Polyester film and method for manufacturing the same, laminated film using the same
A polyester film with recycled PET and modified PBT, optimized for tearability, addresses the challenge of maintaining easy opening after thermal treatments, enhancing usability for retort foods.
Patent Information
- Application Number
- JP2024040584
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-20
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-03
AI Technical Summary
Packaging bags made of PET film do not maintain sufficient tear-opening properties after hot water or retort treatments, making them difficult for elderly, women, and children to open easily.
A polyester film composed of recycled PET and modified PBT with a specific content range and controlled cooling crystallization temperature, combined with a laminated structure, to enhance tearability post-treatment.
The film maintains excellent tearability after hot water and retort treatments, suitable for packaging sensitive contents like retort foods.
Smart Images

Figure 2024134536000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyester film. [Background technology]
[0002] Packaging bags made of various plastic films are widely used for packaging food, medicine, and miscellaneous goods. Among them, biaxially oriented polyethylene terephthalate film (PET film) manufactured by the tubular method, flat-type simultaneous biaxial orientation method, flat-type sequential orientation method, etc. has excellent durability, moisture resistance, mechanical strength, heat resistance, and oil resistance, and is widely used in the food packaging field, etc. Packaging bags made of PET film are often given notches to make them easier to open. However, when tearing from the notch, strong resistance is felt, and if too much force is applied, the contents may scatter. If the contents are easily crumbled snacks such as cookies, they may break when opened, or if the contents are liquids, they may stain clothes. Therefore, as a method for improving the tear-opening properties of packaging bags using PET film, Patent Document 1 discloses that a film made of PET containing modified polybutylene terephthalate (modified PBT) can be torn in a straight line when torn, and a packaging bag using this film can be opened without scattering the contents. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-053258 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, packaging bags using the film disclosed in Patent Document 1 sometimes lack sufficient tear-opening properties after a boiling process in which the contents are heated in hot water, or after a retort process in which the contents are sterilized. An object of the present invention is to provide a polyester film that can be used for packaging bags having excellent tear-opening properties and that can be easily opened even by people with weak strength, such as the elderly, women, and children, even after hot water treatment or retort treatment. [Means for solving the problem]
[0005] As a result of intensive research into solving the above-mentioned problems, the inventors have discovered that a polyester film obtained by forming a polyester film using recycled PET with a specific content of modified PBT into a film having a crystallization temperature of 160°C or less during cooling can suppress hydrolysis during hot water treatment, and can provide a packaging bag that maintains its tear-openability even after hot water treatment or retort treatment, thereby arriving at the present invention. That is, the gist of the present invention is as follows.
[0006] (1) A polyester film containing polyethylene terephthalate and modified polybutylene terephthalate, the content of modified polybutylene terephthalate in the polyester film being 3 to 18 mass %, and characterized in that in differential scanning calorimetry, the temperature at which the film crystallizes when heated from 25°C to 300°C at a heating rate of 20°C / min, held at 300°C for 10 minutes, and then cooled at a cooling rate of 40°C / min (cooling-down crystallization temperature) is 160°C or lower. (2) A method for producing the polyester film according to (1) above, comprising the steps of: (A) A step of obtaining a reaction product by subjecting polyethylene terephthalate to a depolymerization reaction (B) filtering the reaction product and recovering the filtrate. (C) A step of subjecting the filtrate to a polycondensation reaction in the presence of a polymerization catalyst at a temperature of 260° C. or higher and a pressure of 1.0 hPa or lower to obtain recycled polyethylene terephthalate. (D) A step of producing an unstretched film using a raw material containing the recycled polyethylene terephthalate, and then biaxially stretching the unstretched film. (3) A laminate film comprising the polyester film described above in (1) and a sealant resin layer. (4) A laminated film according to (3), characterized in that the tear propagation resistance is 0.35 N or less. (5) The laminate film according to (3) or (4), further comprising a gas barrier layer. (6) A packaging material comprising the polyester film described in (1) above. Effect of the Invention
[0007] The polyester film of the present invention has excellent tearability even after hot water treatment or retort treatment, and can be suitably used as a packaging material for retort foods and the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] <Polyester film> The polyester film of the present invention contains polyethylene terephthalate (PET) and modified polybutylene terephthalate (modified PBT). The polyester film of the present invention may contain other components as described below within the range that does not impair the effects of the present invention. The total content of PET and modified PBT is preferably 60 to 100% by mass, and more preferably 80 to 100% by mass.
[0009] (Polyethylene terephthalate (PET)) In the present invention, PET has terephthalic acid and ethylene glycol as its polymerization components, and other components may be copolymerized therewith within the range that does not impair the effects of the present invention. Examples of other copolymerization components include dicarboxylic acids such as isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, 5-sodium sulfoisophthalic acid, succinic acid, adipic acid, sebacic acid, dodecanedioic acid, dimer acid, maleic anhydride, maleic acid, fumaric acid, itaconic acid, citraconic acid, mesaconic acid, and cyclohexanedicarboxylic acid; oxycarboxylic acids such as 4-hydroxybenzoic acid, ε-caprolactone, and lactic acid; glycols such as 1,3-propanediol, 1,6-hexanediol, and cyclohexanedimethanol; and polyfunctional compounds such as trimellitic acid, trimesic acid, pyromellitic acid, trimethylolpropane, glycerin, and pentaerythritol.
[0010] PET can be obtained by known methods, i.e., a transesterification method from dimethyl terephthalate and ethylene glycol, or a direct esterification method from terephthalic acid and ethylene glycol to obtain an oligomer, which is then subjected to melt polymerization or further solid-state polymerization. As described later, in the method for producing a polyester film of the present invention, PET containing recycled polyethylene terephthalate (recycled PET) is used as the PET.
[0011] (Modified polybutylene terephthalate (modified PBT)) In the present invention, the modified PBT is a polybutylene terephthalate containing polytetramethylene glycol (PTMG) units. In the present invention, the molecular weight of PTMG is preferably 600 to 4000, more preferably 1000 to 3000, and further preferably 1000 to 2000. If the molecular weight of PTMG is less than 600, the obtained film may not have easy tearability, and if it exceeds 4000, the obtained film may have reduced performance such as mechanical strength, dimensional stability, and haze, and may not exhibit stable easy tearability. The content of the PTMG unit in the modified PBT is preferably 5 to 20% by mass, more preferably 10 to 20% by mass, and even more preferably 10 to 15% by mass. If the content of PTMG exceeds 20% by mass, a pulsating phenomenon in which the film pulsates during extrusion may occur, particularly when the film is produced on a mass production scale, and the thickness unevenness of the film may become large. The modified PBT can be obtained by adding PTMG and polycondensing in the polymerization step of PBT, for example, by polycondensation reaction of an ester exchange reaction product of dimethyl terephthalate and 1,4-butanediol with PTMG having a molecular weight of 600 to 4000.
[0012] In the polyester film of the present invention, the content of modified PBT must be 3 to 18 mass%, preferably 3 to 15 mass%, more preferably 3 to 8 mass%, and most preferably 3 to 4 mass%. If the content of modified PBT is less than 3 mass%, it is difficult for the obtained film to have easy tearability. If the content of modified PBT is more than 18 mass%, the packaging bag after retort treatment may have a decreased easy tearability.
[0013] (cooling down crystallization temperature) In differential scanning calorimetry, the polyester film of the present invention must have a crystallization temperature (temperature-drop crystallization temperature (Tc)) of 160° C. or less, preferably 159° C. or less, and more preferably 158° C. or less, when heated from 25° C. to 300° C. at a heating rate of 20° C. / min, held at 300° C. for 10 minutes, and then cooled at a cooling rate of 40° C. / min. When the temperature-drop crystallization temperature of the polyester film is within the above range and the modified PBT content is within the above specific range, the resulting packaging bag has excellent tearability even after hot water treatment or retort treatment.
