Frosted glass-like resin composition and molded article

A thermoplastic resin composition with crosslinked polymer particles and fluorescent dyes or pigments achieves a transparent, fluorescent frosted glass appearance, addressing the need for dual aesthetic properties in plastic products.

JP2024137295APending Publication Date: 2024-10-07SUMIKA COLOR CO LTD
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
JP2023048763
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

There is a lack of molded plastic products that simultaneously exhibit a frosted glass appearance and fluorescent properties, which are desirable for enhancing design appeal while maintaining transparency.

Method used

A thermoplastic resin composition comprising a thermoplastic resin, spherical crosslinked polymer particles or mica particles, and fluorescent dyes or pigments, with specific particle sizes and refractive index differences to achieve a fluorescent frosted glass appearance.

Benefits of technology

The composition produces highly transparent molded articles with a frosted glass appearance and high design quality, combining both fluorescent and matte effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137295000006
    Figure 2024137295000006
  • Figure 2024137295000001
    Figure 2024137295000001
  • Figure 2024137295000002
    Figure 2024137295000002
Patent Text Reader

Abstract

To manufacture a molded article which has high transparency and fluorescence, is frosted glass-like and has high designability.SOLUTION: A thermoplastic resin composition contains (A) a thermoplastic resin, (B) at least one particle selected from spherical crosslinked polymer particles and mica particles, and (C) a dye having fluorescence. Preferably, an amount of the thermoplastic resin (A) is 100 pts.wt., an amount of the particles (B) is 0.2 to 5 pts.wt., and an amount of the dye (C) is 0.0001 to 1 pts.wt.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ground-glass-like resin composition and a molded article having an excellent appearance. [Background technology]

[0002] Plastic containers and other molded products are widely used as a substitute for glass due to their light weight, low price, colorability, and productivity. Among them, thermoplastic resins such as acrylic resin, polyester resin, polystyrene resin, and polycarbonate resin have the characteristics of high transparency, excellent surface gloss, and excellent moldability such as injection molding, extrusion molding, and blow molding. Therefore, they are used in many fields such as cosmetics, food, medicine, healthcare, lighting, and signs, and there are molded products that have a luxurious feel like frosted glass.

[0003] As a method for obtaining a ground-glass appearance in a plastic molded product, Patent Document 1 discloses a technology for eliminating the gloss of the plastic and imparting a matte finish by using spherical beads with high heat resistance and a high refractive index. Patent Document 2 discloses that a polyester resin composition obtained by blending a spherical fine powder of polymethyl methacrylate and a fine powder of calcium carbonate with a polyester resin causes light diffusion in the molded product, resulting in a molded product with a ground-glass appearance.

[0004] In addition, plastic molded products colored with fluorescent dyes or pigments are highly appealing in design and color, and are used in a wide range of fields, such as pachinko parts, lamp cases and covers for automobiles, home appliances, and toys.

[0005] Patent Document 3 describes a method for producing a molded article by melt-kneading a thermoplastic resin and a fluorescent dye. Patent Document 4 describes a method for producing a molded article by melt-kneading a thermoplastic resin and a pigment. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 01-297465 [Patent Document 2] Japanese Patent Application Publication No. 11-001606 [Patent Document 3] JP 2002-30220 A [Patent Document 4] JP2015-193828A Summary of the Invention [Problem to be solved by the invention]

[0007] Although there are molded products that have a ground-glass appearance and molded products that have fluorescence, there are no molded products that combine both, and there was a demand for such products from a design standpoint.

[0008] The present invention has been made in consideration of the above circumstances, and has an object to provide a thermoplastic resin composition that can impart a ground-glass look having fluorescence while maintaining the transparency of plastic. [Means for solving the problem]

[0009] The present inventors have conducted extensive research and have completed the present invention.

[0010] The present invention relates to A thermoplastic resin composition comprising a thermoplastic resin (A) and at least one type of particles (B) selected from bead-like crosslinked polymer particles or mica particles, The present invention relates to a thermoplastic resin composition which further contains at least one colorant (C) selected from dyes or pigments having fluorescent properties.

