Method for manufacturing zinc oxide thin film and method for manufacturing solar cell
A cost-effective method using ethanol, nitric acid, and zinc oxide mixture forms a dense and transparent zinc oxide thin film, addressing inefficiencies in existing methods by ensuring uniformity and density, thereby improving solar cell performance.
Patent Information
- Application Number
- JP2023047929
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for forming a zinc oxide thin film as an electron transport layer in solar cells are costly and inefficient, often requiring high-temperature processing and large-scale equipment, and result in non-uniform, non-dense films with poor transparency.
A method involving a mixture of ethanol, nitric acid, and zinc oxide, applied via spin coating and heated to form a dense and transparent zinc oxide thin film, utilizing specific ratios and conditions to ensure uniformity and density.
The method enables the production of a low-cost, dense, and transparent zinc oxide thin film suitable for solar cells, enhancing electron transport and reducing current leakage, thus achieving high output characteristics comparable to vapor deposition methods.
Smart Images

Figure 2024136719000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a zinc oxide thin film and a method for producing a solar cell. [Background technology]
[0002] In recent years, organic solar cells have been developed that use organic material films as the power generation layer. The electron transport layer that constitutes the organic solar cell is a layer that transports electrons generated in the power generation layer to the electrode, and is composed of a film of metal oxide such as zinc oxide, titanium oxide, or tin oxide. Among these metal oxides, zinc oxide film, which transmits visible light and absorbs ultraviolet light, has attracted attention as a film that constitutes the electron transport layer.
[0003] The film constituting the electron transport layer is required to be dense so that the electrons generated in the power generation layer can flow efficiently to the negative electrode. For this reason, the film of the electron transport layer is generally formed by a deposition method such as sputtering or CVD, but in this case, a large-scale manufacturing device for high-temperature treatment under reduced pressure is required, which requires a lot of time and high cost. As a low-cost and easy film formation method, coating methods such as spin coating, bar coating, roll coating, spray coating, dip coating, and screen printing are known, and are used for forming each layer of the laminated structure constituting the device, surface treatment, etc. In addition, a method of applying the raw material of the film constituting the electron transport layer in a paste form has also been disclosed (Non-Patent Documents 1 and 2).
[0004] However, with these coating methods, it is difficult to uniformly form a dense, thin film that constitutes a solar cell, and even if a thin, uniform film can be formed, it is particularly difficult to form a dense film. Therefore, it is generally believed that films formed by coating methods do not have sufficient transparency. [Prior art documents] [Non-patent literature]
[0005] [Non-Patent Document 1] K Tennakone et al J. Phys. D: Appl. Phys. 1999, 32, 374 [Non-Patent Document 2] N Jamalullail et al. IOP Conf. Ser.:Mater. Sci. Eng. 2018, 374 012048 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing a zinc oxide thin film that enables a dense and transparent zinc oxide thin film to be produced easily at low cost, and a method for producing a solar cell having this zinc oxide thin film as an electron transport layer. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention employs the following means.
[0008] (1) A method for producing a zinc oxide thin film according to one embodiment of the present invention includes a mixture preparation step of preparing a mixture containing ethanol, nitric acid, and zinc oxide, a mixture application step of applying the mixture to a surface of a substrate, and a mixture heating step of heating the mixture applied to the surface of the substrate, thereby converting the mixture into a liquid.
[0009] (2) In the zinc oxide thin film described in (1) above, in the mixture preparation step, the ratio of the mass of the ethanol to the total mass of the ethanol and the nitric acid is preferably 60% or more and 80% or less.
[0010] (3) In the zinc oxide thin film described in either (1) or (2) above, the ratio of the mass of the zinc oxide to the mass of the mixture in the mixture preparation step is preferably 0.9% or more and 1.1% or less.
