Poly(hydroxyalkanoic acid) and production method thereof
A controlled production method for poly(hydroxyalkanoic acid) with low unsaturated groups and reactive terminals addresses the limitations of PHA synthesis, enabling versatile chemical modifications and applications.
Patent Information
- Application Number
- JP2023045910
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polyhydroxyalkanoates (PHA) production methods require genetic manipulation of bacteria, are time-consuming, and result in polymers with limited structural control and unsaturated groups that lead to thermal decomposition, limiting further chemical modifications.
A method to produce poly(hydroxyalkanoic acid) with controlled unsaturated groups (≤0.2 mol%) and terminal reactive groups (hydroxy or carboxyl), using phosphine and sulfonic acid catalysts for esterification, followed by purification, to enable further chemical modifications.
The method allows for the production of poly(hydroxyalkanoic acid) with enhanced chemical reactivity and expanded applications, including polyurethanes and resin compositions.
Smart Images

Figure 2024135291000001 
Figure 2024135291000002
Abstract
Description
[Technical field]
[0001] The present invention relates to poly(hydroxyalkanoic acid) and a method for producing the same. [Background technology]
[0002] In response to the social issue of environmental degradation caused by the mass waste of plastic, there is a growing demand for sustainable products (packaging materials, films) made from resins that are biodegradable in all conditions (seawater, freshwater, soil, compost). Polyhydroxyalkanoates (PHAs) produced by bacteria are examples of resins that are biodegradable under all of the above-mentioned environments. However, controlling the structure of PHA requires genetic manipulation of bacteria, and developing resins with the desired physical properties requires a great deal of time and effort. When PHA is synthesized from the corresponding monomer through chemical polymerization, the degree of freedom in the resin structure is high, but there is a problem that the monomer is susceptible to thermal decomposition, causing polymerization termination. In addition, since PHA that has undergone polymerization termination loses its reactive functional groups, further chemical modification cannot be performed, limiting its uses. Therefore, PHA-based synthetic resins with reduced amounts of decomposition products are needed.
[0003] Patent Document 1 discloses highly isotactic poly(3-hydroxybutyric acid) obtained by ring-opening polymerization of a cyclic dimer of 3-hydroxybutyric acid. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] U.S. Pat. No. 1,095,435 Summary of the Invention [Problem to be solved by the invention]
[0005] However, Patent Document 1 does not specify the amount of unsaturated groups and the terminal structure of the obtained poly(3-hydroxybutyric acid).
[0006] The present invention has been made to solve the above-mentioned problems, and aims to provide a poly(hydroxyalkanoic acid) which contains only a small amount of unsaturated groups (decomposition products) and has terminal groups which are reactive groups such as hydroxyl groups and carboxyl groups, and therefore can be further chemically modified and has a wide range of applications, and a method for producing the same. [Means for solving the problem]
[0007] The present disclosure includes the following embodiments [1] to
[10] . [1] A poly(hydroxyalkanoic acid) comprising at least one hydroxyalkanoic acid unit, The terminal groups of the poly(hydroxyalkanoic acid) are a hydroxy group and a carboxyl group; The poly(hydroxyalkanoic acid) contains a unit having an unsaturated bond in a ratio of 0.2 mol % or less based on the total constitutional units of the poly(hydroxyalkanoic acid), The poly(hydroxyalkanoic acid) has a number average molecular weight of 1,000 to 20,000; The poly(hydroxyalkanoic acid) is characterized in that the isotacticity of the hydroxyalkanoic acid is 98.0 to 100%. [2] The poly(hydroxyalkanoic acid) according to [1], wherein the unit having an unsaturated bond is a carboxylic acid unit having an unsaturated bond. [3] The hydroxyalkanoic acid is 3-hydroxybutyric acid; The poly(hydroxyalkanoic acid) according to [1] or [2], wherein the poly(hydroxyalkanoic acid) is poly(3-hydroxybutyric acid). [4] A method for producing the poly(hydroxyalkanoic acid) according to any one of [1] to [3], A method for producing a poly(hydroxyalkanoic acid), comprising the step of subjecting at least one hydroxyalkanoic acid to an esterification reaction using a catalyst comprising a phosphine and a sulfonic acid. [5] The method for producing a poly(hydroxyalkanoic acid) according to [4], further comprising a washing step using acetone. [6] An amidation product obtained by using the poly(hydroxyalkanoic acid) according to any one of [1] to [3]. [7] A polyurethane obtained by using the poly(hydroxyalkanoic acid) according to any one of [1] to [3]. [8] A resin composition comprising the poly(hydroxyalkanoic acid) according to any one of [1] to [3]. [9] A cured resin product of the resin composition described in [8].
[10] A sheet or film comprising the cured resin described in [9]. Effect of the Invention
[0008] According to the present invention, it is possible to provide a poly(hydroxyalkanoic acid) which contains only a small amount of unsaturated groups (decomposition products) and has terminal groups which are reactive groups such as hydroxyl groups and carboxyl groups, and therefore can be further chemically modified, thereby expanding the range of applications, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described in more detail below. Note that the present invention is not limited to the following embodiments.
[0010] "~" means greater than or equal to the value before the "~", and less than or equal to the value after the "~".
[0011] (Poly(hydroxyalkanoic acid)) A poly(hydroxyalkanoic acid) according to one embodiment of the present invention (a poly(hydroxyalkanoic acid) according to the present embodiment) is a poly(hydroxyalkanoic acid) composed of at least one type of hydroxyalkanoic acid unit. The terminal groups of the poly(hydroxyalkanoic acid) are a hydroxy group and a carboxyl group. The poly(hydroxyalkanoic acid) contains a unit having an unsaturated bond in a ratio of 0.2 mol % or less based on the total constituent units of the poly(hydroxyalkanoic acid). The number average molecular weight of the poly(hydroxyalkanoic acid) is 1,000 to 20,000. The isotacticity of the hydroxyalkanoic acid is 98.0 to 100%.
[0012] The term "hydroxyalkanoic acid unit" (or "structural unit derived from hydroxyalkanoic acid") means one residue of hydroxyalkanoic acid in poly(hydroxyalkanoic acid), specifically, the structure obtained by removing the hydrogen atom in the hydroxy group and the hydroxy residue in the carboxyl group of the hydroxyalkanoic acid. The hydroxyalkanoic acid according to the present embodiment is preferably 3-hydroxybutyric acid. A "unit having an unsaturated bond" (or a "structural unit derived from a compound having an unsaturated bond") is a structural unit other than a hydroxyalkanoic acid unit in a poly(hydroxyalkanoic acid), and refers to one residue of a compound having an unsaturated bond. For example, when the compound having an unsaturated bond is a carboxylic acid having an unsaturated bond, the unit having an unsaturated bond refers to a structure obtained by removing the hydroxy residue in the carboxyl group of the carboxylic acid having an unsaturated bond. The unit having an unsaturated bond according to this embodiment may be a carboxylic acid unit having an unsaturated bond, such as crotonic acid.