[0011] The present invention includes the following inventions. [1] (A) a thermoplastic resin, (B) at least one type of particle selected from spherical crosslinked polymer particles and mica particles, and (C) Fluorescent dye A thermoplastic resin composition comprising: [2] The thermoplastic resin (A) is at least one resin selected from a polyethylene terephthalate resin, a polystyrene resin, and a polymethyl methacrylate resin; In the particles (B), the polymer of the spherical crosslinked polymer particles is at least one selected from the group consisting of crosslinked polystyrene, crosslinked methyl methacrylate-styrene copolymer, crosslinked polymethyl methacrylate, and crosslinked silicone resin, and the mica particles are synthetic mica; The thermoplastic resin composition according to [1], wherein the dye (C) is at least one selected from the group consisting of merocyanine, perylene, acridine, luciferin, pyranine, stilbene, rhodamine, coumarin, 4-(dicyanomethylene)-2-methyl-6-(4-dimethylaminostyryl)-4H-pyran (DCM), pyrromethene, fluorescein, umbelliferone, naphthalimide, diketopyrrolopyrrole, and quinacridone. [3] The thermoplastic resin composition according to [1], wherein the average particle size of the crosslinked polymer particles is 1 μm or more and 50 μm or less, the average sphericity of the crosslinked polymer particles is 0.8 or more, and the average particle size of the mica particles is 1 μm or more and 100 μm or less. [4] The thermoplastic resin composition according to [1], wherein the amount of the thermoplastic resin (A) is 100 parts by weight, the amount of the particles (B) is 0.2 to 10 parts by weight, and the amount of the dye (C) is 0.0001 to 1 part by weight. [5] A thermoplastic resin molded product molded from the thermoplastic resin composition according to [1]. [6] (A) a thermoplastic resin, (B) at least one type of particle selected from spherical crosslinked polymer particles and mica particles, and (C) Fluorescent dye A masterbatch for a thermoplastic resin comprising: A masterbatch for thermoplastic resins, comprising 6 to 100 parts by weight of particles (B) per 100 parts by weight of thermoplastic resin (A). Effect of the Invention

[0012] According to the present invention, it is possible to produce a molded article which is highly transparent, has a ground-glass appearance, and has excellent designability. [Brief description of the drawings]

[0013] [Figure 1] 1 is a graph showing the relationship between the measurement wavelength (horizontal axis) and the excited light emission (vertical axis) (intensity (arbitrary unit)) in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] [Thermoplastic resin (hereinafter sometimes referred to as "resin")] Examples of the resin of the present invention include acrylonitrile-butadiene-styrene resin, low-density polyethylene resin, high-density polyethylene resin, polystyrene resin, polypropylene resin, acrylonitrile-styrene resin, cellulose acetate resin, ethylene-vinyl acetate resin, acrylic-acrylonitrile-styrene resin, acrylic-chlorinated polyethylene resin, ethylene-vinyl alcohol resin, fluororesin, polymethyl methacrylate resin, polyacetal resin, polyamide resin, polyethylene terephthalate resin, polycarbonate resin, polysulfone resin, polyethersulfone resin, methylpentene resin, polyarylate resin, polybutylene terephthalate resin, resin containing an alicyclic structure-containing ethylenically unsaturated monomer unit (e.g., cycloolefin polymer resin), polyphenylene sulfide resin, polyphenylene oxide resin, polyether ether ketone resin, and the like.

[0015] The resin is preferably a resin having excellent transparency and excellent moldability at a predetermined processing temperature. A thermoplastic resin having a total light transmittance of 85 or more at a thickness of 3.0 mm is more preferable, and at least one resin selected from polyethylene terephthalate resin, polystyrene resin, polycarbonate resin, and polymethyl methacrylate resin is preferable. By using a thermoplastic resin having excellent transparency, the ground glass tone tends to become clearer. Two or more of these resins may be used in combination as long as the transparency and mechanical properties are not impaired.

[0016] The thickness of the molded article (i.e., the thickness of the resin) may be 0.1 mm to 30 mm or 0.3 mm to 10 mm. The thickness of the molded article may be 0.2 mm or more, 0.4 mm or more, 0.6 mm or more, 0.8 mm or more, 1 mm or more, 1.2 mm or more, 1.4 mm or more, 1.6 mm or more, 1.8 mm or more, 2 mm or more, 2.2 mm or more, 2.4 mm or more, 2.6 mm or more, 2.8 mm or more, or 3 mm or more. The thickness of the molded article may be 25 mm or less, 20 mm or less, 15 mm or less, 12 mm or less, 10 mm or less, 9 mm or less, 8 mm or less, 7 mm or less, 6 mm or less, 5 mm or less, 4 mm or less, or 3.5 mm or less.

