Resin composition and molded product

By blending specific copolymers with polycarbonate and acrylic resins, the interfacial strength is enhanced, addressing delamination issues and maintaining transparency and mechanical properties in composite molded products.

JP2024132903APending Publication Date: 2024-10-01MITSUBISHI CHEM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024023176
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-15
Filing Date
2024-02-19
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Polycarbonate and acrylic resins are incompatible, leading to weak interfacial strength and easy delamination in composite molded products, especially when using isosorbide-derived polycarbonate and acrylic resins, which can result in poor appearance and impact resistance.

Method used

A resin composition is developed by blending specific copolymers, such as block or graft copolymers, in appropriate amounts with polycarbonate and acrylic resins, where the copolymer contains polymer chains compatible with both, enhancing interfacial strength.

Benefits of technology

The resin composition maintains transparency and mechanical properties while suppressing delamination, ensuring a composite with improved appearance and impact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132903000001
    Figure 2024132903000001
  • Figure 2024132903000002
    Figure 2024132903000002
  • Figure 2024132903000003
    Figure 2024132903000003
Patent Text Reader

Abstract

To provide a resin composition that, when molded, maintains transparency, mechanical properties and impact resistance while suppressing the occurrence of delamination, and also enables the conjugation of polycarbonate resin and acrylic resin without impairing the appearance.SOLUTION: A resin composition comprises a polycarbonate resin (A), an acrylic resin (B), and a copolymer (C). Relative to 100 mass% of the total of the polycarbonate resin (A) and the acrylic resin (B), the content of the copolymer (C) is 0.5 mass% or more and 9.5 mass% or less. The copolymer (C) contains a specific polymer chain (c1) and a specific polymer chain (c2).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition containing a polycarbonate resin and an acrylic resin, and a molded article made using the same. [Background technology]

[0002] Polycarbonate resins are generally produced using raw materials derived from petroleum resources. However, in recent years, due to concerns about the depletion of petroleum resources, development of polycarbonate resins made from biomass resources using plant-derived monomers as raw materials has been promoted. For example, polycarbonate resins produced using isosorbide (ISB) as a plant-derived monomer have been developed and have begun to be used for automobile parts, optical applications, and glass replacement applications (see, for example, Patent Documents 1 and 2).

[0003] Polycarbonate resins obtained from ISB are not only excellent in optical properties, but also have better weather resistance and surface hardness than conventional aromatic polycarbonate resins, and are therefore being deployed in outdoor applications and as a replacement for glass. However, a material that meets all the properties required for these applications has not yet been found, and various methods for improving the properties without impairing the advantages of weather resistance and transparency have been explored. For example, Patent Document 3 reports a case in which scratch resistance and optical properties (low birefringence) were improved by compounding with acrylic resin, a transparent resin that also has excellent weather resistance. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2004 / 111106 [Patent Document 2] International Publication No. 2007 / 148604 [Patent Document 3] Patent Publication No. 2021-88651 Summary of the Invention [Problem to be solved by the invention]

[0005] Polycarbonate resin and acrylic resin are incompatible, so when they are combined, the interfacial strength between them is generally weak. In particular, when polycarbonate resin obtained from ISB is combined with acrylic resin, even a slight impact on the molded product can easily cause delamination marks inside the molded product, resulting in poor appearance.

[0006] An object of the present invention is to provide a resin composition which, when molded, maintains transparency, mechanical properties, and impact resistance while suppressing the occurrence of delamination and enables the composite of a polycarbonate resin and an acrylic resin without impairing the appearance. [Means for solving the problem]

[0007] As a result of extensive research, the present inventors have found that the above object can be achieved by blending a resin blend, which is a specific copolymer, in an appropriate blending amount with a polycarbonate resin and an acrylic resin.

[0008] That is, the gist of the present invention is as follows.

[0009] Aspect 1 of the present invention is The composition comprises a polycarbonate resin (A), an acrylic resin (B), and a copolymer (C), the blending amount of the copolymer (C) is 0.5% by mass or more and 9.5% by mass or less relative to 100% by mass of the total of the polycarbonate resin (A) and the acrylic resin (B); The present invention relates to a resin composition, wherein the copolymer (C) is a copolymer having a polymer chain (c1) and a polymer chain (c2) shown below. Polymer chain (c1): A polymer chain that is compatible with the acrylic resin (B). Polymer chain (c2): A polymer chain containing 50% by mass or more and 100% by mass or less of a (meth)acrylate monomer unit represented by the following general formula (1):

[0010] [ka]

[0011] (In general formula (1), Y represents a hydrogen atom or a methyl group, and m is a natural number of 1 to 30.)

[0012] Aspect 2 of the present invention relates to the resin composition of aspect 1, The present invention relates to a resin composition, in which the polymer chain (c1) contains 80% by mass or more and 100% by mass or less of methyl methacrylate monomer units.

[0013] Aspect 3 of the present invention is a resin composition according to aspect 1 or 2, The present invention relates to a resin composition, wherein the polycarbonate resin (A) has a structural unit derived from a compound represented by the following formula (2):

[0014] [ka]

[0015] A fourth aspect of the present invention relates to a resin composition comprising: The present invention relates to a resin composition, in which the acrylic resin (B) contains 80% by mass or more and 100% by mass or less of methyl methacrylate monomer units.

[0016] A fifth aspect of the present invention relates to a resin composition according to any one of the first to fourth aspects, The present invention relates to a resin composition, wherein the copolymer (C) is a block copolymer and / or a graft copolymer.

[0017] A sixth aspect of the present invention relates to a resin composition comprising: The present invention relates to a resin composition, wherein the copolymer (C) is a macromonomer copolymer composed of a polymer chain (c1) derived from a macromonomer represented by the following general formula (3) and a polymer chain (c2) derived from a comonomer copolymerizable with the macromonomer:

[0018] [ka]

[0019] (In general formula (3), R 0 ~R n are each independently a hydrogen atom, an alkyl group, a cycloalkyl group, an aryl group, or a heterocyclic group. 1 ~X n are each independently a hydrogen atom or a methyl group. Z is a terminal group. n is a natural number from 2 to 10,000.

[0020] A seventh aspect of the present invention is The present invention relates to a molded article made of the resin composition according to any one of the first to sixth aspects. Effect of the Invention

[0021] According to the resin composition of the present invention, when molded, the transparency, mechanical properties, and impact resistance are maintained, while the occurrence of delamination is suppressed when a polycarbonate resin and an acrylic resin are combined, so that the two can be combined without impairing the appearance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] In the present invention, the term "structural unit" refers to a chemical structure formed directly from a monomer by a polymerization reaction, and a chemical structure in which a part of the structure of the structural unit contained in a polymer obtained by a polymerization reaction is converted into another structure by treating the polymer obtained by a polymerization reaction with a chemical reaction. The term "monomer" refers to a compound having polymerizability (polymerizable monomer), and is also called a "monomer." "(Meth)acrylate" is a general term for acrylate and methacrylate.

[0023] The resin composition of the present invention contains a polycarbonate resin (A), an acrylic resin (B), and a copolymer (C). Here, the blending amount of the copolymer (C) is 0.5 mass% or more and 9.5 mass% or less relative to 100 mass% in total of the polycarbonate resin (A) and the acrylic resin (B), and the copolymer (C) has a polymer chain (c1) and a polymer chain (c2) shown below. Polymer chain (c1): A polymer chain that is compatible with the acrylic resin (B). Polymer chain (c2): A polymer chain containing 50% by mass or more and 100% by mass or less of a (meth)acrylate monomer unit represented by the following general formula (1):

[0024] [ka]

[0025] (In general formula (1), Y represents a hydrogen atom or a methyl group, and m is a natural number of 1 to 30.)

[0026] [Polycarbonate resin (A)] The type of polycarbonate resin used in the present invention is not particularly limited. In addition, the polycarbonate resin may be used alone or in any combination of two or more kinds.

[0027] Polycarbonate resin is a polymer having a carbonate bond represented by the general formula: -[-OXOC(=O)-]-, where X is generally a hydrocarbon group but may contain a heteroatom to impart various properties.

[0028] Polycarbonate resins can be classified into aromatic polycarbonate resins in which the carbons directly bonded to the carbonate bonds are aromatic carbons, and aliphatic polycarbonate resins in which the carbons directly bonded to the carbonate bonds are aliphatic carbons, and either of these can be used. From the viewpoint of weather resistance, aliphatic polycarbonate resins are preferred, and aliphatic polycarbonate resins containing alicyclic dihydroxy compounds are more preferred, while aromatic polycarbonate resins are preferred from the viewpoints of heat resistance, mechanical properties, electrical properties, and the like.

