Cathode active material for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery
The positive electrode active material with a specific composition and additional metal elements stabilizes the layered structure, reducing reaction resistance and enhancing battery performance in non-aqueous electrolyte secondary batteries.
Patent Information
- Application Number
- JP2024111751
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-06-27
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-06-23
AI Technical Summary
Existing non-aqueous electrolyte secondary batteries with high Ni content and low Co content face instability in the layered structure due to increased reaction resistance, which is not adequately addressed by current technologies.
A positive electrode active material with a layered structure composed of LiNiαAlβCoγSrO2-w, where α, β, γ, and δ represent the molar ratios of Ni, Al, Co, and Sr, respectively, within specific ranges, along with the inclusion of additional metal elements like Mn, Fe, Ti, Si, Nb, Zr, Mo, or Zn, stabilizes the structure and reduces reaction resistance.
The proposed active material significantly lowers reaction resistance and stabilizes the charge/discharge cycle characteristics, maintaining battery performance and capacity.
Smart Images

Figure 2024133202000006 
Figure 2024133202000001 
Figure 2024133202000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a positive electrode active material for a non-aqueous electrolyte secondary battery, and a non-aqueous electrolyte secondary battery. [Background technology]
[0002] In recent years, non-aqueous electrolyte secondary batteries that include a positive electrode, a negative electrode, and a non-aqueous electrolyte and transfer lithium ions or the like between the positive electrode and the negative electrode to charge and discharge have been widely used as high-output, high-energy-density secondary batteries. From the viewpoint of reducing the resistance and increasing the capacity of the battery, there is a demand for improving the characteristics of a positive electrode active material contained in the positive electrode of the battery.
[0003] For example, Patent Document 1 discloses a positive electrode active material that is a lithium composite oxide having a layered structure and containing Mn, Ni, Co, Sr, and Mo, in which the Mo content is 0.1 mol % to 1.5 mol % and the Mo / Sr content ratio is 0.5 to 2.0 in molar ratio, thereby enabling an increase in capacity and improving charge / discharge cycle characteristics. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5245210 Summary of the Invention
[0005] Incidentally, in the lithium composite oxide contained in the positive electrode active material, a design that increases the Ni content to obtain a high discharge capacity and decreases the Co content to reduce manufacturing costs is conceivable. However, when the ratio of Ni to the total number of moles of metal elements excluding Li is 85 mol % or more and the ratio of Co is 10 mol % or less, the layered structure of the lithium composite oxide becomes unstable, and the reaction resistance of the battery may become high. The technology of Patent Document 1 does not take reaction resistance into consideration, and there is still room for improvement.
[0006] Therefore, an object of the present disclosure is to provide a positive electrode active material including a lithium composite oxide in which the ratio of Ni is 85 mol% or more and the ratio of Co is 10 mol% or less with respect to the total molar amount of metal elements excluding Li, and the reaction resistance of the battery is reduced.
[0007] The positive electrode active material for a non-aqueous electrolyte secondary battery according to one aspect of the present disclosure has a layered structure and has a general formula Li a Ni α Al β Co γ M δ Sr x O 2-w (where 0.95 < a < 1.05, 0.85 ≤ α ≤ 0.95, 0 < β ≤ 0.08, 0 ≤ γ ≤ 0.1, 0 ≤ δ ≤ 0.15, 0 < x ≤ 0.015, 0 ≤ w < 0.05, α + β + γ + δ = 1, and M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo, and Zn) and includes a lithium composite oxide represented by the formula. The layered structure includes a Li layer containing a metal element other than Li, and the ratio of the metal element other than Li present in the Li layer is in the range of 1 mol% or more and 2.5 mol% or less with respect to the total molar amount of metal elements excluding Li in the lithium composite oxide.
[0008] A non-aqueous electrolyte secondary battery according to one aspect of the present disclosure includes a positive electrode including the above positive electrode active material, a negative electrode, and a non-aqueous electrolyte.
[0009] According to the positive electrode active material for a non-aqueous electrolyte secondary battery according to one aspect of the present disclosure, a non-aqueous electrolyte secondary battery having low reaction resistance can be provided.
Brief Description of the Drawings
[0010] [Figure 1] It is a cross-sectional view of a non-aqueous electrolyte secondary battery which is an example of an embodiment.
Modes for Carrying Out the Invention
[0011] The layered structure of the lithium composite oxide includes a transition metal layer such as Ni, a Li layer, and an oxygen layer, and the Li ions present in the Li layer reversibly enter and exit, thereby allowing the charge and discharge reaction of the battery to proceed. Here, in the lithium composite oxide contained in the positive electrode active material, if the ratio of Ni to the total number of moles of metal elements other than Li is 85 mol % or more and the ratio of Co is 10 mol % or less, many Li ions are extracted from the Li layer during charging of the battery, making the layered structure unstable and increasing the reaction resistance of the battery. However, as in the positive electrode active material for non-aqueous electrolyte secondary batteries according to one embodiment of the present disclosure, by containing predetermined amounts of Al and Sr and further containing a predetermined amount of a metal element other than Li in the Li layer, a synergistic effect of the addition of Al and the addition of Sr is generated, and the reaction resistance can be reduced. Since Al does not change its oxidation number during charging and discharging, it is presumed that the structure of the transition metal layer is stabilized by being contained in the transition metal layer. It is presumed that Sr exists as a compound in the layered structure or on the surface of the lithium composite oxide, and that it changes the surface state of the lithium composite oxide through electronic interaction, thereby reducing the resistance. In addition, it is presumed that the presence of a predetermined amount of metal element in the Li layer will hold the Li layer in place and stabilize the layered structure even if many Li ions are extracted from the Li layer during charging of the battery, thereby suppressing deterioration of the charge / discharge cycle characteristics. In the lithium composite oxide of the present disclosure, the metal element present in the Li layer of the layered structure is mainly Ni, but metal elements other than Ni contained in the lithium composite oxide may also be present in the Li layer.