[0017] The resin preferably has a total light transmittance of 55% or more, 60% or more, 65% or more, 70% or more, 75% or more, 80% or more, 85% or more, or 90% or more when the thickness is 2 mm to 5 mm (for example, 2 mm, 3 mm, 4 mm or 5 mm, particularly 3.0 mm). For example, the total light transmittance may be 60% or more and 100% or less when the thickness of the molded article is 2 mm to 5 mm. The total light transmittance may be 56% or more, 58% or more, 60% or more, 62% or more, 64% or more, 66% or more, 68% or more, 70% or more, 72% or more, 74% or more, 76% or more, 78% or more, 80% or more, 82% or more, 84% or more, 86% or more, 88% or more, 90% or more, 92% or more, or 94% or more. The total light transmittance may be 100% or less, 98% or less, 96% or less, 94% or less, 92% or less, 90% or less, or 88% or less.

[0018] The total light transmittance can be measured in accordance with JIS K 7136: 2000. For the measurement, for example, a haze meter (model TC-H3DPK) manufactured by Tokyo Denshoku Co., Ltd. can be used. [Formula] Total light transmittance (Tt) = Linear transmittance (Tp) + Diffuse transmittance (Td)

[0019] [Bead-like cross-linked polymer particles] The bead-like crosslinked polymer particles are spherical and have an average sphericity of preferably 0.8 or more, more preferably 0.85 or more, and even more preferably 0.9 or more. Sphericity is measured by taking a photograph with a microscope, and using the observed particle area and perimeter, (sphericity) = {4π × (area) ÷ (perimeter)} 2 The closer to 1 the particle is, the closer it is to a perfect sphere. The average sphericity is preferably calculated by averaging the sphericities of 100 arbitrarily selected aggregates.

[0020] The bead-like crosslinked polymer particles are not particularly limited, but examples thereof include crosslinked polystyrene resin, methyl methacrylate-styrene copolymer crosslinked particles, crosslinked polymethyl methacrylate resin, silicone resin, and the like.

[0021] The average particle size of the bead-like crosslinked particles is preferably 50 μm or less. When the average particle size is 50 μm or less, light scattering is sufficient, haze is high, and a good ground glass look is obtained. The average particle size of the crosslinked particles is preferably 45 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, 25 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less. The average particle size of the crosslinked particles may be 1 μm or more, 3 μm or more, 5 μm or more, or 10 μm or more.

[0022] The average particle size can be measured using an optical microscope (200 to 500x). The median size (D50) obtained by creating a particle size distribution from the particle sizes of any number of crosslinked particles (for example, 100 or 200) can be used as the average particle size.

[0023] [Mica particles] Examples of mica particles include sericite (silicite), muscovite (white mica), phlogopite (gold mica), synthetic mica, etc. Among these, synthetic mica is preferable. The average particle size of the mica particles may be 1 to 100 μm, 2 to 80 μm, 3 to 70 μm, 4 to 60 μm, 5 to 55 μm, or 7 to 50 μm. The average particle size of the mica particles can be measured in the same manner as the average particle size of the bead-like crosslinked particles. That is, the average particle size of the mica particles may be the median diameter (D50) measured by an optical microscope (200 to 500 times).

[0024] Synthetic mica is generally a colorless, transparent, pure crystal. Synthetic mica may be mica in which hydroxyl groups (OH) are replaced with fluorine atoms (F). In synthetic mica, the iron content may be 100 ppm or less, or 50 ppm or less. In synthetic mica, the amount of heavy metals may be 1 ppm or less, or 0.1 ppm or less. Mica particles (especially synthetic mica particles) are thin plates, thermally and chemically stable, and have a high aspect ratio (ratio of particle size to thickness) (for example, aspect ratio is 10 to 100, 20 to 80, or 30 to 70). Therefore, by orienting the mica particles in a molded product, it is possible to improve mechanical properties such as low warpage, high rigidity, and low shrinkage, and to impart insulation properties, vibration damping properties, etc. Furthermore, it is possible to impart glossiness due to interfacial reflection with the base resin, so it is widely used in the fields of home appliances, heavy electrical machinery, electric wires, etc. Mica is obtained by refining, pulverizing, and classifying mica ore, and the higher the aspect ratio, the more likely it is that specific properties in terms of physical properties will be expressed.

[0025] When mica particles are used, extrusion molding is preferred since it provides good design properties.