[0014] (Tear propagation resistance) The polyester film of the present invention has easy tearability in the machine direction (MD). The excellent easy tearability in the present invention indicates a low tear propagation resistance value evaluated by JISK7128-1. The tear propagation resistance value is 0.1 N or less for a general PET film, but is 1.5 N or more for a laminated film in which the PET film and a 50 μm thick sealant resin layer are laminated. In the fields assumed by the present invention, such as packaging materials for retort curry, the tear propagation resistance value of the laminated film is required to be 0.35 N or less, preferably 0.30 N or less, and more preferably 0.28 N or less, in order for elderly people and children who have weak strength to easily open the package. In the fields assumed by the present invention, the tear propagation resistance value is an important parameter.
[0015] <Production method of polyester film> Next, the method for producing the polyester film of the present invention will be described. To produce the polyester film of the present invention, for example, a mixture of modified PBT and PET is fed into an extruder, heated and melted, extruded into a sheet form from the die orifice of a T-die, and then tightly wound around a cooling drum by an electrostatic casting method or the like and cooled to produce an unstretched film. Next, the obtained unstretched film is stretched both lengthwise and widthwise, and further heat-treated to produce a biaxially stretched film. Examples of the biaxial stretching method include a simultaneous biaxial stretching method using a tenter, a sequential biaxial stretching method using a roll and a tenter, and a tubular method.
[0016] In the production of the polyester film of the present invention, the PET mixed with the modified PBT preferably contains 30% by mass or more, more preferably 40% by mass or more, of recycled polyethylene terephthalate (recycled PET) described below. Furthermore, by setting the content of the modified PBT within a predetermined range, the crystallization temperature upon cooling of the film of the present invention can be set within the above range.
[0017] That is, the method for producing the polyester film of the present invention must include the following steps: (A) A step of obtaining a reaction product by subjecting polyethylene terephthalate to a depolymerization reaction (B) filtering the reaction product and recovering the filtrate. (C) A step of obtaining recycled polyethylene terephthalate (recycled PET) by subjecting the filtrate to a polycondensation reaction in the presence of a polymerization catalyst at a temperature of 260°C or higher and a pressure of 1.0 hPa or lower. (D) A step of producing an unstretched film using a raw material containing the recycled PET, and then biaxially stretching the unstretched film.
[0018] (A) Depolymerization process In the depolymerization step, polyethylene terephthalate is subjected to a depolymerization reaction to obtain a reaction product. The polyethylene terephthalate used in the depolymerization step is preferably polyethylene terephthalate for recycling (PET for recycling). [Recyclable PET] In the present invention, polyethylene terephthalate for recycling (PET for recycling) includes, for example, used PET products and PET pieces generated in the process of manufacturing PET products. The PET products and PET pieces may contain other substances than PET, but the PET content is preferably 70% by mass or more, and more preferably 80% by mass or more. Examples of used PET products include PET molded products (including fibers and films) that were once sold on the market and then collected after use. Representative examples include containers such as PET bottles and packaging materials. In addition, PET pieces generated during the manufacturing process of PET products are PET that did not make it into products. Examples include non-standard resin pellets, materials that are no longer needed during molding (film ends), pieces cut during molding, scraps generated during molding and processing, cut-up transitional products generated when changing brands, and cut-up prototypes and defective products.
[0019] The form of PET for recycling is not limited, and may be the original form of the used PET product or the PET piece, or may be in the form of cut pieces or crushed material (powder) obtained by further processing such as cutting or crushing, or may be in the form of a solid such as a molded body (pellet) obtained by molding these. More specifically, examples include (a) pellets obtained after cooling melted PET scraps, (b) pieces obtained by finely cutting PET molded products such as PET bottles, etc. In addition, the material may be in the form of a liquid (dispersion or solution) obtained by dispersing or dissolving the above-mentioned pieces, crushed material, etc. in a solvent. When producing the film of the present invention using these raw materials, they may be melted at a temperature equal to or higher than their melting points as necessary and charged into a can as a melt.
[0020] [Ethylene terephthalate oligomer, ethylene glycol] In the depolymerization step, the PET for recycling is subjected to a depolymerization reaction, thereby obtaining oligomers and the like that constitute the PET for recycling. In the depolymerization reaction, the PET for recycling can be subjected to the depolymerization reaction alone, but in the present invention, it is preferable to subject the PET for recycling to the depolymerization reaction in the presence of ethylene terephthalate oligomer and ethylene glycol. In the conventional method, depolymerization is carried out using only PET for recycling. In contrast, in the present invention, it is preferable to carry out the depolymerization reaction by adding PET for recycling in the presence of ethylene terephthalate oligomer and ethylene glycol so that the molar ratio (total glycol component / total acid component) of all components of ethylene terephthalate oligomer, ethylene glycol, and PET for recycling falls within the following range: The above molar ratio is preferably from 1.08 to 1.35, more preferably from 1.10 to 1.33, and further preferably from 1.12 to 1.30. Depolymerization at such a molar ratio efficiently precipitates not only various inorganic substances but also non-PET-derived foreign substances, and these foreign substances can be effectively removed in the filtration step described below. In the polycondensation step described below, it becomes possible to obtain recycled polyethylene terephthalate (recycled PET) having a diethylene glycol content and a carboxyl end group concentration within the ranges described below and containing relatively little foreign substances.
[0021] In the production method of the present invention, it is preferable that the above-mentioned depolymerization reaction does not decompose the PET for recycling into monomers, but into oligomers having a repeating unit of about 5 to 20. By controlling the decomposition in this way, not only various inorganic substances but also non-PET-derived foreign substances are efficiently precipitated, so that it is possible to remove a larger amount of foreign substances.
[0022] Both the ethylene terephthalate oligomer and the ethylene glycol may be publicly known or commercially available. They may also be produced by a publicly known production method. In particular, the ethylene terephthalate oligomer may be, for example, an esterification reaction product of ethylene glycol and terephthalic acid. The number-average degree of polymerization of the ethylene terephthalate oligomer is not limited, but may be, for example, about 2 to 20.
[0023] The amount of ethylene terephthalate oligomer used is not particularly limited as long as it can be set to the above molar ratio, but is preferably 0.20 to 0.80 mass% and more preferably 0.30 to 0.70 mass% based on 100 mass% of recycled PET obtained in the polycondensation step described below. If the amount of ethylene terephthalate oligomer used is less than the above range, the recycled PET is likely to block with each other when recycled PET is added, and there is a risk of excessive load being placed on the mixer. On the other hand, if the amount of ethylene terephthalate oligomer used is more than the above range, there will be no particular problem with the depolymerization reaction, but the recycled PET finally obtained may have a low recycling rate.
[0024] The amount of ethylene glycol used is not particularly limited as long as it can be set to the above molar ratio, but from the viewpoint of sufficiently proceeding with the depolymerization reaction, it is preferably 5 to 15 parts by mass, more preferably 5 to 10 parts by mass, per 100 parts by mass of ethylene terephthalate oligomer. If the amount of ethylene glycol used is too large, the carboxyl end group concentration in the recycled PET will be low, and if it is too small, the carboxyl end group concentration will be high, both of which may deviate from the preferred range described below. In particular, if more than 15 parts by mass of ethylene glycol is used, the ethylene terephthalate oligomer will be easily solidified in the reactor, and the subsequent reaction may not be able to continue.
[0025] When ethylene terephthalate oligomer and ethylene glycol are used in the depolymerization step, the mixing method (addition order) is not limited, but it is particularly preferable to add recycled PET to a mixture containing ethylene terephthalate oligomer and ethylene glycol, which can reduce unevenness in the progress of the depolymerization reaction. In addition, when mixing the ethylene terephthalate oligomer with ethylene glycol, for example, it is preferable to add ethylene glycol to the ethylene terephthalate oligomer. In addition, when adding, it is preferable to add the ethylene glycol after making the temperature of the contents uniform while stirring with a stirrer for the purpose of preventing the oligomer from solidifying.
