Polyimide precursor, polyimide and polyimide film
The polyimide precursor with a macromonomer residue improves moisture resistance and dielectric performance, addressing the limitations of conventional polyimides for high-frequency circuit applications.
Patent Information
- Application Number
- JP2023044662
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional polyimides exhibit high moisture absorption and inadequate dielectric properties at frequencies above 10 GHz, limiting their suitability for high-frequency circuit applications.
A polyimide precursor incorporating a specific repeating unit with a macromonomer residue, derived from a vinyl polymer, to reduce moisture absorption and enhance dielectric properties, composed of tetracarboxylic acid and diamine residues, with a preferred composition of 70 mol% or more of this unit.
The resulting polyimide film demonstrates low moisture absorption and excellent dielectric properties above 10 GHz, maintaining physical properties like glass transition temperature and coefficient of linear expansion, suitable for high-frequency circuit boards.
Smart Images

Figure 2024134391000001 
Figure 2024134391000002 
Figure 2024134391000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyimide precursor, a polyimide, and a polyimide film. [Background technology]
[0002] In recent years, the high-speed signal transmission of electronic devices has led to higher frequencies of electrical signals propagating through circuits. As electrical signals become more frequent, there is an increasing demand for lower dielectric constants and dielectric loss tangents in electronic circuit board materials. This is because lowering the dielectric constant and dielectric loss tangent is an effective way to suppress the transmission loss of high-frequency electrical signals. With the advancement of IoT in recent years, there has been a trend toward higher frequencies, and there is a demand for circuit board materials that can suppress transmission loss, for example, even in the range of 10 GHz or higher.
[0003] For example, Patent Document 1 discloses a polyimide containing a diamine residue derived from a specific diamine component and an acid dianhydride residue derived from a specific tetracarboxylic acid component. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2022-154637 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the conventional polyimides as described above have room for improvement in terms of achieving both a low moisture absorption rate and excellent dielectric properties in the range of 10 GHz or higher.
[0006] An object of one aspect of the present invention is to provide a polyimide precursor from which a polyimide film that has a low moisture absorption rate and excellent dielectric properties in the range of 10 GHz or higher and can be used for high-frequency circuit boards is obtained. [Means for solving the problem]
[0007] In order to solve the above problems, a polyimide precursor according to one embodiment of the present invention contains a repeating unit represented by the following general formula (1):
[0008] [ka]
[0009] In formula (1), X 1 and X 2 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; A is a tetravalent tetracarboxylic acid residue; B is a divalent diamine residue; The diamine residue includes a macromonomer residue represented by the following general formula (2):
[0010] [ka]
[0011] In formula (2), R is a vinyl polymer; R 1 is -O-, -O(CO)-, -NH-, -N(CH3)-, or -N(CH2CH3)-; R 2 represents a trivalent or tetravalent group having 1 to 18 carbon atoms, which may have a heteroatom; R 3 each independently represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; n is 1 or 2; When n is 2, there are two R and two R 1 The structures of may be the same or different. Effect of the Invention
[0012] According to one aspect of the present invention, it is possible to provide a polyimide precursor which can be used to obtain a polyimide film which has a low moisture absorption rate and excellent dielectric properties in the range of 10 GHz or more and can be used for high-frequency circuit boards. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] An embodiment of the present invention will be described below, but the present invention is not limited thereto. In this specification, unless otherwise specified, "A to B" representing a numerical range means "A or more and B or less." In addition, in this specification, "(meth)acrylic" means acrylic and / or methacrylic.
[0014] [1. Polyimide precursor] A polyimide precursor according to one embodiment of the present invention includes a repeating unit represented by the following general formula (1):
[0015] [ka]
[0016] In formula (1), X 1 and X 2 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; A is a tetravalent tetracarboxylic acid residue; B is a divalent diamine residue; The diamine residue includes a macromonomer residue represented by the following general formula (2):
[0017] [ka]
[0018] In formula (2), R is a vinyl polymer; R 1 is -O-, -O(CO)-, -NH-, -N(CH3)-, or -N(CH2CH3)-; R2 represents a trivalent or tetravalent group having 1 to 18 carbon atoms, which may have a heteroatom; R 3 each independently represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; n is 1 or 2; When n is 2, there are two R and two R 1 The structures of may be the same or different. 2 RR that binds to 1 -Represents the number of.
[0019] Since the polyimide precursor contains the macromonomer residue, it can be said that a vinyl polymer is introduced as a side chain. By using this polyimide precursor, a polyimide film that has excellent dielectric properties in the region of 10 GHz or more and can be used for high-frequency circuit boards can be obtained. In addition, electronic devices are required to be able to handle various environments. In particular, since the dielectric loss tangent is easily affected by water, a low moisture absorption rate of the material is also important for improving the performance of electronic devices. By using the polyimide precursor, a polyimide film that has excellent dielectric properties and a low moisture absorption rate can be obtained. In addition, the obtained polyimide film does not lose physical properties such as the glass transition temperature and linear expansion coefficient, which are greatly affected by the polyimide main chain, and also has basic properties required for flexible printed circuit boards (FPCs), such as heat resistance.
[0020] The polyimide precursor preferably contains 70 mol % or more of the repeating unit represented by general formula (1) among all repeating units, more preferably 80 mol % or more, even more preferably 90 mol % or more, and particularly preferably 100 mol %. That is, the polyimide precursor may be composed of the repeating unit represented by general formula (1). The terminal of the polyimide precursor may be an amino group.
[0021] <Tetracarboxylic acid residue> The repeating unit includes a tetravalent tetracarboxylic acid residue. The tetracarboxylic acid residue may be a structural unit derived from a tetracarboxylic acid dianhydride. The tetracarboxylic acid dianhydride may be an aliphatic tetracarboxylic acid dianhydride or an aromatic tetracarboxylic acid dianhydride, but is preferably an aromatic tetracarboxylic acid dianhydride from the viewpoint of thermal stability.
[0022] Examples of tetracarboxylic dianhydrides include pyromellitic dianhydride (PMDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA), 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, and 3,4,9,10-perylenetetracarboxylic acid. dianhydride, 1,1-(3,4-dicarboxyphenyl)ethane dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, p-phenylene bis(trimellitic acid monoester dianhydride), ethylene bis(trimellitic acid monoester dianhydride), bisphenol A bis(trimellitic acid monoester dianhydride), etc. Among these, one type may be used alone, or two or more types may be used in combination.
[0023] The tetracarboxylic acid residue may be a structural unit derived from an alkyl monoester or alkyl diester of the tetracarboxylic dianhydride. In this case, X 1 and X 2 At least one of them can be an alkyl group having 1 to 5 carbon atoms.
[0024] <Diamine residue> The repeating unit includes a divalent diamine residue. The diamine residue is a structural unit derived from a diamine. The diamine may include a macromonomer described below as well as a diamine other than the macromonomer. Examples of the diamine other than the macromonomer include aromatic diamines, aliphatic diamines, and polyether diamines. One of these may be used alone, or two or more may be used in combination.