[0029] There is no limitation on the specific type of polycarbonate resin, but examples thereof include polycarbonate polymers obtained by reacting an aromatic dihydroxy compound, an aliphatic dihydroxy compound, an alicyclic dihydroxy compound, an ether-containing dihydroxy compound, a cyclic ether, or the like with a carbonate precursor. The polycarbonate polymer may be linear or branched. The polycarbonate polymer may be a homopolymer consisting of one type of repeating unit, or a copolymer having two or more types of repeating units. In this case, the copolymer may be selected from various copolymer forms such as a random copolymer and a block copolymer. In addition, such a polycarbonate polymer is usually a thermoplastic resin.

[0030] Examples of aromatic dihydroxy compounds that are used as raw materials for aromatic polycarbonate resins include the following compounds.

[0031] 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-diethylphenyl)propane, 2,2-bis(4-hydroxy-(3-phenyl)phenyl)propane, 2,2-bis(4-hydroxy-(3,5-diphenyl)phenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 1,1-bis(4-hydroxyphenyl)-2 -Aromatic bisphenol compounds such as ethylhexane, 1,1-bis(4-hydroxyphenyl)decane, bis(4-hydroxy-3-nitrophenyl)methane, 3,3-bis(4-hydroxyphenyl)pentane, 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenylsulfone, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxy-3-methylphenyl)sulfide, bis(4-hydroxyphenyl)disulfide, 4,4'-dihydroxydiphenyl ether, and 4,4'-dihydroxy-3,3'-dichlorodiphenyl ether; Dihydroxy compounds having an ether group bonded to an aromatic group, such as 2,2-bis(4-(2-hydroxyethoxy)phenyl)propane, 2,2-bis(4-(2-hydroxypropoxy)phenyl)propane, 1,3-bis(2-hydroxyethoxy)benzene, 4,4'-bis(2-hydroxyethoxy)biphenyl, and bis(4-(2-hydroxyethoxy)phenyl)sulfone; 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene , 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene and other dihydroxy compounds having a fluorene ring.

[0032] Among these, from the viewpoints of impact resistance and heat resistance, 2,2-bis(4-hydroxyphenyl)propane (ie, bisphenol A) and 2,2-bis(3-methyl-4-hydroxyphenyl)propane (ie, bisphenol C) are preferred. The aromatic dihydroxy compounds may be used alone or in any combination of two or more.

[0033] Examples of the aliphatic dihydroxy compound, alicyclic dihydroxy compound, and ether-containing dihydroxy compound that are the raw materials for the aliphatic polycarbonate resin include the following compounds. In the present invention, an aliphatic dihydroxy compound refers to a dihydroxy compound having a saturated hydrocarbon group, and does not include cyclic ethers in which a portion of the cyclic hydrocarbon is substituted with a hetero atom.

[0034] Straight-chain aliphatic dihydroxy compounds such as ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 1,5-heptanediol, 1,6-hexanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol; branched-chain aliphatic dihydroxy compounds such as 1,3-butanediol, 1,2-butanediol, neopentyl glycol, and hexylene glycol; Dihydroxy compounds which are primary alcohols of alicyclic hydrocarbons, exemplified by 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, pentacyclopentadecane dimethanol, 2,6-decalin dimethanol, 1,5-decalin dimethanol, 2,3-decalin dimethanol, 2,3-norbornane dimethanol, 2,5-norbornane dimethanol, 1,3-adamantanedimethanol, and dihydroxy compounds derived from terpene compounds such as limonene; dihydroxy compounds which are secondary or tertiary alcohols of alicyclic hydrocarbons, exemplified by 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,3-adamantanediol, hydrogenated bisphenol A, and 2,2,4,4-tetramethyl-1,3-cyclobutanediol; Ether-containing dihydroxy compounds, which are dihydroxy compounds containing an acetal ring, such as oxyalkylene glycols, such as diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol, and spiro glycol (also known as 3,9-bis(1,1-dimethyl-2-hydroxyethyl-2,4,8,10-tetraoxaspiro[5,5]undecane) and dioxane glycol (also known as 2-(1,1-dimethyl-2-hydroxyethyl)-5-ethyl-5-hydroxymethyl-1,3-dioxane).

[0035] Among these, from the viewpoint of improving mechanical properties and flowability during melt molding, it is preferable to contain a structural unit derived from an aliphatic dihydroxy compound or an alicyclic dihydroxy compound, and among these, 1,4-cyclohexanedimethanol and tricyclodecane dimethanol are more preferable, and it is even more preferable to contain a structural unit derived from 1,4-cyclohexanedimethanol. The aliphatic dihydroxy compounds, alicyclic dihydroxy compounds, and ether-containing dihydroxy compounds may be used alone or in any combination of two or more.

[0036] Examples of cyclic ethers that can be used as raw materials for aliphatic polycarbonate resins include the following compounds.

[0037] Cyclic ethers such as 1,2-epoxyethane (i.e., ethylene oxide), 1,2-epoxypropane (i.e., propylene oxide), 1,2-epoxycyclopentane, 1,2-epoxycyclohexane, 1,4-epoxycyclohexane, 1-methyl-1,2-epoxycyclohexane, 2,3-epoxynorbornane, and 1,3-epoxypropane; compounds represented by the following formula (2), i.e., compounds selected from isosorbide, isomannide, isoidite, and the like, which are a group of compounds having a stereoisomeric relationship.

[0038] [ka]

[0039] Among these, isosorbide obtained by dehydration and condensation of sorbitol produced from various starches, which are abundant as plant-derived resources and are easily available, is preferred in terms of availability, ease of production, and properties of the resulting molded products (e.g., heat resistance, impact resistance, surface hardness, carbon neutrality). The cyclic ethers may be used alone or in any combination of two or more kinds.

[0040] Among these dihydroxy compounds that are raw materials for polycarbonate resins, it is preferable to use the compound represented by formula (2) because it utilizes biomass resources and has a low environmental impact. In other words, it is preferable that the polycarbonate resin has a constitutional unit derived from the compound represented by formula (2).

[0041] Of the 100 mol% of the dihydroxy compound-derived structural units in the polycarbonate resin, the proportion of the structural units derived from the compound represented by the formula (2) is preferably 35 mol% or more, more preferably 40 mol% or more. Also, of the 100 mol% of the dihydroxy compound-derived structural units in the polycarbonate resin, the proportion of the structural units derived from the compound represented by the formula (2) is preferably 80 mol% or less, more preferably 70 mol% or less. Of the 100 mol% of the dihydroxy compound-derived structural units in the polycarbonate resin, the proportion of the structural units derived from the compound represented by the formula (2) is preferably 35 mol% or more and 80 mol% or less. When the proportion of the structural units derived from the compound represented by formula (2) among 100 mol % of the structural units derived from a dihydroxy compound in the polycarbonate resin is within the above range, a resin composition having an excellent balance of compatibility with the acrylic resin (B) and copolymer (C) described below, which is less susceptible to delamination and has an excellent appearance can be obtained.

[0042] Examples of carbonate precursors that serve as raw materials for polycarbonate resins include carbonyl halides and carbonic acid diesters.

[0043] Examples of the carbonyl halides include phosgene; and haloformates such as bischloroformates of dihydroxy compounds and monochloroformates of dihydroxy compounds.

[0044] As the carbonic acid diester, a compound represented by the following general formula (4) can usually be used. These carbonic acid diesters may be used alone or in any combination of two or more.

[0045] [ka]

[0046] (In general formula (4), A 1 and A 2 each represents an aliphatic hydrocarbon group having 1 to 18 carbon atoms which may have a substituent, or an aromatic hydrocarbon group which may have a substituent, 1 and A 2 may be the same or different.)

[0047] A 1 and A 2 is preferably a substituted or unsubstituted aromatic hydrocarbon group, more preferably an unsubstituted aromatic hydrocarbon group. Examples of the substituent of the aliphatic hydrocarbon group include an ester group, an ether group, an amide group, and a halogen atom, and examples of the substituent of the aromatic hydrocarbon group include an alkyl group such as a methyl group or an ethyl group.

[0048] Examples of the carbonic acid diester represented by the general formula (4) include diphenyl carbonate (hereinafter sometimes abbreviated as DPC), substituted diphenyl carbonate such as ditolyl carbonate, and dialkyl carbonate such as dimethyl carbonate, diethyl carbonate, and di-tert-butyl carbonate. Of these, preferred are diphenyl carbonate and substituted diphenyl carbonate, and particularly preferred is diphenyl carbonate.

[0049] The carbonate diester may contain impurities such as chloride ions, and these impurities may inhibit the polymerization reaction or deteriorate the hue of the resulting resin. Therefore, it is preferable to use a diester that has been purified, as necessary, by distillation or the like.

