Block copolymer and organic film

A block copolymer with an organic semiconductor and adhesive block connected via a linking group addresses the challenge of complex manufacturing processes in organic semiconductor devices, enhancing adhesion and stability without complicating the process.

JP2024132926APending Publication Date: 2024-10-01MITSUBISHI CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024031504
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-14
Filing Date
2024-03-01
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing methods for improving interlayer adhesion in organic semiconductor devices, such as organic transistors, involve complex manufacturing processes that can lead to device deterioration if not executed perfectly, and there is a need for a simpler and more reliable method to enhance adhesion between organic semiconductor layers and other materials.

Method used

A block copolymer is developed, combining an organic semiconductor block with a π-conjugated polymer skeleton and an adhesive block with a vinyl polymer skeleton, connected via a linking group, which allows for improved adhesion without complicating the manufacturing process.

Benefits of technology

The block copolymer enhances adhesion between organic semiconductor layers and other materials, simplifying the manufacturing process and improving the reliability and stability of the devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132926000001
    Figure 2024132926000001
  • Figure 2024132926000002
    Figure 2024132926000002
  • Figure 2024132926000003
    Figure 2024132926000003
Patent Text Reader

Abstract

To provide an organic semiconductor material suitable for improving adhesiveness between an organic semiconductor material and different materials even without performing a device fabrication process which is more complicated than the conventional process.SOLUTION: There is provided a block copolymer having semiconductor properties and adhesive properties in which an organic semiconductor block having a π-conjugated polymer backbone and an adhesive block having a vinyl polymer backbone are bonded via a linking group. There is provided an organic film using the block copolymer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an organic semiconductor block copolymer having adhesive properties, which is a block copolymer in which an organic semiconductor block having a π-conjugated polymer skeleton and an adhesive block having a vinyl polymer skeleton are bonded via a linking group. The present invention also relates to an organic film using this block copolymer. [Background technology]

[0002] Research into organic electronic devices that can be made large in area and have features such as ultralightness and flexibility has become active, and the development of devices such as organic transistors and organic electroluminescence (EL) devices has attracted attention. In the development of the above devices with a layered structure, improving the adhesion between layers and resolving poor contact is a challenge in improving the performance and durability of the devices. In particular, there is a demand for improving the interlayer adhesion between the organic semiconductor layer and the layer of a different material due to the lack of adhesion of the organic semiconductor material, and studies are being conducted to improve this.

[0003] Non-Patent Document 1 reports that an organic transistor having an electrode / organic semiconductor layer with excellent adhesion is produced by patterning an electrode material on a substrate, preparing a polymethyl methacrylate layer and a polyvinyl alcohol layer, peeling these off from the substrate, attaching the electrode film to an organic semiconductor, and dissolving and removing the polyvinyl alcohol layer with warm water. [Prior art documents] [Non-patent literature]

[0004] [Non-Patent Document 1] Sci.Rep.2020,10,4702. Summary of the Invention [Problem to be solved by the invention]

[0005] However, the device fabrication process in the method described in Non-Patent Document 1 is more complicated than conventional processes. In addition, if polyvinyl alcohol, hot water, etc. are not sufficiently removed in the fabrication process, the device characteristics and long-term stability may be deteriorated.

[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide an organic semiconductor material that is suitable for improving adhesion between an organic semiconductor material and a different material, without performing a device fabrication process that is more complicated than conventional processes. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that the above problems can be solved by a block copolymer in which an organic semiconductor block having a π-conjugated polymer skeleton and an adhesive block having a vinyl polymer skeleton are bonded via a linking group.

[0008] The present invention has been achieved based on these findings, and the gist of the present invention is as follows.

[0009] [1] A block copolymer having semiconducting properties and adhesive properties, characterized in that it comprises an organic semiconductor block having a π-conjugated polymer skeleton and an adhesive block having a vinyl polymer skeleton bonded via a linking group.

[0010] [2] The block copolymer according to [1], wherein the organic semiconductor block is represented by the following formula (I) or the following formula (IV):

[0011] [ka]

[0012] In formula (I), A represents a monomer unit having a thiophene ring which may have a substituent, or a monomer unit having a triarylamine skeleton which may have a substituent. R1 represents a direct bond, a linear or branched alkylene group, or an arylene group which may have a substituent, in which a methylene group (-CH2-) in the alkylene group may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). R2 represents a hydrogen atom, a linear or branched alkyl group, a linear or branched alkoxy group, or an aryl group which may have a substituent. n is a natural number greater than or equal to 2. The wavy line represents a bond to the linking group.

[0013] [ka]

[0014] In formula (IV), A1 represents a monomer unit having a thiophene ring which may have a substituent, or a monomer unit having a triarylamine skeleton which may have a substituent. R 11 and R 21 each independently represents a direct bond, a linear or branched alkylene group, or an arylene group which may have a substituent. A methylene group (-CH-) in the alkylene group may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). n is a natural number greater than or equal to 2. The wavy line represents a bond to the linking group.

[0015] [3] The block copolymer according to [2], wherein A in the formula (I) is a thiophene unit having an alkyl group as a substituent.

[0016] [4] The block copolymer according to [2], wherein A1 in the formula (IV) is a triarylamine unit having an alkyl group as a substituent.

[0017] [5] The block copolymer according to any one of [1] to [4], wherein the adhesive block is represented by the following formula (II): [ka]

[0018] In formula (II), R3 represents a hydrogen atom or a linear or branched alkyl group. R4 represents a linear or branched alkyl group, wherein a methylene group (-CH2-) in the alkyl group may be substituted with an oxygen atom (-O-). R5 represents a hydrogen atom or a linear or branched alkyl group, in which a methylene group (-CH2-) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). R6 represents a direct bond or a linear or branched alkylene group, in which a methylene group (-CH2-) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). m is a natural number greater than or equal to 2. The wavy line represents a bond to the linking group.

[0019] [6] The block copolymer according to any one of [1] to [4], wherein the adhesive block is represented by the following formula (III):

[0020] [ka]

[0021] (In formula (III), R7~R 11 Each independently represents a hydrogen atom or a hydroxyl group. 11 At least one of the groups is a hydroxyl group. R 12represents a hydrogen atom or a linear or branched alkyl group, in which a methylene group (-CH-) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). R 13 represents a direct bond or a linear or branched alkylene group, in which a methylene group (-CH-) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). k is a natural number greater than or equal to 2. The wavy line represents a bond to the linking group.

[0022] [7] The block copolymer according to any one of [1] to [6], wherein the linking group is a divalent group of a triazole ring.

[0023] [8] An organic film using the block copolymer according to any one of [1] to [7]. Effect of the Invention

[0024] Since the block copolymer of the present invention has an adhesive block, it itself has adhesiveness to different types of materials, making it possible to reduce the number of steps in a device fabrication process and to improve the reliability of the fabrication process for the produced device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The following describes in detail the form for carrying out the present invention. However, the following description of the constituent elements is a representative example of an embodiment of the present invention, and the present invention is not limited to these contents.

[0026] In the present invention, the arylene group is an arylene group in a broad sense meaning both an arylene group which is an aromatic hydrocarbon ring linking group and a heteroarylene group which is an aromatic heterocyclic ring linking group. The same applies to an aryl group.

[0027] <Block copolymer> The block copolymer of the present invention is a block copolymer having semiconductor properties and adhesive properties, and is a block copolymer in which an organic semiconductor block having a π-conjugated polymer skeleton and an adhesive block having a vinyl polymer skeleton are bonded via a linking group. The block copolymer of the present invention has both excellent semiconductor properties due to the organic semiconductor block and adhesive properties due to the adhesive block. The blocks constituting the block copolymer are not particularly limited as long as they are a combination that causes phase separation, but it is preferable that the blocks are incompatible with each other. By phase-separating the organic semiconductor block and the adhesive block at the nano level, it is possible to suppress the aggregation of the organic semiconductor block and the adhesive block. Therefore, the block copolymer of the present invention can obtain adhesive properties derived from the adhesive block.

[0028] The total content of the organic semiconductor block and the adhesive block in the block copolymer of the present invention is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and particularly preferably 80% by mass or more, and the upper limit is preferably 90% by mass or less from the viewpoint of securing linking groups. The block copolymer of the present invention may contain only one type of organic semiconductor block, or may contain two or more types of organic semiconductor blocks having different types of substituents in the following formula (I). It may contain only one type, or may contain two or more types.

[0029] <Organic semiconductor block> The organic semiconductor block is preferably a block containing a monomer unit containing a thiophene ring or a triarylamine skeleton as a π-conjugated polymer skeleton, and is preferably a block represented by the following formula (I) or the following formula (IV).

[0030] [ka]

[0031] In formula (I), A represents a monomer unit having a thiophene ring which may have a substituent, or a monomer unit having a triarylamine skeleton which may have a substituent. R1 represents a direct bond, a linear or branched alkylene group, or an arylene group which may have a substituent, in which a methylene group (-CH2-) in the alkylene group may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). R2 represents a hydrogen atom, a linear or branched alkyl group, a linear or branched alkoxy group, or an aryl group which may have a substituent. n is a natural number greater than or equal to 2. The wavy line represents a bond to the linking group.