[0025] Aromatic diamines include 4,4'-diaminodiphenyl ether (ODA), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), paraphenylenediamine (PDA), 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diaminodiphenylmethane, benzidine, 4,4'-diamino-2,2'-dimethylbiphenyl (m-TB), 4,4'-diamino-3,3'-dimethylbiphenyl, 4,4'-diamino-2,2'-dimethoxybiphenyl, and 4,4'-diamino-3,3'-dimethoxybiphenyl. nyl, 3,3'-dichlorobenzidine, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 1,5-diaminonaphthalene, 4,4'-diaminodiphenyl diethyl silane, 4,4'-diaminodiphenyl silane, 4,4'-diaminodiphenyl ethyl phosphine oxide, 4,4'-diaminodiphenyl N-methylamine, 4,4'-diaminodiphenyl N-phenylamine, 1,3-diaminobenzene (metaphenylenediamine, MDA), 1,2-diaminobenzene, and the like.
[0026] Examples of the aliphatic diamine include 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, 1,13-diaminotridecane, 1,14-diaminotetradecane, 1,15-diaminopentadecane, 1,16-diaminohexadecane, 1,17-diaminoheptadecane, 1,18-diaminooctadecane, 1,19-diaminononadecane, 1,20-diaminoeicosane, cyclohexanediamine, and bis-(4-aminocyclohexyl)methane.
[0027] Examples of polyether diamines include amino-modified polyoxyalkylenes (for example, polyoxyethylene, 1,2-polyoxypropylene, 1,3-polyoxypropylene, or copolymers thereof).
[0028] <Macromonomer residue> The repeating units include a macromonomer residue represented by general formula (2). The macromonomer residue is a structural unit derived from a macromonomer represented by the following general formula (3):
[0029] [ka]
[0030] In formula (3), R, R 1 , R 2 , R 3 The definition of n is the same as in formula (2). As the macromonomer represented by formula (3), one type may be used alone, or two or more types may be used in combination.
[0031] The ratio of the macromonomer residue represented by the general formula (2) in 100 mol % of the diamine residue contained in the polyimide precursor is preferably 0.1 mol % or more, more preferably 0.5 mol % or more, even more preferably 1 mol % or more, and particularly preferably 1.5 mol % or more. The ratio of the macromonomer residue is preferably 10 mol % or less, more preferably 8 mol % or less, and even more preferably 6 mol % or less. If the ratio of the macromonomer residue is 0.1 mol % or more, the dielectric constant and the dielectric loss tangent can be further reduced, and the moisture absorption rate can also be further reduced. If the ratio of the macromonomer residue is 10 mol % or less, it is preferable from the viewpoint of heat resistance. It can also be said that the polyimide precursor preferably contains 0.1 to 10 mol % of the macromonomer residue represented by the general formula (2) in 100 mol % of the diamine residue contained in the polyimide precursor.
[0032] R 1 is -O-, -O(CO)-, -NH-, -N(CH3)- or -N(CH2CH3)-. 1 is preferably -O(CO)- or -NH-.
[0033] R 2 R is a trivalent or tetravalent group having 1 to 18 carbon atoms, which may have a heteroatom. 2 The number of carbon atoms in R is preferably 1 to 13, more preferably 1 to 12, and further preferably 1 to 6. 2 Examples of the heteroatom that may be contained include an oxygen atom, a nitrogen atom, a sulfur atom, a phosphorus atom, and a halogen atom (a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom).
[0034] R 2 may be a linear structure, a branched structure, or a cyclic structure. 2 When is a cyclic structure, R 2 may have a heterocyclic structure. More specifically, R 2is preferably a trivalent or tetravalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl or heteroaryl.
[0035] R 2 If R is aryl or heteroaryl, this is preferred because it does not cause salt formation, which occurs when an aliphatic diamine is used. In the method of obtaining a high molecular weight polyimide precursor using an aliphatic diamine, salt formation may occur, but 2 If an aryl or heteroaryl macromonomer is used, salt formation does not occur, and a high molecular weight polyimide precursor can be obtained by the same method as in the past.
[0036] In this specification, trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl refers to a group in which two hydrogen atoms have been removed from a normally monovalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl. In other words, trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl has three bonding sites with other molecules.
[0037] In addition, in this specification, tetravalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl refers to a group in which three hydrogen atoms have been removed from a normally monovalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl. In other words, a tetravalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl has four bonding sites with other molecules.
[0038] R 3 R is a single bond or a divalent group having 1 to 8 carbon atoms, and may have a heteroatom. 3 The number of carbon atoms in R is 0 to 8, preferably 0 to 6, more preferably 0 to 4, and further preferably 0 to 2. 3The number of carbon atoms in R is 0. 3 R is a single bond or consists of only heteroatoms. 3 Examples of the heteroatom that may be contained include an oxygen atom, a nitrogen atom, a sulfur atom, a phosphorus atom, and a halogen atom (a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom).
[0039] R 3 may be a linear structure, a branched structure, or a cyclic structure. 3 When is a cyclic structure, R 3 may have a heterocyclic structure. More specifically, R 3 is preferably a divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl.
[0040] In this specification, divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl refers to a group in which one hydrogen atom is removed from a normally monovalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl. That is, divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl has two bonding sites with other molecules. Note that divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl is also referred to as alkylene, heteroalkylene, cycloalkylene, heterocycloalkylene, arylene, or heteroarylene.
[0041] Specific examples of the macromonomer represented by the above general formula (3) include structures represented by the following formulas (i) to (v).
[0042] [ka]
[0043] R is a vinyl polymer, that is, the macromonomer has a main chain structure composed of constituent units derived from a vinyl monomer.
[0044] The vinyl monomer from which the structural unit constituting the main chain of the macromonomer is derived is not particularly limited as long as it has a vinyl group.Examples of the vinyl monomer include (meth)acrylic acid monomers, styrene monomers, maleimide monomers, chlorine-containing vinyl monomers, fluorine-containing vinyl monomers, silicon-containing vinyl monomers, nitrile group-containing vinyl monomers, amide group-containing vinyl monomers, vinyl esters, alkenes, and conjugated dienes.
[0045] Examples of the (meth)acrylic acid monomer include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, benzyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and the like. propyl, stearyl (meth)acrylate, glycidyl (meth)acrylate, 2-aminoethyl (meth)acrylate, γ-((meth)acryloyloxypropyl)trimethoxysilane, ethylene oxide adduct of (meth)acrylic acid, trifluoromethylmethyl (meth)acrylate, 2-trifluoromethylethyl (meth)acrylate, 2-perfluoroethylethyl (meth)acrylate, 2-perfluoroethyl-2-perfluorobutylethyl (meth)acrylate, 2-perfluoroethyl (meth)acrylate, perfluoromethyl (meth)acrylate, diperfluoromethylmethyl (meth)acrylate, 2-perfluoromethyl-2-perfluoroethylmethyl (meth)acrylate, 2-perfluorohexylethyl (meth)acrylate, 2-perfluorodecylethyl (meth)acrylate, and 2-perfluorohexadecylethyl (meth)acrylate.
[0046] Examples of the styrene monomer include styrene, vinyltoluene, α-methylstyrene, chlorostyrene, styrenesulfonic acid, and salts of styrenesulfonic acid, etc. Examples of the maleimide monomer include maleimide, methylmaleimide, ethylmaleimide, propylmaleimide, butylmaleimide, hexylmaleimide, octylmaleimide, dodecylmaleimide, stearylmaleimide, phenylmaleimide, cyclohexylmaleimide, etc.
