Piezoelectric device, sensor, actuator, and biological information acquisition device

The piezoelectric device with a protective member and oriented optically active polypeptides maintains sensitivity by preventing water vapor contact, addressing the sensitivity loss issue in fibrous polypeptides.

JP2024136264APending Publication Date: 2024-10-04MITSUI CHEMICALS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023047336
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Fibrous optically active polypeptides used in piezoelectric devices easily absorb water, leading to a decrease in piezoelectric sensitivity over time.

Method used

A piezoelectric device comprising a piezoelectric base material covered by a protective member with specific water vapor permeability and a piezoelectric body made of optically active polypeptides, where the orientation degree is 0.50 or more and less than 1.00, and the protective member includes materials like inorganic oxides or diamond-like carbon to prevent water vapor contact.

Benefits of technology

Maintains good piezoelectric sensitivity by effectively suppressing contact between the piezoelectric body and water vapor, ensuring stable performance over time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136264000001_ABST
    Figure 2024136264000001_ABST
Patent Text Reader

Abstract

To provide a piezoelectric device, a sensor, an actuator, and a biological information acquisition device, in which superior piezoelectric sensitivity can be maintained.SOLUTION: A piezoelectric device includes a piezoelectric substrate and a protective member covering an outer periphery of the piezoelectric substrate. The piezoelectric substrate includes an elongated inner conductor, and a piezoelectric body covering an outer peripheral surface of the inner conductor. The piezoelectric body includes fibers comprising an optically active polypeptide. The lengthwise direction of the piezoelectric body is approximately parallel to the main orientation direction of the optically active polypeptide. The degree of orientation F of fibers comprising the optically active polypeptide obtained by the following expression (a) from an X-ray diffraction measurement is 0.50 or more and less than 1.00. The steam permeability at a portion corresponding to 85% or more of a surface area of the protective member is 0.5 g / m2 / day or less. In the expression (a), α represents a half value width (°) of a peak derived from orientation. Degree of orientation F=(180°-α) / 180°...Expression (a)SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a piezoelectric device, a sensor, an actuator, and a bioinformation acquisition device. [Background technology]

[0002] In recent years, applications of piezoelectric materials containing optically active polypeptides (hereinafter referred to as "optically active polypeptides") to piezoelectric devices such as sensors and actuators have been considered. In addition, the use of fibrous optically active polypeptides such as silk as optically active polypeptides has been considered. For example, Patent Document 1 describes a piezoelectric substrate that uses silk, a fibrous optically active polypeptide, as a piezoelectric material. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2018 / 092886 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0004] The fibrous optically active polypeptide used as the piezoelectric body in the piezoelectric substrate described in Patent Document 1 is prone to absorbing moisture, and therefore the piezoelectric sensitivity may decrease over time. Therefore, it is believed that the decrease in piezoelectric sensitivity can be suppressed by suppressing contact between the piezoelectric body and water vapor in the air.

[0005] In view of the above circumstances, an object of an embodiment of the present disclosure is to provide a piezoelectric device, a sensor, an actuator, and a bioinformation acquisition device that maintain good piezoelectric sensitivity. [Means for solving the problem]

[0006] Means for solving the above problems include the following embodiments. <1> A piezoelectric device comprising a piezoelectric substrate and a protective member covering an outer periphery of the piezoelectric substrate, The piezoelectric substrate has an elongated internal conductor and a piezoelectric body covering an outer circumferential surface of the internal conductor; The piezoelectric body includes fibers made of an optically active polypeptide, the length direction of the piezoelectric body is approximately parallel to the main orientation direction of the optically active polypeptide; The degree of orientation F of the fiber made of the optically active polypeptide, which is calculated by the following formula (a) from X-ray diffraction measurement, is 0.50 or more and less than 1.00, The water vapor permeability of a portion corresponding to 85% or more of the surface area of ​​the protective member is 0.5 g / m 2 / day or less piezoelectric device. Orientation degree F=(180°-α) / 180° … Formula (a) [In formula (a), α represents the half-width (°) of the peak due to the orientation.] <2> A portion of the piezoelectric substrate that corresponds to 85% or more of the surface area of ​​the piezoelectric substrate has a water vapor permeability of 0.5 g / m 2 / day or less covered with material, <1> The piezoelectric device according to claim 1 . <3> The protective member includes a layer that exhibits a barrier property against water vapor. <1> or <2> The piezoelectric device according to claim 1 . <4> The layer contains at least one selected from the group consisting of inorganic oxides, inorganic nitrides, inorganic fluorides, and diamond-like carbon. <3> The piezoelectric device according to claim 1 . <5> The protective member includes a metal. <1> ~ <4> 13. The piezoelectric device according to claim 12 . <6> a wiring member electrically connected to the internal conductor of the piezoelectric substrate, the protective member covers the entire piezoelectric substrate and at least a part of the outer periphery of the wiring member; <1> ~ <5> 13. The piezoelectric device according to claim 12 . <7> The protective member is either a tube-shaped member having its ends bonded together or a pair of sheet-shaped members bonded together. <1> ~ <6> 13. The piezoelectric device according to claim 12 . <8> The optically active polypeptide has a β-sheet structure. <1> ~ <7> 13. The piezoelectric device according to claim 12 . <9> The optically active polypeptide comprises fibroin; <1> ~ <8> 13. The piezoelectric device according to claim 12 . <10> <1> ~ <9> A sensor comprising the piezoelectric device according to any one of claims 1 to 5. <11> <1> ~ <9> An actuator comprising the piezoelectric device according to any one of claims 1 to 5. <12> <1> ~ <9> A bioinformation acquisition device comprising the piezoelectric device according to any one of claims 1 to 5.

[0007] According to the present disclosure, there are provided a piezoelectric device, a sensor, an actuator, and a biometric information acquisition device that maintain good piezoelectric sensitivity. [Brief description of the drawings]

[0008] [Figure 1A] FIG. 2 is a schematic side view illustrating the appearance of a piezoelectric substrate according to an embodiment of the present disclosure. [Figure 1B] FIG. 1B is a cross-sectional view taken along line IB-IB of FIG. [Diagram 2] FIG. 2 is a schematic side view illustrating the appearance of a piezoelectric substrate according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] In the present disclosure, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0010] <Piezoelectric device> A piezoelectric device according to the present disclosure includes a piezoelectric substrate and a protective member that covers an outer periphery of the piezoelectric substrate, The piezoelectric substrate has an elongated internal conductor and a piezoelectric body covering an outer circumferential surface of the internal conductor; The piezoelectric body includes fibers made of an optically active polypeptide, the length direction of the piezoelectric body is approximately parallel to the main orientation direction of the optically active polypeptide; The degree of orientation F of the fiber made of the optically active polypeptide, which is calculated by the following formula (a) from X-ray diffraction measurement, is 0.50 or more and less than 1.00, The water vapor permeability of a portion corresponding to 85% or more of the surface area of ​​the protective member is 0.5 g / m 2 / day or less. Orientation degree F=(180°-α) / 180° … Formula (a) [In formula (a), α represents the half-width (°) of the peak due to the orientation.]