[0026] The thermoplastic resin molded article may have a haze of 40-85, 45-80, or 50-75 when the article has a thickness of 3 mm. Haze can be measured in accordance with JIS K 7136, for example, by a haze meter (model TC-H3DPK) manufactured by Tokyo Denshoku Co., Ltd. [Formula] HAZE=(Diffuse transmittance (Td) / Total light transmittance (Td))*100

[0027] In the thermoplastic resin composition, the amount of particles (bead-like crosslinked polymer particles and mica particles) is preferably 0.1 to 10 parts by weight or 0.3 to 5 parts by weight based on 100 parts by weight of the thermoplastic resin (A). When the amount is within the above range, high haze and good ground glass texture are obtained. More preferably, it is 0.2 to 8 parts by weight or 0.3 to 3 parts by weight, for example, 1 to 2.5 parts by weight. Alternatively, the amount of the particles may be 0.1 parts by weight or more, 0.2 parts by weight or more, 0.3 parts by weight or more, 0.5 parts by weight or more, 0.8 parts by weight or more, 1 part by weight or more, 1.5 parts by weight or more, 2 parts by weight or more, 3 parts by weight or more, 4 parts by weight or more, 5 parts by weight or more, 6 parts by weight or more, or 7 parts by weight or more, and the amount of the particles may be 10 parts by weight or less, 9 parts by weight or less, 8 parts by weight or less, 7 parts by weight or less, 6 parts by weight or less, 5 parts by weight or less, 4 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1.5 parts by weight or less, 1 part by weight or less, or 0.5 parts by weight or less, relative to 100 parts by weight of the thermoplastic resin (A).

[0028] In the master batch, the amount of particles (bead-like crosslinked polymer particles and mica particles) is preferably 1 to 100 parts by weight or 5 to 20 parts by weight relative to 100 parts by weight of the thermoplastic resin (A). When the amount is within the above range, the haze is high and a good ground glass texture is obtained. The amount of particles may be 1 part by weight or more, 2 parts by weight or more, 3 parts by weight or more, 5 parts by weight or more, 8 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 25 parts by weight or more, 30 parts by weight or more, 40 parts by weight or more, 50 parts by weight or more, or 60 parts by weight or more relative to 100 parts by weight of the thermoplastic resin (A), and the amount of particles may be 100 parts by weight or less, 90 parts by weight or less, 80 parts by weight or less, 70 parts by weight or less, 60 parts by weight or less, 50 parts by weight or less, 40 parts by weight or less, 30 parts by weight or less, 25 parts by weight or less, 20 parts by weight or less, 15 parts by weight or less, 10 parts by weight or less, or 5 parts by weight or less.

[0029] The smaller the difference in refractive index between the thermoplastic resin and the particles, the more transparency can be maintained, and the easier it is to impart a ground glass look, and the difference in refractive index between the thermoplastic resin and the particles is preferably 0.005 to 0.08, more preferably 0.008 to 0.03. The difference in refractive index may be 0.006 or more, 0.007 or more, 0.008 or more, 0.009 or more, 0.01 or more, 0.011 or more, 0.012 or more, 0.013 or more, 0.014 or more, 0.015 or more, 0.02 or more, 0.025 or more, 0.03 or more, 0.035 or more, 0.04 or more, 0.045 or more, or 0.05 or more. It may be 0.07 or less, 0.065 or less, 0.06 or less, 0.055 or less, 0.05 or less, 0.045 or less, 0.04 or less, 0.035 or less, 0.03 or less, 0.025 or less, 0.02 or less, 0.019 or less, 0.018 or less, 0.017 or less, 0.016 or less, 0.015 or less, 0.014 or less, 0.013 or less, or 0.012 or less.

[0030] The refractive index of thermoplastic resin was measured using a multi-wavelength Abbe refractometer (ATAGO DR-M4 model). First, a small amount of contact liquid (1-bromonaphthalene) was dropped onto the surface of a test piece made by injection molding, and the edge of the test piece was brought into contact with the surface of the prism with the light source facing the light source. After that, the field was adjusted until all colors disappeared, and the boundary between the bright field and the dark field was aligned with the intersection of the crosshairs of the eyepiece to measure the refractive index. A halogen lamp with a wavelength of 589 nm was used as the light source.

