Rubber composition for tire

The rubber composition for tires, featuring a tackifier with specific isopropenyltoluene units and controlled molecular weight, addresses the need for improved wet grip by enhancing dispersibility and energy loss, leading to better braking performance on wet roads.

JP2024135843AActive Publication Date: 2024-10-04MITSUI CHEMICALS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023046726
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04
Estimated Expiration
2043-03-23

AI Technical Summary

Technical Problem

Tires require improved wet grip performance, particularly on wet roads, which is not adequately addressed by conventional tire rubber compositions.

Method used

A rubber composition for tires containing a tackifier with structural units derived from isopropenyltoluene and substantially free of C5 fraction, having a softening point of 85°C to 150°C and a z-average molecular weight less than 4000, is used to enhance wet grip properties.

Benefits of technology

The composition improves wet grip by enhancing tackifier dispersibility, inhibiting rubber movement during dynamic deformation and increasing energy loss, resulting in tires with superior braking performance on wet roads.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135843000003
    Figure 2024135843000003
  • Figure 2024135843000001
    Figure 2024135843000001
  • Figure 2024135843000002
    Figure 2024135843000002
Patent Text Reader

Abstract

To provide a rubber composition for tires for producing tires excellent in wet gripping property by using a tackifier that is a polymer including a structural unit derived from isopropenyl toluene, and substantially free from a structural unit derived from a C5 distillate, and in which a softening point and a z average molecular weight are predetermined rate.SOLUTION: A rubber composition for tires includes a rubber component and a tackifier. The tackifier is a polymer that includes a structural unit derived from isopropenyl toluene and is substantially free of a structural unit derived from a C5 distillate. The softening point of the tackifier is 85°C or higher and 150°C or lower. The z average molecular weight of the tackifier is less than 4,000.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition for tires. [Background technology]

[0002] 2. Description of the Related Art It is known that tires are conventionally manufactured using a rubber composition for tires that contains a rubber component and a tackifier.

[0003] As such a rubber composition for tires, for example, a rubber composition for racing tire treads containing SBR (styrene-butadiene copolymer rubber) and a copolymer resin of an aromatic vinyl compound and a C5 fraction has been proposed (see, for example, Example 2 of Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-195238 Summary of the Invention [Problem to be solved by the invention]

[0005] On the other hand, from the perspective of safety, tires are required to have improved wet grip, which indicates braking performance (braking performance on wet roads).

[0006] The present invention provides a rubber composition for tires, which is a polymer that contains structural units derived from isopropenyl toluene and is substantially free of structural units derived from a C5 fraction, and which uses a tackifier having a softening point and z-average molecular weight in a prescribed ratio, for producing a tire with excellent wet grip performance. [Means for solving the problem]

[0007] The present invention [1] is a rubber composition for tires, comprising a rubber component and a tackifier, wherein the tackifier is a polymer that contains structural units derived from isopropenyl toluene and is substantially free of structural units derived from a C5 fraction, the softening point of the tackifier being 85°C or higher and 150°C or lower, and the z-average molecular weight of the tackifier being less than 4,000.

[0008] The present invention [2] includes the rubber composition for tires according to the above [1], wherein the polymer contains structural units derived from indene, and the structural units derived from indene in the polymer account for 35 mol % or less. Effect of the Invention

[0009] The rubber composition for tires of the present invention contains a tackifier. The tackifier is a polymer that contains structural units derived from isopropenyl toluene and is substantially free of structural units derived from a C5 fraction. The softening point of the tackifier is 85°C or higher and 150°C or lower. The z-average molecular weight of the tackifier is less than 4000. Therefore, a tire with excellent wet grip performance can be manufactured. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a graph showing the relationship between the peak temperature shift value for a rubber composition for a tire that does not contain a tackifier and the ratio of the peak value for a rubber composition for a tire that does not contain a tackifier. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The rubber composition for a tire contains a rubber component and a tackifier.

[0012] <Rubber component> The rubber component may be, for example, a diene rubber.

[0013] Examples of diene rubbers include natural rubber (NR), styrene butadiene rubber (SBR), butadiene rubber (BR), isoprene rubber (IR), butyl rubber (IIR), acrylonitrile butadiene rubber (NBR), ethylene propylene diene rubber (EPDM), and chloroprene rubber (CR).

[0014] As the rubber component, preferably, styrene butadiene rubber (SBR) is used.

[0015] The rubber component may be used alone or in combination of two or more kinds.

