Electrolyte composite body for secondary battery

The electrolyte composite for secondary batteries, with a porous structure and MOF properties, addresses performance issues by ensuring smooth electrolyte flow and high ion conductivity, stabilizing battery performance and extending its life.

JP2024134281AInactive Publication Date: 2024-10-03SEKISUI CHEMICAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023044503
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Secondary batteries require improved performance to meet the demands of increased cruising range, safety, reduced costs, and fast charging in electric vehicles.

Method used

An electrolyte composite for secondary batteries is developed, featuring a porous structure with electrolyte located in its pores, where the pore opening diameter is equal to or greater than the maximum length of the electrolyte, and comprising a metal-organic framework (MOF) with specific properties such as high BET specific surface area, thermal stability, and optimal pore volume, supporting a metal salt electrolyte that enhances ion conductivity.

Benefits of technology

The electrolyte composite improves the performance of secondary batteries by facilitating smooth electrolyte flow and diffusion, increasing ion conductivity, and enhancing thermal stability, thereby stabilizing battery performance and extending its life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134281000002
    Figure 2024134281000002
  • Figure 2024134281000001
    Figure 2024134281000001
Patent Text Reader

Abstract

To enhance the performance of a secondary battery by improving an electrolyte composite body for a secondary battery.SOLUTION: An electrolyte composite body for a secondary battery includes a porous structure and an electrolyte. A part of or all the electrolyte exists in pores of the porous structure. An opening diameter R of the pore measured by a measurement method A below is more than or equal to a maximum length L of a material of the electrolyte.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrolyte composite for a secondary battery. [Background technology]

[0002] In order to achieve carbon neutrality, regulations on automobile exhaust gases are becoming stricter in each country, and the electrification of automobiles is becoming a global trend. In order to further popularize electric vehicles, it is necessary to increase the driving range, improve safety, reduce costs, and enable fast charging. One solution to these problems is to improve the performance of secondary batteries. Solid-state batteries are a type of secondary battery that have improved performance. The performance of solid-state batteries is greatly affected by the solid electrolyte. For example, Patent Document 1 proposes an ion-conductive composite having porous polymer crystal particles whose primary particles have an average particle size within a specific range and a first ionic liquid held in the pores of the porous polymer. According to the invention of Patent Document 1, the ion conductivity is improved. Patent Document 2 proposes a porous coordination polymer-ion composite having an insulating structure composed of a plurality of porous coordination polymers, an ionic liquid held in the pores of the porous coordination polymer, and an ion-conductive substance in some of the voids between the particles of the structure. The invention of Patent Document 2 aims to enable an electrochemical device to operate safely over a wide temperature range. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6369940 [Patent Document 2] Patent No. 5924627 Summary of the Invention [Problem to be solved by the invention]

[0004] However, there is a demand for improved performance of secondary batteries. The present invention aims to provide an electrolyte composite for a secondary battery that can further improve the performance of the secondary battery. [Means for solving the problem]

[0005] The present invention has the following aspects. <1> A porous structure and an electrolyte, a part or all of the electrolyte is located in the pores of the porous structure; An electrolyte composite for a secondary battery, wherein an opening diameter R of the pores measured by the following measurement method A is equal to or greater than a maximum length L of a material constituting the electrolyte. ≪Measurement method A≫ Observe using an atomic resolution analytical electron microscope at an accelerating voltage of 200 KV. Draw one straight imaginary line from any point on the observed image. The imaginary line should pass through 10 randomly selected apertures. Measure the aperture diameters of the 10 apertures on the imaginary line, and take the average value as the aperture diameter R1. <2> The porous structure is a metal organic framework. <1> The electrolyte composite for a secondary battery according to claim 1, <3> The volume occupancy rate of the pores in the porous structure is 30 volume % or more. <1> or <2> The electrolyte composite for a secondary battery according to claim 1, <4> The diameter D of the pores measured by the following measurement method B is equal to or greater than the opening diameter R, <3> 2. The electrolyte composite for a secondary battery according to claim 1 , ≪Measurement method B≫ The pore diameter is measured using a specific surface area / pore size distribution measuring device, and the average value is calculated using the Barrett-Joyner-Halenda method to determine the pore diameter D. <5> The BET specific surface area of ​​the porous structure is 100 to 5000 m 2 / g, <1> ~ <4> 2. The electrolyte composite for a secondary battery according to claim 1 , <6> The thermal decomposition temperature in air is 250°C or higher. <1> ~ <5> 2. The electrolyte composite for a secondary battery according to claim 1 , <7> The electrolyte contains a metal salt containing a metal ion that transfers electrons, The content of the metal salt is 1 to 400 parts by mass relative to 100 parts by mass of the porous structure. <1> ~ <6> 2. The electrolyte composite for a secondary battery according to claim 1 , <8> The electrolyte contains a metal salt containing a metal ion that transfers electrons, and an anion. <1> ~ <7> 2. The electrolyte composite for a secondary battery according to claim 1 , Effect of the Invention

