Liquid crystalline polymer film and method for producing the same, and laminate and multilayer substrate containing liquid crystalline polymer film
A liquid crystal polymer film with crystalline polyimide achieves isotropy and excellent dielectric properties through specific composition and processing, addressing anisotropy and dimensional stability issues in existing methods.
Patent Information
- Application Number
- JP2023045669
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for producing liquid crystal polymer films face challenges in reducing anisotropy, thickness, size, and speed, while also requiring improved dimensional stability and dielectric properties, particularly for use in high-frequency electrical circuit boards.
A liquid crystal polymer film containing a liquid crystal polymer and crystalline polyimide, with specific compositional ratios and processing methods such as die extrusion and stretching, to achieve isotropy and excellent dielectric properties.
The film exhibits superior dimensional stability, isotropy, and dielectric properties, making it suitable for high-frequency electrical circuit boards and other applications.
Smart Images

Figure 2024135132000001 
Figure 2024135132000002 
Figure 2024135132000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid crystal polymer film (particularly a liquid crystal polymer blend film) and a method for producing the same, as well as a laminate and a multilayer substrate containing the liquid crystal polymer film. [Background technology]
[0002] The next generation of communication technology, the 5th generation (5G) mobile communication system, will use higher frequencies and wider bandwidths than ever before. For this reason, substrate films for circuit boards used in 5G mobile communication systems must have low dielectric constants and low dielectric loss tangents (dielectric properties), and various companies are developing them using a variety of materials. One such material is liquid crystal polymer (LCP) film.
[0003] Liquid crystal polymers have a rod-like molecular structure, so they have a strong tendency to be oriented. When liquid crystal polymers are melt-extruded, they tend to be oriented in the flow direction (MD; machine direction) due to shear stress from the die slit and elongational flow. Therefore, liquid crystal polymer films produced by melt extrusion tend to be uniaxially oriented films. Due to the strong orientation of liquid crystal polymers, there was a problem in that the physical properties in the TD (transverse direction) perpendicular to the MD direction were highly anisotropic.
[0004] Several methods have been proposed for producing a film with reduced anisotropy. For example, Patent Document 1 proposes a method of stretching a film (e.g., inflation method). Patent Document 2 proposes a method of obtaining a film without anisotropy by dissolving a liquid crystal polymer in an organic solvent and casting the resulting film. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 5-43664 [Patent Document 2] Patent No. 4742580 Summary of the Invention [Problem to be solved by the invention]
[0006] In the inflation manufacturing method of Patent Document 1, although it is expected to reduce anisotropy to some extent by stretching the film after it is formed, there are still problems with thickening, thickness accuracy, and large-scale / high-speed production. In light of the current situation of a shortage of substrates due to the recent increase in demand for liquid crystal polymer films, improving productivity is extremely important.
[0007] The manufacturing method of Patent Document 2 has the effect of reducing anisotropy by dissolving in an organic solvent, but there are still issues with increasing thickness, size, and speed, and there are concerns about the environmental impact of using organic solvents.
[0008] In the field of electric circuit boards, peeling can occur in high-temperature environments due to the difference in expansion coefficient between the circuit (e.g., copper circuit) and the board, so the board is also required to have good dimensional stability.
[0009] An object of the present invention is to provide a liquid crystal polymer film which is sufficiently superior in dimensional stability, isotropy and dielectric properties.
[0010] Another object of the present invention is to provide a method for producing a liquid crystal polymer film, which can produce a liquid crystal polymer film having sufficiently excellent dimensional stability, isotropy, and dielectric properties using a simple method such as a die extrusion film production method in which a film is produced by extrusion through a die. [Means for solving the problem]
[0011] That is, the gist of the present invention is as follows. <1> A liquid crystal polymer film containing a liquid crystal polymer (A) and a crystalline polyimide (B), The degree of orientation of the liquid crystal polymer (A) is 71% or less, the content of the crystalline polyimide (B) is 1 to 50% by mass based on the total mass of the liquid crystal polymer, The liquid crystal polymer film, wherein the crystalline polyimide (B) has an end / edge strength ratio of 1 or less. <2> The ratio of the thermal expansion coefficient in both MD and TD of the film is 0.5 or more and less than 1.5; <1> The liquid crystal polymer film according to claim 1. <3> The liquid crystal polymer (A) contains, as a monomer component, an aromatic hydroxycarboxylic acid, and further contains or does not contain an aromatic dicarboxylic acid and an aliphatic diol. <1> or <2> The liquid crystal polymer film according to claim 1. <4> The content of the aromatic hydroxycarboxylic acid is 50 mol % or more based on the total amount of monomers constituting the liquid crystal polymer (A), The content of the aromatic dicarboxylic acid is 25 mol% or less based on the total amount of monomers constituting the liquid crystal polymer (A), The content of the aliphatic diol is 25 mol% or less based on the total amount of monomers constituting the liquid crystal polymer (A). <3> The liquid crystal polymer film according to claim 1. <5> The liquid crystal polymer (A) is a copolymer having 6-hydroxy-2-naphthoic acid as a copolymerization component. <1> ~ <4> 2. The liquid crystal polymer film according to claim 1 . <6> The liquid crystal polymer (A) is a copolymer of 6-hydroxy-2-naphthoic acid and 4-hydroxybenzoic acid or a copolymer of 6-hydroxy-2-naphthoic acid, terephthalic acid, and ethylene glycol. <1> ~ <5> 2. The liquid crystal polymer film according to claim 1 . <7> The melting point of the crystalline polyimide (B) measured by differential scanning calorimetry is 270 to 360°C. <1> ~ <6> 2. The liquid crystal polymer film according to claim 1 . <8> The content of the crystalline polyimide (B) is 2 to 35 mass %. <1> ~ <7> 2. The liquid crystal polymer film according to claim 1 . <9> The content of the crystalline polyimide (B) is 2 to 20 mass %. <1> ~ <8> 2. The liquid crystal polymer film according to claim 1 . <10> <1> ~ <9> A method for producing the liquid crystal polymer film according to any one of the above, blending a liquid crystal polymer (A) and a crystalline polyimide (B); A die extrusion film-forming step of melting and kneading the blend mixture and then extruding it through a die to obtain an unstretched film; and A method for producing a liquid crystal polymer film, comprising a stretching step of stretching the unstretched film so as to achieve a degree of orientation of the liquid crystal polymer (A) and an end / edge strength ratio of the crystalline polyimide (B) to obtain a liquid crystal polymer film. <11> The die is a flat die. <10> 2. A method for producing the liquid crystal polymer film according to claim 1 . <12> <1> ~ <9> 2. A laminate having a metal layer on one or both sides of the liquid crystal polymer film according to claim 1. <13> The metal layer is a metal foil; <12> The laminate according to claim 1. <14> The metal layer is formed by sputtering, vapor deposition or plating. <12> The laminate according to claim 1. <15> <12> A multilayer substrate comprising the laminate according to claim 1. <16> The multilayer substrate is an electric circuit substrate or a high-frequency electric circuit substrate; <12> The multilayer substrate according to claim 1 . Effect of the Invention
[0012] According to the present invention, it is possible to provide a liquid crystal polymer film having sufficiently excellent dimensional stability, isotropy and dielectric properties, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] [Liquid crystal polymer film] The liquid crystal polymer film of the present invention (hereinafter sometimes simply referred to as "film") contains a liquid crystal polymer (A) and a crystalline polyimide (B) (hereinafter sometimes referred to as "TPI (B)").
[0014] In the present invention, the liquid crystal polymer (A) refers to a polymer that exhibits a liquid crystal state or has the property of optically birefringence when melted, specifically, a thermotropic liquid crystal polymer that exhibits liquid crystallinity when melted. The liquid crystal polymer (A) is classified into types I, II, and III depending on the heat distortion temperature, and may be any type. The chemical composition of the liquid crystal polymer (A) is not particularly limited as long as it is a thermoplastic liquid crystal polymer that can be melt-formed. Examples of the thermoplastic liquid crystal polymer include thermoplastic liquid crystal polyesters and thermoplastic liquid crystal polyester amides, and among them, thermoplastic liquid crystal polyesters are preferred because they are easily melt-formed.
[0015] The thermoplastic liquid crystal polyester is composed of repeating structural units derived from one or more compounds selected from the group consisting of aromatic diols, aromatic dicarboxylic acids, aromatic hydroxycarboxylic acids, etc. In the present invention, the thermoplastic liquid crystal polyester may contain other components such as aliphatic dicarboxylic acids and aliphatic diols in order to facilitate melt molding.
[0016] Examples of aromatic diols include hydroquinone, resorcinol, 4,4'-dihydroxydiphenyl, 2,6-naphthalenediol, 4,4'-dihydroxydiphenyl ether, bis(4-hydroxyphenoxy)ethane, 3,3'-dihydroxydiphenyl, 3,3'-dihydroxydiphenyl ether, 1,6-naphthalenediol, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)methane, methylhydroquinone, t-butylhydroquinone, phenylhydroquinone, phenoxyhydroquinone, and 4-methylresorcinolhydroquinone.
[0017] From the viewpoints of further improving dimensional stability, isotropy, and dielectric properties, as well as liquid crystal properties and versatility, the aromatic diol is preferably one or more compounds selected from the group consisting of the following group Ia, and is preferably one or more compounds selected from the group consisting of the following group Ib. Group Ia: hydroquinone, resorcinol, 4,4'-dihydroxydiphenyl, 2,6-naphthalenediol, 4,4'-dihydroxydiphenyl ether; Group Ib: hydroquinone, 2,6-naphthalenediol.
[0018] Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,6-naphthalenedicarboxylic acid, diphenylether-4,4'-dicarboxylic acid, diphenoxyethane-4,4'-dicarboxylic acid, diphenoxybutane-4,4'-dicarboxylic acid, diphenylethane-4,4'-dicarboxylic acid, diphenylether-3,3'-dicarboxylic acid, diphenoxyether-3,3'-dicarboxylic acid, and diphenylethane-3,3'-dicarboxylic acid.
