Positive electrode and secondary battery
A positive electrode with a blend of O2, T#2, and O6 transition metal oxides, optimized by specific molar ratios, addresses slow lithium ion diffusion in O2 structures, achieving superior rapid charging and discharging performance and capacity.
Patent Information
- Application Number
- JP2023044731
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Transition metal oxides with an O2 structure exhibit slow lithium ion diffusion rates, leading to low rapid charge/discharge performance despite having a large discharge capacity in high potential regions.
A positive electrode comprising a mixture of transition metal oxides with O2, T#2, and O6 structures, along with O3 structures, optimized by specific molar ratios and chemical compositions, enhances lithium ion diffusion and rapid charging/discharging capabilities.
The electrode achieves excellent rapid charging and discharging performance with a large discharge capacity in high potential regions, outperforming conventional O3 structures.
Smart Images

Figure 2024134430000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a positive electrode and a secondary battery. [Background technology]
[0002] 2. Description of the Related Art In secondary batteries such as lithium ion secondary batteries, transition metal oxides having a layered crystal structure (hereinafter also referred to as "layered positive electrode active materials") are often used as positive electrode active materials. Layered positive electrode active materials are roughly classified according to the space group to which their crystal structure belongs, and examples thereof include transition metal oxides having an O2 type structure, transition metal oxides having an O3 type structure, transition metal oxides having an O6 type structure, transition metal oxides having a T#2 type structure, and transition metal oxides having a P2 type structure.
[0003] For example, Patent Document 1 proposes a method for producing a positive electrode active material, comprising: a Na-doped precursor preparation step for producing a sodium-containing transition metal oxide having a P2 structure belonging to the space group P63 / mmc; and an ion exchange step for substituting at least a portion of the sodium contained in the sodium-containing transition metal oxide with lithium by an ion exchange method, wherein at least lithium iodide is used as a Li ion source in the ion exchange step. For example, Patent Document 2 discloses a method for producing a positive electrode active material, comprising: a Na-doped precursor preparation step of preparing a transition metal oxide having a P2 structure belonging to the space group P63 / mmc and containing at least Na and Mn; and an ion exchange step of substituting at least a portion of the sodium contained in the transition metal oxide with lithium by an ion exchange method, wherein the transition metal composite oxide further contains at least one element selected from the group consisting of Al, Fe, Ca, Ti, Cr, Cu, Zn, Nb, and Mo, and has a composition that does not maintain a charge neutral condition. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-068555 [Patent Document 2] Patent Publication No. 2021-068556 Summary of the Invention [Problem to be solved by the invention]
[0005] Among various layered positive electrode active materials, transition metal oxides with an O2 type structure are stable up to high potentials, and therefore when a secondary battery is made with a positive electrode containing such an oxide, the discharge capacity tends to be large even during charging and discharging in a high potential range (for example, in the range of 2.0 to -4.8 V). Therefore, in recent years, there has been active development of batteries using transition metal oxides with an O2 type structure as a positive electrode active material, instead of the transition metal oxides with an O3 type structure that have been widely used in the past. However, O2-type transition metal oxides tend to have a higher activation energy for the diffusion of ion sources such as lithium ions and a smaller diffusion coefficient than conventional O3-type transition metal oxides, etc. As a result, the diffusion rate of ion sources such as lithium ions inside the positive electrode active material is slow, and rapid charge / discharge performance tends to be low.