[0026] When the recycled PET is added to the mixture, it is preferable to do so under normal pressure while stirring, and more preferable to add it after purging with a small amount of inert gas (generally nitrogen gas is used), which can prevent oxygen from being mixed in and more reliably prevent the deterioration of color tone.
[0027] The reaction temperature during depolymerization (particularly the internal temperature of the reactor) is not limited, but is preferably 245 to 280°C, and more preferably 255 to 275°C. If the reaction temperature during depolymerization is less than 245°C, the reaction product solidifies, the operability decreases, and even if recycled PET is obtained, the diethylene glycol content or the carboxyl end group concentration tends to be too high. If the reaction temperature exceeds 280°C, the diethylene glycol content or the carboxyl end group concentration of the obtained recycled PET may be too high.
[0028] The depolymerization reaction time (the reaction time from the end of the feeding of the PET for recycling) is not particularly limited as long as it is sufficient to complete the depolymerization reaction, but is usually preferably within 4 hours. In particular, from the viewpoints of suppressing the amount of diethylene glycol by-product and suppressing deterioration of the color tone of the polyester, it is more preferably within 2 hours. The lower limit of the reaction time is not limited, and can be, for example, about 1 hour.
[0029] The reaction apparatus is not particularly limited, and known or commercially available apparatuses can be used. In particular, the volume, shape of the stirring blades, etc. of the reaction apparatus may be any generally used esterification reaction apparatus, but in order to efficiently advance the depolymerization reaction, it is preferable to use a reaction apparatus having a distillation column that does not distill ethylene glycol out of the system.
[0030] (B) Filtration process In the filtration step, the reaction product is filtered and the filtrate is collected. The reaction product obtained in the depolymerization step is a liquid that mainly contains depolymerized PET for recycling (particularly regenerated oligomers). In the filtration step, the reaction product (liquid) is filtered with a filter to remove foreign matter, and the filtrate is collected.
[0031] In the above-mentioned depolymerization step, not only various inorganic substances but also non-PET-derived foreign substances are efficiently precipitated, so that the reaction product (liquid) can be filtered with a filter (preferably with a filtration grain size of about 10 to 25 μm) to remove the foreign substances, thereby obtaining a depolymerization product with a low amount of foreign substances. If a filter with a filtration particle size of more than 25 μm is used, foreign matter in the reaction product (liquid) cannot be sufficiently removed, and the resulting recycled PET contains a large amount of foreign matter. For this reason, when such recycled PET is used to produce an unstretched film, the T-die surface (lip surface) may become contaminated, and the film may break during stretching. On the other hand, filters with a filtration particle size of less than 10 μm are prone to clogging with foreign matter, and the filter life is shortened, which is disadvantageous in terms of cost and may also reduce operability. As the filter for the filtration step, a general filter can be used, but it is particularly preferable to use a metal filter. The material is not particularly limited, and examples thereof include stainless steel. The filter type is also not particularly limited, and examples thereof include a screen changer type filter, a leaf disk filter, and a candle type sintered filter. These can also be publicly known or commercially available filters.
[0032] (C) Polycondensation step In the polycondensation step, the filtrate is subjected to a polycondensation reaction in the presence of a polymerization catalyst at a temperature of 260° C. or higher and a pressure of 1.0 hPa or lower to obtain recycled polyethylene terephthalate (recycled PET).
[0033] [Polymerization catalyst] The polymerization catalyst is not limited, but at least one of germanium compounds, antimony compounds, titanium compounds, cobalt compounds, etc. can be used. Among them, it is preferable to use at least one of germanium compounds and antimony compounds. In particular, when the transparency of the obtained recycled PET is important, it is preferable to use a germanium compound. As each of the above compounds, at least one of oxides, inorganic acid salts, organic acid salts, halides, sulfides, etc. of germanium, antimony, titanium, cobalt, etc. can be exemplified.
[0034] The amount of the polymerization catalyst used is not particularly limited, but for example, it is 5×10 -5 mol or more, preferably 6×10 -5 The upper limit of the amount used is, for example, 1×10 -3 The amount is on the order of moles, but is not limited to this amount. In addition, since the polymerization catalyst contained in the PET for recycling may also act as a catalyst during the polycondensation reaction, it is preferable to take into consideration the type and content of the polymerization catalyst contained in the PET for recycling when adding a polymerization catalyst in the polycondensation process.
[0035] [Additives] During the polycondensation reaction, for example, (a) a fatty acid ester capable of adjusting the melt viscosity, (b) a hindered phenol-based antioxidant, (c) a phosphorus compound capable of suppressing thermal decomposition of the resin, and the like can be added as needed in addition to the above-mentioned polymerization catalyst.
[0036] Examples of fatty acid esters include beeswax (a mixture mainly composed of myricyl palmitate), stearyl stearate, behenyl behenate, stearyl behenate, glycerin monopalmitate, glycerin monostearate, glycerin distearate, glycerin tristearate, pentaerythritol monopalmitate, pentaerythritol monostearate, pentaerythritol distearate, pentaerythritol tristearate, pentaerythritol tetrastearate, dipentaerythritol hexastearate, etc. Among these, glycerin monostearate, pentaerythritol tetrastearate, and dipentaerythritol hexastearate are preferred. These can be used alone or in combination of two or more.
[0037] Examples of the hindered phenol antioxidants include 2,6-di-t-butyl-4-methylphenol, n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane, tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, 4,4'-butylidenebis-(3-methyl-6-t-butylphenol), tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, ... Ethylene glycol-bis[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionate], 3,9-bis{2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1'-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane, etc. are used, but tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane is preferred in terms of effectiveness and cost. These can be used alone or in combination of two or more.
[0038] Examples of phosphorus compounds that can be used include phosphorous acid, phosphoric acid, trimethyl phosphite, triphenyl phosphite, tridecyl phosphite, triphenyl phosphate, etc. These can be used alone or in combination of two or more.
[0039] [Reaction conditions] In the polycondensation reaction, the temperature must be 260° C. or higher, and preferably 270° C. or higher, and the pressure must be 1.0 hPa or lower, and preferably 0.8 hPa or lower. If the polycondensation reaction temperature is less than 260°C or the pressure exceeds 1.0 hPa, the polycondensation reaction time will be long, resulting in poor productivity and the resulting recycled PET will have an excessively low concentration of carboxyl terminal groups. On the other hand, if the polycondensation reaction temperature is too high, the resulting recycled PET will be colored due to thermal decomposition, the color tone will deteriorate, and the carboxyl end group concentration will be too high, so in the present invention, the upper limit of the polycondensation reaction temperature is usually preferably 285° C. The lower limit of the pressure can be, for example, about 0.1 hPa, but is not limited thereto.
[0040] [Recycled PET] Recycled PET can be obtained by the above polycondensation reaction. In the present invention, the recycled PET is preferably composed mainly of PET, and the PET content in the recycled PET is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90 to 100% by mass.
[0041] In the present invention, the content of diethylene glycol in the total glycol components of the recycled PET is preferably 0.5 to 4 mol%, more preferably 1 to 3.5 mol%, and even more preferably 1.2 to 3 mol%. In particular, in the production method of the present invention, ethylene glycol is used as one of the raw materials, and the obtained recycled PET has a low content of diethylene glycol, which is a by-product of ethylene glycol, and by having a diethylene glycol content of 4 mol% or less, it is possible to obtain performance with better thermal stability. Therefore, the raw material containing recycled PET can suppress contamination of the surface (lip surface) of the T-die when forming an unstretched film, making it possible to obtain high productivity.
