Electrolyte, electrode additive, electrode, and lithium ion secondary battery
By integrating lithium ion conductive glass ceramic powder and specific lithium salts into the electrolyte, the batteries achieve improved input/output characteristics and capacity retention, addressing the limitations of existing glass-ceramic composite electrolytes in lithium ion secondary batteries.
Patent Information
- Application Number
- JP2023048705
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-07
AI Technical Summary
Existing lithium ion secondary batteries using glass-ceramic composite electrolytes still face issues with input/output characteristics and battery capacity maintenance after charge/discharge cycles, particularly in high-temperature environments, and there is a need for improved reliability and stability against hydrolysis-induced HF generation.
Incorporating lithium ion conductive glass ceramic powder with specific compositions and particle sizes into the electrolyte, along with a lithium salt and ion-conductive polymer, to enhance ionic conductivity and suppress HF generation, thereby improving electrode stability and battery performance.
The proposed solution results in lithium ion secondary batteries with enhanced input/output characteristics and improved battery capacity retention rates after charge/discharge cycles, even in high-temperature conditions, by effectively suppressing HF generation and electrode deterioration.
Smart Images

Figure 2024137256000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to an electrolyte, an electrode additive, and an electrode. Furthermore, the present invention relates to a lithium ion secondary battery including the electrolyte, the electrode additive, or the electrode. [Background technology]
[0002] Conventionally, rechargeable lithium-ion secondary batteries with high energy density have been widely used for applications such as power sources for electric vehicles and mobile devices. Most of the lithium-ion secondary batteries currently available on the market generally use liquid electrolytes (electrolytic solutions) such as organic solvents to achieve high energy densities. These electrolytes are made by dissolving lithium salts in non-aqueous solvents such as carbonate esters and cyclic esters.
[0003] However, lithium-ion secondary batteries using such flammable organic electrolytes have problems such as leakage and fire due to heat generation, and various improvements have been attempted. One of these is lithium secondary batteries using polymer electrolytes. In lithium secondary batteries using polymer electrolytes, the liquid electrolyte is retained in the polymer electrolyte, making it possible to reduce the amount of electrolyte and reduce leakage.
[0004] Since such polymer electrolytes have low lithium ion conductivity, it has been proposed to further incorporate a lithium ion conductive inorganic compound into the polymer electrolyte to solve this problem. For example, Patent Documents 1 and 2 propose glass-ceramic composite electrolytes in which a nonaqueous electrolyte solution is impregnated into a medium containing lithium ion conductive glass-ceramic powder.
[0005] Furthermore, as a solution to the problem of heat generation and ignition in lithium ion secondary batteries due to a chemical reaction between an organic electrolyte solution and an electrode active material, Patent Document 3 proposes a technology in which an electrode contains a specific amount of a lithium ion conductive inorganic solid electrolyte, so that the electrode maintains a high capacity even when stored in a high-temperature environment or even when repeatedly charged and discharged. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Laid-Open No. 2001-15164 [Patent Document 2] Japanese Patent Application Laid-Open No. 2004-303738 [Patent Document 3] Japanese Patent Application Laid-Open No. 2008-117542 Summary of the Invention [Problem to be solved by the invention]
[0007] However, even the lithium-ion secondary batteries using the glass-ceramic composite electrolytes described in Patent Documents 1 and 2 have room for improvement in input / output characteristics and battery capacity maintenance after charge / discharge cycling. Furthermore, Patent Document 3 proposes a lithium-ion secondary battery with high reliability in high-temperature environments using electrodes containing a specific amount of glass ceramics, but there is still room for improvement in input / output characteristics and charge / discharge cycling at room temperature. In the present invention, the input / output characteristics refer to the capacity during high-current discharge relative to the capacity during low-current discharge when the discharge cutoff voltage is reached, or the capacity during high-current charge relative to the capacity during low-current charge when the charge cutoff voltage is reached, in a charge / discharge evaluation of a lithium-ion secondary battery. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems, and have surprisingly found that these problems are caused by the fact that, while the highly dissociated lithium salts used in lithium ion secondary batteries have high ionic conductivity, trace amounts of water present in the electrolyte are hydrolyzed to generate HF, which deteriorates the positive electrode material. Based on this finding, the present inventors have discovered that the above problems can be solved by blending, in the electrolyte, a lithium ion conductive glass-ceramic powder having a main crystalline phase of a specific composition and a small average particle size with an electrolyte solution containing a lithium salt of a specific composition. Based on this finding, the present inventors have completed the present invention.
[0009] That is, according to the present invention, the following inventions are provided. [1] Li 1+x+2y+z A x Ca y T 2-(x+y) Si z P 3-z O 12 (1) (In formula (1), A is at least one selected from the group consisting of Al, Ga, and Y, T is at least one selected from the group consisting of Ti, Ge, and Zr; (0≦x≦1, 0≦y≦1, 0≦z≦1, 0≦x+y≦1, 0≦x+2y+z≦2) A lithium ion conductive glass ceramic powder having a main crystalline phase represented by the formula (I) and an average particle size of 5 μm or less; LiMF m (C2F5) n (2) (In formula (2), M is at least one selected from the group consisting of P, B, Sb, Ta, and Nb, When M is P, Sb, Ta, or Nb, m+n=6, 3≦m≦6, 0≦n≦3; If M is B, then m+n=4, 2≦m≦4, 0≦n≦2. an electrolyte solution containing a lithium salt represented by Electrolytes, including: [2] The specific surface area of the glass ceramic powder is 1 m 2 / g or more. [3] The electrolyte according to [1] or [2], wherein the lithium salt is at least one selected from the group consisting of LiPF6, LiBF4, LiSbF6, LiTaF6, LiNbF6, LiBF3(C2F5), and LiPF3(C2F5)3. [4] The electrolyte according to any one of [1] to [3], further comprising an ion-conductive polymer. [5] A lithium ion secondary battery comprising a positive electrode, a negative electrode, and the electrolyte according to any one of [1] to [4]. [6] An additive used in an electrode of a lithium ion secondary battery, Li 1+x+2y+z A x Ca y T 2-(x+y) Si z P 3-z O 12 (1) (In formula (1), A is at least one selected from the group consisting of Al, Ga, and Y, T is at least one selected from the group consisting of Ti, Ge, and Zr; (0≦x≦1, 0≦y≦1, 0≦z≦1, 0≦x+y≦1, 0≦x+2y+z≦2) A lithium ion conductive glass ceramic powder having a main crystalline phase represented by the formula (I) and an average particle size of 5 μm or less; LiMF m (C2F5) n (2) (In formula (2), M is at least one selected from the group consisting of P, B, Sb, Ta, and Nb, When M is P, Sb, Ta, or Nb, m+n=6, 3≦m≦6, 0≦n≦3; If M is B, then m+n=4, 2≦m≦4, 0≦n≦2. and a lithium salt represented by 10. An electrode additive comprising: [7] The specific surface area of the glass ceramic powder is 1 m 2 / g or more. [8] The electrode additive according to [6] or [7], wherein the lithium salt is at least one selected from the group consisting of LiPF6, LiBF4, LiSbF6, LiTaF6, LiNbF6, LiBF3(C2F5), and LiPF3(C2F5)3. [9] The electrode additive according to any one of [6] to [8], further comprising an ion-conductive polymer.