[0006] In view of the above circumstances, an object of the present disclosure is to provide a positive electrode that has excellent rapid charge / discharge performance when incorporated in a battery and has a large discharge capacity in a high potential region, and a secondary battery including the positive electrode. [Means for solving the problem]
[0007] Means for solving the above problems include the following means. <1> a positive electrode active material A including at least one selected from the group consisting of a transition metal oxide having an O2 type structure, a transition metal oxide having a T#2 type structure, and a transition metal oxide having an O6 type structure; A positive electrode active material B containing a transition metal oxide with an O3 structure; A positive electrode having <2> The molar ratio (A / A+B) of the positive electrode active material A to the total molar amount of the positive electrode active material A and the positive electrode active material B is more than 0.3 and less than 0.7; <1> The positive electrode according to claim 1. <3> The positive electrode active material A contains a transition metal oxide having an O2 type structure. <1> or <2> The positive electrode according to claim 1. <4> The positive electrode active material A and the positive electrode active material B are lithium composite oxides represented by the following formula (1): <1> ~ <3> 13. A positive electrode according to any one of claims 1 to 12. Formula (1): Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O2 (In formula (1), a, b, x, y, z, p, q, and r satisfy the relationships 0≦a≦1, 0≦b≦0.05, x+y+z=1, and 0≦p+q+r≦0.20, respectively, and M represents at least one selected from the group consisting of Li, B, Mg, Al, K, Ca, Ti, Cr, Ga, Zr, Nb, Mo, and W.) <5> The above <1> ~ <4> 2. A secondary battery comprising the positive electrode according to claim 1. Effect of the Invention
[0008] According to one embodiment of the present disclosure, a positive electrode and a battery are provided that provide a battery having excellent rapid charge and discharge performance and a large discharge capacity in a high potential region. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment that is an example of the present disclosure will be described. These descriptions and examples are merely illustrative of the embodiment, and are not intended to limit the scope of the invention. In the present specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range. In addition, in the present specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples.
[0010] <Positive electrode> The positive electrode according to the present disclosure is a positive electrode having a positive electrode active material A including at least one selected from the group consisting of a transition metal oxide having an O2 type structure, a transition metal oxide having a T#2 type structure, and a transition metal oxide having an O6 type structure, and a positive electrode active material B including a transition metal oxide having an O3 type structure.
[0011] The positive electrode according to the present disclosure has the above-mentioned configuration, and when used in a battery, the positive electrode has excellent rapid charge / discharge performance and a large discharge capacity in a high potential region. The mechanism of this action is not necessarily clear, but is presumed to be as follows.
[0012] The positive electrode according to the present disclosure has a positive electrode active material A. The positive electrode active material A, that is, the group consisting of transition metal oxides having an O2 type structure, a T#2 type structure, and an O6 type structure, is stable up to a high potential and therefore has excellent charge / discharge capacity in a high potential region. On the other hand, the positive electrode according to the present disclosure further includes a positive electrode active material B containing a transition metal oxide having an O3 type structure. The transition metal oxide having an O3 type structure has excellent diffusion properties of an ion source such as lithium ions inside the positive electrode active material, and therefore has excellent rapid charge / discharge characteristics. Therefore, it is considered that the positive electrode according to the present disclosure having both the positive electrode active material A and the positive electrode active material B has excellent rapid charge / discharge performance and a large discharge capacity in a high potential region when used in a battery.
[0013] (Cathode active material A) The positive electrode active material A contains at least one selected from the group consisting of transition metal oxides having an O2 type structure, transition metal oxides having a T#2 type structure, and transition metal oxides having an O6 type structure.
[0014] O2-type transition metal oxides belong to the space group P63mc, have an ion source such as lithium ion at the center of an oxygen octahedron, and have a crystal structure in which there are two types of overlapping of oxygen and transition metal per unit cell.Specifically, O2-type transition metal oxides have a crystal structure in which one period is formed by four oxygen layers, two Li layers, and two transition metal layers.
[0015] Transition metal oxides with the T#2 structure belong to the space group Cmca, have a crystal structure in which lithium exists at the center of an oxygen tetrahedron, and there are two types of overlapping of oxygen and transition metal per unit cell.Specifically, transition metal oxides with the T#2 structure have a crystal structure in which one period is formed by four oxygen layers, two Li layers, and two transition metal layers.