[0032] [ka]

[0033] In formula (IV), A1 represents a monomer unit having a thiophene ring which may have a substituent, or a monomer unit having a triarylamine skeleton which may have a substituent. R 11 and R 21 each independently represents a direct bond, a linear or branched alkylene group, or an arylene group which may have a substituent. A methylene group (-CH-) in the alkylene group may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). n is a natural number greater than or equal to 2. The wavy line represents a bond to the linking group.

[0034] When the organic semiconductor block according to the present invention is a block represented by the above formula (I), the block copolymer according to the present invention is usually configured as a block copolymer having one organic semiconductor block and one adhesive block. When the organic semiconductor block according to the present invention is a block represented by the above formula (IV), the block copolymer according to the present invention is usually configured as a block copolymer having one organic semiconductor block interposed between two adhesive blocks.

[0035] [A, A1] (Monomer Unit Having a Thiophene Ring Which May Be Substituted) The thiophene-based compound having a thiophene ring constituting the monomer unit containing a thiophene ring which may have a substituent of A and A1 is not particularly limited as long as it has one or more thiophene rings.

[0036] The thiophene compound may have a monocyclic thiophene ring, may have a condensed thiophene ring, or may have two or more thiophene rings bonded together via a direct bond or other linking group. In the case of a condensed ring, thiophene rings may be condensed together, or a thiophene ring may be condensed with another ring such as a benzene ring. Fused rings or a condensed ring and a thiophene ring may be condensed together via a direct bond or other linking group.

[0037] In addition, when the monomer having a thiophene ring has a substituent, the substituent is not particularly limited, and examples thereof include linear or branched alkyl groups and linear or branched alkoxy groups having 1 to 20 carbon atoms. Among these, linear or branched alkyl groups having 4 to 20 carbon atoms are preferred from the viewpoint of the solubility of the block copolymer.

[0038] Specific examples of thiophene-based compounds constituting A and A1 are given below, but the A and A1 units according to the present invention are in no way limited to these thiophene-based compounds.

[0039] [ka]

[0040] From the viewpoint of the solubility of the block copolymer, A and A1 are preferably thiophene units having an alkyl group having 4 to 20 carbon atoms as a substituent.

[0041] (Monomer Unit Having a Triarylamine Skeleton Which May Have a Substitute) The triarylamine-based compound having a triarylamine skeleton constituting the monomer unit having a triarylamine skeleton which may have a substituent of A and A1 is not particularly limited as long as it has one or more triarylamine skeletons.

[0042] Examples of the triarylamine compound include triphenylamine which may have a substituent, trinaphthylamine which may have a substituent, and diphenylnaphthylamine which may have a substituent.

[0043] In addition, when the monomer having a triarylamine skeleton has a substituent, the substituent is not particularly limited, and examples thereof include linear or branched alkyl groups and linear or branched alkoxy groups having 1 to 20 carbon atoms. Among these, linear or branched alkyl groups having 4 to 20 carbon atoms are preferred from the viewpoint of the solubility of the block copolymer.

[0044] Specific examples of triarylamine compounds constituting A and A1 are given below, but the A and A1 units according to the present invention are in no way limited to these triarylamine compounds.

[0045] [ka]

[0046] From the viewpoint of the solubility of the block copolymer, A and A1 are preferably triphenylamine units having an alkyl group having 4 to 20 carbon atoms as a substituent.

[0047] [R1, R 21 , R 22 ] R in the formula (I) and R in the formula (IV) 21 and R 22 represents a direct bond, a linear or branched alkylene group, or an arylene group which may have a substituent. A methylene group (-CH-) in the alkylene group may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-).

[0048] R1, R 21 and R 22 Specific examples of the linear alkylene group include linear alkylene groups having 1 to 20 carbon atoms, such as a methylene group [-CH2-], an ethylene group [-(CH2)2-], a trimethylene group [-(CH2)3-], and a tetramethylene group [-(CH2)4-]. Specific examples of the branched alkylene group include alkylmethylene groups or dialkylmethylene groups having 2 to 20 carbon atoms, such as -CH(CH3)-, -CH(CH2CH3)-, -C(CH3)2-, -C(CH3)(CH2CH3)-, -C(CH3)(CH2CH2CH3)-, and -C(CH2CH3)2-; -CH(CH3)CH2-, -CH(CH3)CH(CH3)-, -C(CH3)2CH2-, -CH(CH2CH 3) Alkyl alkylene groups such as alkylethylene or dialkylethylene groups having 3 to 20 carbon atoms, such as -CH- and -C(CHCH)-CH-; alkyltrimethylene groups having 4 to 20 carbon atoms, such as -CH(CH)CHCH- and -CHCH(CH)CH-; and alkyltetramethylene groups having 5 to 20 carbon atoms, such as -CH(CH)CHCHCHCH- and -CHCH(CH)CHCH-. The methylene group (-CH2-) of the above alkyl group may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-).

[0049] Specific examples of the arylene group which may have a substituent include arylene groups such as a phenylene group, and heteroarylene groups such as a pyridinylene group. Examples of the substituent which the arylene group may have include an alkyl group having 1 to 20 carbon atoms, and an alkoxy group having 1 to 20 carbon atoms.

[0050] Of these, R1, R 21 and R 22 From the viewpoint of the solubility of the block copolymer, a linear or branched alkyl group, a linear or branched alkoxy group, or the like having 1 to 10 carbon atoms is preferred. In addition, R in formula (IV) 21 and R 22 may be the same or different.

[0051] [R2] In the above formula (I), R2 represents a hydrogen atom, a linear or branched alkyl group, a linear or branched alkoxy group, or an aryl group which may have a substituent.

[0052] Specific examples of the straight-chain alkyl group include straight-chain alkyl groups having 1 to 20 carbon atoms, such as a methyl group [-CH3], an ethyl group [-CH2CH3], a propyl group [-CH2CH2CH3], and a butyl group [-CH2CH2CH2CH3]. Specific examples of branched alkyl groups include branched alkyl groups having 3 to 20 carbon atoms, such as -C(CH3)3, -C(CH2CH3)3, -CH(CH3)CH2CH3, -CH(CH3)CH(CH3)2, and -C(CH3)2CH2CH3.

[0053] Specific examples of linear alkoxy groups include linear alkoxy groups having 1 to 20 carbon atoms, such as a methoxy group [-OCH3], an ethoxy group [-OCH2CH3], a propoxy group [-OCH2CH2CH3], and a butoxy group [-OCH2CH2CH2CH3]. Specific examples of branched alkoxy groups include branched alkoxy groups having 3 to 20 carbon atoms, such as -OC(CH3)3, -OC(CH2CH3)3, -OCH(CH3)CH2CH3, -OCH(CH3)CH(CH3)2, and -OC(CH3)2CH2CH3.

[0054] Specific examples of the aryl group which may have a substituent include aryl groups such as a phenyl group, and heteroaryl groups such as a pyridyl group. Examples of the substituent which the aryl group may have include an alkyl group having 1 to 20 carbon atoms, and an alkoxy group having 1 to 20 carbon atoms.

[0055] Of these, from the viewpoint of the solubility of the block copolymer, R2 is preferably an aryl group such as a phenyl group which may have a substituent, or a heteroaryl group such as a pyridyl group.

[0056] [n] In the formulas (I) and (IV), n is a natural number of 2 or more, which satisfies the number average molecular weight (Mn) of the organic semiconductor block described below.

[0057] [Molecular weight] The semiconductor properties of the organic semiconductor block vary depending on the molecular weight. When used as an optical / electronic functional material, the number average molecular weight (Mn) of the organic semiconductor block is preferably 2000 g / mol or more, more preferably 4000 g / mol or more, and even more preferably 6000 g / mol or more, since a good value of charge mobility, which is an example of a semiconductor property, can be obtained. There is no particular upper limit on the number average molecular weight (Mn) of the organic semiconductor block, but from the viewpoint of solubility and adhesiveness of the block copolymer, it is preferably 100,000 g / mol or less, and more preferably 50,000 g / mol or less.

[0058] Here, the number average molecular weight (Mn) of the organic semiconductor block is a number average molecular weight (polystyrene equivalent) measured by gel permeation chromatography (GPC). Tetrahydrofuran (THF) is preferably used as a solvent for the measurement.

[0059] If the organic semiconductor block has a large molecular weight distribution, it may contain molecules having a molecular weight smaller than the desired range, and the desired charge mobility may not be obtained. Therefore, the molecular weight dispersity (Mw / Mn) of the organic semiconductor block is preferably about 1.0 to 4.0, more preferably about 1.0 to 3.0, and particularly preferably about 1.0 to 2.0. Here, Mw indicates the weight average molecular weight. The weight average molecular weight (Mw) can also be determined by GPC measurement, similarly to the number average molecular weight (Mn).

[0060] <Adhesive block> The adhesive block is not particularly limited as long as it contains a vinyl polymer skeleton and has adhesive properties, but is preferably a block represented by the following formula (II) or (III).

[0061] (Adhesive block represented by formula (II))

[0062] [ka]

[0063] In formula (II), R3 represents a hydrogen atom or a linear or branched alkyl group. R4 represents a linear or branched alkyl group. A methylene group (-CH2-) in the alkyl group may be substituted with an oxygen atom (-O-). R5 represents a hydrogen atom or a linear or branched alkyl group, in which a methylene group (-CH2-) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). R6 represents a direct bond or a linear or branched alkylene group, in which a methylene group (-CH2-) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). m is a natural number greater than or equal to 2. The wavy line represents a bond to the linking group.

