Aggregate composition
An aggregate composition with low moisture content and a water repellent addresses the issue of fluidity loss in mortar and concrete by reducing water absorption, thereby improving their performance.
Patent Information
- Application Number
- JP2023046922
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
The absorption of mixing water by aggregates with low moisture content affects the fluidity of mortar and concrete, necessitating precise measurement of moisture content to adjust the additional water amount, which can impact compressive strength and drying shrinkage.
An aggregate composition containing aggregates with low moisture content (≤1.5%) and a water repellent, such as silicone oil, to suppress water absorption and maintain fluidity.
The composition effectively prevents a decrease in fluidity by using a water repellent, enhancing the performance of mortar and concrete.
Smart Images

Figure 2024135982000001 
Figure 2024135982000002 
Figure 2024135982000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an aggregate composition. [Background technology]
[0002] Aggregates such as sand and gravel are important materials that form the framework of mortar and concrete when mixed with hydraulic compositions such as cement. Since the quality of aggregates has a significant effect on the properties of mortar and concrete, measures may be required in the selection of aggregate types and in the mix proportions of mortar and concrete.
[0003] For example, Patent Document 1 discloses a self-leveling material with excellent surface smoothness. This document discloses that by appropriately adjusting the composition of the self-leveling material and dry-kneading the materials other than water, followed by adding water and kneading, the amount of aggregate and additive for the self-leveling material remaining in a lumpy state is reduced, improving the smoothness. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 7-223855 Summary of the Invention [Problem to be solved by the invention]
[0005] However, mixing water used in the manufacture of mortar and concrete may be absorbed by aggregate, adversely affecting fluidity. This tendency is prominent when aggregate with low moisture content is used. As a countermeasure, a method of increasing mixing water in advance, assuming the amount of water absorbed by aggregate, is known. However, since the moisture content varies depending on the storage environment of the aggregate, in order to appropriately increase the mixing water, it is necessary to accurately grasp the moisture content of the aggregate at the time of use. Therefore, there is a demand for an aggregate composition that can suppress the decrease in fluidity due to the moisture content of the aggregate, since it can omit the effort of measuring the moisture content and prevent adverse effects on the compressive strength, drying shrinkage, etc. of mortar and concrete when the mixing water is not appropriately increased.
[0006] Therefore, a main object of the present invention is to provide an aggregate composition that can suppress a decrease in fluidity due to the moisture content of the aggregate when used as a material for hydraulic compositions such as mortar and concrete. [Means for solving the problem]
[0007] As a result of intensive research to achieve the above object, the present inventors have found that it is possible to suppress a decrease in fluidity by using an aggregate composition containing aggregate and a water repellent agent.
[0008] Further investigation by the present inventors has revealed that the effect of suppressing the decrease in fluidity is high when aggregate with a low moisture content (for example, aggregate with a moisture content of 1.5% or less) is used in the aggregate composition. The present inventors speculate as follows as to the reason why the effect is high when aggregate with a low moisture content is used. It is speculated that the decrease in fluidity of mortar when aggregate with a low moisture content is used occurs because the aggregate absorbs the mixing water of the mortar (there is a difference between the water absorption rate and the moisture content). Therefore, it is believed that by using a water repellent (coating the aggregate with a water repellent), water absorption by the aggregate is suppressed, which makes it possible to suppress the decrease in fluidity.
[0009] The present invention provides aggregate compositions [1] to [4] and mortar or concrete [5]. [1] A composition comprising an aggregate and a water repellent agent; An aggregate composition for mortar or concrete. [2] The moisture content of the aggregate is 1.5% or less; The aggregate composition according to [1]. [3] The water repellent is silicone oil. The aggregate composition according to [1] or [2]. [4] The content of the water repellent is 0.005 to 0.6 parts by mass relative to 100 parts by mass of the aggregate. The aggregate composition according to any one of [1] to [3]. [5] A composition comprising a hydraulic component, the aggregate composition according to any one of [1] to [4], and water; Mortar or concrete. Effect of the Invention
[0010] According to the present invention, there is provided an aggregate composition capable of suppressing a decrease in fluidity due to the moisture content of aggregate when used as a material for a hydraulic composition. Also, according to the present invention, there is provided a mortar or concrete using such an aggregate composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, embodiments of the present invention will be described in detail, however, the present invention is not limited to the following embodiments.