[0011] (4) In the method for producing a zinc oxide thin film described in any one of (1) to (3) above, it is preferable that the mixture is made to contain water in the mixture preparation step, and the ratio of the mass of the water to the mass of the mixture is 11% or more and 13% or less.
[0012] (5) In the method for producing a zinc oxide thin film described in any one of (1) to (4) above, it is preferable that the mixture is applied by a spin coating method in the mixture application step, and the rotation speed of the base material in the spin coating method is 2500 rpm or more and 3500 rpm or less.
[0013] (6) In the method for producing a zinc oxide thin film according to any one of (1) to (5) above, the mixture is preferably heated to a temperature of 340° C. or higher and 360° C. or lower in the mixture heating step.
[0014] (7) In the method for producing a zinc oxide thin film described in any one of (1) to (6) above, it is preferable to further include an oxygen plasma treatment step of performing an oxygen plasma treatment on the surface of the base material before the mixture application step.
[0015] (8) A method for manufacturing a solar cell according to one embodiment of the present invention is a method for manufacturing a solar cell comprising laminating an anode layer, an electron transport layer, a power generation layer, a hole transport layer, and a cathode layer on a base material, the method using a transparent conductive substrate as the base material, and forming a film made of the mixture on the transparent conductive substrate by using the method for manufacturing a zinc oxide thin film described in either (1) or (2) above, thereby forming the electron transport layer. Effect of the Invention
[0016] According to the present invention, it is possible to provide a method for producing a zinc oxide thin film that enables a dense and transparent zinc oxide thin film to be produced easily at low cost, and a method for producing a solar cell that includes this zinc oxide thin film as an electron transport layer. [Brief description of the drawings]
[0017] [Figure 1] 1(a) to 1(c) are diagrams illustrating a method for producing a zinc oxide thin film according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a side view of a solar cell having, as an electron transport layer, the zinc oxide thin film obtained by the zinc oxide thin film manufacturing method of the embodiment. [Diagram 3] 1(a) to 1(c) are diagrams comparing the structures of zinc oxide thin films formed from different materials. [Figure 4] Photographs of the mixtures obtained in Comparative Examples 1 to 4 and Example 1 are shown in (a) to (e). [Diagram 5] 1 is an enlarged SEM image of a portion of the zinc oxide thin film obtained in Comparative Example 3. [Figure 6] 1 is an enlarged SEM image of a portion of the zinc oxide thin film obtained in Comparative Example 4. [Figure 7] 1 is an enlarged SEM image of a portion of the zinc oxide thin film obtained in Example 1. [Figure 8] 1(a) to 1(c) are enlarged SEM images of parts of the zinc oxide thin films obtained in Comparative Examples 3 and 5 and Example 1. [Figure 9] 1(a) to 1(d) are enlarged SEM images of parts of the zinc oxide thin films obtained in Comparative Examples 6 to 8 and 4. [Figure 10] 1 is a graph showing X-ray diffraction patterns for the zinc oxide thin films obtained in Examples 1 to 3. [Figure 11] 1 is a graph showing electromagnetic wave absorption spectra for zinc oxide thin films of Comparative Examples 3 and 4 and Example 1. [Figure 12] 1 is a graph showing current-voltage characteristics for solar cells provided with zinc oxide thin films of Comparative Examples 3 and 4 and Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, the manufacturing method of the zinc oxide thin film and the manufacturing method of the solar cell according to the embodiment of the present invention will be described in detail with reference to the drawings. Note that the drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the characteristics easier to understand, and the dimensional ratios of each component may not necessarily be the same as in reality. In addition, the materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto, and may be appropriately modified and implemented within the scope of the present invention.
[0019] <Method of manufacturing zinc oxide thin film> 1(a) to 1(c) are diagrams illustrating a method for producing a zinc oxide thin film according to one embodiment of the present invention. The method for producing a zinc oxide thin film of this embodiment mainly includes a mixture preparation step, a mixture application step, and a mixture heating step. Each step will be described.