[0050] In the present invention, the method for producing the polycarbonate resin is not particularly limited, and any method may be adopted using the above-mentioned raw materials as appropriate, such as an interfacial polymerization method, a melt transesterification method, a pyridine method, a ring-opening polymerization method of a cyclic carbonate compound, or a solid-phase transesterification method of a prepolymer.

[0051] [Characteristics of polycarbonate resin] (molecular weight) The molecular weight of polycarbonate resin is related to reduced viscosity and 1 It can be expressed as the number average molecular weight measured by H-NMR, etc. The higher the value obtained by these measuring methods, the higher the molecular weight. 1 The number average molecular weight of the polycarbonate resin measured by H-NMR is preferably 8,000 or more, more preferably 9,000 or more, and even more preferably 10,000 or more. 1 The number average molecular weight of the polycarbonate resin measured by H-NMR is preferably 30,000 or less, more preferably 25,000 or less, and even more preferably 20,000 or less. 1 The number average molecular weight of the polycarbonate resin measured by H-NMR is preferably 8,000 or more and 30,000 or less. The reduced viscosity of the polycarbonate resin is preferably 0.3 dL / g or more, more preferably 0.35 dL / g or more, and even more preferably 0.4 dL / g or more. The reduced viscosity of the polycarbonate resin is preferably 1.0 dL / g or less, more preferably 0.8 dL / g or less, and even more preferably 0.7 dL / g or less. The reduced viscosity of the polycarbonate resin is preferably 0.3 dL / g or more and 1.0 dL / g or less. When the measured molecular weight of the polycarbonate resin is within the above range, sufficient mechanical strength is obtained, and the flowability during melt molding can be adjusted to a preferred range.

[0052] (glass transition temperature) The glass transition temperature of the polycarbonate resin is preferably 80° C. or higher, more preferably 85° C. or higher, and even more preferably 90° C. or higher. The glass transition temperature of the polycarbonate resin is preferably 160° C. or lower, more preferably 150° C. or lower, and even more preferably 140° C. or lower. The glass transition temperature of the polycarbonate resin is preferably 80° C. or higher and 160° C. or lower. When the glass transition temperature of the polycarbonate resin is within the above range, the resin has sufficient heat resistance and mechanical properties, and is easily molded.

[0053] [Acrylic resin (B)] The acrylic resin used in the present invention is a thermoplastic acrylic resin.

[0054] The composition of the acrylic resin is preferably one containing 80% by mass or more of methyl methacrylate when the total monomer units constituting the acrylic resin are taken as 100% by mass, more preferably one containing 85% by mass or more, and even more preferably one containing 90% by mass or more. It is also preferable to use one containing 100% by mass or less of methyl methacrylate. The composition of the acrylic resin is preferably one containing 80% by mass or more and 100% by mass or less of methyl methacrylate when the total monomer units constituting the acrylic resin are taken as 100% by mass. When the content of the methyl methacrylate monomer units in the acrylic resin is within the above range, a resin composition having an excellent balance of compatibility with the polycarbonate resin (A) and the copolymer (C), which is less susceptible to delamination and has an excellent appearance, can be obtained.

[0055] The acrylic resin may be a homopolymer of methyl methacrylate, but may also be copolymerized with other vinyl monomers depending on the purpose. The vinyl monomer used in the acrylic resin is not particularly limited, but examples thereof include: (Meth)acrylates such as methyl acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-lauryl (meth)acrylate, n-stearyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, and isobornyl (meth)acrylate; hydroxyl group-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and glycerol (meth)acrylate; Carboxy group-containing vinyl monomers such as (meth)acrylic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxypropyl phthalic acid, 2-(meth)acryloyloxyethyl maleic acid, 2-(meth)acryloyloxypropyl maleic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxypropyl succinic acid, crotonic acid, fumaric acid, maleic acid, itaconic acid, monomethyl maleate, and monomethyl itaconate; Vinyl monomers containing an acid anhydride group, such as maleic anhydride and itaconic anhydride; Epoxy group-containing vinyl monomers such as glycidyl (meth)acrylate, glycidyl α-ethyl acrylate, and 3,4-epoxybutyl (meth)acrylate; Amino group-containing (meth)acrylate vinyl monomers such as dimethylaminoethyl (meth)acrylate and diethylaminoethyl (meth)acrylate; Vinyl monomers containing an amide group, such as (meth)acrylamide, Nt-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, diacetone acrylamide, maleic acid amide, and maleimide; Vinyl monomers such as styrene, α-methylstyrene, vinyltoluene, (meth)acrylonitrile, vinyl chloride, vinyl acetate, and vinyl propionate; polyfunctional vinyl monomers such as divinylbenzene, ethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, allyl (meth)acrylate, and N,N'-methylenebis(meth)acrylamide; These may be used alone or in any combination of two or more.

[0056] Among these, from the viewpoint of improving the thermal decomposition resistance of the acrylic resin, acrylates such as methyl acrylate, ethyl acrylate, and n-butyl acrylate are preferred, and methyl acrylate is more preferred in that the balance of compatibility with the polycarbonate resin (A) and the copolymer (C) described later is less likely to be impaired.

[0057] The amount of monomers other than methyl methacrylate in 100% by mass of all monomer units constituting the acrylic resin is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less.

[0058] The molecular weight of the acrylic resin used in the present invention can be measured by GPC, which will be described later. The mass average molecular weight (Mw) of the acrylic resin used in the present invention is preferably 80,000 or more, more preferably 90,000 or more, and even more preferably 100,000 or more. The mass average molecular weight (Mw) of the acrylic resin used in the present invention is preferably 200,000 or less, more preferably 180,000 or less, and even more preferably 160,000 or less. The mass average molecular weight (Mw) of the acrylic resin used in the present invention is preferably 80,000 or more and 200,000 or less. When the mass average molecular weight of the acrylic resin is within the above range, sufficient mechanical strength is obtained, and the flowability during melt molding can also be adjusted to a preferred range.

[0059] The glass transition temperature of the acrylic resin used in the present invention is preferably 70° C. or higher, more preferably 80° C. or higher, and even more preferably 90° C. or higher. The glass transition temperature of the acrylic resin used in the present invention is preferably 130° C. or lower, more preferably 125° C. or lower, and even more preferably 120° C. or lower. The glass transition temperature of the acrylic resin used in the present invention is preferably 70° C. or higher and 130° C. or lower. When the glass transition temperature of the acrylic resin used in the present invention is within the above range, the mechanical strength of the resin composition of the present invention is not easily impaired and appropriate melt processability is obtained.

[0060] The method for producing the acrylic resin used in the present invention is not particularly limited, and various methods such as solution polymerization, suspension polymerization, emulsion polymerization, bulk polymerization, etc. Aqueous polymerization such as suspension polymerization or emulsion polymerization is preferred because it is easy to control the heat generated by polymerization and has excellent productivity, and suspension polymerization is more preferred because the polymer recovery operation is simpler.

[0061] [Copolymer (C)] The copolymer (C) used in the present invention has a polymer chain (c1) that is compatible with the acrylic resin (B) and a polymer chain (c2) that contains 50% by mass or more and 100% by mass or less of a (meth)acrylate monomer unit represented by the following general formula (1):

[0062] [ka]

[0063] In the above general formula (1), Y represents a hydrogen atom or a methyl group, and m is a natural number of 1 to 30.

[0064] From the viewpoint of compatibility with the polycarbonate resin (A), Y is preferably a methyl group. From the same viewpoint, m is preferably a natural number of 1 to 20, and more preferably a natural number of 1 to 10.

[0065] The polymer chain (c2) has excellent compatibility with the polycarbonate resin (A). As a result, the copolymer (C) having a structure including the polymer chain (c1) and the polymer chain (c2) acts as a compatibilizer for the polycarbonate resin (A) and the acrylic resin (B), improving the strength of the interface between the two and realizing a resin composition that is less susceptible to delamination and has an excellent appearance.

[0066] The copolymer (C) is preferably a block copolymer and / or a graft copolymer (sometimes abbreviated as block-graft copolymer) containing a polymer chain (c1) and a polymer chain (c2). In a block copolymer, the polymer chain (c1) and the polymer chain (c2) are bonded to one polymer chain, while in a graft copolymer, either the polymer chain (c1) or the polymer chain (c2) is a trunk polymer, and the other is a branched polymer that forms a branch polymer. From the viewpoint of easily ensuring the interfacial strength between the polycarbonate resin (A) and the acrylic resin (B), the copolymer (C) is more preferably a graft copolymer, and among these, a graft copolymer in which the polymer chain (c1) is a branch polymer and the polymer chain (c2) is a trunk polymer is even more preferable.

