Solid-state battery and manufacturing method of solid-state battery

By forming a Li-X layer on the surface of the solid electrolyte layer in the negative electrode active material layer, the solid-state batteries achieve improved capacity retention through reduced reductive decomposition and enhanced lithium ion diffusion, addressing the low capacity retention issue.

JP2024135387AActive Publication Date: 2024-10-04TOYOTA JIDOSHA KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023046041
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

The capacity retention rate of solid-state batteries after charge/discharge cycles is low due to the formation of a resistance layer between the solid electrolyte and negative electrode layer during charging and discharging.

Method used

The configuration of the negative electrode active material layer in solid-state batteries includes a Li-X layer formed on the surface of the solid electrolyte layer, where X is at least one of Sn, Zn, or Al, preventing direct contact between metallic lithium and the solid electrolyte, thereby inhibiting reductive decomposition and facilitating easier lithium ion diffusion.

Benefits of technology

This configuration enhances the capacity retention rate of the solid-state batteries by reducing the formation of resistance layers and improving lithium ion diffusion, resulting in higher capacity retention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135387000001
    Figure 2024135387000001
Patent Text Reader

Abstract

To provide a solid-state battery having high capacity retention.SOLUTION: A solid-state battery according to the present disclosure includes a positive electrode layer, a solid electrolyte layer, and a negative electrode layer in this order. The negative electrode layer includes a negative electrode current collector, and a negative electrode active material layer, in this order, in a direction from the negative electrode layer toward a side of the solid electrolyte layer. When the solid-state battery is fully charged, the negative electrode active material layer has a Li layer, a Li-Mg layer or a Li-Mg-X layer, and a Li-X layer, in this order, in the direction. The X is at least one selected from the group consisting of Sn, Zn, and Al. The Li-X layer is formed on a surface of the solid electrolyte layer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a solid-state battery and a method for manufacturing a solid-state battery. [Background technology]

[0002] 2. Description of the Related Art Conventionally, solid-state batteries have been known as lithium-ion secondary batteries having excellent safety. Patent Document 1 discloses an all-solid-state secondary battery (hereinafter, also referred to as a "solid-state battery"). The solid-state battery disclosed in Patent Document 1 is formed by laminating an anode layer, a solid electrolyte layer, and a cathode layer in this order. The anode layer has an anode current collector and a coating layer that coats the anode current collector. The coating layer and the solid electrolyte layer face each other. In the solid-state battery disclosed in Patent Document 1, metallic lithium is deposited between the coating layer and the solid electrolyte layer during charging. Specifically, Patent Document 1 discloses a layer made of zinc formed by sputtering on the surface of the anode current collector as the coating layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-129159 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the solid-state battery disclosed in Patent Document 1 may have a low capacity retention rate after charge-discharge cycles.

[0005] The present disclosure has been made in consideration of the above circumstances. An object of one embodiment of the present disclosure is to provide a solid-state battery having a high capacity retention rate and a method for manufacturing the solid-state battery. [Means for solving the problem]

[0006] Means for solving the above problems include the following embodiments. <1> A solid-state battery including a positive electrode layer, a solid electrolyte layer, and a negative electrode layer in this order, the negative electrode layer includes a negative electrode current collector and a negative electrode active material layer in this order in a direction from the negative electrode layer toward the solid electrolyte layer, when the solid-state battery is fully charged, the negative electrode active material layer has a Li layer, a Li-Mg layer or a Li-Mg-X layer, and a Li-X layer in this order in the direction; The X is at least one selected from the group consisting of Sn, Zn, and Al, The Li-X layer is formed on a surface of the solid electrolyte layer. <2> When the solid-state battery is fully charged, the negative electrode active material layer has the Li-Mg layer or the Li-Mg-X layer, and the Li-X layer. <1> The solid-state battery according to claim 1, <3> When the solid-state battery is fully charged, the negative electrode active material layer has the Li-Mg layer and the Li-Sn layer in this order in the direction. <1> or <2> The solid-state battery according to claim 1, <4> When the solid-state battery is fully charged, the negative electrode active material layer has a Li-Mg-Zn layer and a Li-Zn layer in this order in the direction. <1> or <2> The solid-state battery according to claim 1, <5> When the solid-state battery is fully charged, the negative electrode active material layer has a Li-Mg-Al layer and a Li-Al layer in this order in the direction. <1> or <2> The solid-state battery according to claim 1, <6> When the solid-state battery is fully charged, the negative electrode active material layer has a Li layer and a Li-X layer in this order in the direction. <1> The solid-state battery according to claim 1, <7> When the solid-state battery is fully charged, the negative electrode active material layer has a Li layer and a Li-Sn layer in this order in the direction. <6> The solid-state battery according to claim 1, <8> 1. A method for manufacturing a solid-state battery having a positive electrode layer, a solid electrolyte layer, and a negative electrode layer in this order, comprising: forming an X layer on a surface of the solid electrolyte layer on the negative electrode layer side, The method for producing a solid-state battery, wherein X is at least one selected from the group consisting of Sn, Zn, and Al. <9> the negative electrode layer has a negative electrode current collector, The method further includes forming an Mg layer on a surface of the negative electrode current collector on the side of the solid electrolyte layer. <8> A method for producing the solid-state battery according to claim 1. Effect of the Invention

[0007] According to the present disclosure, a solid-state battery having a high capacity retention rate and a method for manufacturing the solid-state battery are provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In the present disclosure, a numerical range indicated using "~" means a range including the numerical values ​​described before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in stages in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with the upper limit or lower limit of another numerical range described in stages. In the numerical ranges described in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with a value shown in the examples. In the present disclosure, a combination of two or more preferred embodiments is a more preferred embodiment. In the present disclosure, the amount of each component means the total amount of the multiple substances, unless otherwise specified, when there are multiple substances corresponding to each component. In the present disclosure, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.

[0009] (1) Solid state battery The solid-state battery of the present disclosure includes a positive electrode layer, a solid electrolyte layer, and a negative electrode layer in this order. The negative electrode layer includes a negative electrode current collector and a negative electrode active material layer in this order in a direction from the negative electrode layer toward the solid electrolyte layer (hereinafter also referred to as the "SE direction"). When the solid-state battery is fully charged (hereinafter also simply referred to as "fully charged"), the negative electrode active material layer includes a Li (lithium) layer, a Li-Mg (magnesium) layer or a Li-Mg-X layer, and a Li-X layer in this order in the direction. The X (hereinafter also referred to as the "metal element X") is at least one selected from the group consisting of Sn (tin), Zn (zinc), and Al (aluminum). The Li-X layer is formed on the surface of the solid electrolyte layer.