[0020] (Mixture preparation process) As shown in FIG. 1(a), zinc oxide (ZnO) powder A, an ethanol (C2H6O) solution B, and a nitric acid (HNO3) solution C are placed in a specified container 10 and stirred and mixed at a specified temperature to produce a mixture 11 containing zinc oxide, ethanol, and nitric acid.
[0021] The ratios of zinc oxide, ethanol, and nitric acid contained in the mixture are adjusted so that the mixture to be prepared becomes a liquid. The liquid in this embodiment is a mixture in which the same type of solid particles are uniformly (homogenously) distributed therein, and is different from a paste (suspension) in which different types of solid particles are non-uniformly dispersed therein.
[0022] The order of mixing powder A, solution B, and C is not limited. Powder A, solution B, and C may be mixed simultaneously, or two of powder A, solution B, and C may be mixed first, and then the remaining one may be added and mixed.
[0023] The amounts of powder A, solutions B, and C contained in container 10 are adjusted taking into consideration the mass ratios of zinc oxide, ethanol, and nitric acid in mixture 11. That is, the amounts of solutions B and C contained in container 10 are adjusted so that the ratio of the mass of ethanol to the total mass of ethanol and nitric acid is 60% or more and 80% or less, preferably 65% or more and 75% or less, and most preferably 70%. The average particle size of powder A is preferably 0.5 μm or more and 5 μm or less.
[0024] In addition, the amounts of powder A, solutions B, and C contained in container 10 are adjusted so that the ratio of the mass of zinc oxide contained in mixture 11 to the mass of mixture 11 after preparation is 0.9% or more and 1.1% or less, preferably 0.95% or more and 1.05% or less, and most preferably 1%.
[0025] Water may be added to the mixture 11 during the process of mixing the powder A and the solutions B and C. The mass ratio of this water to the mass of the mixture 11 is preferably 11% or more and 13% or less, and most preferably 12%. In this case, the water may be water that is originally contained in the solutions B and C, or water that is newly added during the mixture preparation process.
[0026] (Mixture application process) Next, as shown in FIG. 1(b), the prepared mixture 11 is applied onto one surface 12a of a given base material (substrate) 12. The one surface 12a is preferably flat, but may be curved. Before applying the mixture 11, the method may further include a step of performing an oxygen plasma treatment (oxygen plasma treatment step) on the surface of the base material 12 for the purpose of cleaning. This oxygen plasma treatment can clean the surface of the base material 12 and improve the wettability of the surface of the base material 12 with respect to the mixture 11.
[0027] The substrate 12 is not particularly limited, and examples thereof include those made of glass, silicon, metals such as iron, gold, and copper. The substrate 12 may be a plate-shaped member or a film. A conductive layer (conductive film) may be formed on the surface of the substrate 12. When used as a base substrate for a solar cell, it is preferable to use a substrate such as glass that transmits light (transparent conductive substrate).
[0028] Here, the case where the spin coating method that can be performed in the atmosphere is used as the coating method of the mixture 11 is exemplified, but other coating methods may be used. Examples of other coating methods include bar coating, roll coating, spray coating, dip coating, and screen printing. The spin coating method is the most preferable coating method in this embodiment because it allows easy fine adjustment of the thickness and quality of the film formed by parameters such as the rotation speed and rotation time of the substrate.
[0029] In the spin coating method, a predetermined spin coating device (not shown) is used to apply (drop) the mixture 11 onto one surface 12a of the substrate 12 while rotating the substrate 12 from a nozzle 13 fixed at a predetermined position, forming a thin film (zinc oxide thin film) 11A made of the mixture 11. The parameters of the spin coating method are adjusted so that the thin film 11A has a desired thickness and film quality. For example, when the thickness of the thin film 11A is set to 60 nm to 65 nm, the rotation speed of the substrate 12 is preferably 2500 rpm or more and 3500 rpm or less, more preferably 3000 rpm, the rotation time of the substrate 12 is preferably 25 s or more and 35 s or less, and the temperature during application of the mixture is preferably 190° C. or more and 210° C. or less. In the spin coating method, the centrifugal force generated by the rotation of the substrate 12 is used to spread the applied mixture 11 over the entire surface 12a of the substrate. From the viewpoint of spreading the mixture evenly over the entire surface 12a, the shape of the surface 12a may be circular.