[0012] In this specification, a numerical range indicated using "~" indicates a range including the numerical values before and after "~" as the minimum and maximum values, respectively. In numerical ranges described in stages in this specification, the upper limit or lower limit value described in one numerical range may be replaced with the upper limit or lower limit value of another numerical range described in stages. In numerical ranges described in this specification, the upper limit or lower limit value of the numerical range may be replaced with a value shown in the examples.
[0013] In this specification, unless otherwise specified, the materials exemplified below may be used alone or in combination of two or more within the range of the conditions. When multiple substances corresponding to each component exist, the content of each component means the total amount of the multiple substances unless otherwise specified.
[0014] [Aggregate composition] The aggregate composition of the present embodiment contains aggregate and a water repellent agent.
[0015] <Aggregate> Examples of aggregates that can be used include river sand, river gravel, mountain sand, mountain gravel, land sand, land gravel, sea sand, sea gravel, silica sand, crushed stone, crushed sand, artificial lightweight aggregate, blast furnace slag aggregate, limestone aggregate, recycled aggregate, etc., regardless of their particle size.
[0016] The moisture content of the aggregate may be, for example, 1.5% or less. By making the moisture content of the aggregate 1.5% or less, there is a tendency that the decrease in fluidity can be further suppressed. The moisture content of the aggregate may be 1.4% or less, 1.2% or less, 1.0% or less, 0.8% or less, 0.6% or less, 0.4% or less, 0.2% or less, or 0.1% or less, or may be 0.01% or more, 0.1% or more, 0.2% or more, 0.4% or more, 0.6% or more, 0.8% or more, 1.0% or more, or 1.2% or more.
[0017] In this specification, the moisture content of aggregate means a value measured in accordance with JIS A 1125: 2015, and means the amount of moisture contained in the aggregate at a certain point in time. The moisture content of aggregate varies depending on the temperature and humidity environment, and the value can be reduced, for example, by drying the aggregate.
[0018] The water absorption rate of the aggregate is not particularly limited. In one embodiment, the water absorption rate of the aggregate is 1.6% or less, and may be 1.4% or less, 1.2% or less, or 1.0% or less, and may be 0.3% or more, 0.5% or more, or 0.7% or more. In another embodiment, the water absorption rate of the aggregate is more than 1.6%, and may be 1.8% or more, 2.0% or more, or 2.1% or more, and may be 5.0% or less, 4.0% or less, or 3.0% or less.
[0019] In this specification, the water absorption rate of the aggregate means a value measured in accordance with JIS A 1109:2006, and means the limit amount of water that the aggregate can absorb.
[0020] The content of the aggregate in the total amount of the aggregate composition may be, for example, 80 mass % or more, 90 mass % or more, 95 mass % or more, 98 mass % or more, or 99 mass % or more.
[0021] <Water repellent> The water repellent means a substance that imparts water repellency to the surface of an object to which the water repellent is attached. By including the water repellent in the aggregate composition, it becomes possible to suppress water absorption by the aggregate even when an aggregate with a low moisture content is used. The water repellent may be liquid at room temperature (25°C), and is preferably liquid even at 5°C.
[0022] Examples of the water repellent include silicone oil, hydrocarbon oil (mineral oil) such as liquid paraffin, etc. The water repellent is preferably silicone oil.
[0023] The silicone oil may be straight silicone oil or modified silicone oil. Examples of straight silicone oil include dimethyl silicone oil, methylphenyl silicone oil, and methylhydrogen silicone oil. The silicone oil is preferably straight silicone oil.
[0024] The content of the water repellent may be, for example, 0.005 to 0.6 parts by mass, preferably 0.006 to 0.5 parts by mass, more preferably 0.007 to 0.4 parts by mass, and further preferably 0.010 to 0.2 parts by mass, relative to 100 parts by mass of aggregate. When the blending amount of the water repellent is 0.6 parts by mass or less relative to 100 parts by mass of aggregate, mixing during production of mortar or concrete tends to be easy.
[0025] <Other ingredients> The aggregate composition may contain other components, such as a shrinkage reducing agent.