[0016] The content of the rubber component per 100 parts by mass of the total of the rubber components and the tackifier is, for example, 70 parts by mass or more, preferably 80 parts by mass or more, and for example, 95 parts by mass or less, preferably 90 parts by mass or less.

[0017] <Tackifier> The tackifier is a polymer that contains structural units derived from isopropenyl toluene and is substantially free of structural units derived from a C5 fraction.

[0018] Such a polymer is obtained by polymerizing polymerization components.

[0019] The polymerization components essentially contain isopropenyl toluene.

[0020] In addition, the polymerization components are substantially free of C5 fractions.

[0021] The C5 fraction is obtained by refining and / or cracking petroleum, and generally has a boiling point range of -15°C to 45°C under normal pressure, and includes, for example, unsaturated aliphatic hydrocarbons having 5 carbon atoms and no conjugated double bonds, and unsaturated aliphatic hydrocarbons having 5 carbon atoms and containing conjugated double bonds.

[0022] Examples of unsaturated aliphatic hydrocarbons having 5 carbon atoms and containing no conjugated double bonds include 1-pentene, 2-methyl-1-butene, 3-methyl-1-butene, and 2-pentene.

[0023] Examples of unsaturated aliphatic hydrocarbons having 5 carbon atoms and containing a conjugated double bond include isoprene, 1,3-pentadiene, and cyclopentadiene.

[0024] The polymerization components may also contain other components (except isopropenyltoluene and C5 fractions), such as α-methylstyrene, indene, vinyltoluene, and unsaturated aliphatic hydrocarbons (except C5 fractions).

[0025] The unsaturated aliphatic hydrocarbons (excluding the C5 fraction) are components copolymerizable with isopropenyltoluene, α-methylstyrene, indene, and vinyltoluene, and examples thereof include the C4 fraction.

[0026] The C4 fraction is obtained by refining and / or cracking petroleum. The C4 fraction is a fraction having a boiling point range of −15° C. or more and 45° C. or less under normal pressure, and includes, for example, unsaturated aliphatic hydrocarbons having 4 carbon atoms and no conjugated double bonds, and unsaturated aliphatic hydrocarbons having 4 carbon atoms and containing conjugated double bonds.

[0027] Examples of unsaturated aliphatic hydrocarbons having 4 carbon atoms and containing no conjugated double bonds include 1-butene, isobutene, and 2-butene.

[0028] An example of an unsaturated aliphatic hydrocarbon having 4 carbon atoms and containing a conjugated double bond is 1,3-butadiene.

[0029] As the other component, preferably, indene is used, that is, preferably, as the polymer, a copolymer of isopropenyl toluene and indene is used.

[0030] The other components may be used alone or in combination of two or more kinds.

[0031] In addition, all or a part of the monomers constituting the polymerization components may be derived from fossil fuels or biomass.

[0032] Fossil fuels include petroleum, coal, natural gas, shale gas, or combinations thereof.Biomass is any renewable natural source and its residues, such as from plants or animals, including fungi, yeasts, algae, and bacteria.

[0033] The polymer is obtained by polymerizing the polymerization components in the presence of a Friedel-Crafts catalyst.

[0034] Friedel-Crafts catalysts include, for example, phenol complexes (eg, boron trifluoride phenolate complexes).

[0035] The mixing ratio of the Friedel-Crafts catalyst is, for example, 0.01 part by mass or more and, for example, 1 part by mass or less, relative to 100 parts by mass of the polymerization components.

[0036] As for the polymerization conditions, the polymerization temperature is, for example, −50° C. or higher and, for example, 50° C. or lower. The polymerization time is, for example, 10 minutes or longer and, for example, 10 hours or shorter.

[0037] The reaction is carried out in the presence of a solvent or without a solvent, and is preferably carried out in the presence of a solvent.

[0038] Examples of the solvent include aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, ketones, and alkyl esters. Examples of the solvent include aromatic hydrocarbons. Examples of the aromatic hydrocarbons include toluene and xylene. Examples of the aromatic hydrocarbons include toluene.

[0039] The solvents can be used alone or in combination of two or more kinds.

[0040] This results in a polymer (polymer solution). As such a polymer, preferably, a homopolymer of isopropenyl toluene and a copolymer of isopropenyl toluene and indene are used. As the polymer, more preferably, a copolymer of isopropenyl toluene and indene is used.

[0041] The solids concentration of the polymer solution is, for example, 5 mass % or more, preferably 10 mass % or more, and for example, 70 mass % or less, preferably 60 mass % or less.

