substrate; an electrolysis catalyst layer provided on the titanium substrate and having sheet layers and gap layers alternately laminated thereon; having a first coating film containing titanium oxide on the electrolytic catalyst layer side of the titanium substrate; a second coating film containing titanium oxide on the opposite side of the titanium substrate to the electrolytic catalyst layer side; The average thickness of the first coating is D1, The average thickness of the second coating is D2, The electrodes have D1 and D2 that satisfy 1 [nm]≦D2−D1≦20 [nm]. electrode.
2. The electrode according to claim 1 , wherein D1 is equal to or greater than 10 nm and equal to or less than 50 nm.
3. The D2 is 10 nm or more and 50 nm or less, 3. The electrode according to claim 1, wherein the titanium substrate has a shiny yellow or yellowish surface on the side opposite to the electrolytic catalyst layer.
4. 3. The electrode according to claim 1, wherein D1 and D2 satisfy 3 nm≦D2−D1≦20 nm.
5. 3. The electrode according to claim 1, wherein D2 is within a range satisfying 1 nm≦D2−D1≦20 nm and 10 nm≦D1≦50 nm.
6. 3. The electrode according to claim 1, wherein D1 and D2 satisfy 1 nm≦D2−D1≦10 nm.
7. The first coating is composed of 90 wt % to 100 wt % TiO 2 and The second coating is composed of 90 wt % to 100 wt % TiO 2 3. The electrode according to claim 1 or 2,
8. The first coating contains 95 wt % or more and 100 wt % or less of TiO 2 and The second coating is composed of 95 wt % or more and 100 wt % or less of TiO 2 3. The electrode according to claim 1 or 2,
9. the first coating contains metal elements of 95 atom % or more and 100 atom % or less of Ti, 3. The electrode according to claim 1, wherein the second coating contains metal elements that account for 95 atom % or more and 100 atom % or less of Ti.
10. the first coating contains metal elements of 99 atom % or more and 100 atom % or less of Ti, 3. The electrode according to claim 1, wherein the second coating contains metal elements that account for 99 atom % or more and 100 atom % or less of Ti.
11. an inner region of the first coating includes Ti; The thickness of the inner region of the first coating is 980 nm or more and 50 μm or less, an inner region of the second coating includes Ti; 3. The electrode according to claim 1, wherein the thickness of the inner region of the second coating is 980 nm or more and 50 μm or less.
12. an inner region of the first coating includes Ti; a thickness of the inner region of the first coating is 19.8 times or more and 5000 times or less than a thickness of the first coating; an inner region of the second coating includes Ti; 3. The electrode according to claim 1, wherein the thickness of the inner region of the second coating is 19.8 to 5000 times the thickness of the first coating.
13. The electrode according to claim 1 or 2. A membrane electrode assembly using the electrode according to claim 1.
14. An electrochemical cell using the membrane electrode assembly according to claim 13.
15. A stack using the membrane electrode assembly according to claim 13.
16. An electrolysis device using the stack according to claim 15.
Citation Information
Patent Citations
Laminated catalyst, electrode, membrane electrode composite, electrochemical cell, stack, fuel cell and water electrolysis reversible apparatus, vehicle, and flying body
JP2021045709A
Partial oxidation treatment of electrode
JP1987207855A
Anodically oxidized porous alumina and production method therefor
JP2009256751A
Layered catalyst layer, membrane electrode assembly and electrochemical cell
JP2012204221A
Anodic oxidation treatment process
JP2017050542A