[0030] (Mixture heating process) Next, as shown in FIG. 1(c), a predetermined heating furnace 14 is used to heat and dry the mixture 11 applied to one surface 12a of the substrate. The heating here is intended to sinter and densify the thin film 11A. The substrate 12 to which the mixture 11 is applied is placed in a heating furnace (heating chamber) 14, the inside of the heating furnace 14 is reduced in pressure to 1 atm or less, and the mixture 11 is heated together with the substrate 12 using a heating means (not shown). The heating means is not particularly limited, but examples thereof include a heater, a beam irradiation device, and an induction heating coil. The heating temperature is preferably 340° C. or more and 360° C. or less, more preferably 345° C. or more and 355° C. or less, and most preferably 350° C. The heating time is preferably 80 minutes or more and 120 minutes or less, and more preferably 90 minutes or more and 110 minutes or less.
[0031] In the method for producing a zinc oxide thin film of this embodiment, the ratio of zinc oxide, ethanol, nitric acid, etc. contained in the mixture used as a raw material for the zinc oxide thin film is adjusted so that the mixture becomes a liquid. Through this adjustment, the produced zinc oxide thin film becomes a dense film with high transparency. The zinc oxide thin film of this embodiment can uniformly cover the surface of the substrate that serves as the base. In addition, since the zinc oxide thin film of this embodiment can be produced by a coating method, the production cost can be kept low compared to when produced by other methods.
[0032] <Solar cell manufacturing method> FIG. 2 is a perspective view of a solar cell 100 according to this embodiment. The solar cell 100 can be manufactured by using the above-mentioned manufacturing method of a zinc oxide thin film. Specifically, an electron transport layer 102 made of a zinc oxide thin film is formed on a part of one surface 101a of a base material 101 by using the manufacturing method of a zinc oxide thin film. Furthermore, a power generation layer (photoelectric conversion layer) 103, a hole transport layer 104, and a positive electrode layer 105 are formed (laminated) in this order on the electron transport layer 102. In addition, a negative electrode layer 106 is formed on another part of one surface 101a of the transparent substrate so as to be in contact with the electron transport layer 102. The configuration (laminated structure) of the solar cell shown in FIG. 2 is one example, and other configurations may be used as long as the solar cell operates.
[0033] The substrate 101 is not particularly limited as long as it supports the structure composed of the above-mentioned layers. The substrate 101 is preferably a transparent conductive substrate with excellent light transmittance, and more preferably has a visible light transmittance of 90% or more. The substrate 101 is also preferably flexible. Examples of materials constituting the substrate 101 include glass and plastic film. Examples of resins constituting the plastic film include polyethylene terephthalate and polyethylene naphthalate.
[0034] The power generation layer 103 is a layer that receives light and generates power. The power generation layer 103 includes a donor and an acceptor. The power generation layer 103 may be a layer in which the donor and the acceptor are mixed (bulk heterostructure), or may be a layer in which a donor layer and an acceptor layer are stacked (stacked structure). The power generation layer 103 may be composed of a perovskite-type material. The donor absorbs light and becomes excited. The excited exciton moves to the interface between the donor and the acceptor. When the exciton transfers an electron to the acceptor, the donor generates a cation (hole), and the acceptor generates an anion. The cations and anions flow toward different electrodes, causing a current to flow in an external circuit.
