Iron ion slow-release glass material for algal growth, and algal growth material and artificial reefs, each including the same

A synthetic glass material with optimized SiO2, B2O3, Na2O, K2O, FeO, and Fe2O3 ratios provides continuous iron ion elution for 2 to 5 years, addressing the instability of existing materials and supporting stable algae growth against herbivorous feeding.

JP2024136692APending Publication Date: 2024-10-04TOYO SEIKAN GRP HLDG LTD +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023047881
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing seaweed bed propagation materials either have insufficient iron ion elution during critical periods when algae are susceptible to herbivorous animal feeding or elute iron ions too quickly, failing to support stable algae growth over multiple generations.

Method used

A synthetic glass material composed of specific ratios of SiO2, B2O3, Na2O, K2O, FeO, and Fe2O3, optimized for a boron to silicon molar ratio (B/Si) and potassium to sodium molar ratio (K/Na), allowing continuous elution of iron ions for 2 to 5 years, with a controlled disappearance rate constant (κ) and melting temperature within specific ranges.

Benefits of technology

The glass material ensures continuous elution of iron ions necessary for algae growth, supporting stable algae growth despite herbivorous animal feeding, with a controlled elution period and manufacturing ease.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136692000001_ABST
    Figure 2024136692000001_ABST
Patent Text Reader

Abstract

To continuously leach the iron ions required for algal growth during the period when the attached algae are vulnerable to feeding from herbivorous animals.SOLUTION: An iron ion slow-release glass material for algal growth comprises 40-70 mass% of SiO2, 1-29 mass% of B2O3, 1-35 mass% of Na2O and / or K2O, and 1-40 mass% of FeO and / or Fe2O3.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an iron ion-releasing glass material for algae growth, which is used to supply iron ions necessary for the growth of algae in seawater or the like, and to an algae growth material and an artificial fish reef equipped with the same. [Background technology]

[0002] Conventionally, with regard to artificial fish reefs that are artificially installed in water such as the sea, techniques have been developed for dissolving components containing iron ions into the water in order to enhance the proliferation effect of algae and the like.

[0003] For example, a seaweed bed growth material is known that contains silicon, sodium and / or potassium, and iron in amounts equivalent to 30 to 70 mass% in SiO2 conversion, 10 to 50 mass% in Na2O and / or K2O conversion, and 5 to 50 mass% in Fe2O3 conversion, respectively, and that contains 1 mass% or more of divalent iron (see Patent Document 1).

[0004] Furthermore, a known example of a seaweed bed growth material intended to efficiently dissolve divalent iron ions into water is one whose main components are 15-50 mass% SiO2, 1-35 mass% of one or two of Na2O and K2O, 30-70 mass% B2O3, and 1-40 mass% of one or two of FeO and Fe2O3 (see Patent Document 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 2577319 [Patent Document 2] Patent No. 3357990 Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, the phenomenon of coastal denudation caused by feeding on herbivorous animals has been expanding throughout Japan. One of the reasons for this is thought to be that the amount of food consumed by herbivorous animals such as sea urchins and fish exceeds the amount of algae that grows on fish reefs. In particular, the soft thallus of algae is easily eaten by herbivorous animals from immediately after they sprout to when they are young.

[0007] The seaweed bed propagation material disclosed in Patent Document 1 has the advantage that the elution of iron ions necessary for enhancing the proliferation effect of algae continues for a long period of time (for example, about 10 years). In addition, the seaweed bed propagation material disclosed in Patent Document 2 can efficiently elute iron ions into water, so it is possible to ensure the necessary amount of eluted iron ions with a small amount of seaweed bed propagation material, and has the particular advantage of being able to effectively propagate attached diatoms, which serve as food for young sea urchins and shellfish.

[0008] Therefore, the inventors of the present application conducted intensive research into the application of the seaweed bed growth materials disclosed in the above Patent Documents 1 and 2 to ensure the growth of algae in an amount sufficient to withstand ingestion by herbivorous animals during the period when the algae are most likely to be eaten.

[0009] However, the seaweed bed growth material disclosed in Patent Document 1 may not dissolve enough iron ions during times when algae are likely to be eaten (i.e., it may not be possible to ensure the growth of seaweed that can withstand eating).

