Active material for lithium secondary batteries, electrode for lithium secondary batteries, lithium secondary battery, and battery pack

The niobium titanium composite oxide active material in lithium secondary batteries addresses low energy density and stability issues by enhancing lithium ion conductivity and stability, enabling rapid charging and discharging with improved cycle life.

JP2024133166AInactive Publication Date: 2024-10-01KK TOSHIBA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024110935
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing lithium secondary batteries using titanium oxide as a negative electrode face challenges with low energy density, poor capacity per weight, and instability during rapid charging and discharging due to metallic lithium dendrite formation, leading to potential heat generation and ignition risks.

Method used

A niobium titanium composite oxide active material is developed, comprising phases like Nb2TiO7, Nb10Ti2O29, Nb14TiO37, and Nb24TiO64, with controlled particle size distribution and inclusion of potassium and phosphorus, enhancing lithium ion conductivity and stability, while maintaining high crystallinity.

Benefits of technology

The active material achieves improved energy density, rapid charging and discharging capabilities, and extended cycle life by stabilizing lithium ion insertion and preventing overcharge, reducing the risk of internal short circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133166000001_ABST
    Figure 2024133166000001_ABST
Patent Text Reader

Abstract

To provide an active material capable of realizing a secondary battery capable of indicating excellent input / output characteristics and cycle lifetime characteristics.SOLUTION: An active material is provided. The active material includes an Nb2TiO7 phase and at least one Nb rich phase selected from an Nb10Ti2O29 phase, an Nb14TiO37 phase, and an Nb24TiO64 phase. The active material contains kalium and phosphor, and a total concentration of kalium and phosphor occupying the active material is within a range of 0.01 mass% or more and 5.00 mass% or less. An average crystallite diameter ranges from 80 nm to 150 nm. In a particle size distribution chart obtained by a laser diffraction scattering method, D10 is 0.3 μm or more and D90 is 10 μm or less. The active material satisfies a peak intensity ratio represented by the following formula (1): 0<IB / IA≤0.25.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THE DISCLOSURE The present invention relates to an active material, an electrode, a secondary battery, a battery pack, and a vehicle.

[0002] In recent years, research and development of secondary batteries such as non-aqueous electrolyte secondary batteries, such as lithium ion secondary batteries, as high energy density batteries, has been actively promoted. Secondary batteries such as non-aqueous electrolyte secondary batteries are expected to be used as power sources for vehicles such as hybrid electric vehicles and electric vehicles, and for uninterruptible power sources for mobile phone base stations. Therefore, in addition to high energy density, secondary batteries are also required to have excellent other performances such as rapid charge and discharge performance and long-term reliability. For example, secondary batteries capable of rapid charge and discharge not only significantly reduce charging time, but also improve the power performance of vehicles such as hybrid electric vehicles and efficiently recover regenerative energy from power.

[0003] In order to enable rapid charging and discharging, it is necessary that electrons and lithium ions can move quickly between the positive and negative electrodes. However, when a battery using a carbon-based negative electrode is repeatedly charged and discharged rapidly, dendrites of metallic lithium are precipitated on the electrode, which may cause heat generation or fire due to an internal short circuit.

[0004] Therefore, batteries that use metal composite oxides instead of carbonaceous materials for the anode have been developed. Among them, batteries that use titanium oxide for the anode are capable of stable rapid charging and discharging and have a longer life than batteries that use carbon-based anodes.

[0005] However, titanium oxide has a higher potential relative to metallic lithium than carbonaceous materials, i.e., it is more noble. Moreover, titanium oxide has a low capacity per weight. Therefore, batteries using titanium oxide in the negative electrode have a problem of low energy density.

[0006] For example, the electrode potential of titanium oxide is about 1.5 V (vs. Li / Li) based on metallic lithium. +), which is higher (more noble) than the potential of a carbon-based negative electrode. The potential of titanium oxide is the potential of Ti when electrochemically inserting and extracting lithium. 3+ and Ti 4+ The charge is electrochemically limited because it is caused by an oxidation-reduction reaction between the two. + It is also true that rapid charging and discharging of lithium ions can be performed stably at high electrode potentials of around 1000 kV. Therefore, it has been difficult to lower the electrode potential in order to improve the energy density.

[0007] On the other hand, in terms of capacity per unit weight, the theoretical capacity of titanium dioxide (anatase structure) is about 165 mAh / g, and Li4Ti5O 12 The theoretical capacity of spinel-type lithium-titanium composite oxides such as those shown in Fig. 1 is about 180 mAh / g. On the other hand, the theoretical capacity of general graphite-based electrode materials is 385 mAh / g or more. Thus, the capacity density of titanium oxides is significantly lower than that of carbon-based negative electrodes. This is because the crystal structure of titanium oxides has few sites for absorbing lithium and lithium is easily stabilized in the structure, resulting in a decrease in the actual capacity.

[0008] In view of the above, new electrode materials containing Ti and Nb are being investigated. Such niobium titanium composite oxide materials are expected to have high charge / discharge capacities. In particular, the composite oxide represented by TiNb2O7 has a high theoretical capacity of more than 380 mAh / g. Therefore, the niobium titanium composite oxide is Li4Ti5O 12 However, it has been difficult to significantly reduce both the fine powder and the coarse particles while maintaining high crystallinity, which has led to problems with input / output characteristics and cycle life characteristics. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2019-169343 A [Non-patent literature]

[0010] [Non-Patent Document 1] M.Gasperin, Journal of Solid State Chemistry 53, pp144-147 (1984) [Non-Patent Document 2] Edited by Izumi Nakai et al.: "Practical Application of Powder X-ray Diffraction", First Edition, Asakura Publishing, February 10, 2002, p.97-115 Summary of the Invention [Problem to be solved by the invention]

[0011] The object is to provide an active material capable of realizing a secondary battery capable of exhibiting excellent input / output characteristics and cycle life characteristics, an electrode containing this active material, a secondary battery equipped with this electrode, a battery pack equipped with this secondary battery, and a vehicle equipped with this battery pack. [Means for solving the problem]

[0012] According to a first embodiment, an active material for a lithium secondary battery is provided. The active material includes a Nb2TiO7 phase and a Nb 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 and at least one Nb-rich phase selected from the group consisting of Nb-rich phases. This active material contains potassium and phosphorus, and the total concentration of potassium and phosphorus in the active material is in the range of 0.01 mass% or more and 5.00 mass% or less. The average crystallite diameter is in the range of 80 nm to 150 nm. In a particle size distribution chart obtained by a laser diffraction scattering method, D10 is 0.3 μm or more and D90 is 10 μm or less. The active material satisfies the peak intensity ratio represented by the following formula (1).

[0013] 0 B / I A ≦0.25 (1) ​In formula (1), I A is the peak intensity of the maximum peak that appears at 2θ of 26.0±0.1° and is attributed to the Nb2TiO7 phase in the wide-angle X-ray diffraction peaks using CuKα radiation as an X-ray source, and I B is the peak intensity of the maximum diffraction peak which appears at 2θ of 24.9±0.2° and is attributed to the Nb-rich phase.

[0014] According to a second embodiment, there is provided an electrode for a lithium secondary battery, which includes the active material for a lithium secondary battery according to the first embodiment.

[0015] According to a third embodiment, there is provided a lithium secondary battery comprising a positive electrode, a negative electrode, and an electrolyte. The negative electrode is the lithium secondary battery electrode according to the second embodiment.

[0016] According to a fourth embodiment, there is provided a battery pack including the lithium secondary battery according to the third embodiment.

[0017] According to a fifth embodiment, a vehicle is provided that is equipped with the battery pack according to the fourth embodiment. [Brief description of the drawings]

[0018] [Figure 1] Schematic diagram showing the crystal structure of niobium titanium composite oxide Nb2TiO7. [Diagram 2] FIG. 2 is a schematic diagram showing the crystal structure of FIG. 1 as viewed from another direction. [Diagram 3] FIG. 1 is a plan view that illustrates a particle to be measured in a transmission electron microscope (TEM) observation. [Figure 4] FIG. 1 is a cross-sectional view illustrating an example of a secondary battery according to an embodiment. [Diagram 5] 5 is an enlarged cross-sectional view of a portion A of the secondary battery shown in FIG. 4. [Figure 6] FIG. 4 is a partially cutaway perspective view illustrating a schematic diagram of another example of a secondary battery according to an embodiment. [Figure 7] FIG. 7 is an enlarged cross-sectional view of a portion B of the secondary battery shown in FIG. 6. [Figure 8] FIG. 1 is a perspective view illustrating an example of a battery pack according to an embodiment. [Figure 9] FIG. 1 is an exploded perspective view illustrating an example of a battery pack according to an embodiment. [Figure 10] 10 is a block diagram showing an example of an electric circuit of the battery pack shown in FIG. 9. [Figure 11] 1 is a cross-sectional view illustrating an example of a vehicle according to an embodiment. [Figure 12] FIG. 13 is a diagram illustrating another example of a vehicle according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, the embodiments will be described with reference to the drawings. Note that the same reference numerals are used to designate common components throughout the embodiments, and duplicated descriptions will be omitted. Each figure is a schematic diagram for explaining the embodiments and for facilitating understanding thereof, and the shapes, dimensions, ratios, etc. may differ from those of the actual device, but these can be appropriately modified in design by taking into consideration the following explanation and known techniques.

[0020] Conventionally, when raw materials containing unavoidable impurities are sintered to prepare a niobium titanium composite oxide, the melting point is lowered due to the influence of the impurities, so that coarse particles tend to be generated. Coarse particles are particles that have grown to a large primary particle size. Since coarse particles are easily broken during charging and discharging, it is difficult to form an electronic conductive path between active material particles in an active material containing coarse particles, which may result in a decrease in rate characteristics and a decrease in cycle life characteristics. The crystallinity of the coarse particles grown due to the decrease in melting point is high, so the Mohs hardness is also high. Therefore, for example, when the powder containing the generated coarse particles is pulverized in order to increase the volumetric energy density, not only does the crystallinity decrease, but a lot of fine powder is generated. Since the specific surface area of ​​the generated fine powder is large, it causes a side reaction with the electrolyte during charging and discharging, which is one of the factors that reduces the cycle life characteristics.

[0021] On the other hand, if firing is performed at a temperature lower than usual in order to make the generated coarse particles easier to pulverize, the crystallinity of the particles decreases and the number of unreacted or under-reacted particles increases, which also results in a decrease in rate characteristics, etc. In other words, it has been difficult to obtain a niobium titanium composite oxide powder having high crystallinity and a desirable particle size distribution by simply lowering the firing temperature or pulverizing the powder after firing.

[0022] (First embodiment) According to a first embodiment, an active material is provided. The active material comprises a Nb2TiO7 phase and a Nb 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 and at least one Nb-rich phase selected from the group consisting of Nb-rich phases. This active material contains potassium and phosphorus, and the total concentration of potassium and phosphorus in the active material is in the range of 0.01 mass% or more and 5.00 mass% or less. The average crystallite diameter is in the range of 80 nm to 150 nm. In a particle size distribution chart obtained by a laser diffraction scattering method, D10 is 0.3 μm or more and D90 is 10 μm or less. The active material satisfies the peak intensity ratio represented by the following formula (1).

[0023] 0 B / I A ≦0.25 (1) In formula (1), I A is the peak intensity of the maximum peak that appears at 2θ of 26.0±0.1° and is attributed to the Nb2TiO7 phase in the wide-angle X-ray diffraction peaks using CuKα radiation as an X-ray source, and I B is the peak intensity of the maximum diffraction peak which appears at 2θ of 24.9±0.2° and is attributed to the Nb-rich phase.

[0024] The reason why the active material according to the first embodiment can exhibit excellent input / output characteristics and cycle life characteristics will be described. First, the Nb2TiO7 phase will be described.

[0025] ​ The main phase contained in the active material according to the embodiment is a niobium titanium composite oxide phase represented by a representative composition of Nb2TiO7. The composition of the niobium titanium composite oxide is not limited thereto, but it is preferable that the niobium titanium composite oxide has a symmetry of the space group C2 / m and has a crystal structure having the atomic coordinates described in Non-Patent Document 1 (Journal of Solid State Chemistry 53, pp144-147 (1984)).

[0026] Niobium titanium composite oxide mainly exhibits a monoclinic crystal structure. As an example, schematic diagrams of the crystal structure of monoclinic Nb2TiO7 are shown in Figures 1 and 2.

[0027] As shown in FIG. 1, in the crystal structure of monoclinic Nb2TiO7, metal ions 101 and oxide ions 102 constitute a skeletal structure portion 103. Nb ions and Ti ions are randomly arranged at the positions of the metal ions 101 in a ratio of Nb:Ti=2:1. These skeletal structure portions 103 are arranged alternately in a three-dimensional manner, so that void portions 104 exist between the skeletal structure portions 103. These void portions 104 act as hosts for lithium ions. Lithium ions can be inserted into this crystal structure in an amount of 0 moles to a maximum of 5.0 moles. Therefore, the composition when 0 to 5.0 moles of lithium ions are inserted is Li x It can be expressed as Nb2TiO7(0≦x≦5).

[0028] In FIG. 1, regions 105 and 106 are portions that have two-dimensional channels in the

[0100] and

[0010] directions. As shown in FIG. 2, the crystal structure of monoclinic Nb2TiO7 has a void portion 107 in the

[0001] direction. This void portion 107 has a tunnel structure that is favorable for the conduction of lithium ions, and serves as a conductive path in the

[0001] direction that connects regions 105 and 106. The existence of this conductive path enables lithium ions to travel between regions 105 and 106. In addition, the niobium titanium composite oxide has a low resistance of 1.5 V (vs. Li / Li +Therefore, an electrode containing the niobium titanium composite oxide as an active material can realize a battery capable of stable repeated rapid charging and discharging.

[0029] Furthermore, in the above crystal structure, when lithium ions are inserted into the voids 104, the metal ions 101 constituting the framework are reduced to trivalent, thereby maintaining the electrical neutrality of the crystal. In the niobium titanium composite oxide, not only are Ti ions reduced from tetravalent to trivalent, but Nb ions are reduced from pentavalent to trivalent. This results in a large reduction valence per active material weight. Therefore, even if many lithium ions are inserted, it is possible to maintain the electrical neutrality of the crystal. This results in a higher energy density than compounds such as titanium oxide that contain only tetravalent cations. In addition, the Nb2TiO7 phase has a high energy density compared to Nb, which will be described later. 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 This is because it has a superior weight energy density compared to the Nb 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 This is because the phase contains a large number of Nb atoms per mole, i.e., the weight per mole is large.