[0006] According to the electrolyte composite for a secondary battery of the present invention, the performance of the secondary battery can be further improved. [Brief description of the drawings]

[0007] [Figure 1] 2 is a graph showing the results of analyzing the crystal structure of the porous structure 2 by powder X-ray diffraction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In this specification and claims, the use of "to" indicating a range of numerical values ​​means that the numerical values ​​before and after it are included as the lower limit and upper limit.

[0009] (electrolyte complex) The electrolyte composite for a secondary battery of the present invention (hereinafter, may be simply referred to as "electrolyte composite") has a porous structure and an electrolyte. A part or the whole of the electrolyte is located in the pores of the porous structure. The electrolyte complex is applied to, for example, an electrode layer, an electrolyte layer, etc. of a secondary battery. The electrolyte may be a liquid or a solution. A solution is a liquid in which a solute is dissolved in a solvent. Note that the liquid or solution includes gels. The type of secondary battery is not particularly limited, and examples thereof include a lithium ion battery, an electric double layer capacitor, and a lithium ion capacitor.

[0010] <Porous structure> The porous structure has two or more pores. The pores of the porous structure may be of a cage type or a channel type. The opening diameter R of the pores in the porous structure is equal to or greater than the maximum length L of the material that constitutes the electrolyte. When the opening diameter R is equal to or greater than the maximum length L, the electrolyte can easily enter and exit the pores, and the electrolyte can diffuse more quickly. This facilitates the exchange of protons, further improving the performance of the secondary battery. The "maximum length" is the longest distance in the target material. The opening diameter R of the porous structure is measured by the following measurement method A.

[0011] ≪Measurement method A≫ Observe using an atomic resolution analytical electron microscope at an accelerating voltage of 200 KV. Draw one straight imaginary line from any point on the observed image. The imaginary line should pass through 10 randomly selected apertures. Measure the aperture diameters of the 10 apertures on the imaginary line, and take the average value as the aperture diameter R1.

[0012] An example of the atomic resolution analytical electron microscope is JEM-ARM200F (manufactured by JEOL Ltd.).

[0013] The opening diameter R is, for example, preferably 0.3 nm or more, more preferably 0.5 to 1.0 nm, and even more preferably 1.0 to 3.0 nm. When the opening diameter R is equal to or more than the lower limit, the electrolyte can more smoothly enter and exit the pores, and the performance of the secondary battery can be further improved. When the opening diameter R is equal to or less than the upper limit, the retention of the electrolyte in the pores can be further improved. The opening diameter R is adjusted by the combination of the material of the porous structure, the starting material of the porous structure, and the manufacturing method thereof, and the like.

[0014] The ratio of the pore volume to the volume of the porous structure (volume occupancy) is preferably 20% by volume or more, more preferably 30% by volume or more, and even more preferably 40% by volume or more. When the volume occupancy is equal to or more than the lower limit, the amount of electrolyte carried can be increased, and the performance of the secondary battery can be further improved. The upper limit of the volume occupancy is substantially 70% by volume or less. The volume occupancy is adjusted by the combination of the material of the porous structure, the starting material of the porous structure, and the method of producing the same.

[0015] The sum of the pore volumes in the porous structure (total pore volume) is 0.5 to 5.0 cm 3 / g is preferable, and 1.0 to 5.0 cm 3 / g is more preferable, and 1.1 to 5.0 cm 3 When the total pore volume is equal to or more than the lower limit, the diffusibility of the electrolyte is increased, and the performance of the secondary battery is further improved. When the total pore volume is equal to or less than the upper limit, the specific surface area can be increased. The total pore volume is adjusted by the combination of the material of the porous structure, the starting material of the porous structure, and the production method thereof.

