Method for producing liquid crystalline resin
The use of metal compounds like rubidium, cesium, strontium, and barium in the polycondensation and solid phase polymerization of aromatic hydroxycarboxylic acids enhances reaction rates, addressing slow production issues in conventional methods and producing high-quality liquid crystal resins.
Patent Information
- Application Number
- JP2023048318
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Conventional methods for producing liquid crystal resins face slow reaction rates and decreased productivity due to the time required to achieve desired molecular weights during melt polymerization and subsequent solid phase polymerization.
A method involving polycondensation reaction of aromatic hydroxycarboxylic acids and their derivatives in the presence of metal compounds containing alkali metals (rubidium and cesium) or alkaline earth metals (strontium and barium), followed by solid phase polymerization, to enhance reaction rates.
The method significantly improves reaction rates, allowing for efficient production of liquid crystal resins with enhanced molecular weights and properties.
Smart Images

Figure 2024136990000001 
Figure 2024136990000002 
Figure 2024136990000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a liquid crystalline resin. [Background technology]
[0002] Liquid crystalline resins, typified by liquid crystalline polyester resins and liquid crystalline polyesteramide resins, have a good balance of excellent fluidity, mechanical strength, heat resistance, chemical resistance, electrical properties, etc., and are therefore suitably used widely as high-performance engineering plastics. Known methods for producing liquid crystalline resins include a method of melt-polymerizing raw material monomers and, if necessary, further solid-phase polymerizing the raw material monomers to obtain a liquid crystalline resin, and a method of melt-polymerizing raw material monomers to generate oligomers and then solid-phase polymerizing the oligomers to obtain a liquid crystalline resin. For example, Patent Document 1 proposes a method of obtaining liquid crystalline polyesters by two-stage polymerization of prepolymer melt polymerization and solid-phase polymerization. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2001-139674 A Summary of the Invention [Problem to be solved by the invention]
[0004] If it takes a long time to reach a desired molecular weight in the melt polymerization of the raw material monomers or the subsequent solid-phase polymerization, the reaction rate will be slow and productivity will decrease.
[0005] An object of the present disclosure is to provide a method for producing a liquid crystalline resin having a reaction rate improved compared to conventional methods. [Means for solving the problem]
[0006] The present disclosure includes the following aspects. [1] subjecting raw material monomers containing one or more selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof to a polycondensation reaction; and solid-phase polymerizing a polycondensation reaction product of raw material monomers containing one or more selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof; At least one reaction step selected from said at least one reacting step being carried out in the presence of a metal compound comprising one or more metal atoms selected from the group consisting of alkali metals and alkaline earth metals; When the metal atom is selected from alkali metals, rubidium and / or cesium are selected, and when the metal atom is selected from alkaline earth metals, strontium and / or barium are selected. [2] subjecting a raw material monomer containing one or more selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof to a polycondensation reaction in the presence of a metal compound containing one or more metal atoms selected from the group consisting of rubidium, cesium, strontium, and barium; and The method for producing a liquid crystalline resin according to [1], further comprising solid-phase polymerization of a reaction product obtained in the polycondensation reaction in the presence of a metal compound containing one or more metal atoms selected from the group consisting of rubidium, cesium, strontium, and barium. [3] The method for producing a liquid crystalline resin according to [1] or [2], comprising, prior to the polycondensation reaction, acylating the raw material monomer in the presence of a metal compound containing one or more metal atoms selected from the group consisting of rubidium, cesium, strontium and barium. [4] The method for producing a liquid crystalline resin according to any one of [1] to [3], wherein the metal compound contains at least one selected from the group consisting of acetates, carbonates, oxides, hydroxides and chlorides of the metal atoms. [5] The method for producing a liquid crystalline resin according to any one of [1] to [4], wherein the polycondensation reaction includes carrying out the polycondensation reaction under a reduced pressure of 10,000 to 100 Pa. [6] The method for producing a liquid crystalline resin according to any one of [1] to [4], wherein the polycondensation reaction is carried out under normal pressure. Effect of the Invention
[0007] According to the present disclosure, it is possible to provide a method for producing a liquid crystalline resin with a reaction rate improved compared to conventional methods. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present disclosure will be described in detail, but the scope of the present disclosure is not limited to the embodiment described here, and various modifications can be made within the scope of the present disclosure. In addition, when multiple numerical ranges are described for a specific parameter, any numerical values described therein can be combined to form a suitable numerical range. In addition, the lower limit and / or upper limit of the numerical range described in this disclosure is a numerical value within that numerical range, and may be replaced with a numerical value shown in the examples. The expression "X to Y" indicating a numerical range means "X or more and Y or less". When a specific description described for one embodiment is also applicable to other embodiments, the description may be omitted in other embodiments.
[0009] [Method of manufacturing liquid crystal resin] The method for producing a liquid crystalline resin according to the present embodiment includes the steps of: (i) subjecting raw material monomers containing one or more selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof to a polycondensation reaction; and (ii) subjecting a polycondensation reaction product of raw material monomers containing one or more selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof to solid-state polymerization; At least one reaction step selected from The at least one reaction step is carried out in the presence of a metal compound (hereinafter, also simply referred to as a "metal compound") containing one or more metal atoms selected from the group consisting of alkali metals and alkaline earth metals, When the metal atom is selected from the alkali metals, rubidium and / or cesium are selected, and when the metal atom is selected from the alkaline earth metals, strontium and / or barium are selected. That is, in one embodiment, the at least one step is carried out in the presence of a metal compound comprising one or more metal atoms selected from the group consisting of rubidium, cesium, strontium, and barium.