[0067] Here, it is preferable that the copolymer (C) does not have a crosslinked structure. When the copolymer (C) does not have a crosslinked structure, delamination is less likely to occur and a resin composition having excellent appearance is more likely to be obtained.

[0068] The ratio of the polymer chain (c1) and the polymer chain (c2) contained in the copolymer (C) is not particularly limited as long as both are contained, but the mass ratio of the polymer chain (c1) / polymer chain (c2) is preferably in the range of 10 / 90 to 70 / 30, more preferably in the range of 20 / 80 to 60 / 40, and even more preferably in the range of 30 / 70 to 50 / 50. When the mass ratio of polymer chain (c1) / polymer chain (c2) is within the above range, it is easy to obtain a resin composition which is less susceptible to interlayer peeling and has excellent appearance.

[0069] The molecular weight of the copolymer (C) can be measured by GPC, which will be described later. The mass average molecular weight (Mw) of the copolymer (C) is preferably 30,000 or more, more preferably 40,000 or more, and even more preferably 50,000 or more. The mass average molecular weight (Mw) of the copolymer (C) is preferably 1,500,000 or less, more preferably 1,000,000 or less, and even more preferably 500,000 or less. The mass average molecular weight (Mw) of the copolymer (C) is preferably 30,000 or more and 1,500,000 or less. When the mass average molecular weight of the copolymer (C) is within the above range, the flowability during melt molding can be adjusted to a preferred range without impairing the mechanical properties of the resin composition.

[0070] The number average molecular weight (Mn) of the copolymer (C) is preferably 9,000 or more, more preferably 11,000 or more, and even more preferably 13,000 or more. The number average molecular weight (Mn) of the copolymer (C) is preferably 100,000 or less, more preferably 80,000 or less, and even more preferably 60,000 or less. The number average molecular weight (Mn) of the copolymer (C) is preferably 9,000 or more and 100,000 or less. When the number average molecular weight of the copolymer (C) is within the above range, the flowability during melt molding can be adjusted to a preferred range without impairing the mechanical properties of the resin composition.

[0071] The molecular weight distribution (Mw / Mn) of the copolymer (C) is preferably 1.5 or more, more preferably 2.0 or more, and even more preferably 2.5 or more. Also, it is preferably 30.0 or less, more preferably 20.0 or less, and even more preferably 10.0 or less. The molecular weight distribution (Mw / Mn) of the copolymer (C) is preferably 1.5 or more and 30.0 or less. When the molecular weight distribution of the copolymer (C) is within the above range, the flowability during melt molding can be adjusted to a preferred range without impairing the mechanical properties of the resin composition.

[0072] [Polymer chain (c1)] The polymer chain (c1) plays a role in ensuring compatibility with the acrylic resin (B), and therefore preferably contains 80% by mass or more and 100% by mass or less of methyl methacrylate monomer units. From the viewpoint of compatibility with the acrylic resin (B), the polymer chain (c1) more preferably contains 85% by mass or more and 100% by mass or less of methyl methacrylate monomer units, and even more preferably contains 90% by mass or more and 100% by mass or less.

[0073] The polymer chain (c1) may contain a monomer unit other than methyl methacrylate as long as the compatibility with the acrylic resin (B) is not impaired. The monomer that provides such a monomer unit can be appropriately selected from those exemplified as other vinyl monomers for the acrylic resin (B).

[0074] From the viewpoint of mechanical properties of the resin composition, the polymer chain (c1) has a mass average molecular weight (Mw) of preferably 3,000 or more, more preferably 5,000 or more, and even more preferably 8,000 or more. From the viewpoint of maintaining compatibility with the acrylic resin (B), the mass average molecular weight (Mw) of the polymer chain (c1) is preferably 50,000 or less, more preferably 40,000 or less, and even more preferably 30,000 or less. The mass average molecular weight (Mw) of the polymer chain (c1) is preferably 3,000 or more and 50,000 or less.

[0075] From the viewpoint of compatibility with the acrylic resin (B), the number average molecular weight (Mn) of the polymer chain (c1) is preferably 1,500 or more, more preferably 2,500 or more, and even more preferably 4,000 or more. Also, it is preferably 25,000 or less, more preferably 20,000 or less, and even more preferably 15,000 or less. The number average molecular weight (Mn) of the polymer chain (c1) is preferably 1,500 or more and 25,000 or less.

[0076] From the viewpoint of the stability of the interfacial strength between the acrylic resin (B) and the polycarbonate resin (A), the molecular weight distribution (Mw / Mn) of the polymer chain (c1) is preferably 1.2 or more, more preferably 1.5 or more, and even more preferably 1.8 or more. Also, it is preferably 3.0 or less, more preferably 2.8 or less, and even more preferably 2.5 or less. The molecular weight distribution (Mw / Mn) of the polymer chain (c1) is preferably 1.2 or more and 3.0 or less.

[0077] The polymer chain (c1) has a higher glass transition temperature than the polymer chain (c2) described later. In other words, the polymer chain (c1) also plays a role as a hard component of the copolymer (C), so from the viewpoint of the handleability of the copolymer (C), the glass transition temperature of the polymer chain (c1) is preferably 70°C or higher, more preferably 80°C or higher, and even more preferably 90°C or higher. The glass transition temperature of the polymer chain (c1) is preferably 130°C or lower, more preferably 125°C or lower, and even more preferably 120°C or lower. The glass transition temperature of the polymer chain (c1) is preferably 70°C or higher and 130°C or lower. When the glass transition temperature of the polymer chain (c1) is within the above range, the copolymer (C) has excellent handleability at room temperature, and the fluidity of the resin composition during melt molding can be adjusted within a preferred range.

[0078] [Polymer chain (c2)] The polymer chain (c2) plays a role of ensuring compatibility with the polycarbonate resin (A). Therefore, the polymer chain (c2) contains 50% by mass or more and 100% by mass or less of the (meth)acrylate monomer unit represented by the general formula (1) above.

[0079] Examples of the (meth)acrylate monomer that gives the monomer unit represented by the general formula (1) include 2-methoxyethyl (meth)acrylate and methoxypolyethylene glycol (meth)acrylate. These may be used alone or in any combination of two or more. 2-Methoxyethyl (meth)acrylate is more preferable because it is easy to ensure compatibility with the polycarbonate resin (A), and 2-methoxyethyl acrylate is even more preferable because it is easy to adjust the acrylic resin (B) and the polymer chain (c2) to be completely incompatible.

[0080] From the viewpoint of compatibility with the polycarbonate resin (A), the proportion of the (meth)acrylate monomer unit represented by the general formula (1) in the polymer chain (c2) is preferably 70 mass % or more and 100 mass % or less, and more preferably 90 mass % or more and 100 mass % or less.

[0081] The polymer chain (c2) may contain a structure other than the (meth)acrylate monomer unit represented by the general formula (1) as long as the compatibility with the polycarbonate resin (A) is not impaired. The monomer that gives such a structure can be appropriately selected from those exemplified as other vinyl monomers for the acrylic resin (B).

[0082] The polymer chain (c2) has a lower glass transition temperature than the polymer chain (c1), and also plays a role in imparting appropriate flexibility to the resin composition. In order to impart appropriate flexibility to the resin composition, the glass transition temperature of the polymer chain (c2) is preferably 80° C. or lower, more preferably 60° C. or lower, and even more preferably 40° C. or lower. From the viewpoint of handleability of the copolymer (C) at room temperature, the glass transition temperature of the polymer chain (c2) is preferably -60°C or higher, more preferably -40°C or higher, and even more preferably -20°C or higher. The glass transition temperature of the polymer chain (c2) is preferably from -60°C to 80°C. When the glass transition temperature of the polymer chain (c2) is within the above range, the copolymer (C) has excellent handleability at room temperature, and the resin composition is imparted with appropriate flexibility, allowing the mechanical properties to be adjusted within preferred ranges.

[0083] [Method for producing copolymer (C)] Methods for producing copolymer (C) include a method for obtaining a block copolymer by controlled polymerization, and a method for obtaining a block-graft copolymer by copolymerizing a macromonomer with a comonomer. Here, a macromonomer is a polymer with a polymerizable functional group at one end, and is also known as a macromer. A copolymer of a macromonomer and a comonomer is called a macromonomer copolymer (hereinafter sometimes referred to as "MMCP").

[0084] Methods for synthesizing block copolymers by controlled polymerization include, for example, atom transfer radical polymerization (ATRP), reversible addition-fragmentation chain transfer (RAFT), organometallic-mediated radical polymerization (CMRP), etc. Methods for obtaining block copolymers by controlled polymerization have issues such as limitations on the types of monomers that can be applied, coloration and odor due to catalyst residues used, and reduced durability. On the other hand, a macromonomer copolymer allows efficient bonding of two or more types of polymer chains, and is therefore suitable as a method for producing the copolymer (C) used in the present invention.