[0010] On the other hand, with the seaweed bed propagation material disclosed in Patent Document 2, although the dissolution rate of iron ions is increased, the duration of this increase (i.e., the disappearance lifespan of the seaweed bed propagation material) is short, at around three months, so there is a possibility that the necessary proliferation of algae (including proliferation required for the algae to stably attach to the artificial fish reef over several generations) may not be achieved.

[0011] In response to this, the inventors of the present application have discovered that in order to ensure the proliferation of algae sufficient to withstand grazing, it is necessary to continue dissolving the iron ions necessary for algae growth for approximately 2 to 5 years (i.e., the period during which algae growth is susceptible to the effects of grazing by herbivorous animals).

[0012] In view of the above background, an object of the present invention is to provide an iron ion-releasing glass material that can continuously release the iron ions necessary for algae growth during the period when algae after attachment are susceptible to feeding by herbivorous animals, as well as an algae growth material and an artificial fish reef that include the same. [Means for solving the problem]

[0013] One embodiment of the present invention is an iron ion-releasing glass material for algae growth, which comprises 40-70 mass% SiO2, 1-29 mass% B2O3, 1-35 mass% of either one or both of Na2O and K2O, and 1-40 mass% of either one or both of FeO and Fe2O3.

[0014] According to this embodiment, during the period in which the algae after attachment are susceptible to feeding by herbivorous animals, iron ions necessary for the growth of the algae can be continuously eluted.

[0015] In the above embodiment, the disappearance rate constant κ×10 is expressed by the following formula, which is described by the molar ratio B / Si of boron to silicon and the molar ratio K / Na of potassium to sodium in all components. -4 It is preferable that the range is 1.14 or more and 2.85 or less.

[0016]

number

[0017] Here, κ is defined as follows.

number

[0018] According to this embodiment, the iron ions necessary for the proliferation of algae can be continuously eluted for about 2 to 5 years, a period during which the algae are susceptible to ingestion by herbivorous animals.

[0019] In the above aspect, the elimination rate constant κ×10 -4 It is preferable that the range is 1.425 or more and 2.28 or less.

[0020] According to this embodiment, the iron ions necessary for the proliferation of algae can be continuously eluted for about 2.5 to 4 years, a period during which the algae are susceptible to ingestion by herbivorous animals.

[0021] In the above embodiment, the molar ratio B / Si of boron to silicon, the molar ratio K / Na of potassium to sodium, and the alkali content α in all components are expressed by the following formula: -3 It is preferable that the range is 1.20 or more and 1.45 or less.

[0022]

number

[0023] According to this embodiment, it becomes easy to set the melting temperature of the iron ion-releasing glass material in an appropriate range (ie, 1200 to 1450° C.), and the production thereof becomes easy.

[0024] One aspect of the present invention is an algae growth material comprising the above-mentioned iron ion-release glass material and a substrate to which the iron ion-release glass material is fixed.

[0025] According to this embodiment, it is possible to realize an algae growth material that continuously elutes iron ions necessary for algae growth during the period when the attached algae are susceptible to feeding by herbivorous animals.

[0026] One embodiment of the present invention is an artificial fish reef comprising the iron ion-releasing glass material or the algae growth material.

[0027] According to this embodiment, it is possible to realize an artificial fish reef that continuously dissolves iron ions necessary for the growth of algae during the period when the settled algae are susceptible to being eaten by herbivorous animals. Effect of the Invention

[0028] The iron ion-releasing glass material of the present invention, and the algae growth material and artificial fish reef equipped with the same, are capable of continuously eluting the iron ions necessary for algae growth during the period when the algae are susceptible to feeding by herbivorous animals after attachment. [Brief description of the drawings]

[0029] [Figure 1] Schematic diagram of an artificial fish reef equipped with iron ion-releasing glass material [Diagram 2] Schematic diagram of algae growth material equipped with iron ion-releasing glass material [Diagram 3] Graph showing the relationship between the disappearance rate constant κ×10-4 and B / Si and K / Na DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Hereinafter, with reference to the drawings, an iron ion-releasing glass material for algae growth according to an embodiment of the present invention, and an algae growth material and an artificial fish reef including the same will be described.

[0031] As shown in Fig. 1, an artificial reef 1 according to an embodiment includes at least one tetrabod 2 (i.e., a concrete block consisting of four legs with each apex of a tetrahedron as a tip) that is artificially installed in water such as the ocean. Each tetrabod 2 has a plurality of recesses 2a formed therein. In each recess 2a, an algae growth material 3 for growing algae (e.g., seaweed such as nori, wakame, and kombu) is fixed by adhesive.

