Solar cell and method for manufacturing solar cell

The solar cell design with a laminated metal electrode layer formed by low-pressure spraying and sized metal particles addresses internal stress, enhancing reliability and flexibility.

JP2024135490AInactive Publication Date: 2024-10-04KANEKA CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023046199
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Solar cells experience internal stress in the semiconductor substrate, particularly in back electrode type cells, which reduces their reliability.

Method used

A solar cell design with a band-like metal electrode layer having a laminated structure of a base layer formed by low-pressure spraying of metal particles and a plating layer, where the metal particles are sized between 0.9 μm and 500 μm, and gaps exist at the grain boundaries of the base layer.

Benefits of technology

The design reduces internal stress in the semiconductor substrate, improving the reliability and flexibility of the solar cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135490000001_ABST
    Figure 2024135490000001_ABST
Patent Text Reader

Abstract

To provide a solar cell that reduces internal stress in a semiconductor substrate.SOLUTION: In a solar cell 1 having a semiconductor substrate 11, conductive semiconductor layers 25, 35 disposed on the main surface of semiconductor substrate 11, and metal electrode layers 29, 39 corresponding to the conductive semiconductor layers 25, 35, the metal electrode layers 29, 39 have a band shape, the metal electrode layers 29, 39 have a laminated structure consisting of a base layer 29l, 39l with a layer structure of metal particles deposited in a series, and a metal plating layer 29u, 39u, and viewed from the main surface side of the semiconductor substrate 11, and the size of the metal particles in the base layers 29l, 39l is not less than 0.9 μm and not more than 500 μm.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solar cell and a method for manufacturing a solar cell. [Background technology]

[0002] Solar cells using a semiconductor substrate include a double-sided electrode type solar cell in which electrodes are formed on both the light-receiving surface side and the back surface side, and a back surface electrode type solar cell in which an electrode is formed only on the back surface side. Patent Document 1 discloses a double-sided electrode type solar cell, and Patent Document 2 discloses a back surface electrode type solar cell. As disclosed in Patent Documents 1 and 2, whether it is a double-sided electrode type or a back surface electrode type solar cell, the solar cell includes a semiconductor substrate, a conductive semiconductor layer disposed on the main surface of the semiconductor substrate, and a metal electrode layer corresponding to the conductive semiconductor layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-152620 A [Patent Document 2] JP 2019-121627 A Summary of the Invention [Problem to be solved by the invention]

[0004] As described above, in solar cells, a metal electrode layer is formed on a semiconductor substrate, which causes the semiconductor substrate to warp and generates stress inside the semiconductor substrate. This tendency is more pronounced in back electrode type solar cells. When the internal stress of the semiconductor substrate increases, the reliability of the solar cell decreases.

[0005] An object of the present invention is to provide a solar cell that reduces (suppresses, alleviates) the internal stress in the semiconductor substrate, and a method for manufacturing the solar cell. [Means for solving the problem]

[0006] The solar cell of the present invention is a solar cell comprising a semiconductor substrate, a conductive semiconductor layer arranged on a main surface of the semiconductor substrate, and a metal electrode layer corresponding to the conductive semiconductor layer, wherein the metal electrode layer has a band-like shape and has a layered structure of a base layer having a layered structure in which metal particles are accumulated in a continuous manner, and a metal plating layer, and when viewed from the main surface side of the semiconductor substrate, the size of the metal particles in the base layer is 0.9 μm or more and 500 μm or less.

[0007] The method for manufacturing a solar cell according to the present invention is a method for manufacturing a solar cell as described above, and includes the steps of forming the conductive semiconductor layer on a main surface of the semiconductor substrate, forming the base layer by melting metal particles by discharge in a reduced pressure environment using a reduced pressure spraying method, spraying the molten metal particles with a carrier gas onto the semiconductor substrate, and depositing the metal particles on the conductive semiconductor layer of the semiconductor substrate, and forming a metal plating layer on the base layer using a plating method. Effect of the Invention