[0010] In this disclosure, "when the solid-state battery is fully charged" refers to the time when the state of charge (SOC) of the solid-state battery is 100%. SOC indicates the ratio of the charge capacity to the fully charged capacity of the solid-state battery. At the fully charged capacity, the SOC is 100%. The term "Li layer" refers to a metal layer containing lithium as a main component. Specifically, the term "Li layer" refers to a layer in which the ratio of lithium element is 98 atomic % or more relative to the total amount of all elements constituting the layer, and more preferably, refers to a layer in which the ratio of lithium element is 99.8 atomic % or more relative to the total amount of all elements. The Li layer may have a ratio of lithium element of 100 atomic %. The Li layer may be formed by a precipitation reaction of metallic lithium accompanying charging of a solid-state battery. The term "Li-Mg layer" refers to an alloy layer mainly composed of lithium and magnesium elements. More specifically, the term "Li-Mg layer" refers to a layer in which the ratio of lithium element is 75 atomic % or more and the ratio of magnesium element is 0.3 atomic % or more relative to the total amount of all elements constituting the layer when the solid-state battery is fully charged. The ratio of lithium element may be 75 atomic % to 99.7 atomic %, and the ratio of magnesium element may be 0.3 atomic % to 20 atomic %. The term "Li-Mg-X layer" refers to an alloy layer mainly composed of lithium, magnesium, and metal element X. More specifically, the term "Li-Mg-X layer" refers to a layer in which the ratio of lithium is 45 atomic% or more, the ratio of magnesium is 0.3 atomic% or more, and the ratio of metal element X is 0.1 atomic% or more, relative to the total amount of all elements constituting the layer. The ratio of metal element X may be 0.1 atomic% to 5 atomic%, the ratio of magnesium may be 0.3 atomic% to 45 atomic%, and the ratio of lithium may be 45 atomic% to 99.6 atomic%. The term "Li-X layer" refers to an alloy layer mainly composed of lithium element and metal element X. More specifically, the term "Li-X layer" refers to a layer in which the ratio of lithium element is 80 atomic % or more and the ratio of metal element X is 0.1 atomic % or more relative to the total amount of all elements constituting the layer. The ratio of metal element X may be 0.1 atomic % to 15 atomic %, and the ratio of lithium element may be 80 atomic % to 99.9 atomic %. "The Li-X layer is formed on the surface of the solid electrolyte layer" means that when the solid battery is fully charged, no Li layer is present between the Li-X layer and the solid electrolyte layer.

[0011] The solid-state battery of the present disclosure has the above-described configuration and therefore has a high capacity retention rate. This effect is believed to be due to, but not limited to, the following reasons. It is known that when the solid electrolyte layer and metallic lithium come into physical contact during charging and discharging of a solid-state battery, a reductive decomposition reaction of the solid electrolyte layer proceeds. When the reductive decomposition reaction of the solid electrolyte layer proceeds, a layer (hereinafter also referred to as a "resistance layer") that acts as an interface resistance may be formed between the solid electrolyte layer and the negative electrode layer. As a result, the capacity retention rate of the solid-state battery may decrease. In the present disclosure, the Li-X layer is formed on the surface of the solid electrolyte layer. In other words, no Li layer is interposed between the Li-X layer and the solid electrolyte layer when the solid battery is charged. That is, the reduction decomposition reaction of the solid electrolyte layer is unlikely to proceed. As a result, the resistance layer is unlikely to be formed. Furthermore, in the present disclosure, during charging and discharging of the solid battery, lithium ions are more likely to diffuse at the interface between the solid electrolyte layer and the negative electrode layer than when the Li-X layer is not formed on the surface of the solid electrolyte layer. As a result, it is presumed that the solid battery of the present disclosure has a high capacity retention rate.

[0012] (1.1)Battery structure The structure of the solid-state battery is a laminated structure of a positive electrode layer / anode layer / solid electrolyte layer. The solid-state battery includes a so-called all-solid-state battery using a solid electrolyte as an electrolyte, and the solid electrolyte may contain an electrolytic solution of less than 10 mass% with respect to the total amount of the electrolyte. The solid electrolyte may be a composite solid electrolyte containing an inorganic solid electrolyte and a polymer electrolyte.

[0013] When a set of a positive electrode layer, a solid electrolyte layer, and a negative electrode layer is defined as a power generation unit, the solid-state battery may have only one power generation unit or may have two or more power generation units. When the solid-state battery has two or more power generation units, the power generation units may be connected in series or in parallel.

[0014] The solid-state battery may be configured by sealing the end faces (side faces) of the laminated structure of the positive electrode layer / solid electrolyte layer / negative electrode layer with a resin. The shape of the solid-state battery is not particularly limited, and may be, for example, a coin type, a cylindrical type, a square type, a sheet type, a button type, a flat type, or a laminate type.

[0015] (1.2) Negative electrode layer The solid-state battery includes a negative electrode layer having a negative electrode current collector and a negative electrode active material layer in this order in the SE direction.

[0016] (1.2.1) Negative electrode active material layer The negative electrode layer has a negative electrode active material layer. At the time of full charge, the negative electrode active material layer has a Li layer, a Li-Mg layer or a Li-Mg-X layer, and a Li-X layer in this order in the above direction. The metal element X is at least one selected from the group consisting of Sn, Zn, and Al. The Li-X layer is formed on the surface of the solid electrolyte layer. The layer structure of the negative electrode active material layer was determined in the same manner as described in the Examples.

[0017] The metal element X may be one selected from the group consisting of Sn, Zn and Al. When the metal element X is Sn and the negative electrode active material layer contains Mg, the negative electrode active material layer at full charge tends to contain a Li-Mg layer but not a Li-Mg-Sn layer. This is presumably because the alloying potential of Sn and Li is higher than the Li deposition potential, and the reaction proceeds in two stages. In detail, it is presumed that during charging, the Li-Sn layer is formed first, and then the alloying of Li and Mg and the Li deposition reaction occur, forming the Li-Mg layer. When the metal element X is Zn and the negative electrode active material layer contains Mg, the negative electrode active material layer at full charge tends to contain a Li-Mg-Zn layer but not a Li-Mg layer. This is presumably because the alloying potential of Li-Zn is lower than that of Li-Mg, and thus Li-Zn is formed simultaneously with Li deposition, resulting in a structure mixed with Li-Mg. When the metal element X is Al and the negative electrode active material layer contains Mg, the negative electrode active material layer at full charge tends to contain a Li-Mg-Al layer but not a Li-Mg layer. This is presumably because the alloying potential of Li-Al is lower than that of Li-Mg, and thus the Li-Al is formed simultaneously with Li deposition, resulting in a structure mixed with Li-Mg.

[0018] When the negative electrode active material layer does not contain Mg, the ratio of the metal element X and the ratio of Li are preferably within the following ranges from the viewpoint of increasing the capacity retention rate of the solid-state battery at full charge. That is, the ratio of the metal element X is preferably 0.05 atomic% to 15.0 atomic%, more preferably 0.12 atomic% to 2.0 atomic%, and even more preferably 0.3 atomic% to 1.0 atomic%, based on the total amount of the negative electrode active material layer. The ratio of Li is not particularly limited, and is preferably 85.0 atomic% to 99.5 atomic%, more preferably 98.0 atomic% to 99.88 atomic%, and even more preferably 99.0 atomic% to 99.7 atomic%, based on the total amount of the negative electrode active material layer.

[0019] The method of calculating the ratio is to take out the negative electrode layer from the all-solid-state battery in a fully charged state, perform an ICP (Inductively Coupled Plasma) analysis on the negative electrode layer, and calculate the element ratio of the alloy contained in the negative electrode layer. The calculation method of the ratio is the same below.