[0011] In the piezoelectric device of the present disclosure, the outer periphery of the piezoelectric substrate is covered with a protective member that satisfies certain conditions. This effectively prevents the optically active polypeptide used as the piezoelectric body from coming into contact with water vapor in the air. As a result, it is believed that the good piezoelectric sensitivity of the piezoelectric substrate is maintained.

[0012] In the present disclosure, an "optically active polypeptide" refers to a polypeptide that has an asymmetric carbon atom and has a bias in the abundance of optical isomers. In the present disclosure, "substantially parallel" means that, when the angle between two line segments is expressed in the range of 0° to 90°, the angle between the two line segments is 0° or more and less than 30° (preferably 0° or more and 22.5° or less, more preferably 0° or more and 10° or less, even more preferably 0° or more and 5° or less, and particularly preferably 0° or more and 3° or less). In the present disclosure, the degree of orientation F of a piezoelectric body is an index showing the degree of orientation of an optically active polypeptide contained in the piezoelectric body.

[0013] (Piezoelectric substrate) The piezoelectric substrate included in the piezoelectric device includes a long internal conductor and a piezoelectric body covering the outer peripheral surface of the internal conductor. The shape of the piezoelectric substrate is not particularly limited, and may be, for example, in the form of a cord or ribbon.

[0014] The manner in which the piezoelectric body covers the outer circumferential surface of the internal conductor is not particularly limited. For example, a long piezoelectric body may be wound around the internal conductor. The shape of the long piezoelectric body is not particularly limited, and may be a thread, cord, ribbon, or other shape.

[0015] The method of winding the piezoelectric body around the internal conductor is not particularly limited. For example, the piezoelectric body may be wound spirally around the axial direction of the internal conductor, or may not be wound spirally around the axial direction of the internal conductor. From the viewpoint of improving the piezoelectric sensitivity of the piezoelectric substrate, it is preferable that the piezoelectric body is wound spirally around the axial direction of the internal conductor. The piezoelectric body may be wound so as to overlap, or may be wound so as not to overlap. From the viewpoint of piezoelectric sensitivity, it is preferable that the piezoelectric body covers the entire outer circumferential surface of the internal conductor. The piezoelectric body may be wound directly around the outer circumferential surface of the internal conductor, or may be wound indirectly (for example, with an electrical insulator or the like disposed between the internal conductor and the piezoelectric body).

[0016] In the piezoelectric substrate, when a shear stress is applied to the helically wound piezoelectric body, electric charges are easily generated, which makes it easy for the piezoelectricity to be expressed. The shear stress can be applied to the piezoelectric body by deforming the piezoelectric body. For example, the shear stress can be applied to the piezoelectric body by a first non-plastic deformation, a second non-plastic deformation, a third non-plastic deformation, or the like. The first non-plastic deformation refers to the entire helically wound piezoelectric body being stretched in the direction of the helical axis. The second non-plastic deformation refers to twisting a part of the helically wound piezoelectric body (i.e., twisting a part of the piezoelectric yarn around the helical axis). The third non-plastic deformation refers to bending a part or the whole of the helically wound piezoelectric body.

[0017] The piezoelectric body is preferably wound spirally in one direction around the internal conductor. "Spiral wound in one direction" refers to a first winding manner or a second winding manner. The first winding mode indicates that the piezoelectric yarn is wound spirally around the internal conductor so as to be left-handed (i.e., counterclockwise) from the front side to the back side when viewed from one end of the piezoelectric substrate. The second winding manner indicates that the piezoelectric body is wound in a spiral shape around the internal conductor so as to be right-handed (ie, clockwise) from the front side to the back side when viewed from one end of the piezoelectric substrate. When the piezoelectric body is wound in a spiral shape in one direction, the phenomenon in which the polarities of the generated charges cancel each other out (i.e., the phenomenon in which the piezoelectricity decreases) is suppressed, and therefore the piezoelectricity of the piezoelectric substrate is further improved.

[0018] The embodiment having a piezoelectric body in which the piezoelectric substrate is spirally wound in one direction includes not only an embodiment having only one layer made of a piezoelectric body, but also an embodiment in which multiple layers made of a piezoelectric body are stacked. An example of an embodiment in which multiple layers made of piezoelectric material are stacked on top of each other is an embodiment in which a first layer made of piezoelectric material is spirally wound in one direction, and a second layer made of piezoelectric material is stacked on top of the first layer made of piezoelectric material and spirally wound in the same direction as the first direction. An embodiment of the piezoelectric substrate may include a first layer in which a piezoelectric body is spirally wound in one direction, and a second layer in which a piezoelectric body is spirally wound in a direction different from that of the piezoelectric body in the first layer. In this embodiment, the chirality of the optically active polypeptide contained in the first layer is different from the chirality of the optically active polypeptide contained in the second layer.

[0019] When the piezoelectric body is wound helically around the internal conductor, the helix angle of the piezoelectric body is preferably 20° to 70°, more preferably 25° to 65°, and even more preferably 30° to 60°. In this disclosure, the "helical angle" refers to the angle between the axial direction of the internal conductor and the longitudinal direction of the piezoelectric body. The helical angle is measured by photographing the appearance of the piezoelectric substrate with the piezoelectric body wound helically around the internal conductor (with the external conductor removed, if the piezoelectric substrate has an external conductor, as described below) using an optical microscope. The angles are measured by image processing at five points on the observed piezoelectric substrate, excluding the portion where the angle of the piezoelectric body is extremely misaligned, and the average of the measured values ​​is taken as the helical angle of the piezoelectric body.

[0020] The thickness of the piezoelectric body is not particularly limited, but is preferably 0.02 mm or more and 2.00 mm or less, and more preferably 0.05 mm or more and 1.00 mm or less.

[0021] The piezoelectric body includes fibers made of an optically active polypeptide. Hereinafter, the fibers made of an optically active polypeptide are also referred to as "optically active polypeptide fibers." When the piezoelectric material contains optically active polypeptide fibers, the piezoelectric substrate exhibits piezoelectricity.

[0022] The optically active polypeptide fiber may be contained in a filamentous piezoelectric material. Hereinafter, the filamentous piezoelectric material will also be referred to as "piezoelectric yarn." The piezoelectric yarn may be a twisted yarn or a non-twisted yarn. In particular, the piezoelectric yarn is preferably a twisted yarn from the viewpoint of piezoelectricity. Examples of the non-twisted yarn include a single original yarn (fiber) and an aggregate of multiple original yarns (fibers). The number of original yarns (fibers) constituting the twisted yarn is not particularly limited, and is preferably 3 to 120, and more preferably 4 to 30, from the viewpoint of ensuring the strength of the piezoelectric yarn. The fibers contained in the piezoelectric yarn may be only optically active polypeptide fibers, or a combination of optically active polypeptide fibers and fibers that are not optically active polypeptides. From the viewpoint of improving the piezoelectric sensitivity of the piezoelectric substrate, it is preferable that the fibers contained in the piezoelectric yarn are only optically active polypeptide fibers.