[0008] According to the present invention, it is possible to reduce (suppress, alleviate) the internal stress in the semiconductor substrate in the solar cell. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a diagram showing the solar cell (back electrode type) according to the present embodiment as viewed from the back surface side. [Diagram 2] 2 is a cross-sectional view taken along line II-II of the solar cell (back electrode type) of FIG. 1. [Figure 3A] 3A to 3C are diagrams illustrating a semiconductor layer forming step in the manufacturing method for the solar cell (back electrode type) according to the embodiment. [Figure 3B] 4 is a diagram showing a transparent electrode layer forming step in the manufacturing method for the solar cell (back electrode type) according to the embodiment. FIG. [Figure 3C] 4 is a diagram showing a step of forming a base layer for a metal electrode layer in the manufacturing method for a solar cell (back electrode type) according to the present embodiment. FIG. [Figure 3D]4 is a diagram showing a plating layer forming step of a metal electrode layer in the manufacturing method for a solar cell (back electrode type) according to the present embodiment. FIG. [Figure 4] FIG. 11 is a cross-sectional view of a solar cell (double-sided electrode type) according to a modified example of the present embodiment. [Figure 5A] 3 is an example of an SEM image of the surface of the underlayer of the metal electrode layer in the solar cell of FIG. 2. [Figure 5B] FIG. 5B is an example of an enlarged SEM image of part VB in FIG. 5A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. In each drawing, the same or corresponding parts are denoted by the same reference numerals. For convenience, hatching and reference numerals may be omitted, in which case other drawings shall be referred to.

[0011] (Solar Cell) Fig. 1 is a view of the solar cell according to this embodiment as seen from the back surface side, and Fig. 2 is a cross-sectional view of the solar cell along line II-II in Fig. 1. The solar cell 1 shown in Fig. 1 and Fig. 2 is a back electrode type (also called a back contact type or back junction type) heterojunction solar cell.

[0012] Solar cell 1 includes a semiconductor substrate 11 with two main surfaces, and the main surface of semiconductor substrate 11 has a first region 7 and a second region 8. In the following, the main surface of semiconductor substrate 11 that receives light is referred to as the light-receiving surface, and the main surface of semiconductor substrate 11 opposite the light-receiving surface is referred to as the back surface.

[0013] The first region 7 has a so-called comb shape and includes a plurality of finger portions 7f corresponding to the teeth of the comb and busbar portions 7b corresponding to supports for the teeth of the comb. The busbar portions 7b extend in a first direction (X direction) along one side of the semiconductor substrate 11, and the finger portions 7f extend from the busbar portions 7b in a second direction (Y direction) intersecting the first direction.

[0014] Similarly, the second region 8 has a so-called comb shape and has a plurality of finger portions 8f corresponding to the teeth of the comb and a busbar portion 8b corresponding to a support portion of the teeth of the comb. The busbar portion 8b extends in a first direction along one side portion of the semiconductor substrate 11 opposite the other side portion, and the finger portions 8f extend in a second direction from the busbar portion 8b.

[0015] The finger portions 7f and 8f are strip-shaped extending in the second direction and are alternately provided in the first direction. The first region 7 and the second region 8 may be formed in a stripe pattern.

[0016] 2, the solar cell 1 includes a passivation layer 13 and an optical adjustment layer 15, which are formed (deposited, laminated, formed) in that order on the light-receiving surface side of the semiconductor substrate 11. The solar cell 1 also includes a passivation layer 23, a first conductivity type semiconductor layer 25, and a first electrode layer 27, which are formed (deposited, laminated, formed) in that order on a portion (mainly, the first region 7) of the back surface side of the semiconductor substrate 11. The solar cell 1 also includes a passivation layer 33, a second conductivity type semiconductor layer 35, and a second electrode layer 37, which are formed (deposited, laminated, formed) in that order on another portion (mainly, the second region 8) of the back surface side of the semiconductor substrate 11.

[0017] The semiconductor substrate 11 is formed of a crystalline silicon material such as single crystal silicon or polycrystalline silicon. The semiconductor substrate 11 is, for example, an n-type semiconductor substrate in which a crystalline silicon material is doped with an n-type dopant. The semiconductor substrate 11 may be, for example, a p-type semiconductor substrate in which a crystalline silicon material is doped with a p-type dopant. An example of the n-type dopant is phosphorus (P). An example of the p-type dopant is boron (B). The semiconductor substrate 11 functions as a photoelectric conversion substrate that absorbs incident light from the light-receiving surface side and generates photocarriers (electrons and holes).