[0013] "All structural units of poly(hydroxyalkanoic acid)" means the sum of the number of moles of structural units derived from all monomers constituting poly(hydroxyalkanoic acid). In addition, when the poly(hydroxyalkanoic acid) of the present embodiment contains a hydroxyalkanoic acid unit and a unit having an unsaturated bond, the total structural units of poly(hydroxyalkanoic acid) are the sum of the hydroxyalkanoic acid unit and the unit having an unsaturated bond. The poly(hydroxyalkanoic acid) contains a unit having an unsaturated bond at a ratio of 0.2 mol% or less, preferably at a ratio of 0.18 mol% or less, more preferably at a ratio of 0.15 mol% or less, and even more preferably at a ratio of 0.1 mol% or less, based on the total structural units of poly(hydroxyalkanoic acid). In addition, it may contain a ratio of 0.0001 mol% or more, may contain a ratio of 0.001 mol% or more, or may contain a ratio of 0.01 mol%. When the unit having an unsaturated bond is contained at a ratio of 0.2 mol% or less, it can be substantially ignored when further chemical modification is performed, and the application can be expanded. In this embodiment, the poly(hydroxyalkanoic acid) may be substantially free of units having unsaturated bonds. In the present invention, the phrase "substantially free of units having unsaturated bonds" means that the poly(hydroxyalkanoic acid) may contain units having unsaturated bonds in a proportion of less than 0.01 mol%, less than 0.001 mol%, or less than 0.001 mol% based on the total constituent units of the poly(hydroxyalkanoic acid).
[0014] The poly(hydroxyalkanoic acid) of the present embodiment is a poly(hydroxyalkanoic acid) in which hydroxyalkanoic acid units are successively ester-linked, specifically, a structure in which hydrogen atoms in the hydroxyl groups of hydroxyalkanoic acid and hydroxyl residues in the carboxyl groups are removed is a poly(hydroxyalkanoic acid) in which successive ester bonds are formed. The terminal groups of the poly(hydroxyalkanoic acid) are a hydroxyl group and a carboxyl group.
[0015] [Hydroxyalkanoic acid] Examples of the hydroxyalkanoic acid (HA) according to the present embodiment include glycolic acid, 2-hydroxypropanoic acid (lactic acid), 3-hydroxypropanoic acid, 2-hydroxybutanoic acid (2-hydroxybutyric acid), 3-hydroxybutyric acid, 4-hydroxybutanoic acid, 3-hydroxy-3-methyl-butanoic acid, 2-hydroxypentanoic acid (2-hydroxyvaleric acid), 3-hydroxypentanoic acid, 5-hydroxypentanoic acid, 2-hydroxy-2-methyl-pentanoic acid, 3-hydroxyhexanoic acid, 6-hydroxyhexanoic acid, 6-hydroxyheptanoic acid, 3-hydroxyheptanoic acid, 7-hydroxyheptanoic acid, 3-hydroxyoctanoic acid, 8-hydroxyoctanoic acid, 3-hydroxynonanoic acid, 9-hydroxynonanoic acid, 3-hydroxydecanoic acid, and 10-hydroxydecanoic acid. 1-6 Hydroxy C, optionally having an alkyl group 2-15 Examples include alkanoic acid, 12-hydroxystearic acid, and ricinoleic acid.
[0016] The hydroxyalkanoic acid (HA) may be a corresponding lactone. Examples of lactones include di-C lactones such as β-butyrolactone, β-propiolactone, β-dimethylpropiolactone, γ-butyrolactone, γ-dimethylbutyrolactone, δ-valerolactone, and ε-caprolactone. 1-12 C which may have an alkyl group 3-15 Lactones, etc.
[0017] These hydroxyalkanoic acids and lactones can be used alone or in combination of two or more. Among these hydroxyalkanoic acids, hydroxyalkanoic acids such as 3-hydroxybutyric acid, 3-hydroxypropanoic acid, 4-hydroxybutanoic acid, 3-hydroxyvaleric acid, 3-hydroxyhexanoic acid, 6-hydroxyhexanoic acid, 3-hydroxyheptanoic acid, 3-hydroxyoctanoic acid, 3-hydroxynonanoic acid, and 3-hydroxydecanoic acid are preferred from the viewpoint of biodegradability. 3-10 Alkanoic acid (hydroxy C other than 3-hydroxybutyric acid) 3-10 Alkanoic acid units) or the corresponding lactones are preferred.
[0018] The hydroxyalkanoic acid (HA) according to this embodiment is preferably 3-hydroxybutyric acid (3HB). The 3-hydroxybutyric acid of the present invention may be any of the racemic, (R) and (S) forms. It is particularly preferable to use the (R) form since it has high biodegradability, mechanical properties and melting point.
[0019] Although not particularly limited, suitable examples of the poly(hydroxyalkanoic acid) of the present embodiment include those represented by the following formula (1) and formula (2).
[0020] [ka] (In formula (1), each R independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and o represents a positive integer.)
[0021] In the above formula (1), R in the o hydroxyalkanoic acid units may be the same or different. R in each hydroxyalkanoic acid unit may independently represent a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. R preferably represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and further preferably a methyl group.
[0022] [ka] (In formula (2), R 1 , R 2 are different and each independently represent a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; o, p, and q each independently represent a positive integer.
[0023] In the above formula (2), R 1 , R 2 R each independently preferably represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and more preferably represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. 1 , R 2It is more preferable that one of them is a methyl group.
[0024] [Compounds with unsaturated bonds] The compound having an unsaturated bond according to the present embodiment is not particularly limited as long as it is a compound that reacts with the hydroxyalkanoic acid to become one unit of the poly(hydroxyalkanoic acid). Examples of the unit compound having an unsaturated bond include a carboxylic acid having an unsaturated bond and an alcohol having an unsaturated bond. Examples of carboxylic acids having an unsaturated bond include crotonic acid, acrylic acid, methacrylic acid, eicosadienoic acid, mead acid, eicosatetraenoic acid, arachidonic acid, docosatetraenoic acid, docosapentaenoic acid, and docosapentaenoic acid. Examples of alcohols having an unsaturated bond include allyl alcohol, crotyl alcohol (2-buten-1-ol), cinnamyl alcohol (3-phenyl-2-propen-1-ol), methallyl alcohol (2-methyl-2-propen-1-ol), 3-buten-2-ol, 2-cyclohexen-1-ol, 3-buten-1-ol, 4-penten-1-ol, and 5-hexen-1-ol.
[0025] [Structure and properties of poly(hydroxyalkanoic acid)] "Isotaxi" The poly(hydroxyalkanoic acid) of the present embodiment preferably has high isotacticity (stereoregularity). The isotacticity is preferably 98% or more, and more preferably 99% or more. When the isotacticity is 98%, the poly(hydroxyalkanoic acid) exhibits high crystallinity and exhibits functions such as a high melting point and mechanical properties. Isotaxy can be evaluated by the method described in the Examples below.
[0026] "Number average molecular weight" The number average molecular weight (Mn) of the poly(hydroxyalkanoic acid) of the present embodiment is preferably 1,000 or more, more preferably 2,000 or more, and even more preferably 3,000 or more, and is preferably 20,000 or less, more preferably 15,000 or less, and even more preferably 10,000 or less. When the molecular weight is 1,000 or more, the crystallinity derived from the continuous hydroxyalkanoic acid gives rise to functions such as a high melting point and mechanical properties. When the molecular weight is 20,000 or less, the polymer exhibits moderate solubility and is easy to further chemically modify.
[0027] (Method of producing poly(hydroxyalkanoic acid)) The method for producing a poly(hydroxyalkanoic acid) of one embodiment of the present invention (sometimes referred to as a method for producing a poly(hydroxyalkanoic acid) of the present embodiment or a production method of the present embodiment) is not particularly limited, and examples thereof include a method in which at least one hydroxyalkanoic acid is subjected to a dehydration esterification reaction using a catalyst consisting of a phosphine and a sulfonic acid.