[10] An electrode comprising an active material and the electrode additive according to any one of [6] to [9].
[11] A lithium ion secondary battery comprising an electrode containing an active material and the electrode additive according to any one of [6] to [9]. [Effects of the Invention]
[0010] According to the present invention, it is possible to provide an electrolyte, an electrode additive, and an electrode that can produce a lithium ion secondary battery that is excellent in input / output characteristics and in battery capacity maintenance after charge / discharge cycles. Furthermore, the present invention can provide a lithium ion secondary battery that is excellent in input / output characteristics and in battery capacity maintenance after charge / discharge cycles. [Brief explanation of the drawings]
[0011] [Figure 1] FIG. 10 is a diagram showing the results of measuring the impedance of laminate cells of Example 3 and Comparative Example 4. [Figure 2] FIG. 10 is a diagram showing the results of measuring the impedance of laminate cells of Comparative Examples 3 and 5. [Figure 3] FIG. 10 is a graph showing the results of measuring the discharge capacity of laminate cells of Example 3 and Comparative Example 4. [Figure 4] FIG. 10 is a diagram showing the measurement results of the discharge capacity of the laminate cells of Comparative Examples 3 and 5. [Figure 5] FIG. 10 is a graph showing the results of measuring the discharge capacity of the laminate cells of Example 5 and Comparative Example 10. [Figure 6] FIG. 10 is a graph showing the results of measuring the discharge capacity of the laminate cells of Comparative Examples 9 and 11. DETAILED DESCRIPTION OF THE INVENTION
[0012] (electrolyte) The electrolyte according to the present invention contains a lithium ion conductive glass ceramic powder and an electrolyte solution, and may further contain an ion conductive polymer. Each component will be described in detail below.
[0013] (Lithium ion conductive glass ceramic powder) Lithium ion conductive crystals that do not contain grain boundaries that inhibit ion conduction are advantageous in terms of ion conduction. Glass ceramics, in particular, have almost no voids or grain boundaries that inhibit ion conduction, so they have high ion conductivity and excellent chemical stability. Lithium ion conductive glass ceramic powders are also advantageous in terms of ease of production and cost.
[0014] Here, glass ceramics are materials obtained by heat-treating glass to precipitate a crystalline phase within a glass phase. They refer to materials composed of an amorphous solid and crystals, and further include materials in which the entire glass phase has undergone a phase transition to a crystalline phase, i.e., materials with a crystalline content (crystallinity) of 100% by mass. Even in 100% crystallized materials, glass ceramics have almost no voids between or within the crystal grains. In contrast, commonly known ceramics and sintered bodies inevitably contain voids and grain boundaries between or within the crystal grains due to their manufacturing process, and are therefore distinct from the glass ceramics of the present invention. In particular, with regard to ionic conductivity, the presence of voids and grain boundaries in ceramics results in values significantly lower than the conductivity of the crystal grains themselves. Controlling the crystallization process of glass ceramics can suppress the decrease in intercrystalline conductivity, making it easier to achieve conductivity comparable to the inherent conductivity of the crystal grains themselves.
[0015] The glass ceramic powder used in the present invention is represented by the following formula (1): Li 1+x+2y+z A x Ca y T 2-(x+y) Si z P 3-z O 12(1) (In formula (1), A is at least one selected from the group consisting of Al, Ga, and Y, T is at least one selected from the group consisting of Ti, Ge, and Zr; (0≦x≦1, 0≦y≦1, 0≦z≦1, 0≦x+y≦1, 0≦x+2y+z≦2) The main crystalline phase is represented by the formula:
[0016] In the above formula (1), X is preferably 0.05 or more, more preferably 0.1 or more, and even more preferably 0.2 or more. When X is equal to or greater than these numerical values, the amount of lithium can be increased to increase the conductivity. Furthermore, X is preferably 0.8 or less, more preferably 0.7 or less, and even more preferably 0.6 or less. When X is equal to or less than these numerical values, the stable crystal structure of the glass ceramic powder is maintained, the effect of suppressing HF generation is enhanced, electrode deterioration is suppressed, the input / output characteristics of the lithium ion secondary battery are improved, and the battery capacity retention rate after charge / discharge cycling can be improved. y is preferably 0.025 or more, more preferably 0.05 or more, and even more preferably 0.1 or more. When y is equal to or greater than these values, the amount of lithium can be increased to increase the conductivity. Furthermore, y is preferably 0.9 or less, more preferably 0.7 or less, and even more preferably 0.5 or less. When y is equal to or less than these values, the stable crystal structure of the glass ceramic powder is maintained, the effect of suppressing HF generation is enhanced, electrode deterioration is suppressed, the input / output characteristics of the lithium ion secondary battery are improved, and the battery capacity retention rate after charge / discharge cycling can be improved. z is preferably 0.05 or more, more preferably 0.1 or more, and even more preferably 0.2 or more. If z is at or above these numerical values, the amount of lithium can be increased to raise the conductivity. Also, z is preferably 0.9 or less, more preferably 0.8 or less, and even more preferably 0.7 or less. If z is at or below these numerical values, a stable crystal structure of the glass-ceramics powder can be maintained, the inhibitory effect on HF generation can be enhanced, deterioration of the electrode can be suppressed, the input / output characteristics of the lithium-ion secondary battery can be improved, and the battery capacity retention rate after charge / discharge cycles can be improved.
[0017] In the above formula (1), as one of the preferred embodiments, A is Al and T is Ti. For example, Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 ≤ x ≤ 0.4, 0 < y ≤ 0.6) as the main crystal phase, the glass-ceramics, in mol% in terms of oxides, Li2O: 10 - 25%, Al2O3: 0 - 15%, s TiO2: 25 - 50%, s SiO2: 0 - 15%, s P2O5: 26 - 40% s can be obtained by melting and then rapidly cooling a glass containing each of these components, and then heat-treating this glass to precipitate crystals.
[0018] The upper limit value of the average particle diameter (D 50 ) of the glass-ceramics powder is 5 μm or less, preferably 4 μm or less, and more preferably 3 μm or less. By setting the upper limit value of the average particle diameter to be at or below these numerical values, the specific surface area of the glass-ceramics powder increases, and the inhibitory effect on HF generation is high, so deterioration of the electrode can be suppressed, and the input / output characteristics of the lithium-ion secondary battery and the battery capacity retention rate after charge / discharge cycles can be improved. Also, the average particle diameter (D 50The lower limit of the average particle size is 0.01 μm or more, preferably 0.05 μm or more, and more preferably 0.1 μm or more. By setting the lower limit of the average particle size to these values or more, it is possible to improve the dispersibility in the electrode and the binding between electrode materials. The average particle size in the present invention is the D50 (cumulative 50% diameter) value measured by laser diffraction after dispersing the glass ceramic powder in ethanol or NMP using an ultrasonic bath to a solid content of approximately 0.05 wt%, and specifically, the value measured using a particle size analyzer, Microtrac MT3300EXII, manufactured by Nikkiso Co., Ltd. The average particle size is a value expressed on a volume basis.