[0016] Transition metal oxides with an O6 structure belong to the space group R-3m, have a crystal structure in which lithium exists at the center of an oxygen octahedron, and there are six different ways in which oxygen and transition metals overlap per unit cell. Specifically, transition metal oxides with an O6 structure have a crystal structure in which one period is made up of an O12 layer, six transition metal layers, and six Li layers.
[0017] From the viewpoint of improving the discharge capacity in the high potential region, the positive electrode active material A is preferably at least one selected from the group consisting of a lithium composite oxide having an O2 type structure, a lithium composite oxide having a T#2 type structure, and a lithium composite oxide having an O6 type structure, and is more preferably a lithium composite oxide having an O2 type structure.
[0018] The positive electrode active material A may contain other positive electrode active materials other than the transition metal oxides of the O2 type structure, the transition metal oxides of the T#2 type structure, and the transition metal oxides of the O6 type structure, within the scope of the effects of the present disclosure. Examples of other positive electrode active materials include transition metal oxides of the P2 type structure, transition metal oxides of the spinel type structure, transition metal oxides of the rock salt type structure, and transition metal compounds produced as by-products in the process of synthesizing the transition metal oxides of the O2 type structure, the transition metal oxides of the T#2 type structure, and the transition metal oxides of the O6 type structure. The total amount of the group consisting of the transition metal oxides having an O2 type structure, the transition metal oxides having a T#2 type structure, and the transition metal oxides having an O6 type structure in the positive electrode active material A is preferably 90 mass% or more, more preferably 95 mass% or more, and even more preferably 98 mass% or more.
[0019] (Cathode active material B) The positive electrode active material B contains a transition metal oxide having an O3 type structure.
[0020] The transition metal oxide of the O3 type structure belongs to the space group R-3m, has a crystal structure in which lithium is present at the center of an oxygen octahedron, and there are three types of overlapping between oxygen and the transition metal oxide per unit cell. Specifically, the transition metal oxide of the O3 type structure preferably has a crystal structure in which one period is formed by six oxygen layers, three Li layers, and three transition metal layers.
[0021] The positive electrode active material B may contain other positive electrode active materials other than the transition metal oxide with O3 type structure within the scope of the effects of the present disclosure. Examples of other positive electrode active materials include transition metal oxides with O3 type structure in which Na exists at the center of the oxygen octahedron (i.e., transition metal oxides with O3 type structure that do not satisfy the above definition), transition metal oxides with spinel type structure, transition metal oxides with rock salt type structure, and transition metal compounds that are by-produced in the process of synthesizing transition metal oxides with O3 type structure. The total amount of transition metal oxides having an O3 structure in the positive electrode active material B is preferably 90 mass % or more, more preferably 95 mass % or more, and even more preferably 98 mass % or more.
[0022] [Characteristics related to both positive electrode active material A and positive electrode active material B] The chemical compositions of the positive electrode active material A and the positive electrode active material B may be different or the same. However, from the viewpoint of achieving superior rapid charge / discharge performance and discharge capacity, for example, it is preferable that the chemical compositions of the positive electrode active material A and the positive electrode active material B are the same.
[0023] From the viewpoint of achieving superior rapid charge / discharge performance and discharge capacity, the positive electrode active material A and the positive electrode active material B are preferably a lithium composite oxide represented by the following formula (1). Formula (1): Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O2 (In formula (1), a, b, x, y, z, p, q, and r satisfy the relationships 0≦a≦1, 0≦b≦0.05, x+y+z=1, and 0≦p+q+r≦0.20, respectively, and M represents at least one selected from the group consisting of Li, B, Mg, Al, K, Ca, Ti, Cr, Ga, Zr, Nb, Mo, and W.)
[0024] In terms of achieving better rapid charge / discharge performance and discharge capacity, preferred embodiments of a, b, x, y, z, p, q and r in formula (1) are as follows: The value of a satisfies 0≦a≦1, and preferably satisfies 0.6≦a≦1. b satisfies 0≦b≦0.05, and preferably satisfies 0≦b≦0.01. x, y, and z satisfy x+y+z=1, and preferably satisfy both 0.95≦x+y+z≦1.05 and x+y+z=1. p and q satisfy 0≦p+q+r≦0.20, and preferably satisfy 0≦p+q+r≦0.10.