[0019] From the viewpoints of further improving dimensional stability, isotropy, and dielectric properties, and of expressing liquid crystal properties, the aromatic dicarboxylic acid is preferably one or more compounds selected from the group consisting of Group IIa below, and more preferably one or more compounds selected from the group consisting of Group IIb below. Group IIa: terephthalic acid, 4,4'-diphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, diphenylether-4,4'-dicarboxylic acid, diphenoxyethane-4,4'-dicarboxylic acid, diphenylethane-4,4'-dicarboxylic acid; Group IIb: terephthalic acid, 4,4'-diphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid.
[0020] Examples of aromatic hydroxycarboxylic acids include 4-hydroxybenzoic acid, 3-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 6-hydroxy-1-naphthoic acid, 3-methyl-4-hydroxybenzoic acid, and 3-methoxy-4-hydroxybenzoic acid.
[0021] From the viewpoints of further improving dimensional stability, isotropy, and dielectric properties, and of expressing liquid crystal properties, the aromatic hydroxycarboxylic acid is preferably one or more compounds selected from the group consisting of Group IIIa below, and more preferably one or more compounds selected from the group consisting of Group IIIb below. Group IIIa: 4-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 3-methyl-4-hydroxybenzoic acid, 3-methoxy-4-hydroxybenzoic acid; Group IIIb: 4-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid.
[0022] Examples of aliphatic diols include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2-methyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 2-amino-2-ethyl-1,3-propanediol, 2-amino-2-methyl-1,3-propanediol, 2-ethyl-2-methyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, polyethylene glycol, and polypropylene glycol.
[0023] From the viewpoints of further improving dimensional stability, isotropy, and dielectric properties, as well as versatility and plant-derived materials, the aliphatic diol is preferably one or more compounds selected from the group consisting of Group IVa below, and more preferably one or more compounds selected from the group consisting of Group IVb below. Group IVa: ethylene glycol, 1,3-propanediol, 1,4-butanediol; Group IVb: ethylene glycol.
[0024] Examples of aliphatic dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, hydrogenated dimer acid, fumaric acid, maleic acid, itaconic acid, citraconic acid, and dimer acid.
[0025] From the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, as well as improving versatility, the aliphatic dicarboxylic acid is preferably one or more compounds selected from the group consisting of the following group Va, and preferably one or more compounds selected from the group consisting of the following group Vb. Group Va: oxalic acid, malonic acid, succinic acid; Group Vb: oxalic acid.
[0026] From the viewpoint of further improving dimensional stability, isotropy and dielectric properties, and improving moldability, the liquid crystal polymer (A) preferably contains an aromatic hydroxycarboxylic acid as a monomer component, and may further contain an aromatic dicarboxylic acid and an aliphatic diol. In detail, such a preferred liquid crystal polymer (A) contains an aromatic hydroxycarboxylic acid, and may or may not further contain an aromatic dicarboxylic acid and an aliphatic diol. The contents of the aromatic hydroxycarboxylic acid, aromatic dicarboxylic acid and aliphatic diol in such a preferred liquid crystal polymer (A) are as follows. Aromatic hydroxycarboxylic acid: preferably 50 mol % or more (i.e., 50 to 100 mol %), more preferably 70 mol % or more (i.e., 70 to 100 mol %), further preferably 80 mol % or more (80 to 100 mol %), particularly preferably 90 mol % or more (i.e., 90 to 100 mol %), and most preferably 100 mol %; Aromatic dicarboxylic acid: preferably 25 mol % or less (i.e., 0 to 25 mol %), more preferably 15 mol % or less (i.e., 0 to 15 mol %), even more preferably 10 mol % or less (i.e., 0 to 10 mol %), particularly preferably 5 mol % or less (i.e., 0 to 5 mol %), and most preferably 0 mol %; Aliphatic diol: preferably 25 mol % or less (i.e., 0 to 25 mol %), more preferably 15 mol % or less (i.e., 0 to 15 mol %), even more preferably 10 mol % or less (i.e., 0 to 10 mol %), particularly preferably 5 mol % or less (i.e., 0 to 5 mol %), and most preferably 0 mol %. The content of the compound as a monomer component is expressed as a percentage relative to the total amount of monomers constituting the liquid crystal polymer (A). A content of "0 mol %" means that the liquid crystal polymer (A) does not contain the compound.
[0027] When the liquid crystal polymer (A) contains an aromatic hydroxycarboxylic acid, an aromatic dicarboxylic acid and an aliphatic diol as monomer components, the monomer sequence is not particularly limited, and the liquid crystal polymer (A) may be a random type polyester or a block type polyester. In this case, the liquid crystal polymer (A) is preferably a block type polyester from the viewpoint of further improving dimensional stability, isotropy and dielectric properties. The random type polyester is a polyester in which an aromatic hydroxycarboxylic acid, an aromatic dicarboxylic acid and an aliphatic diol are arranged and polymerized in any order. The block type polyester is a block type polyester containing an ester oligomer portion (block portion) of an aromatic dicarboxylic acid and an aliphatic diol, and an ester oligomer portion (block portion) of an aromatic hydroxycarboxylic acid.
[0028] As the liquid crystal polymer (A), from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, a liquid crystal polymer that is a copolymer (hereinafter, sometimes referred to as copolymer (a1)) having 6-hydroxy-2-naphthoic acid as a copolymerization component is preferable. Among them, from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties and expressing liquid crystal properties, a copolymer of 6-hydroxy-2-naphthoic acid and 4-hydroxybenzoic acid (hereinafter, sometimes referred to as copolymer (a1-1)) or a copolymer of 6-hydroxy-2-naphthoic acid, terephthalic acid, and ethylene glycol (hereinafter, sometimes referred to as copolymer (a1-2)) is more preferable.
[0029] The copolymer (a1) may contain, as a monomer component, one or more compounds selected from the group consisting of the aromatic diols, aromatic dicarboxylic acids, aromatic hydroxycarboxylic acids, aliphatic dicarboxylic acids, and aliphatic diols, in addition to 6-hydroxy-2-naphthoic acid. From the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, the copolymer (a1) preferably contains, as a monomer component, one or more compounds selected from the group consisting of aromatic hydroxycarboxylic acids (other than 6-hydroxy-2-naphthoic acid), aromatic dicarboxylic acids, and aliphatic diols.
[0030] In the copolymer (a1), the content of 6-hydroxy-2-naphthoic acid is preferably 1 to 100 mol%, more preferably 10 to 95 mol%, further preferably 20 to 90 mol%, particularly preferably 20 to 50 mol%, and most preferably 20 to 40 mol%, from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties. At this time, the preferred contents of aromatic hydroxycarboxylic acid (other than 6-hydroxy-2-naphthoic acid), aromatic dicarboxylic acid, and aliphatic diol are as follows. Aromatic hydroxycarboxylic acid (other than 6-hydroxy-2-naphthoic acid): preferably 90 mol % or less (i.e., from 0 to 90 mol %), more preferably 20 to 90 mol %, further preferably 40 to 90 mol %, particularly preferably 60 to 90 mol %, and most preferably 60 to 80 mol %; Aromatic dicarboxylic acid: preferably 25 mol % or less (i.e., 0 to 25 mol %), more preferably 15 mol % or less (i.e., 0 to 15 mol %), even more preferably 10 mol % or less (i.e., 0 to 10 mol %), particularly preferably 5 mol % or less (i.e., 0 to 5 mol %), and most preferably 0 mol %; Aliphatic diol: preferably 25 mol % or less (i.e., 0 to 25 mol %), more preferably 15 mol % or less (i.e., 0 to 15 mol %), even more preferably 10 mol % or less (i.e., 0 to 10 mol %), particularly preferably 5 mol % or less (i.e., 0 to 5 mol %), and most preferably 0 mol %. The content of the compound as a monomer component is expressed as a percentage relative to the total amount of monomers constituting the copolymer (a1). A content of "0 mol %" means that the copolymer (a1) does not contain the compound.
[0031] In the copolymer (a1-1), the content of 6-hydroxy-2-naphthoic acid is preferably 1 to 99 mol%, more preferably 10 to 95 mol%, even more preferably 20 to 90 mol%, particularly preferably 20 to 80 mol%, sufficiently preferably 20 to 50 mol%, and most preferably 20 to 40 mol%, from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties. In the copolymer (a1-1), the content of 4-hydroxybenzoic acid is preferably 1 to 99 mol%, more preferably 5 to 90 mol%, even more preferably 10 to 80 mol%, particularly preferably 20 to 80 mol%, sufficiently preferably 50 to 80 mol%, and most preferably 60 to 80 mol%, from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties.
[0032] The copolymer (a1-1) may be a random type polyester or a block type polyester, and is preferably a random type polyester from the viewpoint of further improving the dielectric properties and heat resistance.
[0033] In the copolymer (a1-2), the content of 6-hydroxy-2-naphthoic acid is preferably 10 to 98 mol%, more preferably 30 to 95 mol%, even more preferably 50 to 95 mol%, particularly preferably 60 to 90 mol%, and most preferably 70 to 90 mol%, from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties. In the copolymer (a1-2), the content of terephthalic acid is preferably 1 to 30 mol %, more preferably 2 to 25 mol %, even more preferably 5 to 20 mol %, particularly preferably 8 to 15 mol %, and most preferably 10 to 15 mol %, from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties. In the copolymer (a1-2), the content of ethylene glycol is preferably 1 to 30 mol %, more preferably 2 to 25 mol %, even more preferably 5 to 20 mol %, particularly preferably 8 to 15 mol %, and most preferably 10 to 15 mol %, from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties.
[0034] The copolymer (a1-2) may be a random type polyester or a block type polyester, and is preferably a block type polyester from the viewpoint of further improving the dielectric properties and heat resistance.