[0020] When the negative electrode active material layer does not contain Mg, the thickness of the Li layer and the thickness of the Li-X layer at full charge may each be within the following ranges. The thickness of the Li layer is not particularly limited and may be 1 μm to 30 μm. The thickness of the Li-X layer is not particularly limited and may be 10 nm to 3000 nm.

[0021] When the negative electrode active material layer contains Mg, the ratio of the metal element X, the ratio of Li, and the ratio of Mg are preferably within the following ranges from the viewpoint of increasing the capacity retention rate of the solid-state battery at full charge. That is, the ratio of the metal element X is preferably 0.05 atomic% to 15.0 atomic%, more preferably 0.12 atomic% to 2.0 atomic%, and even more preferably 0.3 atomic% to 1.0 atomic%, based on the total amount of the negative electrode active material layer. The ratio of Li is not particularly limited, and is preferably 85.0 atomic% to 99.5 atomic%, more preferably 98.0 atomic% to 99.88 atomic%, and even more preferably 99.0 atomic% to 99.7 atomic%, based on the total amount of the negative electrode active material layer. The proportion of Mg is not particularly limited, and is preferably 0.1 atomic % to 25.0 atomic %, more preferably 0.3 atomic % to 20.0 atomic %, and further preferably 0.8 atomic % to 6.0 atomic %, relative to the total amount of the negative electrode active material layer.

[0022] When the negative electrode active material layer contains Mg, the thickness of the Li-Mg layer, the thickness of the Li-Mg-X layer, and the thickness of the Li-X layer may each be within the following ranges when fully charged. The thickness of the Li-Mg layer is not particularly limited and may be 1 μm to 30 μm. The thickness of the Li-Mg-X layer is not particularly limited and may be 1 μm to 30 μm. The thickness of the Li-X layer is not particularly limited and may be 10 nm to 3000 nm. When the negative electrode active material layer contains Mg, the Li-Mg layer or Li-Mg-X layer is preferably formed on the surface of the negative electrode current collector. "The Li-Mg layer or Li-Mg-X layer is formed on the surface of the negative electrode current collector" means that no Li layer is present between the Li-Mg layer or Li-Mg-X layer and the negative electrode current collector when the solid-state battery is fully charged.

[0023] When the solid-state battery is fully charged, the negative electrode active material layer preferably has a Li layer and a Li-X layer in this order in the direction. This allows the capacity retention rate of the solid electrolyte to be higher than when the negative electrode active material layer is a conventional negative electrode active material layer. The conventional negative electrode active material layer has a Li-Zn layer and a Li layer in this order in the SE direction.

[0024] When the solid-state battery is fully charged, the negative electrode active material layer preferably has a Li layer and a Li-Sn layer in this order in the direction, whereby the capacity retention rate of the solid electrolyte is higher than when the negative electrode active material layer has a Li layer and a Li-Al layer or a Li-Zn layer in this order in the SE direction.

[0025] When the solid-state battery is fully charged, the negative electrode active material layer preferably has the Li-Mg layer or the Li-Mg-X layer and the Li-X layer, whereby the capacity retention rate of the solid-state battery is higher than when the negative electrode active material layer has a Li layer and a Li-X layer in this order in the SE direction. The thickness of the Li-X layer is relatively thin, and the Li-X layer may be formed following the surface properties (i.e., uneven shape) of the solid electrolyte layer. The Li-Mg layer or Li-Mg-Zn layer is likely to take in lithium ions and expand when the solid battery is fully charged. This increases the number of contact points between the Li-Mg layer or Li-Mg-Zn layer and the Li-Zn layer. In other words, the number of reaction sites between the solid electrolyte layer and the negative electrode layer increases. As a result, it is presumed that the capacity retention rate of the solid battery will be high.

[0026] When the solid-state battery is fully charged, the negative electrode active material layer preferably has a Li-Mg-Al layer and a Li-Al layer in this order in the direction, whereby the capacity retention rate of the solid-state battery is higher than when the negative electrode active material layer has a Li layer and a Li-X layer in this order in the SE direction.

[0027] When the solid-state battery is fully charged, the negative electrode active material layer preferably has a Li-Mg-Zn layer and a Li-Zn layer in this order in the direction. This allows the capacity retention rate of the solid-state battery to be higher than when the negative electrode active material layer has a Li-Mg-Al layer and a Li-Al layer in this order in the SE direction. This effect is presumed to be due to, but not limited to, the following reasons.

[0028] When the solid-state battery is fully charged, the negative electrode active material layer preferably has the Li-Mg layer and the Li-Sn layer in this order in the direction, whereby the capacity retention rate of the solid-state battery is higher than when the negative electrode active material layer has the Li-Mg layer and the Li-Sn layer in this order in the SE direction.

[0029] In the fully charged state, the negative electrode active material layer may have a Li alloy layer between the Li layer, the Li-Mg layer, or the Li-Mg-X layer and the Li-X layer, within a range that does not impair the effects of the present disclosure. Examples of the Li alloy layer include a Li-In alloy.

[0030] From the viewpoint of increasing the capacity retention rate of the solid-state battery when fully charged, the negative electrode active material layer preferably comprises a Li layer, a Li-Mg layer or a Li-Mg-X layer, and a Li-X layer.

[0031] During discharge (eg, SOC: 0%), the negative electrode active material layer may not have a Li layer.

[0032] (1.2.2) Negative electrode current collector The negative electrode layer has a negative electrode current collector that collects current from the negative electrode layer and is disposed on the opposite side of the negative electrode layer from the solid electrolyte layer. The negative electrode current collector may be made of a material that does not form an alloy with Li, such as stainless steel, aluminum, copper, nickel, iron, titanium, carbon, etc., and is preferably made of copper. The shape of the negative electrode current collector is, for example, a foil or mesh shape. The negative electrode current collector may have a buffer layer, an elastic layer, or a PTC (Positive Temperature Coefficient) thermistor layer disposed on the surface.

[0033] (1.3) Solid electrolyte layer The solid-state battery includes a solid electrolyte layer. The solid electrolyte layer may include a solid electrolyte. The solid electrolyte preferably includes at least one selected from the group of solid electrolytes consisting of a sulfide solid electrolyte, an oxide solid electrolyte, and a halide solid electrolyte.

[0034] The sulfide solid electrolyte preferably contains sulfur (S) as a main component of an anion element, and further preferably contains, for example, Li, A, and S elements. The A element is at least one selected from the group consisting of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In. The sulfide solid electrolyte may further contain at least one of O and a halogen element. Examples of the halogen element (X) include F, Cl, Br, and I. The composition of the sulfide solid electrolyte is not particularly limited, and examples thereof include xLi2S·(100-x)P2S5 (70≦x≦80), yLiI·zLiBr·(100-yz)(xLi2S·(1-x)P2S5) (0.7≦x≦0.8, 0≦y≦30, 0≦z≦30). The sulfide solid electrolyte may have a composition represented by the following general formula (1). Formula (1): Li 4-x Ge 1-x P x S4(0 <x<1) In formula (1), at least a portion of Ge may be substituted with at least one selected from the group consisting of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. At least a portion of P may be substituted with at least one selected from the group consisting of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. At least a portion of Li may be substituted with at least one selected from the group consisting of Na, K, Mg, Ca, and Zn. At least a portion of S may be substituted with a halogen. The halogen is at least one of F, Cl, Br, and I.