[0010] "Liquid crystallinity" refers to the property of being capable of forming an optically anisotropic molten phase. The property of an anisotropic molten phase can be confirmed by a conventional polarized light inspection method using crossed polarizers. More specifically, the anisotropic molten phase can be confirmed by observing a molten sample placed on a Leitz hot stage at a magnification of 40 times under a nitrogen atmosphere using a Leitz polarizing microscope. When a resin having liquid crystallinity is inspected between crossed polarizers, polarized light is usually transmitted even when the resin is in a molten, stationary state, and the resin is optically anisotropic.
[0011] (raw material monomer) The raw material monomer includes one or more compounds selected from the group consisting of aromatic hydroxycarboxylic acids and their polymerizable derivatives. In the present disclosure, the term "polymerizable derivative" refers to a compound that can be polymerized by melt polymerization among compounds whose molecular structure has been partially changed. Examples of the compound include acylated compounds in which a phenolic hydroxyl group and / or an amino group is acylated with an acylating agent, halides in which one or more hydrogen atoms of an aromatic hydrocarbon group are substituted with halogen atoms, acid halides in which a carboxyl group is halogenated with a halogenating agent, acid anhydrides, and alkyl esters (having about 1 to 4 carbon atoms).
[0012] The aromatic hydroxycarboxylic acid and its polymerizable derivative are not particularly limited, and examples thereof include 4-hydroxybenzoic acid (HBA), 6-hydroxy-2-naphthoic acid (HNA), 3-hydroxybenzoic acid, 6-hydroxy-3-naphthoic acid, 6-hydroxy-4-naphthoic acid, 4-hydroxy-4'-carboxydiphenyl ether, 2,6-dichloro-p-hydroxybenzoic acid, 2-chloro-p-hydroxybenzoic acid, 2,6-dimethyl-p-hydroxybenzoic acid, 2,6-difluoro-p-hydroxybenzoic acid, 4-hydroxy-4'-biphenyl carboxylic acid, vanillic acid, and the like. At least one compound selected from these can be used. Among them, it is preferable to use at least one selected from 4-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid in terms of availability.
[0013] The content of the aromatic hydroxycarboxylic acid and its polymerizable derivative is preferably 40 to 70 mol %, more preferably 55 to 65 mol %, based on the total amount of raw material monomers.
[0014] In one embodiment, one or more of the raw material monomers may be an acylated product in which a phenolic hydroxyl group and / or an amino group is acylated with an acylation agent. The acylation reaction will be described later.
[0015] It is preferable that the raw material monomer further satisfies the following (1) or (2). (1) containing at least one compound selected from the group consisting of aromatic or alicyclic dicarboxylic acids and polymerizable derivatives thereof, or (2) At least one compound selected from the group consisting of aromatic or alicyclic dicarboxylic acids and polymerizable derivatives thereof, and at least one compound selected from the group consisting of aromatic or alicyclic diols, aromatic or alicyclic hydroxyamines, aromatic or alicyclic diamines, and polymerizable derivatives thereof.
[0016] The aromatic dicarboxylic acid is not particularly limited, and examples thereof include terephthalic acid (TA), isophthalic acid, 4,4'-diphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and compounds represented by the following general formula (I). General formula (I): TIFF2024136990000001.tif22170(Y:-(CH2) n -(n=1 to 4) and -O(CH2) n O-(n=1 to 4).
[0017] The alicyclic dicarboxylic acid is not particularly limited, and examples thereof include 1,4-cyclohexanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, etc. The polymerizable derivative is not particularly limited, and examples thereof include alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.
[0018] The total content of at least one compound selected from the group consisting of aromatic or alicyclic dicarboxylic acids and polymerizable derivatives thereof is preferably 5 to 50 mol %, more preferably 15 to 25 mol %, based on the total amount of raw material monomers.
[0019] The aromatic diol is not particularly limited, and examples thereof include 2,6-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 4,4'-dihydroxybiphenyl (BP), hydroquinone, resorcinol, a compound represented by the following general formula (II), and a compound represented by the following general formula (III).
[0020] General formula (II): TIFF2024136990000002.tif23170 (X is a group selected from alkylene (C1 to C4), alkylidene, -O-, -SO-, -SO2-, -S-, and -CO-.)
[0021] General formula (III): TIFF2024136990000003.tif26170
[0022] The alicyclic diol is not particularly limited, and examples thereof include 1,4-cyclohexanedimethanol, 1,4-cyclohexanediol, etc. The polymerizable derivative is not particularly limited, and examples thereof include alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.
[0023] The aromatic hydroxyamine is not particularly limited, and examples thereof include N-acetyl-p-aminophenol (APAP), 4-aminophenol, 3-aminophenol, etc. The alicyclic hydroxyamine is not particularly limited, and examples thereof include 4-aminocyclohexanol, 3-aminocyclopentanol, etc. The polymerizable derivative is not particularly limited, and examples thereof include alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.
[0024] Examples of aromatic diamines include 1,4-phenylenediamine, etc. Examples of alicyclic diamines include, but are not limited to, 1,4-cyclohexanediamine, 1,3-cyclopentanediamine, etc. Examples of polymerizable derivatives include, but are not limited to, alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.
[0025] The total content of at least one compound selected from the group consisting of aromatic or alicyclic diols, aromatic or alicyclic hydroxyamines, aromatic or alicyclic diamines, and polymerizable derivatives thereof is preferably 5 to 50 mol %, and more preferably 15 to 25 mol %, based on the total amount of raw material monomers.