[0023] The twist number of the piezoelectric yarn is preferably 500 T / m or less, more preferably 300 T / m or less. When the twist number of the piezoelectric yarn is within this range, the piezoelectric yarn is less likely to break, and the piezoelectric sensitivity of the piezoelectric substrate is superior.

[0024] The thickness of the piezoelectric yarn (when the piezoelectric yarn is an assembly of multiple fibers, the thickness of the entire assembly) is not particularly limited, and is preferably 0.0001 mm to 2 mm, more preferably 0.001 mm to 1 mm, and even more preferably 0.005 mm to 0.8 mm. When the piezoelectric yarn is a single original yarn or an assembly of multiple original yarns, the fineness of each original yarn is preferably 0.01 denier to 10,000 denier, more preferably 0.1 denier to 1,000 denier, and even more preferably 1 denier to 100 denier.

[0025] The piezoelectric yarn may be in the form of an aggregate of a plurality of piezoelectric yarns. The aggregate of a plurality of piezoelectric yarns may be in the form of a cord, a ribbon, etc. The aggregate of a plurality of piezoelectric yarns may be in the form of a bond between the piezoelectric yarns by a resin or the like.

[0026] The optically active polypeptide fiber is preferably a long fiber, in which case the shear stress applied to the piezoelectric substrate is easily transmitted to the piezoelectric substrate, resulting in excellent piezoelectric sensitivity. In the present disclosure, the term "long fiber" refers to a fiber having a length that allows it to be wound continuously from one end to the other end in the longitudinal direction of a piezoelectric substrate. Examples of long fiber optically active polypeptide fibers include silk, wool, mohair, cashmere, camel, llama, alpaca, vicuna, angora, and spider silk. Among these, silk and spider silk are preferred from the viewpoint of piezoelectricity.

[0027] In the present disclosure, the degree of orientation F of the optically active polypeptide fiber is within the range of 0.50 or more and less than 1.00. When the degree of orientation F of the optically active polypeptide fiber is 0.50 or more, the piezoelectric property of the piezoelectric substrate is good.When the degree of orientation F of the optically active polypeptide fiber is less than 1.00, the productivity of the piezoelectric substrate is good. The degree of orientation F of the optically active polypeptide fiber is preferably 0.50 or more and 0.99 or less, more preferably 0.70 or more and 0.98 or less, and even more preferably 0.80 or more and 0.97 or less. An orientation degree F of an optically active polypeptide fiber of 1.00 indicates that the main orientation direction of the optically active polypeptide contained in the optically active polypeptide fiber is parallel to the length direction of the optically active polypeptide fiber. Furthermore, an orientation degree F of an optically active polypeptide fiber of 0.80 or more and less than 1.00 indicates that the main orientation direction of the optically active polypeptide contained in the optically active polypeptide fiber is approximately parallel to the length direction of the optically active polypeptide fiber. The degree of orientation F of an optically active polypeptide fiber is determined by fixing a sample (piezoelectric body) to a sample holder, measuring the azimuth angle distribution intensity near the peak due to orientation (for example, near 2θ=20° in the case of silk) from X-ray diffraction measurement, and calculating using the following formula (a), and means the degree of c-axis orientation. Orientation degree F=(180°-α) / 180° … Formula (a) [In formula (a), α represents the half-width (°) of the peak due to the orientation.]

[0028] In the present disclosure, it is preferable that the length direction of the piezoelectric body and the main orientation direction of the optically active polypeptide contained in the piezoelectric body are approximately parallel. When the length direction of the piezoelectric body is approximately parallel to the main orientation direction of the optically active polypeptide contained in the piezoelectric body, the piezoelectric properties of the piezoelectric substrate are well expressed. Furthermore, since the length direction of the piezoelectric body and the main orientation direction of the optically active polypeptide contained in the piezoelectric body are approximately parallel, the piezoelectric body has excellent tensile strength in the length direction and is less likely to break. When the piezoelectric body is in the form of a piezoelectric thread containing optically active polypeptide fibers (e.g., silk or spider silk), during the process of production of the silk or spider silk, the length direction of the piezoelectric body becomes approximately parallel to the main orientation direction of the optically active polypeptide (e.g., fibroin or spider silk protein) contained in the piezoelectric body. The fact that the length direction of the piezoelectric body and the main orientation direction of the optically active polypeptide contained in the piezoelectric body are approximately parallel can be confirmed by comparing the installation direction of the sample (piezoelectric body) and the azimuth angle of the crystal peak in X-ray diffraction measurement. An example of a method for making the length direction of a piezoelectric body approximately parallel to the main orientation direction of an optically active polypeptide contained in the piezoelectric body is to form a piezoelectric body using optically active polypeptide fibers having an orientation degree F of 0.80 or more and less than 1.00. Specifically, a method for using a twisted yarn made from optically active polypeptide fibers having an orientation degree F of 0.80 or more and less than 1.00 as the piezoelectric body is exemplified.

[0029] From the viewpoints of the piezoelectricity and strength of the piezoelectric body, the optically active polypeptide fiber is preferably made of an optically active polypeptide having a β-sheet structure.

[0030] Examples of optically active polypeptides having a β-sheet structure include optically active animal proteins and optically active synthetic proteins. Examples of optically active animal proteins include fibroin, spider silk protein, sericin, collagen, keratin, elastin, etc. As the spider silk protein, the spider silk protein described in Patent Document 1 can be used. As the spider silk protein, artificial spider silk obtained by an artificial synthesis method can be used. In particular, the optically active polypeptide preferably contains at least one of fibroin and spider silk protein, and more preferably contains fibroin. Examples of synthetic proteins having optical activity include synthetic spider silk (e.g., "QMONOS (registered trademark)", synthetic bagworm silk, synthetic proteins (e.g., "Brewed Protein (registered trademark)", etc.). The form of the synthetic protein having optical activity is preferably thread-like. Thread-like fibers containing the above synthetic proteins can also be obtained from threads or clothing containing "Brewed Protein (registered trademark)".

[0031] Examples of fibers made of optically active polypeptides having a β-sheet structure include fibers made of optically active animal proteins, such as silk, wool, mohair, cashmere, camel, llama, alpaca, vicuna, angora, and spider silk. Among these, from the viewpoint of piezoelectricity, the optically active polypeptide fiber preferably contains at least one of silk and spider silk, more preferably consists of at least one of silk and spider silk, and particularly preferably consists of silk.