[0064] [R3] In the formula (II), R3 represents a hydrogen atom or a linear or branched alkyl group.

[0065] Specific examples of the linear alkyl group of R3 include linear alkyl groups having 1 to 20 carbon atoms, such as a methyl group [-CH3], an ethyl group [-CH2CH3], a propyl group [-CH2CH2CH3], and a butyl group [-CH2CH2CH2CH3]. Specific examples of the branched alkyl group include branched alkyl groups having 3 to 20 carbon atoms, such as -C(CH3)3, -C(CH2CH3)3, -CH(CH3)CH2CH3, -CH(CH3)CH(CH3)2, and -C(CH3)2CH2CH3.

[0066] From the viewpoint of imparting adhesiveness, R3 is preferably a hydrogen atom or a linear alkyl group having 1 to 5 carbon atoms.

[0067] [R4] In the formula (II), R4 represents a linear or branched alkyl group, in which a methylene group (-CH2-) may be substituted with an oxygen atom (-O-).

[0068] Specific examples of the straight-chain alkyl group for R4 include straight-chain alkyl groups having 1 to 20 carbon atoms, such as a methyl group [-CH3], an ethyl group [-CH2CH3], a propyl group [-CH2CH2CH3], a butyl group [-CH2CH2CH2CH3], a pentyl group [-CH2CH2CH2CH2CH3], a hexyl group [-CH2CH2CH2CH2CH2CH3], a heptyl group [-CH2CH2CH2CH2CH2CH2CH3], and an octyl group [-CH2CH2CH2CH2CH2CH2CH2CH3]. Specific examples of branched alkyl groups include branched alkyl groups having 3 to 20 carbon atoms, such as -C(CH3)3, -C(CH2CH3)3, -CH(CH3)CH2CH3, -CH(CH3)CH(CH3)2, and -C(CH3)2CH2CH3.

[0069] From the viewpoint of imparting adhesiveness, R4 is preferably a linear alkyl group having 1 to 50 carbon atoms in which 1 to 24 methylene groups (-CH2-) have been substituted with oxygen atoms (-O-).

[0070] [R5] In the formula (II), R5 represents a hydrogen atom or a linear or branched alkyl group, in which a methylene group (-CH2-) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-).

[0071] Specific examples of the straight-chain alkyl group for R5 include straight-chain alkyl groups having 1 to 20 carbon atoms, such as a methyl group [-CH3], an ethyl group [-CH2CH3], a propyl group [-CH2CH2CH3], a butyl group [-CH2CH2CH2CH3], a pentyl group [-CH2CH2CH2CH2CH3], a hexyl group [-CH2CH2CH2CH2CH2CH3], a heptyl group [-CH2CH2CH2CH2CH2CH2CH3], and an octyl group [-CH2CH2CH2CH2CH2CH2CH2CH3]. Specific examples of branched alkyl groups include branched alkyl groups having 3 to 20 carbon atoms, such as -C(CH3)3, -C(CH2CH3)3, -CH(CH3)CH2CH3, -CH(CH3)CH(CH3)2, and -C(CH3)2CH2CH3.

[0072] From the viewpoints of block copolymer synthesis and imparting adhesiveness, R5 is preferably a linear alkyl group having 5 to 20 carbon atoms in which 3 to 9 methylene groups (-CH2-) are substituted with sulfur atoms (-S-) and / or thiocarbonyl groups (-C(=S)-).

[0073] [R6] In the formula (II), R6 represents a direct bond or a linear or branched alkylene group, in which a methylene group (-CH2-) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-).

[0074] Specific examples of the linear alkylene group of R6 include linear alkylene groups having 1 to 20 carbon atoms, such as a methylene group [-CH2-], an ethylene group [-(CH2)2-], a trimethylene group [-(CH2)3-], and a tetramethylene group [-(CH2)4-]. Specific examples of the branched alkylene group include alkylmethylene groups or dialkylmethylene groups having 2 to 20 carbon atoms, such as -CH(CH3)-, -CH(CH2CH3)-, -C(CH3)2-, -C(CH3)(CH2CH3)-, -C(CH3)(CH2CH2CH3)-, and -C(CH2CH3)2-; -CH(CH3)CH2-, -CH(CH3)CH(CH3)-, -C(CH3)2CH2-, -CH(CH2CH 3) Alkyl alkylene groups such as alkylethylene or dialkylethylene groups having 3 to 20 carbon atoms, such as -CH- and -C(CHCH)-CH-; alkyltrimethylene groups having 4 to 20 carbon atoms, such as -CH(CH)CHCH- and -CHCH(CH)CH-; and alkyltetramethylene groups having 5 to 20 carbon atoms, such as -CH(CH)CHCHCHCH- and -CHCH(CH)CHCH-.

[0075] From the viewpoints of block copolymer synthesis and imparting adhesiveness, R6 is preferably a linear alkylene group having 5 to 20 carbon atoms in which 2 to 8 methylene groups (-CH2-) in the alkylene group are substituted with an oxygen atom (-O-) and / or a carbonyl group (-C(=O)-).

[0076] [m] In formula (II), m is a natural number of 2 or more, which satisfies the number average molecular weight (Mn) of the adhesive block described below.

[0077] (Adhesive block represented by formula (III))

[0078] [ka]

[0079] In formula (II), R3 represents a hydrogen atom or a linear or branched alkyl group. R4 represents a linear or branched alkyl group. A methylene group (-CH2-) in the alkyl group may be substituted with an oxygen atom (-O-). R5 represents a hydrogen atom or a linear or branched alkyl group, in which a methylene group (-CH2-) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). R6 represents a direct bond or a linear or branched alkylene group, in which a methylene group (-CH2-) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). m is a natural number greater than or equal to 2. The wavy line represents a bond to the linking group.

[0080] [R7~R 11 ] In the above formula (III), R7~R 11 R7 to R8 each independently represent a hydrogen atom or a hydroxyl group.11 At least one of these is a hydroxyl group. R7~R 11 The inclusion of hydroxyl groups is expected to result in adhesive properties. From this perspective, R7~R 11 It is preferable that at least two of R7 to R8 are hydroxyl groups. 11 From the viewpoint of the solubility of the block copolymer, the number of hydroxyl groups is preferably 4 or less. R7~R 11 There are no particular limitations on the positions of the hydroxyl groups in formula (III), but from the viewpoint of imparting adhesiveness, the hydroxyl groups are preferably at the m-position and p-position of the phenyl group in formula (III).

[0081] [R 12 ] In the formula (III), R 12 represents a hydrogen atom or a linear or branched alkyl group, in which a methylene group (-CH-) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-).

[0082] R 12 Specific examples of the straight-chain alkyl group include straight-chain alkyl groups having 1 to 20 carbon atoms, such as a methyl group [-CH3], an ethyl group [-CH2CH3], a propyl group [-CH2CH2CH3], a butyl group [-CH2CH2CH2CH3], a pentyl group [-CH2CH2CH2CH2CH3], a hexyl group [-CH2CH2CH2CH2CH2CH3], a heptyl group [-CH2CH2CH2CH2CH2CH2CH3], and an octyl group [-CH2CH2CH2CH2CH2CH2CH2CH3]. Specific examples of branched alkyl groups include branched alkyl groups having 3 to 20 carbon atoms, such as -C(CH3)3, -C(CH2CH3)3, -CH(CH3)CH2CH3, -CH(CH3)CH(CH3)2, and -C(CH3)2CH2CH3.

[0083] R 12From the viewpoints of block copolymer synthesis and imparting adhesiveness, the alkyl group is preferably a linear alkyl group having 5 to 20 carbon atoms, in which 3 to 9 methylene groups (-CH2-) are substituted with sulfur atoms (-S-) and / or thiocarbonyl groups (-C(=S)-).

[0084] [R 13 ] In the formula (III), R 13 represents a direct bond or a linear or branched alkylene group, in which a methylene group (-CH-) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-).

[0085] R 13 Specific examples of the straight-chain alkylene group include straight-chain alkylene groups having 1 to 20 carbon atoms, such as a methylene group [-CH2-], an ethylene group [-(CH2)2-], a trimethylene group [-(CH2)3-], and a tetramethylene group [-(CH2)4-]. Specific examples of the branched alkylene group include alkylmethylene groups or dialkylmethylene groups having 2 to 20 carbon atoms, such as -CH(CH3)-, -CH(CH2CH3)-, -C(CH3)2-, -C(CH3)(CH2CH3)-, -C(CH3)(CH2CH2CH3)-, and -C(CH2CH3)2-; -CH(CH3)CH2-, -CH(CH3)CH(CH3)-, -C(CH3)2CH2-, -CH(CH2CH 3) Alkyl alkylene groups such as alkylethylene or dialkylethylene groups having 3 to 20 carbon atoms, such as -CH- and -C(CHCH)-CH-; alkyltrimethylene groups having 4 to 20 carbon atoms, such as -CH(CH)CHCH- and -CHCH(CH)CH-; and alkyltetramethylene groups having 5 to 20 carbon atoms, such as -CH(CH)CHCHCHCH- and -CHCH(CH)CHCH-.

[0086] R 13From the viewpoints of block copolymer synthesis and imparting adhesiveness, a linear alkylene group having 5 to 20 carbon atoms in which 2 to 8 methylene groups (-CH2-) in the alkylene group are substituted with an oxygen atom (-O-) and / or a carbonyl group (-C(=O)-).