[0035] The melting point of the liquid crystal polymer (A) is not particularly limited, and from the viewpoint of further improving dimensional stability, isotropy and dielectric properties, it is preferably 220 to 360°C, more preferably 270 to 340°C, and even more preferably 270 to 320°C.
[0036] In this specification, the melting point is a temperature determined from the crystal melting peak when measured using a differential scanning calorimeter (DSC-7 model, manufactured by PerkinElmer) at a heating rate of 20° C. / min.
[0037] The melt flow rate (MFR) of the liquid crystal polymer (A) is not particularly limited, and from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, it is preferably 0.5 to 300 g / 10 min, more preferably 2 to 100 g / 10 min, and still more preferably 20 to 100 g / 10 min.
[0038] In this specification, the MFR of the liquid crystal polymer (A) is a value measured at 350° C. under a load of 2.16 kgf in accordance with JIS K 7210.
[0039] The liquid crystal polymer (A) can be produced by polymerizing a specific monomer component by a known method, or can be obtained as a commercial product. When producing a block-type polyester as the liquid crystal polymer (A), the following method can be adopted. For example, first, a monomer component constituting a specific block portion is polymerized in advance to obtain an oligomer. Next, the obtained oligomer is mixed with a monomer component constituting another block portion, and further polymerized.
[0040] Specific examples of commercially available liquid crystal polymers (A) include "LAPEROS" manufactured by Polyplastics, "VECTRA" manufactured by Celanese, "UENO LCP" manufactured by Ueno Pharmaceuticals, "Sumika Super LCP" manufactured by Sumitomo Chemical, "ZYDAR" manufactured by ENEOS, "Sciberas" manufactured by Toray, and "RODRUN" manufactured by Unitika Ltd.
[0041] The content of the liquid crystal polymer (A) is not particularly limited, and from the viewpoint of further improving dimensional stability, isotropy and dielectric properties and improving extrudability, it is preferably 40 to 99 mass%, more preferably 50 to 99 mass%, even more preferably 60 to 98 mass%, particularly preferably 65 to 98 mass%, sufficiently preferably 80 to 98 mass%, and most preferably 85 to 97 mass%, based on the total mass of the liquid crystal polymer film.
[0042] The film of the present invention must contain a crystalline polyimide (B). By stretching a melt-extruded sheet containing a liquid crystal polymer (A) and a predetermined amount of crystalline polyimide (B), the dimensional stability, isotropy, and dielectric properties of the film can be controlled.
[0043] The crystalline polyimide (B) is a polyimide having a heat value of the crystallization heat peak (hereinafter, simply referred to as "crystallization heat value") of 5.0 J / g or more, preferably 10.0 J / g or more, more preferably 20.0 J / g or more, observed when melted and cooled at a temperature drop rate of 10°C / min using a differential scanning calorimeter. The upper limit of the crystallization heat value is not particularly limited, but is usually 45.0 J / g or less. On the other hand, the crystallization heat value of an amorphous polyimide resin is less than 5.0 J / g, particularly less than 1.0 J / g.
[0044] The crystalline polyimide (B) contains, for example, a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2).
[0045] [ka]
[0046] In formula (1), R1 is a residue resulting from an imidization reaction of a diamine compound, and is a divalent group containing at least one alicyclic hydrocarbon structure and having 6 to 22 carbon atoms. Here, the alicyclic hydrocarbon structure means a ring derived from an alicyclic hydrocarbon compound, and the alicyclic hydrocarbon compound may be saturated or unsaturated, and may be monocyclic or polycyclic. Examples of the alicyclic hydrocarbon structure include, but are not limited to, a cycloalkane ring such as a cyclohexane ring, a cycloalkene ring such as a cyclohexene ring, a bicycloalkane ring such as a norbornane ring, and a bicycloalkene ring such as norbornene. Among these, from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, a cycloalkane ring is preferred, a cycloalkane ring having 4 to 7 carbon atoms is more preferred, and a cyclohexane ring is even more preferred. R1 has 6 to 22 carbon atoms, and from the viewpoint of further improving dimensional stability, isotropy and dielectric properties, it preferably has 6 to 17 carbon atoms, and more preferably 8 to 17 carbon atoms. R1 contains at least one alicyclic hydrocarbon structure, and from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, it contains preferably 1 to 3, and more preferably 1, alicyclic hydrocarbon structure.
[0047] R1 is preferably a divalent group represented by the following formula (R1-1) or (R1-2).
[0048] [ka]
[0049] (In formula (R1-1), m11 and m12 each independently represent an integer of 0 to 2, preferably 0 or 1. In formula (R1-2), m13 to m15 each independently represent an integer of 0 to 2, preferably 0 or 1.)
[0050] From the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, R1 is particularly preferably a divalent group represented by the following formula (R1-3).
[0051] [ka]
[0052] In the divalent group represented by the above formula (R1-3), the positional relationship of the two methylene groups to the cyclohexane ring may be either cis or trans, and the ratio of cis to trans may be any value.
[0053] In formula (1), X1 is a residue resulting from an imidization reaction of a tetracarboxylic acid compound, and is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. The aromatic ring may be a single ring or a condensed ring, and examples thereof include a benzene ring, a naphthalene ring, an anthracene ring, and a tetracene ring, but are not limited thereto. Among these, from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred. X1 has 6 to 22 carbon atoms, and from the viewpoint of further improving dimensional stability, isotropy and dielectric properties, it preferably has 6 to 18 carbon atoms, and more preferably has 6 to 10 carbon atoms. X1 contains at least one aromatic ring, and from the viewpoint of further improving dimensional stability, isotropy and dielectric properties, it contains preferably 1 to 3 aromatic rings, and more preferably 1 aromatic ring.
[0054] X1 is preferably a tetravalent group represented by any one of the following formulas (X-1) to (X-4).
[0055] [ka]
[0056] (In formulas (X1-1) to (X1-4), R 11 ~R 18 are each independently an alkyl group having 1 to 4 carbon atoms. p11 to p13 are each independently an integer of 0 to 2, preferably 0. p14, p15, p16 and p18 are each independently an integer of 0 to 3, preferably 0. p17 is an integer of 0 to 4, preferably 0. L 11 ~L 13 are each independently a single bond, an ether group, a carbonyl group, or an alkylene group having 1 to 4 carbon atoms. Since X1 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring, R 12 , R 13 , p12 and p13 are selected so that the tetravalent group represented by formula (X-2) has 10 to 22 carbon atoms. Similarly, L11 and R in formula (X-3) 14 , R 15 , p14 and p15 are selected so that the number of carbon atoms of the tetravalent group represented by formula (X-3) is in the range of 12 to 22, and L12, L13, and R 16 , R 17 , R 18 , p16, p17, and p18 are selected so that the tetravalent group represented by formula (X-4) has 18 to 22 carbon atoms.
[0057] From the viewpoint of further improving the dimensional stability, isotropy, and dielectric properties, X1 is particularly preferably a tetravalent group represented by the following formula (X-5) or (X-6).
[0058] [ka]
[0059] In formula (2), R2 is a residue resulting from an imidization reaction of a diamine compound and is a divalent chain aliphatic group having 5 to 16 carbon atoms, preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms. Here, the chain aliphatic group means a group derived from a chain aliphatic compound, and the chain aliphatic compound may be saturated or unsaturated, linear or branched, and may contain a heteroatom such as an oxygen atom. From the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, R2 is preferably an alkylene group having 5 to 16 carbon atoms, more preferably an alkylene group having 6 to 14 carbon atoms, still more preferably an alkylene group having 7 to 12 carbon atoms, and among these, preferably an alkylene group having 8 to 10 carbon atoms. The alkylene group may be a linear alkylene group or a branched alkylene group, but is preferably a linear alkylene group. From the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, R2 is preferably at least one selected from the group consisting of an octamethylene group and a decamethylene group, and particularly preferably an octamethylene group.
[0060] Another preferred embodiment of R2 is a divalent chain aliphatic group containing an ether group and having 5 to 16 carbon atoms. The number of carbon atoms is preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10. Among these, a divalent group represented by the following formula (R2-1) or (R2-2) is preferred.
[0061] [ka]
[0062] (In formula (R2-1), m21 and m22 each independently represent an integer of 1 to 15, preferably 1 to 13, more preferably 1 to 11, and even more preferably 1 to 9. In formula (R2-2), m23 to m25 each independently represent an integer of 1 to 14, preferably 1 to 12, more preferably 1 to 10, and even more preferably 1 to 8.) Since R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms), m21 and m22 in formula (R2-1) are selected so that the carbon number of the divalent group represented by formula (R2-1) is in the range of 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms). In other words, m21 + m22 is 5 to 16 (preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10). Similarly, m23 to m25 in formula (R2-2) are selected so that the carbon number of the divalent group represented by formula (R2-2) is in the range of 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms). In other words, m23 + m24 + m25 is 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms).
[0063] In formula (2), X2 is a residue resulting from an imidization reaction of a tetracarboxylic acid compound, and is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. It is defined similarly to X1 in formula (1), and preferred embodiments are also similar.
[0064] In the crystalline polyimide (B), the content ratio of the repeating structural unit of formula (1) to the total of the repeating structural units of formula (1) and formula (2) is usually 20 to 70 mol %, and from the viewpoint of further improving the dimensional stability, isotropy and dielectric properties, it is preferably 20 to 60 mol %, more preferably 20 to 50 mol %, even more preferably 25 to 45 mol %, and particularly preferably 30 to 40 mol %.
[0065] The content ratio of the repeating structural unit of formula (1) and the repeating structural unit of formula (2) can be measured by NMR.
[0066] The total content ratio of the repeating structural units of formula (1) and the repeating structural units of formula (2) to all repeating structural units constituting the crystalline polyimide (B) is, from the viewpoint of further improving dimensional stability, isotropy and dielectric properties, preferably 50 to 100 mol %, more preferably 75 to 100 mol %, even more preferably 80 to 100 mol %, particularly preferably 85 to 100 mol %, sufficiently preferably 90 to 100 mol %, and even more preferably 100 mol %.