[0032] Examples of silk include raw silk, refined silk, regenerated silk, and fluorescent silk. As the silk, raw silk or refined silk is preferred, and refined silk is particularly preferred. "Refined silk" refers to silk that has had sericin removed from raw silk, which has a double structure of sericin and fibroin. "Refining" refers to the process of removing sericin from raw silk. Raw silk is a dull white color, but by removing sericin from raw silk (i.e., refining), the color changes from dull white to a lustrous silvery white. Refining also enhances the silk's soft texture.

[0033] When covering the outer periphery of the internal conductor with the piezoelectric body, an adhesive may be used. By using an adhesive, the state in which the piezoelectric body covers the outer periphery of the internal conductor is maintained favorably. As a result, when external stress is applied to the piezoelectric substrate, shear stress caused by the external stress is more likely to act on the piezoelectric yarn.

[0034] Specific examples of adhesives include epoxy-based adhesives, urethane-based adhesives, vinyl acetate resin-based emulsion-type adhesives, ethylene vinyl acetate-based emulsion-type adhesives, acrylic resin-based emulsion-type adhesives, styrene butadiene rubber-based latex-type adhesives, silicone resin-based adhesives, α-olefin-based adhesives, vinyl chloride resin-based solvent-type adhesives, rubber-based adhesives, elastic adhesives, chloroprene rubber-based solvent-type adhesives, nitrile rubber-based solvent-type adhesives, and cyanoacrylate-based adhesives.

[0035] (inner conductor) The piezoelectric substrate includes an elongated inner conductor. The inner conductor functions as the core of the piezoelectric substrate. The internal conductor is preferably a good electrical conductor, such as copper wire, aluminum wire, SUS (Steel Use Stainless) wire, metal wire coated with an insulating film, carbon fiber, resin fiber integrated with carbon fiber, tinsel wire, organic conductive material, etc. The tinsel wire is formed by spirally winding copper foil around a fiber. The outer diameter of the fiber is appropriately adjusted according to the desired characteristics of the piezoelectric substrate, and is preferably 0.1 mm or more and 10 mm or less. Among these, the internal conductor is preferably made of tinsel wire or carbon fiber from the viewpoints of improving the piezoelectric sensitivity and stability of the piezoelectric output and imparting high flexibility, and in particular, tinsel wire is preferable from the viewpoint of low electrical resistance.

[0036] (Outer conductor) From the viewpoint of improving piezoelectric sensitivity and electrostatic shielding properties, it is preferable that the piezoelectric substrate further includes an external conductor. The outer conductor is disposed on the outer periphery of the piezoelectric body, and the inner conductor and the outer conductor are not electrically connected to each other.

[0037] The outer conductor serves as a companion conductor to the inner conductor, for example, to detect electrical signals from the piezoelectric substrate. The external conductor may be disposed on a portion of the outer circumferential surface of the piezoelectric layer, or may be disposed on the entire outer circumferential surface of the piezoelectric layer.

[0038] The outer conductor may or may not be fixed to the piezoelectric body.

[0039] The external conductor is formed, for example, by winding a long conductor around the outer periphery of the piezoelectric body. The cross-sectional shape of the long-sized conductor may be, for example, a circular shape, an elliptical shape, a rectangular shape, an irregular shape, etc. Among these, from the viewpoint of closely adhering to the piezoelectric substrate in a plane and improving the piezoelectric sensitivity of the piezoelectric substrate, the cross-sectional shape of the long-sized conductor is preferably a rectangular shape. The material of the long conductor is not particularly limited, and the following are main examples depending on the cross-sectional shape: Examples of long conductors having a rectangular cross section include copper foil ribbons and aluminum foil ribbons which are formed by rolling copper wires having a circular cross section into a flat plate. Examples of long conductors having a circular cross section include copper wire, aluminum wire, SUS wire, metal wire coated with an insulating film, carbon fiber, resin fiber integrated with carbon fiber, and tinsel wire in which copper foil is spirally wound around fiber. The long conductor may be an organic conductive material coated with an insulating material. Methods for winding a long conductor include, for example, a method of spirally winding copper foil or the like around a piezoelectric substrate, a method of braiding copper wire or the like into a tubular shape and wrapping the piezoelectric substrate, and a method of enclosing the piezoelectric substrate in a cylindrical shape.

[0040] (Electrical insulator) The piezoelectric substrate may further include an outer electrical insulator (hereinafter referred to as a "first insulator"). The first insulator is disposed on the outermost periphery of the piezoelectric substrate. In other words, at least a portion of the outer periphery of the piezoelectric substrate may be formed by the first insulator. It is preferable that the first insulator covers the entire outermost periphery of the piezoelectric substrate. In other words, it is preferable that the entire outer periphery of the piezoelectric substrate is composed of the first insulator. This makes it possible to electrostatically shield the internal conductor. As a result, it is possible to suppress changes in piezoelectric sensitivity caused by external static electricity. The first insulator is formed, for example, by winding a long insulator in a spiral shape around the outer circumferential surface of the outer conductor, or by extrusion molding using a molten insulator. Examples of materials for the first insulator include electrically insulating materials such as polyvinyl chloride resin, polyethylene resin, polypropylene resin, ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene resin (PTFE), tetrafluoroethylene-perfluoropropyl vinyl ether copolymer (PFA), fluororubber, polyester resin, polyimide resin, polyamide resin, polyethylene terephthalate resin (PET), and rubber (including elastomer).

[0041] When the piezoelectric substrate includes an external conductor, it may further include an inner electrical insulator (hereinafter referred to as a "second insulator"), for example, disposed between the piezoelectric body and the internal conductor and / or between the piezoelectric body and the external conductor. This can further prevent short circuits from occurring between the internal conductor and the external conductor, or between the piezoelectric body and the external conductor. The second insulator is formed, for example, by winding a long insulator in a spiral shape around the outer circumferential surface of the outer conductor, or by extrusion molding using a molten insulator. Examples of materials for the second insulator include the same materials as those exemplified as the materials for the first insulator.

[0042] (Functional layer) The piezoelectric substrate may further include a functional layer, such as an easy-adhesion layer, a hard coat layer, a refractive index adjustment layer, an antireflection layer, an antiglare layer, an easy-slip layer, an antiblock layer, a protective layer, an antistatic layer, a heat dissipation layer, an ultraviolet absorbing layer, an anti-Newton ring layer, a light scattering layer, a polarizing layer, a gas barrier layer, a hue adjustment layer, an electrode layer, and the like. The piezoelectric substrate may include only one type of functional layer, or two or more types of functional layers. The material of the functional layer is appropriately selected depending on the function required for the functional layer, and examples thereof include inorganic substances such as metals and metal oxides, organic substances such as resins, composite compositions containing resins and fine particles, etc. Examples of the resin include cured products obtained by curing with temperature or active energy rays.