[0025] x satisfies 0≦x≦1, and preferably satisfies 0.1≦x≦1. The value of y satisfies 0≦y≦0.5, and preferably satisfies 0≦y≦0.33. z satisfies 0≦z≦1, and preferably satisfies 0≦z≦0.67. It is preferable that p satisfies 0≦p≦0.10. It is preferable that q satisfies 0≦q≦0.10. It is preferable that r satisfies 0≦r≦0.10. M represents at least one selected from the group consisting of Li, B, Mg, Al, K, Ca, Ti, Cr, Ga, Zr, Nb, Mo, and W, and preferably contains Al. When M is at least one of Li and K, it is preferable that x, y, z, p, q and r satisfy the relationship: 3≦4x+2y+3z-3p-q-2r≦3.5. When M is at least one of Mg and Ca, it is preferable that x, y, z, p and r satisfy the relationship 3≦4x+2y+3z−2p−r≦3.5. When M is at least one selected from the group consisting of B, Al, Cr, and Ga, it is preferable that x, y, z, p, and q satisfy the relationship: 3≦4x+2y+3z−p+q≦3.5. When M is at least one selected from the group consisting of Ti, Zr and Mo, it is preferable that the relationship 3≦4x+2y+3z+2q+r≦3.5 is satisfied. When M is Nb, it is preferable that the relationship 3≦4x+2y+3z+p+3q+2r≦3.5 is satisfied. When M is W, it is preferable that the relationship 3≦4x+2y+3z+2p+4q+3r≦3.5 is satisfied.
[0026] The lithium composite oxide represented by the above formula (1) is, for example, Li 1.05 Mn 0.33 Ni 0.33 Co 0.33 O2, Li 0.82 Na0Mn 0.5 Ni 0.2 Co 0.3 O2, Li 1.0 Na0Mn 0.5 Ni 0.2 Co 0.3 O2, Li 0.9 Na 0.05 Mn 0.5 Ni 0.2 Co 0.3 O2, Li 0.9 Na0Mn 0.67 Ni 0.33 Co0O2, Li 0.9 Na0Mn 0.5 Ni 0.2 Co 0.2 Al 0.1 O2, Li 0.9 Na0Mn 0.5 Ni 0.1 Co 0.3 Mg 0.1 Among the above, the lithium composite oxide is preferably LiO2, which has excellent rapid charge / discharge performance and discharge capacity. 1.05 Mn 0.33 Ni 0.33 Co 0.33 O2 is preferred.
[0027] From the viewpoint of achieving superior rapid charge / discharge performance and discharge capacity, the molar ratio (A / A+B) of the positive electrode active material A to the total molar amount of the positive electrode active material A and the positive electrode active material B is preferably more than 0.30 and less than 0.70, more preferably 0.35 or more and 0.65 or less, and even more preferably 0.40 or more and 0.60 or less. From the viewpoint of improving the initial discharge capacity, the molar ratio (A / A+B) of the positive electrode active material A to the total molar amount of the positive electrode active material A and the positive electrode active material B is preferably 0.45 or more and 0.75 or less, and more preferably 0.65 or more and 0.75 or less. From the viewpoint of achieving superior rapid charge-discharge performance, the molar ratio (A / A+B) of the positive electrode active material A to the total molar amount of the positive electrode active material A and the positive electrode active material B is preferably 0.25 or more and 0.0.65 or less, and more preferably 0.40 or more and 0.60 or less.
[0028] In order to achieve better rapid charge / discharge performance and discharge capacity, the content of the transition metal oxide having an O2 type structure is preferably more than 0.30 and less than 0.70 relative to the total amount of the transition metal oxide having an O3 type structure and the transition metal oxide having an O2 type structure, more preferably 0.35 to 0.65, and even more preferably 0.40 to 0.60.