[0047] The chlorine-containing vinyl monomer is not particularly limited, but suitable examples include vinyl chloride, vinylidene chloride, and allyl chloride. The fluorine-containing vinyl monomer is, for example, perfluoroethylene, perfluoropropylene, and vinylidene fluoride. The silicon-containing vinyl monomer is, for example, vinyltrimethoxysilane and vinyltriethoxysilane. The nitrile group-containing vinyl monomer is, for example, acrylonitrile and methacrylonitrile. The amide group-containing vinyl monomer is, for example, acrylamide and methacrylamide.
[0048] Examples of vinyl esters include vinyl acetate, vinyl propionate, vinyl pivalate, vinyl benzoate, vinyl cinnamate, etc. Examples of alkenes include ethylene, propylene, butylene, isobutylene, etc. Examples of conjugated dienes include butadiene, isoprene, etc.
[0049] Suitable examples of the vinyl monomer from which the structural units constituting the main chain of the macromonomer are derived include maleic anhydride, maleic acid, monoalkyl esters of maleic acid, dialkyl esters of maleic acid, fumaric acid, monoalkyl esters of fumaric acid, dialkyl esters of fumaric acid, and allyl alcohol.
[0050] The main chain of the macromonomer may be a homopolymer containing only structural units derived from one of the vinyl monomers described above, or may be a copolymer containing structural units derived from any two or more vinyl monomers.
[0051] In particular, since modification of the polymer terminal is relatively easy, the main chain of the macromonomer is preferably composed mainly of one or more of a constituent unit derived from a (meth)acrylic acid monomer, a constituent unit derived from a styrene monomer, or a constituent unit derived from isobutylene. That is, the main chain of the macromonomer is preferably composed mainly of poly(meth)acrylate, polystyrene, or polyisobutylene, and more preferably composed mainly of poly(meth)acrylate or polyisobutylene. In other words, the vinyl polymer is more preferably a poly(meth)acrylic polymer or a polyisobutylene polymer. The main chain of the macromonomer may be a copolymer composed mainly of a constituent unit derived from two or more types selected from the group consisting of a (meth)acrylic acid monomer, a styrene monomer, and isobutylene.
[0052] In this specification, the main chain of the macromonomer mainly comprises poly(meth)acrylate means that the main chain contains 50 mol% or more of structural units derived from (meth)acrylic acid out of 100 mol% of all structural units contained in the main chain. When the main chain of the macromonomer mainly comprises poly(meth)acrylate, the main chain of the macromonomer preferably contains 60 mol% or more of structural units derived from (meth)acrylic acid out of 100 mol% of all structural units contained in the main chain, more preferably contains 70 mol% or more, even more preferably contains 80 mol% or more, even more preferably contains 90 mol% or more, and may even be 100 mol%.
[0053] In this specification, the main chain of the macromonomer being mainly composed of polystyrene means that the main chain contains 50 mol% or more of structural units derived from styrene-based monomers out of 100 mol% of all structural units contained in the main chain. When the main chain of the present terminal-modified vinyl polymer is mainly composed of polystyrene, the main chain of the present terminal-modified vinyl polymer preferably contains 60 mol% or more of structural units derived from styrene-based monomers out of 100 mol% of all structural units contained in the main chain, more preferably 70 mol% or more, even more preferably 80 mol% or more, even more preferably 90 mol% or more, or may even be 100 mol%.
[0054] In this specification, the main chain of the macromonomer being mainly composed of polyisobutylene means that, out of 100 mol% of all structural units contained in the main chain, structural units derived from isobutylene account for 50 mol% or more. When the main chain of the macromonomer is mainly composed of polyisobutylene, the main chain of the macromonomer preferably contains structural units derived from isobutylene at 60 mol% or more, more preferably at 70 mol% or more, even more preferably at 80 mol% or more, even more preferably at 90 mol% or more, and may even be 100 mol%.
[0055] In this specification, the main chain of the macromonomer mainly comprises structural units derived from two or more selected from the group consisting of (meth)acrylic acid monomers, styrene monomers, and isobutylene, meaning that the main chain contains structural units derived from (meth)acrylic acid monomers, styrene monomers, or isobutylene in a total amount of 50 mol% or more out of 100 mol% of all structural units contained in the main chain. When the main chain of the macromonomer mainly comprises structural units derived from two or more selected from the group consisting of (meth)acrylic acid monomers, styrene monomers, and isobutylene, the main chain of the macromonomer preferably contains structural units derived from (meth)acrylic acid monomers, styrene monomers, or isobutylene in a total amount of 60 mol% or more out of 100 mol% of all structural units contained in the main chain, more preferably contains 70 mol% or more, even more preferably contains 80 mol% or more, even more preferably contains 90 mol% or more, and may be 100 mol%.
[0056] The main chain of the macromonomer may contain, in addition to the constituent units derived from the vinyl monomer, constituent units derived from monomers other than the vinyl monomer (other monomers). The content of the constituent units derived from other monomers in the main chain of the macromonomer is preferably less than 50 mol%, more preferably 40 mol% or less, more preferably 30 mol% or less, even more preferably 20 mol% or less, even more preferably 10 mol% or less, and may be 0 mol%, based on 100 mol% of all constituent units contained in the main chain.
[0057] The structure of the main chain of the macromonomer is not particularly limited, and may be a linear structure or a branched structure, i.e., the main chain of the macromonomer may be a linear polymer or a branched polymer.
[0058] The polymerization method for the vinyl polymer that is the main chain of the macromonomer is not particularly limited, and examples thereof include the polymerization methods described in JP-A-2005-232419, JP-A-2006-291073, and JP-A-2016-88944.
[0059] The vinyl polymer, which is the main chain of the macromonomer, may have a structure derived from a substance other than the vinyl monomer (e.g., a polymerization catalyst, etc.) within the vinyl polymer (particularly at the terminal). For example, when a vinyl polymer is polymerized by a polymerization method using mercaptans, which will be described later, the obtained vinyl polymer may have a structure containing an S group derived from the mercaptans at its terminal. When such a vinyl polymer having an S group at its terminal is used as the main chain, the macromonomer may have the above-mentioned R 1 and the main chain structure made of a vinyl monomer may further have a structure containing an S group derived from the above mercaptans.
[0060] As the macromonomer, as described above, the R 1 and the main chain structure consisting of the vinyl monomer, a structure derived from a substance other than the vinyl monomer, such as a polymerization catalyst (for example, a structure containing an S group) may be further included. Such an embodiment is also included in one embodiment of the present invention.
[0061] (Weight average molecular weight) The macromonomer preferably has a weight average molecular weight of 550 or more, more preferably 1,200 or more, and even more preferably 2,400 or more, as measured by size exclusion chromatography (SEC). The weight average molecular weight is preferably 1,100,000 or less, more preferably 200,000 or less, and even more preferably 50,000 or less. According to this configuration, the number of terminal structures introduced into the vinyl polymer can be easily controlled, and a macromonomer having a desired number of terminal structures can be provided.
[0062] (number average molecular weight) The macromonomer preferably has a number average molecular weight of 500 or more, more preferably 1,000 or more, and even more preferably 2,000 or more, as measured by size exclusion chromatography. The number average molecular weight is preferably 600,000 or less, more preferably 100,000 or less, and even more preferably 30,000 or less. According to this configuration, the number of terminal structures introduced into the vinyl polymer can be easily controlled, and a macromonomer having a desired number of terminal structures can be provided.