[0030] Next, Nb 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 The phase will be explained. The basic skeletal structure is similar to the crystal structure of monoclinic Nb2TiO7 shown in Figures 1 and 2. When lithium ions are inserted into the voids 104, the metal ions 101 that make up the skeletal structure are reduced to trivalent ions, thereby maintaining the electrical neutrality of the crystal. 10 Ti2O 29 When lithium ions are inserted into the phase, the composition is LixNb 10 Ti2O29 (0≦x≦22). Nb 14 TiO 37 When lithium ions are inserted into the phase, the composition is LixNb 14 TiO 37 (0≦x≦29). Nb 24 TiO 64 When lithium ions are inserted into the phase, the composition is LixNb 24 TiO 64 It can be expressed as (0≦x≦49).

[0031] Niobium-rich Nb 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 In the Nb2TiO7 phase, the amount of Nb ions reduced from pentavalent to trivalent is greater than in the Nb2TiO7 phase. Therefore, the reduction valence per mole of active material is large. Therefore, even if many lithium ions are inserted, it is possible to maintain the electrical neutrality of the crystal. 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 At least one Nb-rich phase selected from the group consisting of Nb2TiO7 phases can stably maintain a crystal structure even when lithium ions are excessively inserted compared to the Nb2TiO7 phase. As a result, even if lithium ions are excessively inserted into the Nb-rich phase, the active material particles can be stably charged and discharged. That is, the Nb-rich phase has excellent overcharge resistance. In this specification, the Nb-rich phase means a niobium titanium composite oxide phase having an Nb / Ti ratio greater than 2. The active material according to the embodiment may be a niobium titanium composite oxide including the Nb2TiO7 phase and the Nb-rich phase.

[0032] On the other hand, the reduction valence per active material weight of the Nb-rich phase is smaller than that of the Nb2TiO7 phase. In other words, the weight per mole of the Nb-rich phase is large, and therefore the weight energy density is inferior to that of the Nb2TiO7 phase.

[0033] The active material is not only Nb2TiO7 phase but also Nb 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 When the active material contains at least one Nb-rich phase selected from the group consisting of Nb-rich and Nb-rich phases, the potential of the Nb-rich phase is preferentially decreased when the secondary battery is overcharged. Therefore, during charging, the potential rise of the positive electrode can be suppressed while maintaining a constant charging voltage. As a result, the active material according to the embodiment can suppress the generation of oxidizing gas in the positive electrode and the deterioration of the positive electrode, and therefore has excellent cycle life characteristics.

[0034] Furthermore, the Nb-rich phase can alleviate the crystal lattice distortion caused by Li being inserted and removed during charging and discharging. This is because the bond between the oxide ions and the Nb ions that make up the skeleton is stronger. Therefore, the deformation of the crystal lattice during Li charging and discharging can be suppressed, resulting in excellent cycle life characteristics.

[0035] In order to obtain the above-mentioned advantages, it is effective for the active material to contain a predetermined amount of Nb-rich phase. B / I A ) is an amount that satisfies formula 1. However, in an active material containing an Nb-rich phase, as described above, the bond between the oxide ions and the Nb ions that constitute the skeleton becomes strong, and many particles with high hardness are generated. As a result, there are many particles with large particle diameters in the active material, and since D90 is large, there is a problem that it is difficult to obtain high input / output characteristics. In addition, when hard particles are crushed to reduce D90, the crystallinity decreases and the cycle life characteristics decrease. Therefore, it has been difficult to achieve both high input / output characteristics and cycle life in an active material containing an Nb-rich phase.

[0036] The active material according to the embodiment includes potassium element (K) and phosphorus element (P). At least one of potassium and phosphorus is preferably present at the particle interface of the active material particles. Both potassium and phosphorus are present, for example, as oxides. A part of potassium and a part of phosphorus may be incorporated into the crystal phase. Potassium has an effect of lowering the melting point of the active material, and high crystallinity can be obtained at a relatively low sintering temperature. On the other hand, phosphorus has an effect of suppressing particle growth by being present at least in a part of the surface of the active material particles, and preventing the active material particles from necking together and becoming coarse. By the coexistence of both potassium and phosphorus in the active material, even in an active material containing a Nb-rich phase, it is possible to reduce D90 and increase D10, and obtain high crystallinity, and as a result, it is possible to achieve both high input / output characteristics and cycle life.

[0037] The total concentration of potassium and phosphorus in the active material is in the range of 0.01% by mass or more and 5.00% by mass or less. If the concentration is less than 0.01% by mass, the above effect cannot be obtained. If the concentration exceeds 5.00% by mass, potassium occupies the site where Li should be inserted, resulting in a decrease in battery capacity, or the oxide containing phosphorus becomes a resistance component at the particle interface, resulting in a decrease in input / output characteristics. The total concentration of potassium and phosphorus in the active material is preferably in the range of 0.020% by mass or more and 4.00% by mass or less, more preferably in the range of 0.050% by mass or more and 2.50% by mass or less. The total concentration of potassium and phosphorus in the active material may be in the range of more than 0.200% by mass or less and 5.00% by mass or less.

[0038] The concentration of potassium contained in the active material (hereinafter referred to as "C K The potassium concentration C is, for example, in the range of 0.005% by mass to 5.00% by mass, and preferably in the range of 0.01% by mass to 0.2% by mass. K If is too high, the site where Li should be inserted may be occupied by potassium, which may reduce the battery capacity. Alternatively, the flux effect of potassium may cause abnormal particle growth, which may hinder smooth insertion and desorption of Li, which may reduce the input / output characteristics.

[0039] The phosphorus concentration in the active material (hereinafter referred to as "C P ") is, for example, in the range of 0.001% by mass to 1.00% by mass, and preferably in the range of 0.005% by mass to 0.05% by mass. P If the temperature is excessively high, the oxide containing phosphorus may become a resistive component at the particle interface, resulting in a decrease in input / output characteristics.

[0040] Potassium concentration in active material C K and the phosphorus concentration in the active material, C P Ratio to (C K / C P ) is, for example, in the range of 1.0 to 50.0, and preferably in the range of 2.0 to 20.0. K / C P ) may be in the range of 2.0 to 50.0, or may be in the range of 5.0 to 40.0. In the active material according to the embodiment, it is preferable that the potassium concentration is higher than the phosphorus concentration. This is because phosphorus has a strong tendency to remain on the particle surface and has the function of suppressing necking and abnormal growth of particles, but if the phosphorus concentration is higher than the potassium concentration, sufficient crystal growth is not promoted, and the phosphorus remaining on the active material surface hinders the movement of Li ions. This leads to, for example, a decrease in input / output characteristics.

[0041] In a particle size distribution chart obtained by a laser diffraction scattering method for the active material according to the embodiment, the volume frequency 10% (D10) is 0.3 μm or more. A high value of D10 means less fine powder. When D10 is 0.3 μm or more, the active material contains less fine powder, so that side reactions with the electrolyte can be reduced. As a result, a secondary battery exhibiting excellent rate characteristics and cycle life characteristics can be realized. D10 is preferably in the range of 0.4 μm to 1.5 μm, and more preferably in the range of 0.5 μm to 1.0 μm. When D10 is larger than 1.5 μm, the rapid charge / discharge performance tends to be reduced.

[0042] In addition, in the particle size distribution chart, the volume frequency 90% (D90) is 10 μm or less. A low D90 value means a small number of coarse particles. When D90 is 10 μm or less, the active material contains few coarse particles, so that the coarse particles are less likely to crack during charging and discharging. Since the coarse particles do not crack, it is easy to maintain a good electronic conductive path, and side reactions caused by an increase in the specific surface area can also be reduced. Therefore, excellent rate characteristics and cycle life characteristics can be achieved. According to one example, D90 is 5.0 μm or more. D90 is preferably within the range of 6.0 μm to 9.0 μm.

[0043] Conventionally, in order to make D90 10 μm or less, it was necessary to lower the sintering temperature or subject the sintered powder to strong pulverization. Therefore, it was difficult to reduce D90 and increase D10 while maintaining high crystallinity. However, since the active material according to the embodiment contains potassium and phosphorus at a predetermined concentration, it is possible to suppress necking between particles while increasing crystallinity at the annealing stage during active material synthesis. As a result, not only is the number of coarse particles reduced by suppressing particle growth during annealing, but the particles are likely to crumble even if the pulverization after annealing is performed under mild conditions. Therefore, it is possible to crush the coarse particles and reduce D90 without reducing the crystallinity of the active material. Furthermore, the generation of fine powder can also be suppressed by pulverization under mild conditions. That is, it is possible to increase D10. As a result, even if a Nb-rich phase with high hardness of the active material particles coexists, a preferable particle size distribution can be obtained without strong pulverization.

[0044] The average crystallite diameter of the active material is, for example, in the range of 80 nm to 150 nm, preferably in the range of 90 nm to 150 nm, and more preferably in the range of 95 nm to 120 nm. The average crystallite diameter of 80 nm or more means that the crystal structure is firmly formed. Such a crystal structure is not easily deteriorated even when rapid charging and discharging are repeated, which contributes to improving the life performance of the secondary battery. If the average crystallite diameter is larger than 150 nm, the diffusion distance of Li ions becomes longer, and the mobility of Li ions during rapid charging and discharging may decrease.

[0045] Moreover, the active material according to the embodiment satisfies the peak intensity ratio represented by the following formula (1). B / I A ≦0.25 (1) In formula (1), I A is the peak intensity of the maximum peak that appears at 2θ of 26.0±0.1° and is attributed to the Nb2TiO7 phase in the wide-angle X-ray diffraction peaks using CuKα radiation as an X-ray source, and I B The diffraction peak appears at 2θ of 24.9±0.2°, and Nb 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 The wide-angle X-ray diffraction method is performed as described below.

[0046] Peak Intensity I A is the peak intensity (peak height) attributable to the Nb2TiO7 phase. This peak is the peak with the maximum peak intensity within the 2θ range of 26.0±0.1°. Peak intensity I A A larger value means that the weight of the Nb2TiO7 phase in the active material is large.

[0047] Peak Intensity I B is Nb 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 The peak intensity (peak height) attributable to at least one Nb-rich phase selected from the group consisting of Nb-rich phases. This peak is a peak having a maximum peak intensity within the range of 2θ of 24.9±0.2°. B A larger value means that the weight of the Nb-rich phase in the active material is large.

[0048] ​As described above, when the active material contains a Nb-rich phase, the overcharge resistance is improved, and the life characteristics of the secondary battery are improved. However, when the Nb-rich phase is increased without limit, the overcharge resistance is not improved by the amount of increase. In addition, the peak intensity ratio I B / I A If is too large, the active material becomes heavy, reducing the weight energy density. 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 The difference in the volume expansion rate between the Nb-rich phase and at least one Nb-rich phase selected from the group consisting of Nb-rich phases during charge and discharge can cause the electrode to warp or the active material particles to crack, which is not preferable. B / I A ) is less than or equal to 0.25.

[0049] Peak intensity ratio I B / I A should be greater than 0, but the peak intensity ratio I B / I A If is excessively small, the weight of the Nb-rich phase becomes insufficient, and the overcharge resistance and cycle life tend to decrease.

[0050] Peak intensity ratio I B / I A is preferably 0.005 or more and 0.20 or less, more preferably 0.01 or more and 0.15 or less, and even more preferably 0.05 or more and 0.1 or less.

[0051] The active material according to the embodiment may further contain at least one additive element selected from the group consisting of Si, Fe, Ta, Na, Y, Al, and Sn. The amount of the additive element contained in the active material is preferably 0.5 atm% or less with respect to the Nb element in the active material. When the active material contains at least one selected from the group consisting of Fe, Ta, Y, Al, and Sn, the electronic conductivity of the active material can be increased. When the active material contains at least one selected from the group consisting of Si and Na, the capacity decrease due to the Nb-rich phase, which has a large weight, can be reduced.

[0052] The additive element may be Nb2TiO7 phase, and Nb 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 The active material may contain at least one Nb-rich phase selected from the group consisting of Nb2TiO7 and Nb-rich phases. Alternatively, both the Nb2TiO7 phase and the Nb-rich phase may contain an additive element. In either case, however, the content of the additive element is preferably 0.5 atm% or less with respect to the Nb element in the active material.

[0053] The crystal structure of the active material particles can be observed, for example, by powder X-ray diffraction measurement, transmission electron microscope (TEM) observation, etc. The details of these measurement methods will be described later.

[0054] Next, the morphology and specific surface area of ​​the active material according to the embodiment will be described.

[0055] <Form> The form of the active material (niobium titanium composite oxide) according to the embodiment is not particularly limited. The active material may be in the form of primary particles containing, for example, an Nb2TiO7 phase, an Nb-rich phase, potassium and phosphorus. Alternatively, the active material may be a plurality of particles in which primary particles consisting of a single Nb2TiO7 phase and primary particles consisting of a single Nb-rich phase are mixed, and potassium and phosphorus are contained in at least a part of these particles. The above-mentioned primary particles may be aggregated to form secondary particles. The particles of the niobium titanium composite oxide may be a mixture of primary particles and secondary particles.

[0056] The niobium titanium composite oxide particles may have a carbon-containing layer on the surface. The carbon-containing layer may be attached to the surface of the primary particles, or may be attached to the surface of the secondary particles. Alternatively, the niobium titanium composite oxide particles may contain secondary particles formed by agglomeration of primary particles having a carbon-containing layer attached to the surface. Such secondary particles can exhibit excellent electrical conductivity because carbon is present between the primary particles. An embodiment containing such secondary particles is preferable because the active material-containing layer can exhibit lower resistance.