[0012] An example of an embodiment of a nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail below. A cylindrical battery in which a wound electrode body is housed in a cylindrical battery case will be exemplified below, but the electrode body is not limited to the wound type, and may be a laminate type in which a plurality of positive electrodes and a plurality of negative electrodes are alternately laminated one by one with a separator interposed therebetween. In addition, the battery case is not limited to a cylindrical shape, and may be, for example, a square shape, a coin shape, or the like, or may be a battery case made of a laminate sheet including a metal layer and a resin layer.
[0013] Fig. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery 10 according to an embodiment. As illustrated in Fig. 1, the nonaqueous electrolyte secondary battery 10 includes an electrode assembly 14, a nonaqueous electrolyte (not shown), and a battery case 15 that accommodates the electrode assembly 14 and the nonaqueous electrolyte. The electrode assembly 14 has a wound structure in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13 interposed therebetween. The battery case 15 includes a cylindrical outer can 16 with a bottom, and a sealing body 17 that closes the opening of the outer can 16.
[0014] The electrode body 14 is composed of a long positive electrode 11, a long negative electrode 12, two long separators 13, a positive electrode tab 20 joined to the positive electrode 11, and a negative electrode tab 21 joined to the negative electrode 12. The negative electrode 12 is formed to have a size slightly larger than the positive electrode 11 in order to prevent lithium deposition. That is, the negative electrode 12 is formed to be longer in the longitudinal direction and width direction (short direction) than the positive electrode 11. The two separators 13 are formed to have a size at least slightly larger than the positive electrode 11, and are arranged to sandwich the positive electrode 11, for example.
[0015] The nonaqueous electrolyte secondary battery 10 includes insulating plates 18, 19 disposed above and below the electrode body 14. In the example shown in Fig. 1, a positive electrode tab 20 attached to the positive electrode 11 passes through a through hole in the insulating plate 18 and extends toward the sealing body 17, and a negative electrode tab 21 attached to the negative electrode 12 passes outside the insulating plate 19 and extends toward the bottom side of the outer can 16. The positive electrode tab 20 is connected to the lower surface of a bottom plate 23 of the sealing body 17 by welding or the like, and a cap 27 of the sealing body 17 electrically connected to the bottom plate 23 serves as a positive electrode terminal. The negative electrode tab 21 is connected to the inner bottom surface of the outer can 16 by welding or the like, and the outer can 16 serves as a negative electrode terminal.
[0016] The exterior can 16 is, for example, a cylindrical metal container with a bottom. A gasket 28 is provided between the exterior can 16 and the sealing body 17, and the internal space of the battery case 15 is sealed. The exterior can 16 has a grooved portion 22 that supports the sealing body 17 and is formed, for example, by pressing the side portion from the outside. The grooved portion 22 is preferably formed in an annular shape along the circumferential direction of the exterior can 16, and supports the sealing body 17 on its upper surface.
[0017] The sealing body 17 has a structure in which a bottom plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are laminated in this order from the electrode body 14 side. Each member constituting the sealing body 17 has, for example, a disk shape or a ring shape, and each member except the insulating member 25 is electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks so as to push the upper valve body 26 toward the cap 27, and the current path between the lower valve body 24 and the upper valve body 26 is interrupted. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.
[0018] The positive electrode 11, negative electrode 12, separator 13 and nonaqueous electrolyte that constitute the nonaqueous electrolyte secondary battery 10 will be described in detail below, in particular the positive electrode active material contained in the positive electrode active material layer 31 that constitutes the positive electrode 11.
[0019] [Positive electrode] The positive electrode 11 has a positive electrode collector 30 and a positive electrode active material layer 31 formed on both sides of the positive electrode collector 30. For the positive electrode collector 30, a foil of a metal, such as aluminum or an aluminum alloy, that is stable in the potential range of the positive electrode 11, or a film having the metal disposed on the surface layer, can be used. The positive electrode active material layer 31 includes a positive electrode active material, a conductive material, and a binder. The thickness of the positive electrode active material layer 31 is, for example, 10 μm to 150 μm on one side of the positive electrode collector 30. The positive electrode 11 can be produced by applying a positive electrode slurry including a positive electrode active material, a conductive material, a binder, and the like to the surface of the positive electrode collector 30, drying the coating, and then compressing it to form the positive electrode active material layer 31 on both sides of the positive electrode collector 30.
[0020] Examples of the conductive material contained in the positive electrode active material layer 31 include carbon materials such as carbon black, acetylene black, ketjen black, and graphite. Examples of the binder contained in the positive electrode active material layer 31 include fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, and polyolefin. These resins may be used in combination with carboxymethyl cellulose (CMC) or its salt, polyethylene oxide (PEO), or the like.
[0021] The positive electrode active material has a layered structure and has the general formula Li a Ni α Al β Co γ M δ Sr x O 2-w (where 0.95 < a < 1.05, 0.85 ≤ α ≤ 0.95, 0 < β ≤ 0.08, 0 ≤ γ ≤ 0.1, 0 ≤ δ ≤ 0.15, 0 < x ≤ 0.015, 0 ≤ w < 0.05, α + β + γ + δ = 1, and M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo, and Zn) and contains a lithium composite oxide represented by the formula.
[0022] Examples of the layered structure of the lithium composite oxide include a layered structure belonging to the space group R-3m and a layered structure belonging to the space group C2 / m. Among these, a layered structure belonging to the space group R-3m is preferable in terms of high capacity and stability of the crystal structure.
[0023] A representing the ratio of Li in the lithium composite oxide satisfies 0.95 ≤ a < 1.05, and more preferably satisfies 0.97 ≤ a ≤ 1.03. When a is less than 0.95, the battery capacity may decrease compared to the case where a satisfies the above range. When a is 1.05 or more, more lithium compounds need to be added compared to the case where a satisfies the above range, which may not be economical from the perspective of production cost.