[0035] The donor is, for example, a p-type organic semiconductor. A known donor can be used. The donor can be, for example, a conjugated polymer, a phthalocyanine derivative, a porphyrin derivative, a triarylamine derivative, a carbazole derivative, an oligothiophene derivative, or the like. For example, poly(3-hexylthiophene-2,5-diyl) (P3HT) is a conjugated polymer and is used as the donor.
[0036] The acceptor is, for example, an n-type organic semiconductor. The acceptor may be a known one, and may be a non-fullerene-based compound or a fullerene-based compound. The acceptor of the fullerene-based compound is, for example,
[60] PCBM, bis-
[60] PCBM,
[70] PCBM, bis-
[70] PCBM, etc. In addition, a fullerene derivative having a silylmethyl group (SIMEF) is also an example of the acceptor of the fullerene-based compound. The acceptor of the non-fullerene-based compound is, for example, a TTBT-based compound, an ITIC-based compound, an IDT-based compound, an IDTT-based compound, a TTCTT-based compound, PPhTQ, a low band gap material (Y6, Y7, etc.), etc.
[0037] The electron transport layer 102 is a layer that collects electrons generated in the power generation layer 103 and efficiently transports them toward the negative electrode layer 106. Examples of materials constituting the electron transport layer 102 include inorganic materials such as zinc oxide, titanium oxide, tin oxide, niobium oxide, and aluminum oxide, as well as inorganic materials such as PCBM and fullerene C. 60 Examples of n-type semiconductors include organic materials such as those mentioned above.
[0038] The hole transport layer 104 is a layer that collects holes generated in the power generation layer 103 and efficiently transports them toward the positive electrode layer 105. Examples of materials constituting the hole transport layer 102 include p-type semiconductors such as inorganic materials such as nickel oxide, copper iodide, copper oxide, and copper sulfide, and organic materials such as Spiro-OMeTAD, PTAA, and PEDOT:PSS (a composite of poly(3,4-ethylenedioxythiophene) (PEDOT) and polystyrene sulfonic acid (PSS)).
[0039] The positive electrode layer 105 is made of a conductive material such as a metal such as gold, silver, or aluminum, or an organic conductive ink such as PEDOT:PSS, etc. The negative electrode layer 106 is made of a conductive material such as indium tin oxide (ITO), indium zinc oxide (IZO), aluminum zinc oxide (AZO), zinc oxide, tin oxide, titanium oxide, graphene, etc.
[0040] 3(a) to (c) are diagrams showing schematic diagrams of a solar cell in which a zinc oxide thin film (electron transport layer) 11A, a power generation layer 15, a hole transport layer 16, and a positive electrode layer 17 are formed in this order on a substrate 12. The structures of zinc oxide thin film 11A formed from different raw materials as the electron transport layer of the solar cell and the behavior when sunlight L is irradiated on power generation layer 15 are compared.
[0041] FIG. 3(a) shows a schematic diagram of a zinc oxide thin film obtained when a mixture not containing nitric acid is used as a raw material. FIG. 3(b) shows a schematic diagram of a zinc oxide thin film obtained when a mixture not containing ethanol is used as a raw material. The zinc oxide thin film 11A obtained in these cases does not uniformly cover the surface of the substrate 12 and has many pinholes. Therefore, holes (carriers) generated in the power generation layer 15 leak through the pinholes to the negative electrode (not shown), resulting in a loss of current. Therefore, it is difficult to obtain high output from these solar cells.
[0042] FIG. 3(c) shows a schematic diagram of the structure of a zinc oxide thin film obtained when a mixture containing both ethanol and nitric acid is used as the raw material. The zinc oxide thin film obtained in this case uniformly covers the surface of the substrate, is dense, and has no pinholes. Therefore, in this case, it is possible to prevent holes (carriers) generated in the power generation layer 15 from leaking to the negative electrode (not shown), thereby preventing current loss. Therefore, with this solar cell, it is possible to obtain high output.