[0032] The algae growth material 3 comprises a mortar plate 11 (an example of a substrate) having a rectangular shape in a plan view, and an iron ion-releasing glass material 12 (hereinafter simply referred to as "glass material 12") fixed to the upper surface of the plate 11. The glass material 12 contains a large number of vitreous particles, and as shown in Fig. 2, is fixed to the upper surface of the plate 11 in a layered manner. The vitreous particles have a particle size in the range of about 2 to 7 mm (for example, an average particle size of 4.5 mm), for example, and more preferably have a particle size in the range of about 3 to 5 mm.

[0033] The artificial fish reef 1 according to the present invention is not limited to that shown in FIG. 1, but may include blocks or the like made of known materials suitable for fish reefs (including, for example, stone, steel, wood, and concrete) and having a desired form (including changes in shape and size). The form of the algae growth material 3 according to the present invention can also be modified in various ways. Furthermore, the plate 11 is not essential to the algae growth material 3. The algae growth material 3 may have a form in which glass material 12 is contained in a bag-shaped net.

[0034] The glass material 12 contains at least one or two of SiO2, B2O3, Na2O, and K2O, and one or two of FeO and Fe2O3 as components that serve as a source of ions that dissolve in water.

[0035] As a result, silicon ions, boron ions, sodium ions, potassium ions, divalent iron ions, and trivalent iron ions may be eluted from the glass material 12 in the water. However, it is sufficient that at least one of the sodium ions and potassium ions is eluted from the glass material 12. Similarly, it is sufficient that at least one of the divalent iron ions and trivalent iron ions is eluted from the glass material 12. Hereinafter, when there is no need to particularly distinguish between the divalent iron ions and the trivalent iron ions, they will be simply referred to as "iron ions."

[0036] Furthermore, glass material 12 may contain components other than SiO2, B2O3, Na2O, K2O, FeO, and Fe2O3, so long as they do not significantly affect the elution rate of iron ions.

[0037] SiO2 is a main component that forms a three-dimensional mesh structure in glass material 12. The proportion of SiO2 in glass material 12 is preferably set in the range of 40 to 70 mass %.

[0038] B2O3 is a component that, together with SiO2, forms the network structure of the glass material 12, making the skeleton of the network structure fragile and increasing the elution rate of elution components (particularly iron ions in this embodiment) fixed therein. The proportion of B2O3 in the glass material 12 is preferably set in the range of 1 to 29 mass % (less than 30 mass %). If B2O3 is 30 mass % or more, the elution rate of iron ions becomes excessively high, making it difficult to continuously elute iron ions necessary for algae growth during the period when the attached algae are susceptible to feeding by herbivorous animals (i.e., the glass material 12 loses the ability to release iron ions in an early stage).

[0039] Na2O and K2O are components for adjusting the dissolution rate of glass by breaking the mesh structure of glass material 12. The proportion of either one or both of Na2O and K2O (i.e., the total amount thereof) in glass material 12 is preferably set within the range of 1 to 35 mass %.

[0040] FeO and Fe2O3 are components for dissolving divalent iron ions and trivalent iron ions, which play an important role in the growth of algae. The proportion of any one or two of FeO and Fe2O3 (i.e., the sum of them) in the glass material 12 is set in the range of 1 to 40 mass%, more preferably in the range of 5 to 20 mass%. If any one or two of FeO and Fe2O3 are less than 1 mass%, the amount of eluted iron ions necessary for the growth of algae will be insufficient during the period when the algae are susceptible to feeding by herbivorous animals after attachment. If any one or two of FeO and Fe2O3 exceed 40 mass%, they may not be able to enter the mesh structure and may precipitate as metallic iron, making it difficult to uniformly disperse the iron ion component in the glass material 12. Furthermore, by setting the proportion of either one or both of FeO and Fe2O3 in glass material 12 to the range of 5 to 20 mass %, the necessary dissolution rate of iron ions can be more stably ensured while the precipitation of metallic iron in glass material 12 can be more stably prevented.