[0026] Specific examples of the combination of raw material monomers include: (I)(a) comprises at least one compound selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof (preferably, consists of only at least one compound selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof); (II) (a) at least one compound selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof, (b) at least one compound selected from the group consisting of aromatic or alicyclic dicarboxylic acids and polymerizable derivatives thereof, and (c) at least one compound selected from the group consisting of aromatic or alicyclic diols, aromatic hydroxyamines, aromatic diamines, and polymerizable derivatives thereof (preferably consisting of only the above compounds (a), (b), and (c)); The above-mentioned components may be used in combination with a molecular weight regulator, if necessary.
[0027] (metal compound) The metal compound contains one or more metal atoms selected from the group consisting of alkali metals and alkaline earth metals, and when the metal atoms are selected from alkali metals, rubidium and / or cesium are selected, and when the metal atoms are selected from alkaline earth metals, strontium and / or barium are selected. That is, in one embodiment, the metal compound comprises one or more metal atoms selected from the group consisting of rubidium, cesium, strontium, and barium. The metal compound may be used alone or in combination of two or more kinds. In the course of research, the present inventor has found that by using a metal compound containing an alkali metal or alkaline earth metal with a large ionic radius as a catalyst used in the production of a liquid crystal resin, the reaction rate in the acylation reaction, polycondensation reaction, and / or solid-phase polymerization reaction is improved compared to the conventional method. Such a finding has not been known until now. The mechanism is not clear at this stage, but it is presumed that, as a non-limiting mechanism, the large ionic radius increases the catalytic activity and / or makes it difficult for ions to be inactivated. As a result, it is considered that the reaction rate in various reactions is increased. Among the alkali metal atoms, the ionic radius of rubidium is 1.48 Å, the ionic radius of cesium is 1.69 Å, and the ionic radius of potassium is 1.33 Å. Among the alkaline earth metal atoms, the ionic radius of strontium is 1.13 Å, the ionic radius of barium is 1.35 Å, and the ionic radius of calcium is 0.99 Å.
[0028] In one embodiment, the metal compound may include, as an alkali metal atom, a rubidium atom, a cesium atom, as an alkaline earth metal, a strontium atom, a barium atom, or a combination thereof. In one embodiment, the metal compound may include one or more metal atoms selected from the group consisting of rubidium, cesium, and barium.
[0029] In one embodiment, the metal compound preferably includes one or more selected from the group consisting of acetates, carbonates, oxides, hydroxides, and chlorides of one or more metal atoms selected from the group consisting of rubidium, cesium, strontium, and barium, and can include, for example, acetates and / or carbonates, and can include acetates.
[0030] Examples of metal compounds include rubidium acetate, cesium acetate, strontium acetate, barium acetate; rubidium carbonate, cesium carbonate, strontium carbonate, barium carbonate; rubidium oxide, cesium oxide, strontium oxide, barium oxide; rubidium hydroxide, cesium hydroxide, strontium hydroxide, barium hydroxide; rubidium chloride, cesium chloride, strontium chloride, barium chloride, etc. It is preferable to contain one or more selected from these, and two or more may be contained in combination.
[0031] In one embodiment, the metal compound may include one or more selected from rubidium acetate, cesium acetate, strontium acetate, barium acetate; rubidium carbonate, cesium carbonate, strontium carbonate, barium carbonate, and may include one or more selected from rubidium acetate, cesium acetate, strontium acetate, and barium acetate, and may include two or more selected from these in combination. These may be anhydrides or hydrates.
[0032] The total amount of the metal compounds used is preferably 0.001 to 0.2 mol %, more preferably 0.005 to 0.05 mol %, and even more preferably 0.005 to 0.01 mol %, based on the total amount of the raw material monomers.
[0033] (Reaction process) The method for producing a liquid crystalline resin according to the present embodiment includes the steps of: (i) subjecting raw material monomers containing one or more selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof to a polycondensation reaction; and (ii) subjecting a polycondensation reaction product of raw material monomers containing one or more selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof to solid-state polymerization; The method has at least one reaction step selected from the following:
[0034] In the method for producing a liquid crystal resin according to one embodiment, when both steps (i) and (ii) are included, the metal compound is used in step (i), so that step (ii) can be subsequently carried out in the presence of the metal compound. When only step (ii) is included, it is preferable that the polycondensation reaction product of the raw material monomers prepared in advance contains the metal compound. The polycondensation reaction product polycondensed in the presence of the metal compound contains the metal compound.
[0035] In the method for producing a liquid crystalline resin according to one embodiment, the step (ii) is preferably carried out subsequent to the step (i). That is, the method for producing a liquid crystalline resin according to one embodiment includes the steps of: A method for producing a polymerizable composition comprising the steps of: subjecting a raw material monomer containing one or more selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof to a polycondensation reaction in the presence of a metal compound containing one or more metal atoms selected from the group consisting of rubidium, cesium, strontium, and barium; The reaction product obtained in the polycondensation reaction may be subjected to solid-state polymerization in the presence of a metal compound containing one or more metal atoms selected from the group consisting of rubidium, cesium, strontium, and barium.