[0042] In addition, the recycled PET preferably has a carboxyl end group concentration of 40 equivalents / t or less, more preferably 30 equivalents / t or less, even more preferably 25 equivalents / t or less, and most preferably 20 equivalents / t or less. The recycled PET has a carboxyl end group concentration of 40 equivalents / t or less, which is excellent in heat resistance, and it is possible to obtain molded products with excellent heat resistance by various molding methods. The lower limit of the carboxyl end group concentration is preferably 10 equivalents / t from the viewpoint of improving mechanical strength such as tensile elongation during film formation.
[0043] The average pressure rise rate of the recycled PET, as measured by the following method, is preferably 0.6 MPa / h or less, more preferably 0.5 MPa / h or less, and even more preferably 0.4 MPa / h or less. The above average pressure increase rate is an index of the amount of foreign matter such as inorganic matter and non-PET-derived foreign matter, and the lower the average pressure increase rate, the lower the amount of foreign matter. By setting the average pressure increase rate to 0.6 MPa / h or less, it is possible to produce a stretched film with a high stretch ratio, for example, 10 times or more. The lower limit of the average pressure increase rate can be, for example, about 0.01 MPa / h, but is not limited thereto. The above average pressure rise rate is calculated using a pressure rise tester including an extruder and a pressure sensor, the filter is set at the tip of the extruder, polyester resin is melted in the extruder at 300°C, and the molten material is extruded from the filter at a discharge rate of 29.0 g / min. The pressure value at the start of extrusion is defined as the "initial pressure value (MPa)", and the pressure value at the point when extrusion is continued for 12 hours thereafter is defined as the "final pressure value (MPa)". Based on these pressure values, the average pressure rise rate is calculated using the following formula A. Average pressure rise rate (MPa / h) = (final pressure value - initial pressure value) / 12 (Formula A) The extruder, filter, and the like used in the above-mentioned measurements are not limited as long as they satisfy the requirements of the present invention, and publicly known or commercially available extruders, filters, and the like can be used as appropriate.
[0044] The intrinsic viscosity of the recycled PET is not particularly limited, but is usually preferably 0.44 to 0.80, more preferably 0.55 to 0.70. The recycled PET can also be polymerized to a high degree through a solid-phase polymerization process. In this case, the intrinsic viscosity of the resulting recycled PET is usually preferably 0.80 to 1.25.
[0045] (D) Stretching process In the stretching step, an unstretched film is produced using a film-forming raw material containing the recycled PET, and then the unstretched film is biaxially stretched.
[0046] [Film forming raw materials] The content of recycled PET in the film-forming raw material for producing the unstretched film is not limited, and is usually preferably 20% by mass or more, more preferably 24% by mass or more, and from the environmental viewpoint of Ecomark certification, etc., it is preferably 25% by mass or more, more preferably 35% by mass or more, even more preferably 40% by mass or more, and most preferably 50% by mass or more. If the content of recycled PET is too low, the recycle rate of the obtained film will decrease accordingly. The upper limit of the content can usually be set to about 80% by mass, but is not limited thereto. The recycled PET may be made of only one type of material, or may be a mixture of two or more types of recycled PET, or may be a mixture of recycled PET and a resin other than recycled PET. In order to set the crystallization temperature of the film of the present invention within the range specified by the temperature drop, the content of the recycled PET is preferably 30% by mass or more, more preferably 40% by mass or more. The upper limit of the content of the recycled PET can be set to 100% by mass, but is not limited thereto.
[0047] As a film-forming raw material, in addition to the above-mentioned recycled PET (depolymerized-repolycondensed product), in order to increase the recycling rate within a range that does not impair the effects of the present invention, remelted PET for recycling (remelted product) may be used, and polyethylene terephthalate (virgin PET) that does not use recycled PET may also be used.
[0048] The content of the remelted product in the film-forming raw material is usually preferably 75% by mass or less, more preferably 65% by mass or less, even more preferably 50% by mass or less, particularly preferably 40% by mass or less, and most preferably 35% by mass or less. Film-forming raw materials with a remelted product content of more than 75% by mass tend to increase foreign matter or heat-degraded matter, and to cause problems such as breakage during film formation. In addition, the mechanical properties of the resulting film, such as tensile elongation, tend to be reduced. The film scraps and defective products used as the raw material for the remelted product have different concentrations of various additives, such as lubricants such as silica and antioxidants, depending on the brand of the product. Therefore, the greater the content of the remelted product in the film-forming raw material, the greater the variation in the additive concentrations, which may adversely affect the haze, wetting tension of the film surface, printability, etc. of the obtained film. For the reasons mentioned above, in the case of a polyester film composed of multiple layers, the content of remelted products in the surface layer is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less. On the other hand, since the intermediate layer does not affect the film surface properties such as wetting tension and printability even if the intermediate layer contains a large amount of remelted product, the intermediate layer may contain a large amount of remelted product in order to increase the recycling rate. The intermediate layer may contain 100% by mass of remelted product.
[0049] The higher the recycling rate of the polyester film of the present invention, the better. Specifically, it is usually preferably 25% by mass or more, more preferably 35% by mass or more, even more preferably 40% by mass or more, particularly preferably 50% by mass or more, and most preferably 65% by mass or more. The upper limit of the recycling rate can be, for example, about 80% by mass, but is not limited thereto. Therefore, it is preferable to adjust the composition of PET in the film-forming raw material so as to obtain the above recycling rate. In the present invention, the recycling rate R of PET refers to the mass ratio represented by the following formula. R(mass%)=A×B+C (where A indicates the mass ratio (mass%) of recycled PET in depolymerized-repolycondensed PET, B indicates the mass ratio (mass%) of depolymerized-repolycondensed PET in the film, and C indicates the mass ratio (mass%) of remelted PET in the film.)
[0050] [Film forming] The unstretched film can be produced by any known film-forming method, for example, by extruding the melt of the film-forming raw material from a T-die and then cooling it with a casting roll. In this case, it is preferable to precisely control the actual temperature of the casting roll surface in order to make the crystallinity of the unstretched film uniform.
[0051] [Biaxial stretching] The unstretched film is then biaxially stretched, resulting in a film with excellent tensile elongation in both the machine direction (MD) and the transverse direction (TD). The biaxial stretching method is not limited, and examples thereof include simultaneous biaxial stretching and sequential biaxial stretching. From the viewpoint of the surface balance of mechanical properties that reduces the difference between MD and TD for both physical properties of tensile strength and tensile modulus, simultaneous biaxial stretching is preferred, and from the viewpoint of the surface balance of thermal properties that reduces the difference between MD and TD for dry heat shrinkage, sequential biaxial stretching is preferred, and these can be appropriately selected depending on the desired film properties and applications. The stretching ratio can be appropriately set depending on, for example, the application of the film, the desired physical properties, etc., and can be, for example, 2 to 4 times in MD and 2 to 4 times in TD, but is not limited thereto. The stretching temperature is not limited, and may be, for example, in the range of 40 to 220° C. In particular, in the case of sequential stretching, it is preferable that MD stretching is performed at 40 to 80° C., and TD stretching is performed at 80 to 150° C. In addition, in the case of simultaneous biaxial stretching, it is preferable to perform it at 160 to 220° C.
[0052] [Heat treatment] The obtained biaxially stretched film is preferably subjected to a heat treatment at a temperature of about 220 to 240° C. for a short time, if necessary, in order to improve dimensional stability and suppress hot water shrinkage. The deformation and heat imparted during the stretching process cause the crystallization of the stretched film to proceed, and a polyester film having crystallization characteristics represented by a crystallization temperature upon cooling within the range of the present invention makes it easy to appropriately control the surface crystallization degree of the film, and has excellent mechanical properties.