[0041] Glass material 12 can be produced by heating known materials containing the above-mentioned components to a high temperature (e.g., 1200 to 1450°C) to melt them together, and then cooling them. Furthermore, glass material 12 after cooling can be crushed (or pulverized) using a stirring mill or the like, and sized using a sieve to adjust the particle size so that it falls within a desired range (e.g., about 3 to 5 mm). EXAMPLES

[0042] As described below, an experiment was conducted using a glass sample to measure (estimate) the loss of iron ion release lifetime of the glass material 12 (here, the period until the glass material 12 loses its ability to release iron ions after being placed in water).

[0043] (Glass sample raw material) As raw materials for the glass samples, known materials were mixed so that the ratios of SiO2, B2O3, Na2O, K2O, FeO, and Fe2O3 in the components satisfied the above-mentioned ranges, and multiple mixed raw materials with different compositions were obtained. The materials used were flattery silica sand (SiO2) (Flattery Silica Sand-60, International Pier Co., Ltd.), anhydrous borax (Na2B4O7) (PYROBOR Dehydrated Borax, IMC Chemicals, Inc.), boric acid (H3BO2) (Orthoboric Acid, USBorax, Inc.), soda ash (Na2CO3) (Soda Ash Dense, Tokuyama Corp.), potassium carbonate (K2CO3) (Potassium Carbonate, UNID Global Corporation), ferric oxide (Fe2O3) (CY, Chemilite Kogyo Co., Ltd.), and coke (C) (Special Powder No. 100, Josuizai Seizo Co., Ltd.). The mixing ratios of each material are shown in Table 1.

[0044] [Table 1]

[0045] (Method of manufacturing glass samples) Each mixed raw material was placed in a preheated alumina crucible, which was then placed in an electric furnace heated to 1200-1450°C and left for 2 hours. The molten raw materials in the alumina crucible were then poured onto an iron plate to obtain a glass sample. Using the same method, multiple glass samples (sample numbers 1-21) with different compositions were obtained (for details on the composition of each glass sample, see Table 2 below).

[0046] (Method of measuring the disappearance life) In order to estimate the disappearance life of the glass material 12, which can be several years, within a short period of about two months using a glass sample, an accelerated test was carried out under the following conditions 1 and 2.

[0047] Condition 1: Since the disappearance life increases in proportion to the size of the initial grain size of the particles constituting the glass sample, the initial grain size of these particles (i.e., the initial average grain size) was set smaller than the grain size of the actual glass material 12. Condition 2: In order to increase the reactivity of the glass sample in water (i.e., the dissolution rate of iron ions), the temperature of the solvent in which the glass sample was immersed (here, artificial seawater) was set to a temperature higher than room temperature (here, 70°C).

[0048] A 1.25g glass sample (particle size 0.35-0.8mm) was placed in a nylon mesh and suspended (i.e., immersed in) in an Erlenmeyer flask containing 250ml of solvent maintained at 70℃. It was taken out every 3-4 days, dried, and its mass was measured. After the measurement, the glass sample was suspended again in the Erlenmeyer flask in which the solvent had been replaced. By repeating such measurements, data on the change in the mass of the glass sample over time was obtained. The solvent used was artificial seawater prepared by dissolving artificial seawater essence (Marine Essence NK-1, manufactured by Japan Household Salt Co., Ltd.) at 4.16g / 100ml of water.

[0049] (Indicator of disappearance lifespan) If we assume that the initial concentration of the particulate matter that constitutes the glass sample in the solvent is much smaller than the solubility (sink condition) and that the dissolution of the glass in the solvent occurs only by diffusion through the glass surface, the Hixson-Crowell relationship shown in the following equation (1) can be derived.

[0050]

number

[0051] Moreover, the normalized disappearance amount δ of the particles constituting the glass sample can be expressed by the following formula (2) using the above W0 and W.

[0052]

number

[0053] Based on formulas (1) and (2), the normalized loss amount δ can be expressed by the following formula (3) using the loss rate constant κ, where t corresponds to the elapsed time after the start of the iron ion dissolution (i.e., after the iron ion-releasing glass material is immersed in water).

[0054]

number

[0055] In this embodiment, the disappearance rate constant κ×10 -4 [h -1 The disappearance life of the glass samples was evaluated using the index.