[0018] By using crystalline silicon as the material for the semiconductor substrate 11, the dark current is relatively small, and a relatively high output (stable output regardless of illuminance) can be obtained even when the intensity of incident light is low.

[0019] Semiconductor substrate 11 may have a pyramidal fine uneven structure called a texture structure on the light-receiving surface side, which reduces the reflection of incident light on the light-receiving surface and improves the light trapping effect in semiconductor substrate 11.

[0020] Furthermore, the semiconductor substrate 11 may have a pyramidal fine uneven structure, called a texture structure, on the back surface side thereof, which increases the efficiency of collection of light that is not absorbed by the semiconductor substrate 11 and passes through it.

[0021] The passivation layer 13 is formed on the light-receiving surface side of the semiconductor substrate 11. The passivation layer 23 is formed in a first region 7 on the back surface side of the semiconductor substrate 11. The passivation layer 33 is formed in a second region 8 on the back surface side of the semiconductor substrate 11. The passivation layers 13, 23, and 33 are formed of, for example, an intrinsic (i-type) amorphous silicon material. The passivation layers 13, 23, and 33 suppress recombination of carriers generated in the semiconductor substrate 11 and increase the carrier collection efficiency.

[0022] The optical adjustment layer 15 is formed on the passivation layer 13 on the light-receiving surface side of the semiconductor substrate 11. The optical adjustment layer 15 functions as an anti-reflection layer that prevents or suppresses reflection of incident light, and improves the efficiency of light incidence on the semiconductor substrate 11. The optical adjustment layer 15 also functions as a protective layer that protects the light-receiving surface side of the semiconductor substrate 11 and the passivation layer 13. The optical adjustment layer 15 is formed of an insulating material, for example, silicon oxide (SiO), silicon nitride (SiN), or a composite thereof such as silicon oxynitride (SiON).

[0023] The first conductive type semiconductor layer 25 is formed on the passivation layer 23, i.e., in the first region 7 on the back surface side of the semiconductor substrate 11. The first conductive type semiconductor layer 25 is formed of, for example, an amorphous silicon material. The first conductive type semiconductor layer 25 is, for example, a p-type semiconductor layer in which an amorphous silicon material is doped with a p-type dopant (for example, the above-mentioned boron (B)).

[0024] The second conductive type semiconductor layer 35 is formed on the passivation layer 33, i.e., in the second region 8 on the back surface side of the semiconductor substrate 11. The second conductive type semiconductor layer 35 is formed of, for example, an amorphous silicon material. The second conductive type semiconductor layer 35 is, for example, an n-type semiconductor layer in which an amorphous silicon material is doped with an n-type dopant (for example, the above-mentioned phosphorus (P)).

[0025] Alternatively, the first conductive type semiconductor layer 25 may be an n-type semiconductor layer, and the second conductive type semiconductor layer 35 may be a p-type semiconductor layer.

[0026] The first conductive type semiconductor layer 25 and the passivation layer 23, and the second conductive type semiconductor layer 35 and the passivation layer 33 form strips extending in the second direction (Y direction) and are arranged alternately in the first direction (X direction). Parts of the second conductive type semiconductor layer 35 and the passivation layer 33 may overlap parts of the adjacent first conductive type semiconductor layer 25 and passivation layer 23.

[0027] The first electrode layer 27 corresponds to the first conductive type semiconductor layer 25, specifically, is formed on the first conductive type semiconductor layer 25 in the first region 7 on the back surface side of the semiconductor substrate 11. The first electrode layer 27 may have a first transparent electrode layer 28 and a first metal electrode layer 29 formed in this order on the first conductive type semiconductor layer 25 (FIG. 2), or may have only the first metal electrode layer 29 formed on the first conductive type semiconductor layer 25 (not shown).

[0028] The second electrode layer 37 corresponds to the second conductive type semiconductor layer 35, specifically, is formed on the second conductive type semiconductor layer 35 in the second region 8 on the back surface side of the semiconductor substrate 11. The second electrode layer 37 may have a second transparent electrode layer 38 and a second metal electrode layer 39 formed in this order on the second conductive type semiconductor layer 35 (FIG. 2), or may have only the second metal electrode layer 39 formed on the second conductive type semiconductor layer 35 (not shown).