[0035] As the oxide solid electrolyte, it is preferable to contain oxygen (O) as the main component of the anion element. For example, it may contain Li, Q element (Q represents at least one of Nb, B, Al, Si, P, Ti, Zr, Mo, W, and S), and O. Examples of the oxide solid electrolyte include garnet-type solid electrolytes, perovskite-type solid electrolytes, NASICON-type solid electrolytes, Li-P-O-based solid electrolytes, Li-B-O-based solid electrolytes, etc. Examples of the garnet-type solid electrolyte include, for example, Li7La3Zr2O 12 、Li 7-x La3(Zr 2-x Nb x )O 12 (0 ≦ x ≦ 2), Li5La3Nb2O 12 , etc. Examples of the perovskite-type solid electrolyte include, for example, (Li, La)TiO3, (Li, La)NbO3, (Li, Sr)(Ta, Zr)O3, etc. Examples of the NASICON-type solid electrolyte include, for example, Li(Al, Ti)(PO4)3, Li(Al, Ga)(PO4)3, etc. Examples of the Li-P-O-based solid electrolyte include Li3PO4, LIPON (a compound in which a part of O in Li3PO4 is replaced by N), and examples of the Li-B-O-based solid electrolyte include Li3BO3, a compound in which a part of O in Li3BO3 is replaced by C, etc.

[0036] As the halide solid electrolyte, a solid electrolyte containing Li, M, and X (M represents at least one of Ti, Al, and Y, and X represents F, Cl, or Br) is suitable. Specifically, Li 6ー3z Y z X6 (X represents Cl or Br, and z satisfies 0 < z < 2), Li 6-(4-x)b (Ti 1-x Al x ) b F6 (0 < x < 1, 0 < b ≦ 1.5) is preferable. Among Li 6ー3z Y z X6, Li3YX6 (X represents Cl or Br) is more preferable in terms of excellent lithium ion conductivity, and further, Li3YCl6 is preferable. Also, Li 6-(4-x)b (Ti 1-x Alx ) b F6(0 < x < 1, 0 < b ≤ 1.5) is preferably included together with a solid electrolyte such as a sulfide solid electrolyte from the viewpoint of suppressing, for example, the oxidative decomposition of the sulfide solid electrolyte.

[0037] The solid electrolyte layer may have a single-layer structure or a multilayer structure of two or more layers.

[0038] The solid electrolyte layer may contain a binder. Examples of the binder that can be included in the solid electrolyte layer include vinyl halide resins, rubbers, polyolefin resins, etc. Examples of the vinyl halide resin include polyvinylidene fluoride (PVdF), a copolymer of polyvinylidene fluoride and hexafluoropropylene (PVdF-HFP), etc. Examples of the polyolefin resin include butadiene rubber (BR), acrylate butadiene rubber (ABR), styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber (NBR), butyl rubber (isobutylene-isoprene rubber), etc. Examples of the polyolefin resin include polyethylene, polypropylene, etc. The binder (C) may be a diene-based rubber containing a double bond in the main chain, for example, a butadiene-based rubber in which butadiene occupies 30 mol% or more of the whole.

[0039] (1.4) Positive electrode layer The solid battery includes a positive electrode layer. The positive electrode layer may have a positive electrode current collector and a positive electrode active material layer. The positive electrode active material layer is laminated on the main surface of the positive electrode current collector on the solid electrolyte layer side.

[0040] (1.4.1) Positive electrode active material layer The positive electrode active material layer may contain a positive electrode active material.

[0041] (1.4.1.1) Positive electrode active material The positive electrode active material preferably contains a lithium composite oxide. The lithium composite oxide may contain at least one selected from the group consisting of F, Cl, N, S, Br, and I. The lithium composite oxide may have a crystal structure belonging to at least one space group selected from the space groups R-3m, Immm, and P63-mmc (also called P63mc or P6 / mmc). The lithium composite oxide may have an O2 type structure in which the transition metal, oxygen, and lithium are mainly arranged.

[0042] Examples of lithium composite oxides having a crystal structure belonging to R-3m include Li x Me y O α X β (Me represents at least one selected from the group consisting of Mn, Co, Ni, Fe, Al, Cu, V, Nb, Mo, Ti, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, Ag, Ru, W, B, Si, and P, and X represents at least one selected from the group consisting of F, Cl, N, S, Br, and I, and satisfies 0.5≦x≦1.5, 0.5≦y≦1.0, 1≦α<2, and 0<β≦1.)

[0043] Examples of lithium composite oxides having a crystal structure belonging to Immm include Li x1 M 1 A 1 2(1.5≦x1≦2.3, M 1 contains at least one selected from the group consisting of Ni, Co, Mn, Cu and Fe, and A 1 contains at least oxygen, and A 1 The ratio of oxygen in the oxide is 85 atomic % or more. x1 M 1A 1-x2 M 1B x2 O 2-y A 2 y (0≦x2≦0.5, 0≦y≦0.3, and at least one of x2 and y is not 0; M 1Arepresents at least one selected from the group consisting of Ni, Co, Mn, Cu, and Fe, and M 1B represents at least one selected from the group consisting of Al, Mg, Sc, Ti, Cr, V, Zn, Ga, Zr, Mo, Nb, Ta, and W, and A2 represents at least one selected from the group consisting of F, Cl, Br, S, and P.). Examples thereof include composite oxides represented by

[0044] Examples of the lithium composite oxide having a crystal structure belonging to P63-mmc include, for example, M1 x M2 y O2 (where M1 represents an alkali metal (at least one of Na and K is preferable), M2 represents a transition metal (at least one selected from the group consisting of Mn, Ni, Co, and Fe is preferable), and x + y satisfies 0 < x + y ≦ 2). Examples thereof include composite oxides represented by

[0045] Examples of the lithium composite oxide having an O2-type structure include, for example, Li x [Li α (Mn a Co b M c ) 1-α O2 (0.5 < x < 1.1, 0.1 < α < 0.33, 0.17 < a < 0.93, 0.03 < b < 0.50, 0.04 < c < 0.33, and M represents at least one selected from the group consisting of Ni, Mg, Ti, Fe, Sn, Zr, Nb, Mo, W, and Bi). Specific examples thereof include Li 0.744 [Li 0.145 Mn 0.625 Co 0.115 Ni 0.115 O2 and the like.

[0046] (1.4.1.2) Solid electrolyte group The positive electrode layer preferably contains a solid electrolyte selected from the group of solid electrolytes consisting of sulfide solid electrolytes, oxide solid electrolytes, and halide solid electrolytes in addition to the positive electrode active material, and a mode in which at least a part of the surface of the positive electrode active material is coated with a sulfide solid electrolyte, an oxide solid electrolyte, or a halide solid electrolyte is more preferable. As the halide solid electrolyte that coats at least a part of the surface of the positive electrode active material, Li 6-(4-x)b (Ti 1-x Al x ) b F6 (0 < x < 1, 0 < b ≤ 1.5) [LTAF electrolyte] is preferable.