[0042] In such a polymer, the constituent units derived from isopropenyl toluene are, for example, 65 mol% or more, preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and for example, 100 mol% or less, preferably 95 mol% or less.

[0043] In such a polymer, the content of structural units derived from other components (components other than isopropenyl toluene and C5 fraction) is, for example, 0% or more, preferably 5 mol% or more, and for example, 35 mol% or less, preferably 30 mol% or less, more preferably 20 mol% or less, and even more preferably 10 mol% or less.

[0044] In particular, when the other component is indene, the polymer contains a structural unit derived from indene. In the polymer, the structural unit derived from indene is, for example, from the viewpoint of improving wet grip performance, 35 mol % or less, preferably 30 mol % or less, more preferably 20 mol % or less, even more preferably 10 mol % or less, and for example, 1 mol % or more, preferably 5 mol % or more.

[0045] As described above, the polymer is substantially free of structural units derived from a C5 fraction. Specifically, the structural units derived from indene in the polymer are, for example, 3 mol % or less, preferably 1 mol % or less, and more preferably 0.1 mol % or less.

[0046] The ratio of the above constituent units is as follows: 13 It can be measured by C-NMR spectroscopy.

[0047] The softening point of the polymer is 85° C. or higher and 150° C. or lower, preferably 140° C. or lower, more preferably 130° C. or lower, even more preferably 110° C. or lower, and particularly preferably 90° C. or lower.

[0048] When the softening point is within the above range, the wet grip performance can be improved.

[0049] On the other hand, if the softening point is outside the above range, the wet grip performance decreases.

[0050] The softening point can be measured by the ring and ball method (in accordance with JIS K2207).

[0051] The number average molecular weight (Mn) of the polymer, as calculated using standard polystyrene by gel permeation chromatography (GPC), is, for example, 400 or more, preferably 500 or more, and, for example, 2000 or less, preferably 1200 or less, more preferably 1000 or less, even more preferably 900 or less, and particularly preferably 700 or less.

[0052] When the number average molecular weight (Mn) is within the above range, the wet grip performance can be improved.

[0053] The weight average molecular weight (Mw) of the polymer, as calculated using standard polystyrene by gel permeation chromatography (GPC), is, for example, 500 or more, preferably 800 or more, and, for example, 5000 or less, preferably 3000 or less, more preferably 2000 or less, even more preferably 1700 or less, particularly preferably 1500 or less, and most preferably 1000 or less.

[0054] When the weight average molecular weight (Mw) is within the above range, the wet grip performance can be improved.

[0055] The z-average molecular weight (Mz) of the polymer, as calculated using standard polystyrene standards by gel permeation chromatography (GPC), is less than 4,000, preferably 3,000 or less, more preferably 2,600 or less, even more preferably 2,000 or less, particularly preferably 1,500 or less, and most preferably 1,200 or less, and is, for example, 500 or more, preferably 700 or more, more preferably 1,000 or more.

[0056] When the z-average molecular weight (Mz) is within the above range, the wet grip performance can be improved.

[0057] On the other hand, if the z-average molecular weight (Mz) is equal to or greater than the upper limit, the wet grip performance decreases.

[0058] In addition, in the polymer, the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is, for example, 1.10 or more, preferably 1.30 or more, and for example, 2.00 or less, preferably 1.80 or less, more preferably 1.60 or less, and even more preferably 1.40 or less.

[0059] When the ratio is within the above range, the wet grip performance can be improved.

[0060] The tackifiers can be used alone or in combination of two or more kinds.

[0061] The content ratio of the tackifier relative to 100 parts by mass of the rubber component is, for example, 5 parts by mass or more, preferably 15 parts by mass or more, and for example, 35 parts by mass or less, preferably 25 parts by mass or less.

[0062] <Additives> The rubber composition for tires may contain additives in appropriate proportions as necessary, such as antioxidants, ultraviolet absorbers, antistatic agents, antiaging agents, pigments, fillers, antifungal agents, and processing aids.

[0063] <Preparation of Rubber Composition for Tires> The rubber composition for tires is obtained by blending and kneading a rubber component, a tackifier, and additives that are blended as required.

[0064] The rubber composition for tires can be diluted with a known solvent. When the polymerization components are polymerized in the presence of a solvent in the polymerization of the polymer, the solvent can be used as it is.

[0065] In the case where the rubber composition for tires is diluted, the solid content concentration is, for example, 5 mass % or more, preferably 10 mass % or more, and for example, 70 mass % or less, preferably 60 mass % or less.