[0029] The first electrode layer 27 and the second electrode layer 37 are in the form of strips extending in the second direction (Y direction) and are alternately arranged in the first direction (X direction). The first electrode layer 27 and the second electrode layer 37 are separated from each other. That is, the first transparent electrode layer 28 and the second transparent electrode layer 38 are in the form of strips extending in the second direction and are alternately arranged in the first direction. The first transparent electrode layer 28 and the second transparent electrode layer 38 are separated from each other. Also, the first metal electrode layer 29 and the second metal electrode layer 39 are in the form of strips extending in the second direction and are alternately arranged in the first direction. The first metal electrode layer 29 and the second metal electrode layer 39 are separated from each other.

[0030] The first transparent electrode layer 28 and the second transparent electrode layer 38 are made of a transparent conductive material, such as ITO (Indium Tin Oxide: a composite oxide of indium oxide and tin oxide).

[0031] The first metal electrode layer 29 has a first underlayer 29l and a first plating layer 29u, and the second metal electrode layer 39 has a second underlayer 39l and a second plating layer 39u.

[0032] The first underlayer 29l and the second underlayer 39l are formed by a reduced pressure spraying method using particulate metal materials such as silver, copper, and aluminum, as described below. Fig. 5A is an example of a SEM (Scanning Electron Microscope) image of the surfaces of the first underlayer 29l and the second underlayer 39l, and Fig. 5B is an example of an SEM image in which the VB portion of Fig. 5A is enlarged. In the examples of Figs. 5A and 5B, reduced pressure spraying was performed using copper powder with a particle diameter of 8 μm.

[0033] 5A and 5B, the first underlayer 29l and the second underlayer 39l have a layer structure in which metal particles are stacked in a continuous manner. When viewed from the back surface side, the size (particle diameter) of the metal particles in the first underlayer 29l is 0.9 μm or more and 500 μm or less, preferably 0.9 μm or more and 13 μm or less, and when viewed from the back surface side, the size (particle diameter) of the metal particles in the second underlayer 39l is 0.9 μm or more and 500 μm or less, preferably 0.9 μm or more and 13 μm or less.

[0034] Also, in a cross section of the first underlayer 29l along the back surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section of the first underlayer 29l intersecting the back surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section intersecting the back surface, there are gaps at the boundaries between the layer adjacent to the first underlayer 29l, i.e., the first transparent electrode layer 28, and the metal particles of the first underlayer 29l (FIG. 2). Note that, if the first electrode layer 27 does not have the first transparent electrode layer 28, there are gaps at the boundaries between the layer adjacent to the first underlayer 29l, i.e., the first conductive type semiconductor layer 25, and the metal particles of the first underlayer 29l in the cross section intersecting the back surface (not shown).

[0035] In addition, in a cross section of the second underlayer 39l along the back surface, there are gaps at the grain boundaries of the metal particles. In addition, in a cross section of the second underlayer 39l intersecting the back surface, there are gaps at the grain boundaries of the metal particles. In addition, in a cross section intersecting the back surface, there are gaps at the boundary between the layer adjacent to the second underlayer 39l, i.e., the second transparent electrode layer 38, and the metal particles of the second underlayer 39l (FIG. 2). Note that, if the second electrode layer 37 does not have the second transparent electrode layer 38, there are gaps at the boundary between the layer adjacent to the second underlayer 39l, i.e., the second conductive type semiconductor layer 35, and the metal particles of the second underlayer 39l in a cross section intersecting the light receiving surface (not shown).

[0036] As described below, the first plating layer 29u and the second plating layer 39u are formed by a plating method (electrolytic plating method or electroless plating method) using a metal material such as silver, copper, aluminum, etc. As a result, a part of the first plating layer 29u is embedded in gaps between grain boundaries of some of the metal particles on the first plating layer 29u side of the first foundation layer 29l, and a part of the second plating layer 39u is embedded in gaps between grain boundaries of some of the metal particles on the second plating layer 39u side of the second foundation layer 39l.

[0037] (Solar Cell Manufacturing Method) Next, a method for manufacturing a solar cell according to the present embodiment will be described with reference to Figures 3A to 3D. Figure 3A is a diagram showing a semiconductor layer forming step in the method for manufacturing a solar cell according to the present embodiment, and Figure 3B is a diagram showing a transparent electrode layer forming step in the method for manufacturing a solar cell according to the present embodiment. Figure 3C is a diagram showing a base layer forming step for a metal electrode layer in the method for manufacturing a solar cell according to the present embodiment, and Figure 3D is a diagram showing a plating layer forming step for a metal electrode layer in the method for manufacturing a solar cell according to the present embodiment.