[0019] The ionic conductivity of the glass ceramic powder is preferably 1×10 -5 S / cm or more, more preferably 1×10 -4 S / cm or more, and more preferably 1×10 -3 By setting the lower limit of the ionic conductivity to these values or more, the effect of suppressing HF generation is enhanced, electrode deterioration is suppressed, and the input / output characteristics of the lithium-ion secondary battery and the battery capacity retention rate after charge / discharge cycles can be improved. In the present invention, the ionic conductivity is measured by measuring the impedance (1 MHz to 0.1 Hz, ±10 mV, 25°C) using a potentio / galvanostat (SP-300 manufactured by Bio-Logic Science Instruments), calculating the resistance R (Ω) of the sample from the impedance measurement results, and calculating the resistance R (Ω) of the sample based on the thickness L (cm) of the sample and the electrode area S (cm 2 ) and the ionic conductivity σ (Scm -1 ) is the calculated value.
number
[0020] The lower limit of the specific surface area of the glass ceramic powder is preferably 1 m 2 / g or more, and more preferably 3m 2 / g or more, more preferably 5m 2 / g or more, and even more preferably 7m 2 / g or more, and most preferably 10m 2 By setting the lower limit of the specific surface area to these values or more, the effect of suppressing HF generation is enhanced, electrode deterioration is suppressed, and the input / output characteristics of the lithium ion secondary battery and the battery capacity retention rate after charge / discharge cycles can be improved. The upper limit of the specific surface area of the glass ceramic powder is preferably 200 m 2 / g or less, more preferably 100m 2 / g or less, and more preferably 80m 2 By setting the upper limit of the specific surface area to these numerical values or less, it is possible to improve the dispersibility within the electrode and improve the binding between the electrode materials. The specific surface area in the present invention is a value that represents the average value of values measured twice by the BET single-point method using a fully automatic specific surface area analyzer Macsorb HM-1201 manufactured by MOUNTECH.
[0021] The blending amount of the glass ceramic powder is preferably 5% by mass to 95% by mass, more preferably 10% by mass to 90% by mass, and even more preferably 15% by mass to 85% by mass, based on the total amount of the electrolyte. If the blending amount of the glass ceramic powder is within the above range, the structure of the electrolyte can be maintained while suppressing HF generation, thereby improving the input / output characteristics and the battery capacity retention rate after charge / discharge cycling.
[0022] (electrolyte) The electrolyte used in the present invention is a non-aqueous electrolyte containing a lithium salt having a specific composition and further containing an organic solvent.
[0023] (lithium salts) The lithium salt used in the present invention is represented by the following formula (2): LiMF m (C2F5) n (2) (In formula (2), M is at least one selected from the group consisting of P, B, Sb, Ta, and Nb, When M is P, Sb, Ta, or Nb, m+n=6, 3≦m≦6, 0≦n≦3; If M is B, then m+n=4, 2≦m≦4, 0≦n≦2. The lithium salt is represented by the formula:
[0024] In the above formula (2), when M is P, Sb, Ta, or Nb, m is preferably 3.5 or more, more preferably 4.0 or more, and even more preferably 5.0 or more. Also, m is preferably 5.5 or less, more preferably 5.9 or less, and even more preferably 5.8 or less. When M is B, m is preferably 2.5 or more, more preferably 3.0 or more, and even more preferably 3.5 or more. Also, m is preferably 3.95 or less, more preferably 3.9 or less, and even more preferably 3.8 or less. Lithium salts with m within these ranges are highly dissociated and are prone to hydrolysis and HF generation. When these salts are used in the present invention, the effect of suppressing HF generation is enhanced, electrode deterioration is suppressed, and the input / output characteristics of the lithium-ion secondary battery can be improved. When M is P, Sb, Ta, or Nb, n is preferably 0.05 or more, more preferably 0.1 or more, and even more preferably 0.2 or more, and preferably 2.5 or less, more preferably 2.0 or less, and even more preferably 1.0 or less. When M is B, n is preferably 0.05 or more, more preferably 0.1 or more, and even more preferably 0.2 or more, and preferably 1.5 or less, more preferably 1.0 or less, and even more preferably 0.5 or less. If n is within these numerical ranges, the salts are highly stable against hydrolysis, and therefore, when these salts are used in the present invention, electrode deterioration is suppressed and the input / output characteristics of the lithium secondary battery can be improved.
[0025] Examples of the lithium salt represented by the formula (2) include LiPF, LiBF, LiSbF, LiTaF, LiNbF, LiBF(C2F5), and LiPF(C2F5)3. Among these lithium salts, LiPF, LiBF, and LiSbF are preferred because they provide high ionic conductivity and a high degree of dissociation in the electrolyte, thereby enhancing the effect of suppressing HF generation, suppressing electrode deterioration, and improving the input / output characteristics of the lithium ion secondary battery. These lithium salts may be used alone or in combination of two or more.
[0026] The amount of the lithium salt blended is preferably 2% by mass or more and 40% by mass or less, more preferably 3% by mass or more and 30% by mass or less, and even more preferably 4% by mass or more and 20% by mass or less, based on the total amount of the electrolyte. If the amount of the lithium salt blended is within the above range, the shape of the electrolyte is maintained, the ionic conductivity of the electrolyte solution is increased, the effect of suppressing HF generation is enhanced, electrode deterioration is suppressed, and the input / output characteristics of the lithium ion secondary battery can be improved.
[0027] (organic solvent) The organic solvent used in the present invention is not particularly limited, and conventionally known organic solvents for electrolytic solutions can be used. Examples of organic solvents include carbonate-based, ester-based, ether-based, and ketone-based solvents. Specific examples include ethylene carbonate, propylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, sulfolane, 1,2-dimethoxyethane, dimethyl ether, and acetonitrile. These organic solvents may be used alone or in combination of two or more.
[0028] The blending amount of the organic solvent is preferably 5% by mass or more and 50% by mass or less, more preferably 10% by mass or more and 40% by mass or less, and even more preferably 15% by mass or more and 30% by mass or less, based on the total amount of the electrolyte. When the blending amount of the organic solvent is within the above range, the shape of the electrolyte is maintained, the ionic conductivity of the electrolyte solution is increased, the effect of suppressing HF generation is enhanced, deterioration of the electrodes is suppressed, and the input / output characteristics of the lithium ion secondary battery can be improved.
[0029] (ion-conducting polymer) The ion-conductive polymer used in the present invention is not particularly limited, and any conventionally known polymer having lithium ion conductivity can be used. However, a polymer that swells in an electrolyte solution containing a lithium salt and an organic solvent and exhibits high ion conductivity is preferred. Examples of ion-conductive polymers include polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyacrylonitrile, polyethylene oxide, polyacetylene, polydimethylsiloxane, and poly(vinylene carbonate-co-acrylonitrile). Among these ion-conductive polymers, polyvinylidene fluoride-hexafluoropropylene and polyacrylonitrile are preferred. These ion-conductive polymers may be used alone or in combination of two or more.