[0057] <Specific surface area> The specific surface area of ​​the active material according to the embodiment is not particularly limited, but is preferably 0.5 m 2 / g or more 5m 2 / g or less. 2 If the specific surface area is 5 m / g or more, the contact area with the electrolyte can be secured, good discharge rate characteristics can be obtained, and the charging time can be shortened. 2 / g or less, the reactivity with the electrolyte is not too high, and the life characteristics can be improved. In addition, the coating properties of a slurry containing an active material used in the manufacture of an electrode, which will be described later, can be improved.

[0058] Here, the specific surface area is measured by adsorbing molecules with known adsorption occupancy areas onto the powder particle surfaces at liquid nitrogen temperature, and then calculating the specific surface area of ​​the sample from the amount of adsorption. The most commonly used method is the BET method, which uses low-temperature, low-humidity physical adsorption of an inert gas. This is the most famous method for calculating specific surface area, and extends the Langmuir theory, which is a theory of monolayer adsorption, to multilayer adsorption. The specific surface area calculated in this way is called the BET (Brunauer, Emmett, Teller) specific surface area.

[0059] <Method of manufacturing active material> The active material according to the embodiment can be produced, for example, by the synthesis method described below.

[0060] First, the starting materials are mixed. As the starting material containing niobium and titanium, an oxide or salt containing Nb and Ti is prepared. For example, Nb2O5 particles and TiO2 particles can be used as the starting materials. These starting materials are mixed in a ratio of niobium to titanium (M Nb / M Ti ) is in the range of 2.0 to 4.0. Nb " indicates the amount of niobium atoms (molar number) contained in the niobium titanium composite oxide, and "M Ti " indicates the amount (molar number) of titanium atoms contained in the niobium titanium composite oxide. In this specification, "the molar ratio of niobium to titanium (M Nb / M Ti ) is sometimes referred to as the "Nb / Ti ratio."

[0061] After mixing the raw materials, the mixture is pulverized to obtain a mixture as uniform as possible. The mixture is then subjected to pre-calcination (first calcination). The pre-calcination is performed in two or more stages at a temperature range of 500 to 900°C for a total of 10 to 40 hours. This allows the production of highly uniform precursor particles.

[0062] Next, the obtained precursor particles are subjected to main firing (second firing). The main firing is performed at a temperature of 800°C to 1000°C or less for 1 hour to 10 hours. At this point, the firing time may be determined by giving priority to obtaining a desired particle size distribution. The crystallinity of the particles obtained by the main firing may be low. In this way, by performing firing at a relatively low temperature and multiple times from the preliminary firing to the main firing, the generation of coarse particles and fine particles can be suppressed.

[0063] Next, an oxide or salt containing potassium and phosphorus is prepared. The oxide or salt is added to the previously obtained particles after the main calcination so that the potassium and phosphorus content is within the range of 0.010 mass% to 5.00 mass%, and wet-mixed. In this case, it is preferable to wet-mix the supply source containing potassium and phosphorus with a raw material soluble in a solvent such as water, since it can be uniformly distributed on the surface of the calcined particles.

[0064] Next, the mixture of the sintered particles obtained by wet mixing with potassium and phosphorus is subjected to an annealing treatment. The annealing treatment is preferably performed at a temperature of 800°C to 900°C for 1 hour to 10 hours. The flux effect of potassium and phosphorus can suppress grain growth while increasing crystallinity. The powder thus obtained is subjected to mild pulverization for as short a time as possible without applying a strong shear as much as possible. For this pulverization, for example, a roller compactor, a bead mill device, a ball mill device, or the like can be used. This allows the crystallinity to be increased without significantly changing the particle size distribution obtained by the main sintering.

[0065] In addition, by changing the grinding conditions after the annealing, the D10, D50 and D90 of the obtained active material can be controlled. For example, by increasing the grinding time, D10, D50 and D90 tend to be smaller. In addition, for example, by using a grinding medium having a smaller diameter, D10, D50 and D90 tend to be smaller. Alternatively, by subjecting the powder to centrifugation, particles with a small D10 can be collected, or particles with a large D90 can be collected. For example, by mixing the collected particles with a separately synthesized active material, D10, D50 and D90 can be controlled.

[0066] As described above, when manufacturing a niobium titanium composite oxide having a Nb2TiO7 phase and a Nb-rich phase, the particles are sintered to obtain a desired particle size distribution, and then potassium and phosphorus are added to the particles, which are then annealed and then mildly pulverized to obtain an active material powder having high crystallinity and a small proportion of fine powder. This makes it possible to obtain an active material that exhibits excellent input / output characteristics while suppressing the deformation of the crystal lattice during Li charge / discharge and improving cycle life characteristics.

[0067] The niobium titanium composite oxide synthesized by the above method may have lithium ions inserted therein by assembling a battery and then charging it, or may be synthesized as a composite oxide containing lithium by using a compound containing lithium such as lithium carbonate as a starting material.

[0068] <Powder X-ray diffraction measurement and peak intensity ratio of active materials I B / I A Calculation of > The powder X-ray diffraction measurement of the active material can be carried out, for example, as follows. First, the target sample is crushed until the average particle size is about 5 μm. The crushed sample is filled into the holder portion formed on the glass sample plate, with a depth of 0.2 mm. At this time, care is taken to ensure that the sample is filled sufficiently into the holder portion. Also, care is taken to fill the sample with just the right amount so that cracks, voids, etc. do not occur. Next, another glass plate is pressed from the outside to flatten the surface of the sample filled into the holder portion. Care is taken to ensure that the amount of filling is not too much or too little, resulting in unevenness compared to the reference surface of the holder.

[0069] Next, the glass plate filled with the sample is placed in a powder X-ray diffractometer, and a diffraction pattern (XRD pattern; X-Ray Diffraction pattern) is obtained using Cu-Kα radiation.

[0070] In addition, the orientation of the particles may become large depending on the particle shape of the sample. When the orientation of the sample is high, the peak position may shift or the intensity ratio may change depending on how the sample is filled. Samples with extremely high orientation are measured using a glass capillary. Specifically, the sample is inserted into a capillary, and the capillary is placed on a rotating sample stage for measurement. This measurement method can reduce the orientation. As the glass capillary, it is preferable to use a Lindemann glass capillary with a diameter of 1 mm to 6 mmφ.

[0071] When performing powder X-ray diffraction measurement on the active material contained in the electrode, the measurement can be carried out, for example, as follows. First, in order to grasp the crystalline state of the active material, the active material is placed in a state in which lithium ions are completely removed. For example, when the active material is used in a negative electrode, the battery is placed in a completely discharged state. For example, the battery is discharged at a current of 0.1 C in a 25° C. environment until the rated end voltage or the battery voltage reaches 1.0 V, and the current value during discharge is set to 1 / 100 or less of the rated capacity, thereby placing the battery in a discharged state. Residual lithium ions may still be present even in the discharged state.

[0072] Next, the battery is disassembled in a glove box filled with argon, and the electrodes are removed and washed with a suitable solvent. An example of a suitable solvent is ethyl methyl carbonate. If the electrodes are not sufficiently washed, lithium ions remaining in the electrodes may cause impurity phases such as lithium carbonate and lithium fluoride to be mixed in. In that case, it is recommended to use an airtight container in which the measurement atmosphere can be in an inert gas. The washed electrodes are cut to have an area approximately the same as the area of ​​the holder of the powder X-ray diffraction apparatus to prepare the measurement sample. This sample is directly attached to the glass holder and the measurement is performed.

[0073] At this time, the peaks originating from the metal foil, conductive agent, binder, etc., which is the current collector, are measured and understood in advance using XRD. Of course, if these are known in advance, this operation can be omitted. When the peak of the current collector and the peak of the active material overlap, it is desirable to peel off the active material-containing layer from the current collector and measure it. This is to separate the overlapping peaks when quantitatively measuring the peak intensity. The active material-containing layer may be physically peeled off, but it is easier to peel off by applying ultrasonic waves in a solvent. When ultrasonic treatment is performed to peel off the active material-containing layer from the current collector, the electrode body powder (including the active material, conductive agent, and binder) can be recovered by volatilizing the solvent. The recovered electrode body powder can be filled in, for example, a Lindemann glass capillary and measured to perform powder X-ray diffraction measurement of the active material. The electrode body powder recovered by ultrasonic treatment can also be subjected to various analyses other than powder X-ray diffraction measurement.

[0074] The powder X-ray diffraction measurement device used is, for example, SmartLab manufactured by Rigaku Co., Ltd. The measurement conditions are as follows: X-ray source: Cu target Output: 45kV 200mA Soller slit: 5° for both incidence and reception Step width (2θ): 0.02 deg Scan speed: 20deg / min Semiconductor detector: D / teX Ultra 250 Measurement range: 5°≦2θ≦90° Sample plate holder: Flat glass sample plate holder (thickness 0.5 mm).

[0075] When using other equipment, perform the measurement using standard Si powder for powder X-ray diffraction so as to obtain measurement results equivalent to those described above, and adjust the measurement conditions so that the peak intensity and peak top position match those of the above equipment.

[0076] Among the obtained diffraction peaks, the peak intensity I of the peak assigned to the Nb2TiO7 phase having the maximum peak intensity within the range of 2θ of 26.0±0.1° is A In addition, Nb having the maximum peak intensity within the range of 2θ of 24.9±0.2° is determined. 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 The peak intensity I of the peak attributed to at least one Nb-rich phase selected from the group consisting of Nb-rich phases B Then, the peak intensity ratio I B / I A Calculate.

[0077] <Confirmation of crystallite size> The XRD diffraction pattern obtained by powder X-ray diffraction must be applicable to Rietveld analysis. To collect Rietveld data, the step width is set to 1 / 3 to 1 / 5 of the minimum half-width of the diffraction peak, and the measurement time and / or X-ray intensity are appropriately adjusted so that the intensity at the peak position of the most intense reflection is 5000 to 10000 counts.

[0078] The obtained XRD pattern is analyzed by the Rietveld method, in which the diffraction pattern is calculated from a pre-estimated crystal structure model. By fitting all of these calculated values ​​with the actual measured values, the parameters related to the crystal structure (lattice constants, atomic coordinates, occupancy, etc.) can be precisely analyzed. This makes it possible to investigate the characteristics of the crystal structure of the synthesized oxide. It is also possible to investigate the occupancy rate of each site of the constituent elements.

[0079] The fitting parameter S is used as a measure to estimate the degree of agreement between observed and calculated intensities in the Rietveld analysis. The analysis must be performed so that S is smaller than 1.8. In addition, when determining the occupancy rate of each site, the standard deviation σ j must be taken into account. The fitting parameter S and standard deviation σ j is estimated by the formula described in Non-Patent Document 2 (pages 97 to 115). In this method, for the monoclinic niobium titanium composite oxide having the symmetry of the space group C2 / m of the embodiment, fitting is performed assuming that each cation is evenly occupied at each metal cation occupied site of 2a or 4i in the crystal structure, and fitting is performed by setting individual occupancy rates for each element assuming that each cation is unevenly distributed. As a result, it can be determined that the smaller the convergence value of the fitting parameter S, that is, the better the fitting, is closer to the actual occupancy state. This makes it possible to determine whether each cation is randomly arranged or not.

[0080] To determine the crystallite diameter (crystallite size), the diffraction line with the strongest diffraction intensity is selected. For example, Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δIn the compound represented by the formula (110), the peak of the (110) plane is measured. Here, M1 is at least one selected from the group consisting of Zr, Si, and Sn. M2 is at least one selected from the group consisting of V, Ta, Bi, K, Ca, B, Co, Fe, Mn, Ni, Si, P, and Mo. Each subscript in the composition formula is 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3. The crystallite size can be calculated from the half-width of the obtained peak. Here, the crystallite size is calculated from the Scherrer formula shown in the following formula 2.

[0081]

number

[0082] Here, K=0.9, λ=0.15406 nm, β e : Half-width of diffraction peak, β o : Corrected half-width value (0.07°).

[0083] <High frequency inductively coupled plasma optical emission spectrometry> The concentrations of potassium and phosphorus in the active material can be analyzed by high-frequency inductively coupled plasma (ICP) emission spectrometry.

[0084] A part of the active material powder is placed in a suitable solvent and irradiated with ultrasonic waves. For example, the electrode body is placed in ethyl methyl carbonate in a glass beaker and vibrated in an ultrasonic cleaner, whereby the active material-containing layer can be peeled off from the current collector. Next, the peeled active material-containing layer is dried by drying under reduced pressure. The obtained active material-containing layer is pulverized in a mortar or the like to obtain a powder containing the active material, the conductive agent, the binder, and the like. This powder can be dissolved in an acid to prepare a liquid sample containing the active material. In this case, the acid that can be used is hydrochloric acid, nitric acid, sulfuric acid, hydrogen fluoride, or the like. The concentration of potassium and phosphorus contained in the active material can be analyzed by subjecting this liquid sample to ICP emission spectroscopy.

[0085] <TEM observation of active material> Observation with a transmission electron microscope (TEM) can confirm the distribution of each crystal phase. It can also confirm whether the added elements potassium and phosphorus are present at the particle interface. If necessary, energy dispersive X-ray spectroscopy (EDX) may also be performed.

[0086] For observation under a transmission electron microscope, it is desirable to embed the target sample powder in resin and to remove the inside of the specimen by mechanical polishing and ion milling. The same process can also be carried out when the target sample is an electrode body. For example, the electrode body can be embedded in resin as it is and the desired location can be observed, or the current collector (metal foil) can be peeled off from the electrode body and observed as an electrode powder containing a mixture of conductive material and binder. In this way, it is possible to know how the two crystal phases are distributed within the primary particle, and also to know the gradient of the composition within the particle.

[0087] A specific example will be described below with reference to Figure 3. Figure 3 is a plan view that shows a particle to be measured. First, the center of gravity of the particle to be measured is regarded as the center of the particle. Next, five measurement points are set at equal intervals on a line connecting the center of the particle and an arbitrary point on the particle surface. Multi-beam interference images of the particle part at three points in the region perpendicular to each measurement point are examined, and the electron beam diffraction pattern is observed. This observation makes it possible to know the crystal structure contained at the measurement point. For example, by simulating the electron beam diffraction pattern in advance, it is possible to know the crystal structure of the Nb2TiO7 phase and the Nb 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 phase, as well as other phases, can be easily distinguished.