[0067] The crystalline polyimide (B) may further contain a repeating unit of the following formula (3). In this case, the content ratio of the repeating unit of the formula (3) to the total of the repeating unit of the formula (1) and the repeating unit of the formula (2) is preferably 25 mol% or less. On the other hand, the lower limit is not particularly limited, and it is sufficient that it is more than 0 mol%. From the viewpoint of improving heat resistance, the content ratio is preferably 5 mol % or more, more preferably 10 mol % or more, while from the viewpoint of maintaining crystallinity, the content ratio is preferably 20 mol % or less, more preferably 15 mol % or less.
[0068] [ka]
[0069] In formula (3), R3 is a residue resulting from an imidization reaction of a diamine compound, and is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. The aromatic ring may be a single ring or a condensed ring, and examples thereof include a benzene ring, a naphthalene ring, an anthracene ring, and a tetracene ring, but are not limited thereto. Among these, from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred. R3 has 6 to 22 carbon atoms, and preferably 6 to 18 carbon atoms. R3 contains at least one aromatic ring, and preferably contains 1 to 3 aromatic rings. In addition, a monovalent or divalent electron-withdrawing group may be bonded to the aromatic ring. Examples of the monovalent electron-withdrawing group include a nitro group, a cyano group, a p-toluenesulfonyl group, a halogen, a halogenated alkyl group, a phenyl group, and an acyl group. Examples of the divalent electron-withdrawing group include a halogenated alkylene group such as a fluorinated alkylene group (e.g., -C(CF3)2-, -(CF2)p- (wherein p is an integer of 1 to 10)), -CO-, -SO2-, -SO-, -CONH-, -COO-, and the like.
[0070] R3 is preferably a divalent group represented by the following formula (R3-1) or (R3-2).
[0071] [ka]
[0072] (In the formula, m31 and m32 each independently represent an integer of 0 to 2, preferably 0 or 1. m33 and m34 each independently represent an integer of 0 to 2, preferably 0 or 1. R 21 , R 22 , and R 23 are each independently an alkyl group having 1 to 4 carbon atoms, an alkenyl group having 2 to 4 carbon atoms, or an alkynyl group having 2 to 4 carbon atoms. p21, p22, and p23 are integers of 0 to 4, and preferably 0. L21 is a single bond, an ether group, a carbonyl group, or an alkylene group having 1 to 4 carbon atoms. In addition, since R3 is a divalent group having 6 to 22 carbon atoms containing at least one aromatic ring, m31, m32, and R 21 and p21 is selected so that the divalent group represented by formula (R3-1) has 6 to 22 carbon atoms. Similarly, L21, m33, m34, and R in formula (R3-2) 22 , R 23, p22 and p23 are selected so that the divalent group represented by formula (R3-2) has 12 to 22 carbon atoms.
[0073] In formula (3), X3 is a residue resulting from an imidization reaction of a tetracarboxylic acid compound, and is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. It is defined similarly to X1 in formula (1), and preferred embodiments are also similar.
[0074] The crystalline polyimide (B) may further contain a repeating unit represented by the following formula (4).
[0075] [ka]
[0076] In formula (4), R4 is a divalent group containing -SO2- or Si(Rx)(Ry)O-, and Rx and Ry each independently represent a chain aliphatic group having 1 to 3 carbon atoms or a phenyl group. X4 is a residue resulting from an imidization reaction of a tetracarboxylic acid compound, and is a tetravalent group having 6 to 22 carbon atoms containing at least one aromatic ring, and is defined the same as X1 in formula (1), and preferred embodiments are also the same.
[0077] The terminal structure of the crystalline polyimide (B) is not particularly limited, but it is preferable that the terminal has a chain aliphatic group having 5 to 14 carbon atoms. The chain aliphatic group may be saturated or unsaturated, and may be linear or branched. When the crystalline polyimide (B) has the specific group at the terminal, a resin composition having excellent heat aging resistance can be obtained.
[0078] Examples of the saturated chain aliphatic group having 5 to 14 carbon atoms include an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, a lauryl group, an n-tridecyl group, an n-tetradecyl group, an isopentyl group, a neopentyl group, a 2-methylpentyl group, a 2-methylhexyl group, a 2-ethylpentyl group, a 3-ethylpentyl group, an isooctyl group, a 2-ethylhexyl group, a 3-ethylhexyl group, an isononyl group, a 2-ethyloctyl group, an isodecyl group, an isododecyl group, an isotridecyl group, and an isotetradecyl group. Examples of the unsaturated chain aliphatic group having 5 to 14 carbon atoms include a 1-pentenyl group, a 2-pentenyl group, a 1-hexenyl group, a 2-hexenyl group, a 1-heptenyl group, a 2-heptenyl group, a 1-octenyl group, a 2-octenyl group, a nonenyl group, a decenyl group, a dodecenyl group, a tridecenyl group, and a tetradecenyl group.
[0079] Among them, from the viewpoint of further improving dimensional stability, isotropy and dielectric properties, the chain aliphatic group is preferably a saturated chain aliphatic group, and more preferably a saturated linear chain aliphatic group. From the viewpoint of further improving dimensional stability, isotropy and dielectric properties, the chain aliphatic group preferably has 6 or more carbon atoms, more preferably 7 or more carbon atoms, even more preferably 8 or more carbon atoms, and preferably has 12 or less carbon atoms, more preferably 10 or less carbon atoms, and even more preferably 9 or less carbon atoms. The chain aliphatic group may be of only one type, or of two or more types. The chain aliphatic group is particularly preferably at least one selected from the group consisting of an n-octyl group, an isooctyl group, a 2-ethylhexyl group, an n-nonyl group, an isononyl group, an n-decyl group, and an isodecyl group, further preferably at least one selected from the group consisting of an n-octyl group, an isooctyl group, a 2-ethylhexyl group, an n-nonyl group, and an isononyl group, and most preferably at least one selected from the group consisting of an n-octyl group, an isooctyl group, and a 2-ethylhexyl group.
[0080] From the viewpoint of further improving dimensional stability, isotropy and dielectric properties, the crystalline polyimide (B) preferably has only chain aliphatic groups having 5 to 14 carbon atoms at its terminals in addition to terminal amino groups and terminal carboxy groups. When it has groups other than the above at its terminals, the content thereof is preferably 10 mol % or less, more preferably 5 mol % or less, based on the chain aliphatic groups having 5 to 14 carbon atoms.
[0081] From the viewpoint of further improving dimensional stability, isotropy and dielectric properties, the content of the chain aliphatic group having 5 to 14 carbon atoms in the crystalline polyimide (B) is preferably 0.01 mol% or more, more preferably 0.1 mol% or more, and even more preferably 0.2 mol% or more, based on 100 mol% of the total of all repeating units constituting the crystalline polyimide (B). In addition, in order to ensure a sufficient molecular weight and obtain good mechanical properties, the content of the chain aliphatic group having 5 to 14 carbon atoms in the crystalline polyimide (B) is preferably 10 mol% or less, more preferably 6 mol% or less, even more preferably 3.5 mol% or less, even more preferably 2.0 mol% or less, and even more preferably 1.2 mol% or less, based on 100 mol% of the total of all repeating units constituting the crystalline polyimide (B). The content of the chain aliphatic group having 5 to 14 carbon atoms in the crystalline polyimide (B) can be determined by depolymerizing the crystalline polyimide (B).
[0082] From the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, the crystalline polyimide (B) preferably has a melting point of 360° C. or less. From the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, the melting point of the crystalline polyimide (B) is more preferably 270° C. or more, and even more preferably 290° C. or more, and from the viewpoint of achieving high moldability, it is preferably 345° C. or less, more preferably 340° C. or less, and even more preferably 335° C. or less.
[0083] In this specification, the melting point of a polymer is determined from the crystal melting peak measured at a heating rate of 20° C. / min using a differential scanning calorimeter (DSC-7 model, manufactured by PerkinElmer).
[0084] The logarithmic viscosity of a 5% by mass solution of the crystalline polyimide (B) in concentrated sulfuric acid at 30°C is preferably in the range of 0.2 to 2.0 dL / g, more preferably 0.3 to 1.8 dL / g. If the logarithmic viscosity is 0.2 dL / g or more, sufficient mechanical strength is obtained when the resulting resin composition is molded into a molded article, and if it is 2.0 dL / g or less, moldability and handleability are good. The logarithmic viscosity μ is calculated from the following formula by measuring the flow time of concentrated sulfuric acid and the above polyimide resin solution at 30°C using a Cannon-Fenske viscometer. μ=ln(ts / t0) / C t0: Time for concentrated sulfuric acid to flow ts: Flow time of polyimide resin solution C: 0.5 (g / dL)
[0085] From the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, the weight average molecular weight Mw of the crystalline polyimide (B) is preferably in the range of 10,000 to 150,000, more preferably 15,000 to 100,000, even more preferably 20,000 to 80,000, still more preferably 30,000 to 70,000, and even more preferably 35,000 to 65,000.
[0086] The weight average molecular weight Mw of the crystalline polyimide (B) can be measured by gel permeation chromatography (GPC) using polymethyl methacrylate (PMMA) as a standard sample.
[0087] The content of the crystalline polyimide (B) is 1 to 50% by mass relative to the total mass of the liquid crystal polymer film, and is not particularly limited. From the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, it is preferably 2 to 40% by mass, more preferably 2 to 35% by mass, even more preferably 2 to 20% by mass, and particularly preferably 3 to 15% by mass. If the content of the crystalline polyimide (B) is less than 1% by mass, the melt-extruded sheet is likely to break when stretched. Even if it can be stretched without breaking, the degree of orientation of the film increases, and the isotropy becomes insufficient. On the other hand, if the content of the crystalline polyimide (B) exceeds 50% by mass, the dimensional stability decreases, and the linear expansion coefficient required for a circuit board increases, making it impossible to use it as a circuit board.