[0038] 3A, a passivation layer 23 and a first conductive type semiconductor layer 25 are formed on a part of the back surface side of the semiconductor substrate 11, specifically, on the first region 7 (semiconductor layer formation step). An example of a method for forming the passivation layer 23 and the first conductive type semiconductor layer 25 will be described below, but the method for forming the passivation layer 23 and the first conductive type semiconductor layer 25 is not limited thereto.

[0039] For example, a passivation film and a first conductive type semiconductor film may be formed on the entire back surface of semiconductor substrate 11 by using a CVD method or a PVD method, and then passivation layer 23 and first conductive type semiconductor layer 25 may be patterned by using an etching method that uses a mask or a metal mask generated by a photolithography technique. Note that examples of etching solutions for p-type semiconductor films include acidic solutions such as hydrofluoric acid containing ozone and a mixture of nitric acid and hydrofluoric acid, and examples of etching solutions for n-type semiconductor films include alkaline solutions such as an aqueous solution of potassium hydroxide.

[0040] Alternatively, when a passivation layer and a first conductive type semiconductor layer are laminated on the back surface side of the semiconductor substrate 11 using a CVD method or a PVD method, the passivation layer 23 and the p-type semiconductor layer 25 may be deposited and patterned simultaneously using a mask.

[0041] Next, a passivation layer 33 and a second conductive type semiconductor layer 35 are formed on another part of the back surface side of the semiconductor substrate 11, specifically, on the second region 8 (semiconductor layer formation step). An example of a method for forming the passivation layer 33 and the second conductive type semiconductor layer 35 will be described below, but the method for forming the passivation layer 33 and the second conductive type semiconductor layer 35 is not limited thereto.

[0042] For example, as described above, a passivation film and a second conductive type semiconductor film may be formed on the entire back surface side of semiconductor substrate 11 using a CVD method or a PVD method, and then passivation layer 33 and second conductive type semiconductor layer 35 may be patterned using an etching method that uses a mask or a metal mask generated using a photolithography technique.

[0043] Alternatively, when a passivation layer and a second conductive type semiconductor layer are laminated on the back surface side of the semiconductor substrate 11 using a CVD method or a PVD method, the passivation layer 33 and the second conductive type semiconductor layer 35 may be deposited and patterned simultaneously using a mask.

[0044] In this semiconductor layer forming step, a passivation layer 13 may be formed on the entire light-receiving surface side of semiconductor substrate 11.

[0045] 3B, a first transparent electrode layer 28 is formed on the first conductive type semiconductor layer 25, specifically in the first region 7, and a second transparent electrode layer 38 is formed on the second conductive type semiconductor layer 35, specifically in the second region 8 (transparent electrode layer forming step). An example of a method for forming the first transparent electrode layer 28 and the second transparent electrode layer 38 is shown below, but the method for forming the first transparent electrode layer 28 and the second transparent electrode layer 38 is not limited thereto.

[0046] For example, a transparent conductive film may be formed by using a CVD method or a PVD method over the entire back surface side of the semiconductor substrate 11, i.e., on the first conductivity type semiconductor layer 25 and the second conductivity type semiconductor layer 35, and then the transparent conductive film may be patterned by an etching method using a mask or a metal mask generated by a photolithography technique, thereby forming the first transparent electrode layer 28 and the second transparent electrode layer 38 that are separated from each other. An example of the etching method is a wet etching method, and an example of the etching solution is an acidic solution such as hydrochloric acid (HCl).

[0047] Alternatively, when the first transparent electrode layer and the second transparent electrode layer are laminated on the back side of the semiconductor substrate 11 using a CVD method or a PVD method, the first transparent electrode layer 28 and the second transparent electrode layer 38 may be simultaneously deposited and patterned using a mask.

[0048] At this time, the optical adjustment layer 15 may be formed on the entire light-receiving surface side of the semiconductor substrate 11.

