Hydrogenated copolymer, adhesive composition, adhesive film and method for producing hydrogenated copolymer

A hydrogenated copolymer with controlled vinyl aromatic and conjugated diene monomer units addresses adhesive strength issues on complex surfaces, providing enhanced adhesion and film formability without the drawbacks of tackifiers.

JP2024132888APending Publication Date: 2024-10-01ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024016424
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-01-12
Filing Date
2024-02-06
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing hydrogenated copolymers exhibit insufficient adhesive strength on complex surfaces, such as embossed steel plates, and traditional methods to enhance adhesive strength, like using tackifiers, lead to issues like roll wrapping and equipment contamination.

Method used

A hydrogenated copolymer composition comprising specific ranges of vinyl aromatic monomer units and conjugated diene monomer units, with controlled molecular weights and hydrogenation rates, is developed to improve adhesiveness and film formability without adhesive residue.

Benefits of technology

The hydrogenated copolymer achieves excellent adhesion to irregular surfaces, reduces adhesive residue, and enhances film formability while avoiding issues associated with tackifiers, such as roll wrapping and equipment contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132888000001
    Figure 2024132888000001
  • Figure 2024132888000002
    Figure 2024132888000002
  • Figure 2024132888000003
    Figure 2024132888000003
Patent Text Reader

Abstract

To provide a hydrogenated copolymer having excellent adhesion, adhesive residue properties and film formability, an adhesive composition comprising the hydrogenated copolymer and an adhesive film.SOLUTION: There is provided a hydrogenated copolymer (X) which includes a hydrogenated copolymer (A) which is a hydrogenated product of a copolymer having a vinyl aromatic monomer unit and a conjugated diene monomer unit and a hydrogenated copolymer (B) which is a hydrogenated product of a copolymer having a vinyl aromatic monomer unit and a conjugated diene monomer unit, wherein each of (A) and (B) satisfies a predetermined condition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hydrogenated copolymer, an adhesive composition, an adhesive film, and a method for producing the hydrogenated copolymer. [Background technology]

[0002] Block copolymers of vinyl aromatic compounds and conjugated diene compounds have elasticity at room temperature similar to that of vulcanized natural or synthetic rubber even without vulcanization, and at high temperatures they have processability similar to that of thermoplastic resins. For this reason, they have been widely used in fields such as footwear, plastic modification, asphalt modification, adhesives, household products, packaging materials for home appliances and industrial parts, toys, etc. Furthermore, the hydrogenated products of the block copolymers have excellent weather resistance and heat resistance, and therefore are widely used in the fields of automobile parts, medical instruments, etc., in addition to the above-mentioned fields of application.

[0003] In recent years, smartphones, tablets, and flat-screen TVs have become increasingly popular, and surface protection films are now widely used to prevent the optical films and optical resin plates that make up these devices from becoming dirty or scratched during processing and transportation. Background Art Surface protection films have conventionally been used for the purpose of protecting the surfaces of construction materials such as synthetic resin sheets, stainless steel sheets, aluminum sheets, decorative plywood, steel sheets, glass sheets, furniture, fixtures, home appliances, precision machinery, automobiles, and prism sheets used as optical components from scratches, dust, and dirt. A surface protection film has a structure in which an adhesive layer is formed on a predetermined support, and various proposals have been made regarding the adhesive that constitutes the adhesive layer.

[0004] Conventionally, acrylic adhesives and rubber-based adhesives mainly composed of rubber such as natural rubber and polyisobutylene have been mainly used as adhesives for the adhesive layer of the surface protection film. As a method for applying the pressure-sensitive adhesive to a predetermined support, a pressure-sensitive adhesive solution in which the pressure-sensitive adhesive is dissolved in a solvent is applied using a roll, a spray, etc. The application method has the advantage that the pressure-sensitive adhesive layer can be uniformly and thinly applied to the support, but has the problem that the use of a solvent makes it undesirable from the viewpoints of air pollution, occupational safety and health during production, economic efficiency, etc.

[0005] In view of the problems described above, co-extrusion films in which a base layer made of a polyolefin resin and an adhesive layer containing a hydrogenated styrene-based elastomer or an olefin-based elastomer are integrated together have recently been preferably used as surface protection films.

[0006] In addition, the adherends of the surface protection film have become more diverse in recent years, and there are not only adherends with smooth surfaces, but also adherends with complex irregularities on the surface. Adherends with irregularities on the surface include, for example, prism sheets used as optical members and embossed steel plates for building materials. In order to exert good adhesion to such adherends with irregularities on the surface, it is necessary to increase the adhesion of the adhesive layer constituting the surface protection film so that sufficient adhesion can be obtained even with a small contact area, and from this perspective, various materials for constituting the adhesive layer have been proposed.

[0007] For example, Patent Document 1 discloses, as a material for constituting a pressure-sensitive adhesive, a hydrogenated copolymer containing at least one polymer block A consisting of vinyl aromatic monomer units or at least one hydrogenated polymer block C consisting of conjugated diene monomer units and having a specific vinyl bond amount, and at least one hydrogenated random copolymer block B consisting of vinyl aromatic monomer units and conjugated diene monomer units and having a specific vinyl bond amount. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2017 / 126469 Summary of the Invention [Problem to be solved by the invention]

[0009] The hydrogenated copolymer disclosed in Patent Document 1 has the advantages of excellent adhesion to smooth acrylic plates, little change in adhesive strength over time, and little staining due to adhesive residue, but has the problem that the adhesive strength is easily insufficient for adherends that are difficult to adhere to, such as embossed steel plates used for building materials. In view of these problems, a method of producing a pressure-sensitive adhesive by mixing a tackifier with a hydrogenated copolymer in order to obtain sufficient adhesive strength for practical use is known. However, the incorporation of the tackifier causes problems such as roll winding, uneven thickness, equipment contamination, and equipment failure, and there is still room for improvement in terms of film-forming properties, heat resistance, and adhesive residue.

[0010] In view of the problems of the conventional techniques described above, the present invention aims to provide a hydrogenated copolymer which is excellent in the contradictory properties of sufficient adhesion and low adhesive residue even with a reduced amount of or no tackifier, and which also has excellent film-forming properties, and a pressure-sensitive adhesive composition and pressure-sensitive adhesive film containing the hydrogenated copolymer. [Means for solving the problem]

[0011] As a result of intensive research into solving the problems of the conventional techniques, the present inventors have found that, in a hydrogenated copolymer (A) which is a hydrogenated product of a copolymer comprising a conjugated diene monomer unit and a vinyl aromatic monomer unit, and a hydrogenated copolymer (X) which contains a hydrogenated copolymer (B), the hydrogenated copolymer (A) and the hydrogenated copolymer (B) have specific structures and the contents of the hydrogenated copolymer (A) and the hydrogenated copolymer (B) are within predetermined numerical ranges, thereby achieving the above-mentioned object, and have completed the present invention. That is, the present invention is as follows.

[0012] [1] A hydrogenated copolymer (A) which is a hydrogenated copolymer having vinyl aromatic monomer units and conjugated diene monomer units; and a hydrogenated copolymer (B) which is a hydrogenated copolymer having vinyl aromatic monomer units and conjugated diene monomer units, A hydrogenated copolymer (X) that satisfies the following <conditions (1) to (9)>. <Condition (1)>: The hydrogenated copolymer (A) comprises a polymer block (BS1) mainly composed of vinyl aromatic monomer units, The polymer block mainly comprises a conjugated diene monomer unit, or a random copolymer block composed of a conjugated diene monomer unit and a vinyl aromatic monomer unit, the content of all vinyl aromatic monomer units (TS1) in the hydrogenated copolymer (A) is 10 to 40 mass%; The content of the polymer block (BS1) in the hydrogenated copolymer (A) is 10 to 30% by mass. <Condition (2)>: The hydrogenated copolymer (A) has a number average molecular weight (Mn1) of 3,000 to 35,000. <Condition (3)>: The hydrogenated copolymer (B) comprises at least one polymer block (BS2) mainly composed of vinyl aromatic monomer units, At least one random copolymer block consisting of conjugated diene monomer units and vinyl aromatic monomer units is included, The hydrogenated copolymer (B) has a total vinyl aromatic monomer unit (TS2) content of 15 to 40 mass%; The content of the polymer block (BS2) in the hydrogenated copolymer (B) is 10 to 30% by mass. <Condition (4)>: The hydrogenated copolymer (B) has a number average molecular weight (Mn2) of 130,000 to 300,000. <Condition (5)>: The amount of vinyl bonds (Va) before hydrogenation derived from a conjugated diene compound in the hydrogenated copolymer (A) and the amount of vinyl bonds (Vb) before hydrogenation derived from a conjugated diene compound in the hydrogenated copolymer (B) are 50 to 90 mass%. <Condition (6)>: The difference between the vinyl bond content (Va) of the hydrogenated copolymer (A) and the vinyl bond content (Vb) of the hydrogenated copolymer (B) is ±20 (absolute value 20) mass % or less. <Condition (7)>: The ratio (Mn2 / Mn1) of the number average molecular weight (Mn2) of the hydrogenated copolymer (B) to the number average molecular weight (Mn1) of the hydrogenated copolymer (A) is 10 or more. <Condition (8)>: The hydrogenated copolymer (A) has a hydrogenation rate (Ha) of unsaturated double bonds derived from a conjugated diene compound, and the hydrogenated copolymer (B) has a hydrogenation rate (Hb) of unsaturated double bonds derived from a conjugated diene compound of 70% or more. <Condition (9)>: The mass ratio (A) / (B) of the content of the hydrogenated copolymer (A) to the content of the hydrogenated copolymer (B) is 10 / 90 to 50 / 50. [2] The hydrogenated copolymer (X) according to the above item [1], wherein the hydrogenated copolymer (A) has a number average molecular weight (Mn1) of 5,000 to 15,000. [3] the vinyl bond amount (Va) and the vinyl bond amount (Vb) are 60 to 85 mass%; The hydrogenated copolymer (X) according to [1] or [2] above, wherein the hydrogenation rate of the unsaturated double bonds derived from the conjugated diene compound in the hydrogenated copolymer (A) and the hydrogenated copolymer (B) is 85% or more. [4] The hydrogenated copolymer (X) according to any one of the above [1] to [3], wherein a ratio (MnS1 / MnS2) of a molecular weight (MnS1) of a polymer block (BS1) mainly composed of a vinyl aromatic monomer unit in the hydrogenated copolymer (A) to a molecular weight (MnS2) of a polymer block (BS2) mainly composed of a vinyl aromatic monomer unit in the hydrogenated copolymer (B) is 0.05 to 0.5. (MnS1 and MnS2 are calculated as follows. MnS1 = Mn1 × BS1 MnS2 = Mn2 × BS2 ÷ f BS1: Proton nuclear magnetic resonance ( 1The content of the polymer block mainly composed of a vinyl aromatic compound in the hydrogenated copolymer (A) determined by H-NMR BS2: Proton nuclear magnetic resonance ( 1 The content of the polymer block mainly composed of a vinyl aromatic compound in the hydrogenated copolymer (B) determined by H-NMR f: Degree of branching of hydrogenated copolymer (B) determined by GPC-light scattering method with a viscometer [5] The hydrogenated copolymer (X) according to any one of the above [1] to [4], wherein the hydrogenated copolymer (B) has a number average molecular weight (Mn2) of 150,000 to 250,000. [6] The hydrogenated copolymer (X) according to any one of [1] to [5] above, wherein a ratio (Mn2 / Mn1) of the number average molecular weight (Mn2) of the hydrogenated copolymer (B) to the number average molecular weight (Mn1) of the hydrogenated copolymer (A) is 15 or more. [7] The hydrogenated copolymer (X) according to any one of the above [1] to [6], wherein a mass ratio (A) / (B) of a content of the hydrogenated copolymer (A) to a content of the hydrogenated copolymer (B) is 25 / 75 to 50 / 50. [8] The hydrogenated copolymer (X) according to any one of [1] to [7] above, wherein the hydrogenated copolymer (A) and the hydrogenated copolymer (B) satisfy all of the following <conditions (10) to (11)>: <Condition (10)>: The hydrogenated copolymer (A) is a block copolymer represented by the general structural formula: ab or ac. <Condition (11)>: The hydrogenated copolymer (B) is a block copolymer represented by the general structural formula: dedab or dedac. (In the above general structural formula, a and d are polymer blocks mainly composed of vinyl aromatic monomer units, b and e are random copolymer blocks composed of vinyl aromatic monomer units and conjugated diene monomer units, and c is a polymer block mainly composed of conjugated diene monomer units.) [9] The hydrogenated copolymer (X) according to any one of [1] to [7] above, wherein the hydrogenated copolymer (A) and the hydrogenated copolymer (B) have the following general structural formula (a) or (b): (A): The hydrogenated copolymer (A) is represented by the general structural formula: ab, and the hydrogenated copolymer (B) is a block copolymer represented by the general structural formula: dedab. (i): The hydrogenated copolymer (A) is represented by the general structural formula: ac, and the hydrogenated copolymer (B) is a block copolymer represented by the general structural formula: dedec. (In the above general structural formula, a and d are polymer blocks mainly composed of vinyl aromatic monomer units, b and e are random copolymer blocks composed of vinyl aromatic monomer units and conjugated diene monomer units, and c is a polymer block mainly composed of conjugated diene monomer units.)

[10] A pressure-sensitive adhesive composition comprising the hydrogenated copolymer (X) according to any one of [1] to [9] above.

[11] The pressure-sensitive adhesive composition according to

[10] above, which has a weight loss of 0.4% or less after 30 minutes at 200°C as measured by TG-DTA (thermogravimetric differential thermal analysis).

[12] The hydrogenated copolymer (X) according to any one of [1] to [9] above, which has a weight loss of 0.4% or less after 30 minutes at 200°C as determined by TG-DTA (thermogravimetric differential thermal analysis).

[13] A resin substrate layer, and a layer of the pressure-sensitive adhesive composition according to

[10] or

[11] ; A, having an adhesive film.

[14] A method for producing the hydrogenated copolymer (X) according to any one of [1] to [9] and

[12] , The method comprises a step of simultaneously producing the hydrogenated copolymer (A) and the hydrogenated copolymer (B) in one reactor, In the above process, Add raw material monomers for each polymer block and a polymerization initiator in the following order (c) or (d), and then hydrogenate. A method for producing the hydrogenated copolymer (X). (c) First polymerization initiator, d, e, d, second polymerization initiator, a, b (E) First polymerization initiator, d, e, d, second polymerization initiator, a, c (In the above (c) and (d), a and d are polymer blocks mainly composed of vinyl aromatic monomer units, b and e are random copolymer blocks composed of vinyl aromatic monomer units and conjugated diene monomer units, and c is a polymer block mainly composed of conjugated diene monomer units, and raw material monomers for each polymer block are added.) Effect of the Invention

[0013] According to the present invention, there can be provided a hydrogenated copolymer having excellent adhesive properties, adhesive leave behind properties and film-forming properties, an adhesive composition containing the hydrogenated copolymer, and an adhesive film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. Note that the present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content, and the present invention can be carried out in various modifications within the scope of the gist of the present invention.

[0015] [Hydrogenated copolymer (X)] The hydrogenated copolymer (X) of the present embodiment is A hydrogenated copolymer (A) which is a hydrogenated copolymer having vinyl aromatic monomer units and conjugated diene monomer units; and a hydrogenated copolymer (B) which is a hydrogenated product of a copolymer having vinyl aromatic monomer units and conjugated diene monomer units. The hydrogenated copolymer (X) of this embodiment satisfies all of the following <conditions (1) to (9)>. <Condition (1)>: The hydrogenated copolymer (A) comprises a polymer block (BS1) mainly composed of a vinyl aromatic monomer unit (hereinafter, may be referred to as polymer block (BS1)), The polymer block mainly contains a conjugated diene monomer unit, or a random copolymer block (hereinafter sometimes referred to as a random copolymer block) containing a conjugated diene monomer unit and a vinyl aromatic monomer unit, the content of all vinyl aromatic monomer units (TS1) in the hydrogenated copolymer (A) is 10 to 40 mass%; The content of the polymer block (BS1) in the hydrogenated copolymer (A) is 10 to 30% by mass. <Condition (2)>: The hydrogenated copolymer (A) has a number average molecular weight (Mn1) of 3,000 to 35,000. <Condition (3)>: The hydrogenated copolymer (B) comprises at least one polymer block (BS2) mainly composed of a vinyl aromatic monomer unit (hereinafter, may be referred to as polymer block (BS2)), The polymer has at least one random copolymer block (hereinafter, sometimes referred to as a random copolymer block) composed of a conjugated diene monomer unit and a vinyl aromatic monomer unit, The hydrogenated copolymer (B) has a total vinyl aromatic monomer unit (TS2) content of 15 to 40 mass%; The content of the polymer block (BS2) in the hydrogenated copolymer (B) is 10 to 30% by mass. <Condition (4)>: The hydrogenated copolymer (B) has a number average molecular weight (Mn2) of 130,000 to 300,000. <Condition (5)>: The amount of vinyl bonds (Va) before hydrogenation derived from a conjugated diene compound in the hydrogenated copolymer (A) and the amount of vinyl bonds (Vb) before hydrogenation derived from a conjugated diene compound in the hydrogenated copolymer (B) are 50 to 90 mass%. <Condition (6)>: The difference between the vinyl bond content (Va) of the hydrogenated copolymer (A) and the vinyl bond content (Vb) of the hydrogenated copolymer (B) is ±20 (absolute value 20) mass % or less. <Condition (7)>: The ratio (Mn2 / Mn1) of the number average molecular weight (Mn2) of the hydrogenated copolymer (B) to the number average molecular weight (Mn1) of the hydrogenated copolymer (A) is 10 or more. <Condition (8)>: The hydrogenated copolymer (A) has a hydrogenation rate (Ha) of unsaturated double bonds derived from a conjugated diene compound, and the hydrogenated copolymer (B) has a hydrogenation rate (Hb) of unsaturated double bonds derived from a conjugated diene compound of 70% or more. <Condition (9)>: The mass ratio (A) / (B) of the content of the hydrogenated copolymer (A) to the content of the hydrogenated copolymer (B) is 10 / 90 to 50 / 50.