[0030] The amount of the ion-conductive polymer blended is preferably 5% by mass to 70% by mass, more preferably 7% by mass to 50% by mass, and even more preferably 10% by mass to 30% by mass, relative to the total amount of the electrolyte. When the amount of the ion-conductive polymer blended is within the above range, the electrolyte exhibits high ionic conductivity while maintaining its shape, electrode deterioration due to suppressed HF generation is suppressed, and input / output characteristics and the capacity retention rate after charge / discharge cycling can be improved.
[0031] The electrolyte can be made into a self-supporting membrane by molding a slurry made by mixing glass ceramic powder, an ion-conductive polymer, and a solvent in which the ion-conductive polymer dissolves into a sheet and drying the solvent. Alternatively, the slurry can be directly coated onto an electrode to form an electrolyte layer. The self-supporting membrane made of glass ceramic powder and an ion-conductive polymer or the electrolyte layer coated on an electrode can be impregnated with an electrolyte solution made of a lithium salt and an organic solvent and swelled after the solvent has been thoroughly dried, thereby maintaining the electrolyte shape and exhibiting high ionic conductivity.
[0032] The thickness of the electrolyte layer coated on the self-supporting membrane or electrode is preferably 1 μm to 50 μm, more preferably 2 μm to 40 μm, and even more preferably 3 μm to 30 μm. If the thickness of the electrolyte is within the above range, the electrolyte has enough strength to maintain its shape and exhibits high ionic conductivity, thereby improving the input / output characteristics of the battery.
[0033] (lithium-ion secondary battery) The lithium ion secondary battery of the present invention comprises a positive electrode, a negative electrode, and the above-described electrolyte. Each electrode contains an active material and may further contain an electrode additive. Each component will be described in detail below.
[0034] (positive electrode) The positive electrode is not particularly limited, and any conventionally known positive electrode for a lithium ion secondary battery can be used. The positive electrode is not particularly limited as long as it has a positive electrode active material, but for example, it includes a positive electrode current collector and a positive electrode active material layer provided on the surface of the positive electrode current collector. The positive electrode is disposed opposite the negative electrode.
[0035] The positive electrode current collector collects current from the positive electrode active material layer. The type of positive electrode current collector is not particularly limited, but examples include metal foils such as aluminum foil, perforated metal foils such as perforated aluminum foil, expanded metal, and foam metal plates. The material of the positive electrode current collector is not particularly limited, but examples include aluminum, stainless steel, and titanium. The shape and manufacturing method of the positive electrode current collector are not particularly limited, and any shape and manufacturing method may be used.
[0036] The positive electrode active material layer is not particularly limited as long as it contains a positive electrode active material, but may contain, for example, a positive electrode active material, a conductive agent, and a binder.
[0037] The positive electrode active material is a material into which lithium ions are desorbed during charging and into which lithium ions desorbed from the negative electrode active material in the negative electrode active material layer are inserted during discharging. The positive electrode active material is not particularly limited as long as it is a material capable of reversibly inserting and desorbing lithium ions. For example, a lithium-containing compound containing lithium ions as a reactive species is preferred. Examples of the lithium-containing compound include, but are not limited to, lithium cobalt oxide, manganese-substituted lithium cobalt oxide, lithium manganate, lithium nickel oxide, lithium iron phosphate, and lithium manganese phosphate.
[0038] The conductive agent improves the conductivity of the positive electrode active material layer. The conductive agent is not particularly limited, but examples thereof include ketjen black, acetylene black, and graphite.
[0039] The binder binds together the positive electrode active material, conductive agent, etc. Examples of binders include, but are not limited to, polyvinylidene fluoride, styrene-butadiene rubber, carboxymethyl cellulose, cellulose acetate, ethyl cellulose, fluororubber, ethylene-propylene rubber, polyacrylic acid, polyimide, and polyamide.
[0040] (Negative electrode) The negative electrode has a negative electrode current collector and a negative electrode active material layer provided on the surface of the negative electrode current collector facing the positive electrode.
[0041] The negative electrode current collector collects current from the negative electrode active material layer. The type of negative electrode current collector is not particularly limited, but examples include metal foils such as copper foil, perforated metal foils such as perforated copper foil, expanded metal, and foam metal plates. The material of the negative electrode current collector is not particularly limited, but examples include copper, stainless steel, and titanium, with copper being preferred. The shape and manufacturing method of the negative electrode current collector are not particularly limited, and any shape and manufacturing method may be used.
[0042] The negative electrode active material layer is not particularly limited as long as it contains a negative electrode active material, but may contain, for example, a negative electrode active material, a conductive agent, and a binder.
[0043] The negative electrode active material is a material into which lithium ions released from the positive electrode active material in the positive electrode active material layer during charging are inserted and into which lithium ions are released during discharging. The negative electrode active material is not particularly limited as long as it is capable of reversibly inserting and releasing lithium ions. Examples of the negative electrode active material include natural graphite, composite carbonaceous materials formed by coating natural graphite with a dry CVD method or a wet spray method, artificial graphite produced by firing resin materials such as epoxy and phenol, or pitch-based materials derived from petroleum or coal, silicon (Si), graphite mixed with silicon, non-graphitizable carbon materials, lithium titanate, and titanium niobium oxide. Metallic lithium, which deposits lithium ions during charging and dissolves them during discharging, can also be used as the negative electrode.
[0044] The conductive agent and binder may be the same as those used in the positive electrode active material layer.
[0045] (electrode additives) The additive used in the electrode of a lithium ion secondary battery is added to the above-mentioned positive electrode or negative electrode. The electrode additive contains a lithium ion conductive glass ceramic powder and a lithium salt, and may further contain an ion conductive polymer. The lithium ion conductive glass ceramic powder, lithium salt, and ion conductive polymer used in the electrode additive can be the same as the lithium ion conductive glass ceramic powder, lithium salt, and ion conductive polymer used in the above-mentioned electrolyte. The use of such an electrode additive has a high effect of suppressing HF generation, thereby suppressing electrode deterioration, improving the output / input characteristics of the lithium ion secondary battery, and improving the capacity retention rate after charge / discharge cycling.
[0046] The amount of the electrode additive blended is preferably 0.1% by mass or more and 20% by mass or less, more preferably 0.2% by mass or more and 15% by mass or less, and even more preferably 0.3% by mass or more and 10% by mass or less, based on the total amount of the electrode. When the amount of the electrode additive blended is within the above numerical range, electrode deterioration due to suppressed HF generation is suppressed without impairing the electronic conductivity in the electrode due to the conductive additive, and it is possible to improve input / output characteristics and the capacity retention rate after charge / discharge cycling. [Example]
[0047] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention should not be construed as being limited to the contents of the following examples.