[0043] As described above, the zinc oxide thin film obtained in this embodiment is dense and highly transparent, and therefore when used as an electron transport layer of a solar cell, it can prevent leakage of holes generated in the power generation layer and realize excellent output characteristics. According to the method for producing a solar cell of this embodiment, the electron transport layer is formed by a coating method, so that the solar cell can be easily produced at low cost. Furthermore, the solar cell obtained in this embodiment can realize output characteristics equivalent to those of a solar cell in which a vapor deposition method is used to form the electron transport layer. EXAMPLES
[0044] The effects of the present invention will be more clearly understood by the following examples. Note that the present invention is not limited to the following examples, and can be modified as appropriate without departing from the spirit and scope of the present invention.
[0045] Example 1 Using the method for producing a zinc oxide thin film according to the above embodiment, a zinc oxide thin film was produced on one surface of a substrate in the following procedure.
[0046] In the mixture preparation process, 0.7 ml of ethanol solution and 0.3 ml of nitric acid solution were mixed first, and then 10 mg of zinc oxide powder (average particle size: about 1 μm) was added and mixed to prepare 930 mg of mixture. The ratio of the mass of ethanol to the total mass of ethanol and nitric acid in the mixture was set to 70%.
[0047] In the mixture application process, a TCO glass substrate was used as the base material, and 930 mg of the prepared mixture was applied to one surface of the TCO glass substrate by spin coating in five separate applications. In each application, the rotation speed of the substrate during spin coating was 3000 rpm, and the rotation time was 30 minutes.
[0048] In the mixture heating step, the mixture applied to the substrate was heated at 350° C. for 60 minutes in a heating furnace to form a zinc oxide thin film. The formed zinc oxide thin film had a thickness of 60 nm.
[0049] Example 2 A zinc oxide thin film was produced in the same manner as in Example 1, except that the heating temperature in the mixture heating step was 200°C.
[0050] Example 3 A zinc oxide thin film was produced in the same manner as in Example 1, except that the heating temperature in the mixture heating step was 300°C.
[0051] Comparative Example 1 A zinc oxide thin film was prepared in the same manner as in Example 1, except that in the mixture preparation step, 1 ml of a chloroform (CHCl3) solution was used instead of a mixture of ethanol and nitric acid.
[0052] Comparative Example 2 A zinc oxide thin film was prepared in the same manner as in Example 1, except that in the mixture preparation step, 1 ml of a methanol (CH3OH) solution was used instead of a mixture of ethanol and nitric acid.
[0053] Comparative Example 3 A zinc oxide thin film was prepared in the same manner as in Example 1, except that in the mixture preparation step, 1 ml of an ethanol solution not containing nitric acid was used instead of a mixture of ethanol and nitric acid.
[0054] Comparative Example 4 A zinc oxide thin film was prepared in the same manner as in Example 1, except that in the mixture preparation step, 1 ml of a nitric acid solution not containing ethanol was used instead of a mixture of ethanol and nitric acid.
[0055] Comparative Example 5 A zinc oxide thin film was prepared in the same manner as in Example 1, except that in the mixture prepared in the mixture preparation step, the ratio of the mass of ethanol to the total mass of ethanol and nitric acid was set to 90%.
[0056] Comparative Example 6 A zinc oxide thin film was prepared in the same manner as in Example 1, except that in the mixture prepared in the mixture preparation step, the ratio of the mass of ethanol to the total mass of ethanol and nitric acid was set to 50%.
[0057] Comparative Example 7 A zinc oxide thin film was prepared in the same manner as in Example 1, except that in the mixture prepared in the mixture preparation step, the ratio of the mass of ethanol to the total mass of ethanol and nitric acid was set to 30%.
[0058] Comparative Example 8 A zinc oxide thin film was prepared in the same manner as in Example 1, except that in the mixture prepared in the mixture preparation step, the ratio of the mass of ethanol to the total mass of ethanol and nitric acid was set to 10%.