[0053] <Other components in polyester film> Other components contained in the polyester film of the present invention include, for example, additives contained in general films, as described below. The additives include additives that are added for the first time during the production of the film of the present invention, as well as additives and impurities contained in the raw materials.
[0054] The polyester film of the present invention may contain one or more additives such as colorants, fillers, dispersants, antioxidants, UV absorbers, preservatives, antistatic agents, blocking agents, impact modifiers, and inorganic fine particles, provided that the additives do not impair the performance of the film. In particular, the film of the present invention may contain a lubricant for the purpose of improving the slip property of the film. Specific examples of the lubricant include clay, talc, calcium carbonate, zinc carbonate, wollastonite, silica, alumina, magnesium oxide, calcium silicate, sodium aluminate, calcium aluminate, magnesium aluminosilicate, glass balloons, carbon black, zinc oxide, antimony trioxide, zeolite, hydrotalcite, layered silicate, ethylene bisstearic acid amide, and the like. Among these, silica is preferred. The content of the lubricant is not limited, but is usually about 0.01 to 0.3 mass% in the polyester film.
[0055] The polyester film of the present invention may contain other polymers such as polyethylene naphthalate and polycyclohexylene dimethylene terephthalate, provided that the effects of the present invention are not impaired.
[0056] <Polyester film surface> The surface of the polyester film of the present invention may be treated by corona discharge treatment, surface hardening treatment, plating treatment, coloring treatment, or various coating treatments depending on the application. In addition, an adhesion layer, a gas barrier layer, a printing layer, etc. may be provided as necessary.
[0057] <Thickness of polyester film> The thickness of the polyester film of the present invention is preferably 50 μm or less, more preferably 30 μm or less, and most preferably 20 μm or less from the viewpoint of improving tearability, while it is preferably 5 μm or more, and most preferably 10 μm or more from the viewpoint of mechanical strength.
[0058] <Laminated film> The polyester film of the present invention may be in the form of a single layer or a plurality of layers formed by simultaneous melt extrusion or lamination. For example, in addition to a two-kind two-layer structure in which a polyester film (A) containing depolymerized-repolycondensed PET is laminated with a polyester film (B) containing remelted PET, a two-kind three-layer structure in which the film (B) is sandwiched between the films (A) may be used. In a polyester film having a layer structure in which an intermediate layer is sandwiched, such as a two-kind three-layer structure, the intermediate layer film (B) does not constitute the surface of the laminated film, so that it has little effect on bending resistance, strength, surface crystallinity, etc., and the content of remelted PET can be increased. The polyester film of the present invention can be used alone or can be used as a laminate film with other layers (barrier layers such as a gas barrier layer, a printed layer, an adhesive layer, a base resin layer, a sealant resin layer, etc.). The laminate film can have a layer structure of, for example, A / S, A / I / S, A / G / S, A / G / I / S, A / I / G / S, A / B / S, A / I / B / S, A / B / I / S, A / G / B / S, A / B / G / S, A / G / I / B / S, A / G / Examples of the adhesive include, but are not limited to, B / I / S, A / I / G / B / S, A / I / B / G / S, A / B / G / I / S, A / B / I / G / S, B / A / S, B / I / A / S, B / A / I / S, B / G / A / S, B / A / G / S, B / G / I / A / S, B / G / A / I / S, B / I / G / A / S, B / I / A / G / S, B / A / G / I / S, B / A / I / G / S, etc. An adhesive layer may also be provided between the layers.
[0059] (Gas barrier layer) The gas barrier layer is a layer for blocking oxygen and the like. Methods for laminating a gas barrier layer include a method of depositing an inorganic material on the film surface, a method of applying a gas barrier coating liquid and drying it, and a method of laminating an aluminum foil or a gas barrier film. The oxygen permeability of a film laminated with a gas barrier layer is 100 ml / (m 2 ·day·MPa) or less.
[0060] When forming a vapor deposition layer by vapor deposition of an inorganic substance on the film surface, examples of the inorganic substance used include metals such as aluminum, silicon, magnesium, palladium, zinc, nickel, silver, copper, gold, indium, stainless steel, chromium, and titanium, as well as oxides of these metals or compounds thereof.
[0061] In the vapor deposition layer, the content of these inorganic substances is usually within the range of about 95 to 100 mass %, but is not limited to this range.
[0062] The thickness of the deposition layer is not limited, but is usually preferably 0.005 to 0.3 μm, and more preferably 0.01 to 0.15 μm. If the thickness is less than 0.005 μm, the uniformity and thickness of the deposition layer may be insufficient, and sufficient gas barrier properties may not be obtained. On the other hand, if the thickness exceeds 0.3 μm, microcracks may easily occur, and the gas barrier properties may be reduced.
[0063] The method for forming the vapor-deposited layer is not particularly limited, and examples thereof include physical vapor deposition (PVD), chemical vapor deposition (CVD), etc. These methods can be carried out within the range of known conditions.
[0064] When a gas barrier layer is provided by applying a gas barrier coating liquid to a film surface and drying it, examples of the gas barrier coating liquid include a gas barrier coating liquid (I) containing a polyvinylidene chloride, and a gas barrier coating liquid (II) containing an inorganic layered compound and a resin.
[0065] As the polyvinylidene chloride of the gas barrier coating liquid (I), in addition to polyvinylidene chloride (PVDC), polyvinylidene chloride copolymers, which are copolymers of vinylidene chloride and other monomers (vinyl chloride, etc.), can be used.
[0066] The polyvinylidene chlorides to be used may be publicly known or commercially available products. Also, products obtained by publicly known manufacturing methods (such as emulsion polymerization methods) may be used. In this case, in the emulsion polymerization method, the polyvinylidene chlorides can be obtained in the form of latex, and the latex or a liquid with its concentration adjusted may be used as the coating liquid. In this case, the average particle size of the polyvinylidene chlorides in the coating liquid is preferably 0.05 to 0.5 μm, and more preferably 0.07 to 0.3 μm. By adjusting the particle size to such a range, the storage stability and coatability of the latex can be further improved.
[0067] The gas barrier coating solution (II) contains an inorganic layered compound and an optional resin.
[0068] The inorganic layered compound refers to an inorganic compound in which unit crystal layers are stacked on top of each other to form a layered structure. As the inorganic layered compound, clay minerals having swelling and cleavage properties in a solvent are preferred. Examples of such clay minerals include kaolinite, dickite, nacrite, halloysite, antigorite, chrysotile, pyrophyllite, montmorillonite, beidellite, bentonite, nontronite, saponite, sauconite, stevensite hectorite, tetrasilylic mica, sodium teniolite, muscovite, margarite, talc, vermiculite, phlogopite, xanthophyllite, and chlorite. Among them, clay minerals of the smectite group, vermiculite group, and mica group are preferred, and the smectite group is more preferred. Examples of the smectite group include montmorillonite, beidellite, nontronite, saponite, sauconite, stevensite, and hectorite. Furthermore, these clay minerals may be treated with an organic substance such as ion exchange to improve dispersibility, etc., and may also be used as inorganic layered compounds.
[0069] The aspect ratio of the inorganic layered compound is not particularly limited, but is usually preferably about 50 to 5000, and more preferably 200 to 3000. If the aspect ratio is less than 50, the gas barrier property is not sufficiently exhibited. On the other hand, it is technically difficult to obtain an inorganic layered compound having an aspect ratio of more than 3000, and it is expensive in terms of cost and economy. Therefore, from the viewpoint of ease of production, the aspect ratio is preferably 3000 or less.
[0070] In view of gas barrier properties, transparency, film-forming properties, etc., the inorganic layered compound is preferably in the form of a powder, and more preferably has an average particle size of 5 μm or less. In particular, in applications requiring transparency, it is more preferably has an average particle size of 1 μm or less. The lower limit of the average particle size can be, for example, 0.01 μm, but is not limited thereto.