[0016] The BET specific surface area of ​​the porous structure is 100 to 5000 m 2 / g is preferable, and 200 to 5000m 2 / g or more is preferable, and 300 to 5000m 2 When the BET specific surface area is equal to or more than the above lower limit, the performance of the secondary battery can be further improved. The BET specific surface area is a value measured, for example, with BELSORP II (manufactured by Microtrac).

[0017] The diameter D of the pores of the porous structure is equal to or greater than the opening diameter R. When the diameter D is equal to or greater than the opening diameter R, the amount of electrolyte supported can be increased, leading to further improvement in the performance of the secondary battery. The diameter D is measured by the following measurement method B. The diameter D is the so-called average pore diameter. The diameter D is adjusted by the combination of the material of the porous structure, the starting material of the porous structure, and the manufacturing method thereof, and the like. When the pores are of the cage type, the opening diameter R is equal to or less than the diameter D. When the pores are of the channel type, the opening diameter R is equal to the diameter D.

[0018] ≪Measurement method B≫ The pore diameter is measured using a specific surface area / pore size distribution measuring device, and the average value is calculated using the Barrett-Joyner-Halenda method to determine the pore diameter D.

[0019] An example of a specific surface area / pore size distribution measuring device is BELSORP-max-12-N-VP-CM (manufactured by Microtrack BEL Co., Ltd.).

[0020] An example of the measurement conditions using a specific surface area / pore size distribution measuring device is shown below. Pretreatment conditions: vacuum (0.1 Pa or less), 200°C, 5 hours. Measurement pressure range: 3×10 -8 ~0.995P / P0 (relative pressure).

[0021] The diameter D is preferably 0.35 to 5 nm, more preferably 0.5 to 1 nm, and even more preferably 1 to 5 nm. When the diameter D is equal to or greater than the lower limit, the amount of electrolyte supported in the pores is increased, and the performance of the secondary battery is further improved. When the diameter D is equal to or less than the upper limit, the outflow of the electrolyte to the outside of the pores can be further suppressed. The diameter D is adjusted by the combination of the material of the porous structure, the starting material of the porous structure, and the manufacturing method thereof.

[0022] The thermal decomposition temperature of the porous structure in air (atmosphere) is preferably 250° C. or higher, more preferably 280° C. or higher, and even more preferably 300° C. or higher. When the thermal decomposition temperature is equal to or higher than the lower limit, overheating of the battery can be suppressed and the performance of the secondary battery can be more stabilized and the life of the battery can be extended when the porous structure is used as a battery component. The upper limit of the thermal decomposition temperature is not particularly limited, but is substantially equal to or lower than 600° C. The pyrolysis temperature is adjusted by the combination of the material of the porous structure, the starting material of the porous structure, and the method of producing the same, and the like.

[0023] The thermal decomposition temperature can be measured, for example, by thermogravimetric analysis, which uses a thermogravimetric differential thermal analyzer STA7200 (manufactured by Hitachi High-Tech Science Corporation) with an air flow rate of 100 mL / min, a temperature rise rate of 10°C / min, and heating from room temperature to 1000°C, and determines the thermal decomposition temperature from the temperature at which the weight loss begins.

[0024] The material of the porous structure is not particularly limited. Examples of the material of the porous structure include metal-organic frameworks (hereinafter sometimes referred to as "MOFs"), metal oxides (silica, alumina, titania, magnesia, or composites thereof, etc.), ceramics, and covalent organic frameworks (COFs). Among them, MOFs are preferable as the material of the porous structure. With MOFs, pores of a desired opening diameter can be easily formed.

[0025] MOFs are structures in which metal ions and organic bridging ligands (multidentate ligands having two or more coordinating functional groups) are continuously bonded together, and are porous bodies with multiple internal pores. There is no particular limitation on the MOF as long as it conforms to the definition of MOF. Known MOFs include MOFs having multiple metal, metal oxide, metal cluster, or metal oxide cluster structural units, but are not limited thereto.

[0026] Metal atoms constituting MOFs include zinc, cobalt, niobium, zirconium, cadmium, copper, nickel, chromium, vanadium, titanium, molybdenum, magnesium, iron, aluminum, zirconium, etc. However, the metal atoms constituting MOFs are not limited to these. The metal atoms constituting MOFs may be one type alone or two or more types in combination. The metal raw material for MOF is Zr 4+ , Zn2+ , Cu 2+ , Ni 2+ , Co 2+ Complexes having metal ions such as those mentioned above and metal-containing secondary structural units (SBUs) are suitable.