[0028] [Hydroxyalkanoic acid] The hydroxyalkanoic acid used in the production method of this embodiment is the same as that explained in the [Hydroxyalkanoic acid] explained above regarding the poly(hydroxyalkanoic acid) of this embodiment, and preferred examples thereof are also the same.
[0029] [Phosphine] Examples of the phosphine used in the production method of this embodiment include triarylphosphines such as triphenylphosphine, polymer-supported triphenylphosphine (PB-PPh3), tri(o-tolyl)phosphine, and tris(2-methoxyphenyl)phosphine; and trialkylphosphines such as trimethylphosphine, triethylphosphine, tri-n-butylphosphine, tri(tert-butyl)phosphine, and tricyclohexylphosphine. From the viewpoints of safety and ease of handling, the phosphine used in the production method of this embodiment is preferably a triarylphosphine, and more preferably triphenylphosphine or polymer-supported triphenylphosphine (PB-PPh3). The amount of phosphine used is preferably 0.001 mol or more, more preferably 0.05 mol or more, and even more preferably 0.01 mol or more, relative to 100 mol of hydroxyalkanoic acid, and is preferably 10 mol or less, more preferably 6 mol or less, and even more preferably 5.5 mol or less.
[0030] In the production method of the present embodiment, the method of adding the phosphine is not particularly limited, and the phosphine may be added all at once or in several portions. The order of addition of the hydroxyalkanoic acid and the sulfonic acid described below is also not particularly limited, and the phosphine may be mixed with other raw materials first and then reacted, or the phosphine may be reacted first and then added to the mixture during or after the reaction. From the viewpoint of ease of controlling the reaction, it is preferable to first mix the hydroxyalkanoic acid and the sulfonic acid described below, and then react the mixture.
[0031] [Sulfonic acid] Examples of the sulfonic acid used in the manufacturing method of the present embodiment include organic sulfonic acid compounds. Examples of the organic sulfonic acid compounds include aliphatic sulfonic acids such as methanesulfonic acid, ethanesulfonic acid, and butanesulfonic acid, and aromatic sulfonic acids such as benzenesulfonic acid, p-toluenesulfonic acid, naphthalene-α-sulfonic acid, and naphthalene-β-sulfonic acid. Among them, aromatic sulfonic acids are preferred, and p-toluenesulfonic acid is more preferred, from the viewpoints of solubility in organic solvents and affinity with poly(hydroxyalkanoic acid). In the production method of this embodiment, the method of adding the sulfonic acid is not particularly limited, and the sulfonic acid may be added all at once or in several portions.
[0032] The amount of sulfonic acid used is preferably 0.001 mol or more, more preferably 0.05 mol or more, and even more preferably 0.01 mol or more, per 100 mol of hydroxyalkanoic acid, and is preferably 10 mol or less, more preferably 6 mol or less, and even more preferably 5.5 mol or less.
[0033] [Other catalysts] In the production method of this embodiment, other catalysts may be used in combination, such as metal catalysts, base catalysts, and acid catalysts (excluding sulfonic acid). Examples of the metal catalyst include metal compounds containing alkali metals (such as sodium), alkaline earth metals (such as magnesium, calcium, barium, etc.), transition metals (such as manganese, zinc, cadmium, lead, cobalt, titanium, etc.), metals in Group 13 of the periodic table (such as aluminum), metals in Group 14 of the periodic table (such as germanium, tin), and metals in Group 15 of the periodic table (such as antimony). Examples of the base catalyst include tertiary amines (trialkylamines such as trimethylamine and triethylamine, quaternary ammonium salts (tetraalkylammonium halides such as tetraethylammonium chloride and tetraethylammonium bromide, benzyltrialkylammonium halides such as benzyltrimethylammonium chloride, etc.)). Examples of the acid catalyst include inorganic acids (eg, sulfuric acid, hydrogen chloride (or hydrochloric acid), nitric acid, phosphoric acid, etc.) and organic acids.
[0034] [Reaction conditions] In the production method of this embodiment, the esterification reaction may be carried out in the presence or absence of a solvent. Examples of the solvent include hydrocarbons (aliphatic hydrocarbons such as hexane, octane, and cyclohexane, and aromatic hydrocarbons such as toluene, xylene mesitylene, tetralin, chlorobenzene, o-dichlorobenzene, and 1,2,4-trichlorobenzene), halogenated hydrocarbons (dichloromethane, chloroform, carbon tetrachloride, and dichloroethane), ethers (dioxane, tetrahydrofuran, and diphenyl ether), ketones (acetone, methyl ethyl ketone, and the like), esters (methyl acetate, ethyl acetate, and butyl acetate, and the like), amides (dimethylformamide, diethylformamide, dimethylacetamide, diethylacetamide, and N-methylpyrrolidone, and the like), sulfoxides (dimethyl sulfoxide, and the like), and cellosolve acetates (C such as ethyl cellosolve acetate). 1-4 Alkyl cellosolve acetate, etc. These solvents can be used alone or in combination of two or more. In the production method of this embodiment, for example, it is preferable to use halogenated hydrocarbons, and it is more preferable to use dichloroethane such as 1,2-dichloroethane (DCE).
[0035] The reaction atmosphere may be air or an inert gas (nitrogen, helium, etc.) atmosphere, and the synthesis reaction pressure may be normal pressure or reduced pressure. The reaction can be facilitated by distilling water produced in the esterification reaction out of the reaction system. The manufacturing method of this embodiment is preferably carried out in a nitrogen atmosphere, for example.
[0036] The synthesis reaction temperature and reaction time can be appropriately selected depending on the type of raw material used, etc. For example, the reaction may be carried out at a temperature of 80 to 100° C. for 10 to 50 hours.
[0037] [Refining process] The production method of this embodiment preferably further includes a purification step. The purification step may include washing and centrifuging the crude poly(hydroxyalkanoic acid) synthesized by the above method with an organic solvent such as acetone, etc. The washing and centrifuging steps may be repeated 1 to 5 times.
[0038] (polyamide) An application example of the poly(hydroxyalkanoic acid) of the present embodiment includes, for example, a polyamide derived from the poly(hydroxyalkanoic acid) of the present embodiment (sometimes referred to as the "polyamide according to the present embodiment") obtained using the poly(hydroxyalkanoic acid) of the present embodiment. The polyamide according to this embodiment can be synthesized, for example, by the following method. First step: a step of introducing adipic acid into the hydroxyl terminal of the poly(hydroxyalkanoic acid) of the present embodiment to obtain adipic acid-terminated poly(hydroxyalkanoic acid); The second step is to react the adipic acid-terminated poly(hydroxyalkanoic acid) with a diamine such as polybutylene succinate (PBS) having amines at both ends to form a polyamide.
[0039] (Polyurethane) An application example of the poly(hydroxyalkanoic acid) of the present embodiment includes, for example, a polyurethane derived from the poly(hydroxyalkanoic acid) of the present embodiment (sometimes referred to as the "polyurethane of the present embodiment") obtained using the poly(hydroxyalkanoic acid) of the present embodiment. The polyurethane according to the present embodiment can be obtained, for example, by reacting the poly(hydroxyalkanoic acid) according to the present embodiment with a polyisocyanate. If necessary, a polyol other than the poly(hydroxyalkanoic acid) according to the present embodiment, a chain extender, a chain terminator, or a crosslinking agent may be used in combination. The poly(hydroxyalkanoic acid) according to the present embodiment for obtaining the polyurethane is preferably a polyester polyol. Specifically, the polyurethane according to this embodiment is obtained by reacting a polyol with a polyisocyanate, and at least the poly(hydroxyalkanoic acid) according to this embodiment is used as the polyol. Thus, the polyurethane is a reaction product obtained by reacting a polyol with a polyisocyanate, and the polyurethane has a constitutional unit derived from the polyol and a constitutional unit derived from the polyisocyanate, and at least has a constitutional unit derived from the poly(hydroxyalkanoic acid) according to this embodiment.