[0026] The aggregate composition of the present embodiment can be suitably used as a material for mortar or concrete.
[0027] [Mortar or concrete] The mortar or concrete of the present embodiment contains a hydraulic component, the aggregate composition, and water. The mortar or concrete of the present embodiment may further contain inorganic powder, chemical admixtures, and the like.
[0028] <Hydraulic component> The hydraulic component may contain cement. Examples of cement include ordinary Portland cement, high-early-strength Portland cement, ultra-high-early-strength Portland cement, moderate-heat Portland cement, low-heat Portland cement, white Portland cement, blast-furnace cement, fly ash cement, silica cement, etc. The Blaine specific surface area of Portland cement is, for example, 2500 cm 2 / g or more.
[0029] In this specification, the Blaine specific surface area refers to a value measured in accordance with JIS R 5201:1997 or JIS R 2521:1995.
[0030] As cements other than these, rapid hardening cements such as crystalline and / or non-crystalline alumina cements and calcium sulfoaluminate cements may be used. For example, several types of alumina cements with different mineral compositions are known and commercially available, but the main component is monocalcium aluminate (CA), and commercially available products can be used regardless of their type. Among them, 2000 to 6000 cm 2 It is preferable to use an alumina cement having a Blaine specific surface area of 100 / g.
[0031] The hydraulic component may further include gypsum. The gypsum may be anhydrous gypsum, hemihydrate gypsum, or dihydrate gypsum. The gypsum may be a by-product in the hydrofluoric acid manufacturing process or the like, or may be naturally occurring gypsum. The Blaine specific surface area of gypsum is, for example, 2000 cm 2 / g or more.
[0032] The content of the hydraulic component in the total amount of the mortar or the total amount of the concrete may be, for example, 10 to 70 mass %, or may be 15 to 60 mass %.
[0033] <Aggregate composition> The content of the aggregate composition may be, for example, 30 to 300 parts by mass or 50 to 250 parts by mass relative to 100 parts by mass of the hydraulic component.
[0034] <Inorganic powder> Examples of inorganic powders include ground granulated blast furnace slag, fly ash, silica fume, ground calcium carbonate, ground dolomite, etc. The Blaine specific surface area of the inorganic powder is, for example, 3000 cm 2 / g or more.
[0035] The content of the inorganic powder may be, for example, 30 to 300 parts by mass or 50 to 250 parts by mass relative to 100 parts by mass of the hydraulic component.
[0036] <Chemical admixtures> Examples of chemical admixtures include water reducing agents (fluidizing agents), thickening agents, setting retarders (hardening retarders), setting accelerators (hardening accelerators), resin powders, and shrinkage reducing agents.
[0037] Examples of the water-reducing agent include commercially available water-reducing agents such as formaldehyde condensates of melamine sulfonic acid, casein, calcium caseinate, polycarboxylic acid-based, polyether-based, polyether polycarboxylic acid-based, etc. Any type of water-reducing agent can be used.
[0038] The content of the water reducing agent may be, for example, 0.01 to 2.0 parts by mass, or may be 0.05 to 1.0 part by mass, relative to 100 parts by mass of the hydraulic component.
[0039] Examples of the thickener include commercially available thickeners such as cellulose-based, protein-based, latex-based, and water-soluble polymer-based thickeners.
[0040] The content of the thickener may be, for example, 0.01 to 1.6 parts by mass, or may be 0.02 to 0.80 parts by mass, relative to 100 parts by mass of the hydraulic component.
[0041] <Water> Examples of water include tap water, distilled water, deionized water, etc. The amount of water may be, for example, 5 to 80 parts by mass, or 10 to 60 parts by mass, based on 100 parts by mass of the total amount of the components other than water in the mortar or concrete. EXAMPLES
[0042] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.
[0043] [Materials used] <Aggregate> ·No. 6 silica sand (1), water absorption rate 2.20%, coarse grain rate 1.64 ·No. 6 silica sand (2), water absorption rate 0.97%, coarse grain rate 1.31 <Water repellent> Silicone oil (H-SILOXANE, manufactured by Asahi Kasei Wacker Silicone, 100% methylhydrogenpolysiloxane content) <Hydraulic component> Portland cement (JISR5210:2019 high-early-strength Portland cement, manufactured by UBE Mitsubishi Cement, Blaine specific surface area 4250 cm 2 / g) <Chemical admixtures> Water reducing agent (polycarboxylic acid type, Kao Corporation) ·Thickener (hydroxyethyl methylcellulose, Matsumoto Yushi Pharmaceutical Co., Ltd., viscosity: 30000mPa·S)
[0044] The water absorption of the aggregate was measured in accordance with JIS A 1109:2006.