[0048] (Production Example 1 of Lithium Ion Conductive Glass-Ceramic Powder) H3PO4, Al(PO3)3, Li2CO3, SiO2, and TiO2 were used as raw materials, and they were weighed and uniformly mixed so that the composition in terms of mol% of the oxides was 35.0% P2O5, 7.5% Al2O3, 15.0% Li2O, 38.0% TiO2, and 4.5% SiO2. Subsequently, this mixture was placed in a platinum pot and heated and melted in an electric furnace at 1500 °C for 4 hours while stirring the glass melt. Thereafter, the glass melt was dropped into running water to obtain flaky glass, and this glass was crystallized by heat treatment at 950 °C for 12 hours to obtain the target glass ceramics. The precipitated crystal phase was determined by powder X-ray diffraction to be Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 ≦ x ≦ 0.4, 0 < y ≦ 0.6) as the main crystal phase. Also, the ionic conductivity of this glass ceramics was about 1.0×10 -3 S / cm.
[0049] The flakes of the obtained glass ceramics were each pulverized by a laboratory-scale jet mill and classified by a zirconia rotary roller to obtain glass ceramics with an average particle size (D 50 ) of 20 μm. The obtained glass ceramics were pulverized in a dry bead mill to an average particle size (D<00_{}00059>) of 6 μm to obtain glass ceramics powder 1.
[0050] (Production Example 2 of Lithium Ion Conductive Glass Ceramics Powder) Subsequently, the glass ceramics powder 1 obtained above was pulverized under the same conditions with an extended pulverization time to an average particle size (D 50 ) of 1 μm to obtain glass ceramics powder 2. <00_{}00345>
[0051] (Production Example 3 of Lithium Ion Conductive Glass Ceramics Powder) Subsequently, the glass ceramics powder 2 obtained above was pulverized in a wet bead mill with ethanol as a solvent to an average particle size (D<00_{}00061>) The powder was pulverized to 0.4 μm and spray-dried to obtain glass ceramic powder 3.
[0052] (Production Example 1 of Non-Aqueous Electrolyte Solution) A non-aqueous electrolyte solution 1 was obtained by dissolving lithium hexafluorophosphate (LiPF6) at a concentration of 1 mol / L in a solvent prepared by mixing ethylene carbonate (EC) and diethyl carbonate (DEC) in a mass ratio of 1:1.
[0053] (Production Example 2 of Nonaqueous Electrolyte Solution) A non-aqueous electrolyte solution 2 was obtained by dissolving lithium hexafluorophosphate (LiPF6) at a concentration of 1 mol / L in a solvent prepared by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a mass ratio of 3:7.
[0054] (Production Example 3 of Nonaqueous Electrolyte Solution) A non-aqueous electrolyte solution 3 was obtained by dissolving lithium perchlorate (LiClO4) at a concentration of 1 mol / L in a solvent prepared by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a mass ratio of 3:7.
[0055] [Test Example 1] [Example 1] (Electrolyte Production Example 1-1) The glass ceramic powder 3 produced above was vacuum dried at 160°C for 24 hours. Then, the dried glass ceramic powder 3 was added to the non-aqueous electrolyte solution 1 produced above so that the concentration was 8 mass % to obtain an electrolyte. Next, the obtained electrolyte was stored at 60°C for 1 week, and then the H in the electrolyte was measured. + The concentration was evaluated by measuring the acid content. The evaluation results are shown in Table 1. + The concentration was assumed to be entirely from HF.
[0056] [Example 2] (Electrolyte Production Example 1-2) An electrolyte was obtained in the same manner as in Example 1, except that the glass ceramic powder 2 was used instead of the glass ceramic powder 3. Next, in the same manner as in Example 1, H+ The concentration was evaluated by measuring the acid content, and the evaluation results are shown in Table 1.
[0057] [Comparative Example 1] (Electrolyte Production Example 1-3) An electrolyte was obtained in the same manner as in Example 1, except that the glass ceramic powder 1 was used instead of the glass ceramic powder 3. Next, H in the electrolyte was + The concentration was evaluated by measuring the acid content, and the evaluation results are shown in Table 1.
[0058] Comparative Example 2 (Electrolyte Production Example 1-4) The same procedure as in Example 1 was carried out except that the glass ceramic powder 3 was not added and the nonaqueous electrolyte solution 1 was used as it was as the electrolyte. + The concentration was evaluated by measuring the acid content, and the evaluation results are shown in Table 1.
[0059] As shown in the results in Table 1, comparing Examples 1 and 2 with Comparative Example 1, adding a glass ceramic powder with a small average particle size and a large specific surface area to the electrolyte reduced the concentration of HF generated by hydrolysis of the electrolyte, and as a further effect, significantly suppressed the increase in HF concentration after high-temperature storage. Because the by-product HF deteriorates the positive electrode material, suppressing the increase in HF concentration extends the life of the positive electrode material, improving the input / output characteristics of the lithium-ion secondary battery while also improving the capacity retention rate after charge / discharge cycling.
[0060] [Table 1]
[0061] [Test Example 2] (Positive electrode manufacturing example 2-1) Using a mixer (manufactured by Thinky Corporation), lithium cobalt oxide (LiCoO2) (Cellseed C10, manufactured by Nippon Chemical Industry Co., Ltd.): acetylene black (AB) (Li-250, manufactured by Denka Co., Ltd.): polyvinylidene fluoride (PVdF)) (#1120, manufactured by Kureha Corporation): glass ceramic powder 3 were mixed in a weight ratio of 91:4:4:1 using N-methylpyrrolidone (NMP) as a solvent to obtain positive electrode slurry 2-1.
[0062] The obtained positive electrode slurry 2-1 was applied to a 20 μm aluminum current collector foil using a blade coater, and then dried at 120° C. The coated foil was then compressed using a roll press to a thickness of 55 μm and a density of 3.5 g / cm. 3 Subsequently, the mixture was cut into a size of 30 mm x 40 mm using a Thomson punching machine and vacuum dried at 160°C for 24 hours using a glass tube oven to prepare a positive electrode 2-1.
[0063] (Positive electrode manufacturing example 2-2) Using a mixer (manufactured by Thinky Corporation), LiCoO2:AB:PVdF were mixed in a weight ratio of 92:4:4 using NMP as a solvent to obtain a positive electrode slurry 2-2.
[0064] A positive electrode 2-2 was produced in the same manner as in Positive Electrode Production Example 2-1, except that the obtained positive electrode slurry 2-2 was used.
[0065] (Negative electrode manufacturing example 2-1) Using a mixer (made by Thinky Corporation), graphite and PVdF (made by Kureha Corporation, #9130) were mixed in a weight ratio of 90:10 using NMP as a solvent to obtain a negative electrode slurry 2-1.
[0066] The obtained negative electrode slurry 2-1 was applied to a 15 μm copper current collector foil using a blade coater, and then dried at 120° C. The negative electrode slurry 2-1 was then compressed using a roll press to a thickness of 50 μm and a density of 1.6 g / cm. 3 Subsequently, the mixture was cut into a size of 32 mm x 42 mm using a Thomson punching machine and vacuum dried at 160°C for 24 hours using a glass tube oven to prepare a negative electrode 2-1.