[0088] The film of the present invention can obtain the film of the present invention that exhibits the effects of the present invention even if a polymer other than the liquid crystal polymer (A) and the crystalline polyimide (B) (hereinafter, simply referred to as "other polymer") is added in an amount of 25 mass% or less based on the total mass of the liquid crystal polymer film. The other polymer is a polymer that is neither the liquid crystal polymer (A) nor the crystalline polyimide (B), and may be, for example, one or more polymers selected from the group consisting of polyethersulfone, polyetherimide, polyetheretherketone, polyarylate, and polyphenylene sulfide. From the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, polyarylate is preferred.
[0089] Polyarylate is a polyester containing an aromatic dicarboxylic acid and a bisphenol-based diol as monomer components. Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, phthalic acid, chlorophthalic acid, nitrophthalic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, methylterephthalic acid, 4,4'-biphenyldicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-diphenylmethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 4,4'-diphenylisopropylidenedicarboxylic acid, 1,2-bis(4-carboxyphenoxy)ethane, 5-sodium sulfoisophthalic acid, diphenic acid, and derivatives thereof, such as acid halides.
[0090] Examples of bisphenol-based diols include 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), 2,2-bis(3-methyl-4-hydroxyphenyl)propane (bisphenol C), 1,1-bis(4-hydroxyphenyl)cyclohexane (bisphenol Z), 1,1-bis(4-hydroxyphenyl)-1-phenylethane (bisphenol AP), 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, and the like. Examples of such hydroxyphenyl compounds include 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl ketone, 4,4'-dihydroxydiphenyl methane, 4,4'-dihydroxybiphenyl [4,4'-biphenol], 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 4,4'-(1,3-dimethylbutylidene)diphenol, and resorcinol.
[0091] The molecular weight of the polyarylate is not particularly limited, and from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, the inherent viscosity of a resin solution dissolved in 1,1,2,2-tetrachloroethane to a concentration of 1 g / dL at a temperature of 25°C is preferably 0.40 to 1.20 dL / g, and more preferably 0.45 to 1.00 dL / g.
[0092] From the viewpoint of further improving dimensional stability, isotropy and dielectric properties, the content of other polymers is preferably 10 mass % or less (i.e., 0 to 10 mass %), more preferably 5 mass % or less (i.e., 0 to 5 mass %), and even more preferably 3 mass % or less (i.e., 0 to 3 mass %) relative to the total mass of the liquid crystal polymer film.
[0093] The film of the present invention may contain a compatible component to improve the compatibility between the liquid crystal polymer (A) and the crystalline polyimide (B). Examples of the compatible component include epoxy group-containing polyolefin copolymers, maleic anhydride-containing polyolefin copolymers, oxazoline group-containing vinyl copolymers, carboxyl group-containing olefin copolymers, and ionomer resins.
[0094] The content of the compatible component is usually 30 mass% or less (i.e., 0 to 30 mass%) relative to the total mass of the liquid crystal polymer film, and from the viewpoint of improving the compatibility between the liquid crystal polymer (A) and the crystalline polyimide (B) and further improving the dimensional stability, isotropy and dielectric properties, it is preferably 20 mass% or less (i.e., 0 to 20 mass%), more preferably 10 mass% or less (i.e., 0 to 10 mass%), even more preferably 5 mass% or less (i.e., 0 to 5 mass%), sufficiently preferably 1 mass% or less (i.e., 0 to 1 mass%), and even more preferably 0 mass%.
[0095] The film of the present invention may contain various additives as necessary within the range that does not impair the effects of the present invention. Examples of additives include lubricants such as particles and fatty acid esters; colorants such as pigments and dyes; heat stabilizers; color inhibitors, antioxidants, weather resistance improvers, flame retardants, plasticizers, release agents, reinforcers, modifiers, antistatic agents, ultraviolet absorbers, antifogging agents, and various polymer resins. The film of the present invention preferably contains a heat stabilizer to enhance the heat stability during film formation, prevent deterioration of the strength and elongation of the film, and prevent deterioration of the film due to oxidation or decomposition during use. Examples of heat stabilizers include hindered phenol-based heat stabilizers, hindered amine-based heat stabilizers, phosphorus-based heat stabilizers, sulfur-based heat stabilizers, and bifunctional heat stabilizers.
[0096] The content of the above additives is usually 10% by mass or less (i.e., 0 to 10% by mass) relative to the total mass of the liquid crystal polymer film, and from the viewpoint of further improving dimensional stability, isotropy and dielectric properties, it is preferably 5% by mass or less (i.e., 0 to 5% by mass), more preferably 2% by mass or less (i.e., 0 to 2% by mass), even more preferably 1% by mass or less (i.e., 0 to 1% by mass), sufficiently preferably 0.1% by mass or less (i.e., 0 to 0.1% by mass), and even more preferably 0% by mass.
[0097] [Method of manufacturing liquid crystal polymer film] The method for producing a liquid crystal polymer film of the present invention includes a blending step of blending a liquid crystal polymer (A) and a crystalline polyimide (B), a step of forming an unstretched film using the blended mixture, and a stretching step of stretching the unstretched film uniaxially or biaxially.
[0098] (Blending process) In this process, the liquid crystal polymer (A) and the crystalline polyimide (B), as well as the above-mentioned other polymers, compatibilizers, and additives that are added as required, are blended in a predetermined ratio. The blending may be dry blending, which is a simple mechanical blending, or wet blending, which is melted and kneaded to obtain pellets. From the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, the blending is preferably wet blending, and more preferably wet blending is performed after dry blending.
[0099] The dry mixing can be carried out using a mixing device such as a tumbler or a Henschel mixer. The melt kneading device used for wet mixing is not particularly limited, and for example, a single screw or twin screw extruder, various kneaders, etc. are used. In particular, from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, it is preferable to use a twin screw kneading extruder as the melt kneading device. When an extruder is used as the device for the blending step and the film-forming step described later, these steps can be performed in one device.
[0100] (Film forming process) In this step, the blend mixture (e.g., pellets) obtained in the blending step is melted and kneaded, and then the melt-kneaded product is formed into a film. Additives such as compatible components and heat stabilizers may be added in this step. In this step, the melting and kneading can be performed using a single-screw or twin-screw extruder as exemplified in the description of the blending step.
[0101] The film formation can be carried out by a conventionally known method, for example, by extruding the molten mixture through a die to obtain an unstretched film (die extrusion film formation process). In detail, it is preferable to extrude the molten mixture into a film using a flat die such as a T-die. The die extrusion film formation process (particularly the extrusion film formation process using a flat die) is an advantageous process for thickening, thickness accuracy, and large-scale / high-speed production, so the film production method of the present invention is very important from the viewpoint of improving productivity in the current situation where liquid crystal polymer films are in short supply. The film-like molten material can be cooled by contacting it with the cooling surface of a moving cooling body such as a cooling roll or a steel belt to obtain an unstretched film. This unstretched film is an unstretched film oriented in the MD direction.
[0102] (Stretching process) In this process, the unstretched film obtained in the film-forming process is stretched to control the orientation degree of the film within a predetermined range. Specifically, the orientation degree of the liquid crystal polymer (A) and the end / edge strength ratio of the crystalline polyimide (B) are stretched to be within a predetermined range. More specifically, since the unstretched film is strongly oriented in the MD direction, it is stretched at least in the TD direction (for example, uniaxially in the TD direction, or biaxially in both the MD and TD directions) after preheating. From the viewpoint of further improving dimensional stability, isotropy, and dielectric properties, it is preferably stretched only in the TD direction. The preheating temperature is preferably 140°C or higher and lower than the "temperature at which the liquid crystal polymer substantially melts", more preferably 150 to 260°C, even more preferably 170 to 250°C, sufficiently preferably 190 to 230°C, and even more preferably 200 to 220°C. By setting the preheating temperature within this range, if the liquid crystal polymer film contains a predetermined component, it is possible to stably stretch the film without uneven stretching or film breakage. If the temperature is less than 140°C, the film may not be deformed during stretching and may break. On the other hand, if the temperature exceeds the "temperature at which the liquid crystal polymer substantially melts", stretching unevenness may be large and breakage due to melting may occur. When stretching is performed in this temperature range, conventionally, unstretched liquid crystal polymer films tend to break without being stretched in the stretching process of the present invention, but by using the configuration of the liquid crystal polymer film of the present invention, stretching becomes easier. The preheating time of the film before stretching is not particularly limited, and a practical range is 1 to 60 seconds.
[0103] This stretching step gives the unstretched film the desired isotropy described below. The stretching ratio is not particularly limited as long as it can give the unstretched film the desired isotropy. For example, when the stretching ratio in the MD direction is 1 time (particularly 0.7 to 1.3 times), the stretching ratio in the TD direction may be 2.2 to 4.0 times (particularly 2.2 to 3.5 times), and is preferably 2.8 to 3.2 times from the viewpoint of further improving dimensional stability, isotropy, and dielectric properties.
[0104] As the stretching device and stretching method, a conventionally known device and stretching method can be used. Examples of the uniaxial and biaxial stretching methods include a simultaneous biaxial stretching method in which a film is stretched simultaneously in the longitudinal and transverse directions by a tenter-type simultaneous biaxial stretching machine, and a sequential biaxial stretching method in which a film is stretched in the longitudinal direction by a roll-type stretching machine and then stretched in the transverse direction by a tenter-type transverse stretching machine.
[0105] After the stretching, it is preferable to carry out a heat setting treatment while the film is being held by the clips used for stretching. By carrying out the heat setting treatment, the dimensional stability of the obtained film at high temperatures can be improved.
[0106] From the viewpoint of heat resistance and dimensional stability of the film, the heat setting temperature is preferably from 200° C. to “Tm-5”° C., and more preferably from 240° C. to “Tm-10”° C., where Tm is the melting point (° C.) of the liquid crystal polymer (A).