[0024] α, which represents the ratio of Ni to the total number of moles of metal elements excluding Li in the lithium composite oxide, satisfies 0.85 ≤ α ≤ 0.95 in order to increase the battery capacity and add other metal elements.
[0025] β, which represents the ratio of Al to the total number of moles of metal elements excluding Li in the lithium composite oxide, satisfies 0 < β ≤ 0.08. Since the oxidation number of Al does not change during charge and discharge, it is considered that the structure of the transition metal layer is stabilized by being contained in the transition metal layer. On the other hand, when the content rate of Al exceeds 8 mol%, Al impurities are generated and the battery capacity decreases. Al may be uniformly dispersed in the layered structure of the lithium composite oxide, for example, or may be present in a part of the layered structure.
[0026] Co and M (M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo, and Zn) are optional components. γ and δ, which represent the ratios of Co and M to the total number of moles of metal elements excluding Li in the lithium composite oxide, satisfy 0 ≤ γ ≤ 0.1 and 0 ≤ δ ≤ 0.15, respectively. Since Co is expensive, it is desirable to suppress the content rate of Co from the viewpoint of manufacturing cost.
[0027] x, which represents the ratio of Sr to the total number of moles of metal elements excluding Li in the lithium composite oxide, satisfies 0 < x ≤ 0.015. By containing Sr, it is considered that the surface state of the lithium composite oxide can be changed by electron interaction, and thus the resistance can be reduced. Sr exists as a compound in the layered structure or on the surface of the lithium composite oxide, and in either form, it can change the surface state of the lithium composite oxide.
[0028] The content rates of the elements constituting the lithium composite oxide can be measured by an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron probe microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), or the like.
[0029] In the lithium composite oxide, metal elements other than Li are present in the Li layer of the layered structure. The ratio of metal elements other than Li present in the Li layer of the layered structure is in the range of 1 mol% to 2.5 mol% with respect to the total molar amount of metal elements other than Li in the lithium composite oxide in order to reduce the reaction resistance of the battery. When the ratio of metal elements other than Li in the Li layer of the layered structure is less than 1 mol%, the stability of the layered structure in a state in which Li ions are extracted from the Li layer is reduced compared to when the above range is satisfied, and the reaction resistance of the battery is increased. When the ratio of metal elements other than Li in the Li layer of the layered structure is more than 2.5 mol%, the diffusibility of Li ions in the Li layer is reduced compared to when the above range is satisfied, and the battery capacity is reduced and the reaction resistance of the battery is increased. The metal element present in the Li layer of the layered structure is mainly Ni, but may contain other metal elements.
[0030] The proportion of metal elements other than Li in the Li layer of the layered structure can be obtained from the results of Rietveld analysis of the X-ray diffraction pattern obtained by X-ray diffraction measurement of the lithium composite oxide.
[0031] The X-ray diffraction pattern is obtained by a powder X-ray diffraction method using a powder X-ray diffractometer (manufactured by Rigaku Corporation, product name "RINT-TTR", radiation source Cu-Kα) under the following conditions. Measurement range: 15-120° Scan speed: 4° / min Analysis range: 30-120° Background: B-spline Profile function: Split pseudo-Voigt function Constraint condition: Li(3a)+Ni(3a)=1 Ni(3a) + Ni(3b) = α (α is the Ni content in each) ICSD No.:98-009-4814 In addition, the Rietveld analysis software PDXL2 (Rigaku Corporation) is used for the Rietveld analysis of the X-ray diffraction patterns.
[0032] The lithium composite oxide preferably has a lattice constant a indicating the length of the a-axis of the crystal structure obtained from the results of the X-ray diffraction pattern by the above X-ray diffraction in the range of 2.870 Å < a < 2.877 Å, and a lattice constant c indicating the length of the c-axis in the range of 14.18 Å < c < 14.21 Å. When the lattice constant a is 2.870 Å or less, compared with the case where the above range is satisfied, the interatomic distance in the crystal structure becomes narrow and unstable, and the reaction resistance of the battery may increase. Also, when the lattice constant a is 2.877 Å or more, the interatomic distance in the crystal structure becomes wide and unstable, and the output characteristics of the battery may deteriorate compared with the case where the above range is satisfied. Further, when the lattice constant c is 14.18 Å or less, the interatomic distance in the crystal structure becomes narrow and unstable, and the reaction resistance of the battery may increase compared with the case where the above range is satisfied. Also, when the lattice constant c is 14.21 Å or more, the interatomic distance in the crystal structure becomes wide and unstable, and the output characteristics of the battery may deteriorate compared with the case where the above range is satisfied.
[0033] The lithium composite oxide preferably has a crystallite size s calculated by the Scherrer equation from the full width at half maximum of the diffraction peak of the (104) plane of the X-ray diffraction pattern by the above X-ray diffraction in the range of 400 Å ≤ s ≤ 800 Å. When the crystallite size s of the lithium composite oxide is less than 400 Å, compared with the case where the above range is satisfied, the crystallinity decreases and the reaction resistance of the battery may increase. Also, when the crystallite size s of the lithium composite oxide exceeds 800 Å, compared with the case where the above range is satisfied, the diffusivity of Li deteriorates and the output characteristics of the battery may deteriorate. The Scherrer equation is represented by the following formula.
[0034] s = Kλ / Bcosθ In the above formula, s is the crystallite size, λ is the wavelength of the X-ray, B is the full width at half maximum of the diffraction peak of the (104) plane, θ is the diffraction angle (rad), and K is the Scherrer constant. In this embodiment, K is taken as 0.9.
[0035] The content of the lithium composite oxide in the positive electrode active material is preferably 90 mass% or more, and more preferably 99 mass% or more, relative to the total mass of the positive electrode active material, from the standpoint of, for example, improving the capacity of the battery and effectively suppressing deterioration of the charge-discharge cycle characteristics.
[0036] The positive electrode active material of the present embodiment may contain other lithium composite oxides in addition to the lithium composite oxide of the present embodiment, such as lithium composite oxides having a Ni content of 0 mol % or more and less than 85 mol %.