[0071] The content of the inorganic layered compound in the gas barrier layer using the gas barrier coating liquid (II) can be appropriately set within the range of, for example, about 5 to 20% by volume, but is not limited thereto.
[0072] The resin used in the gas barrier coating liquid (II) is not particularly limited, and examples thereof include polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyacrylonitrile, polysaccharides, polyacrylic acid and its esters. Among them, hydrogen-bonding resins in which the mass percentage of hydrogen-bonding groups or ionic groups per unit mass of resin is 20 to 60% are preferred, and hydrogen-bonding resins in which the mass percentage of hydrogen-bonding groups or ionic groups per unit mass of resin is 30 to 50% are more preferred. The term "hydrogen-bonding group" refers to a group having at least one hydrogen bonded directly to an atom (heteroatom) other than carbon. The term "ionic group" refers to a group having at least one positive or negative charge that is localized to such an extent that it can be hydrated by water molecules in water. Examples of the hydrogen-bonding group of the hydrogen-bonding resin include a hydroxyl group, an amino group, a thiol group, a carboxyl group, a sulfonic acid group, and a phosphate group. Examples of the ionic group include a carboxylate group, a sulfonic acid ion group, a phosphate ion group, an ammonium group, and a phosphonium group. Among them, a hydroxyl group, an amino group, a carboxyl group, a sulfonic acid group, a carboxylate group, a sulfonic acid ion group, and an ammonium group are particularly preferred.
[0073] Specific examples of hydrogen-bonding resins include polyvinyl alcohol and its analogs, vinyl alcohol resins such as ethylene-vinyl alcohol copolymers, polysaccharides, polyacrylic acid, sodium polyacrylate, poly-2-hydroxyethyl acrylate, poly-2-hydroxyethyl methacrylate, polyacrylamide, acrylic resins such as ethylene-acrylic acid copolymers and their salts, polyaminoamide resins such as diethylenetriamine-adipic acid polycondensates, polyethylenesulfonic acid, sodium polystyrenesulfonate, polyvinylpyridine and its salts, polyethyleneimine and its salts, polyallylamine and its salts, polyvinylpyrrolidone, polyvinylsulfonic acid and its salts, polyvinylthiol, polyethylene glycol, polypropylene glycol, polyglycerin, etc. Among them, polyvinyl alcohol, ethylene-vinyl alcohol copolymers, and polysaccharides are preferred.
[0074] Here, polyvinyl alcohol is a polymer having a vinyl alcohol monomer unit as a main component. Examples of such polyvinyl alcohol include a polymer obtained by hydrolyzing or transesterifying (saponifying) the acetate portion of vinyl acetate polymer (more precisely, a copolymer of vinyl alcohol and vinyl acetate), and a polymer obtained by saponifying a vinyl trifluoroacetate polymer, a vinyl formate polymer, a vinyl pivalate polymer, a t-butyl vinyl ether polymer, a trimethylsilyl vinyl ether polymer, etc. The saponification degree of polyvinyl alcohol is preferably 70% or more in mole percentage, more preferably 85% or more, and more preferably 98% or more, so-called fully saponified products. The polymerization degree is preferably 100 to 5000, more preferably 200 to 3000.
[0075] The vinyl alcohol fraction of the ethylene-vinyl alcohol copolymer is preferably 40 to 80 mol %, and more preferably 45 to 75 mol %. The melt index of the ethylene-vinyl alcohol copolymer (a value measured under conditions of a temperature of 190°C and a load of 2160 g) is not particularly limited, but is preferably 0.1 to 50 g / 10 min. The ethylene-vinyl alcohol copolymer in the present invention may be modified with a small amount of a copolymerization monomer as long as the object of the present invention is not impaired.
[0076] Polysaccharides are biopolymers synthesized in living systems by condensation polymerization of various monosaccharides, and include those chemically modified based on these. Examples of polysaccharides include cellulose and cellulose derivatives such as hydroxymethylcellulose, hydroxyethylcellulose, and carboxymethylcellulose, amylose, amylopectin, pullulan, curdlan, xanthan, chitin, and chitosan.
[0077] When the resin used in the gas barrier coating liquid (II) is a hydrogen-bonding resin, a crosslinking agent may be used to improve its water resistance. Examples of the crosslinking agent include titanium-based coupling agents, silane-based coupling agents, melamine-based coupling agents, epoxy-based coupling agents, isocyanate-based coupling agents, copper compounds, and zirconium compounds.
[0078] Examples of the dispersion medium that swells and cleaves the inorganic layered compound include water, alcohols (methanol, ethanol, propanol, isopropanol, ethylene glycol, diethylene glycol, etc.), dimethylformamide, dimethylsulfoxide, acetone, etc. In particular, water, alcohol, or a water-alcohol mixture is preferred.
[0079] As the solvent used for preparing the gas barrier coating liquid (II), various organic solvents can be used in addition to water.As the organic solvent, for example, hydrocarbon solvents such as cyclohexane, normal hexane, benzene, etc., alcohol solvents such as methanol, ethanol, propanol, isopropyl alcohol, isobutyl alcohol, etc., ketone solvents such as acetone, ketone, methyl ethyl ketone, etc., ester solvents such as methyl acetate, ethyl acetate, isopropyl acetate, isobutyl acetate, isopentyl acetate, etc., ether solvents such as ethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol monomethyl ether, etc.
[0080] The method for producing the gas barrier coating liquid (II) is not particularly limited, but from the viewpoint of uniformity during blending and ease of operation, the following can be used: a method of mixing a liquid in which a resin is dissolved with a dispersion in which an inorganic layered compound has been previously swollen and cleaved, and then removing the solvent (Method 1), a method of adding a dispersion in which an inorganic layered compound has been swollen and cleaved to a resin, and then removing the solvent (Method 2), a method of adding an inorganic layered compound to a liquid in which a resin is dissolved, and then forming a dispersion in which the inorganic layered compound is swollen and cleaved, and then removing the solvent (Method 3), a method of thermally kneading a resin and an inorganic layered compound (Method 4), etc. From the viewpoint of easily obtaining a large aspect ratio of the inorganic layered compound, the first three methods are preferred.
[0081] When using the gas barrier coating liquid (II), an anchor coating layer may be provided before the gas barrier coating layer is provided in order to increase adhesion to the film surface. The anchor coating liquid used for the anchor coating layer is not particularly limited, but is preferably an isocyanate compound, a mixture and reaction product of one or more of polyurethane and urethane prepolymer, a mixture and reaction product of one or more of polyester, polyol and polyether with isocyanate, or a solution or dispersion thereof. The thickness of the anchor coating layer is not particularly limited, but is preferably 0.02 to 0.2 μm after drying, and more preferably 0.04 to 0.1 μm.
[0082] When the gas barrier coating solution (I) or (II) is used, the gas barrier coating layer may be formed by either an in-line pre-coating method in which the gas barrier coating solution is applied during film formation, or a post-coating method in which the gas barrier coating solution is applied after film formation. In addition, the in-line pre-coating method and the post-coating method can be used in combination. The gas barrier coating layer can be applied using an air knife coater, kiss roll coater, metaling bar coater, gravure roll coater, reverse roll coater, dip coater, die coater, etc., or a method in which any of these are combined. These can be performed using known or commercially available devices.
[0083] The thickness of the gas barrier coat layer is not limited, but is usually preferably 0.01 to 3.0 μm, and more preferably 0.02 to 2.0 μm. If the thickness is less than 0.01 μm, sufficient gas barrier properties may not be obtained. On the other hand, if the thickness exceeds 3.0 μm, the film-forming properties are reduced and the appearance of the film is easily impaired.