[0031] The refractive index of the particles was measured by the Becke method. First, the polymer particles were placed on a slide glass, and a refractive index liquid (CARGILLE's standard refractive index liquid, refractive index nD25 of 1.480 to 1.596, prepared in multiple increments of 0.002) was dropped. Then, after thoroughly mixing the polymer particles and the refractive index liquid, the outline of the polymer particles was observed from above with an optical microscope while irradiating light from a high pressure sodium lamp "NX35" (center wavelength 589 nm) manufactured by Iwasaki Electric Co., Ltd. from below. Then, when the outline was not visible, it was determined that the refractive index of the refractive index liquid and the polymer particles were equal.

[0032] In addition, there is no problem with the observation by the optical microscope as long as the magnification allows the outline of the polymer particles to be confirmed, but for polymer particles with a particle diameter of 5 μm, an observation magnification of about 500 times is appropriate. By the above operation, the closer the refractive index of the polymer particles and the refractive index of the refractive liquid are, the more difficult it is to see the outline of the polymer particles, so the refractive index of the refractive liquid in which the outline of the polymer particles is difficult to see is determined to be equal to the refractive index of the polymer particles.

[0033] In addition, when there is no difference in the appearance of the polymer particles between two types of refractive index liquids with a refractive index difference of 0.002, the intermediate value of these two types of refractive index liquids was determined to be the refractive index of the polymer particles. For example, when tests were performed using refractive index liquids with refractive indices of 1.554 and 1.556, if there is no difference in the appearance of the polymer particles between the two refractive index liquids, the intermediate value of these refractive index liquids, 1.555, was determined to be the refractive index of the polymer particles.

[0034] [Fluorescent material] In this specification, the fluorescent material means a material that selectively absorbs light such as ultraviolet light, visible light, and infrared light, converts the wavelength to the long wavelength side, and emits fluorescence. It is known that fluorescent materials generally have an emission wavelength that is longer than the absorption wavelength, but in order to obtain the ground glass-like resin composition and molded product of the present invention that have excellent appearance, it is desirable that the emission wavelength be in the visible light region (360 nm to 830 nm).

[0035] The present invention provides a thermoplastic resin composition capable of imparting a ground-glass look with fluorescence while maintaining the transparency of plastics, and in order to obtain higher designability, it is more preferable to use a fluorescent material having light-collecting properties. The fluorescent material having light-collecting properties is a material having a function of converting selectively absorbed light to a longer wavelength side as a fluorescent color, and is characterized in that the light is reflected inside the colored material and guided to the edge of the molded product, where it is emitted in a concentrated state from the edge of the molded product, emitting strong light.

[0036] Examples of fluorescent materials include merocyanine, perylene, acridine, luciferin, pyranine, stilbene, rhodamine, coumarin, 4-(dicyanomethylene)-2-methyl-6-(4-dimethylaminostyryl)-4H-pyran (DCM), pyrromethene, fluorescein, umbelliferone, naphthalimide, diketopyrrolopyrrole, quinacridone, etc. Examples of fluorescent materials having more preferable light-collecting properties include perylene, naphthalimide, diketopyrrolopyrrole, quinacridone, etc.

[0037] The resin, particles, and fluorescent material may be mixed as necessary before being melted. Alternatively, the particles, fluorescent material, and a part of the resin may be melt-kneaded in advance to prepare a master powder or master batch having a high concentration of the particles and fluorescent material, and then the resin and the master powder or master batch may be melt-kneaded. Methods for mixing the resin and particles include dry blending.

[0038] <Step of Melting and Kneading Resin and Particles> The resin, particles, and fluorescent material are usually melted using a kneader. Examples of kneaders for melt-kneading the resin, particles, and fluorescent material include various extruders such as single-screw extruders, twin-screw extruders, and multi-screw extruders, as well as batch-type kneaders such as Banbury mixers, intensive mixers, and pressure kneaders; simple kneaders such as Brabender mixers; continuous intensive mixers; and devices that have a single-screw extruder below these kneaders and perform kneading and extrusion simultaneously. The melting temperature (high temperature) is equal to or higher than the melting point of the resin, and may generally be 200 to 350°C, or 230 to 320°C, although it depends on the melting point of the resin.