[0088] <Measurement of particle size distribution of active material particles using laser diffraction scattering method> The electrode powder described in the above section on powder X-ray diffraction measurement is sintered to burn off the conductive agent and binder. The remaining active material particles are dispersed in N-methyl-2-pyrrolidone (NMP) solvent and subjected to ultrasonic treatment to obtain a dispersion solution as a sample for particle size distribution measurement. The particle size distribution of the constituent particles of this dispersion solution is measured using a laser diffraction distribution measurement device. As a measurement device, for example, Microtrack MT3100II manufactured by Microtrack Bell Co., Ltd. can be used.

[0089] The ultrasonic treatment for obtaining the dispersion solvent is carried out by a sample supply system attached to the laser diffraction distribution measurement device, for example, at an output of 40 W for 300 seconds.

[0090] According to a first embodiment, an active material is provided. The active material comprises a Nb2TiO7 phase and a Nb 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 and at least one Nb-rich phase selected from the group consisting of Nb-rich phases. This active material contains potassium and phosphorus, and the total concentration of potassium and phosphorus in the active material is in the range of 0.01 mass% or more and 5.00 mass% or less. The average crystallite diameter is in the range of 80 nm to 150 nm. In a particle size distribution chart obtained by a laser diffraction scattering method, D10 is 0.3 μm or more and D90 is 10 μm or less. The active material satisfies the peak intensity ratio represented by the following formula (1).

[0091] 0 B / I A ≦0.25 (1) In formula (1), I A is the peak intensity of the maximum peak that appears at 26.0±0.1° and is attributed to the Nb2TiO7 phase in the diffraction peaks obtained by wide-angle X-ray diffraction using CuKα radiation as an X-ray source, and I B is the peak intensity of the maximum diffraction peak which appears at 2θ of 24.9±0.2° and is attributed to the Nb-rich phase. ​

[0092] The active material according to the embodiment can realize a secondary battery that can exhibit excellent input / output characteristics and cycle life characteristics.

[0093] Second embodiment According to a second embodiment, an electrode is provided.

[0094] The electrode according to the second embodiment includes the active material according to the first embodiment. The electrode according to the embodiment may be a negative electrode or a positive electrode. The electrode according to the embodiment is, for example, a battery electrode, a secondary battery electrode, or a lithium secondary battery electrode. The electrode may be a negative electrode that includes the active material according to the first embodiment as a negative electrode material.

[0095] The electrode according to the second embodiment may include a current collector and an active material-containing layer. The active material-containing layer may be formed on one or both sides of the current collector. The active material-containing layer may include an active material and, optionally, a conductive agent and a binder.

[0096] The active material-containing layer may contain a single active material according to the first embodiment, or may contain two or more types of active materials according to the first embodiment, or may contain a mixture of one or more types of active materials according to the first embodiment and one or more types of other active materials.

[0097] Other examples of active materials include lithium titanates having the ramsdellite structure (e.g., Li 2+y Ti3O7, 0≦y≦3), lithium titanates with spinel structure (e.g., Li 4+x Ti5O 12 , 0≦x≦3), titanium dioxide (TiO2), niobium pentoxide (Nb2O5), anatase type titanium dioxide, rutile type titanium dioxide, hollandite type titanium composite oxide, and orthorhombic titanium-containing composite oxide. Examples of other active materials further include niobium titanium composite oxides different from the active material according to the first embodiment. The niobium titanium composite oxide may have a monoclinic crystal structure.

[0098] As an example of an orthorhombic titanium-containing composite oxide, Li 2+a M(I) 2-b Ti 6-c M(II) d O 14+σ Here, M(I) is at least one selected from the group consisting of Sr, Ba, Ca, Mg, Na, Cs, Rb, and K. M(II) is at least one selected from the group consisting of Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni, and Al. The subscripts in the composition formula are 0≦a≦6, 0≦b<2, 0≦c<6, 0≦d<6, and -0.5≦σ≦0.5. Specific examples of orthorhombic titanium-containing composite oxides include Li 2+a Na2Ti6O 14 (0≦a≦6).

[0099] As an example of the monoclinic niobium titanium composite oxide, Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δ Here, M1 is at least one selected from the group consisting of Zr, Si, and Sn. M2 is at least one selected from the group consisting of V, Ta, and Bi. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3. Specific examples of monoclinic niobium titanium composite oxides include Li x Examples include Nb2TiO7 (0≦x≦5).

[0100] Another example of monoclinic niobium titanium composite oxide is Ti 1-y M3 y+z Nb 2-z O 7-δ Here, M3 is at least one selected from Mg, Fe, Ni, Co, W, Ta, and Mo. The subscripts in the composition formula are 0≦y<1, 0≦z≦2, and -0.3≦δ≦0.3.

[0101] The conductive agent is blended to improve the current collecting performance and to reduce the contact resistance between the active material and the current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, and carbonaceous materials such as graphite. One of these may be used as the conductive agent, or two or more may be used in combination as the conductive agent. Alternatively, instead of using a conductive agent, a carbon coating or an electronically conductive inorganic material coating may be applied to the surface of the active material particles.

[0102] The binder is blended to fill the gaps between the dispersed active materials and to bind the active materials and the current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene butadiene rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.

[0103] The mixing ratio of the active material, conductive agent and binder in the active material-containing layer can be appropriately changed depending on the application of the electrode. For example, when the electrode is used as a negative electrode of a secondary battery, it is preferable to mix the active material, conductive agent and binder in a ratio of 68% by mass or more and 96% by mass or less, 2% by mass or more and 30% by mass or less, and 2% by mass or more and 30% by mass or less, respectively. By making the amount of the conductive agent 2% by mass or more, the current collection performance of the active material-containing layer can be improved. In addition, by making the amount of the binder 2% by mass or more, the binding property between the active material-containing layer and the current collector becomes sufficient, and excellent cycle performance can be expected. On the other hand, it is preferable to make the conductive agent and the binder 30% by mass or less, respectively, in order to increase the capacity.

[0104] The current collector is made of a material that is electrochemically stable at the potential at which lithium (Li) is inserted and extracted from the active material. For example, when the active material is used as a negative electrode material, the current collector is preferably made of copper, nickel, stainless steel, or aluminum, or an aluminum alloy containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si. The thickness of the current collector is preferably 5 μm or more and 20 μm or less. A current collector having such a thickness can balance the strength and weight of the electrode.

[0105] The current collector may also include a portion on the surface of which no active material-containing layer is formed, and this portion can function as a current collecting tab.

[0106] The electrode can be produced, for example, by the following method. First, the active material according to the embodiment, the conductive agent, and the binder are suspended in a solvent to prepare a slurry. This slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate of an active material-containing layer and a current collector. After that, the laminate is pressed. In this manner, the electrode is produced.

[0107] Alternatively, the electrode may be prepared by the following method: first, the active material, the conductive agent, and the binder are mixed to obtain a mixture, then the mixture is formed into pellets, and then the pellets are placed on a current collector to obtain an electrode.

[0108] The electrode according to the second embodiment contains the active material according to the first embodiment, and therefore this electrode can realize a secondary battery that can exhibit excellent input / output characteristics and cycle life characteristics.

[0109] Third embodiment According to the third embodiment, a secondary battery including a negative electrode, a positive electrode, and an electrolyte is provided. This secondary battery includes the electrode according to the second embodiment as the negative electrode. That is, the secondary battery according to the third embodiment includes an electrode including the active material according to the first embodiment as the negative electrode.

[0110] The secondary battery according to the embodiment may further include a separator disposed between the positive electrode and the negative electrode. The negative electrode, the positive electrode, and the separator may constitute an electrode group. The electrolyte may be held in the electrode group.

[0111] The secondary battery may further include an exterior member that contains the electrode group and the electrolyte.

[0112] Furthermore, the secondary battery may further include a negative electrode terminal electrically connected to the negative electrode and a positive electrode terminal electrically connected to the positive electrode.

[0113] The secondary battery may be, for example, a lithium ion secondary battery. Also, the secondary battery may be a non-aqueous electrolyte secondary battery that contains a non-aqueous electrolyte.

[0114] The negative electrode, the positive electrode, the electrolyte, the separator, the exterior member, the negative electrode terminal, and the positive electrode terminal will be described in detail below.

[0115] (1) Negative electrode The negative electrode may include a negative electrode current collector and a negative electrode active material-containing layer. The negative electrode current collector and the negative electrode active material-containing layer may be the current collector and the active material-containing layer that can be included in the electrode according to the second embodiment, respectively. The negative electrode active material-containing layer includes the active material according to the first embodiment as a negative electrode active material.

[0116] Among the details of the negative electrode, parts that overlap with the details explained in the second embodiment will be omitted.

[0117] The density of the negative electrode active material-containing layer (excluding the current collector), i.e., the electrode density, is 1.8 g / cm 3 More than 3.5g / cm 3 The density of the negative electrode active material-containing layer is preferably 2.5 g / cm or less. A negative electrode having a density in this range of the negative electrode active material-containing layer is excellent in energy density and electrolyte retention. 3 More than 2.9g / cm 3 It is more preferable that:

[0118] The negative electrode can be produced, for example, by the same method as the electrode according to the second embodiment.

[0119] (2) Positive electrode The positive electrode can include a positive electrode current collector and a positive electrode active material-containing layer. The positive electrode active material-containing layer can be formed on one or both sides of the positive electrode current collector. The positive electrode active material-containing layer can contain a positive electrode active material, and optionally a conductive agent and a binder.

[0120] As the positive electrode active material, for example, an oxide or a sulfide can be used. The positive electrode may contain, as the positive electrode active material, one type of compound alone, or a combination of two or more types of compounds. Examples of oxides and sulfides include compounds into which Li or Li ions can be inserted and desorbed.

[0121] Examples of such compounds include manganese dioxide (MnO2), iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide (e.g., Li x Mn2O4 or Li x MnO2; 0 < x ≦ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≦ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≦ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≦ 1, 0 < y < 1), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≦ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≦ 1, 0 < y < 2), lithium phosphate having an olivine structure (e.g., Li x FePO4; 0 < x ≦ 1, Li x Fe 1-y Mn y PO4; 0 < x ≦ 1, 0 < y < 1, Lix CoPO4; 0 < x ≦ 1), iron sulfate (Fe2(SO4)3), vanadium oxide (e.g., V2O5), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≦ 1, 0 < y < 1, 0 < z < 1, y + z < 1) are included.

[0122] Among the above, examples of more preferable compounds as the positive electrode active material include lithium manganese composite oxide having a spinel structure (e.g., Li x Mn2O4; 0 < x ≦ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≦ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≦ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≦ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≦ 1, 0 < y < 2), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≦ 1, 0 < y < 1), lithium iron phosphate (e.g., Li x FePO4; 0 < x ≦ 1), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≦ 1, 0 < y < 1, 0 < z < 1, y + z < 1) are included. When these compounds are used as the positive electrode active material, the positive electrode potential can be increased.

[0123] When a room temperature molten salt is used as the electrolyte of the battery, lithium iron phosphate, Li xIt is preferable to use a positive electrode active material containing VPO4F (0≦x≦1), lithium manganese composite oxide, lithium nickel composite oxide, lithium nickel cobalt composite oxide, or a mixture thereof. These compounds have low reactivity with room temperature molten salts, so that the cycle life can be improved. Details of the room temperature molten salt will be described later.

[0124] The primary particle size of the positive electrode active material is preferably 100 nm or more and 1 μm or less. A positive electrode active material with a primary particle size of 100 nm or more is easy to handle in industrial production. A positive electrode active material with a primary particle size of 1 μm or less can smoothly diffuse lithium ions in the solid.

[0125] The specific surface area of ​​the positive electrode active material is 0.1 m 2 / g or more 10m 2 / g or less. 2 A positive electrode active material having a specific surface area of ​​10m / g or more can secure sufficient sites for absorbing and releasing Li ions. 2 A positive electrode active material having a specific surface area of ​​100 / g or less is easy to handle in industrial production and can ensure good charge-discharge cycle performance.

[0126] The binder is blended to fill the gaps between the dispersed positive electrode active material and to bind the positive electrode active material and the positive electrode current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.

[0127] The conductive agent is blended to improve current collection performance and reduce contact resistance between the positive electrode active material and the positive electrode current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, and carbonaceous materials such as graphite. One of these may be used as the conductive agent, or two or more may be combined and used as the conductive agent. The conductive agent may also be omitted.

[0128] In the positive electrode active material-containing layer, the positive electrode active material and the binder are preferably mixed in proportions of 80% by mass to 98% by mass and 2% by mass to 20% by mass, respectively.

[0129] By making the amount of binder 2% by mass or more, sufficient electrode strength can be obtained. In addition, the binder can function as an insulator. Therefore, by making the amount of binder 20% by mass or less, the amount of insulator contained in the electrode is reduced, and the internal resistance can be reduced.

[0130] When a conductive agent is added, the positive electrode active material, the binder, and the conductive agent are preferably mixed in proportions of 77% by mass or more and 95% by mass or less, 2% by mass or more and 20% by mass or less, and 3% by mass or more and 15% by mass or less, respectively.

[0131] By setting the amount of the conductive agent to 3% by mass or more, the above-mentioned effects can be achieved. Also, by setting the amount of the conductive agent to 15% by mass or less, the ratio of the conductive agent in contact with the electrolyte can be reduced. If this ratio is low, decomposition of the electrolyte during high-temperature storage can be reduced.

[0132] The positive electrode current collector is preferably an aluminum foil or an aluminum alloy foil containing one or more elements selected from Mg, Ti, Zn, Ni, Cr, Mn, Fe, Cu, and Si.

[0133] The thickness of the aluminum foil or aluminum alloy foil is preferably 5 μm or more and 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99 mass% or more. The content of transition metals such as iron, copper, nickel, and chromium contained in the aluminum foil or aluminum alloy foil is preferably 1 mass% or less.

[0134] The positive electrode current collector may also include a portion on the surface of which the positive electrode active material-containing layer is not formed, and this portion can function as a positive electrode current collecting tab.

[0135] The positive electrode can be produced, for example, by using a positive electrode active material in the same manner as in the electrode according to the second embodiment.