[0085] [Macromonomer copolymer] When a macromonomer copolymer is used as the copolymer (C), two methods can be considered: a method in which the polymer chain (c1) is a polymer chain derived from a macromonomer, and a method in which the polymer chain (c2) is a polymer chain derived from a macromonomer. In either case, it can be used as the copolymer (C), but since the polymer chain (c2) contains the monomer unit represented by the general formula (1), its glass transition temperature is lower than that of the polymer chain (c1), and the polymer chain (c2) alone is often difficult to handle at room temperature. Therefore, a method in which the polymer chain (c1) is a polymer chain derived from a macromonomer is preferred. In particular, it is preferred that the copolymer (C) is a macromonomer copolymer composed of a polymer chain (c1) derived from a macromonomer represented by the general formula (3) described later and a polymer chain (c2) derived from a comonomer copolymerizable with the macromonomer.

[0086] In the present specification, unless otherwise specified, a unit derived from a macromonomer corresponds to the polymer chain (c1), and a unit derived from a comonomer copolymerizable with the macromonomer corresponds to the polymer chain (c2). Furthermore, in this specification, a macromonomer that is preferable as a unit constituting the polymer chain (c1) is also simply referred to as a "macromonomer", and a comonomer that is preferable as a unit constituting the polymer chain (c2) is also simply referred to as a "comonomer".

[0087] (Macromonomer) The macromonomer is a polymer having a polymerizable functional group at one end, and its structure is preferably represented by the following general formula (3).

[0088] [ka]

[0089] (In general formula (3), R 0 ~R n are each independently a hydrogen atom, an alkyl group, a cycloalkyl group, an aryl group, or a heterocyclic group. 1 ~X n are each independently a hydrogen atom or a methyl group. Z is a terminal group. n is a natural number from 2 to 10,000.

[0090] In the general formula (3), R 0 and R 1 ~R n are each independently a hydrogen atom, an alkyl group, a cycloalkyl group, an aryl group, or a heterocyclic group. The alkyl group, the cycloalkyl group, the aryl group, or the heterocyclic group may have a substituent.

[0091] The alkyl group may, for example, be a branched or linear alkyl group having a carbon number of 1 to 20. Specific examples include a methyl group, an ethyl group, an n-propyl group, and an i-propyl group. The cycloalkyl group may, for example, be a cycloalkyl group having a carbon number of 3 to 20. Specific examples include a cyclopropyl group, a cyclobutyl group, and an adamantyl group. The aryl group may, for example, be an aryl group having a carbon number of 6 to 18. Specific examples include a phenyl group and a naphthyl group. Examples of the heterocyclic group include heterocyclic groups having a carbon number of 5 to 18. Specific examples include a γ-lactone group and an ε-caprolactone group. R 0 and R 1 ~R n The substituents of each independently include a group or atom selected from the group consisting of an alkyl group, an aryl group, a carboxyl group, an alkoxycarbonyl group (-COOR'), a carbamoyl group (-CONR'R''), a cyano group, a hydroxyl group, an amino group, an amide group (-NR'R''), a halogen, an allyl group, an epoxy group, an alkoxy group (-OR'), and a group exhibiting hydrophilicity or ionicity. R' and R'' each independently include the same groups as R, except for heterocyclic groups. An example of the alkoxycarbonyl group as a substituent is a methoxycarbonyl group. Examples of the carbamoyl group as a substituent include an N-methylcarbamoyl group and an N,N-dimethylcarbamoyl group. An example of the amide group as a substituent is a dimethylamide group. Halogen as a substituent includes, for example, fluorine, chlorine, bromine and iodine. The alkoxy group as the substituent includes, for example, an alkoxy group having a carbon number of 1 to 12. A specific example is a methoxy group. Examples of the hydrophilic or ionic substituent include an alkali salt of a carboxyl group or an alkali salt of a sulfoxyl group, a poly(alkylene oxide) group such as a polyethylene oxide group or a polypropylene oxide group, and a cationic substituent such as a quaternary ammonium base.

[0092] R0 and R 1 ~R n is preferably at least one selected from an alkyl group and a cycloalkyl group, and more preferably an alkyl group. The alkyl group is preferably a methyl group, an ethyl group, an n-propyl group or an i-propyl group, and from the viewpoint of availability, a methyl group is more preferable.

[0093] In the general formula (3), X 1 ~X n are each independently a hydrogen atom or a methyl group, and a methyl group is preferable. Furthermore, from the viewpoint of ease of synthesis of the macromonomer, X 1 ~X n It is preferable that at least half of the groups are methyl groups.

[0094] In general formula (3), Z is a terminal group of the macromonomer. Examples of the terminal group of the macromonomer include a hydrogen atom and a group derived from a radical polymerization initiator, similar to the terminal groups of polymers obtained by known radical polymerization.

[0095] In the general formula (3), n is a natural number of 2 to 10,000. From the viewpoint of maintaining compatibility with the acrylic resin (B), n is preferably 10 to 1,000, and more preferably 20 to 500.

[0096] The preferred ranges of the monomers constituting the macromonomer and their ratios are the same as those described above for the "polymer chain (c1)."

[0097] The preferred ranges of the molecular weight and glass transition temperature of the macromonomer are in accordance with the ranges described above for the "polymer chain (c1)."

[0098] (Method of producing macromonomer) The macromonomer can be produced by a known method. Examples of the method for producing the macromonomer include a method using a cobalt chain transfer agent (U.S. Pat. No. 4,680,352), a method using an α-substituted unsaturated compound such as α-bromomethylstyrene as a chain transfer agent (WO 88 / 004304), a method of chemically bonding a polymerizable group (JP-A-60-133007, U.S. Pat. No. 5,147,952), and a method using thermal decomposition (JP-A-11-240854). Among these, the method for producing the macromonomer is preferably a method using a cobalt chain transfer agent, since it involves fewer production steps and uses a catalyst with a high chain transfer constant.

[0099] (Comonomers copolymerizable with macromonomers) The comonomer is not particularly limited as long as it is copolymerizable with the macromonomer, and various polymerizable monomers can be used as necessary. For example, (Meth)acrylates such as methyl acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-lauryl (meth)acrylate, n-stearyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, phenoxyethyl (meth)acrylate, and methoxypolyethylene glycol (meth)acrylate; hydroxyl group-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and glycerol (meth)acrylate; Carboxy group-containing vinyl monomers such as (meth)acrylic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxypropyl phthalic acid, 2-(meth)acryloyloxyethyl maleic acid, 2-(meth)acryloyloxypropyl maleic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxypropyl succinic acid, crotonic acid, fumaric acid, maleic acid, itaconic acid, monomethyl maleate, and monomethyl itaconate; Vinyl monomers containing an acid anhydride group, such as maleic anhydride and itaconic anhydride; Epoxy group-containing vinyl monomers such as glycidyl (meth)acrylate, glycidyl α-ethyl acrylate, and 3,4-epoxybutyl (meth)acrylate; Amino group-containing (meth)acrylate vinyl monomers such as dimethylaminoethyl (meth)acrylate and diethylaminoethyl (meth)acrylate; Vinyl monomers containing an amide group, such as (meth)acrylamide, Nt-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, diacetone acrylamide, maleic acid amide, and maleimide; Vinyl monomers such as styrene, α-methylstyrene, vinyltoluene, (meth)acrylonitrile, vinyl chloride, vinyl acetate, and vinyl propionate; etc. These may be used alone or in any combination of two or more.

[0100] Among these, examples of monomers preferable as comonomers and the preferable content thereof are in accordance with the ranges described above for "polymer chain (c2)."

[0101] In particular, when a macromonomer copolymer is used as the copolymer (C), it is preferable to use a combination of methacrylate and acrylate among the monomers listed above. From the viewpoint of reactivity between the macromonomer and the comonomer, acrylate is more preferred than methacrylate because of its higher reactivity, but if the amount of acrylate increases too much, the glass transition temperature of the polymer composed of the comonomer decreases, which may impair the handleability of the macromonomer copolymer at room temperature. By using a methacrylate and an acrylate in combination, it is possible to appropriately adjust the reactivity with the macromonomer and the handleability at room temperature.

[0102] When methacrylate and acrylate are used in combination as comonomers, the mass ratio of methacrylate / acrylate is preferably in the range of 0 / 100 to 70 / 30, more preferably in the range of 20 / 80 to 60 / 40, and even more preferably in the range of 30 / 70 to 50 / 50. When the mass ratio of methacrylate / acrylate is within the above range, the reactivity of the macromonomer and the comonomer is high, and the amount of unreacted macromonomer that may be generated during the preparation of the macromonomer copolymer can be minimized, thereby maximizing the effect of the copolymer (C).