[0067] (Separator manufacturing example) A PP separator (manufactured by CSTech, P2010H) was cut into a size of 40 mm x 50 mm using a Thomson punching machine and vacuum dried in a glass tube oven at 60°C for 24 hours.
[0068] [Example 3] (Example of manufacturing a lithium-ion secondary battery cell) The electrode surfaces of the positive electrode 2-1 and the negative electrode 2-1 produced above were placed face to face, a separator was sandwiched between them, and the resultant was wrapped in an aluminum laminate. 0.3 ml of the nonaqueous electrolyte solution 2 obtained above was injected and vacuum impregnated for 30 seconds, and then the resultant was sealed to produce a lithium ion secondary battery cell.
[0069] Comparative Example 3 A lithium ion secondary battery cell was produced in the same manner as in Example 3, except that non-aqueous electrolyte solution 3 was used instead of non-aqueous electrolyte solution 2.
[0070] Comparative Example 4 A lithium ion secondary battery cell was produced in the same manner as in Example 3, except that the positive electrode 2-2 was used instead of the positive electrode 2-1.
[0071] Comparative Example 5 A lithium ion secondary battery cell was produced in the same manner as in Comparative Example 4, except that non-aqueous electrolyte solution 3 was used instead of non-aqueous electrolyte solution 2.
[0072] [Table 2]
[0073] (chemical treatment, degassing) After one charge-discharge cycle (4.35 V - 3.0 V) at 0.05 C, the laminate was opened once, and then vacuum degassed again for 30 seconds before being sealed.
[0074] (Evaluation Method 2-1) The lithium ion secondary battery cells of Example 3 and Comparative Examples 3 to 5 were adjusted to a state of charge of 50% of the discharge capacity, and the impedance of the laminated cells was measured (1 MHz to 0.1 Hz, ±10 mV, 25°C) using a potentio / galvanostat (SP-300 manufactured by Bio-Logic Science Instruments). The measurement results are shown in Figures 1 and 2.
[0075] (Evaluation result 2-1) Comparing the impedance of Example 3 (with glass ceramic powder 3 added) and Comparative Example 4 (without glass ceramic powder added), which used LiPF6 as the lithium salt, we confirmed that the addition of glass ceramic powder 3 reduced the arc on the low-frequency side, which corresponds to the charge transfer resistance, and thus confirmed a reduction in resistance. On the other hand, comparing the impedance of Comparative Example 3 (with glass ceramic powder added) and Comparative Example 5 (without glass ceramic powder added), which used LiClO4 as the lithium salt, we confirmed that the addition of glass ceramic powder did not reduce resistance. When LiPF6, which has high hydrolysis properties, is used, HF is generated, but when LiClO4, which has low hydrolysis properties, HF is not generated. It was confirmed that the combination of LiPF6 and glass ceramic powder in Example 3 suppressed the generation of HF and prevented the deterioration of the positive electrode material, thereby reducing the charge transfer resistance.
[0076] (Evaluation Method 2-2) The lithium-ion secondary battery cells of Example 3 and Comparative Examples 3 to 5 were charged and discharged using an Asuka Electronics charge-discharge tester in the following cycle: CC-CV charge (1C, 4.35V-0.05C cutoff) → rest (10 minutes) → CC discharge (1C, 3V cutoff) → rest (10 minutes), at 45°C. The discharge capacity was measured. The measurement results are shown in Figures 3 and 4.
[0077] (Evaluation result 2-2) Comparing the capacity retention rates of Example 3 (with glass ceramic powder 3 added) and Comparative Example 4 (without glass ceramic powder added), both of which used LiPF6 as the lithium salt, it was found that the addition of glass ceramic powder 3 suppressed the decrease in capacity retention rate after charge-discharge cycling. On the other hand, comparing the capacity retention rates of Comparative Example 3 (with glass ceramic powder 3 added) and Comparative Example 5 (without glass ceramic powder added), both of which used LiClO4 as the lithium salt, it was found that the addition of glass ceramic powder 3 did not suppress the decrease in the capacity retention rate of the battery after charge-discharge cycling. When LiPF6, which has high hydrolysis properties, is used, HF is generated, but when LiClO4, which has low hydrolysis properties, HF is not generated. The combination of LiPF6 and glass ceramic powder in Example 3 suppressed the generation of HF, which in turn suppressed the deterioration of the positive electrode material, thereby suppressing the decrease in capacity retention rate after charge-discharge cycling.
[0078] [Test Example 3] [Example 4] Using a mixer (Thinky Corporation), glass ceramic powder 3 and polyvinylidene fluoride-hexafluoropropylene (PVdF-HFP) were mixed in a weight ratio of 9:1 using acetone as a solvent to obtain a slurry. The resulting slurry was then applied to the surface of aluminum foil using a coater and dried at 60°C. The coating thickness was 20 μm. The foil was punched out using a hand punch Φ20 mm (Nogami Giken) and vacuum dried at 120°C for 24 hours using a glass tube oven. Subsequently, nonaqueous electrolyte solution 2 was added dropwise to impregnate the foil, and the foil was then incorporated into an HS cell (Hosen). The impregnation rate of nonaqueous electrolyte solution 2 was 30% of the total weight.
[0079] Comparative Example 6 A PP separator (CSTech, P2010H) was punched with a hand punch φ20 mm (Nogami Giken) using a Thomson punching machine, and then vacuum dried in a glass tube oven at 60 °C for 24 hours. Next, non-aqueous electrolyte 2 was added dropwise to impregnate the separator, and the separator was then incorporated into an HS cell (Hosen). The impregnation rate of non-aqueous electrolyte 2 was 60% of the total weight.
[0080] Comparative Example 7 The battery was assembled into an HS cell (manufactured by Hohsen) in the same manner as in Example 4, except that non-aqueous electrolyte solution 3 was used instead of non-aqueous electrolyte solution 2.
[0081] [Comparative Example 8] The battery was assembled into an HS cell (manufactured by Hohsen) in the same manner as in Comparative Example 6, except that non-aqueous electrolyte solution 3 was used instead of non-aqueous electrolyte solution 2.
[0082] (Evaluation Method 3-1) Impedance was measured (1 MHz to 0.1 Hz, ±10 mV, 25°C) using a potentio / galvanostat (SP-300 manufactured by Bio-Logic Science Instruments). The ionic conductivity (σ / Scm) was calculated from the relationship between the impedance measurement results (resistance corresponding to the minimum value on the lowest frequency side, or the x-axis intercept if there was no minimum value) and the sample thickness (20 μm) and electrode area (Φ20 mm). -1 The calculation results are shown in Table 3.
[0083] (Evaluation result 3-1) By impregnating a composite electrolyte containing glass ceramic powder 3 with a non-aqueous electrolyte solution containing LiPF6 as a lithium salt, the ionic conductivity could be improved. [Table 3]
[0084] [Test Example 4] (Positive Electrode Manufacturing Example 4-1) Using a mixer (manufactured by Thinky Corporation), lithium cobalt oxide (LiCoO) (Cellseed C10, manufactured by Nippon Chemical Industry Co., Ltd.):acetylene black (AB) (Li-250, manufactured by Denka Co., Ltd.):polyvinylidene fluoride (PVdF)) (#1120, manufactured by Kureha Corporation) were mixed in a weight ratio of 92:4:4 using N-methylpyrrolidone (NMP) as a solvent to obtain positive electrode slurry 4-1.