[0036] <(i) Polycondensation reaction (melt polymerization) process> A method for producing a liquid crystal resin according to an embodiment may include polycondensing a raw material monomer in the presence of a metal compound containing one or more metal atoms selected from the group consisting of alkali metals and alkaline earth metals. When the metal atom is selected from alkali metals, rubidium and / or cesium are selected, and when the metal atom is selected from alkaline earth metals, strontium and / or barium are selected. That is, the method for producing a liquid crystal resin according to one embodiment may include polycondensing the raw material monomer in the presence of a metal compound containing a metal atom selected from the group consisting of rubidium, cesium, strontium, and barium. By polycondensing the raw material monomer in the presence of the metal compound, the time required to reach the final torque can be shortened. As a result, the polycondensation reaction rate can be increased. Specific examples and amounts of the raw material monomer and the metal compound are the same as those described above, and therefore will not be described here. The polycondensation reaction is carried out by melt polymerization. A liquid crystal resin is obtained by polycondensing raw material monomers.
[0037] The polycondensation temperature is, for example, preferably 200 to 400° C., and more preferably 240 to 380° C. The polycondensation reaction may be carried out at a constant temperature or may be increased stepwise to a higher temperature. The polycondensation reaction time is preferably 2 to 12 hours, more preferably 3 to 10 hours, and even more preferably 4 to 7 hours.
[0038] The liquid crystal resin obtained by the polycondensation reaction can be further subjected to solid-phase polymerization to increase the molecular weight. The solid-phase polymerization will be described later. When the liquid crystal resin obtained by the polycondensation reaction is further subjected to solid-phase polymerization, the liquid crystal resin obtained by the polycondensation reaction step is also called a polymer precursor. Examples of the polymer precursor include a prepolymer having a weight-average molecular weight of 50,000 to 400,000 (preferably 70,000 to 300,000) and an oligomer having a weight-average molecular weight of less than 50,000 (preferably less than 40,000). The weight average molecular weight is a value calculated by analysis using gel permeation chromatography.
[0039] In the case of obtaining a prepolymer by a polycondensation reaction, the polycondensation reaction is preferably carried out by starting decompression and setting the pressure at a predetermined reduced pressure after the reaction system has reached a predetermined temperature. In one embodiment, the polycondensation reaction is preferably carried out under a reduced pressure of 10,000 to 100 Pa, more preferably 10,000 to 133 Pa, and further preferably 5,000 to 1,330 Pa. When obtaining an oligomer by polycondensation reaction, the polycondensation reaction is carried out under normal pressure (1.013×10 5 It is preferable that the temperature is 100° C. or less.
[0040] <(ii) Solid phase polymerization process> A method for producing a liquid crystalline resin according to one embodiment may include solid-phase polymerization of a polycondensation reaction product of raw material monomers including one or more selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof. The solid-state polymerization is carried out in the presence of a metal compound containing one or more metal atoms selected from the group consisting of alkali metals and alkaline earth metals. When the metal atoms are selected from alkali metals, rubidium and / or cesium are selected, and when the metal atoms are selected from alkaline earth metals, strontium and / or barium are selected. That is, in one embodiment, the solid-phase polymerization is carried out in the presence of a metal compound containing one or more metal atoms selected from the group consisting of rubidium, cesium, strontium, and barium. The solid-phase polymerization can increase the molecular weight of the polycondensation reaction product (polymer precursor), and a liquid crystal resin excellent in strength and heat resistance can be obtained. By carrying out solid-phase polymerization in the presence of the metal compound, the molecular weight can be increased in a short time. As a result, the solid-phase polymerization reaction rate can be increased. Specific examples and amounts of the raw material monomers and metal compounds are the same as those described above, and therefore descriptions thereof will be omitted here.
[0041] The "polycondensation reaction product of raw material monomers" is also referred to as a polymer precursor herein and means a reaction product obtained by reacting the raw material monomers by a known polycondensation reaction. The polycondensation reaction product of raw material monomers may be a polycondensation reaction product separately prepared using the raw material monomers, or may be a reaction product obtained in the above-mentioned (i) polycondensation reaction step.
[0042] The polycondensation reaction product of the raw material monomers preferably contains a metal compound containing one or more metal atoms selected from the group consisting of rubidium, cesium, strontium, and barium. By containing a metal compound containing one or more metal atoms selected from the group consisting of rubidium, cesium, strontium, and barium, the polymer precursor can be solid-phase polymerized in the presence of the metal compound simply by heating the polymer precursor.
[0043] The solid-phase polymerization can be carried out by a conventional method. For example, the solid-phase polymerization can be carried out by heating the polymer precursor obtained in the polycondensation step at a temperature 10 to 120° C. lower than the liquid crystal formation temperature of the polymer precursor obtained in the polycondensation step under reduced pressure or vacuum in an inert gas stream such as nitrogen gas. Since the melting point of the liquid crystal resin increases as the solid-phase polymerization proceeds, it is also possible to carry out the solid-phase polymerization at a temperature equal to or higher than the original melting point of the polymer precursor. The solid-phase polymerization can be carried out at a constant temperature or can be increased stepwise. The heating method is not particularly limited, and microwave heating, heater heating, etc. can be used. When the polymer precursor is the above-mentioned prepolymer, the prepolymer may be produced by polycondensation reaction, and then the pelletized prepolymer may be subjected to solid-phase polymerization. When the prepolymer is the above-mentioned oligomer, the oligomer may be produced by polycondensation reaction, and then the oligomer may be pulverized to obtain pellets, and then the pellets may be subjected to solid-phase polymerization. The average particle size of the pulverized pellets is not limited, and may be, for example, 1.4 to 2.0 mm. The method of making the average particle size 1.4 to 2.0 mm is not limited, and for example, it can be obtained by classification using sieves with openings of 2.0 mm and 1.4 mm. The average particle size can be measured, for example, using a grain scanner.