[0136] (3) Electrolyte The electrolyte may be, for example, a liquid nonaqueous electrolyte or a gel nonaqueous electrolyte. The liquid nonaqueous electrolyte is prepared by dissolving an electrolyte salt as a solute in an organic solvent. The concentration of the electrolyte salt is preferably 0.5 mol / L or more and 2.5 mol / L or less.

[0137] Examples of the electrolyte salt include lithium salts such as lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), and lithium bistrifluoromethylsulfonylimide (LiN(CF3SO2)2), and mixtures thereof. The electrolyte salt is preferably one that is difficult to oxidize even at high potentials, and LiPF6 is most preferred.

[0138] Examples of organic solvents include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyl tetrahydrofuran (2MeTHF), and dioxolane (DOX); chain ethers such as dimethoxyethane (DME) and diethoxyethane (DEE); γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These organic solvents can be used alone or as a mixed solvent.

[0139] The gelled non-aqueous electrolyte is prepared by combining a liquid non-aqueous electrolyte with a polymeric material, such as polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyethylene oxide (PEO), or a mixture thereof.

[0140] Alternatively, as the nonaqueous electrolyte, in addition to liquid nonaqueous electrolytes and gel nonaqueous electrolytes, room temperature molten salts containing lithium ions (ionic melts), polymer solid electrolytes, inorganic solid electrolytes, and the like may be used.

[0141] Room temperature molten salts (ionic melts) refer to organic salts consisting of a combination of organic cations and anions that can exist as a liquid at room temperature (15°C or higher and 25°C or lower). Room temperature molten salts include room temperature molten salts that exist as a liquid by themselves, room temperature molten salts that become liquid when mixed with an electrolyte salt, room temperature molten salts that become liquid when dissolved in an organic solvent, and mixtures of these. In general, the melting point of room temperature molten salts used in secondary batteries is 25°C or lower. In addition, organic cations generally have a quaternary ammonium skeleton.

[0142] The polymer solid electrolyte is prepared by dissolving an electrolyte salt in a polymer material and solidifying it.

[0143] The inorganic solid electrolyte is a solid material that has Li-ion conductivity.

[0144] The electrolyte may be an aqueous electrolyte that contains water.

[0145] The aqueous electrolyte includes an aqueous solvent and an electrolyte salt. The aqueous electrolyte is, for example, liquid. The liquid aqueous electrolyte is an aqueous solution prepared by dissolving an electrolyte salt as a solute in an aqueous solvent. The aqueous solvent is, for example, a solvent containing water in an amount of 50% by volume or more. The aqueous solvent may be pure water.

[0146] The aqueous electrolyte may be a gel aqueous electrolyte obtained by combining an aqueous electrolyte solution with a polymeric material, such as polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyethylene oxide (PEO), etc.

[0147] The aqueous electrolyte preferably contains 1 mol or more of the aqueous solvent per mol of the solute salt, and more preferably contains 3.5 mol or more of the aqueous solvent per mol of the solute salt.

[0148] The presence of water in aqueous electrolytes can be confirmed by GC-MS (Gas Chromatography - Mass Spectrometry) measurements. The salt concentration and water content in aqueous electrolytes can be calculated, for example, by ICP (Inductively Coupled Plasma) emission spectrometry. The molar concentration (mol / L) can be calculated by weighing a specified amount of aqueous electrolyte and calculating the salt concentration. The number of moles of solute and solvent can also be calculated by measuring the specific gravity of the aqueous electrolyte.

[0149] The aqueous electrolyte is prepared, for example, by dissolving an electrolyte salt in an aqueous solvent at a concentration of 1 to 12 mol / L.

[0150] In order to suppress electrolysis of the aqueous electrolyte, LiOH or Li2SO4 can be added to adjust the pH, preferably 3-13, more preferably 4-12.

[0151] (4) Separator The separator is formed, for example, from a porous film containing polyethylene (PE), polypropylene (PP), cellulose, or polyvinylidene fluoride (PVdF), or a synthetic resin nonwoven fabric. From the viewpoint of safety, it is preferable to use a porous film formed from polyethylene or polypropylene. This is because these porous films melt at a certain temperature and are capable of cutting off electric current.

[0152] A solid electrolyte layer containing solid electrolyte particles can also be used as the separator. The solid electrolyte layer may contain one type of solid electrolyte particles or may contain multiple types of solid electrolyte particles. The solid electrolyte layer may be a solid electrolyte composite membrane containing solid electrolyte particles. The solid electrolyte composite membrane is, for example, a membrane formed from solid electrolyte particles using a polymer material. The solid electrolyte layer may contain at least one selected from the group consisting of a plasticizer and an electrolyte salt. When the solid electrolyte layer contains an electrolyte salt, for example, the alkali metal ion conductivity of the solid electrolyte layer can be further increased.

[0153] Examples of the polymeric material include polyethers, polyesters, polyamines, polyethylenes, silicones, and polysulfides.

[0154] As the solid electrolyte, it is preferable to use an inorganic solid electrolyte. As the inorganic solid electrolyte, for example, an oxide-based solid electrolyte or a sulfide-based solid electrolyte can be mentioned. As the oxide-based solid electrolyte, it is preferable to use a lithium phosphate solid electrolyte having a NASICON structure and represented by the general formula LiM2(PO4)3. In the above general formula, M is preferably at least one element selected from the group consisting of titanium (Ti), germanium (Ge), strontium (Sr), zirconium (Zr), tin (Sn), and aluminum (Al). It is more preferable that the element M contains any one of Ge, Zr, and Ti, and Al.

[0155] A specific example of a lithium phosphate solid electrolyte having a NASICON structure is LATP (Li 1+x Al x Ti 2-x (PO4)3), Li 1+x Al x Ge 2-x (PO4)3, Li 1+x Al x Zr 2-x(PO4)3 can be cited. In the above formula, x is in the range of 0 < x ≤ 5, and preferably in the range of 0.1 ≤ x ≤ 0.5. As the solid electrolyte, it is preferable to use LATP. LATP has excellent water resistance and is less likely to cause hydrolysis in the secondary battery.

[0156] Also, as the oxide-based solid electrolyte, amorphous LIPON (Li 2.9 PO 3.3 N 0.46 ) or garnet-type LLZ (Li7La3Zr2O 12 ) may be used.

[0157] (5) Exterior member As the exterior member, for example, a container made of a laminate film or a metal container can be used.

[0158] The thickness of the laminate film is, for example, 0.5 mm or less, preferably 0.2 mm or less.

[0159] As the laminate film, a multilayer film including a plurality of resin layers and a metal layer interposed between these resin layers is used. The resin layer contains, for example, polymer materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably made of aluminum foil or aluminum alloy foil for weight reduction. The laminate film can be formed into the shape of the exterior member by sealing by heat fusion.

[0160] The thickness of the wall of the metal container is, for example, 1 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less.

[0161] The metal container is made of, for example, aluminum or an aluminum alloy. The aluminum alloy preferably contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains transition metals such as iron, copper, nickel, and chromium, the content of the transition metals is preferably 100 mass ppm or less.

[0162] The shape of the exterior member is not particularly limited. The shape of the exterior member may be, for example, flat (thin), rectangular, cylindrical, coin, or button. The exterior member can be appropriately selected depending on the battery dimensions and the application of the battery.

[0163] (6) Negative terminal The negative electrode terminal can be made of a material that is electrochemically stable at the Li absorption / release potential of the negative electrode active material and has electrical conductivity. Specifically, the material of the negative electrode terminal can be copper, nickel, stainless steel, aluminum, or an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The material of the negative electrode terminal is preferably aluminum or an aluminum alloy. The negative electrode terminal is preferably made of the same material as the negative electrode current collector in order to reduce the contact resistance with the negative electrode current collector.

[0164] (7) Positive terminal The positive electrode terminal has a potential range of 3V to 5V with respect to the redox potential of lithium (vs. Li / Li + ) and can be formed from a material that is electrically stable and conductive. Examples of the material for the positive electrode terminal include aluminum and an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The positive electrode terminal is preferably formed from the same material as the positive electrode current collector in order to reduce the contact resistance with the positive electrode current collector.

[0165] Next, the secondary battery according to the third embodiment will be described more specifically with reference to the drawings.

[0166] Fig. 4 is a cross-sectional view showing an example of a secondary battery according to embodiment 3. Fig. 5 is an enlarged cross-sectional view of part A of the secondary battery shown in Fig. 4.

[0167] The secondary battery 100 shown in Figures 4 and 5 includes a bag-shaped exterior member 2 shown in Figures 4 and 5, an electrode group 1 shown in Figure 4, and an electrolyte (not shown). The electrode group 1 and the electrolyte are stored in the bag-shaped exterior member 2. The electrolyte (not shown) is held in the electrode group 1.

[0168] The bag-shaped exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.

[0169] As shown in Fig. 4, the electrode group 1 is a flat wound-type electrode group. As shown in Fig. 5, the flat wound-type electrode group 1 includes a negative electrode 3, a separator 4, and a positive electrode 5. The separator 4 is interposed between the negative electrode 3 and the positive electrode 5.

[0170] The negative electrode 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b. In the negative electrode 3, in a portion located at the outermost shell of the wound-type electrode group 1, the negative electrode active material-containing layer 3b is formed only on the inner surface side of the negative electrode current collector 3a as shown in Fig. 5. In the other portions of the negative electrode 3, the negative electrode active material-containing layer 3b is formed on both sides of the negative electrode current collector 3a.

[0171] The positive electrode 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b formed on both sides of the positive electrode current collector 5a.

[0172] As shown in FIG. 4, the negative electrode terminal 6 and the positive electrode terminal 7 are located near the outer peripheral end of the wound electrode group 1. The negative electrode terminal 6 is connected to a portion located at the outermost shell of the negative electrode current collector 3a. The positive electrode terminal 7 is connected to a portion located at the outermost shell of the positive electrode current collector 5a. The negative electrode terminal 6 and the positive electrode terminal 7 extend to the outside from an opening of the bag-shaped exterior member 2. A thermoplastic resin layer is provided on the inner surface of the bag-shaped exterior member 2, and the opening is closed by heat sealing.

[0173] The secondary battery according to the third embodiment is not limited to the secondary battery having the configuration shown in FIGS. 4 and 5, but may be a battery having the configuration shown in FIGS.

[0174] Fig. 6 is a partially cutaway perspective view showing typically another example of the secondary battery according to embodiment 3. Fig. 7 is an enlarged cross-sectional view of part B of the secondary battery shown in Fig. 6.

[0175] The secondary battery 100 shown in Figures 6 and 7 includes an electrode group 1 shown in Figures 6 and 7, an exterior member 2 shown in Figure 6, and an electrolyte (not shown). The electrode group 1 and the electrolyte are housed in the exterior member 2. The electrolyte is held in the electrode group 1.

[0176] The exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.

[0177] The electrode group 1 is a laminated type electrode group, as shown in Fig. 7. The laminated type electrode group 1 has a structure in which negative electrodes 3 and positive electrodes 5 are alternately laminated with separators 4 interposed therebetween.

[0178] The electrode group 1 includes a plurality of negative electrodes 3. Each of the plurality of negative electrodes 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b supported on both sides of the negative electrode current collector 3a. The electrode group 1 also includes a plurality of positive electrodes 5. Each of the plurality of positive electrodes 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b supported on both sides of the positive electrode current collector 5a.

[0179] The negative electrode current collector 3a of each negative electrode 3 includes a portion 3c on one side of which the negative electrode active material-containing layer 3b is not supported on any surface. This portion 3c serves as a negative electrode current collector tab. As shown in FIG. 7, the portion 3c serving as the negative electrode current collector tab does not overlap with the positive electrode 5. The multiple negative electrode current collector tabs (portions 3c) are electrically connected to a strip-shaped negative electrode terminal 6. The tip of the strip-shaped negative electrode terminal 6 is pulled out to the outside of the exterior member 2.

[0180] Although not shown, the positive electrode current collector 5a of each positive electrode 5 includes a portion on one side where the positive electrode active material-containing layer 5b is not supported on any surface. This portion serves as a positive electrode current collector tab. The positive electrode current collector tab does not overlap with the negative electrode 3, similar to the negative electrode current collector tab (portion 3c). The positive electrode current collector tab is located on the opposite side of the electrode group 1 to the negative electrode current collector tab (portion 3c). The positive electrode current collector tab is electrically connected to a strip-shaped positive electrode terminal 7. The tip of the strip-shaped positive electrode terminal 7 is located on the opposite side to the negative electrode terminal 6, and is drawn out to the outside of the exterior member 2.

[0181] The secondary battery according to the third embodiment contains, as a negative electrode active material, the active material according to the first embodiment, and therefore the secondary battery can exhibit excellent input / output characteristics and cycle life characteristics.

[0182] (Fourth embodiment) According to a fourth embodiment, there is provided a battery pack. The battery pack according to the fourth embodiment includes a plurality of secondary batteries according to the third embodiment.

[0183] In the battery pack according to the fourth embodiment, the individual cells may be electrically connected in series or in parallel, or may be connected in a combination of series and parallel.

[0184] Next, an example of a battery pack according to a fourth embodiment will be described with reference to the drawings.

[0185] Fig. 8 is a perspective view showing an example of a battery pack according to the fourth embodiment. The battery pack 200 shown in Fig. 8 includes five cells 100a to 100e, four bus bars 21, a positive electrode lead 22, and a negative electrode lead 23. Each of the five cells 100a to 100e is a secondary battery according to the third embodiment.

[0186] The bus bar 21 connects, for example, the negative electrode terminal 6 of one cell 100a and the positive electrode terminal 7 of the adjacent cell 100b. In this way, the five cells 100 are connected in series by the four bus bars 21. That is, the battery pack 200 in FIG. 8 is a five-series battery pack. Although no example is shown, in a battery pack including a plurality of cells electrically connected in parallel, for example, the plurality of negative electrode terminals are connected to each other by a bus bar and the plurality of positive electrode terminals are connected to each other by a bus bar, thereby electrically connecting the plurality of cells.

[0187] The positive terminal 7 of at least one of the five cells 100a-100e is electrically connected to a positive lead 22 for external connection. Also, the negative terminal 6 of at least one of the five cells 100a-100e is electrically connected to a negative lead 23 for external connection.