[0103] The preferred range of the glass transition temperature of the polymer derived from the comonomer is the same as the range described above for the "polymer chain (c2)".

[0104] [Method of manufacturing macromonomer copolymer] The method for producing a macromonomer copolymer includes a step of polymerizing a macromonomer and a comonomer.

[0105] The method for polymerizing the macromonomer and the comonomer is not particularly limited, and various methods such as solution polymerization, suspension polymerization, emulsion polymerization, bulk polymerization, etc. can be used. Aqueous polymerization such as suspension polymerization or emulsion polymerization is preferred because it is easy to control the heat generated by polymerization and has excellent productivity, and suspension polymerization is more preferred because the operation for recovering the polymer is simpler.

[0106] [Resin composition] In the resin composition of the present invention, the blending amount of the copolymer (C) is from 0.5% by mass to 9.5% by mass based on 100% by mass in total of the polycarbonate resin (A) and the acrylic resin (B). The blending amount of the copolymer (C) is more preferably 0.8% by mass or more, and even more preferably 1% by mass or more, and more preferably 7% by mass or less, and even more preferably 5% by mass or less.

[0107] The proportion of the polycarbonate resin (A) in the resin composition of the present invention is preferably 50% by mass or more, more preferably 55% by mass or more, and even more preferably 60% by mass or more. The proportion of the polycarbonate resin (A) in the resin composition of the present invention is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less. The proportion of the polycarbonate resin (A) in the resin composition of the present invention is preferably 50% by mass or more and 90% by mass or less.

[0108] The proportion of the acrylic resin (B) in the resin composition of the present invention is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more. The proportion of the acrylic resin (B) in the resin composition of the present invention is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less. The proportion of the acrylic resin (B) in the resin composition of the present invention is preferably 10% by mass or more and 50% by mass or less.

[0109] By setting the blending ratio of the resin composition of the present invention within the above range, a composite resin material that is less susceptible to delamination and has excellent appearance can be realized, and various required physical properties such as mechanical properties and heat resistance can be balanced at a high level.

[0110] The resin composition of the present invention may contain, in addition to the polycarbonate resin (A), the acrylic resin (B), and the copolymer (C), another resin component (D) as long as the effects of the present invention are not impaired. Examples of other resin components (D) include synthetic resins such as aromatic polycarbonate, aromatic polyester, aliphatic polyester, polyamide, polystyrene, polyolefin, amorphous polyolefin, acrylonitrile-butadiene-styrene copolymer (ABS resin), and acrylonitrile-styrene copolymer (AS resin); elastomers such as acrylic rubber, butadiene rubber, and silicone rubber; and biodegradable resins such as polylactic acid and polybutylene succinate. Among these, aromatic polycarbonate, acrylonitrile-butadiene-styrene copolymer (ABS resin), and acrylonitrile-styrene copolymer (AS resin) are preferred, and acrylonitrile-butadiene-styrene copolymer (ABS resin) and acrylonitrile-styrene copolymer (AS resin) are more preferred, because they are compatible with polycarbonate resin (A) or acrylic resin (B) and can easily adjust the refractive index, fluidity, heat resistance, and the like of each component. These may be used alone or in combination of two or more.

[0111] The resin composition of the present invention may contain other components such as additives in addition to the polycarbonate resin (A), the acrylic resin (B), and the copolymer (C) as long as the effects of the present invention are not impaired. Examples of the additives include antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, fillers and other fillers, neutralizing agents, lubricants, antifogging agents, antiblocking agents, slip agents, dispersants, colorants, flame retardants, antistatic agents, conductivity imparting agents, crosslinking agents, crosslinking assistants, metal deactivators, molecular weight regulators, antibacterial agents, antifungal materials, fluorescent brightening agents, organic diffusing agents, and inorganic diffusing agents.

[0112] [Method of producing resin composition] The resin composition of the present invention can be produced, for example, by a method of mechanically melt-kneading the above-mentioned components constituting the resin composition. The melt kneader may be a single screw extruder, a twin screw extruder, a Brabender, a Banbury mixer, a kneader blender, a roll mill, etc. In the melt kneading, the components may be kneaded all at once, or a multi-stage division kneading method may be used in which an arbitrary component is kneaded and then the remaining components are added and kneaded. Among these, a method in which each component is continuously charged into a twin-screw extruder equipped with a vacuum vent to continuously obtain a resin composition is preferred from the viewpoints of productivity and uniformity of quality. The kneading temperature is preferably 160° C. or higher, more preferably 180° C. or higher, and even more preferably 200° C. or higher. The kneading temperature is preferably 300° C. or lower, more preferably 280° C. or lower, and even more preferably 260° C. or lower. The kneading temperature is preferably 160° C. or higher and 300° C. or lower. If the kneading temperature is within this range, the resin composition can be mixed while suppressing thermal deterioration due to retention in the kneader or heat generation due to shear.

[0113] [Characteristics of resin composition] (transparency) The resin composition of the present invention preferably has a total light transmittance of 80% or more, more preferably 85% or more, and even more preferably 90% or more, as measured by the method described below. The haze value, as measured by the method described below, is preferably 50% or less, more preferably 30% or less, and even more preferably 10% or less. If the haze value is within the above range, the molded article made of the resin composition of the present invention has transparency and can be applied to applications requiring visible light transmittance, such as lighting covers and glass replacements. (Mechanical properties) The resin composition of the present invention preferably has a yield stress of 65 MPa or more, more preferably 70 MPa or more, and even more preferably 75 MPa or more, as evaluated by the method described below. The breaking elongation is preferably 10% or more, more preferably 12% or more, and even more preferably 15% or more. Within the above range, a molded article made of the resin composition of the present invention has hardness and appropriate mechanical properties, and can be used for applications such as housings and glass replacements. (shock resistance) The resin composition of the present invention has a Charpy impact value of 3.0 kJ / m as measured by the method described below. 2 It is preferable that the concentration is 4.0 kJ / m or more. 2 More preferably, 5.0 kJ / m or more. 2 When the content is within the above range, the molded article made of the resin composition of the present invention has appropriate impact resistance and is less likely to break in the usage environment. (Delamination) In the resin composition of the present invention, in terms of suppression of delamination as evaluated by the method described below, it is preferable that the number of sheets on which delamination marks were confirmed is 4 or less out of 10 sheets, and more preferably 2 or less out of 10 sheets.

[0114] [Molded body] The resin composition of the present invention can be processed into various molded articles by molding methods such as injection molding (insert molding, two-color molding, sandwich molding, gas injection molding, etc.), extrusion molding, inflation molding, T-die film molding, laminate molding, blow molding, hollow molding, compression molding, and calendar molding. The molded article of the present invention is made of the resin composition of the present invention. The shape of the molded article is not particularly limited, and examples thereof include a sheet, film, plate, particle, lump, fiber, rod, porous body, foam, etc. EXAMPLES

[0115] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. In the following description, "parts" and "%" mean "parts by mass" and "% by mass". [Evaluation method] (1) Molecular weight and molecular weight distribution of copolymer The mass average molecular weight (Mw) and number average molecular weight (Mn) were measured using gel permeation chromatography (GPC) (manufactured by Tosoh Corporation, trade name: HLC-8420) under the following conditions. Column: TSK GUARD COLUMN SUPER HZ-L (DI 4.6 mm x 35 mm) and two TSK-GEL SUPER HZM-N (DI 6.0 mm x 150 mm) connected in series. Eluent:THF Measurement temperature: 40℃ Flow rate: 0.6mL / min The Mw and Mn were determined using a calibration curve prepared using four types of polymethyl methacrylate having peak top molecular weights of 1590, 10290, 55600 and 141500, manufactured by Polymer Laboratories.

[0116] (2) Glass transition temperature of copolymer The glass transition temperature was measured using a differential scanning calorimeter DSC6220 (manufactured by SII Nano Technology Co., Ltd.). Approximately 10 mg of the copolymer was placed in an aluminum pan manufactured by the same company and sealed. Measurement was started at 30°C under a nitrogen gas flow of 40 mL / min, and the temperature was raised to 180°C at a rate of 10°C / min. The sample was then held at 180°C for 5 minutes and cooled to -50°C at a rate of 10°C / min. The sample was held at -50°C for 5 minutes, and then heated again to 180°C at a rate of 10°C / min. From the DSC data during this second heating, the extrapolated glass transition onset temperature, which is the temperature at the intersection of a straight line extending the low-temperature baseline to the high-temperature side and a tangent drawn at the point where the gradient of the curve of the step-like change in the glass transition is maximum, was calculated and used as the glass transition temperature.