[0085] The obtained positive electrode slurry 4-1 was applied to a 20 μm aluminum current collector foil using a blade coater and then dried at 120 ° C., compacted using a roll press, and vacuum dried at 120 ° C. for 24 hours using a glass tube oven. Subsequently, the slurry was cut into a size of 30 mm × 40 mm using a Thomson punch to produce a positive electrode 4-1.
[0086] (Negative Electrode Manufacturing Example 4-1) Using a mixer (manufactured by Thinky Corporation), lithium titanate (LTO):AB:PVdF were mixed in a weight ratio of 88:5:7 using NMP as a solvent to obtain negative electrode slurry 4-1.
[0087] The obtained negative electrode slurry 4-1 was applied to a 20 μm aluminum current collector foil using a blade coater, and then dried at 120° C., compacted using a roll press, and vacuum dried at 120° C. for 24 hours using a glass tube oven.
[0088] (Production Example 4-1 of a negative electrode coated with a composite electrolyte) Using a mixer (manufactured by Thinky Corporation), the glass ceramic powder 3 and PVdF-HFP were mixed in a weight ratio of 9:1 using acetone as a solvent to obtain a slurry. The obtained slurry was then dip-coated onto the surface of the negative electrode produced above and dried at 60°C. The coating thickness was 20 μm. It was then vacuum-dried at 120°C for 24 hours using a glass tube oven. The composite electrolyte was then cut into a size of 32 mm x 42 mm using a Thomson punching machine to produce negative electrode 4-1 coated with the composite electrolyte.
[0089] [Example 5] (Example of manufacturing a lithium-ion secondary battery cell) The positive electrode 4-1 produced above and the negative electrode 4-1 coated with the composite electrolyte were stacked so that their electrode surfaces faced each other, wrapped in a laminate, and impregnated with 0.3 ml of the nonaqueous electrolyte solution 2 obtained above. The mixture was degassed under vacuum, impregnated with the electrolyte, and excess nonaqueous electrolyte solution 2 was sucked off, to produce a lithium ion secondary battery cell.
[0090] Comparative Example 9 A lithium ion secondary battery cell was produced in the same manner as in Example 5, except that non-aqueous electrolyte solution 3 was used instead of non-aqueous electrolyte solution 2.
[0091] [Comparative Example 10] (Separator manufacturing example) A PP separator (manufactured by CSTech, P2010H) was cut into a size of 40 mm x 50 mm using a Thomson punching machine and vacuum dried in a glass tube oven at 60°C for 24 hours.
[0092] A dried PP separator was sandwiched between the positive electrode 4-1 produced above and a negative electrode not coated with a positive electrode or composite electrolyte, and the resulting laminate was then impregnated with 0.3 ml of non-aqueous electrolyte solution 2. The resulting laminate was degassed under vacuum, impregnated with the electrolyte solution, and excess electrolyte was sucked off to produce a lithium ion secondary battery cell.
[0093] [Comparative Example 11] A lithium ion secondary battery cell was produced in the same manner as in Comparative Example 10, except that non-aqueous electrolyte solution 3 was used instead of non-aqueous electrolyte solution 2.
[0094] (Evaluation Method 4-1) The cells of Example 5 and Comparative Example 10 were charged and discharged (25°C) using an Asuka Electronics charge-discharge tester in the following order: CC-CV charge (0.2C, 2.6V-0.05C cutoff) → rest (10 minutes) → CC discharge (0.2C, 0.5C, 1.0C, 2.0C, 3.0C, 2.0V cutoff) → rest (10 minutes), and the discharge capacities were compared. The capacity retention rates at each current value were compared, with the discharge capacity at 0.2C being 100%. Further, the discharge capacity was similarly compared between the cell of Comparative Example 9 and the cell of Comparative Example 11. The measurement results are shown in FIGS.
[0095] (Evaluation result 4-1) Comparing the cell of Example 5, which used a composite electrolyte containing LiPF6 as the lithium salt, with the cell of Comparative Example 10, which used a PP separator, the cell of Example 5 had high resistance but good input / output characteristics. On the other hand, comparing the cell of Comparative Example 9, which used a composite electrolyte containing LiClO4 as the lithium salt, with Comparative Example 11, which used a PP separator, the cell of Comparative Example 9 had poor input / output characteristics, reflecting its high resistance. While LiPF6 has a high degree of dissociation and high ionic conductivity, it also reacts with water in the electrolyte to generate HF. It is known that cathode materials react with HF and deteriorate, and it is presumed that the composite electrolyte using LiPF6 captured HF, suppressing the deterioration of the cathode material and achieving the above results.
[0096] [Test Example 5] (Positive Electrode Manufacturing Example 5-1) Using a mixer (Thinky Corporation), Li(Ni 0.6 Co 0.2 Mn 0.2 )O2(NCM622):AB:PVdF:glass ceramic powder 3=96.5:1.5:1.5:0.5 by weight blending, and NMP was used as a solvent to obtain a positive electrode slurry 5-1.
[0097] The obtained positive electrode slurry 5-1 was applied to a 20 μm aluminum current collector foil using a blade coater, and then dried at 120° C. The electrode had a capacity of 3.5 mAh / cm 2 It was compacted using a roll press to obtain a particle size of 66 μm and a density of 3.5 g / cm. 3 Subsequently, the mixture was cut into a size of 30 mm x 40 mm using a Thomson punching machine and vacuum dried at 160°C for 24 hours using a glass tube oven to produce a positive electrode 5-1.
[0098] (Positive Electrode Manufacturing Example 5-2) A positive electrode 5-2 was produced in the same manner as in Positive Electrode Production Example 5-1, except that Glass Ceramic Powder 2 (average particle diameter 1.0 μm) was used instead of Glass Ceramic Powder 3 (average particle diameter 0.4 μm).
[0099] (Positive Electrode Manufacturing Example 5-3) A positive electrode 5-3 was produced in the same manner as in Positive Electrode Production Example 5-1, except that Glass Ceramic Powder 1 (average particle diameter 6.0 μm) was used instead of Glass Ceramic Powder 3 (average particle diameter 0.4 μm).
[0100] (Positive Electrode Manufacturing Example 5-4) Using a mixer (manufactured by Thinky Corporation), the ingredients were mixed in a weight ratio of NCM622:AB:PVdF=97:1.5:1.5 using NMP as a solvent to obtain a positive electrode slurry 5-4.
[0101] The obtained positive electrode slurry 5-4 was applied to a 20 μm aluminum current collector foil using a blade coater, and then dried at 120° C. The electrode had a capacity of 3.5 mAh / cm 2 It was compacted using a roll press to obtain a particle size of 66 μm and a density of 3.5 g / cm. 3 Subsequently, the mixture was cut into a size of 30 mm x 40 mm using a Thomson punching machine and vacuum dried at 160°C for 24 hours using a glass tube oven to prepare a positive electrode 5-4.