[0087] [k] In formula (III), k is a natural number of 2 or more, which satisfies the number average molecular weight (Mn) of the adhesive block described below.

[0088] [Molecular weight] The number average molecular weight (Mn) of the adhesive block is preferably 1000 to 50000, and particularly preferably about 2000 to 20000. When the number average molecular weight of the adhesive block is equal to or higher than the above lower limit, it is expected that the adhesive block will impart adhesiveness to the block copolymer, and when the number average molecular weight is equal to or lower than the above upper limit, the solubility of the block copolymer can be ensured.

[0089] Here, the number average molecular weight (Mn) of the adhesive block is a number average molecular weight (polystyrene equivalent) measured by gel permeation chromatography (GPC). Tetrahydrofuran (THF) is preferably used as a solvent for the measurement.

[0090] [Content] The content of the adhesive block in the block copolymer of the present invention is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, based on the total mass of the organic semiconductor block and the adhesive block. On the other hand, it is preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less. If the content of the adhesive block is equal to or more than the lower limit, sufficient adhesion can be obtained, and if it is equal to or less than the upper limit, the organic semiconductor properties of the block copolymer are excellent.

[0091] <Connecting group> In the block copolymer of the present invention, the linking group that bonds the organic semiconductor block and the adhesive block is not particularly limited as long as it can link these blocks together, and examples of the linking group include alicyclic hydrocarbon groups such as a divalent group of a triazole ring (specifically, one having bonds at the 1- and 4-positions of 1,2,3-triazole) and a divalent group of a cyclohexene ring. Among these, a divalent group of a triazole ring is preferred from the viewpoint of block copolymer synthesis.

[0092] <Method of producing block copolymer> The method for producing the block copolymer of the present invention is not particularly limited, but it is preferably produced by a click chemical coupling reaction.

[0093] <Click chemistry coupling reaction> Click chemistry coupling reaction refers to any method in which an azide (N3) compound reacts with an alkyne group to form a 1,2,3-triazole. Click chemistry coupling reaction can be carried out by applying or adapting any Huisgen experimental procedure commonly known to those skilled in the art. Generally, the click chemistry coupling reaction is carried out according to the Huisgen reaction in either organic or aqueous conditions. In organic conditions, the click chemistry coupling reaction is typically carried out in the presence of copper(I) bromide (CuBr) and N,N,N',N',N"-pentamethyldiethylenetriamine (PMDETA). This reaction may in particular be carried out in an organic solvent (e.g. dimethylformamide (DMF), tetrahydrofuran (THF), toluene, dimethylsulfoxide (DMSO)) at temperatures comprised between room temperature and the reflux temperature of the reaction mixture, preferably under anhydrous conditions.

[0094] The block copolymer of the present invention can be produced, for example, by forming 1,2,3-triazole by a click chemical coupling reaction between an organic semiconductor block having a terminal azide group and an adhesive block having a terminal alkyne group. The organic semiconductor block having a terminal azide group and the adhesive block having a terminal alkyne group may be commercially available or may be synthesized by a known production method.

[0095] <Phase separation> In the block copolymer of the present invention, a continuous phase consisting of the organic semiconductor block and a continuous phase consisting of the adhesive block form a lamellar phase structure. The lamellar phase structure allows the organic semiconductor block having semiconductor properties and the adhesive block having adhesive properties to be phase-separated at the nano level, thereby suppressing aggregation of the organic semiconductor block and the adhesive block. Therefore, a film having adhesive properties to different materials can be obtained from the block copolymer of the present invention. The phase structure can be observed by a micrograph (eg, a scanning probe microscope).

[0096] <Film formation method> Although there is no particular limitation on the film-forming method for forming the block copolymer of the present invention into a film to obtain the organic film of the present invention, a wet film-forming method is preferred. Specifically, a spin-coating method and the like can be mentioned. In this case, the conditions of the spin-coating may be appropriately determined according to a conventional method, taking into consideration the viscosity of the block copolymer solution and the like. The block copolymer solution may be prepared according to a standard method using a solvent capable of dissolving the block copolymer. Examples of the solvent include one or a mixture of two or more of chlorobenzene, dichlorobenzene, chloroform, toluene, xylene, THF, etc. Moreover, the block copolymer concentration of the block copolymer solution to be subjected to wet film formation is preferably about 5 to 40 mg / mL.

[0097] <Organic film> As described above, the organic film of the present invention is obtained by forming a film using the block copolymer of the present invention, and has organic semiconductor properties, electrochemical properties, optical properties, and the like derived from the organic semiconductor block, and therefore can be suitably used as, for example, an organic transistor, an organic electroluminescence (EL) device, an organic solar cell, or an optical sensor. The organic film of the present invention may be formed by mixing two or more types of the block copolymer of the present invention, and may contain other components as necessary in addition to the block copolymer of the present invention. Examples of the other components include an organic semiconductor compound, a dopant, a stabilizer, a curing agent, and the like. EXAMPLES

[0098] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0099] [Synthesis Example 1: Synthesis of trimethylsilyl-terminated poly(3-hexylthiophene)]

[0100] [ka]

[0101] Under a nitrogen atmosphere, 0.128 g (0.170 mmol) of bromo-o-tolylbis(triphenylphosphine)nickel(II), 8 mL of dehydrated tetrahydrofuran (THF), and 0.137 g (0.332 mmol) of 1,3-bis(diphenylphosphine)propane (omitted in the above reaction formula) were added to a 30 mL two-neck flask and stirred at room temperature for 30 minutes to prepare bromo-o-tolyl(diphenylphosphinepropane)nickel(II) solution A. In addition, 53 mg (2.18 mmol) of magnesium, 1 mL of dehydrated THF, and several drops of 1,2-dibromoethane were added to another 5 mL vial under a nitrogen atmosphere, and after confirming the generation of ethylene, 0.33 mL (1.85 mmol) of (5-chloro-1-pentynyl)trimethylsilane was added and stirred at room temperature overnight to prepare (5-chloromagnesio-1-pentynyl)trimethylsilane solution B. In a nitrogen atmosphere, 3.18 g (8.52 mmol) of 2-bromo-3-hexyl-5-iodo-thiophene and 200 mL of dehydrated THF were added to another 300 mL two-neck flask and cooled to 0° C. Furthermore, 7.2 mL (8.64 mmol) of a 1.2 M THF solution of isopropyl magnesium chloride-lithium chloride complex was added and stirred at room temperature for 30 minutes to prepare 2-bromo-5-chloromagnesio-3-hexylthiophene solution C. Solution A was added to solution C and polymerized at room temperature for 15 minutes, and then solution B was added and reacted at room temperature for 1 hour to terminate the polymerization.

[0102] The resulting reaction solution was dropped into methanol to obtain a precipitate, which was then collected by filtration, dissolved in benzene, and freeze-dried to obtain the target trimethylsilyl-terminated poly(3-hexylthiophene). Yield 1.26 g (89% yield), number average molecular weight (Mn) (THF GPC, polystyrene standard) 13,000 g / mol, molecular weight dispersity (Mw / Mn) (THF GPC, polystyrene standard) 1.08, number average molecular weight ( 1 H NMR) 7,900 g / mol. The results of NMR analysis of this product are as follows: 1 H NMR(400MHz,CDCl3) δ 6.98(s),6.91(s),6.86(s),2.81(t,J=7.3Hz),2.52(t,J=7.8Hz),2.33(t,J=6.6Hz),1.73-1.67(m),1.51-1.36(m),0.92(s),0.1(s)

[0103] [Synthesis Example 2: Synthesis of ethynyl-terminated poly(3-hexylthiophene) (P3HT)]

[0104] [ka]

[0105] Under a nitrogen atmosphere, 0.504 g (63.8 μmol) of trimethylsilyl-terminated poly(3-hexylthiophene) obtained in Synthesis Example 1 above, 100 mL of dehydrated THF, and 4 mL (4 mmol) of a 1.0 M THF solution of tetrabutylammonium fluoride were added to a 200 mL flask, and the mixture was reacted at 50° C. for 4 hours. The resulting solid was dissolved in benzene and freeze-dried to obtain the target ethynyl-terminated poly(3-hexylthiophene) (P3HT). Yield 0.445g (88% yield), number average molecular weight (Mn) (THF GPC, polystyrene standard) 13000g / mol, molecular weight dispersity (Mw / Mn) (THF GPC, polystyrene standard) 1.09, number average molecular weight ( 1 H NMR) 8,400 g / mol. The results of NMR analysis of this product are as follows: 1 H NMR(400MHz,CDCl3) δ 6.97(s),6.90(s),6.85(s),2.80(t,J=7.7Hz),2.54-2.48(m),2.30-2.26(m),2.00(t,J=2.5Hz) ),1.88(d,J=14.0Hz),1.74-1.66(m),1.41(d,J=13.1Hz),1.34(t,J=3.6Hz),0.91(t,J=6.8Hz)

[0106] [Synthesis Example 3: Synthesis of azide-terminated poly(2-(2-ethoxyethoxy)ethyl acrylate) (P2EEEA)]

[0107] [ka]