[0043] (Protective material) The piezoelectric device of the present disclosure includes a protective member that covers the outer periphery of the piezoelectric substrate, and the water vapor permeability of a portion of the protective member that corresponds to 85% or more of the surface area is 0.5 g / m 2 / day or less. The following protective materials have a surface area with a water vapor permeability of 0.5 g / m 2 The percentage of the area that is less than / day is also called the "barrier area ratio."

[0044] In the present disclosure, the water vapor transmission rate of the protective member is a value measured by the Mocon method.

[0045] The outer periphery of the piezoelectric substrate is covered with a protective material, and a portion of the protective material equivalent to 85% or more of its surface area has a water vapor permeability of 0.5 g / m 2 / day or less (that is, the barrier area ratio of the protective member is 85% or more), sufficient airtightness is ensured around the piezoelectric substrate, and contact between the piezoelectric body and water vapor can be effectively suppressed.

[0046] From the viewpoint of ensuring airtightness around the piezoelectric substrate, the water vapor permeability of the part corresponding to 90% or more of the surface area of ​​the protective member is set to 0.5 g / m 2 / day or less, and the water vapor transmission rate of the portion corresponding to 95% or more of the surface area of ​​the protective member is 0.5 g / m 2 / day or less is more preferable.

[0047] From the viewpoint of ensuring airtightness around the piezoelectric substrate, the water vapor transmission rate of the part corresponding to 85% or more of the surface area of ​​the protective member is set to 0.1 g / m 2 / day or less, and the water vapor transmission rate of the portion corresponding to 85% or more of the surface area of ​​the protective member is 0.02 g / m 2 / day or less is more preferable.

[0048] The water vapor transmission rate of 85% or more of the surface area is 0.5g / m 2 The specific form of the protective member having a surface roughness of 1 / day or less is not particularly limited. In one embodiment, the protective member has a water vapor transmission rate of 0.5 g / m 2 / day or less. In other words, a portion corresponding to 85% or more of the surface area of ​​the protective member may include a layer having a water vapor transmission rate of 0.5 g / m 2 / day or less.

[0049] The material of the protective member is not particularly limited as long as it satisfies the predetermined water vapor transmission rate requirements. For example, the protective member may contain a metal. Examples of metals include aluminum, gold, silver, platinum, palladium, tin, nickel, zinc, magnesium, iron, copper, chromium, cobalt, titanium, indium, germanium, and tantalum, as well as alloys containing the above metals. When the protective member contains a metal, the protective member may contain the metal entirely or may contain only a part of the metal (e.g., the protective member may have a metal layer).

[0050] The protective member may include a layer (hereinafter also referred to as a barrier layer) that exhibits barrier properties against gas molecules such as water vapor and oxygen. The type of the barrier layer is not particularly limited, and examples thereof include a metal foil such as an aluminum foil, a thin film layer, an organic barrier layer, and an organic-inorganic hybrid barrier layer. Examples of the thin film layer include a vapor-deposited metal thin film layer containing the above-mentioned metal or alloy, and a thin film layer containing at least one selected from the group consisting of an inorganic oxide, an inorganic nitride, an inorganic fluoride, and diamond-like carbon (DLC). Examples of inorganic oxides include silicon oxide, aluminum oxide, indium oxide, titanium oxide, lead oxide, tin oxide, indium oxide, rubidium oxide, zinc oxide, iron oxide, magnesium oxide, tantalum oxide, cerium oxide, silicon aluminum oxide, and silicon magnesium oxide. Examples of inorganic nitrides include aluminum nitride, boron nitride, and silicon nitride. Examples of inorganic fluorides include calcium fluoride and magnesium fluoride. The organic barrier layer may include an organic barrier layer comprising a vinylidene chloride based resin, a modified emulsifier, an ethylene vinyl alcohol copolymer, MXD nylon, or a combination thereof.

[0051] A commercially available film may be used as the protective member having a thin film layer. Commercially available films having a thin film layer include brands such as "IB Series" manufactured by Dai Nippon Printing Co., Ltd., "GL, GX Series" manufactured by Toppan Printing Co., Ltd., "Barrierox", VM-PET, BR-PET, VM-CPP, VM-OPP manufactured by Toray Advanced Film Co., Ltd., "Tech Barrier" manufactured by Mitsubishi Plastics, Inc., "ML, V Barrier, Max Barrier" manufactured by Tocello Co., Ltd., and "MOS", "Tetlite", and "Be-Bright" manufactured by Oike Kogyo Co., Ltd., all of which have a water vapor transmission rate of 0.5 g / m. 2 / day or less.

[0052] A commercially available film may be used as the protective member having an organic barrier layer or an organic-inorganic hybrid barrier layer. Examples of commercially available films having an organic barrier layer include "Kuralysta" and "Eval" manufactured by Kuraray Co., Ltd., "Cobarrier" manufactured by Kohjin Co., Ltd., and "Seneci" manufactured by Daicel Corporation.

[0053] From the viewpoint of airtightness of the protective member, the barrier layer is preferably a metal foil, a vapor-deposited metal-based thin film layer, or an organic-inorganic hybrid barrier layer. From the viewpoint of economy, the barrier layer is preferably an aluminum foil or an aluminum vapor-deposited layer. From the viewpoint of being able to grasp the state of the internal piezoelectric substrate, a transparent barrier layer, for example, an organic-inorganic hybrid barrier layer, is preferred.

[0054] The protective member may be in a state where the end of the tubular object is adhered to the protective member. For example, the end of the tubular object may be heat-sealed by heating, or may be adhered to the protective member by an adhesive. The protective member may be a pair of sheet-like materials bonded to each other. For example, the protective member may be formed by arranging a pair of sheet-like materials including a layer that exhibits adhesiveness when heated (hereinafter also referred to as a heat seal layer) so that the heat seal layer sides of the sheets face each other, and bonding at least a part of the heat seal layer by heating. The heat seal layer includes, for example, a resin that is solid at room temperature and melts when heated. The protective member may be in a state where the peripheral portions of the pair of sheets are bonded with an adhesive.

[0055] When a pair of sheets are bonded together to form a protective member, the side of the protective member is provided with a fused portion formed by fusing the heat seal layer of the sheet or an adhesive (i.e., a portion having a water vapor permeability of 0.5 g / m 2 / day) Therefore, from the viewpoint of airtightness of the protective member, the proportion of the fused or bonded parts in the surface area of ​​the protective member is preferably less than 15%, more preferably less than 10%, and even more preferably less than 5%.

[0056] The protective member may have an outer surface protective layer for protecting the outer surface of the protective member. The outer surface protective layer may be a layer containing a resin. When the protective member is formed using a sheet-like material having a heat seal layer and an outer surface protective layer, the outer surface protective layer may be a layer containing a resin that does not melt at a temperature at which the resin contained in the heat seal layer melts.