[0107] The heat setting time is not particularly limited, and may be 1 to 90 seconds, particularly 5 to 30 seconds, from the viewpoint of the heat resistance and dimensional stability of the film.
[0108] After the heat setting treatment, the film is preferably subjected to a relaxation treatment of 1 to 10% while being held by the clip, and may be subjected to a relaxation treatment of 3 to 7%. By performing the relaxation treatment, the dimensional stability of the obtained film at high temperatures can be further improved. The relaxation process can be carried out in either the MD or TD direction.
[0109] (Post-processing) After the stretching step, the obtained stretched film may be subjected to a post-treatment step based on a heat treatment at a relatively high temperature and for a long time. Specifically, the stretched film is heat-treated by being held in a nitrogen atmosphere at a temperature and for a long time compared with the treatment temperature and treatment time in the heat setting treatment step, respectively.
[0110] The heat treatment temperature in the post-treatment step is usually preferably from 230° C. to Tm-5° C., more preferably from 250° C. to Tm-10° C., where Tm is the melting point (° C.) of the liquid crystal polymer (A).
[0111] The heat treatment time in the post-treatment step may usually be from 5 minutes to 12 hours, particularly from 1 hour to 5 hours.
[0112] The obtained film may be cut into sheets or may be wound around a winding roll to form a film roll. From the viewpoint of productivity in use for various applications, it is preferable to form the film roll. When the film roll is formed, it may be slit to a desired width.
[0113] The film of the present invention may be subjected to a surface treatment such as a corona discharge treatment, if necessary.
[0114] In the film of the present invention, the degree of orientation of the liquid crystal polymer (A) is 71% or less, and from the viewpoint of further improving dimensional stability, isotropy and dielectric properties, it is preferably 70% or less. This value is 0% when the liquid crystal polymer (A) is completely randomly oriented in the film plane, and is infinitely large when the liquid crystal polymer (A) is completely uniaxially oriented in the MD direction in the film plane, and is 100% when the liquid crystal polymer (A) is oriented in the TD direction. If the degree of orientation exceeds 71%, the dimensional stability and isotropy are reduced. The degree of orientation is usually 50% or more, particularly 60% or more.
[0115] In this specification, the degree of orientation of the liquid crystal polymer (A) is determined by measuring the azimuth angle intensity distribution by wide-angle X-ray diffraction using an X-ray source: Cu-Kα radiation and an output of 50 kV-300 mA, and calculating the half-width A° at the diffraction peak position based on the following formula: Orientation degree = (180°-A°) / 180°
[0116] In general, the degree of orientation of the liquid crystal polymer (A), which tends to be oriented in the MD direction, should be as low as possible from the viewpoint of the isotropy of the film. However, in the film of the present invention, even if the degree of orientation of the liquid crystal polymer (A) is within the above range, by setting the end / edge strength ratio of the crystalline polyimide (B) within the range described below, more sufficiently excellent isotropy can be obtained.
[0117] In the film of the present invention, the end / edge intensity ratio of the crystalline polyimide (B) is 1 or less (particularly less than 1), and from the viewpoint of further improving dimensional stability, isotropy and dielectric properties, it is preferably 0.8 or less (particularly less than 0.8), more preferably 0.6 or less (particularly less than 0.6), and even more preferably 0.4 or less (particularly less than 0.4). The smaller this value, the more the crystalline polyimide (B) is oriented in the TD direction. If the intensity ratio exceeds 1, the dimensional stability and isotropy are reduced. The intensity ratio is usually 0.01 or more, particularly 0.1 or more.
[0118] In this specification, the end / edge intensity ratio is the end / edge intensity ratio determined by β scan of the peak of TPI(B) at a Bragg angle of 2θ=5°, which is defined based on wide-angle X-ray diffraction.
[0119] The thickness of the film of the present invention (after stretching) is not particularly limited, and may be, for example, 1 μm or more, particularly 10 μm or more. Since the film of the present invention can be produced by a die extrusion film-forming method that is easy to make thick, the thickness is preferably 40 μm or more, more preferably 60 μm or more, even more preferably 100 μm or more, sufficiently preferably 120 μm or more, and even more preferably 140 μm or more. The upper limit of the thickness of the film of the present invention is not particularly limited, and the thickness is usually 1000 μm or less, particularly may be 400 μm or less.
[0120] In this specification, the thickness of a film is the average value of thicknesses measured at random 50 points using a HEIDENHAIN-METRO MT1287 manufactured by HEIDENHAIN AG.
[0121] The film of the present invention is sufficiently excellent in dimensional stability. Dimensional stability refers to a property in which the thermal expansion coefficients in two orthogonal directions (particularly MD and TD) in the film plane are close to the thermal expansion coefficient of copper (18 ppm / °C). For example, the thermal expansion coefficients in both MD and TD of the film of the present invention are 10 ppm / °C or more and 30 ppm / °C or less, preferably 11 ppm / °C or more and less than 29 ppm / °C, more preferably 12 ppm / °C or more and less than 26 ppm / °C, and even more preferably 13 ppm / °C or more and less than 24 ppm / °C.
[0122] The coefficient of linear thermal expansion of the film is determined by applying a load of 40 mN to a 10 mm long sample and measuring the sample length in the temperature range of 25 to 250°C.
[0123] The film of the present invention is also sufficiently excellent in isotropy. Isotropy is a property in which the thermal expansion coefficients in two directions (particularly MD and TD) perpendicular to each other in the film plane are similar to each other. For example, the MD / TD ratio of the thermal expansion coefficients in the MD and TD directions of the film of the present invention is 0.5 or more and less than 1.5, preferably 0.6 or more and less than 1.4, more preferably 0.7 or more and less than 1.3, and even more preferably 0.8 or more and less than 1.2.
[0124] The film of the present invention is also sufficiently excellent in dielectric properties. Dielectric properties refer to the properties of a film having a smaller relative dielectric constant and dielectric loss tangent. For example, the relative dielectric constant of the film of the present invention is 3.2 or less, preferably 3.1 or less. The relative dielectric constant is usually 2.0 or more, particularly 2.5 or more. For example, the dielectric loss tangent of the film of the present invention is 0.0027 or less, preferably 0.0025 or less, more preferably 0.0023 or less, and even more preferably 0.0021 or less. The dielectric loss tangent is usually 0.001 or more, particularly 0.0015 or more.
[0125] The relative dielectric constant and dielectric loss tangent are values measured at 5 GHz using a cavity resonator perturbation method under conditions of temperature 22 to 24° C. and humidity 45 to 55% RH.
[0126] [Laminates and multilayer boards] The liquid crystal polymer film of the present invention is useful as a film base material for electric circuit boards (particularly for high-frequency electric circuit boards). In particular, laminates and multilayer boards for electric circuit boards (particularly for high-frequency electric circuit boards) can be manufactured using the liquid crystal polymer film of the present invention. For example, the liquid crystal polymer film of the present invention can be made into a laminate by forming a metal layer on its surface (for example, one side or both sides). In this case, various metals constituting the metal layer include Cu, Ni alloy, Al, Ag, Au, Sn, stainless steel (SUS), etc. A high-frequency electric circuit board is a board of an electric circuit that behaves at a high frequency of 3 to 300 GHz. The film, laminate, and multilayer board of the present invention have sufficiently excellent dielectric properties even in such a high-frequency environment.
[0127] The method of forming a metal layer on the film surface is not particularly limited, and examples thereof include a method of laminating a metal foil on a film and bonding (fusing) the two layers, a physical method (dry method) such as sputtering or vapor deposition, a chemical method (wet method) such as electroless plating or electrolytic plating after electroless plating, and a method of applying a metal paste. The thickness of the metal layer is not particularly limited, and is, for example, about 500 Å to 100 μm, and the thickness of the metal laminate film is, for example, 3 to 1100 μm, particularly about 10 to 500 μm. The metal laminate film is a laminate having a metal layer on one or both sides of the film of the present invention.
[0128] The laminate of the present invention can be used as a material for multilayer substrates, and can also be suitably used as the following materials or films: high heat dissipation substrates; antenna substrates; packaging materials for medicines; packaging materials for food such as retort foods; packaging materials for electronic parts such as semiconductor packages; electrical insulating materials for motors, transformers, cables, electric wires, multilayer printed wiring boards, etc.; dielectric materials for capacitor applications, etc.; magnetic tape materials such as cassette tapes, magnetic tapes for storing data for digital data storage, and video tapes; protective materials for solar cell substrates, liquid crystal panels, conductive films, glass, digital signage, and other display devices; electronic substrate materials such as LED mounting substrates, organic EL substrates, flexible printed wiring boards, flexible flat cables, flexible antennas, and speaker diaphragms; heat-resistant protective films such as coverlay films for flexible printed wiring and heat-resistant masking tapes; heat-resistant adhesives such as heat-resistant barcode labels and various industrial process tapes. The products can be suitably used as films; heat-resistant reflectors; heat-resistant release films; thermally conductive films; films for semiconductor processes such as dicing tape, dicing tape integrated die attach film (dicing / die attach film), dicing tape integrated die bonding film (dicing / die bonding film), dicing tape integrated wafer back surface protection film, and back gliding film; materials for molding and decoration such as in-mold molding, film insert molding, vacuum molding, and compressed air molding; adhesive materials such as interlayer adhesives for laminates and multilayer printed wiring boards, bonding sheets for flexible printed wiring boards, bonding sheets for flexible flat cables, and bonding sheets for coverlay films; shock absorbing materials such as tube coating, wire coating, shock absorbing films, and sealing films; photographic films; agricultural materials; medical materials; civil engineering and building materials; filtration membranes; household and industrial materials; and films for textile materials.
[0129] The multilayer substrate of the present invention can be obtained by laminating and thermocompressing a plurality of the laminates. The number of the laminates included in the multilayer substrate of the present invention is not particularly limited and may be, for example, 2 to 100, and particularly 2 to 50.