[0188] The battery pack according to the fourth embodiment includes the secondary battery according to the third embodiment, and therefore this battery pack can exhibit excellent input / output characteristics and cycle life characteristics.

[0189] Fifth embodiment According to a fifth embodiment, there is provided a battery pack. The battery pack includes the battery assembly according to the fourth embodiment. The battery pack may include a single secondary battery according to the third embodiment, instead of the battery assembly according to the fourth embodiment.

[0190] The battery pack according to the fifth embodiment may further include a protection circuit. The protection circuit has a function of controlling charging and discharging of the secondary battery. Alternatively, a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source may be used as the protection circuit for the battery pack.

[0191] The battery pack according to the fifth embodiment may further include an external terminal for current flow. The external terminal for current flow is for outputting current from the secondary battery to the outside and / or for inputting current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, current is supplied to the outside through the external terminal for current flow. When the battery pack is charged, a charging current (including regenerative energy from the power of an automobile or the like) is supplied to the battery pack through the external terminal for current flow.

[0192] Next, an example of a battery pack according to a fifth embodiment will be described with reference to the drawings.

[0193] Fig. 9 is an exploded perspective view showing an example of a battery pack according to the fifth embodiment, and Fig. 10 is a block diagram showing an example of an electric circuit of the battery pack shown in Fig. 9.

[0194] The battery pack 300 shown in Figs. 9 and 10 includes a container 31, a lid 32, a protective sheet 33, a battery pack 200, a printed wiring board 34, wiring 35, and an insulating plate (not shown).

[0195] 9 is a bottomed, square container having a rectangular bottom. The container 31 is configured to be able to accommodate a protective sheet 33, a battery pack 200, a printed wiring board 34, and wiring 35. The lid 32 has a rectangular shape. The lid 32 covers the container 31 to accommodate the battery pack 200 and the like. Although not shown, the container 31 and the lid 32 are provided with openings or connection terminals for connection to an external device or the like.

[0196] The battery pack 200 includes a plurality of cells 100, a positive electrode lead 22, a negative electrode lead 23, and an adhesive tape 24.

[0197] At least one of the plurality of unit cells 100 is a secondary battery according to the third embodiment. Each of the plurality of unit cells 100 is electrically connected in series as shown in FIG. 10. The plurality of unit cells 100 may be electrically connected in parallel, or may be connected in a combination of series and parallel connections. When the plurality of unit cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.

[0198] The adhesive tape 24 fastens the plurality of unit cells 100. The plurality of unit cells 100 may be fixed using heat shrink tape instead of the adhesive tape 24. In this case, the protective sheets 33 are disposed on both side surfaces of the battery pack 200, the heat shrink tape is wrapped around the battery pack 200, and the heat shrink tape is then thermally shrunk to bind the plurality of unit cells 100 together.

[0199] One end of the positive electrode lead 22 is connected to the battery pack 200. One end of the positive electrode lead 22 is electrically connected to the positive electrode of one or more cells 100. One end of the negative electrode lead 23 is connected to the battery pack 200. One end of the negative electrode lead 23 is electrically connected to the negative electrode of one or more cells 100.

[0200] The printed wiring board 34 is disposed along one of the short side surfaces of the inner surface of the container 31. The printed wiring board 34 includes a positive connector 342, a negative connector 343, a thermistor 345, a protection circuit 346, wiring 342a and 343a, an external terminal 350 for supplying electricity, a positive wiring (positive wiring) 348a, and a negative wiring (negative wiring) 348b. One main surface of the printed wiring board 34 faces one side of the battery pack 200. An insulating plate (not shown) is interposed between the printed wiring board 34 and the battery pack 200.

[0201] The other end 22a of the positive electrode lead 22 is electrically connected to the positive electrode connector 342. The other end 23a of the negative electrode lead 23 is electrically connected to the negative electrode connector 343.

[0202] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each of the cells 100, and transmits a detection signal to a protection circuit 346.

[0203] The external terminal 350 for current supply is fixed to the other main surface of the printed wiring board 34. The external terminal 350 for current supply is electrically connected to a device present outside the battery pack 300. The external terminal 350 for current supply includes a positive terminal 352 and a negative terminal 353.

[0204] The protection circuit 346 is fixed to the other main surface of the printed wiring board 34. The protection circuit 346 is connected to the positive terminal 352 via a positive wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via a negative wiring 348b. The protection circuit 346 is also electrically connected to the positive electrode connector 342 via a wiring 342a. The protection circuit 346 is electrically connected to the negative electrode connector 343 via a wiring 343a. Furthermore, the protection circuit 346 is electrically connected to each of the plurality of single cells 100 via the wiring 35.

[0205] The protective sheet 33 is disposed on both inner surfaces in the long side direction of the container 31 and on the inner surface in the short side direction that faces the printed wiring board 34 via the battery pack 200. The protective sheet 33 is made of, for example, resin or rubber.

[0206] The protection circuit 346 controls charging and discharging of the multiple cells 100. In addition, the protection circuit 346 cuts off electrical connection between the protection circuit 346 and external terminals 350 (positive terminal 352, negative terminal 353) for supplying electricity to an external device, based on a detection signal transmitted from the thermistor 345, or a detection signal transmitted from each of the cells 100 or the battery pack 200.

[0207] An example of the detection signal transmitted from the thermistor 345 is a signal that detects that the temperature of the cell 100 is equal to or higher than a predetermined temperature. An example of the detection signal transmitted from each cell 100 or the battery pack 200 is a signal that detects overcharging, overdischarging, and overcurrent of the cell 100. When detecting overcharging or the like for each cell 100, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 100.

[0208] The protection circuit 346 may be a circuit included in a device (such as an electronic device or an automobile) that uses the battery pack 300 as a power source.

[0209] As described above, the battery pack 300 includes the external terminal 350 for current supply. Therefore, the battery pack 300 can output a current from the assembled battery 200 to an external device and input a current from the external device to the assembled battery 200 via the external terminal 350 for current supply. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 is supplied to the external device through the external terminal 350 for current supply. When the battery pack 300 is charged, a charging current from the external device is supplied to the battery pack 300 through the external terminal 350 for current supply. When the battery pack 300 is used as an in-vehicle battery, regenerative energy of the vehicle's power can be used as the charging current from the external device.

[0210] The battery pack 300 may include a plurality of assembled batteries 200. In this case, the plurality of assembled batteries 200 may be connected in series, in parallel, or in a combination of series and parallel connections. The printed wiring board 34 and the wiring 35 may be omitted. In this case, the positive electrode lead 22 and the negative electrode lead 23 may be used as a positive terminal and a negative terminal, respectively, of the external terminals for current supply.

[0211] Such a battery pack is used in applications that require excellent cycle performance, for example, when a large current is drawn. Specifically, the battery pack is used, for example, as a power source for electronic devices, a stationary battery, or an on-board battery for various vehicles. An example of the electronic device is a digital camera. The battery pack is particularly suitable for use as an on-board battery.

[0212] The battery pack according to the fifth embodiment includes the secondary battery according to the third embodiment or the battery pack according to the fourth embodiment. Therefore, this battery pack can exhibit excellent input / output characteristics and cycle life characteristics.

[0213] Sixth embodiment According to a sixth embodiment, a vehicle is provided. The vehicle is equipped with the battery pack according to the fifth embodiment.

[0214] In the vehicle according to the sixth embodiment, the battery pack, for example, recovers regenerative energy of the vehicle's motive power. The vehicle may include a mechanism for converting the kinetic energy of the vehicle into regenerative energy.

[0215] Examples of the vehicle according to the sixth embodiment include a two-wheeled to four-wheeled hybrid electric vehicle, a two-wheeled to four-wheeled electric vehicle, an electric-assisted bicycle, and a railroad car.

[0216] The mounting position of the battery pack in the vehicle is not particularly limited. For example, when the battery pack is mounted in an automobile, the battery pack can be mounted in the engine compartment, the rear of the vehicle body, or under the seat of the vehicle.

[0217] The vehicle may be equipped with a plurality of battery packs. In this case, the batteries included in each battery pack may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. For example, when each battery pack includes a battery pack, the battery packs may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. Alternatively, when each battery pack includes a single battery, the batteries may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections.

[0218] Next, an example of a vehicle according to a sixth embodiment will be described with reference to the drawings.

[0219] FIG. 11 is a partial see-through view that illustrates an example of a vehicle according to an embodiment.

[0220] A vehicle 400 shown in Fig. 11 includes a vehicle body 40 and a battery pack 300 according to the embodiment. In the example shown in Fig. 11, the vehicle 400 is a four-wheeled automobile.

[0221] The vehicle 400 may be equipped with a plurality of battery packs 300. In this case, the batteries (e.g., single cells or assembled batteries) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series and parallel connections.

[0222] 11 illustrates an example in which the battery pack 300 is mounted in an engine room located in the front of the vehicle body 40. As described above, the battery pack 300 may be mounted, for example, in the rear of the vehicle body 40 or under a seat. This battery pack 300 can be used as a power source for the vehicle 400. In addition, this battery pack 300 can recover regenerative energy for the motive power of the vehicle 400.

[0223] Next, an embodiment of a vehicle according to the sixth embodiment will be described with reference to FIG.

[0224] Fig. 12 is a diagram illustrating an example of a control system for an electrical system in a vehicle according to embodiment 6. A vehicle 400 illustrated in Fig. 12 is an electric vehicle.

[0225] The vehicle 400 shown in FIG. 12 comprises a vehicle body 40, a vehicle power supply 41, a vehicle ECU (ECU: Electric Control Unit) 42 which is a higher-level control device of the vehicle power supply 41, an external terminal (terminal for connecting to an external power supply) 43, an inverter 44, and a drive motor 45.

[0226] The vehicle 400 has a vehicle power supply 41 mounted, for example, in an engine compartment, the rear of the vehicle body, or under a seat. Note that in the vehicle 400 shown in Fig. 12, the mounting location of the vehicle power supply 41 is shown diagrammatically.

[0227] The vehicle power supply 41 includes a plurality of (eg, three) battery packs 300a, 300b, and 300c, a battery management unit (BMU) 411, and a communication bus 412.

[0228] The battery pack 300a includes an assembled battery 200a and an assembled battery monitoring device 301a (e.g., VTM: Voltage Temperature Monitoring). The battery pack 300b includes an assembled battery 200b and an assembled battery monitoring device 301b. The battery pack 300c includes an assembled battery 200c and an assembled battery monitoring device 301c. The battery packs 300a-300c are battery packs similar to the above-mentioned battery pack 300, and the assembled batteries 200a-200c are assembled batteries similar to the above-mentioned battery pack 200. The assembled batteries 200a-200c are electrically connected in series. The battery packs 300a, 300b, and 300c can be removed independently and replaced with another battery pack 300.

[0229] Each of the assembled batteries 200a-200c includes a plurality of unit cells connected in series. At least one of the plurality of unit cells is the secondary battery according to the second embodiment. The assembled batteries 200a-200c are charged and discharged via a positive terminal 413 and a negative terminal 414, respectively.

[0230] The battery management device 411 communicates with the assembled battery monitoring devices 301a-301c and collects information on the voltage, temperature, and the like of each of the cells 100 included in the assembled batteries 200a-200c included in the vehicle power supply 41. In this way, the battery management device 411 collects information on the maintenance of the vehicle power supply 41.

[0231] The battery management unit 411 and the assembled battery monitoring units 301a-301c are connected via a communication bus 412. In the communication bus 412, one set of communication lines is shared by a plurality of nodes (the battery management unit 411 and one or more assembled battery monitoring units 301a-301c). The communication bus 412 is a communication bus configured based on, for example, the CAN (Control Area Network) standard.

[0232] The battery pack monitoring devices 301a-301c measure the voltage and temperature of each of the cells constituting the battery packs 200a-200c based on commands received through communication from the battery management device 411. However, the temperature can be measured at only a few points per battery pack, and it is not necessary to measure the temperatures of all the cells.

[0233] The vehicle power supply 41 may also have an electromagnetic contactor (for example, a switch device 415 shown in FIG. 12) that switches between the presence and absence of an electrical connection between the positive terminal 413 and the negative terminal 414. The switch device 415 includes a pre-charge switch (not shown) that is turned on when the assembled batteries 200a-200c are charged, and a main switch (not shown) that is turned on when the output from the assembled batteries 200a-200c is supplied to a load. Each of the pre-charge switch and the main switch includes a relay circuit (not shown) that is switched on or off by a signal supplied to a coil disposed near the switch element. The electromagnetic contactor such as the switch device 415 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 that controls the operation of the entire vehicle 400.

[0234] The inverter 44 converts the input DC voltage into a three-phase alternating current (AC) high voltage for driving the motor. The three-phase output terminals of the inverter 44 are connected to the three-phase input terminals of the drive motor 45. The inverter 44 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 for controlling the operation of the entire vehicle. By controlling the inverter 44, the output voltage from the inverter 44 is adjusted.

[0235] The drive motor 45 rotates by electric power supplied from the inverter 44. A driving force generated by the rotation of the drive motor 45 is transmitted to the axles and drive wheels W via, for example, a differential gear unit.

[0236] Although not shown, the vehicle 400 is also equipped with a regenerative braking mechanism (regenerator). The regenerative braking mechanism rotates the drive motor 45 when the vehicle 400 is braked, and converts kinetic energy into regenerative energy as electrical energy. The regenerative energy recovered by the regenerative braking mechanism is input to the inverter 44 and converted into a direct current. The converted direct current is input to the vehicle power source 41.

[0237] One terminal of a connection line L1 is connected to the negative terminal 414 of the vehicle power supply 41. The other terminal of the connection line L1 is connected to a negative input terminal 417 of the inverter 44. A current detection unit (current detection circuit) 416 in the battery management device 411 is provided between the negative terminal 414 and the negative input terminal 417 on the connection line L1.

[0238] One terminal of a connection line L2 is connected to the positive electrode terminal 413 of the vehicle power supply 41. The other terminal of the connection line L2 is connected to a positive electrode input terminal 418 of the inverter 44. A switch device 415 is provided in the connection line L2 between the positive electrode terminal 413 and the positive electrode input terminal 418.

[0239] The external terminal 43 is connected to the battery management unit 411. The external terminal 43 can be connected to, for example, an external power source.