[0057] The thickness of the protective member (when the thickness is not constant, the minimum thickness) is not particularly limited. From the viewpoint of ensuring sufficient airtightness, the thickness of the protective member is preferably 2 μm or more, more preferably 10 μm or more, and further preferably 25 μm or more. From the viewpoint of economic efficiency, the thickness of the protective member is preferably 500 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less.

[0058] In order to ensure airtightness around the piezoelectric substrate, the area equivalent to 85% or more of the surface area of ​​the piezoelectric substrate must have a water vapor permeability of 0.5 g / m 2 It is preferable that the material be covered with a material that is less than 1 / day. In the following, the water vapor permeability of the surface area of ​​the piezoelectric substrate is 0.5 g / m 2 The percentage (%) of the area covered by materials with a density of less than 1 / day is also called the "coverage rate."

[0059] At least 85% of the surface area of ​​the piezoelectric substrate has a water vapor permeability of 0.5g / m 2 / day or less (i.e., the coverage is 85% or more), sufficient airtightness is ensured around the piezoelectric substrate, effectively preventing contact between the piezoelectric body and water vapor.

[0060] To ensure airtightness around the piezoelectric substrate, 90% or more of the surface area of ​​the piezoelectric substrate must have a water vapor permeability of 0.5 g / m 2 / day or less (i.e., the coverage is 90% or more), and more than 95% of the surface area of ​​the piezoelectric substrate is preferably covered with a material having a water vapor transmission rate of 0.5 g / m 2 It is even more preferred that the surface is covered with a material having a surface roughness of 95% or more / day or less (i.e., a coverage rate of 95% or more).

[0061] (Wiring materials) The piezoelectric device of the present disclosure may further include a wiring member electrically connected to the internal conductor of the piezoelectric substrate described above. The wiring member has one end electrically connected to the internal conductor of the piezoelectric substrate, and the other end disposed outside the piezoelectric device. When the piezoelectric device of the present disclosure includes a wiring member, the protective member covers the entire piezoelectric substrate and at least a part of the outer periphery of the wiring member. Since the protective member covers the entire piezoelectric substrate and at least a portion of the outer periphery of the wiring member, airtightness around the piezoelectric substrate is sufficiently ensured, effectively preventing contact between the piezoelectric body and water vapor.

[0062] When the piezoelectric substrate includes an external conductor, the piezoelectric substrate may further include a wiring member electrically connected to the external conductor.

[0063] The form of the wiring member is not particularly limited as long as it can be electrically connected to the internal conductor of the piezoelectric substrate. The wiring member may be, for example, a coaxial cable including a long internal conductor, a dielectric insulating layer disposed around the internal conductor, and an external conductor disposed around the dielectric insulating layer. When the wiring member is a coaxial cable, the inner conductor of the coaxial cable and the inner conductor of the piezoelectric substrate may be electrically connected, and the outer conductor of the piezoelectric substrate may be electrically connected to the outer conductor of the coaxial cable.

[0064] (Example of the structure of the piezoelectric substrate) Specific examples of the configuration of the piezoelectric substrate will be described below with reference to the drawings, but the present disclosure is not limited to the following specific examples.

[0065] Fig. 1A is a schematic side view illustrating the appearance of a piezoelectric substrate 10A according to an embodiment of the present disclosure, and Fig. 1B is a cross-sectional view taken along line IB-IB of Fig. 1A.

[0066] 1A, the piezoelectric substrate 10A includes an elongated internal conductor 12A and a piezoelectric layer 14A. The piezoelectric layer 14A is spirally wound in one direction along the outer circumferential surface of the internal conductor 12A from one end to the other end at a helix angle β1 without any gaps. The piezoelectric layer 14A is formed by winding a piezoelectric yarn 140A counterclockwise around the outer circumferential surface of the internal conductor 12A. The piezoelectric yarn 140A includes an optically active polypeptide fiber. In FIG. 1A, helix angle β1 is the angle between the direction of helix axis G1 (the axial direction of internal conductor 12A) and the length direction of piezoelectric yarn 140A in side view. 1A, the double-headed arrow E1 indicates the main orientation direction of the optically active polypeptide contained in the piezoelectric layer 14A. That is, the main orientation direction of the optically active polypeptide contained in the piezoelectric yarn 140A is approximately parallel to the length direction of the piezoelectric yarn 140A.

[0067] The effects of the piezoelectric substrate 10A will be described below. For example, when tension is applied in the longitudinal direction of the piezoelectric substrate 10A, a shear stress is applied to the optically active polypeptide contained in the piezoelectric layer 14A, and the optically active polypeptide is polarized. This polarization of the optically active polypeptide is thought to occur in phase with the radial direction of the piezoelectric substrate 10A, as shown by the arrows in Figure 1B. This causes the piezoelectricity of the piezoelectric substrate 10A to be expressed.

[0068] FIG. 2 is a schematic side view showing the appearance of a piezoelectric substrate 20A according to an embodiment of the present disclosure. The piezoelectric substrate 20A differs from the piezoelectric substrate 10A shown in FIG. 1A in that, in addition to the internal conductor 12A and the piezoelectric layer 14A, the piezoelectric substrate 20A includes an external conductor 22A disposed around the piezoelectric layer 14A.

[0069] 2, the piezoelectric substrate 20A includes an internal conductor 12A, a piezoelectric layer 14A, and an external conductor 22A. The external conductor 22A is disposed on the outer periphery side of the piezoelectric layer 14A. The external conductor 22A is formed by spirally winding a long conductor (e.g., copper foil) around the piezoelectric layer 14A.

[0070] As shown in Fig. 2, in the piezoelectric substrate 20A, the end of the piezoelectric layer 14A is misaligned with the end of the external conductor 22A. This electrically insulates the internal conductor 12A from the external conductor 22A. However, the method of electrically insulating the internal conductor 12A from the external conductor 22A in the present disclosure is not limited to the configuration shown in Fig. 2.

[0071] Since the piezoelectric substrate 20A includes the internal conductor 12A, an electrical signal (voltage signal or charge signal) generated in the piezoelectric layer 14A can be more easily extracted via the internal conductor 12A. Furthermore, since the piezoelectric substrate 20A includes the external conductor 22A, the inside of the piezoelectric substrate 20A (the piezoelectric layer 14A and the internal conductor 12A) can be electrostatically shielded by the external conductor 22A. This makes it possible to suppress voltage changes in the internal conductor 12A caused by static electricity outside the piezoelectric substrate 20A, resulting in more stable piezoelectricity.

[0072] (Applications of piezoelectric devices) The applications of the piezoelectric device are not particularly limited, and examples thereof include sensors, actuators, energy harvesters, and bioinformation acquisition devices. That is, embodiments of the present disclosure include sensors, actuators, energy harvesters, and biometric information acquisition devices that include the piezoelectric devices of the present disclosure. Specific examples of sensors include force sensors, pressure sensors, displacement sensors, deformation sensors, motion sensors, vibration sensors, impact sensors, and ultrasonic sensors.