[0037] Next, an example of a method for producing a lithium composite oxide will be described.
[0038] The method for producing a lithium composite oxide includes, for example, a first step of obtaining a composite oxide containing Ni, Al and an arbitrary metal element, a second step of mixing the composite oxide obtained in the first step with a lithium compound to obtain a mixture, and a third step of firing the mixture. The ratio of metal elements other than Li in the Li layer of the layered structure of the finally obtained lithium composite oxide, the lattice constant a, the lattice constant c, and the crystallite size s are each adjusted by controlling, for example, the mixing ratio of the raw materials in the second step and the firing temperature and time in the third step.
[0039] In the first step, for example, while stirring a solution of a metal salt containing Ni, Al, and an arbitrary metal element (Co, Mn, Fe, etc.), an alkaline solution such as sodium hydroxide is dropped to adjust the pH to the alkaline side (e.g., 8.5 to 12.5), thereby precipitating (co-precipitating) a composite hydroxide containing Ni, Al, and the arbitrary metal element, and the composite hydroxide is calcined to obtain a composite oxide containing Ni, Al, and the arbitrary metal element. The calcination temperature is not particularly limited, but is, for example, in the range of 300°C to 600°C.
[0040] In the second step, the composite oxide obtained in the first step is mixed with a lithium compound and a strontium compound to obtain a mixture. Examples of the lithium compound include Li2CO3, LiOH, Li2O2, Li2O, LiNO3, LiNO2, Li2SO4, LiOH·H2O, LiH, and LiF. Examples of the strontium compound include Sr(OH)2, SrO, SrCo3, SrSO4, and Sr(NO3)2. The mixing ratio of the composite oxide obtained in the first step and the lithium compound is preferably such that the molar ratio of metal elements other than Li:Li is in the range of 1:0.98 to 1:1.1, in order to easily adjust each of the parameters to the ranges specified above. In the second step, when the composite oxide obtained in the first step is mixed with the lithium compound and the strontium compound, other metal raw materials may be added as necessary. The other metal raw materials are oxides containing metal elements other than the metal elements constituting the composite oxide obtained in the first step.
[0041] In the third step, the mixture obtained in the second step is calcined at a predetermined temperature and time to obtain the lithium composite oxide according to the present embodiment. The calcination of the mixture in the third step includes a multi-stage calcination process including a first calcination process in which the mixture is calcined in a calcination furnace under oxygen flow at a first heating rate to a first set temperature of 450°C to 680°C, and a second calcination process in which the calcined product obtained in the first calcination process is calcined in a calcination furnace under oxygen flow at a second heating rate to a second set temperature of more than 680°C to 800°C. Here, the first heating rate is in the range of 1.5°C / min to 5.5°C / min, and the second heating rate is slower than the first heating rate and is in the range of 0.1°C / min to 3.5°C / min. By such multi-stage firing, in the lithium transition metal oxide of the present embodiment finally obtained, the ratio of metal elements other than Li present in the Li layer of the layered structure, the lattice constant a, the lattice constant c, the crystallite size s, and other parameters can be adjusted to the above-specified ranges. The first heating rate and the second heating rate may be set in multiples for each temperature region as long as they are within the above-specified ranges. The holding time of the first set temperature in the first firing step is preferably 0 hours or more and 5 hours or less, more preferably 0 hours or more and 3 hours or less, in terms of adjusting each of the above parameters of the lithium transition metal oxide to the above-specified ranges. The holding time of the first set temperature is the time during which the first set temperature is maintained after the first set temperature is reached. The holding time of the second set temperature in the second firing step is preferably 1 hour or more and 10 hours or less, more preferably 1 hour or more and 5 hours or less, in terms of adjusting each of the above parameters of the lithium transition metal oxide to the above-specified ranges. The holding time of the second set temperature is the time during which the second set temperature is maintained after the second set temperature is reached. When the mixture is fired, the above parameters are adjusted to fall within the above-specified ranges, for example, in an oxygen flow with an oxygen concentration of 60% or more, and the flow rate of the oxygen flow is set at 10 cm 3 The flow rate can be in the range of 0.2 mL / min to 4 mL / min per kg of mixture and 0.3 L / min or more per kg of mixture.
[0042] [Negative electrode] The negative electrode 12 has a negative electrode current collector 40 and negative electrode active material layers 41 formed on both sides of the negative electrode current collector 40. As the negative electrode current collector 40, a foil of a metal stable within the potential range of the negative electrode 12 such as copper or a copper alloy, a film having such a metal disposed on the surface layer, or the like can be used. The negative electrode active material layer 41 contains a negative electrode active material and a binder. The thickness of the negative electrode active material layer 41 is, for example, 10 μm to 150 μm on one side of the negative electrode current collector 40. The negative electrode 12 can be manufactured by applying a negative electrode slurry containing a negative electrode active material, a binder, etc. to the surface of the negative electrode current collector 40, drying the coating film, and then rolling to form the negative electrode active material layer 41 on both sides of the negative electrode current collector 40.
[0043] The negative electrode active material contained in the negative electrode active material layer 41 is not particularly limited as long as it can reversibly occlude and release lithium ions. Generally, a carbon material such as graphite is used. The graphite may be any of natural graphite such as flake graphite, massive graphite, and earthy graphite, artificial massive graphite, and artificial graphite such as graphitized mesophase carbon microbeads. Further, as the negative electrode active material, a metal that alloys with Li such as Si or Sn, a metal compound containing Si or Sn, a lithium titanium composite oxide, or the like may be used. Further, those provided with a carbon coating may be used. For example, a Si-containing compound represented by SiO y (0.5 ≦ y ≦ 1.6), or Li 2z SiO (2+z) A Si-containing compound in which fine particles of Si are dispersed in a lithium silicate phase represented by (0 < z < 2) may be used in combination with graphite.