[0063] (Molecular weight distribution (Mw / Mn)) The macromonomer has a molecular weight distribution, i.e., a ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) measured by size exclusion chromatography, of preferably 1.8 or less, more preferably 1.7 or less, more preferably 1.6 or less, even more preferably 1.5 or less, even more preferably 1.4 or less, and particularly preferably 1.3 or less. According to this configuration, the number of terminal structures introduced into the vinyl polymer can be easily controlled, and a macromonomer having a desired number of terminal structures can be provided. The lower limit of the molecular weight distribution is theoretically 1.
[0064] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the vinyl polymer in this specification are values measured by SEC and calculated in terms of polystyrene. The specific method for measuring the weight average molecular weight (Mw) and number average molecular weight (Mn) of the vinyl polymer is as described in the Examples.
[0065] The macromonomer represented by the above general formula (3) preferably has a polystyrene-equivalent number average molecular weight of 500 to 600,000 and a molecular weight distribution of 1.8 or less, when measured by size exclusion chromatography.
[0066] (Method of producing macromonomer) The method for producing the macromonomer is not particularly limited as long as it can provide the macromonomer. Preferred examples of the method for producing the macromonomer include the following method (1) and method (2): Method (1): A method comprising the step of reacting a halogen group located at the end of a vinyl polymer with a compound represented by the following general formula (4a):
[0067] [ka]
[0068] In formula (4a), X is -OH, -COOH, -NH2, -N(CH3)H or -N(CH2CH3)H, or a salt thereof; R 2 , R 3 The definition of n is the same as in general formula (2).
[0069] Method (2): A method comprising the steps of reacting a halogen group located at the end of a vinyl polymer with a compound represented by the following general formula (4b) and reducing the resulting reaction product.
[0070] [ka]
[0071] In formula (4b), X is -OH, -COOH, -NH2, -N(CH3)H or -N(CH2CH3)H, or a salt thereof; R 2 , R 3 The definition of n is the same as in general formula (2).
[0072] In the above formulas (4a) and (4b), examples of the salt for X include salts of alkali metals such as potassium and sodium, and salts of alkaline earth metals such as calcium and magnesium.
[0073] Specific methods for producing the macromonomer will be described in detail below using methods (1) and (2) as examples, but the method for producing the macromonomer is not limited to these methods.
[0074] (Method (1)) The method for producing a macromonomer by method (1) (sometimes referred to as the "first method for producing a macromonomer") includes a step of reacting a halogen group located at the end of a vinyl polymer with a compound represented by the above general formula (4a).
[0075] (First reaction step) The method for producing the first macromonomer includes a step of reacting a halogen group located at the end of a vinyl polymer with a compound represented by the above general formula (4a) (sometimes referred to as the "first reaction step"). In this step, the end of the vinyl polymer is modified by reacting the compound represented by the above general formula (4a) with the vinyl polymer, thereby obtaining a macromonomer having a terminal structure derived from the compound represented by the above general formula (4a).
[0076] In the first reaction step, the method for reacting the halogen group located at the terminal of the vinyl polymer with the compound represented by the general formula (4a) is not particularly limited, but may include a method in which the vinyl polymer having a halogen group at its terminal and the compound represented by the general formula (4a) are dissolved in a solvent, and the vinyl polymer and the compound represented by the general formula (4a) in the solvent are heated (and stirred as necessary).
[0077] In the first reaction step, the solvent in which the reaction is carried out is not particularly limited, but since the reaction is a nucleophilic substitution reaction, a polar solvent is preferred. Examples of polar solvents that can be used in the first reaction step include N,N-dimethylacetamide, tetrahydrofuran, dioxane, diethyl ether, acetone, dimethyl sulfoxide, dimethylformamide, hexamethylphosphoric triamide, acetonitrile, etc.
[0078] In the first reaction step, the temperature (heating temperature) at which the vinyl polymer and the compound represented by the general formula (4a) in the solvent are heated is not limited, and is, for example, 30°C to 120°C, preferably 50°C to 100°C, and more preferably 70°C to 90°C.
[0079] The heating time in the first reaction step is not particularly limited, but it is preferable to continue heating until all halogen groups in the vinyl polymer subjected to the reaction are reacted (substituted) with the compound represented by the above general formula (4a). The specific heating time may be, for example, 30 minutes to 6 hours.
[0080] Specific examples of the compound represented by the above general formula (4a) include structures represented by the following formulae (vi) to (x).
[0081] [ka]
[0082] (Method (2)) The method for producing a macromonomer by method (2) (sometimes referred to as the "second method for producing a macromonomer") comprises the steps of reacting a halogen group located at the end of a vinyl polymer with a compound represented by the above general formula (4b) and reducing the resulting reaction product.
[0083] (Second reaction step) The second method for producing a macromonomer includes a step of reacting a halogen group located at the terminal of a vinyl polymer with a compound represented by the above general formula (4b) (sometimes referred to as a "second reaction step"). In this step, the terminal of the vinyl polymer is modified by reacting the terminal of the vinyl polymer with the compound represented by the above general formula (4b), thereby obtaining a terminal-modified vinyl polymer having a terminal structure derived from the compound represented by the above general formula (4b).
[0084] In the second reaction step, the method of reacting the halogen group located at the terminal of the vinyl polymer with the compound represented by the general formula (4b) is not particularly limited, but may include a method of dissolving the vinyl polymer having a halogen group at its terminal and the compound represented by the general formula (4b) in a solvent, and heating (and stirring as necessary) the vinyl polymer and the compound represented by the general formula (4b) in the solvent.
[0085] In the second reaction step, the solvent in which the reaction is carried out is not particularly limited, but since the reaction is a nucleophilic substitution reaction, a polar solvent is preferred. Examples of polar solvents that can be used in the second reaction step include N,N-dimethylacetamide, tetrahydrofuran, dioxane, diethyl ether, acetone, dimethyl sulfoxide, dimethylformamide, hexamethylphosphoric triamide, acetonitrile, etc.
[0086] In the second reaction step, the temperature (heating temperature) at which the vinyl polymer and the compound represented by the general formula (4b) in the solvent are heated is not limited, and is, for example, 30°C to 120°C, preferably 50°C to 100°C, and more preferably 70°C to 90°C.
[0087] The heating time in the second reaction step is not particularly limited, but it is preferable to continue heating until all halogen groups in the vinyl polymer subjected to the reaction are reacted (substituted) with the compound represented by the above general formula (4b). The specific heating time may be, for example, 30 minutes to 6 hours.
[0088] (Reduction process) The second method for producing a macromonomer includes a step of reducing a terminal-modified vinyl polymer having one or more terminal structures derived from the compound represented by the above general formula (4b), i.e., the reaction product obtained in the above second reaction step, in which the reaction product obtained in the above second reaction step is reduced, i.e., the nitro groups at the terminals of the reaction product are reduced and converted to amino groups, thereby obtaining a macromonomer represented by the above general formula (3).
[0089] In the reduction step, the method for reducing the reactant obtained in the second reaction step is not particularly limited, but may include a method in which the reactant obtained in the second reaction step is reacted with a reducing agent.
[0090] Examples of reducing agents that can be used in the reduction step include ammonium chloride, hydrogen, hydrazine, lithium aluminum hydride, and sodium borohydride.