[0047] (1.4.1.3) Conductive aid The positive electrode layer may contain a conductive aid. Examples of the conductive aid include carbon materials, metal materials, and conductive polymer materials. Examples of the carbon material include carbon black (e.g., acetylene black, furnace black, ketjen black, etc.), fibrous carbon (e.g., vapor-grown carbon fiber, carbon nanotube, carbon nanofiber, etc.), graphite, carbon fluoride, etc. Examples of the metal material include metal powder (e.g., aluminum powder, etc.), conductive whiskers (e.g., zinc oxide, potassium titanate, etc.), conductive metal oxides (e.g., titanium oxide, etc.), etc. Examples of the conductive polymer material include polyaniline, polypyrrole, polythiophene, etc. The conductive aid may be used alone as one kind or may be used in combination of two or more kinds.

[0048] (1.4.1.4) Binder The positive electrode layer may contain a binder. Examples of the binder that can be contained in the positive electrode layer are the same as those exemplified as the binder that can be contained in the solid electrolyte layer.

[0049] (1.4.1.5) Other components The positive electrode layer may contain other components. Examples of the other components include thickeners, surfactants, dispersants, wetting agents, antifoaming agents, etc.

[0050] (1.4.2) Positive electrode current collector The positive electrode layer may further include a positive electrode current collector that collects current from the positive electrode layer. The positive electrode current collector is disposed on the opposite side of the positive electrode layer from the solid electrolyte layer. The positive electrode current collector may be, for example, stainless steel, aluminum, copper, nickel, iron, titanium, carbon, etc., and is preferably an aluminum alloy foil or aluminum foil. The aluminum alloy foil and aluminum foil may be manufactured using powder. The shape of the positive electrode current collector is, for example, a foil shape or a mesh shape. The positive electrode current collector may have a buffer layer, an elastic layer, or a PTC (Positive Temperature Coefficient) thermistor layer disposed on the surface.

[0051] (2) Manufacturing method of solid-state batteries The method for producing a solid-state battery according to the present disclosure is a method for producing a solid-state battery having a positive electrode layer, a solid electrolyte layer, and a negative electrode layer in this order. The method for producing a solid-state battery according to the present disclosure includes a step of forming an X layer on the surface of the solid electrolyte layer on the negative electrode layer side (hereinafter, also referred to as an "X layer forming step"). The X is at least one selected from the group consisting of Sn, Zn, and Al.

[0052] In the present disclosure, the term "X layer" refers to a metal layer containing the metal element X as a main component. The ratio of the metal element X in the "X layer" may be 100 atomic % relative to the total amount of all elements constituting the X layer. The "X layer" is a precursor of the "Li-X layer" in the present disclosure. More specifically, the X layer becomes a Li-X layer by incorporating lithium ions when the solid-state battery is charged.

[0053] Since the manufacturing method of the solid-state battery according to the present disclosure has the above configuration, the solid-state battery according to the present disclosure can be produced.

[0054] The method for producing a solid-state battery according to the present disclosure includes a first embodiment and a second embodiment, which will be described later.

[0055] (2.1) First embodiment The method for producing the solid-state battery according to the first embodiment includes an X-layer forming step, a first lamination step (described later), and a first charging step (described later). The X-layer forming step, the first lamination step, and the first charging step are performed in this order.

[0056] According to the first embodiment, a first solid-state battery is obtained. The first solid-state battery includes a positive electrode layer, a solid electrolyte layer, and a negative electrode layer in this order. The negative electrode layer includes a negative electrode current collector and a negative electrode active material layer in this order in the SE direction. When the first solid-state battery is fully charged, the negative electrode active material layer includes a Li layer and a Li-X layer in this order in the SE direction. The Li-X layer is formed on the surface of the solid electrolyte layer.

[0057] (2.1.1) X layer formation process In the X-layer forming step, an X-layer is formed on the surface of the solid electrolyte layer on the negative electrode layer side. This produces a solid electrolyte layer with an X-layer. The solid electrolyte layer with an X-layer has a solid electrolyte layer and an X-layer formed on the surface of the solid electrolyte layer on the negative electrode layer side.

[0058] The method for preparing the solid electrolyte layer may be a known method, such as a pressing method. Examples of the pressing method include roll pressing and cold isostatic pressing (CIP). The pressing pressure is usually 1 MPa to 600 MPa. Examples of the solid electrolyte layer include the same as those exemplified as the solid electrolyte layer contained in the solid battery of the present disclosure.

[0059] The method for forming the X layer is not particularly limited, and may be any known method, such as a dry process or a wet process. In the dry process, the X layer is formed by a process in a gas phase or vacuum. In detail, examples of the dry process include physical vapor deposition (e.g., vacuum deposition, ion plating, sputtering, etc.), chemical vapor deposition (e.g., thermal CVD (Chemical Vapor Deposition), plasma CVD, plasma CVD, etc.), and thermal spraying (e.g., flame spraying, arc spraying, plasma spraying, etc.). In the wet process, the X film is formed using a solution. More specifically, examples of the wet process include plating (e.g., electroplating, electroless plating, electroforming, etc.), electrolytic polymerization, etc.

[0060] Among them, the physical vapor deposition method or the chemical vapor deposition method is preferable as the method for forming the X layer. This method provides a better uniformity of the initial X layer and a better adhesion between the X layer and the solid electrolyte layer than the method for forming the X layer using the pressing method or the fine particle coating method. As a result, a solid battery with a higher capacity retention rate is obtained. This is presumably due to the following reasons. In the physical vapor deposition method or chemical vapor deposition method, the X layer is formed thinner and with a uniform thickness that follows the uneven shape of the interface of the solid electrolyte. In addition, the adhesive strength between the solid electrolyte and the X layer is strong. Therefore, voids are unlikely to form at the interface between the solid electrolyte layer and the X layer. As a result, the battery performance of the solid battery is unlikely to deteriorate. On the other hand, in the pressing method or fine particle coating, the X layer is likely to be formed with an uneven thickness depending on the location of the solid electrolyte interface. For example, the X layer may be embedded in the uneven shape of the interface of the solid electrolyte layer, or may accumulate in the recesses of the interface of the solid electrolyte. This may cause unevenness in the progress of the Li deposition reaction, resulting in the presence of voids at the interface between the X layer and the Li layer. In addition, due to the uneven thickness of the X layer and the weak adhesive strength between the X layer and the solid electrolyte layer, there may be places where the solid electrolyte layer is partially exposed. From there, the reaction with the solid electrolyte may progress, and the battery performance of the solid battery may deteriorate.

[0061] The thickness of the X layer is not particularly limited and may be from 1 nm to 1000 nm.

[0062] (2.1.2) First lamination process In the first lamination step, a negative electrode current collector, a solid electrolyte layer with an X layer, and a positive electrode layer are laminated in this order to form a first battery precursor. The first battery precursor is formed by laminating a negative electrode current collector, an X layer, a solid electrolyte layer, and a positive electrode layer in this order.