[0039] <Other agents> In addition to the resin, particles, and fluorescent material, other agents may be added (or melted). Examples of other agents include dyes, pigments, plasticizers, antioxidants, UV absorbers, light stabilizers, flame retardants, antibacterial agents, antistatic agents, copper damage inhibitors, metal deactivators, tackifiers, antiblocking agents, lubricants, slip agents, internal release agents, anti-fogging agents (anti-drip agents, anti-fog agents), fragrances, surfactants, wetting agents, preservatives, anti-fungal agents, fillers, reinforcing agents, stabilizers, heat retaining agents, foaming agents, vibration-proofing agents, impact resistance improving agents, surface treatment agents, heat retaining agents, surface treatment agents, dispersants, water-repellent materials, etc. The lubricant may, for example, be magnesium stearate. The amount of the other agents may be 0 to 30% by weight, 0.1 to 20% by weight, or 1 to 10% by weight relative to the resin composition.

[0040] <Step of Molding a Resin Composition Obtained by Melting and Kneading a Resin, Particles, and a Fluorescent Material> The molding can be carried out by injection molding, extrusion molding, blow molding, or the like.

[0041] <Manufacturing method of injection molded products> The present invention also relates to a method for producing an injection molded article, which comprises a step of injection molding a resin composition obtained by melting a resin, particles, a fluorescent material, and optionally other agents at a high temperature.

[0042] A typical injection molding machine is used for injection molding. The melt-kneaded resin, particles, and fluorescent material are fed into the injection molding machine. As the injection molding machine, a known one can be used, and examples thereof include a hydraulic injection molding machine, an electric injection molding machine, etc. The injection molding machine can be appropriately selected depending on the size of the injection molded article to be obtained and the size of the mold to be used.

[0043] The clamping pressure can be appropriately selected depending on the size of the mold to be used and the resin capacity. The mold can be heated using an electric heater or a mold temperature regulator with a heat medium circulation. In particular, it is preferable to heat the mold by embedding a heat medium circulation pipe inside the mold, since this allows accurate and rapid control of the surface temperature of the mold and the molded body.

[0044] <Manufacturing method of extrusion molded products> The present invention also relates to a method for producing an extrusion molded article, which comprises a step of extruding a resin composition obtained by melting a resin, particles, a fluorescent material, and optionally other agents at a high temperature.

[0045] For the extrusion molding, a normal T-die extruder, an inflation molding machine, etc. are used. These extruders are connected to a kneader. The melt-kneaded resin, particles, and fluorescent material are fed to the extruder.

[0046] Also, a device in which a kneader and an extrusion molding machine are integrated may be used. As a device in which a kneader and an extrusion molding machine are integrated, a known device may be used, and examples thereof include a continuous intensive mixer; a continuous type kneader such as a kneading type twin screw extrusion molding machine (same direction or different direction); a continuous kneading device using a rotating disk having a grinding mechanism; a single screw extrusion molding machine equipped with a kneading section (Dulmage, CTM, etc.); and a twin screw kneading extrusion molding machine having a kneading disk or a kneading rotor; but there is no particular limitation. Two or more types of kneaders may be used in combination.

[0047] <Manufacturing method of blow molded products> The present invention also relates to a method for producing a blow molded article, which comprises a step of melting a resin, particles, a fluorescent material, and optionally other agents at high temperature to obtain a resin composition, and then blow molding the resulting resin composition.

[0048] For the blow molding, a normal injection blow molding machine or a direct blow molding machine is used. The melt-kneaded resin, particles, and fluorescent material are fed into the blow molding machine. As the blow molding machine, a known one can be used and can be appropriately selected.

[0049] <Pellet manufacturing method> The case where the resin composition is in the form of pellets will be described. The melt-kneaded resin composition may be supplied to a die apparatus. The die device has a supply port to which the extruder is connected, and the melt-kneaded resin, particles, and fluorescent material are supplied from the extruder to the supply port of the die device.

[0050] The resin, particles, and fluorescent material fed from the extruder to the die device are fed to the extrusion molding section of the die device. The resin, particles, and fluorescent material are extruded from the extrusion port of the extrusion molding section to form strands. The diameter of the strand is not particularly limited and can be appropriately changed depending on the purpose, but is, for example, in the range of 0.2 to 10 mm or 0.5 to 5 mm.

[0051] The strands can be cut into pellets after being cooled as necessary. The cutting is carried out by a pelletizer. The most commonly used cooling method is to introduce the extruded strand into a water bath and immerse the strand in the cooling water in the water bath. The strands after cooling are preferably fed to a pelletizer after removing moisture adhering to the surface with a water draining device. The pelletizer cuts the strands by driving a rotary blade or the like. The length of the strands to be cut is not particularly limited and can be appropriately changed depending on the purpose, but is, for example, in the range of 0.5 to 10.0 mm or 1.0 to 5.0 mm. The shape of the pellets includes a cylinder, a prism, etc., but a cylinder is preferred from the viewpoints of ease of production and handling.