[0040] Examples of the chain extender include aliphatic polyol compounds such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, hexamethylene glycol, saccharose, methylene glycol, glycerin, sorbitol, and neopentyl glycol; aromatic polyol compounds such as bisphenol A, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl sulfone, hydrogenated bisphenol A, and hydroquinone; Examples of the chain extenders include aliphatic polyol compounds; water; and amine compounds such as ethylenediamine, 1,2-propanediamine, 1,6-hexamethylenediamine, piperazine, 2-methylpiperazine, 2,5-dimethylpiperazine, isophoronediamine, 4,4'-dicyclohexylmethanediamine, 3,3'-dimethyl-4,4'-dicyclohexylmethanediamine, 1,2-cyclohexanediamine, 1,4-cyclohexanediamine, aminoethylethanolamine, hydrazine, diethylenetriamine, and triethylenetetramine. These chain extenders may be used alone or in combination of two or more. Among these, aliphatic polyol compounds are preferred, and neopentyl glycol is more preferred.
[0041] The content of the poly(hydroxyalkanoic acid) of the present embodiment in 100% by mass of all polyols used in the polyurethane synthesis is preferably 10 to 100% by mass, and more preferably 50 to 100% by mass.
[0042] Examples of polyisocyanates include 1,3- and 1,4-phenylene diisocyanate, 1-methyl-2,4-phenylene diisocyanate, 1-methyl-2,6-phenylene diisocyanate, 1-methyl-2,5-phenylene diisocyanate, 1-methyl-2,6-phenylene diisocyanate, 1-methyl-3,5-phenylene diisocyanate, 1-ethyl-2,4-phenylene diisocyanate, 1-isopropyl-2,4 -phenylene diisocyanate, 1,3-dimethyl-2,4-phenylene diisocyanate, 1,3-dimethyl-4,6-phenylene diisocyanate, 1,4-dimethyl-2,5-phenylene diisocyanate, diethylbenzene diisocyanate, diisopropylbenzene diisocyanate, 1-methyl-3,5-diethylbenzene diisocyanate, 3-methyl-1,5-diethylbenzene-2,4-diisocyanate, 1,3,5- Triethylbenzene-2,4-diisocyanate, naphthalene-1,4-diisocyanate, naphthalene-1,5-diisocyanate, 1-methyl-naphthalene-1,5-diisocyanate, naphthalene-2,6-diisocyanate, naphthalene-2,7-diisocyanate, 1,1-dinaphthyl-2,2'-diisocyanate, biphenyl-2,4'-diisocyanate, biphenyl-4,4'-diisocyanate, 3-3'-dimethylbiisocyanate Aromatic polyisocyanates such as phenyl-4,4'-diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, diphenylmethane-2,4-diisocyanate, and toluene diisocyanate; aliphatic polyisocyanates such as tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate, dodecamethylene diisocyanate, and trimethylhexamethylene diisocyanate;Alicyclic polyisocyanates such as 1,3-cyclopentylene diisocyanate, 1,3-cyclohexylene diisocyanate, 1,4-cyclohexylene diisocyanate, 1,3-di(isocyanatemethyl)cyclohexane, 1,4-di(isocyanatemethyl)cyclohexane, lysine diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 2,4'-dicyclohexylmethane diisocyanate, 2,2'-dicyclohexylmethane diisocyanate, and 3,3'-dimethyl-4,4'-dicyclohexylmethane diisocyanate can be used. These may be used alone or in combination of two or more. Among them, 1,6-hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-diphenylmethane diisocyanate, and toluene diisocyanate are more preferred.;
[0043] In order to control the molecular weight of the resulting polyurethane, a chain terminator having one active hydrogen group may be used as necessary. Examples of these chain terminators include aliphatic monohydroxy compounds having a hydroxyl group, such as methanol, ethanol, propanol, butanol, and hexanol, and aliphatic monoamines having an amino group, such as morpholine, diethylamine, dibutylamine, monoethanolamine, and diethanolamine. These may be used alone or in combination of two or more.
[0044] For the purpose of increasing the heat resistance and strength of the resulting polyurethane, a crosslinking agent having three or more active hydrogen groups or isocyanate groups can be used as necessary.
[0045] The polyurethane according to the present embodiment can be obtained by a known polyurethane manufacturing method. Specifically, for example, a manufacturing method can be mentioned in which a polyol, a polyisocyanate, and the chain extender are charged and reacted. These reactions are preferably carried out at a temperature of 50 to 100°C for 3 to 10 hours. The reaction may also be carried out in an organic solvent.
[0046] Examples of the organic solvent that can be used include ketone solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, methyl ethyl ketone, methyl-n-propyl ketone, acetone, and methyl isobutyl ketone; ester solvents such as methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, isopropyl acetate, isobutyl acetate, isobutyl acetate, and sec-butyl acetate; etc. These organic solvents may be used alone or in combination of two or more.
[0047] The content of the structural unit derived from the poly(hydroxyalkanoic acid) of this embodiment in 100% by mass of the polyurethane of this embodiment is preferably 10 to 98% by mass, and more preferably 20 to 98% by mass, which tends to more suitably obtain the effects. In this specification, the content of each structural unit in the polyurethane is measured by NMR.
[0048] The number average molecular weight (Mn) of the polyurethane according to this embodiment may have a lower limit of 5,000 or more, 6,000 or more, 7,000 or more, 8,000 or more, or 10,000 or more, and an upper limit of 1,000,000 or less, 500,000 or less, 100,000 or less, 500,000 or less, or 15,000 or less. Any combination of these upper and lower limits may be used. The number average molecular weight (Mn) of the polyurethane may be 5,000 to 1,000,000, 6,000 to 500,000, 7,000 to 100,000, 8,000 to 500,000, or 10,000 to 15,000. Within the above range, the effect tends to be more favorably obtained.In this specification, the number average molecular weight (Mn) of the polyurethane is a value measured by GPC.
[0049] (Resin composition) Examples of the resin composition of this embodiment include a thermoplastic resin composition containing the poly(hydroxyalkanoic acid) of this embodiment described above and polyurethane, and a thermosetting resin composition.
[0050] <Thermoplastic resin composition> When the resin composition of the present embodiment is a thermoplastic resin composition, it may further contain, for example, other resins, a crystallization nucleating agent, a heat stabilizer, a hydrolysis inhibitor, other additives, and the like, as necessary.
[0051] [Crystallization nucleating agent] The crystallization nucleating agent used in the thermoplastic resin composition according to the present embodiment may be any crystallization nucleating agent used in thermoplastic resins derived from biomass resources, such as polylactic acid and polybutylene succinate. For example, talc-based nucleating agents, nucleating agents made of metal salt-based materials having a phenyl group, and nucleating agents made of benzoyl compounds are preferably used. Other known crystallization nucleating agents, such as lactate, benzoate, silica, and phosphate salts, may also be used.