[0027] The coordinating functional group of the organic bridging ligand may be any functional group capable of coordinating with a metal atom, and examples thereof include a carboxyl group, an imidazole group, a hydroxyl group, a sulfonic acid group, a pyridine group, a tertiary amine group, an amide group, and a thioamide group. Among these, a carboxyl group is preferred. The two or more coordinating functional groups possessed by the organic bridging ligand may be the same or different from each other. As the organic bridging ligand, typically, one in which two or more coordinating functional groups are substituted on a skeleton having a rigid structure (for example, an aromatic ring, an unsaturated bond, etc.) is used. Specific examples of the organic bridging ligand are given below, but the present invention is not limited thereto. 1,3,5-tris(4-carboxyphenyl)benzene (BTB), 1,4-benzenedicarboxylic acid (BDC), 2,5-dihydroxy-1,4-benzenedicarboxylic acid (DOBDC), cyclobutyl-1,4-benzenedicarboxylic acid (CB BDC), 2-amino-1,4-benzenedicarboxylic acid (H2N BDC), tetrahydropyrene-2,7-dicarboxylic acid (HPDC), terphenyl dicarboxylic acid (TPDC), 2,6-naphthalenedicarboxylic acid (2,6-NDC), pyrene-2,7-dicarboxylic acid (PDC), biphenyl dicarboxylic acid (BPDC), any dicarboxylic acid having a phenyl compound, 3,3',5,5'-biphenyltetracarboxylic acid, imidazole, 2-methylimidazole, benzimidazole, 2-nitroimidazole, cyclobenzimidazole, imidazole-2-carboxaldehyde, 4-cyanoimidazole, 6-methylbenzimidazole, 6-bromobenzimidazole, etc. The organic bridging ligand constituting the MOF may be one type alone or a combination of two or more types.

[0028] Specific examples of MOFs are given below, but the present invention is not limited thereto. Zinc4 O(1,3,5-benzenetribenzoate) 2 MOF-177, also known as IRMOF-I, is 4 O(1,4-benzenedicarboxylate) 3 MOF-5 represented by Mg 2 MOF-74 represented by (2,5-dihydroxy-1,4-benzenedicarboxylate)(Mg);Zn 2 MOF-74(Zn);Cu 2 MOF-505 represented by (3,3',5,5'-biphenyltetracarboxylate);Zn 4 IRMOF-6 represented by O(cyclobutyl-1,4-benzenedicarboxylate);Zn 4 O(2-amino-1,4-benzenedicarboxylate) 3 Represented by IRMOF-3;Zn 4 O(Terphenyl dicarboxylate) 3 or Zn 4 O(Tetrahydropyrene-2,7-dicarboxylate) 3 IRMOF-11;Zn 4 O(Tetrahydropyrene-2,7-dicarboxylate) 3 IRMOF-8 represented by Zn(2-methylimidazolate) 2 ZIF-8 represented by Zn(benzimidazolate)(2-nitroimidazolate); ZIF-68 represented by Zn(cyclobenzimidazolate)(2-nitroimidazolate); ZIF-69 represented by Zn(benzimidazolate) 2 ZIF-7 represented by Co(benzimidazolate) 2 Represented by ZIF-9;Zn 2 (benzimidazolate) represented by ZIF-11; Zn(imidazolate-2-carboxaldehyde) 2ZIF-90 represented by Zn(4-cyanoimidazolate)(2-nitroimidazolate); ZIF-82 represented by Zn(imidazolate)(2-nitroimidazolate); ZIF-70 represented by Zn(imidazolate)(2-nitroimidazolate); ZIF-79 represented by Zn(6-methylbenzimidazolate)(2-nitroimidazolate); ZIF-81 represented by Zn(6-bromobenzimidazolate)(2-nitroimidazolate); Zr 6 (OH) 8 (TBAPy) 2 , Zr 6 (OH) 4 O 4 (bdc) 6 (UiO-66) etc.

[0029] As MOFs, zinc-based MOFs (e.g., ZIF-8), zirconia-based MOFs (e.g., Zr 6 (OH) 8 (TBAPy) 2 ZIF is a material having a zeolite-like topology that contains zinc or cobalt as a metal and an imidazole-based organic bridging ligand (imidazole, benzimidazole, 2-nitroimidazole, 2-methylimidazole, cyclobenzimidazole, imidazole-2-carboxaldehyde, 4-cyanoimidazole, 6-methylbenzimidazole, 6-bromobenzimidazole, etc.) as an organic bridging ligand.