[0016] The hydrogenated copolymer (X) of the present embodiment is substantially a mixture of the hydrogenated copolymer (A) and the hydrogenated copolymer (B). The mixture does not only mean a mixture of multiple types of copolymers, but also means a mixture of multiple types of copolymers produced in one reactor. In other words, it also includes a form in which multiple types of copolymers are produced in one reaction.

[0017] The hydrogenated copolymer (X) of the present embodiment is a mixture in which the hydrogenated copolymer (A) and the hydrogenated copolymer (B) each have different constituent requirements. Even if the hydrogenated copolymer (X) of the present embodiment satisfies the average values ​​of the hydrogenated copolymer (A) and the hydrogenated copolymer (B) in terms of structure and physical properties, if any of the components of the hydrogenated copolymer (A) and the hydrogenated copolymer (B) deviates from the above conditions (1) to (9), the present inventors have found that the adhesive composition using the hydrogenated copolymer (X) of the present embodiment cannot achieve the desired effects in terms of adhesion, adhesive residue, and film-forming properties. Therefore, from the viewpoint of solving the problem of supplying a hydrogenated copolymer having adhesion, adhesive residue, and film-forming properties, it has been found that the structures of the hydrogenated copolymer (A) and the hydrogenated copolymer (B) constituting the hydrogenated copolymer (X) should be specified, rather than the hydrogenated copolymer (X) itself, and the present invention has been completed.

[0018] That is, if the content of vinyl aromatic monomer units in either the hydrogenated copolymer (A) or the hydrogenated copolymer (B) becomes excessive and the above condition is not satisfied, the hydrogenated copolymer (X) becomes hard and brittle, and if the amount of vinyl bonds in either one of them becomes too small and the above condition is not satisfied, the tackiness decreases, and the adhesiveness of the hydrogenated copolymer (X) decreases. From the viewpoint of adhesive residue properties, if the content of vinyl aromatic monomer units in either the hydrogenated copolymer (A) or the hydrogenated copolymer (B) is too small and the above condition is not satisfied, the cohesive force of the vinyl aromatic monomer block will be weakened. Furthermore, if the hydrogenation rate of either the hydrogenated copolymer (A) or the hydrogenated copolymer (B) is too small and the above condition is not satisfied, the hydrogenated copolymer (X) will be prone to thermal degradation and will have poor stability over time. Furthermore, if either the hydrogenated copolymer (A) or the hydrogenated copolymer (B) does not satisfy the above-mentioned conditions (1), (3), (5), (6), and (8), the compatibility between the hydrogenated copolymer (A) and the hydrogenated copolymer (B) also decreases, and the adhesive residue of the hydrogenated copolymer (X) tends to deteriorate. Furthermore, from the viewpoint of film-formability, if the hydrogenation rate of either the hydrogenated copolymer (A) or the hydrogenated copolymer (B) is too low and does not satisfy the above-mentioned condition, the hydrogenated copolymer (X) is prone to thermal degradation, gel generation occurs during molding processing, and the film-formability of the hydrogenated copolymer (X) tends to deteriorate.

[0019] By providing the above-mentioned configuration, a hydrogenated copolymer (X) having excellent adhesion, adhesive leave behind, and film-forming properties, and an adhesive composition containing the hydrogenated copolymer (X) can be obtained, and the hydrogenated copolymer (X) can be used as a material for an adhesive film.

[0020] (Hydrogenated copolymer (A)) The hydrogenated copolymer (X) of this embodiment contains the hydrogenated copolymer (A) which is a hydrogenated product of a copolymer having vinyl aromatic monomer units and conjugated diene monomer units. The hydrogenated copolymer (A) has a polymer block (BS1) mainly composed of vinyl aromatic monomer units, and a polymer block mainly composed of conjugated diene monomer units, or a random copolymer block composed of conjugated diene monomer units and vinyl aromatic monomer units (condition (1)).

[0021] In the hydrogenated copolymer (X), hydrogenated copolymer (A), and hydrogenated copolymer (B) of the present embodiment, when a vinyl aromatic compound is incorporated in each copolymer, the vinyl aromatic compound is in the form of a monomer unit constituting each copolymer, and therefore is referred to as a "vinyl aromatic monomer unit" in this specification. Similarly, when a conjugated diene compound is incorporated into a copolymer, it takes the form of a monomer unit constituting the copolymer, and is therefore referred to as a "conjugated diene monomer unit" in this specification.

[0022] In addition, in this specification, the term "mainly composed of" means that the target monomer unit is contained in the target polymer block in an amount of 95% by mass or more and 100% by mass or less.

[0023] <Vinyl aromatic compounds> Examples of the vinyl aromatic compound used to form the vinyl aromatic monomer units constituting the hydrogenated copolymer (A) include, but are not limited to, styrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylethylene, N,N-dimethyl-p-aminoethylstyrene, and N,N-diethyl-p-aminoethylstyrene. Among these, styrene, α-methylstyrene, and 4-methylstyrene are preferred from the viewpoints of availability and productivity. These may be used alone or in combination of two or more.

[0024] <Conjugated diene compounds> The conjugated diene compound used to form the conjugated diene monomer units constituting the hydrogenated copolymer (A) may be any diolefin having a conjugated double bond, and examples thereof include, but are not limited to, 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, farnesene, and the like. Among these, 1,3-butadiene and isoprene are preferred from the viewpoints of availability and productivity. These may be used alone or in combination of two or more.

[0025] The hydrogenated copolymer (A) has a polymer block (BS1) mainly composed of vinyl aromatic monomer units. The content of the polymer block (BS1) in the hydrogenated copolymer (A) is 10 to 30 mass % (condition (1)), preferably 12 to 28 mass %, more preferably 14 to 26 mass %, and even more preferably 16 to 24 mass %. When the content of the polymer block (BS1) in the hydrogenated copolymer (A) is 10% by mass or more, the compatibility with the hydrogenated copolymer (B) described later is improved, and the adhesive residue and film formability of the adhesive film using the hydrogenated copolymer (X) of this embodiment tend to be good. When the content of the polymer block (BS1) is 30% by mass or less, the hydrogenated copolymer (X) of this embodiment has a low hardness, and the adhesive property of the adhesive film made of the hydrogenated copolymer (X) tends to be good.

[0026] The hydrogenated copolymer (A) has a total vinyl aromatic monomer unit (TS1) content of 10 to 40 mass% (condition (1)), preferably 18 to 40 mass%, more preferably 22 to 40 mass%, and further preferably 25 to 37 mass%. By setting the content of all vinyl aromatic monomer units (TS1) in the hydrogenated copolymer (A) within the above range, the content of the vinyl aromatic monomer units in the random copolymer block (RS1) can be adjusted after setting the content of the polymer block (BS1) mainly composed of vinyl aromatic monomer units in the hydrogenated copolymer (A). As a result, the tan δ peak distribution obtained by dynamic viscoelasticity measurement of the hydrogenated copolymer (X) can be suitably controlled, and the adhesive leave behind and adhesive properties of the adhesive film made of the hydrogenated copolymer (X) tend to be good. In more detail, the tan δ peak distribution of the hydrogenated copolymer (X) of this embodiment is a distribution in which a narrow peak (tan δ peak value of 1 or more) on the low temperature side (-30°C to 0°C) consisting mainly of the hydrogenated copolymer (B) described later overlaps with a broad peak (tan δ peak value of 1 or less) on the high temperature side (-10°C to 20°C) consisting mainly of the hydrogenated copolymer (A). Furthermore, the broad tan δ peak of the hydrogenated copolymer (A) is due to partial compatibility between the low molecular weight polymer block (BS1) and the vinyl aromatic monomer unit in the random copolymer block, and the broad peak on the high temperature side (-10°C to 20°C) of the hydrogenated copolymer (A) tends to improve the adhesiveness of the adhesive film consisting of the hydrogenated copolymer (X).

[0027] When the hydrogenated copolymer (A) contains "a random copolymer block consisting of a conjugated diene monomer unit and a vinyl aromatic monomer unit", the content (RS1) of the vinyl aromatic monomer unit in the random copolymer block (hereinafter, when styrene is used, this may be referred to as the styrene content in the random copolymer block or the random styrene amount) is preferably in the range of 0 to 33 mass%, more preferably in the range of 8 to 30 mass%, and even more preferably in the range of 10 to 25 mass%. When the (RS1) is within the above range, the tan δ peak temperature obtained by measuring the dynamic viscoelasticity of the hydrogenated copolymer (X) is controlled within a preferred range, and the payout property of the adhesive film made of the hydrogenated copolymer (X) tends to be good. The preferred range of the tan δ peak temperature of the hydrogenated copolymer (X) is −30° C. to 20° C., and when the tan δ peak is 20° C. or lower, the adhesiveness tends to be excellent, whereas when the tan δ peak is −30° C. or higher, the adhesive surface tends to have good releasability.

[0028] The total vinyl aromatic monomer unit (TS1) of the hydrogenated copolymer (A), the content of the polymer block (BS1) mainly composed of vinyl aromatic monomer units, and the content of the vinyl aromatic monomer unit (RS1) in the random copolymer block can be measured by nuclear magnetic resonance (NMR). Specifically, they can be measured by the method described in the examples below, and can be controlled to the above-mentioned numerical range by adjusting the amount of vinyl aromatic compound added in the polymerization process and the timing of addition.

[0029] The hydrogenated copolymer (A) has a number average molecular weight (Mn1) of 3,000 to 35,000 (condition (2)). The (Mn1) is preferably 4,000 to 20,000, and more preferably 5,000 to 15,000. When the (Mn1) is 3,000 or more, the adhesive transfer property and film formability of the adhesive film made of the hydrogenated copolymer (X) of the present embodiment tend to be good, and when it is 35,000 or less, the adhesive property of the adhesive film using the hydrogenated copolymer (X) tends to be good. The number average molecular weight (Mn1) of the hydrogenated copolymer (A) can be measured by gel permeation chromatography (hereinafter referred to as GPC) using standard polystyrene as a calibration curve. Specifically, it can be measured by the method described in the examples below. The number average molecular weight (Mn1) of the hydrogenated copolymer (A) can be controlled within the above-mentioned range by adjusting conditions such as the amount of monomer added and the amount of polymerization initiator added in the polymerization step.

[0030] The amount of vinyl bonds (Va) before hydrogenation derived from the conjugated diene compound in the hydrogenated copolymer (A) is 50 to 90 mass % (condition (5)), more preferably 55 to 85 mass %, further preferably 60 to 85 mass %. When the vinyl bond amount (Va) is within the above range, the adhesive property of the adhesive film made of the hydrogenated copolymer (X) of the present embodiment tends to be good.

[0031] In the hydrogenated copolymer (X) of the present embodiment, the difference between the vinyl bond amount (Va) before hydrogenation derived from a conjugated diene compound in the hydrogenated copolymer (A) and the vinyl bond amount (Vb) before hydrogenation derived from a conjugated diene compound in the hydrogenated copolymer (B) described below is within ±20 (absolute value 20) mass% (condition (6)), more preferably within ±15 mass%, and further preferably within ±10 mass%. When the difference between the vinyl bond amount (Va) and the vinyl bond amount (Vb) is within the above range, the compatibility between the hydrogenated copolymer (A) and the hydrogenated copolymer (B) described later is improved, and the adhesive residue and film formability of the pressure-sensitive adhesive film using the hydrogenated copolymer (X) of the present embodiment tend to be good.

[0032] In the present embodiment, the vinyl bond amount refers to the total content of 1,2-vinyl bonds (conjugated dienes incorporated into the polymer via 1,2-bonds) and 3,4-vinyl bonds (conjugated dienes incorporated into the polymer via 3,4-bonds) relative to the total conjugated dienes (here, when 1,3-butadiene is used as the conjugated diene, the 1,2-vinyl bond amount, and when isoprene is used as the conjugated diene, the 3,4-vinyl bond amount).

[0033] The amount of vinyl bonds can be measured by a nuclear magnetic resonance (NMR) spectrometer. The microstructure (cis / trans ratio, amount of vinyl bonds) derived from the conjugated diene compound in the hydrogenated copolymer (A) and the hydrogenated copolymer (B) described later can be arbitrarily controlled by using a polar compound, etc. described later.

[0034] The hydrogenation rate (Ha) (also referred to as hydrogenation rate) of the unsaturated double bonds derived from the conjugated diene compound in the hydrogenated copolymer (A) is 70% or more (condition (8)), more preferably 85% or more, and even more preferably 95% or more. When the hydrogenation rate (Ha) is 70% or more, gelation during film formation of the hydrogenated copolymer (X) of the present embodiment is suppressed, and the heat resistance of the adhesive film is improved, so that the film formability and adhesive residue tend to be good.

[0035] In addition, it is preferable that the amount of vinyl bonds (Va) before hydrogenation of the hydrogenated copolymer (A) is 60 to 85 mass%, the hydrogenation rate of the hydrogenated copolymer (A) is 85% or more, and the vinyl bonds (1,2-vinyl bonds) of the hydrogenated copolymer (A) are selectively hydrogenated in preference to unsaturated double bonds (1,4-bonds) other than vinyl bonds. "Selectively hydrogenated" means that 85% or more of the vinyl bonds before hydrogenation are hydrogenated, and preferably 90% or more of the vinyl bonds before hydrogenation are hydrogenated. When a conjugated copolymer is hydrogenated, the hydrogenation reaction of the 1,2-vinyl bonds proceeds faster than that of the double bonds formed by 1,4-addition. Therefore, when the hydrogenation rate of the unsaturated double bonds derived from the conjugated diene compound is greater than the amount of vinyl bonds before hydrogenation derived from the conjugated diene compound, that is, when (Ha)>(Va) is satisfied, the vinyl bonds are almost hydrogenated to become single-bonded butyl groups. By selectively hydrogenating the vinyl bonds of the hydrogenated copolymer (A), the vinyl bonds that cause deterioration of thermal stability and stickiness are eliminated, and therefore the stickiness and thermal deterioration (oxidative deterioration) of the hydrogenated copolymer (X) can be suppressed. The pellet blocking property of the hydrogenated copolymer (X) is improved, fisheyes in the adhesive film are reduced, and the film thickness stability and the stability of various adhesive properties tend to be improved.

[0036] The hydrogenation rate of the unsaturated double bonds derived from the conjugated diene compound in the hydrogenated copolymer (A) can be controlled, for example, by adjusting the amount of catalyst used during hydrogenation, and the hydrogenation rate can be controlled, for example, by adjusting the amount of catalyst, the amount of hydrogen feed, the pressure, the temperature, etc. during hydrogenation. The hydrogenation rate of the unsaturated double bonds derived from the conjugated diene compound in the hydrogenated copolymer (A) can be measured by a nuclear magnetic resonance (NMR) spectrometer.

[0037] The structure of the hydrogenated copolymer (A) is not limited as long as it has a polymer block (BS1) mainly composed of vinyl aromatic monomer units, and a polymer block mainly composed of conjugated diene monomer units or a random copolymer block composed of conjugated diene monomer units and vinyl aromatic monomer units. For example, it is preferable that the hydrogenated copolymer (A) has a structure represented by the following general formula:

[0038] ab ac abc acb bac cab bab cac aba aca In the above formula, a, b, and c represent polymer blocks (a), (b), and (c), respectively. In each of the general formulae representing the hydrogenated copolymer (A) described above, (a) is a polymer block mainly composed of vinyl aromatic monomer units, (b) is a random copolymer block composed of vinyl aromatic monomer units and conjugated diene monomer units, and (c) is a polymer block mainly composed of conjugated diene monomer units.

[0039] From the viewpoint of productivity, the hydrogenated copolymer (A) preferably has a sequential polymerization structure, and in the above general formula, ab or ac is more preferable (condition (10)). It is most preferable that the hydrogenated copolymer (A) has the same block structure as the terminal of the structure represented by the general formula of the hydrogenated copolymer (B) described later. That is, when the hydrogenated copolymer (B) described later has a structure having an ab block at the terminal, the hydrogenated copolymer (A) also has an ab block, and when the hydrogenated copolymer (B) has an ac block at the terminal, the hydrogenated copolymer (A) also has an ac block. Specifically, the hydrogenated copolymer (A) preferably has the structure ab or ac in the above general formula (condition (10)), and the hydrogenated copolymer (B) described below is preferably a block copolymer represented by the general structural formula: dedab or dedac (condition (11)), where a and d are polymer blocks mainly composed of vinyl aromatic monomer units, b and e are random copolymer blocks composed of vinyl aromatic monomer units and conjugated diene monomer units, and c is a polymer block mainly composed of conjugated diene monomer units. By having the same block, the compatibility between the hydrogenated copolymer (A) and the hydrogenated copolymer (B) tends to be increased, the pellet blocking property of the hydrogenated copolymer (X) of the present embodiment tends to be improved, and the payout property and the adhesion enhancement property of the adhesive film made of the hydrogenated copolymer (X) of the present embodiment tend to be improved.

[0040] From the viewpoint of productivity, the hydrogenated copolymer (A) is preferably polymerized by sequential polymerization. "Polymerized by sequential polymerization" means that the copolymer is sequentially polymerized from one end of the final target polymer structure to the other end, without using a coupling reaction.

[0041] The hydrogenated copolymer (A) preferably has a ratio (Mw1 / Mn1) of the weight average molecular weight (Mw1) to the number average molecular weight (Mn1) of less than 1.20, more preferably 1.15 or less, and even more preferably 1.13 or less. When the (Mw1 / Mn1) is less than 1.20, the mechanical strength of the hydrogenated copolymer (X) tends to be improved. The hydrogenated copolymer (A) does not have a branched structure and tends to be easily produced by sequential polymerization.