[0066] <Action and effect> The rubber composition for tires includes a tackifier. The tackifier is a polymer that includes a structural unit derived from isopropenyl toluene and is substantially free of a structural unit derived from a C5 fraction. The softening point of the tackifier is 85°C or higher and 150°C or lower. The z-average molecular weight of the tackifier is less than 4000. Therefore, a tire with excellent wet grip performance can be manufactured.

[0067] Specifically, even if a tackifier is blended in a rubber composition for tires, if the dispersibility of the tackifier is insufficient, the wet grip performance cannot be improved.

[0068] On the other hand, this rubber composition for tires has a specified formulation, a specified softening point, and a specified z-average molecular weight, and therefore the dispersibility can be improved. As a result, the rubber mobility during dynamic deformation of the tire is hindered, and the wet grip performance can be improved from the viewpoint of increasing the energy loss.

[0069] The evaluation of the dispersibility will be described in detail in the examples described later.

[0070] According to such a rubber composition for tires, a tire having excellent wet grip performance can be produced. EXAMPLES

[0071] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples. Note that "parts" and "%" are based on mass unless otherwise specified. In addition, the specific numerical values ​​of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit value (numerical value defined as "less than or equal to" or "less than") or lower limit value (numerical value defined as "more than or equal to" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention".

[0072] <Ingredient details> Details of the abbreviations used in each Example and Comparative Example are given below. SSBR: Solution polymerization polystyrene butadiene rubber (manufactured by ENEOS Materials, product name "SL552") IPT: Isopropenyl toluene IND: Inden αMS: α-methylstyrene St: styrene C5:C5 fraction

[0073] <Production of tackifier (polymer)> Manufacturing Example 1 A mixture of polymerization components (isopropenyltoluene and indene) and dehydrated and purified toluene (polymerization components / toluene = 1 / 1 (volume ratio)) and a Friedel-Crafts catalyst (boron trifluoride phenolate complex (1.7 times phenol equivalent) diluted 10 times with dehydrated and purified toluene) were continuously fed to the first stage of a 1270 ml capacity autoclave equipped with a stirring blade, and a polymerization reaction was carried out at 5°C. The mass ratio of isopropenyltoluene to indene (isopropenyltoluene / indene) was 75 / 25, the feed rate of the mixture of polymerization components and toluene was 1.0 liter / hour, and the feed rate of the Friedel-Crafts catalyst was 90 milliliters / hour. This resulted in a reaction mixture.

[0074] The reaction mixture was then transferred to the second autoclave, and the polymerization reaction was continued at 25°C. When the total residence time in the first and second autoclaves reached 2 hours, the reaction mixture was continuously discharged from the autoclave, and when the residence time reached three times, 1 liter of the reaction mixture was sampled to terminate the polymerization reaction. After the polymerization was completed, a 1N NaOH aqueous solution was added to the sampled reaction mixture to deash the catalyst residue. Furthermore, the reaction mixture was washed five times with a large amount of water, and the solvent and unreacted polymerization components were distilled off under reduced pressure using an evaporator to obtain a polymer (tackifier) ​​that was a copolymer of isopropenyl toluene and indene.

[0075] Manufacturing Example 2 A polymer (tackifier) ​​which was a copolymer of isopropenyltoluene and indene was obtained according to the same procedure as in Production Example 1. However, the polymerization temperature was changed to 5°C, the mass ratio of isopropenyltoluene to indene (isopropenyltoluene / indene) was changed to 60 / 40, and the supply amount of the Friedel-Crafts catalyst was changed to 120 mL / hour.

[0076] Production Example 3 A polymer (tackifier) ​​which was a homopolymer of isopropenyl toluene was obtained according to the same procedure as in Production Example 1. However, the polymerization temperature was changed to 5°C, the polymerization component was changed to only isopropenyl toluene, and the supply amount of the Friedel-Crafts catalyst was changed to 82 mL / hour.

[0077] Production Example 4 A polymer (tackifier) ​​which was a copolymer of α-methylstyrene and styrene was obtained based on the same procedure as in Production Example 1. However, the polymerization temperature was changed to 25°C, the polymerization components were changed to α-methylstyrene and styrene (α-methylstyrene / styrene=60 / 40 (mass ratio)), and the supply amount of the Friedel-Crafts catalyst was changed to 75 mL / hour.