[0240] In response to operational inputs from the driver or the like, the vehicle ECU 42 coordinates with other management devices and control devices including the battery management device 411 to control the vehicle power supply 41, the switch device 415, the inverter 44, etc. Through the coordinated control of the vehicle ECU 42, etc., the output of power from the vehicle power supply 41 and the charging of the vehicle power supply 41 are controlled, and the entire vehicle 400 is managed. Data relating to the maintenance of the vehicle power supply 41, such as the remaining capacity of the vehicle power supply 41, is transferred between the battery management device 411 and the vehicle ECU 42 via a communication line.

[0241] The vehicle according to the sixth embodiment is equipped with the battery pack according to the fifth embodiment. Therefore, according to this embodiment, it is possible to provide a vehicle equipped with a battery pack that can exhibit excellent input / output characteristics and cycle life characteristics.

[0242] [Example] The above embodiment will now be described in more detail with reference to examples.

[0243] <Synthesis method> Example 1 The active material was synthesized by the solid phase synthesis method described below. First, the main phase was Nb2TiO7 and the coexisting phase was Nb 10 Ti2O 29 The Nb2O5 particles and TiO2 particles were mixed in a molar ratio of 1.1:1 using a dry ball mill so that the Nb / Ti ratio was 2.2. The obtained powder was placed in an alumina crucible and heated at 800°C for 10 hours, then crushed and mixed, and pre-fired (first firing) at 800°C for 10 hours to obtain precursor particles. Next, the obtained precursor particles were fired (second firing) at 1000°C for 5 hours. When the particle size distribution of the particles obtained after firing was examined, D10 was 0.3 μm or more and D90 was 10 μm or less.

[0244] Next, potassium carbonate (K2CO3) and diammonium phosphate ((NH4)2HPO4) were added to the sintered particles so that the concentrations of potassium (K) and phosphorus (P) in the finally obtained active material particles were 0.01% by mass and 0.001% by mass, respectively. The sintered particles to which the K source and P source were added were subjected to wet mixing using pure water to obtain a wet mixture. The wet mixture was then subjected to an annealing treatment to enhance crystallinity. The annealing treatment was performed at 900°C for 3 hours. The powder thus obtained was ground using an agate ball mill using a grinding medium with a diameter of 10 mm at 500 rpm for 10 minutes to obtain the active material powder according to Example 1.

[0245] (Examples 2 to 10) The active material powders of Examples 2 to 10 were obtained in the same manner as in Example 1, except that the amounts of the K source and the P source added were changed so that the particles after the main firing had the potassium concentration and the phosphorus concentration shown in Table 1 below.

[0246] Example 11 An active material powder was obtained in the same manner as in Example 4, except that the annealing treatment was carried out at 800° C. for 1 hour.

[0247] Example 12 An active material powder was obtained in the same manner as in Example 4, except that the annealing treatment was carried out at 800° C. for 3 hours.

[0248] Example 13 An active material powder was obtained in the same manner as in Example 4, except that the annealing treatment was carried out at 900° C. for 5 hours.

[0249] Example 14 An active material powder was obtained in the same manner as in Example 4, except that the annealing treatment was carried out at 900° C. for 10 hours.

[0250] Example 15 An active material powder was obtained in the same manner as in Example 4, except that when mixing the Nb source and Ti source raw materials, Nb2O5 particles and TiO2 particles were mixed in a molar ratio of 1.01:1 using a dry ball mill so that the Nb / Ti ratio was 2.02.

[0251] (Example 16) An active material powder was obtained in the same manner as in Example 4, except that when mixing the Nb source and Ti source raw materials, Nb2O5 particles and TiO2 particles were mixed in a molar ratio of 1.05:1 using a dry ball mill so that the Nb / Ti ratio was 2.1.

[0252] (Example 17) An active material powder was obtained in the same manner as in Example 4, except that when mixing the Nb source and Ti source raw materials, Nb2O5 particles and TiO2 particles were mixed in a molar ratio of 1.5:1 using a dry ball mill so that the Nb / Ti ratio was 3.0.

[0253] (Example 18) An active material powder was obtained in the same manner as in Example 4, except that when mixing the Nb source and Ti source raw materials, Nb2O5 particles and TiO2 particles were mixed in a molar ratio of 1.75:1 using a dry ball mill so that the Nb / Ti ratio was 3.5.

[0254] (Example 19) An active material powder was obtained in the same manner as in Example 4, except that when mixing the Nb source and Ti source raw materials, Nb2O5 particles and TiO2 particles were mixed in a molar ratio of 2:1 using a dry ball mill so that the Nb / Ti ratio was 4.0.

[0255] (Example 20) After obtaining the powder after the annealing treatment by the method according to Example 14, coarse particles of 10 μm or more were removed using a sieve without pulverizing with an agate ball mill, thereby obtaining an active material powder with a reduced specific surface area.

[0256] Example 21 After obtaining the powder after the annealing treatment by the method according to Example 11, the powder was subjected to pulverization at 600 rpm for 30 minutes using an agate ball mill using a pulverization medium with a diameter of 10 mm. Then, fine particles of 0.3 μm or less were removed by centrifugation. Thus, active material particles with an increased specific surface area were obtained.

[0257] Example 22 After obtaining the powder after the annealing treatment by the method according to Example 11, the powder was subjected to pulverization at 800 rpm for 40 minutes using an agate ball mill using a pulverization medium with a diameter of 10 mm. Then, fine particles of 0.3 μm or less were removed by centrifugation. Thus, active material particles with an increased specific surface area were obtained.

[0258] Example 23 An active material powder was obtained in the same manner as in Example 17, except that when mixing the raw materials of the Nb source and the Ti source, mixing was performed using an agate mortar instead of mixing using a dry ball mill. By performing mild mixing using an agate mortar instead of dry mixing using a ball mill, which applies a strong shear, a niobium-rich solid-phase reaction proceeds locally, and Nb is produced as a coexisting phase. 14 TiO 37 is generated.

[0259] (Example 24) An active material powder was obtained in the same manner as in Example 19, except that when mixing the raw materials of the Nb source and the Ti source, mixing was performed using an agate mortar instead of mixing using a dry ball mill. By performing mild mixing using an agate mortar instead of dry mixing using a ball mill, which applies a strong shear, a niobium-rich solid-phase reaction proceeds locally, and Nb is contained as a coexisting phase. 24 TiO 64 is generated.

[0260] Comparative Example 1 An active material powder was obtained in the same manner as in Example 1, except that only potassium carbonate (K2CO3) was added to the particles after main sintering so that the potassium (K) concentration in the finally obtained active material particles was 0.07 mass %.

[0261] Comparative Example 2 An active material powder was obtained in the same manner as in Example 1, except that only diammonium phosphate ((NH4)2HPO4) was added to the particles after main sintering so that the phosphorus (P) concentration in the final active material particles was 0.009 mass%.

[0262] Comparative Example 3 An active material powder was obtained in the same manner as in Example 1, except that potassium carbonate (K2CO3) and diammonium phosphate ((NH4)2HPO4) were added to the particles after main sintering so that the concentrations of potassium (K) and phosphorus (P) in the final active material particles were 5.0 mass% and 2.0 mass%, respectively.

[0263] Comparative Example 4 An active material powder was obtained in the same manner as in Example 1, except that wet mixing was carried out using pure water without adding either the K source or the P source.

[0264] Comparative Example 5 An active material powder was obtained in the same manner as in Example 1, except that, instead of adding a K source and a P source, sodium carbonate (Na2CO3) and iron chloride (FeCl2) were added to the particles after main sintering so that the concentrations of sodium (Na) and iron (Fe) in the finally obtained active material particles were both 0.05 mass%.

[0265] Comparative Example 6 The powder obtained after the annealing treatment by the method according to Example 14 was used as the active material powder according to Comparative Example 6. That is, in Comparative Example 6, the pulverization treatment was not carried out after the annealing treatment.

[0266] Comparative Example 7 After obtaining a powder after annealing treatment by the method according to Example 4, the powder was pulverized using a dry bead mill device using pulverizing media with a diameter of 3 mm for three passes to obtain an active material powder.

[0267] Comparative Example 8 An active material powder was obtained in the same manner as in Example 4, except that when the Nb source and Ti source raw materials were mixed, Nb2O5 particles and TiO2 particles were mixed in a molar ratio of 1:1 so that the Nb / Ti ratio was 2.00, in order to obtain only the Nb2TiO7 phase.

[0268] Comparative Example 9 An active material powder according to Comparative Example 9 was prepared in the same manner as in Example 1, except that the following procedure was performed.

[0269] When mixing the raw materials of the Nb source and the Ti source, the molar ratio of the Nb2O5 particles and the TiO2 particles was set to 1:1 so that only the Nb2TiO7 phase was obtained and the Nb / Ti ratio was 2.00. In addition, when the K source and the P source were added, potassium carbonate (K2CO3) and diammonium phosphate ((NH4)2HPO4) were added to the particles after the main sintering so that the concentrations of potassium (K) and phosphorus (P) in the finally obtained active material particles were 5.0 mass% and 2.0 mass%, respectively.

[0270] Comparative Example 10 An active material powder was obtained in the same manner as in Example 4, except that when mixing the Nb source and Ti source raw materials, Nb2O5 particles and TiO2 particles were mixed in a molar ratio of 2.25:1 using a dry ball mill so that the Nb / Ti ratio was 4.5.

[0271] Comparative Example 11 First, the main phase was Nb2TiO7 and the coexisting phase was Nb 10 Ti2O 29 Nb2O5 particles and TiO2 particles were mixed in a molar ratio of 1.1:1 using a dry ball mill so that the Nb / Ti ratio was 2.2. The obtained powder was placed in an alumina crucible and heated at 800°C for 10 hours, after which it was pulverized and mixed, and then pre-fired (first firing) at 800°C for 10 hours to obtain precursor particles.

[0272] Next, potassium carbonate (K2CO3) and diammonium phosphate ((NH4)2HPO4) were added to the precursor particles so that the concentrations of potassium (K) and phosphorus (P) in the finally obtained active material particles were 0.07% by mass and 0.009% by mass, respectively. The precursor particles to which the K source and P source were added were subjected to wet mixing using pure water to obtain a wet mixture.

[0273] The wet mixture was then subjected to a main firing (second firing) for 3 hours at a temperature of 1150° C. The powder thus obtained was pulverized at 500 rpm for 30 minutes using an agate ball mill using a pulverization medium with a diameter of 10 mm to obtain an active material powder according to Comparative Example 11.

[0274] Comparative Example 12 First, Nb2O5 particles and TiO2 particles were mixed in a molar ratio of 1:1 using a dry ball mill to obtain the Nb2TiO7 phase as the main phase. The obtained powder was placed in an alumina crucible and pre-fired at a temperature of 800°C for 12 hours. The powder obtained after pre-fired was placed in a platinum crucible and pre-fired at a temperature of 1200°C for 5 hours. This powder was crushed in an agate mortar and then sieved with a 25 μm mesh to obtain Nb2TiO7 particles.

[0275] Next, Nb as a subphase 10 Ti2O 29 In order to obtain the Nb2O5 phase, the molar ratio of Nb2O5 particles to TiO2 particles was set to 2.5:1, but the pre-sintering, main sintering, and sieving were performed in the same manner as in the preparation of the main phase. 10 Ti2O 29 The obtained Nb particles 10 Ti2O 29 The particles were mixed with the previously prepared Nb2TiO7 particles so that the particle content was 0.5 mass % to obtain a mixture.

[0276] Potassium carbonate (K2CO3) and diammonium phosphate ((NH4)2HPO4) were added to the resulting mixture so that the concentrations of potassium (K) and phosphorus (P) in the final active material particles were 0.01% by mass and 0.001% by mass, respectively. The mixture to which the K source and P source were added was subjected to wet mixing using pure water to obtain a wet mixture. The wet mixture was then subjected to an annealing treatment at 900°C for 3 hours.

[0277] The powder thus obtained was pulverized in an agate ball mill using pulverizing media with a diameter of 10 mm at 500 rpm for 10 minutes to obtain an active material powder according to Comparative Example 12.

[0278] <Electrochemical measurements> Using the active materials obtained in each example, a cell for electrochemical measurement was produced according to the following procedure.

[0279] 100% by mass of the active material powder obtained in each example, 10% by mass of acetylene black as a conductive agent, 5% by mass of carbon nanofiber, and 10% by mass of polyvinylidene fluoride (PVdF) as a binder were added to N-methylpyrrolidone (NMP) and mixed to obtain a slurry. This slurry was applied to one side of a current collector made of aluminum foil with a thickness of 12 μm, dried, and pressed to obtain an electrode with a density of 2.4 g / cm. 3 The electrodes were prepared as follows.

[0280] On the other hand, an electrolyte was prepared by dissolving LiPF6 supporting salt at a concentration of 1 mol / L in a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:2.

[0281] The obtained electrode was used as a working electrode, and Li metal was used as a counter electrode and a reference electrode. A three-electrode beaker cell was prepared using an electrolyte, and the electrochemical properties were evaluated as described below.

[0282] In this embodiment, the three-electrode beaker cell for this measurement uses lithium metal as the counter electrode, so the electrode potentials of the embodiment and comparative example are nobler than the counter electrode and operate as positive electrodes. Therefore, the definitions of charge and discharge are reversed when the electrodes of the embodiment and comparative example are used as negative electrodes. Here, to avoid confusion, in this embodiment, the direction in which lithium ions are inserted into the electrode is unified as charge, and the direction in which they are removed is unified as discharge. The active material of this embodiment operates as a negative electrode when combined with a known positive electrode material.

[0283] The prepared electrochemical measurement cell was charged and discharged in a potential range of 1.0V to 3.0V based on the metallic lithium electrode. The charge and discharge current value was set to 0.2C (time discharge rate), and the 0.2C discharge capacity was confirmed at room temperature. The 0.2C discharge capacity value is an index of energy density. In addition, in order to investigate the rapid discharge characteristics, after the 0.2C discharge capacity was confirmed, the charging current value was set to 0.2C again, and the 5C rapid discharge capacity was confirmed at room temperature. The 5C discharge capacity was divided by the 0.2C discharge capacity to obtain the discharge capacity ratio (5C / 0.2C). The discharge capacity ratio (5C / 0.2C) is an index for evaluating the rapid charge and discharge characteristics.