[0059] 4(a)-(e) are photographs of the mixtures prepared in the mixture preparation steps of Comparative Examples 1-4 and Example 1, respectively, contained in transparent bottles. The mixtures of Comparative Examples 1-3 are cloudy, whereas the mixtures of Comparative Example 4 and Example 1 are almost transparent. This result shows that at least nitric acid needs to be added to the mixture.
[0060] 5 to 7 are images (upper) of the entire zinc oxide thin film formed using the mixtures of FIG. 4(c) to (e) and images (lower) of a part of the zinc oxide thin film enlarged, respectively. From the image in FIG. 5, it can be seen that in Comparative Example 3, in which a mixture not containing nitric acid was used, zinc oxide particles aggregated at multiple places in the zinc oxide thin film, and a uniform and dense zinc oxide thin film was not obtained. Also, from the image in FIG. 6, it can be seen that in Comparative Example 4, in which a mixture not containing ethanol was used, pinholes extending in the thickness direction were formed at multiple places in the zinc oxide thin film, and a uniform and dense zinc oxide thin film was not obtained. On the other hand, from the image in FIG. 7, it can be seen that in Example 1, in which a mixture containing both nitric acid and ethanol was used, a uniform and dense zinc oxide thin film was obtained throughout the zinc oxide thin film.
[0061] 8(a)-(c) and 9(a)-(d) are magnified images (SEM images) of a part of the zinc oxide thin film formed using the mixtures of Comparative Example 3, Example 1, Comparative Examples 6-8, and 4, respectively. Comparing Figs. 8(a)-(c) shows that as the ratio of the mass of ethanol to the total mass of ethanol and nitric acid becomes higher than 70%, the aggregation of particles in the zinc oxide thin film progresses and the denseness of the zinc oxide thin film is lost. Comparing Figs. 8(c) and 9(a)-(d) shows that as the ratio becomes lower than 70%, the number of pinholes and cracks generated in the zinc oxide thin film increases and the denseness of the zinc oxide thin film is lost.
[0062] FIG. 10 is a graph showing X-ray diffraction patterns of the zinc oxide thin films obtained in Examples 1 to 3. In the X-ray diffraction pattern of the zinc oxide thin film prepared at a heating temperature of 200° C. in the mixture heating step, many peaks of impurities other than zinc oxide are observed, which indicates that zinc oxide molecules are not sufficiently incorporated in the zinc oxide thin film. In the X-ray diffraction patterns of the zinc oxide thin films prepared at heating temperatures of 300° C. and 350° C., peaks corresponding to the crystal planes (100), (002), (101), (102), (110), and (103) of zinc oxide are observed, and the number of peaks of impurities is reduced, which indicates that zinc oxide molecules are sufficiently incorporated in the zinc oxide thin film. From these results, it is understood that the heating temperature of the mixture is preferably in the range of 300° C. or more and 350° C. or less.
[0063] FIG. 11 is a graph showing the electromagnetic wave absorption spectra of the zinc oxide thin films obtained in Comparative Examples 3 and 4 and Example 1. The zinc oxide thin film of Comparative Example 3 shows high absorptance for light (electromagnetic waves) in the wavelength region of 400 nm or more. This is believed to be because most of the light generated in the power generation layer cannot pass through the ethanol in the zinc oxide thin film constituting the electron transport layer, and remains in the power generation layer and is absorbed. The zinc oxide thin films of Comparative Example 4 and Example 1 show low absorptance for light in the same wavelength region. This is believed to be because most of the light generated in the power generation layer passes through the zinc oxide thin film constituting the electron transport layer and is sent to the negative electrode layer.