[0042] (Hydrogenated copolymer (B)) The hydrogenated copolymer (X) of the present embodiment contains the hydrogenated copolymer (B). The hydrogenated copolymer (B) has at least one polymer block (BS2) mainly composed of vinyl aromatic monomer units, and at least one random copolymer block composed of conjugated diene monomer units and vinyl aromatic monomer units (condition (3)).

[0043] <Vinyl aromatic compounds> Examples of the vinyl aromatic compound forming the vinyl aromatic monomer unit of the hydrogenated copolymer (B) include, but are not limited to, styrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylethylene, N,N-dimethyl-p-aminoethylstyrene, and N,N-diethyl-p-aminoethylstyrene. Among these, styrene, α-methylstyrene, and 4-methylstyrene are preferred from the viewpoints of availability and productivity. These may be used alone or in combination of two or more.

[0044] <Conjugated diene compounds> The conjugated diene compound forming the conjugated diene monomer unit of the hydrogenated copolymer (B) may be any diolefin having a conjugated double bond, and examples thereof include, but are not limited to, 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, farnesene, and the like. Among these, 1,3-butadiene and isoprene are preferred from the viewpoints of availability and productivity. These may be used alone or in combination of two or more.

[0045] The hydrogenated copolymer (B) has a polymer block (BS2) mainly composed of vinyl aromatic monomer units, and the content of the polymer block (BS2) is 10 to 30 mass% of the hydrogenated copolymer (B) (condition (3)), preferably 12 to 28 mass%, more preferably 14 to 26 mass%, and even more preferably 16 to 24 mass%. When the content of the polymer block (BS2) is within the above range, the hydrogenated copolymer (X) of the present embodiment tends to have low hardness and high mechanical strength, and the adhesive film tends to have good adhesiveness.

[0046] The hydrogenated copolymer (B) has a total vinyl aromatic monomer unit (TS2) content of 15 to 40 mass% (condition (3)), preferably 18 to 40 mass%, more preferably 22 to 40 mass%, and further preferably 25 to 37 mass%. When the (TS2) is within the above range, the content of the polymer block (BS2) mainly composed of vinyl aromatic monomer units in the hydrogenated copolymer (B) is set, and then the content of the vinyl aromatic monomer unit (RS2) in the random copolymer block is adjusted, whereby the strength of the hydrogenated copolymer (X) of this embodiment can be increased, the tan δ peak distribution obtained by dynamic viscoelasticity measurement can be controlled, and the adhesive leave behind and adhesive properties of the adhesive film made of the hydrogenated copolymer (X) of this embodiment tend to be improved. To explain in more detail, the tan δ peak distribution of the hydrogenated copolymer (X) of this embodiment is a distribution in which a narrow peak (tan δ peak value of 1 or more) on the low temperature side (-30°C to 0°C) mainly composed of the hydrogenated copolymer (B) overlaps with a broad peak (tan δ peak value of 1 or less) on the high temperature side (-10°C to 20°C) mainly composed of the hydrogenated copolymer (A). The narrow peak on the low temperature side (-30°C to 0°C) of the hydrogenated copolymer (B) tends to improve the adhesive residue of the adhesive film composed of the hydrogenated copolymer (X) of this embodiment.

[0047] The hydrogenated copolymer (B) has a random copolymer block composed of a conjugated diene monomer unit and a vinyl aromatic monomer unit, and the content (RS2) of the vinyl aromatic monomer unit in the random copolymer block (hereinafter, when styrene is used, this may be referred to as the styrene content in the random structure or the random styrene amount) is preferably 6 to 33 mass%, more preferably 8 to 30 mass%, and further preferably 10 to 25 mass%. When the content (RS2) of the vinyl aromatic monomer unit in the random copolymer block is within the above-mentioned range, the tan δ peak temperature obtained by dynamic viscoelasticity measurement of the hydrogenated copolymer (X) of the present embodiment can be controlled within a preferred range, and the payout property and adhesion enhancement property of the adhesive film made of the hydrogenated copolymer (X) of the present embodiment tend to be good. The preferred range of the tan δ peak temperature of the hydrogenated copolymer (X) of this embodiment is −30° C. to 20° C., and the adhesiveness tends to be excellent when the tan δ peak is in the range of 20° C. or less. On the other hand, when the tan δ peak is −30° C. or more, the adhesive surface tends to have good releasability.

[0048] The total vinyl aromatic monomer unit (TS2) content of the hydrogenated copolymer (B), the content of the polymer block (BS2) mainly composed of vinyl aromatic monomer units, and the content of the vinyl aromatic monomer unit (RS2) in the random copolymer block can be measured by nuclear magnetic resonance (NMR). Specifically, they can be measured by the method described in the examples below. The contents of (TS2), (BS2) and (RS2) in the hydrogenated copolymer (B) can be controlled within the above numerical ranges by adjusting the amount of the vinyl aromatic compound added in the polymerization step and the timing of its addition.

[0049] The number average molecular weight (Mn2) of the hydrogenated copolymer (B) is from 130,000 to 300,000 (condition (4)), preferably from 140,000 to 275,000, and more preferably from 150,000 to 250,000. When the (Mn2) is 130,000 or more, the adhesive residue of the adhesive film made of the hydrogenated copolymer (X) of this embodiment becomes good, and when the (Mn2) is 300,000 or less, the film-forming property of the adhesive film made of the hydrogenated copolymer (X) tends to be good. The number average molecular weight (Mn2) of the hydrogenated copolymer (B) can be measured by gel permeation chromatography (hereinafter referred to as GPC) using standard polystyrene as a calibration curve. Specifically, it can be measured by the method described in the examples below. The number average molecular weight (Mn2) of the hydrogenated copolymer (B) can be controlled within the above-mentioned range by adjusting conditions such as the amount of monomer added and the amount of polymerization initiator added in the polymerization step.

[0050] The amount of vinyl bonds (Vb) before hydrogenation derived from the conjugated diene compound in the hydrogenated copolymer (B) is 50 to 90 mass % (condition (5)), more preferably 55 to 85 mass %, and further preferably 60 to 85 mass %. When the vinyl bond amount (Vb) is within the above range, the adhesive film made of the hydrogenated copolymer (X) of the present embodiment tends to have good adhesiveness.

[0051] The difference between the vinyl bond amount (Va) before hydrogenation derived from the conjugated diene compound in the hydrogenated copolymer (A) and the vinyl bond amount (Vb) before hydrogenation derived from the conjugated diene compound in the hydrogenated copolymer (B) is within ±20 (absolute value 20) mass% (condition (6)), more preferably within ±15 mass%, and further preferably within ±10 mass%. When the difference between the vinyl bond amount (Va) and the vinyl bond amount (Vb) is within the above-mentioned range, the compatibility between the hydrogenated copolymer (A) and the hydrogenated copolymer (B) is enhanced, and the adhesive residue and film formability of the pressure-sensitive adhesive film using the hydrogenated copolymer (X) of the present embodiment tend to be good.

[0052] In the present embodiment, the vinyl bond content refers to the total content of 1,2-vinyl bonds (conjugated dienes incorporated into the polymer via 1,2-bonds) and 3,4-vinyl bonds (conjugated dienes incorporated into the polymer via 3,4-bonds) relative to the total conjugated dienes (here, when 1,3-butadiene is used as the conjugated diene, the 1,2-vinyl bond content, and when isoprene is used as the conjugated diene, the 3,4-vinyl bond content).

[0053] The amount of vinyl bonds can be measured using a nuclear magnetic resonance (NMR) spectrometer. The microstructure (cis / trans ratio, amount of vinyl bonds) derived from the conjugated diene compound in the hydrogenated copolymer (B) can be arbitrarily controlled by using a polar compound or the like described later.

[0054] The hydrogenation rate (Hb) (also referred to as hydrogenation rate) of the unsaturated double bonds derived from the conjugated diene compound in the hydrogenated copolymer (B) is 70% or more (condition (8)), more preferably 85% or more, and even more preferably 95% or more. When the (Hb) is 70% or more, gelation during film formation of the hydrogenated copolymer (X) of this embodiment is suppressed, and the heat resistance of the adhesive film is improved, so that the film formability and adhesive residue tend to be good.

[0055] It is also preferred that the amount of vinyl bonds (Vb) of the hydrogenated copolymer (B) before hydrogenation is 60 to 85 mass%, the hydrogenation rate of the hydrogenated copolymer (B) is 85% or more, and the vinyl bonds in the hydrogenated copolymer (B) are preferentially hydrogenated selectively. The definition of "selectively hydrogenated" is the same as that of (Va). When (Hb)>(Vb) is satisfied, the vinyl bonds in the hydrogenated copolymer (B) are almost entirely hydrogenated. By selectively hydrogenating the vinyl bonds of the hydrogenated copolymer (B), the vinyl bonds that are the cause of particularly deteriorating thermal stability and stickiness are eliminated, and the stickiness and thermal degradation (oxidative degradation) of the hydrogenated copolymer (X) of this embodiment can be suppressed. As a result, the hydrogenated copolymer (X) of this embodiment has good pellet blocking properties, reduces fisheyes in the adhesive film, and tends to have good film thickness stability and stability of various adhesive properties.

[0056] The hydrogenation rate of the unsaturated double bonds derived from the conjugated diene compound in the hydrogenated copolymer (B) can be controlled, for example, by adjusting the amount of catalyst used during hydrogenation, and the hydrogenation rate can be controlled, for example, by adjusting the amount of catalyst, the amount of hydrogen feed, the pressure, the temperature, etc. during hydrogenation. The hydrogenation rate of the unsaturated double bonds derived from the conjugated diene compound in the hydrogenated copolymer (B) can be measured by a nuclear magnetic resonance (NMR) spectrometer.

[0057] The hydrogenated copolymer (B) is not limited as long as it has a structure having a polymer block mainly composed of vinyl aromatic monomer units and a random copolymer block composed of conjugated diene monomer units and vinyl aromatic monomer units. For example, it is preferable that the hydrogenated copolymer (B) has a structure represented by the following general formula:

[0058] dedab Dedicated deab deac dedb dedic ded (de) n (deab) n (deac) n (de) m -Z (deab) m -Z (deac) m -Z In the above formula, a, b, c, d, and e represent polymer blocks (a), (b), (c), (d), and (e), respectively.

[0059] In each of the general formulae representing the hydrogenated copolymer (B) described above, (a) and (d) are polymer blocks mainly composed of a vinyl aromatic compound, (d) has a molecular weight twice or more, preferably five times or more, of (a), (b) and (e) are random copolymer blocks composed of vinyl aromatic monomer units and conjugated diene monomer units, (e) has a molecular weight twice or more, preferably five times or more, of (b), and (c) is a polymer block mainly composed of conjugated diene monomer units. n is an integer of 1 or more, preferably an integer of 1 to 10, and more preferably an integer of 1 to 5. m is an integer of 2 or more, preferably an integer of 2 to 11, and more preferably an integer of 2 to 8. Z represents a coupling agent residue. Here, the coupling agent residue means a residue of a coupling agent used for bonding between polymer blocks (e), between polymer blocks (b), and between polymer blocks (c) after bonding. The coupling agent is not limited to the following, but examples thereof include polyhalogen compounds and acid esters, which will be described later.

[0060] From the viewpoint of productivity and strength of the sequential polymerization structure, the structure of the hydrogenated copolymer (B) is more preferably dedab or dedac, and the hydrogenated copolymer (B) is most preferably one having the same structure at the end as the block structure of the structure represented by the general formula of the hydrogenated copolymer (A). That is, when the hydrogenated copolymer (B) has an ab block at the end, the hydrogenated copolymer (A) also has an ab block, and when the hydrogenated copolymer (B) has an ac block at the end, the hydrogenated copolymer (A) also has an ac block. By having the same block, the compatibility of the hydrogenated copolymer (A) and the hydrogenated copolymer (B) tends to be increased, the pellet blocking property of the hydrogenated copolymer (X) of this embodiment is improved, and the payout property and adhesion enhancement property of the adhesive film made of the hydrogenated copolymer (X) of this embodiment tend to be improved.

[0061] In addition, from the viewpoint of the balance between adhesive leave behind property and adhesiveness, the hydrogenated copolymer (X) of the present embodiment preferably has a general structural formula of the hydrogenated copolymer (A) and the hydrogenated copolymer (B) shown below as (A) or (B). (A): The hydrogenated copolymer (A) is represented by the general structural formula: ab, and the hydrogenated copolymer (B) is represented by the general structural formula: dedab. (i): The hydrogenated copolymer (A) is represented by the general structural formula: ac, and the hydrogenated copolymer (B) is represented by the general structural formula: dedec. (In the above general structural formula, a and d are polymer blocks mainly composed of vinyl aromatic monomer units, b and e are random copolymer blocks composed of vinyl aromatic monomer units and conjugated diene monomer units, and c is a polymer block mainly composed of conjugated diene monomer units.)

[0062] The hydrogenated copolymer (B) is preferably polymerized by step-growth polymerization, in terms of high elongation and mechanical strength, and in terms of productivity. "Polymerized by step-growth polymerization" means that the copolymer is polymerized step-growth-wise from one end of the final target polymer structure to the other end, without using a coupling reaction.

[0063] The ratio (Mw2 / Mn2) of the weight average molecular weight (Mw2) to the number average molecular weight (Mn2) of the hydrogenated copolymer (B) is preferably less than 1.20, more preferably 1.15 or less, and even more preferably 1.13 or less. When (Mw2 / Mn2) is less than 1.20, the mechanical strength tends to be improved, and the polymer does not have a branched structure and tends to be easily produced by sequential polymerization.

[0064] (Classification of hydrogenated copolymer (A) and hydrogenated copolymer (B)) The hydrogenated copolymer (X) of the present embodiment contains the hydrogenated copolymer (A) and the hydrogenated copolymer (B), and therefore has two or more peaks in the GPC chart. Among them, the hydrogenated copolymer (A) refers to all components having a number average molecular weight of 35,000 or less, and the hydrogenated copolymer (B) refers to all components having a number average molecular weight of 130,000 or more (conditions (2) and (4)). The hydrogenated copolymer (A) and the hydrogenated copolymer (B), which are the components of the hydrogenated copolymer (X) of the present embodiment, can be separated by GPC. Specifically, they can be measured by the method described in the examples below.

[0065] (Relationship between number average molecular weights of hydrogenated copolymers (A) and (B)) In the hydrogenated copolymer (X) of this embodiment, the ratio (Mn2 / Mn1) of the number average molecular weight (Mn2) of the hydrogenated copolymer (B) to the number average molecular weight (Mn1) of the hydrogenated copolymer (A) is 10 or more (condition (7)), preferably 15 or more, more preferably 20 or more, and even more preferably 25 or more. When (Mn1 / Mn2) is 10 or more, the adhesive film using the hydrogenated copolymer (X) of this embodiment tends to have good adhesiveness and adhesive residue. (Mn1 / Mn2) can be controlled within the above-mentioned numerical range by adjusting the polymerization conditions such as the amount of monomer added, the amount of polymerization initiator added, and the polymerization time in the polymerization step of the hydrogenated copolymer (A) and the hydrogenated copolymer (B).

[0066] (Mass ratio of hydrogenated copolymer (A) to hydrogenated copolymer (B)) In the hydrogenated copolymer (X) of the present embodiment, the mass ratio (A) / (B) of the contents of the hydrogenated copolymer (A) and the hydrogenated copolymer (B) is 10 / 90 to 50 / 50 (condition (9)), preferably 20 / 80 to 50 / 50, more preferably 25 / 75 to 50 / 50, and even more preferably 30 / 70 to 50 / 50. When the mass ratio (A) / (B) of the contents of the hydrogenated copolymer (A) and the hydrogenated copolymer (B) is within the above-mentioned range, the adhesive film made of the hydrogenated copolymer (X) of this embodiment tends to have good film formability, adhesiveness, and adhesive residue.

[0067] (Relationship between molecular weights of blocks mainly composed of vinyl aromatic monomer units in hydrogenated copolymers (A) and (B)) In the hydrogenated copolymer (X) of this embodiment, the hydrogenated copolymer (A) and the hydrogenated copolymer (B) each have polymer blocks (BS1) and (BS2) mainly composed of vinyl aromatic monomer units, respectively. The ratio (MnS1 / MnS2) of the molecular weight (MnS1) of the polymer block mainly composed of vinyl aromatic monomer units in the hydrogenated copolymer (A) to the molecular weight (MnS2) of the polymer block mainly composed of vinyl aromatic monomer units in the hydrogenated copolymer (B) is preferably 0.05 to 0.50, more preferably 0.05 to 0.20, and further preferably 0.07 to 0.15. When (MnS1 / MnS2) is in the above-mentioned range, the compatibility between the hydrogenated copolymer (A) and the hydrogenated copolymer (B) and the heat resistance of the hydrogenated copolymer (X) of the present embodiment are maintained good, and the pellet blocking property, the payout property of the adhesive film, and the adhesion enhancement property of the hydrogenated copolymer (X) of the present embodiment tend to be good.

[0068] Incidentally, (MnS1) and (MnS2) can be controlled by adjusting the amount of monomer added during polymerization. MnS1 and MnS2 are calculated by the following method. MnS1 = Mn1 × BS1 MnS2 = Mn2 × BS2 ÷ f BS1: Proton nuclear magnetic resonance ( 1 The content of the polymer block mainly composed of a vinyl aromatic compound in the hydrogenated copolymer (A) determined by H-NMR BS2: Proton nuclear magnetic resonance ( 1 The content of the polymer block mainly composed of a vinyl aromatic compound in the hydrogenated copolymer (B) determined by H-NMR f: Degree of branching of hydrogenated copolymer (B) determined by GPC-light scattering method with a viscometer Mn1: Number average molecular weight of hydrogenated copolymer (A) Mn2: Number average molecular weight of hydrogenated copolymer (B) (Mn1) and (Mn2) can be measured by GPC using standard polystyrene as a calibration curve. (BS1) and (BS2) can be measured by NMR. (f) can be measured by a GPC-light scattering method equipped with a viscosity detector. The specific measurement method will be described later.