[0130] The multilayer substrate of the present invention can be used as a circuit substrate. The circuit substrate can be used as a circuit substrate (or a substrate mounting a semiconductor substrate) on which a semiconductor substrate (e.g., an IC chip) is mounted, an optoelectronic hybrid substrate, or the like. The circuit substrate can be used for a known or conventional transmission line such as a coaxial line, a strip line, a microstrip line, a coplanar line, or a parallel line, or can be used for an antenna. The circuit substrate can be an electric circuit substrate (particularly a high-frequency electric circuit substrate). EXAMPLES
[0131] 1.Measurement method (1) Degree of orientation of LCP in the film Using an X-ray wide-angle diffractometer (Rigaku RINT-TTR III, X-ray source: Cu-Kα ray, output 50 kV-300 mA), the sample was attached to the sample stage so that the X-ray irradiation direction was perpendicular to the film surface. Next, at the Bragg angle of LCP (2θ = about 44°), the sample was rotated from azimuth angle 0° to 360° with the X-ray irradiation direction as the rotation axis, and the diffraction intensity of LCP was measured by the transmission method. From the azimuth angle intensity distribution, the half-width A° at the diffraction peak position was obtained and substituted into the following formula to calculate the degree of orientation. Orientation degree = (180°-A°) / 180°
[0132] (2) End / edge ratio of TPI(B) in the film Using an X-ray wide-angle diffractometer (Rigaku RINT-TTR III, X-ray source: Cu-Kα ray, output 50 kV-300 mA), the sample is attached to the sample stage so that the X-ray irradiation direction is perpendicular to the film surface. The sample is mounted so that the diffraction intensity obtained at 0° with the X-ray irradiation direction as the rotation axis is the intensity in the edge direction, which is the intensity in the TD direction, and the diffraction intensity obtained at 90° is the intensity in the end direction, which is the intensity in the MD direction. Next, the sample was rotated at the Bragg angle (2θ = approximately 5°) of TPI(B) from 0° to 360° in azimuth with respect to the rotation axis, and the diffraction intensity of TPI(B) was measured by the transmission method. The end / edge ratio was calculated by substituting it into the following formula. End / edge ratio = strength in end direction / strength in edge direction
[0133] ·Coefficient of thermal expansion of film The film was cut into pieces of 10 mm x 5 mm in the MD and TD, and the dimensional changes were measured using a thermomechanical analyzer (TMA) under the following conditions. Temperature conditions (i) Heat from 20°C to 255°C at 10°C / min and hold for 5 minutes (first heat-up) (ii) Decrease temperature from 255°C to 25°C at 10°C / min and hold for 60 minutes (iii) Heat from 25°C to 250°C at 10°C / min and hold for 5 minutes (second heating) Load: 40mN constant Sample (measurement) size: length 10mm x width 4mm The temperature range for measuring the average linear expansion coefficient was 25 to 250° C. during the second temperature rise, and the linear expansion coefficient was calculated using the following formula. Average linear expansion coefficient [ppm / ℃] = (dimension at 250℃ - dimension at 25℃) / (dimension at 25℃) / (250℃ - 25℃) × 10 6 The average linear expansion coefficient α [ppm / °C] in the MD and TD directions was determined and evaluated according to the following criteria. ◎◎: α = 13 or more and less than 24 (best); ◎: α = 12 to less than 13 or 24 to less than 26 (excellent); ○: α = 11 or more and less than 12 or 26 or more and less than 29 (good); △: α = 10 or more and less than 11 or 29 or more and less than 30 (no problem in practical use); ×: α=less than 10 or more than 30 (problems in practical use).
[0134] ·Dimensional stability The dimensional stability was evaluated from the evaluation results of the average linear expansion coefficient in the MD and TD directions. ◎◎: The evaluation results for the average linear expansion coefficient in both the MD and TD directions were "◎◎" (best); ◎: The lower of the evaluation results of the average linear expansion coefficient in the MD direction and the TD direction was evaluated as "◎" (excellent); ○: The lower evaluation result of the average linear expansion coefficient in the MD direction and the TD direction was “○” (good); △: The lower of the evaluation results of the average linear expansion coefficient in the MD direction and the TD direction was △ (no problem in practical use); ×: Of the evaluation results of the average linear expansion coefficient in the MD direction and the TD direction, the lower evaluation result was "×" (problematic in practical use).
[0135] ·Isotropic The MD / TD ratio was calculated from the linear thermal expansion coefficient α of the film to evaluate the isotropy. ◎◎: MD / TD ratio = 0.8 or more and less than 1.2 (best); ◎: MD / TD ratio = 0.7 or more and less than 0.8 or 1.2 or more and less than 1.3 (excellent); ○: MD / TD ratio = 0.6 or more and less than 0.7 or 1.3 or more and less than 1.4 (good); △: MD / TD ratio = 0.5 or more and less than 0.6 or 1.4 or more and less than 1.5 (no problem in practical use); ×: MD / TD ratio = less than 0.5 or 1.5 or more (problems in practical use).
[0136] (3) Dielectric constant and dielectric tangent (dielectric properties) of the film The relative permittivity and dielectric loss tangent at 5 GHz were measured by the cavity resonator perturbation method. The size of the sample was 2 mm × 50 mm, and it was conditioned for 12 hours or more at a temperature of 22 to 24°C and a humidity of 45 to 55% RH. Dielectric constant ◎◎: 3.2 or less (best); ×: Over 3.2 (problems in practical use). ·Dielectric tangent ◎◎: 0.0021 or less (best); ◎: More than 0.0021 and less than 0.0023 (excellent); ○: More than 0.0023 and less than 0.0025 (good); △: More than 0.0025 and 0.0027 or less (no problem in practical use); ×: Over 0.0027 (problems in practical use).
[0137] Dielectric The dielectric properties were evaluated based on the evaluation results of the relative dielectric constant and the dielectric loss tangent. ◎◎: The evaluation results for the relative dielectric constant and the dielectric tangent were both "◎◎" (best); ◎: The lower evaluation result of the relative dielectric constant and the dielectric tangent was "◎" (excellent); ○: The lower evaluation result of the relative dielectric constant and the dielectric tangent was “○” (good); △: The lower evaluation result of the relative dielectric constant and the dielectric loss tangent was "△" (no problem in practical use); ×: Of the evaluation results of the relative dielectric constant and the dielectric loss tangent, the lower evaluation result was "×" (problematic in practical use).
[0138] (4) Overall evaluation A comprehensive evaluation was made based on the evaluation results of dimensional stability, isotropy and dielectric property. ◎◎: The evaluation results for dimensional stability, isotropy, and dielectric property were all "◎◎" (best); ◎: The lower evaluation result of the dimensional stability, isotropy, and dielectric property was "◎" (excellent); ○: The lower evaluation result of the dimensional stability, isotropy, and dielectric property was “○” (good); △: The lower evaluation result of the dimensional stability, isotropy, and dielectric property was △ (no problem in practical use); ×: Among the evaluation results of dimensional stability, isotropy, and dielectric property, the lower evaluation result was "×", or breakage occurred during the stretching process (problem in practical use).
[0139] (5) Melting point The melting point of the polymer is a temperature obtained from the crystal melting peak when measured at a heating rate of 20°C / min using a differential scanning calorimeter (PerkinElmer, DSC-7 type). More specifically, first, a predetermined polymer sample is measured under a heating condition of 20°C / min from room temperature, and then the endothermic peak temperature (Tm1) is observed, and the sample is held at a temperature 20°C to 50°C higher than Tm1 for 10 minutes. Next, the sample is cooled to room temperature under a temperature drop condition of 20°C / min, and then the endothermic peak is observed when measured again under a heating condition of 20°C / min, and the temperature showing the peak top is taken as the melting point of the polymer.
[0140] (6) Melt flow rate (MFR) The measurement was performed using a melt indexer F-B01 manufactured by Toyo Seiki Seisakusho Co., Ltd. in accordance with JIS K 7210. The test temperature was 350° C. and the test load was 2.16 kg.
[0141] raw material The raw materials used in the examples and comparative examples are as follows.
[0142] (1) Liquid crystal polymer: LCP1 In a polymerization tube equipped with an agitator, 6230g (72 mol%) of 4-hydroxybenzoic acid, 3300g (28 mol%) of 6-hydroxy-2-naphthoic acid, and 1.02 times the amount of acetic anhydride in terms of the amount of hydroxyl groups (mol) of all monomers were charged, and the temperature was raised from room temperature to 145°C over 1 hour in a nitrogen gas atmosphere, and the temperature was maintained at 145°C for 30 minutes. Next, the temperature was raised to 320°C over 7 hours while distilling off the by-product acetic acid, and the pressure was reduced to 10mmHg over 80 minutes. The polymerization reaction was terminated when a predetermined torque was reached, the contents were removed from the reaction vessel, and pellets of liquid crystal polymer were obtained using a grinder. The melting point (Tm) of the obtained pellets was 280°C, and MFR=100g / 10min.
[0143] (2) Liquid crystal polymer: LCP2 1452g (13 mol%) of polyethylene terephthalate was charged into a polymerization tube equipped with an agitator, and the temperature was raised to 260°C under a nitrogen gas atmosphere. 9292g (87 mol%) of 6-hydroxy-2-naphthoic acid was added in four portions at 20-minute intervals. After the addition was completed, the acidolysis reaction was carried out for 120 minutes while maintaining the temperature. Next, the temperature in the system was lowered to 140°C, and 6650g (117 mol%) of acetic anhydride was added to carry out an acetylation reaction for 2 hours. Finally, the temperature of the reaction system was raised to 300°C over 3 hours, and the pressure was reduced to 10mmHg over 80 minutes. The polymerization reaction was terminated when a predetermined torque was indicated, and the contents were removed from the reaction vessel and pellets of liquid crystal polymer were obtained using a grinder. The melting point (Tm) of the obtained pellets was 285°C, and MFR=80g / 10min.