[0108] In a nitrogen atmosphere, 2.45g (13.0mmol) of 2-(2-ethoxyethoxy)ethyl acrylate, 0.103g (0.204mmol) of 8-azidooctyl 2-((dodecylthio)carbonothioyl)thio)propanoate, 3mL of dehydrated N,N-dimethylformamide (DMF), and 9.5mg (57.9μmol) of azobisisobutyronitrile were added to a 10mL flask, and the reaction solution was bubbled with nitrogen and then reacted at 65℃ for 3 hours. The concentrated solution obtained was purified in methanol using a semipermeable membrane. The solvent was distilled off from the solution inside the semipermeable membrane to obtain the target azide-terminated poly(2-(2-ethoxyethoxy)ethyl acrylate) (P2EEEA). Yield 1.644g (64% yield), number average molecular weight (Mn) (THF GPC, polystyrene standard) 9000g / mol, molecular weight dispersity (Mw / Mn) (THF GPC, polystyrene standard) 1.14, number average molecular weight ( 1 H NMR) 13,000 g / mol. The results of NMR analysis of this product are as follows: 1 H NMR(400MHz,CDCl3) δ 4.42-4.02(b),3.65-3.48(m),2.56-2.22(b),2.07-1.82(b),1.76-1.59(b),1.54-1.40(b),1.37-1.18(m)

[0109] [Example 1] [Synthesis of poly(3-hexylthiophene)-b-poly(2-(2-ethoxyethoxy)ethyl acrylate) (P3HT-b-P2EEEA)]

[0110] [ka]

[0111] Under a nitrogen atmosphere, 0.148 g (17.7 μmol) of ethynyl-terminated poly(3-hexylthiophene) obtained in Synthesis Example 2 above, 0.251 g (19.3 μmol) of azide-terminated poly(2-(2-ethoxyethoxy)ethyl acrylate) obtained in Synthesis Example 3 above, 33.0 mg (0.190 mmol) of N,N,N',N",N"-pentamethyldiethylenetriamine, and 10 mL of dehydrated THF were placed in a 30 mL flask and freeze-degassed three times. Next, 27.0 mg (0.188 mmol) of copper (I) bromide was added and the mixture was allowed to react at 60°C for 4 hours. After the reaction was completed, chloroform was added to the reaction solution, copper was removed using an alumina column, and the target product was then fractionated using high performance liquid chromatography (HPLC). The solvent was removed from the solution obtained using HPLC, and the resulting solid was dissolved in benzene and freeze-dried to obtain the target product, poly(3-hexylthiophene)-b-poly(2-(2-ethoxyethoxy)ethyl acrylate) (P3HT-b-P2EEEA). The yield was 0.156 mg (42% yield), the number average molecular weight (Mn) (THF GPC, using polystyrene standard) was 23,000 g / mol, and the molecular weight dispersity (Mw / Mn) (THF GPC, using polystyrene standard) was 1.08. The results of NMR analysis of this product are as follows: 1 H NMR(400MHz,CDCl3) δ 6.96(s),4.39-4.08(b),3.66-3.48(m),2.79(t,J=7.3Hz),2.41-2.22(b),1.9 9-1.81(b),1.71-1.65(m),1.44-1.34(m),1.19(t,J=6.9Hz),0.90(t,J=6.6Hz)

[0112] [Synthesis Example 4: Synthesis of azide-terminated poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol)]

[0113] [ka]

[0114] In a nitrogen atmosphere, 1.09 g (2.99 mmol) of O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol, 0.111 g (0.220 mmol) of 8-azidooctyl 2-((dodecylthio)carbonothioyl)thio)propanoate, 1.5 mL of dehydrated toluene, and 7.2 mg (43.8 μmol) of azobisisobutyronitrile were added to a 10 mL flask, and the reaction solution was bubbled with nitrogen and then reacted at 60°C overnight. The resulting reaction solution was dropped into methanol to obtain a precipitate. The precipitate collected by filtration was dissolved in benzene and freeze-dried to obtain the target azide-terminated poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol). Yield 0.471g (39%), number average molecular weight (Mn) (THF GPC, polystyrene standard) 3100g / mol, molecular weight dispersity (Mw / Mn) (THF GPC, polystyrene standard) 1.06, number average molecular weight ( 1 H NMR) 5,300 g / mol. The results of NMR analysis of this product are as follows: 1 H NMR(400MHz,CDCl3) δ 6.64-5.83(b),3.44-3.23(b),2.01-1.64(b),1.48-1.10(b),0.94-0.69(b),0.21-0.13(m)

[0115] [Synthesis Example 5: Synthesis of azide-terminated poly(4-vinylcatechol) (PVC)]

[0116] [ka]

[0117] Under a nitrogen atmosphere, 0.255 g (48.2 μmol) of the azide-terminated poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol) obtained in Synthesis Example 4 above, 8 mL of dehydrated THF, and 0.88 mL (10.6 mmol) of a 12 M aqueous HCl solution were added to a 30 mL flask, and the reaction was carried out overnight at 60° C. The resulting reaction solution was separated using ethyl acetate. The concentrated ethyl acetate fraction was dropped into hexane, and the target azide-terminated poly(4-vinylcatechol) (PVC) was recovered by decantation. Yield 98.7 mg (89%), number average molecular weight (Mn) ( 1 H NMR) 3000 g / mol. The results of NMR analysis of this product are as follows: 1 H NMR(400MHz,CDCl3) δ 6.68-5.92(m),3.61-3.53(m),1.83-1.80(m),1.63-1.25(m),0.85(t,J =7.3Hz)

[0118] [Synthesis Example 6: Synthesis of poly(3-hexylthiophene)-b-poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol)]

[0119] [ka]

[0120] Under a nitrogen atmosphere, 0.169 g (20.1 μmol) of ethynyl-terminated poly(3-hexylthiophene) obtained in Synthesis Example 2 above, 0.125 g (23.6 μmol) of azide-terminated poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol) obtained in Synthesis Example 4 above, 27.6 mg (0.159 mmol) of N,N,N',N",N"-pentamethyldiethylenetriamine, and 10 mL of dehydrated THF were added to a 30 mL flask, and the mixture was subjected to freeze-degassing three times. Then, 27.6 mg (0.192 mmol) of copper bromide (I) was added and reacted at 60°C for 4 hours. After the reaction was completed, chloroform was added to the reaction solution, and copper was removed using an alumina column, followed by high performance liquid chromatography. The resulting solution was added dropwise to methanol to obtain a precipitate. The precipitate collected by filtration was dissolved in benzene and freeze-dried to obtain the target compound, poly(3-hexylthiophene)-b-poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol). The yield was 121 mg (46% yield), the number average molecular weight (Mn) (THF GPC, using polystyrene standard) was 19,000 g / mol, and the molecular weight dispersity (Mw / Mn) (THF GPC, using polystyrene standard) was 1.06. The results of NMR analysis of this product are as follows: 1 H NMR(600MHz,CDCl3) δ 6.98(s),6.64-5.92(b),2.81(t,J=7.6 Hz),1.63-1.66(m),1.48-1.40 (m),1.39-1.32(m),1.26-1.19(s),1.06-0.81(m),0.26-0.11(m)

[0121] [Example 2] <Synthesis of poly(3-hexylthiophene)-b-poly(4-vinylcatechol) (P3HT-b-PVC)>

[0122] [ka]

[0123] Under a nitrogen atmosphere, 79 mg (4.16 μmol) of poly(3-hexylthiophene)-b-poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol) obtained in Synthesis Example 6 above, 50 mL of dehydrated THF, and 4 mL (4 mmol) of a 1.0 M THF solution of tetrabutylammonium fluoride were added to a 100 mL flask, and the mixture was allowed to react at room temperature overnight. The resulting reaction solution was dropped into methanol to obtain a precipitate. The precipitate collected by filtration was dissolved in benzene and freeze-dried to obtain the target poly(3-hexylthiophene)-b-poly(4-vinylcatechol) (P3HT-b-PVC). Yield 63.8 mg (97%), number average molecular weight ( 1 H NMR) 11,000 g / mol. The results of NMR analysis of this product are as follows: 1 H NMR(600MHz,CDCl3) δ 7.06-6.85(b),3.00-2.65(b),1.86-1.61(b),1.51-1.39(b),1.39-1.29(b),1.26-1.18(m),1.03-0.65(b)

[0124] [Synthesis Example 7: Synthesis of poly(2,4,6-trimethyl-N,N-diphenylaniline) terminated with tert-butyldimethylsilyl groups at both ends]

[0125] [ka]

[0126] In a nitrogen atmosphere, 0.084 g (0.19 mmol) of ((4-bromobenzyl)oxy)(tert-butyl)dimethylsilane, 0.203 g (1.50 mmol) of 2,4,6-trimethylaniline, 0.455 g (0.15 mmol) of 4,4'-dibromobiphenyl, 0.064 mg (0.06 μmol) of tri-tert-butylphosphonium tetrafluoroborate, and 30 mL of deoxygenated toluene were added to a 100 mL flask, and nitrogen was bubbled into the reaction solution. Next, 0.102 g (0.11 mmol) of tris(dibenzylideneacetone)dipalladium(0) was added and reacted overnight at 80°C. Sodium dimethyldithiocarbamate dihydrate was then added and stirred at 80°C for 1 hour, and the resulting reaction solution was dropped into methanol to precipitate a polymer. The precipitate collected by filtration was dissolved in chloroform, and the solution was dropped into acetone. The obtained precipitate was dissolved in benzene and freeze-dried to obtain the target product, poly(2,4,6-trimethyl-N,N-diphenylaniline) terminated with tert-butyldimethylsilyl groups at both ends. The yield was 940 mg (95% yield), the number average molecular weight (Mn) (THF GPC, using polystyrene standard) was 9600 g / mol, and the molecular weight dispersity (Mw / Mn) (THF GPC, using polystyrene standard) was 1.84. The results of NMR analysis of this product are as follows: 1 H NMR(600MHz,CDCl3) δ 7.40(d,J=8.3 Hz),7.03(d,J=9.0Hz),6.96(s),4.67(s),2.34(s),2.04(s),0.93(s),0.09 (s)