[0117] (3) Transparency The resin composition was injection molded by the method described below to obtain a plate-shaped test piece having a thickness of 2 mm. The total light transmittance (TT) and haze (Hz) of the obtained test piece were measured using a haze meter NDH4000 (manufactured by Nippon Denshoku Industries Co., Ltd.) under a D65 light source in accordance with JIS K7136.

[0118] (4) Mechanical properties The resin composition was injection molded by the method described below to obtain a dumbbell-shaped test piece having a thickness of 4 mm and a gauge length of 115 mm. Using the obtained test piece, a tensile test was performed in accordance with JIS K7139 using an autograph AG-Xplus10kN (manufactured by Shimadzu Corporation) with a chuck length of 115 mm. The tensile test was performed at room temperature of 23°C and a speed of 20 mm / min, and the yield stress and the breaking elongation were obtained from the obtained stress-strain curve. (5) Impact resistance The resin composition was injection molded by the method described below to obtain test pieces for Charpy impact testing in accordance with JIS K7111. A V notch (notch tip diameter r = 0.25) was post-processed in the center of the test piece using a notching machine A-4 (manufactured by Toyo Seiki Seisakusho Co., Ltd.), and a test was performed edgewise on five pieces at a time using a Charpy impact tester DG-CP (manufactured by Toyo Seiki Seisakusho Co., Ltd.) using a 1J hammer. The average value of the obtained impact values ​​was calculated and used as an index of impact resistance.

[0119] (6) Evaluation of delamination The resin composition was injection molded as described below, and when it was removed from the mold, a plate-shaped test piece having a thickness of 2 mm was cut with nippers at the boundary between the runner and the gate and taken out. For multiple test pieces, the vicinity of the cut was visually observed to check for the presence or absence of white interlayer peeling marks inside the plate, and the test pieces were evaluated according to the following criteria. (Evaluation Criteria) ○: Traces of delamination were found on only 2 or fewer sheets out of 10. △: Traces of delamination were observed on 3 to 4 sheets out of 10 sheets. ×: Traces of delamination were found on 5 or more of the 10 sheets.

[0120] [Raw materials used] The abbreviations and manufacturers of the compounds used in the following Examples and Production Examples are as follows.

[0121] MMA: Methyl methacrylate (manufactured by Mitsubishi Chemical Corporation) ·MA: Methyl acrylate (manufactured by Mitsubishi Chemical Corporation) ·MEMA: 2-Methoxyethyl methacrylate (manufactured by Mitsubishi Chemical Corporation) MEA: 2-Methoxyethyl acrylate (Mitsubishi Chemical Corporation) HEMA: 2-hydroxyethyl methacrylate (manufactured by Mitsubishi Chemical Corporation) PhMA: Phenyl methacrylate (manufactured by Mitsubishi Chemical Corporation) BA: n-Butyl acrylate (Mitsubishi Chemical Corporation) St: Styrene (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) AMBN: 2,2'-azobis(2-methylbutyronitrile) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), product name V59 Perocta O: 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate (NOF Corporation) Sodium sulfate (Tokyo Chemical Industry Co., Ltd.) 1-OcSH: 1-Octanethiol (Tokyo Chemical Industry Co., Ltd.) Cobalt(II) acetate tetrahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) Diphenylglyoxime (Tokyo Chemical Industry Co., Ltd., EP grade) Boron trifluoride diethyl ether complex (Tokyo Chemical Industry Co., Ltd., EP grade) Dispersants An aqueous dispersant solution having a solid content of 10% by mass was prepared by the method described in WO 2022 / 114157 and used as a dispersant for suspension polymerization.

[0122] <Production Example 1> Synthesis of chain transfer agent (1) In a synthesis apparatus equipped with a stirrer, 2.00 g (8.03 mmol) of cobalt (II) acetate tetrahydrate, 3.86 g (16.1 mmol) of diphenylglyoxime, and 100 mL of diethyl ether that had been deoxygenated in advance by nitrogen bubbling were placed under a nitrogen atmosphere, and the mixture was stirred at room temperature for 2 hours. Next, 20 mL of boron trifluoride diethyl ether complex was added and stirred for another 6 hours. The obtained product was filtered, the solid was washed with diethyl ether, and dried at 100 mPa or less for 12 hours to obtain 5.02 g (7.93 mmol, yield 99 mass%) of a brown solid chain transfer agent (1).

[0123] <Manufacturing example 2> MM-1 In a separable flask equipped with a cooling tube, 145 parts of deionized water, 0.13 parts of sodium sulfate, and 0.26 parts of a dispersing agent were mixed to prepare an aqueous dispersion for suspension polymerization. Next, 95 parts of MMA and 5 parts of MA as monomers, 0.0016 parts (16 ppm by mass) of the chain transfer agent (1) synthesized in Production Example 1, and 0.1 part of Perocta O as a radical polymerization initiator were mixed to obtain a monomer mixture. The obtained monomer mixture was added to the aqueous dispersion for suspension polymerization, and then the stirring speed was increased while the atmosphere inside the separable flask was replaced with nitrogen by nitrogen bubbling to obtain a monomer dispersion. The monomer dispersion was heated to 80° C. and held for 4 hours, and then heated to 92° C. and held for 2 hours. The resulting polymer suspension was cooled to below 40° C., filtered through a filter cloth, and the filtrate was washed with deionized water and dried at 40° C. for 16 hours to obtain macromonomer MM-1. The relative molecular weight of the obtained MM-1 in terms of PMMA (polymethyl methacrylate) was measured by GPC, and the mass average molecular weight (M w ) is 33,000, and the number average molecular weight (M n ) is 18,000, and the molecular weight distribution (M w / M n ) was 1.83. The evaluation results are shown in Table 1.

[0124] <Manufacturing example 3> MM-2 A macromonomer MM-2 was obtained in the same manner as in Production Example 2, except that the charged composition ratio of the macromonomer was changed according to Table 1. Thereafter, the relative molecular weight was measured in the same manner as in Production Example 2. The evaluation results are shown in Table 1.

[0125] <Manufacturing example 4> MM-3 Macromonomer MM-3 was obtained in the same manner as in Production Example 2, except that the charged composition ratio of the macromonomer was changed according to Table 1. Thereafter, the relative molecular weight was measured in the same manner as in Production Example 2. The evaluation results are shown in Table 1.

[0126] <Manufacturing example 5> MM-4 A macromonomer MM-4 was obtained in the same manner as in Production Example 2, except that the charged composition ratio of the macromonomer was changed according to Table 1. Thereafter, the relative molecular weight was measured in the same manner as in Production Example 2. The evaluation results are shown in Table 1.

[0127] [Table 1]

[0128] <Production Example 6> MMCP-1 An aqueous dispersion for suspension polymerization was prepared by mixing 200 parts of deionized water, 0.1 part of sodium sulfate, and 2.62 parts of a dispersing agent. In a separable flask equipped with a cooling tube, 40 parts of MM-1 synthesized in Production Example 2 as a macromonomer and 60 parts of MEA as a comonomer raw material were added and mixed, and the mixture was heated to 50° C. with stirring to obtain a raw syrup. After cooling the raw syrup to below 40°C, 0.2 parts of AMBN was dissolved as a radical polymerization initiator, and then the aqueous dispersion for suspension polymerization was added. The atmosphere in the separable flask was replaced with nitrogen by bubbling with nitrogen, and the stirring speed was increased to obtain a syrup dispersion. The syrup dispersion was heated to 75° C. and maintained for 3 hours, and then heated to 85° C. and maintained for 30 minutes to complete the polymerization, thereby obtaining a polymer suspension. After the suspension was cooled to below 40° C., the polymer suspension was filtered through a filter cloth, the filtrate was washed with deionized water, and dried at 40° C. for 16 hours to obtain macromonomer copolymer MMCP-1. The relative molecular weight of the obtained MMCP-1 in terms of PMMA was measured by GPC, and the mass average molecular weight (M w ) is 298,000, and the number average molecular weight (M n ) is 57,700, and the molecular weight distribution (M w / M n ) was 5.16. When the glass transition temperature was measured by DSC, two temperatures were detected: -30°C and 100°C. The results are shown in Table 2.

[0129] <Production Examples 7-13> MMCP-2 to MMCP-8 A macromonomer copolymer was obtained in the same manner as in Production Example 6, except that the macromonomer and comonomer were changed according to Table 2. Thereafter, the relative molecular weight and the glass transition temperature were measured in the same manner as in Production Example 6. The evaluation results are shown in Table 2. In addition, in the case of MMCP-4 in Production Example 9, the product contained gel, so that the relative molecular weight could not be measured.