[0049] Next, as shown in FIG. 3C, a first base layer 29l of the first metal electrode layer 29 is formed on the first transparent electrode layer 28, specifically in the first region 7, and a second base layer 39l of the second metal electrode layer 39 is formed on the second transparent electrode layer 38, specifically in the second region 8 (base layer formation process for metal electrode layer).

[0050] For example, the first underlayer 29l and the second underlayer 39l are formed by a reduced pressure thermal spraying method using a particulate metal material. - By discharging plasma or other electrical discharge, the particulate metal material is melted, The molten particles are sprayed onto the target surface by the carrier gas. Depositing molten particles onto the surface of the object; This is a film-forming method in which the molten particles deposited on the surface of the object are instantly cooled to form a metal film.

[0051] As a result, as described above, the first underlayer 29l and the second underlayer 39l have a layer structure in which metal particles are stacked in a continuous manner. Also, in the cross section of the first underlayer 29l and the second underlayer 39l along the back surface, there are gaps at the grain boundaries of the metal particles. Also, in the cross section of the first underlayer 29l and the second underlayer 39l intersecting the back surface, there are gaps at the grain boundaries of the metal particles.

[0052] In addition, in a cross section intersecting the rear surface, there are gaps at the boundary between the layer adjacent to the first underlayer 29l (first transparent electrode layer 28 or first conductive type semiconductor layer 25) and the metal particles of the first underlayer 29l. In addition, in a cross section intersecting the rear surface, there are gaps at the boundary between the layer adjacent to the second underlayer 39l (second transparent electrode layer 38 or second conductive type semiconductor layer 35) and the metal particles of the second underlayer 39l.

[0053] Next, as shown in FIG. 3D, a plating method is used to form a first plating layer 29u of the first metal electrode layer 29 on the first base layer 29l, specifically in the first region 7, and a second plating layer 39u of the second metal electrode layer 39 on the second base layer 39l, specifically in the second region 8 (plating layer formation process of metal electrode layer).

[0054] Through the above steps, the back electrode type solar cell 1 of this embodiment is obtained.

[0055] As described above, according to the manufacturing method for the solar cell of this embodiment, the first underlayer 29l of the first metal electrode layer 29 and the second underlayer 39l of the second metal electrode layer 39 are formed by a reduced pressure spraying method using a particulate metal material. As a result, according to the solar cell 1 of this embodiment, the first underlayer 29l of the first metal electrode layer 29 and the second underlayer 39l of the second metal electrode layer 39 have a layer structure in which metal particles are deposited in a continuous manner.

[0056] Furthermore, in a cross section of the first underlayer 29l and the second underlayer 39l along the back surface, there are gaps at the grain boundaries of the metal particles. Furthermore, in a cross section of the first underlayer 29l and the second underlayer 39l intersecting the back surface, there are gaps at the grain boundaries of the metal particles.

[0057] In addition, in a cross section intersecting the rear surface, there are gaps at the boundary between the layer adjacent to the first underlayer 29l (first transparent electrode layer 28 or first conductive type semiconductor layer 25) and the metal particles of the first underlayer 29l. In addition, in a cross section intersecting the rear surface, there are gaps at the boundary between the layer adjacent to the second underlayer 39l (second transparent electrode layer 38 or second conductive type semiconductor layer 35) and the metal particles of the second underlayer 39l.

[0058] As a result, first foundation layer 29l and second foundation layer 39l have a low Young's modulus and high flexibility, and therefore, according to solar cell 1 of the present embodiment, warping of semiconductor substrate 11 can be reduced, and internal stress of semiconductor substrate 11 can be reduced (suppressed, alleviated).

[0059] Here, as a method for forming a metal electrode layer of a solar cell, a method is known in which a conductive paste (Ag, Cu, Al, etc.) is pattern-printed and fired using a screen printing method to form a metal electrode layer (see, for example, Patent Document 1). According to this method, although material costs can be relatively reduced by pattern printing, the resistance is relatively high.

[0060] Also, as a method for forming a metal electrode layer of a solar cell, a method is known in which a base layer (seed layer) is formed by a sputtering method, the base layer is patterned by a photolithography method, and a plating layer is formed on the base layer by an electrolytic plating method to form a metal electrode layer (see, for example, Patent Document 2). According to this method, the resistance is relatively low, but the material cost is relatively high because part of the base layer is removed when the base layer is patterned by the photolithography method.