[0052] [Heat stabilizers and hydrolysis inhibitors] The thermoplastic resin composition of the present embodiment preferably contains a phenol-based antioxidant and a phosphite-based antioxidant as a heat stabilizer for the resin composition, and a carbodiimide compound-based hydrolysis inhibitor, such as polycarbodiimide resin (product name: Carbodilite, manufactured by Nisshinbo Chemical Co., Ltd.), as a hydrolysis inhibitor. The heat stabilizer and hydrolysis inhibitor to be added may be one selected from the above three types of additives, but the above two types of heat stabilizers and hydrolysis inhibitors have different functions, and it is preferable that each additive is added together. The amount of heat stabilizer and hydrolysis inhibitor to be added varies depending on the type, but generally, it is preferable that each is about 0.1 to 5 parts by mass per 100 parts by mass of the thermoplastic resin composition.
[0053] [Other additives] It is preferable to further add a silicone-based flame retardant, an organometallic salt-based flame retardant, an organophosphorus-based flame retardant, a metal oxide-based flame retardant, a metal hydroxide-based flame retardant, etc. to the thermoplastic resin composition of this embodiment, which improves the flame retardancy and inhibits the spread of fire, and also improves the fluidity of the biodegradable resin composition, thereby ensuring better moldability.
[0054] A filler can be added to the thermoplastic resin composition of the present embodiment. Examples of the filler include talc, mica, montmorillonite, and kaolin. These fillers act as crystal nuclei to promote crystallization of the poly(hydroxyalkanoic acid), improving the impact strength and heat resistance of the molded article. In addition, the rigidity of the molded article can be increased.
[0055] The thermoplastic resin composition of the present embodiment may be appropriately blended with various additives such as antioxidants, antiblocking agents, colorants, flame retardants, release agents, antifogging agents, surface wettability improvers, incineration aids, lubricants, dispersion aids, various surfactants, plasticizers, compatibilizers, weather resistance improvers, ultraviolet absorbers, processing aids, antistatic agents, colorants, lubricants, and release agents. As the plasticizer, any known plasticizer generally used as a plasticizer for polymers can be used without particular limitation, and examples thereof include polyester plasticizers, glycerin-based plasticizers, polyvalent carboxylic acid ester-based plasticizers, polyalkylene glycol-based plasticizers, and epoxy-based plasticizers. There are no particular limitations on the compatibilizer as long as it functions as a compatibilizer for copolymer A and copolymer B. Examples of the compatibilizer include inorganic fillers, glycidyl compounds, polymer compounds grafted or copolymerized with acid anhydrides, and organometallic compounds, and one or more of these may be used. By kneading these materials, the heat resistance, bending strength, impact strength, flame retardancy, etc. are improved, which further promotes the application of the materials to molded articles such as housings for electronic devices, such as notebook computers and mobile phones.
[0056] In addition, various fillers known in the art can be blended as the filler. As functional additives, chemical fertilizers, soil conditioners, plant activators, etc. can also be added. The fillers are broadly classified into inorganic fillers and organic fillers. These can be used alone or in a mixture of two or more kinds.
[0057] Examples of inorganic fillers include anhydrous silica, mica, talc, titanium oxide, calcium carbonate, diatomaceous earth, allophane, bentonite, potassium titanate, zeolite, sepiolite, smectite, kaolin, kaolinite, glass, limestone, carbon, wollastonite, calcined perlite, silicates such as calcium silicate and sodium silicate, hydroxides such as aluminum oxide, magnesium carbonate and calcium hydroxide, salts such as ferric carbonate, zinc oxide, iron oxide, aluminum phosphate and barium sulfate, etc. The content of the inorganic filler in the entire composition is usually 1 to 80% by weight, preferably 3 to 70% by weight, and more preferably 5 to 60% by weight. Examples of organic fillers include raw starch, processed starch, pulp, chitin, chitosan, coconut shell powder, wood powder, bamboo powder, bark powder, kenaf powder, straw powder, etc. These can be used alone or in a mixture of two or more. The amount of organic filler added is usually 0.01 to 70% by weight of the total composition.
[0058] The composition can be prepared by any of the conventionally known mixing / kneading techniques. As the mixer, a horizontal cylindrical type, V-shaped type, double cone type mixer, a blender such as a ribbon blender or a super mixer, or various continuous mixers can be used. As the kneader, a batch type kneader such as a roll or an internal mixer, a one-stage type or two-stage type continuous kneader, a twin screw extruder, a single screw extruder, or the like can be used. As the kneading method, a method of adding various additives, fillers, and thermoplastic resins to the heated and melted material and blending them can be mentioned. In addition, a blending oil or the like can be used for the purpose of uniformly dispersing the various additives.
[0059] <Thermosetting resin composition> When the resin composition of the present embodiment is a thermosetting resin composition, it contains, for example, another resin, a poly(hydroxyalkanoic acid) of the present embodiment having reactive groups such as a hydroxyl group or a carboxyl group as a thermosetting resin main component, and further contains a curing agent such as an isocyanate curing agent or a polyamine curing agent that can thermally react with the reactive groups.
[0060] Examples of the curing agent according to the present embodiment include polyisocyanates having an aromatic structure in their molecular structure, such as tolylene diisocyanate, diphenylmethane diisocyanate, polymeric diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, triphenylmethane triisocyanate, and xylylene diisocyanate, and compounds in which a part of the isocyanate groups of these polyisocyanates is modified with carbodiimide; allophanate compounds derived from these polyisocyanates; polyisocyanates having an alicyclic structure in their molecular structure, such as isophorone diisocyanate, 4,4'-methylenebis(cyclohexylisocyanate), and 1,3-(isocyanatomethyl)cyclohexane; linear aliphatic polyisocyanates, such as 1,6-hexamethylene diisocyanate, lysine diisocyanate, and trimethylhexamethylene diisocyanate, and allophane derivatives thereof. allophanate forms derived from these polyisocyanates; biuret forms derived from these polyisocyanates; trimethylolpropane-modified adducts; polyfunctional isocyanates such as polyisocyanates which are reaction products of the above-mentioned various polyisocyanates with polyol components; polyethylene polyamines such as ethylene diamine, diethylene triamine, triethylene tetramine, tetraethylene pentamine, pentaethylene hexamine, hexaethylene heptamine, heptaethylene octamine, octaethylene nonamine, nonaethylene decamine, piperazine, and N-aminoalkyl piperazines having an alkyl chain with 2 to 6 carbon atoms; and amine compounds such as 3-aminomethyl-3,5,5-trimethylcyclohexylamine (isophorone diamine, or IPDA).
[0061] <Cured product of resin composition> The cured product of the resin composition of the present embodiment is a cured product of the resin composition as the above-mentioned thermoplastic resin composition, or a cured product of the resin composition as the above-mentioned thermosetting resin composition.
[0062] The poly(hydroxyalkanoic acid) in this specification can be used for various applications. Specifically, it can be used for a wide range of applications, such as artificial leather, synthetic leather, shoes, thermoplastic resins, foamed resins, thermosetting resins, paints, laminating adhesives, elastic fibers, urethane raw materials, automobile parts, and sporting goods. Since the poly(hydroxyalkanoic acid) of this embodiment, which has excellent biodegradability, is used, the products for the above applications have excellent biodegradability.