[0102] (Negative Electrode Manufacturing Example 5-1) Using a mixer (made by Thinky Corporation), graphite, carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) were mixed in a weight ratio of 97.5:1:1.5 with water as a solvent to obtain negative electrode slurry 5-1.
[0103] The obtained negative electrode slurry 5-1 was applied to a 15 μm copper current collector foil using a blade coater, and then dried at 60° C. The electrode had a capacity of 3.9 mAh / cm 2 It was compacted using a roll press to a thickness of 83 μm and a density of 1.4 g / cm 3 Subsequently, the mixture was cut into a size of 32 mm x 42 mm using a Thomson punching machine and vacuum dried at 160°C for 24 hours using a glass tube oven to prepare Negative Electrode 5-1.
[0104] (Separator manufacturing example) A PP separator (manufactured by CSTech, P2010H) was cut into a size of 40 mm x 50 mm using a Thomson punching machine and vacuum dried in a glass tube oven at 60°C for 24 hours.
[0105] [Example 6] (Example of manufacturing a lithium-ion secondary battery cell) The electrode surfaces of the positive electrode 5-1 and the negative electrode 5-1 produced above were placed face to face, a separator was sandwiched between them, and the resultant was wrapped in an aluminum laminate. 0.3 ml of the nonaqueous electrolyte solution 2 obtained above was injected and vacuum impregnated for 30 seconds, and then the resultant was sealed to produce a lithium ion secondary battery cell.
[0106] [Example 7] A lithium ion secondary battery cell was produced in the same manner as in Example 6, except that the positive electrode 5-2 was used instead of the positive electrode 5-1.
[0107] [Comparative Example 12] A lithium ion secondary battery cell was produced in the same manner as in Example 6, except that the positive electrode 5-3 was used instead of the positive electrode 5-1.
[0108] [Comparative Example 13] A lithium ion secondary battery cell was produced in the same manner as in Example 6, except that the positive electrode 5-4 was used instead of the positive electrode 5-1.
[0109] (chemical treatment, degassing) After one charge-discharge cycle (4.2 V - 2.5 V) at 0.05 C, the laminate was opened once, and then vacuum degassed again for 30 seconds before being sealed.
[0110] (Evaluation Method 5-1) For the cells of Example 6, Example 7, Comparative Example 12, and Comparative Example 13, a charge / discharge tester manufactured by Asuka Electronics was used to charge and discharge (25°C) in the following sequence: CC-CV charge (0.2C, 4.2V-0.05C cutoff) → rest (10 minutes) → CC discharge (0.2C or 3C, 2.5V cutoff) → rest (10 minutes), and the discharge capacities were compared.
[0111] (Evaluation result 5-1) Comparing Examples 6 and 7 and Comparative Example 12, in which glass ceramic powder was added, with Comparative Example 13, in which no glass ceramic powder was added, it was found that the smaller the average particle size of the glass ceramic powder, the higher the surface area. HF generated by hydrolysis of lithium salt deteriorates the positive electrode material, but the higher the specific surface area of the glass ceramic powder, the greater the HF suppression effect, thereby suppressing the deterioration of the positive electrode material and resulting in high input / output characteristics. [Table 4]
Claims
1. Li 1+x+2y+z A x Ca y T 2-(x+y) Si z P 3-z O 12 (1) In formula (1), A is at least one selected from the group consisting of Al, Ga, and Y; T is at least one selected from the group consisting of Ti, Ge, and Zr; (0≦x≦1, 0≦y≦1, 0≦z≦1, 0≦x+y≦1, 0≦x+2y+z≦2) A lithium ion conductive glass ceramic powder having a main crystal phase represented by the formula (I) and an average particle size of 5 μm or less; LiMF m (C 2 F 5 ) n (2) In formula (2), M is at least one selected from the group consisting of P, B, Sb, Ta, and Nb; When M is P, Sb, Ta, or Nb, m+n=6, 3≦m≦6, 0≦n≦3; When M is B, m+n=4, 2≦m≦4, 0≦n≦2. An electrolyte solution containing a lithium salt represented by the formula: Electrolytes, including:
2. The specific surface area of the glass ceramic powder is 1 m 2 2. The electrolyte of claim 1, wherein the Cr content is 1 / g or more.
3. The lithium salt is LiPF 6 , LiBF 4 , LiSbF 6 , LiTaF 6 , LiNbF 6 , LiBF 3 (C 2 F 5 ), and LiPF 3 (C 2 F 5 ) 3 The electrolyte according to claim 1, which is at least one selected from the group consisting of:
4. The electrolyte of claim 1 further comprising an ion-conducting polymer.
5. A lithium ion secondary battery comprising a positive electrode, a negative electrode, and the electrolyte according to any one of claims 1 to 4.
6. An additive for use in an electrode of a lithium ion secondary battery, Li 1+x+2y+z A x Ca y T 2-(x+y) Si z P 3-z O 12 (1) In formula (1), A is at least one selected from the group consisting of Al, Ga, and Y; T is at least one selected from the group consisting of Ti, Ge, and Zr; (0≦x≦1, 0≦y≦1, 0≦z≦1, 0≦x+y≦1, 0≦x+2y+z≦2) A lithium ion conductive glass ceramic powder having a main crystal phase represented by the formula (I) and an average particle size of 5 μm or less; LiMF m (C 2 F 5 ) n (2) In formula (2), M is at least one selected from the group consisting of P, B, Sb, Ta, and Nb; When M is P, Sb, Ta, or Nb, m+n=6, 3≦m≦6, 0≦n≦3; When M is B, m+n=4, 2≦m≦4, 0≦n≦2. and a lithium salt represented by the formula:
13. An electrode additive comprising:
7. The specific surface area of the glass ceramic powder is 1 m 2 The electrode additive according to claim 6, wherein the Cr content is 1.0 / g or more.
8. The lithium salt is LiPF 6 , LiBF 4 , LiSbF 6 , LiTaF 6 , LiNbF 6 , LiBF 3 (C 2 F 5 ), and LiPF 3 (C 2 F 5 ) 3 The electrode additive according to claim 6, which is at least one selected from the group consisting of:
9. The electrode additive of claim 6 , further comprising an ion-conducting polymer.
10. An electrode comprising an active material and the electrode additive according to any one of claims 6 to 9.
11. A lithium ion secondary battery comprising an electrode containing an active material and the electrode additive according to any one of claims 6 to 9.
Citation Information
Patent Citations
Glass-ceramic composite electrolyte and lithium secondary battery
JP2001015164A
Coated positive electrode active material particle for lithium ion battery, positive electrode for lithium ion battery, and manufacturing method of coated positive electrode active material particle for lithium ion battery
JP2023013685A
Reverse Osmosis Purification Water Treatment System Using Raw Water Bypass Piping
KR102565081B1
Glass ceramic complex electrolyte and lithium secondary battery
JP2004303738A