[0030] MOFs typically have a crystalline structure. Since MOFs have an ordered structure, they tend to crystallize and are easily obtained as single crystals or polycrystals. The crystals may be single crystals or polycrystals. The median size of the crystal structure is preferably 10 nm to 1000 μm, more preferably 30 nm to 100 μm. If the median size of the crystal structure is equal to or greater than the lower limit, the specific surface area is better, and if it is equal to or less than the upper limit, the diffusibility of the substance and the dispersibility of the crystals are better.

[0031] The median size of the crystal structures of MOFs is measured by the following method. An image of the surface of the sample is obtained using a scanning electron microscope or an optical microscope. The magnification is set so that the number of crystals (MOFs) present in the image is 100 to 200. The maximum diameters of all crystals present in the obtained image are measured, and the median value (average value of the minimum and maximum values) is calculated, and this value is regarded as the median value of the size of the crystal structure of the MOF.

[0032] The MOF may be commercially available or may be produced by a known production method. Examples of the production method of the MOF include the method described in International Publication No. 2019 / 039509. Depending on the type and composition of the starting materials (metals, organic ligands) for MOFs, as well as the manufacturing method and conditions, the size of the crystal structure of the resulting MOF and the amount of metal oxide contained will vary, resulting in differences in the pore distribution, pore size, opening size, etc. of the MOF. Taking the method described in International Publication No. 2019 / 039509 as an example, in this method, a material (A) (excluding MOFs) containing a metal atom constituting a MOF, an organic material (B) having two or more metal coordination parts capable of coordinating with the metal atom to generate a crystal, and a coordination promoter (C) that reacts or undergoes a phase transition upon stimulation and can promote the coordination of the metal coordination part of the organic material (B) to the metal atom of the material (A) are stimulated to generate a MOF. In the above method, the type and equivalent of the coordination promoter (C) affect the pore distribution of the generated MOF. For example, by changing the type of base as the coordination promoter (C) (e.g., amine-borane complex, dicyandiamide, hydrazide, imine, oxazolidine, pyridine, tertiary amine, ketoprofenamine salt, secondary amine, primary amine, or a mixture thereof, etc.), MOFs with different opening diameters R and pore diameters can be obtained.

[0033] <Electrolyte> The electrolyte complex contains an electrolyte, and thus can function as an electrolyte layer, an electrode, or the like of a secondary battery. The electrolyte is located partly or entirely in the pores of the porous structure, that is, a part of the electrolyte may be attached to the surface of the porous structure.

[0034] The electrolyte preferably contains a metal salt (sometimes called an "electrolyte metal salt") that contains a metal ion (sometimes called an "electrolyte metal ion") that transfers electrons. By containing the electrolyte metal salt, electrons can be transferred between the electrodes of the secondary battery, thereby enabling charging and discharging.

[0035] Examples of the electrolyte metal ion include an alkali metal ion and an alkaline earth metal ion. The alkali metal ion is preferably a lithium ion, a sodium ion, a potassium ion, etc. The alkaline earth metal ion is preferably a magnesium ion, a calcium ion, etc. Among these, as the electrolyte metal ion, an alkali metal ion is preferable, and a lithium ion is more preferable.

[0036] The electrolyte metal salts include lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and lithium tetrafluoroborate (LiBF 4 ), lithium hexafluorophosphate (LiPF 6 ), lithium perchlorate (LiCIO 4 ) etc.

[0037] The content of the electrolyte metal salt in the electrolyte is preferably 1 to 90 mass %, more preferably 5 to 85 mass %, and even more preferably 10 to 80 mass %, based on the total mass of the electrolyte. When the content of the electrolyte metal salt is equal to or more than the lower limit, the performance of the secondary battery can be further improved. When the content of the electrolyte metal salt is equal to or more than the lower limit, the performance of the secondary battery can be further improved.

[0038] The content of the electrolyte metal salt in the electrolyte composite is preferably 1 to 400 parts by mass, more preferably 2 to 50 parts by mass, and even more preferably 5 to 50 parts by mass, relative to 100 parts by mass of the porous structure. When the content of the electrolyte metal salt is equal to or more than the lower limit, the ion conductivity is further increased, and the performance of the secondary battery can be further improved. When the content of the electrolyte metal salt is equal to or less than the upper limit, the ion conductivity is increased, while the fluidity is reduced, and the suitability as a solid electrolyte is improved.