[0044] <Acylation step> The raw material monomer used in the polycondensation reaction step is preferably one in which a phenolic hydroxyl group or an amino group in the raw material monomer is acylated. In order to increase the acylation reaction rate, the acylation is carried out in the presence of a metal compound containing one or more metal atoms selected from the group consisting of alkali metals and alkaline earth metals, and when the metal atom is selected from alkali metals, it is preferable to select rubidium and / or cesium, and when the metal atom is selected from alkaline earth metals, it is preferable to select strontium and / or barium. That is, the acylation is preferably carried out in the presence of a metal compound containing a metal atom selected from the group consisting of rubidium, cesium, strontium, and barium. The method for producing a liquid crystal resin according to one embodiment may include acylation of the raw material monomer in the presence of a metal compound containing a metal atom selected from the group consisting of rubidium, cesium, strontium, and barium before the polycondensation reaction. Specific examples and amounts of the metal compound are the same as those described above, so they will not be described here.
[0045] Acylation is usually carried out using an acylating agent. Examples of the acylating agent include, but are not limited to, acetic anhydride, propionic anhydride, butyric anhydride, isobutyric anhydride, valeric anhydride, pivalic anhydride, 2-ethylhexanoic anhydride, monochloroacetic anhydride, dichloroacetic anhydride, trichloroacetic anhydride, monobromoacetic anhydride, dibromoacetic anhydride, tribromoacetic anhydride, monofluoroacetic anhydride, difluoroacetic anhydride, trifluoroacetic anhydride, glutaric anhydride, maleic anhydride, succinic anhydride, and β-bromopropionic anhydride. At least one selected from these can be used. Examples of suitable carboxylic anhydrides from the viewpoint of cost and handling include carboxylic anhydrides such as acetic anhydride, propionic anhydride, butyric anhydride, and isobutyric anhydride. Among them, acetic anhydride is preferred from the viewpoint of ease of availability. From the viewpoint of ease of reaction control, the amount of the acylating agent used is preferably 1.0 to 1.1 equivalents, and more preferably 1.01 to 1.05 equivalents, based on the total amount of hydroxyl groups in the substances used in the reaction.
[0046] The acylation can be carried out by a known method, for example, by mixing the raw material monomer with an acylating agent and heating at a temperature range of 120 to 160° C. for about 0.5 to 5 hours to carry out the acylation reaction, thereby obtaining a reaction product containing an acylated compound.
[0047] [Liquid crystal resin] The liquid crystal resin obtained by the method for producing a liquid crystal resin according to the present embodiment preferably contains at least one selected from liquid crystal polyesters and liquid crystal polyesteramides. The liquid crystal polyesters and liquid crystal polyesteramides are not particularly limited, but are preferably aromatic polyesters or aromatic polyesteramides. In addition, polyesters that partially contain aromatic polyesters or aromatic polyesteramides in the same molecular chain may also be used. In one embodiment, the liquid crystal resin obtained preferably contains one or more selected from fully aromatic polyesters and fully aromatic polyesteramides. "Fully aromatic" means that all raw material monomers have aromatic rings.
[0048] The aromatic polyester or aromatic polyester amide contains at least a structural unit derived from an aromatic hydroxycarboxylic acid or a polymerizable derivative thereof, and more specifically, (1) Polyesters consisting essentially of (a) one or more aromatic hydroxycarboxylic acids and their derivatives; (2) Polyesters consisting essentially of (a) one or more aromatic hydroxycarboxylic acids and their derivatives, and (b) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives; (3) polyesters consisting essentially of (a) one or more aromatic hydroxycarboxylic acids and their derivatives, (b) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives, and (c) one or more aromatic diols, alicyclic diols, aliphatic diols, and their derivatives; (4) polyesteramides consisting essentially of (a) one or more aromatic hydroxycarboxylic acids and their derivatives, (c1) one or more aromatic hydroxyamines, aromatic diamines, and their derivatives, and (c2) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives; (5) polyesteramides mainly composed of (a) one or more aromatic hydroxycarboxylic acids and their derivatives, (b) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives, (c1) one or more aromatic hydroxyamines, aromatic diamines, and their derivatives, and (c2) one or more aromatic diols, alicyclic diols, and their derivatives.
[0049] The molecular weight (weight average molecular weight Mw) of the liquid crystal resin is not particularly limited, and for the resin obtained in the polycondensation reaction (melt polymerization) step, it is preferably 50,000 to 500,000, more preferably 75,000 to 400,000. For the resin obtained in the solid phase polymerization step, it is preferably 60,000 to 600,000, more preferably 75,000 to 500,000. The weight average molecular weight Mw can be calculated by analysis using gel permeation chromatography.
[0050] The melting point of the liquid crystal resin is not particularly limited and can be 250 to 380° C. The melt viscosity of the liquid crystal resin is not particularly limited and the resin obtained in the polycondensation reaction (melt polymerization) step can be obtained at a cylinder temperature 10 to 30° C. higher than the melting point of the liquid crystal resin and a shear rate of 1000 sec -1 The melt viscosity measured at a shear rate of 1000 sec is preferably 5 Pa·s or more and 150 Pa·s or less, more preferably 10 Pa·s or more and 100 Pa·s or less. Furthermore, when the solid-state polymerization step is performed, the resin is polymerized at a cylinder temperature 10 to 30°C higher than the melting point of the liquid crystal resin and at a shear rate of 1000 sec -1The melt viscosity measured by is preferably 5 Pa·s or more and 200 Pa·s or less, more preferably 10 Pa·s or more and 150 Pa·s or less. "Cylinder temperature 10 to 30°C higher than the melting point of the liquid crystal resin" means a cylinder temperature at which the liquid crystal resin can be melted to a degree at which the melt viscosity can be measured, and the cylinder temperature higher than the melting point varies depending on the type of raw material resin within the range of 10 to 30°C. The liquid crystal resin can be in the form of a powder / granule mixture, or in the form of a molten mixture (melt-kneaded product) such as pellets. In the present disclosure, the melt viscosity refers to the melt viscosity measured in accordance with ISO11443. EXAMPLES
[0051] The present disclosure will be described in more detail below by showing examples, but interpretation of the present disclosure is not limited to these examples.