[0091] Specific examples of the compound represented by the above general formula (4b) include structures represented by the following formulae (xi) to (xv).
[0092] [ka]
[0093] (Method (3)) In one embodiment of the present invention, as an aspect of the present production method other than the above-mentioned method (1) or method (2), there is provided a method for producing a terminal-modified vinyl polymer, comprising a step of reacting a functional group other than a halogen group, such as a hydroxyl group or a carboxyl group, located at the terminal of a vinyl polymer with a compound represented by the following general formula (4c) (method (3)):
[0094] [ka]
[0095] In formula (4c), X' is -OH, -NH2, -N(CH3)H, -N(CH2CH3)H, -COOH, -COZ or -Z (Z is a halogen atom); R 2 , R 3 The definition of n is the same as in general formula (2). In this specification, the process for producing a terminally modified vinyl polymer by the process (3) is sometimes referred to as the "third process".
[0096] (Third reaction step) The third production method includes a step of reacting a functional group other than a halogen group, such as a hydroxyl group or a carboxyl group, located at the terminal of a vinyl polymer with a compound of the following general formula (4c) (sometimes referred to as a third reaction step). In this step, the terminal of the vinyl polymer is modified by reacting the compound represented by the above general formula (4c) with the terminal of the vinyl polymer, thereby obtaining a terminal-modified vinyl polymer having a terminal structure derived from the compound represented by the above general formula (4c).
[0097] (Vinyl polymer preparation process) The first macromonomer production method and the second macromonomer production method may further include a step of preparing a vinyl polymer having a halogen group at the end (vinyl polymer preparation step). As a method for preparing (polymerizing) a vinyl polymer having a halogen group at the end, various known polymerization methods such as living cationic polymerization and living radical polymerization can be adopted. In addition, the third production method may further include a step of preparing a vinyl polymer having a functional group other than a halogen group at the end. As a method for preparing (polymerizing) a vinyl polymer having a functional group other than a halogen group at the end, a polymerization method using a mercaptan having a hydroxyl group such as mercaptoethanol or a mercaptan having a carboxyl group such as mercaptoacetic acid, as described in JP-A-1-203412, can also be used.
[0098] Hereinafter, a specific embodiment of the vinyl polymer preparation process will be described in detail, taking the living radical polymerization method as an example. As the vinyl monomer serving as the raw material of the vinyl polymer, the above-mentioned vinyl monomers can be appropriately used.
[0099] Examples of living radical polymerization include (a) a polymerization method using a chain transfer agent such as polysulfide, (b) a polymerization method using a radical scavenger such as an organic tellurium compound, a cobalt porphyrin complex, and / or a nitroxide compound, (c) an atom transfer radical polymerization (ATRP) method using an organic halide or the like as an initiator and a transition metal complex as a catalyst, and (d) a polymerization (reversible transfer catalytic polymerization (RTCP)) method using an organic halide or the like as an initiator and an organic molecule having a central atom such as nitrogen or oxygen as a catalyst. Of these, the atom transfer radical polymerization method is preferred because it is easy to control the molecular weight and molecular weight distribution of the vinyl polymer.
[0100] In living radical polymerization, the number of halogen terminal groups of the vinyl polymer obtained can be controlled by controlling the polymerization conditions. For example, the number of halogen terminal groups of the vinyl polymer obtained can be controlled by controlling the type of polymerization initiator. Specifically, when an initiator having one polymerization initiation point is used, a linear vinyl polymer having a halogen group at one end can be prepared.
[0101] Examples of initiators having one polymerization initiation point include ethyl 2-bromoisobutyrate, ethyl bromoacetate, methyl bromoacetate, (1-bromoethyl)benzene, allyl bromide, methyl 2-bromopropionate, methyl chloroacetate, methyl 2-chloropropionate, and (1-chloroethyl)benzene.
[0102] In the living radical polymerization, in addition to the initiator, a polymerization catalyst, a polydentate amine (ligand), a base, a reducing agent, a solvent, etc. may be used. The type and amount of each of these components can be appropriately selected by those skilled in the art.
[0103] <Additives> The polyimide precursor can be a composition containing various additives according to the desired purpose. Examples of such additives include phosphorus compounds (e.g., phosphoric acid, pyrophosphoric acid, polyphosphoric acid, phosphorous acid, hypophosphorous acid, or their alkali metal or alkaline earth metal salts), heat resistance agents, ultraviolet absorbers, light stabilizers, antioxidants, antistatic agents, lubricants, slip agents, crystal nucleating agents, tackifiers, release agents, plasticizers, pigments, dyes, flame retardants, reinforcing materials, inorganic fillers, microfibers, and X-ray opacifiers. As additives, one of the various additives described above may be used alone, or multiple types may be used in combination. In addition, the type and amount of these additives can be appropriately selected by those skilled in the art according to the desired purpose.
[0104] 2. Method for Producing Polyimide Precursor The method for producing the polyimide precursor includes a step (polymerization step) of polymerizing a monomer group including a tetracarboxylic dianhydride or its alkyl monoester or alkyl diester, a macromonomer, and a diamine other than the macromonomer in an organic solvent. The monomer group may optionally include a monomer other than the above (another monomer). The matters described in [1. Polyimide precursor] are appropriately incorporated herein by reference.
[0105] The polymerization method is not particularly limited, and any of the following (1) to (5) can be suitably used. Hereinafter, the tetracarboxylic dianhydride or its alkyl monoester or alkyl diester will also be referred to as the carboxylic acid component, and the macromonomer and the diamine other than the macromonomer will also be referred to as the diamine component. (1) A method in which a diamine component is dissolved in an organic solvent, and the diamine component is reacted with a carboxylic acid component in a substantially equimolar amount to the diamine component to polymerize it. (2) A method in which a carboxylic acid component is reacted with a diamine component in an organic solvent in an amount smaller than that of the carboxylic acid component to obtain a prepolymer having an acid dianhydride group or a carboxyl group at both ends, and then a diamine component is polymerized into the prepolymer in such a manner that the total amount used in the entire polymerization process is substantially equimolar to the carboxylic acid component. (3) A method in which a carboxylic acid component is reacted with a molar excess of a diamine component in an organic solvent to obtain a prepolymer having amino groups at both ends, and then, after additionally adding the diamine component to the prepolymer, a carboxylic acid component is added so that the total amounts of the carboxylic acid component and the diamine component used in the entire polymerization process are substantially equimolar, thereby polymerizing the prepolymer and the carboxylic acid component. (4) A method in which a carboxylic acid component is dissolved and / or dispersed in an organic solvent, and then a diamine component is added in a substantially equimolar amount to the carboxylic acid component, thereby polymerizing the carboxylic acid component and the diamine component. (5) A method in which a mixture of a carboxylic acid component and a diamine component in substantially equimolar amounts is reacted in an organic solvent to polymerize.
[0106] In this specification, substantially equimolar amounts means that the molar ratio between the carboxylic acid component and the diamine component is within the range of 100:98 to 100:102, and preferably 100:100.