[0039] Examples of the electrolyte solvent include non-aqueous organic solvents and ionic liquids. Examples of the organic solvent include ethylene carbonate (EC), dimethyl carbonate (DMC), polyethylene carbonate (PC), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), etc. These organic solvents may be used alone or in combination of two or more. Examples of the ionic liquid include 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide (EMI-TFSI), 1-ethyl-3-methylimidazolium tetrafluoroborate ([C2mim][PF6]), 1-butyl-3-methylimidazolium hexafluorophosphate ([C4mim][BF4]), etc. These ionic liquids may be used alone or in combination of two or more.

[0040] The content of the solvent in the electrolyte is preferably 10 to 90 mass %, more preferably 20 to 90 mass %, and even more preferably 30 to 90 mass %, based on the total mass of the electrolyte. When the content of the solvent is equal to or more than the lower limit, the fluidity of the electrolyte is increased, and the electrolyte can be more smoothly moved in and out of the pores of the porous structure, thereby further improving the performance of the secondary battery.

[0041] The electrolyte may contain anions, such as anions generated from an electrolyte salt.

[0042] The electrolyte may contain, in addition to electrolyte metal ions and a solvent, additives and the like (optional electrolyte components) that can improve charge / discharge stability. The content of the optional electrolyte component in the electrolyte is preferably 0.001 to 30 mass %, more preferably 0.01 to 20 mass %, and further preferably 0.1 to 15 mass %, based on the total mass of the electrolyte.

[0043] The maximum length L of an electrolyte is a value determined by its molecular structure. The maximum length L is the largest value among the maximum molecular lengths of the constituent components of the electrolyte (electrolyte metal ions, solvent, optional electrolyte components, etc.). For example, when an electrolyte contains an electrolyte metal ion and a solvent, the maximum length L of the electrolyte is the longer of the maximum length of the electrolyte metal ion and the maximum length of the solvent.

[0044] The dimensions and maximum lengths of the components of the electrolyte are exemplified below. ·LiTFSI Dimensions: 0.8nm x 0.3nm. Maximum length: 0.8m. ·LiBF 4 Dimensions: 0.45nm x 0.45nm. Maximum length: 0.45 nm. ·DMC Dimensions: 0.4nm x 0.12nm. Maximum length: 0.4 nm. ·EMI-TFSI Dimensions: 1.66nm x 1.03nm. Maximum length: 1.66 nm.

[0045] The electrolyte can be prepared by a conventionally known method. For example, an electrolyte metal salt is added to a solvent and stirred while heating. The temperature during stirring is preferably, for example, 0 to 200° C. The pressure during stirring may be reduced.

[0046] As a method for producing the electrolyte composite, a method in which the porous structure and the electrolyte are mixed and, if necessary, dried under reduced pressure or the like can be mentioned.

[0047] (Electrolyte Composite Composition for Secondary Batteries) The electrolyte composite composition for a secondary battery of the present invention (hereinafter, may be simply referred to as "electrolyte composite composition") contains the above-mentioned electrolyte composite.

[0048] The electrolyte complex composition may contain only the electrolyte complex, or may contain components other than the electrolyte complex (optional components of the composition).

[0049] The optional components of the composition are appropriately determined depending on the application of the electrolyte complex composition. When the electrolyte complex composition is used for forming an electrolyte layer of a secondary battery, the optional components of the composition include a binder, a dispersion medium, a dispersant, etc. When the electrolyte complex composition is used for forming an electrode of a secondary battery, the optional components of the composition include a conductive assistant, a binder, an additive, etc. Examples of binders include polyacrylonitrile, cellulose-based polymers, and polyvinylidene fluoride. Examples of the dispersion medium include ethylene carbonate (EC), dimethyl carbonate (DMC), polyethylene carbonate (PC), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC). Examples of the conductive assistant include Ketjen black and carbon nanotubes. The additives include, for example, carboxymethyl cellulose. These optional components of the composition may be used alone or in combination of two or more.

[0050] When the electrolyte complex composition contains any optional composition components, the content of the porous structure in the electrolyte complex composition is preferably 5 to 90 mass%, more preferably 10 to 90 mass%, and even more preferably 30 to 90 mass%, relative to the total mass of the electrolyte complex composition.

[0051] The electrolyte complex composition can be prepared by a conventionally known method, for example, by adding the electrolyte complex and any optional components to a dispersion medium and stirring the mixture.

[0052] The electrolyte complex composition can be used, for example, by applying it to a substrate, drying it, and forming it into a film or plate, or by pressing the electrolyte complex composition in a container of any shape.