[0029] As long as the positive electrode according to the present disclosure contains a positive electrode active material A and a positive electrode active material B, the state in which each active material is present is not particularly limited. For example, the positive electrode may be a laminate in which a layer A made of a positive electrode active material A and a layer B made of a positive electrode active material B are alternately stacked in a direction facing the current collector, a laminate in which the layers are alternately stacked in a direction opposing the current collector, or a laminate in which the layers are randomly stacked.
[0030] The positive electrode active material A and the positive electrode active material B contained in the positive electrode of the present disclosure are identified as follows. The positive electrode active material is observed by annular bright-field scanning transmission electron microscopy (ABF-STEM) using a transmission electron microscope under conditions of an acceleration voltage of 200 kV or more and a resolution of 0.2 nm or less. Then, the positive electrode active material A and the positive electrode active material B are determined from the observed crystal structure and space group.
[0031] [Other ingredients] The positive electrode according to the present disclosure may contain, as necessary, other components in addition to the positive electrode active material A and the positive electrode active material B. Examples of the other components include a conductive assistant, an electrolyte, a binder, an oxide solid electrolyte, a halide solid electrolyte, a thickener, a surfactant, a dispersant, a wetting agent, an antifoaming agent, and a solvent.
[0032] <Secondary battery> The secondary battery according to the present disclosure includes the positive electrode according to the present disclosure. According to the present disclosure, a secondary battery having excellent rapid charge / discharge performance and large discharge capacity in a high potential region can be obtained.
[0033] The secondary battery preferably includes, for example, a positive electrode according to the present disclosure, a negative electrode, and an electrolyte layer or a separator disposed between the positive electrode and the negative electrode. The secondary battery may further include a positive electrode current collector on the outer peripheral surface side of the positive electrode, and a negative electrode current collector on the outer peripheral surface side of the negative electrode. The secondary battery may be either a so-called solid-state battery using an inorganic solid electrolyte as the electrolyte (the content of the electrolytic solution as the electrolyte is less than 10 mass % of the total amount of the electrolyte), or a liquid battery using an electrolytic solution. EXAMPLES
[0034] Examples will be described below, but the present invention is not limited to these examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.
[0035] <Example 1> [Preparation of transition metal oxides with O2 structure] The raw materials were Mn(NO3)2·6H2O, Ni(NO3)2·6H2O, and Co(NO3)2·6H2O, and were dissolved in pure water so that the molar ratio of Mn, Ni, and Co (Mn / Ni / Co) was 5:2:3 to prepare a raw material solution. This raw material solution and a 12% by mass Na2CO3 solution were simultaneously titrated into a beaker. The titration speed was controlled so that the pH was 7.0 or more and less than 7.1. After the titration was completed, the mixed solution was stirred at 50°C and 300 rpm for 24 hours. The reaction product obtained was washed with pure water, and only the precipitated powder was separated by centrifugation. The obtained powder was dried at 120°C for 48 hours and then crushed in an agate mortar. Na2CO3 was added to the obtained powder, and a mortar with a composition ratio of Na 0.75 Mn 0.5 Ni 0.2 Co 0.3 The mixture was mixed so that the mixture became O2, and a mixed powder was obtained. This mixed powder was pressed with a load of 2 tons using cold isostatic pressing to produce pellets. The obtained pellets were pre-fired in air at 600°C for 6 hours, fired at 700°C for 24 hours, and then cooled to 250°C at 3°C / min. The Na-doped precursor was then synthesized by allowing it to cool. LiNO3 and LiCl were mixed at a ratio of 88:12, and weighed out so that the molar ratio of the amount of Li contained in the mixed powder was 10 times the amount of Na-doped precursor, to obtain a LiNO3·LiCl mixed powder. The LiNO3·LiCl mixed powder was mixed with the Na-doped precursor, and ion exchange was carried out in air at 280°C for 1 hour. After the ion exchange, water was added to dissolve the salt, and the mixture was washed with water to obtain a transition metal oxide with an O2 structure (chemical composition: Li 0.67 Mn 0.5 Ni 0.2 Co 0.3 O2) was obtained.