[0078] Production Example 5 A polymer (tackifier) ​​which was a copolymer of α-methylstyrene and styrene was obtained according to the same procedure as in Production Example 1. However, the polymerization temperature was changed to 5°C, the polymerization components were changed to α-methylstyrene and styrene (α-methylstyrene / styrene=60 / 40 (mass ratio)), and the supply amount of the Friedel-Crafts catalyst was changed to 56 mL / hour.

[0079] Production Example 6 A polymer (tackifier) ​​which was a homopolymer of α-methylstyrene was obtained according to the same procedure as in Production Example 1. However, the polymerization temperature was changed to 5°C, the polymerization component was changed to only α-methylstyrene, and the supply amount of the Friedel-Crafts catalyst was changed to 56 mL / hour.

[0080] Production Example 7 A polymer (tackifier) ​​which was a homopolymer of isopropenyl toluene was obtained according to the same procedure as in Production Example 1. However, the polymerization temperature was changed to 5°C, the polymerization component was changed to only isopropenyl toluene, and the supply amount of the Friedel-Crafts catalyst was changed to 85 mL / hour.

[0081] Production Example 8 A polymer (tackifier) ​​which was a homopolymer of isopropenyl toluene was obtained according to the same procedure as in Production Example 1. However, the polymerization temperature was changed to 20°C, the polymerization component was changed to only isopropenyl toluene, and the supply amount of the Friedel-Crafts catalyst was changed to 65 mL / hour.

[0082] Production Example 9 A polymer (tackifier) ​​which was a copolymer of isopropenyl toluene and a C5 fraction was obtained according to the same procedure as in Production Example 1. However, the polymerization components were changed to isopropenyl toluene and a C5 fraction, and the supply amount of the Friedel-Crafts catalyst was changed to 105 mL / hour.

[0083] <Preparation of Rubber Composition for Tires> Examples 1 to 3 and Comparative Examples 1 to 7 Based on the description in Table 2, the rubber component and the tackifier were mixed and kneaded for about 5 minutes at a temperature of 160°C and a rotor rotation speed of 40 rpm using a Labo Plastomill [Model 4C150, manufactured by Toyo Seiki Seisakusho Co., Ltd.] to prepare a rubber composition for tires.

[0084] <Evaluation> [Constituent units of each component] The structural units of each component in the polymer of each production example were determined based on the following conditions: 13 The results are shown in Table 1. {conditions} Equipment: Bruker Biospin AVANCEIII cryo-500 nuclear magnetic resonance equipment Measurement nucleus: 13C (125MHz) Measurement mode: Single pulse proton broadband decoupling Pulse width: 45° (5.00μsec) Number of points: 64k Measurement range: 250 ppm (-55 to 195 ppm) Repeat time: 5.5 seconds Number of times accumulated: 128 times Measurement solvent: orthodichlorobenzene / benzene-d6 (4 / 1 (volume ratio)) Sample concentration: 60mg / 0.6mL Measurement temperature: 120℃ Window function: exponential (BF: 1.0Hz) Chemical shift reference: δδ signal 29.73 ppm

[0085] [Softening point] The polymers of each production example were measured by the ring and ball method in accordance with JIS K2207. The results are shown in Table 1.

[0086] [Number average molecular weight (Mn), weight average molecular weight (Mw), z-average molecular weight (Mz) and Mw / Mn] For the polymers of each Production Example, the number average molecular weight (Mn), weight average molecular weight (Mw), and z-average molecular weight (Mz) in terms of standard polystyrene were measured by gel permeation chromatography (GPC) under the following measurement conditions, and Mw / Mn was calculated. The results are shown in Table 1. {Measurement conditions} Equipment: GPC HLC-8320 (Tosoh Corporation) Solvent: Tetrahydrofuran Columns: TSKgel G7000 x 1, TSKgel G4000 x 2, TSKgel G2000 x 1 (all manufactured by Tosoh Corporation) Flow rate: 1.0ml / min Sample: 20mg / mL tetrahydrofuran solution Column temperature: 40℃ Detector: Differential refractive index detector Injection volume: 50μl

[0087] [Viscoelasticity] A predetermined amount of the rubber composition for tires of each Example and Comparative Example was filled into a SUS mold, and a manual heat press (PEWR-30 manufactured by Shinto Metal Industries Co., Ltd.) with a heating plate set at 150°C was used to pressurize the composition at a gauge pressure of 9 MPa for 4 minutes, and then the composition was transferred to a cooling plate set at 20°C, compressed at a gauge pressure of 9 MPa, and cooled for 3 minutes. This produced a measurement press sheet with a length of 65 mm, a width of 65 mm, and a thickness of 2 mm. Next, the measurement press sheet was punched to a width of 3 mm to produce a test piece.