[0044] As the binder contained in the negative electrode active material layer 41, a fluorine-containing resin such as PTFE or PVdF, PAN, polyimide, acrylic resin, polyolefin, or the like may be used as in the case of the positive electrode 11, but preferably styrene-butadiene rubber (SBR) is used. Further, the negative electrode active material layer 41 may contain CMC or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol (PVA), or the like.
[0045] [Separator] For example, a porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have a single-layer structure or a laminated structure. In addition, a highly heat-resistant resin layer such as an aramid resin, or a filler layer containing an inorganic compound filler may be provided on the surface of the separator 13.
[0046] [Non-aqueous electrolyte] The non-aqueous electrolyte includes, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. For example, esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these can be used as the non-aqueous solvent. The non-aqueous solvent may contain a halogen-substituted product in which at least a part of the hydrogen of these solvents is substituted with a halogen atom such as fluorine. Examples of the halogen-substituted product include fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, and fluorinated chain carboxylates such as methyl fluoropropionate (FMP).
[0047] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylates such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain carboxylates such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).
[0048] Examples of the above ethers include cyclic ethers such as 1,3 - dioxolane, 4 - methyl - 1,3 - dioxolane, tetrahydrofuran, 2 - methyltetrahydrofuran, propylene oxide, 1,2 - butylene oxide, 1,3 - dioxane, 1,4 - dioxane, 1,3,5 - trioxane, furan, 2 - methylfuran, 1,8 - cineole, crown ether, etc.; and chain ethers such as 1,2 - dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o - dimethoxybenzene, 1,2 - diethoxyethane, 1,2 - dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1 - dimethoxymethane, 1,1 - diethoxyethane, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, etc.
[0049] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-m (C n F 2n+1 ) m (1 < m < 6, n is 1 or 2), LiB 10 Cl 10 , LiCl, LiBr, LiI, lithium chloroborane, lithium lower aliphatic carboxylate, borate salts such as Li2B4O7, Li(B(C2O4)F2), etc.; LiN(SO2CF3)2, LiN(C1F 2p+1 SO2)(C q F 2q+1Examples of the lithium salt include imide salts such as LiPF6, LiPF2, and LiPF6 (p and q are integers of 0 or more). The lithium salt may be used alone or in combination of two or more. Among these, LiPF6 is preferably used from the viewpoints of ion conductivity, electrochemical stability, and the like. The concentration of the lithium salt is, for example, 0.8 mol to 1.8 mol per 1 L of the non-aqueous solvent. Furthermore, vinylene carbonate or a propane sultone-based additive may be added. EXAMPLES
[0050] The present disclosure will be further described below with reference to examples and comparative examples, but the present disclosure is not limited to the following examples. In order to facilitate comparison, comparative examples in which the total molar amount of metal elements other than Li in the lithium composite oxide is not 1 are also included.
[0051] [Preparation of positive electrode active material] <Example 1-1> [Ni 0.86 Al 0.03 Co 0.03 Mn 0.08 The composite hydroxide represented by the formula ](OH)2 was calcined at 500°C for 8 hours to obtain the composite oxide (Ni 0.86 Al 0.03 Co 0.03 Mn 0.08 LiOH, Sr(OH)2, Ti(OH)4 and the above composite oxide were mixed so that the molar ratio of Li to the total amount of Ni, Al, Co, Mn, Ti and Sr was 1.03:1 to obtain a mixture. 3 The mixture was fired at a temperature rise rate of 2.0°C / min from room temperature to 650°C, and then fired at a temperature rise rate of 0.5°C / min from 650°C to 780°C under a flow rate of 2 mL / min per kg of mixture and 5 L / min per kg of mixture. The fired product was washed with water to remove impurities, and a lithium composite oxide was obtained. The composition of the lithium composite oxide obtained above was measured using an ICP optical emission spectrometer (manufactured by Thermo Fisher Scientific, product name "iCAP6300"), and the composition was found to be LiNi 0.85 Al 0.03 Co0.03 Mn 0.08 Ti 0.01 Sr 0.001 This was used as the positive electrode active material of Example 1-1.
[0052] <Comparative Example 1-1> LiOH, Ti(OH)4 and composite oxides (Ni 0.86 Al 0.03 Co 0.03 Mn 0.08 A lithium composite oxide was obtained in the same manner as in Example 1-1, except that Li was mixed with O2) so that the molar ratio of Li to the total amount of Ni, Al, Co, Mn, and Ti was 1.03:1. The composition of the obtained lithium composite oxide was LiNi 0.85 Al 0.03 Co 0.03 Mn 0.08 Ti 0.01 This was used as the positive electrode active material of Comparative Example 1-1.
[0053] <Comparative Example 1-2> [Ni 0.85 Co 0.05 Mn 0.1 ](OH)2 was used to synthesize the complex hydroxide (LiOH and complex oxide (Ni 0.85 Co 0.05 Mn 0.1 A lithium composite oxide was obtained in the same manner as in Example 1-1, except that Li was mixed with O2) so that the molar ratio of Li to the total amount of Ni, Co, and Mn was 1.1:1. 0.85 Co 0.05 Mn 0.1 This was used as the positive electrode active material of Comparative Example 1-2.
[0054] <Comparative Example 1-3> [Ni 0.85 Co 0.05 Mn 0.1 ](OH)2 was used, and LiOH, Sr(OH)2 and the composite oxide (Ni 0.85 Co 0.05 Mn 0.1A lithium composite oxide was obtained in the same manner as in Example 1-1, except that Li was mixed with O2) so that the molar ratio of Li to the total amount of Ni, Co, Mn and Sr was 1.08:1 to obtain a mixture. The composition of the obtained lithium composite oxide was LiNi 0.85 Co 0.05 Mn 0.1 Sr 0.01 This was used as the positive electrode active material of Comparative Example 1-3.
[0055] <Comparative Example 1-4> [Ni 0.88 Al 0.09 Co 0.03 ](OH)2 was used to synthesize the complex hydroxide (LiOH and complex oxide (Ni 0.88 Al 0.09 Co 0.03 A lithium composite oxide was obtained in the same manner as in Example 1-1, except that Li and O2) were mixed so that the molar ratio of Li to the total amount of Ni, Al and Co was 1.03:1. 0.88 Al 0.09 Co 0.03 This was used as the positive electrode active material of Comparative Example 1-4.