[0084] An aluminum foil or a gas barrier film including the above-mentioned vapor deposition layer or gas barrier coat layer may be laminated onto the laminate film of the present invention.
[0085] (Printing layer) The printed layer is a layer on which, for example, letters, patterns, etc. are printed. The ink used to form the printed layer is not particularly limited. For example, toluene-containing ink, non-toluene ink, water-based ink, etc. are included. From the environmental point of view, at least one of non-toluene ink, water-based ink, etc. is preferable.
[0086] (adhesive layer) The adhesive layer may be formed using known or commercially available adhesives. Examples of such adhesives include isocyanate-based, polyurethane-based, polyester-based, polyethyleneimine-based, polybutadiene-based, polyolefin-based, and alkyl titanate-based adhesives. Among these, at least one type of adhesive such as an isocyanate-based, polyurethane-based, or polyester-based adhesive is preferred from the viewpoints of adhesion, heat resistance, water resistance, and the like.
[0087] (Base resin layer) Examples of the base resin layer include thermoplastic resin films such as polyester resin films, polyamide resin films, polypropylene resin films, etc. Furthermore, a gas barrier layer, an easy-adhesion layer, etc. may be laminated on the surface of the base resin layer.
[0088] (Sealant resin layer) The sealant resin layer is not particularly limited as long as it has heat sealability, and examples thereof include at least one of low-density polyethylene, linear low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, polypropylene, ionomer resin, etc. In addition, a gas barrier layer formed by aluminum deposition or the like may be laminated on the surface of the sealant resin layer.
[0089] <Packaging materials> The polyester film or laminated film of the present invention can also be used to form a predetermined bag. The shape of the bag is not limited, and examples of the bag include two-sided bags, three-sided bags, three-sided bags with zippers, palm-shaped bags, gusset bags, bottom gusset bags, stand-up bags, etc. For example, a sealant resin layer such as polyolefin and the film of the present invention can be laminated to form a laminated film using a known method such as dry lamination or extrusion lamination, and the sealant resin layers can be heat-sealed to form a packaging bag. Packaging materials (packaging bags, containers, etc.) containing the polyester film of the present invention are not limited in terms of the contents, and can be widely used for packaging foods, medicines, medical devices, cosmetics, chemicals, miscellaneous goods, electronic components, etc. In particular, packaging bags containing the polyester film of the present invention have excellent tear-opening properties, and therefore are suitable for use with foods such as retort curry that are boiled or cooked in a microwave oven, confectionery and pet food that require prevention of deformation when opened and ease of removal of contents, medicines and medical devices that need to be opened immediately to remove contents, etc. EXAMPLES
[0090] The present invention will be specifically explained below with reference to examples, but the present invention is not limited to these.
[0091] The properties of the polyester film were measured by the following methods. (1) Tear propagation resistance (N) A polyurethane adhesive (Takelac A-525S / A-50, two-component type, manufactured by Mitsui Chemicals) was uniformly applied (application amount 4 g / m) to one side of the polyester film obtained in the Examples and Comparative Examples (the side on the gas barrier layer side if a gas barrier layer was laminated). 2 ), dried, and then dry-laminated with a linear low-density polyethylene (LLDPE) film (TUX-FCS 40 μm, manufactured by Mitsui Chemicals Tohcello) or a non-oriented polypropylene (CPP) film (RXC-22 50 μm, manufactured by Mitsui Chemicals Tohcello) on a hot roll at 100°C to obtain laminated films. Using an autograph AG-IS manufactured by Shimadzu Corporation, the tear propagation resistance in the MD of each of the laminated films was measured in accordance with JIS K7128-1 at a pulling speed of 200 mm / min and in a measurement environment of 23° C.×50% RH.
[0092] (2) Tear propagation resistance after hot water treatment (N) The laminated film of polyester film and LLDPE film obtained in (1) above was made into a three-sided bag shape, and a sample was prepared by filling it with pure water. The sample was immersed in pure water heated to 95°C using a boiling bath for 30 minutes for hot water treatment. After 30 minutes, the pure water in the sample was immediately removed from the treatment water, and the laminated film of polyester film and LLDPE film was cut out from the sample, and the tear propagation resistance in the MD of the laminated film was measured using the method described in (1) above.
[0093] (3) Tear propagation resistance after retort treatment (N) The laminated film of polyester film and CPP film obtained in (1) above was made into a three-sided bag shape, and a sample was prepared by filling it with pure water. The sample was retorted at 120°C for 30 minutes using a high-temperature, high-pressure sterilization cooking device (retort cooker). After the retort treatment and cooling treatment for 10 minutes, the pure water in the sample was drained, and the laminated film of polyester film and CPP film was cut out from the sample, and the tear propagation resistance in the MD of the laminated film was measured by the method described in (1) above.
[0094] (4) Crystallization temperature of polyester film Using a PerkinElmer power-compensated differential scanning calorimeter DSC8000, 10 mg of the polyester film obtained in the Examples and Comparative Examples was measured as a sample in accordance with JIS K7121. The measurement was performed under the conditions of increasing the temperature from 25°C to 300°C at a rate of 20°C / min, holding at 300°C for 10 minutes, and then cooling to 100°C at a rate of 40°C / min. The peak top temperature at which crystallization occurred during cooling was taken as the cooling crystallization temperature Tc.
[0095] (5) Film thickness After the film was conditioned for 2 hours in an environment of 23° C. and 50% RH, the thickness was measured at any 10 points using a thickness gauge (HEIDENHAIN-METRO MT1287 manufactured by Heidenhain), and the average value was taken as the film thickness.
[0096] (6) Oxygen permeability Using a Mocon oxygen barrier measuring device (OX-TRAN 2 / 20), the measurement area was 50 cm 2 The oxygen permeability of the polyester film was measured under an atmosphere of 20°C and 65% RH with a nitrogen gas flow rate of 10 cc / min and an oxygen gas flow rate of 20 cc / min. Measurement took 20 minutes per cycle, and the measurement was terminated when the fluctuation rate of the oxygen permeability at intervals of 3 cycles was within 1%.
[0097] The raw materials used in the examples and comparative examples are as follows. <Recycled PET (depolymerized-repolymerized product A-1)> A slurry of terephthalic acid (TPA) and ethylene glycol (EG) (TPA / EG molar ratio = 1 / 1.6) was supplied to an esterification reactor (ES can) and reacted at a temperature of 250°C and a pressure of 50 hPa to obtain ethylene terephthalate oligomer (number average degree of polymerization: 5) with an esterification reaction rate of 95%. 45.0 parts by mass of the obtained ethylene terephthalate oligomer was charged into an ES can, and then 7.0 parts by mass of ethylene glycol was added while the agitator of the ES can was rotating. When the internal temperature of the ES can stopped decreasing, 55.0 parts by mass of recycled PET (pellets of PET scraps generated in the process of manufacturing PET) was added via a rotary valve over a period of about 2 hours. At this time, the molar ratio of total glycol components to total acid components (G / A) was 1.16. Then, the depolymerization reaction was carried out for 1 hour under heat treatment conditions at 270°C. Next, the obtained depolymerization product was pressure-fed to the polycondensation reactor (PC can) through a candle filter with a mesh size of 20 μm that was set between the ES can and the polycondensation reactor, and then 1.0×10 antimony trioxide was added as a polymerization catalyst. -4mol, and titanium dioxide EG slurry was added to give a concentration of 0.20 mass%, and the PC can was decompressed for 1 hour, after which a melt polymerization reaction was carried out at a final pressure of 0.5 hPa and a temperature of 275°C for 4 hours to obtain recycled PET (depolymerized-repolymerized product A-1) (recycle rate 55 mass%, intrinsic viscosity 0.64, carboxyl terminal group concentration 27 equivalents / t, cooling crystallization temperature 170°C, average pressure rise rate 0.28 MPa / h).