[0088] The test pieces were measured using a rheometer (DVA-225 manufactured by IT Measurement & Control Co., Ltd.) under the conditions of tension mode, frequency of 1 Hz, strain setting of 0.05%, and heating rate of 3°C / min, to determine the tan δ peak temperature, tan δ peak value, and tan δ peak value at -30°C in a temperature distribution of -100 to 200°C. The results are shown in Table 2.

[0089] Additionally, the changes in tan δ peak temperature and tan δ peak value were calculated for the Examples and Comparative Examples containing a tackifier, compared to the rubber composition for tires not containing a tackifier (hereinafter sometimes referred to as "no additive"). Specifically, the peak temperature shift value relative to the no additive (tan δ peak temperature of each Example and Comparative Example - tan δ peak temperature of Comparative Example 1) and the peak value ratio relative to the no additive (tan δ peak value of each Example and Comparative Example / tan δ peak value of Comparative Example 1) were calculated. The results are shown in Table 2.

[0090] <Consideration> FIG. 1 shows the relationship between the peak temperature shift value for no additive and the ratio of the peak value for no additive.

[0091] In Figure 1, the further to the right you go, the larger the peak temperature shift value compared to no additive. If the peak temperature shift value compared to no additive is large and the dispersibility is non-uniform, a broad tan δ peak originating from the tackifier alone will be observed at higher temperatures. Therefore, if the dispersibility is non-uniform, the peak temperature shift value according to the amount added will decrease, indicating that the tackifier has excellent dispersibility.

[0092] In addition, in Figure 1, the higher the graph, the closer the peak value ratio to the no additive sample is to 1. If the dispersibility is non-uniform, a broad tan δ peak originating from the tackifier alone is observed at higher temperatures. Therefore, the peak value ratio to the no additive sample decreases in proportion to the ratio, and when the peak value ratio to the no additive sample is closer to 1, the tackifier has excellent dispersibility.

[0093] That is, it can be seen that the dispersibility of the tackifier improves toward the upper right side in FIG. 1 (specifically, in the region shown by the hatched area in FIG. 1).

[0094] If the dispersibility of the tackifier is improved, the mobility of the rubber during dynamic deformation of the tire is hindered, which increases energy loss, and therefore wet grip performance can be improved.

[0095] 1, it can be seen that Examples 1 to 3, which use a tackifier having a predetermined formulation, a predetermined softening point, and a predetermined z-average molecular weight, are located to the upper right side of Comparative Examples 1 to 7, which do not use a predetermined tackifier. This shows that Examples 1 to 3, which use a predetermined tackifier, have improved dispersibility of the tackifier and can improve wet grip performance compared to Comparative Examples 1 to 7, which do not use a predetermined tackifier.

[0096] In addition, the 10% reduction in tires 4 (4th power of 10)~10 6 It is known that deformation in the (10^6) Hz range corresponds to deformation caused by small irregularities on the road surface. When converting temperature to viscoelasticity using the time-temperature conversion law, this frequency range is considered to be on the low-temperature side. It has also been reported in the literature that tan δ at around -30 to -15°C correlates with the friction force of tires on wet roads. Therefore, a high tan δ peak value at -30°C can improve wet grip performance.

[0097] Moreover, Examples 1 to 3, which use a predetermined tackifier, have higher tan δ peak values ​​at −30° C. than Comparative Examples 1 to 6, which do not use a predetermined tackifier. This shows that Examples 1 to 3 are superior in wet grip property to Comparative Examples 1 to 6.

[0098] [Table 1]

[0099] [Table 2]

Claims

1. Contains a rubber component and a tackifier, The tackifier is a polymer containing structural units derived from isopropenyl toluene and substantially free of structural units derived from a C5 fraction, The softening point of the tackifier is 85° C. or higher and 150° C. or lower, The tackifier has a z-average molecular weight of less than 4,000.

2. The polymer contains a structural unit derived from indene, 2. The rubber composition for a tire according to claim 1, wherein the polymer contains structural units derived from indene in an amount of 35 mol % or less.

Citation Information

Patent Citations

  • Polymer composition and its use

    JP1986266443A

  • Rubber composition and pneumatic tire using the same

    JP2010270255A

  • Rubber composition for tire tread and pneumatic tire

    JP2016113482A

  • Resin composition and molded article

    JP2018090724A

  • Rubber composition for tire and pneumatic tire

    JP2021008587A