[0052] The pellets can be used to obtain molded articles, which can be produced by the above-mentioned methods for producing injection molded articles, the above-mentioned methods for producing extrusion molded articles, blow molding, vacuum molding, inflation molding, calendar molding, slush molding, dip molding, foam molding, and the like. The resulting molded article has a matte finish and a frosted glass appearance. EXAMPLES

[0053] The present invention will be specifically described below with reference to examples and comparative examples, although the present invention is not limited to these examples.

[0054] [Examples 1 to 7] A composition was obtained by dry blending 100 weight percent polyethylene terephthalate resin with bead-shaped crosslinked polymer particles (crosslinked particles) or mica particles, and a fluorescent dye or pigment, as shown in Table 1. The obtained composition was injection molded at a temperature of 280°C using an injection molding machine (product name: IS55FP-1.5 A, manufactured by Shibaura Machine Co., Ltd., mold clamping pressure: 55t) equipped with a three-stage molded plate mold, to obtain an injection molded product as a three-stage molded plate with thicknesses of 1.0 mm / 2.0 mm / 3.0 mm.

[0055] [Table 1]

[0056] Bead-like crosslinked particles or mica particles I: Cross-linked polystyrene particles (particle size 8 μm, refractive index 1.592) II: Mica particles (particle size 40 μm, aspect ratio 100, refractive index 1.525)

[0057] Fluorescent dyes or pigments A: Lumicolor Orange, made by Kashinomote Technologies B: BASF Lumogen F Yellow 083 C: BASF Irgazin Red K3840 D: Clariant PV Fast Red B E: DayGlo ZQ-15 F: DayGlo ZQ-16

[0058] [Comparative Examples 1 and 2] A composition was obtained by dry blending 100 weight percent polyethylene terephthalate resin with bead-like crosslinked particles or mica particles and non-fluorescent dyes or pigments shown in Table 2. The obtained composition was injection molded at a temperature of 280°C using an injection molding machine (product name: IS55FP-1.5 A, manufactured by Shibaura Machine Co., Ltd., mold clamping pressure: 55t) equipped with a three-stage molded plate mold, to obtain an injection molded product as a three-stage molded plate with thicknesses of 1.0 mm / 2.0 mm / 3.0 mm.

[0059] [Table 2]

[0060] [Examples 8 and 9] A composition was obtained by dry blending 100 weight percent polyethylene terephthalate resin with bead-like crosslinked particles or mica particles and fluorescent dyes or pigments shown in Table 3. The obtained composition was formed into a 200 μm thick sheet at 280° C. using a T-die molding machine (40 mm φ T-die extruder, 400 mm wide T-die, manufactured by Sakaguchi Seisakusho Co., Ltd.), to obtain an extrusion molded product.

[0061] [Table 3]

[0062] The molded articles obtained in the examples and comparative examples were evaluated for the following, and the evaluation results are shown in Table 4.

[0063] [Total light transmittance] The total light transmittance of the molded articles obtained in the examples and comparative examples was measured in accordance with JIS K 7361. In Examples 1 to 7 and Comparative Examples 1 and 2, the measurement was performed on a 3.0 mm thick portion of the molded article, and in Examples 8 and 9, the measurement was performed on a 200 μm thick portion of the molded article.

[0064] [HAZE] The haze of the molded articles obtained in the examples and comparative examples was measured in accordance with JIS K 7136. In Examples 1 to 7 and Comparative Examples 1 and 2, the measurement was performed on a 3.0 mm thick portion of the molded article, and in Examples 8 and 9, the measurement was performed on a 200 μm thick portion of the molded article.

[0065] [Ground glass] The ground glass properties were evaluated visually according to the following criteria: For Examples 1 to 7 and Comparative Examples 1 and 2, the evaluation was performed on a 3.0 mm thick portion of the molded product, and for Examples 8 and 9, the evaluation was performed on a 200 μm thick portion of the molded product. ⊚: Good ground glass properties. ○: Ground glass-like ×: No ground glass properties