[0069] The method for measuring the mass fractions (RS1) and (RS2) of the vinyl aromatic monomer units in the random copolymer blocks of the hydrogenated copolymers (A) and (B) and the contents of the polymer blocks (BS1) and (BS2) mainly composed of vinyl aromatic monomer units will be specifically described using the NMR method and taking as an example a case in which the vinyl aromatic compound is styrene and the conjugated diene compound is 1,3-butadiene. The samples were prepared by dissolving 30 mg of hydrogenated copolymer (A) and 30 mg of hydrogenated copolymer (B) in 1 g of deuterated chloroform. 1 H-NMR was measured, and the content (BS) of polymer blocks mainly composed of vinyl aromatic monomer units (in this case, polystyrene blocks) was calculated from the ratio of the integrated value of chemical shifts from 6.9 ppm to 6.3 ppm to the total integrated value. Block styrene strength (b-St strength) = (integrated value of 6.9 ppm to 6.3 ppm) / 2 Random styrene strength (r-St strength) = (integrated value of 7.5 ppm to 6.9 ppm) - 3 × (b-St) Ethylene-butylene strength (EB strength) = Total integrated value - 3 x {(b-St intensity) + (r-St intensity)} / 8 Polystyrene Block Content (BS) =104×(b-St strength) / [104×{(b-St strength)+(r-St strength)}+56×(EB strength)] Styrene content in random copolymer block (RS) =104×(r-St strength) / {104×(r-St strength)+56×(EB strength)}

[0070] (Degree of branching (f) of hydrogenated copolymer (B)) The branching degree (f) of the hydrogenated copolymer (B) can be measured by a GPC-light scattering method equipped with a viscosity detector. Using the hydrogenated copolymer (B) as a sample, carry out GPC-light scattering measurement with a viscosity detector, and based on the standard polystyrene, determine the absolute molecular weight (M) from the results of the light scattering detector and RI detector, and the intrinsic viscosity ([η]) from the results of the RI detector and viscosity detector. Next, the reference intrinsic viscosity ([η]0) is calculated by the following formula. [η]0=a×M b a = -0.788 + 0.421 × (content of vinyl aromatic monomer units in hydrogenated copolymer (B)) -0.342×(RS2)-0.197×(BS2) b = 1.601 - 0.081 x (vinyl aromatic monomer unit content of hydrogenated copolymer (B)) +0.064×(RS2)+0.039×(BS2) RS2: Content of vinyl aromatic monomer units in the random copolymer block of hydrogenated copolymer (B) BS2: Proton nuclear magnetic resonance ( 1 The content of the polymer block mainly composed of vinyl aromatic monomer units in the hydrogenated copolymer (B) determined by H-NMR M: Absolute molecular weight of hydrogenated copolymer (B) Next, the shrinkage factor g is calculated as the ratio of the intrinsic viscosity ([η]) of the hydrogenated copolymer (B) to the reference intrinsic viscosity ([η]0). Shrinkage factor (g)=[η] / [η]0 The resulting shrinkage factor (g) is then used to calculate the branching degree (f), which is defined as g=f / [(f+1)(f+2)] (f≧2).

[0071] (Method for Producing Hydrogenated Copolymer (A) and Hydrogenated Copolymer (B)) Examples of methods for producing the hydrogenated copolymer (A) and the hydrogenated copolymer (B) include, but are not limited to, methods described in JP-B-36-19286, JP-B-43-17979, JP-B-46-32415, JP-B-49-36957, JP-B-48-2423, JP-B-48-4106, JP-B-51-49567, and JP-A-59-166518.

[0072] The copolymer before hydrogenation can be obtained, for example, by a method of carrying out living anionic polymerization using a predetermined monomer in a hydrocarbon solvent using a polymerization initiator such as an organic alkali metal compound, but is not limited to the following. Examples of the hydrocarbon solvent include, but are not limited to, aliphatic hydrocarbons such as n-butane, isobutane, n-pentane, n-hexane, n-heptane, and n-octane; alicyclic hydrocarbons such as cyclohexane, cycloheptane, and methylcycloheptane; and aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene.

[0073] As the polymerization initiator, an organic alkali metal compound that is generally known to have anionic polymerization activity toward conjugated diene compounds and vinyl aromatic compounds can be used. For example, there may be mentioned an aliphatic hydrocarbon alkali metal compound having 1 to 20 carbon atoms, an aromatic hydrocarbon alkali metal compound having 1 to 20 carbon atoms, an organic amino alkali metal compound having 1 to 20 carbon atoms, and the like. The alkali metal contained in the polymerization initiator is not limited to the following, but examples thereof include lithium, sodium, and potassium. One or more types of alkali metals may be contained in one molecule of the organic alkali metal compound. Examples of the polymerization initiator include, but are not limited to, n-propyllithium, n-butyllithium, sec-butyllithium, tert-butyllithium, n-pentyllithium, n-hexyllithium, benzyllithium, phenyllithium, tolyllithium, a reaction product of diisopropenylbenzene and sec-butyllithium, and a reaction product of divinylbenzene, sec-butyllithium, and a small amount of 1,3-butadiene. Furthermore, 1-(t-butoxy)propyllithium disclosed in U.S. Patent No. 5,708,092 and lithium compounds into which one or several molecules of an isoprene monomer have been inserted to improve the solubility thereof, siloxy group-containing alkyllithiums such as 1-(t-butyldimethylsiloxy)hexyllithium disclosed in British Patent No. 2,241,239, amino group-containing alkyllithiums disclosed in U.S. Patent No. 5,527,753, diisopropylamide lithium, hexamethyldisilazide lithium and other aminolithiums can also be used.

[0074] The amount of the lithium compound used as a polymerization initiator depends on the molecular weight of the desired copolymer, but is preferably 0.005 to 6.4 phm (parts by mass per 100 parts by mass of monomer), and more preferably 0.005 to 1.3 phm.

[0075] When a conjugated diene compound and a vinyl aromatic compound are copolymerized using an organic alkali metal compound as a polymerization initiator, a tertiary amine compound or an ether compound can be added in order to adjust the content of vinyl bonds (1,2-bonds or 3,4-bonds) resulting from the conjugated diene compound incorporated in the copolymer and to adjust the random copolymerizability of the conjugated diene compound and the vinyl aromatic compound.

[0076] The tertiary amine compound is not particularly limited, but examples thereof include compounds represented by the following formula: R1R2R3N (In the formula, R1, R2, and R3 are a hydrocarbon group having 1 to 20 carbon atoms or a hydrocarbon group having a tertiary amino group.) Examples of such tertiary amine compounds include, but are not limited to, trimethylamine, triethylamine, tributylamine, N,N-dimethylaniline, N-ethylpiperidine, N-methylpyrrolidine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetraethylethylenediamine, 1,2-dipiperidinoethane, trimethylaminoethylpiperazine, N,N,N',N'',N''-pentamethylethylenetriamine, N,N'-dioctyl-p-phenylenediamine, etc. Among these, N,N,N',N'-tetramethylethylenediamine is preferred.

[0077] As the ether compound, a linear ether compound, a cyclic ether compound, or the like can be used. Examples of the linear ether compound include dialkyl ether compounds of ethylene glycol, such as dimethyl ether, diethyl ether, diphenyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and ethylene glycol dibutyl ether; and dialkyl ether compounds of diethylene glycol, such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, and diethylene glycol dibutyl ether. Examples of cyclic ether compounds include tetrahydrofuran, dioxane, 2,5-dimethyloxolane, 2,2,5,5-tetramethyloxolane, 2,2-bis(2-oxolanyl)propane, and alkyl ethers of furfuryl alcohol.

[0078] The amount of the tertiary amine compound or ether compound used is preferably 0.1 to 4 (mol / mol of alkali metal), more preferably 0.2 to 3 (mol / mol of alkali metal), relative to the amount of the polymerization initiator of the organic alkali metal compound.

[0079] In the process for producing the hydrogenated copolymers (A) and (B), sodium alkoxide may be present when copolymerizing a conjugated diene compound with a vinyl aromatic compound. The sodium alkoxide is, for example, a compound represented by the following formula, but is not limited thereto: In particular, sodium alkoxides having an alkyl group having 3 to 6 carbon atoms are preferred, and sodium t-butoxide and sodium t-pentoxide are more preferred. NaOR (In the formula, R is an alkyl group having 2 to 12 carbon atoms.) The amount of sodium alkoxide used in the polymerization step of the hydrogenated copolymers (A) and (B) is preferably 0.01 or more and less than 0.1 (molar ratio), more preferably 0.01 or more and less than 0.08 (molar ratio), even more preferably 0.03 or more and less than 0.08 (molar ratio), and still more preferably 0.04 or more and less than 0.06 (molar ratio), relative to the vinyl bond amount regulator (tertiary amine compound or ether compound). When the amount of sodium alkoxide is within this range, it tends to be possible to produce at a high productivity a copolymer having a narrow molecular weight distribution, which has a copolymer block containing a conjugated diene monomer unit having a high vinyl bond amount and a polymer block mainly composed of a vinyl aromatic monomer unit having a narrow molecular weight distribution.

[0080] The method for copolymerizing a conjugated diene compound and a vinyl aromatic compound using an organic alkali metal compound as a polymerization initiator is not particularly limited, and may be batch polymerization, continuous polymerization, or a combination thereof. The polymerization temperature is not particularly limited, but is usually from 0 to 180°C, and preferably from 30 to 150°C. The time required for polymerization varies depending on the conditions, but is usually within 48 hours, and preferably 0.1 to 10 hours. It is also preferable to carry out the polymerization in an atmosphere of an inert gas such as nitrogen gas. The polymerization pressure is not particularly limited as long as it is within a pressure range sufficient for maintaining the monomer and the solvent in a liquid phase within the above-mentioned polymerization temperature range.

[0081] Furthermore, at the end of the polymerization, a required amount of a coupling agent having two or more functional groups may be added to carry out a coupling reaction. The coupling agent having two or more functional groups is not particularly limited, and any known coupling agent can be used. Examples of bifunctional coupling agents include, but are not limited to, dihalogen compounds such as dimethyldichlorosilane and dimethyldibromosilane, acid esters such as methyl benzoate, ethyl benzoate, phenyl benzoate, and phthalates. Examples of polyfunctional coupling agents having three or more functional groups include, but are not limited to, 1,1,1,2,2-pentachloroethane, perchloroethane, pentachlorobenzene, perchlorobenzene, octabromodiphenyl ether, decabromodiphenyl ether, polyalcohols having three or more functional groups, epoxidized soybean oil, polyfunctional epoxy compounds such as diglycidyl bisphenol A, epoxy group-containing compounds having two to six functional groups, carboxylic acid esters, polyvinyl compounds such as divinylbenzene, and compounds represented by the formula R1. (4-n) Six n (wherein R1 is a hydrocarbon group having 1 to 20 carbon atoms, X is a halogen, and n is an integer of 3 or 4), and a halogenated tin compound. Examples of halogenated silicon compounds include, but are not limited to, methylsilyl trichloride, t-butylsilyl trichloride, silicon tetrachloride, and brominated versions of these compounds. Examples of the tin halide compound include, but are not limited to, polyvalent halogen compounds such as methyltin trichloride, t-butyltin trichloride, tin tetrachloride, etc. Dimethyl carbonate, diethyl carbonate, etc. can also be used.

[0082] The hydrogenated copolymers (A) and (B) may be obtained by subjecting the living terminals of the block copolymer obtained by the above-mentioned method to an addition reaction with a modifier that generates a functional group-containing atomic group. Examples of functional group-containing atomic groups include, but are not limited to, atomic groups containing at least one functional group selected from the group consisting of a hydroxyl group, a carbonyl group, a thiocarbonyl group, an acid halide group, an acid anhydride group, a carboxyl group, a thiocarboxyl acid group, an aldehyde group, a thioaldehyde group, a carboxylate group, an amide group, a sulfonic acid group, a sulfonate group, a phosphoric acid group, a phosphoric acid ester group, an amino group, an imino group, a nitrile group, a pyridyl group, a quinoline group, an epoxy group, a thioepoxy group, a sulfide group, an isocyanate group, an isothiocyanate group, a silicon halide group, a silanol group, an alkoxy silicon group, a tin halide group, an alkoxy tin group, and a phenyl tin group.

[0083] Examples of the modifying agent having the above-mentioned various functional group-containing atomic groups include, but are not limited to, tetraglycidyl meta-xylylene diamine, tetraglycidyl-1,3-bisaminomethylcyclohexane, ε-caprolactone, δ-valerolactone, 4-methoxybenzophenone, γ-glycidoxyethyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-glycidoxypropyl dimethylphenoxysilane, bis(γ-glycidoxypropyl)methylpropoxysilane, 1,3-dimethyl-2-imidazolidinone, 1,3-diethyl-2-imidazolidinone, N,N'-dimethylpropylene urea, and N-methylpyrrolidone. The amount of the modifying agent added is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, and further preferably 0.3 to 10 parts by mass, based on 100 parts by mass of the copolymer before modification. The temperature for the addition reaction of the modifying agent is preferably 0 to 150°C, more preferably 20 to 120°C. The time required for the modification reaction varies depending on the modification reaction conditions, but is preferably within 24 hours, and more preferably 0.1 to 10 hours.

[0084] The hydrogenated copolymers (A) and (B) constituting the hydrogenated copolymer (X) of the present embodiment are produced by carrying out a hydrogenation step after the above-mentioned polymerization step or after the above-mentioned modification step. The hydrogenation catalyst used for producing the hydrogenated copolymers (A) and (B) is not particularly limited, and for example, the hydrogenation catalysts described in JP-B-42-8704, JP-B-43-6636, JP-B-63-4841, JP-B-1-37970, JP-B-1-53851, JP-B-2-9041, etc. can be used. Preferred hydrogenation catalysts include titanocene compounds and / or mixtures with reducing organometallic compounds. Furthermore, in the case where only the vinyl bonds derived from the conjugated diene compound before hydrogenation are preferentially hydrogenated selectively, a titanocene compound is particularly preferred, and when the hydrogenation rate of the unsaturated double bonds derived from the conjugated diene compound is greater than the amount of vinyl bonds derived from the conjugated diene compound before hydrogenation, 90% or more of the vinyl bonds before hydrogenation can be selectively hydrogenated. The titanocene compound is not particularly limited, but examples thereof include compounds described in JP-A-8-109219, and specific examples thereof include compounds having at least one ligand having a (substituted) cyclopentadienyl structure, an indenyl structure, and a fluorenyl structure, such as biscyclopentadienyltitanium dichloride and monopentamethylcyclopentadienyltitanium trichloride. The reducing organometallic compound is not particularly limited, but examples thereof include organoalkali metal compounds such as organolithium compounds, organomagnesium compounds, organoaluminum compounds, organoboron compounds, and organozinc compounds. The reaction temperature for the hydrogenation reaction is usually from 0 to 200°C, and preferably from 30 to 150°C. The pressure of hydrogen used in the hydrogenation reaction is preferably 0.1 to 15 MPa, more preferably 0.2 to 10 MPa, and further preferably 0.3 to 5 MPa. The reaction time for the hydrogenation reaction is usually 3 minutes to 10 hours, and preferably 10 minutes to 5 hours. The hydrogenation reaction may be carried out by any of a batch process, a continuous process, or a combination thereof.

[0085] After the hydrogenation step, catalyst residues may be removed from the reaction solution, if necessary. Methods for separating the hydrogenated copolymer from the solvent include, but are not limited to, a method in which a polar solvent that is a poor solvent for the hydrogenated copolymer, such as acetone or alcohol, is added to a solution of the hydrogenated copolymer to precipitate and recover the hydrogenated copolymer; a method in which the solution of the hydrogenated copolymer is poured into hot water with stirring and the solvent is removed by steam stripping to recover the hydrogenated copolymer; and a method in which the solvent is distilled off by directly heating the solution of the hydrogenated copolymer.

[0086] The hydrogenated copolymer (X) of this embodiment may contain an antioxidant on the surface and / or inside thereof, for example, by adding the following antioxidant during the production. The following antioxidant may also be added to the pressure-sensitive adhesive composition of the present embodiment, which will be described later.

[0087] Examples of the antioxidant include, but are not limited to, phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, and amine-based antioxidants. Specifically, 2,6-di-t-butyl-4-methylphenol, n-octadecyl-3-(4'-hydroxy-3',5'-di-t-butyl-phenyl)propionate, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane], tris-(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, 4,4'-butylidene-bis-(3-methyl-6-t-butylphenol), 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methyl n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, pentaerythrityl-tetrakis[3 -(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 3,5-di-t-butyl-4-hydroxybenzylphosphonate-diethyl ester, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis(3,5-di-t-butyl-4 -Hydroxybenzylphosphonic acid ethyl) calcium and polyethylene wax (50%) mixture, octylated diphenylamine, 2,4-bis[(octylthio)methyl]-o-cresol, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, butyric acid, 3,3-bis(3-t-butyl-4-hydroxyphenyl)ethylene ester, 1,1,3-tris-(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl) isocyanurate, 2-t-butyl-6-(3'-t-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenyl-acrylate, and 2-[1-(2-hydroxy-3,5-di-t-pentylphenyl)-ethyl]-4,6-di-t-pentylphenyl acrylate.