[0284] Next, in order to confirm that the active material (negative electrode material) according to the embodiment can be stably charged and discharged, a life test was performed on the cells of the embodiment and the comparative example in a 45°C environment, in which 0.2C charging and discharging were repeated in a potential range of 1.0V to 3.0V based on the metallic lithium electrode. After the initial charging and discharging, the AC impedance value of the cell at 1kHz was measured. Then, 100 cycles of charging and discharging were repeated (one cycle is one charge and discharge), and the discharge capacity retention rate and resistance increase rate after 100 cycles were examined. In order to confirm the discharge capacity retention rate after 100 cycles, charging and discharging were again performed at 0.2C (hourly discharge rate), and the discharge capacity after 100 cycles was divided by the initial discharge capacity and multiplied by 100 to calculate the cycle capacity retention rate (%) when the initial discharge capacity was 100%. Similarly, the AC impedance value at 1kHz was measured after 100 cycles, and the resistance increase rate (times) was calculated by dividing it by the AC impedance value after the initial charging and discharging. The discharge capacity retention rate and resistance increase rate after 100 cycles are indexes for evaluating cycle life characteristics.

[0285] <Various evaluations> The active material powders obtained in each example were subjected to powder X-ray diffraction, Rietveld analysis, ICP atomic emission spectrometry, TEM observation, specific surface area measurement by the BET method, and laser diffraction scattering method according to the methods described in the first embodiment.

[0286] The above results are summarized in Tables 1 to 4 below. Note that in the row of Comparative Example 5, the sodium concentration is recorded in the column "K / concentration" instead of the potassium concentration, and the iron concentration is recorded in the column "P / concentration" instead of the phosphorus concentration.

[0287] [Table 1]

[0288] [Table 2]

[0289] [Table 3]

[0290] [Table 4]

[0291] As shown in Examples 1 to 24, the secondary battery including the active material according to the embodiment not only had excellent input / output characteristics and cycle life characteristics, but also had excellent battery capacity. K and phosphorus concentration C P Ratio of (C K / C P When D10 was within the range of 2.0 to 50.0, the effect of crystal growth and the effect of grain growth inhibition were obtained in a well-balanced manner, and the electrochemical reaction in the electrode proceeded smoothly, resulting in excellent battery characteristics. Examples 12 and 13, in which D10 was 0.4 μm or more and D90 was 9.0 μm or less, showed a well-balanced excellent rate characteristic and cycle life characteristic.

[0292] When the addition of potassium and phosphorus was omitted as in Comparative Example 4, the melting point drop did not occur, and the reactivity was low even when annealing was performed. Therefore, active material particles containing unreacted impurity phases and having small crystallite sizes were obtained. When a predetermined amount of sodium and iron was included as in Comparative Example 5, the melting point drop occurred, and the particle properties were equivalent to those of the Examples, but the effect of sodium and iron on the deterioration of battery characteristics was large.

[0293] In Comparative Example 6, the particles were not crushed sufficiently, resulting in an excessively large D90, and thus the battery characteristics were poor, including insufficient formation of electronic conductive paths.On the other hand, in Comparative Example 7, the active material powder was crushed excessively, resulting in reduced crystallinity and a large specific surface area, and thus significantly poor cycle life characteristics.

[0294] When the Nb-rich phase was not included, the stability of the crystal lattice during charging and discharging was reduced, resulting in poor battery characteristics, as shown in Comparative Example 8. On the other hand, when the Nb-rich phase was present in a large amount, the effect of strengthening the bonds between the oxide ions and the Nb ions constituting the framework was excessive, as shown in Comparative Example 10, resulting in poor battery characteristics due to the impediment to the movement of lithium ions.

[0295] As in Comparative Example 11, by firing a mixture containing potassium and phosphorus at a predetermined concentration at high temperature for a long time, crystal growth progresses, but at the same time, grain growth also progresses. Therefore, coarse particles that are difficult to pulverize are generated. When powder containing such coarse particles is pulverized with a ball mill, the amount of fine powder generated when the coarse particles are crushed increases. Therefore, D10 becomes a small value of 0.18 μm, and since many coarse particles remain, D90 is also 10 μm or more. Therefore, the rate characteristic and cycle life characteristic are deteriorated, and the resistance increase after cycling is large. Since there are many coarse particles and fine powders, the reaction in the electrode is nonuniform, and the rate characteristic is deteriorated. Furthermore, the coarse particles collapse due to the change in lattice volume, and the electronic conductive network in the electrode is destroyed. In addition, the presence of fine particles increases the side reaction with the electrolyte, so the resistance increase is large.

[0296] In Comparative Example 12, even when the Nb2TiO7 phase was formed as the main phase, the Nb 10 Ti2O 29 Since firing is continuously performed at high temperatures even during phase formation, niobium titanium composite oxide particles with high hardness are already formed before the addition of the K source and P source. Therefore, when the main phase and subphase are mixed and further potassium and phosphorus are added at a predetermined concentration and then a heat treatment is performed, high-strength particles that are difficult to pulverize even with a ball mill are formed. Therefore, the rate characteristic is extremely low, and the high-strength particles gradually break during charge and discharge cycles, resulting in an increase in resistance and a decrease in capacity.

[0297] According to at least one of the embodiments and examples described above, an active material is provided. The active material includes a Nb2TiO7 phase and a Nb 10 Ti2O 29 Phase, Nb 14 TiO37 Phase and Nb 24 TiO 64 and at least one Nb-rich phase selected from the group consisting of Nb-rich phases. This active material contains potassium and phosphorus, and the total concentration of potassium and phosphorus in the active material is in the range of 0.01 mass% or more and 5.00 mass% or less. The average crystallite diameter is in the range of 80 nm to 150 nm. In a particle size distribution chart obtained by a laser diffraction scattering method, D10 is 0.3 μm or more and D90 is 10 μm or less. The active material satisfies the peak intensity ratio represented by the following formula (1).

[0298] 0 B / I A ≦0.25 (1) In formula (1), I A is the peak intensity of the maximum peak that appears at 2θ of 26.0±0.1° and is attributed to the Nb2TiO7 phase in the wide-angle X-ray diffraction peaks using CuKα radiation as an X-ray source, and I B is the peak intensity of the maximum diffraction peak which appears at 2θ of 24.9±0.2° and is attributed to the Nb-rich phase.

[0299] This active material can realize a secondary battery that can exhibit excellent input / output characteristics and cycle life characteristics.

[0300] Although several embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. The invention as originally claimed in the present application is set forth below. [1] Nb2TiO7 phase and Nb 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO​64 and at least one Nb-rich phase selected from the group consisting of Nb-rich and Nb-rich phases, a total concentration of the potassium and the phosphorus in the active material is within a range of 0.010% by mass or more and 5.00% by mass or less; In a particle size distribution chart obtained by a laser diffraction scattering method, D10 is 0.3 μm or more and D90 is 10 μm or less. The average crystallite size is in the range of 80 nm to 150 nm. An active material that satisfies a peak intensity ratio represented by the following formula (1). 0 B / I A ≦0.25 (1) In the formula (1), I A is the peak intensity of the maximum peak that appears at 2θ of 26.0±0.1° and is attributed to the Nb2TiO7 phase in the diffraction peaks obtained by wide-angle X-ray diffraction using CuKα radiation as an X-ray source, and I B is the peak intensity of the maximum peak which appears at 2θ of 24.9±0.2° in the diffraction peaks and which is attributed to the Nb-rich phase. [2] The potassium concentration C in the active material K and the phosphorus concentration C in the active material. P Ratio to (C K / C P ) is in the range of 2.0 to 50.0. [3] The active material according to [1] or [2], wherein the total concentration of the potassium and the phosphorus in the active material is in the range of 0.050 mass % or more and 2.50 mass % or less. [4] The active material according to any one of [1] to [3], wherein the average crystallite size is 90 nm or more. [5] The BET specific surface area is 0.5 m 2 / g or more 5m 2 / g or less. [6] The active material according to any one of [1] to [5], wherein in the particle size distribution chart, D10 is 0.4 μm or more. ​[7] The active material according to any one of [1] to [6], wherein in the particle size distribution chart, D90 is 9.0 μm or less. [8] Peak intensity ratio I B / I A is in the range of 0.005 or more and 0.20 or less. [9] An electrode comprising the active material according to any one of [1] to [8].

[10] The electrode according to [9], wherein the electrode includes an active material-containing layer containing the active material. A negative electrode; and an electrolyte, The secondary battery according to the present invention, wherein the negative electrode is the electrode according to [9] or

[10] .

[12] A battery pack comprising the secondary battery described in

[11] .

[13] An external terminal for supplying current; The battery pack according to

[12] , further comprising a protection circuit.

[14] The battery pack according to

[12] or

[13] , comprising a plurality of the secondary batteries, the secondary batteries being electrically connected in series, in parallel, or in a combination of series and parallel.

[15] A vehicle equipped with the battery pack according to any one of

[12] to

[14] .

[16] A vehicle as described in

[15] , including a mechanism for converting kinetic energy of the vehicle into regenerative energy. [Explanation of symbols]

[0301] 1...electrode group, 2...exterior member, 3...negative electrode, 3a...negative electrode current collector, 3b...negative electrode active material-containing layer, 3c...negative electrode current collector portion, 4...separator, 5...positive electrode, 5a...positive electrode current collector, 5b...positive electrode active material-containing layer, 6...negative electrode terminal, 7...positive electrode terminal, 21...bus bar, 22...positive electrode side lead, 23...negative electrode side lead, 24...adhesive tape, 31...container, 32...lid, 33...protective sheet, 34...printed wiring board, 35...wiring, 40...vehicle body, 41...vehicle power source, 42...electrical control device, 43...external terminal, 44...inverter, 45...driving motor, 100...secondary battery, 101...metal ion, 102...oxide ion, 103...skeletal structure portion, 104...void portion, 105, 106...area, 2 00... battery pack, 200a... battery pack, 200b... battery pack, 200c... battery pack, 300... battery pack, 300a... battery pack, 300b... battery pack, 300c... battery pack, 301a... battery pack monitoring device, 301b... battery pack monitoring device, 301c... battery pack monitoring device, 341... positive connector, 342... negative connector, 343... thermistor, 344... protection circuit, 345... wiring, 346... wiring, 347... external terminal for energizing, 348a... positive wiring, 348b... negative wiring, 400... vehicle, 411... battery management device, 412... communication bus, 413... positive terminal, 414... negative terminal, 415... switch device, L1... connection line, L2... connection line, W... drive wheel.

Claims

1. Nb 2 TiO 7 phase and Nb 10 Ti 2 O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 and at least one Nb-rich phase selected from the group consisting of Nb-rich phases, Contains potassium and phosphorus, a total concentration of the potassium and the phosphorus in the active material is in the range of 0.010% by mass or more and 5.00% by mass or less; In a particle size distribution chart obtained by a laser diffraction scattering method, D10 is 0.3 μm or more and D90 is 10 μm or less. The average crystallite size is in the range of 80 nm to 150 nm. An active material for a lithium secondary battery, which satisfies a peak intensity ratio represented by the following formula (1): 0<I B / I A ≦0.25 (1) In the formula (1), I A In the wide-angle X-ray diffraction method using CuKα radiation as an X-ray source, a diffraction peak appears at 2θ of 26.0±0.1°, and the Nb 2 TiO 7 is the peak intensity of the maximum peak assigned to the I phase, B is the peak intensity of the maximum peak that appears at 2θ of 24.9±0.2° in the diffraction peak and is attributed to the Nb-rich phase.

2. The potassium concentration C in the active material K and the phosphorus concentration C in the active material. P Ratio to (C K / C P 2. The active material for lithium secondary batteries according to claim 1, wherein the ratio of the y-axis direction of the active material to the z-axis of the lithium secondary battery is in the range of 2.0 to 50.

0.

3. 3. The active material for a lithium secondary battery according to claim 1, wherein a total concentration of the potassium and the phosphorus in the active material is in the range of 0.050% by mass to 2.50% by mass.

4. 4. The active material for a lithium secondary battery according to claim 1, wherein the average crystallite size is 90 nm or more.

5. BET specific surface area is 0.5m 2 / g or more 5m 2 The active material for lithium secondary batteries according to any one of claims 1 to 4, wherein the Mo content is 0.01 to 0.25% by mass.

6. 6. The active material for a lithium secondary battery according to claim 1, wherein in the particle size distribution chart, D10 is 0.4 μm or more.

7. 7. The active material for a lithium secondary battery according to claim 1, wherein in the particle size distribution chart, D90 is 9.0 μm or less.

8. The peak intensity ratio I B / I A The active material for a lithium secondary battery according to any one of claims 1 to 7, wherein is in the range of 0.005 or more and 0.20 or less.

9. An electrode for a lithium secondary battery comprising the active material for a lithium secondary battery according to any one of claims 1 to 8.

10. The electrode for a lithium secondary battery according to claim 9 , wherein the electrode includes an active material-containing layer that contains the active material for a lithium secondary battery.

11. A positive electrode and A negative electrode; A lithium secondary battery comprising: The negative electrode is the lithium secondary battery electrode according to claim 9 or 10.

12. A battery pack comprising the lithium secondary battery according to claim 11.

13. An external terminal for supplying electricity; The battery pack of claim 12 , further comprising a protection circuit.

14. 14. The battery pack according to claim 12, comprising a plurality of the lithium secondary batteries, the lithium secondary batteries being electrically connected in series, in parallel, or in a combination of series and parallel.

15. A vehicle equipped with the battery pack according to any one of claims 12 to 14.

16. 16. The vehicle of claim 15, further comprising a mechanism for converting kinetic energy of the vehicle into regenerative energy.

Citation Information

Patent Citations

  • Active material for battery, nonaqueous electrolyte battery, and battery pack

    JP2015088424A

  • Method for producing negative electrode active material for secondary battery

    JP2017134972A

  • Electrode, nonaqueous electrolyte battery, battery pack and vehicle

    JP2018049705A

  • Active material, electrode, secondary battery, battery pack, and vehicle

    JP2019053945A

  • Active material, electrode, secondary battery, battery pack and vehicle

    JP2019169343A