[0052] (1) Polycondensation reaction [Example 1-1] After the following raw materials were charged into a polymerization vessel, the temperature of the reaction system was raised to 140°C and the reaction was carried out at 140°C for 3 hours (acylation reaction). The acylation rate (acetylation rate) was calculated as follows. The results are shown in Table 1.
[0053] [Acylation (acetylation) rate] After the acylation reaction, 10 mg of the sample was dissolved in 0.5 mL of DMSO-d6. The resulting solution was analyzed using a nuclear magnetic resonance device (AVANCEIII400 manufactured by Bruker). 1 H-NMR measurement was performed to obtain the integral values of the aromatic ring 3-position proton of the unreacted monomer and the aromatic ring 3-position proton of the acylated (acetylated) monomer, and the acylation (acetylation) rate was calculated using the following formula. Acetylation rate = [(proton integral value of acetylated monomer) / ((proton integral value of unreacted monomer)+(proton integral value of acetylated monomer))] × 100 Thereafter, the temperature was further increased to 340°C over 4.5 hours, and the pressure was then reduced to 10 Torr (i.e., 1330 Pa) over 15 minutes, and polycondensation was carried out while distilling off acetic acid, excess acetic anhydride, and other low boiling points (polycondensation reaction step). After the stirring torque reached a predetermined value (0.7 V), nitrogen was introduced to change the pressure from reduced pressure to normal pressure and then to pressurized state, and the polymer was discharged from the bottom of the polymerization vessel. The strands were then pelletized to obtain liquid crystal resin pellets. The time required from the start of pressure reduction until the stirring torque reached a predetermined value (0.7 V) (time to final torque) was measured. The results are shown in Table 1. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated as follows and was 127,000 (prepolymer). (raw materials) 4-Hydroxybenzoic acid (HBA): 188.3 g (60 mol%) 6-Hydroxy-2-naphthoic acid (HNA): 21.4 g (5 mol%) Terephthalic acid (TA): 66.0 g (17.5 mol%) 4,4'-Dihydroxybiphenyl (BP): 52.9 g (12.5 mol%) N-acetyl-p-aminophenol (APAP): 17.2 g (5 mol%) Rubidium acetate (RbOAc): 21.7 mg (0.0068 mol%) Acylating agent (acetic anhydride): 226.9g
[0054] [Weight average molecular weight (Mw)] The obtained liquid crystal resin was dissolved in 3,5-bistrifluoromethylphenol as a solvent by stirring at room temperature for 6 hours. The solution was analyzed by gel permeation chromatography (Tosoh Corporation, "HLC-8320GPC", differential refractometer detector) to calculate the weight average molecular weight (Mw) in terms of standard polystyrene.
[0055] [Example 1-2] Liquid crystal resin pellets were obtained in the same manner as in Example 1-1, except that 28.8 mg (0.0068 mol%) of cesium acetate (CsOAc) was used instead of rubidium acetate. The acylation rate (acetylation rate) was calculated and the time to reach the final torque was measured in the same manner as in Example 1-1. The results are shown in Table 1. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 117,000 (prepolymer).
[0056] [Examples 1-3] Liquid crystalline resin pellets were obtained in the same manner as in Example 1-1, except that 32.2 mg (0.0068 mol%) of strontium acetate 0.5 hydrate (Sr(OAc)2·0.5H2O) was used instead of rubidium acetate. The acylation rate (acetylation rate) was calculated and the time to reach the final torque was measured in the same manner as in Example 1-1. The results are shown in Table 1. The weight average molecular weight (Mw) of the obtained liquid crystalline resin pellets was calculated to be 125,000 (prepolymer).
[0057] [Examples 1-4] Liquid crystal resin pellets were obtained in the same manner as in Example 1-1, except that 38.3 mg (0.0068 mol%) of barium acetate (Ba(OAc)2) was used instead of rubidium acetate. The acylation rate (acetylation rate) was calculated and the time to reach the final torque was measured in the same manner as in Example 1-1. The results are shown in Table 1. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 139,000 (prepolymer).
[0058] [Comparative Example 1-1] Liquid crystal resin pellets were obtained in the same manner as in Example 1-1, except that 14.7 mg (0.0068 mol%) of potassium acetate (KOAc) was used instead of rubidium acetate. The acylation rate (acetylation rate) was calculated and the time to reach the final torque was measured in the same manner as in Example 1-1. The results are shown in Table 1. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 127,000 (prepolymer).
[0059] [Comparative Example 1-2] Liquid crystal resin pellets were obtained in the same manner as in Example 1-1, except that 23.7 mg (0.0068 mol%) of calcium acetate (Ca(OAc)2) was used instead of rubidium acetate. The acylation rate (acetylation rate) was calculated and the time to reach the final torque was measured in the same manner as in Example 1-1. The results are shown in Table 1. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 127,000 (prepolymer).