[0036] [Preparation of transition metal oxides with O3 structure] Mn(NO3)2·6H2O, Ni(NO3)2·6H2O, and Co(NO3)2·6H2O were used as raw materials, and dissolved in pure water so that the molar ratio of Mn, Ni, and Co (Mn / Ni / Co) was 1:1:1 to prepare a raw material solution. This raw material solution and a 12% by mass Na2CO3 solution were simultaneously titrated into a beaker. The titration speed was controlled so that the pH was 7.0 or more and less than 7.1. After the titration was completed, the mixed solution was stirred at 50°C and 300 rpm for 24 hours. The reaction product obtained was washed with pure water, and only the precipitated powder was separated by centrifugation. The obtained powder was dried at 120°C for 48 hours and then crushed in an agate mortar. Li2CO3 was added to the obtained powder, and a mortar with a chemical composition of Li was added. 1.05 Mn 0.33 Ni 0.33 Co 0.33 The mixed powder was pressed under a load of 2 tons using cold isostatic pressing to produce pellets. The resulting pellets were pre-fired in air at 600°C for 6 hours, then fired at 700°C for 24 hours, and cooled to room temperature at a rate of 3°C / min to produce transition metal oxides with an O3 structure (chemical composition: Li 0.67 Mn 0.33 Ni 0.33 Co 0.33 O2) was synthesized.
[0037] [Preparation of Positive Electrode] The target positive electrode active material was obtained by mixing a transition metal oxide with an O2 type structure and a transition metal oxide with an O3 type structure in a ratio of 50:50. 85 g of the positive electrode active material (powder after ball milling) obtained above and 10 g of carbon black, a conductive material, were introduced into 125 mL of a methylpyrrolidone solution of PVDF, in which 5 g of the binder polyvinylidene fluoride (PVDF) was dissolved in n-methylpyrrolidone as a solvent, and kneaded until uniformly mixed to produce a paste. This paste was applied to a 15 μm thick Al foil (current collector) with a basis weight of 6 mg / cm. 2 The electrode was then pressed to a paste thickness of 45 μm and a paste density of 2.4 g / cm. 3 Finally, this electrode was cut to a diameter of 16 mm to obtain a positive electrode.
[0038] [Preparation of negative electrode] The Li foil was cut to a diameter of 19 mm to obtain a negative electrode.
[0039] [Preparation of secondary battery] Using the obtained positive and negative electrodes, a CR2032 type coin cell, which is a lithium ion secondary battery, was fabricated. A PP porous separator was used as the separator, and the electrolyte was a mixed solution of EC (ethylene carbonate) and DMC (dimethyl carbonate) in a volume ratio of 3:7, with lithium hexafluorophosphate (LiPF6) dissolved at a concentration of 1 mol / L as the supporting electrolyte.
[0040] <Examples 2 to 5> The lithium ion secondary batteries of each example were obtained in the same manner as in Example 1, except that in the positive electrode preparation process, the ratio of the transition metal oxide having the O2 type structure to the transition metal oxide having the O3 type structure was set to the specifications shown in Table 1.
[0041] <Comparative Example 1> A lithium ion secondary battery of Comparative Example 1 was obtained in the same manner as in Example 1, except that in the manufacturing process of the positive electrode, no transition metal oxide having an O2 type structure was used.
[0042] <Comparative Example 2> A lithium ion secondary battery of Comparative Example 2 was obtained in the same manner as in Example 1, except that the step of preparing the positive electrode did not include a transition metal oxide having an O3 type structure.