[0063] The method for preparing the negative electrode current collector and the positive electrode layer may be a known method. The negative electrode current collector may be the same as the one exemplified as the negative electrode current collector included in the solid-state battery of the present disclosure. The positive electrode layer may be the same as the one exemplified as the positive electrode layer included in the solid-state battery of the present disclosure.

[0064] The lamination method may be, for example, a pressing method. A slurry may be used when forming the positive electrode layer. The pressing method may be a roll press, a cold isostatic press (CIP), or the like. The pressing pressure is usually 1 MPa to 600 MPa.

[0065] (2.1.3) First charging process In the first charging step, the first battery precursor is charged to produce a first solid state battery.

[0066] When the first charging step is performed, lithium ions move from the positive electrode layer to the negative electrode layer. This causes metallic lithium to be precipitated between the X layer and the negative electrode current collector layer. As a result, the Li layer is selectively formed between the X layer and the negative electrode current collector layer. This is presumably due to the following reason. That is, after charging the solid-state battery, the X layer reacts with Li to form a Li-X layer. The Li-X layer has lithium ion conductivity. Therefore, the lithium ions that have moved from the positive electrode pass through the Li-X layer, reach the negative electrode current collector (or the already precipitated Li) and are precipitated. As a result, the Li layer is selectively formed between the X layer and the negative electrode current collector layer.

[0067] The charging conditions for the first charging step are not particularly limited and may be appropriately selected depending on the thickness of the X layer and the like.

[0068] (2.2) Second embodiment The method for producing a solid-state battery according to the second embodiment includes an X-layer forming step, a step of forming an Mg layer on the surface of the negative electrode current collector on the solid electrolyte layer side (hereinafter also referred to as an "Mg layer forming step"), a second battery precursor forming step, and a second charging step. The order in which the X-layer forming step and the Mg layer forming step are performed is not particularly limited. After the X-layer forming step and the Mg layer forming step are performed, the second battery precursor forming step and the second charging step are performed in this order.

[0069] According to the second embodiment, a second solid-state battery is obtained. The second solid-state battery includes a positive electrode layer, a solid electrolyte layer, and a negative electrode layer in this order. The negative electrode layer includes a negative electrode current collector and a negative electrode active material layer in this order in the SE direction. When the second solid-state battery is fully charged, the negative electrode active material layer includes a Li-Mg layer or a Li-Mg-X layer, and a Li-X layer in this order in the SE direction. The Li-X layer is formed on the surface of the solid electrolyte layer.

[0070] (2.2.1) X layer formation process The X layer forming step is the same as that exemplified as the X layer forming step in the first embodiment.

[0071] (2.2.2) Mg layer formation process In the second embodiment, the negative electrode layer has a negative electrode current collector. In the Mg layer forming step, a Mg layer is formed on the surface of the negative electrode current collector facing the solid electrolyte layer. This produces a negative electrode current collector with a Mg layer. The negative electrode current collector with a Mg layer has a negative electrode current collector and a Mg layer formed on the surface of the negative electrode current collector facing the solid electrolyte layer.

[0072] The method for preparing the negative electrode current collector may be a known method. Examples of the negative electrode current collector include those exemplified as the negative electrode current collector included in the solid-state battery of the present disclosure.

[0073] The method for forming the Mg layer is not particularly limited, and may be the same as the method exemplified for forming layer X. Among them, the method for forming the Mg layer is preferably a physical vapor deposition method or a chemical vapor deposition method.

[0074] The thickness of the Mg layer is not particularly limited and may be from 30 nm to 3000 nm.

[0075] (2.2.3) Second lamination process In the second lamination step, the negative electrode current collector with the Mg layer, the solid electrolyte layer with the X layer, and the positive electrode layer are laminated in this order to form a second battery precursor. The second battery precursor is formed by laminating the negative electrode current collector, the Mg layer, the X layer, the solid electrolyte layer, and the positive electrode layer in this order.

[0076] The method for preparing the positive electrode layer may be a known method. Examples of the positive electrode layer include the same positive electrode layers as those exemplified for the positive electrode layer included in the solid-state battery of the present disclosure.

[0077] The lamination method may be, for example, a pressing method. A slurry may be used when forming the positive electrode layer. The pressing method may be a roll press, a cold isostatic press (CIP), or the like. The pressing pressure is usually 1 MPa to 600 MPa.

[0078] (2.2.4) Second charging process In the second charging step, the second battery precursor is charged to produce a second solid-state battery.

[0079] When the second charging step is performed, lithium ions move from the positive electrode layer to the negative electrode layer. The lithium ions are taken into the Mg layer and the X layer, respectively, to form a Li-Mg layer or a Li-Mg-X layer and a Li-X layer. At this time, no Li layer is formed between the solid electrolyte layer and the negative electrode current collector. This is presumably because the precipitated Li and Mg diffuse into each other, and the concentration difference becomes the driving force to form the Li-Mg layer or the Li-Mg-X layer.

[0080] The charging conditions for the second charging step are not particularly limited and may be appropriately selected depending on the thickness of the Mg layer and the thickness of the X layer, etc. EXAMPLES

[0081] The present disclosure will be described in more detail below with reference to examples, but the invention of the present disclosure is not limited to these examples.

[0082] [1] Examples and Comparative Examples [1.1] Example 1 [1.1.1] Solid state battery LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 A positive electrode mixture containing O2, a binder, and a solvent was applied onto one side of an Al current collector foil to obtain a positive electrode layer. A mixture of a Li2S-P2S5-based material containing LiBr and LiI as a sulfide-based solid electrolyte, a binder, and a solvent was prepared. This mixture was applied onto a resin film to produce a thin solid electrolyte film. The thin solid electrolyte film was applied at a density of 7 ton / cm. 2 The solid electrolyte layer was obtained by pressing the substrate at a pressure of 100 MPa. A Sn material was prepared as a raw material for the modification layer. Using the Sn material and a magnetron sputtering device, Sn was deposited on one surface of the solid electrolyte layer to form a Sn layer (i.e., a modification layer) having a thickness of 100 nm. A Ni current collector was placed as a negative electrode current collector on the surface of the solid electrolyte layer on which the Sn layer was placed. A positive electrode layer was placed on the surface opposite to the surface on which the Sn layer was placed, so that the solid electrolyte layer and the positive electrode layer were in contact with each other. These were cold isostatically pressed (CIP) at 4 ton / cm. 2 The solid-state battery had a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, a Sn layer, and a negative electrode current collector, in this order.

[0083] [1.1.2] Negative electrode active material layer of a solid-state battery when fully charged The charged solid-state battery was cross-sectionally processed, and the negative electrode active material layer was observed with a secondary electron microscope (SEM). The thickness of the layer that appears as a Li layer was confirmed. The type and concentration of the contained metal species and the thickness of the Li-Sn layer were estimated from element mapping and spectrum analysis of each layer with an energy dispersive X-ray analyzer (EDX). This revealed that the negative electrode active material layer of Example 1 had a Li layer and a Li-Sn layer in this order in the SE direction when the solid-state battery was fully charged.