[0056] Based on the above-mentioned normalized loss amount δ, in order to continue the dissolution of iron ions from the glass material 12 for about 2 to 5 years (i.e., the period during which the growth of algae is susceptible to the effects of feeding by herbivorous animals), the rate coefficient κ×10 -4 is within the range of 1.14 or more and 2.85 or less (i.e., 1.14≦κ×10 -4 More preferably, in order to continue the elution of iron ions from the glass material 12 for about 2.5 to 4 years, the rate coefficient κ×10 -4 is within the range of 1.425 or more and 2.28 or less (i.e., 1.42≦κ×10 -4 ≦2.28).

[0057] (Measurement results of disappearance life) Table 2 shows the measurement results of the disappearance life of the glass samples based on the above-mentioned measurement method.

[0058] [Table 2]

[0059] (Relationship between composition parameters and dissipation life) According to the measurement results of the disappearance life of the above-mentioned glass samples, it is possible to realize the target range of the disappearance rate constant κ by setting the proportions of SiO2, B2O3, Na2O, K2O, FeO, and Fe2O3 within the above-mentioned ranges (see sample numbers 9-13). On the other hand, the inventors of the present application have found that it is not possible to stably keep the range of the disappearance rate constant κ within the target range (i.e., 1.14≦κ×10) by simply setting the proportions of SiO2, B2O3, Na2O, K2O, FeO, and Fe2O3 in the glass samples. -4 It was thought that it would be difficult to adjust the solubility of the fluorine-containing compound to a range that satisfies the requirement of ≦2.85.

[0060] As a result of extensive research by the present inventors, it was found that the rate coefficient of the glass sample, κ × 10 -4 In order to stably keep the value within the range of 1.14 to 2.85, it has been found that it is preferable to adopt the molar ratio of boron (B) to silicon (Si) (hereinafter referred to as "B / Si") and the molar ratio of potassium (K) to sodium (Na) (hereinafter referred to as "K / Na") in the glass sample, which have a large effect on the disappearance rate, as parameters to be taken into consideration in determining the composition (hereinafter referred to as "composition parameters"). (See Table 3 for the composition parameters (here, B / Si, K / Na) for each glass sample.)

[0061] [Table 3]

[0062] Therefore, B / Si and K / Na are used as explanatory variables, and the rate coefficient κ×10 -4 A multiple regression analysis was performed using the following as the objective variable: -4 and the correlation coefficient r between B / Si 1-1 was 0.884. The velocity coefficient κ×10 -4 and the correlation coefficient r between K / Na 1-2was 0.476.

[0063] As a result of multiple regression analysis, the following equation (4) was obtained.

[0064]

number

[0065] As shown in Figure 3, this equation (4) is expressed as the velocity coefficient κ × 10 -4 The desired range (i.e., 1.14≦κ×10 -4 3 shows the relationship between B / Si and K / Na (i.e., the colored range in FIG. 3) for keeping the B / Si and K / Na ratio within the range of ≦2.85). By adjusting the components of the glass material 12 so as to satisfy formula (4), it is possible to obtain a glass material 12 that continuously elutes iron ions necessary for algae growth for about 2 to 5 years, a period during which algae are susceptible to ingestion by herbivorous animals.

[0066] (Relationship between composition parameters and melting temperature) Based on the measurement results of the disappearance life of the above-mentioned glass samples, the inventors of the present application conducted intensive studies and found that, in order to set the melting temperature T [°C] of the raw material in the production of the glass sample within a temperature range with a small production load (here, 1200 to 1450°C), it is important to consider, as composition parameters, B / Si, K / Na, and alkali content α (i.e., the ratio of the sum of the masses of sodium (Na) and potassium (K) to the sum of the masses of boron (B), silicon (Si), sodium (Na), potassium (K), and iron (Fe) in the glass sample) which have a large effect on the melting temperature T (see Table 3 above for the composition parameters (here, B / Si, K / Na, and alkali content α) for each glass sample).

[0067] Therefore, B / Si, K / Na, and alkali content α were used as explanatory variables, and the melting temperature T × 10 -3 A multiple regression analysis was performed using the melting temperature T × 10 -3 and the correlation coefficient r between B / Si 2-1was 0.686. Also, the melting temperature T × 10 -3 and the correlation coefficient r between K / Na 2-2 was 0.383. Also, the melting temperature T × 10 -3 and the correlation coefficient r between alkali content α 2-3 was 0.825.

[0068] As a result of multiple regression analysis, the following equation (5) was obtained.