[0088] (Method for Producing Hydrogenated Copolymer (X)) The method for producing the hydrogenated copolymer (X) is not particularly limited, but examples thereof include: (1) a method of polymerizing the hydrogenated copolymer (A) and the hydrogenated copolymer (B) and mixing them before recovering them from the production solvent; (2) a method of mixing the hydrogenated copolymer (A) and the hydrogenated copolymer (B) after removing the solvent and catalyst; (3) a method of adding a polymerization initiator in two stages during the polymerization reaction; (4) a method of adding a protic reagent such as alcohol as a modifier for the living terminal or a polymerization terminator during the polymerization reaction to terminate the reaction of some of the living terminals; (5) a method of adding a protic reagent such as alcohol as a modifier for the living terminals or a polymerization terminator after the polymerization reaction to terminate the reaction of all living terminals, and then adding a new polymerization initiator and monomer to the solution and carrying out polymerization; and (6) a method of adding a liquid hydrogenated copolymer (A) to the hydrogenated copolymer (B) during extrusion kneading. In the method (1), either of the following may be carried out: a method in which polymerization solutions of the hydrogenated copolymer (A) and the hydrogenated copolymer (B) before the hydrogenation reaction are mixed and then the hydrogenation reaction is carried out, or a method in which the hydrogenated copolymer (A) and the hydrogenated copolymer (B) are each hydrogenated and then the respective solutions are mixed. The mixing ratio of the hydrogenated copolymer (A) and the hydrogenated copolymer (B) can be controlled by adjusting the concentration of each polymerization solution and the mixing amount of the solutions. In the method (3), the mixing ratio of the hydrogenated copolymer (A) and the hydrogenated copolymer (B) can be arbitrarily controlled by adjusting the feed rates of the vinyl aromatic compound and the conjugated diene compound, the amount of the polymerization initiator added in two stages, the timing of the second stage addition of the polymerization initiator, etc. In the above-mentioned method (4), the mixing ratio of the hydrogenated copolymer (A) and the hydrogenated copolymer (B) can be arbitrarily controlled by adjusting the feed rates of the vinyl aromatic compound and the conjugated diene compound, the amount of the modifier or the polymerization terminator added during the process, the timing of the addition, etc. The hydrogenated copolymer (A) has a low molecular weight and is less entangled in molecules, so that mixing it before desolvation as in the above methods (1), (3), (4) and (5) enables the desolvation and finishing steps to be carried out at a high rate. The above methods (3), (4) and (5) can simultaneously produce the hydrogenated copolymer (A) and the hydrogenated copolymer (B). Compared with the case where the hydrogenated copolymer (A) and the hydrogenated copolymer (B) are produced separately, the number of production steps can be reduced, and therefore the production efficiency can be improved. From the viewpoints of production efficiency and stability of performance, the above method (3) is preferred.

[0089] The polymerization terminator is not particularly limited, but examples thereof include water, alcohols such as methanol, ethanol, isopropanol, 2-ethylhexanol, heptanol, and mixtures thereof.

[0090] In the method (3) for producing the hydrogenated copolymer (X) of the present embodiment, the hydrogenated copolymer (A) and the hydrogenated copolymer (B) may be produced simultaneously in one reactor. In such a production process, it is preferable to add the raw material monomers of each polymer block and a polymerization initiator in the following order (c) or (d), and then hydrogenate them. (c) First polymerization initiator, d, e, d, second polymerization initiator, a, b (E) First polymerization initiator, d, e, d, second polymerization initiator, a, c In the above (c) and (d), a and d are polymer blocks mainly composed of vinyl aromatic monomer units, b and e are random copolymer blocks composed of vinyl aromatic monomer units and conjugated diene monomer units, and c is a polymer block mainly composed of conjugated diene monomer units, and raw material monomers for each polymer block are added in the production process. In the above (c) and (d), the addition of each monomer of the first polymerization initiator → d → e → d causes polymerization of ded in the hydrogenated copolymer (B), and then the addition of each monomer of the second polymerization initiator → a → b or c causes the hydrogenated copolymer (B) to be polymerized into ab or a after ded. -b or ac is polymerized. The hydrogenated copolymer (A) becomes ab or ac.

[0091] The hydrogenated copolymer (X) of the present embodiment may be pelletized. Examples of the pelletizing method include a method in which the hydrogenated copolymer (X) is extruded in the form of a strand from a single-screw or twin-screw extruder, and then cut in water with a rotary blade installed in front of a die section; a method in which the hydrogenated copolymer is extruded in the form of a strand from a single-screw or twin-screw extruder, and then cooled with water or air, and then cut with a strand cutter; a method in which the copolymer is melt-mixed using an open roll or Banbury mixer, then formed into a sheet using a roll, and then the sheet is cut into strips, and then cut into cubic pellets using a pelletizer. The size and shape of the pellets of the hydrogenated copolymer (X) are not particularly limited. If necessary, a pellet anti-blocking agent may be blended with the pellets of the hydrogenated copolymer (X) for the purpose of preventing pellet blocking. Examples of pellet blocking inhibitors include, but are not limited to, calcium stearate, magnesium stearate, zinc stearate, polyethylene, polypropylene, ethylene bisstearylamide, talc, and amorphous silica. The amount of the pellet antiblocking agent to be added is preferably 500 to 6000 ppm, more preferably 1000 to 5000 ppm, based on the hydrogenated copolymer (X). The pellet antiblocking agent is preferably added in a state of adhering to the pellet surface, but may also be contained to some extent inside the pellet.

[0092] [Adhesive composition] The adhesive composition of the present embodiment contains the hydrogenated copolymer (X) of the present embodiment described above. Constituent materials of the adhesive composition include, in addition to the hydrogenated copolymer (X) of the present embodiment, hydrogenated copolymers other than the hydrogenated copolymer (X), other elastomers, various additives described later, tackifiers, etc. The adhesive composition of the present embodiment can be produced by the method described below.

[0093] The hydrogenated copolymer (X) and the adhesive composition of the present embodiment may contain any additives as necessary. There are no particular limitations on the additives, so long as they are generally compounded with thermoplastic resins or rubber-like polymers, and examples include those described in "Rubber and Plastic Compounding Chemicals" (compiled by Nippon Rubber Digest Co., Ltd.). Specifically, reinforcing fillers, inorganic fillers such as calcium sulfate and barium sulfate; pigments such as carbon black and iron oxide; lubricants such as stearic acid, behenic acid, zinc stearate, calcium stearate, magnesium stearate, and ethylene bisstearamide; antiblocking agents such as stearic acid amide, erucic acid amide, oleic acid amide, stearic acid monoglyceride, stearyl alcohol, petroleum waxes (e.g., microcrystalline wax), and low molecular weight vinyl aromatic resins; release agents; plasticizers such as organic polysiloxanes and mineral oils; antioxidants such as hindered phenol antioxidants and phosphorus-based heat stabilizers; hindered amine light stabilizers and benzotriazole-based ultraviolet absorbers; flame retardants; antistatic agents; reinforcing agents such as organic fibers, glass fibers, carbon fibers, and metal whiskers; colorants; and mixtures thereof.

[0094] [Adhesive film] The pressure-sensitive adhesive film of the present embodiment includes a base layer and a pressure-sensitive adhesive layer provided on the base layer and made of the pressure-sensitive adhesive composition of the present embodiment.

[0095] The adhesive layer of the adhesive film of the present embodiment may contain a tackifier, if necessary. The tackifier is not particularly limited as long as it is a resin that can impart viscosity to the adhesive layer, and examples thereof include known tackifier resins such as hydrogenated terpene resins, rosin-based terpene resins, hydrogenated rosin terpene resins, aromatic modified hydrogenated terpene resins, coumarone resins, phenolic resins, terpene phenolic resins, hydrogenated terpene phenolic resins, aromatic hydrocarbon resins, and aliphatic hydrocarbon resins. Particularly preferred are hydrogenated terpene resins, aromatic modified hydrogenated terpene resins, hydrogenated terpene phenol resins, and terpene phenol resins. The tackifier may be used alone or in combination of two or more kinds. Examples of tackifiers that can be used include those listed in "Rubber and Plastic Compounding Chemicals" (Rubber Digest Co., Ltd.). By using a tackifier, the adhesive strength can be improved. The content of the tackifier in the adhesive layer is preferably 0 to 50% by mass, and in order to effectively prevent increased adhesion and further reduce the amount of adhesive residue upon peeling, the content is more preferably 0 to 20% by mass, and even more preferably 0 to 10% by mass. In particular, it is most preferable that the composition does not contain a tackifier from the viewpoint of preventing contamination of the molding equipment and peripheral equipment when producing a molded article of the adhesive composition. In addition, in order to obtain a moderately low adhesion enhancement property, a moderately low adhesive residue property, and a stronger adhesive strength, the content is more preferably 5 to 50 mass%, and even more preferably 10 to 30 mass%.

[0096] The tackifier component and the content in the adhesive layer of the adhesive composition and adhesive film of this embodiment are generally determined by NMR or GPC, but since the adhesive composition containing no tackifier does not contain such a component because the tackifier is a component that is easily volatilized by heat, the weight loss after 200°C x 30 minutes by TG-DTA (thermogravimetric differential thermal analysis) is 0.4% (wt%) or less. The weight loss is preferably 0.35% or less, more preferably 0.3% or less. The hydrogenated copolymer (X) of the present embodiment has the same characteristics, and when the hydrogenated copolymer (X) of the present embodiment does not contain a tackifier, the weight loss after 30 minutes at 200°C measured by TG-DTA (thermogravimetric differential thermal analysis) is 0.4% or less. The weight loss is preferably 0.35% or less, and more preferably 0.3% or less.

[0097] (base material layer) The material for the base layer is not particularly limited, and either a non-polar resin or a polar resin can be used. In terms of performance, cost, etc., preferred examples of non-polar resins include polyethylene and homo- or block polypropylene, while preferred examples of polar resins include polyester-based resins such as polyethylene terephthalate and polybutylene terephthalate, polyamide-based resins, ethylene-vinyl acetate copolymers, and hydrolysates thereof.

[0098] The thickness of the substrate layer is preferably 1 mm or less, more preferably 300 μm or less, and further preferably 10 to 200 μm. When the thickness of the base layer is 10 μm or more, the adherend can be adequately protected, and when the thickness of the base layer is 1 mm or less, a practically good elastic modulus is obtained, good conformability to unevenness is obtained, and lifting and peeling can be effectively prevented.

[0099] (Adhesive layer) The adhesive layer contains the hydrogenated copolymer (X) of this embodiment. The adhesive layer may contain a hydrogenated copolymer other than the hydrogenated copolymer (X) of this embodiment. The thickness of the adhesive layer is preferably from 1 to 100 μm, more preferably from 2 to 50 μm, and even more preferably from 5 to 25 μm. When the thickness of the adhesive layer is 1 μm or more, it can adhere sufficiently to the adherend, and when the thickness of the adhesive layer is 100 μmm or less, a film with little thickness unevenness is obtained, excessive adhesion is effectively prevented, and a good film with little glue residue when peeled off is obtained.

[0100] (Method for manufacturing resin material constituting adhesive layer of adhesive film) The adhesive composition constituting the adhesive layer of the adhesive film of this embodiment can be produced, for example, by a method of dry blending the hydrogenated copolymer (X) and other components added as necessary, or a method of preparing the composition using an apparatus typically used for mixing polymeric substances. The mixing device is not particularly limited, but examples thereof include kneading devices such as a Banbury mixer, a Labo Plastomill, a single-screw extruder, and a twin-screw extruder. From the viewpoints of productivity and good kneading properties, production by a melt mixing method using an extruder is preferred. In particular, when a tackifier is blended into the material constituting the adhesive layer, the above-mentioned dry blending method may be used. However, since the tackifier is very sticky and in a flake form and therefore difficult to handle, a master batch may be prepared in which the tackifier is pre-kneaded into the above-mentioned hydrogenated copolymer (X). The melting temperature during kneading of the material constituting the adhesive layer can be appropriately set, but is usually in the range of 130 to 300°C, and preferably in the range of 150 to 250°C. The adhesive layer containing the hydrogenated copolymer (X) of this embodiment contains the low molecular weight hydrogenated copolymer (A), and can effectively achieve high adhesion even when no tackifier is contained or when the amount of tackifier is small, so that when no tackifier is contained, all the steps required when the tackifier is contained are not required. Also, when the amount of tackifier is small, the adhesive film can be produced by simply dry blending during the production of the adhesive film, which has the advantage of simplifying the production process and reducing costs.

[0101] The resin material constituting the adhesive layer constituting the adhesive film of this embodiment may be subjected to a foaming treatment in order to achieve the effects of reducing weight, improving flexibility, and improving adhesion. The foaming method is not limited to the following, but includes, for example, a chemical method, a physical method, and the use of thermally expandable microballoons. Bubbles can be distributed inside the material by adding a chemical foaming agent such as an inorganic foaming agent or an organic foaming agent, a physical foaming agent, or a thermally expandable microballoon. In addition, hollow fillers (already expanded balloons) may be added to reduce weight, improve flexibility, and improve adhesion.

[0102] (Method of manufacturing adhesive film) The adhesive film of the present embodiment comprises an adhesive layer containing the hydrogenated copolymer (X) on a base layer. The method for producing the adhesive film of this embodiment is not particularly limited, but examples include a method in which a solution or melt of the adhesive composition constituting the adhesive layer is applied onto a specified film constituting the base layer, and a method in which the base layer and the adhesive layer are laminated using a film extruder. Here, when a solution or melt of the adhesive composition constituting the adhesive layer is used, the adhesive composition may be prepared and then converted into a solution or melt, or a predetermined material may be mixed with a solution or melt of the hydrogenated copolymer (X) to obtain the adhesive composition.

[0103] Methods for applying a solution of the adhesive composition that constitutes the adhesive layer include, but are not limited to, a method in which a resin material is dissolved in a solvent in which it can be dissolved, and the solution is applied onto a film that constitutes the base layer using a coater or the like, and the solvent is then heated and dried.

[0104] The method of melting and applying the adhesive composition constituting the adhesive layer is not limited to the following, but includes, for example, a method of applying the molten adhesive composition onto a film constituting the base layer using a hot melt coater, etc. In this case, it is preferable to use various films having a glass transition temperature, melting point, or softening point higher than the application temperature as the base layer.

[0105] Methods for obtaining an adhesive film using a film extruder include, but are not limited to, a method in which an adhesive layer component consisting of an adhesive composition and a component such as a thermoplastic resin that can constitute a base layer are made into two streams in a melt co-extruder, i.e., the fluid for forming the adhesive layer and the fluid for forming the base layer are merged in a die opening to form a single fluid, which is then extruded to combine the adhesive layer and the base layer.

[0106] In the case of the method of obtaining an adhesive film by a film extruder, the resin material forming the adhesive layer can be produced by previously dry blending each component for the adhesive layer, so that this method is excellent in productivity. In addition, when the adhesive film is extruded by a film extruder, the adhesiveness and adhesive strength of the produced adhesive film tend to be particularly excellent.

[0107] The adhesive film of this embodiment can be temporarily attached to the surfaces of optical system molded bodies such as light guide plates and prism sheets, synthetic resin plates, metal plates, decorative plywood, coated steel plates, various nameplates, and the like, and can be used as a protective film to prevent scratches and dirt on these adherends during processing, transportation, and storage.

[0108] [Uses of hydrogenated copolymer (X), adhesive composition, and molded article] The hydrogenated copolymer (X) or adhesive composition of this embodiment can be used for various applications by blending various additives as necessary. Applications of the hydrogenated copolymer (X) of this embodiment, the pressure-sensitive adhesive composition, and molded articles thereof include, for example, building materials, vibration-damping and soundproofing materials, wire covering materials, high-frequency adhesive compositions, slush molding materials, adhesive compositions, asphalt compositions, automobile interior materials, automobile exterior materials, medical device materials, various containers such as food packaging containers, home electric appliances, industrial parts, toys, etc. EXAMPLES

[0109] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples. First, the evaluation methods and the methods for measuring physical properties applied to the examples and comparative examples are described below.

[0110] [Method of identifying the structures of hydrogenated copolymer (A) and hydrogenated copolymer (B) and method of measuring physical properties] ((1) Number average molecular weight (Mn) of hydrogenated copolymer (A) and hydrogenated copolymer (B) The number average molecular weight of the hydrogenated copolymer was measured using GPC (apparatus: Tosoh HLC8220, column TSKgel SuperH-RC x 2). Tetrahydrofuran was used as the solvent. The measurement was performed at a temperature of 35°C. The polystyrene-equivalent number average molecular weight was determined using a calibration curve prepared using commercially available standard polystyrenes with known number average molecular weights. Here, the number average molecular weight of the hydrogenated copolymer (A) is designated as (Mn1), and the number average molecular weight of the hydrogenated copolymer (B) is designated as (Mn2).

[0111] ((2) Contents of hydrogenated copolymer (A) and hydrogenated copolymer (B) in hydrogenated copolymer (X) The contents of hydrogenated copolymer (A) and hydrogenated copolymer (B) in hydrogenated copolymer (X) were measured using GPC (apparatus: Tosoh HLC8220, column TSKgel SuperH-RC x 2). The solvent used was tetrahydrofuran. The measurement was performed at a temperature of 35°C. The contents of hydrogenated copolymer (A) and hydrogenated copolymer (B) in hydrogenated copolymer (X) were calculated from the area ratio of the peaks derived from hydrogenated copolymer (A) and hydrogenated copolymer (B). The content of hydrogenated copolymer (B) was defined as the content of 100-hydrogenated copolymer (A).

[0112] ((3) Separation of hydrogenated copolymer (A) and hydrogenated copolymer (B) Using GPC [instrument: Waters ACQUITY UPLC H-Class, columns: Waters ACQUITY APC XT900 (2.5 μm, 4.6 × 150 mm), Waters ACQUITY APC XT200 (2.5 μm, 4.6 × 75 mm), Waters ACQUITY APC XT125 (2.5 mm, 4.6 × 75 mm) in series], the low molecular weight component, hydrogenated copolymer (A), and the high molecular weight component, hydrogenated copolymer (B), were separated. The solvent used was chloroform. The hydrogenated copolymer (A) was defined as all components having a number average molecular weight of 35,000 or less, and the hydrogenated copolymer (B) was defined as all components having a number average molecular weight of 130,000 or more, which were separated.