[0043] <Evaluation of discharge capacity and rapid charge / discharge performance in the high potential range> Initial discharge capacity measurement A charge / discharge test was carried out on the secondary batteries of each example using a galvanostat under the conditions of a current of 0.1 C, a charge cut-off voltage of 4.8 V, and a discharge cut-off voltage of 2.0 V. After the first charge was completed, the amount of current required for discharging to 2.0 V was calculated, and the initial discharge capacity (mAh / g) was calculated by dividing the amount by the weight of the active material used in the measurement. The results are shown in Table 1.
[0044] Discharge capacity measurement at 5C A charge / discharge test was carried out on the secondary batteries of each example using a galvanostat under the conditions of a current of 5C, a charge cut-off voltage of 4.8V, and a discharge cut-off voltage of 2.0V. After the first charge was completed, the amount of current required for discharging to 2.0V was calculated, and the discharge capacity (mAh / g) at 5C was calculated by dividing the amount by the weight of the active material used in the measurement. The results are shown in Table 1 as "Discharge capacity at 5C".
[0045] The rapid charge-discharge efficiency was calculated using the following formula from the initial charge-discharge capacity calculated above and the discharge capacity at 5 C. The results are shown in Table 1. Rapid charge / discharge efficiency (%) = (discharge capacity at 5C (mAh) / initial discharge capacity (mAh)) x 100
[0046] Capacity retention after 50 cycles A charge-discharge test was carried out under the same conditions as for the initial discharge capacity, and the first discharge capacity and the 50th discharge capacity were calculated. The 50th discharge capacity was divided by the first discharge capacity to obtain the capacity retention rate after 50 cycles. The results are shown in Table 1.
[0047] In Table 1, [molar ratio A / (A+B)] refers to the molar ratio (A / A+B) of the positive electrode active material A to the total molar amount of the positive electrode active material A and the positive electrode active material B. In Table 1, [O2:O3 molar ratio] refers to the molar ratio of the O2-type transition metal oxide and the O3-type transition metal oxide contained in the positive electrode. In Table 1, for convenience, the O2-type transition metal oxide is referred to as "O2-type" or "O2", and the O3-type transition metal oxide is referred to as "O3-type" or "O3".
[0048] [Table 1]
[0049] As shown in Table 1, it was found that the secondary battery having the positive electrode of the embodiment had superior rapid charge / discharge performance and a larger discharge capacity in a region including a high potential region than the secondary battery having the positive electrode of the comparative example.
Claims
1. a positive electrode active material A including at least one selected from the group consisting of a transition metal oxide having an O2 type structure, a transition metal oxide having a T#2 type structure, and a transition metal oxide having an O6 type structure; A positive electrode active material B containing a transition metal oxide having an O3 structure; A positive electrode having
2. The positive electrode according to claim 1 , wherein a molar ratio (A / A+B) of the positive electrode active material A to a total molar amount of the positive electrode active material A and the positive electrode active material B is greater than 0.3 and less than 0.
7.
3. The positive electrode according to claim 1 , wherein the positive electrode active material A comprises a transition metal oxide having an O2 structure.
4. The positive electrode according to claim 1 , wherein the positive electrode active material A and the positive electrode active material B are a lithium composite oxide represented by the following formula (1): Formula (1): Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O 2 (In formula (1), a, b, x, y, z, p, q, and r satisfy the relationships of 0≦a≦1, 0≦b≦0.05, x+y+z=1, and 0≦p+q+r≦0.20, respectively, and M represents at least one selected from the group consisting of Li, B, Mg, Al, K, Ca, Ti, Cr, Ga, Zr, Nb, Mo, and W.)
5. A secondary battery comprising the positive electrode according to any one of claims 1 to 4.
Citation Information
Patent Citations
Method for producing positive electrode active material and method for manufacturing lithium ion battery
JP2021068555A
Method for producing positive electrode active material and method for manufacturing lithium ion battery
JP2021068556A
Cited By
Positive electrode material, secondary battery, and electronic device
WO2026178688A1