[0084] [1.2] Example 2 [1.2.1] Solid state battery Except for changing the Sn material to an Al material, a solid-state battery was obtained in the same manner as in Example 1. The solid-state battery had a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, an Al layer, and a negative electrode current collector, in this order.

[0085] [1.2.2] Negative electrode active material layer of a solid-state battery when fully charged The cross section of the charged solid-state battery was processed, and the negative electrode active material layer was analyzed in the same manner as in Example 1. This revealed that the negative electrode active material layer of Example 2 had a Li layer and a Li-Al layer in this order in the SE direction when the solid-state battery was fully charged.

[0086] [1.3] Example 3 [1.3.1] Solid state battery Except for changing the Sn material to a Zn material, a solid-state battery was obtained in the same manner as in Example 1. The solid-state battery had a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, a Zn layer, and a negative electrode current collector, in this order.

[0087] [1.3.2] Negative electrode active material layer of a fully charged solid-state battery The cross section of the charged solid-state battery was processed, and the negative electrode active material layer was analyzed in the same manner as in Example 1. This revealed that the negative electrode active material layer of Example 3 had a Li layer and a Li-Zn layer in this order in the SE direction when the solid-state battery was fully charged.

[0088] [1.4] Example 4 [1.4.1] Solid state battery LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 A positive electrode mixture containing O2, a binder, and a solvent was applied onto one side of an Al current collector foil to obtain a positive electrode layer. A mixture of a Li2S-P2S5-based material containing LiBr and LiI as a sulfide-based solid electrolyte, a binder, and a solvent was prepared. This mixture was applied onto a resin film to produce a thin solid electrolyte film. The thin solid electrolyte film was applied at a density of 7 ton / cm. 2The solid electrolyte layer was obtained by pressing the substrate at a pressure of 100 MPa. A Sn material was prepared as a raw material for the modification layer. Using the Sn material and a magnetron sputtering device, Sn was deposited on one surface of the solid electrolyte layer to form a Sn layer (ie, a modification layer) having a thickness of 100 nm. Using an electron beam deposition apparatus, Mg was deposited on one surface of a Ni foil serving as a negative electrode current collector to form a 1000 nm-thick Mg layer. A Ni current collector foil having an Mg layer on one side was placed on the side of the solid electrolyte layer where the Sn layer was placed. A positive electrode layer was placed on the side opposite to the side where the Sn layer was placed, so that the solid electrolyte layer and the positive electrode layer were in contact with each other. These were cold isostatically pressed (CIP) at 4 ton / cm. 2 The solid-state battery had a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, a Sn layer, a Mg layer, and a negative electrode current collector, in this order.

[0089] [1.4.2] Negative electrode active material layer of a fully charged solid-state battery The cross section of the charged solid-state battery was processed, and the negative electrode active material layer was analyzed in the same manner as in Example 1. This revealed that the negative electrode active material layer of Example 4 had a Li-Mg layer and a Li-Sn layer in this order in the SE direction when the solid-state battery was fully charged.

[0090] [1.5] Example 5 [1.5.1] Solid state battery Except for changing the Sn material to an Al material, a solid-state battery was obtained in the same manner as in Example 4. The solid-state battery had a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, an Al layer, an Mg layer, and a negative electrode current collector, in this order.

[0091] [1.5.2] Negative electrode active material layer of a fully charged solid-state battery The cross section of the charged solid-state battery was processed, and the negative electrode active material layer was analyzed in the same manner as in Example 1. This revealed that the negative electrode active material layer of Example 5 had a Li-Mg-Al layer and a Li-Al layer in this order in the SE direction when the solid-state battery was fully charged.

[0092] [1.6] Example 6 [1.6.1] Solid state battery Except for changing the Sn material to a Zn material, a solid-state battery was obtained in the same manner as in Example 4. The solid-state battery had a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, a Zn layer, an Mg layer, and a negative electrode current collector, in this order.

[0093] [1.6.2] Negative electrode active material layer of a solid-state battery when fully charged The cross section of the charged solid-state battery was processed, and the negative electrode active material layer was analyzed in the same manner as in Example 1. This revealed that the negative electrode active material layer of Example 6 had a Li-Mg-Zn layer and a Li-Zn layer in this order in the SE direction when the solid-state battery was fully charged.

[0094] [1.7] Comparative Example 1 [1.7.1] Solid state battery LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 A positive electrode mixture containing O2, a binder, and a solvent was applied onto one side of an Al current collector foil to obtain a positive electrode layer. A mixture of a Li2S-P2S5-based material containing LiBr and LiI as a sulfide-based solid electrolyte, a binder, and a solvent was prepared. This mixture was applied onto a resin film to produce a thin solid electrolyte film. The thin solid electrolyte film was applied at a density of 7 ton / cm. 2 The solid electrolyte layer was obtained by pressing the substrate at a pressure of 100 MPa. A Ni current collector was placed on one side of the solid electrolyte layer as a negative electrode current collector. A positive electrode layer was placed on the side of the solid electrolyte layer opposite to the side on which the Ni current collector was placed so that the solid electrolyte layer and the positive electrode layer were in contact with each other. These were then cold isostatically pressed (CIP) at 4 ton / cm. 2 The solid-state battery had a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, and a negative electrode current collector, in this order.

[0095] [1.7.2] Negative electrode active material layer of a fully charged solid-state battery The solid-state battery of Comparative Example 1 experienced a short circuit during charging, and therefore did not function as a battery.

[0096] [1.8] Comparative Example 2 [1.8.1] Solid state battery LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 A positive electrode mixture containing O2, a binder, and a solvent was applied onto one side of an Al current collector foil to obtain a positive electrode layer. A mixture of a Li2S-P2S5-based material containing LiBr and LiI as a sulfide-based solid electrolyte, a binder, and a solvent was prepared. This mixture was applied onto a resin film to produce a thin solid electrolyte film. The thin solid electrolyte film was applied at a density of 7 ton / cm. 2 The solid electrolyte layer was obtained by pressing the substrate at a pressure of 100 MPa. Using an electron beam deposition apparatus, Mg was deposited on one surface of a Ni foil serving as a negative electrode current collector to form a 1000 nm-thick Mg layer. A Ni current collector foil having an Mg layer on one side was placed on one side of the solid electrolyte layer. A positive electrode layer was placed on the side of the solid electrolyte layer opposite to the side on which the Mg layer was placed, so that the solid electrolyte layer and the positive electrode layer were in contact with each other. These were cold isostatically pressed (CIP) at 4 ton / cm. 2 The solid-state battery had a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, an Mg layer, and a negative electrode current collector, in this order.

[0097] [1.8.2] Negative electrode active material layer of a solid-state battery when fully charged The cross section of the charged solid-state battery was processed, and the negative electrode active material layer was analyzed in the same manner as in Example 1. This revealed that the negative electrode active material layer of Comparative Example 2 had a Li-Mg layer and a Li layer in this order in the SE direction when the solid-state battery was fully charged.