[0073] The bioinformation acquisition device detects the biosignals of a human subject or animal subject (hereinafter, collectively referred to as "subject") using a piezoelectric substrate to acquire the bioinformation of the subject. The biosignals include presence / absence, body movement, pulse wave signal (heart rate signal), respiratory signal, body movement signal, ballistocardiogram, biotremor, etc. Biotremor means rhythmic involuntary movement of a body part (fingers, hand, forearm, upper limb, etc.). The detection of ballistocardiogram also includes the detection of the force effect due to the cardiac function of the body. That is, when the heart pumps blood into the aorta and pulmonary artery, the body experiences a recoil force in the opposite direction to the blood flow. The magnitude and direction of this recoil force change with the functional stage of the heart. This recoil force is detected by sensing the ballistocardiogram outside the body.

[0074] The article to which the biometric information acquisition device is applied is not particularly limited. For example, the biometric information acquisition device may be applied to an article that the subject comes into contact with, such as a seat, a steering wheel, a seat, a seat belt, a shift knob, an armrest, a headrest, a handle, etc. Alternatively, the biometric information acquisition device may be applied to an article that the subject wears, such as clothing, a hat, a wristwatch, etc. The bioinformation acquisition device of the present disclosure is preferably used as a detection unit of an information processing device. The information processing device acquires a biosignal of a subject from the bioinformation acquisition device, and detects abnormalities or abnormal physical conditions of the subject based on the acquired biosignal. The information processing device may utilize artificial intelligence (AI).

[0075] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples. However, the present invention is not limited to the description of these examples.

[0076] [Example 1] (Preparation of piezoelectric yarn) As the optically active polypeptide fiber, 21 denier raw silk was prepared. Raw silk is a long fiber made of optically active polypeptide. The thickness of the raw silk was 0.06 mm to 0.04 mm. The raw silk described above was twisted into six strands (twist number 150 T / m) by a known method, and the resulting yarn was refined to produce a piezoelectric yarn made of refined silk.

[0077] Using a wide-angle X-ray diffraction device (Rigaku's "RINT2550", accessories: rotating sample stage, X-ray source: CuKα, output: 40kV 370mA, detector: scintillation counter), the piezoelectric yarn was fixed to a holder and the azimuthal distribution intensity of the crystal plane peak [2θ=20°] was measured. In the obtained azimuth angle distribution curve (X-ray interference diagram), the degree of orientation F (c-axis orientation) of the optically active polypeptide fiber contained in the piezoelectric yarn was calculated from the half-width (α) of the peak according to the following formula (a). The result was 0.86. Orientation degree (F)=(180°-α) / 180° … (a) (α is the half-width of the peak due to the orientation)

[0078] Since the orientation degree F of the optically active polypeptide fibers contained in the piezoelectric yarn was 0.86 and six-strand single-twisted yarn (piezoelectric yarn) was produced using refined silk, it can be evaluated that the length direction of the piezoelectric yarn and the main orientation direction of the optically active polypeptide contained in the piezoelectric yarn are approximately parallel.

[0079] (Preparation of piezoelectric substrate) As the internal conductor, a tinsel wire "U24-01-00" (wire diameter 0.26 mm, length 200 mm) manufactured by Meisei Sangyo Co., Ltd. was prepared. A layer of piezoelectric yarn (piezoelectric yarn layer) was formed on the outer periphery of the internal conductor by winding the piezoelectric yarn counterclockwise so that the helix angle was about 45°. The formed piezoelectric yarn layer covered the entire outer periphery of the internal conductor. In other words, the outer periphery of the internal conductor was not exposed. An adhesive called "901H3" (a cyanoacrylate adhesive) manufactured by Toagosei Co., Ltd. was dropped onto the outer periphery of the piezoelectric yarn layer and allowed to soak into the interior of the piezoelectric yarn layer. After that, the excess adhesive was immediately wiped off from the outer periphery of the piezoelectric yarn with a Kimwipe, and the adhesive was allowed to harden at room temperature.

[0080] A rolled copper foil ribbon with a rectangular cross section (width: 0.3 mm, thickness: 30 μm) was prepared as the external conductor. This rolled copper foil ribbon was wound clockwise around the outer peripheral surface of the piezoelectric thread layer to form an external conductor on the outer peripheral surface of the piezoelectric thread layer. The external conductor covered the entire outer peripheral surface of the piezoelectric thread layer. In other words, the outer peripheral surface of the piezoelectric thread layer was not exposed.

[0081] An electrical insulator was placed on the outer periphery of the external conductor using polytetrafluoroethylene (PTFE). Specifically, a coating with a thickness of about 130 μm was formed by passing the material through a die for ordinary molten resin coating from an extrusion molding machine. Through the above process, a piezoelectric substrate was produced.

[0082] (Fabrication of Piezoelectric Devices) Two wiring members were connected to the internal conductor and external conductor at one end of the piezoelectric substrate. The wiring members were the same rolled copper foil ribbon used to make the external conductor, and the connections were made by soldering. The end of the piezoelectric substrate opposite to the side where the wiring members were attached was cut so that the length of the piezoelectric substrate was 150 mm.

[0083] We used a Mitsubishi Gas Chemical gas barrier bag [RP system] aluminum bag AB180250PL (180 mm x 250 mm, heat seal layer: polyethylene). The water vapor transmission rate of this aluminum bag was 0.02 g / m, which is below the detection limit of the measurement system. 2 / day and the thickness was 93 μm.

[0084] The aluminum bag was cut to obtain a protective member (15 mm x 190 mm) in which two sheets were sealed at only one of the short sides. The piezoelectric substrate was fixed in the center of the protective member with Kapton tape cut to a width of 4 mm. The two wiring members connected to the piezoelectric substrate were arranged parallel to the axial direction of the piezoelectric substrate, with their ends protruding from the outside of the protective member. In this state, the other three sides were heat sealed to produce a piezoelectric device. A Fuji Impulse V-300 was used as the heat sealer, and heat sealing was performed without using vacuum degassing at memory 4. The seal width was 5 mm on the long side and 10 mm on the short side. The thickness of the fused part formed by heat sealing was 0.04 mm. Through the above steps, a piezoelectric device was fabricated in which the entire internal conductor of the piezoelectric substrate and a portion of the outer periphery of the wiring member were covered with the protective member.