[0056] <Comparative Example 1-5> [Ni 0.88 Al 0.09 Co 0.03 ](OH)2 was used, and LiOH, Sr(OH)2 and the composite oxide (Ni 0.88 Al 0.09 Co 0.03 A lithium composite oxide was obtained in the same manner as in Example 1-1, except that Li was mixed with O2) so that the molar ratio of Li to the total amount of Ni, Al, Co and Sr was 1.03:1. 0.88 Al 0.09 Co 0.03 Sr 0.01 This was used as the positive electrode active material of Comparative Example 1-5.
[0057] <Example 2-1> [Ni 0.94 Al0.05 Co 0.01 A composite hydroxide represented by the formula ](OH)2 was used and calcined at 500°C for 8 hours to obtain a composite oxide (Ni 0.94 Al 0.05 Co 0.01 LiOH, Sr(OH)2, and the above composite oxide were mixed so that the molar ratio of Li to the total amount of Ni, Al, Co, and Sr was 1.03:1 to obtain a mixture. 3 The mixture was fired at a temperature rise rate of 3.0°C / min from room temperature to 650°C, and then fired at a temperature rise rate of 0.5°C / min from 650°C to 700°C under a flow rate of 2 mL / min per kg of mixture and 5 L / min per kg of mixture. The fired product was washed with water to remove impurities, and a lithium composite oxide was obtained. The composition of the resulting lithium composite oxide was LiNi 0.94 Al 0.05 Co 0.01 Sr 0.001 This was used as the positive electrode active material of Example 2-1.
[0058] <Example 2-2> [Ni 0.94 Co 0.05 Mn 0.005 ](OH)2 was used, and LiOH, Nb2O5, Sr(OH)2 and composite oxides (Ni 0.94 Co 0.05 Mn 0.005 A lithium composite oxide was obtained in the same manner as in Example 2-1, except that Li, Ni, Co, Mn, Nb, and Sr were mixed with Li to obtain a mixture having a molar ratio of 1.03:1 between the total amount of Ni, Co, Mn, Nb, and Sr, and the mixture was fired from room temperature to 650°C at a heating rate of 1.5°C / min, and then fired from 650°C to 700°C at a heating rate of 1.0°C / min. The composition of the obtained lithium composite oxide was LiNi 0.94 Al 0.05 Mn 0.005 Nb 0.005 Sr 0.01 This was used as the positive electrode active material of Example 2-2.
[0059] <Comparative Example 2-1> LiOH and composite oxide (Ni 0.94 Al 0.05 Co 0.01 A lithium composite oxide was obtained in the same manner as in Example 2-1, except that Li was mixed with O2) so that the molar ratio of Li to the total amount of Ni, Al and Co was 1.03:1. 0.94 Al 0.05 Co 0.01 This was used as the positive electrode active material of Comparative Example 2-1.
[0060] <Comparative Example 2-2> LiOH, Sr(OH)2 and composite oxides (Ni 0.94 Al 0.05 Co 0.01 A lithium composite oxide was obtained in the same manner as in Example 2-1, except that Li was mixed with O2) so that the molar ratio of Li to the total amount of Ni, Al, Co and Sr was 1.13:1. 0.94 Al 0.05 Co 0.01 Sr 0.01 This was used as the positive electrode active material of Comparative Example 2-2.
[0061] <Comparative Example 2-3> A lithium composite oxide was obtained in the same manner as in Example 2-1, except that the temperature was increased from room temperature to 650°C at a rate of 6.0°C / min, and then increased from 650°C to 750°C at a rate of 5.0°C / min. The composition of the obtained lithium composite oxide was LiNi 0.94 Al 0.05 Co 0.01 Sr 0.01 This was used as the positive electrode active material of Comparative Example 2-3.
[0062] <Example 3-1> [Ni 0.91 Al 0.04 Co 0.05 A composite hydroxide represented by the formula ](OH)2 was used and calcined at 500°C for 8 hours to obtain a composite oxide (Ni 0.91 Al 0.04 Co 0.05LiOH, Sr(OH)2, and the above composite oxide were mixed so that the molar ratio of Li to the total amount of Ni, Al, Co, and Sr was 1.03:1 to obtain a mixture. 3 The mixture was fired at a temperature rise rate of 2.0°C / min from room temperature to 650°C, and then at a temperature rise rate of 0.5°C / min from 650°C to 720°C under a flow rate of 2 mL / min per kg of mixture and 5 L / min per kg of mixture. The fired product was washed with water to remove impurities, and a lithium composite oxide was obtained. The composition of the resulting lithium composite oxide was LiNi 0.91 Al 0.04 Co 0.05 Sr 0.0005 This was used as the positive electrode active material of Example 3-1.
[0063] <Example 3-2> LiOH, Sr(OH)2 and composite oxides (Ni 0.91 Al 0.04 Co 0.05 A lithium composite oxide was obtained in the same manner as in Example 3-1, except that Li was mixed with O2) so that the molar ratio of Li to the total amount of Ni, Al, Co and Sr was 1.01:1. 0.91 Al 0.04 Co 0.05 Sr 0.013 This was used as the positive electrode active material of Example 3-2.
[0064] <Example 3-3> [Ni 0.915 Al 0.04 Co 0.045 ](OH)2, and LiOH, Sr(OH)2, SiO, and composite oxides (Ni 0.91 Al 0.04 Co 0.045 A lithium composite oxide was obtained in the same manner as in Example 3-1, except that Li was mixed with O2) so that the molar ratio of Li to the total amount of Ni, Al, Co, Si and Sr was 1.03:1. 0.91 Al 0.04 Co 0.045S 0.005 Sr 0.001 This was used as the positive electrode active material of Example 3-3.