[0069]

number

[0070] By adjusting the components of glass material 12 so as to satisfy formula (5), it is possible to obtain glass material 12 that continuously dissolves the iron ions necessary for algae growth over a period of approximately 2 to 5 years, a period during which the material is susceptible to ingestion by herbivorous animals, and that has a melting temperature set within an appropriate range (i.e., 1200 to 1450°C).

[0071] According to the above-described embodiments of the iron ion-releasing glass material for algae growth, and the algae growth material and artificial fish reef equipped with the same, the iron ions necessary for algae growth can be continuously eluted during the period when the algae after attachment are susceptible to being eaten by herbivorous animals.

[0072] In addition, by setting the composition parameter values ​​that satisfy the above formula (4), the rate coefficient κ × 10 -4 can be set in an appropriate range (i.e., 1.14≦κ×10−4≦2.85). By setting the composition parameters in this way, the glass material 12 can continuously elute iron ions necessary for algae growth for about 2 to 5 years, a period during which the glass material 12 is susceptible to ingestion by herbivorous animals.

[0073] In addition, by setting the composition parameter values ​​that satisfy the above formula (5), the melting temperature T × 10 -3 within the appropriate range (i.e., 1.20≦T×10 -3≦1.45). By setting the composition parameters in this manner, the melting temperature of glass material 12 can be set in an appropriate range (that is, 1200 to 1450° C.), making it easy to manufacture.

[0074] Although the specific embodiment has been described above, the present invention is not limited to the above embodiment and can be modified in a wide range of ways. [Industrial Applicability]

[0075] The iron ion-releasing glass material for algae growth of the present invention, and the algae growth material and artificial fish reef comprising the same, are capable of continuously eluting the iron ions necessary for algae growth during the period when algae after attachment are susceptible to feeding by herbivorous animals, and are therefore useful as an iron ion-releasing glass material for algae growth, and an algae growth material and artificial fish reef comprising the same, which are used to supply the iron ions necessary for algae growth in seawater, etc. [Explanation of symbols]

[0076] 1:Artificial reef 2: Tetrabod 3: Algae propagation material 11: Plate 12: Iron ion sustained release glass material

Claims

1. An iron ion-releasing glass material for algae growth, comprising: 40 to 70% by mass of SiO 2 and, 1 to 29% by mass of B 2 O 3 and, 1 to 35% by mass of Na 2 O and K 2 One or two of O; 1 to 40% by mass of FeO and Fe 2 O 3 and any one or two of the above.

2. In the following equation described by the molar ratio B / Si of boron to silicon and the molar ratio K / Na of potassium to sodium in all components, the disappearance rate constant κ×10 -4 The iron ion-releasing glass material according to claim 1, wherein the range of is 1.14 or more and 2.85 or less. [0097] Here, κ is defined as follows. [0089] Where: t: time elapsed after the start of iron ion elution W 0 : initial mass of the particle W: Indicates the current mass of the particle.

3. The disappearance rate constant κ×10 -4 The iron ion-releasing glass material according to claim 2, wherein the range of is 1.425 or more and 2.28 or less.

4. In the following formula described by the molar ratio B / Si of boron to silicon, the molar ratio K / Na of potassium to sodium, and the alkali content α in all components, the melting temperature T×10 -3 The iron ion-releasing glass material according to claim 1 , wherein the range of is 1.20 or more and 1.45 or less. ##EQU00011## Here, T and α are as follows: T: melting temperature of the raw material of the iron ion-releasing glass material [°C] α: Ratio of the sum of the masses of sodium and potassium to the sum of the masses of boron, silicon, sodium, potassium, and iron in all components

5. The iron ion-releasing glass material according to claim 1 , A substrate to which the iron ion-releasing glass material is fixed; 2. An algae propagation material comprising:

6. An artificial fish reef comprising the iron ion-releasing glass material according to claim 1 or the algae-growing material according to claim 5.

Citation Information

Patent Citations

  • Colored medical neutral borosilicate glass and preparation method thereof

    CN115368013A

  • Ultraviolet ray absorbing flaky glass

    JP1991040938A

  • Algal field proliferating material and artificial fish reef

    JP1994335330A

  • Porcelain Enamel Having A Metallic Appearance

    US20070265154A1

  • Materials for growing algae and artificial fishing banks

    WO1998024298A1