[0144] (3) Crystalline polyimide: TPI (B) 500g of 2-(2-methoxyethoxy)ethanol (manufactured by Nippon Nyukazai Co., Ltd.) and 218.12g (1.00mol) of pyromellitic dianhydride (manufactured by Mitsubishi Gas Chemical Co., Ltd.) were introduced into a 2L separable flask equipped with a Dean-Stark apparatus, a Liebig condenser, a thermocouple, and four paddle blades, and after nitrogen flow, the mixture was stirred at 150 rpm to obtain a uniform suspension solution. Meanwhile, using a 500mL beaker, 49.79g (0.35mol) of 1,3-bis(aminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Co., Ltd., cis / trans ratio = 7 / 3) and 93.77g (0.65mol) of 1,8-octamethylenediamine (manufactured by Kanto Chemical Co., Ltd.) were dissolved in 250g of 2-(2-methoxyethoxy)ethanol to prepare a mixed diamine solution. This mixed diamine solution was gradually added using a plunger pump. Although the drop generates heat, the internal temperature was adjusted to be within 40 to 80°C. The mixed diamine solution was dropped under nitrogen flow conditions, and the stirring blade rotation speed was 250 rpm. After the drop was completed, 130 g of 2-(2-methoxyethoxy)ethanol and 1.284 g (0.010 mol) of n-octylamine (Kanto Chemical Co., Ltd.), which is a terminal blocking agent, were added and further stirred. At this stage, a pale yellow polyamic acid solution was obtained. Next, the stirring speed was set to 200 rpm, and the polyamic acid solution in the 2L separable flask was heated to 190°C. During the temperature increase, precipitation of polyimide resin powder and dehydration due to imidization were confirmed when the liquid temperature was between 120 and 140°C. After holding at 190°C for 30 minutes, the solution was allowed to cool to room temperature and filtered. The obtained polyimide resin powder was washed with 300 g of 2-(2-methoxyethoxy)ethanol and 300 g of methanol, filtered, and then dried in a dryer at 180° C. for 10 hours to obtain 317 g of polyimide resin 1 powder. The obtained polyimide resin 1 powder was melt-kneaded and extruded using a Labo Plastomill (manufactured by Toyo Seiki Seisakusho Co., Ltd.) at a barrel temperature of 350°C and a screw rotation speed of 70 rpm. The strand extruded from the extruder was air-cooled and then pelletized using a pelletizer (Hoshi Plastics Co., Ltd.'s "Fan Cutter FC-Mini-4 / N"). The obtained pellets were dried at 150°C for 12 hours and then used to prepare a molded product. The IR spectrum of polyimide resin 1 showed characteristic imide ring absorption at ν(C=O) 1768 and 1697 (cm-1). The inherent viscosity was 1.30 dL / g, Tm was 323°C, Tg was 184°C, Tcc was 266°C, heat of crystallization was 25.0 J / g, half-crystallization time was less than 20 seconds, and Mw was 55,000.
[0145] (4) Amorphous polyimide: PI UIP-R (product name) (manufactured by Ube Industries, Ltd.)
[0146] (5) Polyarylate: PAR1 U Polymer (registered trademark) U-100 (manufactured by Unitika Ltd.)
[0147] (6) Polyarylate: PAR2 U Polymer (registered trademark) C Powder (manufactured by Unitika Ltd.)
[0148] (7) Polyetherimide: PEI1 Ultem (registered trademark) RESIN 1000 (manufactured by Savic)
[0149] (8) Polyetherimide: PEI2 Ultem (registered trademark) RESIN 1010 (manufactured by Savic)
[0150] <Example 1> (Blending process) The components shown in Table 1 (liquid crystal polymer components and components other than liquid crystal polymer) were mixed in the ratio shown in Table 1 and kneaded and pelletized using an extruder. The pellets obtained by kneading and pelletizing were dried at 150°C for 12 hours using a vacuum dryer to reduce the moisture content to 50 ppm or less. The pellets dried in this manner are also referred to as raw material A.
[0151] (Film forming process) Raw material A was fed to a full-flight screw single-screw extruder with a screw diameter of 40 mm, heated and melted at 350°C, fed to a T-die with a die width of 350 mm and a lip spacing of 0.6 mm at a rate of 8 kg / hour, and then extruded into a sheet shape onto a metal drum rotated at a speed of 2 m / min and heated to 60°C, to obtain an unstretched film with a thickness of approximately 150 μm.
[0152] (Stretching process) The unstretched film obtained was held at the ends by clips of a tenter-type simultaneous biaxial stretching machine, preheated at 210°C for 20 seconds, and then stretched 3.0 times in the TD direction, followed by heat treatment (heat setting treatment) at 270°C for 10 seconds and slow cooling to room temperature to obtain a film with a thickness of 50 μm.
[0153] <Examples 2 to 9 and Comparative Examples 2, 4, 5, 6, 9 to 11> A liquid crystal polymer film was obtained in the same manner as in Example 1, except that the raw materials to be blended, the blending amounts, the thickness, and the stretching ratio were changed as shown in Table 1.
[0154] <Comparative Examples 1, 3, 7, and 8> An attempt was made to obtain a liquid crystal polymer film in the same manner as in Example 1, except that the raw materials and their amounts were changed as shown in Table 1. However, because the content of crystalline polyimide was low, the film broke during the stretching process, and it was not possible to obtain a film.
[0155] [Table 1]
[0156] <Consideration> The liquid crystal polymer films of Examples 1 to 9 satisfied the requirements of the present invention and were therefore excellent in isotropy and dielectric properties. From the overall evaluation results of isotropy and dielectric properties, the liquid crystal polymer films of Examples 1, 2, and 6 to 9 were preferred, and the liquid crystal polymer films of Examples 1 and 7 were more preferred.
[0157] The liquid crystal polymer films of Comparative Examples 2, 4 and 6 had a lower content of crystalline polyimide than that specified in the present invention, and therefore had a poor MD / TD ratio of the linear thermal expansion coefficient and poor isotropy. The liquid crystal polymer film of Comparative Example 5 had a low TD stretch ratio, and the degree of orientation of the liquid crystal polymer and the strength ratio of the crystalline polyimide were too high, so that the dimensional stability and isotropy were poor. The film of Comparative Example 9 had a crystalline polyimide content greater than that specified in the present invention, and therefore had high MD and TD values of the linear thermal expansion coefficient and was poor in dimensional stability. [Industrial Applicability]
[0158] The liquid crystal polymer film of the present invention is useful as a film substrate for electric circuit boards (particularly for high frequency electric circuit boards).
Claims
1. A liquid crystal polymer film containing a liquid crystal polymer (A) and a crystalline polyimide (B), The orientation degree of the liquid crystal polymer (A) is 71% or less, the content of the crystalline polyimide (B) is 1 to 50% by mass based on the total mass of the liquid crystal polymer, The liquid crystal polymer film, wherein the crystalline polyimide (B) has an end / edge strength ratio of 1 or less.
2. The liquid crystal polymer film according to claim 1 , wherein the ratio of the linear thermal expansion coefficient in both MD and TD directions of the film is 0.5 or more and less than 1.
5.
3. 2. The liquid crystal polymer film according to claim 1, wherein the liquid crystal polymer (A) contains, as monomer components, an aromatic hydroxycarboxylic acid, and further contains or does not contain an aromatic dicarboxylic acid and an aliphatic diol.
4. The content of the aromatic hydroxycarboxylic acid is 50 mol % or more based on the total amount of monomers constituting the liquid crystal polymer (A), The content of the aromatic dicarboxylic acid is 25 mol % or less based on the total amount of monomers constituting the liquid crystal polymer (A), 4. The liquid crystal polymer film according to claim 3, wherein the content of the aliphatic diol is 25 mol % or less based on the total amount of monomers constituting the liquid crystal polymer (A).
5. 2. The liquid crystal polymer film according to claim 1, wherein the liquid crystal polymer (A) is a copolymer having 6-hydroxy-2-naphthoic acid as a copolymerization component.
6. 2. The liquid crystal polymer film according to claim 1, wherein the liquid crystal polymer (A) is a copolymer of 6-hydroxy-2-naphthoic acid and 4-hydroxybenzoic acid or a copolymer of 6-hydroxy-2-naphthoic acid, terephthalic acid and ethylene glycol.
7. 2. The liquid crystal polymer film according to claim 1, wherein the crystalline polyimide (B) has a melting point of 270 to 360° C. as measured by differential scanning calorimetry.
8. 2. The liquid crystal polymer film according to claim 1, wherein the content of the crystalline polyimide (B) is 2 to 35% by mass.
9. 2. The liquid crystal polymer film according to claim 1, wherein the content of the crystalline polyimide (B) is 2 to 20% by mass.
10. A method for producing the liquid crystal polymer film according to any one of claims 1 to 9, comprising the steps of: A step of blending the liquid crystal polymer (A) and the crystalline polyimide (B); A die extrusion film-forming step of melting and kneading the blend mixture and then extruding it through a die to obtain an unstretched film; and A method for producing a liquid crystal polymer film, comprising a stretching step of stretching the unstretched film so as to achieve a degree of orientation of the liquid crystal polymer (A) and an end / edge strength ratio of the crystalline polyimide (B) to obtain a liquid crystal polymer film.
11. The method for producing a liquid crystal polymer film according to claim 10, wherein the die is a flat die.
12. A laminate comprising the liquid crystal polymer film according to any one of claims 1 to 9 and a metal layer on one or both sides thereof.
13. 13. The laminate of claim 12, wherein the metal layer is a metal foil.
14. 13. The laminate according to claim 12, wherein the metal layer is formed by sputtering or vapor deposition.
15. A multilayer substrate comprising the laminate of claim 12.
16. The multi-layer board according to claim 15, wherein the multi-layer board is an electric circuit board or a high-frequency electric circuit board.
Citation Information
Patent Citations
Polyester film and its production
JP1993043664A
Film and laminate using the same
JP4742580B2