[0066] [Fluorescence] The fluorescence intensity of the molded articles obtained in the examples and comparative examples was measured using a spectrofluorophotometer (product name: F-7000, manufactured by Hitachi High-Technologies Corporation). Note that in Examples 1 to 7 and Comparative Examples 1 and 2, the measurement was performed on a 3.0 mm thick portion of the molded article. In addition, the fluorescence was evaluated visually according to the following criteria. Note that in Examples 1 to 7 and Comparative Examples 1 and 2, the measurement was performed on a 3.0 mm thick portion of the molded article, and in Examples 8 and 9, the measurement was performed on a 200 μm thick portion of the molded article. ◎: High fluorescence ○: Fluorescent ×: No fluorescence

[0067] [Design] The molded articles obtained in the Examples and Comparative Examples were visually evaluated for their design, which had both fluorescence and a ground-glass feel, according to the following criteria: In Examples 1 to 7 and Comparative Examples 1 and 2, the molded article was evaluated at a 3.0 mm thick portion, and in Examples 8 and 9, the molded article was evaluated at a 200 μm thick portion. ◎: High fluorescence and good ground glass properties ◯: Fluorescent and good ground-glass properties, or highly fluorescent and ground-glass properties. ×: No fluorescence or ground glass

[0068] [Touch] The molded articles obtained in Examples 8 and 9 were evaluated for feel according to the following criteria. ◎: Highly matte finish 〇: Matte finish

[0069] <Total light transmittance, haze, ground glass properties, fluorescence, design, tactile evaluation> The evaluation results of the molded articles obtained in the Examples and Comparative Examples are shown in Tables 4 and 5. For the maximum emission wavelength in the fluorescence evaluation, the emission emitted upon excitation at each measurement wavelength is detected as a single or multiple peaks as shown in Figure 1 (measurement results of Example 1), and the wavelength at which the fluorescence intensity of each detected single or multiple peaks is maximum is recorded. In Figure 1, the horizontal axis represents wavelength (nm), and the horizontal axis represents intensity (arbitrary units).

[0070] [Table 4]

[0071] [Table 5] [Industrial Applicability]

[0072] According to the present invention, a molded article having a high degree of transparency, fluorescence, and a ground-glass appearance and excellent designability can be obtained.

Claims

1. (A) a thermoplastic resin, (B) at least one type of particle selected from spherical crosslinked polymer particles and mica particles, and (C) Fluorescent dye A thermoplastic resin composition comprising:

2. The thermoplastic resin (A) is at least one resin selected from a polyethylene terephthalate resin, a polystyrene resin, and a polymethyl methacrylate resin; In the particle (B), the polymer of the spherical crosslinked polymer particle is at least one selected from the group consisting of crosslinked polystyrene, crosslinked methyl methacrylate-styrene copolymer, crosslinked polymethyl methacrylate, and crosslinked silicone resin, and the mica particle is synthetic mica; The thermoplastic resin composition according to claim 1, wherein the dye (C) is at least one selected from the group consisting of merocyanine, perylene, acridine, luciferin, pyranine, stilbene, rhodamine, coumarin, 4-(dicyanomethylene)-2-methyl-6-(4-dimethylaminostyryl)-4H-pyran (DCM), pyrromethene, fluorescein, umbelliferone, naphthalimide, diketopyrrolopyrrole, and quinacridone.

3. 2. The thermoplastic resin composition according to claim 1, wherein the average particle size of the crosslinked polymer particles is 1 μm or more and 50 μm or less, the average sphericity of the crosslinked polymer particles is 0.8 or more, and the average particle size of the mica particles is 1 μm or more and 100 μm or less.

4. The thermoplastic resin composition according to claim 1, wherein the amount of the thermoplastic resin (A) is 100 parts by weight, the amount of the particles (B) is 0.2 to 10 parts by weight, and the amount of the dye (C) is 0.0001 to 1 part by weight.

5. A thermoplastic resin molded product obtained by molding the thermoplastic resin composition according to claim 1.

6. (A) a thermoplastic resin, (B) at least one type of particle selected from spherical crosslinked polymer particles and mica particles, and (C) Fluorescent dye A masterbatch for a thermoplastic resin comprising: A masterbatch for a thermoplastic resin, comprising 6 to 100 parts by weight of particles (B) per 100 parts by weight of a thermoplastic resin (A).

Citation Information

Patent Citations

  • Coating composition

    JP1989313575A

  • Building board

    JP1993059213A

  • Thermochromic molding composition which can reversibly change its color from silvery metallic glossy color and product prepared by molding same

    JP1994107852A

  • Surface luminescent aromatic polycarbonate resin composition

    JP1997020860A

  • Sheetlike laminated structure having high design effect and utilization thereof

    JP2003053908A