[0063] The polyurethanes in this specification can be used in a variety of applications. Specifically, they can be used in a wide range of applications, such as artificial leather, synthetic leather, shoes, thermoplastic resins, foamed resins, thermosetting resins, paints, laminating adhesives, vibration-proofing materials, vibration-damping materials, automobile parts, sporting goods, fiber treatment agents, binders, etc. Since the poly(hydroxyalkanoic acid) of this embodiment, which has excellent biodegradability, is used, the products for the above applications have excellent biodegradability.
[0064] The resin composition in the present specification can be used for various applications. Specifically, it can be used for a wide range of applications, such as artificial leather, synthetic leather, shoes, thermoplastic resins, foamed resins, thermosetting resins, paints, laminating adhesives, vibration-proofing materials, vibration-damping materials, automobile parts, sporting goods, fiber treatment agents, binders, etc. Since the poly(hydroxyalkanoic acid) of the present embodiment, which has excellent biodegradability, is used, the products for the above applications have excellent biodegradability.
[0065] (Coating agent) The coating agent contains the poly(hydroxyalkanoic acid) of this embodiment, and further contains other components such as other resins, water, and organic solvents, as necessary.
[0066] The coating agent can be applied to various substrates. An example of the application of the coating agent will be described below. The coating agent is used, for example, for surface coating of the substrate of a food packaging container. Examples of the substrate include plastic films such as styrene-based resin films, polyolefin-based resin films, polyester-based resin films, nylon-based resin films, and laminates thereof. Examples of the substrate include paper, metal-deposited films, aluminum foils, and the like. The coating agent is preferably used for biodegradable substrates. Examples of the biodegradable substrate include paper, polyester-based films, polyolefin-based films, and starch-based films. The coating agent can be used as an ink, an adhesive, or the like.
[0067] (Ink) The ink contains the poly(hydroxyalkanoic acid) of this embodiment and a colorant, and further contains other components such as a pigment dispersant, water, and an organic solvent, as necessary. The ink is, for example, a printing ink. The ink may be, for example, a water-based ink or an ink that does not contain water (solvent-based ink).
[0068] (glue) The adhesive contains the poly(hydroxyalkanoic acid) of this embodiment, and further contains other components such as other resins, curing agents, and organic solvents, as necessary. The adhesive can also be used as an adhesive composition for lamination, which is laminated onto the various substrates described above to produce composite films used primarily as packaging materials for foods, medicines, detergents, and the like. Such adhesives may be, for example, a two-liquid curing adhesive containing the poly(hydroxyalkanoic acid) of the present embodiment, polyester polyol, and polyisocyanate, or a one-liquid adhesive made of an acrylic resin, a urethane resin, or an ethylene-vinyl acetate copolymer. These adhesives may be solvent-based, solventless, aqueous, or alcohol-based, depending on the need.
[0069] (Sheet) The sheet is made of a resin composition containing the poly(hydroxyalkanoic acid) of this embodiment. The resin composition may contain other resins and various additives in addition to the poly(hydroxyalkanoic acid) of this embodiment. Examples of the various additives include plasticizers, antistatic agents, antioxidants, ultraviolet absorbers, lubricants, antiblocking agents, and heat stabilizers. Examples of the sheet include a non-oriented sheet, a biaxially oriented sheet, and a foamed sheet. The uses of the sheet are not particularly limited, but it can be used in a wide range of applications, such as food packaging containers, construction materials, home electrical appliances, and miscellaneous goods.
[0070] (film) The film is made of a resin composition containing the poly(hydroxyalkanoic acid) of the present embodiment. The resin composition may contain other resins and various additives in addition to the poly(hydroxyalkanoic acid) of the present embodiment. Examples of the various additives include plasticizers, antistatic agents, antioxidants, ultraviolet absorbers, lubricants, antiblocking agents, and heat stabilizers. Examples of the film include unstretched films, biaxially stretched films, and uniaxially stretched films, and can be produced by, for example, melting pellets of the film raw material in an extruder and forming the film into a film using a T-die or inflation method. In the T-die method, a biaxially stretched film is obtained by performing longitudinal stretching using the speed difference between rolls and transverse stretching using a tenter.
[0071] (Laminate) The laminate comprises at least one selected from the sheet and film of the present embodiment, and further comprises other components such as a printed layer and a resin film as necessary. The laminate can be obtained, for example, by laminating a film or sheet to one or both sides of at least one selected from the sheets and films of the present embodiment in order to improve mechanical strength, chemical resistance, etc. Specifically, the laminate can be obtained by thermally laminating a polystyrene-based inflation film to at least one of the front side and back side of the sheet or film, or by laminating an olefin-based film (CPP) using an adhesive. The adhesive used is not particularly limited, and may be, for example, the adhesive of the present embodiment or a known adhesive.
[0072] (Molded body) The molded article can be obtained by molding at least one selected from the sheet, film, and laminate of the present embodiment. The molded article can be obtained, for example, by thermoforming the sheet, film, or laminate of the present embodiment. Examples of the thermoforming method include hot plate contact heat molding, vacuum molding, vacuum pressure molding, and plug assist molding, and in particular, indirect heat molding using an infrared heater as a heat source is preferably used. EXAMPLES
[0073] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto.
[0074] (raw materials) p-Toluenesulfonic acid (p-TsOH): (monohydrate, Fujifilm Wako Chemical) Polymer-supported triphenylphosphine (PB-PPh3): (3mmol / g or 1.6mmol / g, Sigma-Aldrich) 1,2-Dichloroethane (DCE): (Fujifilm Wako Chemical) Acetone: (Fujifilm Wako Chemical) Succinic acid: (Fujifilm Wako Chemical) 1,4-Butanediol: (Fujifilm Wako Chemical) N,N-Dimethylaminopyridine: (Fujifilm Wako Chemical) Dichloromethane: (Tokyo Chemical Industry Co., Ltd.) 1-Ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDCI·HCl): (Applo Scientific Limited) γ-(Boc-amino)butyric acid (Boc-GABA): (Tokyo Chemical Industry Co., Ltd.) N,N-Dimethylaminopyridine: (Fujifilm Wako Chemical) Trifluoroacetic acid (TFA): (Fujifilm Wako Chemical) Chloroform: (Fujifilm Wako Chemical) Sodium bicarbonate: (Fujifilm Wako Chemical) Adipic acid: (Fujifilm Wako Chemical) N,N-Diisopropylethylamine: (Tokyo Chemical Industry Co., Ltd.) 7-Aza-1-hydroxybenzotriazole (HOAt): (Tokyo Chemical Industry Co., Ltd.) Poly((R)-3-hydroxybutyric acid) (Mn 40,0000, manufactured by Aldrich)
[0075] (Evaluation method) [ 1 H-NMR spectrum measurement] Measurement equipment: JEOL RESONANCE "JNM-ECM400S" Magnetic field strength: 400MHz Solvent: Deuterated chloroform Sample concentration: 10mg / 1.0mL