[0053] As described above, according to the electrolyte composite of the present embodiment, the opening diameter of the pores in the porous structure is a specific size, so that the electrolyte can smoothly enter and exit the pores. Therefore, the secondary battery using the electrolyte composite can have improved battery performance. EXAMPLES

[0054] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0055] Example 1 <Porous structure 1 (Zr 6 (μ3-OH) 8 (OH) 8 (TBAPy) 2 Preparation of The preparation of the porous structure 1 was carried out with reference to the literature (J. Am. Chem. Soc. 2013, 135, 10294-10297).

[0056] ≪Preparation of 1,3,6,8-tetrakis(p-benzoic acid)pyrene (H4TBAPy)≫ In an argon atmosphere glove box, 4-(methoxycarbonyl)phenyl)boronic acid (1.040 g), 1,3,6,8-tetrabromopyrene (0.500 g), tetrakis(triphenylphosphine)palladium(0) (0.030 g), and potassium tribasic phosphate (1.100 g) were added to 20 mL of dehydrated dioxane and stirred at 130°C for 72 hours. The reaction mixture was then dried under reduced pressure to obtain a solid. The obtained solid was washed with water to remove inorganic impurities. The solid was then extracted with chloroform, washed, and dried to obtain 1,3,6,8-tetrakis(4-(methoxycarbonyl)phenyl)pyrene (TMPPy) (yield 80%). In a 250 mL round-bottom flask, TMPPy (0.58 g) and 1.5 g NaOH were added to a solvent (tetrahydrofuran (THF):H 2100 mL of NaOH solution in which H4TBAPy was dissolved in 1:1 NaOH (volume basis) was added. The mixture in the flask was refluxed overnight and then the solvent was removed by vacuum drying. The recovered material was dissolved in water to obtain a transparent yellow solution. Next, hydrochloric acid was added to the transparent yellow solution to adjust the pH to 1.0, and a yellow precipitate was obtained. The yellow precipitate was collected by filtration, washed, and dried to obtain 0.49 g of H4TBAPy.

[0057] <Preparation of Porous Structure 1> 70mg ZrCl 4 and 2700 mg of benzoic acid were dissolved in dimethylformamide (DMF) to prepare 8 mL of DMF solution. 8 mL of the DMF solution was heated in an oven at 80°C for 1 hour, and then the DMF solution was cooled to room temperature. 40 mg of H4TBAPy was added to the cooled DMF solution, and ultrasonic treatment was performed for 20 minutes to obtain a yellow suspension. This yellow suspension was heated at 120°C for 48 hours, and the purified yellow crystals were collected by filtration. The collected crystals were washed and dried to obtain porous structure 1. The resulting porous structure 1 has a BET specific surface area of ​​2200 m 2 / g, total pore volume 1.3 cm 3 / g, the pore diameter D was 2.65 nm, and the pore opening diameter R was 2.65 nm. The porous structure 1 had channel-type pores.

[0058] <Preparation of electrolyte complex> After dissolving 1.87 g of LiTFSI in 7.65 g of EMI-TFSI, 6 g of propylene carbonate was further added to obtain electrolyte 1. 0.5 g of electrolyte 1 was added to 0.5 g of porous structure 1, and this was mixed at 2000 rpm for 110 minutes, and then subjected to heat treatment at 150° C. for 24 hours under vacuum conditions (0.1 Pa), to obtain the electrolyte complex of this example. The electrolyte complex of this example was in the form of a hard gel.

[0059] <Evaluation> 0.1 g of the electrolyte complex was placed in a stainless steel cylinder with a diameter of 1 cm, and pressed between stainless steel rods at 360 MPa for 1 minute to obtain a flat cylindrical pellet as a sample. The impedance of the obtained pellet was measured, and the ionic conductivity was calculated from the obtained resistance value using the following formula (1). The results are shown in Table 1.

[0060] σ = t / (R × S) (1) where σ is the ionic conductivity (S / cm), t is the thickness of the sample (cm), R is the resistance value (Ω) obtained from the impedance measurement, and S is the area of ​​the sample (cm 2 ).