[0064] Using the zinc oxide thin films obtained in Comparative Examples 3 and 4 and Example 1, solar cells as shown in Fig. 2 were fabricated. A power generation layer, a hole transport layer, and a positive electrode layer were formed on the zinc oxide thin film (electron transport layer). In addition, a negative electrode layer was formed on one side of the TCO glass substrate so as to be in contact with the zinc oxide thin film. The main constituent materials of each layer of the solar cell were as follows. Substrate: Glass Negative electrode layer: ITO Electron transport layer: zinc oxide Power generation layer: P3HT, PCBM Hole transport layer: PEDOT, PSS Positive electrode layer: Gold
[0065] 12 is a graph showing the current-voltage characteristics of solar cells including the zinc oxide thin films obtained in Comparative Examples 3 and 4, and Example 1. The horizontal and vertical axes of the graph respectively show the voltage and current density generated between the positive and negative electrode layers.
[0066] The solar cells equipped with the zinc oxide films of Comparative Examples 3 and 4 did not obtain sufficient current-voltage characteristics. This is because the coverage of the zinc oxide film on the substrate was low, and the holes generated in the power generation layer were not blocked sufficiently, so the holes that would become carriers flowed into the substrate or through the substrate to the negative electrode layer.
[0067] On the other hand, sufficient current-voltage characteristics were obtained in the solar cell equipped with the zinc oxide film of Example 1. This is because the coverage of the zinc oxide film on the substrate is high, the zinc oxide thin film is dense and uniform, the resistance of the interface with the power generation layer is reduced, and the flow (transport) of electrons as carriers is activated. [Industrial Applicability]
[0068] The zinc oxide thin film of the present invention can be applied to various technical fields such as perovskite solar cells, organic solar cells, light-emitting diodes, ultraviolet sensors, biosensors, photodetectors, and thin film transistors. [Explanation of symbols]
[0069] 10...container 11...Mixture 11A...Thin film 12...Base material 12a...One side of the substrate 13 Nozzle 14...Heating furnace A Powder B, C...solution 100...Solar cells 101... Substrate 101a: One side of the board 102...electron transport layer 103 Power generation layer 104...Hole transport layer 105 Positive electrode layer 106 Negative electrode layer
Claims
1. A mixture preparation step of preparing a mixture containing ethanol, nitric acid, and zinc oxide; A mixture application step of applying the mixture to a surface of a substrate; A mixture heating step of heating the mixture applied to the surface of the base material, A method for producing a zinc oxide thin film, comprising: making the mixture into a liquid.
2. 2. The method for producing a zinc oxide thin film according to claim 1, wherein in the mixture preparation step, a ratio of the mass of the ethanol to a total mass of the ethanol and the nitric acid is 60% or more and 80% or less.
3. 3. The method for producing a zinc oxide thin film according to claim 1, wherein in the mixture preparation step, the ratio of the mass of the zinc oxide to the mass of the mixture is 0.9% or more and 1.1% or less.
4. In the mixture preparation step, water is added to the mixture, 3. The method for producing a zinc oxide thin film according to claim 1, wherein the ratio of the mass of the water to the mass of the mixture is 11% or more and 13% or less.
5. In the mixture application step, the mixture is applied by a spin coating method; 3. The method for producing a zinc oxide thin film according to claim 1, wherein the rotation speed of the substrate in the spin coating method is 2500 rpm or more and 3500 rpm or less.
6. 3. The method for producing a zinc oxide thin film according to claim 1, wherein the mixture is heated to a temperature of 340° C. or more and 360° C. or less in the mixture heating step.
7. 3. The method for producing a zinc oxide thin film according to claim 1, further comprising an oxygen plasma treatment step of performing an oxygen plasma treatment on the surface of the substrate before the mixture application step.
8. A method for manufacturing a solar cell including laminating an anode layer, an electron transport layer, a power generation layer, a hole transport layer, and a cathode layer on a substrate, comprising the steps of: A transparent conductive substrate is used as the base material, 3. A method for producing a solar cell, comprising forming a film of the mixture on the transparent conductive substrate by using the method for producing a zinc oxide thin film according to claim 1, thereby forming the electron transport layer.