[0085] In the piezoelectric device fabricated through the above process, if the piezoelectric substrate is embedded in a space measuring 5 mm × 170 mm × 0.04 mm, the water vapor permeability of the side surface (fused portion) of the protective member covering the piezoelectric substrate, excluding the portion crossed by the wiring member (0.3 mm wide × 2 pieces), is 0.5 g / m 2 / day. Therefore, the barrier area ratio of the protective member was calculated by the following formula. Barrier area ratio = {(5 x 170 x 2) / (5 x 170 x 2 + 170 x 0.04 x 2 + (5-0.6) x 0.04 + 5 x 0.04)} x 100 = 99.2%

[0086] In the piezoelectric device fabricated through the above process, the shape of the piezoelectric substrate is a cylinder with a diameter of 0.85 mm and a length of 150 mm, and the water vapor permeability of the surface area of ​​the piezoelectric substrate is 0.5 g / m 2 The percentage of the area covered by materials with a radiation exposure rate of 0.01 mg / day or less (coverage rate) was calculated using the following formula. Surface area A of the piezoelectric substrate = (0.85 x 3.14 x 150) + (0.425 x 0.425 x 3.14 x 2) = 401.484 mm 2 Projected area B of the piezoelectric substrate overlapping the fused part of the protective material = 0.04 × (150 + 0.85) × 2 = 12.068 mm 2 Coverage rate = {(AB) / A} x 100 = 97.0%

[0087] (Measurement of piezoelectric sensitivity) The initial value of the piezoelectric sensitivity was measured using the piezoelectric substrate before the wiring member was attached. Specifically, both ends of the piezoelectric substrate were fixed to a tensile testing machine (distance between chucks: 150 mm), and a stress ranging from 1.0 N to 2.0 N was repeatedly applied in a triangular wave shape at 0.5 Hz periodically. The amount of charge generated on the front and back of the piezoelectric substrate was measured using an electrometer (Keithley's programmable electric meter "617"). The amount of generated charge per unit tensile force was calculated from the slope of the correlation line of the scatter plot with the measured amount of generated charge Q [C] on the Y axis and the tensile force F [N] of the piezoelectric substrate on the X axis, and this was used as the initial value of the piezoelectric sensitivity. The result was 2.5 pC / N mm.

[0088] (High temperature and humidity storage test) The fabricated piezoelectric device was placed in a constant temperature and humidity chamber at 85°C and 85% RH, and removed after 24 hours. The piezoelectric device was removed from the high temperature and humidity chamber and left in an environment at 23°C and 50% RH for 2 hours. The piezoelectric substrate was then removed from the protective material, and the piezoelectric sensitivity of the piezoelectric substrate was measured in the same manner as the initial value. The result was 2.5 pC / N mm, which was maintained at the same value as the initial value.

[0089] [Comparative Example 1] A piezoelectric device was fabricated in the same manner as in Example 1, except that the barrier material used in Example 1 was changed to an AS zippered aluminum bag 230×160+47 [AS ONE Corporation]. Thereafter, a constant temperature and humidity storage test was carried out in the same manner as in Example 1. The measured piezoelectric sensitivity was 1.6 pC / N mm, a large decrease from the initial value.

[0090] The water vapor transmission rate of the aluminum bag used in Comparative Example 1 was 0.99 g / m 2 / day, and the barrier area ratio and coverage ratio were both 0%.

[0091] [Comparative Example 2] A constant temperature and humidity storage test was carried out on the piezoelectric substrate with wiring member produced in Example 1 without covering the outer circumferential surface with a barrier member. The measured piezoelectric sensitivity was 0.5 pC / N mm, which was a significant decrease from the initial value.

[0092] [Example 2] The piezoelectric substrate with wiring member prepared in Example 1 was fixed to the center of an EPDM rubber cushioning material measuring 150 mm x 10 mm x 1.0 mm using a polyimide tape with a width of 5 mm and a thickness of 25 μm. The density of the EPDM rubber cushioning material used was 0.15 g / cm. 3 The rubber hardness is 10 according to the Asker rubber hardness tester type C conforming to JIS K7312. Next, the aluminum bag used in Example 1 was cut to a size of 20 mm x 190 mm, and the EPDM rubber cushioning material with the piezoelectric substrate fixed thereto was covered with the aluminum bag and sealed around the periphery (seal width: 5 mm) to produce a piezoelectric device. Thereafter, a constant temperature and humidity storage test was carried out in the same manner as in Example 1. The measured piezoelectric sensitivity was 2.5 pC / N mm, which was maintained at the same value as the initial value.

[0093] The values ​​of the barrier area ratio and coverage ratio measured in Example 2 were both the same as those in Example 1.

Claims

1. A piezoelectric device comprising a piezoelectric substrate and a protective member covering an outer periphery of the piezoelectric substrate, The piezoelectric substrate has an elongated internal conductor and a piezoelectric body covering an outer circumferential surface of the internal conductor; The piezoelectric body includes fibers made of an optically active polypeptide, the length direction of the piezoelectric body is approximately parallel to the main orientation direction of the optically active polypeptide; The degree of orientation F of the fiber made of the optically active polypeptide, which is calculated by the following formula (a) from X-ray diffraction measurement, is 0.50 or more and less than 1.00, The water vapor permeability of a portion corresponding to 85% or more of the surface area of ​​the protective member is 0.5 g / m 2 / day or less. Orientation degree F=(180°-α) / 180°...Formula (a) [In formula (a), α represents the half-width (°) of the peak due to the orientation.]

2. A portion of the piezoelectric substrate that corresponds to 85% or more of the surface area of ​​the piezoelectric substrate has a water vapor permeability of 0.5 g / m 2 13. The piezoelectric device of claim 1, wherein the piezoelectric device is covered with a material having a surface roughness of less than 100 nm / day.

3. The piezoelectric device according to claim 1 , wherein the protective member includes a layer that exhibits a barrier property against water vapor.

4. The piezoelectric device according to claim 3 , wherein the layer contains at least one selected from the group consisting of inorganic oxides, inorganic nitrides, inorganic fluorides, and diamond-like carbon.

5. The piezoelectric device of claim 1 , wherein the protective member includes a metal.

6. a wiring member electrically connected to the internal conductor of the piezoelectric substrate, The piezoelectric device according to claim 1 , wherein the protective member covers the entire piezoelectric substrate and at least a part of an outer periphery of the wiring member.

7. The piezoelectric device according to claim 1 , wherein the protective member is formed by adhering ends of a tubular member or by adhering a pair of sheet-like members to each other.

8. The piezoelectric device of claim 1 , wherein the optically active polypeptide has a β-sheet structure.

9. The piezoelectric device of claim 1 , wherein the optically active polypeptide comprises fibroin.

10. A sensor comprising the piezoelectric device according to any one of claims 1 to 9.

11. An actuator comprising the piezoelectric device according to any one of claims 1 to 9.

12. A bioinformation acquisition device comprising the piezoelectric device according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Piezoelectric base material, sensor, actuator, biological information acquisition device, and piezoelectric fiber structure

    EP3534419A1

  • Organic substance, film containing the same, and electrical element having the same

    JP2010116563A

  • Sensor circuit

    JP2021173680A

  • Organic material, film comprising the same and electric device comprising the film

    US20100117522A1

  • Piezoelectric substrate, sensor, actuator, biological information acquisition device, and piezoelectric fiber structure

    US20200058844A1