[0098] <Recycled PET (depolymerized-repolymerized product A-2)> In the same manner as in A-1, an ethylene terephthalate oligomer (number average degree of polymerization: 5) with an esterification reaction rate of 95% was obtained. 30.0 parts by mass of the obtained ethylene terephthalate oligomer was charged into an ES can, and then 7.0 parts by mass of ethylene glycol was added while the agitator of the ES can was rotating. When the internal temperature of the ES can stopped decreasing, 70.0 parts by mass of recycled PET (pellets of PET scraps generated in the process of manufacturing PET) was added via a rotary valve over a period of about 2 hours. At this time, the molar ratio (G / A) was 1.10. Then, the depolymerization reaction was carried out for 1 hour under heat treatment conditions at 270°C. The resulting depolymerized polymer was then pumped through a 20 μm pore size candle filter placed between the ES can and the PC can into the PC can, after which 1.0×10 antimony trioxide was added as a polymerization catalyst. -4 mol, and one hour after the PC can was decompressed, a melt polymerization reaction was carried out at a final pressure of 0.5 hPa and a temperature of 275°C for 5 hours to obtain recycled PET (depolymerized-repolymerized product A-2) (recycle rate 70 mass%, intrinsic viscosity 0.65, carboxyl end group concentration 38 equivalents / t, cooling crystallization temperature 170°C, average pressure rise rate 0.3 MPa / h).
[0099] <Remelted product> Film scraps generated during the production of PET films were crushed, remelted at 250 to 290°C, and pelletized, then dried to obtain a remelted product (recycle rate 100% by mass, crystallization temperature upon cooling 179°C).
[0100] <Virgin PET> Polyethylene terephthalate resin UT-CBR (crystallization temperature on cooling: 177°C) manufactured by Nippon Ester Co., Ltd. was used.
[0101] <Modified PBT> 194 parts by mass of dimethyl terephthalate, 108 parts by mass of 1,4-butanediol, and 80 ppm of tetrabutyl titanate (a value converted into the mass of titanium metal relative to the polymer) were subjected to an ester exchange reaction for 2.5 hours while heating from 150 ° C. to 210 ° C. 85 parts by mass of the resulting ester exchange reaction product were transferred to a polymerization vessel, 40 ppm of tetrabutyl titanate was added, 15 parts by mass of PTMG having a molecular weight of 1100 was added, and pressure reduction was started, and finally, under a reduced pressure of 1 hPa, the temperature was raised from 210 ° C., and finally, melt polymerization was performed at a temperature of 245 ° C. for 2 hours to obtain a modified PBT with a relative viscosity of 1.62.
[0102] Example 1 4 parts by mass of modified PBT and 96 parts by mass of PET (recycled PET (depolymerized-repolymerized product A-1) / remelted product / virgin PET (mass ratio: 60 / 20 / 20)) were mixed and melt-kneaded in an extruder, fed into a T-die and extruded into a sheet, which was then wound around a metal drum whose temperature was controlled at 20°C, cooled, and wound up to obtain an unstretched film with a thickness of approximately 120 μm. Next, the ends of this unstretched film were held by clips of a tenter-type simultaneous biaxial stretching device, and the film was simultaneously biaxially stretched at a stretch ratio of 3.0 times in the MD and 3.3 times in the TD under the condition of 180°C. Thereafter, the film was subjected to a heat treatment at 215° C. for 4 seconds with a TD relaxation rate of 5%, slowly cooled to room temperature, and subjected to a corona discharge treatment on one side to obtain a polyester film with a recycling rate of 50.9% by mass and a thickness of 12 μm.
[0103] Examples 2 to 9, Comparative Examples 1 to 8 A polyester film having a thickness of 12 μm was obtained in the same manner as in Example 1, except that the content of modified PBT, the content of PET, and the composition were changed as shown in Table 1.
[0104] Example 10 An unstretched film having a thickness of approximately 180 μm was obtained by the same operation as in Example 1, and then the ends of this unstretched film were held with clips of a tenter-type simultaneous biaxial stretching device and simultaneously biaxially stretched at a stretch ratio of 2.5 times in MD and 2.8 times in TD under the condition of 180°C to obtain a polyester film having a thickness of 25 μm.
[0105] Example 11 A polyester film having a recycling rate of 50.9% by mass and a thickness of 12 μm was obtained in the same manner as in Example 1, except that the film was sequentially biaxially stretched at a stretch ratio of 3.0 in MD and 3.0 in TD.
[0106] Example 12 A polyurethane adhesive (Takelac A-525S / A-50, two-component type, manufactured by Mitsui Chemicals, Inc.) was uniformly applied (application amount 4 g / m) to one side of the polyester film obtained in Example 1. 2 ), dried, and then dry-laminated with aluminum foil having a thickness of 7 μm to obtain a polyester film having an aluminum foil laminated thereon as a gas barrier layer. The oxygen permeability of the obtained laminated polyester film was 0.1 ml / (m 2 ·day·MPa).
[0107] Example 13 Silicon oxide was deposited by vacuum deposition on one side of the polyester film obtained in Example 1 to obtain a polyester film laminated with a gas barrier layer having a thickness of 0.05 μm. The oxygen permeability of the obtained laminated polyester film was 5 ml / (m 2 ·day·MPa).
[0108] The configurations and properties of the polyester films obtained in the respective Examples and Comparative Examples are shown in Table 1.
[0109] [Table 1]
[0110] The polyester films of Examples 1 to 13 were made using PET containing recycled PET, and the content of modified PBT in the films was set to a predetermined ratio, so that the temperature-reducing crystallization temperature satisfied the range specified in the present invention. As a result, the tear propagation resistance after hot water treatment and retort treatment was low, and the films had excellent tearability. On the other hand, the polyester films of Comparative Examples 1 to 4 did not exhibit easy tearing properties because they did not contain modified PBT or the content of modified PBT was below the range specified in the present invention. The polyester films of Comparative Examples 5 to 7 had crystallization temperatures exceeding the range specified in the present invention, and therefore tended to have high tear propagation resistance values after hot water treatment and retort treatment. The polyester film of Comparative Example 8 had a modified PBT content exceeding the range specified in the present invention, and therefore tended to have a high tear propagation resistance value after retort treatment.
Claims
1. A polyester film containing polyethylene terephthalate and modified polybutylene terephthalate, the content of modified polybutylene terephthalate in the polyester film being 3 to 18 mass %, and the polyester film exhibiting a crystallization temperature (cooling-down crystallization temperature) of 160°C or lower when heated from 25°C to 300°C at a heating rate of 20°C / min, held at 300°C for 10 minutes, and then cooled at a cooling rate of 40°C / min in differential scanning calorimetry.
2. A method for producing the polyester film according to claim 1, comprising the steps of: (A) A step of obtaining a reaction product by subjecting polyethylene terephthalate to a depolymerization reaction (B) filtering the reaction product and recovering the filtrate. (C) A step of subjecting the filtrate to a polycondensation reaction in the presence of a polymerization catalyst at a temperature of 260° C. or higher and a pressure of 1.0 hPa or lower to obtain recycled polyethylene terephthalate. (D) A step of producing an unstretched film using a raw material containing the recycled polyethylene terephthalate, and then biaxially stretching the unstretched film.
3. A laminated film comprising the polyester film according to claim 1 and a sealant resin layer.
4. 4. The laminated film according to claim 3, wherein the tear propagation resistance is 0.35 N or less.
5. The laminate film according to claim 3 or 4, further comprising a gas barrier layer.
6. A packaging material comprising the polyester film of claim 1.
Citation Information
Patent Citations
Biaxially stretched polyester film, and method for manufacturing the same
JP2013053258A