[0061] Regarding these points, according to the present embodiment, by using a low-pressure thermal spraying method as a method for forming the base layer of the metal electrode layer of a solar cell, it is possible to relatively reduce the resistance and relatively reduce material costs.

[0062] Furthermore, it has been confirmed that the method for forming the underlayer of the metal electrode layer using the reduced pressure spraying method of this embodiment has equivalent adhesion, resistance, and bonding strength of the metal electrode layer compared to the method for forming the metal electrode layer using a plating method, and furthermore, it is possible to reduce warping of the semiconductor substrate and reduce (suppress, mitigate) the internal stress of the semiconductor substrate.

[0063] The adhesion of the metal electrode layer was evaluated by a cross-cut test conforming to the JIS-K5400 standard. The resistance of the metal electrode layer was evaluated by measuring the volume resistivity and surface resistivity conforming to JIS-C2139-3 and JIS K6911. The bonding strength of the metal electrode layer was evaluated by a tweezers peel strength test conforming to JIS-Z3198-8 and JIS-K6855. The warpage of the semiconductor substrate (internal stress of the semiconductor substrate) was evaluated by a test strip test conforming to JIS-H8626 (quality, item 12, electrodeposition stress).

[0064] Moreover, according to the manufacturing method of the solar cell of this embodiment, the first plating layer 29u of the first metal electrode layer 29 and the second plating layer 39u of the second metal electrode layer 39 are formed by plating. As a result, according to the solar cell 1 of this embodiment, the first metal electrode layer 29 has the first plating layer 29u, and the second metal electrode layer 39 has the second plating layer 39u. Therefore, the resistance of the first metal electrode layer 29 and the second metal electrode layer 39 can be reduced. In addition, the smoothness (surface roughness) of the surfaces of the first metal electrode layer 29 and the second metal electrode layer 39 can be increased, and the solder bondability can be improved.

[0065] Although the embodiment of the present invention has been described above, the present invention is not limited to the above-mentioned embodiment, and various changes and modifications are possible. For example, in the above-mentioned embodiment, a back electrode type solar cell 1 is illustrated (for example, FIG. 2). However, the features of the present invention are not limited to this, and can also be applied to a double-sided electrode type solar cell.

[0066] Fig. 4 is a cross-sectional view of a solar cell according to a modified example of this embodiment. The solar cell 1 shown in Fig. 4 is a double-sided electrode type heterojunction solar cell. The solar cell 1 shown in Fig. 4 includes a passivation layer 23, a first conductivity type semiconductor layer 25, and a first electrode layer 27, which are formed (deposited, laminated, formed) in this order on the light-receiving surface side of a semiconductor substrate 11. The solar cell 1 also includes a passivation layer 33, a second conductivity type semiconductor layer 35, and a second electrode layer 37, which are formed (deposited, laminated, formed) in this order on the back surface side of the semiconductor substrate 11.

[0067] The passivation layer 23 and the first conductive type semiconductor layer 25 are formed in this order on the entire light-receiving surface side of the semiconductor substrate 11. The passivation layer 33 and the second conductive type semiconductor layer 35 are formed on the entire back surface side of the semiconductor substrate 11.

[0068] The first electrode layer 27 corresponds to the first conductive type semiconductor layer 25, and specifically, is formed on the first conductive type semiconductor layer 25. The first electrode layer 27 may have a first transparent electrode layer 28 and a first metal electrode layer 29 formed in this order on the first conductive type semiconductor layer 25 (FIG. 4), or may have only the first metal electrode layer 29 formed on the first conductive type semiconductor layer 25 (not shown).

[0069] The second electrode layer 37 corresponds to the second conductive type semiconductor layer 35, and specifically, is formed on the second conductive type semiconductor layer 35. The second electrode layer 37 may have a second transparent electrode layer 38 and a second metal electrode layer 39 formed in this order on the second conductive type semiconductor layer 35 (FIG. 4), or may have only the second metal electrode layer 39 formed on the second conductive type semiconductor layer 35 (not shown).