[0113] ((4) The total vinyl aromatic monomer unit content (TS), the vinyl aromatic monomer unit content (RS) in the random copolymer block, and the content of the polymer block mainly composed of vinyl aromatic monomer units (BS) in the hydrogenated copolymer (A) and the hydrogenated copolymer (B) The definition is as follows: BS1: Content of polymer blocks mainly composed of vinyl aromatic monomer units in hydrogenated copolymer (A) BS2: Content of polymer blocks mainly composed of vinyl aromatic monomer units in hydrogenated copolymer (B) RS1: Content of vinyl aromatic monomer units in the random copolymer block of hydrogenated copolymer (A) RS2: Content of vinyl aromatic monomer units in the random copolymer block of hydrogenated copolymer (B) TS1: Content of vinyl aromatic monomer units in hydrogenated copolymer (A) TS2: Content of vinyl aromatic monomer units in hydrogenated copolymer (B)

[0114] Hydrogenated copolymer (A) and hydrogenated copolymer (B) were used as the measurement samples. 1Using H-NMR (Joel Resonance Corporation ECS400), the vinyl aromatic monomer units contained in each were classified into those derived from the "polymer block mainly composed of vinyl aromatic compounds" and those derived from the "random copolymer block composed of vinyl aromatic monomer units and conjugated diene monomer units." Deuterated chloroform was used as the solvent, the sample concentration was 50 mg / mL, the observation frequency was 400 MHz, tetramethylsilane was used as the chemical shift standard, the pulse delay was 2.904 seconds, the number of scans was 256, and the measurement temperature was 23°C. The styrene contents of the random and block types were calculated from the integrated intensity of the signals assigned to aromatics and the integrated value per 1H of each bond type, and then the total styrene contents (TS1) (TS2) were calculated, and the styrene contents in the random copolymer blocks (hereinafter sometimes referred to as random styrene amounts) (RS1) (RS2) and the contents of polymer blocks mainly composed of vinyl aromatic monomer units in the hydrogenated copolymers (hereinafter sometimes referred to as styrene blocks) (BS1) (BS2) were calculated. The calculation method is as follows: Styrene block strength (b-St strength) = (integrated value of 6.9 ppm to 6.3 ppm) / 2 Random styrene strength (r-St strength) = (integrated value of 7.5 ppm to 6.9 ppm) - 3 × (b-St) Ethylene-butylene strength (EB strength) = Total integrated value - 3 x {(b-St intensity) + (r-St intensity)} / 8 Styrene block content (BS) =104×(b-St strength) / [104×{(b-St strength)+(r-St strength)}+56×(EB strength)] Styrene content in random copolymer block (RS) =104×(r-St strength) / {104×(r-St strength)+56×(EB strength)}

[0115] ((5) Hydrogenation ratio (H) of double bonds of hydrogenated copolymer (A) and hydrogenated copolymer (B) The hydrogenation rate of the hydrogenated copolymer was measured by a nuclear magnetic resonance spectrometer (BRUKER, DPX-400). The hydrogenated copolymer was used to perform proton nuclear magnetic resonance ( 1 H-NMR (H-NMR) measurements. Specifically, the integral values ​​of the signals at 4.5 to 5.5 ppm derived from the residual double bonds and the signals attributable to the hydrogenated conjugated dienes were calculated, and the ratio thereof was calculated.

[0116] ((6) Branching Degree (f) of Hydrogenated Copolymer (B) The branching degree (f) of the hydrogenated copolymer (B) was measured by a GPC-light scattering method equipped with a viscosity detector. Hydrogenated copolymer (B) was used as a sample and was measured using GPC (Malvern, GPCmax VE-2001, columns: Tosoh, "TSKgel G4000HXL", "TSKgel G5000HXL", "TSKgel G6000HXL") with three detectors connected in that order: a light scattering detector, an RI detector, and a viscosity detector (Malvern's product name "TDA305"). Based on standard polystyrene, the absolute molecular weight (M) was calculated from the results of the light scattering detector and the RI detector, and the intrinsic viscosity ([η]) was calculated from the results of the RI detector and the viscosity detector. Next, the reference intrinsic viscosity ([η]0) was calculated using the following formula. [η]0=a×M b a = -0.788 + 0.421 × (vinyl aromatic compound content of hydrogenated copolymer (B)) -0.342×(RS2)-0.197×(BS2) b = 1.601 - 0.081 x (vinyl aromatic compound content of hydrogenated copolymer (B)) +0.064×(RS2)+0.039×(BS2) RS2: Content of vinyl aromatic monomer units in the random copolymer block of hydrogenated copolymer (B) BS2: Proton nuclear magnetic resonance ( 1The content of the polymer block mainly composed of vinyl aromatic monomer units in the hydrogenated copolymer (B) determined by H-NMR M: Absolute molecular weight of hydrogenated copolymer (B) Subsequently, the shrinkage factor g was calculated as the ratio of the intrinsic viscosity ([η]) of the hydrogenated copolymer (B) to the reference intrinsic viscosity ([η]0). Shrinkage factor (g)=[η] / [η]0 The obtained shrinkage factor (g) was then used to calculate the branching degree (f), defined as g = f / [(f + 1)(f + 2)] (f ≥ 2). The solvent used was tetrahydrofuran (hereinafter also referred to as "THF") containing 5 mmol / L triethylamine. 100 μL of the measurement solution was injected into a GPC measurement device, and the measurement was performed under conditions of an oven temperature of 40° C. and a THF flow rate of 1 mL / min.

[0117] ((7) Calculation of the molecular weight (MnS) of the styrene block of hydrogenated copolymer (A) and hydrogenated copolymer (B) Using the (Mn1), (Mn2), (BS1), (BS2), and (f) measured in (1), (2), and (5), the styrene block molecular weights (MnS1) and (MnS2) of the hydrogenated copolymer (A) and the hydrogenated copolymer (B) were calculated according to the following calculation formula. The calculation results were rounded off to the nearest tenth, and any figures below 500 were set to 0. MnS1 = Mn1 × BS1 MnS2 = Mn2 × BS2 ÷ f

[0118] (Vinyl bond amounts (Va) and (Vb) of hydrogenated copolymer (A) and hydrogenated copolymer (B)) Hydrogenated copolymer (A) and hydrogenated copolymer (B) were used as the measurement samples. 1The amount of vinyl bonds (1,2-bonds) contained in each sample was measured by H-NMR (Joel Resonabce ECS400). Deuterated chloroform was used as the solvent, the sample concentration was 50 mg / mL, the observation frequency was 400 MHz, tetramethylsilane was used as the chemical shift standard, the pulse delay was 2.904 seconds, the number of scans was 256, and the measurement temperature was 23°C. The amount of vinyl bonds was calculated from the ratio of 1,2-bonds to the total of 1,4-bonds and 1,2-bonds after calculating the integral value per 1H of each bond type from the integral value of the signals assigned to 1,4-bonds and 1,2-bonds.

[0119] [Production of hydrogenated copolymer] (Preparation of hydrogenation catalyst) The hydrogenation catalyst used in the hydrogenation reaction of the copolymer was prepared by the following method. A nitrogen-purged reaction vessel was charged with 1 liter of dried and purified cyclohexane, and 100 mmol of bis(cyclopentadienyl)titanium dichloride was added. With sufficient stirring, an n-hexane solution containing 200 mmol of trimethylaluminum was added, and the reaction was carried out at room temperature for approximately 3 days to obtain a hydrogenation catalyst.

[0120] (Hydrogenated copolymer) <Production example 1: Hydrogenated copolymer (X1)> In the case of the hydrogenated copolymer (X1), first, the copolymer (A1) and the copolymer (B1) were subjected to batch polymerization using one reactor, and then a hydrogenation reaction was carried out to obtain the hydrogenated copolymer (A1) and the hydrogenated copolymer (B1). Batch polymerization was carried out using a tank-type reactor (internal volume: 30 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 4.8 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.036 parts by mass of first-stage n-butyllithium (hereinafter also referred to as "NBL1") per 100 parts by mass of the total monomers, 1.50 mol of first-stage N,N,N',N'-tetramethylethylenediamine (hereinafter also referred to as "TMEDA1") per 1 mol of NBL1, and 0.04 mol of sodium t-pentoxide (hereinafter referred to as NaOAm) per 1 mol of first-stage NBL1 were added, and polymerization was carried out at 60°C for 15 minutes. Next, a cyclohexane solution containing 9.8 parts by mass of styrene (concentration 20% by mass) and a cyclohexane solution containing 39.3 parts by mass of butadiene (concentration 20% by mass) were added and polymerization was carried out at 50° C. for 40 minutes. Next, a cyclohexane solution containing 3.8 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.439 parts by mass of n-butyllithium (hereinafter also referred to as "NBL2") for the second stage was added relative to 100 parts by mass of the total monomers, and 0.80 moles of N,N,N',N'-tetramethylethylenediamine (hereinafter also referred to as "TMEDA2") for the second stage was added relative to 1 mole of NBL2, and then a cyclohexane solution (concentration 20% by mass) containing 8.5 parts by mass of styrene was added and polymerization was carried out at 50°C for 15 minutes. Next, a cyclohexane solution containing 3.4 parts by mass of styrene (concentration 20% by mass) and a cyclohexane solution containing 30.5 parts by mass of butadiene (concentration 20% by mass) were added and polymerized at 50° C. for 30 minutes. Then, ethanol was added to terminate the polymerization reaction. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A1)) and a high molecular weight component (hydrogenated copolymer (B1)) by GPC, and each was analyzed. The hydrogenated copolymer (A1) had a total styrene content (TS1) of 28.0 mass%, a styrene block content (BS1) of 20.0 mass%, a random styrene content (RS1) of 10.0 mass%, a number average molecular weight (Mn1) of 9,000, a styrene block molecular weight (MnS1) of 1,800, a vinyl bond content (Va) of 66 mass%, and a hydrogenation rate (Ha) of 100%. In addition, the hydrogenated copolymer (B1) had a total styrene content (TS2) of 31.7 mass%, a styrene block content (BS2) of 15.0 mass%, a random styrene content (RS2) of 19.6 mass%, a number average molecular weight (Mn2) of 224,000, a styrene block molecular weight (MnS2) of 16,800, a vinyl bond content (Vb) of 67 mass%, and a hydrogenation rate (Hb) of 100%. The content ratio of the hydrogenated copolymer (A1) to the hydrogenated copolymer (B1) was (A1) / (B1)=40 / 60. The resulting hydrogenated copolymer (A) had a block structure of ab, and the resulting hydrogenated copolymer (B) had a block structure of dedab. Next, 0.2 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer relative to 100 parts by mass of the hydrogenated copolymer to obtain a hydrogenated copolymer (X1). The analytical results of the obtained hydrogenated copolymer (X1) are shown in Table 1. In addition, a and d are polymer blocks mainly composed of vinyl aromatic monomer units, b and e are random copolymer blocks composed of vinyl aromatic monomer units and conjugated diene monomer units, and c is a polymer block mainly composed of conjugated diene monomer units. The same applies hereinafter.

[0121] <Production example 2: Hydrogenated copolymer (X2)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 4.8 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.036 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.30 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.04 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 9.9 parts by mass of styrene (concentration: 20% by mass) and 39.6 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 3.8 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.539 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.60 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 8.4 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 6.7 parts by mass of styrene (concentration: 20% by mass) and 26.8 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A2)) and a high molecular weight component (hydrogenated copolymer (B2)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X2) are shown in Table 1. Moreover, (RS1) of the hydrogenated copolymer (A2) was 20.0% by mass, and (RS2) of the hydrogenated copolymer (B2) was 20.0% by mass.

[0122] <Production example 3: Hydrogenated copolymer (X3)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 4.8 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.036 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.50 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.04 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 9.9 parts by mass of styrene (concentration: 20% by mass) and 39.6 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 3.8 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.539 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.70 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 8.4 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 6.7 parts by mass of styrene (concentration: 20% by mass) and 26.8 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A3)) and a high molecular weight component (hydrogenated copolymer (B3)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X3) are shown in Table 1. Moreover, (RS1) of the hydrogenated copolymer (A3) was 20.0 mass %, and (RS2) of the hydrogenated copolymer (B3) was 20.0 mass %.

[0123] <Production example 4: Hydrogenated copolymer (X4)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 4.8 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.036 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.50 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.08 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 9.9 parts by mass of styrene (concentration: 20% by mass) and 39.6 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 3.8 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.539 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 1.00 mole of TMEDA2 for the second stage per mole of NBL2 were added, and then 8.4 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 6.7 parts by mass of styrene (concentration: 20% by mass) and 26.8 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A4)) and a high molecular weight component (hydrogenated copolymer (B4)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X4) are shown in Table 1. Moreover, (RS1) of the hydrogenated copolymer (A4) was 20.0 mass %, and (RS2) of the hydrogenated copolymer (B4) was 20.0 mass %.

[0124] <Production Example 5: Hydrogenated copolymer (X5)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 5.6 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.0345 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.40 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.05 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 5.8 parts by mass of styrene (concentration: 20% by mass) and 52.0 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 4.5 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.498 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.60 moles of TMEDA2 for the second stage per mole of NBL2 were added, and then 6.4 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 2.6 parts by mass of styrene (concentration: 20% by mass) and 23.1 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A5)) and a high molecular weight component (hydrogenated copolymer (5)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X5) are shown in Table 1. Moreover, (RS1) of the hydrogenated copolymer (A5) was 10.0% by mass, and (RS2) of the hydrogenated copolymer (B5) was 10.0% by mass.

[0125] <Production Example 6: Hydrogenated copolymer (X6)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 4.8 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.034 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.80 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.06 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 9.8 parts by mass of styrene (concentration: 20% by mass) and 39.1 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 3.7 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.371 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 1.10 moles of TMEDA2 for the second stage per mole of NBL2 were added, and then 8.5 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 34.1 parts by mass of butadiene (concentration: 20% by mass) was added, and polymerization was carried out at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A6)) and a high molecular weight component (hydrogenated copolymer (B6)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X6) are shown in Table 1. Moreover, (RS1) of the hydrogenated copolymer (A6) was 0 mass %, and (RS2) of the hydrogenated copolymer (B6) was 19.2 mass %.

[0126] <Production Example 7: Hydrogenated copolymer (X7)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 7.4 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.036 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 0.80 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 11.0 parts by mass of styrene (concentration: 20% by mass) and 44.1 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 6.3 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.691 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.30 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 8.4 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 3.4 parts by mass of styrene (concentration: 20% by mass) and 19.3 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A7)) and a high molecular weight component (hydrogenated copolymer (B7)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X7) are shown in Table 1. Moreover, (RS1) of the hydrogenated copolymer (A7) was 15.0 mass %, and (RS2) of the hydrogenated copolymer (B7) was 19.9 mass %.

[0127] <Production Example 8: Hydrogenated copolymer (X8)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 4.8 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.038 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.40 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.04 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 9.6 parts by mass of styrene (concentration: 20% by mass) and 38.2 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 3.4 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.287 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.90 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 8.8 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 3.5 parts by mass of styrene (concentration: 20% by mass) and 31.7 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A8)) and a high molecular weight component (hydrogenated copolymer (B8)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X8) are shown in Table 1. Moreover, (RS1) of the hydrogenated copolymer (A8) was 10.0 mass %, and (RS2) of the hydrogenated copolymer (B8) was 19.4 mass %.

[0128] <Production Example 9: Hydrogenated copolymer (X9)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 4.1 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.029 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.70 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.06 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 8.0 parts by mass of styrene (concentration: 20% by mass) and 32.0 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 2.9 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.191 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 1.20 moles of TMEDA2 for the second stage per mole of NBL2 were added, and then 7.9 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 4.5 parts by mass of styrene (concentration: 20% by mass) and 40.5 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A9)) and a high molecular weight component (hydrogenated copolymer (B9)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X9) are shown in Table 1. Moreover, (RS1) of the hydrogenated copolymer (A9) was 10.0% by mass, and (RS2) of the hydrogenated copolymer (B9) was 19.1% by mass.

[0129] <Production Example 10: Hydrogenated copolymer (X10)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 8.5 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.060 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.30 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.04 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 12.4 parts by mass of styrene (concentration: 20% by mass) and 49.5 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 7.0 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.371 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.60 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 4.5 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 3.6 parts by mass of styrene (concentration: 20% by mass) and 14.5 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A10)) and a high molecular weight component (hydrogenated copolymer (B10)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X10) are shown in Table 1. Moreover, (RS1) of the hydrogenated copolymer (A10) was 20.0 mass %, and (RS2) of the hydrogenated copolymer (B10) was 20.0 mass %.

[0130] <Production Example 11: Hydrogenated copolymer (X11)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 6.3 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.040 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 2.00 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.08 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 5.3 parts by mass of styrene (concentration: 20% by mass) and 48.0 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 4.9 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.172 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 2.00 moles of TMEDA2 for the second stage per mole of NBL2 were added, and then 4.6 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 30.8 parts by mass of butadiene (concentration: 20% by mass) was added, and polymerization was carried out at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A11)) and a high molecular weight component (hydrogenated copolymer (B11)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X11) are shown in Table 1. Moreover, (RS1) of the hydrogenated copolymer (A11) was 0 mass %, and (RS2) of the hydrogenated copolymer (B11) was 9.2 mass %.