[0076] [Calculation of unsaturated group content of poly(3-hydroxybutyric acid)] The unsaturated group content of poly(3-hydroxybutyric acid) is 1 Using the H-NMR spectrum data, the integral intensity (M) of the methyl group hydrogen signal (1.1 ppm) relative to the integral intensity (V) of the vinyl hydrogen signal (5.8 ppm) of the crotonoyl component was calculated based on the following formula (A). Unsaturated group content=3×V / M (A)
[0077] [Calculation of remaining hydroxyl groups in poly(3-hydroxybutyric acid)] The ratio was calculated based on the integral intensity (M) of the signal of the methyl group hydrogen relative to the integral intensity (H) of the signal of the α-position hydrogen of the hydroxyl group (4.2 ppm) according to the following formula (B). Residual hydroxyl group content = 3 × H / M (B)
[0078] <Calculation of the degree of polymerization of poly(3-hydroxybutyric acid)> The intensity was calculated based on the integral intensity (E) of the signal of the hydrogen at the α-position of the ester bond (5.2 ppm), the integral intensity (H) of the signal of the remaining hydroxyl group, and the integral intensity (V) of the signal of the vinyl hydrogen of the crotonoyl group, according to the following formula (C). Degree of polymerization = (V + H + E) / (V + H) (C)
[0079] <Taxis calculation> 1 Calculations were made based on the H-NMR spectrum data and on the formulas (D) and (E) shown below. The tacticity of poly((R)-3-hydroxybutyrate) was calculated from the integral intensity (S) of the syndiotactic component signal (d 1.31, d) relative to the integral intensity (I) of the methyl group signal of the isotactic component (d 1.27, d, J = 6.41 Hz) based on the following equation: Isotaxis = I / (I+S) (D) Shinjio Taxi City = S / (I+S) (E)
[0080] <Measurement of number average molecular weight (Mn)> In the examples and comparative examples, the molecular weight of the resin was measured by gel permeation chromatography (GPC) under the following conditions. Measurement equipment: System controller Waters 600 Controller Liquid delivery pump Waters Model Code 60F RI (Differential Refractometer) Detector Waters 2414 Autosampler Waters 717plus Autosampler
[0081] Data processing: Waters Empower3 Measurement conditions Measurement conditions: Column temperature 40℃ Eluent: Chloroform (CHCl3) Flow rate 1.0ml / min Standard: Polystyrene Column: Shodex GPC LF-G x 1 Shodex GPC LF-804 4 pieces Sample: 100 μl of chloroform solution (0.4% by mass, calculated as resin solid content) filtered through a microfilter
[0082] Example 1 "Synthesis of poly(3-hydroxybutyric acid)" p-Toluenesulfonic acid (p-TsOH) (12 mg, 63 mmol) and polymer-supported triphenylphosphine (PB-PPh3) (3 mmol / g; 18 mg, 54 mmol) were weighed into a reaction tube. (R)-3-hydroxybutyric acid (400 mg, 3.85 mmol) was then added. The atmosphere in the reaction vessel was replaced with nitrogen. Under a nitrogen stream, 1,2-dichloroethane (DCE) (0.5 mL) was added using a syringe. The reaction tube was heated to 100°C and stirred. After 22 hours, p-toluenesulfonic acid (24 mg, 126 mmol), PB-PPh3 (3 mmol / g; 36 mg, 108 mmol), and DCE (0.5 mL) were added, and the mixture was heated and stirred again. After 22 hours, p-TsOH (24 mg, 126 mmol), PB-PPh3 (3 mmol / g; 36 mg, 108 mmol), and DCE (0.5 mL) were added and heated and stirred again. After 3 days, DCE (0.5 mL) was added and stirred for 18 hours, after which heating was stopped. The reaction mixture was cooled to room temperature and concentrated to obtain a white solid. Acetone (15 mL) was added to the mixture, and the resulting suspension was transferred to a polypropylene centrifuge tube. After ultrasonic irradiation, the solid was precipitated by centrifugation (6,000 rpm, 5 minutes), and the supernatant was removed by decantation. The acetone washing and centrifugation steps were repeated three times, and then the mixture was dried under reduced pressure to obtain (R)-3HB oligomer (306 mg) as a white solid as the ester (poly(3-hydroxybutyric acid)) of this embodiment.
[0083] The obtained 3HB oligomer was 1 H-NMR spectroscopy was performed, the results of which are shown below. <Poly(3-hydroxybutyric acid) 1 H-NMR spectrum> 1 H-NMR (CDCl3,1% TFA) d 1.27 (d, J = 6.41 Hz, 3H, CH3), 2.59 (dd, J = 15.8, 5.04 Hz, 1H, CHH), 2.69 (dd, J = 15.8, 7.79 Hz, 1H, CHH), 5.24-5.34 (m, 1H, CH).
[0084] 1 By H-NMR analysis, the amount of unsaturated groups was calculated to be 0.1%, the amount of residual hydroxyl groups was calculated to be 0.4%, and the degree of polymerization was calculated to be 200 using the above calculation method. 1 Based on the H-NMR analysis, the tacticity was calculated to be isotacticity = 99.5% and syndiotacticity = 0.5% using the above calculation method. GPC analysis determined Mn 8,993, Mw 15,960, Mw / Mn 1.79.
[0085] (Synthesis Example 1) "Synthesis of PBS with amines at both ends" Succinic acid (2.00g, 16.94mmol), 1,4-butanediol (1.68g, 18.63mmol), N,N-dimethylaminopyridine (0.87g, 7.11mmol), and dichloromethane (53mL) were added to a 100mL recovery flask and completely dissolved. The mixture was then cooled to 0℃, and 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDCI·HCl) (10.23g, 53.35mmol) was added. The mixture was stirred at 0℃ for 0.5h and at room temperature for 3h. After the reaction, 5mL of pure water was added to the solution, and the mixture was concentrated using an evaporator. When acetone (200mL) and pure water (50mL) were added to the residue, a precipitate was confirmed. The precipitate was collected by filtration, washed successively with acetone (100 mL), pure water (100 mL), and acetone (100 mL), and dried in vacuum at 45° C. to obtain a white solid (yield: 2.09 g, 68%).
[0086] The above white solid (m = 11.9, 2.00 g, 16.94 mmol), Boc-GABA (0.39 g, 1.91 mmol), N,N-dimethylaminopyridine (0.07 g, 0.56 mmol), and dichloromethane (18 mL) were added to a 100 mL eggplant flask and cooled to 0. EDCI-HCl (0.80 g, 4.16 mmol) was added at 0 ° C., and the mixture was stirred at room temperature for 2.5 h, and then 18 mL of pure water was added. The precipitate obtained by concentrating the reaction solution with an evaporator was washed with methanol (100 mL × 2) and pure water (100 mL), and dried under reduced pressure to obtain a white solid (2.02 g, yield 95%). 1 In the H-NMR analysis, the degree of polymerization was calculated to be 11.7 based on the area intensity ratio of the signal derived from the Boc group and the signal derived from the PBS main chain. GPC analysis determined Mn 4,100, Mw 5,600, Mw / Mn 1.38.
[0087] The white solid (1.90g, 0.78 mmol) was dissolved in 19mL of chloroform in a 100mL eggplant flask and cooled to 0℃. TFA (19mL) pre-cooled to 0℃ in a refrigerator was added to the reaction solution and stirred at room temperature for 5h. The reaction solution was partitioned with saturated saline (100mL) and chloroform (100mL), and the organic layer was washed with saturated sodium bicarbonate (100mLx2). The organic layer was washed with 1M HClaq. (100mLx2) and saturated saline (100mLx2), and concentrated in an evaporator. The white solid was washed with acetone (100mL) and pure water (100mL), and vacuum dried at 45℃ to obtain PBS with amines at both ends as a white solid (yield 1.36g, 75%). Precursor Boc amino group terminal 1 The disappearance of the 1 H-NMR signal confirmed the completion of the reaction. 1 The degree of polymerization was estimated to be 12.4 by H-NMR analysis.