[0060] [Comparative Example 1-3] Liquid crystal resin pellets were obtained in the same manner as in Example 1-1, except that the above-mentioned metal compounds and other catalysts were not used. The acylation rate (acetylation rate) was calculated and the final torque arrival time was measured in the same manner as in Example 1-1. The results are shown in Table 1. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 123,000 (prepolymer).
[0061] [Table 1]
[0062] (2) Solid-state polymerization of prepolymer [Example 2-1] The liquid crystalline resin pellets (prepolymer) obtained in Example 1-1 were subjected to solid phase polymerization as follows. In a solid-phase polymerization vessel equipped with a nitrogen inlet / outlet, 10 g of the liquid crystal resin pellets (prepolymer) obtained above was charged and placed under a nitrogen atmosphere. The reaction system was heated to 295°C and reacted for 2 hours (solid-phase polymerization step). The temperature was then lowered to room temperature to obtain liquid crystal resin pellets. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 250,000. The solid-state polymerization rate was calculated as follows, and the results are shown in Table 2.
[0063] [Solid phase polymerization rate] The solid-state polymerization rate was calculated by dividing the difference in weight-average molecular weight (Mw) of the liquid crystal resin obtained before and after the solid-state polymerization by the solid-state polymerization time.
[0064] [Example 2-2] The liquid crystal resin pellets (prepolymer) obtained in Example 1-2 were solid-phase polymerized in the same manner as in Example 2-1 to obtain liquid crystal resin pellets. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 226,000. The solid-phase polymerization rate was calculated in the same manner as in Example 2-1. The results are shown in Table 2.
[0065] [Example 2-3] The liquid crystal resin pellets (prepolymer) obtained in Example 1-4 were solid-phase polymerized in the same manner as in Example 2-1 to obtain liquid crystal resin pellets. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 186,000. The solid-phase polymerization rate was calculated in the same manner as in Example 2-1. The results are shown in Table 2.
[0066] [Comparative Example 2-1] The liquid crystal resin pellets (prepolymer) obtained in Comparative Example 1-1 were solid-phase polymerized in the same manner as in Example 2-1 to obtain liquid crystal resin pellets. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 166,000. The solid-phase polymerization rate was calculated in the same manner as in Example 2-1. The results are shown in Table 2.
[0067] [Comparative Example 2-2] The liquid crystal resin pellets (prepolymer) obtained in Comparative Example 1-2 were solid-phase polymerized in the same manner as in Example 2-1 to obtain liquid crystal resin pellets. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 161,000. The solid-phase polymerization rate was calculated in the same manner as in Example 2-1. The results are shown in Table 2.
[0068] [Comparative Example 2-3] The liquid crystal resin pellets (prepolymer) obtained in Comparative Example 1-3 were solid-phase polymerized in the same manner as in Example 2-1 to obtain liquid crystal resin pellets. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 153,000. The solid-phase polymerization rate was calculated in the same manner as in Example 2-1. The results are shown in Table 2.
[0069] [Table 2]
[0070] (3) Solid-state polymerization of oligomers [Example 3-1] After the following raw materials were charged in a polymerization vessel, the temperature of the reaction system was raised to 140°C and reacted at 140°C for 3 hours (acylation reaction). Then, the temperature was further raised to 320°C over 3.5 hours, and polycondensation was carried out for 45 minutes from there while distilling acetic acid, excess acetic anhydride, and other low boiling points under normal pressure (polycondensation reaction step). Then, oligomers were discharged from the bottom of the polymerization vessel while introducing nitrogen. Then, the strands were crushed using a Willey type crusher and classified using a sieve with a mesh size of 2.0 mm and a sieve with a mesh size of 1.4 mm to obtain a liquid crystal resin with an average particle size of 1.4 to 2.0 mm. The weight average molecular weight (Mw) of the obtained liquid crystal resin was calculated to be 33,000 (oligomer). (raw materials) 4-Hydroxybenzoic acid (HBA): 188.3 g (60 mol%) 6-Hydroxy-2-naphthoic acid (HNA): 21.4 g (5 mol%) Terephthalic acid (TA): 66.0 g (17.5 mol%) 4,4'-Dihydroxybiphenyl (BP): 52.9 g (12.5 mol%) N-acetyl-p-aminophenol (APAP): 17.2 g (5 mol%) Cesium acetate (CsOAc): 28.8 mg (0.0068 mol%) Acylating agent (acetic anhydride): 226.9g In a solid-phase polymerization vessel equipped with a nitrogen inlet / outlet, 10 g of the liquid crystal resin (oligomer) having an average particle size of 1.4 to 2.0 mm obtained above was charged and placed under a nitrogen atmosphere. The reaction system was heated to 140°C and dried from there for 3 hours. The temperature was further raised to 280°C over 1.5 hours and reacted from there for 16 hours (solid-phase polymerization step). Thereafter, the temperature was lowered to room temperature to obtain a liquid crystal resin. The weight-average molecular weight (Mw) of the obtained liquid crystal resin was calculated to be 338,000. The solid-phase polymerization rate was calculated in the same manner as in Example 2-1. The results are shown in Table 3.
[0071] [Comparative Example 3-1] A liquid crystal resin having an average particle size of 1.4 to 2.0 mm was obtained in the same manner as in Example 3-1, except that potassium acetate (KOAc) was used instead of cesium acetate. The weight average molecular weight (Mw) of the obtained liquid crystal resin was calculated to be 31,000 (oligomer). The obtained liquid crystal resin (oligomer) having an average particle size of 1.4 to 2.0 mm was solid-phase polymerized in the same manner as in Example 3-1 to obtain a liquid crystal resin. The weight average molecular weight (Mw) of the obtained liquid crystal resin was calculated to be 239,000. The solid-phase polymerization rate was calculated in the same manner as in Example 2-1. The results are shown in Table 3.