[0107] Examples of the organic solvent include sulfoxide solvents such as dimethyl sulfoxide and diethyl sulfoxide; formamide solvents such as N,N-dimethylformamide and N,N-diethylformamide; acetamide solvents such as N,N-dimethylacetamide and N,N-diethylacetamide; pyrrolidone solvents such as N-methyl-2-pyrrolidone and N-vinyl-2-pyrrolidone; phenol solvents such as phenol, o-, m-, or p-cresol, o-, m-, or p-xylenol, o-, m-, or p-halogenated phenol, o-, m-, or p-catechol; ether solvents such as tetrahydrofuran, dioxane, and dioxolane; alcohol solvents such as methanol, ethanol, and butanol; cellosolve solvents such as butyl cellosolve; and organic polar solvents such as hexamethylphosphoramide and γ-butyrolactone. These organic solvents may be used alone or in combination. Additionally, aromatic hydrocarbons such as xylene and toluene can also be used.
[0108] [3. Polyimide] The polyimide according to one embodiment of the present invention is an imidized product of the polyimide precursor. Methods for imidizing the polyimide precursor include a thermal imidization method and a chemical imidization method. In the thermal imidization method, the polyimide precursor solution is heated to imidize the polyimide precursor without using an imidization accelerator. In the chemical imidization method, an imidization accelerator such as a dehydrating agent (dehydration ring-closing agent) represented by an acid dianhydride such as acetic anhydride, and / or a catalyst represented by a tertiary amine such as picoline, quinoline, isoquinoline, or pyridine is added to the polyimide precursor, and the polyimide precursor containing the imidization accelerator is heated to imidize the polyimide precursor.
[0109] An embodiment of the present invention also includes a polyimide film containing the polyimide. The polyimide film has a low moisture absorption rate and excellent dielectric properties in the region of 10 GHz or more, and can be used for flexible wiring boards in electronic devices. The polyimide film can be obtained, for example, by applying a polyimide precursor solution obtained by the above-mentioned method for producing a polyimide precursor onto a support, heating (imidization), and drying.
[0110] [4. Summary] An embodiment of the present invention may include the following features. [1] A polyimide precursor comprising a repeating unit represented by the following general formula (1):
[0111] [ka]
[0112] In formula (1), X 1 and X 2 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; A is a tetravalent tetracarboxylic acid residue; B is a divalent diamine residue; The diamine residue includes a macromonomer residue represented by the following general formula (2):
[0113] [ka]
[0114] In formula (2), R is a vinyl polymer; R 1 is -O-, -O(CO)-, -NH-, -N(CH3)-, or -N(CH2CH3)-; R 2 represents a trivalent or tetravalent group having 1 to 18 carbon atoms, which may have a heteroatom; R 3 each independently represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; n is 1 or 2; When n is 2, there are two R and two R 1 The structures of may be the same or different. [2] The polyimide precursor according to [1], wherein the polyimide precursor contains 0.1 to 10 mol % of a macromonomer residue represented by the general formula (2) in 100 mol % of diamine residues. [3] The polyimide precursor according to [1] or [2], wherein the vinyl polymer is a poly(meth)acrylic polymer or a polyisobutylene polymer. [4] The macromonomer residue is derived from a macromonomer represented by the following general formula (3): The polyimide precursor according to any one of [1] to [3], wherein the macromonomer represented by the following general formula (3) has a polystyrene-equivalent number average molecular weight of 500 to 600,000 and a molecular weight distribution of 1.8 or less, as measured by size exclusion chromatography:
[0115] [ka]
[0116] In formula (3), R is a vinyl polymer; R 1 is -O-, -O(CO)-, -NH-, -N(CH3)-, or -N(CH2CH3)-; R 2 represents a trivalent or tetravalent group having 1 to 18 carbon atoms, which may have a heteroatom; R 3 each independently represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; n is 1 or 2; When n is 2, there are two R and two R 1 The structures of may be the same or different. [5] A polyimide which is an imidization product of the polyimide precursor according to any one of [1] to [4]. [6] A polyimide film comprising the polyimide according to [5].
[0117] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. EXAMPLES
[0118] Hereinafter, one embodiment of the present invention will be described in detail with reference to examples, but the present invention is not limited to the following examples.
[0119] [Analysis method] (Polymerization conversion rate) The conversion rate of monomers to polymers in the production of vinyl polymers was measured using a gas chromatograph (GC (Shimadzu Corporation, GC-2000)). The column used was Agilent J&W GC column HP-1. Toluene was used as the standard.
[0120] (Qualitative and quantitative analysis of functional groups) Qualitative and quantitative analysis of functional groups in polymers 1 The analysis was performed using 1 H NMR (Bruker 400 MHz NMR). 30 mg of the polymer was dissolved in 0.8 g of deuterated chloroform to obtain a solution, which was used as a sample for analysis.
[0121] (Weight average molecular weight (Mw) and number average molecular weight (Mn)) The weight-average molecular weight and number-average molecular weight of the polymer were analyzed using SEC (HLC-8420GPC). The column used was TOSOH TSKgel SuperHM-L, and the standard was a polystyrene standard sample. The eluent was a mixed solvent of chloroform with 1.5% by weight of triethylamine added. 3 mg of the polymer was dissolved in 3 mL of the mixed solvent, and the resulting solution was used as the sample for analysis.
[0122] (Bromine end analysis) After replacing the terminal bromine groups of the polymer with potassium acrylate, 1 The amount of H at the base of the substituent was calculated by H NMR. The method for replacing the terminal bromine group is as follows. A large excess of dimethylacetamide and potassium acrylate was added to the vinyl polymer, and the resulting solution was stirred at 50°C for 30 minutes. An excess of ethyl acetate and water was added to the resulting solution, and only the organic layer was collected from the resulting mixture. The organic layer was then concentrated to obtain a vinyl polymer in which the terminal bromine group had been replaced with potassium acrylate. The resulting vinyl polymer was dissolved in deuterated chloroform, and the resulting solution was used as an analytical sample, 1 H NMR measurement was carried out. As a result, a signal of H at the base of the substituent substituted with potassium acrylate was confirmed in the range of 4.8 to 5.2 ppm, and the amount of terminal bromine of the vinyl polymer was calculated from the integral value.
[0123] (Measurement of coefficient of linear expansion (CTE)) Using a thermal analyzer (Hitachi High-Tech Science Corporation, "TMA / SS6100"), the polyimide film was heated from -10°C to 300°C in a nitrogen atmosphere, then cooled to -10°C and heated again to 300°C, and the linear expansion coefficient was calculated from the amount of distortion during the second heating from 50°C to 250°C. The measurement conditions are shown below. -Sample (polyimide film) size: width 3mm, length 10mm Load: 1g (9.8mN) Heating rate: 10℃ / min.
[0124] (Measurement of dynamic viscoelasticity) The dynamic viscoelasticity of the polyimide film was measured in an air atmosphere using a dynamic viscoelasticity measuring device (Hitachi High-Tech Science Corporation, "DM6100"). The correlation between the storage modulus (E') and the measurement temperature was plotted, and the inflection point temperature was read. In addition, the correlation between Tan δ calculated from the ratio (E' / E") of the storage modulus to the loss modulus (E") and the measurement temperature was plotted, and the Tan δ peak top temperature was read. The measurement conditions are shown below. Width of sample (polyimide film): 9mm -Sample holder (gripper) spacing: 20mm Measurement temperature range: 0℃~400℃ Heating rate: 3℃ / min Distortion amplitude: 10μm ·Measurement frequency: 1Hz, 5Hz, 10Hz Minimum tension / compression force: 100mN Tension / Compression Gain: 1.5 Initial force amplitude: 100mN.