[0061] Example 2 <Preparation of porous structure 2 (ZIF-8)> In a reaction vessel, 56.6 g of 2-methylimidazole was dissolved in a mixture of 19.8 g of ammonia water (concentration 29 mass%) and 37.6 g of water. Then, 60 g of an aqueous solution of zinc nitrate containing 11.88 g of zinc nitrate was added to the reaction vessel and reacted for 15 minutes. The resulting white precipitate was collected by filtration, washed, and vacuum dried at 100°C for 5 hours to obtain a porous structure 2. The crystal structure of the obtained porous structure 2 was measured by powder X-ray diffraction (SmartLab Multipurpose, Rigaku Corporation, CuKα-SF salt 1.54A, scan speed: 40° / min, step: 0.02°), and it was confirmed to be a ZiF-8 structure (Figure 1). Note that Figure 1 is a graph with 2θ (deg.) on the X-axis and X-ray intensity (relative value) on the Y-axis. The resulting porous structure 2 had a BET specific surface area of ​​1907.5 m 2 / g, total pore volume 0.6923 cm 3 / g, the pore diameter D was 1.45 nm, and the pore opening diameter R was 0.53 nm. The porous structure 2 had cage-type pores.

[0062] 0.9g LiBF 4The above was dissolved in 10.7 g of dimethyl carbonate (DMC) to obtain electrolyte 2. 0.6 g of electrolyte 2 was added to 0.3 g of porous structure 2 to obtain a mixture. The obtained mixture was depressurized (0.1 Pa) at room temperature for 5 hours, and then depressurized (0.05 Pa) at 150° C. to obtain the electrolyte complex of this example in the form of a powder. The ionic conductivity of the obtained electrolyte composite was determined in the same manner as in Example 1, and the results are shown in Table 1.

[0063] Comparative Example 1 An electrolyte composite of this example was obtained in the same manner as in Example 1, except that porous structure 2 was used instead of porous structure 1. The ionic conductivity of the obtained electrolyte composite was measured in the same manner as in Example 1, and the result is shown in Table 1.

[0064] [Table 1]

[0065] As shown in Table 1, in Examples 1 and 2 to which the present invention was applied, the ionic conductivity was 3.0 × 10 -4 ~5.4×10 -3 S / cm. In Comparative Example 1, in which the opening diameter R is smaller than the maximum length L of the electrolyte, the ion conductivity is 1.0 × 10 -7 S / cm. From these results, it was confirmed that the application of the present invention can improve the performance of secondary batteries.

Claims

1. A porous structure and an electrolyte, a part or all of the electrolyte is located in the pores of the porous structure; An electrolyte composite for a secondary battery, wherein an opening diameter R of the pores measured by the following measurement method A is equal to or greater than a maximum length L of a material constituting the electrolyte. ≪Measurement method A≫ Observation is performed using an atomic resolution analytical electron microscope at an accelerating voltage of 200 KV. A straight imaginary line is drawn from any point on the observed image, and the imaginary line is made to pass through 10 randomly selected apertures. The opening diameters of the 10 openings on the imaginary line are measured, and the average value is defined as the opening diameter R1.

2. The electrolyte composite for a secondary battery according to claim 1 , wherein the porous structure is a metal-organic framework.

3. 3. The electrolyte composite for a secondary battery according to claim 1, wherein a volume occupancy rate of the pores with respect to the porous structure is 20 volume % or more.

4. 3 . The electrolyte composite for a secondary battery according to claim 1 , wherein a diameter D of the pores measured by the following measurement method B is equal to or larger than the opening diameter R. ≪Measurement method B≫ The diameter of the pores is measured using a specific surface area / pore size distribution measuring device, and the average value is calculated by the Barrett-Joyner-Halenda method to obtain the diameter D of the pores.

5. The BET specific surface area of ​​the porous structure is 100 to 5000 m 2 The electrolyte composite for a secondary battery according to claim 1 or 2, wherein the molecular weight of the electrolyte composite is 1 / g.

6. 3. The electrolyte composite for a secondary battery according to claim 1, which has a thermal decomposition temperature in air of 250° C. or higher.

7. The electrolyte contains a metal salt containing a metal ion that transfers electrons, 3. The electrolyte composite for a secondary battery according to claim 1, wherein the content of the metal salt is 1 to 400 parts by mass with respect to 100 parts by mass of the porous structure.

8. 3. The electrolyte composite for a secondary battery according to claim 1, wherein the electrolyte comprises a metal salt containing a metal ion that transfers electrons, and an anion.

Citation Information

Patent Citations

  • Formation of multi-color decorative sheet

    JP1984024627A

  • Alloy containing nonequilibrium fe3b phase

    JP1988069940A