[0072] [Comparative Example 3-2] A liquid crystal resin having an average particle size of 1.4 to 2.0 mm was obtained in the same manner as in Example 3-1, except that the above-mentioned metal compound and other catalysts were not used. The weight average molecular weight (Mw) of the obtained liquid crystal resin was calculated to be 30,000 (oligomer). The obtained liquid crystal resin (oligomer) having an average particle size of 1.4 to 2.0 mm was solid-phase polymerized in the same manner as in Example 3-1 to obtain a liquid crystal resin. The weight average molecular weight (Mw) of the obtained liquid crystal resin was calculated to be 142,000. The solid-phase polymerization rate was calculated in the same manner as in Example 2-1. The results are shown in Table 3.
[0073] [Table 3]
[0074] As shown in Example 1-1 and Example 1-2 in Table 1, by subjecting the raw material monomer to a polycondensation reaction in the presence of a metal compound containing rubidium or cesium among alkali metals, the time to reach the final torque could be significantly shortened and the molecular weight could be increased in a short time compared to Comparative Example 1-1 in which the raw material monomer was polycondensed in the presence of a metal compound containing potassium, and Comparative Example 1-3 in which the raw material monomer was polycondensed in the absence of a catalyst. In other words, the polycondensation reaction rate was improved compared to the conventional methods. In addition, as shown in Examples 1-3 and 1-4, by subjecting the raw material monomer to a polycondensation reaction in the presence of a metal compound containing strontium or barium among alkaline earth metals, the time to reach the final torque can be significantly shortened and the molecular weight can be increased in a short time, compared to Comparative Example 1-2 in which the raw material monomer was polycondensed in the presence of a metal compound containing calcium, and Comparative Example 1-3 in which the raw material monomer was polycondensed in the absence of a catalyst. In other words, the polycondensation reaction rate was improved compared to the conventional example. In Examples 1-1 to 1-4, a higher acylation rate was achieved than in Comparative Example 1-3 without a catalyst. That is, the acylation reaction rate was improved compared to the conventional example. The same or higher acylation rate was achieved compared to Comparative Example 1-1, in which a metal compound containing potassium was used.
[0075] As shown in Examples 2-1 to 2-3 in Table 2, by solid-state polymerizing a prepolymer in the presence of a metal compound containing one or more metal atoms selected from the group consisting of rubidium, cesium, strontium, and barium, the solid-state polymerization rate was improved compared to Comparative Examples 2-1 and 2-2 in which the prepolymer was solid-state polymerized in the presence of a metal compound containing potassium or calcium, and Comparative Example 2-3 in which the prepolymer was solid-state polymerized in the absence of a catalyst.
[0076] As shown in Example 3-1 in Table 3, by solid-state polymerizing an oligomer in the presence of a metal compound containing one or more metal atoms selected from the group consisting of rubidium, cesium, strontium, and barium, the solid-state polymerization rate was improved compared to Comparative Example 3-1 in which the oligomer was solid-state polymerized in the presence of a metal compound containing potassium, and Comparative Example 3-2 in which the oligomer was solid-state polymerized in the absence of a catalyst. [Industrial Applicability]
[0077] The method for producing a liquid crystalline resin according to the present embodiment has an improved reaction rate compared to conventional methods, and therefore can produce a liquid crystalline resin efficiently, and has industrial applicability.
Claims
1. subjecting raw material monomers including at least one selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof to a polycondensation reaction; Solid-phase polymerizing a polycondensation reaction product of raw material monomers including one or more selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof; At least one reaction step selected from said at least one reacting step being carried out in the presence of a metal compound comprising one or more metal atoms selected from the group consisting of alkali metals and alkaline earth metals; When the metal atom is selected from alkali metals, rubidium and / or cesium are selected, and when the metal atom is selected from alkaline earth metals, strontium and / or barium are selected.
2. A method for producing a polymerizable composition comprising the steps of: subjecting a raw material monomer containing one or more selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof to a polycondensation reaction in the presence of a metal compound containing one or more metal atoms selected from the group consisting of rubidium, cesium, strontium, and barium; 2. The method for producing a liquid crystalline resin according to claim 1, further comprising solid-phase polymerization of the reaction product obtained in the polycondensation reaction in the presence of a metal compound containing one or more metal atoms selected from the group consisting of rubidium, cesium, strontium and barium.
3. 3. The method for producing a liquid crystalline resin according to claim 1, further comprising, prior to the polycondensation reaction, acylating the raw material monomer in the presence of a metal compound containing one or more metal atoms selected from the group consisting of rubidium, cesium, strontium and barium.
4. 3. The method for producing a liquid crystalline resin according to claim 1, wherein the metal compound contains at least one selected from the group consisting of acetates, carbonates, oxides, hydroxides and chlorides of the metal atoms.
5. 3. The method for producing a liquid crystalline resin according to claim 1, wherein the polycondensation reaction includes carrying out the polycondensation reaction under a reduced pressure of 10,000 to 100 Pa.
6. The method for producing a liquid crystal resin according to claim 1 or 2, wherein the polycondensation reaction is carried out under normal pressure.
Citation Information
Patent Citations
Production of polyester
JP1989024828A
Cholesteric liquid crystal polyester
JP1989090219A
Optically active group-containing cholesteric liquid crystalline polyester
JP1991047829A
Electronic equipment system
JP1993014281A
Production of polyester
JP2000143789A