[0131] <Production Example 12: Hydrogenated copolymer (X12)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 4.4 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.042 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.40 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.04 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 5.9 parts by mass of styrene (concentration: 20% by mass) and 67.3 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 3.5 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.284 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.90 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 3.8 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 1.5 parts by mass of styrene (concentration: 20% by mass) and 13.6 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A12)) and a high molecular weight component (hydrogenated copolymer (B12)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X12) are shown in Table 1. Moreover, (RS1) of the hydrogenated copolymer (A12) was 10.0% by mass, and (RS2) of the hydrogenated copolymer (B12) was 8.0% by mass.

[0132] <Production Example 13: Hydrogenated copolymer (X13)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timings of addition of the monomers and additives in the polymerization step were adjusted as shown below. 8.6 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.038 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 0.80 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.04 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 6.0 parts by mass of styrene (concentration: 20% by mass) and 33.7 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 6.6 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.219 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.50 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 9.0 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 5.4 parts by mass of styrene (concentration: 20% by mass) and 230.7 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped, and the amount of hydrogen was adjusted to carry out the hydrogenation reaction partway. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A13)) and a high molecular weight component (hydrogenated copolymer (B13)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X13) are shown in Table 1. Moreover, (RS1) of the hydrogenated copolymer (A13) was 15.0% by mass, and (RS2) of the hydrogenated copolymer (B13) was 15.0% by mass.

[0133] <Production Example 14: Hydrogenated copolymer (X14)> In the case of the hydrogenated copolymer (X14), the copolymer (A14) and the copolymer (B14) were each subjected to batch polymerization in separate reactors, and then each polymerization reaction was terminated. The copolymer (A14) and the copolymer (B14) were solution-blended, and then hydrogenated. [Polymerization of copolymer (A14)] Batch polymerization was carried out using a tank-type reactor (internal volume: 30 L) equipped with a stirrer and a jacket. 20.0 parts by mass of styrene (concentration: 20% by mass) was added. Next, 1.339 parts by mass of NBL per 100 parts by mass of the total monomers, 0.80 mol of TMEDA per 1 mol of NBL, and 0.005 mol of NaOAm per 1 mol of NBL were added, and polymerization was carried out at 50° C. for 15 minutes. Next, 16.0 parts by mass of styrene (concentration: 20% by mass) and 64.0 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped to obtain a copolymer (A14). [Polymerization of copolymer (B14)] Batch polymerization was carried out using a tank-type reactor (internal volume: 30 L) equipped with a stirrer and a jacket. 8.0 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.050 part by mass of NBL per 100 parts by mass of the total monomers, 1.50 mol of TMEDA per 1 mol of NBL, and 0.042 mol of NaOAm per 1 mol of NBL were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 16.5 parts by mass of styrene (concentration: 20% by mass) and 66.1 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 50 minutes. Next, 7.0 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 2.4 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out at 50° C. for 20 minutes. Thereafter, the polymerization reaction was stopped to obtain a copolymer (B14). Furthermore, 40.0 parts by mass (concentration 20% by mass) of the obtained copolymer (A14) and 60.0 parts by mass (concentration 20% by mass) of the copolymer (B14) were blended in a solution, and the hydrogenation catalyst prepared as described above was added in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A14)) and a high molecular weight component (hydrogenated copolymer (B14)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X14) are shown in Table 1. Moreover, (RS1) of the hydrogenated copolymer (A14) was 20.0 mass %, and (RS2) of the hydrogenated copolymer (B14) was 19.4 mass %.

[0134] <Production Example 15: Hydrogenated copolymer (X15)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 4.8 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.039 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.00 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.02 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 8.2 parts by mass of styrene (concentration: 20% by mass) and 32.8 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 1.7 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.097 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.60 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 10.5 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 8.4 parts by mass of styrene (concentration: 20% by mass) and 33.6 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A15)) and a high molecular weight component (hydrogenated copolymer (B15)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X15) are shown in Table 2. Moreover, (RS1) of the hydrogenated copolymer (A15) was 20.0% by mass, and (RS2) of the hydrogenated copolymer (B15) was 20.0% by mass.

[0135] <Production Example 16: Hydrogenated copolymer (X16)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 5.6 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.044 parts by mass of NBL1 for the first stage relative to 100 parts by mass of the total monomers and 0.30 mol of TMEDA1 for the first stage relative to 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 10.7 parts by mass of styrene (concentration: 20% by mass) and 42.9 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 3.5 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.142 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.10 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 7.5 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 6.0 parts by mass of styrene (concentration: 20% by mass) and 23.9 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A16)) and a high molecular weight component (hydrogenated copolymer (B16)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X16) are shown in Table 2. Moreover, (RS1) of the hydrogenated copolymer (A16) was 20.0 mass %, and (RS2) of the hydrogenated copolymer (B16) was 20.0 mass %.

[0136] <Production Example 17: Hydrogenated copolymer (X17)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 5.6 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.044 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.30 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.04 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 11.3 parts by mass of styrene (concentration: 20% by mass) and 45.3 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 4.9 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.348 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.60 moles of TMEDA2 for the second stage per mole of NBL2 were added, and then 6.6 parts by mass of styrene (concentration 20% by mass) and 26.3 parts by mass of butadiene (concentration 20% by mass) were added and polymerized at 50°C for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A17)) and a high molecular weight component (hydrogenated copolymer (B17)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X17) are shown in Table 2. Moreover, (RS1) of the hydrogenated copolymer (A17) was 20.0 mass%, and (RS2) of the hydrogenated copolymer (B17) was 20.0 mass%.

[0137] <Production Example 18: Hydrogenated copolymer (X18)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 5.6 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.050 parts by mass of NBL1 for the first stage relative to 100 parts by mass of the total monomers and 0.30 mol of TMEDA1 for the first stage relative to 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 21.7 parts by mass of styrene (concentration: 20% by mass) and 31.2 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 2.1 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.129 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.20 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 11.9 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 11.9 parts by mass of styrene (concentration: 20% by mass) and 15.8 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated by GPC into a low molecular weight component (hydrogenated copolymer (A18)) and a high molecular weight component (hydrogenated copolymer (B18)), which were analyzed separately. The analytical results of the obtained hydrogenated copolymer (X18) are shown in Table 2. Moreover, (RS1) of the hydrogenated copolymer (A18) was 42.9 mass%, and (RS2) of the hydrogenated copolymer (B18) was 41.2 mass%.

[0138] <Production Example 19: Hydrogenated copolymer (X19)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 4.8 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.034 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.50 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.04 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 9.9 parts by mass of styrene (concentration: 20% by mass) and 39.6 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 3.4 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.405 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.70 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 14.8 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 2.8 parts by mass of styrene (concentration: 20% by mass) and 24.8 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A19)) and a high molecular weight component (hydrogenated copolymer (B19)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X19) are shown in Table 2. Moreover, (RS1) of the hydrogenated copolymer (A19) was 10.0 mass %, and (RS2) of the hydrogenated copolymer (B19) was 19.7 mass %.

[0139] <Production example 20: Hydrogenated copolymer (X20)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 7.4 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.075 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.00 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.02 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 10.2 parts by mass of styrene (concentration: 20% by mass) and 40.8 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 5.3 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.315 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.70 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 7.3 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 5.8 parts by mass of styrene (concentration: 20% by mass) and 23.2 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A20)) and a high molecular weight component (hydrogenated copolymer (B20)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X20) are shown in Table 2. Moreover, (RS1) of the hydrogenated copolymer (A20) was 20.0 mass%, and (RS2) of the hydrogenated copolymer (B20) was 20.0 mass%.

[0140] <Production Example 21: Hydrogenated copolymer (X21)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 1.5 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.026 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 2.00 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.04 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 10.2 parts by mass of styrene (concentration: 20% by mass) and 40.9 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 1.0 part by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.494 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.70 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 9.3 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 3.7 parts by mass of styrene (concentration: 20% by mass) and 33.4 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A21)) and a high molecular weight component (hydrogenated copolymer (B21)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X21) are shown in Table 2. Moreover, (RS1) of the hydrogenated copolymer (A21) was 10.0 mass %, and (RS2) of the hydrogenated copolymer (B21) was 19.8 mass %.

[0141] <Production Example 22: Hydrogenated copolymer (X22)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 11.1 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.033 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.60 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.04 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 3.7 parts by mass of styrene (concentration: 20% by mass) and 33.6 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 9.4 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.439 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.80 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 8.4 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 3.4 parts by mass of styrene (concentration: 20% by mass) and 30.3 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated by GPC into a low molecular weight component (hydrogenated copolymer (A22)) and a high molecular weight component (hydrogenated copolymer (B22)), which were analyzed separately. The analytical results of the obtained hydrogenated copolymer (X22) are shown in Table 2. Moreover, (RS1) of the hydrogenated copolymer (A22) was 10.0% by mass, and (RS2) of the hydrogenated copolymer (B22) was 10.0% by mass.

[0142] <Production Example 23: Hydrogenated copolymer (X23)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 4.8 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.036 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.40 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.04 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 9.9 parts by mass of styrene (concentration: 20% by mass) and 39.6 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 3.8 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.539 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 1.00 mole of TMEDA2 for the second stage per mole of NBL2 were added, and then 8.4 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 6.7 parts by mass of styrene (concentration: 20% by mass) and 26.8 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated by GPC into a low molecular weight component (hydrogenated copolymer (A23)) and a high molecular weight component (hydrogenated copolymer (B23)), and each was analyzed. The analytical results of the obtained hydrogenated copolymer (X23) are shown in Table 2. Moreover, (RS1) of the hydrogenated copolymer (A23) was 20.0 mass %, and (RS2) of the hydrogenated copolymer (B23) was 20.0 mass %.

[0143] <Production Example 24: Hydrogenated copolymer (X24)> In the case of the hydrogenated copolymer (X24), the copolymer (A24) and the copolymer (B24) were each subjected to batch polymerization in separate reactors, and then each polymerization reaction was terminated. The copolymer (A24) and the copolymer (B24) were solution-blended, and then hydrogenated. [Polymerization of copolymer (A24)] Batch polymerization was carried out using a tank-type reactor (internal volume: 30 L) equipped with a stirrer and a jacket. 20.0 parts by mass of styrene (concentration: 20% by mass) was added. Next, 1.339 parts by mass of NBL per 100 parts by mass of the total monomers, 0.80 mol of TMEDA per 1 mol of NBL, and 0.005 mol of NaOAm per 1 mol of NBL were added, and polymerization was carried out at 50° C. for 15 minutes. Next, 16.0 parts by mass of styrene (concentration: 20% by mass) and 64.0 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped to obtain a copolymer (A24). [Polymerization of copolymer (B24)] Batch polymerization was carried out using a tank-type reactor (internal volume: 30 L) equipped with a stirrer and a jacket. 8.0 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.052 part by mass of NBL per 100 parts by mass of the total monomers, 2.00 mol of TMEDA per 1 mol of NBL, and 0.100 mol of NaOAm per 1 mol of NBL were added, and polymerization was carried out at 50° C. for 15 minutes. Next, 16.5 parts by mass of styrene (concentration: 20% by mass) and 66.0 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 40° C. for 60 minutes. Next, 7.0 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 50° C. for 15 minutes. Next, 2.4 parts by mass of butadiene (concentration: 20% by mass) was added, and polymerization was carried out at 40° C. for 20 minutes. Thereafter, the polymerization reaction was stopped to obtain a copolymer (B24). Furthermore, 40.0 parts by mass (concentration 20% by mass) of the obtained copolymer (A24) and 60.0 parts by mass (concentration 20% by mass) of the copolymer (B24) were blended in a solution, and the hydrogenation catalyst prepared as described above was added in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A24)) and a high molecular weight component (hydrogenated copolymer (B24)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X24) are shown in Table 2. Moreover, (RS1) of the hydrogenated copolymer (A24) was 20.0 mass %, and (RS2) of the hydrogenated copolymer (B24) was 19.4 mass %.

[0144] <Production example 25: Hydrogenated copolymer (X25)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timing of addition of the monomers and additives in the polymerization step were adjusted as shown below. 2.4 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.022 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.60 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.04 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 4.9 parts by mass of styrene (concentration: 20% by mass) and 19.7 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 1.9 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.820 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.70 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 14.2 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 11.4 parts by mass of styrene (concentration: 20% by mass) and 45.5 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A25)) and a high molecular weight component (hydrogenated copolymer (B25)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X25) are shown in Table 2. Moreover, (RS1) of the hydrogenated copolymer (A25) was 20.0 mass%, and (RS2) of the hydrogenated copolymer (B25) was 20.0 mass%.

[0145] <Production Example 26: Hydrogenated copolymer (X26)> Batch polymerization was carried out in the same manner as in the case of the hydrogenated copolymer (X1) obtained in Production Example 1, except that the amounts and timings of addition of the monomers and additives in the polymerization step were adjusted as shown below. 4.8 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.036 parts by mass of first-stage NBL1 per 100 parts by mass of the total monomers, 1.50 mol of first-stage TMEDA1 per 1 mol of NBL1, and 0.04 mol of NaOAm per 1 mol of NBL1 were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 9.9 parts by mass of styrene (concentration: 20% by mass) and 39.6 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 40 minutes. Next, 3.8 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.539 parts by mass of NBL2 for the second stage per 100 parts by mass of the total monomers and 0.80 mol of TMEDA2 for the second stage per 1 mol of NBL2 were added, and then 8.4 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out at 50°C for 15 minutes. Next, 6.7 parts by mass of styrene (concentration: 20% by mass) and 26.8 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped, and the amount of hydrogen was adjusted to carry out the hydrogenation reaction partway. The hydrogenated copolymer obtained as above was separated into a low molecular weight component (hydrogenated copolymer (A26)) and a high molecular weight component (hydrogenated copolymer (B26)) by GPC and analyzed separately. The analytical results of the obtained hydrogenated copolymer (X26) are shown in Table 2. Moreover, (RS1) of the hydrogenated copolymer (A26) was 20.0 mass%, and (RS2) of the hydrogenated copolymer (B26) was 20.0 mass%.

[0146] <Production Example 27: Hydrogenated copolymer (B27)> Batch polymerization was carried out using a tank-type reactor (internal volume: 30 L) equipped with a stirrer and a jacket. 8.0 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.073 parts by mass of NBL per 100 parts by mass of the total monomers, 1.50 mol of TMEDA per 1 mol of NBL, and 0.042 mol of NaOAm per 1 mol of NBL were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 16.2 parts by mass of styrene (concentration: 20% by mass) and 64.8 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 50 minutes. Next, 7.0 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.8 parts by mass of styrene (concentration: 20% by mass) and 3.2 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The analytical results of the obtained hydrogenated copolymer (B27) are shown in Table 2. The (RS2) content of the hydrogenated copolymer (B27) was 20.0% by mass.

[0147] <Production Example 28: Hydrogenated copolymer (B28)> Batch polymerization was carried out using a tank-type reactor (internal volume: 30 L) equipped with a stirrer and a jacket. 8.0 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.052 parts by mass of NBL per 100 parts by mass of the total monomers, 1.50 mol of TMEDA per 1 mol of NBL, and 0.042 mol of NaOAm per 1 mol of NBL were added, and polymerization was carried out at 60° C. for 15 minutes. Next, 16.2 parts by mass of styrene (concentration: 20% by mass) and 64.8 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 50 minutes. Next, 7.0 parts by mass of styrene (concentration: 20% by mass) was added, and polymerization was carried out at 60° C. for 15 minutes. Next, 0.8 parts by mass of styrene (concentration: 20% by mass) and 3.2 parts by mass of butadiene (concentration: 20% by mass) were added and polymerized at 50° C. for 30 minutes. Thereafter, the polymerization reaction was stopped and a hydrogenation reaction was carried out. The analytical results of the obtained hydrogenated copolymer (B28) are shown in Table 2. The (RS2) content of the hydrogenated copolymer (B28) was 20.0% by mass.

[0148] The hydrogenated copolymers (X1) to (X26) and the hydrogenated copolymers (B27) and (B28) shown in Tables 1 and 2 were subjected to solvent removal and processed into pellets, and calcium stearate equivalent to 3000 ppm was added to each pellet.

[0149] [Examples 1 to 14], [Comparative Examples 1 to 13], [Example 15, Comparative Examples 14 to 15] The hydrogenated copolymers (X1) to (X14) prepared as described above were designated as [Examples 1 to 14], respectively, and the hydrogenated copolymers (X15) to (X26) and (B27) were designated as [Comparative Examples 1 to 13], respectively. In addition, the hydrogenated copolymer (X3) and the hydrogenated copolymer (B28) were dry-blended with a tackifier (YS Polystar HU (hydrogenated terpene phenol resin) manufactured by Yasuhara Chemical Co., Ltd.) in the amount shown in Table 5 below, and these were designated as [Example 15], [Comparative Example 14], and [Comparative Example 15], respectively.

[0150] (Method for evaluating blocking resistance of hydrogenated copolymer pellets) The hydrogenated copolymers (X1) to (X14) of Examples 1 to 14 and the hydrogenated copolymers (X15) to (X26) and (B27) of Comparative Examples 1 to 13 were evaluated for blocking resistance by the following method. 60 g of sample pellets of the same shape (cylindrical shape with a diameter of about 3 mm × 3 mm) consisting of hydrogenated copolymers (X1) to (X26) and hydrogenated copolymer (B27) were placed in a cylindrical metal container with a diameter of 6 cm, and a weight of 1,160 g was placed on top of them. In this state, the pellets were left to stand in a Geer oven heated to 40°C for 22 hours, after which the pellets were removed from the cylindrical metal container and shaken, and the mass of the pellet clump consisting of three or more consecutive pellets was measured to determine the ratio (%) of the weight of the pellet clump to the total weight of the pellets (60 g). Incidentally, the evaluation was carried out after adding calcium stearate equivalent to 3000 ppm to each sample pellet. <Evaluation method> Those with less than 5% of lumps of 3 or more consecutive balls were rated as ⊚. Those with clumps of three or more consecutive balls at 5% to less than 15% were rated as "good." Those with clumps of 3 or more consecutive balls in the percentage of 15% or more but less than 40% were rated as △. Those with 40% or more of three consecutive balls were marked as ×. The evaluation results are shown in Tables 3 and 4 below.