[0088] Example 2 "Synthesis of Polyamide" (I) Introduction of adipic acid to the hydroxyl terminus of 3HB oligomer The procedure was the same as in Example 1, except that p-toluenesulfonic acid (p-TsOH) (50 mg, 252 mmol), polymer-supported triphenylphosphine (PB-PPh3) (3 mmol / g; 18 mg, 54 mmol), and (R)-3-hydroxybutyric acid (400 mg, 3.85 mmol) were used. (R)-3HB oligomer was obtained as a white solid as the ester (poly(3-hydroxybutyric acid)) of this embodiment. 1 From the H-NMR analysis, the amount of unsaturated groups was calculated to be 0.04% using the above calculation method. 1 Based on the H-NMR analysis, the tacticity was calculated to be isotacticity = 99.0% and syndiotacticity = 1.0% using the above calculation method. GPC analysis determined Mn 1,613, Mw 2,962, Mw / Mn 1.84. The reaction was carried out in the same manner as the above polymerization reaction using the above (R)-3HB oligomer, PB-PPh3 (3 mmol / g; 18 mg, 54 mmol), DCE (0.5 mL), and adipic acid (200 mg). After 22 hours, the reaction solution was returned to room temperature and then concentrated to obtain a white solid. This was suspended in acetone (20 mL), subjected to ultrasonic waves, and centrifuged three times, and the solvent was distilled off by reducing the pressure of the obtained solid. Chloroform (20 mL) was added to the obtained solid, and the insoluble matter was removed by cotton plug filtration. The filtrate was concentrated to obtain adipic acid-terminated 3HB oligomer (125 mg; Mn 3,964, Mw 5,329, Mw / Mn 1.34). 1 In the H-NMR analysis, the methylene skeleton derived from adipic acid was observed at d 1.6 (m, 4H, CH2CH2CH2CH2), d 2.25 (m, 2H, COCH2CH2), and d 2.32 (m, 2H, CH2CH2CO). From the signal intensity ratio (4:33.4) between the methylene of the adipic acid moiety and the methine of the ester moiety of 3HB, the degree of polymerization was estimated to be 33 and the molecular weight to be 3,000.
[0089] (II) Multiblock copolymerization In a 10 mL eggplant flask, the adipic acid-terminated 3HB oligomer (0.03 g, 0.01 mmol) obtained in this example, the amine-terminated PBS (0.02 g, 0.01 mmol) obtained in Synthesis Example 1, and dichloromethane (0.5 mL) were added to obtain a colorless, transparent solution. 7-Aza-1-hydroxybenzotriazole (HOAt) (0.003 g, 0.03 mmol), N,N-diisopropylethylamine (1 drop, 0.01 g, 0.1 mmol), and EDCI HCl (0.005 g, 0.03 mmol) were added in sequence and stirred at room temperature for 7.5 h. The reaction solution was dropped into methanol (50 mL), and the supernatant was filtered to obtain a white solid. This was washed with methanol and pure water in sequence, and dried under reduced pressure at 45 ° C. to obtain a white fibrous solid as a polyamide (yield 0.03 g, 67%). GPC analysis determined Mn 22,921, Mw 61,241, Mw / Mn 2.67.
[0090] Comparative Example 1 "Synthesis of poly(3-hydroxybutyric acid)" In a 100 mL three-neck flask equipped with a nitrogen inlet tube, a thermometer, a stirrer, and a Dean-Stark trap, 400 mg (3.85 mmol) of (R)-3-hydroxybutyric acid, 0.010 g (0.05 mmol) of p-toluenesulfonic acid, and 1 mL of toluene were added, and the mixture was heated for 17 hours at an internal temperature of 100° C. The reaction solution was cooled to room temperature, and 100 mL of methanol was added to precipitate a solid, which was then filtered to obtain poly(3-hydroxybutyric acid). 1 The amount of unsaturated groups was calculated to be 0.8% by H-NMR analysis. GPC analysis determined Mn 4,200, Mw 7,200, Mw / Mn 1.73.
[0091] "Synthesis of Polyamide" The same procedure as in Example 2 was carried out except that the poly(3-hydroxybutyric acid) (unsaturated group content: 0.8%) obtained in Comparative Example 1 was used, but the reaction did not proceed and no polyamide was obtained.
[0092] Comparative Example 2 The same procedure as in Example 2 was carried out except that poly((R)-3-hydroxybutyric acid) purchased from Aldrich was used, but the reaction did not proceed and no polyamide was obtained. The physical properties of the poly((R)-3-hydroxybutyric acid) are shown below. Isotaxy = 100%, syndiotacticity = 0%, Mn 403,000, Mw 769,000, Mw / Mn 1.91, unsaturated group content = 0%.
[0093] (Consideration) The reason why the reaction did not proceed in the poly(3-hydroxybutyric acid) of Comparative Example 1 and polyamide was not obtained is thought to be that the ends were crotonoyl groups, which prevented adipic acid from reacting and prevented both ends from becoming dicarboxylic acids, resulting in no copolymerization. The reason why the reaction did not proceed in the poly(3-hydroxybutyric acid) of Comparative Example 2 and polyamide was not obtained is believed to be that the molecular weight was large and there were almost no active terminals. [Industrial Applicability]
[0094] The poly(hydroxyalkanoic acid) of the present embodiment contains only a small amount of unsaturated groups (decomposition products) and has reactive end groups such as hydroxyl groups and carboxyl groups, and therefore can be further chemically modified, expanding its applications. Resin compositions containing the poly(hydroxyalkanoic acid) of the present embodiment are expected to be used in a variety of applications, such as sustainable product groups (packaging materials, films).
Claims
1. A poly(hydroxyalkanoic acid) composed of at least one hydroxyalkanoic acid unit, The terminal groups of the poly(hydroxyalkanoic acid) are a hydroxy group and a carboxyl group, the poly(hydroxyalkanoic acid) contains a unit having an unsaturated bond in a ratio of 0.2 mol % or less based on the total constitutional units of the poly(hydroxyalkanoic acid); the number average molecular weight of the poly(hydroxyalkanoic acid) is 1,000 to 20,000; A poly(hydroxyalkanoic acid) characterized in that the isotacticity of the hydroxyalkanoic acid is 98.0 to 100%.
2. The poly(hydroxyalkanoic acid) according to claim 1 , wherein the unit having an unsaturated bond is a carboxylic acid unit having an unsaturated bond.
3. the hydroxyalkanoic acid is 3-hydroxybutyric acid, The poly(hydroxyalkanoic acid) of claim 1, wherein the poly(hydroxyalkanoic acid) is poly(3-hydroxybutyric acid).
4. A method for producing the poly(hydroxyalkanoic acid) according to any one of claims 1 to 3, comprising the steps of: A method for producing a poly(hydroxyalkanoic acid), comprising the step of subjecting at least one hydroxyalkanoic acid to an esterification reaction using a catalyst comprising a phosphine and a sulfonic acid.
5. The method for producing a poly(hydroxyalkanoic acid) according to claim 4, further comprising a washing step using acetone.
6. An amidation product obtained by using the poly(hydroxyalkanoic acid) according to any one of claims 1 to 3.
7. A polyurethane obtained by using the poly(hydroxyalkanoic acid) according to any one of claims 1 to 3.
8. A resin composition comprising the poly(hydroxyalkanoic acid) according to any one of claims 1 to 3.
9. A cured resin product of the resin composition according to claim 8.
10. A sheet or film comprising the cured resin according to claim 9.
Citation Information
Patent Citations
Synthesis of crystalline polymers from cyclic diolides