[0127] [Synthesis Example 8: Synthesis of poly(2,4,6-trimethyl-N,N-diphenylaniline) terminated with methylol groups at both ends]

[0128] [ka]

[0129] Under a nitrogen atmosphere, 0.902 g of the poly(2,4,6-trimethyl-N,N-diphenylaniline) terminated with tert-butyldimethylsilyl groups at both ends obtained in Synthesis Example 7 above, 30 mL of THF, and 1.8 mL (1.8 mmol) of a 1.0 M THF solution of tetrabutylammonium fluoride were added to a 100 mL flask, and the mixture was allowed to react at room temperature overnight. The resulting reaction solution was dropped into methanol to precipitate the polymer. The precipitate collected by filtration was dissolved in benzene and freeze-dried to obtain the desired poly(2,4,6-trimethyl-N,N-diphenylaniline) terminated with methylol groups at both ends. The yield was 936 mg (99% yield), the number average molecular weight (Mn) (THF GPC, using polystyrene standard) was 9600 g / mol, and the molecular weight dispersity (Mw / Mn) (THF GPC, using polystyrene standard) was 1.84. The results of NMR analysis of this product are as follows: 1 H NMR(600MHz,CDCl3) δ 7.39(d,J=8.3 Hz),7.01(d,J=8.3Hz),6.94(s),4.59(s),2.32(s),2.02(s)

[0130] [Synthesis Example 9: Synthesis of poly(2,4,6-trimethyl-N,N-diphenylaniline) terminated with alkynyl groups at both ends]

[0131] [ka]

[0132] Under a nitrogen atmosphere, 0.622 g of the methylol-terminated poly(2,4,6-trimethyl-N,N-diphenylaniline) obtained in Synthesis Example 8 above, 50 mL of THF, 2.8 mL of triethylamine, and 15 mL (8.8 mmol) of a 0.34 M dichloromethane solution of 5-hexynoic acid chloride were added to a 100 mL flask, and the mixture was allowed to react at room temperature for 1 hour. The resulting reaction solution was dropped into methanol to precipitate the polymer. The precipitate collected by filtration was dissolved in benzene and freeze-dried to obtain the desired alkynyl-terminated poly(2,4,6-trimethyl-N,N-diphenylaniline). The yield was 536 mg (yield 86%), the number average molecular weight (Mn) (THF GPC, using polystyrene standard) was 8,800 g / mol, and the molecular weight dispersity (Mw / Mn) (THF GPC, using polystyrene standard) was 1.83. The results of NMR analysis of this product are as follows: 1 H NMR(600MHz,CDCl3) δ 7.40(d,J=8.3 Hz),7.02(d,J=8.3Hz),6.95(s),5.03 (s),2.49(t,J=7.6Hz),2.33(s),2.27-2.25(m),2.03(s),1.96(s),1.87(t,J=7.2 Hz)

[0133] [Synthesis Example 10: Synthesis of poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol)-b-poly(2,4,6-trimethyl-N,N-diphenylaniline)-b-poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol)]

[0134] [ka]

[0135] Under a nitrogen atmosphere, 0.406 g of alkynyl-terminated poly(2,4,6-trimethyl-N,N-diphenylaniline) obtained in Synthesis Example 9 above, 0.661 g (0.107 mmol) of azide-terminated poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol) obtained in Synthesis Example 4 above, 0.069 g (0.48 mmol) of copper (I) bromide, 0.071 g (0.41 mmol) of N,N,N',N",N"-pentamethyldiethylenetriamine, and 60 mL of THF were added to a 200 mL flask and reacted at 60°C for 3 hours. Next, 5-hexynoic acid was added and reacted at 60°C for 30 minutes. After the reaction was completed, chloroform was added to the reaction solution and copper was removed using an alumina column. Then, silica gel chromatography was performed to obtain the target product, poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol)-b-poly(2,4,6-trimethyl-N,N-diphenylaniline)-b-poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol). The yield was 736 mg (69% yield), the number average molecular weight (Mn) (THF GPC, using polystyrene standard) was 21,000 g / mol, and the molecular weight dispersity (Mw / Mn) (THF GPC, using polystyrene standard) was 1.53. The results of NMR analysis of this product are as follows: 1 H NMR(600MHz,CDCl3) δ 7.39(d,J=7.6 Hz),7.01(s),6.94(s),6.71-5.78(b),2.43-2.21(b),2.09-1.89(b),1.40-1.18 (m),1.09-0.66(b),0.32-0.14(b)

[0136] [Example 5] <Synthesis of poly(4-vinylcatechol)-b-poly(2,4,6-trimethyl-N,N-diphenylaniline)-b-poly(4-vinylcatechol) (PVC-b-PTAA-b-PVC)>

[0137] [ka]

[0138] Under a nitrogen atmosphere, 0.69 g of poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol)-b-poly(2,4,6-trimethyl-N,N-diphenylaniline)-b-poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol) obtained in the above Synthesis Example 10, 100 mL of THF, and 10 mL (10 mmol) of a 1.0 M THF solution of tetrabutylammonium fluoride were added to a 200 mL flask and reacted at room temperature overnight. The resulting reaction solution was dropped into methanol to precipitate the polymer. The precipitate collected by filtration was dissolved in benzene and freeze-dried to obtain the target poly(4-vinylcatechol)-b-poly(2,4,6-trimethyl-N,N-diphenylaniline)-b-poly(4-vinylcatechol). Yield 254 mg (55%), number average molecular weight (Mn) ( 1 H NMR) 14,000 g / mol. The results of NMR analysis of this product are as follows: 1 H NMR(600MHz,CDCl3) δ 7.47-7.27(b), 7.20-6.62(b),2.47-2.19(b),2.15-1.83(b),1.81-1.50(b),1.48-0.98(b),0.95-0.55(b)

[0139] [Synthesis Example 11: Synthesis of 4'-bromo-N-mesityl-[1,1'-biphenyl]-4-amine]

[0140] [ka]

[0141] In a nitrogen atmosphere, 3.11g (23.0mmol) of 2,4,6-trimethylaniline, 7.30g (23.3mmol) of 4,4'-dibromobiphenyl, 3.56g (37.0mmol) of sodium tert-butoxide, and 50mL of deoxygenated toluene were added to a 200mL flask, and nitrogen was bubbled into the reaction solution. Next, 0.147g (0.180mmol) of [1,1'-bis(diphenylphosphino)ferrocene]palladium(II) dichloride dichloromethane adduct was added and refluxed overnight. Sodium dimethyldithiocarbamate dihydrate was then added and stirred for 1 hour. The resulting reaction solution was washed three times with water, the organic layer was dehydrated with magnesium sulfate, filtered, and the filtrate was concentrated under reduced pressure. The resulting residue was purified by silica gel flash column chromatography (hexane / toluene=1 / 1, v / v) and recrystallized from hexane and toluene to obtain the target compound, 4'-bromo-N-mesityl-[1,1'-biphenyl]-4-amine. The yield was 2.37 g (38%). The results of NMR analysis of this product are as follows: 1 H NMR(400MHz,CDCl3) δ 7.48(d,J=8.8 Hz),7.37(dd,J =10.9,8.6Hz),6.95(s), 6.54(d,J=8.6Hz),5.20(s),2.32(s),2.19(s)

[0142] [Synthesis Example 12: Synthesis of poly(2,4,6-trimethyl-N,N-diphenylaniline) terminated with a tert-butyldimethylsilyl ether group]

[0143] [ka]

[0144] In a nitrogen atmosphere, 0.0822 g (0.273 mmol) of ((4-iodobenzyl)oxy)(tert-butyl)dimethylsilane, 1.10 g (3.00 mmol) of 4'-bromo-N-mesityl-[1,1'-biphenyl]-4-amine obtained in the above Synthesis Example 11, 0.056 mg (0.195 mmol) of tri-tert-butylphosphonium tetrafluoroborate, 0.858 g (8.93 mmol) of sodium tert-butoxide, and 30 mL of deoxygenated toluene were added to a 100 mL flask, and nitrogen was bubbled into the reaction solution. Next, 0.102 g (0.100 mmol) of tris(dibenzylideneacetone)dipalladium(0) was added and reacted overnight at 80°C. Sodium dimethyldithiocarbamate dihydrate was then added and stirred at 80°C for 1 hour, and the resulting reaction solution was added dropwise to methanol to precipitate a polymer. The precipitate collected by filtration was dissolved in chloroform, and the solution was dropped into acetone. The resulting precipitate was dissolved in benzene and freeze-dried to obtain the target poly(2,4,6-trimethyl-N,N-diphenylaniline) terminated with a tert-butyldimethylsilyl ether group. The yield was 584 mg (68% yield), the number average molecular weight (Mn) (THF GPC, using polystyrene standard) was 5600 g / mol, and the molecular weight dispersity (Mw / Mn) (THF GPC, using polystyrene standard) was 1.42. The results of NMR analysis of this product are as follows: 1 H NMR(600MHz,CDCl3) δ 7.39(d,J=8.3Hz),7.01(d,J=8.3Hz),6.94(s),4.65(s),2.32(s),2.02(s),0.91(s),0.08(s)