[0045] [Preparation of aggregates with different moisture contents] 5 kg of aggregate was dried for 2 days in a dryer with a tank temperature of 105±5℃ to prepare aggregate with low moisture content. After spraying water on the dried aggregate and mixing well, it was placed in a plastic bag, sealed, and stored in a temperature-controlled room at 20℃ and 65% RH for 24 hours to prepare aggregates with different moisture contents. The moisture content of the aggregate was measured in accordance with JIS A 1125:2015. The moisture content of each aggregate is shown in Table 1.
[0046] [Table 1]
[0047] [Preparation of aggregate composition] The materials shown in Table 2 were mixed for 3 minutes in the amounts (unit: parts by mass) shown in Table 2 using an Eirich mixer to obtain aggregate compositions A to F of Examples 1-1 to 1-6.
[0048] [Table 2]
[0049] [Preparation of premix mortar] The materials shown in Table 3 were mixed for 3 minutes using an Eirich mixer in the amounts (unit: parts by mass) shown in Table 3 to obtain premix mortars for Reference Examples 2-1 and 2-2, Examples 2-1 to 2-5, and Comparative Examples 2-1 to 2-5.
[0050] [Table 3]
[0051] [Preparation of mortar slurry] 390 g of water was added to 1.5 kg of each premix mortar, and the mixture was kneaded for 3 minutes using a chemical stirrer to obtain mortar slurries of Reference Examples 2-1 and 2-2, Examples 2-1 to 2-5, and Comparative Examples 2-1 to 2-5.
[0052] [Flow value measurement] To evaluate the fluidity, measurements were taken in accordance with JASS 15M-103 "Quality Standards for Self-Leveling Materials by the Architectural Institute of Japan." Measurements were taken in an environment of 20°C and 65% RH. The flow value measurements are shown in Table 4.
[0053] [Table 4]
[0054] As shown in Table 4, the mortar slurry using the aggregate composition containing aggregate and a water repellent agent had a sufficient flow value compared to the mortar slurry not using the aggregate composition.
[0055] In addition, in the mortar slurries using aggregates with high moisture content (moisture content: over 1.5%), the flow values of Reference Example 2-1 and Reference Example 2-2 were all 190 or more, with no significant difference, and therefore no effect of suppressing a decrease in fluidity due to the use of a water repellent was observed. In contrast, in the mortar slurries using aggregates with low moisture content (moisture content: 1.5% or less), the flow values of Examples 2-1 to 2-5 were all 190 or more, and the flow values of Comparative Examples 2-1 to 2-5 were all less than 190, so the effect of suppressing a decrease in fluidity due to the use of a water repellent was high. From these results, it was found that the effect of suppressing a decrease in fluidity was higher as the moisture content of the aggregate in the aggregate composition was lower.
[0056] From these results, it was confirmed that the aggregate composition of the present invention, when used as a material for a hydraulic composition, is capable of suppressing a decrease in fluidity due to the moisture content of the aggregate.
Claims
1. Aggregate and a water repellent agent, An aggregate composition for mortar or concrete.
2. The moisture content of the aggregate is 1.5% or less. The aggregate composition of claim 1.
3. The water repellent is silicone oil. The aggregate composition of claim 1.
4. The content of the water repellent is 0.005 to 0.6 parts by mass relative to 100 parts by mass of the aggregate. The aggregate composition of claim 1.
5. A composition comprising a hydraulic component, the aggregate composition according to any one of claims 1 to 4, and water. Mortar or concrete.
Citation Information
Patent Citations
aggregate
JP1985260448A
High fluidity concrete and its production
JP1998101396A
Method for producing lightweight concrete
JP2020200196A
Self leveling material and method for producing the same
JP2021155314A
Water-repellent-sand mixture and water-repellent-sand structure
WO2014045583A1