[0151] (Production and evaluation of adhesive films) The polyethylene (HDPE, manufactured by Asahi Kasei Chemicals Corporation, product name "Creolex T5070L", MFR (190°C, 2.16 kg load) = 7.0 g / 10 min) constituting the base layer, and the hydrogenated copolymers (X1) to (X26), and the hydrogenated copolymers (B27) and (B28) constituting the adhesive layer were each fed into an extruder in a ratio such that the thickness of the final adhesive film would be the value shown in Tables 3 to 5 below. Using a multi-layer T-die extruder (PLABOR, manufactured by Plastics Engineering Research Institute Co., Ltd.), both layers were integrated and co-extruded by co-extrusion molding under conditions of an extrusion temperature of 200°C and a die temperature of 220°C, to produce adhesive films having a base layer thickness of 42 μm and an adhesive layer thickness of 8 μm for Examples 1 to 15 and Comparative Examples 1 to 15. As the tackifier, YS Polystar HU (hydrogenated terpene phenol resin / manufactured by Yasuhara Chemical Co., Ltd.) was used.

[0152] (Evaluation of film-forming properties) In the film-forming process of the production of the pressure-sensitive adhesive film in Preparation Examples 1 to 15 and Comparative Examples 1 to 15, the film-forming properties were evaluated according to the following criteria. <Evaluation criteria> The samples without any trouble in film formation, gel, foreign matter, or uneven thickness were rated as ⊚. The samples with no trouble in film formation, gel, or foreign matter, but with slight thickness unevenness on both ends, were rated as "good." A sample having no trouble in film formation, a small amount of gel or foreign matter, and slight thickness unevenness overall was rated as .DELTA.. The samples containing a large amount of gel or foreign matter, or having a large amount of uneven thickness, or being unable to be molded due to film formation problems were rated as x. The film formation troubles include roll wrapping, equipment contamination, and film breakage.

[0153] In order to evaluate the adhesive properties of the adhesive films obtained in Examples 1 to 15 and Comparative Examples 1 to 15, the initial adhesiveness, adhesive enhancement, adhesive residue, and payout property were measured and evaluated.

[0154] [Adhesive properties of adhesive film] The measurement device used was a universal tension and compression tester "Technograph TGE-500N: manufactured by Minebea Corporation." (Evaluation of initial adhesion) The adhesive films produced in Examples 1 to 15 and Comparative Examples 1 to 15 were cut to a width of 25 mm and attached to a PMMA plate (arithmetic mean surface roughness: 0.1 μm) and a SUS304 (2B) plate, and then rolled with a 2 kg rubber roll (diameter 10 cm). The films were left for 30 minutes at a temperature of 23°C and a relative humidity of 50%, and then peeled at an angle of 180 degrees at a peeling speed of 300 mm / min. The initial adhesive strength was measured in accordance with the test JIS K6854-2, and the initial adhesiveness was evaluated according to the following criteria. <Evaluation criteria> "PMMA board" Those with a value of 500 (g / 25mm) or more were rated as ◎. Those with a value between 350 (g / 25mm) and 500 (g / 25mm) were rated as "good". Those with a value between 250 (g / 25mm) and 350 (g / 25mm) were rated as △. Those with a value of less than 250 (g / 25 mm) were rated as x. "SUS304(2B) board" Those with a value of 350 (g / 25mm) or more were rated as ◎. Those with a value between 250 (g / 25mm) and 350 (g / 25mm) were rated as "good". Those with a value between 150 (g / 25mm) and 250 (g / 25mm) were rated as △. Those with a value of less than 150 (g / 25 mm) were rated as x.

[0155] (Evaluation of hyperadhesiveness) In Examples 1 to 15 and Comparative Examples 1 to 15, the prepared adhesive film was cut to a width of 25 mm and attached to a SUS304 (2B) plate, and further attached by rolling with a rubber roll (diameter 10 cm) weighing 2 kg. The specimen was then stored in an oven at 80°C for 2 hours and then left at 23°C x 50% relative humidity for 30 minutes. The specimen was then peeled off at an angle of 180 degrees at a peel speed of 300 mm / min, and the adhesive strength was measured in accordance with JIS K6854-2. The adhesion enhancement was evaluated according to the following formula. Adhesion enhancement = (adhesion strength after heating at 80°C for 2 hours) / (initial adhesive strength) The adhesion enhancement was evaluated according to the following criteria, with a smaller value being considered as better. <Evaluation criteria> A score of 1.5 or less was rated as ◎. Values ​​between 1.5 and 2 are marked as "OK." A score between 2 and 3 was rated △. Anything over 3 was marked as x.

[0156] (Evaluation of adhesive residue) In Examples 1 to 15 and Comparative Examples 1 to 15, the prepared adhesive film was cut to a width of 25 mm and attached to a SUS (2B) plate, and further attached by rolling a 2 kg rubber roll (diameter 10 cm). Thereafter, the specimen was stored in an oven at 80° C. for 2 hours and then left at 23° C. and 50% relative humidity for 30 minutes. Thereafter, the specimen was peeled off at an angle of 180° at a peeling speed of 300 mm / min and evaluated according to the following criteria. <Evaluation criteria> Those that left absolutely no glue residue were rated as ⊚. Those that left a faint mark were marked as "O". 1mm 2 The adhesive was rated as △ when it peeled off due to one of the following points. 1mm 2 Two or more of the following, 1mm 2 If more than this amount of adhesive peeled off, it was rated as x.

[0157] (Evaluation of payout ability) In Examples 1 to 15 and Comparative Examples 1 to 15, the adhesive film produced was cut to a width of 25 mm and attached to an HDPE plate, and then rolled with a 2 kg rubber roll (diameter 10 cm). The film was left for 6 hours at a temperature of 23°C and a relative humidity of 50%, and then peeled at 180 degrees at a peeling speed of 300 mm / min. The initial adhesive strength was measured in accordance with the test JIS K6854-2, and evaluated according to the following criteria. The payout property was evaluated according to the following criteria, with a smaller initial adhesive strength being considered to be better. <Evaluation criteria> Those with a value of less than 50 (g / 25 mm) were rated as ⊚. Those between 50 (g / 25mm) and 75 (g / 25mm) were rated as "good". Those between 75 (g / 25mm) and 100 (g / 25mm) were rated as △. Those with a value of 100 (g / 25 mm) or more were rated as ×.

[0158] (Evaluation of equipment contamination) In Examples 3 and 15 and Comparative Examples 14 and 15, the weight loss of the adhesive layer (hydrogenated copolymer (X), or adhesive composition of hydrogenated copolymer + tackifier) ​​of the adhesive film used was measured by thermogravimetric differential thermal analysis, and evaluated according to the following criteria. The equipment contamination resistance was determined to be better when the weight loss rate after heating under the following conditions was smaller, and was evaluated according to the following criteria. <Evaluation criteria> 20 mg of the hydrogenated copolymer or the adhesive composition of the hydrogenated copolymer + tackifier was weighed out, and using TG-DTA (thermogravimetric differential thermal analysis), it was heated to 200°C at 10°C / min in air, held at 200°C, and the weight loss rate after 30 minutes was measured. Weight loss rate: 0.4% by weight or less was rated as ⊚. Weight loss rate: those exceeding 0.4% by weight were marked as x.

[0159] The results of the TG-DTA (thermogravimetric differential thermal analysis): evaluation of the weight loss rate are shown below, and are also shown in Tables 3 and 5. Adhesive composition of Example 3 (hydrogenated copolymer X3) :0.07% by weight (judgment ◎) Adhesive composition of Example 15 (hydrogenated copolymer X3 + tackifier 10% by mass) :0.52% by weight (judgment ×) Adhesive composition of Comparative Example 14 (hydrogenated copolymer B28 + tackifier 10% by mass) :0.43% by weight (judgment ×) Adhesive composition of Comparative Example 15 (hydrogenated copolymer B28 + tackifier 45% by mass) :2.15% by weight (judgment ×)

[0160] [Evaluation results of hydrogenated copolymer and adhesive composition] The physical properties of the hydrogenated copolymers of Production Examples 1 to 28 are shown in Tables 1 to 2 below, and the evaluation results of Examples 1 to 15 and Comparative Examples 1 to 15 are shown in Tables 3 to 5 below.

[0161] [Table 1]

[0162] [Table 2]

[0163] [Table 3]

[0164] [Table 4]

[0165] [Table 5]

[0166] Examples 1 to 15 show the evaluation results of hydrogenated copolymers (X) that satisfy the constituent requirements of the present invention, and Comparative Examples 1 to 15 show the evaluation results of hydrogenated copolymers that do not satisfy the constituent requirements of the present invention. The Examples did not receive any "X" marks among the seven evaluation items. On the other hand, the Comparative Examples received at least one "X". This shows that the Comparative Examples were inferior to the Examples. Moreover, Example 15 is an example in which a tackifier was added, but it was found to be inferior to Example 3 in the evaluations of film-forming property, payout property, and adhesive residue. Furthermore, when comparing Comparative Example 13 with Comparative Examples 14 and 15, it was found that although the initial adhesion improved in correlation with the amount of tackifier added, the film-forming property, payout property, and adhesive residue deteriorated. Also, the results of TG-DTA (thermogravimetric differential thermal analysis) showed that the addition of a tackifier caused a large weight loss and a large volatile content, and thus worsened equipment contamination. [Industrial Applicability]

[0167] The hydrogenated copolymer and adhesive composition of the present invention have industrial applicability in the fields of reinforcing filler compounds, crosslinked products, foams, molded articles such as multilayer films and multilayer sheets, building materials, vibration-damping and soundproofing materials, wire covering materials, high-frequency fusible compositions, slush molding materials, adhesive compositions, asphalt compositions, automobile interior materials, automobile exterior materials, medical device materials, various containers such as food packaging containers, home electric appliances, industrial parts, toys, etc.

Claims

1. A hydrogenated copolymer (A) which is a hydrogenated copolymer having vinyl aromatic monomer units and conjugated diene monomer units; and a hydrogenated copolymer (B) which is a hydrogenated copolymer having vinyl aromatic monomer units and conjugated diene monomer units, A hydrogenated copolymer (X) which satisfies the following conditions (1) to (9): <Condition (1)>: The hydrogenated copolymer (A) comprises a polymer block (BS1) mainly composed of vinyl aromatic monomer units, The polymer block mainly comprises a conjugated diene monomer unit, or a random copolymer block composed of a conjugated diene monomer unit and a vinyl aromatic monomer unit, the content of all vinyl aromatic monomer units (TS1) in the hydrogenated copolymer (A) is 10 to 40 mass%; The content of the polymer block (BS1) in the hydrogenated copolymer (A) is from 10 to 30% by mass. <Condition (2)>: The hydrogenated copolymer (A) has a number average molecular weight (Mn1) of 3,000 to 35,000. <Condition (3)>: The hydrogenated copolymer (B) comprises at least one polymer block (BS2) mainly composed of vinyl aromatic monomer units, At least one random copolymer block consisting of conjugated diene monomer units and vinyl aromatic monomer units is included, the content of all vinyl aromatic monomer units (TS2) in the hydrogenated copolymer (B) is 15 to 40 mass%; The content of the polymer block (BS2) in the hydrogenated copolymer (B) is from 10 to 30% by mass. <Condition (4)>: The hydrogenated copolymer (B) has a number average molecular weight (Mn2) of 130,000 to 300,000. <Condition (5)>: The amount of vinyl bonds (Va) before hydrogenation derived from a conjugated diene compound in the hydrogenated copolymer (A) and the amount of vinyl bonds (Vb) before hydrogenation derived from a conjugated diene compound in the hydrogenated copolymer (B) are 50 to 90 mass%. <Condition (6)>: A difference between the vinyl bond content (Va) of the hydrogenated copolymer (A) and the vinyl bond content (Vb) of the hydrogenated copolymer (B) is ±20% by mass or less (absolute value is 20) . <Condition (7)>: The ratio (Mn2 / Mn1) of the number average molecular weight (Mn2) of the hydrogenated copolymer (B) to the number average molecular weight (Mn1) of the hydrogenated copolymer (A) is 10 or more. <Condition (8)>: The hydrogenated copolymer (A) has a hydrogenation rate (Ha) of unsaturated double bonds derived from a conjugated diene compound, and the hydrogenated copolymer (B) has a hydrogenation rate (Hb) of unsaturated double bonds derived from a conjugated diene compound of 70% or more. <Condition (9)>: The mass ratio (A) / (B) of the content of the hydrogenated copolymer (A) to the content of the hydrogenated copolymer (B) is 10 / 90 to 50 / 50.

2. The number average molecular weight (Mn1) of the hydrogenated copolymer (A) is 5,000 to 15,000. The hydrogenated copolymer (X) according to claim 1.

3. the vinyl bond amount (Va) and the vinyl bond amount (Vb) are 60 to 85 mass%; The hydrogenated copolymer (A) and the hydrogenated copolymer (B) each have a hydrogenation rate of 85% or more of unsaturated double bonds derived from a conjugated diene compound. The hydrogenated copolymer (X) according to claim 1.

4. a ratio (MnS1 / MnS2) of a molecular weight (MnS1) of a polymer block (BS1) mainly composed of a vinyl aromatic monomer unit in the hydrogenated copolymer (A) to a molecular weight (MnS2) of a polymer block (BS2) mainly composed of a vinyl aromatic monomer unit in the hydrogenated copolymer (B) is 0.05 to 0.5; The hydrogenated copolymer (X) according to claim 1. (MnS1 and MnS2 are calculated by the following method. MnS1=Mn1×BS1 MnS2=Mn2×BS2÷f BS1: Proton nuclear magnetic resonance ( 1 The content of the polymer block mainly composed of a vinyl aromatic compound in the hydrogenated copolymer (A) determined by H-NMR BS2: Proton nuclear magnetic resonance ( 1 The content of the polymer block mainly composed of a vinyl aromatic compound in the hydrogenated copolymer (B) determined by H-NMR f: degree of branching of hydrogenated copolymer (B) determined by GPC-light scattering method with a viscosity detector)

5. The number average molecular weight (Mn2) of the hydrogenated copolymer (B) is 150,000 to 250,000. The hydrogenated copolymer (X) according to claim 1.

6. the ratio (Mn2 / Mn1) of the number average molecular weight (Mn2) of the hydrogenated copolymer (B) to the number average molecular weight (Mn1) of the hydrogenated copolymer (A) is 15 or more; The hydrogenated copolymer (X) according to claim 1.

7. The content of the hydrogenated copolymer (A), The mass ratio (A) / (B) of the content of the hydrogenated copolymer (B) is 25 / 75 to 50 / 50, The hydrogenated copolymer (X) according to claim 1.

8. The hydrogenated copolymer (A) and the hydrogenated copolymer (B) All of the following conditions (10) to (11) are met: The hydrogenated copolymer (X) according to claim 1. <Condition (10)>: The hydrogenated copolymer (A) is a block copolymer represented by the general structural formula: a-b or ac. <Condition (11)>: The hydrogenated copolymer (B) is a block copolymer represented by the general structural formula: dedab or dedac. (In the above general structural formula, a and d are polymer blocks mainly composed of vinyl aromatic monomer units, b and e are random copolymer blocks composed of vinyl aromatic monomer units and conjugated diene monomer units, and c is a polymer block mainly composed of conjugated diene monomer units.)

9. The general structural formula of the hydrogenated copolymer (A) and the general structural formula of the hydrogenated copolymer (B) are The following is either (a) or (b): The hydrogenated copolymer (X) according to claim 1. (A): The hydrogenated copolymer (A) is represented by the general structural formula a-b, and the hydrogenated copolymer (B) is a block copolymer represented by the general structural formula dd-a-b. (i): The hydrogenated copolymer (A) is represented by the general structural formula: a-c, and the hydrogenated copolymer (B) is a block copolymer represented by the general structural formula: dedac. (In the above general structural formula, a and d are polymer blocks mainly composed of vinyl aromatic monomer units, b and e are random copolymer blocks composed of vinyl aromatic monomer units and conjugated diene monomer units, and c is a polymer block mainly composed of conjugated diene monomer units.)

10. A pressure-sensitive adhesive composition comprising the hydrogenated copolymer (X) according to claim 1 .

11. The weight loss after 200°C for 30 minutes as measured by TG-DTA (thermogravimetric differential thermal analysis) is 0.4% or less. The adhesive composition according to claim 10.

12. The weight loss after 200°C for 30 minutes as measured by TG-DTA (thermogravimetric differential thermal analysis) is 0.4% or less. The hydrogenated copolymer (X) according to claim 1.

13. A resin substrate layer; A layer of the adhesive composition according to claim 10; A, having an adhesive film.

14. A method for producing the hydrogenated copolymer (X) according to any one of claims 1 to 9 and 12, comprising the steps of: The method includes a step of simultaneously producing the hydrogenated copolymer (A) and the hydrogenated copolymer (B) in one reactor, In the above process, The raw material monomers of each polymer block and a polymerization initiator are added in the following order (c) or (d), and then hydrogenated. A method for producing hydrogenated copolymer (X). (C) First polymerization initiator, d, e, d, second polymerization initiator, a, b (E) First polymerization initiator, d, e, d, second polymerization initiator, a, c (In the above (c) and (d), a and d are polymer blocks mainly composed of vinyl aromatic monomer units, b and e are random copolymer blocks composed of vinyl aromatic monomer units and conjugated diene monomer units, and c is a polymer block mainly composed of conjugated diene monomer units, and raw material monomers for each polymer block are added.)

Citation Information

Patent Citations

  • Hydrogenated copolymer, composition, and molded article

    WO2017126469A1