[0145] [Synthesis Example 13: Synthesis of poly(2,4,6-trimethyl-N,N-diphenylaniline) terminated with a methylol group]

[0146] [ka]

[0147] Under a nitrogen atmosphere, 0.550 g of the tert-butyldimethylsilyl ether group-terminated poly(2,4,6-trimethyl-N,N-diphenylaniline) obtained in Synthesis Example 12 above, 50 mL of THF, and 2.0 mL (2.0 mmol) of a 1.0 M THF solution of tetrabutylammonium fluoride were added to a 200 mL flask, and the mixture was allowed to react at room temperature overnight. The resulting reaction solution was dropped into acetone to precipitate the polymer. The precipitate collected by filtration was dissolved in benzene and freeze-dried to obtain the desired methylol group-terminated poly(2,4,6-trimethyl-N,N-diphenylaniline). The yield was 519 mg (99% yield), the number average molecular weight (Mn) (THF GPC, using polystyrene standard) was 4,900 g / mol, and the molecular weight dispersity (Mw / Mn) (THF GPC, using polystyrene standard) was 1.37. The results of NMR analysis of this product are as follows: 1 H NMR(600MHz,CDCl3) δ 7.40(d,J=9.0 Hz),6.99(d,J=46.1Hz),6.95(s),4.60(s),2.33(s),2.03(s)

[0148] [Synthesis Example 14: Synthesis of poly(2,4,6-trimethyl-N,N-diphenylaniline) terminated with an alkynyl group]

[0149] [ka]

[0150] Under a nitrogen atmosphere, 0.503 g of the methylol group-terminated poly(2,4,6-trimethyl-N,N-diphenylaniline) obtained in Synthesis Example 13 above, 50 mL of THF, 2.0 mL of triethylamine, and 10 mL (6.9 mmol) of a 0.69 M dichloromethane solution of 5-hexynoic acid chloride were added to a 200 mL flask, and the mixture was reacted at room temperature for 1 hour. The resulting reaction solution was dropped into methanol to precipitate the polymer. The precipitate collected by filtration was dissolved in chloroform, and the solution was dropped into methanol. The resulting precipitate was dissolved in benzene and freeze-dried to obtain the target alkynyl group-terminated poly(2,4,6-trimethyl-N,N-diphenylaniline). The yield was 419 mg (93% yield), the number average molecular weight (Mn) (THF GPC, using polystyrene standard) was 8,800 g / mol, and the molecular weight dispersity (Mw / Mn) (THF GPC, using polystyrene standard) was 1.83. The results of NMR analysis of this product are as follows: 1 H NMR(600MHz,CDCl3) δ 7.40(d,J=9.0 Hz),7.02(d,J=8.3Hz),6.95(s),5.03 (s),2.49(t,J=7.2Hz),2.33(s),2.26(td, J =7.1,2.8Hz),2.03(s),1.95(s),1.87 (t,J=7.2Hz)

[0151] [Synthesis Example 15: Synthesis of poly(2,4,6-trimethyl-N,N-diphenylaniline)-b-poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol)]

[0152] [ka]

[0153] Under a nitrogen atmosphere, 0363 g of alkynyl-terminated poly(2,4,6-trimethyl-N,N-diphenylaniline) obtained in Synthesis Example 14 above, 0.552 g (80 μmol) of azido-terminated poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol) obtained in Synthesis Example 4 above, 0.105 g (0.73 mmol) of copper bromide (I), 0.127 g (0.73 mmol) of N,N,N',N",N"-pentamethyldiethylenetriamine, and 60 mL of THF were added to a 200 mL flask, and the mixture was reacted at 60°C for 3 hours. After the reaction was completed, chloroform was added to the reaction solution, and the copper was removed using an alumina column, followed by high performance liquid chromatography. The resulting solution was added dropwise to methanol to obtain a precipitate. The precipitate collected by filtration was dissolved in benzene and freeze-dried to obtain the target compound, poly(2,4,6-trimethyl-N,N-diphenylaniline)-b-poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol). The yield was 357 mg (41% yield), the number average molecular weight (Mn) (THF GPC, using polystyrene standard) was 9700 / mol, and the molecular weight dispersity (Mw / Mn) (THF GPC, using polystyrene standard) was 1.36. The results of NMR analysis of this product are as follows: 1 H NMR(600MHz,CDCl3) δ 7.40(d,J=7.6 Hz),7.02(d,J=8.3Hz),6.96(s),6.72-5.73(b),2.34(s),2.03(s),1.12-0.82(b), 0.30-0.11(b)

[0154] [Example 6] <Synthesis of poly(2,4,6-trimethyl-N,N-diphenylaniline)-b-poly(4-vinylcatechol) (PTAA-b-PVC)>

[0155] [ka]

[0156] Under a nitrogen atmosphere, 321 g of poly(2,4,6-trimethyl-N,N-diphenylaniline)-b-poly(O,O-bis(tert-butyldimethylsilyl)-4-vinylcatechol) obtained in Synthesis Example 15 above, 30 mL of THF, and 10 mL (10 mmol) of a 1.0 M THF solution of tetrabutylammonium fluoride were added to a 200 mL flask, and the mixture was allowed to react at room temperature overnight. The resulting reaction solution was dropped into methanol to precipitate the polymer. The precipitate collected by filtration was dissolved in benzene and freeze-dried to obtain the target poly(2,4,6-trimethyl-N,N-diphenylaniline)-b-poly(4-vinylcatechol). Yield 127 mg (67%), number average molecular weight (Mn) ( 1 H NMR) 7800 g / mol. The results of NMR analysis of this product are as follows: 1 H NMR(600MHz,CDCl3) δ 7.41(d,J=6.9 Hz),7.04(d,J=6.9 Hz),6.97(s),2.35(s),2.04(s)

[0157] [Example 3] <Preparation of adhesiveness evaluation sample> A chlorobenzene solution of P3HT-b-P2EEEA obtained in Example 1 was prepared (solution concentration: 20 mg / mL). The solution was drop-cast onto a glass substrate at room temperature to prepare a sample for evaluating adhesion.

[0158] <Adhesion evaluation> Adhesion Evaluation A tape test was performed in which adhesive tape was applied to the sample and then quickly peeled off, and the results were evaluated according to the following criteria. The evaluation results are shown in Table 1. <Judgment criteria> ◯: No peeling of the film was observed by the tape test. ×: Peeling of the film was observed by tape test.

[0159] [Example 4] In Example 3, a sample for evaluating adhesiveness was prepared and the adhesiveness was evaluated in the same manner as in Example 3, except that the solute was changed to P3HT-b-PVC obtained in the above Example 2. The results are shown in Table 1.

[0160] [Comparative Example 1] A sample for evaluating adhesion was prepared in the same manner as in Example 3, except that the solute was changed to P3HT obtained in the above Synthesis Example 2, and the adhesion was evaluated. The results are shown in Table 1.

[0161] [Comparative Example 2] In Example 3, a sample for evaluating adhesion was prepared in the same manner as in Example 3, except that the solute was changed to a mixture (30:70 mass ratio) of P3HT obtained in the above Synthesis Example 2 and P2EEEA obtained in the above Synthesis Example 3, and the adhesion was evaluated. The results are shown in Table 1.

[0162] [Comparative Example 3] In Example 3, except that the solute was changed to a mixture (80:20 weight ratio) of P3HT obtained in Synthesis Example 2 and PVC obtained in Synthesis Example 5, and the solvent was changed to tetrahydrofuran, an adhesion evaluation sample was prepared in the same manner, and the adhesion evaluation was performed. The results are shown in Table 1.

[0163] [Example 7] <Preparation of adhesiveness evaluation sample> Ultrapure water was added to a 15% by mass aqueous dispersion of tin (IV) oxide (manufactured by Alfa Aesar) to prepare a 7.5% by mass aqueous dispersion of tin oxide. In a nitrogen atmosphere, N,N-dimethylformamide was added as a solvent so that the concentration of lead (II) iodide was 1.3 mol / L, and the mixture was then heated and stirred at 100° C. for 1 hour to prepare perovskite coating solution 1. Under a nitrogen atmosphere, isopropyl alcohol was added as a solvent to formamidine hydroiodide (FAI), methylamine hydrobromide (MABr), and methylamine hydrochloride (MACl) so that the total concentration was 0.54 mol / L (mass ratio 10:1:1.5) to prepare perovskite coating solution 2. A dichlorobenzene solution of PVC-b-PTAA-b-PVC obtained in Example 5 above was prepared (solution concentration: 32 mg / mL). The above-mentioned tin (IV) oxide aqueous dispersion was applied by spin coating on a glass substrate, and heated at 150°C for 10 minutes to form a tin oxide layer with a thickness of 50 nm. In a nitrogen atmosphere, the substrate was spin-coated with perovskite coating solution 1 heated to 100°C, and heated at 100°C for 10 minutes to form a lead iodide layer. On top of this, perovskite coating solution 2 was spin-coated, and heated at 150°C for 20 minutes to form an organic-inorganic hybrid perovskite semiconductor compound (thickness 650 nm). Furthermore, the above-mentioned dichlorobenzene solution of PVC-b-PTAA-b-PVC was spin-coated on top of this, and heated at 90°C for 5 minutes to prepare an adhesion evaluation sample.