[0130] [Table 2]

[0131] [Polycarbonate resin] PC-1: Isosorbide-containing PC resin Durabio D7340R (manufactured by Mitsubishi Chemical Corporation) [Acrylic resin] PMMA-1: PMMA resin Acrylates VH001 (Mitsubishi Chemical Corporation) [Copolymer] MMCP-1: MM-1·MEA copolymer synthesized in Example 6 MMCP-2: MM-2·MEMA·MEA copolymer synthesized in Production Example 7 MMCP-3: MM-2·MEMA·MEA·HEMA copolymer synthesized in Example 8 MMCP-4: MM-2·MEMA·MEA copolymer synthesized in Example 9 MMCP-5: MM-2·MEMA·MEA copolymer synthesized in Example 10 MMCP-6: MM-2·MEMA·MEA copolymer synthesized in Example 11 MMCP-7: MM-3·MEMA·MEA copolymer synthesized in Example 12 MMCP-8: MM-4·St·BA copolymer synthesized in Example 13 [Other resin components] AS-1: AS resin Sunrex SAN-C (manufactured by Techno UMG Co., Ltd.)

[0132] <Example 1> [Production of resin composition] Polycarbonate resin PC-1 and acrylic resin PMMA-1 were used, and each resin was dried at 80°C for 12 hours or more. Then, they were dry-blended with the copolymer MMCP-1 obtained in Production Example 6 in a mass ratio of 60:40:5. The mixture was then melt-kneaded using a φ35 mm twin-screw extruder (TEM-35B manufactured by Shibaura Machine Co., Ltd.) at a cylinder temperature of 240°C to obtain a pellet-shaped resin composition. The obtained resin composition in the form of pellets was molded by an electric injection molding machine (SE100EV-A manufactured by Sumitomo Heavy Industries, Ltd.) to obtain a molded body having a thickness of 2 mm, a dumbbell-shaped molded body, and a molded body for Charpy tests. When the test specimens were separated from the runners, an evaluation of delamination was carried out. The obtained test specimens were then subjected to a transparency evaluation at 23°C, a tensile test, and an impact resistance test. The evaluation results are shown in Table 3.

[0133] <Examples 2 to 10, Comparative Examples 1 to 4> Molded pieces for various evaluations were obtained in the same manner as in Example 1, except that the formulation of the resin composition was changed according to Table 3. Thereafter, each evaluation was carried out in the same manner as in Example 1. The evaluation results are shown in Table 3.

[0134] [Table 3]

[0135] From Examples 1 and 2, it was found that when MMCP-1 and MMCP-2 having a polymer chain (c1) derived from a macromonomer and a polymer chain (c2) derived from a comonomer containing a monomer unit represented by the general formula (1) were used as copolymers, molded articles with excellent appearance and less delamination were obtained. In addition, it was found that these molded articles had high total light transmittance and were transparent, and also had relatively high tensile yield stress and Charpy impact value, and had appropriate mechanical properties.

[0136] From Comparative Example 1, it was found that when none of MMCP-1 to MMCP-8 was included as a copolymer, delamination was likely to occur, the appearance of the molded article was poor, and the Charpy impact value was low, resulting in a molded article with poor impact resistance.

[0137] From Examples 3 and 4, it was found that even when MMCP-3, in which HEMA was introduced as a monomer unit not corresponding to the general formula (1) as the composition of the polymer chain (c2) derived from a comonomer, or MMCP-4, in which the ratio of the polymer chain (c1) derived from a macromonomer and the polymer chain (c2) derived from a comonomer was changed, a molded article that is less likely to undergo delamination and has excellent appearance was obtained. That is, it was found that a molded article that is less likely to undergo delamination and has excellent appearance was obtained as long as the amount of the monomer unit represented by the general formula (1) and the ratio of the polymer chain (c1) and the polymer chain (c2) satisfied the preferred range.

[0138] From Example 5 and Comparative Example 2, it was found that even when an AS resin was used in combination with copolymer (C) as an ingredient other than copolymer (C), the presence of copolymer (C) made it difficult for delamination to occur, resulting in an excellent appearance, and furthermore, as a result of the balance of the refractive indices of the polymer components constituting the resin composition, a molded product with extremely excellent transparency could be obtained.

[0139] From Examples 6 and 7, it was found that, so long as the blending amount of the copolymer (C) satisfies the predetermined range, a molded article which is less susceptible to delamination and has excellent appearance can be obtained.

[0140] It was found from Comparative Example 3 that when the blending amount of copolymer (C) was out of the predetermined range, delamination was likely to occur and a molded article with poor appearance was obtained. This is presumably because, when the blending amount of copolymer (C) is increased, copolymer (C) aggregates in a micelle form, and the effect of improving the interfacial strength between the polycarbonate resin and the acrylic resin is reduced.

[0141] From Examples 8 to 9, it was found that even when using a copolymer (C) with a changed methacrylate / acrylate ratio, as long as the mass average molecular weight (Mw) satisfies a predetermined range, delamination is unlikely to occur and a molded product with excellent appearance can be obtained. The mass average molecular weight (Mw) of the obtained copolymer (C) tends to decrease as the methacrylate ratio increases. This is presumably because acrylate has a higher reactivity with the macromonomer than methacrylate, and the higher the methacrylate ratio, the less likely it is to progress to high molecular weight.

[0142] From Example 10, it was found that, when the mass average molecular weight (Mw) of the polymer chain (c1) derived from the macromonomer satisfies the preferred range, it is possible to obtain a molded article which is less susceptible to delamination and has excellent appearance.

[0143] From Comparative Example 4, it was found that when MMCP-8 not containing the monomer unit represented by the general formula (1) was used as a resin composition, the molded product was easily damaged in appearance due to delamination. This is presumably due to the low compatibility between the polymer chain (c2) derived from the comonomer and the polycarbonate resin, which resulted in a decrease in the interfacial strength between the polycarbonate resin and the acrylic resin. [Industrial Applicability]

[0144] According to the present invention, since the occurrence of delamination is suppressed when a polycarbonate resin and an acrylic resin are composited, a resin composition in which the two are composited without impairing the appearance can be provided. The resin composition of the present invention, when molded, has excellent weather resistance and optical properties in addition to transparency and mechanical properties, and is therefore suitable for use in interior and exterior components of automobiles, building materials used outdoors (lighting covers, carports, highway soundproofing walls, etc.), display front panels, housings for electric and electronic devices, etc.

Claims

1. The composition comprises a polycarbonate resin (A), an acrylic resin (B), and a copolymer (C), the blending amount of the copolymer (C) is 0.5% by mass or more and 9.5% by mass or less with respect to 100% by mass of the total of the polycarbonate resin (A) and the acrylic resin (B); The resin composition, wherein the copolymer (C) is a copolymer having a polymer chain (c1) and a polymer chain (c2) shown below. Polymer chain (c1): A polymer chain that is compatible with the acrylic resin (B). Polymer chain (c2): A polymer chain containing 50% by mass or more and 100% by mass or less of a (meth)acrylate monomer unit represented by the following general formula (1): 【Chemistry 1】 (In general formula (1), Y represents a hydrogen atom or a methyl group, and m represents a natural number from 1 to 30.)

2. The resin composition according to claim 1, wherein the polymer chain (c1) contains 80% by mass or more and 100% by mass or less of methyl methacrylate monomer units.

3. The resin composition according to claim 1 or 2, wherein the polycarbonate resin (A) has a structural unit derived from a compound represented by the following formula (2): 【Chemistry 2】

4. The resin composition according to claim 1 or 2, wherein the acrylic resin (B) contains 80% by mass or more and 100% by mass or less of methyl methacrylate monomer units.

5. The resin composition according to claim 1 or 2, wherein the copolymer (C) is a block copolymer and / or a graft copolymer.

6. The resin composition according to claim 1 or 2, wherein the copolymer (C) is a macromonomer copolymer composed of a polymer chain (c1) derived from a macromonomer represented by the following general formula (3) and a polymer chain (c2) derived from a comonomer copolymerizable with the macromonomer: 【Chemistry 3】 (In general formula (3), R 0 ~R n are each independently a hydrogen atom, an alkyl group, a cycloalkyl group, an aryl group, or a heterocyclic group. 1 ~X n are each independently a hydrogen atom or a methyl group; Z is a terminal group; and n is a natural number from 2 to 10,000.

7. A molded article comprising the resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Polycarbonate resin composition and molded article

    JP2021088651A

  • Polycarbonate and process for producing the same

    WO2004111106A1

  • Polycarbonate copolymer and process for production thereof

    WO2007148604A1