[0065] <Comparative Example 3-1> LiOH and composite oxide (Ni 0.91 Al 0.04 Co 0.05 A lithium composite oxide was obtained in the same manner as in Example 3-1, except that Li was mixed with O2) so that the molar ratio of Li to the total amount of Ni, Al and Co was 1.03:1. 0.91 Al 0.04 Co 0.05 This was used as the positive electrode active material of Comparative Example 3-1.
[0066] <Comparative Example 3-2> LiOH, Sr(OH)2 and composite oxides (Ni 0.91 Al 0.04 Co 0.05 A lithium composite oxide was obtained in the same manner as in Example 3-1, except that Li, Ni, Al, Co, and Sr were mixed in a molar ratio of 1.03:1 between Li and the total amount of Ni, Al, Co, and Sr, and that the mixture was fired from room temperature to 650°C at a heating rate of 3.0°C / min, and then fired from 650°C to 750°C at a heating rate of 1.0°C / min. The composition of the obtained lithium composite oxide was LiNi 0.91 Al 0.04 Co 0.05 Sr 0.02 This was used as the positive electrode active material of Comparative Example 3-2.
[0067] <Comparative Example 3-3> [Ni 0.92 Al 0.04 Co 0.04 The composite hydroxide represented by the formula [OH]2 was used, and LiOH, Mg(OH)2 and the composite oxide (Ni 0.92 Al 0.04 Co 0.04A lithium composite oxide was obtained in the same manner as in Example 3-1, except that Li was mixed with O2) so that the molar ratio of Li to the total amount of Ni, Al, Co and Mg was 1.03:1. 0.91 Al 0.04 Co 0.04 Mg 0.01 This was used as the positive electrode active material of Comparative Example 3-3.
[0068] <Comparative Example 3-4> [Ni 0.92 Al 0.04 Co 0.04 ](OH)2 was used, and LiOH, Ba(OH)2 and the composite oxide (Ni 0.92 Al 0.04 Co 0.04 A lithium composite oxide was obtained in the same manner as in Example 1-1, except that Li was mixed with O2) so that the molar ratio of Li to the total amount of Ni, Al, Co and Ba was 1.03:1. 0.91 Al 0.04 Co 0.04 Ba 0.01 This was used as the positive electrode active material of Comparative Example 3-4.
[0069] <Example 4-1> [Ni 0.88 Al 0.03 Co 0.08 Fe 0.01 A composite hydroxide represented by the formula ](OH)2 was used, and calcined at 400°C for 8 hours to obtain a composite oxide (Ni 0.88 Al 0.03 Co 0.03 Fe 0.01 LiOH, Sr(OH)2, and the above composite oxide were mixed so that the molar ratio of Li to the total amount of Ni, Al, Co, Fe, and Sr was 1.03:1 to obtain a mixture. The mixture was then placed under an oxygen flow with an oxygen concentration of 95% (10 cm 3The mixture was fired at a temperature rise rate of 2.0°C / min from room temperature to 670°C, and then fired at a temperature rise rate of 0.5°C / min from 670°C to 760°C under a flow rate of 2 mL / min per kg of mixture and 5 L / min per kg of mixture. The fired product was washed with water to remove impurities, and a lithium composite oxide was obtained. The composition of the resulting lithium composite oxide was LiNi 0.88 Al 0.03 Co 0.08 Fe 0.01 Sr 0.0008 This was used as the positive electrode active material of Example 4-1.
[0070] <Comparative Example 4-1> LiOH and composite oxide (Ni 0.88 Al 0.03 Co 0.08 Fe 0.01 A lithium composite oxide was obtained in the same manner as in Example 4-1, except that Li and O2) were mixed so that the molar ratio of Li to the total amount of Ni, Al, Co and Fe was 1.03:1. The composition of the obtained lithium composite oxide was LiNi 0.88 Al 0.03 Co 0.08 Fe 0.01 This was used as the positive electrode active material of Comparative Example 4-1.
[0071] The lithium composite oxides (positive electrode active materials) of the Examples and Comparative Examples were subjected to powder X-ray diffraction measurement under the conditions described above to obtain X-ray diffraction patterns. Diffraction lines indicating a layered structure were confirmed in all of the X-ray diffraction patterns of the Examples and Comparative Examples.
[0072] From the X-ray diffraction patterns of each Example and Comparative Example, the proportion of metal elements other than Li, the lattice constant a, the lattice constant c, and the crystallite size s were determined. The results are summarized in Table 1. The measurement method is as described above.
[0073] [Table 1]
[0074] Test cells were fabricated as follows using the lithium composite oxides (positive electrode active materials) of the examples and comparative examples.
[0075] [Preparation of positive electrode] The positive electrode active material of Example 1-1 was mixed in a ratio of 91 parts by mass, 7 parts by mass of acetylene black as a conductive material, and 2 parts by mass of polyvinylidene fluoride as a binder, and this was mixed with N-methyl-2-pyrrolidone (NMP) to prepare a positive electrode slurry. The slurry was then applied to a positive electrode current collector made of aluminum foil with a thickness of 15 μm, and the coating film was dried, and then the coating film was rolled with a rolling roller to prepare a positive electrode. Positive electrodes were also prepared in the same manner in other examples and comparative examples.
[0076] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), methyl ethyl carbonate (MEC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF6) was dissolved in the mixed solvent to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0077] [Preparation of test cell] The positive electrode of Example 1-1 and the negative electrode made of lithium metal foil were laminated so as to face each other through a separator, and then wound to prepare an electrode body (about 66 mAh). Next, the electrode body and the non-aqueous electrolyte were inserted into an aluminum exterior body to prepare a test cell. Positive electrodes were prepared in the same manner in the other examples and comparative examples.