[0125] (Moisture absorption rate measurement) The moisture absorption rate was measured using a thermogravimetric analyzer (TA Instruments' "SDT Q600"). The measurement was performed under a nitrogen atmosphere, and the moisture absorption rate was calculated from the weight change of the polyimide film when it was heated from 20°C to 120°C and then held at 120°C for 120 minutes. The measurement conditions are as follows. -Sample (polyimide film) size: 50mm x 100mm Pre-drying conditions: 150℃ x 30 minutes Humidity conditions: 23℃, 50%RH Measurement sample: The sample was left for one week under the above humidity control conditions and used for the measurement. Heating rate: 20℃ / min.
[0126] (Measurement of dielectric constant (Dk) and dielectric loss tangent (Df)) The dielectric constant and dielectric loss tangent were measured using a network analyzer 8719C manufactured by Hewlett Packard and a cavity resonator vibration method dielectric constant measuring device CP511 manufactured by Kanto Electronics Application Development Co., Ltd. The measurement conditions are as follows. -Sample (polyimide film) size: width 2mm, length 100mm ·Measurement frequency: 10GHz ·Measurement conditions: 23℃, 50%RH environment Measurement sample: The sample was left for 24 hours under the above measurement conditions and used for the measurement.
[0127] [Synthesis of macromonomers] 160 g of methanol, 320 g of butyl acrylate, 55.3 g of ethyl 2-bromoisobutyrate, 4.3 g of triethylamine, 0.16 g of cupric bromide, and 0.16 g of tris[2-(dimethylamino)ethyl]amine were added to the flask. Next, nitrogen was bubbled into the flask. Note that "nitrogen bubbling" refers to the flow of nitrogen into a flask or a target such as a solution to remove oxygen from the target. After the nitrogen bubbling, the mixture in the flask was heated and the temperature was raised to 45°C.
[0128] Separately, 49 g of methanol, 0.25 g of ascorbic acid, and 0.29 g of triethylamine were mixed to obtain a methanol solution, which was then bubbled with nitrogen and added dropwise to the flask at a rate of 5.1 mL / h.
[0129] 0.5 hours after the start of the dropping of the methanol solution, 480 g of butyl acrylate bubbled with nitrogen was dropped into the flask over 1.5 hours. 4 hours after the start of the dropping of the methanol solution, it was confirmed by gas chromatography that the conversion rate of butyl acrylate reached 95% or more, and the dropping of the methanol solution was stopped. Then, the reaction solution in the flask was concentrated at 100°C under vacuum for 1 hour. 800 g of butyl acetate, 8 g of Kyoward 500 (manufactured by Kyowa Chemical Industry), 8 g of Kyoward 700 (manufactured by Kyowa Chemical Industry), and 8 g of Radiolite 900 (manufactured by Showa Chemical Industry) were added to the concentrated reaction solution, and the mixture was stirred at 80°C for 1 hour. Next, the obtained reaction solution was filtered. The obtained filtrate was concentrated at 100°C under vacuum for 2 hours to obtain polybutyl acrylate (polymer 1-1) having bromine at one end. It was confirmed by SEC that the number average molecular weight of the obtained polymer 1-1 was 2574 and the molecular weight distribution was 1.30. Furthermore, it was found that polymer 1-1 has an average of 0.86 bromine terminals per molecule. 1 Confirmed by 1 H NMR.
[0130] 150 g of polymer 1-1 and 150 g of N,N-dimethylacetamide were added to a flask and stirred to make a homogenous mixture. 13.5 g of potassium carbonate and 16.4 g of diaminobenzoic acid were added while stirring. The flask was then heated and stirred at 80°C for 4 hours. After that, 450 g of 1-butanol and 450 g of water were added, and the mixture was stirred at room temperature, allowed to stand for separation, and an extraction operation was performed three times to extract only the organic layer. The organic layer obtained was concentrated at 50°C under vacuum for 1 hour to obtain a terminal-modified vinyl polymer (macromonomer) in which the bromine terminal of polymer 1-1 was replaced with a structure derived from diaminobenzoic acid. It was confirmed by SEC that the number average molecular weight of the obtained macromonomer was 2628 and the molecular weight distribution was 1.19. Furthermore, it was confirmed that the bromine terminal of the macromonomer was completely replaced with the ester group of diaminobenzoic acid. 1 Confirmed by 1 H NMR.
[0131] [Raw material monomers used and their abbreviations] DMF: N,N-dimethylformamide PDA: Paraphenylenediamine MDA: Metaphenylenediamine ODA: 4,4'-diaminodiphenyl ether PMDA: Pyromellitic dianhydride MM: macromonomer.
[0132] [Synthesis of non-thermoplastic polyimide precursors] (Synthesis Example 1) DMF (290.58 g) and ODA (28.11 g) were added to a 2000 mL glass flask, and PMDA (40.83 g) was added while stirring under a nitrogen atmosphere to prepare a reaction solution. After visually confirming that PMDA had dissolved, a solution was prepared by dissolving 4.05 g of PDA in DMF to a solids concentration of 20%, which was added to the reaction solution and stirred for 30 minutes. Finally, a solution was prepared by dissolving 1.01 g of PDA in DMF to a solids concentration of 5%, and this solution was gradually added to the reaction solution while paying attention to the increase in viscosity. When the viscosity of the reaction solution at 23 ° C. reached 2000 poise, the addition and stirring were stopped to obtain a polyimide precursor solution.
[0133] (Synthesis Example 2) DMF (290.41 g), ODA (27.49 g), and MDA (0.41 g) were added to a 2000 mL glass flask, and PMDA (41.02 g) was added while stirring under a nitrogen atmosphere to prepare a reaction solution. After visually confirming that PMDA had dissolved, a solution was prepared by dissolving 4.07 g of PDA in DMF to a solids concentration of 20%, which was added to the reaction solution and stirred for 30 minutes. Finally, a solution was prepared by dissolving 1.02 g of PDA in DMF to a solids concentration of 5%, and this solution was gradually added to the reaction solution while paying attention to the increase in viscosity. When the viscosity of the reaction solution at 23 ° C. reached 2000 poise, the addition and stirring were stopped to obtain a polyimide precursor solution.
[0134] (Synthesis Example 3) DMF (292.98 g), ODA (25.85 g), and MM (5.37 g) were added to a 2000 mL glass flask, and PMDA (38.06 g) was added while stirring under a nitrogen atmosphere to prepare a reaction solution. After visually confirming that PMDA had dissolved, a solution was prepared by dissolving 3.77 g of PDA in DMF to a solids concentration of 20%, which was added to the reaction solution and stirred for 30 minutes. Finally, a solution was prepared by dissolving 0.94 g of PDA in DMF to a solids concentration of 5%, and this solution was gradually added to the reaction solution while paying attention to the increase in viscosity. When the viscosity of the reaction solution at 23 ° C. reached 2000 poise, the addition and stirring were stopped to obtain a polyimide precursor solution.