[0098] [1.9] Comparative Example 3 [1.9.1] Solid state battery LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 A positive electrode mixture containing O2, a binder, and a solvent was applied onto one side of an Al current collector foil to obtain a positive electrode layer. A mixture of a Li2S-P2S5-based material containing LiBr and LiI as a sulfide-based solid electrolyte, a binder, and a solvent was prepared. This mixture was applied onto a resin film to produce a thin solid electrolyte film. The thin solid electrolyte film was applied at a density of 7 ton / cm. 2 The solid electrolyte layer was obtained by pressing the substrate at a pressure of 100 MPa. Using a magnetron sputtering device, Zn was deposited on one surface of a Ni foil serving as a negative electrode current collector to form a Zn layer having a thickness of 100 nm. A Ni current collector foil having a Zn layer on one side was placed on one side of the solid electrolyte layer. A positive electrode layer was placed on the side of the solid electrolyte layer opposite to the side on which the Zn layer was placed, so that the solid electrolyte layer and the positive electrode layer were in contact with each other. These were cold isostatically pressed (CIP) at 4 ton / cm. 2 The solid-state battery had a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, a Zn layer, and a negative electrode current collector, in this order.

[0099] [1.9.2] Negative electrode active material layer of a solid-state battery when fully charged The cross section of the charged solid-state battery was processed, and the negative electrode active material layer was analyzed in the same manner as in Example 1. This revealed that the negative electrode active material layer of Comparative Example 3 had a Li-Zn layer and a Li layer in this order in the SE direction when the solid-state battery was fully charged.

[0100] [2] Capacity retention measurement The capacity retention rate was calculated by comparing the initial discharge capacity with the discharge capacity after 20 repeated charge / discharge cycles, using the following formula (2). Equation (2): Capacity retention rate (%) = (discharge capacity after 20 cycles / discharge capacity after 1 cycle) x 100 The measurement results of the capacity retention rate are shown in Table 1. In Comparative Example 1, the capacity retention rate could not be measured because a short circuit occurred. The allowable range of the capacity retention rate is 75.0% or more.

[0101] [Table 1]

[0102] In Table 1, in "negative electrode active material layer", "-" indicates that there is no layer. In "capacity retention rate", "-" indicates that the capacity retention rate could not be measured. "CC side" in "uncharged" refers to the layer formed on the surface of the negative electrode current collector. "SE side" in "uncharged" refers to the layer formed on the surface of the solid electrolyte layer. "CC side" in "fully charged" refers to the layer of the negative electrode active material layer on the negative electrode current collector side. "SE side" in "fully charged" refers to the layer of the negative electrode active material layer on the solid electrolyte layer side.

[0103] The negative electrode layer of Comparative Example 1 did not have a negative electrode active material layer, and therefore the solid-state battery of Comparative Example 1 experienced a short circuit during charging. The negative electrode active material layers of Comparative Examples 2 and 3 did not have a Li layer, a Li-Mg layer or a Li-Mg-X layer, and a Li-X layer in this order in the SE direction when the solid-state batteries were fully charged. Therefore, the capacity retention rates of Comparative Examples 2 and 3 were less than 75.0%. From these results, it was found that the solid-state batteries of Comparative Examples 1 to 3 did not have a high capacity retention rate.

[0104] The negative electrode active material layer of Example 1 has a Li layer and a Li-Sn layer in this order in the SE direction when the solid-state battery is fully charged. The Li-Sn layer is formed on the surface of the solid electrolyte layer. The negative electrode active material layer of Example 2 has a Li layer and a Li-Al layer in this order in the SE direction when the solid-state battery is fully charged. The Li-Al layer is formed on the surface of the solid electrolyte layer. The negative electrode active material layer of Example 3 has a Li layer and a Li-Zn layer in this order in the SE direction when the solid-state battery is fully charged. The Li-Zn layer is formed on the surface of the solid electrolyte layer. The negative electrode active material layer of Example 4 has a Li-Mg layer and a Li-Sn layer in this order in the SE direction when the solid-state battery is fully charged. The Li-Sn layer is formed on the surface of the solid electrolyte layer. The negative electrode active material layer of Example 5 has a Li-Mg-Al layer and a Li-Al layer in this order in the SE direction when the solid-state battery is fully charged. The Li-Al layer is formed on the surface of the solid electrolyte layer. The negative electrode active material layer of Example 6 has a Li-Mg-Zn layer and a Li-Zn layer in this order in the SE direction when the solid-state battery is fully charged. The Li-Zn layer is formed on the surface of the solid electrolyte layer. Therefore, the capacity retention rates of Examples 1 to 6 were 75.0% or more. From these results, it was found that the solid state batteries of Examples 1 to 6 were solid state batteries with high capacity retention rates.

Claims

1. A solid-state battery including a positive electrode layer, a solid electrolyte layer, and a negative electrode layer in this order, the negative electrode layer includes a negative electrode current collector and a negative electrode active material layer in this order in a direction from the negative electrode layer toward the solid electrolyte layer, when the solid-state battery is fully charged, the negative electrode active material layer has a Li layer, a Li—Mg layer or a Li—Mg—X layer, and a Li—X layer in this order in the direction; The X is at least one selected from the group consisting of Sn, Zn, and Al, The Li-X layer is formed on the surface of the solid electrolyte layer.

2. 2. The solid-state battery according to claim 1, wherein when the solid-state battery is fully charged, the negative electrode active material layer has the Li-Mg layer or the Li-Mg-X layer, and the Li-X layer.

3. 3. The solid-state battery according to claim 1, wherein the negative electrode active material layer has the Li-Mg layer and the Li-Sn layer in this order in the direction when the solid-state battery is fully charged.

4. 3. The solid-state battery according to claim 1, wherein the negative electrode active material layer has a Li-Mg-Zn layer and a Li-Zn layer in this order in the direction when the solid-state battery is fully charged.

5. 3. The solid-state battery according to claim 1, wherein the negative electrode active material layer has a Li-Mg-Al layer and a Li-Al layer in this order in the direction when the solid-state battery is fully charged.

6. 2. The solid-state battery according to claim 1, wherein the negative electrode active material layer has a Li layer and a Li-X layer in this order in the direction when the solid-state battery is fully charged.

7. 7. The solid-state battery according to claim 6, wherein the negative electrode active material layer has a Li layer and a Li-Sn layer in this order in the direction when the solid-state battery is fully charged.

8. 1. A method for manufacturing a solid-state battery having a positive electrode layer, a solid electrolyte layer, and a negative electrode layer in this order, comprising: forming an X layer on a surface of the solid electrolyte layer on the negative electrode layer side, The method for producing a solid-state battery, wherein X is at least one selected from the group consisting of Sn, Zn, and Al.

9. the negative electrode layer has a negative electrode current collector, The method for producing a solid-state battery according to claim 8 , further comprising the step of forming an Mg layer on a surface of the negative electrode current collector on the side facing the solid electrolyte layer.

Citation Information

Patent Citations

  • Three-dimensional composite negative electrode material and preparation method thereof

    CN111682176A

  • Nonaqueous electrolyte secondary battery

    JP1997245836A

  • All-solid battery

    JP2021051866A

  • Metal alloy layers on substrates, methods of making same, and uses thereof

    US20190088986A1

  • Lithium secondary battery

    WO2019230279A1