[0078] [Measurement of reaction resistance] The above test cell was charged at a constant current of 13.2 mA under a temperature condition of 25° C. until the cell voltage reached 4.3 V, and then charged at a constant voltage of 4.3 V until the current value reached 0.66 mA. Subsequently, a constant current discharge was performed at 13.2 mA until the cell voltage reached 2.5 V. Thereafter, again under a temperature condition of 25° C., a constant current charge was performed at 13.2 mA until the cell voltage reached 4.3 V, and then a constant voltage charge was performed at 4.3 V until the current value reached 0.66 mA. Next, the test cell was measured for AC impedance at 20 kHz to 0.01 Hz using an AC impedance measuring device, and a Cole-Cole plot was drawn from the measured data, and the reaction resistance was calculated from the size of the arc between 10 Hz and 0.1 Hz.
[0079] The reaction resistances of the examples and comparative examples are shown in Tables 2 to 5. The reaction resistance of the test cell of Example 1-1 shown in Table 2 is expressed relatively to the reaction resistance of the test cell of Comparative Example 1-1, which is set to 100. Similarly, the reaction resistance of the test cell of Comparative Example 1-3 is expressed relatively to the reaction resistance of the test cell of Comparative Example 1-2, which is set to 100, and the reaction resistance of the test cell of Comparative Example 1-5 is expressed relatively to the reaction resistance of the test cell of Comparative Example 1-4, which is set to 100.
[0080] The reaction resistances of the test cells of Examples 2-1 to 2-2 and Comparative Examples 2-2 to 2-3 shown in Table 3 are expressed relative to the reaction resistance of the test cell of Comparative Example 2-1, which is set to 100.
[0081] The reaction resistances of the test cells of Examples 3-1 to 3-3 and Comparative Examples 3-2 to 3-4 shown in Table 4 are expressed relative to the reaction resistance of the test cell of Comparative Example 3-1, which is set to 100.
[0082] The reaction resistance of the test cell of Example 4-1 shown in Table 5 is expressed relative to the reaction resistance of the test cell of Comparative Example 4-1, which is set to 100.
[0083] [Table 2]
[0084] [Table 3]
[0085] [Table 4]
[0086] [Table 5]
[0087] In Table 2, Example 1-1 containing 0.1 mol% Sr had a lower reaction resistance than Comparative Example 1-1 not containing Sr, demonstrating the effect of containing Sr. In addition, in Comparative Examples 1-2 to 1-5, the Al content was 0 mol% or 9 mol%, which was outside the range of 0<β≦0.08, so the reaction resistance did not change regardless of the presence or absence of Sr. In addition, it is presumed from Example 1-1 that the lithium composite oxide (positive electrode active material) may contain Mn and Ti.
[0088] In Table 3, Example 2-1, in which the ratio of metal elements other than Li in the Li layer is 1.2, had a lower reaction resistance than Comparative Example 2-1 due to the effect of containing Sr. However, Comparative Examples 2-2 and 2-3, in which the ratios of metal elements other than Li in the Li layer are 0.4 and 3.0, respectively, contained Sr but had a higher reaction resistance than Comparative Example 2-1. Also, from Example 2-2, it is presumed that the lithium composite oxide (positive electrode active material) may contain Mn and Nb.
[0089] In Table 4, Examples 3-1 to 3-3 had lower reaction resistance than Comparative Example 3-1 due to the effect of containing Sr. On the other hand, Comparative Example 3-2 contained a large amount of Sr, 2 mol %, and therefore had a higher reaction resistance than Comparative Example 3-1. Comparative Examples 3-3 and 3-4 contained Mg and Ba instead of Sr, respectively, but had almost the same reaction resistance as Comparative Example 3-1. It is also inferred from Example 3-3 that the lithium composite oxide (positive electrode active material) may contain Si.
[0090] Also in Table 5, Example 4-1 containing 0.08 mol % Sr had a lower reaction resistance than Comparative Example 4-1 containing no Sr, demonstrating the effect of containing Sr. Also, from Example 4-1, it is inferred that the lithium composite oxide (positive electrode active material) may contain Fe. [Explanation of symbols]
[0091] REFERENCE SIGNS LIST 10 non-aqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 15 battery case, 16 outer can, 17 sealing body, 18, 19 insulating plate, 20 positive electrode tab, 21 negative electrode tab, 22 grooved portion, 23 bottom plate, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cap, 28 gasket, 30 positive electrode current collector, 31 positive electrode active material layer, 40 negative electrode current collector, 41 negative electrode active material layer
Claims
1. The lithium composite oxide has a layered structure and contains at least Ni, Al, and Sr, a, which indicates the ratio of Ni to the total number of moles of metal elements excluding Li in the lithium composite oxide, is 0.85≦α≦0.95, β, which indicates a ratio of Al to the total number of moles of metal elements excluding Li in the lithium composite oxide, is 0<β≦0.08, x, which indicates a ratio of Sr to the total number of moles of metal elements excluding Li in the lithium composite oxide, is 0<x≦0.015; the layered structure includes a Li layer containing a metal element other than Li, and a ratio of the metal element other than Li present in the Li layer is in the range of 1 mol % or more and 2.5 mol % or less with respect to a total molar amount of the metal elements excluding Li in the lithium composite oxide.
2. 2. The positive electrode active material for a nonaqueous electrolyte secondary battery according to claim 1, wherein the lithium composite oxide has a lattice constant a indicating an a-axis length of a crystal structure and a lattice constant c indicating a c-axis length of a crystal structure obtained from an analysis result of an X-ray diffraction pattern by X-ray diffraction, the lattice constant a being in the ranges of 2.870 Å<a<2.877 Å and 14.18 Å<c<14.21 Å.
3. 3. The positive electrode active material for a nonaqueous electrolyte secondary battery according to claim 1, wherein the lithium composite oxide has a crystallite size s in the range of 400 Å≦s≦800 Å, the crystallite size s being calculated from a half-width of a diffraction peak of a (104) plane in an X-ray diffraction pattern by Scherrer's formula.
4. A non-aqueous electrolyte secondary battery comprising a positive electrode containing the positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 3, a negative electrode, and a non-aqueous electrolyte.
Citation Information
Patent Citations
Lithium-containing composite oxide and production method of the same