[0135] (Synthesis Example 4) DMF (295.08 g), ODA (23.88 g), and MM (10.06 g) were added to a 2000 mL glass flask, and PMDA (35.64 g) was added while stirring under a nitrogen atmosphere to prepare a reaction solution. After visually confirming that PMDA had dissolved, a solution was prepared by dissolving 3.53 g of PDA in DMF to a solids concentration of 20%, which was added to the reaction solution and stirred for 30 minutes. Finally, a solution was prepared by dissolving 0.88 g of PDA in DMF to a solids concentration of 5%, and this solution was gradually added to the reaction solution while paying attention to the increase in viscosity. When the viscosity of the reaction solution at 23 ° C. reached 2000 poise, the addition and stirring were stopped to obtain a polyimide precursor solution.
[0136] (Synthesis Example 5) DMF (327.90 g) and ODA (28.72 g) were added to a 2000 mL glass flask, and PMDA (30.34 g) was added while stirring under a nitrogen atmosphere to prepare a reaction solution. After visually confirming that PMDA had dissolved, the mixture was stirred for 30 minutes. Finally, a solution was prepared by dissolving 0.94 g of PMDA in DMF to a solids concentration of 7.2%, and this solution was gradually added to the reaction solution while paying attention to the increase in viscosity. When the viscosity of the reaction solution at 23°C reached 2000 poise, the addition and stirring were stopped to obtain a polyimide precursor solution.
[0137] (Synthesis Example 6) DMF (329.37 g), ODA (24.74 g), and MM (7.77 g) were added to a 2000 mL glass flask, and PMDA (26.67 g) was added while stirring under a nitrogen atmosphere to prepare a reaction solution. After visually confirming that PMDA had dissolved, the mixture was stirred for 30 minutes. Finally, a solution was prepared by dissolving 0.82 g of PMDA in DMF to a solids concentration of 7.2%, and this solution was gradually added to the reaction solution while paying attention to the increase in viscosity. When the viscosity of the reaction solution at 23°C reached 2000 poise, the addition and stirring were stopped to obtain a polyimide precursor solution.
[0138] (Synthesis Example 7) DMF (331.00 g), ODA (20.30 g), and MM (16.43 g) were added to a 2000 mL glass flask, and PMDA (22.57 g) was added while stirring under a nitrogen atmosphere to prepare a reaction solution. After visually confirming that PMDA had dissolved, the mixture was stirred for 30 minutes. Finally, a solution was prepared by dissolving 0.70 g of PMDA in DMF to a solids concentration of 7.2%, and this solution was gradually added to the reaction solution while paying attention to the increase in viscosity. When the viscosity of the reaction solution at 23°C reached 2000 poise, the addition and stirring were stopped to obtain a polyimide precursor solution.
[0139] [Production of polyimide film] Example 1 26.0 g of a curing agent consisting of acetic anhydride / isoquinoline / DMF (weight ratio 12.42 / 3.93 / 9.65) was added to the polyimide precursor solution (65 g) obtained in Synthesis Example 3, and the solution was stirred and degassed at a temperature below 0°C, and cast onto aluminum foil using a comma coater. This resin film was heated at 110°C for 150 seconds. The self-supporting gel film was then peeled off from the aluminum foil and fixed to a metal frame, and dried and imidized at 250°C for 16 seconds, 320°C for 27 seconds, and 350°C for 37 seconds to obtain a polyimide film with a thickness of about 17 μm. When this film was fixed to a metal frame and heated at 450°C for 2 minutes, it was confirmed that the shape was maintained and that the film was non-thermoplastic.
[0140] (Examples 2 to 4, Comparative Examples 1 to 3) The same procedure as in Example 1 was repeated, except that the polyimide precursor solution obtained in Synthesis Example 3 was changed to the polyimide precursor solution shown in Table 1. When this film was fixed to a metal frame and heated at 450°C for 2 minutes, the shape was maintained, and it was confirmed that all of the films were non-thermoplastic.
[0141] [Evaluation Results] The evaluation results of the examples and comparative examples are shown in Table 1. In Examples 1 to 4, the E' inflection point temperature could not be measured within the measurement temperature range, and therefore "-" is entered.
[0142] [Table 1]
[0143] The molar ratios of monomers in each synthesis example are shown in Table 2.
[0144] [Table 2]
[0145] From Tables 1 and 2, the moisture absorption rate and dielectric constant of Examples 1 to 4 using MM were lower than those of Comparative Examples 1 to 3 not using MM. Furthermore, the dielectric tangent of Examples 1 to 4 was in a good range, while the dielectric tangent of Examples 2 to 4 was particularly low. Furthermore, it can be seen from a comparison of CTE, E' inflection point temperature, and Tg tan δ peak top temperature that Examples 1 to 4 and Comparative Examples 1 to 3 have the same heat resistance. Therefore, it can be seen that Examples 1 to 4 not only have improved moisture absorption rate, dielectric constant, and dielectric tangent, but also have the basic properties required for FPC. [Industrial Applicability]
[0146] An aspect of the present invention can be used, for example, in a high-frequency circuit board in an electronic device.
Claims
1. A polyimide precursor comprising a repeating unit represented by the following general formula (1): 【Chemistry 1】 In formula (1), X 1 and X 2 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; A is a tetravalent tetracarboxylic acid residue; B is a divalent diamine residue; The diamine residue includes a macromonomer residue represented by the following general formula (2): 【Chemistry 2】 In formula (2), R is a vinyl polymer; R 1 -O-, -O(CO)-, -NH-, -N(CH 3 )- or -N(CH 2 CH 3 )—and R 2 is a trivalent or tetravalent group having 1 to 18 carbon atoms, which may have a heteroatom; R 3 each independently represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; n is 1 or 2; When n is 2, there are two R and R 1 The structures of may be the same or different.
2. 2. The polyimide precursor according to claim 1, wherein the polyimide precursor contains 0.1 to 10 mol % of a macromonomer residue represented by the general formula (2) relative to 100 mol % of a diamine residue.
3. 2. The polyimide precursor according to claim 1, wherein the vinyl polymer is a poly(meth)acrylic polymer or a polyisobutylene polymer.
4. The macromonomer residue is derived from a macromonomer represented by the following general formula (3): The polyimide precursor according to claim 1, wherein the macromonomer represented by the following general formula (3) has a polystyrene-equivalent number average molecular weight of 500 to 600,000 and a molecular weight distribution of 1.8 or less, as measured by size exclusion chromatography: 【Chemistry 3】 In formula (3), R is a vinyl polymer; R 1 -O-, -O(CO)-, -NH-, -N(CH 3 )- or -N(CH 2 CH 3 )—and R 2 is a trivalent or tetravalent group having 1 to 18 carbon atoms, which may have a heteroatom; R 3 each independently represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; n is 1 or 2; When n is 2, there are two R and R 1 The structures of may be the same or different.
5. A polyimide which is an imidized product of the polyimide precursor according to any one of claims 1 to 4.
6. A polyimide film comprising the polyimide according to claim 5 .
Citation Information
Patent Citations
Heat resistant resin composition and dust removing substrate using the same
JP2005206786A
Heat-resistant resin, method for producing the same, and dust removing substrate of substrate processing apparatus given by using the resin
JP2006096864A
Compound, polymer, composition, molding, film, cured product, laminate, electronic component, and film-forming method
JP2022169849A
Benzofuran derivative composition, polyimide precursor composition, and method for producing polyimide resin
WO2015052907A1
Polyimide, metal clad laminate sheet and circuit board
JP2022154637A