[0164] <Adhesion evaluation> Adhesion Evaluation A tape test was performed in which adhesive tape was applied to the sample and then quickly peeled off, and the results were evaluated according to the following criteria. The evaluation results are shown in Table 2. <Judgment criteria> ◯: No peeling of the film was observed by the tape test. ×: Peeling of the film was observed by tape test.

[0165] [Example 8] In Example 7, except that the dichlorobenzene solution of PVC-b-PTAA-b-PVC was changed to a dichlorobenzene solution of PVC-b-PTAA-b-PVC to which 10% by mass of 4-isopropyl-4'-methyldiphenyliodonium tetrakis(pentafluorophenyl)borate (TPFB) was added relative to PVC-b-PTAA-b-PVC, an adhesion evaluation sample was prepared in the same manner, and the adhesion evaluation was performed. The results are shown in Table 2.

[0166] [Example 9] In Example 7, except that the dichlorobenzene solution of PVC-b-PTAA-b-PVC was changed to a dichlorobenzene solution of PVC-b-PTAA-b-PVC to which 25% by mass of TPFB was added to PVC-b-PTAA-b-PVC, an adhesion evaluation sample was prepared in the same manner, and the adhesion evaluation was performed. The results are shown in Table 2.

[0167] [Example 10] In Example 7, except that the dichlorobenzene solution of PVC-b-PTAA-b-PVC was changed to a dichlorobenzene solution of PVC-b-PTAA-b-PVC to which 50% by mass of TPFB was added to PVC-b-PTAA-b-PVC, an adhesion evaluation sample was prepared in the same manner, and the adhesion evaluation was performed. The results are shown in Table 2.

[0168] [Example 11] In Example 7, a sample for evaluating adhesion was prepared and the adhesion was evaluated in the same manner, except that the dichlorobenzene solution of PVC-b-PTAA-b-PVC was replaced with the dichlorobenzene solution of PTAA-b-PVC obtained in Example 6. The results are shown in Table 2.

[0169] [Example 12] In Example 8, a dichlorobenzene solution of PVC-b-PTAA-b-PVC in which 10% by mass of TPFB was added to PVC-b-PTAA-b-PVC was used instead of a dichlorobenzene solution of PTAA-b-PVC in which 10% by mass of TPFB was added to PTAA-b-PVC. The adhesiveness evaluation sample was prepared in the same manner, and the adhesiveness was evaluated. The results are shown in Table 2.

[0170] [Example 13] In Example 9, a dichlorobenzene solution of PVC-b-PTAA-b-PVC in which 25% by mass of TPFB was added to PVC-b-PTAA-b-PVC was replaced with a dichlorobenzene solution of PTAA-b-PVC in which 25% by mass of TPFB was added to PTAA-b-PVC. The adhesiveness evaluation sample was prepared in the same manner, and the adhesiveness was evaluated. The results are shown in Table 2.

[0171] [Example 14] In Example 10, except that the dichlorobenzene solution of PVC-b-PTAA-b-PVC in which 50% by mass of TPFB was added to PVC-b-PTAA-b-PVC was changed to a dichlorobenzene solution of PTAA-b-PVC in which 50% by mass of TPFB was added to PTAA-b-PVC, an adhesiveness evaluation sample was prepared in the same manner and adhesiveness evaluation was performed. The results are shown in Table 2.

[0172] [Comparative Example 4] In Example 7, except that the dichlorobenzene solution of PVC-b-PTAA-b-PVC was replaced with an anisole solution of poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA, manufactured by Aldrich), an adhesive evaluation sample was prepared in the same manner and the adhesiveness was evaluated. The results are shown in Table 2.

[0173] [Comparative Example 5] In Example 8, except that the dichlorobenzene solution of PVC-b-PTAA-b-PVC in which 10% by mass of TPFB was added to PVC-b-PTAA-b-PVC was changed to an anisole solution of PTAA in which 10% by mass of TPFB was added to PTAA, an adhesion evaluation sample was prepared in the same manner, and the adhesion evaluation was performed. The results are shown in Table 2.

[0174] [Comparative Example 6] In Example 9, a dichlorobenzene solution of PVC-b-PTAA-b-PVC in which 25% by mass of TPFB was added to PVC-b-PTAA-b-PVC was replaced with an anisole solution of PTAA in which 25% by mass of TPFB was added to PTAA, and an adhesiveness evaluation sample was prepared and adhesiveness evaluation was performed in the same manner. The results are shown in Table 2.

[0175] [Comparative Example 7] In Example 10, except that the dichlorobenzene solution of PVC-b-PTAA-b-PVC in which 50% by mass of TPFB was added to PVC-b-PTAA-b-PVC was replaced with an anisole solution of PTAA in which 50% by mass of TPFB was added to PTAA, an adhesion evaluation sample was prepared in the same manner, and the adhesion evaluation was performed. The results are shown in Table 2.

[0176] [Table 1]

[0177] In Table 1, no peeling of the film was observed by the tape test in the block copolymers of Examples 3 and 4. On the other hand, peeling of the film was observed by the tape test in Comparative Example 1. From these results, it can be seen that the block copolymers of Examples 3 and 4 have an adhesive property improving effect due to the introduction of adhesive blocks. In Comparative Examples 2 and 3, which are mixtures of the polymer constituting the organic semiconductor block of the block copolymer and the polymer constituting the adhesive block, peeling of the film was observed in the tape test. It is considered that in these mixtures, the organic semiconductor block aggregated in the mixture, which is why no improvement in adhesion was observed. On the other hand, in the block copolymers of Examples 3 and 4, the organic semiconductor block and the adhesive block were phase-separated at the nano level, which prevented the aggregation of the organic semiconductor block, and it is believed that this resulted in improved adhesive properties.

[0178] [Table 2]

[0179] In Table 2, in Examples 7 to 14 using the block copolymer of the present invention, no peeling of the film was observed by the tape test, regardless of the presence or absence of TPFB and the amount of TPFB added, whereas in Comparative Examples 4 to 7, peeling of the film was observed. From the above, it was confirmed that the block copolymer of the present invention in which the organic semiconductor block and the adhesive block are bonded via a linking group can improve adhesiveness.

Claims

1. A block copolymer having semiconductor properties and adhesive properties, characterized in that the block copolymer is formed by bonding an organic semiconductor block having a π-conjugated polymer skeleton and an adhesive block having a vinyl polymer skeleton via a linking group.

2. The block copolymer according to claim 1 , wherein the organic semiconductor block is represented by the following formula (I) or the following formula (IV): 【Chemistry 1】 In formula (I), A represents a monomer unit having a thiophene ring which may have a substituent, or a monomer unit having a triarylamine skeleton which may have a substituent. R 1 represents a direct bond, a linear or branched alkylene group, or an arylene group which may have a substituent. 2 -) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). R 2 represents a hydrogen atom, a linear or branched alkyl group, a linear or branched alkoxy group, or an aryl group which may have a substituent. n is a natural number of 2 or more. The wavy line represents a bond to the linking group. 【Chemistry 2】 (In formula (IV), A 1 represents a monomer unit having a thiophene ring which may have a substituent, or a monomer unit having a triarylamine skeleton which may have a substituent. R 11 and R 21 each independently represents a direct bond, a linear or branched alkylene group, or an arylene group which may have a substituent. 2 -) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). n is a natural number of 2 or more. The wavy line represents a bond to the linking group.

3. 3. The block copolymer according to claim 2, wherein A in the formula (I) is a thiophene unit having an alkyl group as a substituent.

4. A in the formula (IV) 1 The block copolymer according to claim 2, characterized in that is a triarylamine unit having an alkyl group as a substituent.

5. 2. The block copolymer according to claim 1, wherein the adhesive block is represented by the following formula (II): 【Chemistry 3】 (In formula (II), R 3 represents a hydrogen atom or a linear or branched alkyl group. R 4 represents a linear or branched alkyl group. 2 -) may be substituted with an oxygen atom (-O-). R 5 represents a hydrogen atom or a linear or branched alkyl group. 2 -) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). R 6 represents a direct bond or a linear or branched alkylene group. 2 -) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). m is a natural number of 2 or more. The wavy line represents a bond to the linking group.

6. The block copolymer according to claim 1, characterized in that the adhesive block is represented by the following formula (III): 【Chemistry 4】 (In formula (III), R 7 ~R 11 Each independently represents a hydrogen atom or a hydroxyl group. 7 ~R 11 At least one of R is a hydroxyl group. 12 represents a hydrogen atom or a linear or branched alkyl group. 2 -) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). R 13 represents a direct bond or a linear or branched alkylene group. 2 -) may be substituted with an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl group (-C(=O)-), or a thiocarbonyl group (-C(=S)-). k is a natural number of 2 or more. The wavy line represents a bond to the linking group.

7. 2. The block copolymer according to claim 1, wherein the linking group is a divalent group of a triazole ring.

8. An organic film comprising the block copolymer according to any one of claims 1 to 7.