[0070] The first transparent electrode layer 28 is formed on the entire surface of the first conductive type semiconductor layer 25, and the second transparent electrode layer 38 is formed on the entire surface of the second conductive type semiconductor layer 35. Meanwhile, the first metal electrode layer 29 and the second metal electrode layer 39 are in the form of strips extending in the second direction, and are arranged alternately in the first direction. The first metal electrode layer 29 has a first base layer 29l and a first plating layer 29u, and the second metal electrode layer 39 has a second base layer 39l and a second plating layer 39u. The second metal electrode layer 39 on the back side may be formed on the entire surface of the second conductive type semiconductor layer 35.

[0071] As described above, the first underlayer 29l and the second underlayer 39l have a layer structure in which metal particles are deposited in series.

[0072] Also, in a cross section of the first underlayer 29l along the light receiving surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section of the first underlayer 29l intersecting the light receiving surface, there are gaps at the grain boundaries of the metal particles. Also, in a cross section intersecting the light receiving surface, there are gaps at the boundary between the layer adjacent to the first underlayer 29l, i.e., the first transparent electrode layer 28, and the metal particles of the first underlayer 29l (FIG. 2). Note that, if the first electrode layer 27 does not have the first transparent electrode layer 28, there are gaps at the boundary between the layer adjacent to the first underlayer 29l, i.e., the first conductive type semiconductor layer 25, and the metal particles of the first underlayer 29l in a cross section intersecting the back surface (not shown).

[0073] In addition, in a cross section of the second underlayer 39l along the back surface, there are gaps at the grain boundaries of the metal particles. In addition, in a cross section of the second underlayer 39l intersecting the back surface, there are gaps at the grain boundaries of the metal particles. In addition, in a cross section intersecting the back surface, there are gaps at the boundary between the layer adjacent to the second underlayer 39l, i.e., the second transparent electrode layer 38, and the metal particles of the second underlayer 39l (FIG. 2). Note that, if the second electrode layer 37 does not have the second transparent electrode layer 38, there are gaps at the boundary between the layer adjacent to the second underlayer 39l, i.e., the second conductive type semiconductor layer 35, and the metal particles of the second underlayer 39l in a cross section intersecting the light receiving surface (not shown). [Explanation of symbols]

[0074] 1. Solar Cell 7 First area 8 Second area 7b, 8b Busbar section 7f,8f Finger section 11 Semiconductor substrate 13,23,33 Passivation layer 25 First conductive type semiconductor layer 27 1st electrode layer 28 First transparent electrode layer 29 First metal electrode layer 29l 1st base layer 29u 1st plating layer 35 Second conductive type semiconductor layer 37 Second electrode layer 38 Second transparent electrode layer 39 Second metal electrode layer 39l 2nd base layer 39u Second plating layer

Claims

1. A solar cell comprising a semiconductor substrate, a conductive semiconductor layer disposed on a main surface of the semiconductor substrate, and a metal electrode layer corresponding to the conductive semiconductor layer, The metal electrode layer has a strip shape, The metal electrode layer has a laminated structure of a base layer having a layer structure in which metal particles are continuously deposited, and a metal plating layer, When viewed from the main surface side of the semiconductor substrate, the size of the metal particles in the underlayer is 0.9 μm or more and 500 μm or less. Solar cell.

2. gaps are present at grain boundaries of the metal particles in a cross section of the underlayer along the main surface of the semiconductor substrate and in a cross section of the underlayer intersecting the main surface of the semiconductor substrate; a part of the plating layer is embedded in gaps between grain boundaries of the metal particles in a part of the underlayer on the plating layer side; The solar cell according to claim 1 .

3. The solar cell according to claim 1 , wherein in a cross section intersecting with a main surface of the semiconductor substrate, a gap exists at a boundary between a layer adjacent to the underlayer and the metal particles of the underlayer.

4. A method for producing a solar cell according to claim 1, comprising the steps of: forming the conductive semiconductor layer on a main surface of the semiconductor substrate; forming the underlayer by melting metal particles by discharge in a reduced pressure environment using a reduced pressure spraying method, spraying the melted metal particles onto the semiconductor substrate using a carrier gas, and depositing the metal particles on the conductive semiconductor layer of the semiconductor substrate; forming a metal plating layer on the underlayer by using a plating method; A method for manufacturing a solar cell, comprising:

Citation Information

Patent Citations

  • Solar cell

    JP2018152620A

  • Method for manufacturing solar cell and solar cell

    JP2019121627A